Characterizing Niobium Nitride Superconducting Microwave Coplanar Waveguide Resonator Array for Circuit Quantum Electrodynamics in Extreme Conditions

Abstract

The high critical magnetic field and relatively high critical temperature of niobium nitride (NbN) make it a promising material candidate for applications in superconducting quantum technology. However, NbN-based devices and circuits are sensitive to decoherence sources such as two-level system (TLS) defects. Here, we numerically and experimentally investigate NbN superconducting microwave coplanar waveguide resonator arrays, with a 100 nm thickness, capacitively coupled to a common coplanar waveguide on a silicon chip. We observe that the resonators' internal quality factor (Qi) decreases from Qi ~ 1.07*10^6 in a high power regime (< nph > = 27000) to Qi ~ 1.36 *10^5 in single photon regime at temperature T = 100 mK. Data from this study is consistent with the TLS theory, which describes the TLS interactions in resonator substrates and interfaces. Moreover, we study the temperature dependence internal quality factor and frequency tuning of the coplanar waveguide resonators to characterise the quasiparticle density of NbN. We observe that the increase in kinetic inductance at higher temperatures is the main reason for the frequency shift. Finally, we measure the resonators' resonance frequency and internal quality factor at single photon regime in response to in-plane magnetic fields B||. We verify that Qi stays well above 10^4 up to B|| = 240 mT in the photon number < nph > = 1.8 at T = 100 mK. Our results may pave the way for realising robust microwave superconducting circuits for circuit quantum electrodynamics (cQED) at high magnetic fields necessary for fault-tolerant quantum computing, and ultrasensitive quantum sensing.

Introduction

Superconducting coplanar waveguide resonators, or CPWs, play an essential role in circuit quantum electrodynamics (cQED) [1, 2, 3], superconducting quantum sensing [4, 5, 6], quantum metrology [7, 8], and quantum computing [9, 10]. The electric field in CPWs can be confined inside the resonator, making them an appropriate choice for coupling between quantum devices. A further benefit of CPWs is their simple geometry, which makes them a fundamental component of quantum circuits. In this regard, it is crucial to maintain a high internal quality factor (QiQ_i) of CPWs in quantum circuits to minimise unwanted losses that affect qubit gate fidelities and qubit relaxation times [11, 12] to achieve robust and fault-tolerant quantum computers [10, 13].

Recently, attention has been on identifying the loss mechanisms contributing to the quality factor of the CPWs [14]. Recent results show that two-level systems (TLSs) and quasiparticle losses are mostly responsible for quantum circuits' decoherence [15, 16, 17, 18]. TLS loss appears when the defects in amorphous material (such as the substrate of quantum circuits and oxides growth on the superconductor) are coupled with the electric field of CPWs. These TLS defects are mostly confined to the ground states at millikelvin temperatures and low powers. They absorb energy from CPWs and dissipate heat to the resonator when defects jump to excited energy states [19]. Accordingly, circuit engineering techniques have been developed on topics of finding low-loss substrate and superconductor materials [20, 21], optimising circuits geometry [22, 23, 24] and improving micro and nanofabrication techniques [25, 26]. Several research groups have pursued these methods to improve the quality factor in the CPWs and achieved a high internal quality factor's CPWs in the quantum devices [27, 28, 29, 30, 31].

Moreover, there has been considerable interest in the characterisation of the quasiparticle loss [32, 33, 34, 35], another cause of loss in CPW. An active area of research is to find the dynamic of the quasiparticle effect on superconducting quantum devices [36, 37, 38], which can host Andreev bound states (ABSs) [39, 40, 41] and Majorana bound states (MBSs) [39, 42]. Emerging MBSs in hybrid superconductor-semiconductor devices require an application of magnetic fields while maintaining the superconductivity [43]. Therefore, topological superconductivity can potentially appear in a hybrid circuit with superconductors, such as niobium titanium nitride (NbTiN) [44, 45], tantalum (Ta) [46], lead (Pb) [47], and niobium nitride (NbN) with their relatively high critical magnetic fields, and also for this purpose, it will be important to characterise the microwave superconducting circuits losses in the presence of the magnetic field.

A main challenge in superconducting circuits operating in extreme conditions, e.g., in the presence of magnetic fields, is achieving high QiQ_i resonance since changes in the magnetic flux density in superconductors cause suppression of superconductivity or a phase transition from superconductor states to normal states. Moreover, in type II superconductors, the superconductor enters to the mixed states when the magnetic field is applied, leading to vortices pinning and flux creep. The following issues need to be addressed to preserve high QiQ_i resonators based on the type II superconductors [30]. First, the QiQ_i becomes more vulnerable to even small magnetic fields due to the creation of Abrikosov vortices: supercurrent regions that circulate around a non-superconducting core [48]. Second, type II superconductors have a lower coherence length in comparison with type I superconductors; therefore, energy losses have a higher value at single photon regimes. The possible solutions to overcome these challenges are to reduce the geometry of the resonator to below magnetic field penetration depth or to define lithographically artificial defect sites to pin the vortices [48, 49, 50, 51].

In this work, we first report the design and fabrication of NbN CPWs arrays on two silicon chips whose frequency resonance window is between 4 GHz and 8 GHz. Following this, we discuss characterisation and analyses of the frequency shift Δf\Delta f and internal quality factor QiQ_i of the CPWs in response to sweeping temperature, microwave power and magnetic field. We further verify that the QiQ_i of CPW in one of the chips increases from Qi∼1.36×105Q_i \sim1.36 \times10^5 in single photon regime to Qi∼1.07×106Q_i \sim1.07 \times10^6 at photon number ⟨nph⟩=2.7×104\langle n_{ph} \rangle= 2.7 \times10^4, at T=100T = 100 mK. Indeed, we find that the Δf\Delta f of the resonator changes when the magnetic field is applied at different temperatures. Moreover, we show that QiQ_i stays above Qi∼104Q_i \sim10^4 at ⟨nph⟩=1.9×105\langle n_{ph} \rangle= 1.9 \times10^5, ⟨nph⟩=6\langle n_{ph} \rangle= 6 and ⟨nph⟩=1.8\langle n_{ph} \rangle= 1.8 when parallel magnetic fields B∥<240B_{\parallel} < 240 mT are applied to the chips at T=100T = 100 mK. These results show that the NbN resonators are promising superconducting material candidates for hybrid quantum electrodynamic circuits requiring magnetic fields.

Method

Design and Fabrication

Our superconducting microwave circuits consist of an array of microwave resonators capacitively coupled to a common coplanar waveguide and fabricated on a 100 nm thin NbN film sputtered on a silicon chip. The silicon substrate is dipped in Buffered Oxide Etchant (BOE) to strip the native SiOx_x from the substrate's surface to achieve a clean substrate-metal interface. Immediately after removing the SiOx_x layer, the chip was placed in the load lock of an MP 600 S Plassys sputter system to prepare for NbN metal deposition [52]. After the load lock pumps down and reaches a low pressure, the sample was transferred to the main chamber to reactively sputter 100 nm of NbN. In the main chamber, by sputtering niobium (Nb) for 15 minutes with 25 sccm of Argon (Ar) and 3.0 sccm of Nitrogen at the base current of 0.85 A, 100 nm NbN film was formed on top of the 525 µm silicon substrate. After removing samples from the load lock of the sputtering machine, ZEP resist was spun and baked at 180 °C on hotplates for four minutes. The resonators were patterned with standard e-beam lithography followed by CF4CF_4/Ar anisotropic dry etch. The resonator length was chosen to have a fundamental frequency mode between 4 – 8 GHz.

Two different types of samples are fabricated and measured, each containing three resonator arrays with 4 µm width, and 2 µm gap, multiplexed to a single feedline. Figure 1(a), and (Figure 1b) show a wire-bonded superconducting CPW chip, and the packaged chip, respectively. A top-view schematic of one resonator is shown in Figure 1(c). Moreover, a zoom-in view of the resonator (R1) and the magnified area showing the gap and width position are schematically depicted in Figure 1(d) and Figure 1(e), respectively. More details of the fabricated superconducting CPW circuits in this study are provided in Table 1.

Image not extracted

Figure 1. NbN based superconducting microwave coplanar waveguide resonators. (a) Optical image of sample 1 which is wire-bonded in the sample holder. (b) Packaged chip for cryogenic microwave spectroscopy. (c) A topview schematic of the superconducting circuit used in the experiments shows three capacitively coupled resonators multiplexed to a common coplanar waveguide (brown dashed line area in Fig. (a)). The length of resonators from left to right are L1=4.688L_1 = 4.688 mm, L2=6.250L_2 = 6.250 mm, L3=7.900L_3 = 7.900 mm. Here, the thickness of NbN film, and silicon substrate is 100 nm, and 525 µm, respectively. (d) Magnified schematic of resonator 1 (blue dashed line in Figure 1(c)). (e) The magnified area shows the resonator's gap and width position (red dashed line in Figure 1(d)).

SampleResonator WidthResonator GapR1 LengthR2 LengthR3 Length
14 μ\mum2 μ\mum4.688 mm6.250 mm7.9 mm
24 μ\mum2 μ\mum4.5 mm5.5 mm6.5 mm

Table 1. NbN superconducting microwave coplanar waveguide resonator array design detail.

Experimental setup

The sample box (Figure 1(b)) was mounted in two different cryogenic setups to collect the data presented in this paper: 1) an adiabatic demagnetization refrigerator (ADR) with a base temperature of T=30T = 30 mK (see the fridge setup in FIG.S1. (a)). 2) a dilution refrigerator (DR) with a base temperature of T=20T = 20 mK (see FIG.S1. (b)). The complex microwave transmission spectroscopy (S21S_{21}) was performed with a MS4642B Keysight Vector Network Analyzer (VNA) by sending signals to ports on the NbN transmission line. In the ADR setup, the input line of the VNA is heavily attenuated (-40 dB) at room temperature. Then, VNA signals were attenuated by -20 dB at T=70T = 70K, 4K, and 0.5 K stages before reaching the transmission line of the sample, suppressing thermal noise and allowing the resonator to reach into the single photon regime. At the T=4T = 4K stage, after the signal passes through the sample box, an isolator is placed to prevent contamination of transmission signals from spurious reflections back to the transmission line. Then, the signal was amplified by a high electron mobility transistor (HEMT) which provided +40 dB amplification. Moreover, an additional +45 dB amplification is provided with a room-temperature amplifier. RF signals generated by the VNA propagate through the ADR before reaching the CPW transmission line, where they excite the resonators. The signal power levels range from -30dBm to 15dBm (see FIG.S1. (a)).

We note that, for magnetic field measurements, we mounted our sample inside a Solenoid (NbTi superconducting magnets) in the ADR such that the NbN transmission line is parallel to the applied magnetic fields. The current in the Solenoid sweeps between -10 A to 10 A, leading to a magnetic field sweep between -800 mT to 800 mT [51]. In this work, we present the microwave power and temperature sweep of sample 2 which are measured in a dilution refrigerator (DR) and the ADR refrigerator, and the magnetic field sweep of sample 1 measured in the ADR refrigerator. The DR cryogenic setup detail is shown in FIG.S1. (b).

Numerical methodology

The extraction of resonator parameters such as resonance frequency (frf_r), internal quality factor (QiQ_i), coupling quality factor (QcQ_c), and loaded quality factor (QlQ_l) from S21S_{21} measurements, is a crucial tasks in the characterisation and design of resonate circuit. To pursue this goal different types of RLC circuit models have been used in previous research based on amplitude or phase of S21S_{21} [28, 53, 54, 55, 56]. Modern methods typically utilize the full complex scattering data provided by VNA as opposed to focusing on the power or amplitude to extract resonator parameters [28, 57, 58]. Using entire complex data results in a better signal-to-noise ratio (SNR) and a more accurate determination of resonator parameters. This article uses a notch-type resonator model to extract resonance frequency and quality factors of the NbN microwave superconducting resonators. The S21S_{21} of notch-type resonators can be evaluated with the following equation [58]:

S21notch(f)=(aeiαe−2πifτ)⏟Environmental effect×[1−(QL∣Qc∣)eiφ1+2iQL(ffr−1)]⏟Ideal resonator(1)S_{21}^{notch}(f)=\underbrace{\left(a e^{i\alpha}e^{-2\pi i f\tau}\right)}_{\text{Environmental effect}}\times\underbrace{\left[1-\frac{\left(\frac{Q_L}{\lvert Q_c\rvert}\right)e^{i\varphi}}{1+2iQ_L\left(\frac{f}{f_r}-1\right)}\right]}_{\text{Ideal resonator}} \tag*{(1)}

The second part of Eq. (1) characterises an ideal notch-type resonator where ff indicates the probe frequency, and φ\varphi quantifies the impedance mismatch. In more detail, φ\varphi indicates the difference between input and output impedance at the ports of the resonator. In an ideal notch-type RLC circuit, the circle (Im(S21S_{21}) and Re(S21S_{21}) circle plot) intersects the real axis at unity, which corresponds to a probe frequency at f→±∞f \to\pm\infty called off-resonant point.

Note that the diameter (dd) of the circle comes from d=Ql∣Qc∣d = \frac{Q_l}{\lvert Q_c\rvert}. However, in experimental measurements from VNA, a rotation in the phase and a change in the amplitude of the circle have been observed. To overcome the above issue, the first term in Eq. (1) has been added to describe the environmental noise. First, an amplitude aa shows the cable damping effect in S21S_{21}, a phase shift α\alpha shows an extra rotation in the phase of S21S_{21} coming from cable length, and finally, an electronic delay τ\tau which changes the initial phase in signal input S21S_{21} to a different value from zero. The length of the cable and the finite speed of light cause an electronic delay. Besides, with a circuit model we also can drive the photon number inside the resonator with the below formula [59]:

Pin=Ptrans+Preflection+Ploss(2)P_{in}=P_{trans}+P_{reflection}+P_{loss} \tag*{(2)}
Ploss=Pin(1−∣S21∣2−∣S11∣2)(3)P_{loss}=P_{in}\left(1-\lvert S_{21}\rvert^{2}-\lvert S_{11}\rvert^{2}\right) \tag*{(3)}
⟨nph⟩=Qi×Plossℏω02=Qi×Pinℏω02(2×QL×Qc−QLQc2)(4)\langle n_{ph}\rangle=Q_i\times\frac{P_{loss}}{\hbar\omega_0^2}=Q_i\times\frac{P_{in}}{\hbar\omega_0^2}\left(2\times Q_L\times\frac{Q_c-Q_L}{Q_c^2}\right) \tag*{(4)}

Where nphn_{ph} is the photon number, PinP_{in} is the input power, PtransP_{trans} is the transmitted power through the feedline, PlossP_{loss} is the source of losses, ℏ\hbar is plank constant and ω0\omega_0 is resonance angular frequency of resonator. A typical result of such a fit is shown in Figure 2, where we show the measured and calculated frequency spectrum of sample 2 at fundamental frequency fr=5.965f_r=5.965 GHz at T=26T=26 mK. Indeed, we investigate QiQ_i relation with power in the DR cryogenic setup to confirm the reproducibility of measurements taken in the ADR and cover a higher range of photon numbers.

Figure 2. (a) Parametric plot and fitted Im (S21S_{21}) and Re (S21S_{21}), (b) Measured and calculated frequency spectrum of sample 2 at fundamental frequency fr=5.9643f_r = 5.9643 GHz at T=26T = 26 mK, same data in (a).

Figure 3(a) shows the frequency spectrum comparison, confirming a good agreement between measurements taken in two different DR and ADR cryogenic setups. In Figure 3(b), we compare extracted QiQ_i and ⟨nph⟩\langle n_{ph}\rangle taken in the ADR and DR cryogenic setup at power range -100 dBm <Pin<<P_{in}< -150 dBm at T=200T=200 mK. The results confirm that both measurement setups are in accordance with each other during power sweep measurements. In the following chapter, we characterise kinetic inductance, TLS loss, and quasiparticle loss.

Image not extracted

Figure 3. (a) Frequency spectrum of sample 2 measured in two different cryogenic setups: the ADR (red dashed-line), and DR (blue dashed-line). A good agreement between the two measurements can be seen at T=200T=200 mK. (b) Measured QiQ_i at fundamental frequency fr=5.96f_r=5.96 GHz in the power range of Pin=−150P_{in}=-150 dBm to -100 dBm at T=200T=200 mK in two different setups.

Results

Kinetic inductance characterisation

In the simplest case of capacitively coupled superconducting quantum circuits, modelling the resonator as an LCLC circuit, the coupling strength gg between the feedline and resonator will be proportional to the impedance of the quantum circuits. In the quarter wavelength resonators impedance ZZ and resonance frequency frf_r of the LCLC circuit can be extracted by the equation Z=Ll+LkClZ = \sqrt{\frac{L_l+L_k}{C_l}} and vph=2πfrknv_{ph} = \frac{2\pi f_r}{k_n} where kn=πn2lk_n = \frac{\pi n}{2l} and vph=1Cl(Ll+Lk)v_{ph} = \frac{1}{\sqrt{C_l(L_l+L_k)}}. Here, LlL_l, LkL_k and ClC_l are geometrical inductance, kinetic inductance, and geometrical capacitance per unit length of transmission line, respectively. Moreover, nn emphasizes on the resonance frequency number (n=1n = 1 for the fundamental mode) [28].

Therefore, characterising the kinetic inductance of superconducting circuits to identify coupling strength and resonance frequency is an essential step toward robust quantum technologies. Moreover, the resonators' kinetic inductance helps us to evaluate quasiparticle loss and frequency shift in superconducting circuits. More details are discussed in § 3.3.

For obtaining kinetic inductance, we first use conformal mapping techniques [60] to extract the geometrical inductance Ll=4.1367×10−7L_l = 4.1367 \times10^{-7} H/m and the capacitance Cl=1.6803×10−10C_l = 1.6803 \times10^{-10} F/m. We obtain kinetic inductance Lk=4.464×10−8L_k = 4.464 \times10^{-8} H/m, which shows lower kinetic inductance compared to previous reports on NbN coplanar waveguide resonators and thin NbN sheets [28, 61, 62]. The following section investigates the effects of power, temperature, and magnetic field on NbN's CPW.

Power dependence QiQ_i

Knowing how sweeping power and temperature affect material defects' behaviour can help us make more robust quantum circuits. To achieve this, we study the resonator’s QiQ_i to an average photon number inside the resonator at three different temperatures: at (i) T=26T = 26 mK, (ii) T=T =

200 mK, and (iii) T=650T = 650 mK. This is done in order to identify the sources of energy loss of the resonator at different temperatures. We split measured losses into three terms, as shown in equation (5). Here, δTLS\delta_{TLS} describes TLS loss, δqp\delta_{qp} is quasiparticle loss, δB\delta_B is vortex and magnetic field loss, and δ0\delta_0 is power and temperature independent loss [33].

δ=δTLS(T,P)+δqp(T)+δB(B)+δ0(5)\delta= \delta_{TLS}(T,P) + \delta_{qp}(T) + \delta_B(B) + \delta_0 \tag*{(5)}

TLS defects in the ground state are the dominant cause of increasing loss at sub-millikelvin temperatures since TLS defect's jumping to the excited states induces heating dissipation in the resonator [19]. Meanwhile, the superconducting energy gap is larger than the thermal noise of the system at temperatures Δ≫kBT\Delta\gg k_B T, where Δ\Delta is superconducting gap, kBk_B is bolt zman constant, so Cooper pair breaking is less likely to happen. Therefore, quasiparticle density becomes negligible. In this case, the loss rates can be characterised [21]:

δTLS(T,P)=1QTLS=1QTLS0tanh⁡(hfr2kBT)(1+nphnc)β(6)\delta_{TLS}(T,P) = \frac{1}{Q_{TLS}} = \frac{1}{Q_{TLS}^{0}} \frac{\tanh\left(\frac{h f_r}{2 k_B T}\right)}{\left(1+\frac{n_{ph}}{n_c}\right)^\beta} \tag*{(6)}

where frf_r is resonance frequency, nphn_{ph} is the average photon number, ncn_c is critical photon number, and 1QTLS0=δTLS0\frac{1}{Q_{TLS}^{0}} = \delta_{TLS}^{0} is TLS loss at zero power and temperature.

As shown in Figure 4, in T=26T = 26 mK, QiQ_i saturates at 10510^5 in single photon regime, and as power rises it goes to surpasses 10610^6. We find an agreement between TLS theory and measurement results, as shown in Figure 4(b). We find that QTLS0Q_{TLS}^{0}, ncn_c and β\beta are 9.5102×1049.5102 \times10^4, 13 and 0.35, respectively. In comparison with previous measurements [27, 28, 29, 30, 63] we achieve a QiQ_i of around one million at only <nph>=2000< n_{ph} > = 2000, at T=26T = 26 mK, which suggests a good improvement in the development of high-QQ superconducting CPWs based on thin NbN films.

Image not extracted

Figure 4. (a) Measured QiQ_i at fundamental frequency fr=5.96f_r = 5.96 GHz in the power range P=−150P = -150 dBm to -100 dBm at T=26T = 26 mK, 200 mK and 650 mK. The shaded area corresponding to deviation/error from the actual data. (b) QiQ_i versus photon number at T=26T = 26 mK fitted with the theoretical model of TLS. These data are measured for sample 2 in the DR.

In comparison, at higher temperatures, TLS defects saturate in a mixture containing equal proportions of ground and excited states; therefore, an energy exchange happens between energy states, reducing the energy loss from TLS defects. However, the energy gap is near the required Cooper pair-breaking energy in this temperature range. Decreasing the superconducting energy gap leads to an increase in quasiparticle density in the resonator, which is the primary cause of energy loss at this temperature range. The quasiparticle loss can be characterised by the below model [64, 65]:

1Qi∼1Qqp=απ2Δℏωrnqp(T)D(EF)Δ(7)\frac{1}{Q_i} \sim\frac{1}{Q_{qp}} = \frac{\alpha}{\pi} \sqrt{\frac{2\Delta}{\hbar\omega_r}\frac{n_{qp}(T)}{D(E_F)\Delta}} \tag*{(7)}

Where α\alpha is the ratio between kinetic inductance and total inductance (LkLk+Ll)\left(\frac{L_k}{L_k+L_l}\right), (see § 3.1), Δ\Delta is NbN superconducting energy gap, D(EF)D(E_F) is density states of Fermi level, and nqpn_{qp} is quasiparticle density. Therefore, as expected from equation (7), the loss of the resonator will be mainly dependent on the temperature, and it will be inconsistent with sweeping power, which is what we see in our measurement at T=650T = 650 mK and depicted in Figure 4(a).

Table 2 compares the highest measured QiQ_i of both samples at millikelvin temperatures during power sweep measurements. It shows that the QiQ_i values are compatible with each other in single photon and high power regimes, even though each sample has been fabricated in a different timeline. These results confirm that thin NbN superconductor film and silicon substrate quality is approximately maintained regardless of the environmental situation and measurement setup.

Temperature dependence of QiQ_i and frf_r

In the next step, we extracted the QiQ_i and frf_r at single photon regime in the temperature ranges between T=100T = 100 mK and 3K. The results show that at around T∼1T \sim1 K, the QiQ_i value is at its highest value, as shown in Figure 5 (a). This behaviour is in good agreement with previous research on TiN and MoRe based microwave resonators [66, 67]. The same investigation has been done for the frequency shift Δf\Delta f of the resonator versus temperature; the data is shown in Figure 5 (b). We observe that at T∼1T \sim1 K, the resonance frequency experiences a noticeable red shift, the same temperature when we extracted the highest Qi=2.57×105±3.9×104Q_i = 2.57 \times10^5 \pm3.9 \times10^4. In more detail, when energy loss is mainly due to TLS defects, the resonance frequency shift also happens due to TLS loss (Figure 5) which can be described by the below model [65]:

Image not extracted

Figure 5. (a) QiQ_i versus temperature at single photon regime. The shaded area corresponds to deviation/ error from the actual data fr=5.952f_r = 5.952 GHz. (b) Resonance frequency shift versus temperature. The blue and red circles show Δfqp\Delta f_{qp} and Δf\Delta f calculated quasiparticle loss frequency shift, and total loss frequency shift, respectively. These results are measured data of sample 2 in the ADR.

ΔfTLS=1QTLS21π[R{Ψ(12+hfr2πikBT)}−ln⁡hfr2πkBT](8)\Delta f_{TLS} = \frac{1}{Q_{TLS}^{2}}\frac{1}{\pi}\left[R\left\{\Psi\left(\frac{1}{2}+\frac{h f_r}{2\pi i k_B T}\right)\right\}-\ln\frac{h f_r}{2\pi k_B T}\right] \tag*{(8)}

where Ψ\Psi is the digamma function. We can plot this function using data extracted from the previous fit in Figure 5 (b). At higher temperatures, due to an increase in quasiparticle density, kinetic inductance increases, which leads to the below frequency red shift [65]:

Δfqp=−12frΔLL=−12αfrΔLkLk=−12αfrΔkBTsinh⁡ΔkBT(9)\Delta f_{qp}=-\frac{1}{2}f_r\frac{\Delta L}{L}=-\frac{1}{2}\alpha f_r\frac{\Delta L_k}{L_k}=-\frac{1}{2}\alpha f_r\frac{\Delta}{k_B T\sinh\frac{\Delta}{k_B T}} \tag*{(9)}

In Figure 5 (b), we plot the measured Δf\Delta f relation with temperature and calculate frequency shifts obtained by equation (9) and equation (10). In this equation, we use the kinetic inductance ratio obtained from section 3.1. This theory agrees well with the measured data extracted from the resonator samples; the plot has been shown in Figure 5 (b):

Δf≈ΔfTLS+Δfqp(10)\Delta f \approx\Delta f_{TLS}+\Delta f_{qp} \tag*{(10)}

We see that Δfqp∼Δf\Delta f_{qp} \sim\Delta f in higher temperatures; therefore, the main reason for resonance shifts in high temperatures is quasiparticle defects. Table 3 shows the highest and lowest QiQ_i in a single photon regime for both samples measured during the temperature sweeps. It shows that QiQ_i remains higher than 10310^3, although we measured our samples at high temperatures which are suspected to have high Cooper pair breaking rates.

Photon numberMax (QiQ_i)Min (QiQ_i)QcQ_cQLQ_L
Sample 1<nph>∼1< n_{ph} > \sim11.957×1051.957 \times10^55.39×1045.39 \times10^424182314
T=700T = 700 mKT=2T = 2 K
Sample 2<nph>∼1< n_{ph} > \sim12.571×1052.571 \times10^57.421×1037.421 \times10^321422118
T=1T = 1 KT=2.9T = 2.9 K

Table 3. The highest and lowest internal quality factors of each sample in single photon regime measured during temperature sweep. Both of these measurements were performed in the ADR setup.

Note that QcQ_c and QlQ_l values of sample 1 differ from the results in Table 2 because we did the wire bonding again due to the destruction of Aluminum wires during temperature sweep measurements. Wire bonding is mainly responsible for the impedance value of superconducting CPW. Therefore, as equation (1) shows, impedance mismatch affects the QcQ_c and QlQ_l.

TT (mK)frf_r (GHz)QiQ_i (high power)QiQ_i (single photon)QcQ_cQLQ_L
Sample 11005.3031.07×1061.07 \times10^61.36×1051.36 \times10^563786340
Sample 1⟨nph⟩∼2.7×104\langle n_{ph} \rangle\sim2.7 \times10^4⟨nph⟩∼1\langle n_{ph} \rangle\sim1
Sample 2265.9529.76×1059.76 \times10^59.57×1049.57 \times10^423082252
Sample 2⟨nph⟩∼2×103\langle n_{ph} \rangle\sim2 \times10^3⟨nph⟩∼1\langle n_{ph} \rangle\sim1

Table 2. Comparing the measured highest internal quality factor of each sample.

Evaluation of the CPWs under parallel magnetic fields

Finally, we examine the behaviour of the resonators when a static magnetic field is applied. The sample box (sample 1) is mounted in a cryogenic setup in the way that the NbN transmission line is positioned parallel to magnetic field B∥B_{\parallel}. We perform three measurements to characterise the magnetic field effect on the resonators. At first, we upsweep B∥B_{\parallel} from 0 to 720 mT with 80 mT steps (see Figure 6 (a)). The results of these measurements indicate that as the magnetic field is increased up to 720 mT, the resonance frequency experiences a redshift, and the dip value decreases because of Cooper pair breaking and emerging Abrikosov vortices.

Figure 6. (a) The S21S_{21} versus frequency spectrum between B∥=0B_{\parallel}=0 T and 720 mT with 80 mT steps at T=100T=100 mK. The shaded area corresponds to frequency shift in magnetic field sweep in the range of Ba<B∥<Bc1B_a<B_{\parallel}<B_{c1}. (b) Extracted frequency shift as a function of B∥B_{\parallel} (mT) with ⟨nph⟩=1.9×105\langle n_{ph}\rangle=1.9\times10^5, 6 and 1.8. A fit of the measurement data with the equation Δfrfr0=−k×B∥\frac{\Delta f_r}{f_{r0}}=-k\times B_{\parallel} which gives k=2.61×10−1 T−2k=2.61\times10^{-1}\ \mathrm{T}^{-2} at T=100T=100 mK and ⟨nph⟩=1.9×105\langle n_{ph}\rangle=1.9\times10^5, 6 and 1.8. (c) QiQ_i as a function of B∥B_{\parallel} at T=100T=100 mK and ⟨nph⟩=1.9×105\langle n_{ph}\rangle=1.9\times10^5, 6 and 1.8. The QiQ_i remains above 10410^4 until B∥=240B_{\parallel}=240 mT at all the mentioned photon numbers. These are measured data of sample 1 in the ADR cryogenic setup.

Trapped flux inside the NbN, as a type II superconductor, strongly depends on sample preparation and geometry. Moreover, existing and stability of these fluxes inside the superconductor, which affect resonator loss, come from two different forces, which appear due to the Meissner effect and Lorentz forces. First forces, due to the Meissner effect, a vortex is pushed toward the edges of the superconductor to expel from it. The second force happened when the vortex is attracted to the centre of the superconductor due to weak interactions of the Meissner screening current. The second one is proportional to the B∥B_{\parallel}, and at a high enough field, the vortex will exist and pin in a stable condition in a line of superconductor thin films [68, 69]. Based on theoretical investigation [68, 69], vortices in thin superconducting film for B∥<BaB_{\parallel} < B_a experience expulsion force, resulting in a more stable condition Ba=πϕ04t2=161B_a = \frac{\pi\phi_0}{4t^2} = 161 mT.

Then vortices begin to align in a straight line when Ba<B∥<Bc1B_a < B_{\parallel} < B_{c1} and the edges of the thin film become vortices free Bc1=1.65×ϕ0t2=341B_{c1} = 1.65 \times\frac{\phi_0}{t^2} = 341 mT. For Bc1<B∥B_{c1} < B_{\parallel}, the density of vortices increases in a way where vortices-vortices interaction should be taken into serious consideration where leading to a higher loss (Figure 6 (a)). Here, ϕ0\phi_0 and tt exhibit flux quantum and thickness, respectively. In the next step, we measure the effect of applying B∥B_{\parallel} on the frf_r and QiQ_i of CPW. As B∥B_{\parallel} increases, frf_r experiences a redshift, as shown in Figure 6 (b), due to the increased rate of Cooper pairs breaking. The frequency shift Δf=f−fr\Delta f = f - f_r can be modelled as a parabolic decrease [70] as Δffr=−k×B∥\frac{\Delta f}{f_r} = -k \times B_{\parallel}, with k=π48(t2e2DℏkBTc)k = \frac{\pi}{48}\left(\frac{t^2 e^2 D}{\hbar k_B T_c}\right), which depends on resonator thickness tt, critical temperature TcT_c and the electron diffusion constant DD in NbN. The electron diffusion constant is approximated to D∼0.683 cm2 s−1D \sim0.683\ \mathrm{cm}^2\ \mathrm{s}^{-1}, consistent with the previous experiments [28, 71, 72].

Figure 6 (c) demonstrates the effect of in-plane magnetic fields on the resonators QiQ_i at T=100T=100 mK, and in ⟨nph⟩=1.9×105\langle n_{ph}\rangle=1.9\times10^5, ⟨nph⟩=6\langle n_{ph}\rangle=6 and ⟨nph⟩=1.8\langle n_{ph}\rangle=1.8. It shows that by increasing the magnetic fields, QiQ_i decreases. However, QiQ_i remains above 10410^4 up to B∥=240B_{\parallel}=240 mT, which shows the resonator's effectiveness under applying magnetic fields. In superconducting resonators, the resonance frequency is determined by the RF surface impedance of the superconductor, which can be affected by flux creep and vortices pinning [68]. As magnetic vortices move and generate electrical resistance and heat, the surface impedance of the superconductor changes, which in turn can lead to a shift in the resonance frequency. The degree of resonance shift depends on several factors, including the strength of the applied magnetic field, the temperature, and the structure of the superconductor, including any defects and impurities or material disorder.

To further study the effect of in-plane magnetic fields on resonance frequency frf_r, we reduced the steps in the magnetic field measurement to 8 mT. We performed an upsweep measurement in the range between 0 mT <B∥<< B_{\parallel} < 80 mT (Figure 7). We observed that frf_r experiences butterfly effects at low magnetic fields 0 mT <B∥<< B_{\parallel} < 32 mT, showing the mobility of the vortices which have a hysteresis effect in the conductivity of the NbN superconductors. Figure 7(a) shows that the changes in the complex conductivity of planar superconducting circuits due to dissipative vortices motions lead to a jump in resonance frequency [73]. Indeed, this jump which occurs at magnetic fields ranging from 16 mT <B∥<< B_{\parallel} < 32 mT suggests a sudden movement or depinning of the vortices in the NbN superconductor. As the magnetic field increases, vortices tend to pin in the superconducting material. As shown in Figure 7(b), we observed that, in a higher magnetic field range between 32 mT <B∥<< B_{\parallel} < 80 mT, the resonance frequencies decrease as the magnetic field increases implying that NbN thin film conductivity wasn’t affected by the mobility of the vortices since no butterfly effect of the resonance frequency is detected [69] [73].

Figure 7. (a) Measured frequency spectrum for an upsweep measurement of between B∥=0B_{\parallel} = 0 mT to 32 mT with a step of 8 mT at temperatures T=100T = 100 mK. In this magnetic field range, we observe a resonance frequency jump at B∥=16B_{\parallel} = 16 mT. (b) Measured frequency spectrum for an upsweep measurement of the magnetic field between B∥=32B_{\parallel} = 32 mT to 80 mT, the resonance frequency shift as expected.

Moreover, to understand the effect of the solenoid on the frf_r of our sample, we increased the magnetic field's range to -160 mT <B∥<< B_{\parallel} < 160 mT. We expected that the Δf\Delta f plot should have a symmetrical shape around B∥=0B_{\parallel} = 0 mT where Δf(B∥=0)=0\Delta f (B_{\parallel} = 0) = 0. However, the maxima (Δf=0\Delta f = 0) shift towards negative fields B∥=−25.6B_{\parallel} = -25.6 mT. This shift may happen due to the remaining magnetic field from the ADR magnet which is responsible for the adiabatic demagnetisation procedure. Besides, we observe a very high jump at Δf(B∥=32\Delta f (B_{\parallel} = 32 mT) at T=100T = 100 mK (see Figure 8). To identify the jump further, we performed temperature dependent measurements at T=100T = 100 mK, 500 mK, 1 K and 1.5 K to examine the effect of temperatures. As shown in Figure 8, we observe a similar jump at all temperatures, which we presume is due to vortices trapped in the NbTi solenoid.

Image not extracted

Figure 8. Measured frequency spectrum with magnetic field sweep raging between −160<B∥ (mT)<160-160 < B_{\parallel}\,(\mathrm{mT}) < 160 with a field step of 8 mT at T=T = (a) 100 mK, (b) 500 mK, (c) 1 K, (d) 1.5 K. Arrows indicate sweep direction.

To further study the progress on the fabrication procedure of NbN coplanar waveguide resonator, we compare our techniques with the most recent reports on NbN superconductor resonators in Table 4. We fabricated our CPW by NbN sputter deposition without heating, which causes a simpler and more robust fabrication procedure compared to atomic layer deposition (ALD) and heating sputtering. Note that the recent goal in quantum circuits research is to reduce the chip footprint, which we also move towards by design and fabrication of λ/4\lambda/4 resonators. To reduce the oxidation of NbN, we used CF4_4 and Ar gases since they are less susceptible to introducing unwanted defects and material added to our superconducting thin film. However, more studies on how the etching gas influences the internal quality factors will be worth investigating.

ArticleWidthGapThicknessTypeMetal depositionEtching
Carter et al [27]12 μm12\,\mathrm{\mu m}8 μm8\,\mathrm{\mu m}300 nm300\,\mathrm{nm}λ/4\lambda/4DC magnetron sputtering + 140 ∘C140\,^{\circ}\mathrm{C} heatingSF₆/CHF₃
Yu et al [28]2 μm2\,\mathrm{\mu m}2 μm2\,\mathrm{\mu m}10 nm10\,\mathrm{nm}λ/2\lambda/2DC magnetron sputteringO₂/SF₆
Wei et al [63]----6 nm6\,\mathrm{nm}λ/2\lambda/2DC magnetron sputteringRIE
Sheagren et al [29]>2 μm>2\,\mathrm{\mu m}--4 nm4\,\mathrm{nm} to 30 nm30\,\mathrm{nm}--Atomic Layer depositionCF₄/CHF₃
Foshat et al [this work]4 μm4\,\mathrm{\mu m}2 μm2\,\mathrm{\mu m}100 nm100\,\mathrm{nm}λ/4\lambda/4SputteringCF₄/Ar

Table 4. Comparison of NbN-based microwave coplanar waveguide resonator design, and fabrication.

Regarding design parameters, we choose 100 nm film thickness for two reasons: not only does 100 nm NbN superconducting thin film have a lower kinetic inductance, and is more robust against noises sources in the cryogenic measurement setup in comparison with thinner films, but it also gives a more robust internal quality factor after applying magnetic fields in comparison to bulk superconducting film [27, 28]. Our resonator has stayed in the middle range of film thickness 4 nm<t<300 nm4\ \mathrm{nm} < t < 300\ \mathrm{nm}. However, finding a sweet spot in NbN film thickness will be worth more investigation. Moreover, we compare our resonator internal quality factor QiQ_i in single photon and high power regimes to recent works to further understand the performance of NbN superconducting resonators.

The results are shown in Table 5. We find that at single photon regime, the QiQ_i is in line with the latest research on superconducting NbN coplanar waveguide resonators, which confirms the reliability of the fabrication process and measurements at different magnetic fields and temperatures.

ArticleTemperatureSingle photon QiQ_iHigh power QiQ_i
Carter et al [27]200 mK200\,\mathrm{mK}4.2×1054.2 \times10^{5}1.7×1061.7 \times10^{6}, <nph>=106<n_{ph}>=10^{6}
Yu et al [28]8 mK8\,\mathrm{mK}10410^{4}10610^{6}, <nph>=105<n_{ph}>=10^{5}
Wei et al [63]30 mK30\,\mathrm{mK}7.5×1047.5 \times10^{4}5×1055 \times10^{5}, <nph>=104<n_{ph}>=10^{4}
Sheagren et al [29]300 mK300\,\mathrm{mK}-->105>10^{5}
Foshat et al [this work]100 mK100\,\mathrm{mK}1.35×1051.35 \times10^{5}1.07×1061.07 \times10^{6}, <nph>=2.7×104<n_{ph}>=2.7 \times10^{4}

Table 5. Comparison of NbN-based coplanar waveguide resonator microwave response detail.

In terms of QiQ_i at high power regime, our resonator has the second highest QiQ_i value, even though we measured at far lower photon number and temperature than Carter, Faustin W., et al work. Our work in NbN based circuits is the first research demonstrating resonance frequency shift and internal quality factor behaviour as a function of temperature from the TLS loss to the quasi-particle loss ranges.

Meanwhile, although we obtained a high internal quality factor, we have not used artificial pinning in our circuit design, leading to a quicker and easier e-beam lithography procedure.

These comparisons confirm that our approach in designing, fabricating, and characterising NbN superconducting CPW is a step towards developing high internal quality factor resonators useful for quantum technology from quantum computing to quantum sensing and metrology.

Conclusion

In summary, we reported the successful design, fabrication and microwave spectroscopy of arrays of CPWs based on superconducting NbN on silicon chips in the cryogenic environment. We studied resonator parameters as a function of microwave power, temperature, and magnetic fields. We studied TLS, quasiparticles, magnetic fields, and temperature-independent losses to identify the loss mechanism in our superconducting circuits. At low temperatures (T=100T = 100 mK), the range in which TLS loss is the dominant reason for the rising loss in CPWs, the quality factor increases from Qi∼1.35×105Q_i \sim1.35 \times10^{5} in the single photon regime to Qi∼1.07×106Q_i \sim1.07 \times10^{6} at high powers. Sweeping temperature from T=100T = 100 mK to 3 K in the single photon regime also confirms that TLS loss decreases when the TLS defects saturate in the energy bands. Moreover, in higher temperatures, the range in which quasiparticle loss is dominant, QiQ_i reduces from 2.571×1052.571 \times10^{5} at T∼1T \sim1 K to 7.421×1037.421 \times10^{3} at T∼3T \sim3 K. To examine the suitability of such superconducting circuits for cQED at high magnetic fields, we studied the microwave response of our CPWs to in-plane magnetic fields B∥B_{\parallel}. Our results showed that the peak of S21S_{21} is stable in the magnetic field ranges between B∥=0B_{\parallel} = 0 mT to 240 mT at T=100T = 100 mK. We extracted Qi>2×104Q_i > 2 \times10^{4} at single photon when B∥=240B_{\parallel} = 240 mT. Our results shall help the development of superconducting microwave quantum circuits compatible with high magnetic fields necessary for applications in fault-tolerant quantum computing, quantum sensing, and quantum metrology.

Acknowledgment

This work was supported in part by the Royal Society Research under Grant RGS/R2/222168, the Research Fellowship from the Royal Society of Edinburgh (K Delfanazari), the Innovate UK (QTools, grant No 79373 and FABU, grant No 50868), the EPSRC Quantum Computing Hub EP/T001062/1, and by the FET Open initiative from the European Union’s Horizon 2020 program under N° 899561. The discussion with Dr A. Sultanov is greatly appreciated.

Appendix

Microwave spectroscopy setup

Figure S.1. (a) Adiabatic demagnetisation refrigerator (ADR) experimental setup schematic used to perform microwave and magnetic field measurements with NbTiN superconducting solenoid, Cean is the current source of NbTi solenoid. (b) Schematic of the dilution refrigerator used to perform microwave measurements.

References

  1. [1]Clerk, A., et al., Hybrid quantum systems with circuit quantum electrodynamics. Nature Physics, 2020. 16(3): p. 257-267.
  2. [2]Blais, A., et al., Quantum-information processing with circuit quantum electrodynamics. Physical Review A, 2007. 75(3): p. 032329.
  3. [3]Frunzio, L., et al., Fabrication and characterization of superconducting circuit QED devices for quantum computation. IEEE transactions on applied superconductivity, 2005. 15(2): p. 860-863.DOI
  4. [4]Danilin, S., N. Nugent, and M. Weides, Quantum sensing with tuneable superconducting qubits: optimization and speed-up. arXiv preprint arXiv:2211.08344, 2022.arxiv.org/abs/2211.08344
  5. [5]Degen, C.L., F. Reinhard, and P. Cappellaro, Quantum sensing. Reviews of modern physics, 2017. 89(3): p. 035002.
  6. [6]Lita, A.E., et al., Development of Superconducting Single-Photon and Photon-Number Resolving Detectors for Quantum Applications. Journal of Lightwave Technology, 2022. 40(23): p. 7578-7597.DOI
  7. [7]Earnest, C.T., et al., Substrate surface engineering for high-quality silicon/aluminum superconducting resonators. Superconductor Science and Technology, 2018. 31(12): p. 125013.DOI
  8. [8]McRae, C., et al., Thin film metrology and microwave loss characterization of indium and aluminum/indium superconducting planar resonators. Journal of Applied Physics, 2018. 123(20): p. 205304.DOI
  9. [9]de Leon, N.P., et al., Materials challenges and opportunities for quantum computing hardware. Science, 2021. 372(6539): p. eabb2823.DOI
  10. [10]Arute, F., et al., Quantum supremacy using a programmable superconducting processor. Nature, 2019. 574(7779): p. 505-510.DOI
  11. [11]Koch, J., et al., Charge-insensitive qubit design derived from the Cooper pair box. Physical Review A, 2007. 76(4): p. 042319.DOI
  12. [12]Harvey, S., et al., Coupling two spin qubits with a high-impedance resonator. Physical Review B, 2018. 97(23): p. 235409.
  13. [13]Behera, B.K., et al., Designing quantum router in IBM quantum computer. Quantum Information Processing, 2018. 18(11): p. 1-13.
  14. [14]McRae, C.R.H., et al., Materials loss measurements using superconducting microwave resonators. Review of Scientific Instruments, 2020. 91(9): p. 091101.DOI
  15. [15]Burnett, J., et al. Noise and loss of superconducting aluminium resonators at single photon energies. in Journal of Physics: Conference Series. 2018. IOP Publishing.DOI
  16. [16]Wisbey, D.S., et al., Effect of metal/substrate interfaces on radio-frequency loss in superconducting coplanar waveguides. Journal of Applied Physics, 2010. 108(9): p. 093918.DOI
  17. [17]Higginbotham, A.P., et al., Parity lifetime of bound states in a proximitized semiconductor nanowire. Nature Physics, 2015. 11(12): p. 1017-1021.DOI
  18. [18]Burnett, J., L. Faoro, and T. Lindström, Analysis of high quality superconducting resonators: consequences for TLS properties in amorphous oxides. Superconductor Science and Technology, 2016. 29(4): p. 044008.DOI
  19. [19]Oliver, W.D. and P.B. Welander, Materials in superconducting quantum bits. MRS bulletin, 2013. 38(10): p. 816-825.
  20. [20]O’Connell, A.D., et al., Microwave dielectric loss at single photon energies and millikelvin temperatures. Applied Physics Letters, 2008. 92(11): p. 112903.
  21. [21]Macha, P., et al., Losses in coplanar waveguide resonators at millikelvin temperatures. Applied Physics Letters, 2010. 96(6): p. 062503.DOI
  22. [22]Woods, W., et al., Determining interface dielectric losses in superconducting coplanar-waveguide resonators. Physical Review Applied, 2019. 12(1): p. 014012.
  23. [23]Wang, H., et al., Improving the coherence time of superconducting coplanar waveguide resonators. Applied Physics Letters, 2009. 95(23): p. 233508.DOI
  24. [24]Lahtinen, V. and M. Möttönen, Effects of device geometry and material properties on dielectric losses in superconducting coplanar-waveguide resonators. Journal of Physics: Condensed Matter, 2020. 32(40): p. 405702.DOI
  25. [25]Sage, J.M., et al., Study of loss in superconducting coplanar waveguide resonators. Journal of Applied Physics, 2011. 109(6): p. 063915.
  26. [26]Verjauw, J., et al., Investigation of microwave loss induced by oxide regrowth in high-Q niobium resonators. Physical Review Applied, 2021. 16(1): p. 014018.DOI
  27. [27]Carter, F.W., et al., Low-loss single-photon NbN microwave resonators on Si. Applied Physics Letters, 2019. 115(9): p. 092602.DOI
  28. [28]Yu, C.X., et al., Magnetic field resilient high kinetic inductance superconducting niobium nitride coplanar waveguide resonators. Applied Physics Letters, 2021. 118(5): p. 054001.DOI
  29. [29]Sheagren, C., et al., Atomic layer deposition niobium nitride films for high-Q resonators. Journal of Low Temperature Physics, 2020. 199(3): p. 875-882.
  30. [30]Foshat, P., et al., Nitride-based superconducting microwave coplanar waveguide resonators with internal quality factors above one million for circuit quantum electrodynamics. Bulletin of the American Physical Society, 2023.
  31. [31]Li, H., et al., Experimental demonstrations of high-Q superconducting coplanar waveguide resonators. Chinese Science Bulletin, 2013. 58(20): p. 2413-2417.
  32. [32]De Visser, P., et al., Evidence of a nonequilibrium distribution of quasiparticles in the microwave response of a superconducting aluminum resonator. Physical review letters, 2014. 112(4): p. 047004.
  33. [33]Valenti, F., et al., Interplay between kinetic inductance, nonlinearity, and quasiparticle dynamics in granular aluminum microwave kinetic inductance detectors. Physical review applied, 2019. 11(5): p. 054087.DOI
  34. [34]Goetz, J., et al., Loss mechanisms in superconducting thin film microwave resonators. Journal of Applied Physics, 2016. 119(1): p. 015304.
  35. [35]Amin, K.R., et al., Loss mechanisms in TiN high impedance superconducting microwave circuits. Applied Physics Letters, 2022. 120(16): p. 164001.
  36. [36]Nsanzineza, I. and B. Plourde, Trapping a single vortex and reducing quasiparticles in a superconducting resonator. Physical review letters, 2014. 113(11): p. 117002.
  37. [37]Gustavsson, S., et al., Suppressing relaxation in superconducting qubits by quasiparticle pumping. Science, 2016. 354(6319): p. 1573-1577.DOI
  38. [38]Taupin, M., et al., Tunable quasiparticle trapping in Meissner and vortex states of mesoscopic superconductors. Nature communications, 2016. 7(1): p. 1-7.DOI
  39. [39]Aguado, R., A perspective on semiconductor-based superconducting qubits. Applied Physics Letters, 2020. 117(24): p. 240501.DOI
  40. [40]Delfanazari, K., et al., On-Chip Andreev Devices: Hard Superconducting Gap and Quantum Transport in Ballistic Nb–In0.75Ga0.25As-Quantum-Well–Nb Josephson Junctions. Advanced Materials, 2017. 29(37): p. 1701836.DOI
  41. [41]Delfanazari, K., et al., On-chip hybrid superconducting-semiconducting quantum circuit. IEEE Transactions on Applied Superconductivity, 2018. 28(4): p. 1-4.DOI
  42. [42]Aasen, D., et al., Milestones toward Majorana-based quantum computing. Physical Review X, 2016. 6(3): p. 031016.DOI
  43. [43]Prada, E., et al., From Andreev to Majorana bound states in hybrid superconductor–semiconductor nanowires. Nature Reviews Physics, 2020. 2(10): p. 575-594.
  44. [44]Chen, J., et al., Ubiquitous non-Majorana zero-bias conductance peaks in nanowire devices. Physical Review Letters, 2019. 123(10): p. 107703.
  45. [45]Zuo, K., et al., Supercurrent interference in few-mode nanowire Josephson junctions. Physical review letters, 2017. 119(18): p. 187704.DOI
  46. [46]Estrada Saldaña, J., et al., Charge localization and reentrant superconductivity in a quasi-ballistic InAs nanowire coupled to superconductors. Science advances, 2019. 5(7): p. eaav1235.DOI
  47. [47]Kanne, T., et al., Epitaxial Pb on InAs nanowires for quantum devices. Nature Nanotechnology, 2021. 16(7): p. 776-781.DOI
  48. [48]Bothner, D., et al., Improving the performance of superconducting microwave resonators in magnetic fields. Applied Physics Letters, 2011. 98(10): p. 102504.DOI
  49. [49]Borisov, K., et al., Superconducting granular aluminum resonators resilient to magnetic fields up to 1 Tesla. Applied Physics Letters, 2020. 117(12): p. 120502.DOI
  50. [50]Bothner, D., et al., Improving superconducting resonators in magnetic fields by reduced field focussing and engineered flux screening. Physical Review Applied, 2017. 8(3): p. 034025.DOI
  51. [51]Baity, P.G., et al., Strong magnon–photon coupling with chip-integrated YIG in the zero-temperature limit. Applied Physics Letters, 2021. 119(3): p. 033502.DOI
  52. [52]Banerjee, A., et al., Optical properties of refractory metal based thin films. Optical Materials Express, 2018. 8(8): p. 2072-2088.
  53. [53]Petersan, P.J. and S.M. Anlage, Measurement of resonant frequency and quality factor of microwave resonators: Comparison of methods. Journal of applied physics, 1998. 84(6): p. 3392-3402.
  54. [54]Deng, C., M. Otto, and A. Lupascu, An analysis method for transmission measurements of superconducting resonators with applications to quantum-regime dielectric-loss measurements. Journal of Applied Physics, 2013. 114(5): p. 054504.DOI
  55. [55]Khalil, M.S., et al., An analysis method for asymmetric resonator transmission applied to superconducting devices. Journal of Applied Physics, 2012. 111(5): p. 054510.DOI
  56. [56]Gao, J., The physics of superconducting microwave resonators. 2008: California Institute of Technology.
  57. [57]Sanchez, M., E. Martin, and J. Zamarro. New vectorial automatic technique for characterisation of resonators. in IEE Proceedings H (Microwaves, Antennas and Propagation). 1989. IET.DOI
  58. [58]Probst, S., et al., Efficient and robust analysis of complex scattering data under noise in microwave resonators. Review of Scientific Instruments, 2015. 86(2): p. 024706.DOI
  59. [59]Bruno, A., et al., Reducing intrinsic loss in superconducting resonators by surface treatment and deep etching of silicon substrates. Applied Physics Letters, 2010. 106(18): p. 182601.
  60. [60]Göpl, M., et al., Coplanar waveguide resonators for circuit quantum electrodynamics. Journal of Applied Physics, 2008. 104(11): p. 113904.
  61. [61]Annunziata, A.J., et al., Tunable superconducting nanoinductors. Nanotechnology, 2010. 21(44): p. 445202.DOI
  62. [62]Niepce, D., J. Burnett, and J. Bylander, High kinetic inductance Nb N nanowire superinductors. Physical Review Applied, 2019. 11(4): p. 044014.DOI
  63. [63]Wei, X.-Y., et al., Compact NbN resonators with high kinetic inductance. Chinese Physics B, 2020. 29(12): p. 128401.
  64. [64]Barends, R., et al., Minimizing quasiparticle generation from stray infrared light in superconducting quantum circuits. Applied Physics Letters, 2011. 99(11): p. 113507.DOI
  65. [65]Scigliuzzo, M., et al., Phononic loss in superconducting resonators on piezoelectric substrates. New Journal of Physics, 2020. 22(5): p. 053027.DOI
  66. [66]Götz, K., et al., Co-sputtered MoRe thin films for carbon nanotube growth-compatible superconducting coplanar resonators. Nanotechnology, 2016. 27(13): p. 135202.DOI
  67. [67]Alexander, A., C.G. Weddle, and C.J. Richardson, Power and temperature dependent model for High Q superconductors. arXiv preprint arXiv:2205.06291, 2022.DOI
  68. [68]Kuit, K., et al., Vortex trapping and expulsion in thin-film YBa 2 Cu 3 O 7− δ strips. Physical Review B, 2008. 77(13): p. 134504.
  69. [69]Stan, G., S.B. Field, and J.M. Martinis, Critical field for complete vortex expulsion from narrow superconducting strips. Physical review letters, 2004. 92(9): p. 097003.
  70. [70]Samkharadze, N., et al., High-kinetic-inductance superconducting nanowire resonators for circuit QED in a magnetic field. Physical Review Applied, 2016. 5(4): p. 044004.DOI
  71. [71]Engel, A., et al., Temperature-dependence of detection efficiency in NbN and TaN SNSPD. IEEE transactions on applied superconductivity, 2013. 23(3): p. 2300505-2300505.DOI
  72. [72]Knehr, E., et al., Nanowire single-photon detectors made of atomic layer-deposited niobium nitride. Superconductor Science and Technology, 2019. 32(12): p. 125007.DOI

Paper details

vlnc:W_dy4r8jpt
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents