betaFeedback

WorksPhysics and Astronomy

High-throughput screening of Heusler alloys for thermoelectrics combining machine-learned densities of states and first-principles transport

Abstract

Thermoelectrics turn waste heat into electricity, but finding new ones requires transport calculations too costly for whole databases. Searches therefore choose what to calculate from the electronic density of states (DOS), increasingly predicted by machine learning, yet such choices are rarely tested. We test them on all 106,235 Heusler structures in the DXMag database, screening 51,257 on density-functional spectra and 54,978 on neural-network predictions, and judging both by 3,625 band-structure and transport calculations. A DOS-derived Seebeck indicator ranks most compounds passing every transport and stability test within the top 1% of their population, and ten of the eleven established half-Heusler thermoelectrics calculated pass. Predicted spectra lose most band gaps, unnoticed by spectral-similarity metrics, yet still rank passing compounds near the top. The screen certifies 80 computational candidates, 61 without reported measurements. Computed or predicted, the DOS can choose what to calculate; only a band structure shows whether a gap exists.

Introduction

Thermoelectric generators convert a temperature difference directly into electrical power and could recover part of the heat that industry and transport reject [1, 2]. Their efficiency is measured by the dimensionless figure of merit zT=S2σT/(κe+κL)zT = S^2 \sigma T/(\kappa_e + \kappa_L), where SS is the Seebeck coefficient (the thermopower), σ\sigma the electrical conductivity, TT the temperature, and κe\kappa_e and κL\kappa_L the electronic and lattice thermal conductivities [3]. The numerator, the power factor S2σS^2 \sigma, is governed by the electronic structure and by the scattering of the carriers. The figure of merit is largest in a doped semiconductor whose chemical potential lies near a band edge, provided that the band gap is wide enough for carriers thermally excited across it not to reduce the thermopower [4]. On the electronic side, a search for new thermoelectrics is therefore a search for semiconductors with suitable band edges.

First-principles calculations can predict the power factor. From a density-functional-theory (DFT) band structure they compute SS and σ/τ\sigma/\tau, the conductivity per relaxation time τ\tau, usually in the constant-relaxation-time approximation (CRTA), in which every electronic state has the same τ\tau [5, 6, 7, 8, 9]. Each such calculation needs a self-consistent DFT run, a band structure on a dense mesh of wavevectors and an interpolation of the bands. Large searches therefore first rank or filter compounds with a cheaper electronic-structure signal, such as a density-of-states (DOS) effective mass [10], a gap near the Fermi level [11] or features of the DOS itself [12]. Such a signal decides which compounds receive a transport calculation at all. Whether a DOS-based decision selects the compounds that the transport calculation would confirm, and whether it still does so when the DOS itself comes from a machine-learning model, has rarely been tested at scale.

Heusler compounds offer a clear baseline for this test, because simple electron-counting rules already predict many of their semiconductors. Half-Heusler compounds (composition XYZ) with eight or eighteen valence electrons per formula unit are often semiconducting, because these counts fill the bonding states formed by hybridisation of the atoms on the different sublattices [13, 14]. The best half-Heusler thermoelectrics have eighteen: n-type MNiSn and p-type MCoSb alloys (M = Ti, Zr, Hf) [15, 16], NbFeSb [17], ZrCoBi [18] and TaFeSb [19] reach figures of merit near or above one at high temperature. Full Heuslers (X2_2YZ) follow the same pattern at 24 valence electrons: Fe2_2-based compounds with this count have large calculated power factors [20], and some full-Heusler semiconductors are predicted to have very low lattice thermal conductivity [21]. Because the good compounds sit at these closed-shell electron counts, counting electrons is already a strong screen, and a DOS screen of this family is useful only if it does better. Heusler compounds are also numerous and structurally varied. They include regular and inverse full-Heusler and half-Heusler prototypes, dozens of elements on each site, and cubic and tetragonal forms of each composition; for many full Heuslers the tetragonal form is the calculated ground state [22]. Transport screens have so far concentrated on cubic structures, above all on half-Heuslers [23, 24], so the tetragonal and metastable structures remain largely unexamined.

The DXMag Computational HeuslerDB of Xiao and Tadano contains these structures [25, 26] (Figure 1a). Like an earlier high-throughput Heusler library [27], it was built to find magnetic materials. Each of 27,864 combinations of composition and prototype was relaxed from several magnetic and tetragonal starting configurations, and every inequivalent energy minimum reached was kept. The result is 106,235 entries, each with its energy and its distance from the convex hull, a measure of thermodynamic stability. A companion archive gives spin- and orbital-resolved DFT densities of states for about half of the entries[28], matched to the database by identifier, these are the lowest-energy cubic entry of every composition and prototype and the tetragonal entries that are ground states. The database contains no charge or thermoelectric transport, only anomalous Hall and Nernst conductivities for 671 entries. Its documentation (https://www.nims.go.jp/group/spintheory/database/) also states that the structures, energies and DOS were computed without spin–orbit coupling (SOC), which splits and shifts the band edges of heavy-element Heuslers[29, 30]. A thermoelectric search of DXMag therefore has the structures it needs, but it must decide from the DOS which of them to calculate, and half of them have no DFT DOS.

Figure 1. One database, two populations. a, The DXMag Heusler database: 27,864 composition–prototype pairs, relaxed from several magnetic and tetragonal starting configurations, give 106,235 energy minima (entries). Its DOS archive holds the spin- and orbital-resolved DFT DOS of the lowest-energy cubic entry of every pair and of the tetragonal entries that are ground states. These 51,257 entries form the training set (vermilion; triangles in later figures): they train the ALIGNN model (30 fold models), and each also receives an out-of-fold prediction. The other 54,978 entries form the prediction set (blue; circles), screened on the five-model mean of the predicted d-DOS and its spread uFu_F. Thumbnails: the DFT d-DOS of the training-set ZrNiSn entry and the predicted d-DOS of the prediction-set ZrNiSn entry (±2.4 eV; spin down below). b, Entries per family, set and state. c, Energy of each prediction entry above its same-family, same-composition training entry (51,103 entries; logarithmic axis); dotted line, 1 meV atom−1^{-1}; 15.1% of all prediction entries lie below 1 meV atom−1^{-1}, most likely relaxations that returned to the training crystal. d-DOS, d-orbital-projected density of states; ALIGNN, atomistic line graph neural network.

A screen can read a gap from the DOS in two ways (Figure 2a–Figure 2c). The simpler is a binary label that asks whether the d-orbital-projected DOS (d-DOS) has a gap at the Fermi level EFE_F. The other follows from transport theory and uses more of the spectrum. The electronic transport coefficient are moments of the transport distribution Σ(ε)∝∑nkvnk2τnkδ(ε−εnk)\Sigma(\varepsilon) \propto\sum_{nk} v_{nk}^{2}\tau_{nk}\delta(\varepsilon-\varepsilon_{nk}), which measures how much current the states at energy ε\varepsilon can carry; εnk\varepsilon_{nk}, vnkv_{nk} and τnk\tau_{nk} are the energy, velocity and relaxation time of an electron in band nn with wavevector kk. The moments are taken over the Fermi window −∂f/∂ε-\partial f/\partial\varepsilon, where ff is the Fermi–Dirac distribution; the window is a few kBTk_BT wide, with kBk_B the Boltzmann constant, so only states near the chemical potential μ\mu contribute. The conductivity is the zeroth moment. The Seebeck coefficient is the first moment divided by the zeroth, that is, it is set by the mean energy of the current-carrying states relative to μ\mu. If v2τv^{2}\tau is the same for all states in the window, Σ(ε)\Sigma(\varepsilon) reduces to the DOS g(ε)g(\varepsilon), and the thermopower takes the Cutler–Mott form[31, 32]. In this form S(μ)S(\mu) is large only where the window-weighted DOS is small and asymmetric about μ\mu, that is, at a band edge or in a gap. Its largest value grows with the width of the gap, as in the Goldsmid–Sharp estimate Eg≈2e∣S∣max⁡Tmax⁡E_g \approx2e|S|_{\max}T_{\max}, where ee is the elementary charge and Tmax⁡T_{\max} the temperature of the thermopower maximum[33, 34]. The second reading of the DOS, which we call the Seebeck indicator, is the largest value of this S(μ)S(\mu). Unlike the label, it weighs how far states lie from μ\mu on the scale of the thermal energy.

Figure 2. From a d-DOS to a screening decision. a, DFT d-DOS of ZrNiSn (training set), per stored cell as screened: spin up above, spin down below; occupied solid, empty tinted; valence d peaks between −1.9-1.9 and −1.5-1.5 eV are clipped (maximum 30). Grey band, the d-DOS gap (spin-summed d-DOS below 0.15 states eV−10.15\ \mathrm{states}\ \mathrm{eV}^{-1}; 0.570.57 eV, against a QE-PBE band gap of 0.500.50 eV). Right, the label test: both spin channels below 0.150.15 (dashed) within ±0.03\pm0.03 eV of EFE_{\mathrm{F}} (dark band). Fermi-window moments (Eqs. (3) and (4)) at the μ\mu of Smax⁡dS_{\max}^{\mathrm{d}}; gg (states eV−1 cell−1\mathrm{eV}^{-1}\ \mathrm{cell}^{-1}) and the scaled window wμw_{\mu} at 900 K (top); gwμg w_{\mu} (bottom), whose larger weight below μ\mu gives L1<0L_{1}<0 and S>0S>0. c, S(μ)S(\mu) (μV K−1\mu\mathrm{V}\ \mathrm{K}^{-1}) and S2L0S^{2}L_{0} (104 μV2 K−2 states eV−110^{4}\ \mu\mathrm{V}^{2}\ \mathrm{K}^{-2}\ \mathrm{states}\ \mathrm{eV}^{-1}) over the ±1\pm1 eV scan for the DFT and the held-out ML-predicted d-DOS of the same crystal (dashed), both per cell; circles, Smax⁡dS_{\max}^{\mathrm{d}}; diamonds, Pmax⁡dP_{\max}^{\mathrm{d}} at μ∗\mu^{*}. The screen ranks ∣S∣|S|; its sign depends on where μ\mu lies. The strip gives the calculated thermopower at 900 K, referred to the QE Fermi level and so kept off the μ\mu axis. d, Descriptor ledger; numbered badges mark the same descriptors in a–c and f (grey: reported only). e, Four calculated training-set entries (tick: the μ\mu of Smax⁡dS_{\max}^{\mathrm{d}}). f, Selection in each set: priority filters order but exclude nothing; bars, runs by the criterion that ordered their round (Supplementary Table S6); criteria (i)–(v) as in § 2.6. d-DOS in archive units (twice the physical values); QE-PBE, Quantum ESPRESSO with the PBE functional; CRTA, constant-relaxation-time approximation; SOC, spin–orbit coupling.

We read both from the d-DOS because the gaps of transition-metal Heuslers open between d-derived states formed by hybridisation of the transition-metal sublattices[13, 35, 36]; the price is that s- and p-derived states inside the d gap are not seen. The d-DOS is also resolved by spin, so that the label can tell half-metals, which are gapped in one spin channel only, and exchange-split magnets apart from non-magnetic semiconductors; the indicator reads the spin sum.

The Cutler–Mott derivation also shows where the approach is expected to fail. A constant v2τv^{2}\tau is a poor assumption at band extrema, where the velocities vanish. For a non-degenerate parabolic band with its edge at ε0\varepsilon_0, Σ∝(ε−ε0)3/2\Sigma\propto(\varepsilon-\varepsilon_0)^{3/2} whereas g∝(ε−ε0)1/2g \propto(\varepsilon-\varepsilon_0)^{1/2}, and the extra power of (ε−ε0)(\varepsilon-\varepsilon_0) in Σ\Sigma raises the mean energy of the current-carrying states by kBTk_BT, so the DOS form underestimates ∣S∣|S| by kB/e≈86 μV K−1k_B/e \approx86\ \mathrm{\mu V\ K^{-1}}, an error comparable with the thermopower thresholds that screens apply.

The conductivity, moreover, depends on the band velocities and on the valley degeneracy and the band mass separately, whereas the DOS combines degeneracy and mass into a single DOS effective mass [37, 38, 39]. Together with the form of the thermopower derived above, these limits lead to two expectations that the calculations of this study can test. A DOS-based indicator should recognise gap-like electronic structure, and so help to choose what to calculate, but it should not rank compounds by power factor. A binary label, which ignores the thermal window, should do worse than the Seebeck indicator.

For the half of DXMag without a DFT spectrum, a machine-learned model is the practical source of one: computing the missing spectra would take 54,978 further DFT calculations, fifteen times the number of transport calculations they are meant to prioritise. Machine-learning models now predict the DOS of a crystal from its composition and structure [40, 41, 42, 43, 44, 45, 46]; among them are atomistic line graph neural networks (ALIGNN) [47], which have been trained on tens of thousands of spectra [43]. Thermoelectric screens assisted by machine learning have instead learned transport labels directly [48, 49]. The closest DOS-based study evaluated a gap feature of predicted spectra on one hundred new DFT calculations, but against the DFT DOS rather than against transport [50]. A good average fit does not show that predicted spectra support screening decisions. A screen depends on whether a gap exists at EFE_F, and modest spectral errors can fill a gap [46] or shift EFE_F [42, 51]. More generally, accurate regression does not guarantee accurate selection [52], especially near a threshold [53, 54]. Apparent accuracy can also be inflated by random splits [55], by near-duplicate entries [56, 57] and by overlap between pretraining and test data [58, 59]. If a screen fails on predicted spectra, it could fail for two different reasons: the DOS may be a poor signal, or the model may be a poor source of it. Only the same screen, run on DFT spectra and assessed in the same way, can tell the two apart.

DXMag makes this separation possible, because its DOS archive divides it into two sets of similar size. We call the 51,257 entries with a DFT d-DOS the training set: they can be screened on their own DFT spectra, and they train the model. The other 54,978 entries form the prediction set, which can be screened only on spectra predicted by an ALIGNN model trained on the training set. Every training entry also has an out-of-fold predicted spectrum, made by the cross-validation model for which it was a test entry, so the fidelity of predicted spectra can be measured on crystals whose DFT spectra are known. The two sets share their compositions but, apart from near-duplicates, not their structures: the prediction set holds the other minima of the same compositions, almost all of them higher in energy. Both are screened by the same code and judged by the same first-principles protocol (Figure 2f). We screen each set separately, select entries for calculation in score-ordered rounds, and assess them in 3,625 first-principles runs, each a Quantum ESPRESSO band structure followed by a BoltzTraP2 transport calculation, recomputing runs of heavy-element compounds with SOC. Because the screen itself chose what to calculate, with only some rounds sampling entries that it would reject, the calculations measure how well the screen concentrates the compounds that pass; they cannot measure how many it misses. Four questions organise the results. (Q1) Does a gap in the d-DOS at EFE_F, read from DFT or from predicted spectra, identify compounds that are gapped in a band-structure calculation? (Q2) Does the Seebeck indicator, on either kind of spectrum, concentrate the entries that pass the first-principles criteria; does it add to electron counting; and does it rank them? (Q3) How do SOC and the choice among structural variants change which entries pass? (Q4) Which compositions pass, and how do they relate to known and less-explored thermoelectric chemistry? The first three questions test the screen. The fourth uses it, and its answer is a list of computational candidates, not of measured thermoelectrics.

Data and methods

The study applies one screen to two kinds of spectra. A difference in outcome can be attributed to the source of the spectra only if both populations are screened by the same code, the predicted spectra come from a documented model, and one recorded first-principles protocol selects and assesses the entries of both. Section 2.1 describes the database and the two populations, Sec. 2.2 the model, Sec. 2.3 the screening indicators, Sec. 2.4 the selection of entries, Secs. 2.5 and 2.6 the first-principles calculations and the certification criteria, and Sec. 2.7 the evaluation; Table 1 summarises where the two populations nonetheless differ.

training setprediction set
Population
entries (DXMag UUIDs)51,25754,978
what the entries arelowest-energy cubic entry of every composition and prototype; lowest tetragonal entry where it is the ground state2,595 lowest tetragonal minima without a spectrum; 52,383 further metastable minima
compositions (strings / reduced formulas)18,792 / 14,58017,149 / 14,291
energy above the training entry of the same family and composition0 (by construction)median 32 meV atom−1^{-1}; 15.1% within 1 meV atom−1^{-1}
DXMag hull distance < 0.10 eV atom−1^{-1}6.0%3.3%
electron-count rule: 18 (half) / 24 (full, inverse)2.5% / 3.1%2.0% / 3.6%
DXMag phonon results8,198 entriesnone
Screen
d-DOS screenedDFT d-DOS of the archive, per stored cellensemble-mean prediction, per atom
label threshold, physical units0.025 (half) or 0.019 (full, inverse) states eV−1^{-1} atom−1^{-1} per spin0.075 states eV−1^{-1} atom−1^{-1} per spin
d-DOS labels: semiconductor / half-metal / metal1,550 / 962 / 48,7452,394 / 473 / 52,111
ensemble-spread priority filternoneuFu_F below its 75th percentile
First-principles assessment
runs (QE-PBE + BoltzTraP2)1,5622,021
certified entries / compositions76 / 7579 / 79

Table 1. The two populations and how each is screened. DXMag release 2025-09-09. Composition strings keep the DXMag site order, so they distinguish half-Heusler site permutations; reduced formulas do not. Label thresholds are converted to physical units (archive factor of two removed); the training-set screen reads the d-DOS per stored primitive cell of three or four atoms. QE-PBE: Quantum ESPRESSO PBE calculations (Sec. 2.5); certified: passing all criteria of Sec. 2.6; uFu_F: ensemble spread (Sec. 2.2); UUID: identifier of a DXMag entry. Per-family values are given in Supplementary Table S1.

Two density-of-states populations from one database

The database. All structures and reference data come from the ternary, DFT-computed part of DXMag [25, 26], metadata release 2025-09-09 (CC BY 4.0; https://www.nims.go.jp/group/spintheory/database/); its machine-learned quaternary and all-d entries [26] are not used. The 27,864 combinations of composition and prototype draw on 41 elements (27 d-block metals, La, Lu and twelve elements of groups 13–15). They comprise 9,396 half-Heusler XYZ, 9,072 regular and 9,072 inverse X2_2YZ, and 324 X3_3Z compounds, which we group with the full Heuslers. Each combination was relaxed with the Vienna Ab initio Simulation Package (VASP), projector-augmented-wave (PAW) potentials and the Perdew–Burke–Ernzerhof (PBE) functional, collinearly spin-polarised and without SOC or a Hubbard correction (as documented on the database page). The relaxations started from several magnetic configurations and a series of tetragonal strains, and every inequivalent minimum, distinguished by energy and magnetic moments, was kept. This gives 106,235 entries: 27,864 ground states and 78,371 metastable states. Each entry lists its cell, positions, energy, formation energy, magnetic moments and distance from a convex hull built with the competing phases of the Open Quantum Materials Database (OQMD, version 1.6) [25, 60, 61]. For a subset, harmonic phonons are given at the commensurate qq-points of a 22×22×22\sqrt{2} \times2\sqrt{2} \times2 supercell. We group the entries into six families: the full, half and inverse prototypes, each in a cubic (Fm3ˉmFm\bar{3}m, F4ˉ3mF\bar{4}3m) and a tetragonal (I4/mmmI4/mmm, I4m2I4m2) form.

Two populations. Spin- and orbital-resolved DOS are distributed separately, as the HeuslerDB electronic-DOS dataset [28] (VASP-PBE, primitive cell [25], pymatgen format [62]). Its archives contain 51,257 spectra, all of which we used, although the record description quotes 51,373. Matched to the database by identifier, the files follow a simple rule: every composition and prototype has the spectrum of its lowest-energy cubic entry, and the lowest-energy tetragonal entry has one where it is the ground state. DOS availability therefore splits the database into two populations of similar size (Table 1). The training set, 51,257 entries with a DFT spectrum, trains the DOS model and is screened on its own DFT spectra. The prediction set, the other 54,978 entries (2,595 lowest tetragonal minima without a spectrum and 52,383 further metastable minima), is screened on predicted spectra (Supplementary Figure S1). Every prediction entry shares its composition with a training entry. Of the 51,103 prediction entries that also have a training entry of the same family, none lies below it, and the median energy difference is 32 meV atom−1^{-1}; 15.1% of all prediction entries lie within 1 meV atom−1^{-1} of their training counterpart, most likely relaxations that returned to the same crystal. The prediction set thus samples alternative configurations of known compositions, not new chemistry. The two sets are screened and evaluated separately throughout and meet only in the final list of compositions.

Figure S1. The two sets and the learning target. a, Entries per structural family in the training set (DFT d-DOS available) and the prediction set (no DOS). b, Energy of each prediction-set entry above the training entry of the same family and composition, for the 51,103 prediction entries that have one; values below 0.01 meV atom−1^{-1} are drawn in the first bin. No prediction entry lies below its training sibling; the dotted line marks 1 meV atom−1^{-1}. c, The learning target for one held-out training entry (CoTiAl, a gapped half-Heusler): the dd-projected DOS per spin channel on the 2,001-point grid, spin down drawn negative. Shaded bands mark the ±2 eV window of the L±2\mathcal{L}_{\pm2} loss term and of the r±2 eVr_{\pm2\,\mathrm{eV}} metric and the ±3 eV window of the slope term; the curve at the bottom is the 700 K Fermi-window weight of the loss (xref)Eq. (S3). Values carry the archive’s factor-of-two normalisation (Note 1). (Detailed version of the target shown in main-text Figure 3 and Figure 4.)

Structures, units and counting. The crystal graphs that the model reads (Sec. 2.2) are built from the structure stored with each spectrum (training set) or from the DXMag cell and positions (prediction set), without relaxation. The archive spectra carry a uniform factor of two: integrating the archive’s spin-resolved total DOS up to EFE_F gives twice the DXMag magnetisation (median ratio 2.00 over 150 magnetic entries; Supplementary Note 1, Figure S2 and Table S2). Archive spectra, model targets and predictions therefore all carry this factor relative to physical values; ratios are unaffected, and absolute thresholds are converted where they matter. We count in three units. An entry is one DXMag record, identified by its universally unique identifier (UUID). A run is one first-principles calculation; of 3,625 runs, 1,562 belong to the training set, 2,021 to the prediction set and 42, run under a composition name without a UUID, to neither. A composition merges entries with the same DXMag composition string across families and sets; because the string keeps the site order, half-Heusler site permutations count as different compositions. Prediction entries that share composition, family and space group with a training entry and differ from it by less than 5 meV atom−1^{-1} in DXMag energy and 1% in volume are near-duplicates (Supplementary Note 2). The reference crystal of a composition is its calculated entry of lowest DXMag energy, and a structural variant is any other calculated entry at least 5 meV atom−1^{-1} above it. Compounds are named conventionally in the text and figures (ZrNiSn for the DXMag string NiZrSn, whose first element occupies the tetrahedral site); Supplementary tables list DXMag strings, and Supplementary Table S3 gives both. Throughout, EFE_F in a d-DOS (model target, label and indicators) is the Fermi level of the archive spectrum; in our first-principles calculations it is their own Fermi level (Sec. 2.5).

Normalisation of the DOS archive

Figure S2. Normalisation of the DOS archive. Moment from the archive’s spin-resolved total DOS, per formula unit of the stored structure, divided by the DXMag magnetisation, for 25 magnetic entries per family (Supplementary Note 1). Dotted lines mark ratios of 1 and 2.

The spin-resolved d-DOS model

Target. For each training entry the archive provides the d-projected DOS Nsd(E)N_s^d(E) of spin channel ss, summed over sites and orbitals, for a structure of NN atoms. The model learns the per-atom d-DOS on a fixed grid of energies measured from EFE_F:

gs(Ek)=max⁡[0,1NNsd(EF+Ek)],Ek=−10+0.01k eV,(1)g_s(E_k)=\max\left[0,\frac{1}{N}N_s^d(E_F+E_k)\right],\qquad E_k=-10+0.01k\ {\rm eV}, \tag*{(1)}

with k=0,…,2000k=0,\ldots,2000; the archive spectra are interpolated linearly onto this grid, without smoothing. The two spin channels together form a vector of 4,002 values (Figure 3a, right). The reasons for the d projection and the spin resolution are given in Sec. 1.

Figure 3. The d-DOS model and its Fermi-focused loss, as implemented. a, Each crystal becomes an atom graph (nodes, atoms; edges, bonds to nearest neighbours) and a line graph (nodes, bonds; edges, pairs of bonds that share an atom, carrying the bond angle). The stock encoder of the atomistic line graph neural network (ALIGNN; grey outline) is followed by the parts specific to this model (blue): a mean over atoms, a three-layer head drawn with bar length proportional to layer width (from the 512 pooled features), and a softplus that keeps the spin-resolved d-DOS non-negative; “two columns identical”: the d-electron count enters twice. Inset energy axis, E−EFE - E_{\mathrm{F}} (eV). The inset is the held-out training-set spectrum at the median rr (DFT d-DOS vermilion, prediction blue). b, The weight w(E)w(E) of LF\mathcal{L}_{\mathrm{F}} as implemented (logarithmic axis), and the energy range, spin channels and weight of each of the five terms of Eq. (2). Settings are those of all 30 fold models (§ 2.2).

Representation and architecture. The model is an atomistic line graph neural network47^{47}, which encodes each crystal as two graphs (Figure 3a). In the atom graph, edges join each atom to its nearest neighbours (12 nearest neighbours with a neighbour-search radius of 8 Å, the settings of the ALIGNN graph builder) and carry radial-basis expansions of the bond length. In the line graph, the nodes are bonds, and the edges join bonds that share an atom and carry the cosine of the angle between them, so that three-body geometry enters the atom features. The line graph matters here because the cubic and tetragonal forms of a Heusler prototype differ in bond angles as well as bond lengths. Each atom starts from 97 features. Ninety-two are the one-hot encoding of nine elemental properties introduced with the crystal graph convolutional neural network (CGCNN)63^{63} and used by default in ALIGNN. The other five are Heusler-motivated: the d-electron count (included twice), the largest magnitude of a common oxidation state, the distance of the d count from half or full filling, and the period of the d shell. These columns are per-atom proxies for the valence-electron counts on which the electron-counting rules of Heuslers rest [13, 14]. The model receives no magnetic moments, so it must infer magnetic order and exchange splitting from the structure alone. The ALIGNN encoder is used without modification apart from its size: eight ALIGNN layers, each an edge-gated convolution on the line graph followed by one on the atom graph, and eight further atom-graph convolutions, all 512 features wide, where the published configuration uses four, four and 256[47]. The task-specific parts are a three-layer head (512, 1,024, 2,048 and 4,002 units, Gaussian error linear unit (GELU) activations, dropout 0.2) acting on the atom-averaged features, and a softplus output, ln⁡(1+ex)\ln(1 + e^x), that keeps the predicted DOS non-negative.

A loss focused on the Fermi level. Thermoelectric screening reads the DOS within a few kBTk_{\mathrm{B}}T of EFE_{\mathrm{F}}, so the loss weights that region most strongly (Figure 3b):

L=0.35LF+0.35L±2+0.15Lcos⁡+0.10Lslope+0.05Lsort.(2)\mathcal{L} = 0.35\mathcal{L}_{\mathrm{F}} + 0.35\mathcal{L}_{\pm2} + 0.15\mathcal{L}_{\cos} + 0.10\mathcal{L}_{\mathrm{slope}} + 0.05\mathcal{L}_{\mathrm{sort}}. \tag*{(2)}

The first two terms are mean-squared errors near EFE_{\mathrm{F}}. LF\mathcal{L}_{\mathrm{F}} is weighted by the Fermi window w(E)=−∂f/∂Ew(E) = -\partial f/\partial E at 700 K, normalised to unit mean over the grid, so that its weight at EFE_{\mathrm{F}} is 83 times the average and 98.7% of it lies within ±0.3\pm0.3 eV; L±2\mathcal{L}_{\pm2} is the mean-squared error within 2 eV of EFE_{\mathrm{F}}. The other three terms compare the spectra as a whole: Lcos⁡\mathcal{L}_{\cos} is the cosine distance between predicted and DFT spectra; Lslope\mathcal{L}_{\mathrm{slope}} compares first and (with weight 0.1) second finite differences within 3 eV of EFE_{\mathrm{F}}, for the spin-up channel only; and Lsort\mathcal{L}_{\mathrm{sort}} is the L1 distance between the sorted values of the two spectra, taken over both spins and all energies. Equations are given in Supplementary Note 3. No term rewards a DOS of exactly zero, so a small residual DOS inside a gap costs little (§ 3.2). The training temperature (700 K) is lower than the screening temperature (900 K), so the window used in training is slightly narrower than the one the indicators use.

Training and prediction. Each family was split by shuffled five-fold cross-validation (seed 42): in each fold, 72% of the family trained a model, 8% served for validation and 20% tested it, giving 30 models. The family models were to be fine-tuned from an all-family model pretrained on every training spectrum;

the run records confirm this for two of the 30 models and leave the parent of the others unconfirmed (Supplementary Table S4 and Figure S3). All were trained with the AdamW optimiser, a reduce-on-plateau learning-rate schedule and stochastic weight averaging (SWA)[64] over the last fifth of the epochs (settings in Supplementary Table S5): 300 epochs with batch size 128 (cubic full Heuslers: 150 or 200 epochs, batch size 64), learning rate 10−310^{-3} and weight decay 5×10−55 \times10^{-5}. Each fold model kept two sets of weights: a best-validation checkpoint, which gives all held-out metrics, and the SWA weights, which give all predictions. Each prediction-set structure was passed through the five SWA models of its family, and the predicted d-DOS is the mean of their outputs. The population standard deviation of the five outputs, us(E)u_{\mathrm{s}}(E), measures their spread; its average over ∣E−EF∣≤2\lvert E - E_{\mathrm{F}}\rvert\le2 eV and both spin channels is uFu_{\mathrm{F}}. Every training crystal was a test entry for one of the five models but a training or validation entry for the other four, so a prediction entry that nearly duplicates a training crystal receives a spectrum close to that crystal’s fitted, in-sample spectrum. Because the pretraining saw every spectrum that later served as a test entry, the held-out metrics of any fine-tuned model are upper bounds. The provenance records are given in Supplementary Note 3, the model and its deployment in Supplementary Figs. S4 and S5, and the implementation details that earlier internal descriptions of the workflow stated differently in Supplementary Note 4.

Figure S3. Training record of cubic full-Heusler fold 1, the only fine-tuning run whose log survives (TensorBoard scalars). a, Training and validation loss. b, Validation Pearson correlation over the concatenated spectra (the selection metric) and the mean per-spectrum correlation within ±2 eV. c, Learning rate of the encoder group, halved by the plateau schedule and set to 5×10−55 \times10^{-5} by the SWA schedule. The dotted line marks the best-validation checkpoint (epoch 2), the green band the SWA window (epochs 120–149).

DOS-derived screening indicators

Fig. 2 shows each descriptor on a real spectrum and how it is used; panel d summarises what each one reads, its role and what it cannot establish. Indicators. As outlined in Sec. 1, replacing the transport distribution[6] by the spin-summed d-DOS g=g↑+g↓g = g_{\uparrow} + g_{\downarrow}, that is, assuming the same v2τv^2\tau for all states in the window, gives the Cutler–Mott form of the thermopower[31, 32]. With the Fermi window wμ(E)=−∂f/∂Ew_{\mu}(E) = -\partial f/\partial E at T=900T = 900 K, the temperature of interest for half-Heusler power generation,

Ln(μ)=∑kg(Ek)wμ(Ek)(Ek−μ)nΔE,(3)L_n(\mu) = \sum_k g(E_k)w_\mu(E_k)(E_k-\mu)^n\Delta E, \tag*{(3)}
S(μ)=−1eTL1(μ)L0(μ),(4)S(\mu) = -\frac{1}{eT}\frac{L_1(\mu)}{L_0(\mu)}, \tag*{(4)}

with ee the elementary charge, ΔE=0.01\Delta E = 0.01 eV, and μ\mu scanned over EF±1E_F \pm1 eV in steps of 0.02 eV. L0L_0 is the DOS averaged over the thermal window around μ\mu, L1L_1 measures how unevenly the states in the window lie above and below μ\mu, and L2L_2 how widely they are spread about μ\mu; S(μ)S(\mu) is thus the mean energy of the window-weighted states relative to μ\mu, divided by −eT-eT. Four indicators are formed:

Smax⁡d=max⁡μ∣S(μ)∣,Pmax⁡d=max⁡μS2L0,S_{\max}^{\mathrm d} = \max_\mu|S(\mu)|,\qquad P_{\max}^{\mathrm d} = \max_\mu S^2L_0,
ξ=(kBT)2L2/L0−(L1/L0)2∣μ∗,L0∗=L0(μ∗),(5)\xi= \left.\frac{(k_{\mathrm B}T)^2}{L_2/L_0-(L_1/L_0)^2}\right|_{\mu^*},\qquad L_0^* = L_0(\mu^*), \tag*{(5)}

where μ∗\mu^* maximises S2L0S^2L_0. The dd-DOS Seebeck indicator Smax⁡dS_{\max}^{\mathrm d} is the largest thermopower that a shift of μ\mu within 1 eV, that is, doping, could reach. Because S(μ)S(\mu) is large only where the window-weighted DOS is small and asymmetric, next to a band edge or a deep minimum, and its maximum grows with the width of a gap[33, 34], Smax⁡dS_{\max}^{\mathrm d} acts as a gap detector smoothed over the thermal window. The other three indicators are Pmax⁡dP_{\max}^{\mathrm d}, the power-factor analogue, in which L0L_0 takes the place of the conductivity; ξ\xi, an inverse energy variance of the transport window, motivated by the argument of Mahan and Sofo that a narrow distribution of carrier energies favours a large figure of merit[65]; and L0∗L_0^*, the window-weighted DOS at the optimum. Smax⁡dS_{\max}^{\mathrm d} and ξ\xi do not depend on the overall scale of gg, whereas Pmax⁡dP_{\max}^{\mathrm d} and L0∗L_0^* do. For 13% of entries in each set the optimum μ∗\mu^* lies at the edge of the scan, where Pmax⁡dP_{\max}^{\mathrm d} and L0∗L_0^* are lower bounds. All four indicators are evaluated in Supplementary Table S12; the main text uses Smax⁡dS_{\max}^{\mathrm d} and Pmax⁡dP_{\max}^{\mathrm d}.

The dd-DOS gap label. An entry is labelled a semiconductor if both spin channels fall below 0.15 states eV−1^{-1} (archive units) somewhere within 0.03 eV of EFE_F, a half-metal if only one does and the spin polarisation at EFE_F exceeds 0.9 in magnitude, and a metal otherwise. The dd-DOS gap is the width of the contiguous region around EFE_F in which gg stays below the same threshold. Because the label tests each channel separately but the gap is measured on their sum, a semiconductor label can carry a gap of zero width (541 training and 1,156 prediction entries). The same code screens both sets, but its input is normalised differently. The prediction set is screened on the per-atom ensemble mean, whereas the training-set screen reads the archive dd-DOS per stored primitive cell, without dividing by its three or four atoms. In physical units the label threshold is therefore 0.075 states eV−1^{-1} atom−1^{-1} per spin in the prediction set and 0.025 or 0.019 in the training set, three to four times stricter (Table 1). Smax⁡dS_{\max}^{\mathrm d} and ξ\xi, which do not depend on the scale of gg, are unaffected, and raw indicator values and label rates are compared only within a population. Two baselines are evaluated alongside the indicators: an earlier composite of four dd-DOS features at EFE_F, computed for the prediction set only, which ordered part of the first selection round (Supplementary Note 5), and the electron-count rule, which flags half-Heuslers with 18 and full and inverse Heuslers with 24 valence electrons.

Selection of entries for first-principles assessment

Entries were calculated in nine successive rounds (Figure 2f). Three priority filters were recorded for each entry: a semiconductor label with a dd-DOS gap of 0.10–1.00 eV; stability (DXMAg hull distance below 0.10 eV atom−1^{-1}, negative formation energy and no phonon instability, that is, DXMAg neither marks the entry unstable nor lists a frequency below −5-5 cm−1^{-1}; an entry lacking a value passed); and, for the prediction set, a model spread uFu_F below its 75th percentile over all families. The filters ordered the selection and excluded nothing. Later rounds, and the analyses below, use a wider gap range, a dd-DOS gap of 0.10–1.40 eV, chosen after the first results. Within each round, entries were grouped into tiers of dd-DOS gap or of model confidence (uFu_F) and ordered within a tier by Pmax⁡dP_{\max}^{\mathrm d} or Smax⁡dS_{\max}^{\mathrm d}; some rounds deliberately sampled other labels (Supplementary Note 2, Table S6 and Figure S6). Because the rounds drew on the two sets in different proportions, the sets were sampled differently. Rounds 7 and 8, ordered by label tiers, supplied 1,318 of the 2,021 prediction-set runs (65%) but 338 of the 1,562 training-set runs (22%), and no certified entry (certification in § 2.6). No round was random, so outcome rates are conditional on the selection, and the screen’s recall, the fraction of all passing compounds that it would find, is not measured. Smax⁡dS_{\max}^{\mathrm d} was identified as the best prioritiser only retrospectively. All indicator values and labels analysed here are those of the final screen.

roundordering criterionrunsTPn/ad-DOS SCDFT gappedqualified runscertified
1highest Pmax⁡dP_{\max}^{d} (early version) and largest ensemble spread564197367054521410061
2Pmax⁡dP_{\max}^{d} order within tiers2842840016325172
3Pmax⁡dP_{\max}^{d} order after priority filters55342612704801898745
4top 100 by Pmax⁡dP_{\max}^{d} among gap-filter rejects10060132740140
5Pmax⁡dP_{\max}^{d} order after semiconductor and gap filters1946611414156280
6Smax⁡dS_{\max}^{d} order, no filters2721898211361197147
7semiconductor label, gap ≥0.714\ge0.714 eV first, by Smax⁡dS_{\max}^{d}40510030504052370
8semiconductor label in confidence tiers (0.10–1.40 eV first)1,2512381,01301,251350
918 or 24 valence electrons22002000
all3,6251,5622,021423,142575309155

Table S6. Provenance of the 3,625 DFT runs by selection round. Rounds were built successively, each ordered by the screening scores current at the time (Methods). T and P give the number of runs from the training and prediction sets, and n/a the runs that could not be attributed. d-DOS SC: runs labelled semiconducting by their set’s screen. DFT gapped: QE-PBE gap of at least 0.136 eV. Qualified runs pass the Seebeck, power-factor and stability criteria.

Figure S6. Selection of entries for DFT. Share of each set’s screened entries that were computed, by d-DOS screen label (a,b; the screened population per label is printed above the bars) and by percentile of the d-DOS Seebeck indicator Smax⁡dS_{\max}^{\mathrm d} within the set (c,d). Selection followed the scores through nine successive selection rounds (Table S6).

First-principles electronic structure and spin–orbit coupling

Self-consistent field (SCF) and non-self-consistent (NSCF) calculations used Quantum ESPRESSO (QE)[66, 67] with the PBE functional[68], the efficiency set of the Standard Solid-State Pseudopotentials (SSSP)[69], Marzari–Vanderbilt smearing of 0.01 Ry[70] and Monkhorst–Pack meshes[71]. Wavefunction cutoffs were set to the largest SSSP value among the species (30–90 Ry; for SOC, 1.15 times the value of the fully relativistic potentials), and the SCF threshold was 10−810^{-8} Ry. The meshes had ni=max⁡(6,round⁡(K/∣ai∣))n_i = \max(6,\operatorname{round}(K/|a_i|)) points along the ii-th reciprocal-lattice direction, where aia_i is the ii-th lattice vector, with K=40K = 40 Å for the shifted SCF mesh and 55 Å for the unshifted NSCF mesh. Every calculation used the DXMAg structure, symmetrised and reduced to its primitive cell with spglib at a tolerance of 10−310^{-3} and not relaxed further (Supplementary Table S7). Compounds containing V, Cr, Mn, Fe, Co or Ni were calculated spin-polarised from ferromagnetic starting moments, with one antiparallel retry on failure; the others were calculated without spin polarisation. Each run’s electronic class follows from its NSCF eigenvalues: metallic if every spin channel has a band crossing EFE_F, half-metallic if some but not all do, and otherwise gapped if the smallest band gap over channels is at least the smearing width, 0.136 eV, and narrow-gap below it. We refer to these calculations as QE-PBE, to the electronic class as the QE-PBE class and to this band gap as the QE-PBE gap. It is read on the NSCF mesh, which for 1,846 runs (98 of the 155 certified entries) is an odd, unshifted mesh that does not contain the X and L points of the face-centred-cubic Brillouin zone; for half-Heuslers whose conduction-band minimum lies at X these gaps are upper bounds.

Runs of compounds containing an element with atomic number Z≥72Z \ge72 (Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Tl, Pb or Bi; 1,956 runs) were eligible for a non-collinear recalculation with SOC. It was attempted for 330 of the 337 gapped and 55 of the 68 narrow-gap runs, for 245 of the 254 metallic runs that met the Seebeck and power-factor criteria, (i) and (ii) of Sec. 2.6, and for 63 other metallic runs. Of these 693 attempts, 607 finished and 86 failed and were not retried (Supplementary Table S8). Each SOC calculation reused the cell, positions and kk-meshes of its scalar-relativistic partner (verified for all pairs) and converged to a non-magnetic state, as did all its scalar partners. It used fully relativistic PSlibrary PAW potentials [72] (version 1.0.0; 0.3.1 for Co and Mn, 0.2.3 for Ir), cutoffs set per compound, enough spinor bands to match the scalar band window, the same smearing and the same transport extraction, so that paired quantities are defined identically. The pairs differ in the pseudopotential family as well as in the treatment of relativity, and a same-potential scalar control was not performed, so paired differences are those of the fully relativistic recalculation as a whole.

Transport and certification

Transport coefficients were computed with BoltzTraP[26] from the NSCF eigenvalues (interpolation multiplier 15) in the constant-relaxation-time approximation (CRTA):

Σαβ(ε)=e2τNk∑n,kvnk,αvnk,β δ(ε−εnk),(6)\Sigma_{\alpha\beta}(\varepsilon)=\frac{e^{2}\tau}{N_{k}}\sum_{n,\mathbf{k}}v_{n\mathbf{k},\alpha}v_{n\mathbf{k},\beta}\,\delta(\varepsilon-\varepsilon_{n\mathbf{k}}), \tag*{(6)}
Λαβ(m)(μ,T)=1V∫Σαβ(ε)(ε−μ)m[−∂f∂ε] dε,(7)\Lambda_{\alpha\beta}^{(m)}(\mu,T)=\frac{1}{V}\int\Sigma_{\alpha\beta}(\varepsilon)(\varepsilon-\mu)^{m}\left[-\frac{\partial f}{\partial\varepsilon}\right]\,\mathrm{d}\varepsilon, \tag*{(7)}

with σ=Λ(0)\sigma=\Lambda^{(0)} and S=−(eT)−1[Λ(0)]−1Λ(1)S=-(eT)^{-1}[\Lambda^{(0)}]^{-1}\Lambda^{(1)}, where NkN_k is the number of kk-points, VV the cell volume and α,β\alpha,\beta Cartesian directions. Unlike Eq. (3), these expressions include the band velocities of all bands. Spin channels were merged with a common τ\tau, tensors were reduced to a third of their trace, and the power factor is reported per relaxation time, PF/τ=S2σ/τ\mathrm{PF}/\tau=S^{2}\sigma/\tau, from 300 to 1200 K. Coefficients were evaluated at the grid point nearest the QE Fermi level, the undoped point, and with μ\mu optimised for PF/τ\mathrm{PF}/\tau within ∣μ−EF∣≤0.5|\mu-E_F|\leq0.5 eV, which represents doping. For gapped runs the QE Fermi level is fixed by the smearing and lies anywhere in the gap (6–94% of the gap above the valence-band maximum in a sample of 80 runs), so the undoped point is a convention rather than an intrinsic chemical potential. For ranking, the window was widened to 1.0 eV and the carrier concentration nn, counted from the undoped point, was capped at ∣n∣≤1020|n|\leq10^{20} or 1021 cm−310^{21}\,\mathrm{cm}^{-3}, separately for hole (p-type) and electron (n-type) doping; points whose Seebeck sign contradicts the carrier type were excluded. Runs completed before the correction of a driver error, which had interpolated the self-consistent instead of the NSCF eigenvalues, were recomputed; we call this the mesh correction (Supplementary Fig. S7).

A run, and the entry it belongs to, is certified if it passes five criteria in sequence: (i) the Seebeck criterion, ∣S∣>60 μV K−1|S|>60\,\mu\mathrm{V\,K}^{-1} at the undoped point at some temperature; (ii) the power-factor criterion, a best PF/τ\mathrm{PF}/\tau, over temperature and over the undoped and the optimised μ\mu, above PF/τ0=1.09×1012 W m−1 K−2 s−1\mathrm{PF}/\tau_0=1.09\times10^{12}\,\mathrm{W\,m}^{-1}\,\mathrm{K}^{-2}\,\mathrm{s}^{-1}; (iii) the stability criterion, a DXMag hull distance below 0.10 eV atom−10.10\,\mathrm{eV\,atom}^{-1}; (iv) a scalar-relativistic QE-PBE gap of at least 0.136 eV; and (v) for compounds with Z≥72Z\geq72, criterion (ii) re-evaluated with SOC. Runs passing (i)–(iii) are qualified; qualified, gapped runs with Z≥72Z\geq72 are the SOC candidates; heavy-element runs without a finished SOC calculation are not certified. The threshold PF/τ0\mathrm{PF}/\tau_0 is the median 900 K value of the first 1,401 completed runs; it was set during the campaign and then held fixed. The same median over mesh-corrected runs, 1.15×1012 W m−1 K−2 s−11.15\times10^{12}\,\mathrm{W\,m}^{-1}\,\mathrm{K}^{-2}\,\mathrm{s}^{-1}, would certify 77 compositions (Supplementary Table S9), and the development of the criteria is recorded in Supplementary Note 6, Table S10 and Fig. S8. The stability threshold is stricter than the 0.22 eV atom−1^{-1} that Xiao and Tadano calibrated on experimentally known Heuslers [25]. Because the best PF/τ\mathrm{PF}/\tau is taken over 300–1200 K while PF/τ0\mathrm{PF}/\tau_0 is a 900 K median, the power-factor criterion falls with high temperature; counts at 900 K are therefore reported alongside, and the sensitivity of the certified count to every threshold is given in Supplementary Table S9. For ranking, each composition is represented by its certified entry with the highest PF/τ\mathrm{PF}/\tau, and compositions are compared on ∣S∣|S| and PF/τ\mathrm{PF}/\tau at 900 K and ∣n∣≤1021 cm−3|n|\leq10^{21}\,\mathrm{cm}^{-3}, with μ\mu in the widened window, for p- and n-type doping separately and with SOC values for heavy compounds; we call this the ranking convention. Pareto layers follow from non-dominated sorting: the first layer holds the compositions that no other composition exceeds in both ∣S∣|S| and PF/τ\mathrm{PF}/\tau for the same carrier type. Certification is a computational status under the CRTA, not a figure of merit: τ\tau and κL\kappa_L are not computed.

Evaluation

Held-out spectra. Each training entry was predicted once, by the best-validation checkpoint of the fold in which it was a test entry. Pearson’s correlation coefficient rr between predicted and DFT spectra was computed per spectrum, over all 4,002 values and within 2 eV of EFE_F, and compared with three baselines that involve no trained model: the family-mean DOS, the DOS of the nearest entry, and the mean DOS of the five nearest entries in element-fraction space. A spectrum is flagged as gapped when gg falls below 0.05 states eV−1 atom−1\mathrm{eV}^{-1}\,\mathrm{atom}^{-1} (archive units) anywhere within 1 eV of EFE_F. With the DFT flag as truth, gapped spectra that the model flags as true positives (TP) and those it misses false negatives (FN); non-gapped spectra are true negatives (TN) or false positives (FP). The recall is TP/(TP + FN), the fraction of gaps that the model detects, and the balanced accuracy (BA) and Matthews correlation coefficient (MCC) are

BA=12[TPTP+FN+TNTN+FP],(8)\mathrm{BA}=\frac{1}{2}\left[\frac{\mathrm{TP}}{\mathrm{TP}+\mathrm{FN}}+\frac{\mathrm{TN}}{\mathrm{TN}+\mathrm{FP}}\right], \tag*{(8)}
MCC=TP TN−FP FN(TP+FP)(TP+FN)(TN+FP)(TN+FN).(9)\mathrm{MCC}=\frac{\mathrm{TP}\,\mathrm{TN}-\mathrm{FP}\,\mathrm{FN}}{\sqrt{(\mathrm{TP}+\mathrm{FP})(\mathrm{TP}+\mathrm{FN})(\mathrm{TN}+\mathrm{FP})(\mathrm{TN}+\mathrm{FN})}}. \tag*{(9)}

Screening performance. Indicators were evaluated within each population on the calculated entries (1,562 training-set and 2,016 prediction-set entries; five prediction entries were calculated twice), with certified entries as positives. We report the area under the receiver-operating-characteristic curve (ROC-AUC), computed as the Mann–Whitney statistic, that is, the probability that a randomly chosen certified entry outranks a randomly chosen uncertified one; the area under the precision–recall curve (precision–recall AUC); and the recovered fraction R(q)R(q), the fraction of all certified entries that lie within the top fraction qq of calculated entries ranked by the indicator, for which random ordering gives qq. ROC-AUC differences were assessed by a paired bootstrap over entries (2,000 resamples), which captures sampling variation within the calculated set but not the effect of the selection. Rank correlations are Spearman’s ρ\rho.

Paired and literature comparisons. SOC effects are summarised over the 607 paired runs by the change of electronic class, the gap difference for runs gapped in both calculations, and the ratio of best PF/τ\mathrm{PF}/\tau values; structural variants are compared with the reference crystal of their composition in the same way. Each certified composition was searched in the literature under its conventional name and assigned the strongest thermoelectric evidence found for the same composition in the same structure type: established (a benchmark in reviews), measured (thermoelectric measurements reported), computed only, or no study found. Compositions whose experimentally reported phase is not the Heusler structure, or for which DFT places another structure below the half-Heusler, were flagged. Every source was checked against its Crossref record (Supplementary Table S3). The audit is targeted rather than exhaustive, and the known-compound check involves no numerical comparison with published coefficients. The distribution is bimodal (Figure 1c), with 15.1% of the set within 1 meV atom−1^{-1}, most likely relaxations that returned to the training crystal.

Results

The screening task

In this study a candidate must be gapped and near-stable (criteria iii and iv of § 2.6), and both properties are rare in DXMag. Judged by their own d-DOS, both populations are overwhelmingly metallic: only 1,550 training entries (3.0%) and 2,394 prediction entries (4.4%) carry a semiconductor label, and 671 and 603 of these have a d-DOS gap within the 0.10–1.40 eV gap range (Figure 2f). Near-stable entries are similarly scarce. Only 6.0% of the training set and 3.3% of the prediction set lie within 0.10 eV atom−1^{-1} of the hull, and no prediction entry lies on it (Table 1). By its own labels, fewer than one entry in a hundred is both gapped and near-stable, so the screen has to find a small minority among metals. The prediction set also lies higher in energy than the training set: its entries lie a median 32 meV atom−1^{-1} above their training counterpart, consistent with its smaller near-stable share.

Predicted spectra reproduce shape but not gaps

Every prediction-set indicator inherits the errors of its predicted spectrum, so we first ask how good these spectra are. On held-out training spectra the mean per-spectrum Pearson correlation with DFT is 0.895 (0.874–0.925 by family; Supplementary Figs. S9–S11 and Table S11). The baselines reach 0.488 for the family-mean spectrum, 0.501 for the nearest composition and 0.605 for the mean of the five nearest (Figure 4d); they involve no pretraining, so the comparison favours the model. Across the range of quality, from the tenth to the ninetieth percentile of rr (Figure 4c), peak positions and band widths are reproduced. The one systematic exception, the filled Zn 3d band near −7 eV of twelve Zn-rich prediction entries, lies outside the screening window (Supplementary Note 3).

Figure 4. Predicted spectra reproduce the shape of the d-DOS but miss most gaps. All panels use the 51,257 held-out training-set spectra, each predicted by the best-validation checkpoint of the fold that held it out; DFT d-DOS as vermilion fill, ML prediction as blue line, spin down below. a,b, ZrNiSn (half-Heusler, 18 valence electrons) and half-metallic Co2_2MnSi with their d-DOS gap labels (∣P∣\lvert P\rvert, spin polarisation at EFE_\mathrm{F}); shading, the d-DOS gap of the label (spin-summed DFT d-DOS below 0.15 around EFE_\mathrm{F}: 0.72 eV for ZrNiSn, none for Co2_2MnSi, whose label rests on one spin channel). Labels in a,b are read per atom, the prediction-set convention, so the ZrNiSn d-DOS gap differs from the per-cell reading of Figure 2a (0.57 eV). c, Entries nearest the 10th to 90th percentiles of per-spectrum Pearson rr; “gap missed” refers to the flag of e. d, rr by family (violins above r=0.4r = 0.4; numbers, spectra below it) and the all-family mean rr of three baselines (grey lines). e, Held-out gap flag, a test separate from the screening label (spin-summed d-DOS below 0.05 anywhere within 1 eV of EFE_\mathrm{F}; DFT as truth); missed gaps in purple. f, Distributions of rr within 2 eV of EFE_\mathrm{F} for the cells of e. DOS values are in archive units, a factor of two above physical values (§ 2.1); the metrics are upper bounds, because pretraining, where used, saw the test spectra (§ 2.2). d-DOS, d-orbital-projected density of states.

Table S11. Held-out d-DOS fidelity by family and DFT outcome per set (complements main-text Figure 4). NtrainN_{\mathrm{train}} and NpredN_{\mathrm{pred}} are the training- and prediction-set sizes. rˉ\bar{r} and rˉ±2 eV\bar{r}_{\pm2\ \mathrm{eV}} are mean per-material Pearson correlations over the full spectrum and within 2 eV of EFE_F; RMSE is in states eV−1atom−1\mathrm{eV}^{-1}\mathrm{atom}^{-1} (archive units). BA and rec. are the balanced accuracy and recall of the held-out d-DOS gap flag. These metrics are upper bounds (best-validation checkpoints; for fine-tuned models the pretraining saw the test spectra). DFT runs and certified compositions are given for the training (T) and prediction (P) sets; PdScAs is certified in two training-set families, so the T rows sum to 76 while the set contains 75 compositions. Baselines on the same held-out spectra: rˉ=0.488\bar{r}=0.488 (family-mean DOS), 0.501 (nearest composition), 0.605 (mean of five nearest compositions).

Gaps are not reproduced. Of the 5,130 held-out spectra whose DFT d-DOS is gapped within 1 eV of EFE_\mathrm{F}, the model flags 778, a recall of 0.15; the balanced accuracy (Eq. (8)) is 0.57 and the Matthews correlation coefficient (Eq. (9)) 0.25 (Figure 4e). The recall varies about eightfold between families, from 0.04 (inverse cubic) to 0.33 (full tetragonal), and is 0.21 for the cubic half-Heuslers that dominate the candidates (Supplementary Table S11). The spectral metric does not register the failure, because a gap is a narrow interval of near-zero weight: filling it barely changes the correlation over the whole spectrum. Spectra with a missed gap have a median rr of 0.909, against 0.912 for correctly non-gapped spectra, and within 2 eV of EFE_F they score higher, 0.889 against 0.866. Spectra in which the model does detect a gap are, by contrast, less faithful (median rr within 2 eV of EFE_F, 0.84; Figure 4f). The misses are systematic, a smoothing of the spectrum across the gap (Figure 4a–Figure 4c).

Several features of the model favour this error. A squared error is small for small values: a residual 0.1 states eV−1^{-1} inside a gap costs one hundredth of a unit error at a d-band peak. The Fermi weight raises the cost by up to 83 near EFE_F, but it falls off within about 0.3 eV, so in gaps several tenths of an electronvolt wide much of the residual lies where the weight is small. If the Fermi level of the archive spectra falls at varying positions inside a gap, as it does in our QE runs (Sec. 2.6), the band edges relative to EFE_F vary between similar compounds, and a least-squares fit averages them into the gap. Finally, the softplus output approaches zero only asymptotically, and the five-model mean used for the prediction set can only add weight where one member places an edge. Two familiar compounds show the two forms that the error takes (Figure 4a,Figure 4b). For ZrNiSn the predicted band edges lie too far apart, so the predicted d-DOS gap is wider than the DFT one, yet residual weight inside it halves the thermopower that a screen would read from the prediction (§ 3.5). For the half-metal Co2_2MnSi the spin-down gap is partly filled, and the label read from the prediction is metal. A further limitation, unrelated to gaps, is that the model receives no magnetic information. It infers the magnetic state, and with it the exchange splitting, from the geometry alone, so distinct magnetic minima at nearly the same geometry receive nearly the same spectrum.

These metrics come from best-validation checkpoints and, for fine-tuned models, from spectra that the pretraining had already seen, so they are upper bounds; the deployed five-model mean was not evaluated on held-out spectra. Because these conditions favour the model, the true gap recall on unseen crystals is unlikely to exceed 0.15. A predicted spectrum can thus be trusted for its shape but not for whether it has a gap near EFE_F, which is what a screen reads. Similar failures have been reported for other machine-learned DOS models: gaps lost to residual in-gap weight[46] or a misplaced EFE_F[51], as well as spurious predicted gaps[50].

A binary gap label fails as a classifier even on DFT spectra

Question Q1 asks whether the d-DOS gap label identifies gapped compounds. On predicted spectra the label could fail simply because the spectra are wrong, so the training set provides the decisive test: there the label reads DFT spectra, and it can be compared with the QE-PBE class of each calculated run (Figure 5a,Figure 5d). Of the 1,170 calculated semiconductor-labelled runs of the training set, 738 (63.1%) are QE-PBE metals and 23 half-metals, so 761 lack a gap in at least one spin channel. In the prediction set, where the labels come from predicted spectra, 1,678 of 1,972 (85.1%) are metals. The failures concentrate outside the gap range. Runs with a near-zero d-DOS gap (below 0.10 eV) are 94% (training) and 98% (prediction) metallic, many of them carrying a zero-width gap, and wide d-DOS gaps above 1.40 eV, common only in the prediction set, are almost all metallic there. Within the gap range, by contrast, 27–73% of training-set runs and 32–51% of prediction-set runs are gapped, depending on the d-DOS-gap tier (Figure 5a,Figure 5d), against at most 0.4% of runs labelled metallic, half-metallic or near-zero-gap. The label thus narrows the search by two orders of magnitude, yet most entries it passes are still metals.

Figure 5. The gap label passes mostly metals; the Seebeck indicator places the certified entries at the top. Top, training set (DFT d-DOS); bottom, prediction set (predicted d-DOS). a,d, QE-PBE class of the calculated runs in each d-DOS gap label (M, metal; HM, half-metal; otherwise gap tier in eV); numbers above the bars, runs; white numbers, gapped share; hatching, labels with fewer than 20 runs. b,e, Calculated entries placed by the rank of Smax⁡dS_{\max}^{\mathrm{d}} within their own population (top fraction, logarithmic, higher rank to the right) and grouped by first-principles outcome (exclusive lanes, so “gapped” means gapped but not certified; entries per lane on the right); bars above each lane, interquartile range and median; upper strip, share of each rank bin that was calculated; certified entries dark green with a dark edge; triangles, training set; circles, prediction set. c,f, Share of certified entries kept when only the highest-ranked fraction of calculated entries is retained, for each screening score (dotted, random order; initial composite, the four-feature d-DOS score that ordered part of the first round, Supplementary Note 5); the key gives the value at 20%. Panels b,c,e,f count entries (1,562 and 2,016; five prediction-set entries were calculated twice), a,d runs. d-DOS, d-orbital-projected density of states; QE-PBE, Quantum ESPRESSO calculation with the PBE functional.

On DFT spectra the failure cannot come from a model, and two features of the label can explain it. The first is the d projection: the d-DOS gap of a gapped entry lies on or above its QE-PBE gap, as expected when s and p states inside a d-orbital gap are ignored (Supplementary Fig. S12); ZnCdAs, a metal with a 1.13 eV d-DOS gap, is an extreme case (Figure 2e). The second is the fixed threshold: a semiconductor label needs only that both spin channels dip below 0.15 states eV−1^{-1} somewhere within 0.03 eV of EFE_{\mathrm{F}}, so a spectrum with a deep minimum near EFE_{\mathrm{F}} passes, and 541 semiconductor-labelled training entries have a d-DOS gap of zero width (Sec. 2.3). The selection rounds show what this costs in practice (Supplementary Table S6). The two rounds ordered by label tier (one of them by Smax⁡dS_{\max}^{\mathrm{d}} within its tiers), 1,656 runs drawn from semiconductor-labelled entries of lower priority, produced 26 gapped and no certified runs, whereas the round ordered by Smax⁡dS_{\max}^{\mathrm{d}} alone produced 119 gapped and 47 certified runs of 272. Later rounds drew on what earlier ones had left, so this contrast overstates the difference, but the label by itself did not find the compounds that transport calculations certify.

A gap is required for certification, but its width also matters. Among gapped runs, the share that passes the Seebeck, power-

factor and stability criteria rises with the QE-PBE gap and is highest for gaps of 0.6–1.2 eV (53–61% in the training set, 58–61% in the prediction set; Supplementary Fig. S12). The rise is consistent with bipolar suppression of the thermopower in narrow-gap compounds at high temperature, where carriers excited across the gap reduce ∣S∣|S|1. The decline beyond 1.2 eV, by contrast, is not physical: the ±0.5\pm0.5 eV chemical-potential window of the certification, measured from a Fermi level that the smearing places somewhere inside the gap, cannot reach the band edges of wide-gap entries.

What the transport calculations certify

The certification criteria (Sec. 2.6) define the entries that an indicator should find. Applying the criteria in sequence shows which of them shape the final list (Figure 6). The Seebeck and power-factor criteria keep 40% of the training-set runs and 19% of the prediction-set runs. Stability then removes three-quarters (training) and three-fifths (prediction) of what remains, and the gap requirement removes 61 and 47 qualified runs, almost all metals (57 and 45). These metals pass the power-factor criterion only when the chemical potential is shifted by several tenths of an electronvolt, a shift that a metal, with its large DOS at EFE_{\mathrm{F}}, cannot sustain. SOC then removes 21 and 19 heavy-element runs that fall below PF/τ0\tau_0, and five and one more remain unresolved without a finished SOC calculation (Sec. 3.6). The result is 76 certified training-set entries (75 compositions) and 79 certified prediction-set entries (79 compositions). Their union contains 80 compositions: 74 certified in both sets, five only in the prediction set (Rh-containing half-Heuslers with Hf, Ta or Bi whose training entries were left unresolved by failed SOC calculations) and one, ScPdAs, only in the training set.

Figure 6. Each criterion removes runs; the certified entries of both sets map to 80 compositions. Calculated runs passing the criteria of Sec. 2.6 in sequence; training set left (vermilion), prediction set right (blue). Bar length is logarithmic in the number of runs (bars start at 10 runs); rows (i)–(v) as in Sec. 2.6 and Fig. 2f; white numbers give runs that pass, grey numbers runs removed, and “kept” the percentage of the runs entering a criterion that pass it. The spin–orbit-coupling (SOC) step also removes heavy-element runs without a finished SOC calculation (five training-set, one prediction-set). The tiles give certified compositions by set.

The thresholds that bind are the hull cut and the power factor, not the thermopower. The certified count is unchanged for Seebeck thresholds between 40 and 100 μV K−1^{-1}, but it moves from 49 to 104 compositions for hull cuts of 0.025 to 0.15 eV atom−1^{-1} and from 105 to 65 for power-factor thresholds of 0.8 to 1.2 PF/τ0\tau_0 (Supplementary Table S9). The criteria were set during the campaign, so the cascade describes the final protocol, not a prospective test.

The Seebeck indicator prioritises but does not rank

Question Q2 asks whether the Seebeck indicator concentrates these entries. Ranked by Smax⁡dS_{\max}^{\mathrm{d}}, the certified entries sit at the top of each population, with median ranks in the top 0.7% (training) and 0.2% (prediction), whereas metals spread across the entire calculated range (Figure 5b,Figure 5e). The prediction set illustrates this. Its calculated entries reach deep into the population (their median lies 64% of the way down the ranking), yet 72 of the 79 certified entries are among the 1,000 highest-ranked of 54,978. Keeping only the fifth of the calculated entries with the highest Smax⁡dS_{\max}^{\mathrm{d}} retains 75% of the certified training-set entries and 91% of the certified prediction-set entries, against 20% for random ordering; in the training set this would cut the calculations needed per certified entry from about 21 to about 5.5 (Figure 5c,Figure 5f).

The ROC-AUC of Smax⁡dS_{\max}^{\mathrm{d}} is 0.869 (training) and 0.938 (prediction), against 0.649 and 0.877 for the power-factor analogue Pmax⁡dP_{\max}^{\mathrm{d}} (paired-bootstrap differences +0.221 [0.171, 0.267] and +0.061 [0.047, 0.076]; Supplementary Tables S12 and S13), and its precision–recall AUC, 0.158 and 0.340, is three to nine times the base rate. The higher prediction-set values do not show that predicted spectra rank better. They can be explained by the selection: 65% of the calculated prediction-set runs, against 22% of training-set runs, come from the low-priority label rounds, which supplied many low-ranked negatives and no certified entry (§ 2.4). Pmax⁡dP_{\max}^{d} does worse because S2L0S^{2}L_{0} rewards a large DOS, which metals have, and because its scale differs between families. The initial four-feature composite, computed for the prediction set only, also ranks the calculated entries less well (ROC-AUC 0.869, 0.068 [0.038, 0.101] below Smax⁡dS_{\max}^{d}), and none of the 100 entries it ranked highest in the whole prediction set was certified (Supplementary Note 5).

Figure 7. The Seebeck indicator tracks computed thermopower but does not rank power factors. a,b, Smax⁡dS_{\max}^{d} (Eq. (5)) of each run against its QE-PBE + BoltzTraP2 maximum undoped ∣S∣|S| (at the QE Fermi level) over 300–1200 K, for the 1,562 training-set (a, DFT d-DOS) and 2,021 prediction-set runs (b, predicted d-DOS), coloured by QE-PBE class; dotted line, the 60 µV K−1^{-1} criterion. The dashed box in a marks the 97 metals with Smax⁡d>400S_{\max}^{d} > 400 µV K−1^{-1}, 85 of them 16- or 17-electron half-Heuslers (open triangle, ZrNiSn of Figure 2). c, Valence electrons per formula unit of these 97 metals (grey) and of the 76 certified training-set entries (dark green); shaded, the closed-shell counts 18 and 24. d,e, Smax⁡dS_{\max}^{d} against QE-PBE gap for the gapped runs of each set; line, Eg=2eSTE_g = 2eST at 900 K, the fixed-temperature form of the Goldsmid–Sharp estimate used here. f, Percentile rank of Smax⁡dS_{\max}^{d} within the certified entries of each set (76 and 79) against best PF/τ\tau. ρ\rho, Spearman’s rank correlation. Sets share a panel only in f (within-set ranks); 42 runs not attributable to one set are omitted; transport in the constant-relaxation-time approximation. d-DOS, d-orbital-projected density of states; QE-PBE, Quantum ESPRESSO calculation with the PBE functional.

These ROC-AUCs come from a score-ordered sample. The hull distance, moreover, enters both a priority filter and criterion (iii), and a feature shared by selection and certification could inflate the apparent performance. On entries that meet the stability criterion alone, however, the ROC-AUCs are 0.873 (training) and 0.927 (prediction), so the shared feature does not drive the result. In the prediction set, all 79 certified entries, and 475 calculated entries in total, are near-duplicates of training entries whose DFT spectra were training targets. This follows mainly from how the database and the model are built: the prediction set holds other minima of the training compositions, and the model, seeing geometry only, gives near-duplicate geometries near-identical spectra. The prediction-set figures therefore test whether the deployed model reproduces decisions for crystals close to its training data, not for new crystals.

Electron counting, the baseline set out in § 1, needs no spectrum at all, so the indicator is worth computing only if it does better. Counting is statistically indistinguishable from the indicator in the training set (ROC-AUC 0.858; difference +0.011 [−0.011, 0.035]) and slightly weaker in the prediction set (0.891). The indicator nevertheless adds information that the rule does not have. Among the 18- and 24-electron entries alone, where the rule has no discriminating power, Smax⁡dS_{\max}^{d} still reaches ROC-AUCs of 0.805 and 0.808 (training and prediction), and 0.829 and 0.836 within the gap range. Among the entries that electron counting already favours, the d-DOS thus separates those that are certified from those that are not.

The indicator works where the label does not because it reads the DOS differently. Smax⁡dS_{\max}^{d} integrates the asymmetry of the DOS over a thermal window several tenths of an electronvolt wide, so it responds to the depth and width of a low-DOS region rather than to a single value below a threshold; a deep minimum raises it even when the minimum is not empty (Fig. 7). Across all calculated runs it tracks the thermopower of the transport calculation, with Spearman correlations of 0.73 (training) and 0.61 (prediction) against the calculated undoped ∣S∣|S|, maximised over temperature (Fig. 7a,b). For gapped runs on DFT spectra it follows the gap closely, as the Goldsmid–Sharp estimate of § 1 suggests: Spearman 0.90 against the QE-PBE gap, with Eg/(2eSmax⁡dT)E_g/(2eS_{\max}^{d}T) a median 0.78 (Fig. 7d). This ratio is our fixed-temperature analogue of the estimate, evaluated at 900 K

@page 12/42 starts_mid=1 ends_mid=1

Figure 7 (PDF p. 12). The Seebeck indicator tracks computed thermopower but does not rank power factors. a,b, Smax⁡dS_{\max}^{d} (Eq. (5)) of each run against its QE-PBE + BoltzTraP2 maximum undoped ∣S∣|S| (at the QE Fermi level) over 300–1200 K, for the 1,562 training-set (a, DFT d-DOS) and 2,021 prediction-set runs (b, predicted d-DOS), coloured by QE-PBE class; dotted line, the 60 µV K−1^{-1} criterion. The dashed box in a marks the 97 metals with Smax⁡d>400S_{\max}^{d} > 400 µV K−1^{-1}, 85 of them 16- or 17-electron half-Heuslers (open triangle, ZrNiSn of Figure 2). c, Valence electrons per formula unit of these 97 metals (grey) and of the 76 certified training-set entries (dark green); shaded, the closed-shell counts 18 and 24. d,e, Smax⁡dS_{\max}^{d} against QE-PBE gap for the gapped runs of each set; line, Eg=2eSTE_g = 2eST at 900 K, the fixed-temperature form of the Goldsmid–Sharp estimate used here. f, Percentile rank of Smax⁡dS_{\max}^{d} within the certified entries of each set (76 and 79) against best PF/τ\tau. ρ\rho, Spearman’s rank correlation. Sets share a panel only in f (within-set ranks); 42 runs not attributable to one set are omitted; transport in the constant-relaxation-time approximation. d-DOS, d-orbital-projected density of states; QE-PBE, Quantum ESPRESSO calculation with the PBE functional.

of training-set runs, come from the low-priority label rounds, which supplied many low-ranked negatives and no certified entry (§ 2.4). Pmax⁡dP_{\max}^{d} does worse because S2L0S^{2}L_{0} rewards a large DOS, which metals have, and because its scale differs between families. The initial four-feature composite, computed for the prediction set only, also ranks the calculated entries less well (ROC-AUC 0.869, 0.068 [0.038, 0.101] below Smax⁡dS_{\max}^{d}), and none of the 100 entries it ranked highest in the whole prediction set was certified (Supplementary Note 5).

These ROC-AUCs come from a score-ordered sample. The hull distance, moreover, enters both a priority filter and criterion (iii), and a feature shared by selection and certification could inflate the apparent performance. On entries that meet the stability criterion alone, however, the ROC-AUCs are 0.873 (training) and 0.927 (prediction), so the shared feature does not drive the result. In the prediction set, all 79 certified entries, and 475 calculated entries in total, are near-duplicates of training entries whose DFT spectra were training targets. This follows mainly from how the database and the model are built: the prediction set holds other minima of the training compositions, and the model, seeing geometry only, gives near-duplicate geometries near-identical spectra. The prediction-set figures therefore test whether the deployed model reproduces decisions for crystals close to its training data, not for new crystals.

Electron counting, the baseline set out in § 1, needs no spectrum at all, so the indicator is worth computing only if it does better. Counting is statistically indistinguishable from the indicator in the training set (ROC-AUC 0.858; difference +0.011 [−0.011, 0.035]) and slightly weaker in the prediction set (0.891). The indicator nevertheless adds information that the rule does not have. Among the 18- and 24-electron entries alone, where the rule has no discriminating power, Smax⁡dS_{\max}^{d} still reaches ROC-AUCs of 0.805 and 0.808 (training and prediction), and 0.829 and 0.836 within the gap range. Among the entries that electron counting already favours, the d-DOS thus separates those that are certified from those that are not.

The indicator works where the label does not because it reads the DOS differently. Smax⁡dS_{\max}^{d} integrates the asymmetry of the DOS over a thermal window several tenths of an electronvolt wide, so it responds to the depth and width of a low-DOS region rather than to a single value below a threshold; a deep minimum raises it even when the minimum is not empty (Fig. 7). Across all calculated runs it tracks the thermopower of the transport calculation, with Spearman correlations of 0.73 (training) and 0.61 (prediction) against the calculated undoped ∣S∣|S|, maximised over temperature (Fig. 7a,b). For gapped runs on DFT spectra it follows the gap closely, as the Goldsmid–Sharp estimate of § 1 suggests: Spearman 0.90 against the QE-PBE gap, with Eg/(2eSmax⁡dT)E_g/(2eS_{\max}^{d}T) a median 0.78 (Fig. 7d}). This ratio is our fixed-temperature analogue of the estimate, evaluated at 900 K with SS maximised over μ\mu rather than at the temperature of the thermopower maximum. The estimate itself becomes unreliable for gaps well below 10kBT10k_{\mathrm{B}}T, about 0.8 eV at 900 K[34], and the ratio lies below one because the d-DOS gap exceeds the QE-PBE gap. On predicted spectra the relation weakens to a Spearman 0.40, and the median ratio rises to 1.87 (Fig. 7e). Residual weight inside a gap lowers the thermopower that the gap implies: for ZrNiSn the predicted d-DOS gap is wider than the DFT one, but Smax⁡S_{\max} falls from 323 to 166 µV K−1^{-1} (Figure 2c; a certified prediction-set entry is shown in Supplementary Fig. S13). The two readings of the DOS respond differently to this error. Residual weight can flip a threshold label, whereas it only lowers Smax⁡dS_{\max}^{\mathrm{d}}, and for these entries it did not remove the certified ones from the top of the ranking.

In the training set, the indicator’s highest-scoring false positives are mostly 16- and 17-electron half-Heuslers (Fig. 7c; IrZrSn in Figure 2e). Of the 1,115 calculated training-set metals, 97 have an Smax⁡S_{\max} above 400 µV K−1^{-1}, higher than most certified entries, and 85 of them are half-Heuslers with 16 or 17 valence electrons. With one or two electrons fewer than eighteen, these compounds have the 18-electron gap in their d-DOS a few tenths of an electronvolt from EFE_{\mathrm{F}}, so the ±1\pm1 eV scan of μ\mu finds it; the undoped compound, however, is a metal, and only 20 of the 97 reach the 60 µV K−1^{-1} Seebeck criterion. Electron counting removes these compounds, which is why it matches the indicator on DFT spectra. Predicted spectra produce no such metals above 400 µV K−1^{-1}, because their residual weight caps the indicator.

The indicator does not, however, rank the candidates. Among certified entries its rank is only weakly correlated with the calculated power factor (Spearman ρ=0.13\rho= 0.13 and 0.29; Fig. 7f). The certified entries might span too narrow a range for a correlation to appear, but over all gapped runs the correlation is no stronger (0.09 and 0.23), so range restriction does not explain it. This is the behaviour anticipated in Sec. 1: the DOS carries neither band velocities nor valley degeneracy separately from band mass[37, 38, 39], and a constant v2τv^{2}\tau fails at band extrema. For ZrNiSn the calculated thermopower at 900 K is −279 µV K−1^{-1} at the undoped point and +145 µV K−1^{-1} at the power-factor optimum (Figure 2c); neither value can be read off the d-DOS curve, in part probably because the QE Fermi level lies higher in the gap than the archive EFE_{\mathrm{F}}, which sits at the valence-side edge of the d-DOS gap. Candidates are therefore ranked only on computed quantities.

Spin–orbit coupling suppresses p-type power factors of heavy-element candidates

Question Q3 asks how SOC and the choice among structural variants change which entries pass. DXMag was built, and our candidates were first qualified, in the scalar-relativistic approximation, without SOC; a heavy-element candidate is certified only if its power factor survives when SOC is included. Across the 607 paired calculations (Figure 8), SOC narrows gaps: of 264 runs gapped in both calculations, 93% have a smaller gap with SOC, by a median of 56 meV (11% of the scalar gap). It changes the class of 76 runs, 64 of them towards metallic behaviour (Figure 8a,Figure 8b). The gap reduction is largest for W-, Pt- and Au-containing compounds (median 148, 101 and 97 meV) and smallest for Pb and Bi (29 and 32 meV), although Pb and Bi are the heaviest of these elements. What matters, then, appears to be how much heavy-atom character the band edges carry. This is consistent with the character of the edges in 18-electron half-Heuslers: both have strong transition-metal d character, and the valence band is mixed with p states of the main-group atom[13], so a heavy transition metal (W, Pt, Au) contributes to both edges, whereas a heavy main-group atom (Pb, Bi) contributes mainly to the valence band.

Figure 8. Spin–orbit coupling suppresses p-type power factors of heavy-element candidates. Paired scalar-relativistic and spin–orbit-coupling (SOC) calculations of the same structure and kk-meshes (§ 2.5); triangles, training set; circles, prediction set (near-duplicate pairs overlap as a triangle on a circle). a, QE-PBE gap without and with SOC for the 351 runs gapped or narrow-gap in at least one calculation; metallic results at zero; solid line, y=xy=x; dotted, the 0.136 eV gapped/narrow boundary. b, Electronic class of all 607 paired runs, including six not attributable to one set, without (rows, totals in parentheses) and with SOC (columns); shading, row fraction; no half-metals occur because all paired runs converged non-magnetic. c, SOC-to-scalar PF/τ\tau ratio at 900 K and ∣n∣≤1021 cm−3\lvert n\rvert\le10^{21}\ \mathrm{cm}^{-3} of the 115 heavy-element runs gapped and qualified (criteria i–iii) without SOC, for p-type (filled markers) and n-type doping (open markers), each run under the first of its heavy elements in the order shown; bars, medians. d, Best PF/τ\tau (300–1200 K) without and with SOC for the same 115 runs; open markers, Au-containing; shaded, below PF/τ0\tau_0. The paired calculations also differ in pseudopotential family. PF/τ\tau, power factor per relaxation time; PF/τ0\tau_0, the power-factor threshold (§ 2.6); QE-PBE, Quantum ESPRESSO calculation with the PBE functional.

For the SOC candidates, the heavy-element runs that are gapped and qualified in the scalar calculation, the effect falls on the power factor rather than on the gap. Of the 115 with a finished SOC calculation, 40 fall below PF/τ0\tau_{0} with SOC, removing 20 of 60 candidate compositions, yet none of the 40 loses its gap (Figure 8d). A gap check, with or without SOC, would not have caught them. Separating the carrier types shows where the loss occurs (Figure 8c). At 900 K and ∣n∣≤1021|n| \leq10^{21} cm−3^{-3} the p-type power factor of the candidates falls to a median 0.76 of its scalar value, whereas the n-type power factor is unchanged (median 1.00; Supplementary Table S8). Both carrier types are computed with the same potentials, so the asymmetry is unlikely to come from the change of pseudopotential. It is what is expected when SOC splits degenerate valence-band states near the band edge, lifting part of their degeneracy, and affects the conduction-band edge much less, as earlier calculations on AniB half-Heuslers and on ZrNiPb found[30, 73]. This asymmetry explains why the effect depends on the heavy element. Ten of the eleven Au-containing candidate compositions are lost (20 of their 22 runs): their p-type power factor had a median ratio 0.49, and all 22 runs had relied on p-type doping; only HfAuAl remains certified. Bi-containing candidates are weakened on the p-type side too (median 0.76), but none of their 12 runs (seven compositions) is lost, because with SOC nine of them reach their best power factor with n-type doping. For ZrCoBi, this weakening of the p-type side agrees with the slight SOC splitting of its valence bands at LL[18].

The change of pseudopotential cannot be excluded entirely. The 27 gapped pairs whose gap changes by less than 10 meV still have a median PF/τ\tau ratio of 0.89, close to the median over all 607 pairs, 0.87 (Supplementary Figure S14); part of the average reduction may therefore come from the change of potential. HfNiSn, an established thermoelectric that falls 4% below PF/τ0\tau_{0} with SOC, lies within this uncertainty. Two certified entries, a near-duplicate pair of NbOsSb, have a scalar gap of 0.26 eV that closes with SOC. They remain certified because criterion (iv) uses the scalar gap, but they should be regarded as marginal.

Figure S14. Effect of spin–orbit coupling on the best PF/τPF/\tau of completed SOC runs. The SOC runs use fully relativistic PSlibrary potentials, so the ratio also reflects the change of pseudopotential family.

Structural variants rarely change the electronic class

The tetragonal and metastable structures of DXMag were one reason to screen the whole database (Sec. 1). Because the prediction set consists of alternative configurations of known compositions, its calculated members show whether a different structure can turn a composition into a candidate. The calculations include 824 structural variants of 491 compositions, entries at least 5 meV atom−1^{-1} above the reference crystal of their composition (median 33 meV atom−1^{-1}, within the range of known metastable crystals[74, 75]), most of them from the prediction set. Their electronic class rarely changes (Figure 9a). Eight hundred pairs are metallic in both crystals. Of the nine variants whose reference crystal is gapped, six remain gapped, two become metallic and one narrow-gap, with power factors from below 1% to about 100% of the reference value. Four variants of metallic references open a narrow gap; their 6 to 26 times larger power factors reflect how small the metallic reference value is. No calculated variant is gapped where the reference crystal of its composition is not.

Figure 9. Figure 9. Higher-energy structural variants rarely change the electronic class. A variant is a calculated entry at least 5 meV atom−1^{-1} above the reference crystal, the lowest-energy calculated entry of its composition in either set (824 variants of 491 compositions; 661 prediction-set, 163 training-set). a, QE-PBE class of the reference crystal (rows, totals in parentheses) against that of the variant (columns); shading, row fraction; dots, the colours of b. b, Best PF/τ\tau (300–1200 K) of each variant relative to its reference, against its energy above it. Grey points are the 800 pairs metallic in both crystals, and the line their median in energy bins up to 1,000 meV atom−1^{-1} (one metallic variant lies at 3,080 meV atom−1^{-1}); coloured markers are the 24 other pairs, coloured by the class of the reference crystal and outlined where the class changes. Triangles, training set; circles, prediction set. QE-PBE class, electronic class from the Quantum ESPRESSO calculation with the PBE functional. TaIrSn, VNiGa and ScPdAs are the certified compositions with a calculated variant; the other labels name the gapped references whose variant changes class.

Three certified compositions have a calculated variant, and none of the variants improves on its reference crystal (Figure 9b). A tetragonal variant of TaIrSn, 78 meV atom−1^{-1} above the certified cubic crystal, remains gapped (0.79 eV against 0.96 eV) and meets the Seebeck, power-factor and stability criteria with 92% of the reference power factor, but lacks an SOC calculation. A tetragonal variant of VNiGa, 11 meV atom−1^{-1} higher, keeps its gap and 98% of the power factor but lies just beyond the hull cut, and a tetragonal variant of ScPdAs keeps a smaller gap (0.18 eV) and fails the hull cut.

This sample cannot establish a general rule. It contains only nine variants of gapped references; it was selected mostly on predicted spectra, which detect few gaps (held-out recall 0.15); and the QE calculations started from ferromagnetic moments without spin polarisation, so the magnetic minima that define much of the prediction set were recalculated without their own magnetic configurations.

The certified compositions in context

The remaining question (Q4) concerns the certified compositions themselves. Because every certified prediction entry is a near-duplicate of a training entry, the 155 certified entries correspond to about 80 distinct crystals. Supplementary Table S14 lists all 80 compositions. All but six are certified only as cubic half-Heuslers; five are cubic full Heuslers, and one, ScPdAs, is certified in a cubic and a tetragonal entry that are the same crystal within numerical precision. Of the 155 entries, 145 have 18 valence electrons and hence have 24. The 24-electron group is the Fe2_2VAl-type full Heuslers Fe2_2NbAl, Fe2_2TaAl, Fe2_2TiSi, Fe2_2HfSi and Ru2_2ZrSi, with QE-PBE gaps of 0.20–0.37 eV and n-type power factors close to PF/τ0\tau_0, the family in which large calculated power factors were reported before.[20] For each of the 80 compositions DXMag gives phonons for a training-set crystal (release 2025-09-09; prediction entries have none), and all 80 are dynamically stable at the commensurate qq-points, whereas 102 of the 530 calculated training runs with phonon results are unstable. Because phonon stability was one of the priority filters

that ordered the selection, this agreement is not an independent test.

Most of the compounds already known to be good thermoelectrics are on the list. Ten of the eleven established half-Heusler thermoelectrics that were calculated (Supplementary Table S15) are certified, in both populations: TiNiSn, ZrNiSn, TiCoSb, ZrCoSb, HfCoSb, VFeSb, NbFeSb[17], TaFeSb[19], NbCoSn and ZrCoBi[18], reviewed together in refs. 16 and 76. The eleventh, HfNiSn, is the SOC-limited case of § 3.6. On the calculated ∣S∣\lvert S\rvert–PF/τ\tau maps the established compounds lie among the other certified compositions rather than above them: NbCoSn is on the p-type Pareto layer, whereas the established n-type MnNiSn sit below PF/τ0\tau_0 in the n-type map at the ranking convention (Figure 10a,Figure 10b). The CRTA power factor per relaxation time is therefore not a merit order. A targeted literature audit places all 80 compositions on a scale of prior evidence (Figure 10c; Supplementary Table S3). Besides the ten established compositions, nine have reported thermoelectric measurements, among them ScPdSb, ScPtSb and YNiSb[77], YNiBi[78], TaCoSn[79] and NbIrSn[80]; 60 have only computational predictions, at least eleven of them only within high-throughput screens[81, 82]; and for NbNiIn no thermoelectric study was found. Sixty-one of the 80 compositions therefore have no reported thermoelectric measurement of the Heusler phase, including six of the eight compositions on the first Pareto layer, which are listed in Table 2.

Certification plots and composition evidence

Figure 10. Certification recovers the established half-Heuslers among mostly unmeasured compositions. a,b, Computed ∣S∣|S| and PF/τ\mathrm{PF}/\tau of the 80 certified compositions (155 certified entries) at 900 K and ∣n∣≤1021 cm−3|n| \le10^{21}\ \mathrm{cm}^{-3} for p-type (a) and n-type (b) doping, one square per composition, with spin–orbit-coupling (SOC) values for atomic number Z≥72Z \ge72. The black line joins the first Pareto layer (named; Table 2), numbers mark the ten certified established thermoelectrics (key in c), and the dashed line is the power-factor threshold PF/τ0\mathrm{PF}/\tau_0; squares below it pass at another temperature, doping or carrier type. †, NbOsSb, certified on a scalar-relativistic gap (0.26 eV) that closes with SOC. c, Prior thermoelectric evidence (Supplementary Table S3) for all 80 compositions and the eight on the Pareto layer; purple outline, share with an orthorhombic phase. d, The 80 compositions by Z-site element, tiles named without the Z element; right, compositions with a reported (+ predicted) orthorhombic phase. Fill gives the evidence class; a purple outline marks an orthorhombic phase, reported (solid) or predicted (dashed). Fill, from dark to light: established, measured, computed only (outlined), no study found (white, outlined). Fe2_2 and Ru2_2 tiles are 24-electron full Heuslers, all others 18-electron compounds. Values in the constant-relaxation-time approximation.

The audit also flags compositions whose experimentally reported phase is not the half-Heusler, and these flags follow the Z-site element. For 17 certified compositions (six of them only through secondary sources) the reported phase is an orthorhombic TiNiSi- or Co2_2Si-type structure, for example HfCoAs[83] and TaRhGe, and NbRhGe[84] (sources for all 17 in Supplementary Table S3), and for six more DFT places an orthorhombic structure below the half-Heusler[85, 86]. ZrCoAs belongs to the series of arsenides in which orthorhombic HfCoAs was reported[83], but its structure could not be confirmed, and it is not counted. The reported phases cover all six certified half-Heuslers with Si, nine of the twelve compositions with Ge and two of the thirteen with As, but none of the 35 with Sn, Sb or Bi (Figure 10d). Three of the eight first-Pareto-layer compositions carry such a flag, NbCoGe and HfCoAs (reported) and VRhGe (predicted), and ZrCoAs may be a fourth. A convex hull built from the phases of a general-purpose database need not contain the competing ternary phase, so a small DXMag hull distance does not establish the half-Heusler structure, and, conversely, published data for the orthorhombic phase say nothing about the half-Heusler one. For the flagged compositions on the first Pareto layer, phase stability has to be settled before transport.

Any ranking of the certified compositions also depends on the transport conditions at which it is read. All 155 entries reach their best CRTA power factor at 1200 K, the top of the temperature scan, and 94 have their optimum at the edge of the chemical-potential window. At 900 K and ∣n∣≤1021 cm−3|n| \le10^{21}\ \mathrm{cm}^{-3}, the convention used for ranking, 91 entries (47 compositions) remain above PF/τ0\tau_0, and at ∣n∣≤1020 cm−3|n| \le10^{20}\ \mathrm{cm}^{-3} none does. The first Pareto layer at that convention comprises NbCoGe, NbCoSn, TiCoAs, VCoSn, NbRhSn and VRhGe for p-type and HfCoAs, ZrCoAs and TiCoAs for n-type doping (Table 2), all cubic half-Heuslers certified in both sets. Against the best point over all conditions (the earlier best-over-all-conditions set is listed in Supplementary Table S16, and the robustness of the certified set is shown in Supplementary Fig. S15), the ranks agree moderately for p-type doping (Spearman 0.67 for ∣S∣|S|, 0.68 for PF/τ\tau) but hardly for n-type (0.07 and −0.23). At this convention most optima sit at the carrier cap (72 of 80 compositions for p-type, 70 for n-type), so the compositions are compared at nearly fixed carrier concentration. There ∣S∣|S| follows the DOS effective mass, whereas the power factor also depends on the conductivity mass. The certified compositions are therefore best read as a set of computational candidates, and the Pareto layer as one convenient view of that set.

compoundsetEgE_gEhullE_{\mathrm{hull}}SOC\multicolumn{3}{c}{p-type}\multicolumn{3}{c}{n-type}lit.
SSPF/τ\taulayerSSPF/τ\taulayer
TiCoAsT+P1.320.031no3121.481−2811.071C
NbCoGeT+P1.090.000no2801.761−2181.113C*
NbCoSnT+P1.040.039no2881.631−2201.023E
VCoSnT+P0.660.036no3201.281−1720.4711M
VRhGeT+P0.450.050no2911.501−1380.6112C†
NbRhSnT+P0.760.044no2411.821−1390.3916C
HfCoAsT+P1.290.003yes2961.394−2211.351C*
ZrCoAsT+P1.230.006no2741.267−2371.191C

Table 2. Table 2. First Pareto layer of the certified compositions. Non-dominated compositions in computed ∣S∣|S| and PF/τ\tau at 900 K and ∣n∣≤1021 cm−3|n| \le10^{21}\ \mathrm{cm}^{-3}, for p- or n-type doping, among the 80 certified compositions; all are cubic half-Heuslers. Set: certified in the training (T) and prediction (P) sets. EgE_g: QE-PBE gap (eV), from Quantum ESPRESSO with the PBE functional. EhullE_{\mathrm{hull}}: DXMag hull distance (eV atom−1^{-1}). SOC: spin–orbit-coupling values used (Z≥72Z \ge72). SS in µV K−1^{-1}, PF/τ\tau in 101210^{12} W m−1^{-1} K−2^{-2} s−1^{-1} (PF/τ0=1.09\tau_0 = 1.09), mostly at the carrier cap (Sec. 3.8); layer: Pareto layer within each carrier type. Constant-relaxation-time values, not zTzT predictions. Lit.: prior thermoelectric evidence (Supplementary Table S3): E, established; M, measured; C, computed only; *orthorhombic phase reported experimentally; †orthorhombic ground state predicted.

Discussion

A DOS-based screen can ask one descriptor three questions: whether a compound is gapped, whether it deserves a transport calculation, and which compound is best. The calculations give each question a different answer (Table 3). A binary label read from the d-DOS at EFE_F answers the first poorly, even on DFT spectra, because the d projection ignores s and p states inside a d-orbital gap and a fixed threshold accepts a deep minimum as a gap; most entries it passes are metals. The Seebeck indicator answers the second. It reads the DOS as the thermopower does, as an asymmetry about a μ\mu weighted over a thermal window, so it responds to the depth and width of a low-DOS region rather than to a single value below a threshold. The same property makes it tolerant of the main error of predicted spectra: residual weight in a gap lowers Smax⁡dS_{\max}^{\mathrm{d}} but, for the entries calculated here, did not remove the certified ones from the top of the ranking. The certified entries had median ranks within the top 1% of each population, and the indicator still separated them from other entries among the 18- and 24-electron compounds that electron counting already favours. The third question lies beyond the DOS, as the derivation in § 1 predicts. The power factor depends on band velocities and valley structure that the DOS does not contain, and the indicator was only weakly correlated with the calculated power factor, among the certified entries and over all gapped runs alike.

resultrests onestablishesmain qualification
held-out rˉ=0.895\bar{r}=0.895, gap recall 0.15held-out training spectra; best-validation modelsshape reproduced, gaps mostly missedupper bound: pretraining, where used, saw the test spectra
63.1% (T) and 85.1% (P) of labelled semiconductors are metalscalculated runs; DFT (T) or predicted (P) d-DOSthe binary gap label fails as a classifier, even on DFT spectrascore-ordered sample; thresholds differ between sets
top 20% by Smax⁡dS_{\max}^{\mathrm{d}} hold 75% (T) and 91% (P) of certified entriescalculated entries of each setthe indicator prioritisesscore-ordered sample; sets sampled differently (65% of P, 22% of T runs from low-priority label rounds); hull shared with a criterion; P certified entries are near-duplicates of T crystals
ROC-AUC of Smax⁡dS_{\max}^{\mathrm{d}} 0.805 (T), 0.808 (P) among 18- and 24-electron entriescalculated entries of each setthe indicator adds to electron countingscore-ordered sample; rule is family-specific (18 half, 24 full and inverse)
ρ(Smax⁡d,PF/τ)=0.13\rho(S_{\max}^{\mathrm{d}},\mathrm{PF}/\tau)=0.13 (T), 0.29 (P); 0.09, 0.23 over gapped runscertified entries; all gapped runsthe indicator does not rank CRTA power factor per τ\tau
80 certified compositions (47 at 900 K, ∣n∣≤1021 cm−3\lvert n\rvert\le10^{21}\ \mathrm{cm}^{-3})QE-PBE + BoltzTraP2, both setsa CRTA list under declared criteria≈80 distinct crystals; criteria set during the campaign; no τ\tau, κL\kappa_L; wide gaps under-represented
SOC: p-type PF/τ\tau ratio 0.76, n-type 1.00; 40 of 115 SOC-calculated candidates fall below PF/τ0\tau_0607 paired heavy-element runsthe SOC penalty is carrier-selective (p-type)selected subset; pseudopotentials also change
no variant gapped where its reference crystal is not824 calculated variantswithin the calculated sample, variants add no gapped crystal9 gapped-reference pairs; chosen on predicted labels; magnetic states not reproduced
10 of 11 established half-Heuslers certifiedknown compositions calculatedcriteria recover known chemistrytests the criteria, not the ranking

Table 3. What each headline result establishes. T, training set; P, prediction set. Near-duplicates are prediction entries that nearly duplicate a training entry (defined in Sec. 2.1). CRTA, constant-relaxation-time approximation; SOC, spin–orbit coupling.

These answers suggest an order of steps for screens of this kind. Stability comes first, because certification requires it. Electron counting comes with it, because it costs nothing and removes the indicator’s typical high-scoring false positive: a 16- or 17-electron half-Heusler whose 18-electron gap lies within the scanned range of μ\mu but not at EFE_{\mathrm{F}}, which describes 85 of the 97 calculated training-set metals with Smax⁡dS_{\max}^{\mathrm{d}} above 400 μ\muV K−1^{-1}. Smax⁡dS_{\max}^{\mathrm{d}}, from a DFT or a predicted DOS, then orders what remains; in the training set, calculating only the top fifth would have cut the calculations per certified entry from about 21 to about 5.5, at the cost of a quarter of the certified entries. A first-principles band structure then decides whether a gap exists, because neither the label nor a predicted spectrum can. Heavy-element compounds need a fully relativistic recalculation before they are ranked:

SOC moved 40 of the 115 gapped, qualified heavy-element runs below PF/τ0\mathrm{PF}/\tau_0, mostly through the p-type power factor (part of the reduction may come from the change of pseudopotential), and none of them lost its gap. Only explicit transport, ideally with scattering, should rank the certified compounds.

This order leaves phase competition open. A hull built from a general-purpose database need not contain the TiNiSi- and Co2_2Si-type phases reported or predicted for 23 of the 80 certified compositions, all but one of them with Si, Ge or As on the Z site (§ 3.8). For this chemistry a small hull distance is therefore a weaker guarantee of the Heusler structure than its value suggests[87]. Adding these orthorhombic structures to the reference hull would make the stability step of the order meaningful where it is now weakest.

For the machine-learned spectra, the model reproduced the shape of the d-DOS but missed most gaps, and the correlation coefficient by which DOS models are usually judged did not register the failure. On predicted spectra the indicator still placed the certified entries near the top, and the form of the error is consistent with this. Residual weight inside a gap, which an EFE_{\mathrm{F}}-weighted least-squares objective makes cheap (§ 3.2), turns a threshold label into a wrong answer but only compresses the thermopower indicator: on predicted spectra Smax⁡dS_{\max}^{\mathrm{d}} follows the QE-PBE gap with a Spearman correlation of 0.40 instead of 0.90, yet 72 of the 79 certified prediction entries ranked among the 1,000 highest of 54,978. For screening, the useful measure of a DOS model is therefore the fidelity of the decisions made from it: whether a gap is detected, and whether the ranking of entries survives.

The predicted spectra did not, however, extend the list of candidates, and neither did the structural variants. Every certified prediction entry is a near-duplicate of a training entry, including those of the five compositions certified only in the prediction set, whose training entries were left unresolved by failed SOC calculations; the prediction-set figures therefore describe spectra close to the training data. Within the calculated sample, moreover, no variant was gapped where its reference crystal was not: the tetragonal and metastable minima that motivated the screen added structural variety but no candidate. The model sees geometry only, without magnetic moments, and so assigns near-duplicate geometries near-identical spectra; resolving the two spin channels helps the label separate half-metals, but the indicator reads the spin sum, so spin resolution does not change it. The ensemble spread uFu_F ordered the selection, but whether it marks the reliable predictions was not assessed. Three changes would make such a model more useful to a screen, each following from a result here. Gap recall and the yields of screening decisions (for example, the fraction of selected entries that are certified) should be reported alongside spectral metrics, because the correlation missed the failure. Evaluation should use splits that hold out whole compositions in every training stage, because pretraining here saw the test spectra. And the loss should include a term on the weight inside DFT gaps, because the present objective leaves that weight cheap.

The strongest results of this study involve no machine learning: on DFT spectra the gap label fails as a classifier, the Seebeck indicator concentrates the certifiable entries, and transport calculations are needed to rank them. These results rest on a selection ordered by the screen, with criteria set during the campaign, so the screen’s recall is unmeasured and the certified count depends on the thresholds; the list is a prioritised sample, not a census. It is also biased against wide gaps, because the ±0.5\pm0.5 eV window of the certification, measured from a Fermi level placed by the smearing, cannot reach the band edges of many entries with gaps above about 1.2 eV.

The electronic classes also carry the biases of the calculations, two of which act on the gap in opposite directions. PBE underestimates gaps[88, 89], whereas the unshifted NSCF meshes, which miss the X point in many runs, overestimate them where the conduction-band minimum lies there. The QE runs started from ferromagnetic moments or without spin polarisation, so they do not reproduce the magnetic configuration of each DXMag entry, and the magnetic minima of the prediction set were tested as structures only. The undoped point of the Seebeck criterion is set by the smearing, and optima at the edges of the temperature and chemical-potential scans make the reported power factors bounds within the scanned conditions.

The candidate list rests on CRTA transport at the PBE level, without τ\tau, κL\kappa_L, convergence studies or relaxation in QE. Calculations that go beyond the CRTA show how much scattering can change such conclusions. For half-Heuslers, energy-dependent electron–phonon scattering can reorder power factors relative to the CRTA[90] and accounts for their unusually large values[91], and the assumed scattering model changes the predicted benefit of band alignment[92]. In other materials, scattering-resolved calculations have ranked carrier mobilities across a range of semiconductors better than the CRTA[93], improved high-throughput transport predictions for chalcogenides[94] and removed the expected benefit of band convergence in Zintl and full-Heusler compounds[95]. The lattice term, which is not computed here, also varies widely: κL\kappa_L spans more than two orders of magnitude across mechanically stable half-Heuslers[81]. A computational prediction can also be hard to test: an ab initio estimate of zT>2zT>2 for n-type LiZnSb[5] could not be tested, because the samples made were p-type, with zTzT of 0.02–0.08 at 523 K[96].

The model evaluation, finally, is favourable by construction: pretraining overlapped the test spectra, the splits were random within families, the parent of 28 of the 30 models is unconfirmed, and the deployed five-model mean was not evaluated on held-out spectra. These qualifications bear on the prediction-set figures; the results on DFT spectra do not depend on the model. The 80 certified compositions are therefore candidates for calculations beyond the constant-relaxation-time approximation, not predicted thermoelectrics. The next steps follow from the limitations above, in order: phase competition against TiNiSi- and Co2_2Si-type structures, first for the 23 compositions with a reported or predicted orthorhombic phase; scattering-limited transport and lattice thermal conductivity for those that remain; and synthesis, beginning with the compositions whose half-Heusler phase has already been made.

Data availability

The DXMag structures and metadata (release 2025-09-09) and the HeuslerDB electronic-DOS dataset (doi:10.48505/nims.5794) are available from NIMS under CC BY 4.0 (https://www.nims.go.jp/group/spintheory/database/)[28]; the DFT spectra used for training are not redistributed. The machine-learned d-DOS of the 54,978 prediction-set entries (five-model mean and spread), the held-out predictions of the best-validation checkpoints of the same fold models for the 51,257 training-set entries, the prediction-set screening table, the input structures, an index of DXMag identifiers and metadata, and the 30 trained model weights with their configurations are deposited at Zenodo under CC BY 4.0 (doi:10.5281/zenodo.23329059). The per-run first-principles results of all 3,625 runs (electronic class, QE-PBE gap, transport summaries, certification status and screening indicators), the 607 paired scalar and SOC results, the structural-variant comparison, the rankings of the 80 certified compositions and the literature-status table are included in the code repository.

Code availability

The code used to train and apply the d-DOS model, compute the screening indicators, run and aggregate the Quantum ESPRESSO and BoltzTraP2 calculations, and produce the figures and tables is available at https://github.com/yednaph/heusler-dos-te-screening (release v1.0.0). It is released under the MIT licence, except the first-principles workflow, which is released under GPL-3.0-or-later because it derives from BoltzTraP2. Inputs that are not redistributed are listed in the repository.

Acknowledgements

We thank E. Xiao and T. Tadano for making the DXMag Computational HeuslerDB and its electronic-DOS dataset openly available. The d-DOS models were trained and applied on Aurora, the high-performance computing cluster (NVIDIA H100 GPU server) at Sardar Vallabhbhai National Institute of Technology, Surat, whose computing time we acknowledge; the first-principles calculations were run on local workstations.

Author contributions

S.R.: Methodology, Software, Investigation, Formal analysis, Data curation, Visualization, Writing – original draft. H.P.: Methodology, Software, Validation, Supervision, Project administration, Writing – review & editing. R.D.: Visualization, Writing – review & editing. All authors reviewed the manuscript.

Competing interests

The authors declare no competing interests.

Supplementary Information for “High-throughput screening of Heusler alloys for thermoelectrics combining machine-learned densities of states and first-principles transport”

Shivam Randive; Ayana Ghosh; Rahul Dixit; Himanshu Pandey

All figures and tables are generated from stored results by the scripts of the code repository (main text, Code availability). Throughout, “training set” denotes entries screened on their DFT d-DOS and “prediction set” entries screened on ML-predicted d-DOS. The two sets are reported separately, and their raw screening scores are not compared.

normalisation of the DOS archive

For a sample of magnetic training entries (∣M∣≥1 μB|M| \ge1\,\mu\mathrm{B} per formula unit in DXMag; 25 per family, fixed random seed), the archive’s spin-resolved total DOS was integrated up to EFE_{\mathrm{F}}, m=∫EF[D↑(E)−D↓(E)] dEm = \int^{E_{\mathrm{F}}} [D^{\uparrow}(E) - D^{\downarrow}(E)]\,\mathrm{d}E, and divided by the number of formula units of the structure stored with the spectrum. The ratio of this moment to the DXMag total magnetisation per formula unit is 2.00 (median; interquartile range 1.97–2.03) and lies between 1.99 and 2.01 in every family (Supplementary Fig. S2). The archive DOS therefore carries a factor of two relative to its stored structure, and so do the per-atom d-DOS targets of the main text (Eq. (1)) and the model’s predictions. The d-projected channel is assumed to carry the same factor; this was not checked separately. An earlier audit of 340 files, which integrated the total DOS to EFE_{\mathrm{F}} and compared it with the valence-electron count, found the same factor. Ratios of DOS values, and hence the d-DOS Seebeck indicator Smax⁡dS^{\mathrm{d}}_{\max} and the Mahan–Sofo sharpness ξ\xi, are unaffected. Absolute thresholds are affected: the 0.15 states eV−1^{-1} classifier threshold, the 0.05 states eV−1^{-1} atom−1^{-1} gap flag and the g(EF)=2g(E_{\mathrm{F}}) = 2 reference of the initial composite score (Supplementary Note 5) all correspond to half these values in physical units. The training-set screen, which works per stored cell, differs further by the number of atoms in that cell (three or four). Supplementary Table S2 lists the consequences for each indicator and threshold. Script: scripts/figures/dos_normalisation_check.py.

selection rounds and counting units

Selection rounds. DFT calculations were not drawn from a single ranked list. Nine selection rounds (rounds 1–9, Supplementary Table S6) were assembled in succession between July and October 2026, each ordered by the screening scores current when it was built (main text, Methods). Most rounds followed the d-DOS power-factor indicator Pmax⁡dP^{\mathrm{d}}_{\max}; round 6 followed the d-DOS Seebeck indicator Smax⁡dS^{\mathrm{d}}_{\max} without priority filters; rounds 7 and 8 took semiconductor-labelled entries by gap tier; and round 9 took entries obeying the electron-count rule (18 or 24 valence electrons). Later rounds were therefore shaped by what earlier rounds had shown, and outcome rates differ strongly between rounds (Supplementary Table S6). No round was a random or stratified sample, so every rate reported in the paper is conditional on this selection and the recall of the screen is not measured.

Counting units. Runs are individual QE-PBE/BoltzTraP2 calculations: 3,625 in total, of which 1,562 are from the training set, 2,021 from the prediction set and 42 could not be attributed unambiguously to either set; these 42 are excluded from all per-set statistics. Entries are distinct DXMag records (UUIDs); all matching is by UUID, never by formula, because different entries can share a formula. Compositions merge entries with the same DXMag composition string across structural variants and across sets; the string keeps the site order, so it distinguishes half-Heusler site permutations, which a reduced formula does not. The certified counts are 76 training-set and 79 prediction-set entries, corresponding to 75 and 79 compositions; their union is 80 compositions (74 certified in both sets, 5 in the prediction set only, 1 in the training set only).

Near-duplicate entries. Because every prediction-set entry shares its composition with a training-set entry, some computed entries in the two sets are near-duplicates of the same crystal: a prediction-set entry is a near-duplicate of a training-set entry when the two share composition, family and space group and differ by less than 5 meV atom−1^{-1} in DXMag energy and 1% in volume. Among all computed entries, 475 prediction-set entries have such a near-duplicate training-set entry (largest differences 4.78 meV atom−1^{-1} and 0.86% in volume). Among the 155 certified entries, 79 prediction-set entries have a near-duplicate training-set entry (largest differences: 1.73 meV atom−1^{-1} in DXMag energy and 0.20% in volume), so the 155 entries correspond to about 81 distinct crystals, or 80 when the cubic and tetragonal PdScAs entries, which are the same crystal within numerical precision, are counted once, as in the main text. This is why certified results are reported per set and merged only at the level of compositions, with provenance.

d-DOS model and training details

The main text summarises the d-DOS model; this note gives the full specification as read from the training and inference code, the per-fold configuration files, the tensor shapes of the deployed checkpoints and the surviving run records (settings collected in Supplementary Table S5).

Representation. ALIGNN represents a crystal by its atom graph GG, with atoms as nodes and neighbour pairs (including periodic images) as edges, and by the line graph L(G)L(G), whose nodes are the bonds of GG and whose edges connect pairs of bonds that share an atom and carry the bond angle θ\theta. Graphs use the 12-nearest-neighbour rule of the package with an 8 Å cutoff, and are built from the structure stored with each training spectrum or from the listed DXMag cell of a prediction-set entry, without relaxation. Bond lengths are expanded in 80 radial basis functions and bond-angle cosines in 40, with 64-dimensional embeddings. Each atom carries 97 input features: the 92 CGCNN descriptors plus five Heusler-specific features, namely the d-electron count, the largest magnitude of a common oxidation state, the distance of the d count from a half-filled or filled shell, the period of the d shell (its principal quantum number plus one) and a duplicate of the d-electron count. The d count is read from the electron configuration, so p-block elements with a filled d shell (Ga to Bi) carry a value of ten.

Edge-gated convolution. For node features hi\mathbf{h}_i and edge features eij\mathbf{e}_{ij}, each convolution computes

mij=Ahi+Bhj+Ceij,ηij=sigm⁡(mij)∑ksigm⁡(mik)+ϵ(10)\mathbf{m}_{ij}=A\mathbf{h}_i+B\mathbf{h}_j+C\mathbf{e}_{ij},\qquad \boldsymbol{\eta}_{ij}=\frac{\operatorname{sigm}(\mathbf{m}_{ij})}{\sum_k\operatorname{sigm}(\mathbf{m}_{ik})+\epsilon} \tag*{(10)}
hi′=hi+SiLU⁡[BN⁡(Uhi+∑jηij⊙Vhj)],eij′=eij+SiLU⁡[BN⁡(mij)](11)\mathbf{h}'_i=\mathbf{h}_i+\operatorname{SiLU}\left[\operatorname{BN}\left(U\mathbf{h}_i+\sum_j\boldsymbol{\eta}_{ij}\odot V\mathbf{h}_j\right)\right],\qquad \mathbf{e}'_{ij}=\mathbf{e}_{ij}+\operatorname{SiLU}\left[\operatorname{BN}(\mathbf{m}_{ij})\right] \tag*{(11)}

where mij\mathbf{m}_{ij} is the edge message, ηij\boldsymbol{\eta}_{ij} the normalised edge gate, AA, BB, CC, UU, VV are learned matrices, sigm is the logistic function, ϵ\epsilon a small constant that prevents division by zero, BN batch normalisation, SiLU⁡(x)=xsigm⁡(x)\operatorname{SiLU}(x)=x\operatorname{sigm}(x), ⊙\odot the element-wise product, and the sums over jj and kk run over the neighbours of node ii. An ALIGNN layer applies this update first on L(G)L(G), where the nodes are bonds and the edges bond pairs carrying the angle expansion, and then on GG, using the updated bond features as edge features; angular information thereby reaches the atom features. The encoder has eight ALIGNN layers followed by eight graph-convolution layers acting on GG alone, all with 512 features (package default: four and four layers of 256 features). The atom features are then averaged over the crystal into one 512-value vector. No layer of the encoder was modified.

Output head. The single linear output layer of the package was replaced by a head 512 → 1024 → 2048 → 4002 with GELU activations and dropout 0.2 after the first two layers, followed by softplus⁡(z)=ln⁡(1+ez)\operatorname{softplus}(z)=\ln(1+e^z), so that the predicted spin-resolved d-DOS y^∈R4002\hat{\mathbf{y}}\in\mathbb{R}^{4002} (2 × 2,001 points, −10 to 10 eV in steps of 0.01 eV) is non-negative. The model has 42,520,354 trainable parameters, 1.08 × 10710^7 of them in the head.

Loss. The loss, evaluated on the softplus output and averaged over a batch, is

L=0.35LF+0.35L±2+0.15Lcos+0.10Lslope+0.05Lsort.(12)\mathcal{L}=0.35\mathcal{L}_{\mathrm{F}}+0.35\mathcal{L}_{\pm2}+0.15\mathcal{L}_{\mathrm{cos}}+0.10\mathcal{L}_{\mathrm{slope}}+0.05\mathcal{L}_{\mathrm{sort}}. \tag*{(12)}

LF=14002∑kw~k(y^k−yk)2\mathcal{L}_{\mathrm{F}}=\frac{1}{4002}\sum_k\tilde{w}_k(\hat{y}_k-y_k)^2 is a mean-squared error weighted by the Fermi window w(E)=−∂f/∂Ew(E)=-\partial f/\partial E at 700 K, normalised to unit mean (w~k\tilde{w}_k). L±2\mathcal{L}_{\pm2} is the mean-squared error within ∣Ek∣≤2|E_k|\leq2 eV, averaged over the two spin channels. Lcos=1−y^⋅y/(∥y^∥∥y∥+ϵ)\mathcal{L}_{\mathrm{cos}}=1-\hat{\mathbf{y}}\cdot\mathbf{y}/(\lVert\hat{\mathbf{y}}\rVert\lVert\mathbf{y}\rVert+\epsilon) is the cosine distance. Lslope\mathcal{L}_{\mathrm{slope}} is the mean-squared error of first differences plus 0.1 times that of second differences over ∣Ek∣≤3|E_k|\leq3 eV; as implemented it acts on the spin-up channel only. Lsort\mathcal{L}_{\mathrm{sort}} is the L1 distance between the sorted values of prediction and target over the whole 4,002-value vector, so it pools both spin channels and ignores energy positions. Two further terms in the code had zero weight. At 700 K the normalised Fermi weight has a full width at half maximum of 0.21 eV and a peak of 83 at EFE_F, and 99% of it lies within ±0.3 eV; per energy bin near EFE_F, LF\mathcal{L}_{\mathrm{F}} therefore outweighs L±2\mathcal{L}_{\pm2} by a factor of about 17.

Training. Each family was divided by shuffled five-fold cross-validation (seed 42), with 10% of the non-test entries held out for validation, so that each model trained on 72% of its family, was selected on 8% and tested on 20%. Optimisation used AdamW (learning rate 10−310^{-3}, weight decay 5×10−55\times10^{-5}, gradient clipping at 1.0) with a reduce-on-plateau schedule (factor 0.5; patience 25, or 15 for cubic full-Heusler folds 0–2). The schedule monitors the validation loss. Stochastic weight averaging (SWA) averaged the weights over the last 20% of epochs, during which a single annealed learning rate of 5×10−55\times10^{-5} applied to all parameters; the batch-normalisation statistics were then re-estimated in one pass with momentum 0.1. Runs lasted 300 epochs with batch size 128, except cubic full Heusler (150 or 200 epochs, batch 64). The best-validation checkpoint, chosen on the Pearson rr over the concatenated validation spectra before SWA starts, gives all held-out metrics; the SWA weights give all predictions. Data augmentation, early stopping and learning-rate warm-up were configured but not executed. Seeds were fixed and cuDNN was set to deterministic mode; bitwise reproducibility was not tested.

Pretraining and fine-tuning. An all-family (foundation) model of the same architecture was first trained on all 51,257 training-set spectra for 100 epochs (SWA from epoch 85). Its validation subset was part of its own training data, so every later test entry was seen during pretraining. Fine-tuning loads all weights of the parent’s SWA checkpoint, including the head, and trains the encoder at the learning rate and weight decay scaled by ss and the head at the full rate. A variance-aware initialisation of the last output layer was used only for the foundation run.

Provenance record. For cubic full-Heusler folds 0 and 1, the run metadata and optimiser states show initialisation from the pretrained model with s=0.1s=0.1. For the other 28 models, four project sources give different parents (Supplementary Table S4), the checkpoints do not record them, the launch script was edited after training, and the code silently falls back to random initialisation if a parent path is missing; their parent, learning-rate scaling and weight loading are therefore unconfirmed. The only surviving training record, that of cubic full-Heusler fold 1 (Supplementary Fig. S3), shows the validation rr peaking at epoch 2 (0.827) and declining to 0.786 by epoch 149, while the validation loss rose from 0.050 to 0.058. The best-validation checkpoints are those of epoch 2 (fold 1) and epoch 0 (fold 0); the SWA weights average epochs 120–149.

Inference. All six screening scripts specify the five SWA fold models of the entry’s family; the mean of their softplus outputs is the predicted d-DOS and their population standard deviation us(E)u_s(E) its spread, whose mean over ∣E∣≤2|E| \le2 eV and both channels is uFu_F. The run summaries for cubic full and inverse Heuslers list five checkpoints (4,504 entries in 219 s; 6,702 in 316 s), and the stored arrays confirm five members in every family (Note 4). Per-member predictions were not saved. The final re-screen was completed on 23 August 2026; its command-line arguments were not logged. The predicted d-DOS feeds the indicators Smax⁡dS_{\max}^{d}, Pmax⁡dP_{\max}^{d}, ξ\xi and L0∗L_0^{*} of the main text. One systematic artefact lies outside the screening window: for 42 held-out and 12 prediction-set spectra, all of Zn-rich compounds, the filled Zn 3d band near −7-7 eV is predicted too high, so that the occupied d-states per atom (physical units) exceed ten, which no DFT target does; it does not enter any indicator, which uses states within about 2 eV of EFE_F.

Software and hardware. alignn 2026.4.1, PyTorch 2.2.2 (CUDA 12.1), DGL 1.1.3 and Python 3.11 (versions at export), on NVIDIA H100 GPUs; spglib 2.0.2, BoltzTraP2 24.7.2 and Quantum ESPRESSO 7.1 for the DFT part (Supplementary Table S7).

Supplementary Note 4: implementation record

This note records implementation facts that earlier descriptions of the workflow stated differently, and how each was established. The main text follows the implementation throughout.

  1. Ensemble size. All six screening scripts specify the five fold models of the family, and the two surviving inference summaries list five checkpoints. The stored arrays confirm this for every family: for nn members the ratio of the population standard deviation to the mean cannot exceed n−1\sqrt{n-1}, and its maximum is exactly 2.000 (n=5n = 5) in all six families.

  1. Transfer lineage. Initialisation from the all-family model is recorded in the run files for two of the 30 models (cubic full Heusler, folds 0 and 1); for the others the parent is not recorded (Supplementary Table S4 and Note 3).

Table S4. Parent model of each family according to each project source. “Scratch”: random initialisation; “chain”: the single sequence full cubic → full tetragonal, inverse cubic → inverse tetragonal → half cubic → half tetragonal. Transfer script: submit_transfer.sh; pipeline document: docs/PHYSICS_AND_PIPELINE.md. Only the last column rests on run records.

familypresentation (slide 20)transfer scriptpipeline doc., chainpipeline doc., tableproject overviewrun records
full cubicfoundationscratch–scratchfoundationfoundation, s=0.1s = 0.1 (folds 0, 1)
full tetragonalfull cubicfull cubicfull cubic (fold-0 SWA)full cubicfoundationnone
inverse cubicfull cubicfull cubicfull cubic (fold-0 SWA)full cubicfoundationnone
inverse tetragonalinverse cubic full cubicinverse cubic scratchchaininverse cubic scratchfoundation foundationnone none
half cubichalf cubichalf cubicchain (after inverse tetragonal)half cubicfoundationnone
half tetragonalhalf cubichalf cubicchainhalf cubicfoundationnone

Table S4.

  1. Loss. Five terms are active, with the weights of Eq. (12) in all 30 configuration files; the code defaults (seven terms) were overridden. Of the two zero-weight terms, the asymmetric peak term indexes the spin-down window one bin early; it has no effect on any model. The sorted-value term, named after the Wasserstein distance in the code, pools both spin channels and ignores energy positions, and the slope term acts on the spin-up channel only.

  1. Interpolation and features. Targets are linearly interpolated. The five Heusler-specific features are those of Note 3.

  1. Normalisation layers. The encoder uses batch normalisation; after SWA its statistics were re-estimated in one pass over the training data with the default momentum of 0.1, that is as an exponential rather than a cumulative average.

  1. Configured but not executed. Data augmentation, early stopping and learning-rate warm-up appear in the configuration files but were not executed.

  1. Evaluation. All held-out metrics were computed with the best-validation checkpoints, and the pretrained model had seen every test entry. The SWA window is the last 20% of each run: epochs 240–299 for the 300-epoch runs and 120–149 or 160–199 for the cubic full-Heusler runs of 150 and 200 epochs.

  1. Determinism and versions. The code fixes the seeds and sets cuDNN to deterministic mode; bitwise reproducibility was not tested. The training script was modified after training, and no version-control commit was recorded; the released code is that of the repository cited in the main text.

  1. Structures. The inference code reads the DXMag cell and positions unchanged; no structure was relaxed.

  1. Grouped splits. Splits grouped by the ZZ-site element were prepared but never evaluated.

  1. Parameter count. The deployed checkpoints have 42,520,354 trainable parameters (from the tensor shapes); counts of about 4.257×1074.257 \times10^{7} include the batch-normalisation statistics.

  1. Screening statements. The power-factor threshold was derived from the first 1,401 runs of the campaign and then held fixed; metallic shares are reported per set (63.1% and 85.1%); and the priority filters ordered the selection rounds without excluding entries.

Supplementary Note 5: the initial composite score

In the initial screen (July 2026) the prediction set was ranked by a composite score computed from the ensemble-mean d-DOS (called D34 in the project code),

Q=sMϕ11+∣g(EF)−2∣exp⁡[−min⁡±1 eVg↑min⁡±1 eVg↓](13)Q = s_{\mathrm{M}} \phi\frac{1}{1 + \lvert g(E_F) - 2 \rvert} \exp\left[-\min_{\pm1\,\mathrm{eV}} g_{\uparrow}\min_{\pm1\,\mathrm{eV}} g_{\downarrow}\right] \tag*{(13)}

where sM=max⁡s∣π2kB2Tgs′(EF)/3egs(EF)∣s_{\mathrm{M}} = \max_{s} \left|\pi^{2} k_{\mathrm{B}}^{2} T g_{s}'(E_{\mathrm{F}})/3e g_{s}(E_{\mathrm{F}})\right| is the larger over the two spin channels ss of the Mott-formula Seebeck coefficient at T=700T = 700 K, and ϕ\phi is the larger over the channels of the peak height within 2 eV of EFE_{\mathrm{F}} divided by its full width at half maximum. Values are in archive units, so the reference g(EF)=2g(E_{\mathrm{F}}) = 2 corresponds to 1 per atom physically (Supplementary Note 1). The score exists for the prediction set only. Taking the larger single-channel Mott term ignores that the two spin channels conduct in parallel, S=(σ↑S↑+σ↓S↓)/(σ↑+σ↓)S = (\sigma_{\uparrow}S_{\uparrow} + \sigma_{\downarrow}S_{\downarrow})/(\sigma_{\uparrow} + \sigma_{\downarrow}), so that a large term in a weakly conducting channel is outweighed by the other, more conducting channel. This is one reason why the score rewarded metals. Of its 100 best prediction-set entries, 83 carried a metal label, 98 lay at least 0.1 eV atom−1^{-1} above the hull, 7 were computed and none was certified (Supplementary Fig. S8a).

development of the workflow

The certification criteria and the indicators of the main text are the final protocol. They were reached while the 3,625 calculations proceeded, and each step was motivated by a first-principles observation (Table S10): an earlier composite score was replaced by the Cutler–Mott indicators, stability, label and ensemble spread became priority filters, the electronic class was taken from the QE-PBE band structure, a single power-factor threshold was fixed from the first 1,401 runs, a QE-PBE gap became a requirement, heavy-element runs were re-checked with SOC, and ranking moved to computed transport. Because these choices were made after part of the results had been seen, the cascade of the main text is not a prospective test; the sensitivity of the certified count to each threshold is given in Table S9.

casequalified runsgapped qualifiedcertified entriescertified compositions
declared (baseline)30920115580
threshold from corrected runs (1.154e+12)29519314977
threshold ×0.8353228205105
threshold ×0.933722018796
threshold ×1.128318513670
threshold ×1.225017412665
threshold ×1.51611076735
Seebeck criterion ∣S∣>40|S| > 4034920115580
Seebeck criterion ∣S∣>80|S| > 8028220115580
Seebeck criterion ∣S∣>100|S| > 10024920115580
hull < 0.0251481129549
hull < 0.0520615212364
hull < 0.15395249203104

Table S9. Table S9. Sensitivity of qualified-run and certified counts to the power-factor threshold, the Seebeck criterion and the hull-distance cut. “Threshold from corrected runs” uses the median of mesh-corrected runs instead of the declared value. Compositions are counted over both sets.

Supplementary Tables

familysetentriescompositionsatoms/cellhull<0.10 (%)median hull∣M∣>0.1\lvert M\rvert> 0.1 (%)18 e−^{-} (%)24 e−^{-} (%)
full cubicT9,3969,39649.50.3767.03.74.8
P4,5043,57247.30.4160.03.26.6
full tetraT8,0478,047813.50.2825.03.13.6
P13,4797,81685.50.3736.62.24.0
half cubicT9,3969,39633.70.6566.59.44.8
P4,9143,90734.60.6862.411.63.8
half tetraT6,9096,90961.50.5827.66.15.6
P10,8966,25660.70.7140.24.74.5
inverse cubicT9,0729,07242.20.4569.43.74.9
P6,7024,45341.90.5060.72.86.2
inverse tetraT8,4378,43785.30.3124.62.94.7
P14,4838,07682.20.4136.62.35.1

Table S1. Characterisation of the two sets by family (T, training set; P, prediction set). Compositions are site-ordered DXMag composition strings; atoms per listed cell are medians; hull distances in eV atom−1^{-1}; ∣M∣\lvert M\rvert in μB\mu_{\mathrm{B}} per formula unit, as a share of entries with a known moment; VEC is the valence-electron count per formula unit.

quantityprediction set (per atom, ×2\times2)training-set screen (per cell, ×2N\times2N)consequence
Smax⁡dS_{\max}^{\mathrm{d}}, sharpness ξ\xiinvariantinvariantnone
Pmax⁡dP_{\max}^{\mathrm{d}}, L0∗L_{0}^{*} (scale-dependent)×2\times2, uniform×6\times6 (half) or ×8\times8 (full, inverse)rankings within the prediction set unchanged; in the training set Pmax⁡dP_{\max}^{\mathrm{d}} favours full and inverse over half Heuslers by 4/3, which affects the Pmax⁡dP_{\max}^{\mathrm{d}}-ordered rounds and their training-set AUC
classifier threshold 0.15physical 0.075 per atom and spinphysical 0.025 (half) or 0.019 (full, inverse)training-set label 3–4×\times stricter, by family; d-DOS gap widths and the 0.10–1.40 eV window select different populations in the two sets
held-out gap flag 0.05 (spin-summed)physical 0.025 per atomnot useddefines the confusion matrix of main-text Figure 4e
initial composite score: 1/(1+∣g(EF)−2∣)1/(1 + \lvert g(E_{\mathrm{F}}) - 2\rvert) and exp⁡(−min⁡g↑min⁡g↓)\exp(-\min g_{\uparrow}\min g_{\downarrow})peak at physical 1; exponent ×4\times4not computedevaluated as implemented; its failure stands
loss termsMSE terms ×4\times4, cosine invariantnot usedrelative term weights shift uniformly

Table S2. Consequences of the DOS normalisation for each indicator and threshold (Supplementary Note 1).

compositionconventionalclasspoly.evidenceprincipal source (DOI)
CoHfSbHfCoSbestablishedExperimental: pristine and Pt/Sn-doped HfCoSb synthesised and Seebeck/resistivity measured; parent of the widely studied p-type (Hf,Zr,Ti)CoSb(Sn) half-Heusler family.Xia 2000, J. Appl. Phys. 88, 1952 (10.1063/1.1305829)
CoNbSnNbCoSnestablishedExperimental: phase-pure/directionally solidified NbCoSn synthesised with measured Seebeck, resistivity and PF; Pt-substituted n-type NbCoSn with measured zT.Kimura 2008, Appl. Phys. Lett. 92, 012105 (10.1063/1.2828713)
CoTiSbTiCoSbestablishedExperimental: pristine TiCoSb and (Ti,Zr,Hf)CoSb compounds synthesised with measured resistivity, Seebeck and thermal conductivity; long-standing p/n-type half-Heusler TE family.Sekimoto 2005, Mater. Trans. 46, 1481 (10.2320/matertrans.46.1481)
CoZrBiZrCoBiestablishedExperimental: p-type ZrCoBi-based half-Heuslers synthesised with measured zT and device conversion efficiency.Zhu 2018, Nat. Commun. 9, 2497 (10.1038/s41467-018-04958-3)
CoZrSbZrCoSbestablishedExperimental: pristine and doped ZrCoSb synthesised with measured Seebeck/resistivity; core member of p-type MCoSb half-Heusler family.Xia 2000, J. Appl. Phys. 88, 1952 (10.1063/1.1305829)
FeNbSbNbFeSbestablishedExperimental: p-type NbFeSb-based half-Heuslers (Ti/Hf/Zr-doped) synthesised with measured zT > 1; widely recognised TE family.Fu 2015, Nat. Commun. 6, 8144 (10.1038/ncomms9144)
FeTaSbTaFeSbestablishedExperimental: TaFeSb-based half-Heuslers (Ti-substituted Ta1-xTixFeSb) synthesised by inverse design with measured high zT; also highlighted computationally.Zhu 2019, Nat. Commun. 10, 270 (10.1038/s41467-018-08223-5)
FeVSbVFeSbestablishedExperimental: pristine and doped FeVSb synthesised and Seebeck/resistivity/thermal conductivity measured in several independent studies; p-type FeVSb-based alloys are a recognised HH TE family.Young 2000, Journal of Applied Physics 87, 31-321 (10.1063/1.371863)
NiTiSnTiNiSnestablishedExperimental: canonical n-type MNiSn HH thermoelectric; pristine and Sb-doped TiNiSn synthesised and S/PF/zT measured in many studies.Bhattacharya 2000, Applied Physics Letters 77, 2476-2478 (10.1063/1.1318237)
NiZrSnZrNiSnestablishedExperimental: canonical n-type HH thermoelectric; pristine and doped ZrNiSn synthesised and S/PF/zT measured extensively.Uher 1999, Physical Review B 59, 8615-8621 (10.1103/physrevb.59.8615)
CoTaSnTaCoSnexp. investig.Experimental: half-Heusler TaCoSn first synthesised and TE properties measured for pristine and Nb/Sb-alloyed n-type samples (zT reported); earlier computational prediction.Li 2019, ACS Appl. Mater. Interfaces 11, 41321 (10.1021/acsami.9b13603)
CoVSnVCoSnexp. investig.One experimental study (powder metallurgy + SPS) gave multiphase non-stoichiometric CoVSn with measured, very low zT; preceded by computational prediction of high p-type performance.Hooshmand Zaferani 2020, Energies 13, 1459 (10.3390/en13061459)
Fe2TiSiFe2TiSiexp. investig.Experimental but limited: L2_1 Fe2TiSi realised only as epitaxial thin films (sputtering, MBE); one film study measured room-temperature Seebeck and thermal conductivity; computational TE prediction (Bilec 2015).Shimanuki 2020, J. Appl. Phys. 127, 055106 (10.1063/1.5414949)
IrNbSnNbIrSnexp. investig.Half-Heusler NbIrSn synthesised; room-temperature Seebeck coefficient and resistivity measured.Hohl 1998, J. Phys.: Condens. Matter 10, 7843 (10.1088/0953-8984/10/35/016)
IrNbSnNbIrSnexp. investig.Computational only: dedicated first-principles TE study (electron and phonon transport, zT) of pristine HH NbIrSn; also included in a high-throughput PF/zT screen.
NiScSbScNiSbexp. investig.Experimental: pristine ScNiSb synthesised and S, rho, kappa, zT measured in several independent studies; doped variants also measured.Synoradzki 2019, Materials 12, 1723 (10.3390/ma1201723)
NiYBiYNiBiexp. investig.One dedicated experimental study (synthesis and measured S, sigma, kappa of pristine YNiBi), plus several ab initio PF studies.Li 2015, Journal of Applied Physics 117, 205101 (10.1063/1.4921811)
NiYSbYNiSbexp. investig.Experimental thermopower/transport of pristine YNiSb measured in a comparative ScMSb/YMSb study; ab initio work predicts a high p-type PF.Oestreich 2003, Journal of Physics: Condensed Matter 15, 635-640 (10.1088/0953-8984/15/4/304)
PdScSbScPdSbexp. investig.Experimental: pristine polycrystalline ScPdSb was synthesised and its thermoelectric properties (Seebeck, resistivity, zT near 300 K) measured in one study; later a DFT+BoltzTraP study computed p-type transport.Oestreich 2003, J. Phys.: Condens. Matter 15, 635 (10.1088/0953-8984/15/4/304)
PtScSbScPtSbexp. investig.Experimental: pristine polycrystalline ScPtSb was synthesised and thermoelectric properties measured (one study, small zT near 300 K); later DFT+BoltzTraP predicted it to have the largest p-type power factor of ScMSb.Oestreich 2003, J. Phys.: Condens. Matter 15, 635 (10.1088/0953-8984/15/4/304)
AuHfAlHfAuAlcomp. investig.High-throughput half-Heusler transport/quality-factor screen only. Computational only: listed among AFLOW thermodynamically stable half-Heuslers with a high-throughput lattice-thermal-conductivity estimate and in an ML/DFT kappa_L dataset; no dedicated TE transport study, synthesis or measurement found.Pak 2025, J. Mater. Chem. A 13, 19455 (10.1039/d5ta00397k)

Table S3. Prior thermoelectric evidence for the 80 certified compositions (targeted literature audit, Methods). DXMag site-ordered composition and conventional name; class by the strongest evidence for the same composition in the same structure type; polymorph: the composition is reported experimentally in an orthorhombic structure (exp.) or such a ground state is predicted (pred.); screen-level predictions count as computational. Absence of a report is not evidence that none exists. Every DOI was checked against its Crossref record.

compositionconventionalclasspoly.evidenceprincipal source (DOI)
CoHfAsHfCoAscomp. investig.exp. [83 ICSD 406953, Pnma]Dedicated DFT thermoelectric study; also in high-throughput screens. Computational screening only: kappa_L estimate in AFLOW-based high-throughput screen and an n-type conductivity-effective-mass descriptor in a 69-compound half-Heusler band-engineering table; no dedicated TE study or measurement found.Yang 2022, J. Solid State Chem. 314, 123386 (10.1016/j.jssc.2022.123386)
CoHfBiHfCoBicomp. investig.Computational TE predictions only (DFT/Boltzmann transport of Bi-based 18-electron half-Heuslers XYBi incl. HfCoBi); no synthesis or measured TE data for pristine HfCoBi found.Paul 2024, ACS Appl. Energy Mater. 7, 9595 (10.1021/acsaem.4c01652)
CoNbGeNbCoGecomp. investig.exp. (Jeitschko 1969, via Singh 2019 (sec.))Computational only: first-principles cubic-vs-orthorhombic stability and Boltzmann TE transport for cubic CoNbGe; kappa_L estimate in AFLOW high-throughput screen.Singh 2019, J. Phys.: Condens. Matter 32, 055505 (10.1088/1361-648x/ab4e71)
CoTaGeTaCoGecomp. investig.exp. (Jeitschko 1969, via Singh 2019 (sec.))Computational only: first-principles phase-stability and Boltzmann TE transport for cubic CoTaGe; kappa_L estimate in high-throughput screen.Singh 2019, J. Phys.: Condens. Matter 32, 055505 (10.1088/1361-648x/ab4e71)
CoTaSiTaCoSicomp. investig.exp. (Landolt-Bornstein, via patent (sec.))Computational only: first-principles TE transport for hypothetical cubic CoTaSi, whose reported ground state is orthorhombic; kappa_L estimate in high-throughput screen.Singh 2019, J. Phys.: Condens. Matter 32, 055505 (10.1088/1361-648x/ab4e71)
CoTiAsTiCoAscomp. investig.High-throughput half-Heusler transport/quality-factor screen only. Known only computationally: kappa_L estimate in AFLOW high-throughput screen and a DFT optoelectronic/elastic study of CoTiX (X = P, As, Sb); no TE transport study or measurement found.Pak 2025, J. Mater. Chem. A 13, 19455 (10.1039/d5ta00397k)
CoTiBiTiCoBicomp. investig.Computational TE predictions only (DFT elastic/phonon/Boltzmann TE of ZrCoBi and TiCoBi; Bi-based XYBi screening); no synthesis or measurement found.Chen 2023, Eur. Phys. J. Plus 138, 966 (10.1140/epjp/s13360-023-04592-z)
CoVGeVCoGecomp. investig.exp. (Jeitschko 1969, via Singh 2019 (sec.))Computational only: first-principles cubic stability and Boltzmann TE transport for cubic CoVGe; kappa_L estimate in high-throughput screen.Singh 2019, J. Phys.: Condens. Matter 32, 055505 (10.1088/1361-648x/ab4e71)
CoVSiVCoSicomp. investig.exp. (Landolt-Bornstein, via patent (sec.))Computational only: first-principles TE transport for hypothetical cubic CoVSi (ground state reported orthorhombic).Singh 2019, J. Phys.: Condens. Matter 32, 055505 (10.1088/1361-648x/ab4e71)
CoZrAsZrCoAscomp. investig.High-throughput half-Heusler transport/quality-factor screen only. Known only computationally: kappa_L estimate in AFLOW high-throughput screen and a DFT elastic/electronic/optical (photovoltaic-oriented) study; TE only mentioned as a possible application.Pak 2025, J. Mater. Chem. A 13, 19455 (10.1039/d5ta00397k)
Fe2HfSiFe2HfSicomp. investig.Computational only: DFT (FP-LAPW) structural, optoelectronic and TE properties of L2_1 Fe2HfSi under pressure; also in a DFT Fe2YZ band-engineering TE screen.Azam 2023, RSC Adv. 13, 15437 (10.1039/d3ra00362k)
Fe2NbAlFe2NbAlcomp. investig.Computational only: DFT prediction of large power factor (Fe2YZ band engineering) and DFT lattice-dynamics/TE study of Fe2MAl (M = V, Nb, Ta).Ye 2024, npj Quantum Mater. 9, 60 (10.1038/s41535-024-00671-1)
Fe2TaAlFe2TaAlcomp. investig.Computational only: DFT electronic structure and TE (BoltzTraP) of Fe2TaZ (Z = Al, Ga, In) and Fe2YZ band-engineering TE prediction.Khandy 2018, RSC Adv. 8, 40996 (10.1039/c8ra04433c)
FeNbAsNbFeAscomp. investig.High-throughput half-Heusler transport/quality-factor screen only. Computational screening only: kappa_L estimate in AFLOW high-throughput screen and an n-type effective-mass descriptor in a half-Heusler band-engineering table; no dedicated TE study.Pak 2025, J. Mater. Chem. A 13, 19455 (10.1039/d5ta00397k)
FeTaAsTaFeAscomp. investig.Computational only: high-throughput DFT (deformation-potential PF, Slack kappa) identifies TaFeAs as a novel stable half-Heusler and the best TE candidate of its set; kappa_L in AFLOW screen.Bilinska 2023, Crystals 13, 1378 (10.3390/cryst13091378)
FeVAsVFeAscomp. investig.Computational only: high-throughput DFT (PF/ZT) study names VFeAs among novel stable half-Heuslers with TE potential.Bilinska 2023, Crystals 13, 1378 (10.3390/cryst13091378)
IrNbGeNbIrGecomp. investig.exp. (Mishra 2001 (Z. Naturforsch.))Computational only: DFT/BoltzTraP2 power factor and zT (deformation-potential relaxation time, Slack kappa_L) for pristine cubic HH NbIrGe in a high-throughput study; no HH synthesis found.Bilinska 2023, Crystals 13, 1378 (10.3390/cryst13091378)
IrTaGeTaIrGecomp. investig.HH TaIrGe has been synthesised as a p-type transparent conductor, not a TE study; the TE evidence is computational (DFT/BoltzTraP zT under strain), on pristine material.Nisha 2021, Journal of Solid State Chemistry 303, 122524 (10.1016/j.jssc.2021.122524)
IrTaSiTaIrSicomp. investig.exp. (orthorhombic TaIrSi literature (row notes))High-throughput half-Heusler transport/quality-factor screen only. No TE study of cubic HH TaIrSi found; the literature concerns the orthorhombic polymorph (structure/magnetism, superconductivity).Pak 2025, J. Mater. Chem. A 13, 19455 (10.1039/d5ta00397k)
IrTaSnTaIrSncomp. investig.Computational only: DFT/BoltzTraP3 TE study of pristine HH TaIrSn reporting large predicted zT; other DFT papers cover its optical/thermodynamic properties.Kaur 2017, Physics Letters A 381, 3760-3765 (10.1016/j.physleta.2017.09.043)
IrTiAsTiIrAscomp. investig.Computational only: first-principles TE study (S, sigma, kappa, zT) of pristine HH TiIrAs and TiIrSb.Kaur 2017, Journal of Alloys and Compounds 727, 1171-1177 (10.1016/j.jallcom.2017.08.216)
IrVGeVIrGecomp. investig.pred. [85 predicted]Computational only: DFT study of structural, vibrational and TE properties of pristine HH VYGe (Y = Rh, Co, Ir); also in a high-throughput PF/zT screen.Solola 2023, Computational Condensed Matter 36, e00827 (10.1016/j.cocom.2023.e00827)

Table 4.

compositionconventionalclasspoly.evidenceprincipal source (DOI)
NiHfGeHfNiGecomp. investig.exp. (Mallick 2025 (row notes))Computational only for the HH polymorph: DFT/BoltzTraP zT prediction for pristine HH NiHfGe, plus DFT stability/elastic work (Osafile 2021, Mol. Phys. 119, e1936249, doi 10.1080/00268976.2021.1936249, verified).Bendahma 2019, Computational Condensed Matter 21, e00407 (10.1016/j.cocom.2019.e00407)
NiHfSiHfNiSicomp. investig.exp. (Saurabh 2021)Computational only for the HH polymorph: TB-mBJ DFT study of NiHfZ (Z = Si, Ge) that includes transport/TE quantities; DFT stability study (Osafile 2021).Nazir 2026, Silicon 18, 3035-3051 (10.1007/s12633-026-03704-5)
NiScAsScNiAscomp. investig.pred. [85 predicted]Computational only: several DFT+Boltzmann TE studies of pristine HH ScNiAs (NiTZ family; XNiAs X = Sc, Y; Ni-based HH high-throughput).Jaishi 2021, AIP Advances 11, 025304 (10.1063/5.0031512)
NiScBiScNiBicomp. investig.Computational only: ab initio power-factor and TE studies of p-type ScNiBi (with YNiBi, LuNiBi).Winiarski 2020, Acta Physica Polonica A 138, 533-538 (10.12693/aphyspola.138.533)
NiTiGeTiNiGecomp. investig.exp. (Downie 2023)Computational only for the HH polymorph: included in DFT/Boltzmann high-throughput TE studies (Ni-based HH; 18-electron HH PF/zT screen).Chen 2021, ACS Omega 6, 18269-18280 (10.1021/acsomega.1c02172)
NiTiPbTiNiPbcomp. investig.pred. [86 predicted]Computational only: dedicated DFT TE study of pristine HH TiXPb (X = Ni, Pd, Pt), with low predicted kappa_L.Khatri 2024, Computational Materials Science 244, 113250 (10.1016/j.commatsci.2024.113250)
NiTiSiTiNiSicomp. investig.exp. (Downie 2023)Computational only for the HH polymorph: DFT/Boltzmann TE of pristine HH NiTiSi in a Ni-based HH high-throughput study; also a 2020 conference DFT TE abstract (Bati et al., MDPI IOCC 2020; DOI not verified).Chen 2021, ACS Omega 6, 18269-18280 (10.1021/acsomega.1c02172)
NiVGaVNiGacomp. investig.Computational only: DFT/Boltzmann TE (PF, zT) of pristine HH NiVGa in Ni-based HH screens.Chen 2021, ACS Omega 6, 18269-18280 (10.1021/acsomega.1c02172)
NiZrGeZrNiGecomp. investig.exp. (Saurabh 2021)High-throughput half-Heusler transport/quality-factor screen only. No TE study of the cubic HH polymorph found; experimental TE transport exists only for orthorhombic TiNiSi-type ZrNiGe (a semimetal).Pak 2025, J. Mater. Chem. A 13, 19455 (10.1039/d5ta00397k)
NiZrSiZrNiSicomp. investig.exp. (Saurabh 2022 (row notes))High-throughput half-Heusler transport/quality-factor screen only. No TE study of the cubic HH polymorph found; experimental TE transport exists only for orthorhombic TiNiSi-type ZrNiSi.Pak 2025, J. Mater. Chem. A 13, 19455 (10.1039/d5ta00397k)
OsNbSbNbOsSbcomp. investig.High-throughput half-Heusler transport/quality-factor screen only. Predicted thermodynamically stable HH (DFT and CALYPSO structure search) in an inverse-design TE paper whose experimental work covered TaFeSb, not NbOsSb; no TE calculation or measurement of NbOsSb found.Pak 2025, J. Mater. Chem. A 13, 19455 (10.1039/d5ta00397k)
OsTaSbTaOsSbcomp. investig.High-throughput half-Heusler transport/quality-factor screen only. Predicted thermodynamically stable HH (DFT and CALYPSO structure search) in the TaFeSb discovery paper; no TE calculation or measurement of TaOsSb found.Pak 2025, J. Mater. Chem. A 13, 19455 (10.1039/d5ta00397k)
PdScAsScPdAscomp. investig.pred. [85 predicted]Cubic F-43m: computational only, a DFT/deformation-potential TE study of pristine PdMX (M = Sc, Y; X = P, As, Sb) giving kappa_L and zT for PdScAs; also an ML power-factor prediction.Rani 2023, Materials Today Communications 36, 106461 (10.1016/j.mtcomm.2023.106461)
PdTiPbTiPdPbcomp. investig.Computational only: a single PBE-GGA DFT study of pristine PdTiZ (Z = Ge, Pb) including Boltzmann-transport thermoelectric properties.Kalita 2022, Int. J. Quantum Chem. 122, e26951 (10.1002/qua.26951)
PdTiSnTiPdSncomp. investig.Computational only: DFT+Boltzmann prediction of p-type TE performance of pristine TiPdSn, and a hybrid-DFT (CRYSTAL) TE study of TiMSn (M = Ni, Pd, Pt) including defects.Kaur 2017, EPL 117, 47002 (10.1209/0295-5075/117/47002)
PdZrSnZrPdSncomp. investig.Computational only: one DFT + Boltzmann-transport study (electronic, phonon, effective mass, ZT) of pristine PdXSn (X = Zr, Hf).Rani 2022, Molecules 27, 6567 (10.3390/molecules27196567)
PtNbGaNbPtGacomp. investig.Computational only: DFT (GGA/mBJ) + Boltzmann transport assessment of pristine PtNbZ (Z = Al, Ga, In) for TE use; a separate hybrid-DFT study covers structure/electronic/optical properties only.Abdullah 2025, RSC Adv. 15, 47036 (10.1039/d5ra06109a)
PtNbInNbPtIncomp. investig.Computational only: DFT (GGA/mBJ) + Boltzmann transport assessment of pristine PtNbZ (Z = Al, Ga, In); a separate hybrid-DFT study covers structure/electronic/optical properties only.Abdullah 2025, RSC Adv. 15, 47036 (10.1039/d5ra06109a)
PtTaGaTaPtGacomp. investig.Computational only: DFT stability and Boltzmann-transport power-factor study of pristine XTaZ (X = Pd, Pt; Z = Al, Ga, In) half-Heuslers; a separate hybrid-DFT study covers structure/electronic/optics.Khandy 2021, Sci. Rep. 11, 20756 (10.1038/s41598-021-00314-6)
PtVGaVPtGacomp. investig.High-throughput half-Heusler transport/quality-factor screen only. Computational only and not TE: a hybrid-DFT study of PtYZ (Y = V, Nb, Ta; Z = Al, Ga, In) reports structure, stability, electronic and optical properties; no transport/TE calculation or measurement for PtVGa was found.Pak 2025, J. Mater. Chem. A 13, 19455 (10.1039/d5ta00397k)
RhHfSbHfRhSbcomp. investig.Computational only: an ab initio study of pristine MRhSb (M = Ti, Zr, Hf) including BoltzTraP Seebeck/TE properties alongside elastic, thermodynamic and optical properties.Benzoudji 2019, Chin. J. Phys. 59, 434 (10.1016/j.cjph.2019.04.009)

Table 5.

compositionconventionalclasspoly.evidenceprincipal source (DOI)
RhNbGeNbRhGecomp. investig.exp. ([84], isostructural with TaRhGe (sec.))Computational only: DFT study of electronic, elastic, thermoelectric and optical properties of XRhZ (X = V, Nb; Z = Si, Ge), plus a DFT TE preprint on RhNbZ (Z = Ge, Sn).Ahmed 2024, East Eur. J. Phys. (2024 no. 1), 294 (10.26565/2312-4334-2024-1-26)
RhNbSnNbRhSncomp. investig.Computational only: Boltzmann transport + deformation-potential + Slack-model TE study of pristine XRhSn (X = V, Nb, Ta), plus a DFT TE preprint on RhNbZ (Z = Ge, Sn).Yang 2023, J. Supercond. Nov. Magn. 36, 1043 (10.1007/s10948-023-06536-1)
RhTaGeTaRhGecomp. investig.exp. ([84])Computational only: WIEN2k + BoltzTraP study of pristine RhTaZ (Z = Si, Ge, Sn) concluding high predicted ZT; compound itself listed as previously reported in ICSD.Boudjeltia 2021, Mod. Phys. Lett. B 35, 2150400 (10.1142/s0217984921504005)
RhTaSnTaRhSncomp. investig.Computational only: DFT+Boltzmann assessment of p-type TaRhSn, and a later Boltzmann/deformation-potential study of n-type XRhSn (X = V, Nb, Ta).Kaur 2017, Ceram. Int. 43, 15160 (10.1016/j.ceramint.2017.08.046)
RhTiAsTiRhAscomp. investig.exp. ((Weber 2017))High-throughput half-Heusler transport/quality-factor screen only. Computational only and not TE: TiRhAs appears in Materials Project (F-43m entry) and in a phonon/vibrational-entropy phase-stability study comparing the cubic half-Heusler and a distorted orthorhombic polymorph; no TE study found.Pak 2025, J. Mater. Chem. A 13, 19455 (10.1039/d5ta00397k)
RhTiBiTiRhBicomp. investig.Computational only: DFT + semiclassical Boltzmann study of pristine RhBiX (X = Ti, Zr, Hf) including lattice thermal conductivity and ZT.Wei 2023, RSC Adv. 13, 11513 (10.1039/d3ra01262j)
RhTiSbTiRhSbcomp. investig.Computational only: an ab initio study of MRhSb (M = Ti, Zr, Hf) including BoltzTraP Seebeck coefficients; a second DFT study covers structural, mechanical and phonon properties (no TE).Benzoudji 2019, Chin. J. Phys. 59, 434 (10.1016/j.cjph.2019.04.009)
RhVGeVRhGecomp. investig.pred. ([85 predicted])Computational only: WIEN2k + BoltzTraP TE study of pristine RhVX (X = Si, Ge), and a DFT electronic/elastic/TE/optical study of XRhZ (X = V, Nb; Z = Si, Ge).Mebed 2022, Int. J. Mod. Phys. B 37, 2350163 (10.1142/s0217979223501631)
RhZrBiZrRhBicomp. investig.Computational TE only: ab initio transport/ZT predictions for ideal ZrRhBi (also RhBiX study); the compound was synthesised (multiphase, high purity, F-43m confirmed by XRD/TEM) but no measured TE data were found.Vikram 2017, J. Mater. Chem. A 5, 6131 (10.1039/c7ta00920h)
Ru2ZrSiRu2ZrSicomp. investig.Computational only: one DFT study of L2_1 Ru2ZrSi reporting TE transport and ZT; separately, an experimental/theoretical Ru2TiSi study proposes Zr/Hf substitution on the Ti site (alloyed, not Ru2ZrSi itself).Benidris 2021, Solid State Commun. 339, 114466 (10.1016/j.ssc.2021.114466)
RuNbAsNbRuAscomp. investig.pred. ([86 predicted])Computational only: DFT + semiclassical Boltzmann study of pristine p-type RuVAs and RuNbAs (Seebeck, conductivity, lattice thermal conductivity, ZT).Cherifi 2020, Phys. Status Solidi B 257, 2000271 (10.1002/pssb.202000271)
RuNbSbNbRuSbcomp. investig.Computational only: first-principles TE assessments of XRuSb (X = V, Nb, Ta) and of NbMSb (M = Fe, Ru, Os).Kaur 2017, J. Phys. Chem. Solids 110, 108 (10.1016/j.jpcs.2017.05.006)
RuTaAsTaRuAscomp. investig.Computational only: one DFT + Boltzmann study of TaRuAs including substitutional doping on Ru and As sites.Nadhreen 2026, Ann. Phys. (Berlin) 538, e00096 (10.1002/andp.202500096)
RuTaSbTaRuSbcomp. investig.Computational only: first-principles prediction of high p-type ZT for RuTaSb (low band effective mass) and follow-up DFT studies of pristine and Bi-substituted TaSbRu.Fang 2017, Phys. Chem. Chem. Phys. 19, 4411 (10.1039/c6cp07897d)
RuVAsVRuAscomp. investig.Computational only: DFT + Boltzmann TE study of pristine p-type RuVAs/RuNbAs; a further DFT study covers structural, thermodynamic, mechanical and electronic properties (no TE).Cherifi 2020, Phys. Status Solidi B 257, 2000271 (10.1002/pssb.202000271)
RuVSbVRuSbcomp. investig.Computational only: first-principles TE assessment of pristine XRuSb (X = V, Nb, Ta).Kaur 2017, J. Phys. Chem. Solids 110, 108 (10.1016/j.jpcs.2017.05.006)
NiNbInNbNiInunderexploredNo dedicated TE (or other) study of HH NbNiIn found; it appears only as a computed database entry (Materials Project).

Table 6.

itemsetting
encoderALIGNN 2026.4.1, layers unchanged; 8 ALIGNN + 8 graph-convolution layers; 512 features; batch normalisation (package default 4 + 4 layers, 256 features)
inputs97 atom features (92 CGCNN + 5 Heusler-specific); bond length: 80 radial basis functions; angle cosine: 40; embeddings 64
graphcutoff 8 Å; at most 12 neighbours; line graph of bond pairs; structures not relaxed
readoutmean over atoms
head and output512 → 1024 → 2048 → 4002; GELU; dropout 0.2 after the first two layers; softplus; 1.08×1071.08 \times10^{7} of 4.25×1074.25 \times10^{7} trainable parameters
lossfive weighted terms, Eq. (2) (loss equation of the main text)
optimiserAdamW; learning rate 10−310^{-3}; weight decay 5×10−55 \times10^{-5}; gradient clipping 1.0; float32
schedulereduce-on-plateau (factor 0.5; patience 25, or 15 for cubic full-Heusler folds 0–2); minimum 10−710^{-7}
weight averagingSWA over the last 20% of epochs; learning rate annealed to 5×10−55 \times10^{-5} over 10 epochs; batch-normalisation statistics re-estimated
epochs, batch300, 128; cubic full Heusler: 150 (folds 0, 1) or 200 (folds 2–4), 64
splitsfive-fold per family, shuffled (seed 42); 10% of non-test entries for validation (72/8/20%)
checkpointsbest-validation checkpoint, highest validation rr over concatenated spectra before SWA (metrics); SWA weights (inference)
transferpretrained on all 51,257 spectra (100 epochs, SWA from epoch 85); encoder at 0.1× learning rate verified for two folds (cubic full Heusler, folds 0, 1)
hardwareone NVIDIA H100 NVL GPU per run; PyTorch 2.2.2 (CUDA 12.1), DGL 1.1.3, Python 3.11

Table S5. d-DOS model and training settings, read from the training code, the per-fold configuration files and the tensor shapes of the deployed checkpoints (Supplementary Note 3).

itemsetting
code, functionalQuantum ESPRESSO 7.1; PBE
pseudopotentialsSSSP 1.3.0 efficiency; PSlibrary fully relativistic PAW for SOC (1.0.0; 0.3.1 for Co and Mn, 0.2.3 for Ir)
cutoffslargest SSSP value of the species: 30–90 Ry (wavefunctions), 240–1,080 Ry (density); SOC: 1.15× (wavefunction) and 1.10× (density) the pseudopotential values
smearing, SCFMarzari–Vanderbilt, 0.01 Ry; convergence threshold 10−810^{-8} Ry; local-TF mixing, β=0.3\beta= 0.3
k-meshesni=max⁡(6,round⁡(K/ai))n_i = \max(6, \operatorname{round}(K/a_i)); SCF K=40K = 40 Å, shifted (63(6^3–113)11^3); NSCF K=55K = 55 Å, unshifted (93(9^3–153)15^3)
bandsNel/2+50N_{\mathrm{el}}/2 + 50; SOC: 2.4
magnetismcollinear; starting moments 0.2–0.4 μB\mu_{\mathrm{B}} on V, Cr, Mn, Fe, Co, Ni (antiparallel retry on SCF failure); SOC runs non-magnetic
geometryDXMG cell reduced to the primitive cell (spglib, tolerance 10−310^{-3}); no relaxation
BoltzTraP224.7.2; interpolation multiplier 15; spins merged, common τ\tau; T=300T = 300–1200 K in steps of 100 K
chemical potential∣μ−EF∣≤0.5|\mu- E_{\mathrm{F}}| \le0.5 eV (certification); ≤1.0\le1.0 eV with carrier caps 102010^{20} and 102110^{21} cm−3^{-3} (ranking)

Table S7. QE-PBE and BoltzTraP2 settings, read from the input and output files of the calculations.

elementrunsPF ratioΔEg\Delta E_g (meV)runslostPF ratio∣S∣|S| ratioσ/τ\sigma/\tau ratiop, 900 Kn, 900 Kcompositions lost
Hf990.88−3927120.860.990.850.821.00AuHfGa, AuHfIn, IrHfSb, NiHfSn, PdHfSn, PtHfSi
Ta820.80−553240.810.990.820.840.91NiTaGa, PtTaAl
W660.89−14800––––––
Re180.16–00––––––
Os810.88−49400.881.000.890.851.08–
Ir930.81−571840.761.000.830.780.99IrHfSb, IrTiSb
Pt890.87−10120100.700.940.800.560.98PtHfSi, PtTaAl, PtTiGe, PtTiSi, PtTiSn
Au600.80−9722200.550.910.660.491.03AuHfGa, AuHfIn, AuScSi, AuTiAl, AuTiGa, AuTiIn, AuZrAl, AuZrGa, AuZrIn, AuZrTl
Tl810.77−56220.550.880.710.461.11AuZrTl
Pb750.83−29400.880.941.000.771.01–
Bi650.84−321200.971.010.960.760.97–
all6070.87−56115400.820.970.860.761.0020 compositions

Table S8. Table S8. Spin–orbit coupling by heavy element. Paired scalar-relativistic and SOC runs of the same structure (analysis/soc_paired.py). A compound is counted under every heavy element it contains. PF ratio: median of best PF/τ\tau with SOC over best PF/τ\tau without; ΔEg\Delta E_g: median SOC minus scalar gap over runs gapped in both; ∣S∣|S| and σ/τ\sigma/\tau ratios at the respective optima. Scalar candidates are the heavy-element runs that are gapped and meet criteria (i)–(iii) without SOC; a run is lost when its SOC power factor falls below PF/τ0\tau_0. Lost compositions lose every candidate run. Of the 693 SOC calculations attempted, 607 finished and 86 failed and were not retried; only finished pairs are counted.

acts onwhat the first-principles results showedrevisionevidence after the revision
R1screenThe initial composite score (four d-DOS features at EFE_F) favoured metals: of its 100 top prediction-set entries, 83 carried a metal label, 7 were computed, none was certifiedrank by Cutler–Mott moments of the whole d-DOStop 100 by Smax⁡dS_{\max}^{\mathrm{d}}: 83 semiconductor labels, 98 computed, 35 certified; DROC-AUC vs composite = +0.068 [0.038, 0.101] (P)
R2screen98 of those 100 entries lie at least 0.1 eV atom−1^{-1} above the DXMag hullpriority filters on stability, the semiconductor label and ensemble spreadfilters order the selection rounds; the hull distance also enters certification
R3certificationmost d-DOS “semiconductors” are QE-PBE metals: 63.1% (T), 85.1% (P)classify every run by its QE-PBE band gapgapped runs pass the transport criteria most often for Eg=0.6E_g = 0.6–1.2 eV: 53–61% (T), 58–61% (P), 58–61% certified compositions vary smoothly: 105 (0.8×) to 65 (1.2×); 77 with the threshold for the corrected runs
R4certificationa threshold chosen during the campaign can be tuned to its resultsone power-factor threshold, the median 900 K PF/τ\tau of the first 1,401 runs, then held fixed
R5certification108 of the 309 qualified runs lack a QE-PBE gap (102 metals, 6 narrow-gap) and pass only with a shifted chemical potentialrequire a QE-PBE gap ≥0.136\ge0.136 eV201 gapped qualified runs remain (102 T, 99 P)
R6certificationspin–orbit coupling lowers the best PF/τ\tau (median ratio 0.87 over 607 runs)re-check compounds containing elements with atomic number ≥72\ge72 with SOC35 of 56 (T) and 40 of 59 (P) heavy gapped runs stay above the threshold; 5 Rh-based (T) unresolved, 1 (P) not run
R7rankingamong certified entries Smax⁡dS_{\max}^{\mathrm{d}} barely orders the DFT power factor (Spearman 0.13 T, 0.29 P)rank only on computed ∣S∣|S| and PF/τ\tau at fixed carrier concentration∣S∣|S| ranks stable across conventions (Spearman 0.87), PF/τ\tau ranks not (0.19); first Pareto layer in the main-text Pareto table

Table S10. Table S10. Development of the workflow (Supplementary Note 6). Each row gives the first-principles observation, the change it motivated and the evidence after it; T and P denote the training and prediction sets.

familyNtrainN_{\mathrm{train}}rˉ\bar{r}rˉ±2 eV\bar{r}_{\pm2\ \mathrm{eV}}RMSEBArec.NpredN_{\mathrm{pred}}DFT runs TDFT runs Pcertified comp. Tcertified comp. P
full cubic9,3960.8980.8570.3120.560.134,50422018555
full tetra8,0470.9250.8400.2260.660.3313,4799544200
half cubic9,3960.8740.8650.4230.580.214,9146144387074
half tetra6,9090.8840.8070.3370.620.2510,89620546610
inverse cubic9,0720.8760.8260.3320.520.046,70229412000
inverse tetra8,4370.9170.7990.2310.560.1214,48313437000
all51,2570.8950.8340.3120.570.1554,9781,5622,0217579

:::

Table S12. Indicator triage metrics within each set. ROC-AUC, PR-AUC and the fraction of certified entries captured in the top 10, 20 and 30% of each pre-DFT score, among computed entries of the stated subset. PR-AUC should be compared with the base rate given for each subset.

scoreROC-AUCPR-AUCtop 10%top 20%top 30%
prediction set, all computed: n=2,016n=2,016, positives = 79 (base rate 0.039)
Smax⁡dS_{\max}^{\mathrm{d}}0.9380.3400.710.910.99
Pmax⁡dP_{\max}^{\mathrm{d}}0.8770.1370.370.800.97
ξ\xi0.8520.1520.530.760.89
L0∗L_0^*0.7920.1170.180.380.72
initial composite0.8690.1680.460.760.90
electron count 18/240.8910.1570.400.801.00
random0.4940.0390.110.200.28
prediction set, d-DOS gap 0.10–1.40 eV: n=586n=586, positives = 79 (base rate 0.135)
Smax⁡dS_{\max}^{\mathrm{d}}0.8360.4060.350.600.77
Pmax⁡dP_{\max}^{\mathrm{d}}0.7510.2480.140.390.56
ξ\xi0.7140.2430.190.470.58
L0∗L_0^*0.6910.2690.170.290.38
initial composite0.7740.3040.290.480.62
electron count 18/240.7120.2130.160.320.47
random0.4690.1280.110.190.25
prediction set, 18 or 24 electrons: n=502n=502, positives = 79 (base rate 0.157)
Smax⁡dS_{\max}^{\mathrm{d}}0.8080.4070.300.540.71
Pmax⁡dP_{\max}^{\mathrm{d}}0.6880.2320.100.290.46
ξ\xi0.6720.2400.130.380.54
L0∗L_0^*0.5850.2390.150.180.32
initial composite0.7360.3060.240.380.57
electron count 18/240.5000.1570.100.200.30
random0.4770.1520.110.190.27
prediction set, half cubic: n=438n=438, positives = 74 (base rate 0.169)
Smax⁡dS_{\max}^{\mathrm{d}}0.7990.4070.300.500.68
Pmax⁡dP_{\max}^{\mathrm{d}}0.6900.2400.080.310.49
ξ\xi0.6640.2530.140.380.54
L0∗L_0^*0.6070.2460.140.190.31
initial composite0.6640.2410.140.350.41
electron count 18/240.6410.2210.130.260.39
random0.4690.1600.090.200.28
training set, all computed: n=1,562n=1,562, positives = 76 (base rate 0.049)
Smax⁡dS_{\max}^{\mathrm{d}}0.8690.1580.320.750.91
Pmax⁡dP_{\max}^{\mathrm{d}}0.6490.0640.070.200.47
ξ\xi0.6870.0810.160.420.58
L0∗L_0^*0.5570.0540.080.110.17
electron count 18/240.8580.1530.310.630.94
random0.5740.0750.200.330.42
training set, d-DOS gap 0.10–1.40 eV: n=661n=661, positives = 76 (base rate 0.115)
Smax⁡dS_{\max}^{\mathrm{d}}0.8290.3500.360.610.72

::: Table S13. Paired-bootstrap differences in ROC-AUC (2,000 resamples over computed entries, seed 0) within each set.

setsubsetcomparisonnnpos.Δ\DeltaAUC95% CI
prediction setall computedSmax⁡d−Pmax⁡dS_{\max}^{d} - P_{\max}^{d}2,01679+0.061[+0.047, +0.076]
prediction setall computedSmax⁡d−S_{\max}^{d} - composite2,01679+0.068[+0.038, +0.101]
prediction setall computedSmax⁡d−S_{\max}^{d} - electron count2,01679+0.047[+0.029, +0.063]
prediction setall computedSmax⁡d−ξS_{\max}^{d} - \xi2,01679+0.085[+0.053, +0.124]
prediction set18 or 24 electronsSmax⁡d−Pmax⁡dS_{\max}^{d} - P_{\max}^{d}50279+0.120[+0.081, +0.159]
prediction set18 or 24 electronsSmax⁡d−S_{\max}^{d} - composite50279+0.072[+0.007, +0.133]
prediction set18 or 24 electronsSmax⁡d−ξS_{\max}^{d} - \xi50279+0.136[+0.086, +0.186]
training setall computedSmax⁡d−Pmax⁡dS_{\max}^{d} - P_{\max}^{d}1,56276+0.221[+0.171, +0.267]
training setall computedSmax⁡d−S_{\max}^{d} - electron count1,56276+0.011[−0.011, +0.035]
training setall computedSmax⁡d−ξS_{\max}^{d} - \xi1,56276+0.183[+0.134, +0.238]
training set18 or 24 electronsSmax⁡d−Pmax⁡dS_{\max}^{d} - P_{\max}^{d}49876+0.248[+0.178, +0.317]
training set18 or 24 electronsSmax⁡d−ξS_{\max}^{d} - \xi49876+0.208[+0.137, +0.277]

Table S13. Paired-bootstrap differences in ROC-AUC (2,000 resamples over computed entries, seed 0) within each set.

scoreROC-AUCPR-AUCtop 10%top 20%top 30%
Pmax⁡dP_{\max}^{d}0.5500.1170.040.120.23
ξ\xi0.5600.1280.050.210.38
L0∗L_0^*0.5220.1430.090.130.24
electron count 18/240.7540.2090.180.360.54
random0.5740.1720.220.320.41
training set, 18 or 24 electrons: n=498n = 498, positives = 76 (base rate 0.153)
Smax⁡dS_{\max}^{d}0.8050.3370.260.510.64
Pmax⁡dP_{\max}^{d}0.5570.1590.070.140.32
ξ\xi0.5960.1900.120.290.47
L0∗L_0^*0.4740.1630.110.140.22
electron count 18/240.5000.1530.100.200.30
random0.5670.2250.180.300.40
training set, half cubic: n=614n = 614, positives = 70 (base rate 0.114)
Smax⁡dS_{\max}^{d}0.7650.2020.110.340.64
Pmax⁡dP_{\max}^{d}0.6180.1380.070.170.41
ξ\xi0.6000.1480.140.300.44
L0∗L_0^*0.5650.1490.100.130.22
electron count 18/240.7320.1930.170.340.51
random0.5410.1510.140.230.34

Table 7.

Table S14. All 80 certified compositions, with computed SS (µV K−1^{-1}) and PF/τ\tau (1012^{12} W m−1^{-1} K−2^{-2} s−1^{-1}) at 900 K and ∣n∣≤1021|n| \le10^{21} cm−3^{-3} for p- and n-type doping. Set: certified in the training (T) and/or prediction (P) set. EgE_g: QE-PBE gap; EhullE_{\mathrm{hull}}: DXMag hull distance (eV atom−1^{-1}); SOC: values with spin–orbit coupling. CRTA values, not zTzT predictions.

compositionfamilysetEgE_g (eV)EhullE_{\mathrm{hull}}SOCp-type SSp-type PF/τ\taun-type SSn-type PF/τ\tau
AuHfAlhalf cubicT+P0.640.033yes2220.57−1290.54
CoHfAshalf cubicT+P1.290.003yes2961.39−2211.35
CoHfBihalf cubicT+P0.980.000yes2651.19−2171.15
CoHfSbhalf cubicT+P1.150.016yes2931.33−2131.00
CoNbGehalf cubicT+P1.090.000no2801.76−2181.11
CoNbSnhalf cubicT+P1.040.039no2881.63−2201.02
CoTaGehalf cubicT+P1.220.000yes2821.52−2030.79
CoTaSihalf cubicT+P1.270.095yes2591.40−2060.89
CoTaSnhalf cubicT+P1.070.038yes2961.39−1880.71
CoTiAshalf cubicT+P1.320.031no3121.48−2811.07
CoTiBihalf cubicT+P0.910.000yes2861.08−2520.72
CoTiSbhalf cubicT+P1.080.029no3011.35−2570.89
CoVGehalf cubicT+P0.680.002no3101.43−1460.48
CoVSihalf cubicT+P0.580.038no2951.40−1440.44
CoVSnhalf cubicT+P0.660.036no3201.28−1720.47
CoZrAshalf cubicT+P1.230.006no2741.26−2371.19
CoZrBihalf cubicT+P0.990.000yes2801.19−2170.98
CoZrSbhalf cubicT+P1.080.000no2831.27−2170.95
compositionfamilysetEgE_g (eV)EhullE_{\mathrm{hull}}SOCp-type SSp-type PF/τ\taun-type SSn-type PF/τ\tau
Fe2_2HfSifull cubicT+P0.330.082yes2080.83−2390.89
Fe2_2NbAlfull cubicT+P0.300.000no2121.08−2210.81
Fe2_2TaAlfull cubicT+P0.290.000yes1870.77−2190.83
Fe2_2TiSifull cubicT+P0.370.020no1900.77−2610.86
FeNbAshalf cubicT+P0.570.000no2311.37−1470.35
FeNbSbhalf cubicT+P0.600.011no2371.31−1480.37
FeTaAshalf cubicT+P0.920.000yes2311.27−1020.36
FeTaSbhalf cubicT+P0.930.000yes2381.23−1120.36
FeVAshalf cubicT+P0.360.009no2461.26−1360.61
FeVSbhalf cubicT+P0.390.002no2531.18−1520.60
IrNbGehalf cubicT+P0.690.000yes2391.63−880.43
IrNbSnhalf cubicT+P0.620.000yes2491.60−880.40
IrTaGehalf cubicT+P1.000.000yes2371.40−960.50
IrTaSihalf cubicT+P0.870.080yes2301.33−780.36
IrTaSnhalf cubicT+P0.960.000yes2471.31−920.40
IrTiAshalf cubicT+P0.670.020yes1920.78−1710.92
IrVGehalf cubicT+P0.360.000yes2611.28−1480.73
NiHfGehalf cubicT+P0.580.001yes1720.80−1430.83
NiHfSihalf cubicT+P0.710.090yes2110.92−1440.81
NiNbInhalf cubicT+P0.140.075no1150.75−1220.47
NiScAshalf cubicT+P0.480.043no1510.67−1821.12
NiScBihalf cubicT+P0.190.022yes1020.38−1580.88
NiScSbhalf cubicT+P0.270.010no1410.66−1600.89
NiTiGehalf cubicT+P0.640.012no2301.02−1710.72
NiTiPbhalf cubicT+P0.350.073yes2060.70−1670.62
NiTiSihalf cubicT+P0.760.092no2661.08−1700.73
NiTiSnhalf cubicT+P0.460.043no2240.93−1610.64
NiVGahalf cubicT+P0.390.096no1781.04−2250.72
NiYBihalf cubicT+P0.210.010yes870.27−1500.97
NiYSbhalf cubicT+P0.300.002no1410.59−1530.98
NiZrGehalf cubicT+P0.690.002no2161.01−1460.80
NiZrSihalf cubicT+P0.820.085no2831.22−1480.79
NiZrSnhalf cubicT+P0.510.019no1960.87−1380.70
OsNbSbhalf cubicT+P0.260.000yes1781.13−1130.69
OsTaSbhalf cubicT+P0.560.000yes1720.97−1250.88
PdScAshalf cubicT0.440.096no1430.56−1871.18
PdScSbhalf cubicT+P0.280.014no1370.61−1610.87
PdTiPbhalf cubicT+P0.370.096yes2070.66−1870.55
PdTiSnhalf cubicT+P0.480.000no2160.94−1870.66
PdZrSnhalf cubicT+P0.470.000no1680.82−1390.62
PtNbGahalf cubicT+P0.550.000yes1551.04−1370.35
PtNbInhalf cubicT+P0.470.075yes1541.12−1380.55
PtScSbhalf cubicT+P0.630.017yes1200.32−1980.97
PtTaGahalf cubicT+P1.050.009yes1630.99−1200.47
PtVGahalf cubicT+P0.330.097yes1861.04−1370.51
RhHfSbhalf cubicP1.100.020yes1480.80−2111.05
RhNbGehalf cubicT+P0.760.066no2331.81−1440.39
RhNbSnhalf cubicT+P0.760.044no2411.82−1390.39
RhTaGehalf cubicP1.160.017yes2781.68−1470.34
RhTaSnhalf cubicP1.080.044yes2961.47−1140.39
RhTiAshalf cubicT+P0.830.033no2031.12−1620.60
RhTiBihalf cubicP0.700.037yes2100.78−2580.66
RhTiSbhalf cubicT+P0.750.031no2141.08−1750.58
RhVGehalf cubicT+P0.450.050no2911.50−1380.61
RhZrBihalf cubicP0.990.014yes1670.68−2301.12
Ru2_2ZrSifull cubicT+P0.200.000no880.54−1921.10
RuNbAshalf cubicT+P0.450.038no1871.29−1100.64
RuNbSbhalf cubicT+P0.450.022no2001.34−1030.54
RuTaAshalf cubicT+P0.430.000yes1921.23−1110.71
RuTaSbhalf cubicT+P0.730.022yes2051.25−1100.60
RuVAshalf cubicT+P0.250.020no2081.19−1590.85
RuVSbhalf cubicT+P0.260.074no2271.22−1640.80

Table S14.

compositionDXMag stringcomputed incertified inEgE_g (eV)outcome
TiNiSnNiTiSnP+TP+T0.46certified
ZrNiSnNiZrSnP+TP+T0.51certified
HfNiSnNiHfSnP+T-0.39SOC PF/τ\tau 1.046 below threshold
TiCoSbCoTiSbP+TP+T1.08certified
ZrCoSbCoZrSbP+TP+T1.08certified
HfCoSbCoHfSbP+TP+T1.15certified
VFeSbFeVSbP+TP+T0.40certified
NbFeSbFeNbSbP+TP+T0.60certified
TaFeSbFeTaSbP+TP+T0.93certified
NbCoSnCoNbSnP+TP+T1.04certified
ZrCoBiCoZrBiP+TP+T1.00certified

Table S15. Established half-Heusler thermoelectric compositions in the campaign. The list is taken from the reviews and studies cited in the main text [76, 16, 17, 19] and is not exhaustive. DXMag writes half-Heusler compositions in site order. EgE_g: QE-PBE gap of the reported entry. The certified prediction-set entries are near-duplicates of the training-set entries. No numerical comparison with published coefficients is made. Script: scripts/figures/known_hh_check.py.

compositionfamilysetSSPF/τ\taucombined rank
CoNbGehalf cubicT+P2872.111
RhNbGehalf cubicT+P2112.642
RhTaSnhalf cubicP2991.724
IrTaGehalf cubicT+P3111.3630
CoTaSihalf cubicT+P3191.3630
CoHfAshalf cubicT+P3351.3530
CoTiAshalf cubicT+P3591.3334

Table S16. Earlier best-over-all-conditions Pareto set, as presented in the project’s internal ranking: each composition at its best PF/τ\tau over 300–1200 K with re-optimised doping (∣μ−EF∣≤0.5|\mu- E_F| \le0.5 eV). SS in µV K−1^{-1}, PF/τ\tau in 101210^{12} W m−1^{-1} K−2^{-2} s−1^{-1}. All optima lie at 1200 K; the main text therefore ranks at 900 K and fixed carrier concentration.

Supplementary Figures

Figure S4. The d-DOS model: a stock ALIGNN encoder with a task-specific head, output and loss. Grey cards are components of the ALIGNN package used unchanged, with the settings of this work in navy; navy cards are specific to the d-DOS task. Graphs are built from the structure stored with each training spectrum or from the listed DXMag cell for prediction-set entries, without relaxation. The five Heusler atom features are the d-electron count, the largest common oxidation state, the distance of the d count from a half-filled or filled shell, the principal quantum number of the d shell, and a second copy of the d-electron count. The output spectrum is a held-out entry with the median Pearson rr (grey, DFT; blue, prediction from the best-validation checkpoint). The bottom row gives the five loss terms and their weights (Eq. (12); Supplementary Note 3).

Figure S5. How the 30 deployed models were obtained and applied. a, Transfer-learning lineage. A foundation model trained on all 51,257 training-set spectra initialises the family models. The solid arrow, foundation to cubic full Heusler with the encoder at 0.1×0.1\times the head’s learning rate, is recorded in the run files of folds 0 and 1. The dashed tree is the lineage of the training plan; four project sources give different parents and no checkpoint records it (Table S4). b, Training of each family: the data partition of one fold, and the validation correlation of cubic full-Heusler fold 1 over its 150 epochs (TensorBoard record), with the best-validation checkpoint (orange) at epoch 2 and the SWA window (green). The best-validation checkpoint gives the held-out metrics; the SWA weights give the predictions. c, Inference for the prediction set. Each entry is routed by family to that family’s five SWA fold models; the mean of their softplus outputs is the predicted d-DOS, and their spread us(E)u_s(E), through its Fermi-window mean uFu_F, is the uncertainty used by the reliability filter. Five members are specified in the screening scripts of all six families; run summaries confirming them survive for two families.

Figure S7. Effect of the mesh correction on the best PF/τ\tau of scalar-relativistic runs, comparing interpolation of the non-self-consistent eigenvalues with the earlier, erroneous interpolation of the shifted self-consistent mesh.

Figure S8. a, Composition of the 100 highest-ranked prediction-set entries by the initial composite score (Supplementary Note 5), the d-DOS power-factor indicator Pmax⁡dP_{\max}^{\mathrm{d}} and the d-DOS Seebeck indicator Smax⁡dS_{\max}^{\mathrm{d}}. b,e, Smax⁡dS_{\max}^{\mathrm{d}} of each set against the DFT intrinsic maximum ∣S∣|S| (300–1200 K), coloured by QE-PBE class; open circles mark certified entries, and the dotted line is the Seebeck criterion. Horizontal axes are set-specific. c,f, Smax⁡dS_{\max}^{\mathrm{d}} against the DFT best power factor among certified entries, with Spearman’s ρ\rho. d,g, ROC-AUC with which each pre-DFT score ranks certified entries among computed entries: overall (filled) and within three subsets (open). Paired-bootstrap differences are printed with 95% intervals. The initial composite score exists only for the prediction set. Scores are compared only within a set; “18/24 e−” is the subset obeying the electron-count rule. (More detailed version of main-text Figure 5 and 7; panel a documents the initial composite score.)

Figure S9. Held-out spectral fidelity by family (training set, five-fold cross-validation, best-validation checkpoints). Cumulative distributions of per-material Pearson rr over the full spectrum and within 2 eV of EFE_F.

Figure S10. Energy-resolved mean absolute error of the predicted d-DOS, averaged over the five folds of each family. The absolute error is small near EFE_F partly because the d-DOS itself is small there. It should not be read as higher accuracy at the Fermi level (compare main-text Figure 4e,Figure 4f).

Figure S11. Held-out d-DOS fidelity in detail (training set, best-validation checkpoints; the population panels of main-text Figure 4 in full). a, Confusion matrix of the held-out gap flag. b, A real gap filled by the prediction (YScGe). c, A spurious gap opened in a metal (ReTiTl); hatching, the ±1\pm1 eV flag window; tan strip, the label window. d,e, Cumulative distributions of the per-spectrum Pearson rr over the full spectrum and within 2 eV of EFE_F for the four cells of a.

Figure S12. The screen’s labels tested by QE-PBE, per set. Top row, training set (screen on DFT d-DOS); bottom row, prediction set (screen on ML-predicted d-DOS). a,d, QE-PBE electronic class of the computed runs in each screen label: M, metal; HM, half-metal; otherwise semiconductor by d-DOS gap tier in eV. White numbers give the gapped share and the numbers above the bars give the runs per label. b,e, d-DOS gap assigned by the screen against the QE-PBE gap for runs labelled semiconductor; points below the line have no QE-PBE gap, and the dashed line is parity. c,f, Share of gapped runs that are qualified runs (meeting the Seebeck criterion, above the power-factor threshold and stable), by QE-PBE gap, with the number of runs per bin; the green band marks 0.6–1.2 eV. All denominators are within a set. (Detailed version of main-text Figure 5a,Figure 5d with gap parity and qualified-run rates.)

Figure S13. The indicator for a prediction-set entry (CoTiSb, certified). a, Predicted d-DOS, ensemble mean ± spread. b, Cutler–Mott Seebeck coefficient at 900 K from the predicted d-DOS, with its maximum Smax⁡dS_{\max}^{d}, and the QE-PBE + BoltzTraP2 Seebeck coefficient of the same entry at EFE_F and at its power-factor optimum.

Figure S15. What survives, and how robustly. a, Best PF/τ\tau of heavy (Z≥72Z \ge72) gapped qualified runs with a completed SOC run, scalar-relativistic against SOC. Symbols are coloured when the SOC value stays above the power-factor threshold (dotted lines) and grey otherwise; triangles mark the training set and open circles the prediction set. The SOC runs use fully relativistic PSlibrary potentials, so the comparison also reflects a change of pseudopotential family. b, PF/τ\tau of the 155 certified entries under four conventions, counting how many stay above the declared power-factor threshold (dashed): best value over 300–1200 K with ∣μ−EF∣≤0.5|\mu-E_{\mathrm{F}}| \le0.5 eV (the certification basis); 900 K in the same window; and 900 K with the carrier concentration capped at 1021 cm−310^{21}\ \mathrm{cm}^{-3} or 1020 cm−310^{20}\ \mathrm{cm}^{-3}. Horizontal jitter is for display only. c, Certified compositions against the power-factor threshold relative to its declared value; the diamond marks the threshold re-derived from mesh-corrected runs. d,e, Computed ∣S∣|S| and PF/τ\tau of the 80 certified compositions at 900 K and ∣n∣≤1021 cm−3|n| \le10^{21}\ \mathrm{cm}^{-3}, for p-type (d) and n-type (e) doping, coloured by the set(s) in which each composition is certified; the green line marks the first Pareto layer, and open squares mark the established half-Heusler thermoelectrics of Table S15. SOC values are used for compounds with Z≥72Z \ge72. (Complements main-text Figure 10 and Figure 8d; panel b gives the transport conventions referred to in the main text.)

References

  1. [1]Lon E. Bell. Cooling, Heating, Generating Power, and Recovering Waste Heat with Thermoelectric Systems. Science, 321(5895):1457–1461, September 2008. ISSN 1095-9203. doi: 10.1126/science.1158899.DOI
  2. [2]Jian He and Terry M. Tritt. Advances in thermoelectric materials research: Looking back and moving forward. Science, 357(6358):eaak9997, September 2017. ISSN 1095-9203. doi: 10.1126/science.aak9997.DOI
  3. [3]G. Jeffrey Snyder and Eric S. Toberer. Complex thermoelectric materials. Nature Materials, 7(2):105–114, February 2008. doi: 10.1038/nmat2090.DOI
  4. [4]J. O. Sofo and G. D. Mahan. Optimum band gap of a thermoelectric material. Physical Review B, 49(7):4565–4570, February 1994. ISSN 1095-3795. doi: 10.1103/physrevb.49.4565.DOI
  5. [5]Georg K. H. Madsen. Automated Search for New Thermoelectric Materials: The Case of LiZnSb. Journal of the American Chemical Society, 128(37):12140–12146, August 2006. doi: 10.1021/ja062526a.DOI
  6. [6]Georg K. H. Madsen, Jesús Carrete, and Matthieu J. Verstraete. BoltzTraP2, a program for interpolating band structures and calculating semi-classical transport coefficients. Computer Physics Communications, 231:140–145, October 2018. doi: 10.1016/j.cpc.2018.05.010.DOI
  7. [7]Jiong Yang, Huanming Li, Ting Wu, Wenqing Zhang, Lidong Chen, and Jihui Yang. Evaluation of Half-Heusler Compounds as Thermoelectric Materials Based on the Calculated Electrical Transport Properties. Advanced Functional Materials, 18(19):2880–2888, October 2008. doi: 10.1002/adfm.200701369.DOI
  8. [8]Wei Chen, Jan-Hendrik Pöhls, Geoffroy Hautier, Danny Broberg, Saurabh Bajaj, Umut Aydemir, Zachary M. Gibbs, Hong Zhu, Mark Asta, G. Jeffrey Snyder, Bryce Meredig, Mary Anne White, Kristin Persson, and Anubhav Jain. Understanding thermoelectric properties from high-throughput calculations: trends, insights, and comparisons with experiment. Journal of Materials Chemistry C, 4(20):4414–4426, 2016. doi: 10.1039/c5tc04339e.DOI
  9. [9]Francesco Ricci, Wei Chen, Umut Aydemir, G. Jeffrey Snyder, Gian-Marco Rignanese, Anubhav Jain, and Geoffroy Hautier. An ab initio electronic transport database for inorganic materials. Scientific Data, 4(1):170085, July 2017. doi: 10.1038/sdata.2017.85.DOI
  10. [10]Prashun Gorai, Vladan Stevanović, and Eric S. Toberer. Computationally guided discovery of thermoelectric materials. Nature Reviews Materials, 2(9):17053, August 2017. doi: 10.1038/natrevmats.2017.53.
  11. [11]Francesco Ricci, Alexander J. Jackson, Anubhav Jain, Gian-Marco Rignanese, and Geoffroy Hautier. Gapped metals as thermoelectric materials revealed by high-throughput screening. Journal of Materials Chemistry A, 8(34):17579–17594, 2020. ISSN 2050-7496. doi: 10.1039/d0ta05197g.
  12. [12]Xue Jia, Yanshuai Deng, Xin Bao, Honghao Yao, Shan Li, Zhou Li, Chen Chen, Xinyu Wang, Jun Mao, Feng Cao, Jiehe Sui, Junwei Wu, Cuiping Wang, Qian Zhang, and Xingjun Liu. Unsupervised machine learning for discovery of promising half-Heusler thermoelectric materials. npj Computational Materials, 8(1):34, 2022. doi: 10.1038/s41524-022-00723-9.DOI
  13. [13]Hem Chandra Kandpal, Claudia Felser, and Ram Seshadri. Covalent bonding and the nature of band gaps in some half-Heusler compounds. Journal of Physics D: Applied Physics, 39(5):777–785, February 2006. doi: 10.1088/0022-3727/39/5/s02.DOI
  14. [14]Tanja Graf, Claudia Felser, and Stuart S.P. Parkin. Simple rules for the understanding of Heusler compounds. Progress in Solid State Chemistry, 39(1):1–50, May 2011. doi: 10.1016/j.progsolidstchem.2011.02.001.DOI
  15. [15]Shuo Chen and Zhifeng Ren. Recent progress of half-Heusler for moderate temperature thermoelectric applications. Materials Today, 16(10):387–395, October 2013. ISSN 1369-7021. doi: 10.1016/j.mattod.2013.09.015.
  16. [16]Robert J. Quinn and Jan-Willem G. Bos. Advances in half-Heusler alloys for thermoelectric power generation. Materials Advances, 2(19):6246–6266, 2021. doi: 10.1039/d1ma00707f.DOI
  17. [17]Chenguang Fu, Shengqiang Bai, Yintu Liu, Yunshan Tang, Lidong Chen, Xinbing Zhao, and Tiejun Zhu. Realizing high figure of merit in heavy-band p-type half-Heusler thermoelectric materials. Nature Communications, 6(1):8144, September 2015. doi: 10.1038/ncomms9144.
  18. [18]Hangtian Zhu, Ran He, Jun Mao, Qing Zhu, Chunhua Li, Jifeng Sun, Wuyang Ren, Yumei Wang, Zishang Liu, Zhongjia Tang, Andrej Sotnikoy, Zhiming Wang, David Broido, David J. Singh, Gang Chen, Kornelius Nielsch, and Zhifeng Ren. Discovery of ZrCoBi based half Heuslers with high thermoelectric conversion efficiency. Nature Communications, 9(1):2497, June 2018. ISSN 2041-1723. doi: 10.1038/s41467-018-04958-3.
  19. [19]Hangtian Zhu, Jun Mao, Yuwei Li, Jifeng Sun, Yumei Wang, Qing Zhu, Guannan Li, Qichen Song, Jiawei Zhou, Yuhao Fu, Ran He, Tian Tong, Zihang Liu, Wuyang Ren, Li You, Zhiming Wang, Jun Luo, Andrei Sotnikov, Jiming Bao, Kornelius Nielsch, Gang Chen, David J. Singh, and Zhifeng Ren. Discovery of TaFeSb-based half-Heuslers with high thermoelectric performance. Nature Communications, 10(1):270, January 2019. doi: 10.1038/s41467-018-08223-5.DOI
  20. [20]Daniel I. Bilc, Geoffroy Hautier, David Waroquiers, Gian-Marco Rignanese, and Philippe Ghosez. Low-Dimensional Transport and Large Thermoelectric Power Factors in Bulk Semiconductors by Band Engineering of Highly Directional Electronic States. Physical Review Letters, 114(13):136601, 2015. doi: 10.1103/PhysRevLett.114.136601.DOI
  21. [21]Jiangang He, Maximilian Amsler, Yi Xia, Shahab Naghavi, Vinay I. Hegde, Shiqiang Hao, Stefan Goedecker, Vidvuds Ozoliņš, and Chris Wolverton. Ultralow Thermal Conductivity in Full Heusler Semiconductors. Physical Review Letters, 117(4):046602, 2016. doi: 10.1103/PhysRevLett.117.046602.DOI
  22. [22]Sergey V. Fealey, Yari Ferrante, Jaewoo Jeong, Mahesh G. Samant, Barbara Jones, and Stuart S. P. Parkin. Origin of the Tetragonal Ground State of Heusler Compounds. Physical Review Applied, 7(3):034022, 2017. doi: 10.1103/physrevapplied.7.034022.
  23. [23]Jesús Carrete, Natalio Mingo, Shidong Wang, and Stefano Curtarolo. Nanograined Half-Heusler Semiconductors as Advanced Thermoelectrics: An Ab Initio High-Throughput Statistical Study. Advanced Functional Materials, 24(47):7427–7432, 2014. doi: 10.1002/adfm.201401201.DOI
  24. [24]Sandip Bhattacharya and Georg K. H. Madsen. A novel p-type half-Heusler from high-throughput transport and defect calculations. Journal of Materials Chemistry C, 4(47):11261–11268, 2016. doi: 10.1039/c6tc04259g.DOI
  25. [25]Enda Xiao and Terumasa Tadano. High-throughput computational screening of full-Heusler compounds with phonon considerations for enhanced material discovery. Acta Materialia, 297:121312, September 2025. doi: 10.1016/j.actamat.2025.121312.DOI
  26. [26]Enda Xiao and Terumasa Tadano. Accurate screening of functional materials with machine-learning potential and transfer-learned regressions: Heusler alloy benchmark. npj Computational Materials, 12(1):133, 2026. doi: 10.1038/s41524-026-02013-0. Published online 19 February 2026; article number 133. Preprint: arXiv:2508.20556.DOI
  27. [27]Stefano Sanvito, Corey Oses, Junkai Xue, Anurag Tiwari, Mario Zic, Thomas Archer, Pelin Tozman, Munsuwamy Venkatesan, Michael Coey, and Stefano Curtarolo. Accelerated discovery of new magnets in the Heusler alloy family. Science Advances, 3(4):e1602241, 2017. doi: 10.1126/sciadv.1602241.DOI
  28. [28]Terumasa Tadano. HeuslerDB_elecDOS_ver1.0. Dataset, National Institute for Materials Science (archives dated 241229), CC BY 4.0, 2025. URL https://doi.org/10.48505/nims.57494.
  29. [29]Stanislav Chadov, Xiaoliang Qi, Jürgen Kübler, Gerhard H. Fecher, Claudia Felser, and Shou Cheng Zhang. Tunable multifunctional topological insulators in ternary Heusler compounds. Nature Materials, 9(7):541–545, 2010. doi: 10.1038/nmat2770.DOI
  30. [30]San-Dong Guo. Importance of spin–orbit coupling in power factor calculations for half-Heusler ANiB (A = Ti, Hf, Sc, Y; B = Sn, Sb, Bi). Journal of Alloys and Compounds, 663:128–133, April 2016. ISSN 0925-8388. doi: 10.1016/j.jallcom.2015.12.139.
  31. [31]Melvin Cutler and N. F. Mott. Observation of Anderson Localization in an Electron Gas. Physical Review, 181(3):1336–1340, May 1969. doi: 10.1103/physrev.181.1336.DOI
  32. [32]M. Jonson and G. D. Mahan. Mott’s formula for the thermopower and the Wiedemann–Franz law. Physical Review B, 21(10):4223–4229, May 1980. doi: 10.1103/physrevb.21.4223.DOI
  33. [33]H. J. Goldsmid and J. W. Sharp. Estimation of the thermal band gap of a semiconductor from Seebeck measurements. Journal of Electronic Materials, 28(7):869–872, 1999. doi: 10.1007/s11664-999-0211-y.DOI
  34. [34]Zachary M. Gibbs, Hyun-Sik Kim, Heng Wang, and G. Jeffrey Snyder. Band gap estimation from temperature dependent Seebeck measurement—Deviations from the 2e|S|maxTmax relation. Applied Physics Letters, 106(2):021112, January 2015. ISSN 1077-3118. doi: 10.1063/1.4905922. Erratum: Appl. Phys. Lett. 108, 090901 (2016).DOI
  35. [35]I. Galanakis, P. H. Dederichs, and N. Papanikolaou. Origin of the gap in the half-ferromagnetic Heusler alloys. Physical Review B, 66(13):134428, 2002. doi: 10.1103/PhysRevB.66.134428.DOI
  36. [36]I. Galanakis, P. H. Dederichs, and N. Papanikolaou. Slater–Pauling behavior and origin of the half-metallicity of the full-Heusler alloys. Physical Review B, 66(17):174429, 2002. doi: 10.1103/PhysRevB.66.174429.DOI
  37. [37]Yanzhong Pei, Xiaoya Shi, Aaron LaLonde, Heng Wang, Lidong Chen, and G. Jeffrey Snyder. Convergence of electronic bands for high performance bulk thermoelectrics. Nature, 473(7345):66–69, 2011. doi: 10.1038/nature09996.DOI
  38. [38]Zachary M. Gibbs, Francesco Ricci, Guodong Li, Hong Zhu, Kristin Persson, Gerbrand Ceder, Geoffroy Hautier, Anubhav Jain, and G. Jeffrey Snyder. Effective mass and Fermi surface complexity factor from ab initio band structure calculations. npj Computational Materials, 3(1):8, 2017. doi: 10.1038/s41524-017-0013-3.DOI
  39. [39]Guangzong Xing, Jifeng Sun, Yuwei Li, Xiaofeng Fan, Weitao Zheng, and David J. Singh. Electronic fitness function for screening semiconductors as thermoelectric materials. Physical Review Materials, 1(6):065405, November 2017. doi: 10.1103/physrevmaterials.1.065405.DOI
  40. [40]Byung Chul Yeo, Donghun Kim, Chansoo Kim, and Sang Soo Han. Pattern Learning Electronic Density of States. Scientific Reports, 9(1):5879, April 2019. doi: 10.1038/s41598-019-42277-9.DOI
  41. [41]Anand Chandrasekaran, Deepak Kamal, Rohit Batra, Chiho Kim, Lihua Chen, and Rampi Ramprasad. Solving the electronic structure problem with machine learning. npj Computational Materials, 5(1):22, February 2019. doi: 10.1038/s41524-019-0162-7.DOI
  42. [42]Chiheb Ben Mahmoud, Andrea Anelli, Gábor Csányi, and Michele Ceriotti. Learning the electronic density of states in condensed matter. Physical Review B, 102(23):235130, December 2020. doi: 10.1103/physrevb.102.235130.DOI
  43. [43]Prathik R. Kaundinya, Kamal Choudhary, and Surya R. Kalidindi. Prediction of the Electron Density of States for Crystalline Compounds with Atomistic Line Graph Neural Networks (ALIGNN). JOM, 74(4):1395–1405, March 2022. doi: 10.1007/s11837-022-05199-y.DOI
  44. [44]Victor Fung, P. Ganesh, and Bobby G. Sumpter. Physically Informed Machine Learning Prediction of Electronic Density of States. Chemistry of Materials, 34(11):4848–4855, May 2022. doi: 10.1021/acs.chemmater.1c04252.DOI
  45. [45]Namkyeong Lee, Heewoong Noh, Sungwon Kim, Dongmin Hyun, Gyoung S. Na, and Chanyoung Park. Density of States Prediction of Crystalline Materials via Prompt-guided Multi-Modal Transformer. In Advances in Neural Information Processing Systems 36 (NeurIPS 2023), pages 61678–61698. Curran Associates, 2023. doi: 10.52202/075280-2694.DOI
  46. [46]Wei Bin Howl, Pol Febrer, Sanggyu Chong, Arslan Mazitov, Filippo Bigi, Matthias Kellner, Sergey Pozdnyakov, and Michele Ceriotti. A universal machine learning model for the electronic density of states. Digital Discovery, 5(4):1635–1649, 2026. doi: 10.1039/d5dd00557d.
  47. [47]Kamal Choudhary and Brian DeCost. Atomistic Line Graph Neural Network for improved materials property predictions. npj Computational Materials, 7(1):185, November 2021. doi: 10.1038/s41524-021-00650-1.DOI
  48. [48]Kamal Choudhary, Kevin F Garritty, and Francesca Tavazza. Data-driven discovery of 3D and 2D thermoelectric materials. Journal of Physics: Condensed Matter, 32(47):475501, August 2020. doi: 10.1088/1361-648X/aba06b.DOI
  49. [49]Ye Sheng, Yasong Wu, Jiong Yang, Wencong Lu, Pierre Villars, and Wenqing Zhang. Active learning for the power factor prediction in diamond-like thermoelectric materials. npj Computational Materials, 6(1):171, 2020. doi: 10.1038/s41524-020-00439-8.
  50. [50]Shufeng Kong, Francesco Ricci, Dan Guevarra, Jeffrey B. Neaton, Carla P. Gomes, and John M. Gregoire. Density of states prediction for materials discovery via contrastive learning from probabilistic embeddings. Nature Communications, 13(1):949, February 2022. doi: 10.1038/s41467-022-28543-x.DOI
  51. [51]Wei Bin How, Sanggyu Chong, Federico Grasselli, Kevin K. Huguenin-Dumittan, and Michele Ceriotti. Adaptive energy reference for machine-learning models of the electronic density of states. Physical Review Materials, 9(1):013802, January 2025. doi: 10.1103/physrevmaterials.9.013802.
  52. [52]Christopher K. H. Borg, Eric S. Muckley, Clara Nyby, James E. Saal, Logan Ward, Apurva Mehta, and Bryce Meredig. Quantifying the performance of machine learning models in materials discovery. Digital Discovery, 2(2):327–338, 2023. doi: 10.1039/d2dd00113f.DOI
  53. [53]Christopher J. Bartel, Amalie Trewartha, Qi Wang, Alexander Dunn, Anubhav Jain, and Gerbrand Ceder. A critical examination of compound stability predictions from machine-learned formation energies. npj Computational Materials, 6(1):97, July 2020. doi: 10.1038/s41524-020-00362-y.DOI
  54. [54]Janosh Riebesell, Rhys E. A. Goodall, Philipp B. Nemecek, Yuan Chiang, Bowen Deng, Gerbrand Ceder, Mark Asta, Alpha A. Lee, Anubhav Jain, and Kristin A. Persson. A framework to evaluate machine learning crystal stability predictions. Nature Machine Intelligence, 7(6):836–847, June 2025. doi: 10.1038/s42256-025-01055-1.DOI
  55. [55]Bryce Meredig, Erin Antono, Carena Church, Maxwell Hutchinson, Julia Ling, Sean Paradiso, Ben Blaizsik, Ian Foster, Brenna Gibbons, Jason Hattrick-Simpers, Apurva Mehta, and Logan Ward. Can machine learning identify the next high-temperature superconductor? Examining extrapolation performance for materials discovery. Molecular Systems Design & Engineering, 3(5):819–825, 2018. doi: 10.1039/c8me00012c.DOI
  56. [56]Sadman Saeed Ome, Nihan Gu, Rongzhong Dong, Ming Hu, and Jianjun Hu. Structure-based out-of-distribution (OOD) materials property prediction: a benchmark study. npj Computational Materials, 10(1):144, July 2024. doi: 10.1038/s41524-024-01316-4.
  57. [57]Kangming Li, Daniel Persaud, Kamal Choudhary, Brian DeCost, Michael Greenwood, and Jason Hattrick-Simpers. Exploiting redundancy in large materials datasets for efficient machine learning with less data. Nature Communications, 14(1):7283, November 2023. doi: 10.1038/s41467-023-42992-y.DOI
  58. [58]Sayash Kapoor and Arvind Narayanan. Leakage and the reproducibility crisis in machine-learning-based science. Patterns, 4(9):100804, September 2023. doi: 10.1016/j.patter.2023.100804.DOI
  59. [59]Inbal Magar and Roy Schwartz. Data Contamination: From Memorization to Exploitation. In Proceedings of the 60th Annual Meeting of the Association for Computational Linguistics (Volume 2: Short Papers), pages 157–165. Association for Computational Linguistics, 2022. doi: 10.18653/v1/2022.acl-short.18.DOI
  60. [60]James E. Saal, Scott Kirklin, Muratahan Aykol, Bryce Meredig, and C. Wolverton. Materials Design and Discovery with High-Throughput Density Functional Theory: The Open Quantum Materials Database (OQMD). JOM, 65(11):1501–1509, September 2013. doi: 10.1007/s11837-013-0755-4.DOI
  61. [61]Scott Kirklin, James E Saal, Bryce Meredig, Alex Thompson, Jeff W Doak, Muratahan Aykol, Stephan Rühl, and Chris Wolverton. The Open Quantum Materials Database (OQMD): assessing the accuracy of DFT formation energies. npj Computational Materials, 1(1):15010, December 2015. doi: 10.1038/npjcompumats.2015.10.DOI
  62. [62]Shyue Ping Ong, William Davidson Richards, Anubhav Jain, Geoffroy Hautier, Michael Kocher, Shreyas Cholia, Dan Gunter, Vincent L. Chevrier, Kristin A. Persson, and Gerbrand Ceder. Python Materials Genomics (pymatgen): A robust, open-source python library for materials analysis. Computational Materials Science, 68:314–319, February 2013. doi: 10.1016/j.commatsci.2012.10.028.DOI
  63. [64]Pavel Izmailov, Dmitrii Podoprikhin, Timur Garipov, Dmitry Vetrov, and Andrew Gordon Wilson. Averaging Weights Leads to Wider Optima and Better Generalization. In Proceedings of the 34th Conference on Uncertainty in Artificial Intelligence (UAI), 2018. arXiv:1803.05407.arxiv.org/abs/1803.05407
  64. [65]G. D. Mahan and J. O. Sofo. The best thermoelectric. Proceedings of the National Academy of Sciences, 93(15):7436–7439, July 1996. doi: 10.1073/pnas.93.15.7436.DOI
  65. [66]Paolo Giannozzi, Stefano Baroni, Nicola Bonini, Matteo Calandra, Roberto Car, Carlo Cavazzoni, Davide Ceresoli, Guido L Chiarotti, Matteo Cococcioni, Ismaila Dabo, Andrea Dal Corso, Stefano de Gironcoli, Stefano Fabris, Guido Fratesi, Ralph Gebauer, Uwe Gerstmann, Christos Gougoussis, Anton Kokalj, Michele Lazzeri, Layla Martin-Samos, Nicola Marzari, Francesco Mauri, Riccardo Mazzarello, Stefano Paolini, Alfredo Pasquarello, Lorenzo Paulatto, Carlo Sbraccia, Sandro Scandolo, Gabriele Sclauzero, Ari P Seitonen, Alexander Smogunov, Paolo Umari, and Renata M Wentzcovitch. QUANTUM ESPRESSO: a modular and open-source software project for quantum simulations of materials. Journal of Physics: Condensed Matter, 21(39):395502, September 2009. doi: 10.1088/0953-8984/21/39/395502.DOI
  66. [67]P Giannozzi, O Andreussi, T Brumme, O Bunau, M Buongiorno Nardelli, M Calandra, R Car, C Cavazzoni, D Ceresoli, M Cococcioni, N Colonna, I Carnimeo, A Dal Corso, S de Gironcoli, P Delugas, R A DiStasio, A Ferretti, A Floris, G Fratesi, G Fugallo, R Gebauer, U Gerstmann, F Giustino, T Gorni, J Jia, M Kawamura, H-Y Ko, A Kokalj, E Küçükbenli, M Lazzeri, M Marsili, N Marzari, F Mauri, N L Nguyen, H-V Nguyen, A Otero-de-la Roza, L Paulatto, S Poncé, D Rocca, R Sabatini, B Santra, M Schlipf, A P Seitonen, A Smogunov, I Timrov, T Thonhauser, P Umari, N Vast, X Wu, and S Baroni. Advanced capabilities for materials modelling with Quantum ESPRESSO. Journal of Physics: Condensed Matter, 29(46):465901, October 2017. doi: 10.1088/1361-648X/aa8f79.DOI
  67. [68]John P. Perdew, Kieron Burke, and Matthias Ernzerhof. Generalized Gradient Approximation Made Simple. Physical Review Letters, 77(18):3865–3868, October 1996. doi: 10.1103/physrevlett.77.3865.DOI
  68. [69]Gianluca Prandini, Antimo Marrazzo, Ivano E. Castelli, Nicolas Mounet, and Nicola Marzari. Precision and efficiency in solid-state pseudopotential calculations. npj Computational Materials, 4(1):72, December 2018. doi: 10.1038/s41524-018-0127-2.DOI
  69. [70]Nicola Marzari, David Vanderbilt, Alessandro De Vita, and M. C. Payne. Thermal Contraction and Disordering of the Al(110) Surface. Physical Review Letters, 82(16):3296–3299, April 1999. doi: 10.1103/physrevlett.82.3296.DOI
  70. [71]Hendrik J. Monkhorst and James D. Pack. Special points for Brillouin-zone integrations. Physical Review B, 13(12):5188–5192, June 1976. doi: 10.1103/physrevb.13.5188.DOI
  71. [72]Andrea Dal Corso. Pseudopotentials periodic table: From H to Pu. Computational Materials Science, 95:337–350, December 2014. doi: 10.1016/j.commatsci.2014.07.043.DOI
  72. [73]San-Dong Guo. Thermoelectric properties of half-Heusler ZrNiPb by using first principles calculations. RSC Advances, 6(53):47953–47958, 2016. doi: 10.1039/c6ra08461c.DOI
  73. [74]Wenhao Sun, Stephen T. Dacek, Shyue Ping Ong, Geoffroy Hautier, Anubhav Jain, William D. Richards, Anthony C. Gamst, Kristian A. Persson, and Gerbrand Ceder. The thermodynamic scale of inorganic crystalline metastability. Science Advances, 2(11):e1600225, November 2016. ISSN 2375-2548. doi: 10.1126/sciadv.1600225.DOI
  74. [75]Muratahan Aykol, Shyam S. Dwaraknath, Wenhao Sun, and Kristin A. Persson. Thermodynamic limit for synthesis of metastable inorganic materials. Science Advances, 4(4):eaaoq0148, 2018. doi: 10.1126/sciadv.aaoq0148.DOI
  75. [76]Wolfgang G. Zeier, Jennifer Schmitt, Geoffroy Hautier, Umut Aydenmir, Zachary M. Gibbs, Claudia Felser, and G. Jeffrey Snyder. Engineering half-Heusler thermoelectric materials using Zintl chemistry. Nature Reviews Materials, 1(6):16032, May 2016. doi: 10.1038/natrevmats.2016.32.DOI
  76. [77]J Oestreich, U Probst, F Richardt, and E Bucher. Thermoelectrical properties of the compounds ScM^IIISb and YM^IIISb (M^III = Ni, Pd, Pt). Journal of Physics: Condensed Matter, 15(4):635–640, 2003. doi: 10.1088/0953-8984/15/4/304.
  77. [78]Shanming Li, Huaizhou Zhao, Dandan Li, Shifeng Jin, and Lin Gu. Synthesis and thermoelectric properties of half-Heusler alloy YNiBi. Journal of Applied Physics, 117(20):205101, 2015. doi: 10.1063/1.4921811.DOI
  78. [79]Shan Li, Hangtian Zhu, Jun Mao, Zhenzhen Feng, Xiaofang Li, Chen Chen, Feng Cao, Xingjun Liu, David J. Singh, Zhifeng Ren, and Qian Zhang. n-Type TaCoSn-Based Half-Heuslers as Promising Thermoelectric Materials. ACS Applied Materials & Interfaces, 11(44):41321–41329, October 2019. ISSN 1944-8252. doi: 10.1021/acsami.9b13603.
  79. [80]Heinrich Hohl, Art P Ramirez, Claudia Goldmann, Gabriele Ernst, Bernd Wölfling, and Ernst Bucher. New compounds with MgAgAs-type structure: NbIrSn and NbIrSb. Journal of Physics: Condensed Matter, 10(35):7843–7850, 1998. doi: 10.1088/0953-8984/10/35/016.DOI
  80. [81]Jesús Carrete, Wu Li, Natalio Mingo, Shidong Wang, and Stefano Curtarolo. Finding Unprecedentedly Low-Thermal-Conductivity Half-Heusler Semiconductors via High-Throughput Materials Modeling. Physical Review X, 4(1):011019, February 2014. doi: 10.1103/physrevx.4.011019.DOI
  81. [82]Angela Pak, Kamil Ciesielski, Maria Wróblewska, Eric S. Toberer, and Elif Ertekin. Mapping the configuration space of half-Heusler compounds via subspace identification for thermoelectric materials discovery. Journal of Materials Chemistry A, 13(25):19455–19470, 2025. doi: 10.1039/d5ta00397k.
  82. [83]H. Kleinke and H. F. Franzen. Crystal Structures, Bonding and Electronic Structures of MM′As, a Series of New Ternary Arsenides (M = Zr, Hf; M′ = Fe, Co, Ni). Zeitschrift für anorganische und allgemeine Chemie, 624(1):51–56, 1998. doi: 10.1002/(sici)1521-3749(199801)624:1<51::aid-zaac51>3.0.co;2-q.doi.org/10.1002/(sici)1521-3749(199801)624:1<51::aid-zaac51>3.0.co;2-q
  83. [84]Tim Dinges, Matthias Eul, and Rainer Pöttgen. TaRhGe with TiNiSi-type Structure. Zeitschrift für Naturforschung B, 65(1):95–98, 2010. doi: 10.1515/znb-2010-0117.DOI
  84. [85]Romain Gautier, Xiuwen Zhang, Linhua Hu, Liping Yu, Yuyuan Lin, Tor O. L. Sunde, Danbee Chon, Kenneth R. Poepplmeier, and Alex Zunger. Prediction and accelerated laboratory discovery of previously unknown 18-electron ABX compounds. Nature Chemistry, 7(4):308–316, 2015. doi: 10.1038/nchem.2207.DOI
  85. [86]Kaja Bilińska and Maciej J. Winiarski. High-Throughput Exploration of Half-Heusler Phases for Thermoelectric Applications. Crystals, 13(9):1378, 2023. doi: 10.3390/cryst13091378.DOI
  86. [87]Christopher J. Bartel. Review of computational approaches to predict the thermodynamic stability of inorganic solids. Journal of Materials Science, 57(23):10475–10498, 2022. doi: 10.1007/s10853-022-06915-4.DOI
  87. [88]John P. Perdew and Mel Levy. Physical Content of the Exact Kohn-Sham Orbital Energies: Band Gaps and Derivative Discontinuities. Physical Review Letters, 51(20):1884–1887, November 1983. doi: 10.1103/physrevlett.51.1884.DOI
  88. [89]Pedro Borlido, Thorsten Aull, Ahmad W. Huran, Fabien Tran, Miguel A. L. Marques, and Silvana Botti. Large-Scale Benchmark of Exchange–Correlation Functionals for the Determination of Electronic Band Gaps of Solids. Journal of Chemical Theory and Computation, 15(9):5069–5079, July 2019. ISSN 1549-9626. doi: 10.1021/acs.jctc.9b00322.DOI
  89. [90]Patrizio Graziosi, Chathurangi Kumarasinghe, and Neophytos Neophytou. Material Descriptors for the Discovery of Efficient Thermoelectrics. ACS Applied Energy Materials, 3(6):5913–5926, May 2020. doi: 10.1021/acsaem.0c00825.DOI
  90. [91]Jiawei Zhou, Hangtian Zhu, Te-Huan Liu, Qichen Song, Ran He, Jun Mao, Zihang Liu, Wuyang Ren, Bolin Liao, David J. Singh, Zhifeng Ren, and Gang Chen. Large thermoelectric power factor from crystal symmetry-protected non-bonding orbital in half-Heuslers. Nature Communications, 9(1):1721, April 2018. ISSN 2041-1723. doi: 10.1038/s41467-018-03866-w.DOI
  91. [92]Chathurangi Kumarasinghe and Neophytos Neophytou. Band alignment and scattering considerations for enhancing the thermoelectric power factor of complex materials: The case of Co-based half-Heusler alloys. Physical Review B, 99(19):195202, May 2019. ISSN 2469-9969. doi: 10.1103/physrevb.99.195202.DOI
  92. [93]Alex M. Ganose, Junsoo Park, Alireza Faghaninia, Rachel Woods-Robinson, Kristin A. Persson, and Anubhav Jain. Efficient calculation of carrier scattering rates from first principles. Nature Communications, 12(1):2222, April 2021. doi: 10.1038/s41467-021-22440-5.DOI
  93. [94]Lili Xi, Shanshan Pan, Xin Li, Yonglin Xu, Jianye Ni, Xin Sun, Jiong Yang, Jun Luo, Jinyang Xi, Wenhao Zhu, Xinran Li, Di Jiang, Richard Dronkowski, Xun Shi, G. Jeffrey Snyder, and Wenqing Zhang. Discovery of High-Performance Thermoelectric Chalcogenides through Reliable High-Throughput Material Screening. Journal of the American Chemical Society, 140(34):10785–10793, 2018. doi: 10.1021/jacs.8b04704.DOI
  94. [95]Junsoo Park, Maxwell Dylla, Yi Xia, Max Wood, G. Jeffrey Snyder, and Anubhav Jain. When band convergence is not beneficial for thermoelectrics. Nature Communications, 12(1):3425, June 2021. doi: 10.1038/s41467-021-23839-w.DOI
  95. [96]Eric S. Toberer, Andrew F. May, Cidney J. Scanlon, and G. Jeffrey Snyder. Thermoelectric properties of p-type LiZnSb: Assessment of ab initio calculations. Journal of Applied Physics, 105(6):063701, 2009. doi: 10.1063/1.3091267.DOI

Paper details

vlnc:W_d7sj963e
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 12

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents