Local electronic structure of interstitial hydrogen in MgH2_2 inferred from muon study

Abstract

Magnesium hydride has great potential as a solid hydrogen (H) storage material because of its high H storage capacity of 7.6 wt%. However, its slow hydrogenation and dehydrogenation kinetics and the high temperature of 300 ∘^\circC required for decomposition are major obstacles to small-scale applications such as automobiles. The local electronic structure of interstitial H in MgH2_2 is an important fundamental knowledge in solving this problem, which has been studied mainly based on density functional theory (DFT). However, few experimental studies have been performed to assess the results of DFT calculations. We have therefore introduced muon (Mu) as pseudo-H into MgH2_2 and investigated the corresponding interstitial H states by analyzing their electronic and dynamical properties in detail. As a result, we observed multiple Mu states similar to those observed in wide-gap oxides, and found that their electronic states can be attributed to relaxed-excited states associated with donor/acceptor levels predicted by the recently proposed "ambipolarity model". This provides an indirect support for the DFT calculations on which the model is based via the donor/acceptor levels. An important implication of the muon results for improved hydrogen kinetics is that dehydrogenation, serving as a reductionreduction for hydrides, stabilizes the interstitial H−^- state.

Introduction

Hydrogen (H\mathrm{H}) storage materials are attracting attention for their importance as a core energy carrier in hydrogen energy production and utilization systems toward a decarbonized society [1, 2]. Therefore, there is a need for materials that can safely and efficiently store H\mathrm{H} and easily control the absorption and release of H\mathrm{H}. In particular, solid materials such as metal hydrides are characterized by high safety and high volume and weight densities, and there are great expectations for their practical use [3].

Among metal hydrides, magnesium hydrides have always attracted considerable interest. Magnesium reacts reversibly with H\mathrm{H} to form hydride (MgH2\mathrm{MgH}_2), which has great potential as a solid H\mathrm{H} storage material because of its high H\mathrm{H} storage capacity of 7.6 wt%. However, its slow hydrogenation and dehydrogenation rates and the high temperature of 300 °C required for decomposition are major obstacles to small-scale applications such as automobiles [3, 4]. Several experimental and theoretical studies have already been published on H\mathrm{H} kinetics in MgH2\mathrm{MgH}_2 to solve the problem. However, most of them have concentrated only on macroscopic analysis by thermodynamic measurements of the effects of ball milling, heavy ion irradiation, or the addition of trace metals or their oxides on the reaction kinetics [5, 6, 7, 8, 9, 10, 11].

Understanding the atomic-level mechanisms of hydrogenation and dehydrogenation processes is key to engineering solutions for accelerating these processes and lowering the decomposition temperatures. In MgH2\mathrm{MgH}_2, the local electronic state of isolated H\mathrm{H} at the interstitial site (Hi\mathrm{H_i}) is also one of the most fundamental pieces of information in elucidating the rate-limiting processes in H\mathrm{H} kinetics. Meanwhile, experimental means to study the microscopic states of isolated H\mathrm{H} in trace amounts in solids are limited, and so far the ab initio calculations based on density functional theory (DFT) have been the primary tool for this purpose [10, 12, 13]. However, there have been few experimental studies to assess the theoretical predictions to date.

To overcome this situation, we have introduced positive muon (μ+\mu^+) into MgH2\mathrm{MgH}_2, and investigated their electronic states and dynamical properties in detail using muon spin rotation (μ\muSR). Because the mass of μ+\mu^+ is two orders of magnitude (about 206 times) greater than the electron mass, the adiabatic approximation is sufficient for understanding μ+\mu^+-electron interaction. In fact, the difference in the Bohr radius between a μ+\mu^+ binding a single electron, known as muonium, and the corresponding H0\mathrm{H}^0 atom in vacuum is only 0.43%, implying that they have nearly the same electronic structure in the matter. Hereafter, the elemental symbol Mu will be introduced to denote μ+\mu^+ as pseudo-H, and the valence electronic states of Mu will be denoted as Mu+\mathrm{Mu^+}, Mu0\mathrm{Mu^0}, and Mu−\mathrm{Mu^-}. For deliberately avoiding distinction between Mu+\mathrm{Mu^+} and Mu−\mathrm{Mu^-}, both are referred to together as “diamagnetic Mu” and Mu0\mathrm{Mu^0} is called “paramagnetic Mu”.

In comparing experimental and theoretical results, there is an important issue to be pointed out at this stage. In conventional μ\muSR experiments, μ+\mu^+s are implanted as a relatively high-energy ion beam (typical kinetic energy of ∼\sim4 MeV), which generates free carriers and excitons in insulator crystals due to the associated electronic excitation towards the end of the radiation track [14, 15, 16]. These often propagate rapidly in the crystal, and there is experimental evidence that Mu acts as a capture center to form relaxed-excited states upon interaction with free carriers and/or excitons [17]. Accordingly, these Mu states do not necessarily correspond to the electronic state predicted from the thermodynamic charge conversion level (E+/−E^{+/-}) obtained by DFT calculations for thermal equilibrium conditions. Moreover, Mu is often observed to be accompanied by fast spin relaxation, which is due to spin/charge exchange interactions with excited carriers and/or excitons. While these phenomena are not observed for H in thermal equilibrium without such carriers, they can be regarded to simulate H in bulk excited states induced by light or electric fields, and Mu is useful as a microscopic probe for such states.

Another well-known evidence that Mu exhibits relaxed-excited states is that two or more different Mu electronic states are often observed simultaneously in the same material. In particular, two paramagnetic Mu states, the tetrahedral center Mu0\mathrm{Mu^0} and the bond center Mu0\mathrm{Mu^0}, have long been known in elemental semiconductors and III-V compound semiconductors [18], and these have been attributed to the states associated with the temporal acceptor and donor levels (E0/−E^{0/-} and E+/0E^{+/0}) rather than E+/−E^{+/-} [19]. With this in mind, we have recently focused on the diamagnetic Mu states, which are observed in pairs with Mu0\mathrm{Mu^0} in many wide-gap oxides but whose origin has been unexplored, and conducted an extensive survey to compare the previous experimental results and DFT calculations in the literature. As a result, assuming that the diamagnetic Mu corresponds to the donor-like state which is ionised because the E+/0E^{+/0} level is located within the conduction band, we found that the valence of the paired Mu states can be predicted from the positions of E0/−E^{0/-} and E+/0E^{+/0} in the band structure [17]. This allows us to describe the previous experimental results in a unified manner, and we call it the “ambipolarity model” because it is ascribed to the fact that the ambipolarity, which is the true nature of H, is expressed through these relaxed-excited states.

MgH2_2 crystalises in a stable rutile structure with few H vacancies at ambient condition (the decomposition reaction is endothermic [4]). It is a typical ionic insulator with a band gap above 5 eV, and the ambipolarity model combined with the results of DFT calculations for H predicts that Mu simultaneously takes on both acceptor and donor-like electronic states. The present experimental results are consistent with this prediction, suggesting that the ambipolarity model holds semi-quantitatively in MgH2_2. In the following, we will therefore organise the experimental results in terms of this model and attempt to interpret them based on their consistency with the predictions from the corresponding DFT calculations.

µSR Experiment and DFT Calculations

The sample used for μ\muSR measurements was obtained from a commercial vendor (Fujifilm Wako Chmicals Co.) as a powdered reagent sealed with inert gas. Immediately after opening the container, approximately 2 g of the powder was pressurised and shaped into a disk covered with aluminum foil, mounted on a temperature-controlled cryostat, and then degassed into a vacuum. The μ\muSR experiments were performed using the ARTEMIS spectrometer installed in the S1 area at the Materials and Life Science Experimental Facility in J-PARC, where a nearly 100% spin-polarised pulsed muon beam (25 Hz, with the full width at half-maximum of 80 ns and a momentum of 27 MeV/c) was transported to the sample. μ\muSR spectra [time-dependent positron asymmetry, A(t)A(t)] were measured from room temperature to 5 K in zero magnetic field (ZF) and under longitudinal magnetic fields (LF, 0.01–0.4 T).

The donor/acceptor levels for H assessed in this work are those based on Ref. [13]. They performed DFT calculations with screened hybrid functions of Heyd, Scuseria, and Ernzerhof (HSE) as implemented in the Vienna Ab initio Simulation Package (VASP) code. The amount of exact exchange mixed into the HSE generalized gradient functional is taken to 33%, which reproduces the experimentally observed lower limit of the band gap (5.2 eV). Defect calculations were performed for a supercell containing 72 atoms with 2×2×32 \times2 \times3 iterations of the primitive cell. A mesh of 2×2×22 \times2 \times2 special kk points and an energy cutoff value of 270 eV for the plane-wave basis set were used for the defective supercells. For charged defects, the number of electrons in the supercell was varied according to the format described in Ref. [20] and the electrons were localized on the impurity.

We have also performed DFT calculations to investigate in detail the local structure of H-related defects and to evaluate hyperfine parameters of Mu0^{0} and Δ\Delta of the diamagnetic Mu; the comparison of these with experimental values allows us to identify the corresponding donor/acceptor states involving Mu. The DFT calculations were within the generalized gradient approximation (GGA) and the projector augmented wave method as implemented in the QUANTUM ESPRESSO (QE) code [21]. The defects were simulated using 48-atom host supercell with 2×2×22 \times2 \times2 iterations of the primitive cell, and the Brillouin-zone integrations implemented by summations over a Monkhorst-Pack kk-point mesh of 3×3×53 \times3 \times5, with an energy cutoff of 100 Ry for the plane-wave basis set. The calculated lattice parameters c=0.301c = 0.301 nm, c/a=0.668c/a = 0.668, and u=0.304u = 0.304 are in good agreement with experimental values of 0.301 nm, 0.67, and 0.304 [22]. The band structure calculated for special kk-points is shown in Figure 1, which is in good agreement with the previous GGA calculations for the host [12]. It is noteworthy that the band gap is indirect (3.71 eV), and that the relatively steep dispersion near the conduction band minimum (CBM) and valence band maximum (VBM) suggests high mobility of excited carriers as well as a long lifetime.

Band structure of MgH2

Figure 1. Band structure of MgH2_2 calculated by QUANTUM ESPRESSO code (see text). Filled circles indicate the conduction band minimum and valence band maximum.

Result

Figure 2 shows the observed ZF/LF-μ\muSR time spectra at characteristic temperatures. It can be seen that A(t)A(t) mainly consists of two components, a paramagnetic component (labeled Mup_{\mathrm{p}}) whose asymmetry is gradually recovered by LF ≃\simeq 0.05–0.4 T and a component described by the Kubo-Toyabe function at ZF [equation (A3)] [23]. At lower temperatures, two more components emerges in the low LF range [Figure 2(a), labeled Mup2_{\mathrm{p2}} and MuS_{\mathrm{S}}, respectively], suggesting that the spectra consist of four components in total.

μSR time spectra under zero and longitudinal magnetic fields in MgH2 at typical temperatures

Figure 2. μ\muSR time spectra under zero and longitudinal magnetic fields in MgH2_2 at typical temperatures. (a) 5 K, (b) 56 K, (c) 130 K, (d) 204 K, (e) 298 K. (a)–(d): Right: time spectrum shows an initial paramagnetic Mu (Mup_{\mathrm{p}}, whose asymmetry is recovered by a longitudinal field) that exhibits conversion to a diamagnetic Mu state (Mud).Anotherparamagneticstate(Mu_{\mathrm{d}}). Another paramagnetic state (Mu_{\mathrm{p2}}$, showing fast relaxation) and a diamagnetic Mu component showing the lineshape well represented by the Kubo-Toyabe relaxation function (MuKT_{\mathrm{KT}}) can be seen. The solid line shows the result of the global fit based on the model (see text).

It is also noticeable in Figure 2(a) that these four components appear sequentially with increasing LF. This indicates that their hyperfine interactions (including those with nuclear magnetic moments) are mutually distinct, and each component can be identified by the magnitude of its characteristic LF. Therefore, even though these spectra do not show a significant change with temperature, a reliable analysis can be performed by building a model that reproduces their detailed LF dependence. In fact, it turns out from the LF-dependence that Mup_{\mathrm{p}} and Mup2_{\mathrm{p2}} components are paramagnetic states, while Mu3S_{3\mathrm{S}} and MuKT_{\mathrm{KT}} are diamagnetic states. The Mu3S_{3\mathrm{S}} component, which shows relatively fast exponential relaxation, is interpreted to be due to the H-Mu-H complex according to the previous report [24].

A closer look at the time spectra shows that, in order to correctly reproduce their time evolution, it is necessary to take into account the effects of the various spin/charge dynamics to which these states are subjected. More specifically, the sharp decrease of the initial asymmetry [A(0)A(0)] in the spectra at 0–10 mT from 0.22 (=AtotA_{\mathrm{tot}}) to the value roughly corresponding to that of MuKT_{\mathrm{KT}} [AKT∼A_{\mathrm{KT}}\sim0.09–0.14] within ∼\sim0.5 μ\mus at all temperatures suggests that the asymmetry corresponding to the spin-triplet state of Mup_{\mathrm{p}} [≃(Atot−AKT)/2\simeq(A_{\mathrm{tot}}-A_{\mathrm{KT}})/2, see equation (A10) in Appendix § 4] is lost due to the fast spin/charge exchange reaction with the excited carriers [18] or some epithermal processes [25, 26, 27]. In Figure 2(a), (Figure 2d) and (Figure 2e), there are nonrelaxing asymptotic components in the spectra with LF ≥\geq 50 mT, whose asymmetry recovers with increasing LF, suggesting a transition to the diamagnetic state (labeled Mud_{\mathrm{d}}) via an irreversible charge conversion reaction [28]. Furthermore, in the spectra in Figure 2(b) and (Figure 2c), the final Mud_{\mathrm{d}} state shows a slow relaxation where the decay rate is almost independent of LF, suggesting that fast fluctuations of the hyperfine field occur with increasing temperature even in the final state.

Based on the above observations, the time spectra were analyzed by the least-squares curve fits using the following phenomenological model for the spin/charge dynamics.

A(t)=ApdGpd(t)+Ap2Gp2(t)+AKTGzKT(t)+A3SGz3S(t),(1)A(t)=A_{\mathrm{pd}}G_{\mathrm{pd}}(t)+A_{\mathrm{p2}}G_{\mathrm{p2}}(t) +A_{\mathrm{KT}}G_z^{\mathrm{KT}}(t)+A_{3\mathrm{S}}G_z^{3\mathrm{S}}(t), \tag*{(1)}
Gpd(t)=fe−(λp+κ)tgz(xp)+(1−f)e−λdt,(2)G_{\mathrm{pd}}(t)=f e^{-(\lambda_{\mathrm{p}}+\kappa)t}g_z(x_{\mathrm{p}})+(1-f)e^{-\lambda_{\mathrm{d}}t}, \tag*{(2)}
λp=νp2(1+xp2),f=λpλp+κ,λd≃2Δd2νdω2+νd2,(3)\lambda_{\mathrm{p}}=\frac{\nu_{\mathrm{p}}}{2(1+x_{\mathrm{p}}^2)},\quad f=\frac{\lambda_{\mathrm{p}}}{\lambda_{\mathrm{p}}+\kappa},\quad\lambda_{\mathrm{d}}\simeq\frac{2\Delta_{\mathrm{d}}^2\nu_{\mathrm{d}}}{\omega^2+\nu_{\mathrm{d}}^2}, \tag*{(3)}
Gp2(t)=e−λp2tgz(xp2),λp2≃νp22(1+xp22),(4)G_{\mathrm{p2}}(t)=e^{-\lambda_{\mathrm{p2}}t}g_z(x_{\mathrm{p2}}),\quad\lambda_{\mathrm{p2}}\simeq\frac{\nu_{\mathrm{p2}}}{2(1+x_{\mathrm{p2}}^2)}, \tag*{(4)}

where ApdA_{\mathrm{pd}} is the sum of partial asymmetry for Mup_{\mathrm{p}} and Mud_{\mathrm{d}} components, Ap2A_{\mathrm{p2}}, AKTA_{\mathrm{KT}}, and A3SA_{3\mathrm{S}} are the partial asymmetry of the respective Mup2_{\mathrm{p2}}, MuKT_{\mathrm{KT}}, and Mu3S_{3\mathrm{S}} (Atot=Apd+Ap2+AKT+A3SA_{\mathrm{tot}}=A_{\mathrm{pd}}+A_{\mathrm{p2}}+A_{\mathrm{KT}}+A_{3\mathrm{S}}), GzKT(t;ΔKT,νKT)G_z^{\mathrm{KT}}(t;\Delta_{\mathrm{KT}},\nu_{\mathrm{KT}}) is the Kubo-Toyabe function for MuKT_{\mathrm{KT}} with ΔKT\Delta_{\mathrm{KT}} and νKT\nu_{\mathrm{KT}} being the linewidth and fluctuation frequency, Gz3S(t;ω3S,λ3S)G_z^{3\mathrm{S}}(t;\omega_{3\mathrm{S}},\lambda_{3\mathrm{S}}) is the relaxation function for the H-Mu-H complex state, ff is the fractional yield of Mup_{\mathrm{p}}, νp\nu_{\mathrm{p}} is the spin/charge exchange rate, κ\kappa is the charge conversion reaction rate from Mup_{\mathrm{p}} to Mud_{\mathrm{d}} [28], gz(x)=(12+x2)/(1+x2)g_z(x)=(\frac{1}{2}+x^2)/(1+x^2) is the initial polarization of the paramagnetic Mu, xp=B0(γμ−γe)/ωpx_{\mathrm{p}}=B_0(\gamma_\mu-\gamma_{\mathrm{e}})/\omega_{\mathrm{p}}, ωp\omega_{\mathrm{p}} is the hyperfine parameter (angular frequency) of Mup_{\mathrm{p}}, Δd\Delta_{\mathrm{d}} is the nuclear magnetic dipolar linewidth, ω=γμB0\omega=\gamma_\mu B_0, and νd\nu_{\mathrm{d}} is the fluctuation rate of Δd\Delta_{\mathrm{d}} including the effect of spin/charge exchange reaction. The parameter ff is determined by the competition between κ\kappa (varies with temperature) and λp\lambda_{\mathrm{p}}, and it also depends on LF. For Mup2_{\mathrm{p2}}, the relaxation due to the spin/charge exchange reaction (λp2\lambda_{\mathrm{p2}}) is considered as in the case of Mup_{\mathrm{p}}. νp2\nu_{\mathrm{p2}} is the spin/charge exchange rate for the Mup2_{\mathrm{p2}} component, xp2=B0(γμ−γe)/ωp2x_{\mathrm{p2}}=B_0(\gamma_\mu-\gamma_{\mathrm{e}})/\omega_{\mathrm{p2}}, and ωp2\omega_{\mathrm{p2}} is the hyperfine parameter of Mup2_{\mathrm{p2}}. [See Appendix § 4 for details on these relaxation functions, including the derivation of the equations (3)–(4).]

A schematic representation of the relationship between the four states and the meaning of the parameters in the equations (1)–(4) is shown in Figure 3.

Schematic diagram of the phenomenological model

Figure 3. A schematic diagram of the phenomenological model involving Mup_{\mathrm{p}}/Mud_{\mathrm{d}}, MuKT_{\mathrm{KT}}, Mup2_{\mathrm{p2}}, and Mu3S_{3\mathrm{S}} states and their spin/charge exchange reactions represented by equations (1)–(4). Here, the paramagnetic state are expressed as para and the diamagnetic states as dia. Since all the initial Mu states are relaxed-excited states (non-equilibrium), the arrow labeled “kBTk_{\mathrm{B}}T” represents the process of approaching thermal equilibrium by annealing as the temperature is increased.

In the curve-fit analysis, ωp\omega_{\mathrm{p}} showed a considerable temperature dependence [ωp/2π\omega_{\mathrm{p}}/2\pi ranging from 0.52(4) to 1.73(5) GHz] in accordance with varying νp\nu_{\mathrm{p}} and κ\kappa [see Figure A1 in Appendix § 4]. In particular, in the region where νp≳ωp/2π\nu_{\mathrm{p}}\gtrsim\omega_{\mathrm{p}}/2\pi [above ∼\sim150 K, see Figure 4(c)], ωp\omega_{\mathrm{p}} dropped sharply with decreasing accuracy. This is because the effective hyperfine parameter is reduced when the duration for a 1s orbital electron to exert a continuous hyperfine field on μ+\mu^{+} (∼1/νp\sim1/\nu_{\mathrm{p}}) becomes shorter than the spin rotation period due to the hyperfine interaction (∼2π/ωp\sim2\pi/\omega_{\mathrm{p}}) [18, 29, 30]. Such an effect, also known as “motional narrowing” in magnetic resonance, could account for the temperature dependence of ωp\omega_{\mathrm{p}} correlated with νp\nu_{\mathrm{p}}. In the following, in order to examine the temperature variation of other parameters without the effect of ωp\omega_{\mathrm{p}} ambiguity, the analysis was performed with ωp/2π\omega_{\mathrm{p}}/2\pi fixed at 0.721 GHz, the average value below 50 K where AtotA_{\mathrm{tot}} was also nearly constant.

Temperature dependence of the parameters obtained from the analysis

Figure 4. Temperature dependence of the parameters obtained from the analysis of ZF/LF-μ\muSR time spectra: (a) the initial asymmetry of each component, (b) the fractional yield of Mup_{\mathrm{p}}, (c) spin/charge fluctuation frequency of the Mup_{\mathrm{p}} component (νp\nu_{\mathrm{p}}) and conversion rate to Mud_{\mathrm{d}} (κ\kappa), (d), (e) nuclear dipolar linewidths of Mud_{\mathrm{d}} and MuKT_{\mathrm{KT}} (Δd\Delta_{\mathrm{d}} and ΔKT\Delta_{\mathrm{KT}}) and their fluctuation frequencies (νd\nu_{\mathrm{d}} and νKT\nu_{\mathrm{KT}}), (f) hyperfine parameters of the Mup2_{\mathrm{p2}} component (ωp2\omega_{\mathrm{p2}}) and its spin fluctuation frequency (νp2\nu_{\mathrm{p2}}), (g) the precession frequency (ω3S\omega_{3\mathrm{S}}) and relaxation rate (λ3S\lambda_{3\mathrm{S}}) of the H-Mu-H three-spin system.

Temperature dependence of the hyperfine parameter and spin/charge exchange and conversion rates

Figure A1. Temperature dependence of (a) the hyperfine parameter (ωp\omega_{\mathrm{p}}), (b) spin/charge exchange rate (νp\nu_{\mathrm{p}}) and conversion rate (κ\kappa) for the Mup_{\mathrm{p}} state obtained in the global curve-fit analysis in which ωp\omega_{\mathrm{p}} was allowed to vary as a free parameter, where νp\nu_{\mathrm{p}} was hardly determined above ∼150\sim150 K.

Although the result still showed a strong correlation between νp\nu_{\mathrm{p}} and κ\kappa, this can be reasonably understood by assuming that the charge conversion process occurs as part of the spin/charge exchange reaction (Figure 3, top left). The Mu3S_{3\mathrm{S}} signal was hard to be discerned from those of other components above ∼\sim150 K, and A3SA_{3\mathrm{S}} was set to zero for the analysis of data at higher temperatures. Meanwhile, since ωp2\omega_{\mathrm{p2}} showed a tendency of changing with temperature, we assumed that the hyperfine interaction of the second paramagnetic component Mup2_{\mathrm{p2}} could change with temperature (see below). As indicated by the solid curves in Figure 2, this phenomenological model reasonably reproduces the experimental data including the LF dependence at all temperatures. The temperature dependence of the parameters obtained from the curve-fits is shown in Figure 4.

The electronic state of Mu0^{0} is characterized by a relatively large hyperfine parameter (ωp/ωvac∼0.12\omega_{\mathrm{p}}/\omega_{\mathrm{vac}}\sim0.12–0.39). As is evident in Figure 4(a), (Figure 4b) and (Figure 4c), the decrease in ApdA_{\mathrm{pd}} and total signal amplitude AtotA_{\mathrm{tot}} seen over 50–150 K is in line with the decrease in conversion rate κ\kappa. On the other hand, νp\nu_{\mathrm{p}} appears to be almost constant over this temperature range. Therefore, the decrease of ApdA_{\mathrm{pd}} and AtotA_{\mathrm{tot}} suggests that the spin relaxation is induced by the fast spin/charge exchange reaction (νp\nu_{\mathrm{p}}) as the lifetime of the Mup_{\mathrm{p}} state (κ−1\kappa^{-1}) becomes longer. The magnitude of Δd\Delta_{\mathrm{d}} provides a clue to the local electronic structure of the final Mud_{\mathrm{d}} state.

local electronic structure of the final Mud_{\mathrm{d}} state. As shown in Figure 4(d), the average value of Δd\Delta_{\mathrm{d}} in the 50–150 K region is 2.71(2) MHz.

Regarding MuKT_{\mathrm{KT}} characterized by the quasi-static Kubo-Toyabe relaxation, the magnitude of the linewidth ΔKT\Delta_{\mathrm{KT}} again provides a strong clue to the microscopic local structure. As shown in Figure 4(e), ΔKT\Delta_{\mathrm{KT}} is 0.30–0.36 MHz in all temperature regions, while it is calculated to be greater than 0.63 MHz for any interstitial site without lattice relaxation. Although an exotic Mu state in which Mu is delocalized over two neighboring sites has been proposed in previous studies [31], another possibility is more likely from DFT calculations for H, as discussed below.

While the accuracy of the deduced parameters shown in Figure 4(f) seems limited due to its small amplitude (Ap2/Atot≲5A_{\mathrm{p2}}/A_{\mathrm{tot}}\lesssim5–10%), we find for the Mup2_{\mathrm{p2}} component that the entire time spectrum can be consistently reproduced when we assume that the relaxation is that exhibited by a paramagnetic state with ωp2/2π=20(7)\omega_{\mathrm{p2}}/2\pi=20(7)–274(41) MHz. The magnitude of ωp2\omega_{\mathrm{p2}} is a few % of ωvac\omega_{\mathrm{vac}} and significantly smaller than ωp\omega_{\mathrm{p}}. It is noticeable that ωp2\omega_{\mathrm{p2}} shows an increase of almost one order of magnitude in the 50–150 K region from both low and high temperatures. As discussed before, the effective hyperfine parameter would be reduced when νp2≫ωp2/2π\nu_{p2} \gg\omega_{p2}/2\pi, which seems to be the case for the change below ∼50\sim50 K. On the other hand, the decrease above 150 K is not accompanied by such an increase in νp2\nu_{p2}. Therefore, this may suggest a transition to a new paramagnetic state. It should be noted, however, that artifacts from the analysis with fixed ωp\omega_p may have affected the results.

Finally, let us give a brief overview on the Mu3S_{3\mathrm{S}} state. The corresponding signal exhibits relatively large relaxation rate at all temperatures, λ3S≫ω3S\lambda_{3\mathrm{S}} \gg\omega_{3\mathrm{S}}, which makes it difficult to clearly identify the oscillatory signal characteristic to the three-spin systems. While the mean value of ω3S/2π\omega_{3\mathrm{S}}/2\pi averaged over temperature can be derived to be 0.41(2) MHz [ω3S=2.6(1)\omega_{3\mathrm{S}} = 2.6(1) MHz, corresponding H-Mu distance rt=0.098(5)r_t = 0.098(5) nm], the actual systematic uncertainty is presumed to be larger than that determined statistically. The signal appears to merge with that of the Kubo-Toyabe component above ∼150\sim150 K, implying the instability of the H-Mu-H state.

Discussion

Predictions based on the ambipolarity model and DFT calculations

In order to compare these results with the predictions of ambipolarity model plus DFT calculations, we extracted information related to the formation energy of H-related defects from the literature [13] and summarized it for Mu as shown in Figure 5. The thermodynamic defect formation energy Ξq\Xi^q of Hq^q (with q=0,±q = 0,\pm being the valence) in a certain material is evaluated by DFT calculations using the following formula,

Formation energy of H-related defects versus the Fermi level, and schematic band diagrams

Figure 5. The formation energy (Ξq\Xi^q) of H-related defects vs the Fermi level (EFE_F) in MgH2_2 obtained by DFT calculations, where (a) is for the case of interstitial H atoms (Hiq\mathrm{H}_i^q, q=0,±q = 0,\pm), and (b) is for the interstitial molecules [H2]iq[\mathrm{H}_2]_i^q, q=0,±,2±q = 0,\pm,2\pm, respectively corresponding to Mui_i and [HMu]i_i. Paramagnetic states are expressed as “para” and the diamagnetic states as “dia”. The levels for acceptor (E0/−E^{0/-}) and donor (E+/0E^{+/0}) are determined as cross points between Ξ±(EF)\Xi^{\pm}(E_F) and Ξ0(EF)\Xi^0(E_F). The dashed line shows the intrinsic charge neutral level (EFintE_F^{\mathrm{int}}) obtained from the DFT calculation. (Adapted from Ref. [13]) Schematic band diagrams for the single electron energy associated with the donor/acceptor levels (single-charge conversion levels only) in (a) and (b) are shown in (c) and (d), respectively. The level indicated by a dashed line near the CBM in (d) is a shallow state suggested from DFT calculations. For the corresponding local electronic structure, see Figure 6,Figure 7. (e), (f) Schematic of Ξq\Xi^q versus configuration coordinate (QQ) for Mui0_i^0 and the charged states, where ElrE_{\mathrm{lr}} is the lattice relaxation energy, EelE_{\mathrm{el}} is the Coulomb energy, and VV is the potential barrier between the two states. Mui0_i^0 is expected to be observed as a relaxed excited state for (e) V>0V > 0 but not for (f) V=0V = 0.

Ξq(EF)=Etot[Hq]−Etot[host]+qEF+nHμH,(5)\Xi^q(E_F) = E_{\mathrm{tot}}[\mathrm{H}^q] - E_{\mathrm{tot}}[\mathrm{host}] + qE_F + n_{\mathrm{H}}\mu_{\mathrm{H}}, \tag*{(5)}

where Etot[Hq]E_{\mathrm{tot}}[\mathrm{H}^q] and Etot[host]E_{\mathrm{tot}}[\mathrm{host}] are the total energies calculated for the supercell with and without Hq^q between lattices, respectively, and EFE_F is the Fermi energy. μH\mu_{\mathrm{H}} is the H chemical potential that represents the change in Ξq\Xi^q when H is removed (nH=−1n_{\mathrm{H}} = -1) or added (nH=+1n_{\mathrm{H}} = +1) to the host crystal upon defect formation. We assume that Mu’s experimental results correspond to calculations in the limit where the added H is dilute, i.e., under H-poor conditions in terms of chemical potential. This is supported by the fact that the sample was immediately transferred from the inert gas-tight container to a vacuum environment, where the H partial pressure in the sample environment was kept negligibly small. In addition, previous μ\muSR experiments have shown that the yield of H-Mu-H complexes, which assumes the pre-existence of extra Hi_i atoms, is small for as-prepared samples and increases with dehydrogenation processes such as milling and oxidation catalyst incorporation [24]. The present experimental result is similar to that of this as-prepared

sample (see below), suggesting that the amount of extra H was small. We also point out that a part of the extra Hi_i contributing to the H-Mu-H complexes could be that ejected from the lattice point by elastic scattering with incident muons (see Appendix § 5).

Based on Figure 5 and the ambipolarity model, the following predictions can be made. Firstly, regarding the general trend of Ξq\Xi^q obtained for interstitial H (Hi_i) shown in Figure 5(a), the E0/−E^{0/-} and E+/0E^{+/0} levels are on the higher energy side than the E+/−E^{+/-} level, indicating the negative UU character due to strong electron-phonon interactions [32]. Moreover, both E0/−E^{0/-} and E+/0E^{+/0} form apparently deep gap levels, in which the existence of two paramagnetic Mu states (Mui0_i^0’s) may be expected. However, as shown in Figure 5(e) and (Figure 5f), whether Mui0_i^0 can actually exist as a relaxed excited state depends on the presence of a potential barrier VV at the transition to the charged states. As we will see below, V>0V > 0 is inferred for the transition to Mui+_i^+, while V≃0V \simeq0 is suggested for the transition to Mui−_i^- because the Mui0_i^0 state corresponding to the acceptor level is not observed in the experiment (although this does not rule out the possibility of short-lived Mui0_i^0). Note that the one-electron energy levels shown in Figure 5(c) correspond to EelE_{\rm el}, not E−/0E^{-/0}. Regarding the Hi−_i^- state (corresponding to Mui−_i^-), it is predicted to accompany significant local lattice relaxation; Hi−_i^- pushes away the surrounding ligand H−^- atoms by 0.052 nm while it attracts Mg2+^{2+} [12]. On the other hand, the charged donor-like H (Hi+_i^+, corresponding to Mui+_i^+) binds strongly to the ligand H, forming a neutral HMu molecule corresponding to the onsite H2_2 molecule [12]. The single-electron energetics are shown in Figure 5(c).

Secondly, provided that Mu can form an interstitial molecule with a pre-existing Hi_i atom (denoted as [HMu]i_i), the electronic states for the interstitial H2_2 molecules ([H2_2]i_i) predicted by the DFT calculations can provide the basis for discussing those of [HMu]i_i. As shown in Figure 5(b), the [HMu]i0_i^0 state is stable over a wide EFE_F region in the band gap, showing lower formation energy than that for [HMu]i+_i^+ and [HMu]i−_i^- (i.e., positive-UU), and can exist even in thermal equilibrium. The E0/−E^{0/-} and E+/0E^{+/0} levels are closer to the band edge than for the isolated Mu, and E0/−E^{0/-} appears to overlap the conduction band minimum (CBM). Regarding the local structure, the [HMu]i+_i^+ molecule is pulled to ligand H−^- to form a paramagnetic complex state (see below). The double charge conversion levels for [HMu]i2+_i^{2+} and [HMu]i2−_i^{2-} are closer to the charge neutral level (EF0E_F^0) and form deeper levels. The [HMu]i2+_i^{2+} molecular states are unstable, and both H and Mu are presumed to form onsite neutral H2_2 and HMu molecules with ligand H−^-, respectively. The corresponding single-electron energetics are shown in Figure 5(d).

Local electronic structure of each Mu state

In order to obtain further clues about the correspondence between these DFT predictions and the experimental results for Mu, we have investigated the local defect structure associated with these acceptor/donor levels in each of the above two cases by QE calculations. The obtained local structures for Hi_i and [H2_2]i_i are shown in Figure 6 and Figure 7, respectively, where those for Hi_i are in good agreement with earlier GGA results using VASP code [12]. We found that the E+/0E^{+/0} level associated with Hi_i (= Mui_i) and that of the [H2_2]i_i molecule (= [HMu]i_i) have a finite unpaired electron density in the band gap (i.e., the paramagnetic states). This is consistent with the experimental observation of two paramagnetic states, Mup_p and Mup2_{p2}. The hyperfine parameters calculated by GIPAW module of the QE suite for these states are listed in Table 1. They exhibit a common character that the Fermi contact interaction is predominant. For the other diamagnetic states, the nuclear dipolar width Δ\Delta are summarized in Table 2.

Local structure of interstitial H in positive, neutral, and hydride states

Figure 6. Local structure of interstitial H (Hi_i) in (a) positive, (b) neutral, and (c) hydride states which are substituted with Mu (red balls), viewed from bb (left) and cc (right) axes, respectively.

Local structure of an interstitial hydrogen molecule

Figure 7. Local structure of an interstitial hydrogen molecule in (a) [H2]i0[\mathrm{H}_{2}]_{\mathrm{i}}^{0} and (b) [H2]i+[\mathrm{H}_{2}]_{\mathrm{i}}^{+} states with one H atom substituted by Mu (red balls), viewed from bb (left) and cc (right) axes, respectively. There are two inequivalent H denoted by labels I and II for (b), where the case with HI_{\mathrm{I}} replaced with Mu is shown. The hyperfine parameters for (b) are distributed over four H atoms indicated by a dashed ellipse.

Magnetic dipolar term (MHz)Principal axis
Hi0\mathrm{H}_{\mathrm{i}}^{0}ωxx/2π\omega_{xx}/2\pi −0.0295(0, 0, 1)
ωyy/2π\omega_{yy}/2\pi −1.8829(0.5514, −0.8342, 0)
ωzz/2π\omega_{zz}/2\pi 1.9125(−0.8342, −0.5514, 0)
Fermi contact term (MHz)
ωc/2π\omega_{\mathrm{c}}/2\pi 630.013—
[H2]i+[\mathrm{H}_{2}]_{\mathrm{i}}^{+}, I
Magnetic dipolar term (MHz)Principal axis
ωxx/2π\omega_{xx}/2\pi −19.1146(0.4991, −0.8665, 0)
ωyy/2π\omega_{yy}/2\pi −19.5940(0, 0, 1)
ωzz/2π\omega_{zz}/2\pi 38.7086(−0.8665, −0.4991, 0)
Fermi contact term (MHz)
ωc/2π\omega_{\mathrm{c}}/2\pi 267.150—
[H2]i+[\mathrm{H}_{2}]_{\mathrm{i}}^{+}, II
Magnetic dipolar term (MHz)Principal axis
ωxx/2π\omega_{xx}/2\pi −3.1894(0, 0, 1)
ωyy/2π\omega_{yy}/2\pi −4.7335(0.3198, −0.9475, 0)
ωzz/2π\omega_{zz}/2\pi 1.9125(−0.9475, −0.3198, 0)
Fermi contact term (MHz)
ωc/2π\omega_{\mathrm{c}}/2\pi 271.750—
Mu h.f. (GHz)Mui0(ωc)\mathrm{Mu}_{\mathrm{i}}^{0}(\omega_{\mathrm{c}}) 2.003[HMu]i+(ωc)[\mathrm{HMu}]_{\mathrm{i}}^{+}(\omega_{\mathrm{c}}) (I) 0.849 / (II) 0.864
Exp. (GHz)Mup(ωp)\mathrm{Mu}_{\mathrm{p}}(\omega_{\mathrm{p}}) 0.524(4)–1.73(5)Mup2(ωp2)\mathrm{Mu}_{\mathrm{p2}}(\omega_{\mathrm{p2}}) 0.020(7)–0.274(41)

Table 1. Calculated hyperfine parameters for the paramagnetic states: Hi0\mathrm{H}_{\mathrm{i}}^{0} [corresponding to Figure 6(b)] and those for each H in [H2]i+[\mathrm{H}_{2}]_{\mathrm{i}}^{+} molecule [I and II in Figure 7(b)]. The values for Mu must be multiplied by 3.18. The bottom rows show experimental values for paramagnetic Mu states in comparison with those for candidate paramagnetic states inferred from DFT calculations.

Mui\mathrm{Mu}_{\mathrm{i}}[HMu]i[\mathrm{HMu}]_{\mathrm{i}}
Electronic state / Δ\Delta (MHz)Mui+\mathrm{Mu}_{\mathrm{i}}^{+} / 3.64Mui−\mathrm{Mu}_{\mathrm{i}}^{-} / 0.3685[HMu]i0,2±[\mathrm{HMu}]_{\mathrm{i}}^{0,2\pm} / 3.2–3.9
Exp. (MHz)Mud\mathrm{Mu}_{\mathrm{d}} (Δd\Delta_{\mathrm{d}}) / 2.71(2)MuKT\mathrm{Mu}_{\mathrm{KT}} (ΔKT\Delta_{\mathrm{KT}}) / 0.330(4)Mu3S\mathrm{Mu}_{3\mathrm{S}} (ω3S\omega_{3\mathrm{S}}) / 2.6(1)

Table 2. Calculated nuclear dipolar linewidth Δ\Delta for the diamagnetic Mu states. The bottom row shows experimental values for diamagnetic Mu corresponding to each state in the upper row.

Given that the Mu states associated with the defect levels in Figure 5(c) and (d) are meaningful only in the non-equilibrium state, there is no guarantee that the electronic structures of Mu discussed below correspond to those in thermal equilibrium. However, since the latter are generally not significantly altered by EFE_F, it is reasonable to assume that, among the relaxed-excited states, those that can also exist in thermal equilibrium have the same electronic structure as the latter. Specifically, for the Mui_i states (negative-UU centers), Mui0_i^0 has no corresponding state in thermal equilibrium, but Mui+_i^+ states correspond to those in thermal equilibrium (and to Hi+_i^+); for the [HMu]i_i molecules (positive-UU centers), all states possibly correspond to those in thermal equilibrium (and to [H2_2]i_i). In light of the above considerations, we discuss the correspondence between these levels and the experimentally observed Mu states.

• Mup_p and Mud_d

As mentioned earlier, there is considerable uncertainty in the experimental estimate of ωp\omega_p (see the bottom row of Table 1 and Figure A1), making it difficult to determine whether Mup_p corresponds to Mui0_i^0 or [HMu]i+_i^+ from the value of ωp\omega_p alone. Since Mup_p/Mud_d is considered to be a pair with MuKT_{KT} from the antipolarity model, let us first discuss the attribution of Mud_d. The empirical rule in the model suggests that the yields of paired acceptor-like and donor-like Mu are nearly equal to satisfy overall charge neutrality. Given that ApdA_{pd} is comparable with AKTA_{KT} over the wide temperature range and that MuKT\mathrm{Mu}_{\mathrm{KT}} is attributed to Mui−\mathrm{Mu}_{\mathrm{i}}^{-} (see below), it is reasonable to ascribe Mud\mathrm{Mu}_{\mathrm{d}} to Mui+\mathrm{Mu}_{\mathrm{i}}^{+}, and thus Mup\mathrm{Mu}_{\mathrm{p}} is ascribed to Mui0\mathrm{Mu}_{\mathrm{i}}^{0}. The latter is also in line with the fact that the maximum value of ωp\omega_{\mathrm{p}} [= 2π×1.73(5)2\pi\times1.73(5) GHz, realized when the “motional narrowing” effect is negligible] is about 86% of the value predicted from ωc\omega_{\mathrm{c}} of Hi0\mathrm{H}_{\mathrm{i}}^{0} (= 2π×2.0032\pi\times2.003 GHz), which is closer than that of [H2]i+[\mathrm{H}_{2}]_{\mathrm{i}}^{+} (= 2π×0.852\pi\times0.85–0.860.86 GHz). Furthermore, this result indicates that the potential barrier for the transition from Mui0\mathrm{Mu}_{\mathrm{i}}^{0} to Mui+\mathrm{Mu}_{\mathrm{i}}^{+} is positive [V>0V > 0, see Figure 5(e)].

For the experimental value of Δd\Delta_{\mathrm{d}}, it can be explained when the H-Mu distance is r=0.083r = 0.083 nm, about 11% larger than the p-p distance of 0.078 nm estimated from

the QE calculation. The relatively large νd\nu_{\mathrm{d}} (150–230 MHz) suggests that even after Mup\mathrm{Mu}_{\mathrm{p}} (= Mui0\mathrm{Mu}_{\mathrm{i}}^{0}) destabilizes and transitions to Mud\mathrm{Mu}_{\mathrm{d}} (= Mui+\mathrm{Mu}_{\mathrm{i}}^{+}), a fast spin/charge exchange reaction (Mui++e−⇄Mui0\mathrm{Mu}_{\mathrm{i}}^{+} + e^{-} \rightleftarrows\mathrm{Mu}_{\mathrm{i}}^{0}) persists with the excitonic carriers.

MuKT\mathrm{Mu}_{\mathrm{KT}}

The linewidth ΔKT\Delta_{\mathrm{KT}} of the MuKT\mathrm{Mu}_{\mathrm{KT}} component [= 0.330(4) MHz on average, see Figure 4(e)] is in good agreement with 0.3685 MHz expected for Mui−\mathrm{Mu}_{\mathrm{i}}^{-} that accompanies significant outward relaxation of the surrounding H−^{-}. Considering that the incident μ+\mu^{+} is accompanied by ∼102\sim10^{2} electron-hole pairs (see Appendix B), it may be allowed to assume that the probability of capturing two electrons and taking the anion state is sufficiently high. As discussed earlier, the reason why the relaxed excited state Mu0\mathrm{Mu}^{0} associated with this state is not observed is presumably because there is no potential barrier for the transition to Mui−\mathrm{Mu}_{\mathrm{i}}^{-} [V≃0V \simeq0, see Figure 5(f)]. This unusual situation may be related to the large lattice relaxation around Mui−\mathrm{Mu}_{\mathrm{i}}^{-} and the strong binding energy due to the associated Coulomb interaction. Thus, MuKT\mathrm{Mu}_{\mathrm{KT}} is ascribed to the diamagnetic state associated with the effective acceptor level of isolated Mui\mathrm{Mu}_{\mathrm{i}} (i.e., MuKT=Mui−\mathrm{Mu}_{\mathrm{KT}} = \mathrm{Mu}_{\mathrm{i}}^{-}). From the fact that ApdA_{\mathrm{pd}} and AKTA_{\mathrm{KT}} are comparable and account for the majority of the μSR\mu\mathrm{SR} signal, we conclude that the major part of the observed relaxed-excited Mu states can be explained by the pair Mui+\mathrm{Mu}_{\mathrm{i}}^{+} and Mui−\mathrm{Mu}_{\mathrm{i}}^{-}.

Mup2\mathrm{Mu}_{\mathrm{p2}}

Apart from the cases below 50 K, where νp2>ωp2\nu_{\mathrm{p2}} > \omega_{\mathrm{p2}} and thus ωp2\omega_{\mathrm{p2}} is not well defined, ωp2/2π\omega_{\mathrm{p2}}/2\pi is 0.1–0.3 GHz for 50–150 K and 20–50 MHz above ∼150\sim150 K, which do not correspond to the hyperfine parameters (ωc\omega_{\mathrm{c}}) of any state in Table 1. However, given that Mup\mathrm{Mu}_{\mathrm{p}} corresponds to Mui0\mathrm{Mu}_{\mathrm{i}}^{0}, the only remaining possibility for Mup2\mathrm{Mu}_{p2} is to be attributed to [HMu]i+[\mathrm{HMu}]_{i}^{+}.

As shown in Figure 7(b) and Table 1, our QE calculations indicate that the local structure of [H2]i+[\mathrm{H}_{2}]_{i}^{+} is complicated, resulting in the two inequivalent H sites with different hyperfine parameters (labeled I and II). Since the Fermi contact term may be strongly dependent on the choice of PAW dataset, one cannot rule out the possibility that the calculated value for such a complex local structure may be highly indeterminate. Meanwhile, ωp2\omega_{p2} is comparable with the value expected from the dipolar terms: e.g., for [H2]i+[\mathrm{H}_{2}]_{i}^{+}-I, the powder average [(ωxx2+ωyy2+ωzz2)/3]1/2×3.18=87.4[(\omega_{xx}^{2}+\omega_{yy}^{2}+\omega_{zz}^{2})/3]^{1/2}\times3.18=87.4 MHz. Although this may just be a coincidence, it reminds us that such polaronic states have been reported in some wide-gap oxides (e.g., SrTiO3_3 [33], which are supposedly induced by Mu-exciton interaction [17]), and Mup2\mathrm{Mu}_{p2} may correspond to such a state.

Mu3S_{3S}

The ambipolarity model suggests that the Mu3S_{3S} state (which is paired with Mup2\mathrm{Mu}_{p2}) corresponds to the diamagnetic [HMu]i0[\mathrm{HMu}]_{i}^{0} state associated with the E−/0E^{-}/0 level near the CBM. As shown in Table 2, the fact that the value of ω3S\omega_{3S} is comparable with the calculated Δ\Delta also supports this conjecture. Although the fast relaxation of the signal makes it difficult to examine the local electronic structure in detail, it is plausible that the Mu3S_{3S} state consists of the [HMu]i0[\mathrm{HMu}]_{i}^{0} molecule bonded to a ligand H−^{-} via the hydrogen bonding. It is likely that the H-Mu-H signal reported earlier also stems from the same complex state. As noted in the discussion about the chemical potential of H in equation (5), since extra Hi_{i} must exist beforehand for Mu3S_{3S} to be observed, the amplitude of the signal should be proportional to the amount of such Hi_{i}. Therefore, the present experimental result suggests that a relatively small amount of Hi_{i} existed in the as-prepared sample.

Dynamical model

Applying these attributed electronic states of Mu to the phenomenological model, Figure 3 is updated to Figure 8. Based on this, we consider a scenario that explains the rough temperature variation of each state observed in Figure 4. AKTA_{\mathrm{KT}} shows a marked increase above 150 K, which is clearly correlated with the increase in the charge transfer reaction rate κ\kappa from Mui0\mathrm{Mu}_{i}^{0} (= Mup\mathrm{Mu}_{p}) to Mui+\mathrm{Mu}_{i}^{+} (= Mud\mathrm{Mu}_{d}). This suggests that the transition from Mui0\mathrm{Mu}_{i}^{0} to Mui−\mathrm{Mu}_{i}^{-} via Mui+\mathrm{Mu}_{i}^{+} is accelerated by the annealing effect with increasing temperature. A similar transition from Mu3S_{3S} to MuKT−\mathrm{Mu}_{\mathrm{KT}}^{-} is suggested to occur in parallel with that for Mui+\mathrm{Mu}_{i}^{+}. These annealing-induced transitions are explained by the fact that the formation energy Eq(EF)E^{q}(E_{\mathrm{F}}) of Mui−\mathrm{Mu}_{i}^{-} is lower than those of Mui0\mathrm{Mu}_{i}^{0} around EF≃E+/0E_{\mathrm{F}}\simeq E^{+/0} and [HMu]i0[\mathrm{HMu}]_{i}^{0} around EF≃E0/−E_{\mathrm{F}}\simeq E^{0/-}, as shown in Figure 5(a) and (b).

Electronic states of Mu estimated on the basis of the ambipolarity and phenomenological model

Figure 8. The electronic states of Mu estimated on the basis of the ambipolarity and phenomenological model shown in Figure 3, where Mui0=Mup\mathrm{Mu}_{i}^{0}=\mathrm{Mu}_{p}, Mui+=Mud\mathrm{Mu}_{i}^{+}=\mathrm{Mu}_{d}, Mui−=MuKT−\mathrm{Mu}_{i}^{-}=\mathrm{Mu}_{\mathrm{KT}}^{-}, [HMu]i+=Mup2[\mathrm{HMu}]_{i}^{+}=\mathrm{Mu}_{p2}, and [HMu]i0=Mu3S[\mathrm{HMu}]_{i}^{0}=\mathrm{Mu}_{3S}. The possibility is shown that Mui+\mathrm{Mu}_{i}^{+}, Mui−\mathrm{Mu}_{i}^{-}, and [HMu]i0[\mathrm{HMu}]_{i}^{0} states may be affected by spin fluctuations of the nearby H centers in the relaxed-excited state (denoted as H∗^{*}), a factor not explicitly taken into account in the analysis.

The dynamic model we introduced in equations (1)–(4) cannot distinguish whether the fluctuation of the internal magnetic field felt by Mu is due to carrier motion or self-

diffusion of Mu. The carrier motion is a strong candidate as the cause of the fluctuations, since the band structure in Figure 1 predicts that both electrons and holes are only weakly localized in MgH2_2. Regarding the Mu motion, the diamagnetic Mui_{i} is also considered to be localized (at least in the time scale of μ\muSR) because it is bonded to the ligand H−^{-} (Mui+\mathrm{Mu}_{i}^{+}) or accompanying large lattice distortions (Mui−\mathrm{Mu}_{i}^{-}, as inferred from νKT\nu_{\mathrm{KT}}; see the next section for more detail). On the other hand, it is known that the acceptor-like neutral Mui0\mathrm{Mu}_{i}^{0} can exhibit rapid long-range diffusion (e.g., in alkali halides [34, 35] and III-V semiconductors [36, 37]). When Mui0\mathrm{Mu}_{i}^{0} exhibits self-diffusion, the fluctuation of the nuclear hyperfine (NHF) interaction between 1s orbital electron and proton nuclear spins also induces Mui0\mathrm{Mu}_{i}^{0} spin relaxation. In this case, the magnetic field dependence of the longitudinal relaxation rate is expected to be weaker than that for λp\lambda_{p} [see equation (3)], and to vary significantly with the jump frequency of Mui0\mathrm{Mu}_{i}^{0} [34, 35, 36, 37]. However, λp\lambda_{p} is so large (>101>10^{1} MHz) over the wide temperature range (5–298 K) that such a possibility as the origin of longitudinal relaxation seems unlikely. Moreover, the present experimental results suggest that even if the Mui0\mathrm{Mu}_{i}^{0} state exists, it is converted to Mui−\mathrm{Mu}_{i}^{-} in a short lifetime (∼κ−1\sim\kappa^{-1}). Regarding the [HMu]i[\mathrm{HMu}]_{i} states, they have a mass one order of magnitude larger than Mu, and are considered to be even more localized than the diamagnetic Mui_{i}. Therefore, the values of the dynamical parameters introduced in the model can be interpreted as mainly reflecting the carrier motion.

Finally, regarding the initial electronic states of Mup_{p}/Mud_{d}-MuKT_{\mathrm{KT}} pair (i.e., Mui0\mathrm{Mu}_{i}^{0}/ Mui+\mathrm{Mu}_{i}^{+} and Mui−\mathrm{Mu}_{i}^{-}), neutral and negative ionic states are predominant as a whole. As shown in Figure 5, the EFintE_{\mathrm{F}}^{\mathrm{int}} level is close to the CBM, and the formation energy EFintE_{\mathrm{F}}^{\mathrm{int}} for all electronic states is neutral or negative ionic ground state. Therefore, the population of Mu valence for the relaxed-excited states implies that the overall charge average is close to that of thermal equilibrium. In other words, the reason why Mu (and H) simultaneously assumes donor and acceptor states in the relaxed-excited state is presumably to maintain the global charge neutrality of the system consisting of the host and H.

In conclusion, assuming that the electronic state of Mu implanted into MgH2_2 takes the two pairs of defect centers (relaxed-excited states) associated with the donor/acceptor levels for interstitial Mu and HMu molecule states predicted from the DFT calculations, a scenario that coherently describe the present experimental results can be constructed.

Implications to the kinetics and diffusion of interstitial H

Now, let us discuss what we can learn for H kinetics from these results. It has been reported that the addition of a few % of transition metals such as Ti significantly improves the H kinetics [38, 39, 40]. DFT calculations suggest that, when a transition metal exhibits negative UU character to accompany a double charge conversion level ETM+/−E_{\mathrm{TM}}^{+/-} in the host, the addition of the transition metal is expected to shift the Fermi level by ΔE=ETM+/−−EFint\Delta E = E_{\mathrm{TM}}^{+/-} - E_{\mathrm{F}}^{\mathrm{int}} [13]. As can be seen in Figure 5(a), for ΔE>0\Delta E > 0 (as predicted for Ti), the interstitial H is stable in the Hi−_{\mathrm{i}}^{-} state, and this is assumed to be the cause of the kinetic improvement by avoiding binding of Hi_{\mathrm{i}} to the ligand H−^{-}.

On the other hand, it is also reported that ball milling with a small amount of Nb2_2O5_5 improves the kinetics [41]. From μ\muSR in the samples after milling with 5 wt% Nb2_2O5_5, a decrease of the characteristic temperature TdT_{\mathrm{d}} where diffusion motion of H and/or Mu sets in (as inferred from sharp decrease in ΔKT\Delta K_{\mathrm{T}}) from 650 K to about 450 K was observed [24]. Assuming that Nb2_2O5_5 is an oxidation catalyst and that stabilization of the Hi−_{\mathrm{i}}^{-} state is the key to improving kinetics, it can be interpreted that Nb2_2O5_5 raises bulk EFE_{\mathrm{F}} by causing dehydrogenation;

MgH2⟶MgH2−δ+δ2H2+δe−.\mathrm{MgH}_2 \longrightarrow\mathrm{MgH}_{2-\delta} + \frac{\delta}{2}\mathrm{H}_2 + \delta e^{-}.

The fact that a similar effect is obtained in the case of ball milling alone suggests that the increased surface area also promotes dehydrogenation reactions by atmospheric oxygen. It is paradoxical that dehydrogenation corresponds to reduction for hydrides.

Meanwhile, it has also been reported that the formation of the Mu3S_{3\mathrm{S}} state (corresponding to the H−^{-}-H+^{+}-H−^{-} complex state) is promoted in those samples [24]. Since such hydrogen bond formation is expected to be rather unfavorable from a diffusion point of view, it is assumed that the reason why H kinetics improves with Nb2_2O5_5 addition is because the effect of stabilizing Hi−_{\mathrm{i}}^{-} outweighs that of hydrogen bond formation; the upward shift of EFE_{\mathrm{F}} will eventually lead to the dissociation reaction,

Hi−−Hi+−Hi−+2e−⟶H−+[H2]i−+e−⟶H−+2Hi−.\mathrm{H}_{\mathrm{i}}^{-}\mathrm{-H}_{\mathrm{i}}^{+}\mathrm{-H}_{\mathrm{i}}^{-} + 2e^{-} \longrightarrow\mathrm{H}^{-} + [\mathrm{H}_2]_{\mathrm{i}}^{-} + e^{-} \longrightarrow\mathrm{H}^{-} + 2\mathrm{H}_{\mathrm{i}}^{-}.

A similar situation is suggested from an earlier μ\muSR study for the effect of Ti-doping to NaAlH4_4 [42, 43].

Regarding the MuKT_{\mathrm{KT}} state corresponding to Hi−_{\mathrm{i}}^{-}, the magnitude of ΔKT\Delta K_{\mathrm{T}} is found to vary very little over the entire temperature range, indicating that the Mu site remains unchanged over the time range of ∼101 μs\sim10^{1}\,\mu\mathrm{s}. The fluctuation frequency νKT\nu_{\mathrm{KT}} shows nearly constant value of ∼0.1\sim0.1 MHz below 150 K, which is unlikely to be attributed to thermally activated diffusive motion of MuKT_{\mathrm{KT}}. The non-monotonic temperature dependence of νKT\nu_{\mathrm{KT}} above 150 K also suggests that the cause is non-thermal. In addition, the paramagnetic Mu components (Mup_{\mathrm{p}}/Mud_{\mathrm{d}} and Mup2_{\mathrm{p2}}) show fast spin and/or charge exchange reaction with excited carriers even below 150 K. Considering that the frequency of paramagnetic fluctuations (>102> 10^{2} MHz) are far from the sensitive range for the diamagnetic Mu, these observations suggest that the fluctuations of ΔKT\Delta K_{\mathrm{T}} is induced by the relaxation of proton spins of the nearby H(’s) in the relaxed-excited states (denoted as H*) generated upon muon implantation (see Figure 8).

Note that H* can be any of the observed four Mu states with H substituting for Mu, which may be appropriately referred to Hp_{\mathrm{p}}/Hd_{\mathrm{d}}, HKT_{\mathrm{KT}}, Hp2_{\mathrm{p2}}, and H3S_{3\mathrm{S}}. The proton spin relaxation rates λ∗\lambda^{*} in these states can be evaluated by reducing those for the diamagnetic Mu (inferred from Figure 4) by a factor R2≡[γp/γμ]2R^{2} \equiv[\gamma_{\mathrm{p}}/\gamma_{\mu}]^{2} (=0.0986= 0.0986) for the same fluctuation as observed in Mu, e.g., λ∗=R2λ3S∼0.2\lambda^{*} = R^{2}\lambda_{3\mathrm{S}} \sim0.2–0.5 MHz for the H3S_{3\mathrm{S}} state. This implies that further experimental verification will be necessary to determine whether the fluctuations of nuclear dipolar fields exerted by H to the Mg atom binding a negative muon (pseudo-Na atom) observed by negative muon μ\muSR [44] can be solely attributed to H diffusion, because the pseudo-Na atoms can accompany nearby H*’s due to local electronic excitations which are much stronger than that in positive muon implantation [45].

Acknowledgement

We acknowledge helpful discussions with J. Sugiyama, I. Umegaki, and H. Kageyama. The μ\muSR experiments were conducted under the Inter-University Research Program (Proposal No. 2019MS02) supported by the Institute of Materials Structure Science, High Energy Accelerator Research Organization (KEK), Japan. This work was supported by the MEXT Elements Strategy Initiative to Form Core Research Center for Electron Materials (Grant No. JPMXP0112101001), JSPS KAKENHI (Grant Nos. 19K15033, 17H06153, 20K12484, 21H05102), Core-to-Core Program (JPJSCCA20180006), and JST MIRAI Program (JPMJMI21E9).

Data Availability: The data that supports the findings of this study are available within the article.

Details of μ\muSR data analysis

The spin relaxation of the diamagnetic Mu is governed by a random local fields at the Mu site HnH_n from the nuclear magnetic moments, and the magnitude of the relaxation rate is determined by the second moment of HnH_n,

Δ2=γμ2⟨∣Hn∣2⟩=γμ2∑nfn∑i∑α,β[γn(A^dni)αβIni]2(6)\Delta^2 = \gamma_\mu^2 \langle|H_n|^2 \rangle= \gamma_\mu^2 \sum_n f_n \sum_i \sum_{\alpha,\beta} [\gamma_n (\hat{A}_d^{ni})^{\alpha\beta} I_{ni}]^2 \tag*{(6)}

where γμ=2π×135.53\gamma_\mu= 2\pi\times135.53 MHz/T is the gyromagnetic ratio of Mu spin, IniI_{ni} is the nnth kind of nuclear spin at distance rnir_{ni} (n=1,2n = 1, 2 for 1^1H, 25^{25}Mg) on the iith lattice point (with γnIni\gamma_n I_{ni} being the effective magnetic moment considering the electric quadrupole interaction for Ini≥1I_{ni} \ge1), γn\gamma_n and fnf_n are the gyromagnetic ratio and natural abundance (or occupation) of the nnth nuclear spin, A^dni\hat{A}_d^{ni} is the magnetic dipole tensor

(A^dni)αβ=1rni3(3αniβnirni2−δαβ)(α,β=x,y,z),(7)(\hat{A}_d^{ni})^{\alpha\beta} = \frac{1}{r_{ni}^3}\left(\frac{3\alpha_{ni}\beta_{ni}}{r_{ni}^2} - \delta_{\alpha\beta}\right) \quad(\alpha,\beta= x,y,z), \tag*{(7)}

representing the hyperfine interaction between Mu and nuclear magnetic moments at rni=(xni,yni,zni)r_{ni} = (x_{ni},y_{ni},z_{ni}) being the position vector of the nucleus seen from Mu. The sum in equation (A1) takes all x,y,zx,y,z for β\beta, and x,yx,y for the α\alpha components that are effective for longitudinal relaxation when z^\hat{z} is the LF direction; the zz component does not contribute to the relaxation because it gives a magnetic field parallel to the Mu spin.

When the coordination of the nuclear magnetic moment viewed from Mu is isotropic and the number of coordination NN is sufficiently large (N≥4N \ge4), the time-dependent spin relaxation under zero external field is described by the Gaussian Kubo-Toyabe (GKT) function

GzKT(t;Δ)=13+23(1−Δ2t2)e−12Δ2t2.(8)G_z^{\mathrm{KT}}(t;\Delta) = \frac{1}{3} + \frac{2}{3}(1-\Delta^2t^2)e^{-\frac{1}{2}\Delta^2t^2}. \tag*{(8)}

In the case of fluctuating Δ\Delta over time (e.g., due to the self-diffusion of Mu), GzKT(t;Δ)G_z^{\mathrm{KT}}(t;\Delta) is subject to the modulation and adiabatically approaches exponential decay with increasing fluctuation rate ν\nu, where the detailed lineshape of GzKT(t;B0,Δ,ν)G_z^{\mathrm{KT}}(t;B_0,\Delta,\nu) as a function of ν\nu and LF (=B0= B_0) are found elsewhere [23]. For a small number of nuclei, the time evolution of the Mu spin polarization exhibits considerable deviation form the GKT function. The exact time dependence can be derived from the density matrix of the Mu-nucleus spin system for the N=1N = 1 and 22 cases [46, 47, 48] and the latter is introduced to describe H-Mu-H hydrogen bonding state [42, 24]. Assuming a static collinear geometry with μ+\mu^+ at the center of the line joining two other nuclear spins (I=1/2I = 1/2), the time evolution of muon polarization as a cubic average is calculated by solving a simple three-spin model to yield [46]

Gz3S(t)=16{3+cos⁡(3ω3St)+α+cos⁡(β+ω3St)+α−cos⁡(β−ω3St)}e−λ3St(9)G_z^{3S}(t) = \frac{1}{6}\{3+\cos(\sqrt{3}\omega_{3S}t)+\alpha_+\cos(\beta_+\omega_{3S}t)+\alpha_-\cos(\beta_-\omega_{3S}t)\}e^{-\lambda_{3S}t} \tag*{(9)}

where α±=1±1/3\alpha_\pm= 1 \pm1/\sqrt{3}, β±=(3±3)/2\beta_\pm= (3 \pm\sqrt{3})/2, ω3S\omega_{3S} is the dipolar interaction frequency

ω3S=γμγ1rt3,(10)\omega_{3S} = \frac{\gamma_\mu\gamma_1}{r_t^3}, \tag*{(10)}

with rtr_t being the distance between μ+\mu^+ and the proton nucleus, γ1/2π=42.58\gamma_1/2\pi= 42.58 MHz/T for 1^1H, and λ3S\lambda_{3S} is the relaxation rate describing the influence of local fields from outer-shell nuclear magnetic moments [48] and spin/charge exchange interaction.

In the case of fast fluctuation (ν>Δ\nu> \Delta), we have an approximated form of the GKT function

GzKT(t;B0,Δ,ν)≃exp⁡(−λt),(11)G_z^{\mathrm{KT}}(t;B_0,\Delta,\nu) \simeq\exp(-\lambda t), \tag*{(11)}

where

λ≃2Δ2νω2+ν2,(12)\lambda\simeq\frac{2\Delta^2\nu}{\omega^2+\nu^2}, \tag*{(12)}

and ω=γμB0\omega= \gamma_\mu B_0. Note that when the fluctuation rate satisfies the condition ν≫ω\nu\gg\omega, equation (A7) is least dependent on B0B_0.

The magnitude of Δ\Delta is sensitive to the size of the nearest-neighbor nuclear magnetic moment γnIni\gamma_n I_{ni} and the distance ∣rni∣|r_{ni}| from Mu, and the position occupied by Mu as pseudo-H can be estimated by comparing the experimentally obtained Δ\Delta with the calculated value at the candidate sites. We used the DipElec code [49] to calculate Δ\Delta for MgH2_2.

The μ\muSR time spectrum shown by the paramagnetic Mu is complicated by the hyperfine interaction between μ+\mu^+ and the bound electron. In addition to the limited time resolution of pulsed beam experiments, it is difficult to directly observe the Mu spin precession motion associated with transitions between hyperfine levels due to the dominance of fast spin/charge exchange reactions in MgH2_2. Even in such a case, important information can be extracted by examining the response of the time spectrum Gz(t)G_z(t) to the LF in detail.

First, consider Mu0^0 under a magnetic field (B0B_0) applied parallel the initial Mu polarization (∥z\parallel z) without spin fluctuations (static). In this case, we have

Gz(t)=12(1+x2)[(1+2x2)+cos⁡(ωc1+x2t)],(13)G_z(t) = \frac{1}{2(1+x^2)}\left[(1+2x^2)+\cos(\omega_c\sqrt{1+x^2}t)\right], \tag*{(13)}

where x=B0/Bcx = B_0/B_c with Bc=ℏωc/(γμ−γe)B_c = \hbar\omega_c/(\gamma_\mu-\gamma_e) being the effective local field exerted on μ+\mu^+, ωc\omega_c is the hyperfine parameter (angular frequency for the isotropic Fermi contact term), and γe\gamma_e is the electron gyromagnetic ratio (=2π×28024.2= 2\pi\times28024.2 MHz/T) [18]. For the zero external field (x=0x = 0),

Gz(t)=12(1+cos⁡ωct).(14)G_z(t) = \frac{1}{2}(1+\cos\omega_ct). \tag*{(14)}

The implication is that a half of the ground state is not an eigenstate of the hyperfine interaction, so the corresponding component exhibits oscillation between the spin-singlet and triplet states with ωc\omega_c. In a practical material, ωc\omega_c is often smaller than that in a vacuum (ωvac=2π×4463.3\omega_{\mathrm{vac}} = 2\pi\times4463.3 MHz) due to the effect of dielectric constant, etc., but it is often not visible in ordinary time-resolution measurements (i.e., the second term is zero when time-averaged). Thus, half of the implanted muons effectively lose their polarization upon Mu0^{0} formation (also called the missing fraction), and only the triplet state [the first term of equation (A8)] becomes observable. The situation is similar for B0>0B_{0} > 0, where the time-averaged polarization at t=0t = 0 is

GZ(t)≃G‾Z(0)=1+2x22(1+x2)≡gZ(x).(15)G_{Z}(t) \simeq\overline{G}_{Z}(0) = \frac{1 + 2x^{2}}{2(1 + x^{2})} \equiv g_{Z}(x). \tag*{(15)}

As xx is normalized by ωc\omega_{\mathrm{c}}, the field dependence of G‾Z(0)\overline{G}_{Z}(0) varies with ωc\omega_{\mathrm{c}}. Moreover, Mu0^{0} in MgH2_{2} is subjected to the NHF interaction between the bound electron and surrounding H atoms which have proton nuclear spins [18]. This further reduces G‾Z(0)\overline{G}_{Z}(0) to 1/2×1/3=1/61/2 \times1/3 = 1/6, reflecting the random orientation of the nuclear spins, and leads to a two-step recovery of G‾Z(0)\overline{G}_{Z}(0) with respect to xx [50]. In any case, the magnitude of ωc\omega_{\mathrm{c}} can be determined by comparing the magnetic field dependence of experimentally obtained G‾Z(0)\overline{G}_{Z}(0) with equation (A10).

The effect of spin fluctuations on Mu0^{0} under LF can be derived by approximating the spin/charge exchange reaction with excited carriers by a strong collision model. In particular, when the reaction rate ν\nu is lower than ωc\omega_{\mathrm{c}}, the time-dependent polarization is given by the following equations [28].

GZ(t)≃gZ(x)exp⁡(−λt),(16)G_{Z}(t) \simeq g_{Z}(x)\exp(-\lambda t), \tag*{(16)}
λ≃ν2(1+x2).(17)\lambda\simeq\frac{\nu}{2(1+x^{2})}. \tag*{(17)}

As mentioned in the main text, we attempted to derive the hyperfine parameter (ωp\omega_{\mathrm{p}}) of a paramagnetic state (Mup_{\mathrm{p}}) and other kinetics parameters describing its dynamical properties by using equation (3) [whose magnetic field dependence originates from equations (A10)–(A12)] by a global curve fit that simultaneously analyzes the spectra of different magnetic fields. As a result, ωp\omega_{\mathrm{p}} increases significantly from around 20 K to 150 K, and shows a sharp decrease at the high temperature side above 150 K [Figure A1(a)]. Moreover, the latter is strongly correlated with the increase of the spin/charge fluctuation rate νp\nu_{\mathrm{p}}, leaving it hardly determined above ∼150\sim150 K [Figure A1(b)]. Therefore, we adopted the hypothesis that the original ωp\omega_{\mathrm{p}} should be approximately constant, and derived the temperature dependence of the other parameters with ωp\omega_{\mathrm{p}} fixed to some appropriate value. The temperature dependence of ωp\omega_{\mathrm{p}} (ωp2\omega_{\mathrm{p2}}) and its relationship to νp\nu_{\mathrm{p}} (νp2\nu_{\mathrm{p2}}) are discussed in the main text.

Muon irradiation effect

In general, the energy imparted in a solid by the irradiation of charged particles consists of two types of energy: the kinetic energy of the atoms that make up the solid and the excitation energy of the electron system. The former is due to elastic collisions between incident particles and atoms, and the latter is due to inelastic collisions. Irradiation damage (atomic displacement), usually seen in metals and semiconductors, occurs when atoms gain energy above the knock-on threshold (Ed≃15E_{\mathrm{d}} \simeq15–30 eV) and are ejected from a lattice point [14]. Provided that the mass of the incident particle is mm, the energy is EE, and the mass of the target atom is MM, ejection occurs when the energy ΔE\Delta E imparted to the atom by the collision exceeds EdE_{\mathrm{d}}, i.e.,

ΔE=4mME(m+M)2>Ed.(18)\Delta E = \frac{4mME}{(m+M)^{2}} > E_{\mathrm{d}}. \tag*{(18)}

When the incident particle is a muon (m=mμ≪Mm = m_{\mu} \ll M), the minimum kinetic energy E0E_{0} required to eject the target atom is given by

E0=(m+M)24mMEd≃M4mμEd.(19)E_{0} = \frac{(m+M)^{2}}{4mM}E_{\mathrm{d}} \simeq\frac{M}{4m_{\mu}}E_{\mathrm{d}}. \tag*{(19)}

Therefore, it is inferred that in the region E>E0E > E_{0}, muon kinetic energy is consumed mainly by the atomic displacement process.

On the other hand, in the region of E≤E0E \leq E_{0} (i.e., ΔE≤Ed\Delta E \leq E_{\mathrm{d}}), the energy loss due to excitation of the electronic system becomes dominant. Since the energy required for the formation of electron-hole pairs is known to be approximately ε≃2.8Eg\varepsilon\simeq2.8E_{\mathrm{g}} with the band gap as EgE_{\mathrm{g}} [15], the number of electron-hole pairs produced is roughly estimated as

neh≃E0ε=E02.8Eg.(20)n_{\mathrm{eh}} \simeq\frac{E_{0}}{\varepsilon} = \frac{E_{0}}{2.8E_{\mathrm{g}}}. \tag*{(20)}

Assuming Ed=30E_{\mathrm{d}} = 30 eV and Eg=5E_{\mathrm{g}} = 5 eV, the values of E0E_0 and nehn_{\mathrm{eh}} estimated for the constituent atoms of MgH2_2 are summarized in Table B1. From the weighted average of these values, it is estimated that about 10210^2 electron-hole pairs per muon are formed in MgH2_2. Since such electronic excitations are dominant in the final stage of energy loss of the incident particles, electron-hole pairs are also expected to be distributed near the end of the radiation track.

AtomE0E_0(eV)nehn_{\mathrm{eh}}
H674.8
Mg1619116

Table B1. The minimum kinetic energy E0E_0 of the incident muon required for each target atom to undergo displacement in MgH2_2, and the number of electron-hole pairs nehn_{\mathrm{eh}} produced by electronic excitation below E0E_0, where Ed=30E_{\mathrm{d}} = 30 eV and Eg=5E_{\mathrm{g}} = 5 eV.

From the above discussion, H is special in that muons with relatively low kinetic energy are inferred to displace H atoms in solids. Considering that the formation energy of H vacancies in MgH2_2 is predicted to be comparable with that for the interstitial H (Hi_{\mathrm{i}}) [12], it is possible that the ejected H exists as Hi_{\mathrm{i}} in the vicinity of the muon stopping position.

References

  1. [1]Dresselhaus M S and Thomas I L 2001 Nature 414 332–337
  2. [2]Schlapbach L and Züttel A 2001 Nature 414 353–358
  3. [3]Sakintuna B, Lamari-Darkrim F and Hirscher M 2007 Int. J. Hydrogen Energy 32 1121–1140
  4. [4]Felderhoff M and Bogdanović B 2009 Int. J. Mol. Sci. 10 325–344
  5. [5]Huot J, Liang G, Boily S, Van Neste A and Schulz R 1999 J. Alloys Compd. 293–295 495–500
  6. [6]Oelerich W, Klassen T and Bormann R 2001 Adv. Eng. Mater. 3 487–490
  7. [7]Fernández J and Sánchez C 2002 J. Alloys Compd. 340 189–198
  8. [8]Liang G 2004 J. Alloys Compd. 370 123–128
  9. [9]Conradi M S, Mendenhall M P, Ivanic T M, Carl E A, Browning C D, Notten P H L, Kalisvaart W P, Magusin P C M M, Bowman R C, Hwang S J and Adolph N L 2007 J. Alloys Compd. 446–447 499–503
  10. [10]Du A J, Smith S C, Yao X D, Sun C H, Li L and Lu G Q 2008 Appl. Phys. Lett. 92 163106
  11. [11]Evard E, Gabis I and Yartys V 2010 Int. J. Hydrogen Energy 35 9060–9069
  12. [12]Park M S, Janotti A and Van de Walle C G 2009 Phys. Rev. B 80(6) 064102
  13. [13]Roy A, Janotti A and Van de Walle C G 2013 Appl. Phys. Lett. 102 033902
  14. [14]Thompson M W 1974 Defects and Radiation Damage in Metals Cambridge Monographs on Physics (Cambridge University Press, Cambridge)
  15. [15]Aligr R C and Bloom S 1975 Phys. Rev. Lett. 35(22) 1522–1525
  16. [16]Itoh N 1997 Nucl. Instr. Meth. Phys. Res. B 122 405–409
  17. [17]Hiraishi M, Okabe H, Koda A, Kadono R and Hosono H 2022 J. Appl. Phys. 132 105701
  18. [18]Patterson B D 1988 Rev. Mod. Phys. 60(1) 69–159
  19. [19]Lichti R L, Chow K H and Cox S F J 2008 Phys. Rev. Lett. 101(13) 136403
  20. [20]Van de Walle C G and Neugebauer J 2004 J. Appl. Phys. 95 3851–3879
  21. [21]Giannozzi P, Baroni S, Bonini N, Calandra M, Car R, Cavazzoni C, Ceresoli D, Chiarotti G L, Cococcioni M, Dabo I, Corso A D, de Gironcoli S, Fabris S, Fratesi G, Gebauer R, Gerstmann U, Gougoussis C, Kokalj A, Lazzeri M, Martin-Samos L, Marzari N, Mauri F, Mazzarello R, Paolini S, Pasquarello A, Pautal l o T, Sbraccia C, Scandolo S, Scuseria G, Seitsonen A P, Smogunov A, Umari P and Wentzcovitch R M 2009 J. Phys.: Condens. Matter 21 395502
  22. [22]Bortz M, Bertheville B, Böttger G and Yvon K 1999 J. Alloys Compd. 287 L4–L6
  23. [23]Hayano R S, Uemura Y J, Imazato J, Nishida N, Yamazaki T and Kubo R 1979 Phys. Rev. B 20(3) 850–859
  24. [24]Umegaki I, Nozaki H, Harada M, Higuchi Y, Noritake T, Matsumoto M, Towata S, Ansaldo E J, Brewer J H, Koda A, Miyake Y and Sugiyama J 2014 J. Phys.: Conf. Series 551 012036
  25. [25]Walker D C 1983 Muon and Muonium Chemistry (Cambridge University Press, Cambridge)
  26. [26]Percival P W, Adamson-Sharpe K M, Brodovitch J C, Leung S K and Newman K E 1985 Chemical Physics 95 321–330
  27. [27]Storchak V, Brewer J H, Morris G D, Arseneau D J and Senba M 1999 Phys. Rev. B 59(16) 10559–10572
  28. [28]Kadono R, Macrae R M and Nagamine K 2003 Phys. Rev. B 68(24) 245204
  29. [29]Nosov N and Yakovleva I 1965 Nuclear Physics 68 609–631
  30. [30]Chow K H, Kiefl R F, Hitti B, Estle T L and Lichti R L 2000 Phys. Rev. Lett. 84(10) 2251–2254
  31. [31]Sugiyama J, Umegaki I, Matsumoto M, Miwa K, Nozaki H, Higuchi Y, Noritake T, Forslund O K, Månsson M, Cottrell S P, Koda A, Ansaldo E J and Brewer J H 2019 Sustainable Energy Fuels 3(4) 956–964
  32. [32]Anderson P W 1975 Phys. Rev. Lett. 34(15) 953–955
  33. [33]Ito T U, Higemoto W, Koda A and Shimomura K 2019 Appl. Phys. Lett. 115 192103
  34. [34]Kiefl R F, Kadono R, Brewer J H, Luke G M, Yen H K, Celio M and Ansaldo E J 1989 Phys. Rev. Lett. 62(7) 792–795
  35. [35]Kadono R, Kiefl R F, Ansaldo E J, Brewer J H, Celio M, Kreitzman S R and Luke G M 1990 Phys. Rev. Lett. 64(6) 665–668
  36. [36]Kadono R, Kiefl R F, Brewer J H, Luke G M, Pfi z T, Riseman T M and Sternlieb B J 1991 Hyperfine Interact. 64 635–640
  37. [37]Kadono R, Matsushita A, Nagamine K, Nishiyama K, Chow K H, Kiefl R F, MacFarlane A, Schumann D, Fujii S and Tanigawa S 1994 Phys. Rev. B 50(3) 1999–2002
  38. [38]Liang G, Huot J, Boily S, Van Neste A and Schulz R 1999 J. Alloys Compd. 292 247–252
  39. [39]Varin R A, Czujko T, Wasmund E B and Wronski Z S 2007 J. Alloys Compd. 432 217–231
  40. [40]Amama P B, Grant J T, Spowart J E, Shamberger P J, Voevodin A A and Fisher T S 2011 J. Mater. Res. 26 2725–2734
  41. [41]Hanada N, Ichikawa T and Fujii H 2007 J. Alloys Compd. 446–447 67–71
  42. [42]Kadono R, Shimomura K, Satoh K H, Takeshita S, Koda A, Nishiyama K, Akiba E, Ayabe R M, Kuba M and Jensen C M 2008 Phys. Rev. Lett. 100(2) 026401
  43. [43]Hiraishi M, Okabe H, Koda A, Kadono R and Hosono H arXiv:2110.09024
  44. [44]Sugiyama J, Umegaki I, Nozaki H, Higemoto W, Hamada K, Takeshita S, Koda A, Shimomura K, Ninomiya K and Kubo M K 2018 Phys. Rev. Lett. 121(8) 087202
  45. [45]Okumura T, Azuma T, Bennett D A, Caradonna P, Chiu I, Doriese W B, Durkin M S, Fowler J W, Gard J D, Hashimoto T, Hayakawa R, Hilton G C, Ichihome Y, Indelicato P, Isobe T, Kanda S, Kato D, Katsuragawa M, Kawamura N, Kino Y, Kubo M K, Mine K, Miyake Y, Morgan K M, Ninomiya K, Noda H, O’Neil G C, Okada S, Okutsu K, Osawa T, Paul N, Reintsema C D, Schmidt D R, Shimomura K, Strasser P, Suda H, Swetz D S, Takahashi T, Takeda S, Takeshita S, Tampo M, Tatsuno H, Tong X M, Ueno Y, Ullom J N, Watanabe S and Yamada S 2021 Phys. Rev. Lett. 127(5) 053001
  46. [46]Brewer J H, Kreitzman S R, Noakes D R, Ansaldo E J, Harshman D R and Keitel R 1986 Phys. Rev. B 33(11) 7813–7816
  47. [47]Nishiyama K, Nishiyama S W and Higemoto W 2003 Physica B: Condens. Matter 326 41–45
  48. [48]Wilkinson J M and Blundell S J 2020 Phys. Rev. Lett. 125(8) 087201
  49. [49]Kojima K M, Yamanobe J, Eisaki H, Uchida S, Fudamoto Y, Gat I M, Larkin M I, Savici A, Uemura Y J, Kyriakou P P, Rovers M T and Luke G M 2004 Phys. Rev. B 70(9) 094402
  50. [50]Beck R, Meier P F and Schenck A 1975 Z. Physik B 22 109–115

Paper details

vlnc:W_fbmk89e2
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents