Influence of CaO and SiO2 additives on the sintering behavior of Cr,Ca:YAG ceramics prepared by solid-state reaction sintering

Abstract

Optical ceramics of yttrium aluminum garnet (Y3-xCaxAl4.95Cr0.05O12) doped with 0.1 at.% of chromium ions and 0.5, 0.8, and 1.2 at.% of calcium ions were prepared by reactive sintering in vacuum at 1750 degrees C. The influence of SiO2 and CaO sintering aids on the optical properties and microstructure of Cr,Ca:YAG ceramics was investigated. A decrease in CaO concentration led to a reduction of Cr,Ca:YAG transparency from 81 to 0 percent at 1064 nm; moreover, ceramics with lower CaO content exhibited abnormal grains and high porosity. These features were attributed to interactions between silica and calcium oxide during vacuum sintering. Two mechanisms are proposed to explain the effect of CaO and SiO2 on the formation of Ca,Cr:YAG ceramics. The first involves the formation of a liquid phase due to the CaO-SiO2 interaction during the heating stage, resulting in abnormal grain growth. The second mechanism is the mutual consumption of Si4+ and Ca2+ ions during the isothermal stage of sintering, which leads to a decrease in Cr4+ concentration. Both mechanisms negatively affect the optical and laser properties of the ceramics.

Introduction

During the last few decades, YAG based solid-state materials doped with Cr4+\mathrm{Cr}^{4+} have been widely used and investigated as tunable solid-state lasers for the 1.35-1.55 μm\mu\mathrm{m} spectral region [1] and as passive Q-switch lasers [2, 3, 4]. Much attention has been given to the Cr4+\mathrm{Cr}^{4+}:YAG saturated absorber used in microchip Q-switched lasers, which allows generating ultra-short (up to few dozen picoseconds) high power in the maximum pulse. YAG ceramics have not yet been extensively employed for microchips, and, among the advantages, they withstand high concentration of doping ions, the fabrication is easy and they are high-temperature resistant.

The main characteristic of Cr4+\mathrm{Cr}^{4+}:YAG materials is the necessity to use divalent additives for charge compensation. Yttrium-aluminum-garnet crystal (YAG) has a cubic structure and belongs to the Ia-3d space group with the stoichiometric formula [C]3[A]2[D]3O12[\mathrm{C}]_{3}[\mathrm{A}]_{2}[\mathrm{D}]_{3}\mathrm{O}_{12}, where C, A and D denote dodecahedral, octahedral, and tetrahedral lattice sites, respectively [5, 6]. The possibility of using Cr4+\mathrm{Cr}^{4+}:YAG materials as Q-switched lasers is based on the large ground-state absorption cross-section and excited-state lifetime of tetrahedral coordinated Cr4+\mathrm{Cr}^{4+} ions. During vacuum sintering, Cr dopants incorporate into the YAG lattice in the trivalent state, replacing Al3+\mathrm{Al}^{3+} in the octahedral positions [7, 8]. After vacuum sintering, only Cr3+\mathrm{Cr}^{3+} exists, because the formation of Cr4+\mathrm{Cr}^{4+} requires high-temperature air annealing. Cr4+\mathrm{Cr}^{4+}:YAG ceramics must contain divalent additives such as Ca2+\mathrm{Ca}^{2+} or Mg2+\mathrm{Mg}^{2+} for stabilizing Cr4+\mathrm{Cr}^{4+} in the tetravalent state [7, 9].

One of the ways to create highly transparent YAG ceramics is using SiO2\mathrm{SiO}_{2} sintering aids. Ikesue et al. [10] first reported highly efficient laser gain of transparent Nd:YAG ceramics produced by sintering a powdered mixture of Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}, Y2O3\mathrm{Y}_{2}\mathrm{O}_{3}, and Nd2O3\mathrm{Nd}_{2}\mathrm{O}_{3} at 1750°C for 8 h. They found that the addition of 0.14 wt.% (1.35 mol%) SiO2\mathrm{SiO}_{2} is crucial for sintering transparent Nd:YAG ceramics. This phenomenon has been later confirmed and, nowadays, different concentrations of SiO2\mathrm{SiO}_{2} are commonly added as a sintering aid to produce Nd:YAG ceramics of laser-quality [11, 12, 13, 14]. The most popular model for describing the interaction between SiO2\mathrm{SiO}_{2} and YAG is the formation of a liquid phase [15] or an increase in the concentration of cation vacancies [16] due to the incorporation of Si4+\mathrm{Si}^{4+} ions into the YAG lattice.

The presence of SiO2\mathrm{SiO}_{2} has a negative effect on the properties of Cr4+\mathrm{Cr}^{4+}:YAG ceramics, as it leads to a decrease in optical transparency [17] and inhibits the Cr3+→Cr4+\mathrm{Cr}^{3+} \to\mathrm{Cr}^{4+} ions conversion efficiency [18], consequently, it is not convenient to produce Cr4+\mathrm{Cr}^{4+}:YAG ceramics. The reason for such behaviour has not yet been revealed. Understanding the interactions between SiO2\mathrm{SiO}_{2} and CaO during vacuum sintering will allow expanding our knowledge about ceramics sintering. Moreover, shedding light on these interactions enables to understand how to use CaO\mathrm{CaO} and SiO2\mathrm{SiO}_{2} additives to create doped Cr4+\mathrm{Cr}^{4+}:YAG\mathrm{YAG} ceramics for laser applications.

Therefore, the purpose of this work is to investigate the interaction between SiO2\mathrm{SiO}_{2} and CaO\mathrm{CaO} compounds during vacuum sintering of Ca,Cr:YAG\mathrm{Ca,Cr:YAG} ceramics.

Experimental

In the present work, high purity Al2O3\mathrm{Al}_{2}\mathrm{O}_{3} (purity >99.99%>99.99\%, Baikowski, d=0.15-0.3 μ\mum), Y2O3\mathrm{Y}_{2}\mathrm{O}_{3} (purity >99.999%>99.999\%, Alfa Aesar, d=<10<10 μ\mum), Y2O3\mathrm{Y}_{2}\mathrm{O}_{3} (purity >99.97%>99.97\%, Alfa Aesar, d=<100<100 nm), CaO\mathrm{CaO} (purity >99.999%>99.999\%, Sigma Aldrich, d=<0.1<0.1 μ\mum) powders were used as starting materials. Tetraethoxysilane (TEOS, purity >99.999%>99.999\%, Sigma-Aldrich, USA) was used as an original substance of SiO2\mathrm{SiO}_{2} for sintering aid. Powders were taken in the YAG stoichiometric ratio, the concentration of Ca2+\mathrm{Ca}^{2+} and Cr3+\mathrm{Cr}^{3+} was calculated to replace Y3+\mathrm{Y}^{3+} and Al3+\mathrm{Al}^{3+} respectively.

The powder mixtures were ball milled in anhydrous alcohol for 15 hours using high purity Al2O3\mathrm{Al}_{2}\mathrm{O}_{3} balls, then dried at 70°C and granulated by sieving. The compacts were prepared by uniaxial pressing at P = 250 MPa. Before vacuum sintering, they were annealed in the air for two hours at 600°C. Sintering was performed in a vacuum furnace at 1750°C and a vacuum of 10−510^{-5} Pa for 10 hours. For recharging Cr3+\mathrm{Cr}^{3+} in its tetravalent state, air annealing at 1490°C for 20 hours was performed. The samples of Cr,Ca:YAG\mathrm{Cr,Ca:YAG} ceramics were obtained with a diameter of 10 mm and a thickness of 1.2 mm.

Cr,Ca:YAG\mathrm{Cr,Ca:YAG} ceramics doped with different concentration of calcium 0.5, 0.8, 1.2 at% were labelled as Ca=0.5, Ca=0.8 and Ca=1.2 respectively. Figure 1 reports a photograph of the mirror-polished Cr,Ca:YAG\mathrm{Cr,Ca:YAG} ceramics after vacuum sintering and followed air annealing. The concentration of chromium oxide was constant and set at 0.1 at.%. All samples were doped with 0.5 wt.% TEOS which yields silica levels of approximately 0.14 wt.%.

Photograph of mirror polished Ca=0.5, Ca=0.8 and Ca=1.2 samples

Figure 1. Photograph of the mirror polished a) Ca=0.5, b) Ca=0.8 and c) Ca=1.2 samples after vacuum sintering and d) Ca=0.5, e) Ca=0.8 and f) Ca=1.2 after followed air annealing at 1490°C for 20 h.

The linear optical transmission spectra of Cr,Ca:YAG\mathrm{Cr,Ca:YAG} ceramics were collected with the UV/Vis spectrophotometer “Analytik Jena specord 200” at the range 190-1100 nm. Cr,Ca:YAG\mathrm{Cr,Ca:YAG} ceramics morphology was studied using a JEOL JSM- 6390LV scanning electron microscope, the elemental analysis was performed on Silicon Drift Detector (SSD) X-MaxN Oxford Instruments. To obtain XRD spectra, a DRON 3 type diffractometer was used. The measurement of the variation in elements concentration was carried out by chemical analysis under each stage of ceramics production; the methodology is described in detail in ref. [19].

Results

The aim of this work is to understand the influence of dopant interactions on YAG ceramics prepared by solid-state reaction (SSR) sintering in a vacuum, taking as a reference the interaction between CaO and SiO2_2. The vacuum sintering process can be separated into two stages: heating and isothermal annealing. During the heating stage, the ceramic density increased from 70 to 99.9 %, while only a fraction of the porosity was removed during isothermal annealing [16]. Therefore, the heating stage is a pivotal step in ceramics sintering, and we speculate that the CaO - SiO2_2 interaction at an early preparation stage can significantly change the final microstructure of the YAG ceramics obtained after sintering. Below, the properties of Cr,Ca:YAG ceramics with different CaO/SiO2_2 ratio are presented, we expect that the dissimilar properties exhibited by the samples are ascribable to a different interaction between CaO and SiO2_2 during the initial stage.

Structural characterization

The X-ray diffraction patterns of the prepared samples coincided with the crystal structure of pure YAG phase and corresponded to the Inorganic Crystal Structure Database (ICSD) Card N 170158 (Figure 2). New peaks and/or peak shifts were not observed in the Cr,Ca:YAG diffraction pattern compared to the pure YAG one. It can be noted that the sensitivity of XRD analysis was close to 1 at.%, indicating that a small concentration of impurities might be present in the samples.

X-ray diffraction patterns of the prepared samples and pure YAG ICSD reference pattern

Figure 2. The X-ray diffraction patterns of the prepared samples and pure YAG ICSD reference pattern (Card N 170158).

Our experiment shows that increasing the concentration of Ca from 0.5 to 0.8 led to a stabilization of the grain size and inhibited anomalous grain growth. The grain structure of Cr,Ca:YAG ceramics was investigated by SEM analysis after thermal etching at 1490°C for 20 hours in air ambient. Ca=0.5 sample had a bimodal grain size distribution: most of the grains were in the range 0.5–4.5 μm\mu\mathrm{m}, with peaks also at 1 μm\mu\mathrm{m} and 2 μm\mu\mathrm{m}, whereas larger grains from few dozens to few hundred microns were also detected. An increase in Ca concentration led to a reduction in grain size and to the disappearance of the abnormally large grains. Ca=0.8 and Ca=1.2 samples have grain size distribution from 0.5 to 2 μm\mu\mathrm{m} with average grain size 0.9 ±\pm 0.05 μm\mu\mathrm{m} (Figure 3a). The standard deviation was calculated using the Student’s t-test.

Figure 3. a) Grain size distribution of the samples. c) SEM image surface of Ca=0.5 sample after air annealing at 1490°C for 20 hours. b) SEM image surface of Ca=0.8 sample after air annealing at 1490°C for 20 hours. d) SEM image surface of Ca=1.2 sample after air annealing at 1490°C for 20 hours

The SEM analysis shows the appearance of a precipitate on the surface of Ca=0.8 and Ca=1.2 samples after air annealing. It means that the microstructure of the samples correlates with the presence of additives on the surface. Ca=0.5 sample has a clean surface (Figure 1b), while in the case of Ca=0.8 sample, we observed the formation of a precipitate covering 0.5% of the surface and organized in round shapes with size 1-2 μm1\text{-}2\,\mu\mathrm{m} (Figure 1c). Rising the concentration of Ca to 1.2 led to a change in the shape of the precipitate to dendrites and increasing its size up to 70 μm\mu\mathrm{m} with 7% covering of the surface (Figure 1d).

We suppose that the observed precipitate originates from the bulk of the ceramics and has grown as islands of thin films on the sample surface. These observed impurity phases in the SEM images look darker than the YAG matrix background, indicating the presence of a high concentration of ions lighter than Y3+Y^{3+} or Al3+Al^{3+} in the precipitate.

Figure 4 shows the maps of the area with precipitate particles on the surface of Ca = 1.2 sample by EDS analysis of selected elements: Al, Ca, O, and Y. Only basic elements of YAG: Al, O and Y were detected in the area of pure surface, whereas Ca was revealed in the precipitate. The EDS analysis depth is 11-3 μm3\,\mu\mathrm{m}, and the Y and Al signals coming from the YAG matrix penetrate through the precipitated particle lying on the surface. Evidently, these particles are of submicron thickness and contain Ca.

SEM surface image and EDS mapping of a precipitate on Cr,Ca:YAG ceramics

Figure 4. Precipitate on the surface of ceramics of Cr,Ca:YAG (1.2 at% Ca) after air annealing at 1490°C for 20 hours:(a) SEM surface image, EDS mapping of: (b) O, (c) Al, (d) Y, (e) Ca.

Summarizing, we detected the appearance of a precipitate on the samples' surfaces. After vacuum sintering, the surface of the samples was clean without any precipitates. Annealing in air leads to the appearance of the precipitate on the surface of Ca=0.8 and Ca=1.2 samples. We suppose that the diffusion of Ca2+Ca^{2+} ions from the bulk to the ceramic surface during air annealing leads to the formation of a Ca-rich phase. After softly polishing of samples, the surface became clean again, meaning that the Ca-phase is extremely thin.

Probably, the presence of a Ca-rich phase at the grain boundary in Ca=0.8 and Ca=1.2 samples causes the suppression of grain growth in these samples compared to the low calcium content Ca=0.5 sample.

Chemical analysis

The YAG ceramics sintering takes place in several steps and occurs at extremely high temperatures for a long time, meaning that the chemical composition of the samples can change during the process. The chromium and calcium compounds have the highest saturated vapor pressure among all components. Figure 5 shows a dependence of the initial compounds of the Cr,Ca:YAG ceramics powder mixture saturated vapor pressure on the temperature [20]. It is worth to note that chromium oxide and calcium oxide possess a vapor pressure few orders in magnitude higher than yttrium and aluminum oxides.

Temperature dependence of saturated vapor pressure of initial compounds

Figure 5. Temperature dependence of saturated vapor pressure of initial compounds: i) Cr2_2O3_3 ii) SiO2_2 iii) CaO iv) Al2_2O3_3 v) Y2_2O3_3 [20]

A variation of chromium and calcium content in the Cr,Ca:YAG ceramics due to evaporation under vacuum synthesis can strongly affect the sintering process and the functional properties of Cr,Ca:YAG ceramics. The Ca=0.8 sample was investigated by means of elemental chemical analysis. In particular, we analyzed the change in the original powders content after thermal treatment of the initial powder mixture at 600°C, followed by vacuum sintering and air annealing. Table 1 reports the chemical analysis of Ca=0.8 sample, where the steps are indicated as follow: ”Powder” - powders mixture, ”600°C” - a mixture of the original powder thermally treated at 600°C, ”1750°C” – Cr,Ca:YAG ceramics after vacuum sintering.

StageElement content, wt.%
YAlCaCr
Powder43.622.10.180.038
600°C44.522.70.170.038
1750°C39.821.10.140.035

Table 1. The chemical analysis of Ca=0.8 sample.

We detected a decrease in Ca and Cr amounts in the sample during vacuum sintering. The initial element concentrations after thermal treatment at 600°C did not practically change compared to the powder mixture according to the results of the chemical analysis. But the vacuum sintering process led to a decrease in Cr and Ca content of 14 % and 7 % respectively.

Concentration of Cr3+Cr^{3+} and Cr4+Cr^{4+} ions

We found that vacuum sintering induces the formation of Cr4+Cr^{4+} ions. Transmission spectra of the samples after vacuum sintering show only the formation of Cr3+Cr^{3+} ions (see Figure 6). The two broad absorption bands correspond to the 4A2→4T2{}^{4}A_{2} \rightarrow{}^{4}T_{2} and 4A2→4T1{}^{4}A_{2} \rightarrow{}^{4}T_{1} transitions centred at 590 and 430 nm respectively, which are responsible for the bright green color of Cr3+Cr^{3+}:YAG ceramics. After vacuum sintering, Ca=1.2, Ca=0.8 and Ca=0.5 samples had transmittance of 81, 24 and 0 % respectively at λ=1064\lambda=1064 nm.

Figure 6. a) Optical in-line transmittance spectra of i) Ca=0.5, ii) Ca=0.8 and iii) Ca=1.2 samples, b) comparison of transmittance spectra between a fully reduced and a fully oxidized Ca=1.2 sample.

Cr,Ca:YAG ceramics transparency decreased after annealing in air at 1490°C for 20 hours due to the formation of Cr4+\mathrm{Cr}^{4+} absorption centres in visible and near-infrared spectral region. The formation of Cr4+\mathrm{Cr}^{4+} ions in Cr,Ca:YAG ceramics takes place during annealing in an oxidizing ambient where the tetravalent additives can be stabilized through the formation of structural defects in the lattice such as divalent additives [21, 22].

The concentration of Cr3+\mathrm{Cr}^{3+} and Cr4+\mathrm{Cr}^{4+} ions in different lattice positions for Cr,Ca:YAG ceramics was calculated from the Cr4+\mathrm{Cr}^{4+} absorptions spectra, for a detailed explanation of the methodology, refer to [23]. The calculated Cr4+\mathrm{Cr}^{4+} concentrations are reported in Table 2. According to the calculations, Ca=1.2 sample contains CrA4+\mathrm{Cr}_{A}^{4+} and CrD4+\mathrm{Cr}_{D}^{4+} ions close to 9.8⋅1017 cm−39.8 \cdot10^{17}\ \mathrm{cm}^{-3} and 3.6⋅1017 cm−33.6 \cdot10^{17}\ \mathrm{cm}^{-3} respectively. In the case of sample Ca=0.8, the amounts of CrA4+\mathrm{Cr}_{A}^{4+} and CrD4+\mathrm{Cr}_{D}^{4+} ions were 3.8⋅1017 cm−33.8 \cdot10^{17}\ \mathrm{cm}^{-3} and 1.5⋅1017 cm−31.5 \cdot10^{17}\ \mathrm{cm}^{-3}, respectively. The Cr3+\mathrm{Cr}^{3+} ions concentration was corrected for the Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3} losses determined by elemental chemical analysis and the amount of Cr4+\mathrm{Cr}^{4+} ions. The sample Ca=1.2 has a higher concentration of Cr4+\mathrm{Cr}^{4+} ions both in the octahedral and in the tetrahedral sites in comparison to the other samples. The Cr4+/Crtotal\mathrm{Cr}^{4+}/\mathrm{Cr}_{total} ratio is linearly dependent on Ca2+\mathrm{Ca}^{2+} concentration and we found it to be 6.6 %, 2.6 % and 0 % for samples Ca=1.2, Ca=0.8 and Ca=0.5. Less than 1% of Ca2+\mathrm{Ca}^{2+} ions are involved in the formation of Cr4+\mathrm{Cr}^{4+} ions, which is much less than what found for samples without SiO2\mathrm{SiO}_{2} [23].

SampleN0⋅1017N_{0} \cdot10^{17}, cm−3\mathrm{cm}^{-3}part of Cr4+\mathrm{Cr}^{4+} ions, %Cr4+\mathrm{Cr}^{4+} ratio
SampleCrA3+\mathrm{Cr}_{A}^{3+}CrA4+\mathrm{Cr}_{A}^{4+}CrD4+\mathrm{Cr}_{D}^{4+}CrA4+/Ca2+\mathrm{Cr}_{A}^{4+}/\mathrm{Ca}^{2+}CrA4+/Crtotal\mathrm{Cr}_{A}^{4+}/\mathrm{Cr}_{total}ND/NAN_{D}/N_{A}
Ca = 1.21909.83.60.86.60.37
Ca = 0.81993.81.50.52.60.39

Table 2. Parameters of the samples: assignment, N0N_{0} - concentration of absorbing center, ND/NAN_{D}/N_{A} - tetrahedral to octahedral Cr4+\mathrm{Cr}^{4+} ions concentration ratio.

Discussion

In this paper, we examined the influence of dopants and their interaction on optical properties and microstructure of YAG-doped ceramics. We suppose that one of the reasons for the dramatic change in microstructure and transparency of the samples is the influence of CaO and SiO2_{2} interactions on the stability of the pore network. Solid-state vacuum sintering of Cr,Ca:YAG ceramics can be considered as a two-stage process: heating and isothermal annealing. During the first stage, the following modifications take place: (i) formation of necks between grains, (ii) necks evolution into grain boundaries, (iii) formation of an open pore network, (iv) thinning of the diameter of the pore channels, (v) their collapse into closed pores [24]. The critical diameter of the pore channels depends on the relation between grain boundary mass transport and surface mass transport before collapsing into close porosity. Smaller pores are removed more easily from the ceramic bulk than larger pores. Therefore, the formation of different intergrains phases (i.e.i.e. in the case of CaO\mathrm{CaO} and SiO2\mathrm{SiO}_{2} interactions) can change the diameter of the pore channels, thus affecting the properties of the final Cr,Ca:YAG\mathrm{Cr,Ca:YAG} ceramics [25]. Our Discussion section is divided into two subsections: in the first one (4.1), the influence of CaO\mathrm{CaO} and SiO2\mathrm{SiO}_{2} interactions during the heating stage of sintering is presented; in the second one (4.2), the influence of Ca2+\mathrm{Ca}^{2+} and Si4+\mathrm{Si}^{4+} ions interaction on sample properties is reported.

Influence of CaO\mathrm{CaO} and SiO2\mathrm{SiO}_{2} interactions

The interactions between CaO\mathrm{CaO} and SiO2\mathrm{SiO}_{2} dopants led to the formation of several intermediate phases characterized by different Ca-doping levels, the presence of these phases explains the observed properties of the samples. During vacuum sintering, the initial compounds (Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}, Y2O3\mathrm{Y}_{2}\mathrm{O}_{3}) and dopants (Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3}, CaO\mathrm{CaO}, SiO2\mathrm{SiO}_{2}) interact, leading to the formation of intermediate phases which can alter the sintering behavior. The amount of CaO\mathrm{CaO} and Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3} was negligibly small compared to Al2O3\mathrm{Al}_{2}\mathrm{O}_{3} and Y2O3\mathrm{Y}_{2}\mathrm{O}_{3} and the amount of CaO\mathrm{CaO} was much higher than Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3} while the concentrations of CaO\mathrm{CaO} and SiO2\mathrm{SiO}_{2} are comparable. Moreover, the CaO\mathrm{CaO} and SiO2\mathrm{SiO}_{2} low solubility in YAG is in contrast with Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3}, which is well soluble in YAG. Therefore, a variation in CaO\mathrm{CaO} concentration did not have any influence on its interaction with Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}, Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3} and Y2O3\mathrm{Y}_{2}\mathrm{O}_{3} but, in the case of CaO\mathrm{CaO}-SiO2\mathrm{SiO}_{2} interactions, the opposite behavior is observed.

We suppose that the properties of the samples can be explained by the different interactions between CaO\mathrm{CaO} and SiO2\mathrm{SiO}_{2} taking place at the YAG grain boundaries during the heating stage. Due to the low solubility of Ca2+\mathrm{Ca}^{2+} and Si4+\mathrm{Si}^{4+} ions, only a fraction of the CaO\mathrm{CaO} and SiO2\mathrm{SiO}_{2} can dissolve into the YAG matrix. CaO\mathrm{CaO} and SiO2\mathrm{SiO}_{2} dopants are located at the grain boundaries during the heating stage of vacuum sintering and the interaction between these dopants leads to the formation of different intermediate compounds, which chemical composition can be predicted from the SiO2\mathrm{SiO}_{2}-CaO\mathrm{CaO} phase diagram by considering the initial SiO2/CaO\mathrm{SiO}_{2}/\mathrm{CaO} ratio. It should be noted that correlating the CaO\mathrm{CaO} concentration with the optical properties of the samples based only on the binary phase diagram of CaO\mathrm{CaO}-SiO2\mathrm{SiO}_{2} is not correct: the entire CaO\mathrm{CaO}-Cr2O3\mathrm{Cr}_{2}\mathrm{O}_{3}-Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}-Y2O3\mathrm{Y}_{2}\mathrm{O}_{3}-SiO2\mathrm{SiO}_{2} system should be considered, which is a too complicated system. Although the binary phase diagram of CaO\mathrm{CaO}-SiO2\mathrm{SiO}_{2} does not provide a true representation of the system, it does allow estimating its behavior.

The SiO2\mathrm{SiO}_{2}-CaO\mathrm{CaO} ratio in Ca=0.5\mathrm{Ca}=0.5, Ca=0.8\mathrm{Ca}=0.8 and Ca=1.2\mathrm{Ca}=1.2 samples were 37-63 mol. %, 26-74 mol. % and mol. 20-80%. According to the CaO\mathrm{CaO}-SiO2\mathrm{SiO}_{2} phase diagram, [26] the interaction between CaO\mathrm{CaO} and SiO2\mathrm{SiO}_{2} in the Ca=0.5\mathrm{Ca}=0.5 sample can lead to the formation of a mixture of rankinite (Ca3Si2O7\mathrm{Ca}_{3}\mathrm{Si}_{2}\mathrm{O}_{7}) and wollastonite (CaSiO3\mathrm{CaSiO}_{3}), which eutectic composition melts at 1450 °C. We suppose that the formation of a liquid near 1450°C leads to an early collapsing of the pore channel, which results in the formation of large pores, detected by SEM (see Figure 3b). In the case of Ca=0.8\mathrm{Ca}=0.8 and Ca=1.2\mathrm{Ca}=1.2 samples, the lowest temperature at which the liquid can appear is 2057 °C, when the eutectic composition of larnite (Ca2SiO4\mathrm{Ca}_{2}\mathrm{SiO}_{4}) and CaO\mathrm{CaO} is much higher than the ceramics sintering temperature (1750°C). We assume that the absence of a liquid phase is the reason for a normal pore evolution which results in the formation of high-density Cr,Ca:YAG ceramics without large pores.

The CaO\mathrm{CaO} excess, which does not interact with SiO2\mathrm{SiO}_{2}, segregates at the grain boundaries as has been reported in our previous work, see ref. [21]. The presence of extra CaO\mathrm{CaO} at the grain boundaries suppresses grain growth, explaining the absence of abnormal grains in the Ca=0.8\mathrm{Ca}=0.8 and Ca=1.2\mathrm{Ca}=1.2 samples. The extra CaO\mathrm{CaO} is also responsible for the formation of the Ca-rich phases on the ceramic surface after air annealing (see Figure 3d) due to the high partial pressure of CaO\mathrm{CaO} vapor, see Figure 5. It should be noted that there is evidence that air annealing decreases CaO\mathrm{CaO} content, see ref. [21], but, as far as we know, there are not yet data in the literature about the decrease in the calcium-silica phases emerging on the grain boundaries and whether they remain after air annealing. Light scattering on these phases can worsen the optical quality of ceramics.

Influence of Ca2+\mathrm{Ca}^{2+} and Si4+\mathrm{Si}^{4+} interactions

The SiO2\mathrm{SiO}_{2} additive does not only influence the processes under the heating stages, but also the final isothermal stage of YAG ceramics sintering thanks to the ability to generate cation vacancies in the YAG lattice. Kuklja et al. proposed that the incorporation of Si4+\mathrm{Si}^{4+} in the YAG crystal lattice introduces an extra positive charge [27]. To compensate for this charge, cation vacancies are generated. The appearance of cation vacancies increases Y3+\mathrm{Y}^{3+} and Al3+\mathrm{Al}^{3+} ions diffusivity in the YAG, which causes an increase in ceramics densification compared to Si-undoped YAG [28].

The incorporation of Ca2+\mathrm{Ca}^{2+} ions in the YAG crystal lattice leads to the formation of [Ca2+⋯Si4+][\mathrm{Ca}^{2+}\cdots\mathrm{Si}^{4+}] neutral complexes, limiting the formation of cation vacancies and thus decreasing ceramics densification. The solubility of Ca2+\mathrm{Ca}^{2+} and Si4+\mathrm{Si}^{4+} ions in the YAG is very low when they solute individually. Ca2+\mathrm{Ca}^{2+} solubility in the YAG is 300- 400 ppm [29], the solubility limit of Si4+\mathrm{Si}^{4+} in YAG is up to 600 ppm [30]. However, simultaneous doping of YAG with Ca2+\mathrm{Ca}^{2+} and Si4+\mathrm{Si}^{4+} significantly increases the solubility of both ions [31], evidenced by the presence of [Ca2+⋯Si4+][\mathrm{Ca}^{2+}\cdots\mathrm{Si}^{4+}] complexes. We assume that Si4+\mathrm{Si}^{4+} mostly combines with Ca2+\mathrm{Ca}^{2+} when there is enough Ca2+\mathrm{Ca}^{2+} and, in this case, the generation of cation vacancies does not occur. The lack of cation vacancies causes the deterioration of the ceramic densification, which results in a worsening of its optical quality.

The use of Cr4+\mathrm{Cr}^{4+}:YAG ceramics as Q-switches requires not only high optical quality, but also high Cr4+\mathrm{Cr}^{4+} ions absorption at laser wavelength (∼1\sim1 μm). Therefore, the Cr3+\mathrm{Cr}^{3+} to Cr4+\mathrm{Cr}^{4+} transformation was investigated. As shown in Table 3, less than 1% of Ca2+\mathrm{Ca}^{2+} and 2.6% to 6.6% of Cr3+\mathrm{Cr}^{3+} ions participate in the Cr3+→Cr4+\mathrm{Cr}^{3+}\rightarrow\mathrm{Cr}^{4+} ions valence transformation. The absorbance of CrD4+\mathrm{Cr}^{4+}_{\mathrm{D}} ions at λ=1030\lambda=1030 nm was close to 1 cm−1\mathrm{cm}^{-1}, which is less than in the case of Cr,Ca:YAG ceramics without SiO2\mathrm{SiO}_{2} additives [18, 23].

The Si4+\mathrm{Si}^{4+} ion influence on Cr4+\mathrm{Cr}^{4+} ions concentration is mediated by the formation of [Ca2+⋯Si4+][\mathrm{Ca}^{2+}\cdots\mathrm{Si}^{4+}] neutral complexes, which take away part of Ca2+\mathrm{Ca}^{2+} ions necessary to compensate for the Cr4+\mathrm{Cr}^{4+} positive charge [32]. The dissolution of Ca2+\mathrm{Ca}^{2+} ions in the YAG lattice normally generates neutral complexes with oxygen vacancies. During air annealing, these complexes are destroyed and Ca2+\mathrm{Ca}^{2+} ions recharge Cr3+\mathrm{Cr}^{3+} to Cr4+\mathrm{Cr}^{4+}. But the presence of Si4+\mathrm{Si}^{4+} leads to the formation of neutral complexes [Ca2+⋯Si4+][\mathrm{Ca}^{2+}\cdots\mathrm{Si}^{4+}] in place of Ca2+\mathrm{Ca}^{2+} ions stabilized by oxygen vacancies.

In summary, we propose and discussed two mechanisms of CaO\mathrm{CaO} and SiO2\mathrm{SiO}_{2} influence on the formation of Ca,Cr:YAG ceramics. The first one consists in the appearance of a liquid phase due to CaO\mathrm{CaO}-SiO2\mathrm{SiO}_{2} interaction with a specific ratio under the heating stage of the ceramics sintering. Under this way, the abnormal growth of ceramics grains occurs. The second mechanism consists of the mutual consumption of Si4+\mathrm{Si}^{4+} ions and Ca2+\mathrm{Ca}^{2+} ions under the isothermal stage of ceramic sintering, leading to a decrease of Cr4+\mathrm{Cr}^{4+} concentration. Both mechanisms have a negative effect on the optical and laser properties of the ceramics.

However, some remarks are worth noting: our hypotheses were supported only by the interaction between CaO\mathrm{CaO} and SiO2\mathrm{SiO}_{2} during sintering, and we did not perform a study of the phase composition and morphology of the samples during the heating stage. Future work will include an evaluation of phase composition and morphology evolution of the samples during the heating stage.

Conclusions

The influence of SiO2\mathrm{SiO}_{2} and CaO sintering aids on the optical properties and the microstructure of Cr,Ca:YAG ceramics was evaluated in this work. We found that the interactions between CaO and SiO2\mathrm{SiO}_{2} compounds, as well as the presence of Ca2+\mathrm{Ca}^{2+} and Si4+\mathrm{Si}^{4+} ions have a negative impact on the properties of Cr,Ca:YAG ceramics. Decreasing the concentration of CaO led to a decrease in Cr,Ca:YAG ceramics transparency from 81 to 0 % at 1064 nm, moreover, the sample with the lowest concentration of CaO (0.5 at.%) had abnormally large grains and high porosity. The difference in microstructure of Cr,Ca:YAG ceramics was explained through the interaction of CaO and SiO2\mathrm{SiO}_{2} on the YAG grain boundaries during the heating stage. The appearance of a liquid phase at 1450°C resulting from the interaction between CaO and SiO2\mathrm{SiO}_{2} leads to early collapse of the pore channels that results in the formation of large pores and abnormal grains in the ceramics. The Ca2+\mathrm{Ca}^{2+} - Si4+\mathrm{Si}^{4+} interaction in the YAG lattice reduces both ceramics density and Cr4+\mathrm{Cr}^{4+} concentrations. Ca2+\mathrm{Ca}^{2+} and Si4+\mathrm{Si}^{4+} form neutral complexes that inhibit the generation of cation vacancies. The lack in cation vacancies results in a decrease of Al3+\mathrm{Al}^{3+} and Y3+\mathrm{Y}^{3+} diffusion during ceramics sintering and to the deterioration of the ceramic's optical quality. The combination of Ca2+\mathrm{Ca}^{2+} and Si4+\mathrm{Si}^{4+} ions is responsible for the decrease in the concentration of Cr4+\mathrm{Cr}^{4+} ions formed by Cr3+\mathrm{Cr}^{3+} oxidation due to a lack of charge compensator for the extra charge of Cr4+\mathrm{Cr}^{4+}. Therefore, the sintering aid SiO2\mathrm{SiO}_{2}, which is widely used in ceramic technology, should not be used to prepare Cr4+\mathrm{Cr}^{4+}:YAG ceramics when great optical quality is desired.

Acknowledgments: The authors are grateful to Dr. A.G. Doroshenko and Dr. S.V. Parkhomenko for their help in sintering of the sample. Authors thank Dr. P.V. Mateychenko for providing SEM and EDS measurements at the center for the sharing of scientific equipment "Microscopic and spectroscopic methods for studying the surface of solids" of the STC “Institute for Single Crystals” National Academy of Sciences of Ukraine.

References

  1. [1]Angert, N. B., Borodin, N. I., Garmash, V. M., Zhitnyuk, V. A., Okhrimchuk, A. G., Siyuchenko, O. G., & Shestakov, A. V. (1988). Lasing due to impurity color centers in yttrium aluminum garnet crystals at wavelengths in the range 1.35–1.45 μm. Soviet Journal of Quantum Electronics, 18(1), 73.DOI
  2. [2]Ubizskii, S., Buryy, O., Börger, A., & Becker, K. D. (2009). Investigation of the chromium ions recharging kinetics in Cr, Mg: YAG crystal during high-temperature annealing. physica status solidi (a), 206(3), 550-561.DOI
  3. [3]Wajler, A., Kozłowska, A., Nakielska, M., Leśniewska-Matys, K., Sidorowicz, A., Podniesiński, D., & Putyra, P. (2014). Nonlinear Absorption of Submicrometer Grain-Size Cobalt-Doped Magnesium Aluminate Transparent Ceramics. Journal of the American Ceramic Society, 97(6), 1692-1695.DOI
  4. [4]Balashov, V. V., Bezotosnyi, V. V., Cheshev, E. A., Gordeev, V. P., Kanaev, A. Y., Kopylov, Y. L., ... & Tupitsyn, I. M. (2019). Composite Ceramic Nd3+:YAG/Cr4+:YAG Laser Elements. Journal of Russian Laser Research, 40(3), 237-242.
  5. [5]Chaika, M., Vovk, O., Mancardi, G., Tomala, R., & Strek, W. (2020). Dynamics of Yb2+ to Yb3+ ion valence transformations in Yb: YAG ceramics used for high-power lasers. Optical Materials, 101, 109774.DOI
  6. [6][6]. Tsiumra, V., Krasnikov, A., Zazubovich, S., Zhydachevskyy, Y., Vasylechko, L., Baran, M., ... & Suchocki, A. (2019). Crystal structure and luminescence studies of microcrystalline GGG:Bi3+ and GGG:Bi3+, Eu3+ as a UV-to-VIS converting phosphor for white LEDs. Journal of Luminescence, 213, 278-289.DOI
  7. [7]Chaika, M. A., Mancardi, G., Tomala, R., Stek, W., & Vovk, O. M. (2020). Effects of divalent dopants on the microstructure and conversion efficiency of Cr4+ ions in Cr,Me:YAG (Me-Ca, Mg, Ca/Mg) transparent ceramics. Processing and Application of Ceramics, 14(1), 83-89.DOI
  8. [8]Buryy, O. A., Ubizskii, S. B., Melnyk, S. S., & Matkovskii, A. O. (2004). The Q-switched Nd: YAG and Yb: YAG microchip lasers optimization and comparative analysis. Applied Physics B, 78(3-4), 291-297.DOI
  9. [9]Feldman, R., Shimony, Y., & Burshtein, Z. (2003). Dynamics of chromium ion valence transformations in Cr,Ca:YAG crystals used as laser gain and passive Q-switching media. Optical Materials, 24(1-2), 333-344.DOI
  10. [10]Ikesue, A., Yoshida, K., Yamamoto, T., & Yamaga, I. (1997). Optical scattering centers in polycrystalline Nd: YAG laser. Journal of the American Ceramic Society, 80(6), 1517-1522.DOI
  11. [11]Chretien, L., Bonnet, L., Boulesteix, R., Maitre, A., Salle, C., & Brenier, A. (2016). Influence of hot isostatic pressing on sintering trajectory and optical properties of transparent Nd: YAG ceramics. Journal of the European Ceramic Society, 36(8), 2035-2042.DOI
  12. [12]Liu, B., Li, J., Ivanov, M., Liu, W., Ge, L., Xie, T., ... & Guo, J. (2015). Diffusion-controlled solid-state reactive sintering of Nd:YAG transparent ceramics. Ceramics International, 41(9), 11293-11300.DOI
  13. [13]Vorona, I. O., Yavetskiy, R. P., Shpilinskaya, O. L., Kos’yanov, D. Y., Doroshenko, A. G., Parkhomenko, S. V., ... & Tolmachev, A. V. (2015). The effect of residual porosity on the optical properties of Y₃Al₅O₁₂:Nd³⁺ laser ceramics. Technical Physics Letters, 41(5), 496-499..DOI
  14. [14]Chaika, M. A., Tomala, R., Strek, W., Hreniak, D., Dluzewski, P., Morawiec, K., ... & Lesniewska-Matys, K. (2019). Kinetics of Cr³⁺ to Cr⁴⁺ ion valence transformations and intra-lattice cation exchange of Cr⁴⁺ in Cr,Ca:YAG ceramics used as laser gain and passive Q-switching media. The Journal of Chemical Physics, 151(13), 134708.DOI
  15. [15]Fabrichnaya, O., Seifert, H. J., Weiland, R., & Ludwig, T. (2001). Phase Equilibria and Thermodynamics in the YO-AlO–SiO System.
  16. [16]Stevenson, A. J., Li, X., Martinez, M. A., Anderson, J. M., Suchy, D. L., Kupp, E. R., ... & Messing, G. L. (2011). Effect of SiO₂ on densification and microstructure development in Nd:YAG transparent ceramics. Journal of the American Ceramic Society, 94(5), 1380-1387.DOI
  17. [17]M. A. Chaika, O. M. Vovk, N. A. Safronova, A. G. Doroshenko, S. V. Parkhomenko, A. V. Tolmachev, (2016) Mutual influence of additives of Ca and Si on properties of Cr-doped YAG ceramics, Functional materials 23(3), 398–403.DOI
  18. [18]Zhou, T., Zhang, L., Yang, H., Qiao, X., Liu, P., Tang, D., & Zhang, J. (2015). Effects of sintering aids on the transparency and conversion efficiency of Cr⁴⁺ ions in Cr:YAG transparent ceramics. Journal of the American Ceramic Society, 98(8), 2459-2464.DOI
  19. [19]O. V.Gayduk, (2017) Control of chromium dopant content in optical ceramics Cr:YAG, Functional materials 24(2), 318–321.DOI
  20. [20]L. Gurvich, I. Veits, C. Alcock, Thermodynamics properties of individual substances, New York, NY (US): Hemisphere Publishing Corp., 1989.
  21. [21]Chaika, M. A., Dluzewski, P., Morawiec, K., Szczepanska, A., Jablonska, K., Mancardi, G., Doroshenko, A. G. (2019). The role of Ca²⁺ ions in the formation of high optical quality Cr⁴⁺,Ca:YAG ceramics. Journal of the European Ceramic Society, 39(11), 3344-3352.DOI
  22. [22]Balabanov, S. S., Bykov, Y. V., Egorov, S. V., Eremeev, A. G., Gavrishchuk, E. M., Khazanov, E. A., Zelenogorskii, V. V. (2013). Yb:(YLa)₂O₃ laser ceramics produced by microwave sintering. Quantum Electronics, 43(4), 396.DOI
  23. [23]Chaika, M. A., Dulina, N. A., Doroshenko, A. G., Parkhomenko, S. V., Gayduk, O. V., Tomala, R., ... & Vovk, O. M. (2018). Influence of calcium concentration on formation of tetravalent chromium doped Y3Al5O12 ceramics. Ceramics International, 44(12), 13513-13519.DOI
  24. [24]Chaika, M., Paszkowicz, W., Strek, W., Hreniak, D., Tomala, R., Safronova, N., ... & Vovk, O. (2019). Influence of Cr doping on the phase composition of Cr, Ca: YAG ceramics by solid state reaction sintering. Journal of the American Ceramic Society, 102(4), 2104-2115.DOI
  25. [25]A. Ragulya, V. Skorokhod, Consolidated nanostructured materials, Naukova Dumka, Kiev 374.
  26. [26]Rankin, G. A. (1915). The ternary system CaO-Al₂O₃-SiO₂, with optical study by FE Wright. American Journal of Science, (229), 1-79.
  27. [27]Kuklja, M. M. (2000). Defects in yttrium aluminium perovskite and garnet crystals: atomistic study. Journal of Physics: Condensed Matter, 12(13), 2953.DOI
  28. [28]Kochawattana, S., Stevenson, A., Lee, S. H., Ramirez, M., Gopalan, V., Dumm, J., ... & Messing, G. L. (2008). Sintering and grain growth in SiO₂ doped Nd: YAG. Journal of the European Ceramic Society, 28(7), 1527-1534.
  29. [29]Schuh, L., Metselaar, R., & de With, G. (1989). Electrical transport and defect properties of Ca-and Mg-doped yttrium aluminum garnet ceramics. Journal of applied Physics, 66(6), 2627-2632.DOI
  30. [30]Y Wang, Y., Zhang, L., Fan, Y., Luo, J., McCready, D. E., Wang, C., & An, L. (2005). Synthesis, characterization, and optical properties of pristine and doped yttrium aluminum garnet nanopowders. Journal of the American Ceramic Society, 88(2), 284-286.DOI
  31. [31]Kuru, Y., Onur Savasir, E., Zeynep Nergiz, S., Oncel, C., & Ali Gulgun, M. (2008). Enhanced co-solubilities of Ca and Si in YAG (Y₃Al₅O₁₂). physica status solidi c, 5(10), 3383-3386..
  32. [32]Chaika, M. A., Vovk, O. M., Doroshenko, A. G., Klochkov, V. K., Mateychenko, P. V., Parkhomenko, S. V., & Fedorov, O. G. (2017). Influence of Ca and Mg doping on the microstructure and optical properties of YAG ceramics. Functional Materials. 24(2), 237-243.DOI

Paper details

vlnc:W_dchvv8y6
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents