Terahertz Optical Properties and Birefringence in Single Crystal Vanadium doped [100] \b{eta}-Ga2O3

Abstract

We report the Terahertz optical properties of the Vanadium doped [100] \b{eta}-Ga2O3 using Terahertz Time-Domain Spectroscopy (THz-TDS). The V-doped \b{eta}-Ga2O3 crystal shows strong birefringence in the 0.2-2.4 THz range. Further, phase retardation by the V-doped \b{eta}-Ga2O3 has been measured over the whole THz range by Terahertz Time-Domain Polarimetry (THz-TDP). It is observed that the V-doped \b{eta}-Ga2O3 crystal behaves both as a quarter waveplate (QWP) at 0.38, 1.08, 1.71, 2.28 THz, and a half waveplate (HWP) at 0.74 and 1.94 THz, respectively.

Introduction

In recent years β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} has been extensively studied due to its material properties such as wideband gap (4.9 eV), high electric field breakdown (8 MV/cm), and good thermal and chemical stability [1, 2]. These properties make β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} a promising candidate for many semiconductor devices like Schottky barrier diodes [3], UV photodetectors [4], field-effect transistors [5], etc. In addition to these applications, the high-frequency applications of β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} are also under active investigation, and a proper understanding of material properties at high frequencies is required. Over the last two decades, advances in the generation and detection of Terahertz (THz) radiation enabled researchers to investigate a wide range of material properties in this wavelength range[6]. In particular, Terahertz time-domain spectroscopy (THz-TDS) has evolved into an effective tool for characterizing the optical properties of materials at THz frequencies [7]. It is a non-destructive, contactless technique suitable even for examining highly fragile materials like thin films [8], biological tissues [9], etc. Many semiconductors such as ZnO [10], GaN [11], Graphene [12] have been characterized extensively using THz-TDS. However, there are only a few THz studies on doped and undoped β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} [13, 14, 15, 16].

In this work, we used the THz-TDS to report the optical properties of Vanadium doped β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} at THz frequencies. Furthermore, we employed the THz polarimetry (TDP) technique to determine the phase retardation and polarization of the THz wave transmitted through the V-doped β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} crystal. We show that the V-doped β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} behaves as a QWP and an HWP at different THz frequencies. To the best of our knowledge, the Terahertz optical properties of V-doped β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} crystal have never been investigated before.

Results and Discussion

Single Crystals of [100] oriented Vanadium doped β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} were grown at TIFR using the optical float zone technique [17]. β\beta-Ga2O3\mathrm{Ga}_{2}\mathrm{O}_{3} has a base-centered monoclinic structure with C2/m space group symmetry [18] and the corresponding a, b, c are 12.21Å, 3.03 Å, 5.79 Å respectively and β\beta=103.83°.

By carefully tuning the growth parameters, electrically resistive V-doped β\beta-Ga2_2O3_3 single crystals can be grown. These V-doped crystals have significantly different optical properties compared to the undoped crystal ones, details of which are given in the supplementary information. A cleaved slice of the V-doped β\beta-Ga2_2O3_3 crystal was used in this study, with a thickness of ∼\sim0.822 mm. The refractive index of the crystal is in general a complex number and the permittivity of the crystal can be calculated using well-known relations [7]. The permittivity of a crystal is a direct measure of the polarizability of the constituent atomic lattice of the crystal and the electron charge distribution in it under an externally applied electric field. The frequency of this field can be from DC to THz and beyond. The low-symmetry (C2/m) of monoclinic β\beta-Ga2_2O3_3 results in strongly anisotropic dielectric permittivity parameters along with different crystal directions. Thus, it is imperative to study the response of this crystal under different orientations with respect to the incident THz polarization direction. We have extensively studied the effect of polarizability in changing the polarization state of the transmitted THz signal through the crystal.

A THz-TDS setup (shown in Figure 3 of the supplementary information) is used for measuring the THz transmission and state of polarization through the V-doped crystal. The setup consists of a femtosecond (fs) pulsed laser (FemtoSource Synergy, 800 nm, 80 MHz, 10 fs) and a standard four-parabolic mirror configuration. The laser beam is divided into a pump and probe beam. The pump beam generates THz radiation using an LT-GaAs-based photoconductive antenna (BATOP GmbH). The probe beam is optically delayed and is used for detection purpose. A 2mm thick ZnTe crystal with <110> orientation is used for detecting the generated THz using the standard electro-optic technique. The entire setup is purged with nitrogen to eliminate any unwanted absorption of the THz due to the water vapor present in the ambient air.

THz TDP setup schematic, electric-field projections, and simulated polarization amplitudes

Figure 3. (a) THz TDP setup schematic. (b) Electric field EE projections leading to the measured signal S(ϕ)S(\phi). (c) Simulated amplitude S(ϕ)S(\phi), for the co-and cross-linear polarization (CoLP, CLP), circular polarization (CP) and elliptical polarization (b/ab/a).

The V-doped crystal was oriented with the b-axis parallel to the incident electric field, and the transmitted THz field was measured. After that, the V-doped crystal was rotated by 90° in the sample plane and the transmitted THz field was measured. Figure 1 (a, Figure 1b) illustrates the transmitted THz electric fields. Figure 1 (a) shows that the transmitted temporal THz field along θ\theta=0° is shifted by 0.62 ps compared to the one along θ\theta=90°, suggesting a strong birefringence in the V-doped Ga2_2O3_3 crystal. Furthermore, Figure 1 (b) illustrates the frequency domain THz spectrum.

Transmitted time-domain THz electric field and corresponding frequency domain spectra

Figure 1. (a) The transmitted time-domain THz electric field along b-axis of V-doped crystal for θ\theta=0° and θ\theta=90°, (b) Corresponding frequency domain spectra for θ\theta=0° and θ\theta=90°.

The refractive index and extinction coefficient are calculated to get a better insight into the birefringence of the V-doped crystal. The THz time-domain signals are Fourier transformed to obtain the corresponding frequency domain spectra. The complex-valued transfer function is calculated by normalizing the sample spectrum with the reference spectrum which is then used to determine the complex refractive index (detailed derivation is provided in the supplementary information). Figure 2 (a, b) shows the refractive indices and extinction coefficients for θ=0∘\theta=0^\circ and θ=90∘\theta=90^\circ with respect to the frequency. Large birefringence is observed across the 0.2 to 2.4 THz range. The refractive index along θ=0∘\theta=0^\circ and θ=90∘\theta=90^\circ at 1 THz is 3.40±\pm0.01 and 3.10±\pm0.01, respectively. The overall contrast in the refractive index across the frequency range is evaluated to be ∣0.3±0.02∣|0.3\pm0.02|. To the best of our knowledge, this is the highest among any doped or undoped Ga2O3\mathrm{Ga}_2\mathrm{O}_3 crystals [13], [15]. Furthermore, the extinction coefficient is extremely low (order of 10−210^{-2}) throughout the frequency range, indicating that the V-doped crystal has a minimal loss. The high transmittance and minimal loss make such V-doped β\beta-Ga2O3\mathrm{Ga}_2\mathrm{O}_3 crystals promising candidates for further research into THz frequency applications, especially in the design of polarizing optical elements.

Calculated complex refractive index and corresponding extinction coefficient

Figure 2. (a) The calculated complex refractive index for θ=0∘\theta=0^\circ and θ=90∘\theta=90^\circ, (b) The corresponding extinction coefficient for θ=0∘\theta=0^\circ and θ=90∘\theta=90^\circ.

To map the polarisation of the THz field modified by the V-doped crystal, a THz-Time Domain Polarimetry approach similar to [19] is employed. Figure 3 (a) shows a simplified schematic of the setup. The incident THz field is parallel to the x-axis. The V-doped crystal is mounted on a motorized rotating stage and is oriented with the b-axis being parallel to the electric field. The V-doped crystal is followed by a pair of linear THz wire grid polarisers (Tydex) in Polarizer-Analyser configuration. The Polarizer is oriented at an angle ϕ\phi with respect to the x-axis and is mounted on a motorized rotation stage. The Analyser is fixed and positioned along the x-axis. This technique allows us to precisely determine the phase retardation induced by the V-doped crystal without rotating the ZnTe. The V-doped crystal is rotated by an angle θ\theta, and for each θ\theta, the Polarizer (ϕ\phi) is rotated by complete 360 degrees in 10∘^\circ steps. When the incident THz field is transmitted through the V-doped crystal, the electric field can be expressed as

E⃗=acos⁡(ωt)x^+bcos⁡(ωt+δ)y^(1)\vec{E}=a\cos(\omega t)\hat{x}+b\cos(\omega t+\delta)\hat{y} \tag*{(1)}

Where a, b, and δ\delta are co-polarisation, cross-polarisation, and phase retardation, respectively. As shown in Figure 3 (b), the THz field after passing through the V-doped crystal is successively projected along with the Polarizer and Analyzer [20]. The resulting electric field on the ZnTe detector is given as,

S(ϕ)=∣cos⁡ϕ∣[(acos⁡ϕ+bsin⁡ϕcos⁡δ)2+(bsin⁡ϕsin⁡δ)2]12(2)S(\phi)=|\cos\phi|\left[(a\cos\phi+b\sin\phi\cos\delta)^2+(b\sin\phi\sin\delta)^2\right]^{\frac{1}{2}} \tag*{(2)}

The polarization parameters are obtained by measuring S(ϕ)S(\phi) as a function of the polarizer angle ϕ\phi. If the crystal acts as a QWP, then a=ba=b, δ=π/2\delta=\pi/2, and the equation (2) will be simplified to S(ϕ)=a∣cos⁡ϕ∣S(\phi)=a\lvert\cos\phi\rvert. However, if the crystal acts as an HWP then for an x-polarised incident electric field, we will have a y-polarised electric field at the output; thus a=0a=0, δ=π\delta=\pi, and the equation (2) will be simplified to S(ϕ)=b/2∣sin⁡2ϕ∣S(\phi)=b/2\lvert\sin2\phi\rvert. Furthermore, we will have elliptically polarized light for a≠ba\ne b and δ=π/2\delta=\pi/2. All of the preceding cases are demonstrated in Figure 3 (c).

For each value of ϕ\phi, a full scan over 360∘360^\circ rotation of the Polarizer is performed (in 10∘10^\circ steps), and the corresponding THz field is measured. Polarization parameters of the THz field transmitted from the V-doped Ga2O3\mathrm{Ga}_2\mathrm{O}_3 crystal are obtained by fitting the measured data to equation (2). The normalized polar plots for the measured data and corresponding fitting are shown in Figure 4. As seen from Figure 4 (a, Figure 4b), the V-doped crystal behaves as a QWP at 0.38, 1.08, 1.71, and 2.28 THz and as an HWP at 0.74, 1.94 THz for θ=40∘\theta= 40^\circ (see Figure 3 (c) for reference). There is a slight mismatch between the fit and measured data at 1.71 and 2.28 THz due to the presence of water lines at these frequencies. Furthermore, polar plots for θ=50∘\theta= 50^\circ are plotted as illustrated in Figure 4 (c, Figure 4d), which shows a similar trend at the corresponding frequencies. The transition from left to right-handedness is observed in the transmitted THz wave for the linear polarization case. Correspondingly, a slight right tilt in the circular polarization case is also seen for θ=50∘\theta= 50^\circ with respect to θ=40∘\theta= 40^\circ. Figure 4 (e, Figure 4g) illustrates the amplitude ratio and phase retardation profile at θ=40∘\theta= 40^\circ and θ=50∘\theta= 50^\circ, respectively. The limit for both the phase tolerance and amplitude ratio (b/ab/a) lies within ±10%\pm10\%. The amplitude ratio and phase retardation values are within the tolerance limit at the frequencies where the V-doped crystal behaves as a QWP and HWP, as shown in Figure 4 (e, Figure 4g). In addition to this, a polar plot at 1.4 THz where the elliptical polarisation behaviour dominates is given at both θ=40∘\theta= 40^\circ and θ=50∘\theta= 50^\circ in Figure 4 (f).

Polar maps and fitted polarization parameters at various THz frequencies

Figure 4. Polar map for normalized amplitude S(ϕ)S(\phi) at various THz frequencies. (a, b) 0.38, 0.74, 1.08, 1.71, 1.94, and 2.28 THz for θ=40∘\theta=40^\circ. (c, d) 0.38, 0.74, 1.08, 1.71, 1.94, and 2.28 THz for θ=50∘\theta=50^\circ. (e, g) As a function of frequency, the corresponding fitted polarization parameters are plotted. The black curve represents the amplitude ratio b/ab/a, while the red curve illustrates phase retardation δ/π\delta/\pi. (f) Polar map at 1.40 THz for θ=40∘\theta=40^\circ and θ=50∘\theta=50^\circ.

Figure 5 (a, Figure 5b) illustrates the calculated co- and cross-polarization parameters as a function of azimuthal angle with respect to frequency. Figure 5 shows that the co- and cross-polarization parameters follow a complementary pattern across the frequency range, i.e., when co-polarization is maximum, cross-polarization is minimum, and vice versa. The crystal behaves as an HWP at 0.74 and 1.94 THz, where the co-polarization is minimum and cross-polarization is maximum. Moreover, the QWP type behaviour is seen at 0.38, 1.08, 1.71, and 2.28 THz when the co and cross-polarization are equal, and the phase retardation is δ=π/2\delta= \pi/ 2 as seen previously. For further investigating the polarization state of the transmitted THz wave, we calculated the polarization orientation angle ψ\psi and ellipticity angle χ\chi using the Stokes parameters.

Experimental co- and cross-polarization parameter as a function of azimuthal angle with respect to frequency

Figure 5. Figure 5: (a, b) Experimental co- and cross-polarization parameter as a function of azimuthal angle with respect to the frequency, respectively.

S02=S12+S22+S32.(3)S_0^2 = S_1^2 + S_2^2 + S_3^2. \tag*{(3)}

Where

S0=a2+b2,(4)S_0 = a^2 + b^2, \tag*{(4)}
S1=a2−b2,(5)S_1 = a^2 - b^2, \tag*{(5)}
S2=2abcos⁡δ,(6)S_2 = 2ab\cos\delta, \tag*{(6)}
S3=2absin⁡δ.(7)S_3 = 2ab\sin\delta. \tag*{(7)}

And

Ψ=12tan⁡−1[S2S1],0≤Ψ≤π,(8)\Psi= \frac{1}{2}\tan^{-1}\left[\frac{S_2}{S_1}\right], \qquad0 \le\Psi\le\pi, \tag*{(8)}
χ=12sin⁡−1[S3S0],−π4≤χ≤π4.(9)\chi= \frac{1}{2}\sin^{-1}\left[\frac{S_3}{S_0}\right], \qquad-\frac{\pi}{4} \le\chi\le\frac{\pi}{4}. \tag*{(9)}

Figure 6 (a) shows the ellipticity (χ\chi) as a function of frequency, as the azimuth angle is varied over 90°. For certain azimuth angles (θ\theta=45°), the V-doped crystal acts as a QWP at 0.38, 1.08, 1.71, and 2.28 THz. Furthermore, in between these frequencies, a linear polarization state is also observed at 0.74 and 1.94 THz, where it behaves as a half-wave plate. Figure 6 (b) shows the evolution of the orientation angle (Ψ\Psi) as a function of frequency, as the azimuth angle is varied over 90°. Here, the transition from left-hand polarization to right-hand polarization of the transmitted THz field is clearly visible, which is consistent with the previous findings (see Figure 4 (a, Figure 4b, Figure 4c and Figure 4d)) [21].

Ellipticity and orientation angle as functions of azimuthal angle and frequency

Figure 6. (a) Ellipticity (χ\chi) as a function of azimuthal angle with respect to the frequency. (b) Orientation angle (Ψ\Psi) as a function of azimuthal angle with respect to the frequency.

Conclusion

In conclusion, we report the first Terahertz optical study on V-doped β\beta-Ga2_2O3_3 using the THz-TDS technique. It was observed that V-doped β\beta-Ga2_2O3_3 has significant THz transmission and shows a strong birefringence in the 0.2-2.4 THz range. In addition, a THz polarimetry technique was used to accurately determine the phase retardation and polarization of the transmitted THz field through the V-doped β\beta-Ga2_2O3_3 crystal. The V-doped β\beta-Ga2_2O3_3 crystal behaves as a QWP at 0.38, 1.08, 1.71, and 2.28 THz, while an HWP type behaviour is observed between these frequencies at 0.74 and 1.94 THz, respectively. Due to its high transmission and low losses, V-doped β\beta-Ga2_2O3_3 opens up new possibilities for developing THz QWP, HWP, segmented waveplates, etc., and new opportunities for device integration requiring intrinsic polarisation control of THz light.

Supplementary Materials

See the supplementary information for detailed analysis.

Data Availability

Analysis program of the THz-TDP will be available upon request to the Author (A.P.)

Authors’ Contribution

(A.P.) and (S.C.) contributed equally to the THz measurement and data analysis. (A.P.) build and characterized the THz-TDP setup. (M.N.) and (R.K.) has grown the crystals. (A.T.) and (A.B.) supervised the growth of crystals. (S.P.) supervised the overall THz experiments, analysis, and setup build-up.

Acknowledgment

We thank the Department of Atomic Energy (DAE) and Tata Institute of Fundamental Research (TIFR), Mumbai, for the resources, and the work is supported by DAE Grant ID RTI4003.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. [1]A. J. Green et al., “3.8-MV/cm Breakdown Strength of MOVPE-Grown Sn-Doped β-Ga2O3 MOSFETs,” IEEE Electron Device Lett., vol. 37, no. 7, pp. 902–905, 2016, doi: 10.1109/LED.2016.2568139.DOI
  2. [2]D. Ma, Nan and Tanen, Nicholas and Verma, Amit and Guo, Zhi and Luo, Tengfei and Xing, Huili and Jena, “Intrinsic electron mobility limits in β-Ga2O3,” Appl. Phys. Lett., vol. 109, no. 21, p. 212101, 2016.
  3. [3]Q. He et al., “Schottky barrier diode based on β-Ga2O3 (100) single crystal substrate and its temperature-dependent electrical characteristics,” Applied Physics Letters, vol. 110, no. 9. 2017, doi: 10.1063/1.4977766.DOI
  4. [4]X.-Z. Qian, Ling-Xuan and Zhang, Hua-Fan and Lai, PT and Wu, Ze-Han and Liu, “High-sensitivity β-Ga2O3 solar-blind photo detector on high temperature pretreated c-plane sapphire substrate,” Opt. Mater. Express, vol. 7, no. 10, pp. 3643–3653, 2017.
  5. [5]S. Krishnamoorthy et al., “Modulation-doped β-(Al0.2Ga0.8)2O3/Ga2O3 field-effect transistor,” Appl. Phys. Lett., vol. 111, no. 2, pp. 3–7, 2017, doi: 10.1063/1.4993569.DOI
  6. [6]M. Tonouchi, “Cutting-edge terahertz technology,” Nat. Photonics, vol. 1, no. 2, pp. 97–105, 2007, doi: 10.1038/nphoton.2007.3.DOI
  7. [7]J. Neu and C. A. Schmuttenmaer, “Tutorial: An introduction to terahertz time domain spectroscopy (THz-TDS),” J. Appl. Phys., vol. 124, no. 23, 2018, doi: 10.1063/1.5047659.DOI
  8. [8]P. U. Jepsen et al., “Metal-insulator phase transition in a VO2 thin film observed with terahertz spectroscopy,” Phys. Rev. B - Condens. Matter Mater. Phys., vol. 74, no. 20, pp. 1–9, 2006, doi: 10.1103/PhysRevB.74.205103.DOI
  9. [9]P. H. Siegel, “Terahertz technology in biology and medicine,” IEEE Trans. Microw. Theory Tech., vol. 52, no. 10, pp. 2438–2447, 2004, doi: 10.1109/TMTT.2004.835916.DOI
  10. [10]H. Němec et al., “Influence of the electron-cation interaction on electron mobility in dye-sensitized ZnO and TiO2 nanocrystals: A study using ultrafast terahertz spectroscopy,” Phys. Rev. Lett., vol. 104, no. 19, pp. 1–4, 2010, doi: 10.1103/PhysRevLett.104.197401.DOI
  11. [11]W. Zhang, A. K. Azad, and D. Grischkowsky, “Terahertz studies of carrier dynamics and dielectric response of n-type, freestanding epitaxial GaN,” Appl. Phys. Lett., vol. 82, no. 17, pp. 2841–2843, 2003, doi: 10.1063/1.1569988.DOI
  12. [12]P. R. Whelan, K. Iwaszczuk, R. Wang, S. Hofmann, P. Bøggild, and P. U. Jepsen, “Robust mapping of electrical properties of graphene from terahertz time-domain spectroscopy with timing jitter correction,” Opt. Express, vol. 25, no. 3, p. 2725, 2017, doi: 10.1364/oe.25.002725.DOI
  13. [13]V. C. Agulto et al., “Anisotropic complex refractive index of β-Ga2O3bulk and epilayer evaluated by terahertz time-domain spectroscopy,” Appl. Phys. Lett., vol. 118, no. 4, pp. 8–13, 2021, doi: 10.1063/5.0031531.DOI
  14. [14]P. Gopalan et al., “The anisotropic quasi-static permittivity of single-crystal β - Ga2O3measured by terahertz spectroscopy,” Appl. Phys. Lett., vol. 117, no. 25, 2020, doi: 10.1063/5.0031464.DOI
  15. [15]N. Blumenschein, C. Kadlec, O. Romanyuk, T. Paskova, J. F. Muth, and F. Kadlec, “Dielectric and conducting properties of unintentionally and Sn-doped β-Ga2O3 studied by terahertz spectroscopy,” J. Appl. Phys., vol. 127, no. 16, p. 165702, Apr. 2020, doi: 10.1063/1.5143735.DOI
  16. [16]H. Jiang et al., “Terahertz emission spectroscopy and microscopy on ultravide bandgap semiconductor ß-Ga2O3,” Photonics, vol. 7, no. 3, 2020, doi: 10.3390/PHOTONICS7030073.DOI
  17. [17]Emroj Hossain, Ruta Kulkarni, Rajib Mondal, Swati Guddolian, A. Azizur Rahman, Arumugam Thamizhavel and Arnab Bhattacharya, “Optimization of Gas Ambient for High Quality β-Ga2O3 Single Crystals Grown by the Optical Floating Zone Technique,” ECS J. Solid State Sci. Technol., vol. 8, no. 7, p. Q3144, 2019.DOI
  18. [18]S. Geller, “Crystal Structure of β-Ga2O3,” J. Chem. Phys., vol. 33, no. 3, p. 676, Aug. 2004, doi: 10.1063/1.1731237.
  19. [19]J.-B. Masson and G. Gallot, “Terahertz achromatic quarter-wave plate,” Opt. Lett., vol. 6, no. 30, pp. 265–267, 2006.pubmed.ncbi.nlm.nih.gov/16441051
  20. [20]C. J. Yang et al., “Birefringence of orthorhombic DyScO3: Toward a terahertz quarter-wave plate,” Appl. Phys. Lett., vol. 118, no. 22, 2021, doi: 10.1063/5.0043216.DOI
  21. [21]Z. Li, W. Liu, H. Cheng, S. Chen, and J. Tian, “Realizing Broadband and Invertible Linear-to-circular Polarization Converter with Ultrathin Single-layer Metasurface,” Sci. Rep., vol. 5, no. December, pp. 1–9, 2015, doi: 10.1038/srep18106.DOI

Paper details

vlnc:W_f9sauemt
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 3

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy