Fermiology and Band Structure of Oxygen-Terminated Ti3C2Tx MXene

Abstract

The class of two-dimensional carbides and nitrides known as MXenes exhibit remarkable electronic properties. Tailoring these properties, however, requires an in-depth understanding of the band structure and Fermi-surface topology. Surface oxidation of MXenes has previously hampered the characterization of their Fermi surface, which is crucial for understanding the topology and anisotropy in the electronic structure and, ultimately, for tailoring electronic properties. Here, we reveal the Fermi surface topology and band structure of purely oxygen-terminated Ti3C2Tx MXene achieved through rigorous thin film sample preparation and ultrahigh vacuum annealing. Polarized synchrotron radiation-based angle-resolved photoemission spectroscopy reveals electron pockets, bulk band gaps, and a Dirac-like feature in the anisotropic electronic band structure. This paves the way for a fundamental understanding of band engineering of electronic transport properties, providing insights of importance for energy storage devices, transparent conductors, and catalysis.

The quantum phenomena occurring in graphene [1] has sparked significant interest in the exploration of two-dimensional (2D) materials with diverse electronic and optical properties that do not exist in bulk materials. 2D crystals with trigonal symmetry, e.g., with hexagonal honeycomb structure, are known to host Dirac fermions at the corners of the hexagonal Brillouin zone (BZ), denoted Dirac points, conical band crossings corresponding to a zero bandgap [2]. There, charge-carriers behave as massless fermions, which has led to the emergence of Dirac physics, inducing new physical phenomena such as Klein tunneling and Zitterbewegung, and of utmost importance for topological insulators [3, 4]. Beyond elemental 2D materials, such as graphene, silicene [5], most recently goldene [6], and binary compounds like hexagonal boron nitride (h-BN), molybdenum disulfide (MoS2_2), tungsten disulfide (WS2_2), there are great prospects for the large class of tunable 2D materials known as MXenes (Mn+1_{n+1}Xn_nTx_x), where M represents a transition metal, X can be either carbon or nitrogen, and T denotes termination species [7]. These materials offer a wide range of compositional variables that can be manipulated to achieve specific properties [8], for possible applications as transistors and spintronics [9], 2D-based electronics and displays [10], supercapacitors [11], and transparent conductive electrodes [12].

In Mn+1_{n+1}Xn_nTx_x, where n = 1, 2, or 3, the n+1 M and n X monolayers are arranged in an alternating sequence, as depicted in Figure 1(a). The properties are largely determined by the terminating species, including fluorine, hydroxide, chlorine, and atomic oxygen, for applications in semiconducting materials and electrochemical energy storage [13]. To prevent property deterioration [14], caution must be exercised in avoiding oxidation of the MXene surfaces. From density functional theory (DFT), there are many studies of band structures in MXenes and how they depend on termination, primarily relying on ground state DFT calculations at 0 K [15, 16, 17]. These calculations indicate that bare Mn+1Xn\mathrm{M}_{n+1}\mathrm{X}_n layers exhibit metallic characteristics, with a finite density of states at the Fermi level (EFE_{\mathrm{F}}), while Mn+1XnTx\mathrm{M}_{n+1}\mathrm{X}_n\mathrm{T}_x can display semiconducting behavior [15, 16, 17] that can be altered by different termination species. However, consensus regarding the specific species inducing semiconducting behavior remains elusive. Of particular interest is the prediction of Fashandi et al. [18] who predicted that under certain circumstances, Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x could exhibit Dirac points with giant spin-orbit splitting around the EFE_{\mathrm{F}}, which is further supported by simliar predictions by others [19, 20, 21].

Crystal structure model, LEED image, Brillouin zones, and structure models

Figure 1. (Color online) (a) Crystal structure model of a Ti3C2\mathrm{Ti}_{3}\mathrm{C}_{2} sheet terminated by O occupying hollow fcc-sites (Ofcc\mathrm{O}_{\mathrm{fcc}} between the surface Ti atoms on both upper and lower surfaces with optional bridge sites (Ob\mathrm{O}_{\mathrm{b}}). (b) Representative LEED image after annealing showing hexagonal 1x1 spots taken at an electron beam energy of 98 eV. (c) Brillouin zones of the hexagonal honeycomb unit cell with symmetry points at: Γˉ\bar{\Gamma} (0,0,0)(0,0,0) Mˉ\bar{M} (12,0,0)(\frac{1}{2},0,0) Kˉ\bar{K} (23,13,0)(\frac{2}{3},\frac{1}{3},0). (d) Structure models of a Ti3C2O2\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{2} 1x1 unit cell and a 2x2 Ti3C2O1.5\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{1.5} supercell seen from above the surface.

Despite this interest in MXenes, there has been limited effort directed towards comprehending the fundamental properties of their Fermi surfaces (FS), known as fermiology, and its effect on the material characteristics. Angle-resolved photoemission spectroscopy (ARPES) is a powerful experimental method to investigate FSs [22] but the surface must be perfectly clean and well ordered. This condition was not previously met for MXenes, as surfaces are often disordered and contaminated with a mixture of organics and residues from the synthesis. Schultz et al. [23] applied ARPES on delaminated Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x, but the terminations were mixed, and the data was azimuthally averaged due to randomly oriented flakes in the measured film, hindering the extraction of the shape and size of the FS.

Here, we investigate the electronic band structure and FS of a thin film stacked-nanosheet Ti3C2Ox\mathrm{Ti}_3\mathrm{C}_2\mathrm{O}_x sample with pure oxygen termination obtained from etched Ti3AlC2\mathrm{Ti}_3\mathrm{AlC}_2-phase deposited on a cc-axis-oriented sapphire (Al2O3\mathrm{Al}_2\mathrm{O}_3) substrate (see Supplementary Information). By utilizing synchrotron-radiation-based ARPES at various excitation energies, we reveal inherent 2D features within the electronic structure and map the FS topology, including the orbital characteristics of the band structure and probing the broad momentum and energy range across the entire Brillouin zone. We provide direct experimental evidence for conical band crossings, analogous to Dirac points, at 1.5 eV binding energy below the EFE_{\mathrm{F}}.

Sample preparation was performed to achieve oxygen as sole termination species [24] (see SI). Figure 1(b) shows the evolution of low electron energy diffraction (LEED) spots during heat cycles in the form of high temperature flashes described in the SI. XPS surface characterization showed that the surface is exclusively oxygen-terminated (Figure S5) and the final sharp LEED spots indicate a clean well-ordered hexagonal MXene surface. Figure 1(c) shows four adjacent Brillouin zones (BZ) with high symmetry points at: (23,13,0)\left(\frac{2}{3},\frac{1}{3},0\right) indicated along the two dashed high-symmetry lines; Figure 1(d) shows models of a 1x1 unit cell and a 2x2 structure. The 2D hexagonal surface Brillouin zone (SBZ) of Ti3C2Ox\mathrm{Ti}_3\mathrm{C}_2\mathrm{O}_x has the distances between symmetry points: Γ−M‾=2π/a3=1.180 A˚−1\overline{\Gamma\mathrm{-}M}=2\pi/a\sqrt{3}=1.180\ \text{\AA}^{-1}, Γ−K‾=Γ−M‾/cos⁡(30∘)=1.362 A˚−1\overline{\Gamma\mathrm{-}K}=\overline{\Gamma\mathrm{-}M}/\cos(30^\circ)=1.362\ \text{\AA}^{-1}, K−M‾=tan⁡(30∘)Γ−M‾=0.681 A˚−1\overline{\mathrm{K\mathrm{-}M}}=\tan(30^\circ)\overline{\Gamma\mathrm{-}M}=0.681\ \text{\AA}^{-1}.

Photon energy scans

Figure S5. Photon energy scans (60-180 eV) at 45 K along the Mˉ\bar{M}-Γˉ\bar{\Gamma}-Mˉ\bar{M} and Kˉ\bar{K}-Mˉ\bar{M}-Kˉ\bar{K} directions where the energy independence indicates 2D surface states along the horizontal dashed lines close to the EFE_{\mathrm{F}}.

Figure 2 shows ARPES measurements at 180 eV photon energy of Ti3C2Ox\mathrm{Ti}_3\mathrm{C}_2\mathrm{O}_x along the M−Γ−M‾\overline{\mathrm{M\mathord{-}\Gamma\mathord{-}M}} (top panel) and the K−Γ−K‾\overline{\mathrm{K\mathord{-}\Gamma\mathord{-}K}} (bottom panel) direction. The shape of the overlaid calculated bands for the Ti3C2O2\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{2} unit cell are generally in good agreement with the measured overview ARPES data. Near EFE_{\mathrm{F}}, the valence band mainly consists of metallic Ti 3d3d-t2gt_{2g} states, that provide the dominant contribution to conduction. Between 0.5-2 eV binding energy, a bulk bandgap is narrowest in the vicinity of the Γˉ\bar{\Gamma}-point where there are highly dispersing bands. The absence of any kzk_{z} dispersion when varying the photon energy are a clear indication of the 2D character of the metallic bands at EFE_{\mathrm{F}} (see SI). Below the bandgap, there are bonding states between Ti 3d3d-ege_{g} and C 2p2p orbitals [17, 21]. At higher binding energy (EbE_{\mathrm{b}}), there is a belt of flat bands with high intensity down to 8 eV, where a second bulk bandgap occurs in the region between 9-10.5 eV.

Band structure and constant-energy contour maps

Figure 2. (Color online) (top) Band structure along the Mˉ\bar{M}-Γˉ\bar{\Gamma}-Mˉ\bar{M}-Γˉ\bar{\Gamma}-Mˉ\bar{M} high symmetry direction. (bottom) Band structure along the Kˉ\bar{K}-Γˉ\bar{\Gamma}-Kˉ\bar{K}-Mˉ\bar{M}-Kˉ\bar{K}-Γˉ\bar{\Gamma} high symmetry direction. Black and white areas represent the lowest and the highest intensities, respectively, in a logarithmic intensity scale with an overlayed calculated band structure of Ti3_3C2_2O2_2 unit cell model.

Figure 3(a) shows a magnification of the dispersion map around the Γˉ\bar{\Gamma}-point where the horizontal dashed lines, denoted (b), (c), (d) at binding energies 0 eV, 1 eV, and 2 eV below the EFE_{\mathrm{F}}, are constant energy contour cuts from the measured volume data. The FS of Ti3C2Ox\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{x} in Figure 3(b) exhibits an intense pocket of highly dispersing light electron bands centered at the Γˉ\bar{\Gamma} point with heavier bands forming radial pockets pointing towards the Kˉ\bar{\mathrm{K}}-points at the corners of the BZ. Between the radial electron pockets, there are lens-shaped lobes of dark empty areas pointing towards the Mˉ\bar{\mathrm{M}}-points. Hence, the FS has a hexagonal warping with six-fold symmetry, centered around the Γˉ\bar{\Gamma}-point of the BZ. The topology of the FS is thus very sensitive to the exact position of the EFE_{\mathrm{F}}, that depends on the coverage and type of Tx\mathrm{T}_{x}. At the EFE_{\mathrm{F}}, hole-like Ti 3dxy3d_{xy}, heavy hole bands govern the conductivity along the basal plane, while electron-like Ti 3dz23d_{z^{2}} bands at the Γˉ\bar{\Gamma}-point govern the conductivity along the cc-axis (S1).

Image not extracted

Figure 3. (Color online) (a) Measured band structure of Ti3_3C2_2Ox_x at 180 eV. Constant energy contour surface maps at (b) the EF_F at 0 eV, (c) 1 eV, and (d) 2 eV below EF_F as indicated by the horizontal lines in (a).

In contrast to the FS, the surface map at 1 eV binding energy below EFE_{\mathrm{F}} (Figure 3c), displays symmetrical six-fold elliptical lobes of heavy electron bands extending radially from the center of the BZ towards the Mˉ\bar{\mathrm{M}}-points with a dark area around the Γˉ\bar{\Gamma}-point that signifies a band gap. At 2 eV below the EFE_{\mathrm{F}}, the energy cut in Figure 3(d) exhibits weaker electron pockets pointing towards the Mˉ\bar{\mathrm{M}}-points.

Figure 4 shows polarization-dependent dispersion maps at a photon energy of 40 eV along the Kˉ\bar{\mathrm{K}}-Mˉ\bar{\mathrm{M}}-Kˉ\bar{\mathrm{K}} BZ edge with (a) horizontal and (b) vertical polarization. With horizontal polarization (a), O 2pz2p_{z} and Ti 3dz23d_{z^{2}} orbitals are mainly probed perpendicular to the basal abab-plane. The two intense spots at 5.4 eV binding energy halfway along the Kˉ\bar{\mathrm{K}}-Mˉ\bar{\mathrm{M}} direction are associated with both Ofcc\mathrm{O}_{\mathrm{fcc}} (oxygen occupying a surface fcc-site) and Ob\mathrm{O}_{\mathrm{b}} 2pz2p_{z} orbitals [24]. In case (b), an elongated intense spot is centered at the Mˉ\bar{\mathrm{M}}-point at 5.2 eV. Here, the highly dispersing bands exhibit a shape of an hourglass, like a Dirac point, with a band crossing at 1.5 eV The highest intensity around the Mˉ\bar{\mathrm{M}}-point is attributed to O 2pxy2p_{xy} orbitals in the basal abab-plane. With the Eˉ\bar{\mathrm{E}}-vector aligned perpendicularly to the Ti3C2Ox\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{x} surface, there would only be intensity from O in the points halfway between the Mˉ\bar{\mathrm{M}} and the Kˉ\bar{\mathrm{K}} and thus only an Ofcc\mathrm{O}_{\mathrm{fcc}} contribution probed. Thus, for the vertical pp-polarization (b), when the photon Eˉ\bar{\mathrm{E}}-vector is in the basal abab-plane, the bonding O 2pxy2p_{xy} and Ti 3dx2−y23d_{x^{2}-y^{2}}, 3pxy3p_{xy}, orbitals are probed along the Ti3C2Ox\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{x} surface, showing a peak at 5.2 eV as only Ob\mathrm{O}_{\mathrm{b}} is observed. When the Eˉ\bar{\mathrm{E}}-vector is perpendicular to the basal abab-plane (a), domains of Ofcc\mathrm{O}_{\mathrm{fcc}} are observed at a higher EbE_{\mathrm{b}} together with Ob\mathrm{O}_{\mathrm{b}} at 0.2 eV lower EbE_{\mathrm{b}}.

The observations in Figure 4 are supported by previous valence band XPS studies [24] that showed that for mixed Ofcc\mathrm{O}_{\mathrm{fcc}} and Ob\mathrm{O}_{\mathrm{b}} terminations, Ofcc\mathrm{O}_{\mathrm{fcc}} shifts to lower binding energy in the VB so that the peaks of Ofcc\mathrm{O}_{\mathrm{fcc}} and Ob\mathrm{O}_{\mathrm{b}} coincide. The peaks are well separated for horizontal polarization (Figure 4(a)), indicating that there are areas on the Ti3_3C2_2Ox_x surface where there is only Ofcc_{\mathrm{fcc}}, while other areas have only Ob_{\mathrm{b}} or both Ofcc_{\mathrm{fcc}} and Ob_{\mathrm{b}}. As shown by the polarization dependence in Figure 4, the orbital extent and direction of the oxygen atom is different for Ofcc_{\mathrm{fcc}} and Ob_{\mathrm{b}}, with one perpendicular and two angularly directed lone-pair orbitals, respectively. [23] (see Supplementary Information section S2).

Polarization-dependent measurements at 40 eV and 84 K along the BZ edge

Figure 4. (Color online) Polarization-dependent measurements at 40 eV and 84 K along the BZ edge with integrated intensities in the right panels: (a) linear horizontal ss-polarization with components both along the cc-axis (O 2pz2p_z and Ti 3dz23d_{z^2} orbitals) and along the basal abab-plane. (b) linear vertical pp-polarization along the basal abab-plane (O 2pxy2p_{xy} and Ti 3dx2−y23d_{x^2-y^2}, Ti 2pxy2p_{xy} orbitals). The intense white areas around 5.2-5.4 eV on a logarithmic intensity scale (yellow color) are due to O 2pz2p_z and O 2pxy2p_{xy} states, respectively, while the black areas represent the band gap.

The electrons at the FS control the transport properties, where the conductivity is proportional to the Fermi velocity (vFv_{\mathrm{F}}), the concentration of Fermi electrons, i.e., the density of states at EFE_{\mathrm{F}}, and inversely proportional to the relaxation time [25]. Based on DFT calculations of the band dispersions and the effective mass approximation, the conductivity of Ti3_3C2_2O2_2 is estimated to be ∼1.8×105 Ω−1m−1\sim1.8 \times10^{5}\,\Omega^{-1}\mathrm{m}^{-1} with a relaxation time of about 1 fs [26] (see SI).

As the coverage of oxygen increases [24], there is an evolution of electronic properties as the adsorbed O experience mutual interaction with other O and alters the energy bands so that the bulk band gap within the occupied Ti 3d3d states becomes narrower and shifts upwards in energy. At full oxygen coverage on the fcc-site of Ti3_3C2_2Ox_x, Bader charge calculations indicate that each adsorbed O gains an effective charge of -1.114e while the C atoms gain -1.667e and the central and surface Ti atoms loose +1.686e and +1.938e, respectively. The electronic orbitals and FS can be further modified by the coverage of the termination species on the bridge site between the Ti atoms. The 2D behavior of the electronic transport properties of Ti3_3C2_2-based MXene indicate that the interplanar interactions between the Ti3_3C2_2Ox_x sheets are sufficiently weak so that the single sheet electronic features are highly preserved and behaves as stacked independent MXene sheets.

Different roles of the bands that crosses the EFE_{\mathrm{F}} both along and perpendicular to the basal plane are identified. The slope of the density of states (DOS) is rapidly increasing towards the conduction band. As the carrier velocities are perpendicular to the FS, they mainly contribute to the basal abab-plane except at the Γˉ\bar{\Gamma}-point. O-terminated MXenes are predicted to show the highest resistivity among the inherent -F, -O and -OH species as the surface functionalization alters the electronic resistance through a decrease of the carrier concentration. Previous DFT studies predicted that termination of Ti3_3C2_2Tx_x with -F, -O or -OH significantly alters and reduces the electronic states near EFE_{\mathrm{F}} [27, 28], while a local maximum in the DOS at EFE_{\mathrm{F}} is predicted for bare Ti3_3C2_2. This enables that the in-plane electrical conductivity of the Ti3_3C2_2Tx_x films can be tailored in a large range from zero to 2.9-4.8 x105^{5} S/m [25], 2.4 x105^{5} S/m [29] and 3.33 x105^{5} S/m [30]. This is also supported by theoretical band structures, indicating that Ti3_3C2_2O2_2 is metallic.

The calculated vFv_{\mathrm{F}} of Ti3_3C2_2Ox_x, with electron-like bands at the Γˉ\bar{\Gamma}-point shows a velocity component along the kzk_z axis. The other bands are active hole-like bands with large velocity contributions confined at the Kˉ\bar{\mathrm{K}}-point within the basal xyxy-plane (Figure S1). These results thus show that Ti3_3C2_2Ox_x is characterized by a clear carrier-type anisotropy, i.e., positive (hole) charge carriers within the basal abab-plane and negative (electron) charge carriers govern the properties perpendicular to the surface. A parallel can be drawn with the thermoelectric properties (Seebeck coefficient) of the parent 3D MAX phases, where the electronic structure has been well studied [31]. Two types of bands contribute and sums up to the total Seebeck coefficient [29]; hole-like bands in the basal abab-plane and electron-like bands along the caxis that both contribute but with opposite sign. This effect has been experimentally evidenced by anisotropic states in the electronic structure of Ti3_3SiC2_2 [32], which exhibits a highly unusual feature of near-zero Seebeck coefficient in a wide temperature range [33]. Similarly, Ti3_3C2_2Ox_x behaves as a p-type material along the in-plane direction, having predominantly itinerant positive charges, while the behavior is n-type perpendicular to the basal planes. The type of termination species and coverage as well as the charge-carrier phonon coupling determines the carrier mobility of the material. This should also be true for related Ti-based MXenes such as Ti2_2CTx_x.

X-ray diffractograms of Ti3AlC2 MAX-phase and Ti3C2Tx MXene

Figure S1. X-ray diffractograms (2-90°) of Ti3AlC2\mathrm{Ti}_3\mathrm{AlC}_2 MAX-phase and Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x MXene, where the (002) peak is located at 2θ=9.689∘2\theta=9.689^\circ and 6.558∘6.558^\circ, respectively.

The results also have implications for intercalation of ions between 2D Ti3_3C2_2Ox_x layers, a promising approach for energy storage devices, such as capacitors, batteries, and hydride electrochemical devices, where different ions can be considered as charge carriers [34]. Ti3_3C2_2Ox_x could also be of significance as gas sensors of, e.g., ethanol, methanol and acetone, H2_2O, H2_2S and CH4_4. Ti3_3C2_2Ox_x-based gas sensors should show high selectivity and sensitivity to adsorption of ammonia at room temperature [35]. This gas sensitivity mechanism is due to charge-transfer between the gas molecules and the O and Ti atoms on the surface. Upon adsorption, charge-transfer alters the shape of the FS and causes a significant change in the resistivity of Ti3_3C2_2Ox_x. This knowledge can be utilized for materials engineering of gas sensors, in energy storage units and water splitting for hydrogen production for circular electric energy production.

The development of such devices requires a proper description of the Ti3_3C2_2Ox_x surface, including correct identification of the band structure, FS, termination species, surface site occupancies, and bonding configurations. This work provides information about the topology of the FS for pure O-termination yielding an exhaustive description of the fermiology, identifying conical band crossings with Dirac-like appearance at 1.5 eV, and brings us closer to a better understanding of the 2D properties of MXenes and their unique characteristics important for future energy storage devices, transparent conductors, and catalysis.

From a scientific perspective, conical band crossings below the EF_\mathrm{F} are interesting because they may move in energy toward the EF_\mathrm{F} by interaction with other states through surface reconstruction, hybridization or coupling effects, especially under doping or external field influence. Furthermore, the position of these states below the EF_\mathrm{F} means they could participate in thermally activated processes, affecting the overall conductivity and potentially influencing phenomena like thermoelectric efficiency or magnetoresistance. Their stability and accessibility through techniques like ARPES make them important for investigating fundamental quantum effects in 2D materials and can guide efforts in band structure engineering for enhanced material performance in electronic applications.

Furthermore, the metallicity observed in oxygen-terminated Ti3_3C2_2Tx_x MXene is intriguing in Fermiology because oxygen passivation generally leads to insulating surfaces by creating a bandgap. Typically, in surface science, oxygen termination of a material passivates surface states by saturating dangling bonds, effectively reducing the density of states at the Fermi level and shifting the material’s behavior towards insulating. However, in Ti3_3C2_2Tx_x MXene, despite oxygen termination, metallicity is preserved.

This behavior suggests unconventional electronic structure characteristics at the Fermi surface, with oxygen contributing electronic states that do not localize or create a significant bandgap. In the context of Fermiology, this is particularly compelling as it implies that the Fermi surface of these materials can host itinerant electrons despite surface passivation, potentially due to unique hybridization between oxygen and the Ti transition metal atoms. This phenomenon opens up new possibilities for studying electron transport, electron-phonon interactions, and potential superconductivity in materials with mixed metallic and insulating character.

Conflict of interests: The authors declare no competing interests.

Acknowledgments: We acknowledge the MAX IV Laboratory for the ARPES beamtime at BLOCH. Research conducted at MAX IV, a Swedish national user facility, is supported by the Swedish Research council under contract 2018-07152, the Swedish Governmental Agency for Innovation Systems under contract 2018-04969, and Formas under contract 2019-02496. The computations were enabled by resources provided by the Swedish National Infrastructure for Computing (SNIC) at the National Supercomputer Centre (NSC) partially funded by the Swedish Research Council through grant agreement no. 2016-07213. M.M. acknowledges financial support from the Swedish Energy Research (Grant No. 43606-1) and the Carl Tryggers Foundation (CTS23:2746, CTS20:272, CTS16:303, CTS14:310). The research leading to these results has received funding from the Swedish Government Strategic Research Area in Materials Science on Functional Materials at Linköping University (Faculty Grant SFO-Mat-LiU No. 2009-00971). P.E. also acknowledges funding from the Swedish Research Council (VR) under Project No. 2021-03826 and the Knut and Alice Wallenberg Foundation through the Wallenberg Academy Fellows program (grant no. KAW 2020.0196). We also thank Dr. Joseph Halim at Linköping University for preparing the thin film MAX phase through magnetron sputtering and the etching of the thin film sample.

[?] See Supplemental Material at http://link.aps.org/supplemental/[url], which includes Refs. [?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?, ?] for additional information about the sample preparation, ARPES measurements, computational details, Fermi velocities, charge-density difference plots, surface coverage and supercells.

[?] L.-Å. Näslund, P. O. Å. Persson, J. Rosen; J. Phys. Chem. C 124 27732–42 (2020).

[?] M. Magnuson, J. Halim, L.-Å. Näslund; J. Elec. Spec. 224, 27-32 (2018).

[?] M. Magnuson, J.-P. Palmquist, M. Mattesini et al.; Phys. Rev. B 72, 245101 (2005).

[?] M. Shekhirev et al.; Prog. Mat. Sci. 120, 100757 (2021).

[?] M. Anayee et al.; This: Chem. Mater. 34, 958 (2022).

[?] P. E. Blöchl, Phys. Rev. B 50, 17953 (1994).

[?] G. Kresse and J. Hafner, Phys. Rev. B 47, 558 (1993); ibid. 49, 14 251 (1994).

[?] A. V. Terentjev, L. A. Constantin, and J. M. Pitarke; Phys. Rev. B 98, 214108 (2018).

[?] S. Grimme, J. Comput. Chem. 25, 1463 (2004); ibid. 27, 1787 (2006).

[?] A. I. Liechtenstein, V. I. Anisimov, and J. Zaanen, Phys. Rev. B 52, R5467 (1995).

[?] M. A. Gluba and N. H. Nickel, PRB 87, 085204 (2013).

[?] A. Janotti, D. Segev, and C. G. Van de Walle, PRB 74, 045202 (2006).

[?] P. V. C. Medeiros, S. Stafström and J. Björk; Phys. Rev. B 89, 041407(R), (2014).

[?] M. Kawamura; Comp. Phys. Comm., 239, 197 (2019).

[?] M. Lindroos, S. Sahrakorpi, V. Arpiainen et al.; J. Phys. Chem. Sol. 67, 244 (2006).

[?] V. N. Strocov; J. Elec. Spec. Relat. Phen. 130, 65 (2003).

[?] S. Moser; . Elec. Spec. Relat. Phen. 214, 29 (2017).

[?] D Pinek, T. Ito, M Ikemoto et al.; Phys. Rev. B 98, 035120 (2018).

[?] D. Pinek, T. Ito, K. Furuta et al.; Phys. Rev. B 104, 195118 (2021)

[?] T. Ito, D. Pinek, T. Fujita et al.; Phys. Rev. B 96, 195168 (2017).

[?] L.-Å. Näslund, I. Persson; Appl. Surf. Sci. 593, 153442 (2022).

[?] L.-Å. Näslund, I. Persson; 2D Mater. 5, 015002 (2018).

[?] L.-Å. Näslund, P. O. Å. Persson, J. Rosen; J. Phys. Chem. C, 124, 27732 (2020).

[?] M. Benchakar, L. Loupias, C. Garnero et al.; Appl. Surf. Sci. 530 147209 (2020).

[?] V. Natu, M. Benchakar, C. Canaff et al.; Matter 4, 1224 (2021).

Figures

Panel (a): Band structure along the $\overline{\mathrm{M}}$–$\overline{\Gamma}$–$\overline{\mathrm{M}}$–$\overline{\Gamma}$–$\overline{\mathrm{M}}$ path
Panel (b): Band structure along the $\overline{\mathrm{K}}$–$\overline{\Gamma}$–$\overline{\mathrm{K}}$–$\overline{\mathrm{M}}$–$\overline{\mathrm{K}}$ path

Figure 5.

Fermiology and Band Structure of Oxygen-Terminated Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXene

Martin Magnuson; Per Eklund; Craig Polley

Supplementary information

Methods

Sample preparation

MXenes synthesized as thin films are most suitable for ARPES measurements and these are the highest quality samples available. Synthesis of MXenes from thin MAX-phase films yields significantly more well-ordered, cleaner and atomically flatter surfaces with fewer impurities and dislocations, resulting in sharper, more intense XPS peaks compared to bulk and freestanding sheet/foil counterparts. The thin film Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} stacked nanosheet sample was prepared from a thin film of Ti3AlC2\mathrm{Ti}_{3}\mathrm{AlC}_{2} MAX-phase deposited on a cc-axis-oriented sapphire (Al2O3\mathrm{Al}_{2}\mathrm{O}_{3}) substrate with an area of 10×10 mm210 \times10\ \mathrm{mm}^{2} using DC magnetron sputtering in an ultrahigh vacuum system. The deposition was performed using elemental Ti, Al and C targets with diameters of 75, 50 and 75 mm, respectively. Prior to deposition, the substrate was preheated inside the deposition chamber at 780 °C for 1 h. The Ti and C targets were ignited at 780 °C with powers of 92 and 142 W, respectively, for 30 s forming an incubation layer of TiC before the Al target was ignited at a power of 26 W. The duration of sputtering was 10 min, which produced a film of about 30 nm thickness. The Ti3AlC2\mathrm{Ti}_{3}\mathrm{AlC}_{2} thin film was thereafter converted into Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXene by etching in 50 % concentrated hydrofluoric acid for 1 h at room temperature. After etching, the sample was rinsed in deionized water and ethanol.

Formation of a high-quality MAX phase film was confirmed using Ni-filtered Cu Kα\alpha radiation (λ=1.5406\lambda= 1.5406 Å) in a normal Bragg–Brentano geometry of an X’Pert Panalytical x-ray diffraction (XRD) system [1]. Figure S1 shows ordinary qq-2θ2\theta diffractograms of the deposited Ti3AlC2\mathrm{Ti}_{3}\mathrm{AlC}_{2} film and the etched Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} MXene sample. Due to the limited diffraction volume, XRD of thin films exhibit higher noise levels compared to bulk materials and include peaks from both the substrate and growth layer. To minimize air exposure [2], the sample was subjected to XRD measurements for a brief duration of 10 minutes, after which it was stored under an argon (Ar) atmosphere. Mounting the Ti3C2Tx\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{T}_{x} film on the sample holder was performed in a glovebag filled with nitrogen gas (N2\mathrm{N}_{2}).

As observed in the diffractogram in Figure S1, the main diffraction peaks originate from Ti3AlC2(000l)\mathrm{Ti}_{3}\mathrm{AlC}_{2}(000l) together with a smaller peak from the TiC(111)\mathrm{TiC}(111) seed layer and a strong peak from the a-Al2O3(0006)\mathrm{Al}_{2}\mathrm{O}_{3}(0006) substrate (S). The low intensities of the small additional peaks show that the films mainly consist of single-phase MAX phase. Furthermore, the fact that the diffractograms only show Ti3AlC2\mathrm{Ti}_{3}\mathrm{AlC}_{2} of {000l}\{000l\}-type is a signature of epitaxial films [3]. The epitaxial growth behaviour has also been documented by transmission electron microscopy (TEM) [4].

The diffractograms clearly show the effect of HF etching on the Al layer. The position of the (002) peak, located at 2θ=9.6893∘2\theta= 9.6893^\circ, allows for the calculation of the interlayer spacing and cc-axis=2∗d0022*d_{002} by applying Bragg’s Law. Based on the diffractogram presented in Figure S1, the cc-axis lattice parameter of the Ti3AlC2\mathrm{Ti}_{3}\mathrm{AlC}_{2} film was determined to be 18.24 Å. After etching, the (002) peak shifts to a lower angle of 2θ=6.5578∘2\theta= 6.5578^\circ, corresponding to an expanded cc-axis lattice parameter of 26.94 Å. The exact position of the (002) peak and the corresponding cc-axis depends on the etching process [5, 6].

The Ti3C2Tx\mathrm{Ti}_3\mathrm{C}_2\mathrm{T}_x thin film sample on the Al2O3\mathrm{Al}_2\mathrm{O}_3 substrate was stored in a vacuum suitcase and transported in Ar atmosphere to the MAX IV Laboratory synchrotron radiation facility and placed in the ARPES preparation chamber. Impurities such as TiO2\mathrm{TiO}_2 and other surface contaminations were thereby avoided. The termination species (Tx\mathrm{T}_x) were identified in a previous study as fluorine (F) and oxygen (O) by core-level X-ray photoelectron spectroscopy (XPS) [7]. A heat treatment up to 750 °C for 10 hours removed all the F species and pure O termination was obtained.

ARPES measurements

The ARPES data were measured at the BLOCH beamline at the 1.5 GeV storage ring at the MAX IV Laboratory in Lund, Sweden. Initially, degassing was applied using a low direct current through the sample in UHV (4×10−104\times10^{-10} mBar) for 5 hours. Two different annealing steps were then applied. In the first annealing step with 0.3 A/13.9 V, the sample gently glowed dull red >500°C for 10 minutes at a pressure of 1.9×10−91.9\times10^{-9} mBar. In the second annealing step, the current was increased to 0.4 A for 5 minutes at >600-700 °C. After the second step, the LEED image shown in Figure 1b was taken at a beam energy of 98 V and a filament current of 1.85 A in the ARPES chamber.

During the ARPES measurements, the spot size on the sample surface was 10 × 10 μ\mum. A Scienta Omicron DA30-L hemispherical electron energy analyzer was used for electron detection. Overview ARPES data were obtained using a photon energy of 180 eV at 45 K with a pass energy of 50 eV. Due to a small amount of charging of the underlying sapphire substrate, each spectrum was slightly shifted to bring the intensity cutoff at the sample Fermi level (EFE_{\mathrm{F}}) to a binding energy of zero. The small photon-induced charging offset varied with photon flux and energy but remained otherwise stable over time. Further ARPES measurements using horizontal s- and vertical p-polarization at low photon energy (40 eV) were performed to gain insight about 2D features and the orbital character. Qualitatively, the bands were the same everywhere on the sample but the O coverage appeared to be different in certain spots on the surface.

Computational details

First-principles calculations were performed by means of density functional theory (DFT) and the projector augmented wave method (PAW) [8] as implemented in the Vienna ab-initio simulation package (VASP) [9]. The PAW method was used together with the exchange-correlation (XC) functional PBE-SOL [10] within the Generalized Gradient Approximation (GGA), incorporating the Grimme van der Waals DFT-D2 scheme [11] and accounting for the effect of spin-orbit interaction. The plane-wave expansion cutoff energy was set to 700 eV, with 80 k-points between each pair of high-symmetry points and a 30x30x30 k-point mesh for the Fermi surface calculations.

Calculations we made using a 1x1 primitive cell Ti3C2O2\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{2} multilayer structure with O located at the threefold fcc site between three surface Ti atoms with a unit cell width of 3.075 Å and a height of 20.51 Å. The Ti-O distance was 2.047 Å. GGA+U with U=2.8 eV and a PBE-SOL potential was applied to improve the description of the Ti 3d electrons. The on-site Coulomb correction (GGA+U) [12] for Ti was calculated as U=2.8 [13], reflecting the screened atomic correlation energy [14].

A 2x2 supercell with a bridge-site coverage of Ti3C2O0.25\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{0.25} on each surface side was needed to explain a faint flat band along the Γˉ\bar{\Gamma}-Mˉ\bar{\mathrm{M}} direction that suggests a partly mixed phase of termination species sites. A representative 2x2 Ti3C2O1O0.5\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{1}\mathrm{O}_{0.5} supercell with mixed oxygen sites (total x=1.5) used in the calculations is shown in Figure 1(d) including oxygen on both fcc and bridge sites. The bands in the 2x2 supercell were unfolded into a 1x1 primitive cell representation by applying the effective band structure method using the program BandUP [15]. The Fermi velocities of Ti3C2O2\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{2} and Ti3C2\mathrm{Ti}_{3}\mathrm{C}_{2} were calculated using the FermiSurfer software [16].

Fermi velocities

Figure S2 shows calculated Fermi velocities for a) Ti3C2O2\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{2} and b) Ti3C2\mathrm{Ti}_{3}\mathrm{C}_{2} (bare MXene) of multilayer structures with electron and hole bands crossing the EF_{\mathrm{F}} and c) closeups of the active bands centred around the Mˉ\bar{\mathrm{M}} symmetry point with electron bands in the corners at the Γˉ\bar{\Gamma} symmetry point. The carrier velocities are orthogonal to the FS and are reflected the inclination of the bands where they cross the EF_{\mathrm{F}}. A higher inclination implies higher Fermi velocity of the charge carriers and increases the transport properties. The values of the Fermi velocities were deduced from the slope of the highest band dispersion that crosses the EF_{\mathrm{F}} around the Kˉ\bar{\mathrm{K}}-points. As shown in Figure S2 for Ti3C2O2\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{2}, the Fermi velocity is highest in the red-colored bands in the vicinity of the Kˉ\bar{\mathrm{K}}-points in the basal abab-plane while there is mostly an out of the plane velocity component at the Γˉ\bar{\Gamma}-point. As shown for metallic bare MXene in Figure S2, the plaquettes of the FS should give rise to more out-of-plane conduction than in the case of Ti3C2O2\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{2} that has a narrow rod-like surface state feature at the Γˉ\bar{\Gamma}-point. The transversal parts of the FS in Ti3C2O2\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{2} results in significant in-plane conduction. At zero temperature, the bands up to the FS corresponds to occupied (ground) states while those above are unoccupied (excited) states. The occupied states close the FS determines the plasmon frequencies of the electron and hole carriers as well as the electrical conductivity. As the electron velocities are orthogonal to the FS, the flat hole bands wrapped around the Kˉ\bar{K}-points are responsible for the in-plane conductivity in Ti3C2O2\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{2}, indicating that the conductivity is much higher in the basal abab-plane than along the cc-axis. This can also be corroborated with the large difference in effective masses of the holes and electrons in-plane vs out-of-plane that gives rise to a significant anisotropy in the conduction properties. In the basal abab-plane, the effective masses of the holes are an order of magnitude smaller than those of the electrons that leads to and increased carrier mobility [14]. This shows that mainly hole carriers are responsible for the in-plane conduction in Ti3C2O2\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{2}.

Figure S2. a) (left) Calculated Fermi velocities vFv_{\mathrm{F}} for a Ti₃C₂O₂ multilayer structure compared to b) Ti₃C₂ (bare MXene) with electron and hole bands crossing the EFE_{\mathrm{F}}. Fermi lines in the Γˉ\bar{\Gamma}-plane in the Brillouin zone is shown in the right figures. c) Closeup of the active hole bands (red) in Ti₃C₂O₂ (left) compared to less active bands in Ti₃C₂ (right) in rhombohedral Brillouin zones centered around the Mˉ\bar{M} symmetry point. The FS velocity moduli vFv_{\mathrm{F}} is shown by the color scales.

Charge-density difference plots

Figure S3 illustrates a tentative bonding model shown as calculated charge-density difference plots of Ti3C2Ox\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{x} surfaces with -O (red) adsorbed on a three-fold coordinated hollow fcc-site (a) involving σ\sigma-bonds in a yellow triangular negatively charged volume, where the corners are directed towards the three Ti atoms with positively charged volumes in blue and (b): on a bridge site between two Ti atoms with π\pi-bonds the O atoms obtain a linear yellow negatively charged volume. The direction of the electronic charge-transfer is indicated by arrows that is also similar in the case of additionally adsorbed H2O\mathrm{H}_{2}\mathrm{O} on top of the O species.

Charge-density difference plots of Ti3C2Ox surfaces with O adsorbed on fcc and bridge sites

Figure S3. Charge-density difference plots of Ti3C2Ox\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{x} surfaces with -O (red) adsorbed on a three-fold hollow fcc-site between three Ti atoms gives σ\sigma-bonds (b) Bridge site between two Ti atoms gives π\pi-bonds. Blue and brown spheres are Ti and C atoms and the arrows indicate charge-transfer from Ti toward the O atoms.

Band structure details

Figure S4 shows a close-up of the bands along the Γˉ\bar{\Gamma}-Mˉ\bar{M}-Kˉ\bar{K}-Γˉ\bar{\Gamma} high symmetry EE-kk cuts extracted from a 3D map measured with horizontal polarization at 180 eV and 45 K. The dispersive electron and hole bands in the vicinity of the EFE_{\mathrm{F}} are responsible for the formation of electron and hole pockets in the vicinity of the FS. Notably, the bands at the Γˉ\bar{\Gamma}-point and Mˉ\bar{M}-points form electron pockets mainly consisting of dz2d_{z^{2}} orbitals perpendicular to the basal plane while the bands at the Kˉ\bar{K}-points at the corners of the BZ form hole pockets that mainly consists of in-plane dxyd_{xy} and dx2−y2d_{x^{2}-y^{2}} orbitals. As a result of the strong Ti 3d3d – C 2p2p covalent bonding in the basal plane, the energy dispersion of the band structure is much stronger in-plane than along the cc-axis giving rise to a characteristic 2D character of the material. Thus, the metallic conduction predominantly originates from the Ti 3d3d states in the vicinity of the EFE_{\mathrm{F}}. Generally, the band structure of Ti3_{3}C2_{2}Tx_{x} exhibits similarities to that of graphene at the Kˉ\bar{K} and Mˉ\bar{M} points. This is attributed to the behavior of bulk MXene as an assemblage of independent single MXene layers, analogous to the structure of multilayer graphene. When including the spin-orbit interaction in the modelling, two quasi-double-degenerated bands occur with a splitting of 12.9 meV at the Kˉ\bar{K}-point.

The experimental band broadening compared to theoretical predictions is attributed to the kzk_{z}-dispersion (k-orthogonal), as comprehensively described in the references [18, 19, 20]. In three-dimensional (bulk) materials, ARPES reveals a strong and well-defined E(k)E(k) dependence. In contrast, for a monolayer, such as graphene, there is minimal kk-dependence, resulting in a nearly straight line at a specific energy. When ARPES probes more than one monolayer (2-3 monolayers, with a probe depth of approximately 5 Å at 50 eV), the contributions from layers beyond the top atomic layer shift the energies into a curvature, leading to a broadening of E(k)E(k). This broadening has been observed in ARPES measurements of Ti3_{3}SiC2_{2} by Pinek et al. [21], who also investigated V2_{2}AlC [22], Ti2_{2}SnC [23], and Cr2_{2}AlC [24]. To measure the band structure and FS, Schultz et al. [25] applied ARPES on delaminated Ti3_{3}C2_{2}Tx_{x}, but the terminations were mixed, and the data was azimuthally averaged due to randomly oriented flakes in the measured film, hindering measurements along specific symmetry lines and the extraction of the shape of the FS.

Figure S5 shows photon energy scans (60-180 eV) at 45 K along the Mˉ\bar{M}-Γˉ\bar{\Gamma}-Mˉ\bar{M} and Kˉ\bar{K}-Mˉ\bar{M}-Kˉ\bar{K} directions with the energy independent features (dark areas) along the horizontal dashed lines close to the EFE_{\mathrm{F}}. These energy-independent features are hallmarks of 2D surface states because they reflect the lack of dispersion with momentum perpendicular to the surface, indicative of states localized at the surface layer. These features provide crucial insights into the electronic structure and dimensionality of the material being studied.

Close-up of a high symmetry cut

Figure S4. Close-up of a Γˉ\bar{\Gamma}-Mˉ\bar{M}-Kˉ\bar{K}-Γˉ\bar{\Gamma} high symmetry cut extracted from a 3D map measured with horizontal polarization at 45 K. Calculated bands are overlayed in white color.

Figure S6 shows core-level XPS spectra measured at the same beamtime as the LEED and ARPES experiments. The overview spectrum (a) shows the expected peaks, and that the surface is clean from contaminats and only contains Ti, C and O. The Auger peaks in the overview spectrum were identified by altering the photon energy, as their energy positions remain constant on a kinetic energy scale but shift on a binding energy scale, unlike the core-level peaks.

Core-level XPS spectra of Ti3C2Ox

Figure S6. (top) overview XPS spectra of Ti3C2Ox\mathrm{Ti}_{3}\mathrm{C}_{2}O_x and (bottom) core level XPS (a) O 1s1s, (b) Ti 2p2p, and (c) C 1s1s. The O 1s1s spectra show that the Ti3C2Ox\mathrm{Ti}_{3}\mathrm{C}_{2}O_x sample has O surface termination both on the fcc-site and on the bridge-site. All spectra were measured with a photon energy of 642 eV.

The O 1s1s spectrum (b) exhibits a double feature where the peak at 531.2 eV is due to O bonded to the fcc site (OfccO_{\mathrm{fcc}}) while the peak at 530 eV is due to O bonded to the bridge site [26]. Initially, before annealing, regions of the sample only showed the OfccO_{\mathrm{fcc}} peak at 531.2 eV. Previous combined XPS and TEM studies also showed that O occupies two different sites on the Ti3C2\mathrm{Ti}_{3}\mathrm{C}_{2} surface [27]. The O component with the highest EbE_b and largest bandwidth corresponds to OfccO_{\mathrm{fcc}} with chemical bonds to three Ti surface atoms in a hollow site while the ObO_{\mathrm{b}} component with the lowest EbE_b and smallest bandwidth corresponds to a bridge site between two surface Ti atoms [26]. A previous valence band XPS study [28] showed that for mixed OfccO_{\mathrm{fcc}} and ObO_{\mathrm{b}} terminations, OfccO_{\mathrm{fcc}} shifts to lower binding energy in the VB so that the peaks of OfccO_{\mathrm{fcc}} and ObO_{\mathrm{b}} coincide. In case there is only OfccO_{\mathrm{fcc}} or if there is only ObO_{\mathrm{b}} then these peaks are separated.

The Ti 2p2p spectrum (c) shows that the sample surface is free from oxidized material such as TiO2\mathrm{TiO}_{2}, as there are no oxide peaks at approximately 459 eV and 465 eV [29, 30] [31]. The single C 1s1s peak (d) at 282.0 eV shows that the sample surface is free from C contamination. Contaminated MXene surfaces exhibit a peak at approximately 284.5 eV, due to graphite-like carbon, a residual product from etching, while hydrocarbon groups produce a peak at 284.5 eV [26, 27, 29].

Coverage-dependent flat band along the M‾\overline{\mathrm{M}}-Γ‾\overline{\Gamma}-M‾\overline{\mathrm{M}} direction

Figure S7: (left) shows detailed EE-kk cuts measured at 120 eV with horizonal polarization at 20 K along the M‾\overline{\mathrm{M}}-Γ‾\overline{\Gamma}-M‾\overline{\mathrm{M}} direction. The second derivative (right) reveals a weak flat band at 1.45 eV. Black and white areas represent the highest and lowest intensities, respectively, on a linear intensity scale.

Detailed E-k cuts and second derivative along the M-Gamma-M direction

Figure S7. (left) Detailed EE-kk cuts measured at 120 eV with horizonal polarization at 20 K along the M‾\overline{\mathrm{M}}-Γ‾\overline{\Gamma}-M‾\overline{\mathrm{M}} direction. The second derivative (right) reveals a weak flat band at 1.45 eV. Black and white areas represent the highest and lowest intensities, respectively, on a linear intensity scale.

Figure S8-Figure S8: shows a set of more detailed EE-kk cuts measured at 120 eV with horizonal polarization at 20 K along the M‾\overline{\mathrm{M}}-Γ‾\overline{\Gamma}-M‾\overline{\mathrm{M}} and K‾\overline{\mathrm{K}}-M‾\overline{\mathrm{M}}-K‾\overline{\mathrm{K}} directions. The second derivative on the right reveals a weak flat band at 1.5 eV along the M‾\overline{\mathrm{M}}-Γ‾\overline{\Gamma}-M‾\overline{\mathrm{M}} direction and a Dirac-like band crossing along the K‾\overline{\mathrm{K}}-M‾\overline{\mathrm{M}}-K‾\overline{\mathrm{K}} direction.

Detailed E-k cuts measured at 120 eV with horizontal polarization at 20 K

Figure S8. (a, c) Detailed EE-kk cuts measured at 120 eV with horizontal polarization at 20 K along the Mˉ\bar{M}-Γˉ\bar{\Gamma}-Mˉ\bar{M} and K-Mˉ\bar{M}-K directions revealing a Dirac-like band crossing at 1.55 eV at the Mˉ\bar{M}-point. The second derivative (b, d) on the right reveals a weak flat band at 1.45 eV along the Mˉ\bar{M}-Γˉ\bar{\Gamma}-Mˉ\bar{M} direction. Black and yellow areas represent the lowest and highest intensities, respectively, on a linear intensity scale.

Unfolded supercell band structure calculations

Figure S9 shows unfolded bands along the Kˉ\bar{K}-Mˉ\bar{M}-Kˉ\bar{K} direction of a Ti3C2Ofcc\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{\mathrm{fcc}} supercell model exhibiting a Dirac-like band crossing at 1.5 eV at the Mˉ\bar{M}-symmetry point.

Unfolded band structure and 2x2 supercell model

Figure S9. Unfolded bands along the Kˉ\bar{K}-Mˉ\bar{M}-Kˉ\bar{K} direction of Ti3C2Ofcc\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{\mathrm{fcc}} (left) with a 2x2 supercell model (right) shows a band crossing at 1.5 eV at the Mˉ\bar{M}-symmetry point.

Figure S10 shows unfolded bands along the Mˉ\bar{M}-Γˉ\bar{\Gamma}-Mˉ\bar{M}-Γˉ\bar{\Gamma}-Mˉ\bar{M} and Kˉ\bar{K}-Γˉ\bar{\Gamma}-Kˉ\bar{K}-Mˉ\bar{M}-Kˉ\bar{K}-Γˉ\bar{\Gamma} directions of Ti3C2OfccOb\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{\mathrm{fcc}}\mathrm{O}_{\mathrm{b}} in a 2x2 supercell model (right). A faint flat band is discerned at 1.5 eV only along the Mˉ\bar{M}-Γˉ\bar{\Gamma}-Mˉ\bar{M} direction in some areas of the sample. Mixed Ofcc\mathrm{O}_{\mathrm{fcc}} and Ob\mathrm{O}_{\mathrm{b}} oxygen sites were needed to reproduce this band.

Unfolded bands and 2x2 supercell models for Ti3C2O_aO_b

Figure S10. Unfolded bands along the Mˉ\bar{\mathrm{M}}-Γˉ\bar{\Gamma}-Mˉ\bar{\mathrm{M}}-Γˉ\bar{\Gamma}-Mˉ\bar{\mathrm{M}} (top) and Kˉ\bar{\mathrm{K}}-Γˉ\bar{\Gamma}-Kˉ\bar{\mathrm{K}}-Mˉ\bar{\mathrm{M}}-Kˉ\bar{\mathrm{K}}-Γˉ\bar{\Gamma} (bottom) directions of Ti3C2OaOb\mathrm{Ti}_{3}\mathrm{C}_{2}\mathrm{O}_{a}\mathrm{O}_{b} with a 2×22 \times2 supercell model (right) shows a flat band at 1.5 eV along the Mˉ\bar{\mathrm{M}}-Γˉ\bar{\Gamma}-Mˉ\bar{\mathrm{M}} direction. The Ofcc\mathrm{O}_{\mathrm{fcc}} atoms are illustrated by red color, and the Ob\mathrm{O}_{b} atoms by orange color.

References

References

  1. [1]L.-Å. Näslund, P. O. Å. Persson, J. Rosen; J. Phys. Chem. C 124 27732–42 (2020).
  2. [2]M. Magnuson, J. Halim, L.-Å. Näslund; J. Elec. Spec. 224, 27-32 (2018).
  3. [3]M. Magnuson, J.-P. Palmquist, M. Mattesini et al.; Phys. Rev. B 72, 245101 (2005).
  4. [4]J. Halim et al.; Chem. Mater. 26, 2374–2381 (2014).
  5. [5]M. Shekhirev et al.; Prog. Mat. Sci 120, 100757 (2021).
  6. [6]M. Anayee et al.; This: Chem. Mater. 34, 958 (2022).
  7. [7]L.-Å. Näslund, M. Mikkelä, E. Kokkonen et al.; 2D Mater, 8, 045026 (2021).
  8. [8]P. E. Blöchl, Phys. Rev. B 50, 17953 (1994).
  9. [9]G. Kresse and J. Hafner, Phys. Rev. B 47, 558 (1993); ibid. 49, 14 251 (1994).
  10. [10]A. V. Terentjev, L. A. Constantin, and J. M. Pitarke; Phys. Rev. B 98, 214108 (2018).
  11. [11]S. Grimme, J. Comput. Chem. 25, 1463 (2004); ibid. 27, 1787 (2006).
  12. [12]A. I. Liechtenstein, V. I. Anisimov, and J. Zaanen, Phys. Rev. B 52, R5467 (1995).
  13. [13]M. A. Gluba and N. H. Nickel, PRB 87, 085204 (2013).
  14. [14]A. Janotti, D. Segev, and C. G. Van de Walle, PRB 74, 045202 (2006).
  15. [15]P. V. C. Medeiros, S. Stafström and J. Björk; Phys. Rev. B 89, 041407(R), (2014).
  16. [16]M. Kawamura; Comp. Phys. Comm., 239, 197 (2019).
  17. [17]T. Hu, M. Hu, B. Gao, W. Li, X. Wang; J. Phys. Chem. C 122, 18501 (2018).
  18. [18]M. Lindroos, S. Sahrakorpı, V. Arpiainen et al.; J. Phys. Chem. Sol. 67, 244 (2006).
  19. [19]V. N. Strocov; J. Elec. Spec. Relat. Phen. 130, 65 (2003).
  20. [20]S. Moser; . Elec. Spec. Relat. Phen. 214, 29 (2017).
  21. [21]D. Pinek, T. Ito, K. Furuta et al.; Phys. Rev. B 102, 075111 (2020).
  22. [22]D Pinek, T. Ito, M Ikemoto et al.; Phys. Rev. B 98, 035120 (2018).
  23. [23]D. Pinek, T. Ito, K. Furuta et al.; Phys. Rev. B 104, 195118 (2021)
  24. [24]T. Ito, D. Pinek, T. Fujita et al.; Phys. Rev. B 96, 195168 (2017).
  25. [25]T. Schultz, N. C. Frey, K. Hantanasirisakul et al.; Chem. Mater. 31, 6590 (2019).
  26. [26]L.-Å. Näslund, I. Persson; Appl. Surf. Sci. 593, 153442 (2022).
  27. [27]L.-Å. Näslund, I. Persson; 2D Mater. 5, 015002 (2018).
  28. [28]L.-Å. Näslund, P. O. Å. Persson, J. Rosen; J. Phys. Chem. C, 124, 27732 (2020).
  29. [29]M. Benchakar, L. Loupias, C. Garnero et al.; Appl. Surf. Sci. 530 147209 (2020).
  30. [30]V. Natu, M. Benchakar, C. Canaff et al.; Matter 4, 1224 (2021).

Paper details

vlnc:W_fnbbtyhq
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents