First principle study of structural, elastic, electronic and optical properties of Pb0.5Sn0.5TiO3 and Pb0.5Sn0.5Ti0.5(Zr0.5)O3

Abstract

The structural, electronic, elastic and optical properties of tetragonal (P4mm) phase of Pb0.5Sn0.5TiO3 (PSTO) and Pb0.5Sn0.5Ti0.5(Zr0.5)O3 (PSTZO) are examined by first-principles calculations based on the density functional theory (DFT) using the pseudo-potential plane wave (PP-PW) scheme in the frame of generalized gradient approximation (GGA). We have calculated the ground state properties such as equlibrium lattice constants, volume, bulk modulus and its pressure derivative. From elastic constants, mechanical parameters such as anisotropy factor, elastic modulus and Poisson's ratio are obtained from the Voigt-Reuss-Hill average approximation. Rather than their averages, the directional dependence of elastic modulus, and Poisson's ratio are modelled and visualized in the light of the elastic properties of both systems. In addition, some novel results, such as Debye temperatures, and sound velocities are obtained. Moreover, we have presented the results of the electronic band structure, densities of states and charge densities. These results were in favourable agreement with the existing theoretical data. The optical dielectric function and energy loss spectrum of both systems are also computed. Born effective charge (BEC) of each atoms for both systems is computed from functional perturbation theory (DFPT). Finally, the spontaneous polarization is also determined from modern theory of polarization to be 0.8662 C/m2 (PSTO) and 1.0824 C/m2 (PSTZO).

Introduction

Perovskite (ABO3\mathrm{ABO}_{3}) has held the interest of crystallography for a significant period of time due to the wide range of compositions and the existence of unique properties such as ferroelectricity. The development of perovskite type materials exhibiting a very high dielectric constant and spontaneous polarization is of considerable interest since they play an important role in electronics /microelectronics and have various technological applications [1, 2, 3, 4, 5, 6]. Most of the ferroelectric materials used for device applications are Pb-based such as lead titanate (PbTiO3\mathrm{PbTiO}_{3}), lead zirconate titanate Pb(ZrxTi1−x)O3\mathrm{Pb}(\mathrm{Zr}_{x}\mathrm{Ti}_{1-x})\mathrm{O}_{3} (PZT) (xx = composition), lead lanthanum zirconate titanate (Pb1−xLax)(ZryTi1−y)1−x/4O3(\mathrm{Pb}_{1-x}\mathrm{La}_{x})(\mathrm{Zr}_{y}\mathrm{Ti}_{1-y})_{1-x/4}\mathrm{O}_{3} (PLZT) and lead magnesium niobate Pb(Mg,Nb)O3\mathrm{Pb}(\mathrm{Mg},\mathrm{Nb})\mathrm{O}_{3} (PMN) [7, 8, 9, 10]. Nowadays, there is observed environmental as well as health concern regarding the toxicity of lead based oxides which are volatile during processing. The volatilization of toxic lead oxide during high-temperature sintering not only causes environmental pollution but also generates instability in composition and affects the electrical properties of the products. Moreover, the products containing Pb-based gadgets are not recyclable [11]. An increased environmental awareness over the past 20 years has resulted in several governmental regulations world-wide that are putting increasingly stringent requirements on the use of materials in electronic devices [12, 13]. Consequently, this has opened the searches on identifying new and more environmentally friendly ferroelectric materials and other alternative compounds as well as on seeking novel Pb-free ferroelectric materials with cation displacements of comparable (or greater) magnitude for their application in the future sustainable electroactive

This work is licensed under a Creative Commons Attribution 4.0 International License. Further distribution of this work must maintain attribution to the author(s) and the published article’s title, journal citation, and DOI. materials [14, 15, 16]. The total replacement of Pb-based materials in technological devices remains almost improbable because of the unsatisfactory performance of other materials. However, modification efforts to reduce the consumption of toxic Pb2+\mathrm{Pb}^{2+}, such as by substitution or doping techniques, remain necessary. As reported by Taib et al. [14] in order to decrease the harm of Pb2+\mathrm{Pb}^{2+} element, the potential elements such as Sn2+\mathrm{Sn}^{2+} and Ge2+\mathrm{Ge}^{2+} are eventually expected to be more environmental friendly materials. Cohen and Ganesh [17] reported that a novel compound of Pb0.5Sn0.5ZrTiO3\mathrm{Pb}_{0.5}\mathrm{Sn}_{0.5}\mathrm{ZrTiO}_{3} (PSZT) has much higher values of piezoelectric coefficients than PZT. Roy and Vanderbilt [18] also explained that strong ferroelectric properties could exist in double rock-salts PbSnZrTiO6\mathrm{PbSnZrTiO}_{6}. By substitution reducing the concentration of Pb2+\mathrm{Pb}^{2+} we mainly focus on the investigation of structural, elastic, electronic, spontaneous polarization and optical properties of PSTO and PSTZO compounds. The paper is organized as follows. In section 2, the techniques for the calculations are described, and the computational details are presented. In section 3, the present results of the structural, electronic, elastic, and optical properties for both systems are discussed and compared with the available previous results. Finally, the conclusion of the present work is drawn in the last section.

Computational details

The first principles calculations were conducted using the density functional theory (DFT) as implemented in Quantum Espresso software Package (QE) [19] open source code within General Gradient Approximation (GGA) functional [20]. The atomic crystal structures of supercell 1×1×21 \times1 \times2 of PSTO and PSTZO were designed in tetragonal (P4mm, 99 space group) phase for the composition of Ti/Zr 50/50 and Pb/Sn 50/50 as illustrated in Figure 1. The direct substitutive point defect techniques were used to replace Pb by Sn and Ti by Zr atom. The ultra-soft pseudopotentials [21] were used to treat the interaction of the electrons with the ion cores, where Pb (6s, 6p), Sn (5s, 5p), Ti (4p, 3d), Zr (4d, 5s) and O (2s, 2p) electrons were treated as valence states. A plane-wave cut-off energy of 80 Ry and the Brillouin zone with 4×4×44 \times4 \times4 Monkhorst Pack [22] k-point were applied. Geometric optimization was performed under the convergence criteria: energy 1.0⋅10−41.0 \cdot10^{-4}, force 1.0⋅10−31.0 \cdot10^{-3} Ry/Bohr, cell 5.0⋅10−15.0 \cdot10^{-1} kbar. Density functional perturbation theory (DFPT) [23] was used to calculate the Born effective charge (BEC) of the systems. In addition, the spontaneous polarization was computed using the Berry-phase approach [24]. Using this approach, the total polarization PP for a given crystalline geometry can be calculated as the sum of ionic and electronic contributions.

Figure 1. (Colour online) The crystal structure of a) PSTO and b) PSTZO.

Result and discussions

Structure properties

The equilibrium lattice constant is a fundamental part of the structural information related to crystal structures. To calculate the theoretical lattice constant, the cutoff energy and k-point sampling obtained from total energy convergence test are employed. In our computations, the lattice constant was varied

with 0.1 Bohr radius increments. From Figure 2, the optimized equilibrium lattice constant of PSTO is a=3.978a = 3.978 Å and c=8.353c = 8.353 Å and also the optimized equilibrium lattice constant of PSTZO is a=4.025a = 4.025 Å and c=8.610c = 8.610 Å, which are in better agreement with the previous theoretical facts [24, 25, 26]. The computed lattice constants and its atomic positions are significant factors of the material stability.

Figure 2. (Colour online) The energy with respect to lattice constant of a) PSTO and b) PSTZO.

Moreover, equation of state (EOS) is a pressure-volume (PVPV) or energy-volume (EVEV) relation describing the behavior of a solid under compression or expansion. The relationship between PVPV and EVEV curve is shown in Figure 3. A series of total energy calculations as a function of volume can be fitted to an equation of state according to Murnaghan E(V)E(V) curve [27].

Figure 3. (Colour online) The total energy and pressure with respect to volume.

E(V)=Eo+V{BB′[(VoV)B′B′−1+1]−BVoB′−1}(1)E(V) = E_o + V \left\{ \frac{B}{B'} \left[ \left(\frac{V_o}{V}\right)^{\frac{B'}{B'-1}} + 1 \right] - \frac{BV_o}{B'-1} \right\} \tag*{(1)}

where EoE_o, VoV_o, BB, B′B' are parameters of the fit: EoE_o is the minimum energy, VoV_o is the equilibrium cell volume, BB and B′B' are the bulk modulus and its derivative of the material, respectively. The calculated values of lattice constant, bulk modulus, volume, and pressure derivatives of bulk modulus are summarized in Table 1.

SourceLattice constants (Å)VV (Å3^{3})BBB′B'
Pb0.5_{0.5}Sn0.5_{0.5}TiO3_3Our worka=3.978a = 3.978 and c=8.353c = 8.353129.59129.5910.39
Pb0.5_{0.5}Sn0.5_{0.5}Ti0.5_{0.5}(Zr0.5_{0.5})O3_3Our worka=4.025a = 4.025 and c=8.616c = 8.616143.27200.29.70

Table 1. Computed equilibrium lattice constants, volume, bulk modulus and bulk modulus derivatives of compounds in tetragonal phase.

Elastic properties

Elastic constants are fundamental and indispensable to describe the mechanical properties of materials. They can be used to determine the elastic moduli, Poisson’s ratio nn, and elastic anisotropy factor of materials. Elastic properties are also closely associated with many fundamental solid-state properties, such as acoustic velocity, thermal conductivity, Debye temperature, inter-atomic potentials, and so on. When a crystal is subjected to an external loading (with the stress state described by a stress tensor σij\sigma_{ij}), its shape and dimensions are changed. The change of a crystal geometry can be described using the strain tensor (εkl\varepsilon_{kl}). The relation between these two tensors (within the linear elastic limit) can be expressed by means of the generalized form of Hooke’s law [28].

Cijkl=(∂σij∂εkl)x=(1V∂2E∂εij∂εkl)x(2)C_{ijkl} = \left(\frac{\partial\sigma_{ij}}{\partial\varepsilon_{kl}}\right)_{x} = \left(\frac{1}{V}\frac{\partial^{2} E}{\partial\varepsilon_{ij}\partial\varepsilon_{kl}}\right)_{x} \tag*{(2)}

The nonzero components of the elastic constant tensor for each crystal point group can be derived using the group theory [29]. The form of the elastic constants tensor depends on the Laue class obtained by adding an inversion center to the group operations. The Laue classes are eleven geometric crystal classes containing centrosymmetric crystallographic types of point groups and their subgroups [29]. Specifically, for tetragonal system the Laue class D4h (4/mmm) is used and there are also six independent elastic constants C11C_{11}, C12C_{12}, C13C_{13}, C33C_{33}, C44C_{44} and C66C_{66} which should satisfy the Born stability criteria [30].

C11−C12>0,C11+C33−2C13>0,C11>0,C33>0,C44>0,C66>0,2C11+C33+2C12+4C13>0\begin{aligned} C_{11}-C_{12} &> 0,\qquad C_{11}+C_{33}-2C_{13}>0,\qquad C_{11}>0,\\ C_{33} &> 0,\qquad C_{44}>0,\qquad C_{66}>0,\\ 2C_{11}+C_{33}+2C_{12}+4C_{13} &> 0 \end{aligned}

and

13(C12+2C13)<B<13(C11+2C33).(3)\frac{1}{3}(C_{12}+2C_{13}) < B < \frac{1}{3}(C_{11}+2C_{33}). \tag*{(3)}

We have calculated the six independent elastic constants of PSTO and PSTZO using stress-strain relation. At zero pressures, the calculated elastic constants of PSTO (C11=260.12C_{11}=260.12 GPa, C12=108.7C_{12}=108.7 GPa, C13=111.30C_{13}=111.30 GPa, C33=158.1C_{33}=158.1 GPa, C44=87.61C_{44}=87.61 GPa, and C66=94.1C_{66}=94.1 GPa). Similarly, the elastic constants of PSTZO (C11=252.49C_{11}=252.49 GPa, C12=96.37C_{12}=96.37 GPa, C13=102.23C_{13}=102.23 GPa, C33=147.24C_{33}=147.24 GPa, C44=73.82C_{44}=73.82 GPa, and C66=79.11C_{66}=79.11 GPa). The computed elastic constants satisfy the mechanical stability conditions, and which are in reasonable agreement with those obtained by Marton and Elsasser [31]. Moreover, the elastic modulus was calculated using the Voigt-Reuss-Hill approximation [32]. For a tetragonal system, Voigt bulk modulus (BVB_{\mathrm{V}}) and shear modulus (GVG_{\mathrm{V}}) are:

BV=19[(C11+C22+C33)+2(C12+C23+C31)],B_{\mathrm{V}}=\frac{1}{9}[(C_{11}+C_{22}+C_{33})+2(C_{12}+C_{23}+C_{31})],

Figure 4. (Colour online) Directional dependence of a) EE, b) GG and c) nn of PSTZO.

GV=115[(C11+C22+C33)−(C12+C23+C31)+3(C44+C55+C66)](4)G_{\mathrm{V}} = \frac{1}{15}\left[(C_{11}+C_{22}+C_{33})-(C_{12}+C_{23}+C_{31})+3(C_{44}+C_{55}+C_{66})\right] \tag*{(4)}

and the Reuss bulk modulus (BRB_{\mathrm{R}}) and shear modulus (GRG_{\mathrm{R}}) are expressed as

BR=[(S11+S22+S33)+2(S12+S23+S31)]−1,B_{\mathrm{R}}=\left[(S_{11}+S_{22}+S_{33})+2(S_{12}+S_{23}+S_{31})\right]^{-1},
GR=15[4(S11+S22+S33)−(S12+S13+S23)+3(S44+S55+S66)]−1(5)G_{\mathrm{R}}=15\left[4(S_{11}+S_{22}+S_{33})-(S_{12}+S_{13}+S_{23})+3(S_{44}+S_{55}+S_{66})\right]^{-1} \tag*{(5)}

the Hill’s average for the shear modulus (GG) and bulk modulus (BB) is given by

G=12(GV+GR),B=12(BV+BR)(6)G=\frac{1}{2}(G_{\mathrm{V}}+G_{\mathrm{R}}), \qquad B=\frac{1}{2}(B_{\mathrm{V}}+B_{\mathrm{R}}) \tag*{(6)}

while Young’s modulus (EE) and Poisson’s ratio (nn) are given by

E=9BG3B+G,n=3B−2G2(3B+G).(7)E=\frac{9BG}{3B+G}, \qquad n=\frac{3B-2G}{2(3B+G)}. \tag*{(7)}

The calculated bulk, shear, and Young’s modulus of PSTO at zero pressure are 144.12, 72.45, and 186.15 GPa, respectively, which are in better agreement with the corresponding theoretical data [31]. The obtained BB, GG, and EE of PSTZO are 134.34, 65.311, and 168.60 GPa, respectively, which are comparable with the theoretical values [31]. From the results obtained, PSTO is stiffer than PSTZO. The B/GB/G ratio allows us to assess the ductility/brittleness of materials. According to Pugh [33], 1.75 is the critical value that separates the brittleness and ductility behaviors of materials. When the ratio of B/GB/G is of a value higher than the critical one, then the material is associated with ductility. However, when the ratio of B/GB/G value is lower than the critical value, the material is considered to be brittle. Both PSTO (B/G=1.989B/G = 1.989) and PSTZO (B/G=2.056B/G = 2.056) compounds are categorized as ductile because the value of B/GB/G are higher than the critical value. The Poisson’s ratio (nn) is a mechanical parameter which provides useful information on the characteristic of the bonding forces. In the evaluation of Poisson’s ratio, 0.25 and 0.5 are the lower and upper limits of the central force, respectively [34]. The Poisson’s ratio of 0.284 and 0.290 values are obtained for PSTO and PSTZO at zero pressure, respectively. This indicates that the inter-atomic forces are central.

Figure 5. (Colour online) Directional dependence of a) EE, b) GG and c) nn of PSTO.

The universal anisotropic index (AUA^{U}) is a measure to quantify the elastic anisotropic characteristics based on the contributions of both bulk and sheared modulus [35]:

AU=5GVGR+BVBR−6,(8)A^{U} = \frac{5G_{V}}{G_{R}} + \frac{B_{V}}{B_{R}} - 6, \tag*{(8)}

where, GVG_{V} and BVB_{V} are sheared and bulk modulus obtained from Voigt approximation, respectively. Similarly, GRG_{R} and BRB_{R} are sheared and bulk modulus acquired from Reuss approximation. As it is described in the equation (8), when the universal anisotropic index (AUA^{U}) is equal to zero, the crystal is isotropic. The variation from zero defines the level of elastic anisotropy. Therefore, the obtained universal anisotropic index at zero pressure (AUA^{U}) is 0.56 for PSTO and 0.70 for PSTZO.

For anisotropic materials, there is a real need to analyze and visualize the directional elastic properties such as Young’s modulus, shear modulus and Poisson’s ratio rather than their averages. Detailed tensorial analyses are also necessary to find materials with targeted or anomalous mechanical properties. We have calculated the orientation dependence of Young’s modulus EE, shear modulus GG, and Poisson’s ratio nn of both materials as depicted in figure 4 and 5. As a result, the maximum and minimum values of EE, GG, and nn ratio along the normal direction of 111 and 100 planes are summarized in table 2.

Young’s modulus (EE)shear modulus (GG)Poisson ratio (nn)
Emax⁡E_{\max}Emin⁡E_{\min}Gmax⁡G_{\max}Gmin⁡G_{\min}nmax⁡n_{\max}nmin⁡n_{\min}
Pb0.5Sn0.5TiO3\mathrm{Pb}_{0.5}\mathrm{Sn}_{0.5}\mathrm{TiO}_{3}227.2690.9294.1142.920.660.06
Pb0.5Sn0.5Ti0.5(Zr0.5)O3\mathrm{Pb}_{0.5}\mathrm{Sn}_{0.5}\mathrm{Ti}_{0.5}(\mathrm{Zr}_{0.5})\mathrm{O}_{3}195.3487.3279.1142.040.600.13

Table 2. Variations of the Young’s modulus (EE), shear modulus (GG) and Poisson ratio (nn).

vlv_lvtv_tvmv_mθD\theta_D
Pb0.5Sn0.5TiO3\mathrm{Pb}_{0.5}\mathrm{Sn}_{0.5}\mathrm{TiO}_{3}6159.2264765.5843734.693466.451
Pb0.5Sn0.5Ti0.5(Zr0.5)O3\mathrm{Pb}_{0.5}\mathrm{Sn}_{0.5}\mathrm{Ti}_{0.5}(\mathrm{Zr}_{0.5})\mathrm{O}_{3}5624.2794380.9023381.050432.861

Table 3. The calculated longitudinal, transverse, average sound velocity (vlv_l, vtv_t and vmv_m in m/s) and Debye temperatures (θD\theta_D in K).

As a fundamental parameter, the Debye temperature θD\theta_D correlates with many physical properties of solids, such as specific heat, elastic constant and melting temperature. One of the standard methods to calculate the Debye temperature can be estimated from the averaged sound velocity vmv_m is given by

θD=hk[3nπ(NAρM)]13vm(9)\theta_D = \frac{h}{k}\left[\frac{3n}{\pi}\left(\frac{N_A\rho}{M}\right)\right]^{\frac{1}{3}}v_m \tag*{(9)}

where hh is the Planck’s constant, kk is the Boltzmann’s constant, NAN_A is the Avogadro’s number and vmv_m is the average sound velocity.

vm=[13(2vt3+1vl3)]−13(10)v_m = \left[\frac{1}{3}\left(\frac{2}{v_t^3}+\frac{1}{v_l^3}\right)\right]^{-\frac{1}{3}} \tag*{(10)}

where, vlv_l and vtv_t are the longitudinal and transverse elastic sound velocities of the material that are determined by bulk modulus and shear modulus [36, 37].

vl=(B+43Gρ)12(11)v_l = \left(\frac{B+\frac{4}{3}G}{\rho}\right)^{\frac{1}{2}} \tag*{(11)}
vt=(Gρ)12(12)v_t = \left(\frac{G}{\rho}\right)^{\frac{1}{2}} \tag*{(12)}

Based on the calculated elastic properties, the result of sound velocities and Debye temperatures are listed in table 3 accordingly. It can be pointed out that the calculated Debye temperature of PSTO is 466.451 K and PSTZO is 432.861 K.

Electronic properties

Electronic band structures are a representation of the allowed electronic energy levels of solid materials and are used to better inform their electrical properties. From the calculations, the electronic band gap shows that the PSTO and PSTZO give the indirect band gap value of 1.51 eV, and 1.63 eV, respectively. The results obtained are in better agreement with the previous theoretical results [25]. The computed electronic band structure of the compounds is shown in Figure 6 (a and b). Further explanation of the nature of the electronic band gap of ferroelectric compounds is carried out through the density of state. In solid-state physics, density of states (DOS) shows the number of states per interval of energy as a function of energy, while the PDOS shows the projection of total DOS onto different angular momentum components. More specifically, from the PDOS, the contribution of specific atomic orbitals to the electronic bands and the interaction between different atomic orbitals is revealed. Total density of states (DOS) and projected density of states (PDOS) of tetragonal, PSTO and PSTZO are shown in Figure 7 and 8. The distribution of total density of states and partial density of states is plotted in the range of −20.0 to 12.0 eV. The highest valence band of the compounds is mainly dominated by electron O 2pp, Sn 5ss and Pb 6ss orbitals. While the lowest conduction band mainly originates from the Ti 3dd, Zr 4dd, and Sn 5pp states. Thus, it can be inferred that both are a good ferroelectric material due to special hybridization between special lone pair Pb 6ss and O 2pp at valence band.

Figure 6. (Colour online) Electronic band structure of a) PSTO , and b) PSTZO.

Figure 7. (Colour online) Total density of states (TDOS) of (a) PSTO, and b) PSTZO.

Born effective charges and spontaneous polarization

Born effective charges

The polarization induced by atomic displacements, given by the Born effective charges Z∗Z^* [38], plays a key role in understanding both the polar ground state and the lattice dynamics. The Born effective charges are

Ziαβ∗=Ωe∂Pα∂uiβ,(13)Z^{*}_{i\alpha\beta} = \frac{\Omega}{e}\frac{\partial P_{\alpha}}{\partial u_{i\beta}}, \tag*{(13)}

where α\alpha and β\beta denote directions. PP is the component of the polarization in the αth\alpha^{th} direction and uiβu_{i\beta} is the periodic displacement of the ithi^{th} atom in the βth\beta^{th} direction. Ω\Omega is the volume and ee is the electron charge. Born effective charge (BEC or, Z∗Z^*), also known as transverse or dynamic effective charge, is a fundamental quantity that manifests coupling between lattice displacements and electrostatic fields [38]. BEC is important in terms of theoretical study of ferroelectrics since the ferroelectric transition takes place from the competition of long-range coulomb interactions and short-range forces.

In the present work, we have evaluated the BEC tensors of each ion in tetragonal phase of PSTO and PSTZO in the framework of density functional perturbation theory (DFPT). As presented in Table 4 and Table 5, the Born effective dynamical charge of each compounds atom is larger than the nominal ionic charge. The calculated BECs are in agreement with the former results [39]. The large values of BEC of each atom compared to the nominal ionic charge show the importance of the ions as the driving force of the ferroelectric distortion.

Pb0.5_{0.5}Sn0.5_{0.5}TiO3_3Sn0.5_{0.5}Pb0.5_{0.5}Ti0.5_{0.5}(Zr0.5_{0.5})O3_3
ZPb∗Z^{*}_{Pb}Z∗Z^{*}Pb11_{11}3.89705ZPb∗Z^{*}_{Pb}Z∗Z^{*}Pb11_{11}3.91831
Z∗Z^{*}Pb22_{22}3.89705Z∗Z^{*}Pb22_{22}3.91831
Z∗Z^{*}Pb33_{33}3.79810Z∗Z^{*}Pb33_{33}2.41891
ZSn∗Z^{*}_{Sn}Z∗Z^{*}Sn11_{11}4.29538ZSn∗Z^{*}_{Sn}Z∗Z^{*}Sn11_{11}4.17773
Z∗Z^{*}Sn22_{22}4.29538Z∗Z^{*}Sn22_{22}4.17773
Z∗Z^{*}Sn33_{33}3.88430Z∗Z^{*}Sn33_{33}2.15989
ZTi∗Z^{*}_{Ti}Z∗Z^{*}Ti11_{11}6.98907ZTi∗Z^{*}_{Ti}Z∗Z^{*}Ti11_{11}5.47072
Z∗Z^{*}Ti22_{22}6.98907Z∗Z^{*}Ti22_{22}5.47072
Z∗Z^{*}Ti33_{33}6.00741Z∗Z^{*}Ti33_{33}5.26044
ZZr∗Z^{*}_{Zr}Z∗Z^{*}Zr11_{11}5.10754
Z∗Z^{*}Zr22_{22}5.10754
Z∗Z^{*}Zr33_{33}6.58694

Table 4. BEC tensor of Pb, Sn, Zr and Ti of Pb0.5_{0.5}Sn0.5_{0.5}TiO3_3 and Sn0.5_{0.5}Pb0.5_{0.5}Ti0.5_{0.5}(Zr0.5_{0.5})O3_3 in ferroelectric phase.

O1_1O2_2O3_3
Pb0.5_{0.5}Sn0.5_{0.5}TiO3_3−2.7600-2.76\quad0\quad0 0−2.7600\quad-2.76\quad0 00−4.940\quad0\quad-4.94−5.7400-5.74\quad0\quad0 0−2.4400\quad-2.44\quad0 00−2.510\quad0\quad-2.51−2.4400-2.44\quad0\quad0 0−5.7400\quad-5.74\quad0 00−5.510\quad0\quad-5.51
Sn0.5_{0.5}Pb0.5_{0.5}Ti0.5_{0.5}(Zr0.5_{0.5})O3_3−1.9200-1.92\quad0\quad0 0−1.9200\quad-1.92\quad0 00−4.380\quad0\quad-4.38−4.5100-4.51\quad0\quad0 0−2.8000\quad-2.80\quad0 00−1.810\quad0\quad-1.81−2.8000-2.80\quad0\quad0 0−4.5100\quad-4.51\quad0 00−1.810\quad0\quad-1.81

Table 5. BEC tensor of oxygen Pb0.5_{0.5}Sn0.5_{0.5}TiO3_3 and Sn0.5_{0.5}Pb0.5_{0.5}Ti0.5_{0.5}(Zr0.5_{0.5})O3_3 in ferroelectric phase.

Spontaneous polarization

An accurate quantitative method for computing the polarization to all orders in displacement is the so-called Berry phase (or modern) theory of polarization [24]. The spontaneous polarization (PP) of the compounds is obtained from the sum of both ionic polarization (PionP_{\mathrm{ion}}) and electronic polarization (PelP_{\mathrm{el}})

Pion+Pel=∣e∣Ω∑kZkuk+(−2∣e∣i2π3∫Adk∑n=1M∫0G∥⟨unk|∂∂k∥|unk⟩dk∥)(14)P_{\mathrm{ion}} + P_{\mathrm{el}} = \frac{|e|}{\Omega}\sum_{k} Z_k u_k + \left(-\frac{2|e|i}{2\pi^3}\int_A d\mathbf{k}\sum_{n=1}^{M}\int_{0}^{G_{\parallel}}\left\langle u_{n\mathbf{k}}\middle|\frac{\partial}{\partial k_{\parallel}}\middle|u_{n\mathbf{k}}\right\rangle dk_{\parallel}\right) \tag*{(14)}

Figure 8. (Colour online) Partial density of states (PDOS) of a) PSTO and b) PSTZO.

where in the electronic contribution, the sum nn runs over all MM occupied bands, and where k∥k_{\parallel} is parallel to the direction of polarization, and G∥G_{\parallel} is a reciprocal lattice vector in the same direction. The states unku_{nk} is the lattice-periodical part of the Bloch wave function. The integral over the perpendicular directions can easily be converged with a few k-points. The ionic part of polarization is a well-defined quantity from electromagnetic theory. However, the electronic part of of polarization cannot be directly evaluated on the basis of localized contributions. The calculated spontaneous polarization at the equilibrium lattice constant using Berry’s phase approach was determined to be 0.8662 C/m2^{2} (PSTO) and 1.0824 C/m2^{2} (PSTZO). The computed spontaneous polarization shows a high ferroelectric behavior compared to prototypical ferroelectric perovskites [40, 41].

Optical dielectric functions

The optical properties can be explained in detail through the knowledge of the complex dielectric function ε(ω)=ε1(ω)+iε2(ω)\varepsilon(\omega)=\varepsilon_{1}(\omega)+i\varepsilon_{2}(\omega). The imaginary part of the dielectric function ε2(ω)\varepsilon_{2}(\omega) is calculated by the sum of all possible direct transitions from the occupied to unoccupied states over the Brillouin zone [42].

ε2(ω)=2πe2Ωε0∑k,v,c∣⟨ψkc∣u⋅r∣ψkv⟩∣2δ[Ekc−Ekv−E],(15)\varepsilon_{2}(\omega)=\frac{2\pi e^{2}}{\Omega\varepsilon_{0}}\sum_{k,v,c}\left|\langle\psi^{c}_{k}|\mathbf{u}\cdot\mathbf{r}|\psi^{v}_{k}\rangle\right|^{2}\delta[E^{c}_{k}-E^{v}_{k}-E], \tag*{(15)}

where ee refers to electron charge, and ψkc\psi^{c}_{k} and ψkv\psi^{v}_{k} are the conduction band (CB) and valence band (VB) wave functions at kk, respectively. The real and imaginary dielectric functions are linked by the

Kramer-Kronig relation, which is used to calculate the real part ε1(ω)\varepsilon_{1}(\omega) of the dielectric function

ε1(ω)=1+2πP∫0∞ω′ε2(ω′)ω′2−ω2 dω′(16)\varepsilon_{1}(\omega)=1+\frac{2}{\pi}P\int_{0}^{\infty}\frac{\omega'\varepsilon_{2}(\omega')}{\omega'^{2}-\omega^{2}}\,\mathrm{d}\omega' \tag*{(16)}

where P is the principal value of the integral, P=lim⁡a→0∫−∞ω−aε(ω′)ω′−ω dω′+lim⁡a→0∫ω+a+∞ε(ω′)ω′−ω dω′P=\lim_{a\to0}\int_{-\infty}^{\omega-a}\frac{\varepsilon(\omega')}{\omega'-\omega}\,\mathrm{d}\omega'+\lim_{a\to0}\int_{\omega+a}^{+\infty}\frac{\varepsilon(\omega')}{\omega'-\omega}\,\mathrm{d}\omega'. As it is shown in Figure 9 (a and b), the real and the imaginary parts of complex dielectric function completely describe the optical properties of a medium for different photon energies. For the real part ε1(ω)\varepsilon_{1}(\omega) of the dielectric function, the highest peak for PSTO it appears around 0.23 Ry (3.13 eV), while for PSTZO it appears at 0.25 Ry (3.40 eV). While, the imaginary part ε2(ω)\varepsilon_{2}(\omega) of the dielectric function illustrates the optical transition mechanism. Each peak in the imaginary part of the dielectric function corresponds to an electronic transition. The major ε2(ω)\varepsilon_{2}(\omega) peaks for PSTO located at 0.37 Ry (5.03 eV), 0.54 Ry (7.34 eV), 1.27 Ry (17.27 eV) and 1.51 Ry (20.54 eV), correspond to the transition from occupied VB O 2p2p, Pb 6s6s, Sn 5s5s and O 2s2s to unoccupied CB Ti 3d3d, Pb 5p5p and Sn 5p5p. For PSTZO, the ε2(ω)\varepsilon_{2}(\omega) peaks 0.28 Ry (3.80 eV), 0.36 Ry (4.89 eV), 0.85 Ry (11.56 eV) and 1.89 Ry (25.71 eV) originate from the transition of O 2p2p, Pb 6s6s, Sn 5s5s and O 2s2s occupied to unoccupied CB Ti 3d3d, Zr 4d4d, Pb 5p5p and Sn 5p5p. In the light of ε1(ω)\varepsilon_{1}(\omega) and ε2(ω)\varepsilon_{2}(\omega), the electron energy-loss function is defined as

Figure 9. Figure 9. (Colour online) Calculated real (ε1(ω)\varepsilon_{1}(\omega)), imaginary (ε2(ω)\varepsilon_{2}(\omega)) dielectric function and energy-loss function L(ω)L(\omega).

L(ω)=−Im⁡(1ε(ω))=ε2(ω)ε12(ω)+ε22(ω)(17)L(\omega)=-\operatorname{Im}\left(\frac{1}{\varepsilon(\omega)}\right)=\frac{\varepsilon_{2}(\omega)}{\varepsilon_{1}^{2}(\omega)+\varepsilon_{2}^{2}(\omega)} \tag*{(17)}

The electron energy loss function L(ω)L(\omega) is another useful tool to investigate the behavior of a material with the light. This property of a medium or a material measures the propagation loss of energy inside the medium or material. As shown in Figure 9 (c and d) the major peak of L(ω)L(\omega) occurs at 1.76 Ry (23.94 eV) for PSTO and at 2.1 Ry (28.57 eV) for PSTZO. The sharp peaks of L(ω)L(\omega) associated with the plasma oscillation and their corresponding frequencies are called plasma frequencies [43].

Conclusions

In summary, the structural, elastic, electronic and optical properties of PSTO and PSTZO were extensively studied using pseudo-potential plane-wave (PPs-PW) approach in the framework of density functional theory. The exchange-correlation potential was calculated within the framework of generalized gradient approximation (GGA). The equilibrium lattice parameter, bulk modulus and its pressure derivative were computed from equation of state (EOS). The obtained structural lattice constant shows a better agreement with the previous theoretical data. From the study of elastic properties, the calculated bulk modulus BB, Young’s modulus EE, shear modulus GG and Poisson’s ratio nn of PSTO are 144.12, 72.45, 186.15 GPa and 0.284, respectively. The obtained BB, GG, EE and nn of PSTZO are also 134.34, 65.311, 168.60 GPa and 0.29, respectively, which are consistent with the previously reported data. The computed B/GB/G ratio implies that both systems are ductile materials. Moreover, regarding the band structure, we found that the PSTO compound has 1.51 eV indirect bandgap, whereas PSTZO is found to be 1.63 eV indirect bandgap. The optical properties such as dielectric constant, and energy loss function were also investigated.

The calculated BEC of atoms of both compounds are larger than the nominal ionic charge, which are in agreement with the former results. The large values of Born effective dynamical charge show the importance of the ions as the driving force of the ferroelectric distortion. Using the Berry phase approach, spontaneous polarization was determined to be 0.8662 C/m2^{2} (PSTO) and 1.0824 C/m2^{2} (PSTZO). The obtained spontaneous polarization of both materials shows a high ferroelectric behavior compared to prototypical ferroelectric materials and they can be the best choice of future ferroelectric materials.

Acknowledgements

The author would like to acknowledge the East African Institute for fundamental Research (EAIFR), ICTP’s partner institute for High Performance Clusters machine support during the computation.

Першопринципні дослідження структурних, пружних, електронних та оптичних властивостей Pb0.5Sn0.5TiO3\mathrm{Pb}_{0.5}\mathrm{Sn}_{0.5}\mathrm{TiO}_{3} і Pb0.5Sn0.5Ti0.5(Zr0.5)O3\mathrm{Pb}_{0.5}\mathrm{Sn}_{0.5}\mathrm{Ti}_{0.5}(\mathrm{Zr}_{0.5})\mathrm{O}_{3}

Ш.Г. Кума; М.М. Волдемаріам

Структурні, електронні, пружні та оптичні властивості тетрагональної (P4mm\mathrm{P4mm}) фази Pb0.5Sn0.5TiO3\mathrm{Pb}_{0.5}\mathrm{Sn}_{0.5}\mathrm{TiO}_{3} (PSTO) та Pb0.5Sn0.5Ti0.5(Zr0.5)O3\mathrm{Pb}_{0.5}\mathrm{Sn}_{0.5}\mathrm{Ti}_{0.5}(\mathrm{Zr}_{0.5})\mathrm{O}_{3} (PSTZO) досліджуються за допомогою першопринципних розрахунків на основі теорії функціоналу густини (DFT) з використанням процедури псевдопотенціальної плоскої хвилі (PP-RPW) в рамках узагальненого градієнтного наближення (GGA). Ми розрахували такі властивості основного стану, як рівноважні сталі гратки, об’єм, об’ємний модуль та похідну від нього по тиску. З пружних констант механічні параметри, такі як коефіцієнт анізотропії, модуль пружності та коефіцієнт Пуассона, отримуються із середнього наближення Фойгта-Ройсса-Хілла. Замість їхніх середніх значень, залежність модуля пружності та коефіцієнта Пуассона за напрямками моделюються та візуалізуються з урахуванням пружних властивостей обох систем. Крім того, отримуються деякі нові результати, такі як температура Дебая та швидкість звуку. Більше того, ми представили результати електронної зонної структури, густини станів та густини заряду. Ці результати добре узгоджуються з існуючими теоретичними даними. Також обчислено оптичну діелектричну функцію та спектр втрат енергії обох систем. Ефективний заряд (BEC) кожного атома для обох систем обчислюється на основі теорії збурення функціоналу густини (DFPT). Нарешті, спонтанна поляризація також визначається із сучасної теорії поляризації: 0,8662 C/м20{,}8662\ \mathrm{C}/\mathrm{м}^{2} (PSTO) та 1,0824 C/м21{,}0824\ \mathrm{C}/\mathrm{м}^{2} (PSTZO).

References

  1. [1]Rodel J., Jo W., Seifert K.T., Anton E.M., Granzow T., Damjanovic D., J. Am. Ceram. Soc., 2009, 92, 1153–1177, doi:10.1111/j.1551-2916.2009.03061.x.DOI
  2. [2]Kittel C., Gress J.M., Lessard A., Einführung in die Festkörperphysik, 1969.
  3. [3]Dove M.T., Am. Mineral., 1997, 82, 213–244, doi:10.2138/am-1997-3-401.DOI
  4. [4]Resta R., Rev. Mod. Phys., 1994, 66, 899, doi:10.1103/RevModPhys.66.899.DOI
  5. [5]Knapp M.C., Woodward P.M., J. Solid State Chem., 2006, 179, 1076–1085, doi:10.1016/j.jssc.2006.01.005.DOI
  6. [6]Jaffe B., Piezoelectric Ceramics, Elsevier, Amsterdam, 2012.
  7. [7]Sani A., Noheda B., Kornev I.A., Bellaiche L., Bouvier P., Kreisel J., Phys. Rev. B, 2004, 69, 020105, doi:10.1103/PhysRevB.69.020105.DOI
  8. [8]Noheda B., Cox D.E., Shirane G., Guo R., Jones B., Cross L.E., Phys. Rev. B, 2000, 63, 014103, doi:10.1103/PhysRevB.63.014103.DOI
  9. [9]Noheda B., Cox D.E., Shirane G., Gao J., Ye Z.G., Phys. Rev. B, 2002, 66, 054104, doi:10.1103/PhysRevB.66.054104.DOI
  10. [10]Wang L., Yuan P., Wang F., Liang E., Sun Q., Guo Z., Jia Y., Bull. Mater. Sci., 2014, 49, 509–513, doi:10.1016/j.materresbull.2013.08.075.DOI
  11. [11]Bell A.J., Deubzer O., MRS Bulletin, 2018, 43, 581–587, doi:10.1557/mrs.2018.154.DOI
  12. [12]Robinson B.H., Sci. Total Environ., 2009, 408, 183–191, doi:10.1016/j.scitotenv.2009.09.044.DOI
  13. [13]Babu B.R., Parande A.K., Basha C.A., Waste Manag. Res., 2007, 25, 307–318, doi:10.1177/0734242X07076941.DOI
  14. [14]Taib M.F.M., Yaakob M.K., Badrudin F.W., Rasiman M.S.A., Kudin T.T., Hassan O.H., Yahya M.Z.A., Integr. Ferroelectr., 2014, 155, 23–32, doi:10.1080/10584587.2014.905105.DOI
  15. [15]Zhao L., Liu Q., Gao J., Zhang S., Li J.F., Adv. Mater., 2017, 29, 1701824, doi:10.1002/adma.201701824.DOI
  16. [16]Coondoo I., Panwar N., Kholkin A., Adv. Dielectr., 2013, 3, 1330002, doi:10.1142/S2010135X13300028.DOI
  17. [17]Cohen R., Ganesh P., Class of Pure Piezoelectric Materials, United State Patent: US 2009/0291324 A1.
  18. [18]Roy A., Vanderbilt D., Phys. Rev. B, 2011, 83, 134116, doi:10.1103/PhysRevB.83.134116.DOI
  19. [19]Giannozzi P., Baroni S., Bonini N., Calandra M., Car R., Cavazzoni C., Ceresoli D., Chiarotti G.L., Cococcioni M., Dabo I., Dal Corso A., J. Phys.: Condens. Matter, 2009, 21, 395502, doi:10.1088/0953-8984/21/39/395502.DOI
  20. [20]Perdew J.P., Burke K., Ernzerhof M., Phys. Rev. Lett., 1996, 77, 3865, doi:10.1103/PhysRevLett.77.3865.DOI
  21. [21]Hasnip P.J., Pickard C.J., Comput. Phys. Commun., 2006, 174, 24–29, doi:10.1016/j.cpc.2005.07.011.DOI
  22. [22]Monkhorst H.J., Pack J.D., Phys., Rev. B, 1976, 13, 5188, doi:10.1103/PhysRevB.13.5188.DOI
  23. [23]Gonze X., Lee C., Phys. Rev. B, 1997, 55, 10355, doi:10.1103/PhysRevB.55.10355.DOI
  24. [24]Resta R., Vanderbilt D., In: Physics of Ferroelectrics. Topics in Applied Physics, Vol 105. Springer, Berlin, Heidelberg, 2007, 31–68, doi:10.1007/978-3-540-34591-6_2.DOI
  25. [25]Hussin N.H., Taib M.F.M., Hassan O.H., Yahya M.Z.A., Mater. Res. Express, 2017, 4, 074001, doi:10.1088/2053-1591/aa6c42.DOI
  26. [26]Wang J., Pang X., Akin M., Lin Z., J. Mater. Chem., 2010, 20, 5945–5949, doi:10.1039/C0JM00270D.DOI
  27. [27]Murnaghan F.D., PNAS, 1944, 30, 244, doi:10.1073/pnas.30.9.244.DOI
  28. [28]Luan X., Qin H., Liu F., Dai Z., Yi Y., Li Q., Crystals, 2018, 8, 307, doi:10.3390/cryst8080307.DOI
  29. [29]Nye J.F., Physical Properties of Crystals: Their Representation by Tensors Matrices, Oxford University Press, Oxford, 1985.
  30. [30]Weiner J.H., Statistical Mechanics of Elasticity, Dover Publications, New York, 2012.
  31. [31]Marton P., Elsässer C., Phys. Status Solidi B, 2011, 248, 2222–2228, doi:10.1002/pssb.201046598.DOI
  32. [32]Zuo L., Humbert M., Esling C., J. Appl. Cryst., 1992, 25, 751–755, doi:10.1107/S0021889892004874.
  33. [33]Pugh S.F., Philos. Mag., 1954, 45, 823–843, doi:10.1080/14786440808520496.DOI
  34. [34]Ravindran P., Fast L., Korzhavyi P.A., Johansson B., Wills J., Eriksson O., J. Appl. Phys., 1998, 84, 4891–4904, doi:10.1063/1.368733.DOI
  35. [35]Ranganathan S.I., Ostoja-Starzewski M., Phys. Rev. Lett., 2008, 101, 055504, doi:10.1103/PhysRevLett.101.055504.DOI
  36. [36]Long J., Yang L., Wei X., J. Alloys Compd., 2013, 549, 336–340, doi:10.1016/j.jallcom.2012.08.120.DOI
  37. [37]Lu H., Long J., Yang L., Huang W., Int. J. Mod. Phys. B, 2014, 28, 1450057, doi:10.1142/S021797921450057X.DOI
  38. [38]Gonze X., Allan D.C., Teter M.P., Phys. Rev. Lett., 1992, 68, 3603, doi:10.1103/PhysRevLett.68.3603.DOI
  39. [39]Saghi-Szabo G., Cohen R.E., Krakauer H., Phys. Rev. B, 1999, 59, 12771, doi:10.1103/PhysRevB.59.12771.
  40. [40]Zhang Y., Sun J., Perdew J.P., Wu X., Phys. Rev. B, 2017, 96, 035143, doi:10.1103/PhysRevB.96.035143.DOI
  41. [41]Kuma S., Woldermariam M.M., Adv. Condens. Matter Phys., 2019, 2019, 201?315?
  42. [42]Gajdoš M., Hummer K., Kresse G., Furthmüller J., Bechstedt F., Phys. Rev. B, 2006, 73, 045112, doi:10.1103/PhysRevB.73.045112.DOI
  43. [43]He Y., Zeng T., J. Phys. Chem. C, 2010, 114, 18023–18030, doi:10.1021/jp101598j.

Paper details

vlnc:W_dbmjnqu7
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents