WorksPhysics and Astronomy
A first-principles investigation of the linear thermal expansion coefficients of BeF: Giant thermal expansion
Abstract
We present the results of a theoretical investigation of the linear thermal expansion coefficients (TECs) of BeF, within a direct Gruneisen formalism where symmetry-preserving deformations are employed. The required physical quantities such as the optimized crystal structures, elastic constants, mode Gruneisen parameters, and phonon density of states are calculated from first-principles. BeF shows an extensive polymorphism at low pressures, and the lowest energy phases [-cristobalite with space group (SG) P and its similar phase with SG P] are considered in addition to the experimentally observed -quartz phase. For benchmarking purposes, similar calculations are performed for the rutile phase of ZnF, where the volumetric TEC (), derived from the calculated linear TECs along the () and () directions, is in very good agreement with experimental data and previous theoretical results. For the considered phases of BeF, we do not find any negative thermal expansion (NTE). However we observe diverse thermal properties for the distinct phases. The linear TECs are very large, especially of the -cristobalite phase and its similar phase, leading to giant ( at 300 K). The giant arises from large Gruneisen parameters of low-frequency phonon modes, and the C13 elastic constant that is negatively signed and large in magnitude for the -cristobalite phase. The elastic constants, high-frequency dielectric constants, Born effective charge tensors, and thermal properties of the above phases of BeF are reported for the first time and hence serve as predictions.
Introduction
Beryllium fluoride () is known to exist in glass and crystalline phases and has a variety of technological applications. glass has a large bandgap of about 13.8 eV, the lowest refractive index and highest Abbe number of any inorganic material, and exceptional resistance to damage. These properties have enabled the manufacturing of special glasses [from and its mixtures with fluorides and other difluorides] that have excellent transmittance in the UV region[1, 2] and for use in high-power laser systems[3]. The LiF– mixture is a primary coolant and fuel solvent in molten salt nuclear reactors[4]. In protein crystallography, is used to restrict protein motion to facilitate the crystallography process[5]. Very recently, crystalline is predicted to be a better neutron filter than , which has been considered an effective neutron filter candidate[6]. The main aim of this work is to investigate, for the first time, the linear thermal expansion coefficients (TECs) of a few low-energy crystalline phases of . We also consider a benchmark system that has exceptional electric and optical properties, and interesting technological applications ranging from catalysis to spectroscopy and laser applications[7].
Single crystal has been grown and found to have a crystal structure remarkably similar to that of the -quartz () structure[8], which has a trigonal symmetry with space group (SG) (#152). A recent first-principles study has revealed that shows extensive polymorphism at low pressures[9]. Interestingly, three crystal phases [namely, (i) the -cristobalite phase that has a tetragonal symmetry with SG (#92), (ii) a similar phase to the -cristobalite phase (hereafter referred to as the -cristobalite phase) with SG (#96) , and (iii) the -2 4 phase with SG (#15)] are predicted to be energetically more stable than -quartz. However, these phases have a very small stability pressure range (less than 0.4 GPa), and the -quartz phase transforms to the coesite-I phase SG at 3.1 GPa. The high-pressure phases of have been the subject of other first-principles calculations[10]. Very recently, first-principles calculations have also been employed to construct the - phase diagram of [11]. The HSE06 optical bandgap of the -quartz structure is found to be about 10.6 eV, and increases by increasing the applied pressure[9]. The lattice vibrations, inelastic scattering cross-sections, and neutron transmission of BeF have been thoroughly investigated[6] using first-principles calculations and compared to those of MgF.
The benchmark system ZnF crystallizes in the tetragonal rutile structure with SG (#136). Very recently, Raman scattering measurements with the use of the diamond anvil cell have been employed to investigate the structural phase transformations of ZnF under high pressures[12]. This experimental work is supplemented by first-principles calculations. In addition to the structural stability and pressure variation of the Raman active phonon modes, the electronic bandgap of the considered phases as a function of pressure has been investigated at the HSE06 level. Neutron diffraction has been employed to study the temperature dependence of the lattice parameters and unit cell volume of ZnF[13], and NTE has been observed in a small temperature range (below 75 K). This NTE behavior has been supported by first-principles calculations[13, 14]. However, only the volumetric TEC has been theoretically investigated.
In the present work, the linear TECs of BeF and ZnF are investigated by employing the recently introduced direct approach[15] in which the symmetry of the deformed structures could be preserved. Since this approach has not been applied to systems with tetragonal symmetry, ZnF is thus chosen as a suitable benchmark system because of its tetragonal crystal structure, in addition to the existence of experimental and previous theoretical results of its volumetric thermal expansion. The elastic constants and phonon frequencies required to compute linear TECs are calculated from first-principles. For BeF, the -quartz, -cristobalite and -cristobalite phases are considered. Moreover, the relative stability of the above three phases of BeF will be also investigated using different levels of approximation of the exchange-correlation potential.
Methodology
The linear TECs of the considered phases of ZnF and BeF are calculated within the Grüneisen formalism following the procedure described in Refs. [16, 17, 18, 19, 20, 21, 22]. To compute the mode Grüneisen parameters we considered two types of symmetry-preserving deformations obtained by changing the in-plane () or out-of-plane () lattice parameters by . These deformations allow for the full utilization of the tetragonal or trigonal point-group symmetry[23] of the considered systems, which minimizes the required number of independent atomic displacements (i.e., number of supercells) to calculate the phonon frequencies within the direct method[24, 25, 26, 27, 28]. The amplitude of atomic displacements, from the corresponding equilibrium positions, is 0.015 Å. The supercell sizes are of for ZnF, and for the -quartz, -cristobalite, and -cristobalite phases of BeF. The adequacy of these supercells have been checked by considering larger ones for each of these systems, and we found that such actions do not alter appreciably our main results and conclusions. The determination of the linear TECs also requires the elastic constants that may be obtained through fittings of energy versus strain curves[29, 30]. Specifically, these TECs at temperature in the () and () directions of the above systems are given by
where are the elastic constants, and is the volume of the primitive cell. The phonon density of states (PDOS) weighted by the Grüneisen parameters are
with the Grüneisen parameter for the deformation of type (with for in-plane and for out-of-plane deformations). The derivative measures the change of the frequency with respect to the strain parameter [15]. The summation is over all frequencies for the phonon band index and vector in the Brillouin zone (BZ). The are calculated from
where is the contribution of the phonon modes with frequency to the specific heat. Here, , and and are the Planck and Boltzmann constants, respectively. The maximum (minimum) frequency is denoted by ().
The DFT calculations of the optimized structural parameters, phonon frequencies, and elastic constants are performed by employing the projector augmented wave (PAW) method, as implemented in the Vienna Ab-Initio Simulation Package (VASP). A relatively high cutoff energy of 600 eV is used for the plane-wave basis. Geometry optimization is stopped when the maximum force on each atom is less than eV/Å. We find that phonon frequency shifts are more consistent when we use the local density approximation (LDA) for BeF, and the PBE_sol functional of the generalized gradient approximation (GGA) for ZnF. Therefore, for the linear TECs only the results of these calculations are reported.
| Phase | Approach | (Å) | (Å) | (meV) | ||||
| -quartz | LDA | 4.5958 | 5.0529 | 0.4579 | 0.4098 | 0.2867 | 0.2290 | |
| PBE_sol | 4.7301 | 5.1814 | 0.4662 | 0.4138 | 0.2737 | 0.2188 | ||
| PBE | 4.8497 | 5.3070 | 0.4756 | 0.4176 | 0.2575 | 0.2053 | ||
| PBE[6] | 4.8282 | 5.2837 | 0.4740 | 0.4171 | 0.2601 | 0.2075 | ||
| LDA[31] | 4.6663 | 5.1608 | ||||||
| Expt.[8] | 4.7390 | 5.1875 | 0.4700 | 0.4164 | 0.2671 | 0.2131 | ||
| -cristobalite | LDA | 4.5967 | 6.1773 | 0.3226 | 0.2230 | 0.1454 | 0.2000 | 25 |
| PBE_sol | 4.8087 | 6.5984 | 0.3044 | 0.2378 | 0.1112 | 0.1825 | ||
| PBE | 4.8934 | 6.7428 | 0.2988 | 0.2400 | 0.1001 | 0.1769 | ||
| LDA[31] | 4.695 | 6.318 | ||||||
| LDA[11] | 4.684 | 6.373 | ||||||
| PBE[11] | 4.960 | 6.910 |
Table 1. Calculated lattice constants and internal parameters of the -quartz and -cristobalite phases of BeF. Also shown are the relative energy () of the -cristobalite phase with respect to that of -quartz, and the available experimental data (measured at 100 K) and other theoretical results.
Results and discussion
Structural properties
We start with the benchmark system, ZnF, which at ambient conditions crystallizes in the rutile structure, shown in Figure 1(a). This crystal structure has a tetragonal symmetry and six atoms per primitive unit cell. The two Zn atoms occupy the Wyckoff sites and the four F atoms are located at the sites. Therefore, this structure is characterized by three crystallographic parameters: two lattice parameters ( and ) and an internal parameter for the coordinates of the four F atoms (). The structural parameters obtained using the PBE_sol functional are Å, Å, , while the corresponding LDA results are Å, Å, . These calculated values are in very good agreement with the experimental data Å, Å, [32] and Å, Å, [13]. As expected, the LDA lattice parameters are underestimated while those of the PBE_sol are slightly overestimated.

Figure 1. The crystal structures of (a) rutile ZnF, (b) -quartz BeF, and (c) -cristobalite BeF. The -cristobalite BeF structure which is similar to the -cristobalite BeF structure is not shown. The small gray balls represent the F atoms. The axis of the three crystal structures is along the vertical direction.
| System | Phase | Approach | |||||||
| BeF | -quartz | LDA | 46.975 | 14.223 | 12.067 | −6.401 | 75.287 | 31.745 | |
| PBE_sol | 42.278 | 4.991 | 3.760 | −9.077 | 53.009 | 30.548 | |||
| -cristobalite | LDA | 33.309 | 7.300 | −5.087 | 22.487 | 35.810 | 13.731 | ||
| PBE_sol | 32.589 | 4.839 | −5.336 | 24.412 | 37.813 | 16.078 | |||
| ZnF | Rutile | LDA | 139.442 | 121.550 | 109.127 | 220.673 | 36.583 | 91.826 | |
| PBE_sol | 128.470 | 98.717 | 94.547 | 200.902 | 35.523 | 83.001 | |||
| Expt.[33] | 125.5 | 91.8 | 83.0 | 192.2 | 39.5 | 80.7 |
Table 2. Calculated elastic constants of the -quartz and -cristobalite phases of BeF, and the rutile phase of ZnF.
For BeF, the three considered crystal structures are -quartz [Fig.1(b)], -cristobalite [Fig.1(c)] and -cristobalite. The -quartz phase has trigonal symmetry and nine atoms in the conventional hexagonal unit cell. The three Be atoms occupy the Wyckoff sites and the six F atoms occupy the sites. On the other hand, the -cristobalite phase has a tetragonal symmetry and twelve atoms per primitive unit cell. The four Be atoms occupy the Wyckoff sites and the eight F atoms occupy the sites. Therefore, each of these two structures has six crystallographic parameters: two lattice parameters ( and ), and four internal parameters (denoted as , , and ). The atomic coordinates of the -cristobalite phase can be obtained from those of the -cristobalite by mirror-image transformation , and the lattice parameters of the two structures are identical. Therefore, only the structure parameters of the first two crystal structures are reported. Our LDA, PBE_sol, and PBE results, shown in Table I, are in good agreement with available experimental data and other theoretical calculations. The PBE_sol results lie between the corresponding LDA and PBE results and show the best agreement with the experimental data for the -quartz.
Elastic properties and stability
We show in Table I the LDA, PBE_sol and PBE relative energies () of the -cristobalite phase with respect to those of -quartz. According to the PBE and PBE_sol calculations the latter phase is slightly more stable, in accordance with the Nelson et al. [9] GGA calculations. However, the LDA calculations lead to an opposite conclusion. Similar conclusions have recently been reached by Masoumi [11], using both LDA and GGA calculations. These results show that these two phases have extremely close cohesive energies.
The -quartz phase of BeF with a trigonal crystal symmetry has six independent elastic constants[34]. On the other hand, the rutile phase of ZnF and -cristobalite phase of BeF (both have a tetragonal crystal symmetry) also have six independent elastic constants[34]. The elastic constants of these phases, obtained by using the LDA and PBE_sol functionals are shown in Table II. There are two features to note from this table. First, our results for the rutile ZnF are in very good agreement with the available experimental values[33]. Secondly, the PBE_sol values are systematically smaller than the corresponding LDA values, which is expected since the PBE_sol GGA functional leads to softer materials than LDA (see above). The calculated elastic constants are used in the calculations of the linear TECs (see § 1.1).
The elastic constants could be used to investigate the mechanical stability of the crystal structure. For -quartz structure, the Born stability criteria[34] are
and
Note that the same expression of appears in Eq. (1). As for the rutile and -cristobalite phases (of tetragonal (I) class)[35], the Born stability criteria are: , , and . The elastic constants reported in
| System | Phase | Approach | DC | atom | Born effective charge | |||||||||
| BeF | AQ | PBE_sol | 1.902 | 1.912 | Be | 1.728 | 0.000 | 0.000 | 0.000 | 1.914 | 0.081 | 0.000 | −0.079 | 1.866 |
| F | −0.747 | 0.221 | −0.115 | 0.213 | −1.074 | 0.337 | −0.095 | 0.345 | −0.933 | |||||
| LDA | 1.887 | 1.896 | Be | 1.727 | 0.000 | 0.000 | 0.000 | 1.918 | 0.080 | 0.000 | −0.0758 | 1.864 | ||
| F | −0.746 | 0.226 | −0.124 | 0.218 | −1.076 | 0.343 | −0.104 | 0.356 | −0.932 | |||||
| BeF | AC | PBE_sol | 1.723 | 1.718 | Be | 1.832 | 0.005 | −0.045 | 0.005 | 1.832 | 0.049 | 0.100 | −0.101 | 1.810 |
| F | −1.221 | −0.117 | 0.377 | −0.101 | −0.611 | 0.061 | 0.380 | 0.100 | −0.905 | |||||
| LDA | 1.827 | 1.818 | Be | 1.823 | 0.005 | −0.036 | 0.005 | 1.823 | 0.036 | 0.110 | −0.110 | 1.790 | ||
| F | −1.199 | −0.135 | 0.329 | −0.120 | −0.624 | 0.076 | 0.333 | 0.115 | −0.896 | |||||
| ZnF | Rutile | PBE_sol | 2.549 | 2.664 | Zn | 2.222 | −0.162 | 0.000 | −0.162 | 2.222 | 0.00 | 0.000 | 0.000 | 2.424 |
| F | −1.111 | −0.409 | 0.000 | −0.409 | −1.111 | 0.000 | 0.000 | 0.000 | −1.200 | |||||
| LDA | 2.547 | 2.653 | Zn | 2.206 | −0.1493 | 0.000 | −0.1493 | 2.206 | 0.000 | 0.000 | 0.000 | 2.392 | ||
| F | −1.103 | −0.395 | 0.000 | −0.395 | −1.103 | 0.000 | 0.000 | 0.000 | −1.196 | |||||
| Expt.[36] | 2.6 | 2.1 |
Table 3. Calculated high-frequency dielectric constants (DCs) and Born effective charges of the -quartz (AQ) and -cristobalite (AC) phases of BeF, and the rutile phase of ZnF.
Table II show that these criteria are satisfied, and therefore the considered phases of ZnF and BeF are mechanically stable. The mechanical stability of these crystal structures can also be inferred from phonon dispersion relations, discussed below.
C Phonon dispersion relations
Since the considered crystals are polar in character we perform non-analytical correction (NAC) to their dynamical matrices. To do that, we have calculated the high-frequency dielectric constant and Born effective charge tensors, and the results are listed in Table III. The features to note from this table are the following. (i) The calculated results have a very weak dependence on the used exchange-correlation functional. (ii) The effective charges in the ZnF are larger than in BeF, which shows that the ionicity of Zn-F bond is larger than that in Be-F. This is consistent with the corrected Allred-Rochow electronegativity values[39] (larger for Be). (iii) Our calculated and components of the dielectric constant are in very good agreement with available experimental data[36], while that of is larger than the measured one. However, the comparable values of diagonal components of the dielectric constant in our calculations are consistent with the experimental and calculated values for other metal fluorides crystallizing in the rutile structure (such as MgF and FeF)[40].
Figure 2 shows the calculated phonon dispersion relations and PDOS of the rutile ZnF, with and without NAC. Also shown are the calculated Zn and F projected PDOS, with NAC, and the available experimental data[37, 38]. The frequency spans across an interval of about 500 cm. The features to note from this figure are the following. (i) As expected, the NAC leads to longitudinal optical-traverse optical (LO-TO) splitting, near the point. The strongest effects are felt by high-frequency optical modes. However, the effects of the NAC on the calculated PDOS are quite small. (ii) Experimental data are available only for infrared[37] and Raman[12, 38] active modes at the -points. The reported frequencies of the latter modes are in very good agreement with each other, and hence only those of Ref. [38] are shown in Figure 2. For the designation of these phonon modes see Ref.[40]. Fig 2 shows that these experimental data agree reasonably well with our first-principles results.
Figure 2. Calculated phonon dispersion relations and PDOS of ZnF, with (black solid curves) and without (red dashed curves) non-analytic correction (NAC). The Zn and F projected PDOS, with NAC, and also shown. Symbols: available experimental data[37, 38].
Figure 3 shows the phonon dispersion relations of the -quartz and -cristobalite phases of BeF, taking into account the NAC. Also shown are the PDOS, and Be and F projected PDOS of the -cristobalite phase. The results of the -cristobalite phase are very similar to those of -cristobalite and hence are not shown. The features to note from this figure are the following. (i) The very wide frequency range of the phonon modes in these systems, compared to that of ZnF. This can be understood as a consequence of the rather large mass difference between Be and Zn atoms. (ii) The frequency range of both phases of BeF can be separated, according to the character of the phonon modes, into three sub-regions. (a) The lower frequency region between 0 and about 700 cm, where the phonon modes are mainly due to the vibrations of F atoms. The contribution of the Be atoms becomes appreciable above 300 cm. It is worth noting that in the case of ZnF the dominance of the vibrations of the F atoms occurs in the upper part of the frequency range because the Zn atom is heavier than the F atom. (b) A narrow intermediate region at about 770 cm, where the rather localized phonon modes originate from vibrations involving both Be and F atoms. (c) The upper-frequency region, where the phonon modes originate mainly from vibrations of Be atoms. (iii) The opening of two frequency gaps, between (a) and (b), and between (b) and (c) sub-regions. These frequency gaps can be understood as a consequence of the localization of phonon modes in the (b) sub-region.
Figure 3. Calculated phonon dispersion relations of the (a) -quartz and (b) -cristobalite phases of BeF. (c) PDOS, and the Be and F projected PDOS of the -cristobalite phase.
Thermal expansion
The calculated linear and volumetric TECs of the considered phases of ZnF₂ and BeF₂, according to the procedure described in § 1.1, are depicted in Figure 4 and Figure 5, respectively. It is worth mentioning that, as expected, the NACs to the dynamical matrices have negligible effects on the calculated linear TECs.
Figure 4. Calculated linear and volumetric TECs of ZnF₂ using the LDA, compared to the available experimental data[13] and previous theoretical results[13, 14].
Figure 5. Calculated linear and volumetric TECs with PBE sol of the three considered phases of BeF₂. Note the difference in the scales of the two panels.
We will first look at the TECs of ZnF₂. The important features to note from Figure 4 are the following. (i) The NTE at low temperatures is mostly due to . The negative values of are smaller (in magnitude) than those of and lie in a considerably shorter -range. This is clear from the magnitude and the location of the minimum values: at 55 K, and at 40 K. These results are consistent with observed -variations of the and lattice parameters at low temperatures (see Figure 3 of Ref. [13]). (ii) The calculated from the linear TECs (i.e., ) are in good agreement with the previous direct theoretical calculations[13, 14], and the results of all these theoretical calculations are in a qualitative agreement with experimental data[13]. This finding reflects the accuracy and reliability of our calculated linear TECs. (iii) is systematically and appreciably larger than . For example, at 300 K the calculated value of (of ) is about 60% larger than that of (of ).
As for the thermal expansion of the considered phases of BeF₂, the features to note from Figure 5 are the following. (i) Unlike ZnF₂, the calculated values of both and are always positive for all of the considered phases of BeF₂. (ii) Both and of the -cristobalite structure are very close to those of -cristobalite, and hence only those of the former phase will be discussed below. (iii) In the considered -range, of the -quartz structure is slightly larger than , whereas of the -cristobalite phase is much smaller than . (iv) The large and lead to very large for both phases of BeF₂. For example, at 300 K, the values of are of 77.6 and 169.9 respectively for the above two phases of BeF₂, compared to that of 20.0 for ZnF₂. Our largest calculated linear TEC is of at 300 K for of the -cristobalite phase. This is indeed large compared to the experimental linear TECs at 300 K of four fluorites, i.e., CaF₂, SrF₂, BaF₂, and PbF₂[41] that range between 18.1 and 29 , but still is somewhat smaller than the measured linear TEC value of 163.9 of an Ti-Nb alloy[42].
The key physically insightful quantity for the interpretation of the above results is the PDOS weighted by the Grüneisen parameters, , defined in Eq. (2). Figure 6 shows of ZnF, and the -quartz and -cristobalite phases of BeF. The important features to note from this figure are the following. (i) For ZnF, the low-frequency modes () have negative Grüneisen parameters, which lead to negative in this range. Since low-frequency modes are easily thermally excited, this finding explains the observed NTE in ZnF. Moreover, by inspecting the differences between and one can easily understand why is always lower than . (ii) The of the considered phases of BeF are always positive, which reflects the dominance of positive mode Grüneisen parameters in these phases. This explains the lack of NTE in the considered phases of BeF. (iii) The and of -quartz BeF have comparable magnitudes, with being smaller than for , which explain the comparable magnitudes and ordering of its and . (iv) The peak in of the -cristobalite phase around is much higher than that of the , which results in a large compared to . This finding means that, in this -range, the positive mode Grüneisen parameters associated with the out-of-plane deformation are significantly larger than those associated with the in-plane deformation. The large Grüneisen parameters can be viewed as a manifestation of strong anharmonic effects in the -cristobalite and -cristobalite structures of BeF. However, it should be noted that large Grüneisen parameters are not the only factor that is responsible for the giant of the -cristobalite: the elastic property via the negative (and with a large magnitude) elastic constant (see Table II and Eq. (1)) plays also a major role. The above findings explain the much larger volumetric TEC of the -cristobalite phase of BeF, compared to that of the -quartz phase, which, in turn, is larger than that of ZnF.
Figure 6. The PDOS weighted by the Grüneisen parameters of the rutile ZnF₂, and the α-quartz and α-cristobalite phases of BeF₂.
Summary
First-principles calculations are performed to investigate the structural, elastic, and vibrational properties of the rutile structure of ZnF and three crystal structures of BeF (-quartz, -cristobalite and its similar phase with space group ). The so-obtained phonon density of states, mode Grüneisen parameters, and elastic constants are used to study the linear thermal expansion coefficients (TECs) of the compounds mentioned above, within a Grüneisen formalism. We have used deformations that preserve the symmetry of the crystal to obtain the Grüneisen parameters. The considered crystal structures of both systems are found to be mechanically stable. The calculated physical quantities for both systems are in very good agreement with the available experimental data and previous theoretical results. For ZnF, the calculated linear TECs, and , along the and the directions are consistent with the experimental -variations of the corresponding lattice parameters, respectively. The volumetric TEC computed from these linear TECs is in qualitative agreement with experiment at low temperatures, including negative thermal expansion (NTE) behavior. The considered phases of BeF are not NTE materials, and their linear TECs are much higher than those of ZnF, especially for the -cristobalite phase. The elastic constants, high-frequency dielectric constants, Born effective charge tensors, and TECs of the considered phases of BeF are reported in this work for the first time and could serve as predictions.
Acknowledgment
We thank the National Supercomputing Center, Singapore (NSCC) and A*STAR Computational Resource Center, Singapore (ACRC) for computing resources. We also thank Iyad Al-Qasir for fruitful discussions. This work is supported by RIE2020 Advanced Manufacturing and Engineering (AME) Programmatic Grant No A1898b0043.
References
- [1]J. Parker and P. France, in Glasses and glass-ceramics, edited by M. H. Lewis (Chapman and Hall, 2011) p. 156.
- [2]F. Gan, Optical properties of fluoride glasses: a review, Journal of Non-Crystalline Solids 184, 9 (1995).DOI
- [3]M. J. Weber, C. F. Cline, W. L. Smith, D. Milam, D. Heiman, and R. Hellwarth, Measurements of the electronic and nuclear contributions to the nonlinear refractive index of beryllium fluoride glasses, Appl. Phys. Lett. 32, 403 (1978).DOI
- [4]L. Mei, X. Cai, D. Jiang, J. Chen, W. Guo, and W. Xiong, Investigation of thermal neutron scattering data for BeF₂ and LiF crystals, J. Nucl. Sci. Tech. 50, 419 (2013).DOI
- [5]R. Kagawama, M. Montgomery, K. Braig, A. Leslie, and J. Walker, The structure of bovine F₁-ATPase inhibited by ADP and beryllium fluoride, EMBO J. 23, 2734 (2004).
- [6]I. Al-Qasir and A. Qteish, Neutron filter efficiency of beryllium and magnesium fluorides, J. Appl. Cryst. 50, 441 (2017).DOI
- [7]J. K. Kaawar and B. Paulus, A computational study of the structure of zinc fluoride surfaces, AIP Conf. Proc. 1653, 020051 (2015).DOI
- [8]P. Ghalsasi and P. S. Ghalsasi, Single crystal X-ray structure of BeF₂: α-quartz, Inorg. Chem. 50, 86 (2011).DOI
- [9]J. R. Nelson, R. J. Needs, and C. J. Pickard, High-pressure phases of group II difluorides: polymorphism and superionicity, Phys. Rev. B 95, 054118 (2017).DOI
- [10]M. S. Rakitin, A. R. Oganov, H. Niu, M. M. D. Esfahani, X.-F. Zhou, G.-R. Qian, and V. L. Solozhenko, Novel phase of beryllium fluoride at high pressure, Phys. Chem. Chem. Phys. 17, 26283 (2015).DOI
- [11]N. Masoumi, First-principles DFT study of imide and fluoride analogs of silicon oxide, silicon oxynitride, and their alloys, Ph.D. thesis, Arizona State University, Cambridge, MA (2021).
- [12]D. Kurzydłowski, A. Oleksiak, S. B. Pillai, and P. K. Jha, High-pressure phase transitions of zinc difluoride up to 55 GPa, Inorg. Chem. 59, 2584 (2020).DOI
- [13]T. Chatterji, M. Zbiri, and T. C. Hansen, Negative thermal expansion in znf2, Appl. Phys. Lett. 98, 181911 (2011).DOI
- [14]L. Wang, P.-F. Yuan, F. Wang, Q. Sun, E.-J. Liang, and Y. Jia, Theoretical study of negative thermal expansion mechanism of ZnF2, Materials Research Bulletin 47, 1113 (2012).DOI
- [15]C. K. Gan and K. T. E. Chua, Large thermal anisotropy in monoclinic niobium trisulfide: A thermal expansion tensor study, J. Phys.: Condens. Matter 31, 265401 (2019).DOI
- [16]E. Grǖneisen, Handb. Phys. 10, 1 (1926).
- [17]T. H. K. Barron, J. G. Collins, and G. K. White, Thermal expansion of solids at low temperatures, Adv. Phys. 29, 609 (1980).
- [18]P. K. Schelling and P. Keblinski, Thermal expansion of carbon structures, Phys. Rev. B 68, 035425 (2003).
- [19]Y. Ding and B. Xiao, Thermal expansion tensors, Gruneisen parameters and phonon velocities of bulk MT2 (M=W and Mo; T=S and Se) from first principles calculations, RSC Adv. 5, 18391 (2015).DOI
- [20]C. K. Gan, J. R. Soh, and Y. Liu, Large anharmonic effect and thermal expansion anisotropy of metal chalcogenides: The case of antimony sulfide, Phys. Rev. B 92, 235202 (2015).DOI
- [21]G. Liu, H. M. Liu, J. Zhou, and X. G. Wan, Temperature effect on lattice and electronic structures of WTe2 from first-principles study, J. Appl. Phys. 121, 045104 (2017).DOI
- [22]J. Liu and P. B. Allen, Internal and external expansions of wurtzite ZnO from first principles, Comput. Mater. Sci. 154, 251 (2018).DOI
- [23]C. K. Gan, Y. Liu, T. C. Sum, and K. Hippalgaonkar, Efficacious symmetry-adapted atomic displacement method for lattice dynamical studies, Comput. Phys. Comm. 259, 107635 (2021).DOI
- [24]W. Frank, C. Elsässer, and M. Fähnle, Ab initio force-constant method for phonon dispersions in alkali metals, Phys. Rev. Lett. 74, 1791 (1995).pubmed.ncbi.nlm.nih.gov/10057758
- [25]K. Parlinski, Z. Q. Li, and Y. Kawazoe, First-principles determination of the soft mode in cubic ZrO2, Phys. Rev. Lett. 78, 4063 (1997).
- [26]G. Kresse, J. Furthmüller, and J. Hafner, Ab initio force constant approach to phonon dispersion relations of diamond and graphite, Europhys. Lett. 32, 729 (1995).DOI
- [27]C. K. Gan, X. F. Fan, and J.-L. Kuo, Composition-temperature phase diagram of BeₓZn₁₋ₓO from first principles, Comput. Mater. Sci. 49, S29 (2010).DOI
- [28]Y. Liu, K. T. E. Chua, T. C. Sum, and C. K. Gan, First-principles study of the lattice dynamics of Sb2S3, Phys. Chem. Chem. Phys. 16, 345 (2014).DOI
- [29]A. Dal Corso, Elastic constants of beryllium: a first-principles investigation, J. Phys.: Condens. Matter 28, 075401 (2016).DOI
- [30]C. K. Gan and C. H. Lee, Anharmonic phonon effects on linear thermal expansion of trigonal bismuth selenide and antimony telluride crystal, Comput. Mater. Sci. 151, 49 (2018).DOI
- [31]F. Yu, M. Xu, M. Jiang, and J.-X. Sun, The phase transitions and electronic structures of crystalline BeF2 under high-pressure: First-principle calculations, Solid State Commun. 169, 14 (2013).DOI
- [32]N. O’Toole and V. Streltsov, Synchrotron x-ray analysis of the electron density in CoF2 and ZnF2, Acta Cryst. B 57, 128 (2001).pubmed.ncbi.nlm.nih.gov/11262426
- [33]D. S. Rimai, Elastic properties of ZnF2 between 4.2 and 300 K, Phys. Rev. B 16, 4069 (1977).
- [34]W. Pabst and E. C. Gregorová, Elastic properties of silica polymorphs - A review, Ceramics-Silikáty 57, 167 (2013).
- [35]F. Mouhat and F.-X. Coudert, Necessary and sufficient elastic stability conditions in various crystal systems, Phys. Rev. B 90, 224104 (2014).DOI
- [36]E. C. Alaoui-Bichri, J. Giordano, R. Almairac, C. Benoit, and P. Nassiri, Properties, J. Physique 41, 543 (1980).
- [37]J. A. S. Barker, Transverse and longitudinal optic mode study in MgF2 and ZnF2, Phys. Rev. 136, A1290 (1964).
- [38]S. P. S. Porto, P. A. Fleury, and T. C. Damen, Raman spectra of TiO2, MgF2, ZnF2, FeF2, and MnF2, Phys. Rev. 154, 522 (1967).
- [39]A. Qteish, Electronegativity scales and electronegativity-bond ionicity relations: A comparative study, J. Phys. Chem. Solids 124, 186 (2019).DOI
- [40]C. Benoit and J. Giordano, Dynamical properties of crystals of MgF2, ZnF2 and FeF2. II. Lattice dynamics and infrared spectra, J. Phys. C: Solid State Phys 21, 5209 (1988).
- [41]R. B. Roberts and G. K. White, Thermal expansion of fluorites at high temperatures, J. Phys. C: Solid State Phys. 19, 7167 (1986).DOI
- [42]M. Bönisch, A. Panigrahi, M. Stoica, M. Calin, E. Ahrens, M. Zehetbauer, W. Skrotzki, and J. Eckert, Giant thermal expansion and α-precipitation pathways in Ti-alloys, Nature Commun. 8, 1429 (2017).DOI