betaFeedback

WorksPhysics and Astronomy

Pseudosymmetry in Tetragonal Perovskite SrIrO3_3 Synthesized under High Pressure

Abstract

In this study, we report a tetragonal perovskite structure of SrIrO3_3 (P4/mmm, a = 3.9362(9) Å, c = 7.880(3) Å) synthesized at 6 GPa and 1400 °°C, employing the ambient pressure monoclinic SrIrO3_3 with distorted 6H structure as a precursor. The crystal structure of tetragonal SrIrO3 was evaluated on the basis of single crystal and powder X-ray diffraction. A cubic indexing was observed attributed to overlooked superlattice reflections. Weak fractional peaks in the H and K dimensions suggest possible structure modulation by oxygen defects. Magnetization study reveals weak paramagnetic behavior down to 2 K, indicative of the interplay between spin-orbit coupling, electron correlations, and crystal electric field. Additionally, measurements of electrical resistivity display metallic behavior with an upturn at about 54 K, ascribed to weak electron localization and possible structural defects.

Introduction

Iridates is an ideal system for investigating the intriguing quantum physics arising from the significant spin-orbit coupling (SOC). The exotic electronic quantum phenomena primarily arise from the interplay between the robust SOC and other fundamental interactions which have comparable energy scales, including crystal electric field and electron correlations, leading to competition between them. The SOC is typically negligible in the 3d3d transition metal systems. However, in the case of 5d5d transition metal compounds, such as the iridates, the SOC plays a crucial role in the observed physics behaviors, for example, superconductivity[1], Kitaev quantum spin liquid[2], Weyl semimetal behavior[3, 4], quantum criticality[5, 6], and quantum Hall effects[7]. Among iridate compounds, the Ruddlesden–Popper phase Srn+1IrnO3n+1\mathrm{Sr}_{n+1}\mathrm{Ir}_{n}\mathrm{O}_{3n+1}, specifically, Sr2IrO4\mathrm{Sr}_{2}\mathrm{IrO}_{4} (n=1n = 1) and Sr3Ir2O7\mathrm{Sr}_{3}\mathrm{Ir}_{2}\mathrm{O}_{7} (n=2n = 2), have been intensively studied for novel physics with strong SOC on Ir sites.[8, 9, 10, 11, 12]

In Sr2IrO4\mathrm{Sr}_{2}\mathrm{IrO}_{4} and Sr3Ir2O7\mathrm{Sr}_{3}\mathrm{Ir}_{2}\mathrm{O}_{7}, [IrO6][\mathrm{IrO}_{6}] octahedra arrange along the abab-plane forming the two-dimensional patterns. Conversely, owing to the enhanced interlayer hopping induced by the three-dimensional continuous arrangement of [IrO6][\mathrm{IrO}_{6}] octahedra, in comparison with Sr2IrO4\mathrm{Sr}_{2}\mathrm{IrO}_{4} and Sr3Ir2O7\mathrm{Sr}_{3}\mathrm{Ir}_{2}\mathrm{O}_{7} which are insulators with canted antiferromagnetic ordering, SrIrO3\mathrm{SrIrO}_{3} (n=∞n = \infty) exhibits a paramagnetic semimetal ground state.[13, 14] Thus, SrIrO3\mathrm{SrIrO}_{3} is positioned in proximity to a multi-phase boundary where the transitions of metal-insulator and magnetic ground states occur. These transitions are governed by the combination of multiple interactions, resulting in a complex interplay of competing effects.[13]

Instead of the bulk, most of current SrIrO3\mathrm{SrIrO}_{3} studies focus on constructing heterostructure thin films based on SrIrO3\mathrm{SrIrO}_{3} and other ABO3\mathrm{ABO}_{3} perovskite oxides (for example, CaMnO3\mathrm{CaMnO}_{3}) using molecular beam epitaxy along particular crystallographic orientations, such as the [111] direction and the [1] direction.[15, 16, 17, 18] The component layers require thickness at unit cell scale and lattice quality at atomic level, which sets a big challenge in sample preparation. On the other hand, the high pressure and high temperature synthesis provides a new approach to novel materials.[19] Recently, the non-centrosymmetric Sr2IrO4\mathrm{Sr}_{2}\mathrm{IrO}_{4} was first discovered at 6 GPa and 1400 °C,[20] which further inspires us to investigate SrIrO3\mathrm{SrIrO}_{3} under high pressure and high temperature conditions.

Herein, we report the synthesis, structural characterization, magnetic and electrical resistivity study on the tetragonal SrIrO3\mathrm{SrIrO}_{3} synthesized at 6 GPa and 1400 °C for 3 hours (serial number TT-1446). Employing single crystal and powder X-ray diffraction (XRD), the tetragonal symmetry was carefully examined, excluding the possibility of pseudo cubic symmetry observed. Moreover, weak fractional peaks with the tetragonal space group in the H and K dimensions in the reciprocal space suggest possible structure modulation by oxygen defects. The magnetization study of tetragonal SrIrO3\mathrm{SrIrO}_{3} shows weak paramagnetic behavior down to 2 K. Furthermore, our electrical resistivity measurement demonstrates metallic property with a resistivity upturn at ∼54\sim54 K due to weak electron localization and possible structural defects in the presence of SOC.

Experimental Section

High-Pressure Synthesis. The high-pressure synthesis was conducted using a Walker-type[21] multi-anvil apparatus (MA) at Lamont-Doherty Earth Observatory. The starting material was as-synthesized ambient pressure SrIrO3\mathrm{SrIrO}_{3} phase, which was prepared by thoroughly mixing the materials SrCO3\mathrm{SrCO}_{3} and Ir, and subsequently heating them to 900 °C for 12 hrs, then regrinding and reannealing at 1000 °C for 72 hrs.[22] The sample was kept at 120 °C overnight to remove the moisture before high-pressure experiments. The sample was then loaded in a platinum capsule inside an Al2O3\mathrm{Al}_{2}\mathrm{O}_{3} crucible that was inserted into a Ceramacast 646 octahedral pressure medium lined on the inside with a LaCrO3\mathrm{LaCrO}_{3} heater and kept at 6 GPa and 1400 °C for 3 hours before quenching to room temperature and then decompressed to ambient pressure overnight (serial number TT-1446). The pressure applied in the press has been calibrated using the phase transitions of bismuth at room temperature. To ensure accurate temperature readings, thermocouples are positioned as close as possible to the sample for direct temperature measurement.

Chemical Composition Determination. The recovered high-pressure product was examined for purity and homogeneity using a Zeiss Sigma field emission scanning electron microscope (SEM) with Oxford INCA PentalFETx3 energy-dispersive spectroscopy (EDS) system (model 8100). An accelerating voltage of 20 kV was employed for imaging and analysis.

Phase Analysis by Powder X-ray Diffraction. The phase identity and purity were examined using a Bruker Davinci powder X-ray diffractometer with Cu Kα\alpha radiation (λ=1.5406\lambda= 1.5406 Å). Room temperature measurements were carefully performed with a step size of 0.010° at a scan speed of 5.00 sec/step over a Bragg angle (2θ2\theta) range of 5–120°.

Home Laboratory Single Crystal X-ray Diffraction. The room temperature crystal structure was determined using a Bruker D8 Quest Eco single crystal X-ray diffractometer, equipped with Mo Kα\alpha radiation (λ=0.7107\lambda= 0.7107 Å) with an ω\omega of 2.0° per scan and an exposure time of 10 s per frame. A SHELXTL package with the direct methods and full-matrix least-squares on the F2F^{2} model was used to determine the crystal structure.[23, 24]

Synchrotron Single Crystal X-ray Diffraction. The experiments were carried out on the QM2 beamline at the Cornell High Energy Synchrotron Source (CHESS). The sample was affixed to a Kapton mount using GE varnish and all data was collected at room temperature. We used an X-ray energy of 18 keV (0.6888 Å wavelength) and data was collected with a Pilatus 6M photon counting detector operating at a 10 Hz framerate while continuously rotating the sample angle (ψ\psi) through 360 degrees (gives one image every 0.1 degree). We combined scans taken with the sample angle χ\chi angles of 0, 90, and 100 degrees in order to fill in gaps in the detector and reduced the data using a cubic unit cell, lattice parameters 3.937 Å.

Physical Properties Measurement. Temperature and field-dependent magnetization and electrical resistivity measurements were performed with a Quantum Design DynaCool physical property measurement system (PPMS) at a temperature range of 1.8–300 K and applied fields up to 9 T using 11.0 mg sample in total. Electrical resistivity measurements were conducted with a four-probe method using platinum wires on a polycrystalline sample in the dimensions of 1.0 mm×0.8 mm×0.5 mm1.0\ \mathrm{mm}\times0.8\ \mathrm{mm}\times0.5\ \mathrm{mm}.

Results and Discussion

Crystal Structure Determination and Phase Analysis. The ambient pressure SrIrO3\mathrm{SrIrO}_{3} (mC-SrIrO3\mathrm{SrIrO}_{3}) crystallizes in a monoclinic distortion of the hexagonal BaTiO3\mathrm{BaTiO}_{3}-type structure. Under pressure, an orthorhombic perovskite SrIrO3\mathrm{SrIrO}_{3} (oP-SrIrO3\mathrm{SrIrO}_{3}) in the GdFeO3\mathrm{GdFeO}_{3}-type structure was reported at above 20 kbar at 1650 °C and above 50 kbar at 700 °C.[25] Here we performed our high pressure synthesis at 6 GPa and 1400 °C. Prior to pressurization, the precursor phase, as-synthesized mC-SrIrO3\mathrm{SrIrO}_{3}, was confirmed by powder XRD, with the pattern and Rietveld refinement presented in Figure 1a. Around 7% SiO2\mathrm{SiO}_{2} (by weight) was added as an impurity phase to account for peaks that could not be indexed to mC-SrIrO3\mathrm{SrIrO}_{3} (refer to Table S1–Table S4 for details). Figure 1b shows the powder XRD pattern of our recovered product, where diffraction peak positions clearly illustrate the appearance of a new phase after high pressure and high temperature treatment.

Powder XRD pattern and Rietveld refinement of ambient pressure mC-SrIrO3 and high pressure tP-SrIrO3

Figure 1. Powder XRD pattern and Rietveld refinement of ambient pressure mCmC-SrIrO3\mathrm{SrIrO}_{3} and high pressure tPtP-SrIrO3\mathrm{SrIrO}_{3} synthesized at 6 GPa and 1400 °C. Bragg peak positions of each phase are represented by vertical tick marks. The crystal structures are also shown. Sr, green; Ir, blue; O, red.

CompoundmC-SrIrO3_3
SymmetryC2/cC2/c
Unit cell dimensionsa=5.60047(27)a = 5.60047(27) Å
b=9.6254(4)b = 9.6254(4) Å
c=14.1673(8)c = 14.1673(8) Å
β=93.1816(28)∘\beta= 93.1816(28)^\circ
Volume762.53(8) Å3^3
wRwR13.796%
Goodness-of-fit2.11
Reduced χ2\chi^24.46

Table S1. Table S1 Structure parameters from powder XRD Rietveld refinement of mC-SrIrO3_3.

mC-SrIrO3\mathrm{mC\text{-}SrIrO_3}Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
Ir1_14a4a00010.0312(13)
Ir2_28f8f0.9804(4)0.66219(30)0.84618(14)10.0360(8)
Sr1_14e4e00.0008(9)1/41/410.0374(30)
Sr2_28f8f0.0110(7)0.6680(6)0.09820(26)10.0317(19)
O1_14e4e00.560(4)1/41/410.071(5)
O2_28f8f0.214(4)0.2655(24)0.2594(15)10.071(5)
O3_38f8f0.827(4)0.3692(25)0.0411(14)10.071(5)
O4_48f8f0.897(5)0.145(3)0.3950(13)10.071(5)
O5_58f8f0.283(5)0.415(3)0.0917(16)10.071(5)

Table S4. Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^2). (UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.) UeqU_{\mathrm{eq}} values of all the oxygen atoms were constrained to be equal.

To determine the crystal structure of the recovered product as well as initialize Rietveld refinements of the powder XRD pattern, single crystal XRD experiments were first completed at home laboratory. Limited by onsite X-ray diffraction data quality, two structure models were proposed. One is cubic perovskite structure (a=3.9403(6) A˚a = 3.9403(6)\,\text{Å}) with the space group Pm3ˉmPm\bar{3}m (#221), denoted as cP-SrIrO3\mathrm{SrIrO}_{3}, the other is tetragonal structure with cc lattice parameter twice of the others (a=3.9362(9) A˚a = 3.9362(9)\,\text{Å}, c=7.880(3) A˚c = 7.880(3)\,\text{Å}, tP-SrIrO3\mathrm{SrIrO}_{3}) in P4/mmmP4/mmm (#123). The cubic structure model was slightly preferred. Crystallographic data and our single crystal XRD refinement details were summarized in Table S5–Table S8. Figure S1 provides regenerated reciprocal lattice planes from single crystal XRD based on these two structure models. Additionally, homogenous chemical element distribution of the recovered product was confirmed by scanning electron microscopy (SEM) and energy-dispersive spectroscopy (EDS) analysis on a single crystal sample (Figure S2 and Figure S3).

Regenerated reciprocal lattice planes of tP-SrIrO3, cP-SrIrO3, and oP-SrIrO3

Figure S1. Regenerated reciprocal lattice planes of tPtP-SrIrO3\mathrm{SrIrO}_{3}, cPcP-SrIrO3\mathrm{SrIrO}_{3}, and oPoP-SrIrO3\mathrm{SrIrO}_{3}.

SEM image and EDS spectra of a single crystal sample

Figure S2. SEM and EDS analysis of a single crystal sample. The formula obtained was calibrated to Ir and listed in the figure.

EDS mapping analysis of a single crystal sample

Figure S3. EDS mapping analysis of a single crystal sample. This confirms the homogenous chemical element distribution of the sample.

Chemical FormulaSrIrO3\mathrm{SrIrO}_{3}
Formula weight327.82 g/mol327.82\ \mathrm{g/mol}
Space GroupP4/mmmP4/mmm
Unit cell dimensionsa=3.9362(9) A˚a = 3.9362(9)\ \text{Å}
c=7.880(3) A˚c = 7.880(3)\ \text{Å}
Volume122.09(7) A˚3122.09(7)\ \text{Å}^{3}
Density (calculated)8.917 g/cm38.917\ \mathrm{g/cm}^{3}
Absorption coefficient76.005 mm−176.005\ \mathrm{mm}^{-1}
F(000)F(000)278
2θ2\theta range5.165.16 to 79.32∘79.32^\circ
Total Reflections1131
Independent reflections243 [Rint=0.0438R_{\mathrm{int}} = 0.0438]
Refinement methodFull-matrix least-squares on F2F^{2}
Data / restraints / parameters243 / 0 / 18
Final RR indicesR1 (I>2σ(I))=0.0596R_{1}\ (I>2\sigma(I)) = 0.0596; wR2 (I>2σ(I))=0.1247wR_{2}\ (I>2\sigma(I)) = 0.1247
R1 (all)=0.0648R_{1}\ (\text{all}) = 0.0648; wR2 (all)=0.1289wR_{2}\ (\text{all}) = 0.1289
Largest diff. peak and hole+14.926 e/A˚3+14.926\ \mathrm{e/\mathring{A}^{3}} and −12.448 e/A˚3-12.448\ \mathrm{e/\mathring{A}^{3}}
R.M.S. deviation from mean1.467 e/A˚31.467\ \mathrm{e/\mathring{A}^{3}}
Goodness-of-fit on F2F^{2}1.122

Table S5. Crystallographic data and single crystal XRD refinement of tP\mathit{tP}-SrIrO3\mathrm{SrIrO}_{3}.

cP-SrIrO3_3Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
Ir1b1b1/21/21/21/21/21/210.0021(3)0.0021(3)
Sr1a1a00010.0131(5)0.0131(5)
O3c3c1/21/21/21/2010.091(12)0.091(12)

Table S8. Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^{2}). (UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.)

cPcP-SrIrO3\mathrm{SrIrO}_{3} and tPtP-SrIrO3\mathrm{SrIrO}_{3} were then taken as starting parameters for the Rietveld refinements. Considering the inclusion of about 3% IrO2\mathrm{IrO}_{2} (by weight) as a secondary phase, both structure models yielded reasonable refinement parameters (details provided in Table S9–Table S12).

CompoundtPtP-SrIrO3_3
SymmetryP4/mmmP4/mmm
Unit cell dimensionsa=3.94447(22)a = 3.94447(22) Å
c=7.8938(8)c = 7.8938(8) Å
Volume122.818(6)122.818(6) Å3^3
wRwR16.957%
Goodness-of-fit2.37
Reduced χ2\chi^25.62
Weight fractiontPtP-SrIrO3_3: 0.971
IrO2_2: 0.029

Table S9. Structure parameters from powder XRD Rietveld refinement of tPtP-SrIrO3_3 + IrO2_2.

cPcP-SrIrO3_3Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
Ir1a1a00010.00153(24)
Sr1b1b1/21/21/210.0162(5)
O3d3d1/20010.0191(21)

Table S12. Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^{2}). (UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.)

A minor difference was noted between these two models specifically within the dd-spacing range of 0.9–1.5 Å. Unlike tPtP-SrIrO3\mathrm{SrIrO}_{3}, cPcP-SrIrO3\mathrm{SrIrO}_{3} failed to address extra weak but clearly resolved diffraction peaks, as presented in Figure 2, suggesting a lower symmetry. The reported oPoP-SrIrO3\mathrm{SrIrO}_{3} (PbnmPbnm, a=5.5909(1)a = 5.5909(1) Å, b=7.8821(1)b = 7.8821(1) Å, c=5.5617(1)c = 5.5617(1) Å)[22, 26] model was also evaluated, however, the absence of diffraction peaks indicative of orthorhombic symmetry excludes its possibility as the optimized structure model (details shown in Figure S4, Table S13 and Table S14).

Zoom-in powder XRD pattern of the recovered product and Rietveld refinement using tP-SrIrO₃ and cP-SrIrO₃ models

Figure 2. Zoom-in powder XRD pattern of the recovered product and Rietveld refinement using tPtP-SrIrO3_3 and cPcP-SrIrO3_3 models. Bragg peak positions of each phase are represented by vertical tick marks. The crystal structures are also shown. Sr, green; Ir, blue; O, red. Stars indicate diffraction peaks for which the cPcP-SrIrO3_3 model failed to account in comparison to tPtP-SrIrO3_3.

Zoom-in powder XRD Rietveld refinements of $tP$-SrIrO$_3$ and $oP$-SrIrO$_3$

Figure S4. Zoom-in powder XRD Rietveld refinements of tPtP-SrIrO3_3 and oPoP-SrIrO3_3.

CompoundoP−SrIrO3oP-\mathrm{SrIrO}_{3}
SymmetryPnmaPnma
Unit cell dimensionsa=5.59521(15)a = 5.59521(15) Å
b=7.89005(25)b = 7.89005(25) Å
c=5.56572(16)c = 5.56572(16) Å
Volume245.707(9)245.707(9) Å3^{3}
wRwR15.296%
Goodness-of-fit2.14
Reduced χ2\chi^{2}4.58
Weight fractionoP−SrIrO3oP-\mathrm{SrIrO}_{3}: 0.974
IrO2\mathrm{IrO}_{2}: 0.026

Table S13. Structure parameters from powder XRD Rietveld refinement of oP−SrIrO3oP-\mathrm{SrIrO}_{3} + IrO2\mathrm{IrO}_{2}.

oP−SrIrO3oP-\mathrm{SrIrO}_{3}Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
Ir4b4b1/20010.00144(22)
Sr4c4c0.5251(5)1/40.4838(7)10.0081(5)
O1_{1}4c4c0.510(4)1/40.995(11)10.0293
O2_{2}8d8d0.273(4)0.016(4)0.729(8)10.0293

Table S14. Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^{2}). (UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.)

To further assess the accuracy of the cubic indexing suggested by our in-house single crystal XRD analysis for the crystal structure of our recovered product, we carried out synchrotron single crystal XRD experiments at the Cornell High Energy Synchrotron Source (CHESS). For a better comparison, we reduced our data using cubic symmetry and the unit cell of cPcP-SrIrO3_3 structure model. Figure 3 provides the regenerated reciprocal lattice planes (HK−1)(HK-1), (HK−1.5)(HK-1.5), and (HK−2)(HK-2). The clearly resolved, relatively intense peaks on the (HK−1.5)(HK-1.5) plane corroborate the unit cell doubling along the cc-axis, aligning with our tPtP-SrIrO3_3 structure model. Moreover, weaker fractional diffraction peaks in the H and K dimensions suggest possible structure modulation due to oxygen defects in tPtP-SrIrO3_3. Furthermore, the (HK−2)(HK-2) plane reveals distinct incommensurate peaks likely resulting from twinning in the single crystals.

Regenerated reciprocal lattice planes

Figure 3. Regenerated reciprocal lattice planes, (HK-1), (HK-1.5), and (HK-2) obtained from data reduction of our synchrotron single crystal XRD using cubic symmetry and the unit cell of cPcP-SrIrO3\mathrm{SrIrO}_{3}.

Following the discussion, we identified the optimized structure model of our recovered product as tPtP-SrIrO3\mathrm{SrIrO}_{3} in space group P4/mmmP4/mmm (#123) with the unit cell parameters a=b=3.9362(9)a = b = 3.9362(9) Å and c=7.880(3)c = 7.880(3) Å. Figure 4 presents a comparative analysis of the crystal structure and lattice parameters of cPcP-SrIrO3\mathrm{SrIrO}_{3}, tPtP-SrIrO3\mathrm{SrIrO}_{3}, and oPoP-SrIrO3\mathrm{SrIrO}_{3}. Overall, tPtP-SrIrO3\mathrm{SrIrO}_{3} shows a ~4.0% volume compression per chemical formula compared to mCmC-SrIrO3\mathrm{SrIrO}_{3} under ambient pressure. The average Sr–O and Ir–O bond lengths measure 2.77(4) Å and 1.969(1) Å, respectively. The asymmetric Ir–O distances in octahedral IrO6\mathrm{IrO}_{6} indicate the existence of polar local distortions. The phase was quenched from high pressure high temperature synthesis and thus can be metastable at ambient conditions. The external pressure is a possible reason for the polar local distortion to be stabilized. Unlike common observations in ambient and high pressure SrIrO3\mathrm{SrIrO}_{3}[22, 26] and Sr2IrO4\mathrm{Sr}_{2}\mathrm{IrO}_{4}[20, 27], the absence of [IrO6\mathrm{IrO}_{6}] octahedra rotation, tilt, and oxygen site disorder indicate potential linear Ir–O–Ir exchange interactions in this tPtP-SrIrO3\mathrm{SrIrO}_{3}.

Crystal structures and lattice parameter comparison of cP-SrIrO3, tP-SrIrO3, and oP-SrIrO3

Figure 4. Crystal structure and lattice parameter comparison of cPcP-SrIrO3_3, tPtP-SrIrO3_3, and oPoP-SrIrO3_3. Sr, green; Ir, blue; O, red.

Magnetization: Temperature-dependent Paramagnetism. Similar to monoclinic SrIrO3\mathrm{SrIrO}_{3} and orthorhombic SrIrO3\mathrm{SrIrO}_{3}, a paramagnetic susceptibility was observed in tetragonal SrIrO3\mathrm{SrIrO}_{3}, as displayed in Figure 5a. There is no obvious split between zero-field cooled (ZFC) and field-cooled (FC) modes (See Figure S5 for details). The initial examination of the data highlighted the small value of positive magnetic susceptibility and its noisy temperature dependence, especially above 50 K. The magnetic susceptibility below 50 K was fitted to the modified Curie-Weiss law (Equation (1)).

Magnetization of tetragonal SrIrO3 synthesized under high pressure

Figure 5. Magnetization of tetragonal SrIrO3\mathrm{SrIrO_3} synthesized under high pressure. (a) Magnetic susceptibility measured under ZFC mode at 1000 Oe. Inset, ZFC data fitted by Curie-Weiss model. (b) Field-dependent magnetization at 1.8 K, 10 K, 100 K and 300 K.

Temperature-dependent magnetic susceptibility in ZFC and FC modes at 1000 Oe

Figure S5. Temperature-dependent magnetic susceptibility in ZFC and FC modes at 1000 Oe. No significant split between ZFC and FC curves was observed.

χ=χ0+CT−θCW(1)\chi= \chi_{0} + \frac{C}{T-\theta_{\mathrm{CW}}} \tag*{(1)}

where θCW\theta_{\mathrm{CW}} is Curie temperature, χ0\chi_{0} is the temperature independent magnetic susceptibility, and CC is Curie constant. The data was well described by Curie-Weiss model down to 2 K, yielding θCW\theta_{\mathrm{CW}} of -0.01(1) K and the effective magnetic moment per Ir ion, μeff\mu_{\mathrm{eff}}, of 0.494(2) μB\mu_{\mathrm{B}}. The temperature-independent magnetic susceptibility χ0\chi_{0} is equal to 8.9(1) ×10−4\times10^{-4} emu/mol, which is larger than that of the reported orthorhombic SrIrO3\mathrm{SrIrO}_{3}.

Figure 5b shows field dependent magnetization of tetragonal SrIrO3\mathrm{SrIrO}_{3}. At 300 K, 100 K, and 1.8 K, a clear diamagnetic contribution was observed, becoming significant at high magnetic fields. However, at 10 K, the field-dependent magnetization exhibited unusual behavior, indicating that a standard Curie-Weiss model is insufficient to describe the magnetization behavior of this system. Considering that tetragonal SrIrO3\mathrm{SrIrO}_{3} behaves as a metal above 50 K (see our electrical resistivity data below), the magnetic susceptibility of non-localized conduction electrons should be taken into account. Then another possible interpretation of the magnetization data arises from itinerant magnetism due to intense electron–electron correlations. Consequently, a monotonically increasing temperature dependent magnetization is not always expected in various fields. This can explain the weak magnetization observed and the small fitted effective moment. Note that different contributions in magnetization are not mutually exclusive. Below 50 K, the localization of electrons was enhanced and a possible Curie-Weiss paramagnetism arises from the local moment. The more accurate magnetic structure and overall spin dynamics should be determined through further experiments.

Electrical Resistivity: Metal with a Low Temperature Upturn. Figure 6 illustrates the temperature-dependent electrical resistivity of tetragonal SrIrO3\mathrm{SrIrO_3} from 2–300 K, noting a room temperature resistivity of 0.038(1) Ω\Omega cm. The resistivity data shows metallic behavior with an upturn at 54(2) K, a feature also reported in bulk orthorhombic SrIrO3\mathrm{SrIrO_3}[22] and monoclinic SrIrO3\mathrm{SrIrO_3} thin film systems[15, 16, 18], typically associated with a metal-insulator transition. Note that in the whole temperature range studied, the electrical resistivity only changed from 0.038 Ω\Omega cm to around 0.033 Ω\Omega cm, with approximately 13% at maximum. Suggested by magnetization, a possible explanation for the resistivity upturn involves weak electron localization, attributable to intense electron-electron correlations, and possible structural defects in the polycrystalline sample.[30] In iridates, Ir 5d5d orbitals are highly extended in space and overlap with oxygen pp orbitals, which induces interlayer hopping. Different from Sr2IrO4\mathrm{Sr_2IrO_4} and Sr3Ir2O7\mathrm{Sr_3Ir_2O_7} with two-dimensional [IrO6\mathrm{IrO_6}] interlayer hopping, SrIrO3\mathrm{SrIrO_3} with the enhanced interlayer hopping induced by the [IrO6\mathrm{IrO_6}] three-dimensionality becomes, consequently, a metal at room temperature.[10, 31] From the electronic state point of view, the bands that cross through the Fermi surface are half-filled and largely split. At low temperatures, electron localization is enhanced, and then the gap opens, contributing to the resistivity upturn. Figure S6 provides our measurements in the different sequence of cooling and warming, confirming the low-temperature resistivity upturn.

Temperature-dependent electrical resistivity of tetragonal SrIrO$_3$ at $\mu_0H = 0$ T

Figure 6. Temperature-dependent electrical resistivity of tetragonal SrIrO3_3 at μ0H=0\mu_0H = 0 T. An upturn was observed at ∼54\sim54 K.

Temperature-dependent electrical resistivity of $tP$-$\mathrm{SrIrO}_{3}$ in different cooling and warming modes

Figure S6. Temperature-dependent electrical resistivity of tPtP-SrIrO3\mathrm{SrIrO}_{3} in different cooling and warming modes.

Conclusion

In conclusion, we reported the new tetragonal perovskite SrIrO3\mathrm{SrIrO}_{3} (P4/mmmP4/mmm, a=3.9362(9)a = 3.9362(9) Å, c=7.880(3)c = 7.880(3) Å) synthesized at 6 GPa and 1400 °C. The tetragonal crystal structure was determined based on single crystal and powder XRD results with exclusion of pseudo cubic symmetry. Weak fractional peaks in the H and K dimensions suggest possible structure modulation by oxygen defects. Magnetization study indicated weak paramagnetic behavior down to 2 K, with a small fitted effective magnetic moment of 0.494(2) μB\mu_{\mathrm{B}}, resulting from itinerate electrons. Moreover, electrical resistivity study demonstrated metallic property with an upturn at 54(2) K, attributed to weak electron localization and structural defects. This tetragonal SrIrO3\mathrm{SrIrO}_{3} provides another example that how high pressure can induce novel physical properties in quantum materials.

Acknowledgments

The work at Michigan State University was supported by U.S. DOE-BES under Contract DE-SC0023648. The work at Brown University was supported by the U.S. Department of Energy, Office of Science, Office of Basic Energy Sciences, under Award Number DE-SC0021265. This work is based on research conducted at the Center for High-Energy X-ray Sciences (CHEXS), which is supported by the National Science Foundation (BIO, ENG and MPS Directorates) under award DMR-1829070.

Supporting Information

Regenerated reciprocal lattice planes of tPtP-SrIrO3\mathrm{SrIrO}_{3}, cPcP-SrIrO3\mathrm{SrIrO}_{3}, and oPoP-SrIrO3\mathrm{SrIrO}_{3}; SEM and EDS analysis of a single crystal sample; zoom-in powder XRD Rietveld refinement of tPtP-SrIrO3\mathrm{SrIrO}_{3} and oPoP-SrIrO3\mathrm{SrIrO}_{3}; magnetic susceptibility of tPtP-SrIrO3\mathrm{SrIrO}_{3}; electrical resistivity of tPtP-SrIrO3\mathrm{SrIrO}_{3} in different cooling and warming modes; structure parameters from powder XRD Rietveld refinement of mCmC-SrIrO3\mathrm{SrIrO}_{3}, mCmC-SrIrO3\mathrm{SrIrO}_{3}+SiO2\mathrm{SiO}_{2}, tPtP-SrIrO3\mathrm{SrIrO}_{3}+IrO2\mathrm{IrO}_{2}, cPcP-SrIrO3\mathrm{SrIrO}_{3}+IrO2\mathrm{IrO}_{2}, and oPoP-SrIrO3\mathrm{SrIrO}_{3}+IrO2\mathrm{IrO}_{2}; crystallographic data and single crystal XRD refinement of tPtP-SrIrO3\mathrm{SrIrO}_{3} and cPcP-SrIrO3\mathrm{SrIrO}_{3}; atomic coordinates and equivalent isotropic atomic displacement parameters.

References

Pseudosymmetry in Tetragonal Perovskite SrIrO3\mathrm{SrIrO}_{3} Synthesized under High Pressure

Haozhe; Alberto de la; Joseph T.; David; Patrick M.; Kemp W.; Weiwei

Supporting Information

mC-SrIrO3_3Wyck.xxyyzzOcc.UeqU_{\rm eq}
Ir1_14a4a00010.0301(13)
Ir2_28f8f0.9803(4)0.66351(31)0.84596(13)10.0347(8)
Sr1_14e4e00.9980(9)1/410.0436(26)
Sr2_28f8f0.0107(7)0.6655(7)0.09845(27)10.0382(17)
O1_14e4e00.570(4)1/410.065(5)
O2_28f8f0.203(5)0.2647(25)0.2606(16)10.065(5)
O3_38f8f0.828(4)0.3653(26)0.0416(15)10.065(5)
O4_48f8f0.901(5)0.157(3)0.3995(14)10.065(5)
O5_58f8f0.300(5)0.415(3)0.0933(16)10.065(5)

Table S2. Table S2 Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^2). (UeqU_{\rm eq} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.) UeqU_{\rm eq} values of all the oxygen atoms were constrained to be equal.

CompoundmC-SrIrO3\mathrm{mC\text{-}SrIrO_3}
SymmetryC2/cC2/c
Unit cell dimensionsa=5.60065(26)a = 5.60065(26) Å
b=9.6260(4)b = 9.6260(4) Å
c=14.1681(8)c = 14.1681(8) Å
β=93.1818(27)∘\beta= 93.1818(27)^\circ
Volume762.65(7)762.65(7) Å3^3
wRwR12.993%
Goodness-of-fit1.99
Reduced χ2\chi^23.96
Weight fractionmC-SrIrO3\mathrm{mC\text{-}SrIrO_3}: 0.928
SiO2\mathrm{SiO_2}: 0.072

Table S3. Structure parameters from powder XRD Rietveld refinement of mC-SrIrO3\mathrm{mC\text{-}SrIrO_3} + SiO2\mathrm{SiO_2}.

tP\mathit{tP}-SrIrO3\mathrm{SrIrO}_{3}Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
Ir2g2g000.25009(13)0.25009(13)10.0021(4)0.0021(4)
Sr₁1d1d1/21/21/21/21/21/210.0002(6)0.0002(6)
Sr₂1c1c1/21/21/21/2010.053(4)0.053(4)
O₁4i4i01/21/20.248(10)0.248(10)10.09(2)0.09(2)
O₂1b1b001/21/210.11(7)0.11(7)
O₃1a1a00010.07(4)0.07(4)

Table S6. Atomic coordinates and equivalent isotropic atomic displacement parameters (Ų). (UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.)

Chemical FormulaSrIrO3\mathrm{SrIrO_3}
Formula weight327.82 g/mol
Space GroupPm3‾mPm\overline{3}m
Unit cell dimensionsa=3.9403(6) A˚a = 3.9403(6)\ \text{Å}
Volume61.18(3) A˚361.18(3)\ \text{Å}^{3}
Density (calculated)8.898 g/cm38.898\ \text{g}/\text{cm}^{3}
Absorption coefficient75.841 mm−175.841\ \text{mm}^{-1}
F(000)F(000)139
θ\theta range5.1745.174 to 39.622∘39.622^\circ
Total Reflections510
Independent reflections60 [Rint=0.0389]60\ [R_{\mathrm{int}} = 0.0389]
Refinement methodFull-matrix least-squares on F2F^{2}
Data / restraints / parameters60 / 0 / 6
Final RR indicesR1 (I>2σ(I))=0.0215; wR2 (I>2σ(I))=0.0537R_{1}\ (I>2\sigma(I)) = 0.0215;\ wR_{2}\ (I>2\sigma(I)) = 0.0537
R1 (all)=0.0215; wR2 (all)=0.0537R_{1}\ (\mathrm{all}) = 0.0215;\ wR_{2}\ (\mathrm{all}) = 0.0537
Largest diff. peak and hole+2.835 e/A˚−3+2.835\ \text{e}/\text{Å}^{-3} and −5.662 e/A˚−3-5.662\ \text{e}/\text{Å}^{-3}
R.M.S. deviation from mean0.594 e/A˚−30.594\ \text{e}/\text{Å}^{-3}
Goodness-of-fit on F2F^{2}1.329

Table S7. Crystallographic data and single crystal XRD refinement of cP-SrIrO3_3.

tPtP-SrIrO3_3Wyck.xxyyzzOcc.UeqU_{\mathrm{eq}}
Ir2g2g000.24197(18)10.00034(24)
Sr1_11d1d1/21/21/210.0110
Sr2_21c1c1/21/2010.0278(11)
O1_14i4i01/20.2824(22)10.0235
O2_21b1b001/210.0235
O3_31a1a00010.0235

Table S10. Atomic coordinates and equivalent isotropic atomic displacement parameters (Å2^2). (UeqU_{\mathrm{eq}} is defined as one third of the trace of the orthogonalized UijU_{ij} tensor.)

CompoundcPcP-SrIrO3_3
SymmetryPm−3mPm\mathord{-}3m
Unit cell dimensionsa=3.94478(7)a = 3.94478(7) Å
Volume61.386(3) Å3^{3}
wRwR17.524%
Goodness-of-fit2.45
Reduced χ2\chi^{2}6.00
Weight fractioncPcP-SrIrO3_3: 0.974; IrO2_2: 0.026

Table S11. Structure parameters from powder XRD Rietveld refinement of cPcP-SrIrO3_3 + IrO2_2.

References

  1. [1]Laurell, P.; Fiete, G. A., Topological Magnon Bands and Unconventional Superconductivity in Pyrochlore Iridate Thin Films. Phys. Rev. Lett. 2017, 118 (17), 177201.DOI
  2. [2]Takagi, H.; Takayama, T.; Jackeli, G.; Khaliullin, G.; Nagler, S. E., Concept and realization of Kitaev quantum spin liquids. Nat. Rev. Phys. 2019, 1 (4), 264-280.DOI
  3. [3]Yang, K.-Y.; Lu, Y.-M.; Ran, Y., Quantum Hall effects in a Weyl semimetal: Possible application in pyrochlore iridates. Phys. Rev. B 2011, 84 (7), 075129.DOI
  4. [4]Wan, X.; Turner, A. M.; Vishwanath, A.; Savrasov, S. Y., Topological semimetal and Fermi-arc surface states in the electronic structure of pyrochlore iridates. Phys. Rev. B 2011, 83 (20), 205101.DOI
  5. [5]Tokiwa, Y.; Ishikawa, J. J.; Nakatsuji, S.; Gegenwart, P., Quantum criticality in a metallic spin liquid. Nat. Mater. 2014, 13 (4), 356-359.DOI
  6. [6]Savary, L.; Moon, E.-G.; Balents, L., New Type of Quantum Criticality in the Pyrochlore Iridates. Phys. Rev. X 2014, 4 (4), 041027.DOI
  7. [7]Xiao, D.; Zhu, W.; Ran, Y.; Nagaosa, N.; Okamoto, S., Interface engineering of quantum Hall effects in digital transition metal oxide heterostructures. Nat. Commun. 2011, 2 (1), 596.
  8. [8]Kim, B. J.; Ohsumi, H.; Komesu, T.; Sakai, S.; Morita, T.; Takagi, H.; Arima, T., Phase-Sensitive Observation of a Spin-Orbital Mott State in Sr2IrO4. Science 2009, 323 (5919), 1329-1332.DOI
  9. [9]Cao, G.; Bolivar, J.; McCall, S.; Crow, J. E.; Guertin, R. P., Weak ferromagnetism, metal-to-nonmetal transition, and negative differential resistivity in single-crystal Sr2IrO4. Phys. Rev. B 1998, 57 (18), R11039-R11042.DOI
  10. [10]Moon, S. J.; Jin, H.; Kim, K. W.; Choi, W. S.; Lee, Y. S.; Yu, J.; Cao, G.; Sumi, A.; Funakubo, H.; Bernhard, C.; Noh, T. W., Dimensionality-Controlled Insulator-Metal Transition and Correlated Metallic State in 5d Transition Metal Oxides Srₙ₊₁IrₙO₃ₙ₊₁ (n = 1, 2, and ∞). Phys. Rev. Lett. 2008, 101 (22), 226402.DOI
  11. [11]Fujiyama, S.; Ohashi, K.; Ohsumi, H.; Sugimoto, K.; Takayama, T.; Komesu, T.; Takata, M.; Arima, T.; Takagi, H., Weak antiferromagnetism of Jeff = 1/2 band in bilayer iridate Sr3Ir2O7. Phys. Rev. B 2012, 86 (17), 174414.DOI
  12. [12]Nie, Y. F.; King, P. D. C.; Kim, C. H.; Uchida, M.; Wei, H. I.; Faeth, B. D.; Ruf, J. P.; Ruff, J. P. C.; Xie, L.; Pan, X.; Fennie, C. J.; Schlom, D. G.; Shen, K. M., Interplay of Spin- Orbit Interactions, Dimensionality, and Octahedral Rotations in Semimetallic SrIrO₃. Phys. Rev. Lett. 2015, 114 (1), 016401.
  13. [13]Cao, G.; Durairaj, V.; Chikara, S.; DeLong, L. E.; Parkin, S.; Schlottmann, P., Non-Fermi-liquid behavior in nearly ferromagnetic SrIrO₃ single crystals. Phys. Rev. B 2007, 76 (10), 100402.DOI
  14. [14]Fujioka, J.; Okawa, T.; Yamamoto, A.; Tokura, Y., Correlated Dirac semimetallic state with unusual positive magnetoresistance in strain-free perovskite SrIrO₃. Phys. Rev. B 2017, 95 (12), 121102.DOI
  15. [15]Biswas, A.; Kim, K.-S.; Jeong, Y. H., Metal insulator transitions in perovskite SrIrO₃ thin films. J. Appl. Phys. 2014, 116 (21), 213704.
  16. [16]Wu, F.-X.; Zhou, J.; Zhang, L. Y.; Chen, Y. B.; Zhang, S.-T.; Gu, Z.-B.; Yao, S.-H.; Chen, Y.-F., Metal–insulator transition in SrIrO₃ with strong spin–orbit interaction. J. Phys.: Condens. Matter 2013, 25 (12), 125604.DOI
  17. [17]Liu, Z. T.; Li, M. Y.; Li, Q. F.; Liu, J. S.; Li, W.; Yang, H. F.; Yao, Q.; Fan, C. C.; Wan, X. G.; Wang, Z.; Shen, D. W., Direct observation of the Dirac nodes lifting in semimetallic perovskite SrIrO₃ thin films. Sci. Rep. 2016, 6 (1), 30309.DOI
  18. [18]Gu, M.; Zhu, R.; Zhang, X.; Wang, Z.; An, Q.; Yang, F.; Liu, X.; Gao, P.; Meng, M.; Guo, J., Modulation of the Metal–Nonmetal Crossover in SrIrO₃/CaMnO₃ Superlattices. ACS Appl. Electron. Mater. 2022, 4 (7), 3707-3713.
  19. [19]Cheng, J. G.; Ishii, T.; Kojitani, H.; Matsubayashi, K.; Matsuo, A.; Li, X.; Shirako, Y.; Zhou, J. S.; Goodenough, J. B.; Jin, C. Q.; Akaogi, M.; Uwatoko, Y., High-pressure synthesis of the BaIrO₃ perovskite: A Pauli paramagnetic metal with a Fermi liquid ground state. Phys. Rev. B 2013, 88 (20), 205114.DOI
  20. [20]Wang, H.; Marshall, M.; Wang, Z.; Plumb, K. W.; Greenblatt, M.; Zhu, Y.; Walker, D.; Xie, W., Non-Centrosymmetric Sr₂IrO₄ Obtained Under High Pressure. Inorg. Chem. 2023, 62 (5), 2161-2168.DOI
  21. [21]Walker, D.; Carpenter, M. A.; Hitch, C. M., Some simplifications to multianvil devices for high pressure experiments. Am. Mineral. 1990, 75 (9-10), 1020-1028.
  22. [22]Zhao, J. G.; Yang, L. X.; Yu, Y.; Li, F. Y.; Yu, R. C.; Fang, Z.; Chen, L. C.; Jin, C. Q., High-pressure synthesis of orthorhombic SrIrO₃ perovskite and its positive magnetoresistance. J. Appl. Phys. 2008, 103 (10), 103706.DOI
  23. [23]Sheldrick, G., SHELXT - Integrated space-group and crystal-structure determination. Acta Cryst. A 2015, 71 (1), 3-8.DOI
  24. [24]Sheldrick, G., Crystal structure refinement with SHELXL. Acta Cryst. C 2015, 71 (1), 3-8.DOI
  25. [25]Longo, J. M.; Kafalas, J. A.; Arnott, R. J., Structure and properties of the high and low pressure forms of SrIrO3. J. Solid State Chem. 1971, 3 (2), 174-179.DOI
  26. [26]Puggioni, D.; Rondinelli, J. M., Comment on “High-pressure synthesis of orthorhombic SrIrO3 perovskite and its positive magnetoresistance” [J. Appl. Phys. 103, 103706 (2008)]. J. Appl. Phys. 2016, 119 (8).
  27. [27]Huang, Q.; Soubeyroux, J. L.; Chmaissen, O.; Sora, I. N.; Santoro, A.; Cava, R. J.; Krajewski, J. J.; Peck, W. F., Neutron Powder Diffraction Study of the Crystal Structures of Sr2RuO4 and Sr2IrO4 at Room Temperature and at 10 K. J. Solid State Chem. 1994, 112 (2), 355-361.DOI
  28. [30]Zhang, L.; Pang, B.; Chen, Y. B.; Chen, Y., Review of Spin–Orbit Coupled Semimetal SrIrO3 in Thin Film Form. Crit. Rev. Solid State Mater. Sci. 2018, 43 (5), 367-391.DOI
  29. [31]Kim, J. W.; Choi, Y.; Kim, J.; Mitchell, J. F.; Jackeli, G.; Daghofer, M.; van den Brink, J.; Khaliullin, G.; Kim, B. J., Dimensionality Driven Spin-Flop Transition in Layered Iridates. Phys. Rev. Lett. 2012, 109 (3), 037204.DOI

Paper details

vlnc:W_ecgxvrxr
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents