Abstract

The integration of two-dimensional Ti3C2Tx MXenes into Halide Perovskite (HaP) optoelectronics has shown immense potential for enhancing device performance, yet the fundamental chemical interactions within the precursor ink (a critical stage determining the final material state) remain largely unexplored. This study presents a comprehensive investigation into the chemical stability and surface evolution of Ti3C2Tx MXenes when exposed to the individual and combined components of a model methylammonium lead iodide (MAPbI3) solution. By combining detailed X-ray Photoelectron Spectroscopy (XPS) analysis with Density Functional Theory (DFT) calculations, we decouple the complex interactions between MXenes and the ink constituents. We demonstrate that elemental iodine (I2) and polyiodides (In-) act as aggressive oxidizers, triggering rapid degradation and dissolution of the MXene flakes. Conversely, lead iodide (PbI2) induces a slower oxidation process driven by the strong adsorption of Pb2+ ions onto oxygen terminated sites. In stark contrast, methylammonium iodide (MAI) exhibits a stabilizing effect: it adsorbs onto the MXene surface via hydrogen bonding, effectively passivating the flakes and retarding degradation. In addition, our results reveal that the sequence of precursor addition governs the MXene surface state, requiring extra caution, but also enabling further tunability. These findings provide a critical view on how MXene integration with materials, in general, and HaP in particular, should be perceived, providing a fundamental for their rational engineering.

Introduction

MXenes are a family of two-dimensional (2D) materials sharing the common formula Mn+1XnTxM_{n+1}X_nT_x, where M stands for a transition metal (Ti, V, Nb, Mo, etc.), X – for C or/and N, and TxT_x is a surface termination group, with –F, =O and –OH being the most common ones[1, 2]. After their introduction in 2011 by Gogotsi, Naguib et al.[3], MXenes attracted vast attention from a very broad scientific community. For example, they showed significant improvements in electrochemical cells for energy storage[4, 5, 6], demonstrated environmental remediation[7, 8], and the ability to be integrated into flexible and printable electronics[9, 10], sensors[11, 12], biomedicine[13, 14], and more.

The origin behind what renders MXenes with such wide applicability is, at their core, their chemical versatility – particularly the M metal and the chemically-active and dynamically-changing surface chemistry of the TxT_x group[1, 2]. Even without changing the M metal backbone, changes in the TxT_x group show, for example, the ability to change MXene’s electrical conductivity or chemical potential[15], stabilize colloidal solutions via surface modification[16], or make them hydrophilic or hydrophobic on demand[17]. All of these lead to a pronounced integrability of MXenes with different classes of materials, including polymers, nanomaterials, organic molecules[18, 19, 20, 21, 22, 23, 24], and so on.

A more recent rising interest within the scientific and technological communities, which will form the focus of this work, is the fusion between MXenes and Halide Perovskite (HaP) systems[25]. HaPs are mostly famous due to their outstanding photovoltaic performance as light-harvesting materials, demonstrating results that show a potential alternative or an enhancement to Si-based solar cells[26, 27], with a light-to-electron conversion efficiency of over 26% alone or 30% in tandem with Si[28, 29]. Besides photovoltaics, HaPs show success in other technological fields, such as photo-sensors, hard-radiation detectors, light-emitting diodes, and more[30].

HaPs are ABX3ABX_3 structures, where A is a monovalent organic or inorganic cation like methylammonium (MA+\mathrm{MA}^{+}), formamidinium (FA+\mathrm{FA}^{+}) or Cs+\mathrm{Cs}^{+}, B is a divalent cation such as Pb2+\mathrm{Pb}^{2+} or Sn2+\mathrm{Sn}^{2+}, and X is a monovalent anion, such as I−\mathrm{I}^{-} or Br−\mathrm{Br}^{-}[31]. Their technological superiority is attributed to a number of coexisting properties, such as long exciton recombination lifetime[32, 33], formation of electronically non-active defects (“defect-tolerance”)[34], and/or the capability for spontaneous self-healing[35, 36]. These features are, to the great extent, attributed to high structural and ionic dynamics[37], or to bulk point defects that are rather benign (in contrast to classical semiconductors, such as Si, GaAs)[34]. Unlike bulk defects, surface defects do play a major role and are used in tuning HaPs’ properties[38]. Therefore, two-dimensional defects, especially those with chemical versatility, such as MXenes, can play a crucial role in actively controlling the functional properties of HaP-based systems.

Both MXenes and HaPs are prone to changes in response to variations in their chemical environment. HaPs require only solution chemistry to form high-quality films[39, 40], such as spin coating of an ink-like solution, which offers an advantage in simplicity and fabrication costs. Low temperature rapid structural arrangement, however, also presents several drawbacks associated with the high chemical sensitivity of the materials during both fabrication and operation[41, 42]. Unencapsulated devices tend to rapidly degrade due to ambient oxygen and humidity[43], and when encapsulated, hysteresis indicates severe ion migration and internal chemical dissociation, which may lead to contact degradation as a result of interaction with chemically active species, such as polyhalides[44]. The ability to manipulate HaPs’ chemical environment, especially surface/interface, will make HaPs more versatile and chemically robust.

This is exactly the motivation that ignited the fusion between HaPs and MXenes. Since the pioneering work by Guo Z. et al.[45], increasing number of studies have explored the integration of MXenes into HaP-based solar-cell architectures, demonstrating improvements in the overall device performance. MXenes were integrated as either passivation layers, when the flakes are located at the interface between the HaP and charge transport layers (CTLs), or reinforcements, when MXenes are directly mixed with HaP, CTLs, or both[46, 47, 48, 49, 50, 51, 52]. Since MXenes have highly tunable surface chemistry[53, 54], while the surface chemistry of HaPs is known to strongly affect their work function[38], their integration allows tuning the band alignment with the CTLs, thus directly impacting the power conversion efficiency of the respective devices[55, 56, 57, 58]. Other reports claim that MXenes help reduce trap state densities, improve charge carrier mobilities, or improve morphological features in the HaP layers[59, 60]. For example, MXenes were found to interact with undercoordinated Pb2+\mathrm{Pb}^{2+} ions in Pb-based HaPs[61, 62] and, supposedly, act as defect-passivation agents. MXenes were shown to impact the morphology of the HaP films via promoting nucleation, leading to films with larger grains[63, 64, 65]. Since surfaces are the source of functionally-meaningful defects[38], larger grains will directly reduce the density of such defects. Overall, MXenes act as promising additives for enhancing the efficiency and shelf life of HaP-based devices[66, 67].

However, unlike the functional aspects of the MXene–HaP integration, the chemical aspects arising from their interaction have received very little attention. Given that both HaPs and MXenes are strongly influenced by their chemical environment, a fundamental understanding of the MXene-HaP interaction mechanisms and binding chemistry is necessary, and will likely explain the observed, yet poorly-understood, functionality changes. HaPs’ formation, degradation, and self-healing are closely related to their subtle chemical nature[41], so it is likely to assume there will be an active interplay between MXenes and HaPs. The chemistry occurring between MXenes and HaPs may impose positively or negatively on the perovskite system, more specifically, impact on ion-migration related hysteresis, degradation of contacts[44], impose electronically-active (surface) defects[38], and/or form intermediate structural states that promote nucleation during film formation.

While there are assumptions on why MXenes may affect HaPs, until now, there is actually no knowledge about the state in which MXenes are integrated with HaPs, in particular, their termination composition and oxidation state of the M metal. The latter is a critical measure for degradation and loss of structural integrity of MXene flakes, which typically occurs through increasing the oxidation state of the M metal[68]. It is well-known that the MXenes’ termination groups, TxT_x, can be exchanged or modified when exposed to different chemical environments[69, 70]. Therefore, it is reasonable to assume that when MXenes are exposed to a HaP-precursor solution, it will alter the MXenes from their initial as-cast form. With the chemical changes of the MXenes, the MXene-HaP system’s behavior must, consequently, also change. At these interphases, local changes in the chemical potential may lead to doping and/or trapping defect states, trap impurities such as oxygen, or limit ion migration. Therefore, understanding the state of MXenes after their exposure to HaP-related precursors is among the first things we must ask ourselves to establish a predictive understanding of how MXene integration influences the properties and performance of HaP-MXene systems.

HaP-precursor solution (or as will be denoted later - a “HaP-ink”) is where the interaction with MXenes is most likely to be immediately important. HaP film preparation techniques[71, 72] include a broad set of precursors[31] and solvents[73, 74, 75], which create a variety of different potential chemical environments for MXenes before an actual crystallization of the HaP in a film. Solvated HaP components may contain corrosive and aggressive species, especially halides and polyhalides, like In−I_n^-[76, 77]. While MXenes are highly active and rather prone to oxidation and other chemical reactions[68, 78, 79], the impact of these surrounding chemical species on them is unknown and must be carefully investigated. Thus, one may expect a large scope of possible processes to happen to MXenes in a HaP-ink: from standard oxidation and decomposition to functional group exchange or complex electrostatic and chemical adsorption. Similar processes have already been observed when MXenes were exposed to different aqueous and organic solutions[68, 78, 79, 80].

This paper focuses on providing a clear picture of the chemistry and composition of MXenes just before they are integrated into a HaP solid matrix, meaning within the precursor solution. We explicitly focus on understanding the chemistry of MXenes in HaP-inks, which we believe to be a critical gap that hinders further development of MXene-HaP integration technology. In particular, this study will cover the most abundantly studied Ti3C2Tx\mathrm{Ti_3C_2T_x} MXene and a MAPbI3\mathrm{MAPbI_3}[81] HaP-ink as a model system. While this study does not cover all the possible chemical specificities of different HaP-MXene systems, it provides a pioneering and essential step towards a more complete understanding of MXene-HaP composite films.

In particular, well-characterized Ti3C2Tx\mathrm{Ti_3C_2T_x} MXene flakes were exposed to complete or partial MAPbI3\mathrm{MAPbI_3}-inks solutions, where a combinatorial set of MAI, PbI2\mathrm{PbI_2}, and I2\mathrm{I_2} precursors was dissolved in DMSO. Supported by various probing methods, we use X-ray Photoelectron Spectroscopy (XPS) as the main tool to examine what happens to the state of MXenes as they are extracted from the HaP-inks. Together with a detailed experimental investigation, we include a critical first-principles Density Functional Theory (DFT) study to support and explain our experimental findings. Our results show that the chemical nature of the termination groups and MXenes’ stability are time-dependent in some solutions, while more stable in others. We show that different species composing the HaP-precursor solution, in particular MAI, PbI2\mathrm{PbI_2} and In−\mathrm{I_n^-}, have each a unique role in the overall stability of MXenes in the MXene-HaP suspension. Using the data gathered from the combinatorial set of precursors, we will demonstrate experimentally, and support theoretically: the possitive protective effect of MAI; the mild but significant degrative effect of PbI2\mathrm{PbI_2}, showing Pb cations adsorption alongside slow degradation of the MXenes; the fast and detrimental effect of I2\mathrm{I_2}, or polyiodides, on on the stability of MXenes. We note that while MAI and PbI2\mathrm{PbI_2} are abundantly present in MAPbI3\mathrm{MAPbI_3} as its binaries, I2\mathrm{I_2} is typically not added to HaP-inks intentionally, but it is known as a product that may spontaneously form inside halide solutions[76, 77] or films[82, 83, 84], thus understanding its role around MXenes is of non-negligible importance.

We note that the current study focuses solely on the MXene side, which was previously neglected, and aims to provide a fundamental understanding for explaining and engineering functional behavior in working HaP–MXene–based devices. Our deduced fundamental insights broaden the core understanding of MXene chemistry in a hybrid organic-inorganic environment. While not directly targeting the incorporation of MXenes with HaPs for improving them on a device level, this study poses a critical milestone for a greater, more general understanding of MXenes and optoelectronic composites made with them.

Materials and Methods

Given our use case-study focuses on Ti3C2Tx\mathrm{Ti_3C_2T_x} MXenes and MAPbI3\mathrm{MAPbI_3} HaP, we started with a careful in-house preparation of Ti3C2Tx\mathrm{Ti_3C_2T_x} MXenes using well-known practices[85, 86], followed by their detailed characterization. Next, we integrated the freshly prepared MXenes with a combinatorial set of MAPbI3\mathrm{MAPbI_3}-related precursors, dissolved in DMSO. We note that we majorly focused on DMSO in our use-case, but we later demonstrated the use of other solvents, such as DMF. To track the state of the immersed MXenes, we then analyzed them after one hour and one week of immersion. We were focusing on the changes in MXenes’ chemistry after their exposure to the inks, and targeted the factors that led to these changes. While the major part of this work focused on suspended MXenes that were extracted via filtering, in some cases, where we found it necessary, we also characterized precipitants that were observed at the bottom of the mixed inks, and the inks themselves. In this paper we frequently use the term “ink” to label HaP-precursor solutions with or without MXenes, although we would like to underscore that we do not target ink formulation for industrial purposes, although it may be used for that regardless. A ‘block-scheme’, summarizing the conducted research, is given in Figure 1Figure 1; the following parts of the manuscript are organized in accordance with this skeleton.

Illustrative block-schema of the conducted study

Figure 1. Illustrative block-schema of the conducted study: HaP-ink and Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXene preparation, MXene+HaP ink formation, handling and characterization.

Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes synthesis

For the synthesis of high quality Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes we etched a Ti3AlC2\mathrm{Ti}_{3}\mathrm{AlC}_{2} MAX phase precursor with a mixture of HCl and HF acids, followed by delamination with LiF[85]. The supporting batch of Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes was synthesized using common HF-based etching protocol[86].

The precursor Ti3AlC2\mathrm{Ti}_{3}\mathrm{AlC}_{2} MAX phase was prepared through a high temperature synthesis method, according to ref. [87]. The MAX phase was ground and passed through a sieving mesh of 45 μ\mum. DDW, HCl and HF were intermixed in a volume ratio of 3 : 6 : 1, reaching the final volume of 20 mL. 1 g of the meshed Ti3AlC2\mathrm{Ti}_{3}\mathrm{AlC}_{2} MAX powder was slowly immersed into the acidic solution; the solution temperature was brought up to 35°C, and the etching reaction was sustained for 24 hours under permanent magnetic stirring at 550 rpm.

After the completion of the reaction, pH of the solution was neutralized (reaching pH > 5) to separate the stacked MXene sheets and to remove unreacted slurry using repeated centrifugation. After each centrifugation cycle, the clear supernatant was discarded into waste, and the black precipitate was dispersed in fresh DDW. In total, we performed 12 centrifugation cycles at 3500 rpm for 5 minutes each. After the final centrifugation step, the obtained product was again re-dispersed in 50 mL of fresh DDW, and then admixed with 1 g of LiF to delaminate MXene sheets. The solution was left to stir at 40°C for another 24 hours. One more centrifugation cycle at 5000 rpm for 5 minutes was performed to separate MXenes from LiF leftovers, after which the final centrifugation at 3500 rpm for 15 min segregated single-flake suspension from non-delaminated particles. After that, the black supernatant was frozen with the liquid nitrogen and freeze-dried (lyophilized) for 3 days to eliminate water and preserve re-dispersibility. The obtained spongy powder was stored in a vacuumized desiccator.

We investigated MXenes with two different combinations of initial functional groups (provided from two different synthesis routes) and followed their modification after being immersed into the HaP-inks. As a second synthesis route, we chose to use the classical HF etching reaction[86], which is described in more detail in Section SA in the SI. Overall, MXenes prepared using this method are denoted as HF-MXenes (or HF-Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_x), and used as a supplementary batch of material. The reason we consider two different MXene preparation methods is to at least slightly control the TxT_x termination group identity, where HCl+HF+LiF and HF etching methods are expected to result in a greater portion of either =O, or –F functional groups, respectively. We note that we know both approaches end up with a mixed =O, –F, and –OH termination, and what we attempted is to modify the ratio between these species. The quality of the prepared MXenes was validated prior to the following experiments (see Figure 2 in the Results section and Figure S1 in the SI). We note that HCl+HF+LiF-etched MXenes are found to be of higher quality, i.e., almost non-oxidized and naturally single-flake.

Characterization of the as-cast Ti3C2Tx MXenes

Figure 2. Characterization of the as-cast Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes. (a) XRD pattern of as-cast Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes and Ti3AlC2\mathrm{Ti}_{3}\mathrm{AlC}_{2} MAX phase; (b) Raman spectrum. (c) TEM image of single-layer Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} flakes with respective SAED pattern, and (d) - Ti2p, C1s, O1s, F1s XPS core spectra. The XPS peaks’ notation follows ref. [98].

XRD patterns, Raman spectra, and XPS core spectra of as-cast HF-$\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x}$ MXenes

Figure S1. (a) XRD patterns of as-cast HF-Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes and the respective Ti3AlC2\mathrm{Ti}_{3}\mathrm{AlC}_{2} MAX phase precursor; (b) Raman spectra, and (c) Ti2p\mathrm{Ti}_{2p}, C1s\mathrm{C}_{1s}, O1s\mathrm{O}_{1s}, F1s\mathrm{F}_{1s} XPS core spectra of as-cast HF-Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes.

MXene-based HaP-inks preparation

To study the interaction chemistry between Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_x MXenes and HaP precursor species, we prepared solutions with different precursor combinations of the widely used MAPbI3_3 perovskite[81], meaning MAI, PbI2_2 and I2_2. The overall description of the studied set of samples is given in Table 1, the block-scheme of their preparation is given in Figure 1. In more detail, following Table 1, the inks with different combinations of components were prepared by adding only a sub-set of MAPbI3_3 precursors into the solvent, followed by stirring and sonication until complete dissolution. Then, Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_x MXenes were added into the solutions, followed by a 30-minute sonication in an ice bath under argon bubbling to achieve homogeneous dispersions. The inks were stored in the sealed vials in a desiccator with a controlled-atmosphere (with desiccant and vacuumized).

LabelMAI [1.0 M]PbI2_2 [1.0 M]I2_2 [1.0 M]
1-sol---
2-MX--
3-MPXX-
4-MPIXXX
5-I--X
6-PI-XX
7-P-X-
8-MIX-X

Table 1. Denotation and composition of Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXene-based HaP-ink samples used in this work. All noted additives are of 1 M (mol/L); MXene concentration was targeted to be 2.5⋅10−32.5 \cdot10^{-3} M (500 μ\mug mL−1^{-1}); the actual volume of each solvent (DMSO or DMF) was 2 mL.

To study the occurring chemistry, we analyzed the suspended MXenes in the solution, the separated dispersed MXenes, the residual solutions, and, in some cases, undesired precipitates. In order to test the chemistry across different timescales and track the evolution of the system, we examined the MXenes either after a short exposure (~1 hour) or a long (~1 week) storage. The 1-hour exposure is relevant to represent the use-case when MXenes are being dispersed in a freshly prepared HaP-ink, while 1 week scale is relevant to simulate the long-term storage conditions. For a solvent, we primarily used DMSO, but also had a comparison with DMF – both solvents are commonly employed in the HaP preparation processes separately or mixed[73, 74]. For simplification, when noting ‘solvent’, we refer to DMSO; when DMF is used we will explicitly mention so within the text.

To extract dispersed Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_x MXenes, we passed the content of the reaction vial through a 0.4 μ\mum pore-size PVDF filter membrane using vacuum-assisted filtration in a Buchner flask. When testing DMF as a solvent, we used a polyethylene filter instead (as DMF dissolves PVDF). The filtered solid was dried, and the residual solution of the ink was collected and analyzed separately. In cases when we observed precipitated solids forming in our reaction vials, they were collected and further analyzed. Any long-term storage was done in a vacuumized desiccator.

Characterization methods

To study the type of chemical bonds in as-cast Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_x MXenes and MXenes reacted with HaP-precursor solutions, we used XPS. We employed ESCALAB photoelectron / Auger electron spectroscope (Thermo Fisher Scientific, Massachusetts, USA) in the XPS mode, with Al Kα\alpha X-ray source and 500 μ\mum spot size. The analysis of the MXenes that were extracted from the precursor inks was performed directly on PVDF membranes, due to the limited amount of these materials. The substrate was not probed since the spot size was smaller than the MXenes-covered area. All the scans were obtained in a CAE analyzer mode with a pass energy of 20 eV and a step size of 0.1 eV. To gain a sufficient signal-to-noise ratio, the total number of scan repetitions was between 5 to 15, depending on the obtained intensity. For an extra set of experiments, we used the same facility in the UPS mode, with a HeII photon source, -5 V sample biasing, and 3 repetitive scans for each measurement.

To analyze the structural nature of as-cast MXenes, reaction products (filtered MXenes from HaP-inks) and precipitants, we used Panalytical Empyrean X-ray diffractometer (Malvern Panalytical, Malvern, UK) with Cu Kα\alpha radiation, operating at 45 V and 40 mA. All the scans were taken in a Bragg-Brentano mode with a 2θ\theta range of 3 − 70°, with a step size of 0.026°, and a counting time of 60 sec per step. The raw MXenes were measured as free powders on a zero-background substrate. The reacted MXenes were measured on a filtration membrane and background-corrected with a blank filter paper.

To analyze the chemical nature of dry MXenes (in a solid form on a glass substrate) and selected inks (in a liquid form inside a sealed quartz cuvette), we used Raman spectroscopy measurements. Spectra were collected with a confocal Horiba LabRam HR Evolution micro-Raman system equipped with a Syncerity Open Electrode CCD detector (deep-cooled to 60°C, 1024 ×\times 256 pixels) and Synapse FIVIS EM-CCD. The light source was a 532 nm laser at 0.36 and 1.15 mW for liquid and solid samples, respectively. The laser was focused onto the surface of the solid or liquid with a 50x LWD objective (Olympus LMPlanFL-N, NA = 0.5), the measurements were taken using a 600 grooves/mm grating, and 100-120 μ\mum confocal hole; exposure time varied between 0.5 - 60 seconds at the range of 56-3500 cm−1\mathrm{cm}^{-1}. Several spots on each sample were recorded for the sake of gaining reliable statistics. LabSpec software (version 6.5.2.11) was used to operate the equipment and process the data.

We employed Transmission Electron Microscopy (TEM), using FEI Tecnai T12 G2 TWIN (FEI Company, Oregon, USA) and JEOL JEM-2100F (Jeol Ltd., Tokyo, Japan) TEMs, operating at 120 kV and 200 kV accelerating voltages, respectively, to visualize the morphology of as-cast Ti3_3C2_2Tx_x MXenes, and MXenes reacted with selected HaP precursor inks, as well as of the precipitants from selected inks. We also performed SAED and EDS analysis of the respective products, using JEOL 50 mm2^2 Si(Li) EDS detector equipped on JEM-2100F TEM. For as-cast MXene material analysis, low-concentration MXene-DDW suspensions (diluted until a pronounced light-green color) were drop-cast onto lacey carbon TEM grids that were pre-cleaned using plasma.

We used Cary 5000 UV-Vis-NIR Spectrophotometer (Agilent Technologies, California, USA) to study optical transmission spectra of MXene-containing and reference inks, to track their evolution upon aging. All the UV-Vis scans were measured in the wavelength range from 500 to 920 nm, with the step size of 1 nm and a counting time of 0.3 sec per step, all of them were background-corrected to a vial with pure solvent.

For a number of supplementary studies, we also used methods such as AFM, Confocal Microscopy, FTIR, and NMR. The detailed description of the conducted tests is given in the Supporting Methods section in the SI.

DFT calculations

To support our experimental observations, we investigated a monolayer Ti3_3C2_2Tx_x MXene with various surface terminations using DFT calculations. All the computations were performed with a plane-wave (PW) basis set as implemented in the Quantum ESPRESSO v7.2 software package[88]. The ion cores were modeled using ultrasoft pseudopotentials from the GBRV database[89]. The generalized gradient approximation of the Perdew–Burke–Ernzerhof exchange correlation functional was used in all calculations[90]. A kinetic energy cutoff of 60 Ry was employed for the wavefunctions, and 400 Ry – for the charge density, across all simulations. The Methfessel–Paxton smearing method was employed with a smearing width of 0.01 Ry, using the local-TF mixing scheme. Both atomic positions and lattice parameters were relaxed to preserve periodicity, with convergence criteria set to the default thresholds 10−410^{-4} a.u. for the energies and 10−410^{-4} a.u. for the forces in the geometry optimization. Target Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXene structures were modeled as two-dimensional monolayers by isolating a single MXene layer and introducing a vacuum region ∼20\sim20 Å along the zz-direction to eliminate interlayer interactions. A two-dimensional Coulomb cutoff approach was applied to properly treat the charged species adsorption on slabs, which suppresses spurious periodic image interactions along the vacuum direction.

We considered 4∗4∗14*4*1 supercell with a 3∗3∗13*3*1 k-point sampling for all the studies. In general, surface terminations bind to the exposed titanium atoms on the outer surfaces of the Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} monolayer. Depending on their chemical nature and size, these terminations preferentially adsorb at either on-top sites of surface Ti atoms or at hollow sites above the underlying atoms. We investigated a range of surface terminations, including =O, –F, –OH, and their mixtures. The results indicate that all these terminations exhibit a strong preference for hollow-site adsorption, which plays a critical role in stabilizing the monolayer structure and modulating the surface reactivity, and nicely correlates with the available literature[91]. Adsorption energies are determined by comparing the total energy of the surface with the adsorbed species to the sum of the energies of the clean surface and the isolated adsorbate.

Results and Discussions

Preliminary validation of prepared Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes

Before moving forward to the MXene–HaP interaction experiments, we validate the quality and oxidation state of the as-cast Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes, before they were exposed to the HaP-precursor solutions. In Figure 2 we summarize the characterization results of the produced MXenes. In Figure 2a and Figure 2b we validated the formation of the desired Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes via XRD and Raman (see the detailed discussion in Section SB in the SI). Characteristic TEM image and the respective SAED pattern in Figure 2c show high-quality single-layer flakes of Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes with a typical hexagonal symmetry and lateral sizes of a few micrometers, which is rather large for MXenes and happens due to the optimal etching protocol[92]. AFM profiling revealed the thickness of ∼2\sim2 nm, confirming the 2D flakes are mono-layered[93]. We also note that TEM does not reveal any undesired oxidation or damage. Overall, the conducted characterization confirms the formation of the high-quality Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} product. Detailed analysis about HF-Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes characterization is given in Section SC in the SI, and in Figure S1.

To further confirm the Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes quality, and to form a baseline for comparing pristine MXenes with MXenes that are exposed to the HaP-precursor solutions, we probe their surface chemistry using XPS analysis, as shown in Figure 2d. We note that while there are several notations for peak assignment in the MXene community for Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x}[94, 95, 96, 97], in this work we follow the comprehensive MXene XPS study by Natu, Barsoum, et al.[98].

Ti2p XPS spectrum can be deconvoluted into five doublets, positioned at Binding Energies (BE) of 455.4, 456.3, 457.1, 457.9 and 459.4 eV, where the first four correspond to Ti2+\mathrm{Ti}^{2+} and Ti3+\mathrm{Ti}^{3+} ions bonded to the carbon core and coordinated with =O/–OH and –F functional groups (C–Ti–T), and the fifth one – to some minority of TiO2−xF2x\mathrm{TiO}_{2-x}\mathrm{F}_{2x} oxofluoride contamination. C1s spectrum was deconvoluted into 3 peaks at BE of 282, 283, and 284.7 eV. The latter peak was used for charge compensation alignment, although we also kept an eye on the first one, whose positioning at the BE of 282 eV is rather universal for Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes[98]. These peaks indicate Ti–C–Ti, C–Ti–O and C–C bonding, respectively. We would like to highlight the low amount of C–C carbon in our samples, which typically originates from over-etching or organic contaminants; this speaks in favor of the optimal etching conditions[99]. O1s spectrum was deconvoluted into 4 peaks at BE of 529.9, 530.9, 532.5 and 534.3 eV, referring to C–Ti–O, TiO2−xF2x\mathrm{TiO}_{2-x}\mathrm{F}_{2x}, C–Ti–O/OH/F at the “bridge” site and adsorbed/intercalated H2O\mathrm{H}_{2}\mathrm{O}, respectively. Since the lowest BE peak (529.9 eV) that refers to the oxygen termination is predominant, we conclude that =O population on the surface is significantly higher than that of –OH. However, in the following sections, we will raise some doubts regarding the accuracy of this notation, as some of our evidence suggests otherwise. F1s spectrum was deconvoluted into 2 peaks at BE of 685.3 and 686.5 eV, indicating C–Ti–F functionalization and the minor trace of AlFx\mathrm{AlF}_{x} secondary phase, respectively.

We clearly see the formation of a mixed-type =O, –F, and –OH surface termination groups, where, following Natu’s analysis[98], the initial ratio between oxygen- and fluorine-based ones is close to 1 : 1, and their overall stoichiometry reaches Ti3C2(O/OH)0.9F1.1\mathrm{Ti}_{3}\mathrm{C}_{2}(\mathrm{O}/\mathrm{OH})_{0.9}\mathrm{F}_{1.1}, demonstrating almost complete (~Ti3C2T2\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{2}) flake functionalization, i.e. the coverage of the MXene with termination groups.

General trends in the chemistry of MXenes in HaP-precursor solutions

After validating the formation of high-quality Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes, we exposed them to the HaP-precursor solutions with different precursor components (following Table 1), and followed the chemical state of both the MXenes and the hosting solutions. Our preliminary tests showed that some of the MXene-containing solutions (also denoted as “inks”) became rather unstable, causing color-change of the solution, which indicated degradation processes. Among the tested inks, we found that some of them are significantly more stable than the others. To gain an in-depth understanding, a thorough study has been conducted after exposing MXenes to the HaP-inks, and observing them after 1 hour and after 1 week. Following Table 1, the study included a combinatorial set of DMSO-based solutions of the precursors, where, MAI, PbI2\mathrm{PbI}_{2}, and I2\mathrm{I}_{2} were added together or in part. This allowed us to isolate and identify (de)stabilization key factors and study the changes that happen to MXenes, including oxidation and surface chemistry changes in the suspended MXenes, providing critical fundamental understanding for the integration of MXenes with HaPs.

To provide insight into the changes in the chemical state and environment of the suspended MXenes, we used the unreacted MXenes as our benchmark and carried out XPS characterization on the remaining filtered solids. We found Ti2p and O1s core-level spectra to be the most chemically sensitive and indicative, as presented in Figure 3, while the complementary F1s core-level spectra are presented in Figure S2.

Complete Ti and O XPS comparison between MXenes extracted from the HaP-precursor solutions

Figure 3. Complete Ti and O XPS comparison between MXenes extracted from the HaP-precursor solutions. (a) Ti2p, and (b) O1s XPS core spectra of the as-cast Ti3C2Tx MXenes and MXenes extracted from solutions 1–8 after 1 hour and 1 week of exposure. In (a), the typical peak position that indicates MXene oxidation (Ti3+→Ti4+; Ti3C2Tx → TiO2-xF2x) is marked by a red vertical dashed line. In (b), the typical position referring to C – Ti – O termination group bonding is marked by the green vertical dashed line, the position referring to MXene oxidation is marked by a red line, while the positions marked with cyan and gray refer to new bonding types that we associate with Ti3C2Tx reacting with MAI and PbI2, respectively. The nature of this bonding is discussed in detail in the text.

F1s XPS core spectra of as-cast Ti3C2Tx MXenes and MXenes extracted from solutions 1–8 after 1 hour and 1 week of exposure

Figure S2. F1s XPS core spectra of the as-cast Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes and MXenes extracted from solutions 1–8 after 1 hour and 1 week of exposure. The typical position referring to C – Ti – F termination group bonding is marked by the magenta vertical dashed line.

We start with identifying inks that oxidize the MXenes (Ti3+→Ti4+; Ti3C2Tx → TiO2 / TiO2-xF2x), and whether the oxidation is instantaneous or slow. The most informative XPS feature for the oxidation state of Ti in the Ti3C2Tx MXenes is the Ti2p spectrum, and in particular the peak around 459.5 eV that indicates the presence of a Ti4+ [98] (see the vertical red dashed line in Figure 3a). First, we verify that the pure solvent (DMSO; ink 1-sol) does not oxidize MXenes, as no increase at ~459.5 eV is observed in the respective Ti2p spectra. A similar result is seen by the O1s edge (Figure 3b), showing no evidence for an extra signal that could relate to the formation of a TiO2 phase, which would appear at ~530.8 eV[98]; the broad peak at ~531.6 eV can be attributed to the intercalated solvent[100]. After verifying DMSO itself does not harm our MXenes, we focus on the interaction of the MXenes with MAI, PbI2, and I2. Initial XPS analysis identified the following phenomena:

MAI containing ink – 1M MAI in DMSO (2-M) – Similar to the pure solvent, MAI does not lead to the oxidation of the Ti3C2Tx MXenes even after 1 week. If we follow the TxT_x termination groups in the O1s (Figure 3b) and F1s (Figure S2) edges for ink 2-M, we find that after 1 hour the BEs are slightly down-shifted, proposing MAI is interacting with the MXene and acting as an electron donor. However, after 1 week the BEs return to their pure-MXene positions – a phenomenon that we will discuss later. In 2-M and other MAI- and/or I2-containing inks (8-MI, 5-I), a characteristic broad peak in the O1s XPS core spectra appears, located around 532.1 eV. For ink 5-I we use this characteristic peak with caution, though, since the presence of I2\mathrm{I}_2 has an oxidizing and destructive effect on MXenes, as will be discussed later on in detail. We also note that this peak does not appear in all PbI2\mathrm{PbI}_2-containing inks, even in the presence of MAI.

PbI2\mathrm{PbI}_2 containing ink - 1M PbI2\mathrm{PbI}_2 in DMSO (7-P) – After a short exposure (1 hour), PbI2\mathrm{PbI}_2 does not show a significant change in the Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x MXene, the same as MAI, but after 1 week, the MXenes are found to be strongly oxidized, as indicated by the ~459.5 eV peak of Ti2p\mathrm{Ti}2p. The O1s edge spectra show a similar trend, where the O1s peak at ~530 eV, which is typical for the MXene oxygen termination group, decreases and broadens, while the signal close to 530.8 eV increases (red dashed line in Figure 3b), supporting the formation of Ti4+\mathrm{Ti}^{4+}. The fluorine edge spectra (Figure S2) show little shift in the peak position of the F1s peak, but also show a significant broadening with the oxidation of Ti, which we attribute to the weaker signal due to the lower amount of the surviving MXenes. We note that, unlike oxygen, which stays attached to Ti after oxidation, fluorine will deplete. Finally, we see from the O1s spectra that all PbI2\mathrm{PbI}_2-containing systems (including: 3-MP, 4-MPI, 6-PI and 7-P) have a characteristic peak at the BE of ~531.4 eV.

MAI-PbI2_2 combined ink – (1:1) MAI:PbI2_2 in DMSO (3-MP) – If we look at the combined effect of MAI and PbI2\mathrm{PbI}_2 on the MXenes (ink 3-MP), the system does not show severe oxidation of MXenes, and from the perspective of the titanium (Ti2p) and fluoride (F1s) spectra, it behaves similarly to the one in 2-M. Interestingly, from the perspective of oxygen (O1s), the system behaves similarly to 7-P. This suggests that the Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x MXenes’ =O termination groups will favor interaction with PbI2\mathrm{PbI}_2-related species over MAI ones.

Overall, if we look at the O1s edge, we can suggest the type of interactions one may expect between =O and MAI / PbI2\mathrm{PbI}_2. For the case of MAI, a =O---H-N hydrogen bond can be expected, which should increase the electron density around oxygen as a result of electron withdrawal from the hydrogen. The new =O---H-N structure may energetically resemble an –OH termination group, which is associated with a ~532 eV feature in O1s spectra[94, 97, 98], which thus can explain the characteristic feature at ~532.1 eV that appears in MAI-containing inks (2-M, 8-MI). PbI2\mathrm{PbI}_2 shows a similar effect on the oxygen spectrum, with the appearance of a characteristic peak at ~531.4 eV, which can be explained by the chemical adsorption of Pb onto oxygen termination groups. We note that PbI2\mathrm{PbI}_2 should be fully soluble in DMSO at the concentration we use (1 M), so we may expect to see the adsorption of Pb2+\mathrm{Pb}^{2+} ions onto negatively-charged Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x MXenes. The adsorption is likely followed by Pb2+→Pb0\mathrm{Pb}^{2+} \to\mathrm{Pb}^{0} reduction and Ti3+→Ti4+\mathrm{Ti}^{3+} \to\mathrm{Ti}^{4+} oxidation – a mechanism closely resembling the one suggested in MXene-based water remediation studies[80, 101]. We also note that O1s core spectra appear much stronger modified upon interaction with MAI and PbI2\mathrm{PbI}_2 species, compared to F1s. This suggests that the chemical interactions in our systems mostly involve =O termination groups, while –F groups stay, to a large extent, inert.

I2\mathrm{I}_2 containing ink – 1M I2\mathrm{I}_2 in DMSO (5-I) – not less importantly, we would like to briefly mention the strong and destructive effect of I2\mathrm{I}_2 or In−\mathrm{I}_n^- polyiodides. In short, Figure 3 shows that any solution that contains elemental I2\mathrm{I}_2, including: 4-MPI, 5-I, 6-PI, 8-MI, ends up having degraded Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x MXenes, even just after 1 hour of exposure, as observed by the pronounced oxidation of Ti from the uprise in the signal at BEs of 458.5-459.5 eV. The slight shift of the Ti4+\mathrm{Ti}^{4+}-oxide peak towards lower BEs might be related to the formation of titanium oxo-iodides[102], as iodine has lower electronegativity compared to oxygen. If we look at the time scale of degradation, 8-MI is exceptional, showing significantly slower oxidation of Ti. This hints that MAI may possess a protective effect on Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x from reacting with surrounding halides. The nature of I2\mathrm{I}_2-assisted degradation and MAI-assisted preservation will be discussed in detail later on.

To summarize the main characteristic behavior when adding MXenes to MAI, PbI2\mathrm{PbI}_2 and I2\mathrm{I}_2 containing DMSO solutions, we suggest the following schematic chemical equations:

[−Ti3+=O]n+H−NH2CH3I⟹[−Ti3+=O]n− ⁣ ⁣− ⁣ ⁣−H−NH2CH3I(1)[-\mathrm{Ti}^{3+}=\mathrm{O}]_{n}+\mathrm{H}-\mathrm{NH}_{2}\mathrm{CH}_{3}\mathrm{I}\Longrightarrow[-\mathrm{Ti}^{3+}=\mathrm{O}]_{n}\mathbin{-\!\!-\!\!-}\mathrm{H}-\mathrm{NH}_{2}\mathrm{CH}_{3}\mathrm{I} \tag*{(1)}
[−Ti3+=O]n+[Pb2+⋯2I−](DMSO)⟹[−Ti3+=O]n−Pb2++2I−⟹[−Ti4+=O]n−Pb0+2I−(2)[-\mathrm{Ti}^{3+}=\mathrm{O}]_{n}+[\mathrm{Pb}^{2+}\cdots2\mathrm{I}^{-}]_{\mathrm{(DMSO)}}\Longrightarrow[-\mathrm{Ti}^{3+}=\mathrm{O}]_{n}-\mathrm{Pb}^{2+}+2\mathrm{I}^{-}\Longrightarrow[-\mathrm{Ti}^{4+}=\mathrm{O}]_{n}-\mathrm{Pb}^{0}+2\mathrm{I}^{-} \tag*{(2)}
[−Ti3+=O]n+12I2⟹[−Ti4+=O]n+I−(3)[-\mathrm{Ti}^{3+}=\mathrm{O}]_{n}+\frac{1}{2}\mathrm{I}_{2}\Longrightarrow[-\mathrm{Ti}^{4+}=\mathrm{O}]_{n}+\mathrm{I}^{-} \tag*{(3)}

In the following section, we will further justify these proposed mechanisms using DFT calculations and N1s, Pb4f and I3d XPS core spectra. Moreover, we will follow the degradation kinetics, focusing on I2\mathrm{I}_{2} and PbI2\mathrm{PbI}_{2} oxidation effects, as well as the MAI protective effect.

DFT investigation of the MAI, PbI2\mathrm{PbI}_{2} (Pb2+\mathrm{Pb}^{2+}) and I2\mathrm{I}_{2} interaction with Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x}

To support the suggested equations, we studied the adsorption behavior of MAI, PbI2\mathrm{PbI}_{2}, and I2\mathrm{I}_{2} on a bare, and on =O, –F, or mixed (=O/–F) terminated Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXene surfaces by means of first-principles DFT methods. For the latter case, we considered 1 : 1 atomic ratio between O and F, as expected from the as-cast Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} characterization given in § 3.1. The snapshots of the examined systems after structural relaxation are given in Figure 4 for the most realistic cases of MAI, PbI2\mathrm{PbI}_{2}, and Pb2+\mathrm{Pb}^{2+} on the mixed-terminated Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXene, and in Figure S3 for all the rest. The calculated adsorption energies are summarized in Table 2. We note that our calculations did not include the solvent, as it would majorly complicate the calculations. While we bear this fact in mind, the solvent, however, did not interact with the MXene (cf., 1-sol), thus we can more confidently assume that the calculations represent the general trend of the interactions between the MXene and the different chemical species.

Figure 4. The snapshots showing DFT structurally-relaxed models for MAI, PbI2\mathrm{PbI}_2, and Pb2+\mathrm{Pb}^{2+} interaction with the realistic mixed-terminated (O/F) Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x MXene surfaces - top and side views. Gray, black, red, green, blue, white, purple, and pink atoms represent Ti, C, O, F, N, H, I, and Pb, respectively.

bare=O–Fmixed O/F–OH
MAI-2.9917-0.8196-0.4917-0.7490-1.3918
PbI2\mathrm{PbI}_2-6.3497-0.1437-0.0755-0.0632-2.4924
I2\mathrm{I}_2-6.5633-0.0280-0.0188-0.0291-5.4798
Pb2+\mathrm{Pb}^{2+}-11.9035-9.3532-8.4894-8.6833-15.9649

Table 2. Calculated adsorption energies (EaE_\mathrm{a} in eV) for MAI, PbI2\mathrm{PbI}_2, Pb2+\mathrm{Pb}^{2+}, I−\mathrm{I}^{-} and I2\mathrm{I}_2 species on Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x MXene surfaces with various terminations: bare (no termination groups attached), pure =O, pure –F, pure –OH, and mixed O/F (in 1 : 1 ratio).

Snapshots showing DFT structurally-relaxed models for I$_2$ interaction with =O terminated Ti$_3$C$_2$T$_x$, –F terminated Ti$_3$C$_2$T$_x$, –OH terminated Ti$_3$C$_2$T$_x$, and bare Ti$_3$C$_2$T$_x$ surfaces; top and side views; panel d.

Figure S3. The snapshots showing DFT structurally-relaxed models for a) MAI, b) PbI2_2, c) Pb2+^{2+}, and d) I2_2 interaction with Ti3_3C2_2Tx_x MXene surfaces - top and side views. For each studied species, four different MXene termination states are presented: =O, –F, –OH terminated and bare surfaces. The snapshots for the most realistic mixed-terminated (O/F) Ti3_3C2_2Tx_x surfaces are given in Figure 4 in the main text. Gray, black, red, green, blue, white, purple, and pink atoms represent Ti, C, O, F, N, H, I, and Pb, respectively.

Starting with CH3NH3I\mathrm{CH}_{3}\mathrm{NH}_{3}\mathrm{I} (MAI), on the bare Ti3C2\mathrm{Ti}_{3}\mathrm{C}_{2} surface it undergoes dissociation, with I−\mathrm{I}^{-} ions preferentially occupying hollow adsorption sites acting as halide termination groups, while one of the hydrogen atoms bonded to the nitrogen in the methylammonium (CH3NH3+\mathrm{CH}_{3}\mathrm{NH}_{3}^{+}) cation interacts directly with the Ti3C2\mathrm{Ti}_{3}\mathrm{C}_{2} surface. However, we know that bare Ti3C2\mathrm{Ti}_{3}\mathrm{C}_{2} MXene is rarely the case, and our material shows almost full termination coverage, as discussed in § 3.1. In case of the terminated MXene surfaces, we found that with both =O and –F termination groups CH3NH3I\mathrm{CH}_{3}\mathrm{NH}_{3}\mathrm{I} favor bonding via the amine (-NH3\mathrm{NH}_{3}), forming a hydrogen bond. If we compare the initial and the final states of the iodine (I−\mathrm{I}^{-}) atom in CH3NH3I\mathrm{CH}_{3}\mathrm{NH}_{3}\mathrm{I}, we find it is somewhat dissociated, and closest to another -NH3\mathrm{NH}_{3} hydrogen. Similar general behavior was observed for the surface with mixed terminations (=O/–F), whose adsorption characteristics closely resembled those of fully =O- or –F-functionalized surfaces. Although for both –F and =O terminations we see a negative adsorption energy, we found that bonding with the =O species is energetically more favorable. The adsorption energies, calculated with respect to the isolated terminated surfaces and a free CH3NH3I\mathrm{CH}_{3}\mathrm{NH}_{3}\mathrm{I} molecule, are −0.82 eV, −0.49 eV, and −0.75 eV for =O, –F, and mixed-terminated surfaces, respectively.

Similar to MAI, on the bare Ti3C2\mathrm{Ti}_{3}\mathrm{C}_{2} surface, PbI2\mathrm{PbI}_{2} does not show a molecular adsorption – it dissociates into Pb and I species that both bond chemically to the surface. In case of either =O, or –F termination (or in the mixed case), we see weak adsorption with characteristic energies of -0.144, and -0.075 eV, respectively. However, it is likely that during the dissolution process, Pb2+\mathrm{Pb}^{2+} and I ions will be solvated in DMSO; therefore, we studied the adsorption behavior of Pb2+\mathrm{Pb}^{2+} ions in addition to PbI2\mathrm{PbI}_{2} molecule. Unlike PbI2\mathrm{PbI}_{2}, Pb2+\mathrm{Pb}^{2+} demonstrates drastically stronger adsorption with much lower free energies of -9.35, -8.49 and -8.68 eV for =O, –F and mixed-terminated surfaces, respectively. This clearly suggests the preference of reaction in Eq. (2) over the one in Eq. (1) when both MAI and PbI2\mathrm{PbI}_{2} are added to the system, which supports our experimental observations and related hypothesis for the preferential adsorption of Pb in pink 3-MP. Also, we see the tendency of the energetic preference of adsorption onto =O termination groups with respect to –F, similar to what was discussed earlier for MAI.

To gain better understanding about the behavior of I2\mathrm{I}_2 around MXenes, we also performed DFT investigation. In case of bare Ti3C2\mathrm{Ti}_3\mathrm{C}_2 MXene surface, the calculations revealed that I2\mathrm{I}_2 is unstable in its molecular form: it dissociates into I−\mathrm{I}^{-} ions that preferentially adsorb at unoccupied “top” sites above the surface Ti atoms. In contrast, adsorption studies on =O, –F, and mixed-terminated MXenes show that iodine molecules remain intact and do not dissociate. We note that I2\mathrm{I}_2 does not exhibit stable adsorption and remains at distances greater than 3.5 Å from the functionalized surfaces, indicating weak or negligible interaction. The obtained results suggest that the observed destructive Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x – I2\mathrm{I}_2 interaction happens on unoccupied termination sites, which are often regarded as structural defects at edges or pores. This may also hint that the impeded I2\mathrm{I}_2-assisted degradation of the Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x MXenes in presence of MAI or PbI2\mathrm{PbI}_2 is related to them blocking the defect sites, providing an effective protective effect. Indeed, we saw that bare Ti3C2\mathrm{Ti}_3\mathrm{C}_2 possesses significant adsorption capacity towards MAI, PbI2\mathrm{PbI}_2 and Pb2+\mathrm{Pb}^{2+}.

Finally, we should note the potential contribution of an –OH termination group. Although we base our analysis regarding the ratio between =O and –OH on ref. 98, it is possible that we underestimate the real amount of –OH on our MXenes. If we follow the complete analysis of the DFT work that we show in Figure S3 and Table S1, we see that the interaction of the different studied species with –OH termination group is dramatically different from =O, –F and mixed cases. For example, MAI interaction with the –OH group is energetically the strongest, and the configuration of the adsorbed molecule is completely different from other studied cases (see Figure S3), with I-ions bonded to the termination hydrogen. The same implies to I2_2 adsorption onto the –OH termination, which also appears to be the most energetically preferrable among the studied configurations, except for the bare Ti3_3C2_2 surface. This suggests that an –OH—I bond should exist, which would explain the appearence of the characteristic peak at ~532.1 eV that we see in Figure 3 for 5-I, where we don’t have MA+^+ cations at all. The adsorption energies of PbI2_2 and Pb2+^{2+} on –OH are also the lowest with respect to the other examined terminations.

These critical DFT-based insights clearly support Eq. (1), and allow us to expand it to the following equations:

[−Ti3+=O]n+H−NH2CH3I⟹[−Ti3+=O]n−−−H−NH2CH3I(4)[{-}\mathrm{Ti}^{3+}=\mathrm{O}]_n+\mathrm{H}{-}\mathrm{NH}_2\mathrm{CH}_3\mathrm{I}\Longrightarrow[{-}\mathrm{Ti}^{3+}=\mathrm{O}]_n{-}{-}{-}\mathrm{H}{-}\mathrm{NH}_2\mathrm{CH}_3\mathrm{I} \tag*{(4)}
[−Ti3+=O−H]n+I⋅NH3CH3⟹[−Ti3+=O−H]n−−−I⋅NH3CH3(5)[{-}\mathrm{Ti}^{3+}=\mathrm{O}{-}\mathrm{H}]_n+\mathrm{I}\cdot\mathrm{NH}_3\mathrm{CH}_3\Longrightarrow[{-}\mathrm{Ti}^{3+}=\mathrm{O}{-}\mathrm{H}]_n{-}{-}{-}\mathrm{I}\cdot\mathrm{NH}_3\mathrm{CH}_3 \tag*{(5)}

This explains what happens in ink 2-M upon Ti3_3C2Tx_2T_x MXene addition. MAI molecules tend to adsorb onto Ti3_3C2Tx_2T_x surface, preferring oxygen or, if available, –OH termination sites. Thus, the small down-shifts in both O1s and F1s spectra after one hour (see 2-M in Figure 3b and Figure S2) may suggest the non-selective MAI adsorption onto various termination groups, while an extra peak at ~532.1 eV is more likely indicative of the –OH—I interaction as suggested in Eq. (1)′′.

We note that since the XPS notation reference we use [98] does not provide strong confidence about the ability to clearly distinguish between =O and –OH groups, we complemented it with an additional FTIR measurement. We compared the as-cast Ti3_3C2Tx_2T_x MXenes with those where we attempted to artificially convert the –OH groups into =O through annealing the MXenes in an Ar-filled quartz ampule following ref. [103]. The resulting spectra are given in Figure S4. We note the intensity of the peak associated with the –OH groups at ~1380 cm−1^{-1} decreases after annealing, while the Ti-O-related signal at ~665 cm−1^{-1}, on the contrary, builds up[104]. This allows us to safely assume that the as-cast Ti3_3C2Tx_2T_x MXenes that we use in our study contain a certain, non-negligible amount of –OH terminations on their surface.

Baseline-corrected FTIR spectra plot showing transmittance versus wavelength for Ti$_3$C$_2$T$_x$ MXenes and annealed Ti$_3$C$_2$T$_x$ MXenes, with labels Ti–O, C–F, O–H, C=O, CO$_2$, and –O–H

Figure S4. Figure S4. Baseline-corrected FTIR spectra for as-cast Ti3_3C2_2Tx_x MXenes and MXenes calcinated at 300°C for 1 hour in the quartz ampule filled with Ar through 3 sequential pump-purge cycles. According to ref. 9, this treatment is expected to convert −OH-\mathrm{OH} surface termination groups into =O=\mathrm{O} ones. Peak assignment was done according to ref. 10.

Overall, Table 2 provides an interesting insight that may explain the mechanistic origin for the protective role of MAI and, to some extent, PbI2_2. Considering bare and –OH termination sites have the most significant adsorption energies, compared to =O and –F, one can conclude that the adsorption of MAI onto bare or –OH terminated sites is supposed to slow down, or even block, the potential oxidizing species, such as I2_2 or Pb2+^{2+}. In case of the strongly oxidizing I2_2, MAI seems to significantly impede the degradation of MXenes, as shown in ink 8-MI (and later further analyzed in § 3.5). In case of the milder oxidation of MXenes via PbI2_2, MAI seems to completely prevent PbI2_2-related oxidation, as evident in ink 3-MP. While the interaction with –OH is more reasonable due to its potential natural abundance, protective effect can be attributed to MAI’s interaction with bare/defective MXene sites, such as edges, which are known to be weak-links and highly reactive[105].

As for the Pb+2^{+2} interaction, significantly higher adsorption energies on all possible functional groups suggest a strong, and likely covalent adsorption. The relatively lower energies for =O and –OH termination groups can explain an extra peak in the respective O1s XPS spectra, supporting the formation of the =O/–OH – Pb bond, as suggested in Eq. (2). In case of the competitive processes involving Pb2+^{2+} and MAI, the former will likely get adsorbed onto MXenes due to much stronger adsorption energies, which clarifies the situation observed in ink 3-MP. If we look at the charges on the outer Ti atoms and termination groups before and after the studied interaction processes, as shown in Table S-T1, we see that in case of both MAI and Pb2+\mathrm{Pb}^{2+} adsorption the TxT_x slightly acquires charge, indicating electron withdrawal from the adsorbed species. Interestingly, similar trends in charge-density variations are evident in the BE chemical shifts in the XPS measurements, as we mentioned earlier, and as we will see in further detail in the following sections.

Comprehensive analysis of MXene interaction chemistry with HaP-precursor components

Based on the results so far, we can summarize our findings in the following way:

  1. MAI is adsorbing to MXenes, supposedly through selective adsorption at =O or, if available, –OH terminations, or active bare sites. Its adsorption is likely promoting a stabilization effect that protects MXenes from oxidation;

  2. PbI2\mathrm{PbI}_2, and more likely Pb2+\mathrm{Pb}^{2+} as its binary, adsorbs onto Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x MXenes selectively (preferentially at =O, or –OH terminations), and expectedly acts as a reducing agent that promotes the oxidation of the Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x MXene;

  3. Free I2\mathrm{I}_2 or polyiodides degrade Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x rapidly via a redox reaction, with a simultaneous formation of Ti4+\mathrm{Ti}^{4+} and I−\mathrm{I}^{-} species. The reaction is expected to happen at bare surface sites.

To support the DFT prediction, suggesting MAI and Pb2+\mathrm{Pb}^{2+} adsorption, we performed UPS measurements to evaluate whether the work function of the filtered MXenes has changed, as an indication for surface modifications; see Figure S4. Our starting work function (ink 1-sol) is 4.67 eV, which is in line with previous works[53, 106, 107]. When we measure MXenes extracted from inks 2-M and 7-P, which correspond to MAI and Pb2+\mathrm{Pb}^{2+} adsorption, respectively, we observe clear shifts in the work function to 4.87 eV with MAI and 4.49 eV with PbI2\mathrm{PbI}_2. We note that the ± 200 meV difference from the pristine state is of the order one will gain by exchanging the MXene surface from fully O-terminated to fully F-terminated[53], and comparable to other reported surface modification strategies[107]. This highlights the importance of knowing the exact surface chemistry of MXenes, prior to their incorporation in devices. In particular for HaPs, such changes in work function may lead to significant effects in optoelectronic devices, such as solar cells, LEDs, and others.

Overall, these conclusions provide us with an important framework and general guidelines for understanding the HaP-solution – MXene system. However, they still lack the evidence that can provide us with an in-depth understanding of the degradation mechanisms and kinetics, and the actual state of the MXenes in cases where the MXenes are not degraded. In this section, we would like to shed light on these three mechanisms, providing a deeper understanding of the nature of passivation and degradation of the Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x MXene when exposed to MAI, PbI2\mathrm{PbI}_2, and I2\mathrm{I}_2. We will explore the XPS of MAI (N1s and I3d) and PbI2\mathrm{PbI}_2 (Pb4f and I3d) components in the characteristic MAI- and PbI2\mathrm{PbI}_2-containing inks, and will provide the degradation kinetics distinguishing between the specific role of I2\mathrm{I}_2 and that of PbI2\mathrm{PbI}_2.

MXene passivation chemistry with MAI

Starting with MAI – the only non-aggressive species in our set – we focus on solutions 2-M, 3-MP and 8-MI. 2-M and 3-MP show minimal degradation, and overall are significantly more stable than the rest of the inks. In 8-MI the degradation seems to be evident, but is rather mild compared to other I2\mathrm{I}_2 containing inks. After focusing on the O1s and F1s XPS spectra in the Section Error! Reference source not found., suggesting chemical adsorption of MAI in 2-M and 8-MI, and of Pb2+\mathrm{Pb}^{2+} in 3-MP, here we further investigate the I3d and N1s core spectra, which are given in Figure 5.

N1s and I3d XPS core spectra

Figure 5. (a) N1s and (b) I3d XPS core spectra of the nitrogen- and iodine-based species from Ti3_3C2_2Tx_x MXenes extracted from inks that focus on the effect of MAI: 2-M 3-MP, 8-MI after 1 hour, and 1 week of exposure. The typical N1s and I3d peak positions for nitrogen and iodine in MAI{sup}108` are marked by cyan and dark-red vertical lines, respectively.

After short exposure to ink 2-M, N1s peak is located at 402.1 eV, and the I3d consists of two doublets: one located at 619.3 eV, and the second one at 619.9 eV. All these peak positions are up-shifted with respect to what is expected for a free-standing MAI (401.9 eV for N and 619 eV for I)[108]. Coupled with the evidence on oxygen and fluorine termination group shifts discussed above (O1s: 529.9 → 529.6 eV; F1s: 685.3 → 685.0 eV), these minor effects may suggest non-selective adsorption of MAI onto the MXene, as suggested in Eq. (1). After 1 week in 2-M, however, we see a strong effect showing that both N and I signals are significantly shifted towards lower BEs of 400.9 and 618 eV, respectively. Simultaneously, in Figure 3b and Figure S2, we can see that the terminal oxygen and fluorine peaks shift to their original positions. We attribute it to the transition from a non-selective bonding to a selective adsorption onto the –OH termination sites that follows the DFT calculated models (Figure 4 and Figure S3) and Eq. (1)’’, where the –OH termination group acts as an electron donor[109, 110].

As a complementary confirmation regarding the interaction of MAI with the Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes, we performed 1H{}^{1}\mathrm{H} solution NMR measurements. For this we used 1M ink 2-M-type solutions with deuterated DMSO (DMSO-d6) to avoid the interference between DMSO and MAI methyl signals in the 1H{}^{1}\mathrm{H} spectrum, with and without MXenes. The resulting 1H{}^{1}\mathrm{H} spectra, displaying the CH3\mathrm{CH}_{3} and NH3\mathrm{NH}_{3} signals, are given in Figure S6. Following the addition of MXenes, we observed a 5.8 ±\pm 0.6% and 4.7 ±\pm 0.6% signal loss for CH3\mathrm{CH}_{3} and NH3\mathrm{NH}_{3} respectively, indicative of MAI surface binding. Additionally, both signals exhibited a 0.02 ppm shift and broadening, most evidently for the CH3\mathrm{CH}_{3} signal, as the NH3\mathrm{NH}_{3} signal is likely motionally narrowed due to fast exchange of its labile protons. These observations strongly support the evidence we collected so far regarding the chemical interaction occurring between Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes and MAI molecules. Table S-T2 summarizes the 1H{}^{1}\mathrm{H} relaxation rates for the CH3\mathrm{CH}_{3} and NH3\mathrm{NH}_{3} groups with and without MXenes in the solution. The relaxation rates showed very slight changes between the MXene-containing sample and the reference, with the transverse relaxation rate unchanged within error. As adsorbed states are characterized by rapid transverse relaxation R2\mathrm{R}_{2}, measurable surface exchange would increase the observed R2\mathrm{R}_{2} in the MXene-containing sample[111].The unchanged R2\mathrm{R}_{2}, alongside the equivalent signal loss for both signals, indicate that MAI is effectively irreversibly adsorbed on the NMR timescale and sequestered by the Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes.

1H NMR spectra of MAI solutions with and without Ti3C2Tx MXenes

Figure S6. 1H^{1}\mathrm{H} (a) CH3\mathrm{CH}_{3} and (b) NH3\mathrm{NH}_{3} NMR spectra of 1M ink 2-M-type solutions with deuterated DMSO (DMSO-d6d_{6}), with and without Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes.

As for ink 8-MI, after 1 hour the trend is similar to what we observe for the material extracted from 2-M, where we associate the minor shifts to the adsorption of MAI on top of Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} through a hydrogen bonding, where hydrogen donates electrons to the termination groups. In contrast to 2-M, however, after 1 week in 8-MI we do not see any significant down-shifts in the position of N1s and I3d peaks, only the increase in the relative intensity for the peak that closer resembles a free-standing MAI. Most likely, this is due to the propagating degradation of MXenes in this ink (see Ti2p core spectra in Figure 3), leaving us with some precipitated MAI on the degraded Ti4+Ox\mathrm{Ti}^{4+}\mathrm{O}_{x}.

As for the passivation effect of MAI, we see that the degradation in 3-MP and 8-MI by both PbI2\mathrm{PbI}_{2} and I2\mathrm{I}_{2} is practically stopped or strongly impeded with respect to the inks that do not contain MAI. Given the experimental and DFT-based evidence we collected, MAI should occupy bare MXene sites, which act as activated spots for degradation. Therefore, having MAI that will be attached to the bare sites (which can also be referred to as defect sites) is likely to provide protection from the aggressive I2\mathrm{I}_{2} attack. Since Pb2+\mathrm{Pb}^{2+} competes with MAI on the adsorption on the =O functional groups, MAI is likely passivating the MXene, or reacts with Pb2+\mathrm{Pb}^{2+} to form [MAI + PbI2\mathrm{PbI}_{2}] complexes[112], thus effectively reducing the overall available Pb2+\mathrm{Pb}^{2+} for adsorption and oxidation (cf. Eq. (2)).

If we focus on a charge density in means of the XPS peak shift (Figure 5) for ink 3-MP, after 1 hour there is a minor down-shift in both N1s and I3d. Overall, such behavior is very different compared to that of inks 2-M and 8-MI. Following the previous discussion on the O1s spectrum in Figure 3b, and the energy values for adsorption of MAI and Pb2+\mathrm{Pb}^{2+} (Table 2), we noticed that Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} favors Pb-related adsorption (Eq. (2)) rather than MAI-related adsorption (Eq. (1)’ or (1)’’). Overall, the assembly of the findings supports a negligible interaction of MAI with the MXene in ink 3-MP and a rather preferential adsorption of Pb as =O/–OH – Pb. Hence, we attribute the small chemical shifts in the positions of N1s and I3d peaks after 1 hour to the interaction of MAI with the adsorbed Pb as =O/–OH – Pb⋯MAI. We note that after 1 week both N1s and I3d signals are matching a free-standing MAI (see dashed vertical lines in Figure 5), suggesting weak MAI-surface interaction. In addition, we note that in ink 3-MP [MAI + PbI2_2]-based complexes should form[113, 114], so the observations for 3-MP ink may relate to the adsorption of these whole complexes onto Ti3_3C2_2Tx_x MXene surface.

MXene oxidation chemistry with PbI2_2

Next, we shift our focus to inks 3-MP, 4-MPI, 6-PI, and 7-P, to better understand the chemistry around PbI2_2 + Ti3_3C2_2Tx_x in DMSO. PbI2_2-containing inks are used for a two-step HaP films preparation[71], so knowing the chemistry of MXenes in these solutions has an immediate practical impact. Focusing on ink 7-P, we saw PbI2_2 leads to an accelerated oxidation of the MXene (see Figure 3). To understand the nature of this degradation, we again turn to XPS, where now we focus on the Pb and I core spectra, namely Pb4f and I3d. In Figure 6 we analyze these spectra for MXenes after exposure to inks 3-MP, 4-MPI, 6-PI and 7-P after 1 hour and 1 week.

Pb4f and I3d XPS core spectra

Figure 6. (a) Pb4f and (b) I3d XPS core spectra of the lead- and iodine-based species adsorbed at Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x MXenes extracted from that focus on the effect of PbI2\mathrm{PbI}_2: 3-MP, 4-MPI, 6-PI, and 7-P, after 1 hour, and 1 week of exposure. The typical peak positions for nitrogen and iodine in PbI2\mathrm{PbI}_2 are marked by a gray vertical dashed line in (a), and dark-red line in (b), respectively. The typical peak position for iodine in MAI is marked by a yellow vertical dashed line in (b). The position marked with red in (a) refers to the bonding type that we associate with Pb selective adsorption onto Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x oxygen termination groups.

Focusing on ink 7-P, where we can isolate the effect from PbI2_2, in Figure 6a we see two distinct states of Pb. Following Keersmaecker et al.[115], the first, and more dominant, peak at 138.2 eV is attributed to a crystalline PbI2_2, and the second up-shifted component at 138.9 eV can be attributed to a fully coordinated Pb. We associate the appearance of the strongly coordinated Pb to its adsorption onto Ti3_3C2_2Tx_x MXene, as suggested by Eq. (2), and also supported by the DFT results. Moreover, it perfectly aligns with the available evidence of MXenes reacting with undercoordinated Pb2+^{2+} defects in HaPs[61, 62], and nicely supports this conception. We expect this adsorption to be =O (or –OH) group specific, following much more pronounced changes in O1s core spectra (see Figure 3b) with respect to F1s (Figure S2). Further support can be found in the fact that the location of the peak also perfectly agrees with the one reported for the study of Ti3_3C2_2Tx_x-mediated Pb extraction from aquatic solutions[116].

Generally, it has been reported that Ti3_3C2_2Tx_x MXenes are efficient in adsorbers for Pb[101, 117]; thus, it reasonable to assume that a similar behavior may happen in other solvents. To further understand the nature of the Pb adsorption on Ti3_3C2_2Tx_x in DMSO, we measured in a TEM isolated flakes that were extracted from ink 7-P (see Figure S7). EDS analysis from the thinnest region on a Ti3_3C2_2Tx_x flake detected Pb atoms in a ratio of ~1 : 1 with respect to Ti, while almost no iodine was detected at the same positions, supporting that Pb signal does not come from PbI2_2. When studying their diffraction via SAED (see Figure S7), we found only Ti3_3C2_2Tx_x MXene diffraction peaks (typical for 001 zone-axis), without any evidence for additional peaks that could relate to a PbI2_2 phase.

Characteristic TEM image with respective SAED pattern and EDS analysis results for Ti3C2Tx MXene flakes extracted from ink 7-P

Figure S7. Characteristic TEM image with respective SAED pattern and EDS analysis results for Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x MXene flakes extracted from ink 7-P. EDS analysis in three given positions (marked with red stars) revealed high amount of the adsorbed Pb (discussed in the main text). The selected area, from which the SAED pattern was taken, is highlighted in TEM image by the blue circle. SAED analysis supported the TEM observations, where no PbI2\mathrm{PbI}_2 crystals were detected in the studied region.

As a supporting test, we checked Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x flakes extracted from ink 6-PI, and indeed much lower content of lead was observed with respect to Ti (Pb : Ti atomic ratio was ≤1:5\le1 : 5). This suggests that in ink 6-PI the processes of Pb adsorption and I2\mathrm{I}_2-mediated degradation are running in parallel, where iodine is oxidizing MXenes, leaving fewer active sites to adsorb Pb. To support this, we return to the XPS results in Figure 6. Interestingly, in ink 6-PI we see almost the same pattern after 1 hour exposure as in ink 7-P; however, it drastically changes after 1 week. After long exposure to 6-PI, the Pb4f spectrum reveals the absolute dominance of the pure PbI2\mathrm{PbI}_2-related signal at 138.2 eV meaning that upon the I2\mathrm{I}_2-assisted degradation of Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x, the adsorbed Pb transforms back to a PbI2\mathrm{PbI}_2 phase, possibly acting as a nucleation site for further PbI2\mathrm{PbI}_2 growth as the solvent dries.

Whenever MAI is added to the system (see Figure 6a - 3-MP and 4-MPI), we find that initially, after 1 hour, the peak related to the coordinated Pb is not as pronounced compared to 7-P and 6-PI. This supports our earlier suggestion of a competition between Pb and MAI adsorption on MXenes, or complex formation with MAI that reduce the activity of Pb to adsorb onto MXenes – both of which suggest impeded occupancy of Pb on the MXene. Moreover, the whole XPS core spectra are significantly shifted towards lower BEs, suggesting a very different and highly reducing chemical environment. The local formation of MAPbI3\mathrm{MAPbI}_3 phase is also possible, which may lead to similar chemical shifts[115]. In addition, when we add MAI, we observe some metallic Pb0\mathrm{Pb}^0, which actually speaks in favor of MAPbI3\mathrm{MAPbI}_3 phase formation after filtration and solvent drying, and a consequent Pb reduction to Pb0\mathrm{Pb}^0 by the probing X-rays – a phenomenon that is typical for XPS measurements of MAPbI3\mathrm{MAPbI}_3[118]. After 1 week of exposure, however, the pattern in 3-MP almost perfectly resembles the one in 7-P, supporting that Pb adsorption indeed happens, or [MAI + PbI2\mathrm{PbI}_2] complex reacts with the surface through Pb.

If we analyze I3d core spectra in Figure 6b, we see that in 7-P and 6-PI, iodine seems to be coming predominantly from PbI2\mathrm{PbI}_2-like phase[115], while in 3-MP and 4-MPI it is shifted closer to what is expected for a free-standing MAI[108]. These positions support the previous discussion of favoring Pb-adsorption, followed by a weaker MAI attachment.

To summarize, the demonstrated findings provide solid support to the first part of Eq. (2), meaning the adsorption of Pb2+\mathrm{Pb}^{2+} onto Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x, while the evidence of MXene oxidation (Figure 3a) supports the second part. The adsorption of metals onto MXenes was reported for several divalent ones, including Pb2+\mathrm{Pb}^{2+}[80, 101]. Having confirmed that the adsorption process is really happening, we expect the oxidation part in Eq. (2) to be a realistic concept of what is happening next, due to the observed oxidation of Ti shown in Figure 3. We note that Pb0\mathrm{Pb}^{0} was directly observed only in inks 3-MP and 4-MPI, as discussed above, but not in 7-P and 6-PI (see Figure 6a), where partial reduction of Pb was observed as a slight shift of PbI2\mathrm{PbI}_{2}-related peak towards lower BEs. One possible reason can be a rapid oxidation of the adsorbed Pb0\mathrm{Pb}^{0} while solvent drying during the sample preparation for XPS. Thus, we re-write Eq. (2) in a more cautious form as follows:

[−Ti3+=O]n+[Pb2+](DMSO)⟹[−Ti3+=O]n− ⁣ ⁣− ⁣ ⁣−Pb2+⟹[−Tiδ+=O]n− ⁣ ⁣− ⁣ ⁣−Pbδ−(6)[-\mathrm{Ti}^{3+}=\mathrm{O}]_{n}+[\mathrm{Pb}^{2+}]_{\mathrm{(DMSO)}}\Longrightarrow[-\mathrm{Ti}^{3+}=\mathrm{O}]_{n}\mathbin{-\!\!-\!\!-}\mathrm{Pb}^{2+}\Longrightarrow[-\mathrm{Ti}^{\delta+}=\mathrm{O}]_{n}\mathbin{-\!\!-\!\!-}\mathrm{Pb}^{\delta-} \tag*{(6)}

Implications to the joint effects of MAI + PbI2\mathrm{PbI}_{2} with Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_{x} MXene

As discussed earlier, both PbI2\mathrm{PbI}_{2} and MAI get preferably adsorbed onto oxygen (or –OH) termination groups, but the oxidation of Ti in ink 3-MP is suppressed (unlike what we observe in ink 7-P), which suggests that Pb is further complexed with MAI, or MAI is complexed with the MXene. When we leave ink 3-MP intact at room temperature or cooled down, it transforms from dark-green transparent liquid to pale white-yellow suspension within several hours (see Figure S8). If we heat up the vial above 70°C upon mixing, it reversibly turns back to its original state (a dark-green color is preserved even after several weeks), which indirectly supports complex formation.

Photos of the vial and XRD patterns

Figure S8. (a) photos of the vial with ink 3-MP after several days of storage in the ambient conditions (left), and after “remediation” by heating at 70°C for an hour (right); (b) XRD patterns of as-cast Ti3_3C2_2Tx_x MXenes and materials (MXenes + adsorbed or surrounding species) extracted from solutions 1-3 after 1 week exposure; (c) supplementary representation of the same XRD patterns, but 3-MP plotted at the logarithmic scale to highlight the lower intensity peaks; (d) - supplementary representation of the same XRD patterns, but in low 2θ\theta range of 3-13° to highlight the shifts in characteristic (002) MXene reflection (2θ\theta positions for each case are given at the graphs).

To further distinguish the nature of MXenes after inks 2-M and 3-MP, we checked XRD patterns of Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_{x} MXenes extracted from inks 1-sol, 2-M and 3-MP (Figure S8), using the same samples that we used for XPS tests. We see that after 1-sol and 2-M the material does not exhibit any extra reflections except for the (002) MXene peak. However, after ink 3-MP we no longer observe any MXene-related reflections, suggesting the MXene flakes are significantly separated and lose any periodicity. Instead, we start seeing characteristic peaks of PbI2\mathrm{PbI}_{2} and MAI phases. If we highlight low intensity peaks by plotting the pattern at the logarithmic scale (Figure S8), we will see the plethora of them, proving large degree of complexation between the components in this system, as well as some partial nucleation of PbI2\mathrm{PbI}_{2} and MAI around MXenes. We note that it is unusual to see MAI / PbI2\mathrm{PbI}_{2} peaks without MAPbI3\mathrm{MAPbI}_{3}, since MAPbI3\mathrm{MAPbI}_{3} often rapidly forms when these two binaries are present in the same space. This may indicate, though, that MAI and PbI2\mathrm{PbI}_{2} are spatially separated on the MXenes, or that the HaP decomposes into its binaries before the measurement. While it is out of the scope of the current work, we will be looking into it in the following studies.

When we focus on the position of (002) Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_{x} MXene reflection (see Figure S8), we see that it shifts from the original 6.53° to 4.72° after exposure to ink 1-sol, due to intercalation of DMSO molecules[100, 119], and to 4.95° after ink 2-M. This indicates a different intercalation state after ink 2-M, compared to ink 1-sol, and serves as extra indirect evidence for MXenes’ interaction with MAI.

Noting that MAI and PbI2\mathrm{PbI}_{2} compete for adsorption on the MXene, we further evaluate the ability to control the MXene surface chemistry by a sequential exposure to these different elements. To do that, we soak the MXenes into a solution that contains only MAI (2-M like), wait for 1 hour, and only then add dissolved PbI2\mathrm{PbI}_{2} in DMSO. Following Figure S9, we do not see Pb adsorption, but rather MAI adsorption. This is evident by the characteristic O1s peaks at ~532.0 eV and ~531.5 eV, which are attributed to MAI (–OH—I like; Eq. (1)″) and PbI2\mathrm{PbI}_{2} (=O/–OH — Pb like; Eq. (2)″) related adsorption, respectively. We found that if we start with MAI, even after the addition of PbI2\mathrm{PbI}_{2}, the characteristic peak remained on the position associated with MAI adsorption, i.e., –OH—I like at ~532.1 eV. This is in contrast to the original 3-MP experiment shown in Figure 3b, where we show that when PbI2\mathrm{PbI}_{2} is there from the start, the surface of the MXene would be =O/–OH — Pb like. Moreover, we do not see the characteristic coordinated Pb peak at 138.9 eV in the respective Pb4f core spectra, which further confirms the absence of interaction between Pb ions and MXene surface groups.

O1s, N1s, I3d and Pb4f XPS core spectra of Ti3C2Tx MXenes after exposure to methylammonium iodide and lead iodide

Figure S9. O1s, N1s, I3d and Pb4f XPS core spectra of Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x MXenes after exposure to (a) ink 3-MP (MAI+PbI2_2) for 1 week (copy of the result from the main text, given here for comparison), (b) MAI for 1 day., and (c) after consequent exposure to MAI (1 day) and PbI2_2 (for another 1 hour). The typical position referring to: C – Ti – O (TxT_x), nitrogen and iodine in MAI, and lead in PbI2_2 are marked with green, cyan, dark-brown and gray vertical dashed lines, respectively. Extra peaks that we associate with the formation of the –OH–I and =O/–OH–Pb bonds in the O1s spectra are additionally marked with the cyan and gray lines, respectively.

These results clearly suggest that the functional control of MXenes can be achieved not only through chemical environment and time, but also by controlling the sequence chemicals are added. We should note that we are not aware of other publications that showed a similar attribute in MXenes, in general, and this work is likely to be the first to report it. Interestingly, such an attribute is rather common in coordination chemistry and the stabilization of nano-particles[120], where the sequence of precursor addition determines the coordinated species (the ligands) and their overall stabilization. Therefore, we should be able to design MXenes with specifically functionalized surfaces by simply controlling the sequence of the added components before implementation – an idea we are currently investigating and will report in a future work.

Functionally, if MAI or Pb+MAI are adsorbed onto the MXene, they both can act as nucleation centers – a statement that was hypothesized several times[48, 63, 64, 65], but without a solid support. Particularly, we note a recent publication[121] that suggests that exposure to MAI prior to bringing Ti3_3C2_2Tx_x MXenes in contact with MAPbI3_3 is beneficial for the formation of a less-defective HaP-MXene interface. The authors suggested chemical adsorption of MAI based on indirect empirical evidence from the device functionality. Our results clearly shed light on many of these hypothesized statements, providing a solid ground for this result with additional critical insights – both empirical and theoretical – and providing a better platform for further engineering HaP integration with MXenes.

MXene degradation chemistry with I2_2

Finally, we will focus on the effect of I2_2 on MXenes when added to different inks (4-MPI, 5-I, 6-PI, and 8-MI), mostly on the degradation kinetics and the chemical origin for the degradation. In addition, we will elaborate on the differences between I2_2- and PbI2_2-based degradation.

As mentioned earlier, while MAI and PbI2_2 are the natural binaries of MAPbI3_3, I2_2 is typically not intestinally added to HaP-inks, but it is known as a product that may spontaneously form inside halide solutions[76, 77] or films[82, 83, 84]. While we used a very high concentration of 1M I2_2, which is likely not something one will intentionally introduce in a realistic HaP-based ink, we wanted to compare the strength of its effect with that of MAI and PbI2_2. This allowed us to observe the strong and detrimental effect of I2_2 on the MXenes, as well as to see the clear protective nature of MAI on MXenes, and the different characteristic degradation mechanism compared to that of PbI2_2.

To analyze the degradation kinetics, we employed optical transmission experiments of the various inks. The principle behind this experiment is the fact that optical opacity to transmitted light should decrease once MXenes’ density decreases due to degradation. MXenes scatter light due to their metallic nature, but once dissolved or oxidized to a TiO2_2 form, light transmission should increase (see the schematic illustration of this principle in Figure 7a). As a control, the impact of the solution without MXenes is shown in Figure S10, where we prepared inks without adding Ti3_3C2_2Tx_x and measured their optical transmission spectra. It is expected that I2_2 will lead to optical absorption, and indeed, in the solutions where we added I2_2, we found an absorption band below 780 nm. Since above 780 nm all the solutions stop absorbing light, we could isolate the scattering effect due to the MXenes and use the transmitted light intensity as a metric to the Ti3_3C2_2Tx_x MXenes concentration. Therefore, to follow their degradation we focused on the intensity changes at 920 nm – well above the iodine-related absorption (< 780 nm) or MXene-related plasmon-related absorption at 780-800 nm[122].

Optical transmission study of MXene degradation

Figure 7. Optical transmission study of MXene degradation. (a) schematics of the conducted light transmission experiment that follows MXene dissolution – as MXenes dissolve, more light passes through. (b,d) Representative optical transmission spectra of MXene-containing solutions for studying (b) the effect of I2\mathrm{I}_{2} and MAI (5-I, 2-M, and 8-MI) and (d) the effect PbI2\mathrm{PbI}_{2} (7-P, 6-PI and 4-MPI), after day 1 and day 9; 2-M, 7-P, and 4-MPI show no significant change in their spectrum with time; (c,e) time-dependent transmittance at 920 nm following the dissolution of MXenes with time. The results are respective to the solutions presented in (b,d); a reference solution (without Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_x MXene addition) is added as a benchmark. The thickness of the “pure solvent” line in (c,e) estimates the error following Figure S8.

Optical transmission spectra of reference solutions without MXenes

Figure S10. Transmission control experiment. Optical transmission spectra of the different reference solutions (4-8), without Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXene addition, showing the baseline transmission spectrum from, where we can determine that at 920 nm there is no absorption coming from the chemical species that are not MXenes.

As a quasi-quantitative calibration to MXene’s concentration, we prepared fresh DMSO solution in which we suspended known concentrations of Ti3_3C2_2Tx_x: 10, 50, 100, 200, 300, 400, and 500 μg mL−1^{-1} ; right after suspending the MXenes in the solvent, we measured their optical transmission spectra. The resulting spectra are given in Figure S11-Figure S11, and the derived calibration curve (intensity values at 920 nm) is given in Figure S11. We see a perfect logarithmic decay in the light transmission intensity with increasing Ti3_3C2_2Tx_x concentration. A similar calibration test was performed with a DMSO+MAI solution, to show that the effect on the transmission intensity depends on the MXene concentration and not the solution itself. As we will see below, the relevant calibration concentration for our decay experiments is marked by a green zone in Figure S11.

Transmission–Concentration calibration experiment

Figure S11. Transmission–Concentration calibration experiment. UV-Visible optical transmission spectra of (a) DMSO, and (b) DMSO+MAI solutions with known concentrations of Ti3_3C2Tx_2T_x MXenes: 10, 50, 100, 200, 300, 400, and 500 μ\mug mL−1^{-1}; (c) transmittance at the wavelength of 920 nm for the reference DMSO, and DMSO+MAI solutions with known concentrations of Ti3_3C2Tx_2T_x MXenes (calibration curves) as a function of Ti3_3C2Tx_2T_x MXene concentration in 10-500 μ\mug mL−1^{-1} range. The green zone in c represents the relevant calibration region in our decay experiments that are discussed in the main text.

Following the calibration and control experiments, to investigate the aging kinetics due to the addition of I2\mathrm{I}_{2}, we followed the optical transmission spectra for inks 2-M, 5-I and 8-MI after 1, 2, 3, 7 and 9 days (Figure 7b). It is easy to see that between day 1 and day 9 in inks 5-I and 8-MI, there is an increase in the transmission intensity along the spectrum, where in ink 5-I it is much faster. In Figure 7c we show the changing intensity at 920 nm, so we can follow the degradation kinetics. Overall, by plotting and comparing the degradation kinetics curves from all the inks: 2,5,8 in Figure 7c; 4,6,7 in Figure 7d; and 1,2,3 in Figure S12, we found that the degradation kinetics in 5-I is the fastest, while inks 1-sol, 2-M, 3-MP show no degradation. Inks 6-PI and 8-MI show somewhat slower degradation with respect to that of 5-I, while 4-MPI and 7-P show strongly impeded degradation.

Plot of transmittance at 920 nm versus time in days, showing pure solvent, 1 - sol, 2 - M, and 3 - MP

Figure S12. Time dependences of the transmittance at the wavelength of 920 nm for the stable Ti3_3C2_2Tx_x MXene-containing solutions (1-sol, 2-M and 3-MP) and the reference solution (without Ti3_3C2_2Tx_x MXene addition).

We clearly see that with MAI and PbI2\mathrm{PbI}_{2} (compare 5-I, 8-MI, and 6-PI in Figure 7c,Figure 7e), the MXene dissolution is impeded, where their combined effect can effectively stop MXene dissolution (Figure 7e), but not their oxidation (Figure 3). Following Figure S12, indeed, we do not see inks 1-sol, 2-M, 3-MP degrade, as expected from the earlier XPS study (Figure 3), confirming the high stability of Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_x in these media. We note that the reverse trend of the transmittance decrease with time for inks 3-MP and 2-M might be associated with flake agglomeration or complex formation.

Focusing on the effect of I2_2, if we quantify the degradation due to I2_2 in ink 5-I using the calibration curve in Figure S11, we can estimate that after 1 hour we already lose more than 50% of the initial MXenes, and after a week, more than 80%. Keeping Ti3_3C2_2Tx_x MXenes in ink 5-I for 2 weeks led to no material on PVDF membrane upon vacuum filtration, which supports the assumption the I2_2 leads to the dissolution of MXenes. We note that degradation due to I2_2 starts with a quick process that spans about 1-2 days, then follows a slower degradation step, as clearly shown for inks 5-I, 6-PI and 8-MI in Figure 7c,Figure 7e. From this simple qualitative analysis, and following DFT-related discussion in Section 3.2.1, we suggest that halide species attack defective sites of Ti3_3C2_2Tx_x MXene flakes, break them down to smaller pieces, leading to a fast reduction in the scattering intensity due to particle size. The slow step, then, is a dissolution that occurs from the MXene edges until complete disappearance.

As for PbI2_2-containing inks, we do not see an increase in transmittance for inks 7-P and 4-MPI (see Figure 7d,Figure 7e), suggesting that in these inks the degradation of Ti3_3C2_2Tx_x MXenes is mostly via their oxidation but not dissolution. Regardless the reason, this process is much slower compared to the rapid oxidation by I2_2. As for the possible mechanistic explanation, our suggestion is that PbI2_2-containing solutions are expected to lead to degradation following Eq. (2)’, where we suppose Pb adsorption followed by Ti oxidation that leads to the flake’s oxidation without dissolution, keeping it structurally intact. Alternatively, the oxidation process happens slowly only when the MXenes are exposed to air. The dissolution process when I2_2 is added may be related to the formation of TiI4_4, which is known to be soluble in DMSO[123]. These alternative mechanisms need to be investigated separately.

We would like to briefly mention a rather unique phenomenon we observed in ink 4-MPI, where we noticed the formation of a precipitants within the solution, even without MXenes (see Figure S13). As a side note to this work, we studied the precipitants that formed in the body of ink 4-MPI, and compared this solution to the stable ink 3-MP (see SI, Section SD). We observed these precipitants right inside the volume of the ink (without the filtration or solvent drying) using a confocal microscope, and compared inks with and without Ti3_3C2_2Tx_x MXene addition; the respective characteristic images are given in Figure S13. In the absence of MXenes, we observed the formation of large, elongated rods with lengths above 100 μ\mum. Ti3_3C2_2Tx_x addition led to their shortening and disoriented ”hedgehog”-like morphology, which supports the idea that MXenes play a role in nucleation functionality, as previously suggested[48, 63, 64, 65]. Further details can be found in Section SD in the SI.

Confocal microscopy images, XRD pattern, and TEM images with SAED patterns

Figure S13. (a) confocal microscopy images of solutions 3-MP and 4-MPI with and without Ti3_3C2_2T_x$ MXenes; (b) XRD pattern of precipitates from 4-MPI before and after heating them at 140°C; (c) TEM images of precipitates extracted from 4-MPI with respective SAED patterns at various tilt angles.

To understand the chemistry behind the I2_2-based degradation of MXenes, we studied the Raman spectra of the solutions, in which we suspended the MXenes. Figure 8a shows the Raman spectra of the freshly prepared inks 3-MP, 4-MPI and 5-I, with and without the addition of Ti3_3C2_2Tx_x.

Raman spectra of solutions 3-MP, 4-MPI, and 5-I with and without Ti3C2Tx MXenes addition, and of 5-I with and without excessive Ti3C2Tx MXenes addition

Figure 8. (a) Raman spectra of the solutions 3-MP, 4-MPI, and 5-I with and without Ti3_3C2Tx_2T_x MXenes addition; (b) Raman spectra of 5-I with and without an excessive addition of Ti3_3C2Tx_2T_x MXenes (3 mg mL−13\ \mathrm{mg}\ \mathrm{mL}^{-1} concentration compared to 1 mg mL−11\ \mathrm{mg}\ \mathrm{mL}^{-1} for regular inks): as-prepared (fresh) and after 1 week storage in a dark place.

In ink 4-MPI we see one dominant peak at 110 cm−1^{-1} that is indicative of I3−_3^- stretching mode; the broad peak at 140-146 cm−1^{-1} originates from the asymmetric I3−_3^- vibration. Since MAI is a source for I−^-, In−_n^- polyiodides will naturally form when exposed to I2_2[124, 125] and if the MAI : I2_2 stoichiometry is ∼1:1\sim1 : 1, the most dominant polyiodide will be I3−_3^-. A supplementary Raman study on ink 8-MI shows a similar result (see Figure S14), confirming the formation of I3−_3^-. We note that I3−_3^- peak intensity is very strong, partially because it may fall into Raman resonance conditions, making [PbI2_2]-related features and DMSO features absent. The most aggressive ink, 5-I, also demonstrated the existence of polyiodides, but with richer iodine chemistry. Except for the I3−_3^- feature at 110 cm−1^{-1} and 140 cm−1^{-1}, we also revealed peaks at 168 and 187 cm−1^{-1}, referring to I5−_5^- and I2_2 species, following:

Supplementary Raman spectra of the solutions

Figure S14. Supplementary Raman spectra of the solutions (a) 4-MPI and 8-MI, both containing mixtures of MAI and elemental I2_2, and (b) 3-MP and 7-P, both containing PbI2_2, all without Ti3_3C2_2T_x$ MXenes addition.

I2+I−↔I3−(7)I_2 + I^- \leftrightarrow I_3^- \tag*{(7)}
I3−+I2↔I5−(8)I_3^- + I_2 \leftrightarrow I_5^- \tag*{(8)}

With no MAI influence, which provides a source of I−^-, we have an excess of I2_2 with respect to a minority of the spontaneously forming I−^-[126], leading to the formation of I5−_5^- and I3−_3^- species. The iodine and polyiodide modes in all the spectra were assigned in accordance with refs [126, 127, 128, 129]. We note that the broad feature at 114 cm−1114\ \mathrm{cm}^{-1} that we see in ink 3-MP, and also observed in 7-P (see Figure S14), can be attributed to PbI2\mathrm{PbI}_{2}-DMSO or [MAI + PbI2\mathrm{PbI}_{2}]-DMSO complexes[130, 131].

When adding MXenes (full lines in Figure 8), 3-MP and 4-MPI show no changes in the chemical environment, as an identical shape appears for both spectra, with and without MXenes. When adding MXenes to ink 5-I, however, we do notice a slight increase in the relative intensity of I3−\mathrm{I}_{3}^{-} and I5−\mathrm{I}_{5}^{-} related peaks with respect to the I2\mathrm{I}_{2} feature; however, the effect is rather weak. Since this effect was a result of MXene addition, to enhance it, we increased MXene concentration to 15 mmol L−115\ \mathrm{mmol\ L}^{-1} (or 3 mg mL−13\ \mathrm{mg\ mL}^{-1}) – 6 times higher than in our standard studied inks (see Figure 8b). With a much more pronounced effect, we now see that after 1 week of storage in darkness (so no light-induced polyiodide conversion occurred), MXene-containing inks show a very clear increase in I3−\mathrm{I}_{3}^{-} and I5−\mathrm{I}_{5}^{-} features with respect to I2\mathrm{I}_{2}, while fresh inks with and without MXenes barely differ from each other. We note that with time, even without MXenes, we see spontaneous formation of I3−\mathrm{I}_{3}^{-} and I5−\mathrm{I}_{5}^{-}, likely due to residual exposure to light, but it is clear that the presence of MXenes accelerates their formation.

The origin for the spontaneous formation of I3−\mathrm{I}_{3}^{-} and I5−\mathrm{I}_{5}^{-} is clear: since I2\mathrm{I}_{2} is in excess, a spontaneous reduction of I2\mathrm{I}_{2} to I−\mathrm{I}^{-} leads to an increase in the concentration of I−\mathrm{I}^{-}, which is the source for In−\mathrm{I}_{n}^{-} polyhalides. I5−\mathrm{I}_{5}^{-} also forms since I2\mathrm{I}_{2} is in excess, and stays in excess even after the reduction of I2\mathrm{I}_{2} within the time frame of the experiment. We note that if the ratio between I2\mathrm{I}_{2} and I−\mathrm{I}^{-} had increased closer to equimolarity (1 : 1), we would have measured a spectrum similar to 4-MPI or 8-MI.

Overall, polyiodides are known to be extremely aggressive and corrosive species[76, 77], which suggests a redox reaction between MXenes and polyiodides. If we look on the electrochemical potentials for the oxidation of Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_{x} MXenes to TiO2\mathrm{TiO}_{2} (Eox=−0.54 eVE_{\mathrm{ox}}=-0.54\ \mathrm{eV}) and the reduction of iodine (Ered=+0.54 eVE_{\mathrm{red}=+0.54\ \mathrm{eV}}})[132] in aqueous solutions, we see that energetically it is easy to explain the redox reaction. If we add the fact that higher polyhalides have slightly more positive reduction potential than that of free iodine (I5−>I3−>I2\mathrm{I}_{5}^{-}>\mathrm{I}_{3}^{-}>\mathrm{I}_{2})[133], we can explain our finding that ink 5-I is the most reactive towards Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_{x} (Figure 7b,Figure 7d), since in Figure 8 we show that it contains the highest concentration of I3−\mathrm{I}_{3}^{-} and I5−\mathrm{I}_{5}^{-} species. Following the above, we can explain the degradation reactivity of MXenes with In−\mathrm{I}_{n}^{-}, shown in Figure 3a, by expanding Eq. (3) as follows:

2Ti3++I2→2Ti4++2I−(9)2\mathrm{Ti}^{3+}+\mathrm{I}_{2}\rightarrow2\mathrm{Ti}^{4+}+2\mathrm{I}^{-} \tag*{(9)}
(n−1)Ti3++In−→(n−1)Ti4++nI−(10)(n-1)\mathrm{Ti}^{3+}+\mathrm{I}_{n}^{-}\rightarrow(n-1)\mathrm{Ti}^{4+}+n\mathrm{I}^{-} \tag*{(10)}

We remind that the pronounced formation of I−\mathrm{I}^{-} in presence of MXenes also nicely supports our DFT-based assumption discussed in Section 3.2.1. As for whether it follows the formation of TiIx\mathrm{TiI}_{x} species that can further dissolve in DMSO[123] – it is a matter to be studied.

We underscore that a very minor addition of MXenes (two to three orders of magnitude smaller molar ratio with respect to iodine) is already manifested in a pronounced change of the inks’ chemistry. When a stabilizing agent comes into play, such as MAI in our case, degradation slows down, as shown when comparing 8-MI with 5-I (see Figure 3, Figure 4, Figure 7b,Figure 7d). The inhibition of MXene degradation by MAI is likely to be affected by the interaction of MAI with polyiodides (like in inks 4-MPI and 8-MI)[124], but also due to the adsorption reaction with MXenes, as was discussed in the previous sections.

Exploring the broader applicability of our findings

To understand whether what we observed are the general trends, we carried out a number of supplementary studies, changing the type of MXenes, the solvent, or the halide salts.

Type of MXene: First, we studied the behavior of a supplementary HF-Ti3_3C2Tx_2T_x MXene batch upon their exposure to inks 1-3, the respective XPS spectra for both the Ti core and the termination groups, =O and –F, are given in Figure S15. As we noted before, the initial state of the HF-MXenes is somewhat more oxidized, and the further oxidation due to PbI2_2 (in ink 3-MP) is more obvious. This can be related to higher natural defectivity of MXenes prepared using solely HF[86, 99]. The evolution of functional groups is similar to what we observed for our main batch, although we see an unexpected modification of F1s core spectra in parallel with O1s after inks 2-M and 3-MP. Likely since HF-Ti3_3C2Tx_2T_x has more –F terminations, the reaction with MAI appears on fluorine sites as well, because, as we showed in Section 3.2.1, the formation of –F—I bonds is also energetically favorable. As a rather obvious result, to avoid accelerated degradation we suggest using the least defective MXenes possible for integration with HaPs, and using a passivating molecules or cations (MAI or MA+^{+}), as was also suggested elsewhere[121]. As we realize that pre-exisiting defects on MXenes may play an important practical role, an important conclusion is that our, and others’, theoretical studies are limited to a high-quality isolated flakes of Ti3_3C2Tx_2T_x, while an important complementary work is needed to understand the interaction between the defect states of MXenes with its surrounding. Overall, although the observed trends could remain similar, the details on the termination group population and defects will affect the MXene – HaP-precursor interactions.

XPS core spectra for HF-Ti3C2Tx MXenes

Figure S15. Changing the MXene preparation protocol: Ti3C2Tx→HF\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} \rightarrow\mathrm{HF}-Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x}. Ti2p\mathrm{Ti}_{2p}, O1s\mathrm{O}_{1s}, F1s\mathrm{F}_{1s}, I3d\mathrm{I}_{3d} and N1s\mathrm{N}_{1s} XPS core spectra for as-cast HF-Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes and HF-MXenes extracted from MXene-containing solutions 1-3 after 1 week of exposure.

Solvent: To check the effect on the exploited solvent, we investigated the similar set of inks, but with DMF being a solvent instead of DMSO. Ti2p XPS core spectra of Ti3_3C2Tx_2T_x MXenes extracted from these inks are presented in Figure S16, while Figure S14 provides the respective O1s, F1s, I3d and N1s spectra. Here we see some clear differences with respect to when using DMSO as a solvent. First of all, the oxidation of MXenes in DMF-based inks is significantly faster than in DMSO. Second, we do not actually see the interaction between MAI and Ti3_3C2Tx_2T_x in this case, neither from O1s and F1s, nor from I3d and N1s core spectra, as no characteristic chemical shifts or extra peaks occur, unlike what was discussed in the previous sections. These results mean that the solvent has an impact on the MXene – HaP-precursor behavior, possibly due to differences in the coordination chemistry between the solvents. with the different species in the ink, and require a complementary study of the behavior of MXenes in the hosting solutions with tools similar to what we provide in this work.

XPS core spectra for Ti3C2Tx MXenes with DMF as a solvent

Figure S16. Changing the solvent: DMSO →\rightarrow DMF. (a) Ti2p\mathrm{Ti}_{2p} XPS core spectra of as-cast Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes and MXenes extracted from solutions 1-8, with DMF as a solvent; (b) O1s\mathrm{O}_{1s}, F1s\mathrm{F}_{1s}, I3d\mathrm{I}_{3d} and N1s\mathrm{N}_{1s} XPS core spectra of as-cast Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes and MXenes extracted from stable MXene-containing solutions 1-3, with DMF as a solvent. MXene extraction was performed after 1 week of exposure.

Precursors: Finally, we checked if similar effects happen in the presence of alternative organic and metal salts, i.e. formamidinium (FAI) instead of MAI, and CuI instead of PbI2_2; all using DMSO as a solvent. If we change MAI with FAI, the termination group XPS core spectra modification also takes place, as evidenced in Figure S17, suggesting similar hydrogen-bond mediated adsorption processes. O1s core spectra evolution looks similar to the case of MAI, but we also observe changes in F1s spectra (an extra peak arising at higher BEs), suggesting that FAI may be less selective between different termination groups. Figure S17 provides Ti2p, Cu2p and I3d XPS spectra after Ti3_3C2_2Tx_x MXenes interaction with DMSO+CuI ink. Similar to Pb-salt, we detect copper in more richer chemical state than what is expected for pure copper iodide[134], suggesting the interaction of CuI with Ti3_3C2_2Tx_x. The pronounced shift of Ti2p core spectrum towards higher BEs also speaks in favor of the strong interaction between the MXene and the metal halide, which nicely correlates with what was shown in one of the earlier works on copper adsorption for water remediation[135].

XPS core spectra of as-cast and extracted Ti3C2Tx MXenes

Figure S17. Changing the organic- and metal-halide species: MAI → FAI and PbI2_2 → CuI. (a) O1s, F1s, I3d and N1s XPS core spectra of as-cast Ti3_3C2_2Tx_x MXenes and MXenes extracted from DMSO+FAI solution (similar to 2-M); (b) Ti2p, Cu2p and I3d XPS core spectra of as-cast Ti3_3C2_2Tx_x MXenes and MXenes extracted from DMSO+CuI solution (similar to 7-P). MXene extraction was performed after 1 week of exposure.

Overall, we see that the MXene-HaP system is very much chemistry specific. While the use-case we chose draw the general trends in the interaction between MXenes and HaP-related precursors, the details may matter. In particular we found that the solvent and the state of the MXene itself play a significant role, but also that clear similarities between very different chemical environments (e.g., when changing the precursors) do exist. Concluding the supplementary set of tests, we underscore that what we provide in this work is a foundation, as well as an established experimental infrastructure, for further studies in different environments and with different MXenes. That would allow use-case specific understanding of MXenes chemistry and stability in chemically-active media, not necessarily HaP-related.

Summary and Outlook

As an overall conclusive remarks, the thorough analysis of Ti3_3C2_2Tx_x MXene stability upon interaction with MAI, PbI2_2 and I2_2 in DMSO-based HaP-inks allowed us to identify the following phenomena:

  1. MAI, and likely other amino-halide salts, are not harmful to MXenes even after long-term exposure. They tend to adsorb onto the Ti3_3C2_2Tx_x surface through the formation of hydrogen bonds of –N–H with =O and –F termination atoms, or –I with –OH. We note that the XPS quantification analysis that we use here[98] does not allow us to properly estimate the population of –OH termination groups on our MXenes, however, we can be confident about their presence on the surface based on the FTIR analysis, as well as overall knowledge about MXenes. These groups are expected to strongly affect the MAI adsorption behavior, and MAI shows much higher affinity towards –OH. We associate at least one of the observed XPS features to the formation of an –OH–I bond, where adsorbed iodine act as an electron acceptor. Moreover, MAI was found to provide the overall passivation effect through blocking the bare and defective sites, inhibiting, for example, free-halide assisted degradation.

  1. Metal halide salts, like PbI2_2, when being solvated in DMSO, donate Pb2+^{2+} ions to adsorb onto Ti3_3C2_2Tx_x surface through =O (or –OH) terminations, and promote the oxidation of MXenes. These important finding suggests, for example, that it is not recommended to use the two-step fabrication process for HaP[71], where PbI2_2 is deposited first from a polar aprotic solvent (incl. DMSO), followed by exposure to MAI. While HaP preparation immediately after admixing MXenes into the metal halide precursor can still be implemented, long-term storage of such inks will likely change the content of the ink over time, and with it the quality of the deposited film. Since the proposed mechanism closely resembles MXene-mediated heavy metal adsorption from the aquatic environment, we expect similar mechanisms when other metal salts

are being used, such as Cu- or Sn-based ones. We predict similar behavior also for monovalent metals, such as Cs, which can be used as an A-site cation for some HaPs, although this hypothesis is left to be proved.

  1. Clearly, the addition of free halides, such as I2\mathrm{I}_2, into MXene-containing HaP-inks triggers the rapid degradation of the Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x phase. Halide molecules attack the defect sites on MXene basal planes of edges, causing fast redox reaction with the formation of I−\mathrm{I}^{-}, and further polyiodides, and Ti oxidation to Ti4+\mathrm{Ti}^{4+}. Although competitive species, such as MAI or PbI2\mathrm{PbI}_2, may impede this process through blocking available sites, the reaction inevitably propagates, leading to severe Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x MXene degradation. Thus, further researchers should avoid preparing such solutions in their work, and should take into account the possible formation of polyhalides due to improper storage conditions (the access of light should be minimized).

  1. Despite the potential degradation, it was encouraging to find that Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x MXene surface chemistry strongly depends on a sequence of HaP-precursor addition within a HaP-ink. For example, a simultaneous exposure to both MAI and PbI2\mathrm{PbI}_2 will result in the preferable adsorption of Pb species onto Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x surface, while preliminary exposure to MAI will enrich the adsorption sites with MAI species, blocking further Pb adsorption. The ability to construct chemically-defined Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x-Pb and Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x-MAI surfaces prior to actual HaP crystallization allows us to effectively control and tune MXene-HaP interaction. The effect of such chemical control over MXene-HaP interfaces on morphological, chemical and optoelectronic properties of the resulting bulk composites is the main topic of our ongoing research.

  1. Last, but not least our evidence shows that –F, =O or –OH termination groups have a different interaction nature or interaction power with the additives, and play an important role in both the activity of MXenes and their role in MXene-HaP composites. By understanding this, now one may, for example, engineer MXene-HaP interaction from very strong, with a predominant =O or –OH termination of Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x surface, to relatively weak, if the MXenes are enriched with –F terminations. Preparing such MXenes using known protocols[103, 136], and studying their properties upon HaP-ink exposure is our plan for the future research.

Given this fundamental understanding, we can suggest that commonly applied steps, such as storing the inks refrigerated, and in low oxygen/humidity conditions (e.g., glovebox)[137, 138], should minimize their degradation, although the above mentioned reactions will still take place. We strictly suggest using the most well-optimized MXene synthesis protocols[85, 86], to minimize the defectiveness of the obtained flakes, which act as active sites and increase their susceptibility to degradation. We found that the reported processes are strongly solvent-dependent, so a follow-up study focused on Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2T_x MXene stability and surface chemistry evolution in various HaP-relevant solvents (DMF, GBL, acetonitrile, etc.) is a necessity.

This research establishes the understanding that MXenes have a variety of degrees of freedom that directly impact their state, thus cannot be overlooked or can be harnessed to engineer their integration. Overall, it is clear that when it comes to the integration of MXenes with HaPs, we have to take into account that what we add is not what we finally have in our layer – not because of the solvent, but because of the precursors. To this end, also the sequence at which we add MXenes and the duration we hold them in the solution play a role in defining their chemical state – both at the level of the Ti-oxidation and the identity of the termination groups chemistry. These findings put in doubt past research that completely overlooked these points, and provide a critical view on how MXene integration, in general, should be perceived.

Acknowledgments

K.S. thanks Dr. Natalia Froumin for the assistance in XPS data analysis and interpretation.

Y.R. and T.G.M. acknowledge the Ministry of Energy, Israel, Grant #223-11-057, for their support in this project.

T.G.M. acknowledges funding from the Ministry of Innovation, Science and Technology, Israel, Grant #5802.

Supporting Information

Supplementary Methods

To analyze the thicknesses and lateral dimensions of as-cast Ti3_3C2Tx_2T_x MXene flakes we used CoreAFM Atomic Force Microscope (Nanosurf, Liestal, Switzerland). For this, small amounts of MXene powders were dispersed in the AR-grade dehydrated ethanol (30 minutes sonication in an ice bath at 37 kHz was used to achieve homogeneous colloidal dispersions), then drop-cased onto flat Si substrates and analyzed in a semi-contact mode after drying.

We exploited IKI Zeiss LSM880 Confocal Laser Scanning Microscope (Zeiss, Oberkochen, Germany) as a specific tool to observe the volume of the inks that were drop-casted onto the glass slide and sandwiched between two slides, without the necessity to filter them or do any other modification.

FTIR spectra were acquired from KBr + Ti3_3C2Tx_2T_x MXene (or annealed Ti3_3C2Tx_2T_x) pellets using a Nicolet Impact 410 spectrophotometer (Nicolet, USA). The measurements were performed in the spectral range from 400 to 4000 cm−1^{-1} with a step size of 7.7 cm−1^{-1}, all the spectra were automatically background-corrected.

NMR measurements were performed on a 11.7 Tesla, Bruker AVANCE III spectrometer using a 5 mm BBFO probe with a 500.08 MHz 1^{1}H Larmor frequency. The samples were measured under deuterium locking and shimmed manually on the reference sample, which subsequently related any residual inhomogeneity to the particle organization in the Ti3_3C2Tx_2T_x MXene-containing sample. The 1^{1}H longitudinal and transverse relaxation rates for each sample were measured using inversion recovery (IR) and Carr-Purcell-Meiboom-Gill (CPMG) experiments, respectively. The spectra were acquired with a relaxation delay equal to 5 times T1_1 to ensure steady state quantitative measurements, with a 9 μ\mus pulse (calibrated with respect to a 90° flip angle) and 16 scans. Bruker Topspin software was used for initial spectral processing, followed by signal integration and plotting in MATLAB (R2023B).

For NMR measurements, the sample containing 1M methylammonium iodide (MAI) in 0.5 mg mL−1^{-1} Ti3_3C2_2Tx_x MXene dispersion in DMSO-d6_6 was prepared by mixing equal parts of 2M MAI stock solution and 1 mg mL−1^{-1} MXene dispersion in DMSO-d6_6, the mixing continued overnight for stabilization. For the reference sample, the 2M MAI stock solution was diluted with the equal part of DMSO-d6_6. Sample preparation and packing of the NMR tube were performed in an Ar-filled glovebox (O2_2, H2_2O < 0.5 ppm). A sealed capillary containing Benzene-D6_6 (Sigma Aldrich, 99.5%) was placed inside the NMR tube as a non-interacting chemical shift reference.

Section SA

HF-MXenes synthesis

For the HF-based etching reaction[1], 1 g of the precursor Ti3AlC2\mathrm{Ti}_{3}\mathrm{Al}\mathrm{C}_{2} was added into 5 wt.% solution of HF in DDW and stirred for 24 hours at room temperature. When the reaction was finished, the pH was neutralized (pH >5> 5) through 8 centrifugation cycles at 3500 rpm for 5 min each. After washing, the supernatant was vacuum-filtered through the polyvinylidene difluoride (PVDF) membrane with 0.22 μm\mu\mathrm{m} pore size to collect Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} multilayered particles, natural for this preparation method. The membrane with the material dried and stored in a vacuumized desiccator.

Section SB

Validation of as-cast Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes: XRD ana Raman analysis

Powder XRD and Raman validated the synthesis of a desired Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXene phase. In Error! Reference source not found.a we see the XRD pattern showing the characteristic (002) peak at 6.53°, which is shifted from the (002) Ti3AlC2\mathrm{Ti}_{3}\mathrm{Al}\mathrm{C}_{2} MAX phase at 9.5°. The shift to smaller angles and broadening indicates the expansion of the interlayer spacing during etching, delamination, and functional group attachment[2]. Raman spectrum, provided in Error! Reference source not found.b, is also rather typical for Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes[3], showing the common vibrations for delaminated MXenes. The vibrations around 200 cm−1\mathrm{cm}^{-1} consist of EgE_g (Ti, C, O) and A1gA_{1g} (Ti, C, O), which are the in-plane and out-of-plane vibrations of titanium atoms at the outer interfaces of the flakes, as well as carbon and surface termination groups, respectively. The region between 580–730 cm−1\mathrm{cm}^{-1} is assigned mainly to carbon vibrations (both EgE_g and A1gA_{1g})[4]. The region of 230–470 cm−1\mathrm{cm}^{-1} represents in-plane vibration (EgE_g) of functional groups attached to titanium atoms.

Section SC

Validation of as-cast HF-Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes

Results of the complex initial characterization of as-cast HF-Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes[1] are given in Figure S1. Briefly, the provided characterization proves sufficient quality of the prepared materials. XRD pattern of HF-MXenes (Figure S1) possesses repeating (002)-(004)-(006)-(008) reflections, because, unlike milder protocols that yield single- or few-flake MXene clays (see Figure 2a[5]), HF etching yields stacked multilayer MXene particles[1]. Raman spectrum (Figure S1) is very similar to what is provided in Figure 2b[3, 4], and does not indicate any extra phases. A shift for the A1gA_{1g} of titanium indicates increased stiffness for the titanium environment and can result from a different assembly or oxidation[3, 4]. Ti2p\mathrm{Ti}_{2p}, C1s\mathrm{C}_{1s}, O1s\mathrm{O}_{1s} and F1s\mathrm{F}_{1s} XPS spectra (Figure S1,Figure S1) were deconvoluted similarly to what is described in § 3.1 of the main text[6]. We can note slightly richer –F functionalization of HF-MXenes with respect to the regular ones, as well as the slight over-oxidation of the product (C-C carbon and TiO2−xF2x\mathrm{TiO}_{2-x}\mathrm{F}_{2x} signals arising), resulting from the harsher etching environment.

Section SD

XRD and TEM-SAED analysis of precipitates from ink 4-MPI

XRD analysis of precipitants from ink 4-MPI, given in Figure S13, reveals that initially they possess very complex structure, which most likely contains solvent molecules involved[7]. Thus, after drying the precipitate at 140°C for several minutes, we observed only reflections originating from PbI2\mathrm{PbI_2} and MAPbI3\mathrm{MAPbI_3} phases. Precipitants from ink 4-MPI were also deposited onto a grid and analyzed by TEM, the respective images and the varying-tilt SAED patterns are given in Figure S13. Precipitant particles show quite pronounced hexagon-shape core with randomly oriented needles at the periphery. We used varying-tilt ED measurements to confirm the crystal structure of the core, which turned out to be PbI2\mathrm{PbI_2}. The same experiment for the needles turned out to be rather challenging, as they were found to rapidly decompose and change morphology under the electron beam. We assume them to be MAPbI3\mathrm{MAPbI_3} perovskite due to the initial composition of the ink, particle shape, and the illumination-sensitive behavior[8], which confirms our assumptions from the XRD analysis The reason behind spontaneous precipitant formation in ink 4-MPI could be that in its complex chemical environment MAI is partially blocked by iodine, as suggested from Raman analysis, which promotes PbI2\mathrm{PbI_2} nucleation. The interior of PbI2\mathrm{PbI_2} particles reacts with MAI, leading to MAPbI3\mathrm{MAPbI_3} formation and growth. Ti3C2Tx\mathrm{Ti_3C_2T_x} presence here simply provides more available sites for lead iodide nucleation, as MXenes were shown to strongly adsorb Pb. As this solution does not transmit light above 780 nm, unlike its Ti3C2Tx\mathrm{Ti_3C_2T_x}-free counterpart (see Figure S10 and Figure 7d), we assume MXene flakes survive in the core of the observed particles, as they are protected from the aggressive halide environment by the surrounding particle.

a. MAI; =O terminated Ti3C2Tx surface; –F terminated Ti3C2Tx surface; –OH terminated Ti3C2Tx surface; Bare Ti3C2Tx surface

Figure 9 (PDF p. 45). a. MAI. =O terminated Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_x surface; –F terminated Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_x surface; –OH terminated Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_x surface; Bare Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}T_x surface.

Structural models of PbI$_2$ on Ti$_3$C$_2T_x$ surfaces

Figure b.

Figure c.

bare=O–F–OHmixed O/F
Outer Ti11.125610.581210.723810.757110.6442
Tx_x group-6.74687.55350.62616.753
after MAI adsorption
Outer Ti11.068810.583110.725410.752910.6468
difference0.0568-0.0019-0.00160.0042-0.0026
Tx_x group-6.80657.57240.64336.8099
difference--0.0597-0.0189-0.0172-0.0569
after Pb2+^{2+} adsorption
Outer Ti11.04810.578510.716810.7510.6414
difference0.07760.00270.0070.00710.0028
Tx_x group-6.81917.56530.68226.8458
difference--0.0723-0.0118-0.0561-0.0928

Table S-T1. Calculated electrical charge values (in the units of elemental charge) for outer Ti atoms (atoms bonded to termination groups) and TxT_x groups of: bare (no termination groups attached), pure =O, pure –F, pure –OH, and mixed O/F (in 1 : 1 ratio) terminated Ti3_3C2Tx_2T_x MXenes before and after MAI, and Pb2+^{2+} adsorption. The difference in charge due to adsorption is given below each respective line, where a negative sign corresponds to electron acceptance, and a positive – to electron donation. Significant values are highlighted in bold. Values for the inner Ti and C atoms are not given here, as they were found unaffected by the adsorption.

UPS spectra and valence band regions for Ti₃C₂Tₓ MXenes with MAI- and PbI₂-based species adsorbed on their surface

Figure S5. UPS work function evaluation for Ti3C2Tx\mathrm{Ti_3C_2T_x} MXenes with MAI- and PbI2\mathrm{PbI_2}-based species adsorbed on their surface: (a) complete UPS spectra for Ti3C2Tx\mathrm{Ti_3C_2T_x} MXenes extracted from inks 1-sol, 2-M and 7-P after 1 hour of exposure; the secondary electron cutoff region and its linear fitting is highlighted in the insert; (b) zoomed-in valence band region and its linear fitting for the UPS spectra given in (a).

1H^{1}\mathrm{H} relaxation ratesR1R_{1} (s−1\mathrm{s}^{-1})R2R_{2} (s−1\mathrm{s}^{-1})
CH3\mathrm{CH}_{3}NH3\mathrm{NH}_{3}CH3\mathrm{CH}_{3}NH3\mathrm{NH}_{3}
1M MAI in DMSO-d6d_{6}0.394 ± 0.0031.05 ± 0.010.43 ± 0.027.1 ± 0.1
1M MAI in DMSO-d6d_{6} + Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x}0.368 ± 0.0040.99 ± 0.010.45 ± 0.027.1 ± 0.2
ΔR2\Delta R_{2} (with Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes – without)--0.02 ± 0.030 ± 0.2

Table S-T2. 1H^{1}\mathrm{H} relaxation rates for CH3\mathrm{CH}_{3} and NH4\mathrm{NH}_{4} NMR spectra of 1M ink 2-M-type solutions with deuterated DMSO (DMSO-d6d_{6}), with and without Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXenes.

Area NumberTi (at. %)Pb (at. %)
166.533.5
250.149.9
350.249.8

Table S7.

Supplementary Reference List

  1. Alhabeb, M.; Maleski, K.; Anasori, B.; Lelyukh, P.; Clark, L.; Sin, S.; Gogotsi, Y. Guidelines for Synthesis and Processing of Two-Dimensional Titanium Carbide (Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXene). Chem. Mater. 2017, 29 (18), 7633–7644. https://doi.org/10.1021/acs.chemmater.7b02847.

  1. Shekhirev, M.; Shuck, C. E.; Sarycheva, A.; Gogotsi, Y. Characterization of MXenes at Every Step, from Their Precursors to Single Flakes and Assembled Films. Progress in Materials Science 2021, 120, 100757. https://doi.org/10.1016/j.pmatsci.2020.100757.

  1. Berger, E.; Lv, Z.-P.; Komsa, H.-P. Raman Spectra of 2D Titanium Carbide MXene from Machine-Learning Force Field Molecular Dynamics. J. Mater. Chem. C 2023, 11 (4), 1311–1319. https://doi.org/10.1039/D2TC04374B.

  1. Sarycheva, A.; Gogotsi, Y. Raman Spectroscopy Analysis of the Structure and Surface Chemistry of Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXene. Chem. Mater. 2020, 32 (8), 3480–3488. https://doi.org/10.1021/acs.chemmater.0c00359.

  1. Thakur, A.; Chandran B.S., N.; Davidson, K.; Bedford, A.; Fang, H.; Im, Y.; Kanduri, V.; Wyatt, B. C.; Nemani, S. K.; Poliukhova, V.; Kumar, R.; Fakhraai, Z.; Anasori, B. Step-by-Step Guide for Synthesis and Delamination of Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXene. Small Methods 2023, 7 (8), 2300030. https://doi.org/10.1002/smtd.202300030.

  1. Natu, V.; Benchakar, M.; Canaff, C.; Habrioux, A.; Célérier, S.; Barsoum, M. W. A Critical Analysis of the X-Ray Photoelectron Spectra of Ti3C2Tz\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{z} MXenes. Matter 2021, 4 (4), 1224–1251. https://doi.org/10.1016/j.matt.2021.01.015.

  1. Lee, S. J.; Heo, J. H.; Im, S. H. Large-Scale Synthesis of Uniform PbI2(DMSO)\mathrm{PbI}_{2}(\mathrm{DMSO}) Complex Powder by Solvent Extraction Method for Efficient Metal Halide Perovskite Solar Cells. ACS Appl. Mater. Interfaces 2020, 12 (7), 8233–8239. https://doi.org/10.1021/acsami.9b20493.

  1. Li, Y.; Zhou, W.; Li, Y.; Huang, W.; Zhang, Z.; Chen, G.; Wang, H.; Wu, G.-H.; Rolston, N.; Vila, R.; Chiu, W.; Cui, Y. Unravelling Degradation Mechanisms and Atomic Structure of Organic-Inorganic Halide Perovskites by Cryo-EM. Joule 2019, 3 (11), 2854–2866. https://doi.org/10.1016/j.joule.2019.08.016.

  1. Li, M.; Dong, X.; Li, Q.; Liu, Y.; Cao, S.; Hou, C.-C.; Sun, T. Engineering MXene Surface via Oxygen Functionalization and Au Nanoparticle Deposition for Enhanced Electrocatalytic Hydrogen Evolution Reaction. Small Methods 2025, 9 (4), 2401569. https://doi.org/10.1002/smtd.202401569.

  1. Liu, Z.; Lv, H.; Xie, Y.; Wang, J.; Fan, J.; Sun, B.; Jiang, L.; Zhang, Y.; Wang, R.; Shi, K. A 2D/2D/2D Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} @ TiO2\mathrm{TiO}_{2} @ MoS2\mathrm{MoS}_{2} Heterostructure as an Ultrafast and High-Sensitivity NO2\mathrm{NO}_{2} Gas Sensor at Room-Temperature. J. Mater. Chem. A 2022, 10 (22), 11980–11989. https://doi.org/10.1039/D1TA09369J.

References

  1. [1]2D Metal Carbides and Nitrides (MXenes): Structure, Properties and Applications; Anasori, B., Gogotsi, Y., Eds.; Springer International Publishing: Cham, 2019. https://doi.org/10.1007/978-3-030-19026-2
  2. [2]Natu, V.; Barsoum, M. W. MXene Surface Terminations: A Perspective. J. Phys. Chem. C 2023, 127 (41), 20197–20206. https://doi.org/10.1021/acs.jpcc.3c04324
  3. [3]Naguib, M.; Kurtoglu, M.; Presser, V.; Lu, J.; Niu, J.; Heon, M.; Hultman, L.; Gogotsi, Y.; Barsoum, M. W. Two-Dimensional Nanocrystals Produced by Exfoliation of Ti3AlC2. Advanced Materials 2011, 23 (37), 4248–4253. https://doi.org/10.1002/adma.201102306
  4. [4]Ren, C. E.; Zhao, M.-Q.; Makaryan, T.; Halim, J.; Boota, M.; Kota, S.; Anasori, B.; Barsoum, M. W.; Gogotsi, Y. Porous Two-Dimensional Transition Metal Carbide (MXene) Flakes for High-Performance Li-Ion Storage. ChemElectroChem 2016, 3 (5), 689–693. https://doi.org/10.1002/celc.201600059
  5. [5]Wu, C.; Huang, C.; Zhang, Z.; Xie, Y.; Gao, Z.; Wang, H. Bulk Ti3C2Tx Anodes for Superior Sodium Storage Performance: The Unique Role of O-Termination. Mater. Chem. Front. 2021, 5 (6), 2810–2823. https://doi.org/10.1039/D0QM01073A
  6. [6]MXenes for Rechargeable Batteries Beyond the Lithium-Ion - Ming - 2021 - Advanced Materials - Wiley Online Library. https://onlinelibrary.wiley.com/doi/full/10.1002/adma.202004039 (accessed 2024-12-17)DOI
  7. [7]Soni, V.; Singh, P.; Phan Quang, H. H.; Parwaz Khan, A. A.; Bajpai, A.; Van Le, Q.; Thakur, V. K.; Thakur, S.; Nguyen, V.-H.; Raizada, P. Emerging Architecture Titanium Carbide (Ti3C2Tx) MXene Based Photocatalyst toward Degradation of Hazardous Pollutants: Recent Progress and Perspectives. Chemosphere 2022, 293, 133541. https://doi.org/10.1016/j.chemosphere.2022.133541
  8. [8]Lim, S.; Kim, J. H.; Park, H.; Kwak, C.; Yang, J.; Kim, J.; Ryu, S. Y.; Lee, J. Role of Electrostatic Interactions in the Adsorption of Dye Molecules by Ti3C2-MXenes. RSC Adv. 2021, 11 (11), 6201–6211. https://doi.org/10.1039/D0RA10876F
  9. [9]Abdolhosseinzadeh, S.; Schneider, R.; Jafarpour, M.; Merlet, C.; Nüesch, F.; Zhang, C. (John); Heier, J. MXene Inks for High-Throughput Printing of Electronics. Advanced Electronic Materials n/a (n/a), 2400170. https://doi.org/10.1002/aelm.202400170
  10. [10]Luo, Y.; Que, W.; Bin, X.; Xia, C.; Kong, B.; Gao, B.; Kong, L. B. Flexible MXene-Based Composite Films: Synthesis, Modification, and Applications as Electrodes of Supercapacitors. Small 2022, 18 (27), 2201290. https://doi.org/10.1002/smll.202201290
  11. [11]Pazniak, H.; Varezhn­ikov, A. S.; Kolosov, D. A.; Plugin, I. A.; Vito, A. D.; Glukhova, O. E.; Sheverdyaeva, P. M.; Spasova, M.; Kaikov, I.; Kolesnikov, E. A.; Moras, P.; Bainyashev, A. M.; Solomatin, M. A.; Kiselev, I.; Wiedwald, U.; Sysoev, V. V. 2D Molybdenum Carbide MXenes for Enhanced Selective Detection of Humidity in Air. Advanced Materials 2021, 33 (52), 2104878. https://doi.org/10.1002/adma.202104878
  12. [12]Wu, M.; An, Y.; Yang, R.; Tao, Z.; Xia, Q.; Hu, Q.; Li, M.; Chen, K.; Zhang, Z.; Huang, Q.; Ma, S.; Zhou, A. V2CTx and Ti3C2Tx MXenes Nanosheets for Gas Sensing. ACS Appl. Nano Mater. 2021, 4 (6), 6257–6268. https://doi.org/10.1021/acsanm.1c01059
  13. [13]Lu, H.; Wang, J.; Li, H.; Zhou, W.; Yuan, Q.; Liu, S. Efficient Photothermal Conversion of MXenes and Their Application in Biomedicine. Mater. Chem. Front. 2023, 7 (19), 4372–4399. https://doi.org/10.1039/D3QM00220A
  14. [14]Sundaram, A.; Ponraj, J. S.; Wang, C.; Peng, W. K.; Manavalan, R. K.; Dhanabalan, S. C.; Zhang, H.; Gaspar, J. Engineering of 2D Transition Metal Carbides and Nitrides MXenes for Cancer Therapeutics and Diagnostics. J. Mater. Chem. B 2020, 8 (23), 4990–5013. https://doi.org/10.1039/D0TB00251H
  15. [15]Lipatov, A.; Goad, A.; Loes, M. J.; Vorobeva, N. S.; Abourahma, J.; Gogotsi, Y.; Sinitskii, A. High Electrical Conductivity and Breakdown Current Density of Individual Monolayer Ti3C2Tx MXene Flakes. Matter 2021, 4 (4), 1413–1427. https://doi.org/10.1016/j.matt.2021.01.021
  16. [16]Maleski, K.; Mochalin, V. N.; Gogotsi, Y. Dispersions of Two-Dimensional Titanium Carbide MXene in Organic Solvents. Chem. Mater. 2017, 29 (4), 1632–1640. https://doi.org/10.1021/acs.chemmater.6b04830
  17. [17]Zhang, B.; Wong, P. W.; Guo, J.; Zhou, Y.; Wang, Y.; Sun, J.; Jiang, M.; Wang, Z.; An, A. K. Transforming Ti3C2Tx MXene’s Intrinsic Hydrophilicity into Superhydrophobicity for Efficient Photothermal Membrane Desalination. Nat Commun 2022, 13 (1), 3315. https://doi.org/10.1038/s41467-022-31028-6
  18. [18]Ronchi, R. M.; Marchiori, C. F. N.; Araujo, C. M.; Arantes, J. T.; Santos, S. F. Thermoplastic Polyurethane – Ti3C2(Tx) MXene Nanocomposite: The Influence of Functional Groups upon the Matrix–Reinforcement Interaction. Applied Surface Science 2020, 528, 146526. https://doi.org/10.1016/j.apsusc.2020.146526
  19. [19]Lee, J. T.; Wyatt, B. C.; Davis, G. A. Jr.; Masterson, A. N.; Pagan, A. L.; Shah, A.; Anasori, B.; Sardar, R. Covalent Surface Modification of Ti3C2Tx MXene with Chemically Active Polymer Ligands Producing Highly Conductive and Ordered Microstructure Films. ACS Nano 2021, 15 (12), 19600–19612. https://doi.org/10.1021/acsnano.1c06670
  20. [20]Zhu, S.; Wang, C.; Shou, H.; Zhang, P.; Wan, P.; Guo, X.; Yu, Z.; Wang, W.; Chen, S.; Chu, W.; Song, L. In Situ Architecting Endogenous Heterojunction of MoS2 Coupling with Mo2CT MXenes for Optimized Li+ Storage. Advanced Materials 2022, 34 (5), 2108809. https://doi.org/10.1002/adma.202108809
  21. [21]Li, X.; Yin, X.; Han, M.; Song, C.; Xu, H.; Hou, Z.; Zhang, L.; Cheng, L. Ti3C2 MXenes Modified with in Situ Grown Carbon Nanotubes for Enhanced Electromagnetic Wave Absorption Properties. J. Mater. Chem. C 2017, 5 (16), 4068–4074. https://doi.org/10.1039/C6TC05226F
  22. [22]Zhao, C.; Wang, Q.; Zhang, H.; Passerini, S.; Qian, X. Two-Dimensional Titanium Carbide/RGO Composite for High-Performance Supercapacitors. ACS Appl. Mater. Interfaces 2016, 8 (24), 15661–15667. https://doi.org/10.1021/acsami.6b04767
  23. [23]Qiu, X.; Dai, L.; Li, H.; Qu, K.; Li, R. Pillaring Behavior of Organic Molecules on MXene: Insights from Molecular Dynamics Simulations. Langmuir 2023, 39 (42), 14912–14921. https://doi.org/10.1021/acs.langmuir.3c01682
  24. [24]Mozafari, M.; Soroush, M. Surface Functionalization of MXenes. Mater. Adv. 2021, 2 (22), 7277–7307. https://doi.org/10.1039/D1MA00625H
  25. [25]Qamar, S.; Fatima, K.; Ullah, N.; Akhter, Z.; Waseem, A.; Sultan, M. Recent Progress in Use of MXene in Perovskite Solar Cells: For Interfacial Modification, Work-Function Tuning and Additive Engineering. Nanoscale 2022, 14 (36), 13018–13039. https://doi.org/10.1039/D2NR02799B
  26. [26]Lin, H.; Yang, M.; Ru, X.; Wang, G.; Yin, S.; Peng, F.; Hong, C.; Qu, M.; Lu, J.; Fang, L.; Han, C.; Procel, P.; Isabella, O.; Gao, P.; Li, Z.; Xu, X. Silicon Heterojunction Solar Cells with up to 26.81% Efficiency Achieved by Electrically Optimized Nanocrystalline-Silicon Hole Contact Layers. Nat Energy 2023, 8 (8), 789–799. https://doi.org/10.1038/s41560-023-01255-2
  27. [27]Park, N.-G.; Segawa, H. Research Direction toward Theoretical Efficiency in Perovskite Solar Cells. ACS Photonics 2018, 5 (8), 2970–2977. https://doi.org/10.1021/acsphotonics.8b00124
  28. [28]Green, M. A.; Dunlop, E. D.; Yoshita, M.; Kopidakis, N.; Bothe, K.; Siefer, G.; Hao, X.; Jiang, J. Y. Solar Cell Efficiency Tables (Version 65). Progress in Photovoltaics: Research and Applications 2025, 33 (1), 3–15. https://doi.org/10.1002/pip.3867
  29. [29]Min, H.; Lee, D. Y.; Kim, J.; Kim, G.; Lee, K. S.; Kim, J.; Paik, M. J.; Kim, Y. K.; Kim, K. S.; Kim, M. G.; Shin, T. J.; Il Seok, S. Perovskite Solar Cells with Atomically Coherent Interlayers on SnO2 Electrodes. Nature 2021, 598 (7881), 444–450. https://doi.org/10.1038/s41586-021-03964-8
  30. [30]Chouhan, L.; Ghimire, S.; Subrahmanyam, C.; Miyasaka, T.; Biju, V. Synthesis, Optoelectronic Properties and Applications of Halide Perovskites. Chem. Soc. Rev. 2020, 49 (10), 2869–2885. https://doi.org/10.1039/C9CS00848A
  31. [31]Mitzi, D. B. Synthesis, Structure, and Properties of Organic-Inorganic Perovskites and Related Materials. In Progress in Inorganic Chemistry; John Wiley & Sons, Ltd, 1999; pp 1–121. https://doi.org/10.1002/9780470166499.ch1
  32. [32]Bisquert, J. Interpretation of the Recombination Lifetime in Halide Perovskite Devices by Correlated Techniques. J. Phys. Chem. Lett. 2022, 13 (31), 7320–7335. https://doi.org/10.1021/acs.jpclett.2c01776
  33. [33]Jiang, J.; Sun, X.; Chen, X.; Wang, B.; Chen, Z.; Hu, Y.; Guo, Y.; Zhang, L.; Ma, Y.; Gao, L.; Zheng, F.; Jin, L.; Chen, M.; Ma, Z.; Zhou, Y.; Pad­ture, N. P.; Beach, K.; Terrones, H.; Shi, Y.; Gall, D.; Lu, T.-M.; Wertz, E.; Feng, J.; Shi, J. Carrier Lifetime Enhancement in Halide Perovskite via Remote Epitaxy. Nat Commun 2019, 10 (1), 4145. https://doi.org/10.1038/s41467-019-12056-1
  34. [34]Rakita, Y.; Lubomirsky, I.; Cahen, D. When Defects Become ‘Dynamic’: Halide Perovskites: A New Window on Materials? Mater. Horiz. 2019, 6 (7), 1297–1305. https://doi.org/10.1039/C9MH00606K
  35. [35]Ceratti, D. R.; Rakita, Y.; Cremonesi, L.; Tenne, R.; Kalchenko, V.; Elbaum, M.; Oron, D.; Potenza, M. A. C.; Hodes, G.; Cahen, D. Self-Healing Inside APbBr3 Halide Perovskite Crystals. Advanced Materials 2018, 30 (10), 1706273. https://doi.org/10.1002/adma.201706273
  36. [36]Cahen, D.; Kronik, L.; Hodes, G. Are Defects in Lead-Halide Perovskites Healed, Tolerated, or Both? ACS Energy Lett. 2021, 6 (11), 4108–4114. https://doi.org/10.1021/acsenergylett.1c02027
  37. [37]Lim, J.; Kober-Czerny, M.; Lin, Y.-H.; Ball, J. M.; Sakai, N.; Duijnstee, E. A.; Hong, M. J.; Labram, J. G.; Wenger, B.; Snaith, H. J. Long-Range Charge Carrier Mobility in Metal Halide Perovskite Thin-Films and Single Crystals via Transient Photo-Conductivity. Nat Commun 2022, 13 (1), 4201. https://doi.org/10.1038/s41467-022-31569-w
  38. [38]Cahen, D.; Rakita, Y.; Egger, D. A.; Kahn, A. Surface Defects Control Bulk Carrier Densities in Polycrystalline Pb-Halide Perovskites. Advanced Materials 2024, 36 (50), 2407098. https://doi.org/10.1002/adma.202407098
  39. [39]Zheng, D.; Raffin, F.; Volovitch, P.; Pauporté, T. Control of Perovskite Film Crystallization and Growth Direction to Target Homogeneous Monolithic Structures. Nat Commun 2022, 13 (1), 6655. https://doi.org/10.1038/s41467-022-34332-3
  40. [40]Mathies, F.; List-Kratochvil, E. J. W.; Unger, E. L. Advances in Inkjet-Printed Metal Halide Perovskite Photovoltaic and Optoelectronic Devices. Energy Technology 2020, 8 (4), 1900091. https://doi.org/10.1002/ente.201900991
  41. [41]Misra, R. K.; Aharon, S.; Li, B.; Mogilyansky, D.; Visoly-Fisher, I.; Etgar, L.; Katz, E. A. Temperature- and Component-Dependent Degradation of Perovskite Photovoltaic Materials under Concentrated Sunlight. J. Phys. Chem. Lett. 2015, 6 (3), 326–330. https://doi.org/10.1021/jz502642b
  42. [42]Aristidou, N.; Sanchez-Molina, I.; Chotchuangchutchaval, T.; Brown, M.; Martinez, L.; Rath, T.; Haque, S. A. The Role of Oxygen in the Degradation of Methylammonium Lead Trihalide Perovskite Photoactive Layers. Angewandte Chemie International Edition 2015, 54 (28), 8208–8212. https://doi.org/10.1002/anie.201503153
  43. [43]Chu, Q.-Q.; Sun, Z.; Wang, D.; Cheng, B.; Wang, H.; Wong, C.-P.; Fang, B. Encapsulation: The Path to Commercialization of Stable Perovskite Solar Cells. Matter 2023, 6 (11), 3838–3863. https://doi.org/10.1016/j.matt.2023.08.016
  44. [44]Bisquert, J.; Guerrero, A.; Gonzales, C. Theory of Hysteresis in Halide Perovskites by Integration of the Equivalent Circuit. ACS Phys. Chem Au 2021, 1 (1), 25–44. https://doi.org/10.1021/acsphyschemau.1c00009
  45. [45]Guo, Z.; Gao, L.; Xu, Z.; Teo, S.; Zhang, C.; Kamata, Y.; Hayase, S.; Ma, T. High Electrical Conductivity 2D MXene Serves as Additive of Perovskite for Efficient Solar Cells. Small 2018, 14 (47), 1802738. https://doi.org/10.1002/smll.201802738
  46. [46]Song, Y.; Cong, J.; Yu, W.; Jiang, H.; Zhang, L.; Wang, Y.; Lu, M.; Wang, F.; Fan, L.; Liu, X.; Wei, M.; Yang, L.; Yang, N. Functionalized MXene Nanosheets for Buried Interface Double-Sided Engineering to Achieve Efficient Perovskite Solar Cells. Electrochimica Acta 2024, 497, 144584. https://doi.org/10.1016/j.electacta.2024.144584
  47. [47]Wu, C.; Fang, W.; Cheng, Q.; Wan, J.; Wen, R.; Wang, Y.; Song, Y.; Li, M. MXene-Regulated Perovskite Vertical Growth for High-Performance Solar Cells. Angewandte Chemie International Edition 2022, 61 (43), e202210970. https://doi.org/10.1002/anie.202210970
  48. [48]Agresti, A.; Pazniak, A.; Pescetelli, S.; Di Vito, A.; Rossi, D.; Pecchia, A.; Auf der Maur, M.; Liedl, A.; Larciprete, R.; Kuznetsov, D. V.; Saranin, D.; Di Carlo, A. Titanium-Carbide MXenes for Work Function and Interface Engineering in Perovskite Solar Cells. Nat. Mater. 2019, 18 (11), 1228–1234. https://doi.org/10.1038/s41563-019-0478-1
  49. [49]Tian, C.; Yan, Y.; Feng, S.; Wang, J.; Niu, Y.; Li, X.; Ju, H.; Xu, Q.; Huang, Y.; Dong, H.; Liang, Z.; Dong, B.; Li, L.; Yang, Y. An Effective Modulation of Bulk Perovskite by V2CTx Nanosheets for Efficient Planar Perovskite Solar Cells. J. Mater. Chem. A 2023, 11 (10), 5015–5026. https://doi.org/10.1039/D2TA05836G
  50. [50]Single-Layered MXene Nanosheets Doping TiO2 for Efficient and Stable Double Perovskite Solar Cells / Journal of the American Chemical Society. https://pubs.acs.org/doi/full/10.1021/jacs.0c12739 (accessed 2026-07-16)
  51. [51]CsPbBr3 Perovskite Nanocrystal Grown on MXene Nanosheets for Enhanced Photoelectric Detection and Photocatalytic CO2 Reduction / The Journal of Physical Chemistry Letters. https://pubs.acs.org/doi/full/10.1021/acs.jpclett.9b02605 (accessed 2026-07-16)
  52. [52]Ansari, R. M.; Yadav, A.; Singh, S.; Irziqat, B.; Aivalioti, C.; Zhou, R.; Abulikemu, M.; Azam, A.; Fatayer, S.; Ahmad, S. Additive Engineering of Ruddlesden–Popper Perovskites with MXene Nanoflakes: Toward Enhanced Photoresponsivity, Detectivity, and Stability. ACS Materials Lett. 2025, 7 (6), 2115–2124. https://doi.org/10.1021/acs材料ialslett.4c02691
  53. [53]Di Vito, A.; Pecchia, A.; Auf der Maur, M.; Di Carlo, A. Nonlinear Work Function Tuning of Lead-Halide Perovskites by MXenes with Mixed Terminations. Advanced Functional Materials 2020, 30 (47), 1909028. https://doi.org/10.1002/adfm.201909028
  54. [54]El-Demellawi, J. K.; Mansour, A. E.; El-Zohry, A. M.; Hedhili, M. N.; Yin, J.; Emwas, A.-H. M.; Maity, P.; Xu, X.; Bakr, O. M.; Mohammed, O. F.; Alshareef, H. N. Tuning the Work Function of Ti3C2Tx MXene by Molecular Doping without Changing Its Surface Functional Groups. ACS Materials Lett. 2022, 4 (12), 2480–2490. https://doi.org/10.1021/acs materialeslett.2c00796
  55. [55]Palei, S.; Murali, G.; Kim, C.-H.; In, I.; Lee, S.-Y.; Park, S.-J. A Review on Interface Engineering of MXenes for Perovskite Solar Cells. Nano-Micro Lett. 2023, 15 (1), 123. https://doi.org/10.1007/s40820-023-01083-9
  56. [56]Karimipour, M.; Paingott Parambil, A.; Tabah Tanko, K.; Zhang, T.; Gao, F.; Lira-Cantu, M. Functionalized MXene/Halide Perovskite Heterojunctions for Perovskite Solar Cells Stable Under Real Outdoor Conditions. Advanced Energy Materials 2023, 13 (44), 2301959. https://doi.org/10.1002/aenm.202301959
  57. [57]Aftab, S.; Abbas, A.; Iqbal, M. Z.; Hussain, S.; Kabir, F.; Hegazy, H. H.; Xu, F.; Kim, J. H.; Goud, B. S. Two-Dimensional MXene Incorporating for Electron and Hole Transport in High-Performance Perovskite Solar Cells. Materials Today Energy 2023, 36, 101366. https://doi.org/10.1016/j.mtener.2023.101366
  58. [58]Wang, Y.; Xiang, P.; Ren, A.; Lai, H.; Zhang, Z.; Xuan, Z.; Wan, Z.; Zhang, J.; Hao, X.; Wu, L.; Sugiyama, M.; Schwingenschlögl, U.; Liu, C.; Tang, Z.; Wu, J.; Wang, Z.; Zhao, D. MXene-Modulated Electrode/SnO2 Interface Boosting Charge Transport in Perovskite Solar Cells. ACS Appl. Mater. Interfaces 2020, 12 (48), 53973–53983. https://doi.org/10.1021/acsami.0c17338
  59. [59]Liu, X. (Xiao); Zhang, Z.; Jiang, J.; Tian, C.; Wang, X.; Wang, L.; Zhang, Z.; Wu, X.; Zheng, Y.; Liang, J.; Chen, C.-C. Chlorine-Terminated MXene Quantum Dots for Improving Crystallinity and Moisture Stability in High-Performance Perovskite Solar Cells. Chemical Engineering Journal 2022, 432, 134382. https://doi.org/10.1016/j.cej.2021.134382
  60. [60]Li, Y.; Wang, D.; Yang, L.; Yin, S. Preparation and Performance of Perovskite Solar Cells with Two Dimensional MXene as Active Layer Additive. Journal of Alloys and Compounds 2022, 904, 163742. https://doi.org/10.1016/j.jallcom.2022.163742
  61. [61]Wei, X.; Sun, Y.; Zhang, Y.; Yu, B.; Yu, H. A X-Bit Optimized 2D Solid Solution Ti3CNTx MXene as the Electron Transport Layer toward High-Performance Perovskite Solar Cells. Nano Energy 2025, 133, 110513. https://doi.org/10.1016/j.nanoen.2024.110513
  62. [62]Li, Y.; Zou, Y.; Yang, S.; Wang, H.; Yu, W.; Guo, H.; Li, X.; Cao, Y.; Liu, Y.; Tang, Z.; Qu, B.; Xiao, L.; Chen, Z. Improving Carrier Transport for Stable and Efficient Perovskite Solar Cells via MXene-Modified 2D Perovskite Capping Layer. Chemical Engineering Journal 2024, 500, 156686. https://doi.org/10.1016/j.cej.2024.156686
  63. [63]Huang, W.; Ding, L.; Wang, D.; Cai, P.; Wang, J.; Gao, R.; Hu, H.; Ye, Y.; Huang, C.; Xue, X.; Peng, H.; Sun, L. Tetrabutylammonium Hydroxide-Functionalized Ti3C2Tx MXene for Significantly Improving the Photovoltaic Performance of Perovskite Solar Cells. ACS Appl. Mater. Interfaces 2024, 16 (46), 63569–63579. https://doi.org/10.1021/acsami.4c13540
  64. [64]Nath, B.; Khasnabis, S.; Ramamurthy, P. C.; Mahapatra, D. R.; Hedge, G. Interfacial Engineering Using Ammonia-Functionalized MXene in Perovskite Solar Cells. Nanotechnol. Environ. Eng. 2023, 8 (4), 847–858. https://doi.org/10.1007/s41204-023-00333-w
  65. [65]Zhao, Y.; Zhang, X.; Han, X.; Hou, C.; Wang, H.; Qi, J.; Li, Y.; Zhang, Q. Tuning the Reactivity of PbI2 Film via Monolayer Ti3C2Tx MXene for Two-Step-Processed CH3NH3PbI3 Solar Cells. Chemical Engineering Journal 2021, 417, 127912. https://doi.org/10.1016/j.cej.2020.127912
  66. [66]Zhang, Y.; Xu, L.; Sun, J.; Wu, Y.; Kan, Z.; Zhang, H.; Yang, L.; Liu, B.; Dong, B.; Bai, X.; Song, H. 24.11% High Performance Perovskite Solar Cells by Dual Interfacial Carrier Mobility Enhancement and Charge-Carrier Transport Balance. Advanced Energy Materials 2022, 12 (37), 2201269. https://doi.org/10.1002/aenm.202201269
  67. [67]Sahare, S.; Solovan, M.; Smirnova, M.; Scheibe, B.; Jancelewicz, M.; Nowaczyk, G.; Kempiński, M.; Ziółek, M. MXenes as a Hole Transport Interfacial Layer for Efficient and Air-Stable Quasi-2D Perovskite Solar Cells. J. Mater. Chem. C 2024, 12 (23), 8357–8367. https://doi.org/10.1039/D4TC00466C
  68. [68]Sunderiya, S.; Suragtkhuu, S.; Purevdorj, S.; Ochirkhuyag, T.; Bat-Erdene, M.; Myagmarsereejid, P.; Slattery, A. D.; Bati, A. S. R.; Shapter, J. G.; Odkhuu, D.; Davaasambuu, S.; Batmunkh, M. Understanding the Oxidation Chemistry of Ti3C2Tx (MXene) Sheets and Their Catalytic Performances. Journal of Energy Chemistry 2024, 88, 437–445. https://doi.org/10.1016/j.jechem.2023.09.037
  69. [69]Chen, W.; Tang, J.; Cheng, P.; Ai, Y.; Xu, Y.; Ye, N. 3D Porous MXene (Ti3C2Tx) Prepared by Alkaline-Induced Flocculation for Supercapacitor Electrodes. Materials 2022, 15 (3), 925. https://doi.org/10.3390/ma15030925
  70. [70]Cui, W.; Chen, S.; Duan, J.; Zhang, R. Surface Functional Group Regulation of TiCT Based on Atmospheric Pressure Cold Plasma. Contributions to Plasma Physics 2024, 64 (9), e202300103. https://doi.org/10.1002/ctpp.202300103
  71. [71]Burschka, J.; Pellet, N.; Moon, S.-J.; Humphry-Baker, R.; Gao, P.; Nazeeruddin, M. K.; Grätzel, M. Sequential Deposition as a Route to High-Performance Perovskite-Sensitized Solar Cells. Nature 2013, 499 (7458), 316–319. https://doi.org/10.1038/nature12340
  72. [72]Kim, H.-S.; Lee, C.-R.; Im, J.-H.; Lee, K.-B.; Moehl, T.; Marchioro, A.; Moon, S.-J.; Humphry-Baker, R.; Yum, J.-H.; Moser, J. E.; Grätzel, M.; Park, N.-G. Lead Iodide Perovskite Sensitized All-Solid-State Submicron Thin Film Mesoscopic Solar Cell with Efficiency Exceeding 9%. Sci Rep 2012, 2 (1), 591. https://doi.org/10.1038/srep00591
  73. [73]Alharbi, E. A.; Alyamani, A. Y.; Kubicki, D. J.; Uhl, A. R.; Walder, B. J.; Alanazi, A. Q.; Luo, J.; Burgos-Caminal, A.; Albadri, A.; Albrithen, H.; Alotaibi, M. H.; Moser, J.-E.; Zakeeruddin, S. M.; Giordano, F.; Emsley, L.; Grätzel, M. Atomic-Level Passivation Mechanism of Ammonium Salts Enabling Highly Efficient Perovskite Solar Cells. Nat Commun 2019, 10 (1), 3008. https://doi.org/10.1038/s41467-019-10985-5
  74. [74]Ceratti, D. R.; Tenne, R.; Bartezzaghi, A.; Cremonesi, L.; Segev, L.; Kalchenko, V.; Oron, D.; Potenza, M. A. C.; Hodes, G.; Cahen, D. Self-Healing and Light-Soaking in MAPbI3: The Effect of H2O. Advanced Materials 2022, 34 (35), 2110239. https://doi.org/10.1002/adma.202110239
  75. [75]Yoo, J. J.; Wieghold, S.; Sponseller, M. C.; Chua, M. R.; Bertram, S. N.; Hartono, N. T. P.; Tresback, J. S.; Hansen, E. C.; Correa-Baena, J.-P.; Bulović, V.; Buonassisi, T.; Shin, S. S.; Bawendi, M. G. An Interface Stabilized Perovskite Solar Cell with High Stabilized Efficiency and Low Voltage Loss. Energy Environ. Sci. 2019, 12 (7), 2192–2199. https://doi.org/10.1039/C9EE00751B
  76. [76]McIndoe, J. S.; Tuck, D. G. Studies of Polyhalide Ions in Aqueous and Non-Aqueous Solution by Electrospray Mass Spectrometry. Dalton Trans. 2003, No. 2, 244–248. https://doi.org/10.1039/B208035B
  77. [77]Calabrese, V. T.; Khan, A. Polyiodine and Polyiodide Species in an Aqueous Solution of Iodine + KI: Theoretical and Experimental Studies. J. Phys. Chem. A 2000, 104 (6), 1287–1292. https://doi.org/10.1021/jp992847r
  78. [78]Marquez, K. P.; Sisican, K. M. D.; Ibabao, R. P.; Malenab, R. A. J.; Judicpa, M. A. N.; Henderson, L.; Zhang, J.; Usman, K. A. S.; Razal, J. M. Understanding the Chemical Degradation of Ti3C2T MXene Dispersions: A Chronological Analysis. Small Science 2024, 4 (10), 2400150. https://doi.org/10.1002/smsc.202400150
  79. [79]Zhang, C. J.; Pinilla, S.; McEvoy, N.; Cullen, C. P.; Anasori, B.; Long, E.; Park, S.-H.; Seral-Asc aso, A.; Shmeliov, A.; Krishnan, D.; Morant, C.; Liu, X.; Duesberg, G. S.; Gogotsi, Y.; Nicolosi, V. Oxidation Stability of Colloidal Two-Dimensional Titanium Carbides (MXenes). Chem. Mater. 2017, 29 (11), 4848–4856. https://doi.org/10.1021/acs.chemmater.7b00745
  80. [80]Othman, Z.; Mackey, H. R.; Mahmoud, K. A. A Critical Overview of MXenes Adsorption Behavior toward Heavy Metals. Chemosphere 2022, 295, 133849. https://doi.org/10.1016/j.chemosphere.2022.133849
  81. [81]Targhi, F. F.; Jalili, Y. S.; Kanjouri, F. MAPbI3 and FAPbI3 Perovskites as Solar Cells: Case Study on Structural, Electrical and Optical Properties. Results in Physics 2018, 10, 616–627. https://doi.org/10.1016/j.rinp.2018.07.007
  82. [82]Zhuang, J.; Wang, J.; Yan, F. Review on Chemical Stability of Lead Halide Perovskite Solar Cells. Nano-Micro Lett. 2023, 15 (1), 84. https://doi.org/10.1007/s40820-023-01046-0
  83. [83]Ren, X.; Wang, J.; Lin, Y.; Wang, Y.; Xie, H.; Huang, H.; Yang, B.; Yan, Y.; Gao, Y.; He, J.; Huang, J.; Yuan, Y. Mobile Iodides Capture for Highly Photolysis- and Reverse-Bias-Stable Perovskite Solar Cells. Nat. Mater. 2024, 23 (6), 810–817. https://doi.org/10.1038/s41563-024-01876-2
  84. [84]Bitton, S.; Tessler, N. Perovskite Ionics – Elucidating Degradation Mechanisms in Perovskite Solar Cells via Device Modelling and Iodine Chemistry. Energy Environ. Sci. 2023, 16 (6), 2621–2628. https://doi.org/10.1039/d3ee00881a
  85. [85]Thakur, A.; Chandran B.S., N.; Davidson, K.; Bedford, A.; Fang, H.; Im, Y.; Kanduri, V.; Wyatt, B. C.; Nemani, S. K.; Poliukhova, V.; Kumar, R.; Fakhraai, Z.; Anasori, B. Step-by-Step Guide for Synthesis and Delamination of Ti3C2Tx MXene. Small Methods 2023, 7 (8), 2300030. https://doi.org/10.1002/smtd.202300030
  86. [86]Alhabeb, M.; Maleski, K.; Anasori, B.; Lelyukh, P.; Clark, L.; Sin, S.; Gogotsi, Y. Guidelines for Synthesis and Processing of Two-Dimensional Titanium Carbide (Ti3C2Tx MXene). Chem. Mater. 2017, 29 (18), 7633–7644. https://doi.org/10.1021/acs.chemmater.7b02847
  87. [87]Ratzker, B.; Messer, O.; Goldstein, D.; Maman, N.; Ezersky, V.; Sokol, M. Challenges and Opportunities Utilizing Multilayer MXene as Precursors for Oriented TiCx in Ceramic Composites. Materials Today Advances 2024, 24, 100531. https://doi.org/10.1016/j.mtadv.2024.100531
  88. [88]Giannozzi, P.; Baroni, S.; Bonini, N.; Calandra, M.; Car, R.; Cavazzoni, C.; Ceresoli, D.; Chiarotti, G. L.; Cococcioni, M.; Dabo, I.; Dal Corso, A.; de Gironcoli, S.; Fabris, S.; Fratesi, G.; Gebauer, R.; Gerstmann, U.; Gougoussis, C.; Kokaly, A.; Lazzeri, M.; Martin-Samos, L.; Marzari, N.; Mauri, F.; Mazzarello, R.; Paolini, S.; Pasquarello, A.; Paulatto, L.; Sbraccia, C.; Scandolo, S.; Sclauzero, G.; Seitsonen, A. P.; Smogunov, A.; Umari, P.; Wentz covitch, R. M. QUANTUM ESPRESSO: A Modular and Open-Source Software Project for Quantum Simulations of Materials. J. Phys.: Condens. Matter 2009, 21 (39), 395502. https://doi.org/10.1088/0953-8984/21/39/395502
  89. [89]Garrity, K. F.; Bennett, J. W.; Rabe, K. M.; Vanderbilt, D. Pseudopotentials for High-Throughput DFT Calculations. Computational Materials Science 2014, 81, 446–452. https://doi.org/10.1016/j.commatsci.2013.08.053
  90. [90]Perdew, J. P. Generalized Gradient Approximation Made Simple. Phys. Rev. Lett. 1996, 77 (18), 3865–3868. https://doi.org/10.1103/PhysRevLett.77.3865
  91. [91]Xie, Y. Hybrid Density Functional Study of Structural and Electronic Properties of Functionalized Ti<span Class="aps-Inline-Formula"><math Xmlns="http://Www.W3.Org/1998/Math/MathML" Display="inline"><mrow><msub><mrow></mrow><mrow><mi>n</Mi><mo>−</Mo><mn>1</Mn></Mrow></msub><msub><mi>X</Mi><mi>n</Mi></msub></mrow></math></span> (<span Class="aps-Inline-Formula"><math Xmlns="http://Www.W3.Org/1998/Math/MathML" Display="inline"><mrow><mi>X</Mi><mo>=</Mo><mi Mathvariant="normal">C</Mi></Mrow></Math></span>, N) Monolayers. Phys. Rev. B 2013, 87 (23). https://doi.org/10.1103/PhysRevB.87.235441
  92. [92]Li, Y.; Hu, Y.; Wei, H.; Cao, W.; Qi, Y.; Zhou, S.; Zhang, P.; Li, H.; Li, G.-L.; Chai, R. Two-Dimensional Ti3C2Tx MXene Promotes Electrophysiological Maturation of Neural Circuits. Journal of Nanobiotechnology 2022, 20 (1), 398. https://doi.org/10.1186/s12951-022-01590-8
  93. [93]Eom, W.; Shin, H.; Ambade, R. B.; Lee, S. H.; Lee, K. H.; Kang, D. J.; Han, T. H. Large-Scale Wet-Spinning of Highly Electroconductive MXene Fibers. Nat Commun 2020, 11 (1), 2825. https://doi.org/10.1038/s41467-020-16671-1
  94. [94]Brette, F.; Célérier, S.; Canaff, C.; Loupias, L.; Paris, M.; Habrioux, A.; Boucher, F.; Mauchamp, V. XPS Binding Energy Shifts in 2D Ti3C2Tz MXene Go Largely Beyond Intuitive Explanations: Rationalization from DFT Simulations and Experiments. Small Methods n/a (n/a), 2400848. https://doi.org/10.1002/smtd.202400848
  95. [95]Näs̆lund, L.-Å.; Kokkonen, E.; Magnuson, M. Interaction and Kinetics of H2, CO2, and H2O on Ti3C2Tx MXene Probed by X-Ray Photoelectron Spectroscopy. Applied Surface Science 2025, 684, 161926. https://doi.org/10.1016/j.apsusc.2024.161926
  96. [96]Mičušik, M.; Šlouf, M.; Stepura, A.; Soyka, Y.; Ovodok, E.; Procházka, M.; Omastová, M. Aging of 2D MXene Nanoparticles in Air: An XPS and TEM Study. Applied Surface Science 2023, 610, 155351. https://doi.org/10.1016/j.apsusc.2022.155351
  97. [97]Eom, W.; Shin, H.; Han, T. H. Tracking the Thermal Dynamics of Ti3C2Tx MXene with XPS and Two-Dimensional Correlation Spectroscopy. Applied Physics Letters 2023, 122 (21), 211601. https://doi.org/10.1063/5.0143298
  98. [98]Natu, V.; Benchakar, M.; Canaff, C.; Habrioux, A.; Célérier, S.; Barsoum, M. W. A Critical Analysis of the X-Ray Photoelectron Spectra of Ti3C2Tz MXenes. Matter 2021, 4 (4), 1224–1251. https://doi.org/10.1016/j.matt.2021.01.015
  99. [99]Wang, S.; Liu, Y.; Liu, Y.; Hu, W. Effect of HF Etching on Titanium Carbide (Ti3C2Tx) Microstructure and Its Capacitive Properties. Chemical Engineering Journal 2023, 452, 139512. https://doi.org/10.1016/j.cej.2022.139512
  100. [100]Arole, K.; Pas, S. E.; Thakur, R. M.; Amjouny, L. A.; Kabir, M. H.; Dujovic, M.; Radovic, M.; Lutkenhaus, J. L.; Green, M. J.; Liang, H. Effects of Intercalation on ML-Ti3C2Tz MXene Properties and Friction Performance. ACS Appl. Mater. Interfaces 2024, 16 (46), 64156–64165. https://doi.org/10.1021/acsami.4c12659
  101. [101]Liao, M.; Zheng, Z.; Jiang, H.; Ma, M.; Wang, L.; Wang, Y.; Zhuang, S. MXenes as Emerging Adsorbents for Removal of Environmental Pollutants. Science of The Total Environment 2024, 912, 169014. https://doi.org/10.1016/j.scitotenv.2023.169014
  102. [102]Siuzdak, K.; Szkoda, M.; Sawczak, M.; Lisowska-Oleksiak, A.; Karczewski, J.; Ryl, J. Enhanced Photoelectrochemical and Photocatalytic Performance of Iodine-Doped Titania Nanotube Arrays. RSC Adv. 2015, 5 (62), 50379–50391. https://doi.org/10.1039/C5RA08407E
  103. [103]Li, M.; Dong, X.; Li, Q.; Liu, Y.; Cao, S.; Hou, C.-C.; Sun, T. Engineering MXene Surface via Oxygen Functionalization and Au Nanoparticle Deposition for Enhanced Electrocatalytic Hydrogen Evolution Reaction. Small Methods 2025, 9 (4), 2401569. https://doi.org/10.1002/smtd.202401569
  104. [104]Liu, Z.; Lv, H.; Xie, Y.; Wang, J.; Fan, J.; Sun, B.; Jiang, L.; Zhang, Y.; Wang, R.; Shi, K. A 2D/2D/2D Ti3C2Tx@TiO2@MoS2 Heterostructure as an Ultrafast and High-Sensitivity NO2 Gas Sensor at Room-Temperature. J. Mater. Chem. A 2022, 10 (22), 11980–11989. https://doi.org/10.1039/D1TA09369J
  105. [105]Xia, F.; Lao, J.; Yu, R.; Sang, X.; Luo, J.; Li, Y.; Wu, J. Ambient Oxidation of Ti3C2 MXene Initialized by Atomic Defects. Nanoscale 2019, 11 (48), 23330–23337. https://doi.org/10.1039/C9NR07236E
  106. [106]Schultz, T. Work Function and Energy Level Alignment Tuning at <math Xmlns="http://Www.W3.Org/1998/Math/MathML"><mrow><msub><mi>Ti</Mi><mn>3</Mn></Msub><msub><mi Mathvariant="normal">C</Mi><mn>2</Mn></Msub><msub><mi Mathvariant="normal">T</Mi><mi>x</Mi></Msub></mrow></Math> MXene Surfaces and Interfaces Using (Metal-)Organic Donor/Acceptor Molecules. Phys. Rev. Mater. 2023, 7 (4). https://doi.org/10.1103/PhysRevMaterials.7.045002
  107. [107]Xie, C.; Xu, S.; Cheng, Y.; Cui, X.; Yang, L.; Wu, R.; Yang, W.; Huang, Z. Stepwise Regulating the Work Function of Ti3C2Tx MXene by Charge Transfer Doping Scheme for Optoelectronic Applications. Materials Today Physics 2025, 58, 101849. https://doi.org/10.1016/j.mtphys.2025.101849
  108. [108]Tsai, K.-W.; Chueh, C.-C.; Williams, S. T.; Wen, T.-C.; Jen, A. K. Y. High-Performance Hole-Transporting Layer-Free Conventional Perovskite/Fullerene Heterojunction Thin-Film Solar Cells. J. Mater. Chem. A 2015, 3 (17), 9128–9132. https://doi.org/10.1039/C5TA01343G
  109. [109]Zhang, Q.; Wang, J.; Yu, Q.; Li, Q.; Fan, R.; Li, C.; Fan, Y.; Zhao, C.; Cheng, W.; Ji, P.; Sheng, J.; Zhang, C.; Xie, S.; Henkelman, G.; Li, H. Metal/MXene Composites via in Situ Reduction. Nat. Synth 2025, 4 (2), 252–261. https://doi.org/10.1038/s44160-024-00660-z
  110. [110]Alyasi, H.; Wahib, S.; Gomez, T. A.; Rasool, K.; Mahmoud, K. A. The Power of MXene-Based Materials for Emerging Contaminant Removal from Water - A Review. Desalination 2024, 586, 117913. https://doi.org/10.1016/j.desal.2024.117913
  111. [111]An, Y.; Sedinkin, S. L.; Venditti, V. Solution NMR Methods for Structural and Thermodynamic Investigation of Nanoparticle Adsorption Equilibria. Nanoscale Adv. 2022, 4 (12), 2583–2607. https://doi.org/10.1039/d2na00099g
  112. [112]Jiang, J.; Vicent-Luna, J. M.; Tao, S. The Role of Solvents in the Formation of Methylammonium Lead Triiodide Perovskite. Journal of Energy Chemistry 2022, 68, 393–400. https://doi.org/10.1016/j.jechem.2021.12.030
  113. [113]Xiang, W.; Zhang, J.; Liu, S. (Frank); Albrecht, S.; Hagfeldt, A.; Wang, Z. Intermediate Phase Engineering of Halide Perovskites for Photovoltaics. Joule 2022, 6 (2), 315–339. https://doi.org/10.1016/j.joule.2021.11.013
  114. [114]Robles Montes, F.; Rosiles-Perez, C.; Arias Ramos, C. F.; Hu, H.; Sosa Sánchez, J. L.; Jiménez González, A. E. Study of DMSO Concentration on the Optical and Structural Properties of Perovskite CH3NH3PbI3 and Its Use in Solar Cells. Journal of Solid State Chemistry 2022, 312, 123158. https://doi.org/10.1016/j.jssc.2022.123158
  115. [115]De Keersmaecker, M.; Dietrich, P.; Bahri, M.; Browning, N. D.; Armstrong, N. R.; Ratcliff, E. L. Activated Corrosion and Recovery in Lead Mixed-Halide Perovskites Revealed by Dynamic Near-Ambient Pressure X-Ray Photoelectron Spectroscopy. J. Am. Chem. Soc. 2025, 147 (10), 8881–8892. https://doi.org/10.1021/jacs.5c00668
  116. [116]Wang, Y.; Chen, W.; Yang, X.; Li, A.; Lu, T.; Qiu, G. Enhanced Removal of Lead Ions from Wastewaters by Electrochemical Adsorption Using Nitrogen-Doped Ti3C2Tx MXene. Chemical Engineering Journal 2024, 498, 155463. https://doi.org/10.1016/j.cej.2024.155463
  117. [117]Jun, B.-M.; Her, N.; Park, C. M.; Yoon, Y. Effective Removal of Pb(II) from Synthetic Wastewater Using Ti3C2Tx MXene. Environ. Sci.: Water Res. Technol. 2019, 6 (1), 173–180. https://doi.org/10.1039/C9EW00625G
  118. [118]Li, Y.; Zhou, W.; Li, Y.; Huang, W.; Zhang, Z.; Chen, G.; Wang, H.; Wu, G.-H.; Rolston, N.; Vila, R.; Chiu, W.; Cui, Y. Unravelling Degradation Mechanisms and Atomic Structure of Organic-Inorganic Halide Perovskites by Cryo-EM. Joule 2019, 3 (11), 2854–2866. https://doi.org/10.1016/j.joule.2019.08.016
  119. [119]Liu, W.; Li, L.; Hu, C.; Chen, D.; Shen, G. Intercalation of Small Organic Molecules into Ti3C2T MXene Cathodes for Flexible High-Volume-Capacitance Zn-Ion Microsupercapacitor. Advanced Materials Technologies 2022, 7 (12), 2200158. https://doi.org/10.1002/admt.202200158
  120. [120]Kim, J. S.; Chang, H.; Kang, S.; Cha, S.; Cho, H.; Kwak, S. J.; Park, N.; Kim, Y.; Kang, D.; Song, C. K.; K ваг, J.; Hahn, J.-S.; Lee, W. B.; Hyeon, T.; Park, J. Critical Roles of Metal–Ligand Complexes in the Controlled Synthesis of Various Metal Nanoclusters. Nat Commun 2023, 14 (1), 3201. https://doi.org/10.1038/s41467-023-38955-y
  121. [121]Chunlim, H.; Depjian, M.; Srisawad, K.; Meekati, T.; Wongratanaphisan, D.; Ruankham, P.; Kanjanaboos, P.; Pakawatpanurut, P. Solution-Processed, Binder-Free Pristine Ti3C2Tx MXene Electrodes Enabled by MAI Passivation for High-Performance, Scalable Perovskite Solar Cells. Applied Surface Science Advances 2025, 28, 100803. https://doi.org/10.1016/j.apsadv.2025.100803
  122. [122]Liu, Z.; Alshareef, H. N. MXenes for Optoelectronic Devices. Advanced Electronic Materials 2021, 7 (9), 21000295. https://doi.org/10.1002/aelm.202100295
  123. [123]Gao, C.-H.; Zhang, Y.; Zhang, C.-C.; Li, M.; Ma, X.-J.; Wang, K.-L.; Igbari, F.; Wang, Z.-K.; Liao, L.-S. TiI4-Doping Induced Bulk Defects Passivation in Halide Perovskites for High Efficient Photovoltaic Devices. Organic Electronics 2021, 88, 105973. https://doi.org/10.1016/j.orgel.2020.105973
  124. [124]Petrov, A. A.; Belich, N. A.; Grishko, A. Y.; Stepanov, N. M.; Dorofeev, S. G.; Maksimov, E. G.; Shelvekov, A. V.; Zakeeruddin, S. M.; Graetzel, M.; Tarasov, A. B.; Goodilin, E. A. A New Formation Strategy of Hybrid Perovskites via Room Temperature Reactive Polyiodide Melts. Mater. Horiz. 2017, 4 (4), 625–632. https://doi.org/10.1039/C7MH00201G
  125. [125]Rakita, Y.; Gupta, S.; Cahen, D.; Hodes, G. Metal to Halide Perovskite (HaP): An Alternative Route to HaP Coating, Directly from Pb(0) or Sn(0) Films. Chem. Mater. 2017, 29 (20), 8620–8629. https://doi.org/10.1021/acs.chemmater.7b02314
  126. [126]Klaeboe, Peter. The Raman Spectra of Some Iodine, Bromine, and Iodine Monochloride Charge-Transfer Complexes in Solution. J. Am. Chem. Soc. 1967, 89 (15), 3667–3676. https://doi.org/10.1021/ja00991a001
  127. [127]Svensson, P. H.; Kloo, L. Synthesis, Structure, and Bonding in Polyiodide and Metal Iodide–Iodine Systems. Chem. Rev. 2003, 103 (5), 1649–1684. https://doi.org/10.1021/cr0204101
  128. [128]Stegemann, H.; Rohde, A.; Reiche, A.; Schnittke, A.; Füllbier, H. Room Temperature Molten Polyiodides. Electrochimica Acta 1992, 37 (3), 379–383. https://doi.org/10.1016/0013-4686(92)87025-U
  129. [129]Congeduti, A.; Nardone, M.; Postorino, P. Polarized Raman Spectra of a Single Crystal of Iodine. Chemical Physics 2000, 256 (1), 117–123. https://doi.org/10.1016/S0301-0104(00)00085-9
  130. [130]Ledinský, M.; Löper, P.; Niesen, B.; Holovský, J.; Moon, S.-J.; Yum, J.-H.; De Wolf, S.; Fejfar, A.; Ballif, C. Raman Spectroscopy of Organic–Inorganic Halide Perovskites. J. Phys. Chem. Lett. 2015, 6 (3), 401–406. https://doi.org/10.1021/jz5026323
  131. [131]Ben-Uliel, T.; Aviv, H.; Zhou, J.; Li, M.; Avadyayev, S.; Kapon, O.; Damle, V.; Yi, C.; Tischler, Y. Raman Scattering Obtained from Laser Excitation of MAPbI3 Single Crystal. Applied Materials Today 2020, 19, 100571. https://doi.org/10.1016/j.apmt.2020.100571
  132. [132]Nayak, P.; Yang, M.; Wang, Z.; Li, X.; Miao, R.; Compton, R. G. Single-Entity Ti3C2Tx MXene Electro-Oxidation. Applied Materials Today 2022, 26, 101335. https://doi.org/10.1016/j.apmt.2021.101335
  133. [133]Schranger, H.; Khosravi, S.; Fitzek, H.; Abbas, Q. Elaborating the Iodine/Polyiodide Equilibrium Effects in Nanoporous Carbon-Based Battery Electrode via Extreme Mass Asymmetry in Hybrid Cells. ChemElectroChem 2021, 8 (16), 3155–3160. https://doi.org/10.1002/celc.202100458
  134. [134]Liu, A.; Zhu, H.; Park, W.-T.; Kang, S.-J.; Xu, Y.; Kim, M.-G.; Noh, Y.-Y. Room-Temperature Solution-Synthesized p-Type Copper(I) Iodide Semiconductors for Transparent Thin-Film Transistors and Complementary Electronics. Advanced Materials 2018, 30 (34), 1802379. https://doi.org/10.1002/adma.201802379
  135. [135]Shahzad, A.; Rasool, K.; Miran, W.; Nawaz, M.; Jang, J.; Mahmoud, K. A.; Lee, D. S. Two-Dimensional Ti3C2Tx MXene Nanosheets for Efficient Copper Removal from Water. ACS Sustainable Chem. Eng. 2017, 5 (12), 11481–11488. https://doi.org/10.1021/acssuschemeng.7b02695
  136. [136]Natu, V.; Pai, R.; Sokol, M.; Carey, M.; Kalra, V.; Barsoum, M. W. 2D Ti3C2Tz MXene Synthesized by Water-Free Etching of Ti3AlC2 in Polar Organic Solvents. Chem 2020, 6 (3), 616–630. https://doi.org/10.1016/j.chempr.2020.01.019
  137. [137]Kumar, S.; Kumari, N.; Singh, T.; Seo, Y. Shielding 2D MXenes against Oxidative Degradation: Recent Advances, Factors and Preventive Measures. Journal of Materials Chemistry C 2024, 12 (23), 8243–8281. https://doi.org/10.1039/D4TC00884G
  138. [138]Kumar, S.; Park, H. M.; Singh, T.; Kumar, M.; Seo, Y. Long-Term Stability Studies and Applications of Ti3C2Tx MXene. International Journal of Energy Research 2023, 2023 (1), 5275439. https://doi.org/10.1155/2023/5275439

Paper details

vlnc:W_fmetz9h6
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents