betaFeedback

WorksPhysics and Astronomy

Recombination velocities at grain boundaries in solar-cell absorbers – revisited

Abstract

The present work revisits the recombination velocities (sGBs_{\mathrm{GB}}) of minority-charge carriers determined at grain boundaries in polycrystalline absorber materials for solar cells. The equations describing sGBs_{\mathrm{GB}} as well as the barriers for electrons and holes were derived. It is shown that for given net-doping density and absolute temperature, the experimentally determined recombination velocity of a specific grain boundary depends only on the excess-charge density at this planar defect as well as on the prefactor sGB,0s_{\mathrm{GB,0}} describing the nonradiative recombination. Value ranges for these two quantities can be determined for any measured sGBs_{\mathrm{GB}} value. When analyzing sGBs_{\mathrm{GB}} datasets acquired on various (Ag,Cu)(In,Ga)Se2_2 and microcrystalline Si absorbers, it is apparent that both, the excess-charge density and the prefactor sGB,0s_{\mathrm{GB,0}}, remain within about the same orders of magnitude for all grain boundaries analyzed in a specific absorber. The broad range of the recombination velocities over several orders magnitude indicate upward as well as downward band bending, and the band-bending values are on the order of several ±\pm10 meV for all materials analyzed.

Introduction

In the photovoltaic solar cells appropriate for low-cost production at high conversion efficiencies, most of the solar absorbers, with the exception of monocrystalline, wafer-based Si, are polycrystalline. Therefore, grain boundaries are present at densities corresponding to the average grain sizes in these absorbers. Since the (two-dimensional, projected) density of point defects at a grain-boundary plane is enhanced with respect to those (three-dimensional) in the grain interiors of the adjacent grains, the nonradiative recombination rate is enhanced and contributes to a corresponding loss in the open-circuit voltage of the solar cell. The quantification of the grain-boundary recombination via the recombination velocity sGBs_{\mathrm{GB}} and the effects on the device performance have been revised recently [1]. It was clarified that sGBs_{\mathrm{GB}} can be expressed by a prefactor containing an effective defect density at the grain boundary and its capture cross-section multiplied by an exponential function depending on the band bending at the grain-boundary plane. However, for the case of a grain-boundary plane as opposed to for a surface, the derivation for equation describing the recombination velocity sGBs_{\mathrm{GB}} has not yet been published. Moreover, the available literature (e.g., [2]) provides equations only for the barriers of the majority charge-carriers at the grain boundary (i.e., upward/downward band bending for nn-type/pp-type semiconductors).

The present work first derived the equations of sGBs_{\mathrm{GB}} for low-injection and high-injection conditions. Also, the barriers of the majority charge-carriers at the grain boundary were calculated. It became apparent that the barriers for electrons or holes, provided that the net-doping density is sufficiently high, depend for a given net-doping density and absolute temperature only on the excess-charge density at the grain boundary. It is highlighted that each sGBs_{\mathrm{GB}} value determined experimentally at a grain boundary can be simulated using appropriate values for the excess-charge density at the grain boundary and for the prefactor sGB,0ns_{\mathrm{GB},0}^{n} describing the enhanced nonradiative recombination, and that the ranges of these values remain within the similar orders of magnitude for various photovoltaic absorber materials.

Theory

Basic considerations

We assume a pp-type semiconductor with net-doping density NAN_{\mathrm{A}}. This also includes the case of a compensated, pp-type semiconductor, for which the doping density is Na−NdN_{\mathrm{a}} - N_{\mathrm{d}} (i.e., the difference between the densities of ionized acceptor and donor states). For this case, we write for the hole concentration in thermodynamic equilibrium: p0=NA=Na−Ndp_0 = N_{\mathrm{A}} = N_{\mathrm{a}} - N_{\mathrm{d}}. Moreover, the electron density in the bulk under illumination is equal to the excess electron density: n=n0+Δn≈Δnn = n_0 + \Delta n \approx\Delta n. The hole density in the bulk under illumination is equal to the sum of the net-doping density NAN_{\mathrm{A}} and the excess electron density: p=p0+Δp=NA+Δnp = p_0 + \Delta p = N_{\mathrm{A}} + \Delta n, provided that charge carriers are not separated by strong internal electrical fields.

It is also assumed that under illumination, the quasi-Fermi levels are constant throughout the semiconductor. Then, at a grain-boundary plane, the electron and hole densities can be expressed by

nGB=Δnexp⁡(−ΦGB/kBT)(1)n_{\mathrm{GB}} = \Delta n \exp(-\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T) \tag*{(1)}

and

pGB=(NA+Δn)exp⁡(ΦGB/kBT),(2)p_{\mathrm{GB}} = (N_{\mathrm{A}} + \Delta n) \exp(\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T), \tag*{(2)}

where Δn\Delta n is the electron density at the edges of the space-charge regions at the these planar defects, ΦGB\Phi_{\mathrm{GB}} is the band bending at the grain-boundary plane (which either drives electrons/holes to or repels them from the grain boundary), kBk_{\mathrm{B}} is the Boltzmann constant, and TT the absolute temperature.

We consider the following scenario at the grain-boundary. In the case of a compensated, pp-type semiconductor at room temperature, there are various positively charged donor and negatively charged acceptor states, in addition to neutral defect states. Each defect state exhibits a charge state (positive, negative, or neutral) and contributes to Shockley-Read-Hall (SRH) recombination. The present grain-boundary model simplifies this complex situation by assuming one effective defect state at midgap position (since for such a defect, the SRH recombination is most effective) with density NGB,recombN_{\mathrm{GB,recomb}} and its capture cross-sections for electrons and holes, σn\sigma_n and σp\sigma_p; and another effective defect state with density NGB,chargeN_{\mathrm{GB,charge}} beyond the demarcation levels. This effective defect state exhibits an excess charge corresponding to whether the density of positively or that of negatively charged defect states at the grain boundary are larger (see Figure 1).

Schematic equilibrium band diagram of a p-type semiconductor at room temperature around a grain-boundary plane

Figure 1. Schematic equilibrium band diagram of a pp-type semiconductor at room temperature around a grain-boundary (GB) plane. In case of a compensated semiconductor, positively charged donor (ND+N_{\mathrm{D}}^{+}) as well as negatively charged acceptor states (NA−N_{\mathrm{A}}^{-}) are present, in addition to neutral defect states (not depicted here). The GB model in the present work assumes a simplified scenario with one effective defect density NGB,recombN_{\mathrm{GB,recomb}} at midgap position for the SRH recombination and another effective defect density NGB,chargeN_{\mathrm{GB,charge}}, which can be positive or negative, depending on whether the density of positively or that of negatively charged defect states are larger. ECE_{\mathrm{C}}, EVE_{\mathrm{V}}, and EFE_{\mathrm{F}} depict the conduction-band and valence-band edges as well as the Fermi level.

Since the effective, charged defect density NGB,chargeN_{\mathrm{GB,charge}} features a positive or negative excess charge, the free charge carriers redistribute correspondingly, provided that the net-doping density (NAN_{\mathrm{A}}) is sufficiently large (Figure 2). We note that for very small netdoping densities, the free charge carriers are captured by the defect state (trap), i.e., the grain interiors can be considered to be depleted of free charge carriers [2]. According to Poisson’s equation, the redistribution of free charge carriers results in spatial variations in the electrostatic potential and thus, in band bending. We note that for very large charge densities, theoretically, the upward band bending (pp-type semiconductor) can take values above the Fermi level; however, the grain-boundary model in the present work does not consider such a scenario.

Schematics depicting the origin of the band bending at a grain-boundary (GB) plane in a p-type semiconductor

Figure 2. Schematics depicting the origin of the band bending at a grain-boundary (GB) plane in a pp-type semiconductor at room temperature. Free charge carriers (holes) redistribute correspondingly, provided that the net-doping density (p0p_0) is sufficiently large. According to Poisson’s equation, the redistribution of free charge carriers results in downward (positive excess charge) or in upward band bending (negative excess charge).

Derivation of the equation for the recombination rate at a grain boundary

We use an equation describing the SRH recombination rate for an effective, deep defect level (NGB,recombN_{\mathrm{GB,recomb}}); it is very similar to the one used for the SRH bulk recombination rate RSRH=(np−ni2)/(nτp+pτn)R_{\mathrm{SRH}} = (np - n_i^2)/(n\tau_p + p\tau_n) (τp\tau_p and τn\tau_n are the hole and electron lifetimes, nin_i the intrinsic charge-carrier concentration). At a grain boundary, n=nGBn = n_{\mathrm{GB}} and p=pGBp = p_{\mathrm{GB}}. Moreover, we assume ni2≪npn_i^2 \ll np. The recombination rate at the grain boundary can be expressed by

RGB=Δnexp⁡(−ΦGB/kBT)(NA+Δn)exp⁡(ΦGB/kBT)Δnexp⁡(−ΦGB/kBT)(sGB,0p)−1+(NA+Δn)exp⁡(ΦGB/kBT)(sGB,0n)−1=Δn(NA+Δn)Δnexp⁡(−ΦGB/kBT)(sGB,0p)−1+(NA+Δn)exp⁡(ΦGB/kBT)(sGB,0n)−1(3)\begin{aligned} R_{\mathrm{GB}} &= \frac{\Delta n \exp(-\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)(N_{\mathrm{A}}+\Delta n)\exp(\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)}{\Delta n\exp(-\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)\left(s_{\mathrm{GB},0}^{p}\right)^{-1}+(N_{\mathrm{A}}+\Delta n)\exp(\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)\left(s_{\mathrm{GB},0}^{n}\right)^{-1}} \\ &= \frac{\Delta n(N_{\mathrm{A}}+\Delta n)}{\Delta n\exp(-\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)\left(s_{\mathrm{GB},0}^{p}\right)^{-1}+(N_{\mathrm{A}}+\Delta n)\exp(\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)\left(s_{\mathrm{GB},0}^{n}\right)^{-1}} \tag*{(3)} \end{aligned}

Here, sGB,0ps_{\mathrm{GB},0}^{p} and sGB,0ns_{\mathrm{GB},0}^{n} are the recombination velocity parameters of holes and electrons at the grain boundary (we use expressions similar to those used at semiconductor surfaces [3]):

sGB,0p=NGB,recombσpvth(4)s_{\mathrm{GB},0}^{p}=N_{\mathrm{GB,recomb}}\sigma_{p}v_{\mathrm{th}} \tag*{(4)}

and

sGB,0n=NGB,recombσnvth,(5)s_{\mathrm{GB},0}^{n}=N_{\mathrm{GB,recomb}}\sigma_{n}v_{\mathrm{th}}, \tag*{(5)}

where vthv_{\mathrm{th}} is the thermal velocity of holes and of electrons (we assume that they are same). Using Eqs. 4 and 5, Eq. 3 changes to:

RGB=Δn(NA+Δn)Δnexp⁡(−ΦGB/kBT)(NGB,recombσpvth)−1+(NA+Δn)exp⁡(ΦGB/kBT)(NGB,recombσnvth)−1=Δn(NA+Δn)NGB,recombvthΔnexp⁡(−ΦGB/kBT)σp−1+(NA+Δn)exp⁡(ΦGB/kBT)σn−1=ΔnNGB,recombvth[Δn/(NA+Δn)]exp⁡(−ΦGB/kBT)σp−1+exp⁡(ΦGB/kBT)σn−1(6)\begin{aligned} R_{\mathrm{GB}} &= \frac{\Delta n(N_{\mathrm{A}}+\Delta n)}{\Delta n\exp(-\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)(N_{\mathrm{GB,recomb}}\sigma_{p}v_{\mathrm{th}})^{-1}+(N_{\mathrm{A}}+\Delta n)\exp(\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)(N_{\mathrm{GB,recomb}}\sigma_{n}v_{\mathrm{th}})^{-1}} \\ &= \frac{\Delta n(N_{\mathrm{A}}+\Delta n)N_{\mathrm{GB,recomb}}v_{\mathrm{th}}}{\Delta n\exp(-\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)\sigma_{p}^{-1}+(N_{\mathrm{A}}+\Delta n)\exp(\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)\sigma_{n}^{-1}} \\ &= \frac{\Delta nN_{\mathrm{GB,recomb}}v_{\mathrm{th}}}{[\Delta n/(N_{\mathrm{A}}+\Delta n)]\exp(-\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)\sigma_{p}^{-1}+\exp(\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)\sigma_{n}^{-1}} \tag*{(6)} \end{aligned}

Equations for the recombination velocity at a grain boundary

The following approach is corresponding to the work by Brody and Rohatgi [4] who calculated the recombination velocity for a semiconductor surface. For a grain boundary, the effective recombination velocity is defined as

sGB:=RGBΔn=NGB,recombvth[Δn/(NA+Δn)]exp⁡(−ΦGB/kBT)σp−1+exp⁡(ΦGB/kBT)σn−1.(7)\begin{aligned} s_{\mathrm{GB}} &:= \frac{R_{\mathrm{GB}}}{\Delta n} \\ &= \frac{N_{\mathrm{GB,recomb}}v_{\mathrm{th}}}{[\Delta n/(N_{\mathrm{A}}+\Delta n)]\exp(-\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)\sigma_{p}^{-1}+\exp(\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)\sigma_{n}^{-1}}. \tag*{(7)} \end{aligned}

We may consider two different injection conditions:

Low-injection condition

Here, we need to assume not only that Δn≪NA\Delta n \ll N_{\mathrm{A}}, but also that the downward band bending ΦGB\Phi_{\mathrm{GB}} is not too strong; i.e., only if

Δn≪NA[exp⁡(−2ΦGB/kBT)σn/σp−1],(8)\Delta n \ll\frac{N_{\mathrm{A}}}{[\exp(-2\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)\sigma_{n}/\sigma_{p}-1]}, \tag*{(8)}

then Δn/(NA+Δn)]exp⁡(−ΦGB/kBT)σp−1≈0\Delta n/(N_{\mathrm{A}}+\Delta n)]\exp(-\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)\sigma_{\mathrm{p}}^{-1}\approx0 in Eq. (7), and this equation becomes

sGB=NGB,recombσnvthexp⁡(−ΦGBkBT).(9)s_{\mathrm{GB}}=N_{\mathrm{GB,recomb}}\sigma_{\mathrm{n}}v_{\mathrm{th}}\exp\left(-\frac{\Phi_{\mathrm{GB}}}{k_{\mathrm{B}}T}\right). \tag*{(9)}

We note that in order for Eq. (8) to hold, ΦGB\Phi_{\mathrm{GB}} for the downward band bending must remain small. For ΦGB=−100\Phi_{\mathrm{GB}}=-100 meV and σn/σp≈1\sigma_{\mathrm{n}}/\sigma_{\mathrm{p}}\approx1, the factor [exp⁡(−2ΦGB/kBT)σn/σp−1][\exp(-2\Phi_{\mathrm{GB}}/k_{\mathrm{B}}T)\sigma_{\mathrm{n}}/\sigma_{\mathrm{p}}-1] becomes about 3000. We consider ΦGB=−100\Phi_{\mathrm{GB}}=-100 meV as a lower limit.

High-injection condition

Δn≫NA\Delta n\gg N_{\mathrm{A}}: Δn/(NA+Δn)≈1\Delta n/(N_{\mathrm{A}}+\Delta n)\approx1

Also: ΦGB≈0\Phi_{\mathrm{GB}}\approx0 since nGB≈pGBn_{\mathrm{GB}}\approx p_{\mathrm{GB}}

⇒sGB=NGB,recombvth(σp−1+σn−1)−1.(10)\Rightarrow s_{\mathrm{GB}}=N_{\mathrm{GB,recomb}}v_{\mathrm{th}}\left(\sigma_{\mathrm{p}}^{-1}+\sigma_{\mathrm{n}}^{-1}\right)^{-1}. \tag*{(10)}

The dependencies of GB and sGB vs. NGB and n

We note that for low-injection conditions, sGBs_{\mathrm{GB}} (Eq. (9)) is a function of NGB,recombN_{\mathrm{GB,recomb}}, of σn\sigma_{\mathrm{n}}, and of ΦGB\Phi_{\mathrm{GB}}. For downward band bending at the grain-boundary plane in a pp-type semiconductor, ΦGB\Phi_{\mathrm{GB}} is expressed by [2]

ΦGBdown=−(qNGB,charge+)28ϵ0ϵrNA.(11)\Phi_{\mathrm{GB}}^{\mathrm{down}}=-\frac{\left(qN_{\mathrm{GB,charge}}^{+}\right)^2}{8\epsilon_{0}\epsilon_{\mathrm{r}}N_{\mathrm{A}}}. \tag*{(11)}

where ϵ0\epsilon_{0} and ϵr\epsilon_{\mathrm{r}} are the dielectric permittivities of the vacuum and of the semiconductor (see also Sec. A.2 in the Appendix). Note that Eq. 11 is only valid for semiconductors that exhibit net-doping densities sufficiently large so that the trap states represented by the density of recombination centers NGB,recombN_{\mathrm{GB,recomb}} do not capture all free charge carriers; i.e., in case the grains in the polycrystalline semiconductor are only partly depleted. The expression for the upward band bending is different (see Sec. A.1 in the Appendix):

ΦGBup=kBTqNGB,charge−4ϵ0ϵrNA.(12)\Phi_{\mathrm{GB}}^{\mathrm{up}}=\frac{\sqrt{k_{\mathrm{B}}TqN_{\mathrm{GB,charge}}^{-}}}{4\sqrt{\epsilon_{0}\epsilon_{\mathrm{r}}N_{\mathrm{A}}}}. \tag*{(12)}

Note that for the derivation of 12, the Boltzmann approximation was used; thus, ΦGBup<EF−EV\Phi_{\mathrm{GB}}^{\mathrm{up}}<E_{\mathrm{F}}-E_{\mathrm{V}}, which is about 100-150 meV for net-doping densities NAN_{\mathrm{A}} of about 101410^{14} to 101610^{16} cm−3^{-3}. In the present work, we assume an upper limit for ΦGBup\Phi_{\mathrm{GB}}^{\mathrm{up}} of 100 meV.

It is convenient to rewrite Eq. (9) for low-injection conditions using Eqs. (4) and (5):

sGB=sGB,0nexp⁡(−ΦGB(NGB,charge)kBT).(13)s_{\mathrm{GB}}=s_{\mathrm{GB},0}^{\mathrm{n}}\exp\left(-\frac{\Phi_{\mathrm{GB}}(N_{\mathrm{GB,charge}})}{k_{\mathrm{B}}T}\right). \tag*{(13)}

Thus, for given net-doping density NAN_{\mathrm{A}} and absolute temperature TT, ΦGB\Phi_{\mathrm{GB}} is a function of NGB,chargeN_{\mathrm{GB,charge}}, and sGBs_{\mathrm{GB}} is a function of NGB,chargeN_{\mathrm{GB,charge}} and sGB,0ns_{\mathrm{GB,0}}^{n}. We can now vary both quantities within certain intervals and check the resulting value ranges for ΦGB\Phi_{\mathrm{GB}} and sGBs_{\mathrm{GB}}. For the following considerations, we set ϵr=12\epsilon_{\mathrm{r}}=12 and T=300 KT=300\ \mathrm{K}. Corresponding to the considerations above, the current grain-boundary model is only valid for band bending values ΦGB\Phi_{\mathrm{GB}} within the interval of about −100-100 to +100 meV+100\ \mathrm{meV}.

While in microcrystalline Si, the pp-type net-doping density is corresponding to the density of doping atoms (e.g., B for pp-type Si), in compensated semiconductors such as CdTe or CuInSe2_2, the pp-type conductivity is determined by a slight excess of acceptor over donor densities, which are both on the order of about 101710^{17}-1019 cm−310^{19}\ \mathrm{cm}^{-3} [5, 6, 7]. Assuming a grain-boundary width of <1 nm<1\ \mathrm{nm} [8], the density of net charges at the grain-boundary plane would result to about 10910^{9}-1011 cm−210^{11}\ \mathrm{cm}^{-2}. However, the general picture of a grain boundary is that it acts as a sink for point defects segregating during the growth from the grain interiors to these planar defects. Therefore, it is appropriate to assume a slightly larger range for NGB,chargeN_{\mathrm{GB,charge}} of about 10910^{9}-1012 cm−210^{12}\ \mathrm{cm}^{-2}. Since for our model to be valid, ΦGBdown\Phi_{\mathrm{GB}}^{\mathrm{down}} and ΦGBup\Phi_{\mathrm{GB}}^{\mathrm{up}} must not exceed ∓100 meV\mp100\ \mathrm{meV}, there is an upper limit for NGB,chargeN_{\mathrm{GB,charge}}, which depends on the net-doping density NAN_{\mathrm{A}}. Using Eqs. 11 and 12, the downward and upward band bending values ΦGBdown\Phi_{\mathrm{GB}}^{\mathrm{down}} and ΦGBup\Phi_{\mathrm{GB}}^{\mathrm{up}} were calculated for various net-doping densities NAN_{\mathrm{A}} (see Figure 3). Apparently, the upper limits for NGB,chargeN_{\mathrm{GB,charge}}, i.e., for which the corresponding downward (upward) band bending values exceed ∓100 meV\mp100\ \mathrm{meV}, are about 3×10103 \times10^{10} (7×10107 \times10^{10}), 6×10106 \times10^{10} (2×10112 \times10^{11}), 3×10113 \times10^{11} (7×10117 \times10^{11}), and 6×10116 \times10^{11} (2×10122 \times10^{12}) cm−2\mathrm{cm}^{-2} for NA=1×1014N_{\mathrm{A}}=1 \times10^{14}, 1×10151 \times10^{15}, 1×10161 \times10^{16}, and 1×1017 cm−31 \times10^{17}\ \mathrm{cm}^{-3}.

Downward and upward band bending as a function of charged defect density for various net-doping densities

Figure 3. (a) Downward band bending ΦGBdown\Phi_{\mathrm{GB}}^{\mathrm{down}} and (b) upward band bending ΦGBup\Phi_{\mathrm{GB}}^{\mathrm{up}}, calculated as a function of the charged defect density NGB,chargeN_{\mathrm{GB,charge}} for various net-doping densities NAN_{\mathrm{A}} using Eqs. 11 and 12.

Assuming a net-doping density of NA=2×1016 cm−3N_{\mathrm{A}}=2 \times10^{16}\ \mathrm{cm}^{-3}, sGBs_{\mathrm{GB}} for downward and upward band bending were calculated using Eq. 13. Since the experimentally determined sGBs_{\mathrm{GB}} values that are on the order of 10010^{0}-104 cm/s10^{4}\ \mathrm{cm/s} [9, 10, 11, 12], the appropriate value range for sGB,0ns_{\mathrm{GB,0}}^{n} is about 10−110^{-1}-104 cm/s10^{4}\ \mathrm{cm/s}. In Figure 4, we plotted the value range of sGBs_{\mathrm{GB}} as a function of the value ranges of NGB,chargeN_{\mathrm{GB,charge}} and sGB,0ns_{\mathrm{GB,0}}^{n}. We consider the upper limits for NGB,chargeN_{\mathrm{GB,charge}} with respect to the downward and upward band bending mentioned above, 3×10113 \times10^{11} and 9×1011 cm−29 \times10^{11}\ \mathrm{cm}^{-2}. The lower limit of NGB,chargeN_{\mathrm{GB,charge}} was set to 1×109 cm−21 \times10^{9}\ \mathrm{cm}^{-2}.

Recombination velocity for downward and upward band bending

Figure 4. The recombination velocity sGBs_{\mathrm{GB}} for (a) downward and (b) upward band bending as a function of the charged defect density NGB,chargeN_{\mathrm{GB,charge}} and of the prefactor sGB,0ns_{\mathrm{GB,0}}^{n}, calculated using Eqs. 11, 12, and 13 for NA=2×1016 cm−3N_{\mathrm{A}} = 2 \times10^{16}\ \mathrm{cm}^{-3}. Highlighted by red (a) and blue (b) rectangles are the value ranges for the evaluation of the experimental sGBs_{\mathrm{GB}} data given in Figure 5.

From Figure 4, it is clear that one specific sGBs_{\mathrm{GB}} value can be represented assuming a certain pair of NGB,chargeN_{\mathrm{GB,charge}} and sGB,0ns_{\mathrm{GB,0}}^{n} values; and it is a range of appropriate values each that results in the same recombination velocity sGBs_{\mathrm{GB}}. Table 1 provides several ranges of sGBs_{\mathrm{GB}} values as well as the ranges of the corresponding NGB,chargeN_{\mathrm{GB,charge}} and sGB,0s_{\mathrm{GB,0}} values, assuming that they remain within the assumed intervals (0.01 to 3.3 or 0.01 to 9.1×1011 cm−29.1 \times10^{11}\ \mathrm{cm}^{-2} and 1×10−11 \times10^{-1} to 1×105 cm/s1 \times10^{5}\ \mathrm{cm/s}).

Band-bending typesGBs_{\mathrm{GB}} (cm/s)NGB,chargeN_{\mathrm{GB,charge}} (101110^{11} cm−2^{-2})sGB,0ns_{\mathrm{GB},0}^{n} (cm/s)
Upward1-20.01-9.11-100
Upward10-200.01-9.110-1000
Upward100-2000.01-9.1100-10000
Downward100-2000.01-3.32-200
Downward1000-20000.01-3.320-2000
Downward10000-200000.01-3.3200-20000

Table 1. Ranges of the recombination velocity sGBs_{\mathrm{GB}} and the corresponding NGB,chargeN_{\mathrm{GB,charge}} and sGB,0ns_{\mathrm{GB},0}^{n} intervals, extracted from Figure 4a and Figure 4b. Note that the excess charge density represented by NGB,chargeN_{\mathrm{GB,charge}} is positive for downward and negative for upward band bending.

While the results depicted in Table 1 are mathematically sound, the question is whether they can be confined to narrower intervals with respect to material properties in the solar-cell absorbers. In a polycrystalline semiconductor grown at elevated temperatures, the interdiffusion of constituing elements results in a rather homogeneous distribution of point defects, both, in the bulk and at grain boundaries. It does not mean identical, but certainly similar values for NGB,chargeN_{\mathrm{GB,charge}} and for sGB,0ns_{\mathrm{GB,0}}^{n}. Thus, it is appropriate to assume that within a specific absorber material, the NGB,chargeN_{\mathrm{GB,charge}} and sGB,0ns_{\mathrm{GB,0}}^{n} values remain within the same orders of magnitude. In the following section, we will check whether under this assumption, experimental sGBs_{\mathrm{GB}} values from the same polycrystalline semiconductor can be successfully reproduced using Eq. 13.

Comparison with experimental results

The recombination velocity sGBs_{\mathrm{GB}} of a specific grain boundary in a polycrystalline semiconductor can be determined by evaluating cathodoluminescence (CL) intensity distributions across this planar defect. The corresponding procedure is described in Ref. [1].

As shown in the previous section, for a specific sGBs_{\mathrm{GB}} value, always, ranges of NGB,chargeN_{\mathrm{GB,charge}} and sGB,0ns_{\mathrm{GB},0}^{n} values can be determined. We will now apply this approach to experimentally measured sGBs_{\mathrm{GB}} values. (We note that in the evaluation procedure described in Ref. [1], the median value of all experimental sGBs_{\mathrm{GB}} values from a specific absorber is assumed to be the sGBs_{\mathrm{GB}} value for ΦGB=0\Phi_{\mathrm{GB}} = 0 eV, i.e., equal to the prefactor sGB,0ns_{\mathrm{GB},0}^{n}; however, we find that it is more appropriate to assume that sGB,0ns_{\mathrm{GB},0}^{n} varies between two grain boundaries in the same material, and thus, this approach was improved by the present work.).

Figure 5 provides the simulations of experimental sGBs_{\mathrm{GB}} values, ranging from about 20 to 5200 cm/s, which were determined by means of CL on a high-efficiency Cu(In,Ga)Se2_2 layer [1, 10] with NA=2×1016N_{\mathrm{A}} = 2 \times10^{16} cm−3^{-3}. We would like to remind that we assume similar (but not identical) defect properties at the corresponding grain boundaries and therefore, determine the value ranges for NGB,chargeN_{\mathrm{GB,charge}} and sGB,0ns_{\mathrm{GB},0}^{n} that can be used to simulate successfully the experimental sGBs_{\mathrm{GB}} values; i.e., these NGB,chargeN_{\mathrm{GB,charge}} and sGB,0ns_{\mathrm{GB},0}^{n} value ranges are always the same for each sGBs_{\mathrm{GB}} dataset.

Experimental grain-boundary recombination velocity ranges

Figure 5. Experimental sGBs_{\mathrm{GB}} values [1, 10] as a function of (a) the defect density NGB,chargeN_{\mathrm{GB,charge}}, of the prefactor sGB,0ns_{\mathrm{GB,0}}^{n} (b), as well as of the band bending ΦGB\Phi_{\mathrm{GB}} (c). NGB,chargeN_{\mathrm{GB,charge}} was restricted to 0.3-3 (downward) and 0.9-9 ×1011 cm−2\times10^{11}\,\mathrm{cm}^{-2} (upward band bending), sGB,0ns_{\mathrm{GB,0}}^{n} to the interval 100-1000 cm/s. The blue bars stand for downward band bending, the red ones for upward band bending.

It is apparent from Figure 4a and Figure 4b that experimental sGBs_{\mathrm{GB}} values ranging over several orders of magnitude (i.e., 20 to 5200 cm/s) cannot be simulated assuming small NGB,chargeN_{\mathrm{GB,charge}} values on the order of 10910^{9}-101010^{10} cm−2^{-2}. Therefore, the simulations shown in Figure 5 are based on NGB,chargeN_{\mathrm{GB,charge}} values restricted to 0.3-3 (downward) and 0.9-9 ×1011\times10^{11} cm−2^{-2} (upward band bending). For sGB,0ns_{\mathrm{GB},0}^{n}, a value range of 100-1000 cm/s, on the same order of magnitude as the median of the experimental sGBs_{\mathrm{GB}} values, 300 cm/s, was found to be appropriate. These intervals are highlighted in Figure 4a and Figure 4b by a red and a yellow rectangle.

The ranges of NGB,chargeN_{\mathrm{GB,charge}} and sGB,0ns_{\mathrm{GB,0}}^{n} that result in the corresponding, experimental sGBs_{\mathrm{GB}} values are given in Figure 5a and Figure 5b. Figure 5c depicts the ranges for the band-bending values ΦGB\Phi_{\mathrm{GB}}. It is apparent from Figure 5 that several sGBs_{\mathrm{GB}} values can be modeled assuming both, downward and upward band bending. The true excess charge state of these grain boundaries cannot be revealed by the approach in the present work, but may be assessed by electrical analyses in scanning-probe microscopy, such as by conductive atomic force microscopy. Nevertheless, the ranges of NGB,chargeN_{\mathrm{GB,charge}} and sGB,0ns_{\mathrm{GB,0}}^{n} (Figure 5) can be used as input parameters in multidimensional device simulations.

In the Appendix Sections B.1 and B.2, evaluations of the sGBs_{\mathrm{GB}} values as the one shown in Figure 5 are demonstrated for (Ag,Cu)(In,Ga)Se2_2 and Si solar-cell absorbers. It is apparent that basically, the sGBs_{\mathrm{GB}} values for an individual absorber material always exhibit distributions over several orders of magnitude and thus, the magnitudes as well as the distributions of NGB,chargeN_{\mathrm{GB,charge}}, sGB,0ns_{\mathrm{GB,0}}^{n}, and ΦGB\Phi_{\mathrm{GB}} are similar to those in Figure 5. Overall, we simulated the experimental sGBs_{\mathrm{GB}} values from various multicrystalline Si, (Ag,Cu)(In,Ga)Se2_2, CdTe, kesterite-type, and halide-perovskite absorbers successfully by always using NGB,chargeN_{\mathrm{GB,charge}} and sGB,0ns_{\mathrm{GB,0}}^{n} ranges on the same orders of magnitude for a specific absorber (not all data shown in the present work). Thus, the presented approach is a general procedure to estimate the orders of magnitude of the effective defect density and its capture cross-section for any photovoltaic absorber material.

Correlation of excess charges and compositional changes at grain-boundary planes

In polycrystalline compound semiconductors, grain boundaries feature changes in composition within a very narrow range on the order of 0.1-1 nm. These changes have been interpreted as atomic / ionic reconstructions of the atomic planes adjacent to the grain boundary [8, 13]. It is a valid question of whether different NGB,chargeN_{\mathrm{GB,charge}} and σneff\sigma_{n}^{\mathrm{eff}} values, leading to substantially different recombination velocities sGBs_{\mathrm{GB}}, are related to different types of compositional changes found at different grain boundaries [14, 15]. In order to address this question, it makes sense to regard the orders of magnitude of the charge densities at the grain-boundary plane (that are screened by the free charge carriers) as well as those of the detected compositional changes. Since the NGB,chargeN_{\mathrm{GB,charge}} values were found to be on the order of 101010^{10} to 101110^{11} cm−2^{-2}, and since the width of the grain boundary can be estimated to about 0.1-1 nm, the total charge density is about 101710^{17}-101910^{19} cm−3^{-3}. On the other hand side, the changes in composition, also including impurity atoms, are typically on the order of 0.01-1 at.%, i.e., about 101910^{19}-102110^{21} cm−3^{-3} (see also Figure 6). Thus, the change in the charge density NGB,chargeN_{\mathrm{GB,charge}} at a grain boundary can be orders of magnitude smaller than the changes in composition that can easily be detected by available characterization techniques with suitable spatial resolution and sensitivity (e.g., atom-probe tomography); under ideal conditions, the total charge density and the chemical sensitivity of the analysis tool (referring to the detection of lateral changes in composition, not to the detection of impurities) may exhibit the same order of magnitude (101910^{19} cm−3^{-3}). Nevertheless, in general, it is very difficult (if not impossible) to verify whether or not a direct correlation exists between changes in the charge density and changes in the composition.

Schematics showing charge density at a grain-boundary plane and compositional changes

Figure 6. Schematics of the charge density at a grain-boundary plane (left) and the magnitude of the compositional changes around this planar defect (right). From the considerations and results in the present work, the effective charge density can be assumed to be about 101710^{17}-101910^{19} cm−3^{-3}, while the compositional changes typically detected via various microscopic analysis tools resides on larger orders of magnitude (101910^{19}-102110^{21} cm−3^{-3}); thus, effects of the local composition on the charge density present at a specific grain boundary can not be verified easily by the available analysis tools.

Conclusions

The present work revisited the determination procedures and magnitudes of recombination velocities at grain boundaries. It was described that experimentally measured recombination velocities sGBs_{\mathrm{GB}} can be simulated using specific value pairs of the charged defect density NGB,chargeN_{\mathrm{GB,charge}} and of the prefactor sGB,0ns_{\mathrm{GB,0}}^{n}. For one specific (experimental) sGBs_{\mathrm{GB}} value, always intervals of appropriate NGB,chargeN_{\mathrm{GB,charge}} and sGB,0ns_{\mathrm{GB,0}}^{n} values are found. However, for the experimentally measured sGBs_{\mathrm{GB}} values ranging from several 10010^{0} to several 10410^{4} cm/s, the intervals for NGB,chargeN_{\mathrm{GB,charge}} exhibit about the same orders of magnitude, about 101010^{10} to 101110^{11} cm−2^{-2}, with resulting values for the prefactor sGB,0s_{\mathrm{GB,0}} of about 10210^{2} to 10310^{3} cm/s. Finally, it has been outlined that the compositional changes at the grain boundaries that may be linked to changes in charged defect densities leading to enhanced nonradiative recombination are so small that their detection is very difficult using the currently available analytical tools.

Acknowledgements

The authors are grateful to Ulrike Bloeck (HZB) for assistance with the cross-sectional specimen preparation for SEM. The present work was supported by the project “EFFCIS-II” funded by the Federal Ministry for Economic Affairs and Climate Action (BMWK) under contract numbers 03EE1059B (HZB) and 03EE1059C (MLU).

Appendix

Derivation of band bending values at grain boundaries

Negative excess charge at grain boundary

We assume a grain-boundary plane with negligible thickness and negative excess charge density N‾GB,charge\overline{N}_{\mathrm{GB,charge}} at position x=0x=0. At sufficiently high net-doping density in a pp-type semiconductor, this excess charge will be screened by free holes (x≥0x \ge0):

ρ(x)=qNAAexp⁡(−x/w),(14)\rho(x) = qN_{\mathrm{A}}A\exp(-x/w), \tag*{(14)}

where qq is the charge of a hole, ww is the screening length (on both sides of the grain-boundary plane. Assuming a symmetrical distribution of ρ(x)\rho(x) around x=0x=0, the following equation must hold:

1q∫0∞ρ(x) dx=N‾GB,charge2⇔1q∫0∞qNAAexp⁡(−x/w) dx=N‾GB,charge2⇔A=N‾GB,charge2wNA(15)\begin{aligned} \frac{1}{q}\int_{0}^{\infty}\rho(x)\,\mathrm{d}x = \frac{\overline{N}_{\mathrm{GB,charge}}}{2} \\ &\Leftrightarrow\frac{1}{q}\int_{0}^{\infty}qN_{\mathrm{A}}A\exp(-x/w)\,\mathrm{d}x = \frac{\overline{N}_{\mathrm{GB,charge}}}{2} \\ &\Leftrightarrow A = \frac{\overline{N}_{\mathrm{GB,charge}}}{2wN_{\mathrm{A}}} \tag*{(15)} \end{aligned}

The electrical field is calculated via

F(x)=−qNAAwϵ0ϵrexp⁡(−x/w),(16)F(x) = -\frac{qN_{\mathrm{A}}Aw}{\epsilon_{0}\epsilon_{\mathrm{r}}}\exp(-x/w), \tag*{(16)}

Integration of F(x)F(x) results in the electrostatic potential:

ϕ(x)=−qNAAw22ϵ0ϵrexp⁡(−x/w).(17)\phi(x) = -\frac{qN_{\mathrm{A}}Aw^{2}}{2\epsilon_{0}\epsilon_{\mathrm{r}}}\exp(-x/w). \tag*{(17)}

The hole density p(x)p(x)

p(x)=ρ(x)/q+NA=NAAexp⁡(−x/w)+NA(18)p(x) = \rho(x)/q + N_{\mathrm{A}} = N_{\mathrm{A}}A\exp(-x/w) + N_{\mathrm{A}} \tag*{(18)}

must fulfill the continuity equation

div⁡→j⃗(x)−ddtp(x)=0⇔ddxj(x)=qddx[μp(x)F(x)−Dddxp(x)]=0⇔p(x)F(x)−kBTqddxp(x)=0⇔−p(x)ddxϕ(x)−kBTqddxp(x)=0(19)\overrightarrow{\operatorname{div}}\vec{j}(x)-\frac{\mathrm{d}}{\mathrm{d}t}p(x)=0 \\ \Leftrightarrow\frac{\mathrm{d}}{\mathrm{d}x}j(x)=q\frac{\mathrm{d}}{\mathrm{d}x}\left[\mu p(x)F(x)-D\frac{\mathrm{d}}{\mathrm{d}x}p(x)\right]=0 \\ \Leftrightarrow p(x)F(x)-\frac{k_{\mathrm{B}}T}{q}\frac{\mathrm{d}}{\mathrm{d}x}p(x)=0 \\ \Leftrightarrow-p(x)\frac{\mathrm{d}}{\mathrm{d}x}\phi(x)-\frac{k_{\mathrm{B}}T}{q}\frac{\mathrm{d}}{\mathrm{d}x}p(x)=0 \tag*{(19)}

assuming a stationary case (ddtp(x)=0)\left(\frac{\mathrm{d}}{\mathrm{d}t}p(x)=0\right) and using Einstein’s relationship qD=μkBTqD=\mu k_{\mathrm{B}}T. Applying Eqs. A.5 and A.4, Eq. A.6 becomes

[NAAexp⁡(−xw)+NA]qNAAwϵ0ϵrexp⁡(−xw)−kBTqNAAwexp⁡(−xw)=0⇔NAAexp⁡(−xw)[(Aexp⁡(−xw)+1)−kBTϵ0ϵrq2NAw2]=0⇔NGB,charge−2wNAexp⁡(−xw)+1−kBTϵ0ϵrq2NAw2=0(20)\left[N_{\mathrm{A}}A\exp\left(-\frac{x}{w}\right)+N_{\mathrm{A}}\right]\frac{qN_{\mathrm{A}}Aw}{\epsilon_{0}\epsilon_{\mathrm{r}}}\exp\left(-\frac{x}{w}\right)-\frac{k_{\mathrm{B}}T}{q}\frac{N_{\mathrm{A}}A}{w}\exp\left(-\frac{x}{w}\right)=0 \\ \Leftrightarrow N_{\mathrm{A}}A\exp\left(-\frac{x}{w}\right)\left[\left(A\exp\left(-\frac{x}{w}\right)+1\right)-\frac{k_{\mathrm{B}}T\epsilon_{0}\epsilon_{\mathrm{r}}}{q^{2}N_{\mathrm{A}}w^{2}}\right]=0 \\ \Leftrightarrow\frac{N_{\mathrm{GB,charge}}^{-}}{2wN_{\mathrm{A}}}\exp\left(-\frac{x}{w}\right)+1-\frac{k_{\mathrm{B}}T\epsilon_{0}\epsilon_{\mathrm{r}}}{q^{2}N_{\mathrm{A}}w^{2}}=0 \tag*{(20)}

using A=NGB,charge−/(2wNA)A=N_{\mathrm{GB,charge}}^{-}/(2wN_{\mathrm{A}}) (Eq. A.2). In the following, we consider the limit case of large NAN_{\mathrm{A}} and small NGB,charge−N_{\mathrm{GB,charge}}^{-}, i.e., NGB,charge−/(2wNA)exp⁡(−x/w)≤NGB,charge−/(2wNA)≪1N_{\mathrm{GB,charge}}^{-}/(2wN_{\mathrm{A}})\exp(-x/w)\leq N_{\mathrm{GB,charge}}^{-}/(2wN_{\mathrm{A}})\ll1; as outlined in the present work, this condition is fulfilled for various polycrystalline absorber materials. Thus, Eq. A.7 becomes

1−kBTϵ0ϵrq2NAw2=0⇔w2=kBTϵ0ϵrq2NA⇔w=kBTϵ0ϵrq2NA,(21)1-\frac{k_{\mathrm{B}}T\epsilon_{0}\epsilon_{\mathrm{r}}}{q^{2}N_{\mathrm{A}}w^{2}}=0 \\ \Leftrightarrow w^{2}=\frac{k_{\mathrm{B}}T\epsilon_{0}\epsilon_{\mathrm{r}}}{q^{2}N_{\mathrm{A}}} \\ \Leftrightarrow w=\sqrt{\frac{k_{\mathrm{B}}T\epsilon_{0}\epsilon_{\mathrm{r}}}{q^{2}N_{\mathrm{A}}}}, \tag*{(21)}

which is exactly the equation for the Debye screening length (see, e.g., Ref. [16]). For the amplitude AA follows

A=NGB,charge−2wNA=qNGB,charge−2kBTϵ0ϵrNA.(22)A=\frac{N_{\mathrm{GB,charge}}^{-}}{2wN_{\mathrm{A}}} \\ =\frac{qN_{\mathrm{GB,charge}}^{-}}{2\sqrt{k_{\mathrm{B}}T\epsilon_{0}\epsilon_{\mathrm{r}}N_{\mathrm{A}}}}. \tag*{(22)}

We can use the equations for ww and AA (Eqs. A.8 and A.9) to determine the electrostatic potential ϕ\phi (Eq. A.4) at position x=0x=0:

ϕ(x=0)=−qNA2ϵ0ϵrqNGB,charge−2kBTϵ0ϵrNAkBTϵ0ϵrq2NA=−kBTNGB,charge−4ϵ0ϵrNA.(23)\phi(x=0)=-\frac{qN_{\mathrm{A}}}{2\epsilon_{0}\epsilon_{\mathrm{r}}}\frac{qN_{\mathrm{GB,charge}}^{-}}{2\sqrt{k_{\mathrm{B}}T\epsilon_{0}\epsilon_{\mathrm{r}}N_{\mathrm{A}}}}\frac{k_{\mathrm{B}}T\epsilon_{0}\epsilon_{\mathrm{r}}}{q^{2}N_{\mathrm{A}}} \\ =-\frac{\sqrt{k_{\mathrm{B}}T N_{\mathrm{GB,charge}}^{-}}}{4\sqrt{\epsilon_{0}\epsilon_{\mathrm{r}}N_{\mathrm{A}}}}. \tag*{(23)}

The upward band bending ΦGBup=−qϕ(x=0)\Phi_{\mathrm{GB}}^{\mathrm{up}}=-q\phi(x=0) results to

ΦGBup=kBTqNGB,charge−4ϵ0ϵrNA.(24)\Phi_{\mathrm{GB}}^{\mathrm{up}}=\frac{\sqrt{k_{\mathrm{B}}TqN_{\mathrm{GB,charge}}^{-}}}{4\sqrt{\epsilon_0\epsilon_{\mathrm{r}}N_{\mathrm{A}}}}. \tag*{(24)}

Positive excess charge at grain boundary

We assume a grain-boundary plane with negligible thickness and positive excess charge density NGB,charge+N_{\mathrm{GB,charge}}^{+} at position x=0x=0. At sufficiently high net-doping density in a pp-type semiconductor, this excess charge will be screened by ionized acceptors:

ρ(x)=−qNA.(25)\rho(x)=-qN_{\mathrm{A}}. \tag*{(25)}

The electrical field is calculated via

F(x)=qNA(w+x)ϵ0ϵr,(26)F(x)=\frac{qN_{\mathrm{A}}(w+x)}{\epsilon_0\epsilon_{\mathrm{r}}}, \tag*{(26)}

Integration of F(x)F(x) results in the electrostatic potential for −w≤x≤w-w\leq x\leq w:

ϕ(x)=qNA(w+x)22ϵ0ϵr.(27)\phi(x)=\frac{qN_{\mathrm{A}}(w+x)^2}{2\epsilon_0\epsilon_{\mathrm{r}}}. \tag*{(27)}

Using NA=NGB,charge+/(2w)N_{\mathrm{A}}=N_{\mathrm{GB,charge}}^{+}/(2w), the downward band bending ΦGBdown=−qϕ(x=0)\Phi_{\mathrm{GB}}^{\mathrm{down}}=-q\phi(x=0) results in

ΦGBdown=−(qNGB,charge+)28ϵ0ϵrNA.(28)\Phi_{\mathrm{GB}}^{\mathrm{down}}=-\frac{\left(qN_{\mathrm{GB,charge}}^{+}\right)^2}{8\epsilon_0\epsilon_{\mathrm{r}}N_{\mathrm{A}}}. \tag*{(28)}

Case studies of recombination velocities at grain boundaries in (Ag,Cu)(In,Ga)Se2_2 and microcrystalline Si solar-cell absorbers

Case study I: evaluation of recombination velocities at grain boundaries in (Ag,Cu)(In,Ga)Se2_2 solar-cell absorbers

The following results were gathered on a Cu(In,Ga)Se2_2 solar-cell absorber with [Ga]/([Ga]+[In]) (GGI) ratio of 0.34 and on a (Ag,Cu)(In,Ga)Se2_2 solar-cell absorber with [Ag]/([Ag]+[Cu]) (AAC) ratio of 0.14. We note that the results shown below are not representative for (Ag,Cu)(In,Ga)Se2_2 layers with similar GGI ratios.

Experimental recombination velocities at grain boundaries

Figure A1. Experimental sGBs_{\mathrm{GB}} values from a Cu(In,Ga)Se2_2 layer with GGI=0.34 [11] as a function of (a) the defect density NGB,chargeN_{\mathrm{GB,charge}}, (b) of the prefactor sGB,0ns_{\mathrm{GB},0}^{n}, as well as (c) of the band bending ΦGB\Phi_{\mathrm{GB}}. The net-doping density was NA=1×1016 cm−3N_{\mathrm{A}} = 1 \times10^{16}\,\mathrm{cm}^{-3}, while NGB,chargeN_{\mathrm{GB,charge}} was restricted to 0.2-2 (downward) and 0.7-7 ×1011 cm−2\times10^{11}\,\mathrm{cm}^{-2} (upward band bending), sGB,0ns_{\mathrm{GB},0}^{n} to the interval 10-100 cm/s (the median of the experimental sGBs_{\mathrm{GB}} values was about 30 cm/s). The blue bars stand for downward band bending, the red ones for upward band bending.

Three panels showing $s_{\mathrm{GB}}$ values as functions of defect density, prefactor, and band bending

Figure A2. sGBs_{\mathrm{GB}} values from a (Ag,Cu)(In,Ga)Se2_2 layer with AAC=0.14 [12] as a function of (a) the defect density NGB,chargeN_{\mathrm{GB,charge}}, (b) of the prefactor sGB,0ns_{\mathrm{GB},0}^{n}, as well as (c) of the band bending ΦGB\Phi_{\mathrm{GB}}. The net-doping density was NA=1×1015 cm−3N_{\mathrm{A}} = 1 \times10^{15}\ \mathrm{cm}^{-3}, while NGB,chargeN_{\mathrm{GB,charge}} was restricted to 0.06-0.6 (downward) and 0.2-2 ×1011 cm−2\times10^{11}\ \mathrm{cm}^{-2} (upward band bending), sGB,0ns_{\mathrm{GB},0}^{n} to the interval 60-600 cm/s (the median of the experimental sGBs_{\mathrm{GB}} values was about 100 cm/s). The blue bars stand for downward band bending, the red ones for upward band bending.

Case study II: evaluation of recombination velocities at grain boundaries in wafer-based, microcrystalline Si solar-cell

The sGBs_{\mathrm{GB}} values in the following viewgraph were extracted from Sio et al. [9], who determined the recombination velocities at grain boundaries by means of photoluminescence imaging in multicrystalline Si wafers which underwent various treatments (gettered, hydrogenated, as well as gettered and hydrogenated). An interesting fact from this work is that the treated Si wafers do not exhibit smaller sGBs_{\mathrm{GB}} values than the as-cut Si wafer. It is noted by Sio et al. [9] that the applied procedure cannot detect sGBs_{\mathrm{GB}} values of smaller than about 200 cm/s, which definitely has an impact on the magnitudes of the extracted NGB,chargeN_{\mathrm{GB,charge}} and sGB,0ns_{\mathrm{GB},0}^{n} values.

sGB values from a multicrystalline Si wafer as a function of defect density, prefactor, and band bending

Figure A3. sGBs_{\mathrm{GB}} values from a multicrystalline Si wafer (as-cut) [9] as a function of (a) the defect density NGB,chargeN_{\mathrm{GB,charge}}, (b) of the prefactor sGB,0ns_{\mathrm{GB},0}^{n}, as well as (c) of the band bending ΦGB\Phi_{\mathrm{GB}}. The net-doping density was NA=2×1016 cm−3N_{\mathrm{A}} = 2 \times10^{16}\ \mathrm{cm}^{-3}, while NGB,chargeN_{\mathrm{GB,charge}} was restricted to 0.2-2 (downward) and 0.7-7 ×1011 cm−2\times10^{11}\ \mathrm{cm}^{-2} (upward band bending), sGB,0ns_{\mathrm{GB},0}^{n} to the interval 200-2000 cm/s (the median of the experimental sGBs_{\mathrm{GB}} values was about 1000 cm/s). The blue bars stand for downward band bending, the red ones for upward band bending.

References

  1. [1]J. Quirk, M. Rothmann, W. Li, D. Abou-Ras, and K. P. McKenna, Applied Physics Reviews 11, 011308 (2024).
  2. [2]J. Y. W. Seto, Journal of Applied Physics 46, 5247 (1975).
  3. [3]A. G. Aberle, Progress in Photovoltaics: Research and Applications 8, 473 (2000).
  4. [4]J. Brody and A. Rohatgi, Solid-State Electronics 45, 1549 (2001).
  5. [5]H. Neumann and R. Tomlinson, Solar Cells 28, 301 (1990).
  6. [6]B. E. McCandless, W. A. Buchanan, C. P. Thompson, G. Sriramagiri, R. J. Lovelett, J. Duenow, D. Albin, S. Jensen, E. Coalgrove, J. Moseley, H. Moutinho, S. Harvey, M. Al-Jassim, and W. K. Metzger, Scientific Reports 8 (2018).
  7. [7]M. A. Scarpulla, B. McCandless, A. B. Phillips, Y. Yan, M. J. Heben, C. Wolden, G. Xiong, W. K. Metzger, D. Mao, D. Krasikov, I. Sankin, S. Grover, A. Munshi, W. Sampath, J. R. Sites, A. Bothwell, D. Albin, M. O. Reese, A. Romeo, M. Nardone, R. Klie, J. M. Walls, T. Fiducia, A. Abbas, and S. M. Hayes, Solar Energy Materials and Solar Cells 255, 112289 (2023).
  8. [8]D. Abou-Ras, B. Schaffer, M. Schaffer, S. S. Schmidt, R. Caballero, and T. Unold, Physical Review Letters 108, 075502 (2012).
  9. [9]H. Sio and D. Macdonald, Solar Energy Materials and Solar Cells 144, 339 (2016).
  10. [10]M. Krause, A. Nikolaeva, M. Maiberg, P. Jackson, D. Hariskos, W. Witte, J. A. Márquez, S. Levchenko, T. Unold, R. Scheer, and D. Abou-Ras, Nature Communications 11, 4189 (2020).
  11. [11]S. Thomas, W. Witte, D. Hariskos, S. Paetel, C. Song, H. Kempa, M. Maiberg, N. El-Ganainy, and D. Abou-Ras, Progress in Photovoltaics: Research and Applications 33, 265 (2024).
  12. [12]S. Thomas, W. Witte, D. Hariskos, R. Gutzler, S. Paetel, C. Song, H. Kempa, M. Maiberg, and D. Abou-Ras, Progress in Photovoltaics: Research and Applications 32, 930 (2024).
  13. [13]D. Abou-Ras, S. S. Schmidt, R. Caballero, T. Unold, H. Schock, C. T. Koch, B. Schaffer, M. Schaffer, P. Choi, and O. Cojocaru-Mirédin, Advanced Energy Materials 2, 992 (2012).
  14. [14]D. Abou-Ras, S. S. Schmidt, N. Schäfer, J. Kavalakkatt, T. Rissom, T. Unold, R. Mainz, A. Weber, T. Kirchartz, E. S. Sanli, P. A. van Aken, Q. M. Ramasse, H. Kleebe, D. Azulay, I. Balberg, O. Millo, O. Cojocaru-Mirédin, D. Barragan-Yani, K. Albe, J. Haarstrich, and C. Ronning, physica status solidi (RRL) – Rapid Research Letters 10, 363 (2016).
  15. [15]O. Cojocaru-Mirédin, T. Schwarz, and D. Abou-Ras, Scripta Materialia 148, 106 (2018).
  16. [16]S. Sze and K. K. Ng, Physics of Semiconductor Devices, Wiley, 2006.

Paper details

vlnc:W_fwu7qsrn
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents