WorksPhysics and Astronomy

HPHT growth of centimeter-sized cubic boron nitride crystals

Abstract

Single crystals of cubic boron nitride (cBN) exceeding 10 mm in size were grown by the high-pressure high-temperature (HPHT) temperature-gradient method using a Ni-Cr-based solvent catalyst. Compared with the previously reported maximum crystal size of approximately 3 mm, this improvement was achieved by maintaining a stable precursor flux during one week of growth at a source temperature of 1950 °C. In contrast to diamonds, which were grown with the same HPHT cell and showed nearly isometric shapes, the cBN crystals had elongated shapes. We attribute this cBN morphology to a localized growth near the BN source due to the relatively low effective diffusivity of boron and nitrogen species in the metallic solvent.

Introduction

Cubic boron nitride (cBN) is the closest rival of diamond in applications that require extreme hardness, high thermal conductivity and thermal stability, wide optical transparency down to deep ultraviolet range, and low dielectric constant. Such applications include windows for synchrotrons and high-power lasers, heat spreaders, and ultraviolet optoelectronic devices. Compared with diamond, cBN has slightly lower hardness and thermal conductivity and a somewhat higher refractive index, but it possesses a wider bandgap (see Table 1 [1, 2, 3]) and substantially higher oxidation resistance. Whereas bulk diamond begins to oxidize in air at approximately 800 °C, cBN remains stable above 1400 °C. [4].

Materialaa (nm)nnEgE_\mathrm{g} (eV)KK (GPa)Knoop (GPa)κ\kappa (W/m·K)
cBN0.36172.16.240050-80740
Diamond0.35672.45.544057-104600-2000

Table 1. Comparison of basic properties of c-BN and diamond [1, 2, 3, 4]: lattice constant aa, refractive index nn, band gap EgE_\mathrm{g}, bulk modulus KK, Knoop hardness, and thermal conductivity κ\kappa.

Most of the applications mentioned above, especially those related to windows, require high-quality bulk single crystals, which can only be synthesized by the high-pressure high-temperature (HPHT) technique. Since the first report on the HPHT growth of cBN crystals with the maximum size reaching 0.3 mm in 1957 [5], only a ten-fold size increase has been achieved thus far [6], which is by far insufficient for applications. Crystal quality also remained limited, as indicated by relatively broad Raman lines, with the best reported values of 3-4 cm−1^{-1} [7].

During the same period, HPHT diamond synthesis advanced to single crystals exceeding 28 mm in size [8], with Raman linewidths routinely reaching the intrinsic limit of approximately 1.5 cm−1^{-1} in large crystals [9].

Several difficulties were mentioned in growing large cBN crystals. One was handling of the solvent catalyst, which typically contained an alkali or alkali earth metal and hence required handling in a dry inert atmosphere [10, 11, 12]. This issue was resolved by using an alkali-free Ni-based solvent, yet spontaneous secondary nucleation resulted in interaction among nearby crystallites and formation of irregular morphologies. This limited the synthesis time to ca. 3 hours at 1300–1700 °C in previous studies [11, 12]. Finally, a higher temperature is required to convert hexagonal BN (hBN) into cBN as compared to the graphite-diamond transition (see Figure 1). This difference originates from a higher activation energy for the conversion, and thus slower growth rates for cBN [5]. Due to the interaction among growing crystals and difficulties in maintaining relatively high temperatures and pressures, in the past experiments, either the duration was too short or the temperature was too low for growing crystals larger than 3 mm [11].

Phase diagram for the hBN-cBN and graphite-diamond conversions

Figure 1. Phase diagram for the hBN-cBN (gray line) and graphite-diamond conversion (black line); colored areas with temperature are indicated by colored arrows [5]. Top photographs show representative morphologies for large diamond and cBN crystals: isometric for diamond and elongated for cBN. Symbols summarize the maximum pressure-temperature-duration parameters reported in the literature [7, 10, 13, 14, 15]. The red dot corresponds to this work.

In this work, we optimized the HPHT cell geometry and solvent-catalyst composition and maintained stable growth for up to 168 h at 1950 °C. These improvements enabled the growth of cBN single crystals with a size exceeding 10 mm and a Raman linewidth as low as 1.8 cm−1^{-1} (see Figure 2)

Luminescence and Raman spectra of best cBN crystal

Figure 2. Luminescence and Raman spectra of best cBN crystal synthesized in this work, measured under 633, 532 and 355 nm excitation. Inset shows a photograph of the largest crystal.

Experimental details

Diamond and cBN crystals were synthesized at 6.5–7.0 GPa using the temperature gradient HPHT method and a cubic 6-anvil press designed in China. The growth duration was 48-168 hours. Diamond or cBN was used as the seed material. The seed region (see Figure 3a) was heated up to 1600-1900 °C, while the source region was maintained at a higher temperature, producing a vertical temperature gradient of 1-5 °C/mm. Heat losses through the pressure medium and cell walls also produced a radial temperature gradient of approximately 3–12 °C/mm. Low gradient resulted in lack of growth (see center-left region in Figure 3c), and hence the gradient distribution was carefully adjusted via the HPHT cell design to yield crystal nucleation on all seeds.

Schematic and photographs of the HPHT growth

Figure 3. a) Schematic of the HPHT growth. b-d) Photographs of the solvent with diamond (b) and cBN crystals (c-d). Small seed crystals can be discerned on some crystals. In c) the thermal gradient was low near the center resulting in lack of nucleation, while the shift of the symmetry axis from center to the left resulted from overheating of the left side of the cell that reduced the temperature gradient in the left part. Red arrows indicate the directions of lateral thermal gradients.

High-purity (<0.30% oxygen) hexagonal boron nitride was used as the BN source. During the growth, it was dissolved in a Ni-based solvent-catalyst based on a Ni–Cr alloy (20-30 wt% Cr) with minor additions of Mg, Ti, Al, Si, or their combinations. The last four elements comprised less than 10 wt%; they acted as getters of oxygen, which is known to impart yellow color to cBN [16]. For diamond growth, we used a high-purity graphite source and a Fe-Co (65-35 wt%) catalyst. The source, solvent and growth zone were arranged in a geometry designed to maintain continuous liquid transport while reducing direct contact of the source with the region of crystal growth. The HPHT cell was primarily constructed from CsCl and phase-stabilized ZrO2_2, selected for their mechanical and thermal stability under the applied conditions.

The as-grown crystals were thoroughly cleaned using nitric acid, aqua regia and distilled water. Their phase composition was evaluated by Raman spectroscopy and X-ray diffraction. Their optical properties were reported elsewhere [16] and are partly shown in Figure 2 and Figure 4. Raman spectra were acquired with a WITec alpha 300R setup under 355, 532, or 632 nm excitation. For Brillouin spectroscopy we employed a TFP-2 spectrometer (JRS Scientific) equipped with a tandem 3+3 pass Fabry-Perot interferometer and a 532 nm laser. Fourier-transform infrared (FTIR) absorption spectra were recorded with a Vertex70v spectrometer from Bruker. Measurements were performed in vacuum to avoid atmospheric instabilities. For XRD we used a Rigaku MiniFlex 600 diffractometer and Ni-filtered CuKα radiation. All measurements were performed at ambient temperature.

Characteristic room-temperature spectra of reported cBN crystals

Figure 4. Characteristic room-temperature spectra of reported cBN crystals: a) XRD, b) Brillouin, c) UV-visible and d) FTIR – experimental spectrum and calculated spectrum from ref. [17].

Results and discussion

The inset photographs in Figure 1 show characteristic morphologies observed in this work: isometric for diamond and elongated for cBN. Both materials exhibited well-defined facets and sharp Raman peaks, with a full width at half maximum (FWHM) of 1.6 cm−1^{-1} for diamond and 1.8 cm−1^{-1} for cBN.

No additional phases were detected in cBN by Raman, XRD, Brillouin and FTIR spectroscopies as shown in Figure 2 and Figure 4: Raman spectra of Figure 2 reveal peaks at 1055 and 1305 cm−1^{-1} associated with the transverse optical (TO) and longitudinal optical (LO) modes of cBN. Luminescence is negligible under 355, 532 or 633 nm excitation, except for the dislocation-related [16] blue band excited at 355 nm.

The XRD pattern of Figure 4a consists of a single peak at 50.45° associated with (200) crystal planes. Its FWHM = 0.1° is rather narrow and is limited by the instrumental resolution.

The Brillouin spectrum of Figure 4b shows two peaks at 81 and 136 GHz corresponding to transverse acoustic (TA) and longitudinal acoustic (LA) modes of a (111)-oriented cBN crystal. Within the experimental accuracies, their position matches those reported for high-quality cBN crystals grown at the National Institute of Materials Science in Japan. The resulting longitudinal sound velocity of 17.1 km/s is consistent with previous results and is only slightly below that of diamond (~17.5–18.6 km/s) [18].

UV-visible optical absorption spectra shown in Figure 4c reveal a sharp onset near 200 nm, which corresponds to the bandgap absorption in cBN, together with oxygen-related broadband absorption that imparts most cBN crystals with yellow, amber or brown color [16]. Gettering of oxygen during the growth can yield colorless cBN crystals.

FTIR absorption (Figure 4d) reveals an intrinsic two-phonon spectrum of cBN that matches rather well to the calculation results of reference [17]. No significant infrared-active impurities such as C–O, C=O, N-H or C-H could be detected.

To quantify the elongated shape of cBN crystals, in Figure 5 we plotted the aspect ratio, namely the ratio of the longest and shortest dimensions (length/width), as a function of crystal length. The aspect ratio quickly increases with crystal size for cBN, but not for diamond. Meanwhile, Figure 3c demonstrates that the long axis of the cBN crystals is oriented approximately perpendicular to the vertical axis of the HPHT cell.

Aspect ratio of cBN and diamond crystals as a function of crystal length

Figure 5. Aspect ratio for cBN and diamond crystals grown in the same HPHT setup. Inset shows photographs of two cBN samples with indicated length.

We tentatively explain this unusual cBN orientation as follows. At the high temperatures of HPHT synthesis, boron readily reacts with the components of the solvent, namely Ni, Cr, Ti and Al, while Ti and Al also readily react with nitrogen [19]. These reactions should limit effective mass transport of boron-, and possibly nitrogen-containing species in the solvent, resulting in BN accumulation near the source. Consequently, lateral flow of the source material produced by the unavoidable lateral temperature gradients may become comparable to or even exceed the vertical flow. The situation is different for diamond because of negligible reactivity of carbon with the Fe-Co solvent [19] and hence its faster vertical diffusion.

The observed elongation could in principle originate from either anisotropic crystal-growth kinetics or anisotropic mass transport. The fact that the morphology changes systematically with crystal size and that pronounced elongation occurs despite the use of a nominally symmetric cell suggests that transport limitations may play an important role; nevertheless, distinguishing transport from intrinsic facet-dependent growth kinetics requires further experiments.

Conclusions

We succeeded in growing high-quality single crystals of cubic boron nitride with a size exceeding 10 mm and Raman linewidth as narrow as 1.8 cm−11.8\ \mathrm{cm}^{-1}. This was achieved by optimizing the HPHT cell geometry and the composition of the solvent-catalyst, avoiding the use of moisture-sensitive alkali-based alloys. The crystals exhibited pronounced elongation, which we tentatively attribute to limited effective mass transport of boron- and nitrogen-containing growth species through the metallic solvent. Future work will focus on developing solvent systems with lower chemical affinity for these elements in order to promote faster and more isotropic crystal growth.

Acknowledgments

CzechNanoLab project LM2023051 funded by MEYS CR is gratefully acknowledged for the financial support of the measurements at CEITEC Nano Research Infrastructure. K.I. Is grateful to Jakub Krčma and Michal Urbánek for help with Brillouin measurements.

References

  1. [1]A. Tararan, S. di Sabatino, M. Gatti, T. Taniguchi, K. Watanabe, L. Reining, L. H. G. Tizei1, M. Kociak, and A. Zobelli, Optical gap and optically active intragap defects in cubic BN, Phys. Rev. B 98 (2018) 094106, https://doi.org/10.1103/PhysRevB.98.094106
  2. [2]Haynes, William M., ed. (2016), CRC Handbook of Chemistry and Physics (97th ed.), CRC Press, ISBN 9781488754293 6-155
  3. [3]G. Leichtfried et al. (2002). "13.5 Properties of synthetic diamond and cubic boron nitride". In P. Beiss; et al. (eds.). Landolt-Börnstein – Group VIII Advanced Materials and Technologies: Powder Metallurgy Data. Refractory, Hard and Intermetallic Materials. Landolt-Börnstein - Group VIII Advanced Materials and Technologies. Vol. 2A2. Berlin: Springer. pp. 118–139. doi:10.1007/b83029. ISBN 978-3-540-42961-6
  4. [4]L. Vel, G. Demazeau, J. Etourneau, Cubic boron nitride: synthesis, physicochemical properties and applications, Mater. Sci. Eng. B 10 (1991) 149, https://doi.org/10.1016/0921-5107(91)20121-B
  5. [5]R. H. Wentorf, Cubic Form of Boron Nitride, J. Chem. Phys. 26 (1957) 956, https://doi.org/10.1063/1.1745964
  6. [6]T. Taniguchi, High-Pressure Synthesis of Polymorphic form of Boron Nitride Crystals and Their Impurity Control, Journal of the Society of Materials Science, 67 (2018) 508, https://doi.org/10.2472/jsms.67.508
  7. [7]T. Taniguchi, S. Yamaoka, Spontaneous nucleation of cubic boron nitride single crystal by temperature gradient method under high pressure, J. Cryst. Growth 222 (2001) 549, https://doi.org/10.1016/S0022-0248(00)00907-6
  8. [8]U. F. S. D’Haenens-Johansson, J. E. Butler, A. N. Katrusha, Synthesis of Diamonds and Their Identification, Reviews in Mineralogy & Geochemistry 88 (2022) 689, https://doi.org/10.2138/rmg.2022.88.13
  9. [9]N. V. Surovtsev, I. N. Kurachenkov, Effect of Nitrogen Impurities on the Raman Line Width in Diamond, Revisited, Crystals 7 (2017) 239, https://doi.org/10.3390/cryst7080239
  10. [10]T. Taniguchi, K. Watanabe, Synthesis of high-purity boron nitride single crystals under high pressure by using Ba–BN solvent, J. Cryst. Growth 303 (2007) 525, https://doi.org/10.1016/j.jcrysgro.12.061
  11. [11]Y. Kubota and T. Taniguchi, Synthesis of Cubic Boron Nitride Crystals Using Ni–Cr and Ni–Cr–Al Solvents under High Pressure, Japanese J. Appl. Phys. 48 (2009) 071004, https://doi.org/10.1143/JJAP.48.071004
  12. [12]Y. Kubota and T. Taniguchi, Synthesis of Cubic Boron Nitride Using Ni–Mo Alloy as a Solvent, Japanese J. Appl. Phys. 47 (2008) 8375, https://doi.org/10.1143/JJAP.47.8375
  13. [13]T. Taniguchi, S. Yamaoka, Growth of cubic boron nitride single crystal under high pressure using temperature gradient method, Rev. High Press. Sci. and Techn. 7, (1998) 980, https://doi.org/10.4131/jshpreview.7.980
  14. [14]M. Kagami, H. Kanada, M. Akaishi, A. Nukui, T. Osawa, S. Yamaoka, Crystal growth of cubic boron nitride using Li₃BN₂ solvent under high temperature and pressure, J. Cryst. Growth 94 (1989) 261, https://doi.org/10.1016/0022-0248(89)90624-6
  15. [15]O. Mishima, S. Yamaoka, O. Fukunaga, Crystal growth of cubic boron nitride by temperature difference method at ~55 kbar and ~1800 °C, J. Appl. Phys. 61 (1987) 2822, https://doi.org/10.1063/1.338774
  16. [16]K. Iakoubovskii, A. Katrusha, W. Peng, J. Peng, Optical centers in cubic boron nitride and diamond: remarkable similarities, Diam. Relat. Mater. 169 (2026) 114127, ArXiv 2608.03901, https://doi.org/10.1016/j.diamond.2026.114127
  17. [17]O. Kutsay, C. Yan, Y.M. Chong, Q. Ye, I. Bello, W.J. Zhang, J.A. Zapien, Z.F. Zhou, Y.K. Li, V. Garashchenko, A.G. Gontar, N.V. Novikov, S.T. Lee, Studying cubic boron nitride by Raman and infrared spectroscopies, Diam. Relat. Mater. 19 (2010) 968, http://dx.doi.org/10.1016/j.diamond.2010.02.033
  18. [18]J. S. Zhang, J. D. Bass, T. Taniguchi, A. F. Goncharov, Y.-Y. Chang, S. D. Jacobsen, Elasticity of cubic boron nitride under ambient conditions, J. Appl. Phys. 109 (2011) 063521, https://doi.org/10.1063/1.3561496
  19. [19]I. Barin, Thermochemical data of pure substances, Wiley, 1989, ISBN 089573866X.

Paper details

vlnc:W_df6pjxr2
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 1

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents