Spin Relaxation and Electrical Control of Spin Transport in Few-Layer TdT_{\rm d}-MoTe2_2

Abstract

We report electrical tuning of spin relaxation in atomically thin TdT_{\rm d}-MoTe2_2, a representative low-symmetry transition metal dichalcogenide. Weak antilocalization measurements reveal strong spin–orbit interaction with spin–orbit lengths of tens of nanometers, consistent with recent theoretical predictions. Despite the semimetallic nature of TdT_{\rm d}-MoTe2_2, in the ultrathin limit the spin–orbit scattering time can be tuned electrostatically by up to threefold. We further investigate vertical electric field effects on the spin–orbit length and time, and demonstrate the modulation of the Rashba parameters. Relation between spin–orbit scattering time and the diffusion coefficient indicates that spin relaxation is governed by the D'yakonov–Perel' mechanism in both monolayer and bilayer TdT_{\rm d}-MoTe2_2. These results establish few-layer TdT_{\rm d}-MoTe2_2 as a platform for electrically tunable spin transport, thereby providing insight into spin relaxation in low-symmetry transition metal dichalcogenides.

Introduction

Low-symmetry transition metal dichalcogenides (LS-TMDs) have recently attracted considerable attention in spintronics. Unlike conventional heavy metals such as Pt or W, LS-TMDs exhibit a canted spin Hall effect (SHE), where the spin current, charge current, and spin polarization are not mutually orthogonal [1]. This effect induces an out-of-plane antidamping torque on ferromagnets with perpendicular magnetic anisotropy, offering potential for high-density spintronic applications [2].

TdT_{\mathrm{d}}-MoTe2_2 is a representative LS-TMD and widely known for its topologically nontrivial band structures. Bulk TdT_{\mathrm{d}}-MoTe2_2 has been theoretically [3, 4] and experimentally [5, 6] established as a type-II Weyl semimetal, while the quantum spin Hall state has been theoretically proposed for monolayer TdT_{\mathrm{d}}-MoTe2_2 [7]. In addition to these intriguing topological properties, TdT_{\mathrm{d}}-MoTe2_2 is also a promising material for spintronics applications. In bulk TdT_{\mathrm{d}}-MoTe2_2, the canted SHE [1, 8, 9, 10] and also out-of-plane antidamping torque [11, 12, 13, 14] have been experimentally demonstrated. In the few-layer thin films, breaking the glide-plane symmetry along the cc-axis further induces intriguing spin transport phenomena, such as the planar SHE [15].

To fully exploit these functionalities, electrical control of spin transport is essential. In closely related systems with the same crystal structure, such as monolayer (1 L) WTe2_2, vertical electric fields can induce atomic displacements and the resulting lateral dipole moments, which affect the out-of-plane spin component and activate the D’yakonov–Perel’ (DP) spin relaxation channel [16, 17]. These results suggest that similar electric-field control may also be possible in TdT_{\mathrm{d}}-MoTe2_2. Theoretically, for example, spin relaxation in 1 L TdT_{\mathrm{d}}-MoTe2_2 is predicted to be tunable by carrier doping [18]. However, such electrical control of spin transport in TdT_{\mathrm{d}}-MoTe2_2 remains largely unexplored in experiments. In addition to the technical challenges, there remain fundamental open questions in spin transport in this material, notably a substantial discrepancy between theoretically predicted and experimentally reported spin relaxation lengths, whose origin remains unsolved. For instance, nonlocal measurements in few-layer TdT_{\mathrm{d}}-MoTe2_2 have reported micrometer-scale spin relaxation lengths at room temperature [15], which are two orders of magnitude longer than both theoretical predictions for 1 L TdT_{\mathrm{d}}-MoTe2_2 [18] and experimental values reported for WTe2_2 [19]. Such inconsistencies hinder a quantitative understanding of spin transport in TdT_{\mathrm{d}}-MoTe2_2 and call for more robust experimental approaches to evaluate spin–orbit interactions and spin relaxation.

Weak antilocalization (WAL) measurements provide a reliable and well-controlled method to evaluate spin–orbit interactions and spin relaxation [20]. Whereas WAL signals have been observed in thin TdT_{\mathrm{d}}-MoTe2_2 [21, 22, 23], previous analyses of WAL in thin TdT_{\mathrm{d}}-MoTe2_2 did not explicitly incorporate the spin–orbit length (LsoL_{\mathrm{so}}) in the fitting procedure. As a result, the evaluation of spin relaxation is indirect, which may partly account for the discrepancies between experimental results and theoretical predictions. Furthermore, the dominant spin relaxation mechanism has not been clearly established in previous experimental studies.

Here, we present a systematic study of spin relaxation and electrical control of spin transport in few-layer TdT_{\mathrm{d}}-MoTe2_2 (1–6 layers), using low-temperature magnetotransport measurements. By explicitly including LsoL_{\mathrm{so}} for fitting WAL signals, we directly evaluate the spin relaxation. The extracted LsoL_{\mathrm{so}} is on the order of several tens of nanometers, consistent with theoretical estimates [18]. In the ultrathin limit, we demonstrate electrostatic gate control of spin transport, achieving a threefold modulation of the spin relaxation time (τso\tau_{\mathrm{so}}). From the relation between τso\tau_{\mathrm{so}} and the diffusion coefficient, we identify the DP mechanism as the dominant spin relaxation process in both 1 L and 2 L samples. Furthermore, dual-gate measurements allow us to isolate the effects of vertical electric fields, revealing variations in τso\tau_{\mathrm{so}} and the Rashba parameters.

The present paper is organized as follows. Section II describes the experimental methods. Section III presents the experimental results and analyses, including weak antilocalization for different thicknesses (Sec. III A), gate control of spin transport (Sec. III B), identification of spin relaxation mechanisms (Sec. III C) and vertical electric field effects on spin relaxation (Sec. III D). § 4 summarizes the main results of this work.

Methods

Few-layer TdT_{\mathrm{d}}-MoTe2_2 flakes are mechanically exfoliated on a Si/SiO2_2 chip inside a glovebox (O2_2 and H2_2O < 0.5 ppm) from high-quality crystals grown by the flux method, with a residual-resistivity ratio (RRR) of ∼1000\sim1000. The exfoliated flakes are assembled into devices using a standard dry-transfer technique with a polycarbonate (PC) film on a polydimethylsiloxane (PDMS) polymer and hBN [24, 25], and are placed on prefabricated Au/Ti or Pt/Ti electrodes on SiO2_2 or hBN substrates. The top hBN layer serves as a protective encapsulation, preventing degradation of TdT_{\mathrm{d}}-MoTe2_2 in ambient conditions [26, 27]. For dual-gated devices, few-layer graphene is used as gate electrodes with hBN as the dielectric. Immediately after fabrication, the samples are mounted in a 3^3He cryostat, sealed in a vacuum can, and cooled down. Electrical transport measurements are performed using a lock-in technique at a frequency of 77 Hz. The flake thickness is determined by atomic force microscopy after the transport measurements. In this study, we analyze data from one 1 L, three 2 L, three 4 L, and one 6 L samples. Further details of the fabrication process are provided in Refs. [28, 29].

Measurement and analysis

Weak antilocalization for different thicknesses

In this subsection we show some representative WAL curves obtained from few-layer TdT_{\mathrm{d}}-MoTe2_2 in different thicknesses. WAL arises from quantum interference of time-reversed electron trajectories in diffusive conductors with strong spin–orbit interaction (SOI), leading to a characteristic magnetoconductivity peak around zero magnetic field [30]. The WAL line shape is governed primarily by the phase coherence length LφL_{\varphi} and the spin–orbit length LsoL_{\mathrm{so}}. LφL_{\varphi} characterizes the length scale over which electrons preserve their phase coherence, whereas LsoL_{\mathrm{so}} represents the characteristic length over which electron spins are randomized by spin–orbit scattering. By fitting the WAL curves, these characteristic lengths can be extracted quantitatively. We first show in Figure 1(a) the magnetoconductivity variations, Δσ(B)=σ(B)−σ(0)\Delta\sigma(B)=\sigma(B)-\sigma(0), for three different thicknesses (1 L, 2 L, and 4 L). Here the conductivity is derived from the measured resistance RR assuming the two-dimensional system as σ=d/(RW)\sigma=d/(RW), where dd and WW are the center-to-center distance between the two electrodes and the width of the sample, respectively. All curves exhibit peaks around zero magnetic field, a hallmark of WAL, indicating the presence of strong SOIs in TdT_{\mathrm{d}}-MoTe2_2. Figure 1(b) displays WAL curves for a 6 L sample at different temperatures, where the peak around the zero magnetic field is suppressed with increasing temperature. These curves allow quantitative evaluation of the spin–orbit scattering time as well as the phase coherence time [30]. For quantitative analysis, we use the theoretical framework developed by Iordanskii, Lyanda-Geller, and Pikus (ILP), which assumes a system with broken inversion symmetry and explicitly takes the spin–orbit field BsoB_{\mathrm{so}} into account [31, 32, 33, 34]. Here we employ a standard formula for WAL, and do not explicitly include contributions from topological channels such as Weyl fermions and topological surface or edge states. This is because, even if a Weyl semimetal phase persists in few-layer TdT_{\mathrm{d}}-MoTe2_2, it has not been experimentally established that the Fermi level lies sufficiently close to the Weyl points for Weyl-related transport to make a significant contribution. Moreover, our magnetotransport measurements do not allow us to separately identify contributions from topological states. In the ILP model, Δσ(B)\Delta\sigma(B) under a perpendicular magnetic field BB is expressed as

Figure 1. (a) Magnetoconductivity variation [Δσ(B)][\Delta\sigma(B)] at 4 K obtained from 1 L, 2 L and 4 L TdT_{\mathrm{d}}-MoTe2_2. Solid curves are fits by using the 1IL formula. (b) Δσ(B)\Delta\sigma(B) for a 6 L sample at different temperatures with fits using the ILP formula. (c) 1/τφ1/\tau_{\varphi} obtained from the fits in (b) as a function of temperature (TT). (d) Thickness (tt) dependence of the spin–orbit length (LsoL_{\mathrm{so}}). The data are obtained from the fits at 4 K (1 L–4 L) and 3.5 K (6 L).

Δσ(B)=Ne2πℏ[F(Bφ+BsoB)+12F(Bφ+2BsoB)−12F(BφB)],(1)\Delta\sigma(B)=\frac{N e^{2}}{\pi\hbar}\left[F\left(\frac{B_{\varphi}+B_{\mathrm{so}}}{B}\right)+\frac{1}{2}F\left(\frac{B_{\varphi}+2B_{\mathrm{so}}}{B}\right)-\frac{1}{2}F\left(\frac{B_{\varphi}}{B}\right)\right], \tag*{(1)}

where

F(z)=ψ(12+z)−ln⁡(z)(2)F(z)=\psi\left(\frac{1}{2}+z\right)-\ln(z) \tag*{(2)}

with ψ\psi as the Digamma function and B{φ,so}=B_{\{\varphi,\mathrm{so}\}}= ℏ/(4eL{φ,so}2)\hbar/(4eL_{\{\varphi,\mathrm{so}\}}^2). Here LφL_{\varphi} and LsoL_{\mathrm{so}} are the phase coherence and spin–orbit lengths, respectively. They can be associated with the phase coherence time (τφ\tau_{\varphi}) and spin–orbit time (τso\tau_{\mathrm{so}}) as L{φ,so}=Dτ{φ,so}L_{\{\varphi,\mathrm{so}\}}=\sqrt{D\tau_{\{\varphi,\mathrm{so}\}}} with the diffusion coefficient DD. Theoretical fits for experimental results provide estimates of LφL_{\varphi} and LsoL_{\mathrm{so}}, both of which are treated as fitting parameters in Eq. (1).

To account for the semimetallic nature of TdT_d-MoTe2_2, we introduce a prefactor NN in Eq. (1), which is treated as the effective number of coherent transport channels [35]. The effective value of NN may depend on the relative mobilities and scattering rates of the individual channels. For each device, we compared fits obtained with N=1N=1 and N=2N=2 using the same fitting range and procedure. The value of NN was selected on a device-by-device basis according to the fit quality and was then kept fixed throughout the gate-voltage series for that device. In particular, N=1N=1 was adopted for the 1 L device because it consistently yielded better fits than N=2N=2 over the entire gate-voltage range. Therefore, the observed gate dependence, including the approximately threefold modulation of τso\tau_{\mathrm{so}}, does not arise from changing NN with gate voltage.

The solid lines shown in Figure 1(a) are fits based on Eq. (1). The ILP model reproduces the essential low-field features of the experimental WAL curves and provides a reasonable description of the magnetoconductivity in the diffusive regime. Small systematic deviations emerge at higher magnetic fields, possibly due to contributions not captured by the approximate ILP model.

Note that Eq. (1) is an approximated version of the full ILP formula, where the kk-cubic SOI is considered while the kk-linear SOI is not taken into account [31]. This equation is often employed for analyzing WAL signals in systems lack of inversion symmetry [33, 34]. In Appendix A, we assess the validity of Eq. (1) by fiting the experimental results using the full ILP formula while varying the ratio between the kk-cubic and kk-linear SOI terms for different layer thicknesses and for a monolayer sample under different vertical electric fields. The fitting results systematically favor the small kk-linear SOI regime, supporting the use of Eq. (1) in the systematic WAL analysis presented below. Detailed fitting comparisons and quantitative evaluations of the fitting quality are provided in Appendix A.

From the fits, we extract LφL_{\varphi} and LsoL_{\mathrm{so}}. Figure 1(c) shows the temperature dependence of τφ−1\tau_{\varphi}^{-1} for the 6 L sample, calculated from LφL_{\varphi} and DD obtained from the resistance measurements at each temperature. Almost linear relation shows that the phase relaxation is driven by electron–electron scattering [36]. We present in Figure 1(d) the spin–orbit length LsoL_{\mathrm{so}} as a function of thickness. LsoL_{\mathrm{so}} is in between 6–45 nm, and these values are in accordance with theoretical estimates [17, 18] and also experimentally obtained value in a recent experiment for a similar LS-TMD WTe2_2 [19].

Gate modulation of spin transport in monolayer TdT_d-MoTe2_2

Next, we study the gate modulation of spin transport in TdT_d-MoTe2_2. In this subsection, we focus on effects from the carrier density modulation by gating. In bulk crystals, the semimetallic nature leads to strong screening, making it difficult to modulate spin and charge transport using conventional electrostatic gating. However, when the sample thickness becomes comparable to or smaller than the nanometer-scale screening length, a gate electric field can effectively penetrate the material and control transport. Figure 2(a) shows Δσ(B)\Delta\sigma(B) measured in a 1 L sample at different VgV_g at 237 mK. Note that this sample does not show superconductivity at this temperature [29]. The pronounced change in Δσ(B)\Delta\sigma(B) with VgV_g indicates that the spin-relaxation properties are significantly modulated by electrostatic gating.

Gate-dependent transport for the 1 L sample at 237 mK

Figure 2. Gate-dependent transport for the 1 L sample at 237 mK. (a) Magnetoconductivity variation Δσ(B)\Delta\sigma(B) as a function of BB measured at selected gate voltages (VgV_{\mathrm{g}}). The solid lines are the fits using the equation (1). (b) LφL_{\varphi} and LsoL_{\mathrm{so}} as a function of VgV_{\mathrm{g}}. (c) VgV_{\mathrm{g}} dependence of the resistance RR. Inset: The diffusion coefficient DD as a function of VgV_{\mathrm{g}} calculated from RR in the main panel. The top axis is in the unit of Δn=Cg(Vg−V0)/e\Delta n=C_{\mathrm{g}}(V_{\mathrm{g}}-V_{0})/e, where CgC_{\mathrm{g}} and V0V_{0} are the capacitance of the hBN gate dielectric and the gate voltage at the charge neutrality point, respectively. (d) VgV_{\mathrm{g}} dependence of τso\tau_{\mathrm{so}} calculated from LsoL_{\mathrm{so}} obtained from the fits in (a), exhibiting the threefold variation. The inset shows a similar VgV_{\mathrm{g}} dependence for τφ\tau_{\varphi}.

By fitting the magnetoconductivity curves [solid lines in Figure 2(a)], we extract LφL_{\varphi} and LsoL_{\mathrm{so}}, which are summarized in Figure 2(b). While LφL_{\varphi} decreases monotonically with increasing VgV_g, LsoL_{\mathrm{so}} exhibits only a weak gate dependence. We can obtain L{φ,so}L_{\{\varphi,\mathrm{so}\}} using the diffusion coefficient DD. DD is calculated from the conductivity σ\sigma as D=hσ/(4meπ2)D=h\sqrt{\sigma}/(4me\pi\sqrt{2}), where m=0.37m0m=0.37m_0 is the effective mass with m0m_0 the electron mass [37]. The longitudinal resistance, shown in Figure 2(c), exhibits a strong gate dependence with a charge neutrality point at Vg∼8 VV_g\sim8\ \mathrm{V}, indicating that the sample is hole-doped at Vg=0 VV_g=0\ \mathrm{V}. The VgV_g dependence of DD is presented in the inset of Figure 2(c). Using this DD, we calculate and plot τso\tau_{\mathrm{so}} as a function of VgV_g in Figure 2(d). τso\tau_{\mathrm{so}} increases by a factor of three as with VgV_g varies from −14-14 to 14 V14\ \mathrm{V}. This pronounced gate modulation of τso\tau_{\mathrm{so}} constitutes a central result of this work. Previous studies of WAL in thin TdT_d-MoTe2_2 have either not explored gate modulation [21, 22] or reported only weak modulation, likely due to limited electrostatic tunability [23]. Note that this threefold modulation of τso\tau_{\mathrm{so}} does not imply a corresponding threefold modulation of the intrinsic SOI because τso\tau_{\mathrm{so}} also depends on momentum relaxation, as discussed in the later subsection.

We also investigate the origin of the gate dependence of LφL_{\varphi}. From Figure 2(b) and (Figure 2c), we find that LφL_{\varphi} decreases as the resistance increases. This can be explained by enhanced electron–electron scattering, as the screening becomes weaker when the carrier density decreases. It is also consistent with the relation between τφ\tau_{\varphi} and VgV_g as shown in the inset of Figure 2(d), where τφ\tau_{\varphi} becomes smaller with increasing resistance. At this low temperature (T=237 mKT=237\ \mathrm{mK}), phonons are negligible, thus electron–phonon scattering is ineffective. We note the electron–electron and momentum scattering play different roles. At low temperatures, electron–electron interactions can provide a dominant phase relaxation mechanism, whereas momentum scattering, including impurity scattering, affects the spin relaxation through the DP mechanism.

Identification of spin relaxation mechanisms

The opposite trend for τso\tau_{\mathrm{so}} and DD in regard to VgV_{\mathrm{g}}, shown in Figure 2, can be understood from the underlying spin relaxation mechanism. Here we investigate the dominant spin relaxation mechanism in few-layer TdT_{\mathrm{d}}-MoTe2_2. In diffusive metals such as TdT_{\mathrm{d}}-MoTe2_2, two spin relaxation mechanisms are generally considered [38]: the Elliott–Yafet (EY) mechanism [39] and the D’yakonov–Perel’ (DP) mechanism [40]. In the EY mechanism, electron spins relax via momentum scattering through spin–orbit coupling, leading to the relation τso∝τp\tau_{\mathrm{so}} \propto\tau_{\mathrm{p}}, where τp\tau_{\mathrm{p}} is the momentum relaxation time. On the other hand, the DP mechanism is closely associated with systems lacking inversion symmetry. Spin splitting caused by broken inversion symmetry can be interpreted as a momentum-dependent effective Zeeman field B(k)\mathbf{B}(\mathbf{k}). Between successive momentum scattering events, electron spins precess around B(k)\mathbf{B}(\mathbf{k}), which promotes spin relaxation. In this case, the spin relaxation time follows the inverse dependence τso∝τp−1\tau_{\mathrm{so}} \propto\tau_{\mathrm{p}}^{-1}, in contrast to the EY mechanism.

The dominant spin relaxation mechanism can therefore be identified by examining the relationship between τso\tau_{\mathrm{so}} and DD (∝τp\propto\tau_{\mathrm{p}}). We investigate the dependence of τso−1\tau_{\mathrm{so}}^{-1} on DD for 1 L and 2 L TdT_{\mathrm{d}}-MoTe2_2 samples. Figure 3(a) shows the results for the 1 L sample. The large gate tunability of DD in the 1 L sample allows us to determine the dominant spin relaxation mechanism within a single device. We find that τso−1\tau_{\mathrm{so}}^{-1} is approximately proportional to DD, demonstrating that the DP mechanism governs spin relaxation in 1 L TdT_{\mathrm{d}}-MoTe2_2. We also show the corresponding results for the 2 L samples in Figure 3(b). Due to the limited gate tunability of DD within a single device in 2 L sample, data from multiple devices are plotted. The observed increase of τso−1\tau_{\mathrm{so}}^{-1} with increasing DD indicates that the DP mechanism dominates spin relaxation in the 2 L samples.

Figure 3. (a) Inverse of τso\tau_{\mathrm{so}} as a function of the diffusion coefficient DD for a single 1 L TdT_{\mathrm{d}}-MoTe2_2 sample. An almost linear relation between the two quantities shows the dominant DP spin relaxation mechanism, as guided by the light-blue line proportional to DD. (b) A similar plot as (a) for multiple 2 L samples. The light-blue line is proportional to DD.

The dominance of the DP mechanism in 2 L samples is consistent with the absence of inversion symmetry in 2 L TdT_{\mathrm{d}}-MoTe2_2, as in the bulk. By contrast, inversion symmetry is preserved in 1 L TdT_{\mathrm{d}}-MoTe2_2, whose crystal structure is the same as inversion-symmetric 1T′1T'-MoTe2_2. However, inversion symmetry can be broken by the presence of a substrate and a gate electric field normal to the sample plane [41]. In addition, although our samples are encapsulated with hBN on both sides, asymmetry between the top and bottom interfaces may be introduced during device fabrication, for example, through surface oxidation as reported for WTe2_2 [42]. A difference in the dielectric environment between the two sides can also break inversion symmetry [43]. Another possible factor is an intermediate metastable state between the inversion-symmetric 1T′1T' phase and the inversion-asymmetric TdT_{\mathrm{d}} phase reported by a recent Raman spectroscopy study [44]. Such extrinsic symmetry breaking can generate an effective spin–orbit field, thereby enhancing DP-type spin relaxation relative to the EY mechanism [17].

Vertical electric field dependence of spin relaxation

To disentangle the effects of vertical electric fields from the carrier density modulation, we performed measurements on dual-gate samples incorporating both top and bottom gates. The vertical electric field EzE_z is given by Ez=ϵtVt/dt−ϵbVb/dbE_z = \epsilon_{\mathrm{t}}V_{\mathrm{t}}/d_{\mathrm{t}} - \epsilon_{\mathrm{b}}V_{\mathrm{b}}/d_{\mathrm{b}}, where ϵt,b\epsilon_{\mathrm{t,b}}, Vt,bV_{\mathrm{t,b}}, and dt,bd_{\mathrm{t,b}} denote the relative dielectric constant, gate voltage, and thickness of the hBN layers for the top (tt) and bottom (bb) gates, respectively.

Figure 4(a) shows the dependence of LφL_{\varphi} and LsoL_{\mathrm{so}} on EzE_z for the 1 L sample measured at 237 mK [see the device structure shown in Figure 4(e)]. To vary EzE_z over a wide range, measurements were performed for several values of Δn\Delta n [=ϵ0ϵtVt/(edt)+ϵ0ϵbVb/(edb)= \epsilon_0\epsilon_{\mathrm{t}}V_{\mathrm{t}}/(e d_{\mathrm{t}}) + \epsilon_0\epsilon_{\mathrm{b}}V_{\mathrm{b}}/(e d_{\mathrm{b}}), where ϵ0\epsilon_0 and ϵ\epsilon are the vacuum dielectric constant and the elementary charge, respectively]. Note that the range over which Δn\Delta n is varied here is much smaller than in Figure 2 [see the top axis of Figure 2(c)], indicating that the observed behavior primarily reflects the effect of the vertical electric field rather than carrier doping. While LφL_\varphi shows a clear dependence on EzE_z, LsoL_\mathrm{so} remains nearly constant.

Vertical electric field dependence of characteristic lengths, spin relaxation times, Rashba parameters, and schematic dual-gate device structure

Figure 4. (a) Vertical electric field (EzE_z) dependence of the characteristic length (LφL_\varphi and LsoL_\mathrm{so}) at different carrier densities (Δn\Delta n) for the 1 L sample. (b) τφ\tau_\varphi and τso\tau_\mathrm{so}, (c) βR\beta_R and (d) αR\alpha_R for different Δn\Delta n plotted as a function of EzE_z. Correspondence between the symbol and Δn\Delta n is the same for three figures. All data are taken at T=237T = 237 mK. (e) Schematic illustration of the dual-gate device structure.

In Figure 4(b), we also plot τ{φ,so}\tau_{\{\varphi,\mathrm{so}\}} derived from L{φ,so}L_{\{\varphi,\mathrm{so}\}}. The EzE_z dependence is more pronounced for τφ\tau_\varphi than τso\tau_\mathrm{so}. Although the variation is modest, τso\tau_\mathrm{so} shows a systematic decrease with increasing EzE_z. This trend is qualitatively consistent with a previous theoretical study on the conduction bands of WTe2_2 [17]. The extracted L{φ,so}L_{\{\varphi,\mathrm{so}\}} and τ{φ,so}\tau_{\{\varphi,\mathrm{so}\}} are not symmetric with respect to Ez=0E_z = 0, suggesting the presence of an internal electric field, as discussed above.

To quantitatively evaluate the effect of EzE_z on the spin–orbit interaction, we first estimate the cubic Rashba parameter βR=Δso/kF3\beta_R = \Delta_\mathrm{so}/k_F^3, where kF=2πnk_F = \sqrt{2\pi n} is the Fermi wave number and nn is the total carrier density obtained from magnetoresistance fitting [29], considering that Eq. (1) assumes the cubic Rashba SOI. Based on the DP spin relaxation, the spin splitting is given by Δso=ℏ/(2τpτso)\Delta_\mathrm{so} = \hbar/(2\sqrt{\tau_p\tau_\mathrm{so}}) [45], and the resulting βR\beta_R as a function of EzE_z is shown in Figure 4(c). Note that βR\beta_R (also αR\alpha_R as discussed below) depends not only on EzE_z but also on nn, through the kF=2πnk_F = \sqrt{2\pi n} and τp\tau_p. The carrier doping effect is manifested as vertical shifts in βR\beta_R for different Δn\Delta n due to the non-negligible change of kF3k_F^3 in the denominator. On the other hand, although the modulation of βR\beta_R by EzE_z is moderate, it is clearly visible at fixed Δn\Delta n when comparing the data points of the same color in Figure 4(c). We also plot the linear Rashba parameter calculated as αR=Δso/kF\alpha_R = \Delta_\mathrm{so}/k_F in Figure 4(d), which presents more than 20 % variation in the same range of Δn\Delta n. As for the Fermi level dependence of the Rashba parameters, both Rashba parameters increase as the hole density decreases (from positive to negative Δn\Delta n), corresponding to the Fermi level approaching the valence band edge. This behavior is consistent with previous studies on the related material monolayer WTe2_2, where electric-field-induced spin splitting becomes more pronounced near the band edge [17, 46].

Conclusion

In conclusion, we have characterized spin relaxation and demonstrated electrostatic control of spin transport in few-layer TdT_{\mathrm{d}}-MoTe2_2. Pronounced WAL signals reveal strong SOIs, and analysis based on the ILP model yields spin–orbit lengths on the order of several tens of nanometers, in quantitative agreement with theoretical estimates. In 1 L TdT_{\mathrm{d}}-MoTe2_2, we achieve substantial gate modulation of the spin–orbit time, reaching a threefold variation. The vertical electric field dependence further demonstrates electrical control of Rashba parameters. We also identify the dominant spin relaxation mechanism, showing that DP relaxation governs spin dynamics in both 1 L and 2 L samples.

While previous experiments have reported significantly longer spin relaxation lengths [15], the origin of this discrepancy remains an open question and may reflect differences in measurement schemes. Overall, this work establishes LS-TMDs as a platform for electrically tunable spin transport and advances the understanding of spin relaxation in these materials.

We gratefully acknowledge J. Nitta and H. Yang for fruitful discussions, and thank M. Imai, S. Sasaki, and H. Murofushi for their support in the experiments. This project is financially supported in part by the JPSJ KAKENHI (Grant No. JP23H04869, No. JP21H01022, No. JP21H01041, No. JP21H04652, No. JP21K18181, No. JP21H05236, No. JP20H00354, No. JP19H05790, No. JP22H00112, No. JP24H00827 and No. JP26K00669). K.W. and T.T. acknowledge support from JSPS KAKENHI (Grants No. 21H05233 and No. 23H02052), the CREST (JPMJCR24A5), JST, and the World Premier International Research Center Initiative (WPI), MEXT, Japan.

Fitting the experimental results using the full Iordanskii Lyanda-Geller Pikus (ILP) formula

While in the main text we employ an approximated version of the ILP formula, in this subsection we compare it with the full ILP formula [31]. The full ILP formula is expressed as

Δσ=−Ne24π2ℏ{1a0+2a0+1+(B~so/B)a1[a0+(B~so/B)]−2(Bso1/B)+2ln⁡(BtrB)+ψ(12+BφB)+3C−∑n=1∞[3n−3an2+2an(B~so/B)−1−2(2n+1)(Bso1/B)[an+(B~so/B)]an−1an+1−2(Bso1/B)[(2n+1)an−1]]},(3)\Delta\sigma= -\frac{N e^{2}}{4\pi^{2}\hbar}\left\{\frac{1}{a_{0}}+\frac{2a_{0}+1+(\widetilde{B}_{\mathrm{so}}/B)}{a_{1}[a_{0}+(\widetilde{B}_{\mathrm{so}}/B)]-2(B_{\mathrm{so1}}/B)}+2\ln\left(\frac{B_{\mathrm{tr}}}{B}\right)+\psi\left(\frac{1}{2}+\frac{B_{\varphi}}{B}\right)+3C-\sum_{n=1}^{\infty}\left[\frac{3}{n}-\frac{3a_{n}^{2}+2a_{n}(\widetilde{B}_{\mathrm{so}}/B)-1-2(2n+1)(B_{\mathrm{so1}}/B)}{[a_{n}+(\widetilde{B}_{\mathrm{so}}/B)]a_{n-1}a_{n+1}-2(B_{\mathrm{so1}}/B)[(2n+1)a_{n}-1]}\right]\right\}, \tag*{(3)}

where

B~so=Bso1+Bso3,Bso1=ℏ4eD∣Ω1∣2τ1,Bso3=ℏ4eD∣Ω3∣2τ3=Bso,Btr=ℏ4eDτp,\widetilde{B}_{\mathrm{so}}=B_{\mathrm{so1}}+B_{\mathrm{so3}},\quad B_{\mathrm{so1}}=\frac{\hbar}{4eD}|\Omega_{1}|^{2}\tau_{1},\quad B_{\mathrm{so3}}=\frac{\hbar}{4eD}|\Omega_{3}|^{2}\tau_{3}=B_{\mathrm{so}},\quad B_{\mathrm{tr}}=\frac{\hbar}{4eD\tau_{p}},
1τm=∫[1−cos⁡(mθ)]W(θ) dθ,an=n+12+(BφB)+(B~soB).(4)\frac{1}{\tau_{m}}=\int[1-\cos(m\theta)]W(\theta)\,d\theta,\quad a_{n}=n+\frac{1}{2}+\left(\frac{B_{\varphi}}{B}\right)+\left(\frac{\widetilde{B}_{\mathrm{so}}}{B}\right). \tag*{(4)}

W(θ)W(\theta) and CC are the scattering probability by an angle θ\theta and the Euler constant, respectively. Ω1\Omega_{1} and Ω3\Omega_{3} are the spin precession vector originated from the Rashba and Dresselhaus SOI, and proportional to the wave number kk and k3k^{3}, respectively. Bso3B_{\mathrm{so3}} is equivalent to BsoB_{\mathrm{so}} in the main text. Note that, for simplicity, we set τ1=τ3=τp\tau_{1}=\tau_{3}=\tau_{p}. To fit the experimental data, we truncate the infinite sum in (A1) at n=20000n=20000. The parameter BtrB_{\mathrm{tr}} is determined independently from transport measurements. The equation (1) in the main text is obtained by setting Bso1=0B_{\mathrm{so1}}=0 in Eqs. (3) and (4) [31].

To investigate the effects of Bso1B_{\mathrm{so1}} and Bso3B_{\mathrm{so3}} terms in the fits, we define the factor rr given by the ratio between the two terms (r=Bso1/Bso3r=B_{\mathrm{so1}}/B_{\mathrm{so3}}), and at fixed rr, we carry out fitting by treating BφB_{\varphi} and B~so\widetilde{B}_{\mathrm{so}} as fitting parameters.

Figure 5 presents the fits at different rr from r=0r=0 to r=1000r=1000 for the samples with different thicknesses and vertical electric fields. The obtained fitting parameters and the residual sum of squares (RSS) for the condition shown in Figure 5(a) are given in Table I as representative results. The inset of Figure 5 shows the RSS as a function of rr, which clearly shows that the better fit is obtained in the limit of r→0r\to0 (Bso1→0B_{\mathrm{so1}}\to0) and validates the analysis using Eq. (1).

Comparison of the WAL fits using the Eq. (A1) for different $r$

Figure 5. Comparison of the WAL fits using the Eq. (A1) for different rr. The inset shows the evolution of RSS as a function of rr. (a) and (b) are the data taken from a 4 L sample (MTS3) at 1.4 K and Vg=0V_g=0 for the different fitting range. (c) is from a 2 L (MTS4) sample, and (d)–(f) compares the results for a 1 L (MTS11) samples under different vertical electric field (EzE_z) conditions.

rrBϕB_\phi [T]Bso1B_{\mathrm{so1}} [T]Bso3B_{\mathrm{so3}} [T]RSS
01.30×10−2±6.66×10−51.30 \times10^{-2} \pm6.66 \times10^{-5}00.164±2.37×10−30.164 \pm2.37 \times10^{-3}1.35×10−31.35 \times10^{-3}
11.34×10−2±6.99×10−51.34 \times10^{-2} \pm6.99 \times10^{-5}0.127±1.74×10−30.127 \pm1.74 \times10^{-3}0.127±1.74×10−30.127 \pm1.74 \times10^{-3}1.60×10−31.60 \times10^{-3}
101.41×10−2±7.61×10−51.41 \times10^{-2} \pm7.61 \times10^{-5}0.311±3.75×10−30.311 \pm3.75 \times10^{-3}3.11×10−2±3.75×10−43.11 \times10^{-2} \pm3.75 \times10^{-4}2.29×10−32.29 \times10^{-3}
1001.43×10−2±7.93×10−51.43 \times10^{-2} \pm7.93 \times10^{-5}0.345±3.98×10−30.345 \pm3.98 \times10^{-3}3.45×10−3±3.98×10−53.45 \times10^{-3} \pm3.98 \times10^{-5}2.73×10−32.73 \times10^{-3}
10002.14×10−2±6.88×10−42.14 \times10^{-2} \pm6.88 \times10^{-4}4.46±0.4864.46 \pm0.4864.46×10−3±4.86×10−44.46 \times10^{-3} \pm4.86 \times10^{-4}2.02×10−22.02 \times10^{-2}

Table 1. Values of the fitting parameters obtained from the fits using Eq. (A1) for different rr for the case shown in Figure 5(a).

Inplane magnetic field dependence of weak antilocalization

Previous theoretical and experimental studies for few-layer TdT_d-MoTe2_2 have pointed out the spin polarization anisotropy, particularly for the conduction bands [18, 37, 47, 48, 49]. To explore effects of the spin polarization anisotropy on WAL in few-layer TdT_d-MoTe2_2, we measure the inplane magnetic-field dependence of WAL using a 4 L TdT_d-MoTe2_2 sample.

Figure 6(a) presents Δσ(B⊥)\Delta\sigma(B_\perp) measured at 1.5 K and Vg=0V_g = 0 V for different orientations of the in-plane magnetic field (B∥B_\parallel). Here we explicitly write a perpendicular magnetic field as B⊥B_\perp to distinguish it from B∥B_\parallel. The magnitude of B∥B_\parallel is fixed at 1 T, and the relative angle θ\theta between B∥B_\parallel and the longitudinal direction of the TdT_d-MoTe2_2 flake is varied (see the schematic in the inset of Figure 6 for the definition of θ\theta). The variation in the WAL curves is small, and LsoL_{\mathrm{so}} values obtained from the ILP fits are given in Figure 6(c) for θ\theta from 0° to 90°. These results indicate that the spin polarization of the carriers is almost insensitive to an in-plane magnetic field of at least 1 T.

Figure 6. (a) Δσ(B)\Delta\sigma(B) curves taken from a 4 L sample (MTS22) with in-plane magnetic field (B∥=1B_{\parallel}=1 T) at four different angles and at Vg=0V_g=0 V. The angle is defined in the inset. The black solid curve represents the fit using the ILP formula for the data at θ=0∘\theta=0^\circ. (b) Gate voltage dependence of the resistance of the sample. It is electron-doped at Vg=0V_g=0 V and the Fermi level approaches to the CNP as VgV_g is swept toward a negative voltage. (c) Full angular dependence of LsoL_{\mathrm{so}} at Vg=−60V_g=-60 V, shown together with the data at Vg=0V_g=0 V. Particularly for Vg=−60V_g=-60 V, LsoL_{\mathrm{so}} is almost independent of the in-plane magnetic field of B∥=1B_{\parallel}=1 T.

We next measure the in-plane magnetic-field dependence of WAL in a different carrier-doping regime. In TMDs, the spin polarization structure changes depending on the position of the Fermi level, and the spin polarization anisotropy in the conduction bands becomes maximal when the Fermi level approaches the valley extrema. As shown in Figure 6(b), the sample is electron-doped, and by applying a negative gate voltage, the Fermi level can be tuned closer to the charge neutrality point. The spin-orbit length LsoL_{\mathrm{so}}, obtained from fits to the WAL signals at Vg=−60V_g = -60 V, is plotted in Figure 6(c) as a function of θ\theta over a broader range of θ=0∘\theta= 0^\circ–180∘180^\circ. Similar to the case at Vg=0V_g = 0 V, LsoL_{\mathrm{so}} is almost independent of the direction of B∥B_\parallel.

Within the framework of the D’yakonov–Perel’ spin relaxation mechanism (see the discussion in the main text for details), the spin-splitting energy Δso\Delta_{\mathrm{so}} is given by Δso=ℏ/2τpτso\Delta_{\mathrm{so}} = \hbar/2\sqrt{\tau_p\tau_{\mathrm{so}}} [45], where τp\tau_p is the momentum relaxation time. We estimate Δso≈8.7\Delta_{\mathrm{so}} \approx8.7 meV, which is much larger than the energy scale of a 1 T magnetic field (∼0.1\sim0.1 meV), assuming a commonly used gg-factor of g=2g=2. Therefore, the spins are so strongly locked by the spin–orbit field along the direction around bb-axis that they remain unaffected by an in-plane magnetic field of B∥=1B_{\parallel}=1 T. To investigate the in-plane spin polarization anisotropy, therefore, much larger B∥B_{\parallel} is required, which is inaccessible in our present experimental setup.

Crystal structure of TdT_d-MoTe2_2

We here show the crystal structure of TdT_d-MoTe2_2. Figure 7 show the side (left panel) and top (right panel) view of the crystal structure of TdT_d-MoTe2_2. One mirror plane MxM_x normal to the aa-axis as well as a glide plane M~y\widetilde{M}_y exist in bulk TdT_d-MoTe2_2, the latter is absent for few-layer samples, presenting a highly anisotropic nature of the material.

Figure 7. The crystal structure of TdT_d-MoTe2_2 from the side view (left panel) and the top view (right panel). M~y\widetilde{M}_y is the glide plane parallel to the cc-axis and MxM_x is the mirror plane normal to the aa-axis.

Summary of the samples and samples pictures

In this subsection, we summarize the samples employed in this study with BtrB_{\mathrm{tr}}, a magnetic field range used for the fits, LφL_{\varphi} and LsoL_{\mathrm{so}} obtained from the fits shown with the standard deviation. These data are presented in Table II. We also show the sample pictures of some of the representative samples for the present study in Figure 8.

Pictures of samples used for this study

Figure 8. Pictures of some of the samples used for this study. (a) presents a 2 L sample (MTS10) while (b) shows a 4 L sample (MTS22).

Sample NameNumber of LayersBtrB_{tr} [T]Fitting range [T]LϕL_{\phi} [nm]LsoL_{so} [nm]TT [K]
MTS1117.8×1027.8 \times10^{2}428.92±0.0328.92 \pm0.0313.85±0.0213.85 \pm0.020.24
MTS424.7–12272.2±0.172.2 \pm0.110.9±0.110.9 \pm0.14
MTS1024.5225.0±0.0225.0 \pm0.0213.2±0.0113.2 \pm0.014
MTS18230232.7±0.132.7 \pm0.118.8±0.118.8 \pm0.14
MTS342.5243.6±0.143.6 \pm0.121.3±0.121.3 \pm0.14
MTS742.01.451.6±0.251.6 \pm0.227.3±0.127.3 \pm0.12.2
MTS2241.640.5158±1.2158 \pm1.234.0±0.534.0 \pm0.51.4
MTS660.250.2112.4±1.8112.4 \pm1.837.9±0.937.9 \pm0.93.5

Table 2. Summary of the samples employed in this study and parameters relevant to the fits.

References

  1. [1]J. Zhou, J. Qiao, A. Bournel, and W. Zhao, Intrinsic spin hall conductivity of the semimetals MoTe₂ and WTe₂, Phys. Rev. B 99, 060408 (2019).DOI
  2. [2]Y. Liu, G. Shi, D. Kumar, T. Kim, S. Shi, D. Yang, J. Zhang, C. Zhang, F. Wang, S. Yang, Y. Pu, P. Yu, K. Cai, and H. Yang, Field-free switching of perpen- dicular magnetization at room temperature using out-of-plane spins from TaIrTe₄, Nature Electronics 6, 732 (2023).
  3. [3]A. A. Soluyanov, D. Gresch, Z. Wang, Q. Wu, M. Troyer, X. Dai, and B. A. Bernevig, Type-II Weyl semimetals, Nature 527, 495 (2015).DOI
  4. [4]Y. Sun, S.-C. Wu, M. N. Ali, C. Felser, and B. Yan, Prediction of Weyl semimetal in orthorhombic MoTe₂, Phys. Rev. B 92, 161107(R) (2015).DOI
  5. [5]K. Deng, G. Wan, P. Deng, Z. Zhang, S. Ding, E. Wang, M. Yan, H. Huang, H. Zhang, Z. Xu, J. Denlinger, A. Fedorov, H. Yang, W. Duan, H. Yao, Y. Wu, S. Fan, H. Zhang, X. Chen, and S. Zhou, Experimental observation of topological Fermi arcs in type-II Weyl semimetal MoTe₂, Nature Physics 12, 1105 (2016).DOI
  6. [6]J. Jiang, Z. K. Liu, Y. Sun, H. F. Yang, C. R. Rajamathi, Y. P. Qi, L. X. Yang, C. Chen, H. Peng, C.-C. Hwang, S. Z. Sun, S.-K. Mo, I. Vobornik, J. Fujii, S. S. P. Parkin, C. Felser, B. H. Yan, and Y. L. Chen, Signature of type-II Weyl semimetal phase in MoTe₂, Nature Communications 8, 13973 (2017).DOI
  7. [7]X. Qian, J. Liu, L. Fu, and J. Li, Quantum spin Hall effect in two-dimensional transition metal dichalcogenides, Science 346, 1344 (2014).
  8. [8]A. M. Hoque, D. Khokhlov, K. Zollner, B. Zhao, B. Karpiak, J. Fabian, and S. P. Dash, All-electrical creation and control of spin-galvanic signal in graphene and molybdenum ditelluride heterostructures at room temperature, Communications Physics 4, 124 (2021).DOI
  9. [9]C. K. Safeer, N. Ontoso, J. Ingla-Aynés, F. Herling, V. T. Pham, A. Kurzmann, K. Ensslin, A. Chuvilin, I. Robredo, M. G. Vergniory, F. de Juan, L. E. Hueso, M. R. Calvo, and F. Casanova, Large multidirectional spin-to-charge conversion in low-symmetry semimetal MoTe₂ at room temperature, Nano Letters 19, 8758 (2019).DOI
  10. [10]N. Ontoso, C. K. Safeer, F. Herling, J. Ingla-Aynés, H. Yang, Z. Chi, B. Martin-Garcia, I. n. Robredo, M. G. Vergniory, F. de Juan, M. Reyes Calvo, L. E. Hueso, and F. Casanova, Unconventional charge-to-spin conversion in graphene/MoTe₂ van der waals heterostructures, Phys. Rev. Appl. 19, 014053 (2023).
  11. [11]D. MacNeill, G. M. Stiehl, M. H. D. Guimaraes, R. A. Buhrman, J. Park, and D. C. Ralph, Control of spin-orbit torques through crystal symmetry in WTe₂/ferromagnet bilayers, Nature Physics 13, 300 (2017).
  12. [12]D. MacNeill, G. M. Stiehl, M. H. D. Guimarães, N. D. Reynolds, R. A. Buhrman, and D. C. Ralph, Thickness dependence of spin-orbit torques generated by WTe₂, Phys. Rev. B 96, 054450 (2017).DOI
  13. [13]S. Liang, S. Shi, C.-H. Hsu, K. Cai, Y. Wang, P. He, Y. Wu, V. M. Pereira, and H. Yang, Spin-orbit torque magnetization switching in MoTe₂/permalloy heterostructures, Advanced Materials 32, 2002799 (2020).arxiv.org/abs/2006.16618
  14. [14]G. M. Stiehl, R. Li, V. Gupta, I. E. Baggarı, S. Jiang, H. Xie, L. F. Kourkoutis, K. F. Mak, J. Shan, R. A. Buhrman, and D. C. Ralph, Layer-dependent spin-orbit torques generated by the centrosymmetric transition metal dichalcogenide β-MoTe₂, Phys. Rev. B 100, 184402 (2019).DOI
  15. [15]P. Song, C.-H. Hsu, G. Vignale, M. Zhao, J. Liu, Y. Deng, W. Fu, Y. Liu, Y. Zhang, H. Lin, V. M. Pereira, and K. P. Loh, Coexistence of large conventional and planar spin Hall effect with long spin diffusion length in a low-symmetry semimetal at room temperature, Nature Materials 19, 292 (2020).DOI
  16. [16]L.-k. Shi and J. C. W. Song, Symmetry, spin-texture, and tunable quantum geometry in a WTe₂ monolayer, Phys. Rev. B 99, 035403 (2019).DOI
  17. [17]J. Xu, H. Tanaka, A. Grieder, J. Simoni, R. Sundararaman, and Y. Ping, Spin relaxation and diffusion in monolayer 1T’-WTe₂ from first-principles (2024), arXiv:2408.08416 [cond-mat.mes-hall].arxiv.org/abs/2408.08416
  18. [18]M. Vila, C.-H. Hsu, J. H. Garcia, L. A. Benítez, X. Waintal, S. O. Valenzuela, V. M. Pereira, and S. Roche, Low-symmetry topological materials for large charge-to-spin interconversion: The case of transition metal dichalcogenide monolayers, Phys. Rev. Res. 3, 043230 (2021).DOI
  19. [19]E. Zhang, R. Chen, C. Huang, J. Yu, K. Zhang, W. Wang, S. Liu, J. Ling, X. Wan, H.-Z. Lu, and F. Xiu, Tunable positive to negative magnetoresistance in atomically thin WTe₂, Nano Letters 17, 878 (2017).DOI
  20. [20]Y. Niimi, D. Wei, H. Idzuchi, T. Wakamura, T. Kato, and Y. Otani, Experimental verification of comparability between spin-orbit and spin-diffusion lengths, Phys. Rev. Lett. 110, 016805 (2013).pubmed.ncbi.nlm.nih.gov/23383824
  21. [21]C. H. Naylor, W. M. Parkin, J. Ping, Z. Gao, Y. R. Zhou, Y. Kim, F. Streller, R. W. Carpick, A. M. Rappe, M. Drndic, J. M. Kikkawa, and A. T. C. Johnson, Monolayer single-crystal 1T’-MoTe₂ grown by chemical vapor deposition exhibits weak antilocalization effect, Nano Letters 16, 4297 (2016).
  22. [22]Q. Wang, P. Yu, X. Huang, J. Fan, X. Jing, Z. Ji, Z. Liu, G. Liu, C. Yang, and L. Lu, Observation of weak anti-localization and electron-electron interaction on few-layer 1T’-MoTe₂ thin films, Chinese Physics Letters 35, 077303 (2018).DOI
  23. [23]P. Song, C. Hsu, M. Zhao, X. Zhao, T.-R. Chang, J. Teng, H. Lin, and K. P. Loh, Few-layer 1T’-MoTe₂ as glass semimetal with thickness dependent carrier transport, 2D Materials 5, 031010 (2018).
  24. [24]P. J. Zomer, M. H. D. Guimaraes, J. C. Brant, N. Tombros, and B. J. van Wees, Fast pick up technique for high quality heterostructures of bilayer graphene and hexagonal boron nitride, Applied Physics Letters 105, 013101 (2014).DOI
  25. [25]F. Pizzocchero, L. Gammelgaard, B. S. Jessen, J. M. Caridad, L. Wang, J. Hone, P. Bøggild, and T. J. Booth, The hot pick-up technique for batch assembly of van der Waals heterostructures, Nature Communications 7, 11894 (2016).DOI
  26. [26]Y. Gang, J. Liang, C.-w. Cho, S. Li, Y. Guo, X. Ma, X. Wu, J. Wen, X. Du, M. He, C. Liu, S. A. Yang, K. Wang, and L. Zhang, Bandgap opening in MoTe₂ thin flakes induced by surface oxidation, Frontiers of Physics 15, 33602 (2020).DOI
  27. [27]L. Yang, H. Wu, W. Zhang, Z. Chen, J. Li, X. Lou, Z. Xie, R. Zhu, and H. Chang, Anomalous oxidation and its effect on electrical transport originating from surface chemical instability in large-area, few-layer 1T′-MoTe₂ films, Nanoscale 10, 19906 (2018).
  28. [28]T. Wakamura, M. Hashisaka, S. Hoshino, M. Bard, S. Okazaki, T. Sasagawa, T. Taniguchi, K. Watanabe, K. Muraki, and N. Kumada, Gate-tunable giant superconducting nonreciprocal transport in few-layer T_d-MoTe₂, Phys. Rev. Res. 6, 013132 (2024).
  29. [29]T. Wakamura, M. Hashisaka, Y. Nomura, M. Bard, S. Okazaki, T. Sasagawa, T. Taniguchi, K. Watanabe, K. Muraki, and N. Kumada, Systematic study of superconductivity in few-layer T_d-MoTe₂, Phys. Rev. B 113, 094503 (2026).DOI
  30. [30]G. Bergmann, Weak localization in thin films: a time-of-flight experiment with conduction electrons, Physics Reports 107, 1 (1984).DOI
  31. [31]S. V. Iordanskii, Y. B. Lyanda-Geller, and G. E. Pikus, Weak localization in quantum wells with spin-orbit interaction, JETP Letters 60, 206 (1994).
  32. [32]W. Knap, C. Skierbiszewski, A. Zduniak, E. Litwin-Staszewska, D. Bertho, F. Kobbi, J. L. Robert, G. E. Pikus, F. G. Pikus, S. V. Iordanskii, V. Mosser, K. Zekentes, and Y. B. Lyanda-Geller, Weak antilocalization and spin precession in quantum wells, Phys. Rev. B 53, 3912 (1996).DOI
  33. [33]C. Niu, G. Qiu, Y. Wang, Z. Zhang, M. Si, W. Wu, and P. D. Ye, Gate-tunable strong spin-orbit interaction in two-dimensional tellurium probed by weak antilocalization, Phys. Rev. B 101, 205414 (2020).DOI
  34. [34]H. Nakamura, T. Koga, and T. Kimura, Experimental evidence of cubic Rashba effect in an inversion-symmetric oxide, Phys. Rev. Lett. 108, 206601 (2012).pubmed.ncbi.nlm.nih.gov/23003162
  35. [35]J. Wang, W. Powers, Z. Zhang, M. Smith, B. J. McIntosh, S. K. Bac, L. Riney, M. Zhukovskiy, T. Orlova, L. P. Rokhinson, Y.-T. Hsu, Y. Liu, and B. A. Assaf, Observation of coexistence weak localization and superconducting fluctuations in strained Sn₁₋ₓInₓTe thin films, Nano Letters 22, 792 (2022).DOI
  36. [36]B. L. Altshuler, A. G. Aronov, and D. E. Khmelnitsky, Effects of electron-electron collisions with small energy transfers on quantum localisation, Journal of Physics C: Solid State Physics 15, 7367 (1982).DOI
  37. [37]D. A. Rhodes, A. Jindal, N. F. Q. Yuan, Y. Jung, A. Antony, H. Wang, B. Kim, Y.-c. Chiu, T. Taniguchi, K. Watanabe, K. Barmak, L. Balicas, C. R. Dean, X. Qian, L. Fu, A. N. Pasupathy, and J. Hone, Enhanced superconductivity in monolayer T_d-MoTe₂, Nano Letters 21, 2505 (2021).
  38. [38]J. Fabian and S. D. Sarma, Spin relaxation of conduction electrons, Journal of Vacuum Science & Technology B: Microelectronics and Nanometer Structures Processing, Measurement, and Phenomena 17, 1708 (1999).
  39. [39]R. J. Elliott, Theory of the effect of spin-orbit coupling on magnetic resonance in some semiconductors, Phys. Rev. 96, 266 (1954).DOI
  40. [40]M. Dyakonov and V. Perel, Spin orientation of electrons associated with the interband absorption of light in semiconductors, Soviet Physics JETP 33, 1053 (1971).
  41. [41]Y. Zhang, J. van den Brink, C. Felser, and B. Yan, Electrically tuneable nonlinear anomalous Hall effect in two-dimensional transition-metal dichalcogenides WTe₂ and MoTe₂, 2D Materials 5, 044001 (2018).DOI
  42. [42]Z. Fei, W. Zhao, T. A. Palomaki, B. Sun, M. K. Miller, Z. Zhao, J. Yan, X. Xu, and D. H. Cobden, Ferroelectric switching of a two-dimensional metal, Nature 560, 336 (2018).
  43. [43]S. Wu, J. S. Ross, G.-B. Liu, G. Aivazian, A. Jones, Z. Fei, W. Zhu, D. Xiao, W. Yao, D. Cobden, and X. Xu, Electrical tuning of valley magnetic moment through symmetry control in bilayer MoS₂, Nature Physics 9, 149 (2013).DOI
  44. [44]F.-T. Huang, S. Joon Lim, S. Singh, J. Kim, L. Zhang, J.-W. Kim, M.-W. Chu, K. M. Rabe, D. Vanderbilt, and S.-W. Cheong, Polar and phase domain walls with conducting interfacial states in a Weyl semimetal MoTe₂, Nature Communications 10, 4211 (2019).
  45. [45]G. M. Minkov, A. A. Shorbotov, A. V. Germanenko, O. E. Rut, V. A. Larionova, and B. N. Zvonkov, Antilocalization and spin-orbit coupling in the hole gas in strained GaAs/InₓGa₁₋ₓAs/GaAs quantum well heterostructures, Phys. Rev. B 71, 165312 (2005).DOI
  46. [46]S.-Y. Xu, Q. Ma, H. Shen, V. Fatemi, S. Wu, T.-R. Chang, G. Chang, A. M. M. Valdivia, C.-K. Chan, Q. D. Gibson, J. Zhou, Z. Liu, K. Watanabe, T. Taniguchi, H. Lin, R. J. Cava, L. Fu, N. Gedik, and P. Jarillo-Herrero, Electrically switchable Berry curvature dipole in the monolayer topological insulator WTe₂, Nature Physics 14, 900 (2018).DOI
  47. [47]J. Cui, P. Li, J. Zhou, W.-Y. He, X. Huang, J. Yi, J. Fan, Z. Ji, X. Jing, F. Qu, Z. G. Cheng, C. Yang, L. Lu, K. Suenaga, J. Liu, K. T. Law, J. Lin, Z. Liu, and G. Liu, Transport evidence of asymmetric spin-orbit coupling in few-layer superconducting 1T_d-MoTe₂, Nature Communications 10, 2044 (2019).
  48. [48]X.-Z. Li, Z.-B. Qi, Q. Wu, and W.-Y. He, Topological superconductivity in monolayer T_d-MoTe₂, Communications Physics 7, 396 (2024).
  49. [49]Q. Wang, J. Li, J. Besbas, C.-H. Hsu, K. Cai, L. Yang, S. Cheng, Y. Wu, W. Zhang, K. Wang, T.-R. Chang, H. Lin, H. Chang, and H. Yang, Room-temperature nanoseconds spin relaxation in WTe₂ and MoTe₂ thin films, Advanced Science 5, 1700912 (2018).arxiv.org/abs/1803.00305

Paper details

vlnc:W_ezaqqc7b
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 2

downloads · 2

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents