Antisymmetric interlayer exchange coupling spontaneously built in synthetic antiferromagnetic structure by film growth

Abstract

The antisymmetric-type long-range exchange interaction between two ferromagnetic layers through a nonmagnetic layer, called antisymmetric interlayer exchange coupling (AIEC), has recently been discovered and attracted much attention. This paper reports that the AIEC is naturally built in synthetic antiferromagnets depending on the thin film growth condition. For the synthetic antiferromagnets consisting of Pt/Co/Ir/Co/Pt layers, two kinds of film growth parameters are examined: the effects of epitaxial growth and oblique incident of sputter-deposition. The present results indicate that the spatial fluctuations in thicknesses are one of the major sources inducing the AIEC while the epitaxial growth, which leads to the sharp interfaces and the uniformity in layer thicknesses, effectively suppresses the unexpected AIEC. In addition, the oblique sputter-deposition provides the large AIEC and the anisotropic distribution of AIEC direction in the case of textured films. The findings in this study provide key factors for designing the AIEC and is useful to develop emerging computing technologies with artificial three-dimensional topological magnetic structures.

Introduction

Long-range exchange interaction between ferromagnetic layers separated by a nonmagnetic layer, which is called the interlayer exchange coupling (IEC), leads to the antiparallel alignment of magnetization vectors for the adjacent ferromagnetic layers [1, 2, 3, 4]. The artificial antiferromagnetic spin structure is well known as a synthetic antiferromagnet (SyAF), and is a vital component for the contemporary spintronic applications such as magnetic random access memories because the antiparallel alignment of magnetization vectors reduces the stray magnetic field from the memory cell and at the same time makes the memory cell insensitive to external magnetic field disturbance. In addition to the practical applications, the SyAFs have recently attracted renewed interest as an academic subject in the research field of antiferromagnetic spintronics. Antiferromagnetic spintronics [5, 6] exploits the characteristics of antiferromagnet: low magnetic susceptibility, lack of stray magnetic field, and high frequency dynamics coming from the antiferromagnetic resonance. These characteristics will allow us to develop next-generation spintronic applications with higher storage density and faster operation speed than the conventional ferromagnet-based spintronic applications. Although most works were done for bulk antiferromagnets such as CuMnAs [7, 8] and NiO [9, 10], considering that one carries out the systematic investigation, e.g., interplay between the antiferromagnetic spin structure and the conduction electron spin, a SyAF is favorable because the magnetic anisotropy and exchange coupling constants for the SyAF can be controlled by tuning the layer thicknesses and the well-defined magnetization alignments and domain structures can be exploited [11, 12, 13, 14, 15].

The IEC was discovered by Peter Grünberg and co-workers in 1986 for the ferromagnetic Fe layers separated by the non-ferromagnetic Cr layers [1]. The exchange energy of IEC is given by E=−J(m1⋅m2)E=-J(\mathbf{m}_1 \cdot\mathbf{m}_2), where m1\mathbf{m}_1 and m2\mathbf{m}_2 represent the magnetization vectors of two FM layers. The sign of the exchange coupling constant JJ determines whether m1\mathbf{m}_1 and m2\mathbf{m}_2 are coupled ferromagnetically or antiferromagnetically. After the discovery of IEC, many researchers have studied the IEC in various combinations of ferromagnets and nonmagnets [3, 4]. The recent studies on antiferromagnetic spintronics discovered the antisymmetric type of long-range exchange interaction in the SyAFs, called antisymmetric IEC (AIEC) [16, 17, 18]. The AIEC emerges in the SyAFs with in-plane spatial inversion symmetry breaking. The AIEC energy is expressed as DAIEC⋅(m1×m2)\mathbf{D}_{\mathrm{AIEC}} \cdot(\mathbf{m}_1 \times\mathbf{m}_2), where DAIEC\mathbf{D}_{\mathrm{AIEC}} is the AIEC vector determined by system symmetry. In the Cartesian coordinate system, given that m1\mathbf{m}_1 and m2\mathbf{m}_2 pointing in the zz direction are coupled via the IEC and the inversion symmetry is broken along the yy direction, one may anticipate the existence of DAIEC\mathbf{D}_{\mathrm{AIEC}} along the xx direction. As a result, the noncolinear magnetization alignment between m1\mathbf{m}_1 and m2\mathbf{m}_2 appears.

Chiral magnetic structures due to the AIEC will be a building block of artificial three-dimensional topological magnetic structures and have potential use for emerging computing technologies [19, 20, 21]. For some spintronic applications utilizing only the collinear magnetization alignments, on the other hand, such a chiral magnetic structure is an obstacle for stable device operation. These points suggest the significance of controllability of AIEC in the SyAF. Although there are several reports on the observation of AIEC [22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32] and its application to the magnetization switching technique based on the spin-orbit interaction, that is spin-orbit torque magnetization switching [24, 25, 28, 29, 31, 32], the origin of in-plane spatial inversion symmetry breaking has not been obvious for most studies and the control of DAIEC\mathbf{D}_{\mathrm{AIEC}} has not fully been achieved. Our previous work [23] utilized the wedge-shaped ferromagnetic Co and nonmagnetic Ir layers in the perpendicularly magnetized Pt/Co/Ir/Co/Pt structures, and expected that the wedge shapes provide the in-plane spatial inversion symmetry breaking along the slope directions. Although we concluded that the insertion of wedge-shaped layers is effective to enhance the magnitude of AIEC, the DAIEC\mathbf{D}_{\mathrm{AIEC}} showed the different direction for that expected from the slope directions. These experimental facts imply that there are other sources inducing the finite AIEC.

This idea was also supported by the fact of the small but non-negligible AIEC even for the non-wedged samples [23]. Another research group also has pointed out the difficulty in controlling the direction of DAIEC\mathbf{D}_{\mathrm{AIEC}} [22]. Thus, the clarification of source for the AIEC without a wedge-shaped layer insertion is inevitable for improving the controllability of AIEC and further enhancing the magnitude of AIEC.

This paper reports the experimental investigation of the AIEC naturally built in Pt/Co/Ir/Co/Pt structures by thin film growth. Two kinds of thin film growth parameters are examined. One is whether the layers are epitaxially grown or not. The Pt/Co/Ir/Co/Pt layers were grown on different substrates: an Al2_2O3_3 (0001) single crystal substrate and a thermally-oxidized Si (Si-O) substrate. The other is the effect of oblique incidence of sputtered atoms to the substrate. The thin film growth was carried out with or without the substrate rotation. The magnitude and direction of AIEC are investigated using four kinds of samples, and the contribution of thin film growth condition to the AIEC is discussed. Based on the key factors for enhancing or suppressing the AIEC, large AIEC is demonstrated.

Experimental Procedure

As schematically illustrated in Figure 1(a), the common layer stacking among the samples is Pt (4.5)/Co (tCot_{\mathrm{Co}})/Ir (tIrt_{\mathrm{Ir}})/Co (0.5)/Pt (2.7) (in nanometer). The thin films were prepared on Al2_2O3_3 (0001) single crystal substrates or Si-O substrates using a magnetron sputtering system with the base pressure of ∼2×10−5\sim2 \times10^{-5} Pa. The magnetron sputtering system is equipped with three sputtering cathodes. The cathode #1 has a revolving target changer with Ta and Pt sputtering targets, and Ta or Pt is sputter-deposited at the incident angle of 0∘0^\circ, that is normal to the substrate surface. The cathode #2 and the cathode #3 have Co and Ir sputtering targets, respectively, and the incident angles are set to be 45° as illustrated in Figure 1(b).

Schematic illustrations of layer stackings, sputtering configuration, Hall effect device, and thickness variation

Figure 1. Schematic illustrations of (a) layer stackings on Si-O substrate and Al2_2O3_3 (0001) single crystal substrate, and (b) configuration of substrate and sputtering cathode for Co target. (c) Optical image of the device together with the terminal configuration for the Hall effect measurement. The definition of in-plane magnetic field angle ϕ\phi is also shown. (d) The thickness variation as a function of position in the 10 mm ×\times 10 mm substrate.

For the samples on the Si-O substrates, which are labelled Sample A, the 2 nm-thick Ta buffer layer was deposited before the deposition of 4.5 nm-thick bottom Pt layer. All the layers were deposited at room temperature (RT). In contrast to Sample A, the samples on the Al2O3\mathrm{Al}_{2}\mathrm{O}_{3} (0001) single crystal substrates, which are labelled Sample B, do not involve the Ta buffer layer. Instead of insertion of Ta buffer layer, the 4.5 nm-thick bottom Pt layer was deposited at 300°C, and the other layers were deposited at RT.

In order to examine the effect of oblique incidence of sputtered atoms to the substrate, Sample A and Sample B were deposited with or without the substrate rotation. For the samples deposited with the substrate rotation, which are called Sample A-w and Sample B-w, we expect that the effect of oblique incidence is averaged out and disappears. On the other hand, for the samples deposited without the substrate rotation, the substrate rotation was stopped only during the deposition of Co layers and the side of substrate was aligned to the incident direction of sputtered atoms as shown in Figure 1(b). These samples without the substrate rotation are labelled Sample A-w/o and Sample B-w/o. Since one may think the oblique incidence gives rise to the gradient of layer thickness, prior to the thin film preparation, the position dependence of film thickness was measured for the sample deposited without the substrate rotation on the Si-O substrate with the size of 10 mm × 10 mm. The thickness variation as a function of position in the 10 mm × 10 mm substrate is plotted in Figure 1d. The oblique incidence does not induce the clear thickness gradient.

The thin films were patterned into a Hall-bar shape using photolithography and Ar-ion milling. In this study, the devices with different channel widths dd were fabricated, where d=5d = 5, 10 and 20 μ\mum. Figure 1(c) displays the optical image of the device with d=10d = 10 μ\mum together with the terminal configuration for the Hall effect measurement. The electrical contact pads of Cr (20 nm)/Au (200 nm) were fabricated using photolithography and ion-beam sputtering. The longitudinal direction of the channel was designed to coincide with the in-plane projection component of the oblique incidence. In order to evaluate the AIEC, the additional in-plane magnetic field HipH_{\mathrm{ip}} was applied under the sweep of out-of-plane magnetic field HzH_z [18, 23]. The definition of in-plane magnetic field angle ϕ\phi is also shown in Figure 1(c). ϕ=0∘\phi= 0^{\circ} corresponds to the longitudinal direction of the channel, that is the same direction as the in-plane projection component of the oblique incidence.

The structural characterization was carried out using reflection high-energy electron diffraction (RHEED) and scanning transmission electron microscopy (STEM) with energy dispersive x-ray spectroscopy (EDS). Magnetic hysteresis loops were measured using the polar magneto-optical Kerr effect (MOKE). The Hall effect was measured employing the physical properties measurement system with the maximum field of 9 T, and the probe station with a magnet which produces a magnetic field in any direction. All the measurements were performed at RT.

Results and Discussion

Structural Characterization

Figure 2 displays the RHEED patterns for the bottom Pt, the bottom Co, the Ir and the top Co layers of (a) Sample A on Si-O and (b) Sample B on Al2_2O3_3 (0001). tCot_{\mathrm{Co}} was 0.9 nm for both samples whereas tIrt_{\mathrm{Ir}} was 0.5 nm for Sample A and 0.7 nm for Sample B. Sample A exhibits diffusive streaks overlapped with thin arcs. During the RHEED observation, these patterns do not vary with changing the direction of observation (incident angle of electron beam), which indicates that Sample A has a texture structure. On the other hand, Sample B shows the clear streaks for all the layers than those for Sample A, and the patterns vary by changing the direction of observation.

These results indicate that Sample B was epitaxially grown on the Al2O3\mathrm{Al_2O_3} (0001) single crystal substrate. Compared with the previous structural analysis for the Co/Ir/Co stacks grown on the Al2O3\mathrm{Al_2O_3} (0001) [33], Sample A is the (111)-oriented texture film and Sample B is the (111)-oriented epitaxial film.

The cross-sectional high-angle annular dark-field (HAADF)-STEM images and STEM-EDS elemental maps for Sample A and Sample B are given in Figure 3, where tCot_{\mathrm{Co}} and tIrt_{\mathrm{Ir}} were 0.9 nm and 0.7 nm, respectively, for both samples. These samples were deposited with the substrate rotation. One can see the clear layered structures for both Sample A and Sample B. Particularly, even 0.5 nm-thick Co layers form the continuous morphologies. Remarkable differences between these samples are that the well-ordered atomic arrangement is observed for Sample B thanks to the epitaxial growth and that Sample B possesses the sharper interfaces than Sample A. It is noted that there are non-negligible spatial fluctuations in thicknesses for both Sample A and Sample B.

Cross-sectional HAADF-STEM images and STEM-EDS elemental maps for Samples A and B

Figure 3. Cross-sectional high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) images and STEM-energy-dispersive x-ray spectroscopy (EDS) elemental maps for Sample A on Si-O and [(a) and (b)] and Sample B on Al2_2O3_3 (0001) [(c) and (d)].

Hall loops and magneto-optical Kerr effect loops

Figure 4 shows the transverse resistance RxyR_{xy} as a function of HzH_z for (a) Sample A-w, (b) Sample A-w/o, (c) Sample B-w, and (d) Sample B-w/o, where tCot_{\mathrm{Co}} and tIrt_{\mathrm{Ir}} are 1.3 nm and 0.5 nm, respectively, for all the samples. These Hall loops were measured with the magnetic field applied in the range of −9 T≤μ0Hz≤9 T-9\ \mathrm{T} \leq\mu_0 H_z \leq9\ \mathrm{T}. The additional HipH_{\mathrm{ip}} was not applied. The insets of Figure 4 are the polar MOKE loops measured in the magnetic field range of −2 T≤μ0Hz≤2 T-2\ \mathrm{T} \leq\mu_0 H_z \leq2\ \mathrm{T}. From the comparison between the Hall loops and the polar MOKE loops, it is confirmed that the anomalous Hall effect (AHE) proportional to the perpendicular component of net magnetization of two Co layers is the dominant in RxyR_{xy}. Also, both Hall loops and polar MOKE loops indicate that the two Co magnetizations are antiferromagnetically aligned for all the samples at low HzH_z. Since tIr=0.5t_{\mathrm{Ir}} = 0.5 nm is the first peak of JJ for the Co/Ir/Co systems and the strong antiferromagnetic coupling is achieved [14, 33], even the application of μ0Hz=9\mu_0 H_z = 9 T is not sufficient to align the Co magnetization vectors in parallel. Thus, the Hall loops for all the samples are not saturated in the field range of −9-9 T ≤μ0Hz≤9\le\mu_0 H_z \le9 T. Since the similar Hall loops were obtained for all four samples, all four samples possess the comparable strength of antiferromagnetic coupling.

Transverse resistance $R_{xy}$ as a function of $H_z$ for Samples A-w, A-w/o, B-w, and B-w/o

Figure 4. Transverse resistance RxyR_{xy} as a function of HzH_z for (a) Sample A-w, (b) Sample A-w/o, (c) Sample B-w, and (d) Sample B-w/o, where tCot_{\mathrm{Co}} and tIrt_{\mathrm{Ir}} are 1.3 nm and 0.5 nm, respectively. The additional HipH_{\mathrm{ip}} was not applied. The insets are the polar MOKE loops.

Evaluation of antisymmetric interlayer exchange coupling

The magnitude of AIEC is evaluated by measuring the RxyR_{xy} - HzH_z curves with the application of additional HipH_{\mathrm{ip}}. As explained in Figure 1(c), ϕ=0∘\phi= 0^\circ is aligned with the longitudinal direction of the channel, corresponding to the in-plane projection component of the oblique incidence in the cases of Sample A-w/o and Sample B-w/o. Figure 5(a) shows the RxyR_{xy} - HzH_z curves with μ0Hip=50\mu_0 H_{\mathrm{ip}} = 50 mT applied at ϕ=150∘\phi= 150^\circ and 330∘330^\circ for the Hall device of Sample A-w/o with d=20 μmd = 20\ \mu\mathrm{m}. tCot_{\mathrm{Co}} and tIrt_{\mathrm{Ir}} are 1.3 nm and 0.5 nm, respectively. Under the additional HipH_{\mathrm{ip}} application, the presence of AIEC leads to the asymmetry in the up-to-down (UD) and down-to-up (DU) switching fields for the net magnetization because the preferred magnetic chirality is dictated by the AIEC. According to the previous work [18, 23], the application of HipH_{\mathrm{ip}} lifts the degeneracy in the energies of magnetization switching for tail-to-tail and head-to-head configurations of two Co layers, resulting in the asymmetry in the UD and DU switching events. The magnitude of unidirectional shift of RxyR_{xy} - HzH_z curve is related to the magnitude of AIEC. The UD and DU switching fields HswH_{\mathrm{sw}} are obviously different, and the directions of shift in the RxyR_{xy} - HzH_z curves are also different between the cases at ϕ=150∘\phi= 150^\circ and 330∘330^\circ. From the measurement of RxyR_{xy} - HzH_z curve under the HipH_{\mathrm{ip}} application, the values of μ0Hsw\mu_0 H_{\mathrm{sw}} as a function of ϕ\phi are plotted for the UD and DU switching events in Figure 5(b) and Figure 5(c), respectively. The experimental data are numerically fitted with μ0Hsw=μ0Hsw0+μ0Hshiftcos⁡(ϕ−ϕAS)\mu_0 H_{\mathrm{sw}} = \mu_0 H_{\mathrm{sw}}^0 + \mu_0 H_{\mathrm{shift}} \cos(\phi- \phi_{\mathrm{AS}}). μ0Hshift\mu_0 H_{\mathrm{shift}} represents the magnitude of AIEC, and ϕAS\phi_{\mathrm{AS}} is the direction of AIEC, which corresponds to the in-plane direction orthogonal to DAIEC\mathbf{D}_{\mathrm{AIEC}}. μ0Hsw0\mu_0 H_{\mathrm{sw}}^0 is the baseline in the angular dependence of switching field. μ0Hshift=15.4\mu_0 H_{\mathrm{shift}} = 15.4 mT (14.7 mT) and ϕAS=151∘\phi_{\mathrm{AS}} = 151^\circ (153∘^\circ) are evaluated for the UD (DU) switching events for the Hall device of Sample A-w/o with d=20d = 20 μ\mum.

Plots of $R_{xy}$–$H_z$ curves and switching fields

Figure 5. (a) RxyR_{xy} - HzH_z curves with μ0Hip=50\mu_{0}H_{\mathrm{ip}} = 50 mT applied at ϕ=150∘\phi= 150^\circ (cyan) and 330∘330^\circ (magenta) for the Hall device of Sample A-w/o with d=20d = 20 μm. tCot_{\mathrm{Co}} and tIrt_{\mathrm{Ir}} are 1.3 nm and 0.5 nm, respectively. (b) μ0Hsw\mu_{0}H_{\mathrm{sw}} as a function of ϕ\phi for the UD and (c) DU switching events. The black solid circles denote the experimental data while the red curves represent the numerical fit.

Figure 6 summarizes the values of μ0Hshift\mu_0 H_{\mathrm{shift}} and ϕAS\phi_{\mathrm{AS}} plotted as pole figures for the Hall devices of (a) Sample A-w, (b) Sample A-w/o, (c) Sample B-w, and (d) Sample B-w/o, where tCot_{\mathrm{Co}} and tIrt_{\mathrm{Ir}} are 1.3 nm and 0.5 nm, respectively. In order to discuss the statistical trends of HshiftH_{\mathrm{shift}} and ϕAS\phi_{\mathrm{AS}}, many devices fabricated on the identical substrate were measured: 25 devices for Sample A-w, 23 devices for Sample A-w/o, 36 devices for Sample B-w, and 35 devices for Sample B-w/o. Those data points involve both the UD and DU switching events for the Hall devices with d=5d = 5 μ\mum (circles), 10 μ\mum (triangles), and 20 μ\mum (squares).

Discussion

First let us discuss the effect of epitaxial growth on the AIEC from the results for Sample A-w and Sample B-w, which are the (111)-oriented texture film on the Si-O substrate and the (111)-oriented epitaxial film on the Al2_2O3_3 (0001) substrate, respectively. Both samples exhibit non-negligible HshiftH_{\mathrm{shift}}, and the values of μ0Hshift\mu_0 H_{\mathrm{shift}} are randomly distributed with respect to ϕAS\phi_{\mathrm{AS}}. The trend of random distribution is obvious for Sample B-w. In the case of Sample B-w, the maximum μ0Hshift\mu_0 H_{\mathrm{shift}} is 8.5 mT and most data points are less than 5 mT. In addition, no particular ϕAS\phi_{\mathrm{AS}} with large AIEC is observed. Compared to Sample B-w, the result for Sample A-w has more scattered data points. Although many devices exhibit μ0Hshift\mu_0 H_{\mathrm{shift}} less than 5 mT, one device exhibits a large μ0Hshift\mu_0 H_{\mathrm{shift}} close to the 15 mT. Since the films of Sample A-w and Sample B-w were deposited with the substrate rotation, it is natural that any anisotropic properties induced by the film growth process, e.g., effect of oblique incident or induced magnetic anisotropy, are averaged out, and one may anticipate that no AIEC exists if an ideally uniform layer stacking is achieved. However, the present samples are not the case. These experimental results indicate that there exists an unexpected AIEC. One useful finding in this study is that the epitaxial growth is effective to suppress the unexpected AIEC. The HAADF-STEM images shown in Figure 3 suggest that both Sample A-w and Sample B-w involve the spatial fluctuations in thicknesses, and that the fluctuation is more remarkable for Sample A-w. Considering these experimental facts, the thickness fluctuation is one of the possible sources of breaking the in-plane spatial inversion symmetry, leading to the non-negligible AIEC. Compared with the textured film, the epitaxial growth leads to the sharp interfaces and the uniform layer thicknesses, resulting in the smaller magnitude of AIEC for the epitaxial film.

Next, in order to examine the effect of oblique incidence of sputtered atoms to the substrate, we compare the results between Sample A-w and Sample A-w/o. The remarkable anisotropic distribution in HshiftH_{\mathrm{shift}} is observed for Sample A-w/o, which was the textured film deposited without the substrate rotation. The largest μ0Hshift\mu_0H_{\mathrm{shift}} among all four samples is obtained for Sample A-w/o, which is 16.7 mT. Several devices for Sample A-w/o also exhibit the large μ0Hshift\mu_0H_{\mathrm{shift}} close to 15 mT. Although ϕAS\phi_{\mathrm{AS}} for the devices showing large μ0Hshift\mu_0H_{\mathrm{shift}} does not strictly follow the direction of in-plane projection component of the oblique incidence, which is ϕAS=0∘\phi_{\mathrm{AS}} = 0^\circ or 180∘180^\circ, the anisotropic distribution in HshiftH_{\mathrm{shift}} mainly centered around ϕAS=180∘\phi_{\mathrm{AS}} = 180^\circ and the large values of μ0Hshift\mu_0H_{\mathrm{shift}} indicate that the oblique sputter-deposition obviously contributes to the induction of AIEC.

A coupled of previous studies also reported the growth-induced AIEC for CoFeB / Pt / Co [Ref. 24] and [Pt/Co]3/Ru/[Co/Pt]2[\mathrm{Pt}/\mathrm{Co}]_3/\mathrm{Ru}/[\mathrm{Co}/\mathrm{Pt}]_2 [Ref. 31], in which the CoFeB layer and Pt layers, respectively, were grown by the oblique sputter-deposition. Our experimental results for the textured film (Sample A-w/o) are qualitatively consistent with the tendency of the previous studies [24, 31]. However, the control of ϕAS\phi_{\mathrm{AS}} for our case is yet to be enough compared to the previous work [24], which reported the well-controlled ϕAS\phi_{\mathrm{AS}} by oblique deposition. Although the reason for the difference between the present work and the previous ones is not clear at present, since the effect of oblique sputter-deposition is largely affected by the specifications of equipment, e.g., the pressure of process gas (Ar gas in the present study) during deposition, the distance between the substrate and the sputtering target, those technical differences in the sputter-deposition condition might be factors for difference in the controllability of ϕAS\phi_{\mathrm{AS}}. In contrast to the control of ϕAS\phi_{\mathrm{AS}}, the Sample A-w/o exhibit the larger AIEC than the previous study [31]. According to Ref. 31, the interlayer Dzyaloshinskii–Moriya interaction (DMI) effective field HDMIH_{\mathrm{DMI}}, which corresponds to the effective field of AIEC, is evaluated from the equation of (μ0HswUD+μ0HswDU)/2=μ0HDMIcos⁡(ϕ−ϕAS)(\mu_0 H_{\mathrm{sw}}^{\mathrm{UD}} + \mu_0 H_{\mathrm{sw}}^{\mathrm{DU}})/2 = \mu_0 H_{\mathrm{DMI}} \cos(\phi- \phi_{\mathrm{AS}}), where μ0HswUD\mu_0 H_{\mathrm{sw}}^{\mathrm{UD}} and μ0HswDU\mu_0 H_{\mathrm{sw}}^{\mathrm{DU}} are the values of μ0Hsw\mu_0 H_{\mathrm{sw}} for the UD and DU switching events, respectively. For the device of Sample A-w/o shown in Figure 5, μ0HDMI\mu_0 H_{\mathrm{DMI}} is estimated to be 15 mT, which is larger than the previous values [31]. This large μ0HDMI\mu_0 H_{\mathrm{DMI}} is attributable to the large IEC (large saturation field more than 9 T shown in Figure 4) thanks to the Ir spacer layer because there exists the correlation between IEC and AIEC [23, 26, 27].

Another important finding is obtained from the result of Sample B-w/o, which is the epitaxial film deposited without the substrate rotation. Although the distribution of HshiftH_{\mathrm{shift}} for Sample B-w/o is anisotropic in comparison to Sample B-w, the increase in HshiftH_{\mathrm{shift}} is not significant in comparison to the cases of the textured films, i.e., Sample A-w and Sample A-w/o. This implies that the oblique sputter-deposition is not so effective in the case of epitaxial films. This is attributable to the well-ordered atomic arrangement of the epitaxial films, and the epitaxial growth may hinder the preferential crystal growth due to the oblique incidence of sputtered atoms onto the substrate.

One may consider that the existence of edges in the microfabricated Hall devices also affects the evaluation of HshiftH_{\mathrm{shift}} because edges may be possible nucleation sites for reversed magnetic domain. In Figure 6(b) for Sample A-w/o, which possesses the large AIEC, the Hall devices with the widest channel of d=20 μmd = 20\ \mu\mathrm{m} exhibit the most remarkable anisotropic distribution in HshiftH_{\mathrm{shift}}. This experimental fact implies that a Hall device with a wider channel is suitable to clearly observe the AIEC because of suppression of edges effect on the magnetization reversal process. In other words, the optimization of device design may lead to the improvement of the controllability of ϕAS\phi_{\mathrm{AS}} and the further enhancement of AIEC.

Pole figures of $\mu_0 H_{\mathrm{shift}}$ as a function of $\phi_{\mathrm{AS}}$ for Hall devices of Samples A-w, A-w/o, B-w, and B-w/o

Figure 6. Pole figures of μ0Hshift\mu_0 H_{\mathrm{shift}} as a function of ϕAS\phi_{\mathrm{AS}} for the Hall devices of (a) Sample A-w, (b) Sample A-w/o, (c) Sample B-w, and (d) Sample B-w/o, where tCot_{\mathrm{Co}} and tIrt_{\mathrm{Ir}} are 1.3 nm and 0.5 nm, respectively. The data points were obtained from 25 devices for Sample A-w, 23 devices for Sample A-w/o, 36 devices for Sample B-w, and 35 devices for Sample B-w/o. Those data points involve both the UD and DU switching events for the Hall devices with d=5d = 5 µm (circles), 10 µm (triangles), and 20 µm (squares).

The present experimental results and the above discussion allow us to mention key factors for enhancing the AIEC: (i) non-epitaxial growth, (ii) oblique sputter-deposition, and (iii) large IEC. These also provide useful knowledge when one considers applications. As mentioned in the introductory paragraph, the AIEC is available to form chiral magnetic structures and is expected to have potential use for emerging computing technologies. Toward this goal, a textured film structure and the usage of oblique sputtering enable us to induce the large AIEC in SyAFs. On the other hand, for some spintronic applications with the collinear magnetization alignment, an unexpected chiral magnetic structure should be got rid of for the stable device operation. From the viewpoint of such demand, the epitaxial growth of thin films is an effective way to suppress the AIEC.

Summary

We carried out the experimental investigation on the AIEC naturally built in the SyAFs consisting of Pt/Co/Ir/Co/Pt layers by thin film growth. By comparing the results for the textured samples and the epitaxial samples, we conclude that the spatial fluctuations in thicknesses are one of the major sources inducing the AIEC. It was also found that the epitaxial growth is effective in suppressing the unexpected AIEC because of sharp interfaces and the uniform layer thicknesses.

On the other hand, the oblique sputter-deposition provides the large AIEC and the anisotropic distribution of AIEC direction in the case of textured films. These findings are useful not only to develop emerging computing technologies with artificial three-dimensional topological magnetic structures but also to improve the stable operation of conventional spintronic applications.

Acknowledgments

The authors thank R. Umetsu for her help in carrying out a part of the transport measurement, T. Sasaki and T. Endo for their help in doing the film deposition by ion beam sputtering, and S. Ito for his help in observing the scanning transmission electron microscopy images. The device fabrication was partly carried out at the Cooperative Research and Development Center for Advanced Materials, IMR, Tohoku University. This work was supported by JSPS KAKENHI Grant-in-Aid for Scientific Research (A) (JP23H00232).

Reflection high-energy electron diffraction patterns for Samples A and B

Figure 2. (a) Reflection high-energy electron diffraction (RHEED) patterns for the bottom Pt, the bottom Co, the Ir and the top Co layers of (a) Sample A on Si-O and (b) Sample B on Al2_2O3_3 (0001). tCot_{\mathrm{Co}} was 0.9 nm for both samples, and tIrt_{\mathrm{Ir}} was 0.5 nm for Sample A and 0.7 nm for Sample B.

References

  1. [1]P. Grünberg, R. Schreiber, Y. Pang, M. B. Brodsky, and H. Sowers, Phys. Rev. Lett. 57, 2442 (1986).
  2. [2]P. Bruno, and C. Chappert, Phys. Rev. Lett. 67, 1602 (1991).
  3. [3]S. S. P. Parkin, Phys. Rev. Lett. 67, 3598 (1991).
  4. [4]D. E. Bürgler, P. Grünberg, S. O. Demokritov, and M. T. Johnson, “Interlayer Exchange Coupling in Layered Magnetic Structures” in Handbook of Magnetic Materials, volume 13 (ed. K. H. J. Buschow, Elsevier 2001).
  5. [5]V. Baltz, A. Manchon, M. Tsoi, T. Moriyama, T. Ono, and Y. Tserkovnyak, Rev. Mod. Phys. 90, 015005 (2018).
  6. [6]A. Hirohata, D. C. Lloyd, T. Kubota, T. Seki, K. Takanashi, H. Sukegawa, Z. Wen, S. Mitani, and H. Koizumi, IEEE Access 11, 117443 (2023).
  7. [7]P. Wadley, B. Howells, J. Železný, C. Andrews, V. Hills, R. P. Campion, V. Novák, K. Olejník, F. Maccherozzi, S. S. Dhesi, S. Y. Martin, T. Wagner, J. Wunderlich, F. Freimuth, Y. Mokrousov, J. Kuneš, J. S. Chauhan, M. J. Grzybowski, A. W. Rushforth, K. Edmond, B. L. Gallagher, and T. Jungwirth, Science 351, 587 (2016).
  8. [8]S. Y. Bodnar, L. Šmejkal, I. Turek, T. Jungwirth, O. Gomonay, J. Sinova, A. A. Sapozhnik, H. J. Elmers, M. Kläui, and M. Jourdan, Nat. Commun. 9, 348 (2018).
  9. [9]T. Moriyama, K. Oda, T. Ohkochi, M. Kimata, and T. Ono, Sci. Rep. 8, 14167 (2018).
  10. [10]T. Yamazaki, T. Seki, T. Kubota, and K. Takanashi, Appl. Phys. Exp. 16, 083003 (2023).
  11. [11]T. Seki, H. Tomita, T. Shinjo, and Y. Suzuki, Appl. Phys. Lett. 97, 162508 (2010).
  12. [12]S.-H. Yang, K.-S. Ryu, and S. S. P. Parkin, Nat. Nanotech. 10, 221 (2015).
  13. [13]R. A. Duine, K.-J. Lee, S. S. P. Parkin, and M. D. Stiles, Nat. Phys. 14, 217 (2018).
  14. [14]H. Masuda, Y. Yamane, T. Seki, K. Raab, T. Dohi, R. Modak, K. Uchida, J. Ieda, M. Kläui, and K. Takanashi, Appl. Phys. Lett. 122, 162402 (2023).
  15. [15]J. Godinho, P. K. Rout, R. Salikhov, O. Hellwig, Z. Šobán, R. M. Otxoa, K. Olejník, T. Jungwirth, and J. Wunderlich, npj Spintronics 2, 39 (2024).
  16. [16]E. Y. Vedmedenko, P. Riego, J. A. Arregi, and A. Berger, Phys. Rev. Lett. 122, 257202 (2019).
  17. [17]A. Fernández-Pacheco, E. Vedmedenko, D. Petit, and R. P. Cowburn, Nat. Mater. 18, 679 (2019).
  18. [18]D.-S. Han, K. Lee, J.-P. Hanke, Y. Mokrousov, K.-W. Kim, W. Yoo, Y. L. W. van Hees, T.-W. Kim, R. Lavrijsen, C.-Y. You, H. J. M. Swagten, M.-H. Jung, and M. Kläui, Nat. Mater. 18, 703 (2019).
  19. [19]Z. Luo, T. P. Dao, A. Hrabec, J. Vijayakumar, A. Kleibert, M. Baumgartner, E. Kirk, Jizhai Cui, T. Savchenko, G. Krishnaswamy, L. J. Heyderman, and P. Gambardella, Science 363, 1435 (2019).
  20. [20]A. Fernández-Pacheco, R. Streubel, O. Fruchart, R. Hertel, P. Fischer, R. P Cowburn, Nat. Commun. 8, 15756 (2017).
  21. [21]A. Hrabec, Z. Luo, L. J. Heyderman, P. Gambardella, Appl. Phys. Lett. 117, 130503 (2020).
  22. [22]C. O. Avci, C.-H. Lambert, G. Sala, and P. Gambardella, Phys. Rev. Lett. 127, 167202 (2021).
  23. [23]H. Masuda, T. Seki, Y. Yamane, R. Modak, K. Uchida, J. Ieda, Y. C. Lau, S. Fukami, and K. Takanashi, Phys. Rev. Appl. 17, 054036 (2022).
  24. [24]Y.-H. Huang, C.-C. Huang, W.-B. Liao, T.-Y. Chen, and C.-F. Pai, Phys. Rev. Appl. 18, 034046 (2022).
  25. [25]Y.-C. Li, Y.-H. Huang, C.-C. Huang, Y.-T. Liu, and C.-F. Pai, Phys. Rev. Appl. 20, 024032 (2023).
  26. [26]F. S. Gao, S. Q. Liu, R. Zhang, J. H. Xia, W. Q. He, X. H. Li, X. M. Luo, C. H. Wan, G. Q. Yu, G. Su, and X. F. Han, Appl. Phys. Lett. 123, 192401 (2023).
  27. [27]S. Liang, R. Chen, Q. Cui, Y. Zhou, F. Pan, H. Yang, and C. Song, Nano Lett. 23, 8690 (2023).
  28. [28]K. Wang, L. Qian, S.-C. Ying, and G. Xiao, Commun. Phys. 4, 10 (2020).
  29. [29]W. He, C. Wan, C. Zheng, Y. Wang, X. Wang, T. Ma, Y. Wang, C. Guo, X. Luo, M. E. Stebliv, G. Yu, Y. Liu, A. V. Ognev, A. S. Samardak, and X. Han, Nano Lett. 22, 6857 (2022).
  30. [30]F. Kammerbauer, W.-Y. Choi, F. Freimuth, K. Lee, R. Frömter, D.-S. Han, R. Lavrijsen, H. J. M. Swagten, Y. Mokrousov, and M. Kläui, Nano Lett. 23, 7070 (2023).
  31. [31]Y.-H. Huang, J.-H. Han, W.-B. Liao, C.-Y. Hu, Y.-T. Liu, and C.-F. Pai, Nano Lett. 24, 649 (2024).
  32. [32]X. Zhao, H. Sun, R. Han, H. Qin, L. Wen, H. Wang, D. Wei, and J. Zhao, APL Mater. 12, 041103 (2024).
  33. [33]H. Masuda, T. Seki, Y.-C. Lau, T. Kubota, and K. Takanashi, Phys. Rev. B 101, 24413 (2020).

Paper details

vlnc:W_drehudzm
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents