Current-driven transient dynamics of magnetic-octupole domain walls in noncollinear antiferromagnets

Abstract

Current-driven magnetic-octupole domain walls in noncollinear antiferromagnets are promising for fast spintronic devices, yet their transient dynamics are not yet fully understood. Here, we investigate spin-orbit-torque-driven domain-wall motion in Mn3_\text{3}Sn using a multipole micromagnetic framework. The three symmetry-related 60° walls exhibit equivalent current-driven dynamics, unlike their field-driven motion. For a representative 60° wall, the post-pulse motion is governed by relaxation of the current-induced rotation of the surrounding octupole domains, with a characteristic time of approximately 33 ps quantitatively captured by a uniform-domain analytic model. By resolving spatially nonuniform texture dynamics beyond this analytic description, the simulations further reveal an additional slow relaxation in a composite 180° wall associated with the relative motion of its constituent walls. The post-pulse response also varies systematically with the exchange stiffness and magnetic anisotropies. These results identify distinct domain and internal-coordinate relaxation channels and establish the intrinsic time scales governing pulse-controlled positioning of magnetic-octupole domain walls in antiferromagnetic spintronic devices.

Introduction

Current-driven domain-wall motion underpins proposed spintronic architectures for memory, logic, and unconventional computing [1, 2, 3, 4, 5, 6]. Antiferromagnets are attractive because they offer ultrafast dynamics and weak stray fields [7, 8, 9, 10]. However, their small net magnetization makes electrical detection and manipulation challenging. Noncollinear antiferromagnets provide a distinct opportunity because their spin textures can be represented by cluster magnetic multipoles that govern macroscopic responses such as the anomalous Hall, Nernst, magneto-optical Kerr, and spin Hall effects [11, 12, 13, 14, 15]. In Mn3Sn\mathrm{Mn}_3\mathrm{Sn}, the inverse triangular spin structure is described by a cluster magnetic-octupole order parameter, and magnetic domains correspond to different orientations of this octupole moment. Magnetic-octupole domains and domain walls have been detected through Hall and Nernst transport, directly visualized by magneto-optical imaging, and manipulated using magnetic fields and electrical currents [13, 16, 17, 18, 19]. Recent studies have demonstrated experimentally and theoretically that magnetic-octupole domain walls in noncollinear antiferromagnets can exhibit fast current-driven motion, highlighting their potential for electrically controlled antiferromagnetic domain-wall devices [18, 20, 21, 22].

The transient response of a domain wall after a driving force is applied or removed can reveal dynamical memory associated with the relaxation of the wall profile or other coupled degrees of freedom. In conventional ferromagnets, deformation of a moving wall can be described in terms of a Döring-like effective mass, giving rise to finite acceleration and deceleration times [23, 24, 25, 26, 27]; inertial effects have also been predicted to govern switching in antiferromagnets [28]. Using a multipole micromagnetic framework, we recently

showed that field-driven magnetic-octupole domain walls in $\mathrm{Mn}_3\mathrm{Sn}$ deform and acquire a Döring-like effective mass [29]. Current-induced spin-orbit torque, however, acts simultaneously on the wall and the surrounding octupole domains. Previous theoretical work has investigated the SOT-driven dynamics of spatially uniform $\mathrm{Mn}_3\mathrm{Sn}$, including its response to current pulses {citep}[30]`. How these uniform order-parameter dynamics couple to the translational motion of a spatially nonuniform texture, and how additional internal degrees of freedom modify the transient response of a composite wall, remains unresolved.

Here, we investigate the current-driven transient dynamics of magnetic-octupole domain walls in Mn3Sn\mathrm{Mn}_3\mathrm{Sn} using a multipole micromagnetic model. We first show that, unlike field-driven motion, spin-orbit torque produces identical steady-state and transient dynamics for the three symmetry-related types of 60∘60^\circ walls. For a representative 60∘60^\circ wall, a dc current drives steady translational motion, whereas pulse termination produces a finite velocity relaxation and post-pulse displacement. We show that this delayed response is governed by the relaxation of the current-induced rotation of the surrounding octupole domains and that its characteristic time is consistent with the uniform-domain relaxation determined by the damping and sixfold anisotropy. We further show that a 180∘180^\circ wall behaves as a composite object consisting of three coupled 60∘60^\circ walls. Its post-pulse dynamics exhibit a fast domain-relaxation component and an additional slow mode associated with the relative separations among the constituent walls. These results reveal distinct relaxation mechanisms governing the transient motion of current-driven magnetic-octupole domain walls.

Model

We simulate the current-driven dynamics of magnetic-octupole domain walls using the multipole micromagnetic framework developed for Mn3Sn\mathrm{Mn}_3\mathrm{Sn} [29]. In this framework, the noncollinear spin configuration within each magnetic unit cell is represented by a vector-like cluster magnetic-octupole order parameter, g\mathbf{g} Figure 1(a), and the corresponding coarse-grained field G(r,t)\mathbf{G}(\mathbf{r},t) describes spatially varying octupole textures. The dynamics of G\mathbf{G} are calculated using the octupole equation of motion,

Figure 1. Magnetic-octupole domain wall and dc-current-driven motion in Mn3_3Sn. (a) Inverse-triangular spin structure and the corresponding cluster magnetic-octupole order parameter g\mathbf{g}. (b) Representative equilibrium profile of a 60° wall connecting domains with Φoct=+30∘\Phi_{\mathrm{oct}}=+30^\circ and −30∘-30^\circ. (c) Heavy-metal/Mn3_3Sn bilayer geometry, where JhmJ_{\mathrm{hm}} generates a spin current jsj_{\mathrm{s}} with σSOT∥−z^\boldsymbol{\sigma}_{\mathrm{SOT}}\parallel-\hat{\mathbf{z}}. (d) Domain-wall displacement Δq\Delta q under different JhmJ_{\mathrm{hm}}. (e) Steady-state velocity vDW,sv_{\mathrm{DW,s}} as a function of JhmJ_{\mathrm{hm}}.

G˙(r,t)=−γμ0G×Heff,(1)\dot{\mathbf{G}}(\mathbf{r},t)=-\gamma\mu_0\mathbf{G}\times\mathbf{H}_{\mathrm{eff}}, \tag*{(1)}

with an effective field,

Heff=16μ0αmsρ(∂Ec∂Φoct−ℏσSOT,zθSHJhm2ehMn3Sn)z^,(2)\mathbf{H}_{\mathrm{eff}}=\frac{1}{6\mu_0\alpha m_{\mathrm{s}}\rho}\left(\frac{\partial E_{\mathrm{c}}}{\partial\Phi_{\mathrm{oct}}}-\frac{\hbar\sigma_{\mathrm{SOT},z}\theta_{\mathrm{SH}}J_{\mathrm{hm}}}{2eh_{\mathrm{Mn_3Sn}}}\right)\hat{\mathbf{z}}, \tag*{(2)}

where σSOT,z=σSOT⋅z^\sigma_{\mathrm{SOT},z}=\boldsymbol{\sigma}_{\mathrm{SOT}}\cdot\hat{\mathbf{z}} is the out-of-plane component of the spin-polarization direction (σSOT,z=−1\sigma_{\mathrm{SOT},z}=-1 in the present geometry), ρ\rho is the magnetic-unit-cell density, Φoct\Phi_{\mathrm{oct}} is the in-plane orientation of the octupole order, and EcE_{\mathrm{c}} is the coarse-grained octupole energy density containing the exchange and in-plane anisotropy contributions. Here, JhmJ_{\mathrm{hm}} is the in-plane charge-current density in the adjacent heavy-metal layer, and the second term represents the corresponding spin-orbit torque. Note that the Dzyaloshinskii–Moriya contribution is included in the exchange stiffness [29].

Unless otherwise stated, we use the same material parameters as in Ref. [29]: an effective octupole magnetization of G0=6.1×103 A m−1G_0=6.1\times10^3\ \mathrm{A\,m^{-1}}, a sixfold in-plane anisotropy constant of K6=37.5 J m−3K_6=37.5\ \mathrm{J\,m^{-3}}, and exchange stiffness constants of Aex,x=Aex,y=7.3×10−13 J m−1A_{\mathrm{ex},x}=A_{\mathrm{ex},y}=7.3\times10^{-13}\ \mathrm{J\,m^{-1}} and Aex,z=5.6×10−13 J m−1A_{\mathrm{ex},z}=5.6\times10^{-13}\ \mathrm{J\,m^{-1}}. Here K6K_6 denotes the full sixfold anisotropy-barrier height, such that E6=(K6/2)(1+cos⁡6Φoct)E_6=(K_6/2)(1+\cos6\Phi_{\mathrm{oct}}). We use a Gilbert damping constant of α=0.003\alpha=0.003, a sublattice moment of ms=3μBm_{\mathrm{s}}=3\mu_{\mathrm{B}}, and a gyromagnetic ratio of ∣γ∣=1.76×1011 rad s−1 T−1|\gamma|=1.76\times10^{11}\ \mathrm{rad\,s^{-1}\,T^{-1}}. Note that G0G_0 is the effective magnetization associated with the octupole order and is numerically equal to the small net ferromagnetic-moment density. For the spin-orbit-torque-driven simulations, we use a spin Hall angle of θSH=0.1\theta_{\mathrm{SH}}=0.1, a Mn3_3Sn thickness of hMn3Sn=40 nmh_{\mathrm{Mn_3Sn}}=40\ \mathrm{nm}, and a spin polarization σSOT∥−z^\boldsymbol{\sigma}_{\mathrm{SOT}}\parallel-\hat{\mathbf{z}}. The spin-orbit torque is treated as an effective torque averaged over the Mn3_3Sn thickness, representing the net torque transferred to the exchange-coupled magnetic order without explicitly resolving its spatial variation along the film thickness.

Unless otherwise noted, the sixfold anisotropy is the only in-plane anisotropy in Sec. III; the twofold term is introduced only for the composite 180° wall in Secs. IV and V. The simulations are performed on a one-dimensional grid along xx with a cell size of 10×10×10 nm310\times10\times10\ \mathrm{nm^3} and a total length of 20 μm20\ \mathrm{\mu m}, using periodic boundary conditions in the yy- and zz-directions and free boundary conditions along xx. The wall position q(t)q(t) is obtained by linear interpolation of the octupole-angle profile between neighboring cells.

Current-driven motion of a 60° octupole domain wall

We first consider the three symmetry-related types of 60° magnetic-octupole domain walls connecting the +90∘+90^\circ and +30∘+30^\circ, +30∘+30^\circ and −30∘-30^\circ, and −30∘-30^\circ and −90∘-90^\circ domains. Our simulations show that all three walls exhibit identical steady-state and transient dynamics under the present spin-orbit-torque geometry. This equivalence follows from the symmetry of the driving term. Because the spin polarization is normal to the kagome plane, the spin-orbit torque is invariant under the transformation Φoct→Φoct+60∘\Phi_{\mathrm{oct}}\to\Phi_{\mathrm{oct}}+60^\circ, which maps the three wall types onto one another. In contrast, an in-plane magnetic field couples to the absolute orientation of the octupole order and renders the three walls dynamically inequivalent [29]. We therefore focus below on the representative wall between the Φoct=+30∘\Phi_{\mathrm{oct}}=+30^\circ and −30∘-30^\circ domains Figure 1(b). In the heavy-metal/Mn3_3Sn bilayer geometry, an in-plane charge-current density JhmJ_{\mathrm{hm}} generates a transverse spin current jsj_{\mathrm{s}} that is injected into Mn3_3Sn with spin polarization σSOT∥−z^\boldsymbol{\sigma}_{\mathrm{SOT}}\parallel-\hat{\mathbf{z}}. The resulting spin-orbit torque drives the magnetic-octupole domain wall Figure 1(c). The instantaneous wall position q(t)q(t) is defined as the position at which the local octupole angle equals the average orientation of the two surrounding domains,

Φoct[q(t),t]=Φ‾oct(t)=ΦL(t)+ΦR(t)2,(3)\Phi_{\mathrm{oct}}[q(t),t]=\overline{\Phi}_{\mathrm{oct}}(t)=\frac{\Phi_{\mathrm{L}}(t)+\Phi_{\mathrm{R}}(t)}{2}, \tag*{(3)}

where ΦL(t)\Phi_{\mathrm{L}}(t) and ΦR(t)\Phi_{\mathrm{R}}(t) are the octupole angles far from the wall on its left and right sides, respectively. The domain-wall velocity is defined as vDW=dq/dtv_{\mathrm{DW}} = dq/dt.

We first examine the motion of a 60° magnetic-octupole domain wall under a dc current. For all current densities considered, the wall displacement Δq\Delta q increases linearly with time Figure 1(d), demonstrating steady translational motion driven by spin-orbit torque. The slope of Δq(t)\Delta q(t) increases with JhmJ_{\mathrm{hm}}, and the steady-state velocity extracted from the slopes, vDW,sv_{\mathrm{DW,s}}, increases linearly with the applied current density JhmJ_{\mathrm{hm}} Figure 1(e). All current densities considered here lie well below the threshold for continuous octupole rotation, Jc=6ehMn3SnK6/(ℏθSH)≃1.4×1011 A m−2J_{\mathrm{c}} = 6 e h_{\mathrm{Mn_3Sn}} K_6/(\hbar\theta_{\mathrm{SH}}) \simeq1.4 \times10^{11}\ \mathrm{A\,m^{-2}}, so that the surrounding domains remain close to their equilibrium orientations throughout and the wall moves in a steady, nonprecessional regime [29].

Next, we investigate the transient dynamics of the 60° magnetic-octupole domain wall using a rectangular current pulse with a duration of 5 ns. The pulse duration is much longer than the relevant relaxation times, ensuring that the wall reaches its steady-state velocity before pulse termination. Upon pulse termination at toff=5 nst_{\mathrm{off}} = 5\ \mathrm{ns}, the domain-wall velocity decays over a finite time rather than vanishing immediately Figure 2(a). The residual velocity drives continued wall motion after the current is removed, producing a finite post-pulse displacement, Δqpost\Delta q_{\mathrm{post}}.

Figure 2. Transient dynamics of a 60° magnetic-octupole domain wall under pulsed-current excitation. (a) Domain-wall velocity vDW(t)v_{\mathrm{DW}}(t) for a 5-ns current pulse with Jhm=10×109 A m−2J_{\mathrm{hm}} = 10 \times10^9\ \mathrm{A\,m^{-2}}. (b) Post-pulse velocity decay for several current densities, plotted as a function of tt. Solid lines are single-exponential fits, yielding ⟨τv⟩≃32.6 ps\langle\tau_v\rangle\simeq32.6\ \mathrm{ps}. (c) Post-pulse displacement Δqpost\Delta q_{\mathrm{post}} as a function of the velocity at pulse termination. The linear fit yields τq≃32.4 ps\tau_q \simeq32.4\ \mathrm{ps}. (d) Schematic octupole-angle profiles during steady-state motion and after relaxation, illustrating the residual domain rotation and the resulting post-pulse displacement. (e) Domain-wall velocity as a function of the current-induced average rotation of the surrounding domains, ΔΦ‾oct\Delta\overline{\Phi}_{\mathrm{oct}}. Data for different current densities collapse onto a single curve.

The velocity transients following pulse termination are well described by an exponential decay,

vDW(t)=vDW(toff)e−(t−toff)/τv(t≥toff),(4)v_{\mathrm{DW}}(t) = v_{\mathrm{DW}}(t_{\mathrm{off}}) e^{-(t-t_{\mathrm{off}})/\tau_v} \qquad(t \ge t_{\mathrm{off}}), \tag*{(4)}

where tofft_{\mathrm{off}} denotes the pulse-off time and τv\tau_v is the velocity-relaxation time. As shown in Figure 2(b), this form reproduces the post-pulse velocity decay, yielding a characteristic relaxation time of ⟨τv⟩≃32.6 ps\langle\tau_v\rangle\simeq32.6\ \mathrm{ps} that is essentially independent of the applied current density. The same relaxation time governs the onset of the motion: the velocity rise following the leading edge of the pulse, vDW(t)=vDW,s[1−e−t/τv]v_{\mathrm{DW}}(t) = v_{\mathrm{DW,s}}[1-e^{-t/\tau_v}], is the exact mirror of the post-pulse decay of Eq. (4), with the same τv\tau_v within the fitting accuracy. For an exponential decay, the corresponding post-pulse displacement is

Δqpost=∫toff∞vDW(t) dt=τvvDW(toff).(5)\Delta q_{\mathrm{post}} = \int_{t_{\mathrm{off}}}^{\infty} v_{\mathrm{DW}}(t)\,\mathrm{d}t = \tau_v v_{\mathrm{DW}}(t_{\mathrm{off}}). \tag*{(5)}

Consistent with Eq. (5), Δqpost\Delta q_{\mathrm{post}} increases linearly with the velocity at pulse termination Figure 2(c). The slope yields τq≃32.4 ps\tau_q \simeq32.4\ \mathrm{ps}, in excellent agreement with the velocity-relaxation time ⟨τv⟩≃32.6 ps\langle\tau_v\rangle\simeq32.6\ \mathrm{ps} obtained independently from the velocity decay. This agreement provides a consistency check of the single-exponential description and confirms that integration of the residual velocity quantitatively accounts for the observed post-pulse displacement.

To identify the origin of the delayed wall motion, we examine the current-induced rotation of the octupole domains on the two sides of the wall. During current-driven motion, the orientations ΦL(t)\Phi_{\mathrm{L}}(t) and ΦR(t)\Phi_{\mathrm{R}}(t) deviate from their equilibrium values while their angular difference remains fixed at 60° Figure 2(d). The two domains therefore undergo a common rotation rather than changing their relative orientation.

We characterize this collective domain rotation by

ΔΦ‾oct(t)=Φ‾oct(t)−Φ‾oct(0),(6)\Delta\overline{\Phi}_{\mathrm{oct}}(t) = \overline{\Phi}_{\mathrm{oct}}(t) - \overline{\Phi}_{\mathrm{oct}}^{(0)}, \tag*{(6)}

where Φ‾oct(t)\overline{\Phi}_{\mathrm{oct}}(t) is the instantaneous average orientation used in Eq. (3), and Φ‾oct(0)\overline{\Phi}_{\mathrm{oct}}^{(0)} is its equilibrium value. After pulse termination, the residual domain rotation therefore sustains the wall motion until the surrounding domains return to equilibrium, as illustrated in Figure 2(d).

The characteristic relaxation time of the surrounding domains can be obtained analytically from the uniform-octupole equation of motion derived in Ref. [29]. Writing Φ‾oct=Φ‾oct(0)+δΦ\overline{\Phi}_{\mathrm{oct}} = \overline{\Phi}_{\mathrm{oct}}^{(0)} + \delta\Phi and linearizing the sixfold anisotropy about an equilibrium orientation gives an overdamped relaxation, δΦ(t)∝exp⁡(−t/τΦ)\delta\Phi(t) \propto\exp(-t/\tau_{\Phi}), with

τΦ=αmsρ3∣γ∣K6,(7)\tau_{\Phi} = \alpha\frac{m_s\rho}{3|\gamma|K_6}, \tag*{(7)}

where ρ\rho is the magnetic-unit-cell density. For the parameters used here, Eq. (7) gives τΦ≃32.9\tau_{\Phi} \simeq32.9 ps. The velocity-relaxation time of the domain wall, ⟨τv⟩≃32.6\langle\tau_v\rangle\simeq32.6 ps [Fig. 2(b)], agrees with τΦ\tau_{\Phi}. This confirms that the uniform in-plane octupole degree of freedom supports a single relaxational mode within the present reduced model. Equation (7) shows that the relaxation is set entirely by material parameters, τΦ∝α/K6\tau_{\Phi} \propto\alpha/K_6 [31].

This behavior follows directly from a collective-coordinate description of the wall. Writing Φoct(x,t)=Φw[x−q(t)]+ΔΦ‾oct(t)\Phi_{\mathrm{oct}}(x,t)=\Phi_w[x-q(t)]+\overline{\Delta\Phi}_{\mathrm{oct}}(t), where Φw\Phi_w is the equilibrium wall profile, the wall velocity is then set by the instantaneous domain rotation alone,

vDW=3δw2ΔΦ‾octτΦ,(8)v_{\mathrm{DW}}=\frac{3\delta_w}{2}\frac{\overline{\Delta\Phi}_{\mathrm{oct}}}{\tau_{\Phi}}, \tag*{(8)}

where δw=πAex/(3K6)≃146\delta_w=\pi\sqrt{A_{\mathrm{ex}}}/(3\sqrt{K_6})\simeq146 nm is the 60° wall width [29]. Note that all angles in equations are expressed in radians, whereas the figures use degrees.

Equation (8) shows that the instantaneous wall velocity is determined by the rotation of the surrounding domains rather than directly by the applied current. The predicted slope of 116 m s−1^{-1} per degree of domain rotation is in quantitative agreement with Figure 2(e). After pulse termination, the residual domain rotation decays as ΔΦ‾oct(t)=ΔΦ‾oct(toff)exp⁡[−(t−toff)/τΦ]\overline{\Delta\Phi}_{\mathrm{oct}}(t)=\overline{\Delta\Phi}_{\mathrm{oct}}(t_{\mathrm{off}})\exp[-(t-t_{\mathrm{off}})/\tau_{\Phi}]. Combining this relaxation with Eq. (8) and integrating the resulting velocity gives

Δqpost=32δwΔΦ‾oct(toff).(9)\Delta q_{\mathrm{post}}=\frac{3}{2}\delta_w\overline{\Delta\Phi}_{\mathrm{oct}}(t_{\mathrm{off}}). \tag*{(9)}

The explicit relaxation-time dependence therefore cancels. For a given residual domain rotation, the post-pulse displacement is independent of the damping, while the exchange stiffness and sixfold anisotropy enter through the wall width δw\delta_w. Equation (9) predicts approximately 3.8 nm of post-pulse displacement per degree of residual domain rotation, consistent with the product of the independently obtained slopes in Figure 2(c) and Figure 2(e).

Current-driven motion of a 180° octupole domain wall

We next examine the dynamics of a 180° magnetic-octupole domain wall. Owing to the sixfold in-plane anisotropy of Mn3_3Sn, a 180° wall forms a staircase-like structure consisting of three coupled 60° walls [17, 29]. In the absence of magnetostatic energy or an additional anisotropy, however, the relative separations between the constituent walls are not uniquely determined. To stabilize the composite wall structure, we introduce an additional twofold anisotropy along the yy direction, as in our previous work [29],

Eani=K62(1+cos⁡6Φoct)+K22(1+cos⁡2Φoct),(10)E_{\mathrm{ani}}=\frac{K_6}{2}(1+\cos6\Phi_{\mathrm{oct}})+\frac{K_2}{2}(1+\cos2\Phi_{\mathrm{oct}}), \tag*{(10)}

where K6K_6 and K2K_2 denote the sixfold and twofold anisotropy barriers, respectively. We use K2=10K_2=10 J m−3^{-3}, corresponding to approximately 27% of K6=37.5K_6=37.5 J m−3^{-3}. Such a twofold anisotropy can be induced in Mn3_3Sn by in-plane tensile strain [32, 33, 34, 35, 36].

The equilibrium profile of the resulting 180° wall is shown in Figure 3(a). The wall position q(t)q(t) is defined using Eq. (3), with ΦL\Phi_L and ΦR\Phi_R taken from the far-left and far-right domains, respectively. Under a dc current, the composite wall undergoes steady translational motion, and its steady-state velocity vDW,sv_{\mathrm{DW,s}} increases with JhmJ_{\mathrm{hm}} [Fig. 3(b)].

Figure 3. Current-driven dynamics of a 180° magnetic-octupole domain wall. (a) Equilibrium octupole-angle profile of the domain wall, showing the wall position q(t)q(t), the constituent-wall positions x+60(t)x_{+60}(t) and x−60(t)x_{-60}(t), and the internal separations d1d_1 and d2d_2. (b) Steady-state velocity vDW,sv_{\mathrm{DW,s}} as a function of JhmJ_{\mathrm{hm}}. (c) Domain-wall velocity under a 5-ns current pulse with Jhm=10×109J_{\mathrm{hm}}=10\times10^9 A m−2^{-2}. (d) Post-pulse velocity decay fitted by fast and slow exponential components with relaxation times τ1\tau_1 and τ2\tau_2. (e) Current-density dependence of τ1\tau_1 and τ2\tau_2, with average values of approximately 25.8 ps and 225.5 ps, respectively. (f) Post-pulse displacement Δqpost\Delta q_{\mathrm{post}} as a function of vDW(toff)v_{\mathrm{DW}}(t_{\mathrm{off}}). The linear fit yields τq,eff≃51.5\tau_{q,\mathrm{eff}}\simeq51.5 ps.

We next apply a rectangular current pulse with a duration of 5 ns. During the pulse, the wall velocity approaches a steady-state value, whereas after pulse termination it decays gradually toward zero [Fig. 3(c)]. In contrast to the single-exponential relaxation of the 60° wall, the post-pulse velocity of the 180° wall cannot be described by a single relaxation time. Instead, it is well reproduced by a sum of two exponential components,

vDW(t)=A1e−(t−toff)/τ1+A2e−(t−toff)/τ2,(11)v_{\mathrm{DW}}(t)=A_{1}e^{-(t-t_{\mathrm{off}})/\tau_{1}}+A_{2}e^{-(t-t_{\mathrm{off}})/\tau_{2}}, \tag*{(11)}

for t≥tofft \ge t_{\mathrm{off}}, where A1A_{1} and A2A_{2} are the amplitudes of the fast and slow components, respectively, and τ1\tau_{1} and τ2\tau_{2} are their corresponding relaxation times. As shown in Figure 3(d), the fast component governs the initial velocity decay, while the slow component produces a longer relaxation tail.

Both relaxation times depend only weakly on the applied current density [Fig. 3(e)]. Their average values are ⟨τ1⟩≃25.8\langle\tau_{1} \rangle\simeq25.8 ps and ⟨τ2⟩≃225.5\langle\tau_{2} \rangle\simeq225.5 ps. The fast relaxation time is of the same order as the velocity-relaxation time of the 60∘60^\circ wall, but it is about 20% shorter than the uniform-domain value τΦ≃32\tau_{\Phi} \simeq32 ps. The slow time scale is nearly one order of magnitude larger. Since the uniform in-plane octupole coordinate supports only a single relaxation mode within the present model, the appearance of two time scales, together with the shift of the faster one away from τΦ\tau_{\Phi}, indicates that the translational motion of the composite wall is coupled to additional internal degrees of freedom that are absent for an isolated 60∘60^\circ wall.

For the double-exponential relaxation, the post-pulse displacement is given by

Δqpost=∫toff∞vDW(t) dt=A1τ1+A2τ2.(12)\Delta q_{\mathrm{post}}=\int_{t_{\mathrm{off}}}^{\infty}v_{\mathrm{DW}}(t)\,\mathrm{d}t=A_{1}\tau_{1}+A_{2}\tau_{2}. \tag*{(12)}

Because the velocity at pulse termination is vDW(toff)=A1+A2v_{\mathrm{DW}}(t_{\mathrm{off}})=A_{1}+A_{2}, an effective displacement-relaxation time can be defined as

τq,eff=A1τ1+A2τ2A1+A2,(13)\tau_{q,\mathrm{eff}}=\frac{A_{1}\tau_{1}+A_{2}\tau_{2}}{A_{1}+A_{2}}, \tag*{(13)}

such that Δqpost=τq,effvDW(toff)\Delta q_{\mathrm{post}}=\tau_{q,\mathrm{eff}}v_{\mathrm{DW}}(t_{\mathrm{off}}), with ⟨τq,eff⟩≃52.4\langle\tau_{q,\mathrm{eff}}\rangle\simeq52.4 ps from the fitted amplitudes. Consistent with this relation, Δqpost\Delta q_{\mathrm{post}} increases linearly with the velocity at pulse termination [Fig. 3(f)], and the slope yields τq,eff≃51.5\tau_{q,\mathrm{eff}} \simeq51.5 ps. The two values of τq,eff\tau_{q,\mathrm{eff}} are considerably larger than τ1\tau_{1}: although the slow component carries only about 14% of the velocity at pulse termination, its nearly ninefold longer relaxation time makes it responsible for more than half of the total post-pulse displacement.

Internal dynamics of a 180° domain wall

To investigate the internal dynamics accompanying the slow relaxation of the 180∘180^\circ wall, we track the relative positions of its three constituent 60∘60^\circ walls. As shown in Figure 3(a), we define x+60(t)x_{+60}(t) and x−60(t)x_{-60}(t) as the positions satisfying

Φoct[x±60(t),t]=Φoct[q(t),t]±60∘,(14)\Phi_{\mathrm{oct}}[x_{\pm60}(t),t]=\Phi_{\mathrm{oct}}[q(t),t]\pm60^\circ, \tag*{(14)}

respectively, where q(t)q(t) is the overall wall position defined by Eq. (3). The two internal separations are then defined as

d1(t)=q(t)−x+60(t),d2(t)=x−60(t)−q(t).(15)\begin{aligned} d_{1}(t)&=q(t)-x_{+60}(t),\\ d_{2}(t)&=x_{-60}(t)-q(t). \tag*{(15)} \end{aligned}

These quantities characterize the relative separations among the three constituent 60∘60^\circ walls while remaining insensitive to a common rotation of the surrounding octupole domains.

Figure 4(a) schematically compares the octupole-angle profiles during steady-state motion and after relaxation following pulse termination. During current-driven motion, d1d_{1} and d2d_{2} become unequal, indicating an asymmetric deformation of the domain wall. Because isolated 60∘60^\circ domain walls exhibit equivalent current-driven motion, this asymmetry suggests that the additional twofold anisotropy and the mutual coupling among the three constituent walls govern the internal deformation of the composite wall. After the current is removed, the two separations return toward their common equilibrium value while the wall undergoes an additional displacement Δqpost\Delta q_{\mathrm{post}}.

Figure 4. Internal separation dynamics and tunability of the post-pulse motion of a 180° magnetic-octupole domain wall. (a) Octupole-angle profiles during steady-state motion and after relaxation following pulse termination. The internal separations are defined as d1=q−x+60d_{1}=q-x_{+60} and d2=x−60−qd_{2}=x_{-60}-q. During current-driven motion, d1d_{1} and d2d_{2} become unequal; after pulse termination, they return toward equilibrium while the wall undergoes an additional displacement Δqpost\Delta q_{\mathrm{post}}. (b) Time evolution of d1d_{1} and d2d_{2} for Jhm=10×109 A m−2J_{\mathrm{hm}}=10\times10^{9}\ \mathrm{A\,m^{-2}}, with relaxation times τd1≃240\tau_{d_{1}}\simeq240 ps and τd2≃280\tau_{d_{2}}\simeq280 ps. (c)–(e) Dependence of Δqpost\Delta q_{\mathrm{post}} on Aex,xA_{\mathrm{ex},x}, K6K_{6}, and K2K_{2}, respectively.

The time evolutions of d1d_{1} and d2d_{2} are shown in Figure 4(b) for Jhm=10×109 A m−2J_{\mathrm{hm}}=10\times10^{9}\ \mathrm{A\,m^{-2}}. During the current pulse, d1d_{1} decreases while d2d_{2} increases from their equilibrium values. Following pulse termination at toff=5t_{\mathrm{off}}=5 ns, both separations relax toward equilibrium, with characteristic time scales of τd1≃240\tau_{d_{1}}\simeq240 ps and τd2≃280\tau_{d_{2}}\simeq280 ps. These time scales are approximately one order of magnitude longer than the fast velocity-relaxation time τ1\tau_1 and are close to the slow component τ2≃230\tau_2 \simeq230 ps. Together with the single relaxation mode of the uniform in-plane octupole coordinate, this correspondence supports the assignment of the fast and slow velocity components predominantly to the domain-rotation and antisymmetric internal-separation channels, respectively. The coupling of these two relaxation channels accounts for the double-exponential velocity response in Eq. (11).

We finally examine the parameter dependence of the post-pulse motion of the 180° wall by varying Aex,xA_{\mathrm{ex},x}, K6K_6, and K2K_2 while keeping the pulse conditions and all other independent parameters fixed. Figure 4(c)–Figure 4(e) show that Δqpost\Delta q_{\mathrm{post}} increases with Aex,xA_{\mathrm{ex},x} but decreases with K6K_6 and K2K_2, with a particularly strong dependence on the sixfold anisotropy. The Dzyaloshinskii–Moriya contribution is incorporated into Aex,xA_{\mathrm{ex},x} following Ref. [29]. These parameter dependences reflect both the relaxation of the surrounding domains and changes in the internal structure of the composite wall. Although the K2K_2 dependence is weaker than that of K6K_6, its effect on Δqpost\Delta q_{\mathrm{post}} cannot be accounted for solely by the small change in the uniform-domain relaxation, suggesting that changes in the widths and overlap of the constituent walls also contribute. This interpretation is consistent with the previously reported reduction in the total width of the 180° wall with increasing $K_2 {citep}[29]`.

The relaxation channels identified above set the time scale over which a wall settles into a well-defined position after a current pulse. Defining the settling time as the time required to complete 95% of Δqpost\Delta q_{\mathrm{post}}, the 60° wall reaches within 5% of its final post-pulse position in approximately 100 ps. For the representative 180° wall at Jhm=10×109J_{\mathrm{hm}} = 10 \times10^9 A m−2^{-2}, the fitted amplitudes and relaxation times in Eq. (11) give a settling time of approximately 550 ps. The internal degrees of freedom of the composite wall therefore increase the post-pulse settling time by a factor of about five, providing an intrinsic time scale relevant to pulse-controlled positioning and subsequent position readout. The strain-induced twofold anisotropy provides an experimentally accessible means of tuning the post-pulse displacement.

Conclusion

We have investigated the current-driven transient dynamics of magnetic-octupole domain walls in Mn3_3Sn using a multipole micromagnetic framework. For a 60° wall, the post-pulse motion is governed by the relaxation of the current-induced rotation of the surrounding domains, with a characteristic time quantitatively reproduced by a uniform-domain analytic model. For a composite 180° wall, the simulations reveal an additional slow relaxation associated with the relative separations among its constituent walls, which substantially extends the time required for the wall to reach its final post-pulse position. The post-pulse response also varies systematically with the exchange stiffness and magnetic anisotropies, with the strain-induced twofold anisotropy providing an experimentally accessible means of tuning the post-pulse displacement. These results identify distinct domain and internal-coordinate relaxation channels and establish the intrinsic time scales governing pulse-controlled positioning and subsequent readout of magnetic-octupole domain walls in antiferromagnetic spintronic devices.

Acknowledgements

This work was supported by the National Science Foundation (NSF) through the Center for Advanced Semiconductor Chips with Accelerated Performance (ASAP) Industry-University Cooperative Research Center under NSF Cooperative Agreement No. EEC-2231625.

Data availability

The data that support the findings of this study are available from the corresponding author upon reasonable request.

References

References

  1. [1]D. A. Allwood, G. Xiong, C. C. Faulkner, D. Atkinson, D. Petit, and R. P. Cowburn, Magnetic Domain-Wall Logic, Science 309, 1688 (2005).
  2. [2]S. S. P. Parkin, M. Hayashi, and L. Thomas, Magnetic Domain-Wall Racetrack Memory, Science 320, 190 (2008).DOI
  3. [3]D. Kumar, T. Jin, R. Sbiaa, M. Kläui, S. Bedanta, S. Fukami, D. Ravelosona, S.-H. Yang, X. Liu, and S. N. Piramanayagam, Domain wall memory: Physics, materials, and devices, Physics Reports 958, 1 (2022).DOI
  4. [4]C. H. Marrows, J. Barker, T. A. Moore, and T. Moorsom, Neuromorphic computing with spintronics, npj Spintronics 2, 12 (2024).DOI
  5. [5]G. Venkat, D. A. Allwood, and T. J. Hayward, Magnetic domain walls: Types, processes and applications, Journal of Physics D: Applied Physics 57, 063001 (2024).arxiv.org/abs/2305.17800
  6. [6]B. B. Vermeulen, B. Sorée, S. Couet, K. Temst, and V. D. Nguyen, Progress in Spin Logic Devices Based on Domain-Wall Motion, Micromachines 15, 696 (2024).DOI
  7. [7]T. Jungwirth, X. Marti, P. Wadley, and J. Wunderlich, Antiferromagnetic spintronics, Nature Nanotechnology 11, 231 (2016).
  8. [8]V. Baltz, A. Manchon, M. Tsoi, T. Moriyama, T. Ono, and Y. Tserkovnyak, Antiferromagnetic spintronics, Reviews of Modern Physics 90, 015005 (2018).DOI
  9. [9]A. Dal Din, O. J. Amin, P. Wadley, and K. W. Edmonds, Antiferromagnetic spintronics and beyond, npj Spintronics 2, 25 (2024).DOI
  10. [10]S. A. Siddiqui, J. Sklenar, K. Kang, M. J. Gilbert, A. Schleife, N. Mason, and A. Hoffmann, Metallic antiferromagnets, Journal of Applied Physics 128, 040904 (2020).DOI
  11. [11]M.-T. Suzuki, T. Koretsune, M. Ochi, and R. Arita, Cluster multipole theory for anomalous Hall effect in antiferromagnets, Physical Review B 95, 094406 (2017).DOI
  12. [12]S. Nakatsuji, N. Kiyohara, and T. Higo, Large anomalous Hall effect in a non-collinear antiferromagnet at room temperature, Nature 527, 212 (2015).
  13. [13]T. Higo, H. Man, D. B. Gopman, L. Wu, T. Koretsune, O. M. J. van ’t Erve, Y. P. Kabanov, D. Rees, Y. Li, M.-T. Suzuki, S. Patankar, M. Ikhlas, C. L. Chien, R. Arita, R. D. Shull, J. Orenstein, and S. Nakatsuji, Large magneto-optical Kerr effect and imaging of magnetic octupole domains in an antiferromagnetic metal, Nature Photonics 12, 73 (2018).DOI
  14. [14]T. Chen, T. Tomita, S. Minami, M. Fu, T. Koretsune, M. Kitani, I. Muhammad, D. Nishio-Hamane, R. Ishii, F. Ishii, R. Arita, and S. Nakatsuji, Anomalous transport due to Weyl fermions in the chiral antiferromagnets Mn₃X, X = Sn, Ge, Nature Communications 12, 572 (2021).
  15. [15]S. Shim, M. Mehrhaeen, J. Sklenar, S.-L. Zhang, A. Hoffmann, and N. Mason, Spin-Polarized Antiferromagnetic Metals, Annual Review of Condensed Matter Physics 16, 103 (2025).
  16. [16]H. Reichlova, T. Janda, J. Godinho, A. Markou, D. Kriegner, R. Schlitz, J. Zelezny, Z. Soban, M. Bejarano, H. Schultheiss, P. Nemec, T. Jungwirth, C. Felser, J. Wunderlich, and S. T. B. Goennenwein, Imaging and writing magnetic domains in the non-collinear antiferromagnet Mn₃Sn, Nature Communications 10, 5459 (2019).DOI
  17. [17]S. Sugimoto, Y. Nakatani, Y. Yamane, M. Ikhlas, K. Kondou, M. Kimata, T. Tomita, S. Nakatsuji, and Y. Otani, Electrical nucleation, displacement, and detection of antiferromagnetic domain walls in the chiral antiferromagnet Mn₃Sn, Communications Physics 3, 111 (2020).DOI
  18. [18]M. Wu, T. Chen, T. Nomoto, Y. Tserkovnyak, H. Isshiki, Y. Nakatani, T. Higo, T. Tomita, K. Kondou, R. Arita, S. Nakatsuji, and Y. Otani, Current-driven fast magnetic octupole domain-wall motion in noncollinear antiferromagnets, Nature Communications 15, 4305 (2024).DOI
  19. [19]M.-W. Yoo, V. O. Lorenz, A. Hoffmann, and D. G. Cahill, Thermal contribution to current-driven antiferromagnetic-order switching, APL Materials 12, 081107 (2024).
  20. [20]Z. Xu, Y. Zhou, X. Zhang, Y. Qiao, Z. Xu, D. Shao, and Z. Zhu, Spin-orbit torque-driven chiral domain wall motion in Mn₃Sn, Applied Physics Letters 127, 02402 (2025).arxiv.org/abs/2409.18554
  21. [21]Y. Yamane, O. Gomonay, and J. Sinova, Dynamics of non-collinear antiferromagnetic textures driven by spin current injection, Physical Review B 100, 054415 (2019).
  22. [22]O. Gomonay, T. Jungwirth, and J. Sinova, High antiferromagnetic domain wall velocity induced by Néel spin-orbit torques, Physical Review Letters 117, 017202 (2016).DOI
  23. [23]W. Döring, Über die Trägheit der Wände zwischen Weißschen Bezirken, Zeitschrift für Naturforschung A 3, 373 (1948).DOI
  24. [24]E. Saitoh, H. Miyajima, T. Yamaoka, and G. Tatara, Current-induced resonance and mass determination of a single magnetic domain wall, Nature 432, 203 (2004).pubmed.ncbi.nlm.nih.gov/15538364
  25. [25]L. Thomas, R. Moriya, C. Rettner, and S. S. Parkin, Dynamics of Magnetic Domain Walls Under Their Own Inertia, Science 330, 1810 (2010).DOI
  26. [26]J. Torrejon, E. Martinez, and M. Hayashi, Tunable inertia of chiral magnetic domain walls, Nature Communications 7, 13533 (2016).DOI
  27. [27]M.-W. Yoo, F. Mineo, and J.-V. Kim, Analytical model of the deformation-induced inertial dynamics of a magnetic vortex, Journal of Applied Physics 129, 053903 (2021).DOI
  28. [28]A. V. Kimel, B. A. Ivanov, R. V. Pisarev, P. A. Usachev, A. Kirilyuk, and T. Rasing, Inertia-driven spin switching in antiferromagnets, Nature Physics 5, 727 (2009).DOI
  29. [29]M.-W. Yoo, R. Winkler, and A. Hoffmann, Micromagnetic simulations for magnetic multipoles, Applied Physics Reviews 13, 021423 (2026).
  30. [30]A. Shukla, S. Qian, and S. Rakheja, Order parameter dynamics in Mn₃Sn driven by DC and pulsed spin–orbit torques, APL Materials 11, 091110 (2023).DOI
  31. [31]S. T. Konakanchi, S. Banerjee, M. M. Rahman, Y. Yamane, S. Kanai, S. Fukami, and P. Upadhyaya, Electrically tunable picosecond-scale octupole fluctuations in chiral antiferromagnets, Physical Review Letters 135, 136704 (2025).DOI
  32. [32]T. Higo, K. Kondou, T. Nomoto, M. Shiga, S. Sakamoto, X. Chen, D. Nishio-Hamane, R. Arita, Y. Otani, S. Miwa, and S. Nakatsuji, Perpendicular full switching of chiral antiferromagnetic order by current, Nature 607, 474 (2022).DOI
  33. [33]M. Ikhlas, S. Dasgupta, F. Theuss, T. Higo, S. Kittaka, B. J. Ramshaw, O. Tchernyshyov, C. W. Hicks, and S. Nakatsuji, Piezomagnetic switching of the anomalous Hall effect in an antiferromagnet at room temperature, Nature Physics 18, 1086 (2022).DOI
  34. [34]J.-Y. Yoon, P. Zhang, C.-T. Chou, Y. Takeuchi, T. Uchimura, J. T. Hou, J. Han, S. Kanai, H. Ohno, S. Fukami, and L. Liu, Handedness anomaly in a non-collinear antiferromagnet under spin–orbit torque, Nature Materials 22, 1106 (2023).DOI
  35. [35]Z. He and L. Liu, Magnetic dynamics of strained non-collinear antiferromagnet, Journal of Applied Physics 135, 093902 (2024).
  36. [36]A. Shukla, S. Qian, and S. Rakheja, Impact of strain on the SOT-driven dynamics of thin film Mn₃Sn, Journal of Applied Physics 135, 123903 (2024).

Paper details

vlnc:W_dwnhwwan
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents