WorksPhysics and Astronomy
Resolving the Electronic Ground State of La3Ni2O7-δ Films
Abstract
The recent discovery of a superconductivity signature in La3Ni2O7-δ under a pressure of 14 GPa, with a superconducting transition temperature of around 80 K, has attracted considerable attention. An important aspect of investigating electronic structures is discerning the extent to which the electronic ground state of La3Ni2O7-δ resembles the parent state of the cuprate superconductor, a charge transfer insulator with long-range antiferromagnetism. Through X-ray absorption spectroscopy, we have uncovered the crucial influence of oxygen ligands on the electronic ground states of the Ni ions, displaying a charge transfer nature akin to cuprate but with distinct orbital configurations. Both in-plane and out-of-plane Zhang-Rice singlets associated with Ni d_(x^2-y^2 ) and d_(z^2) orbitals are identified, together with a strong interlayer coupling through inner apical oxygen. Additionally, in La3Ni2O7-δ films, we have detected a superlattice reflection (1/4, 1/4, L) at the Ni L absorption edge using resonant X-ray scattering measurements. Further examination of the resonance profile indicates that the reflection originates from the Ni d orbitals. By evaluating the reflection's azimuthal angle dependence, we have confirmed the presence of collinear antiferromagnetic spin ordering and charge-like anisotropy ordered with the same periodicity. Notably, our findings reveal a microscopic relationship between these two components in the temperature dependence of the scattering intensity of the reflection. This investigation enriches our understanding of high-temperature superconductivity in La3Ni2O7-δ under high pressure.
Emails: [email protected], [email protected], [email protected]
Introduction
Unconventional superconductors, such as copper-oxide and iron-based compounds, often show superconductivity alongside the destruction of long-range antiferromagnetic ordering when they reach a critical carrier concentration level through doping. As the doping levels increase, the superconducting state may coexist or compete with various electronically ordered phases [1]. For example, cuprate superconductors may exhibit the development of spin and charge order, known as 'stripe' [2, 3, 4], while several Fe-based superconductors demonstrate electronic nematic order, breaking discrete rotational symmetry near or within the superconducting phase [5, 6, 7]. Understanding the relationship between superconductivity and various emergent electronic orders is crucial for uncovering the mystery of high-temperature superconductivity.
The discovery of the signature of superconductivity in under a pressure of 14 GPa with K has garnered considerable interest recently as a promising high-temperature superconductor derived from a transition metal outside copper-oxides or iron-chalcogenides [8]. Furthermore, these bilayer 327-type nickelates, unlike the infinite layer 112-type nickelates, have a completely different electronic configuration compared to cuprates, i.e., they are not engendered by a (half-filled) Mott state but are potentially more complex ground states. However, the research landscape is intricating, with ongoing debates on whether superconductivity is bulk or filamentary [9, 10, 11, 12], complicated by the reported intergrowth of different Ruddlesden-Popper (RP) phases [13, 14, 15, 16]. Despite the nuances of sample synthesis, substantial theoretical progress has been made in understanding the superconducting mechanism in pressurized [17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39]. However, it is essential to note that the orbital configuration of Ni ions and the role of the oxygen ligands in remain elusive [40, 41, 42, 43]; it is unclear whether it resembles cuprates, which are charge-transfer insulators, or is more akin to infinite-layer nickelates, which are Mott-Hubbard insulators [44, 45, 46, 47, 48, 49]. Besides, the potential for electronic ordering, like long-range antiferromagnetic order, has not been fully resolved [50, 51, 52, 53, 54, 55, 56, 57].
In the present work, we used X-ray absorption spectroscopy (XAS) at the O absorption edge and resonant X-ray scattering (RXS) measurements at the Ni absorption edge to investigate the electronic ground state of single-crystalline LaNiO films. In the electronic structure, we have identified in-plane and out-of-plane mobile carrier peaks linked to the Ni and orbitals, along with substantial interlayer coupling facilitated by the inner apical oxygen. Moreover, we have established the presence of collinear antiferromagnetic spin ordering and anisotropic charge-like ordering with a matching periodicity. Notably, the two orders are interconnected yet display distinct temperature-dependent behaviors. These findings offer pivotal insights into the electronic structures of LaNiO and aid in comprehending the underlying mechanism of electron pairings for superconductivity under pressurized conditions.
RESULTS AND DISCUSSION
Figure 1a plots a schematic of the crystal structure of LaNiO. In Figure 1b, we present the temperature-dependent resistivity measurements on two representative films of LaNiO. These films were synthesized under different oxygen pressures, leading to oxygen variation. The resistivity versus temperature for Film 1 demonstrates insulating behavior. However, for Film 2, the resistivity decreases with decreasing temperature and exhibits an upturn around 80 K, indicating a transition to an insulator. This metal-to-insulator transition is likely due to disorder, given the negligible magnetoresistance across the transition temperature (see supplementary materials for more details). Notably, the resistivity versus temperature for Film 2 resembles that of the bulk crystal, known for its superconductivity under pressure [8]. Since Film 1 was grown with a lower oxygen pressure than Film 2, we anticipate Film 1 to be less stoichiometric than Film 2 regarding oxygen content [40, 41, 43, 58, 59, 60, 61, 62]. The stark contrast in resistivity as a function of temperature between the two films may arise from the variation in oxygen content, which could be crucial in understanding the electronic structure and origin of the superconductivity of this material under pressure [8, 9, 10, 11, 61].

Figure 1. Superlattice reflection with wave vector at in La₃Ni₂O₇. a, Crystal structure of La₃Ni₂O₇ with lattice parameters Å and Å. The green, blue, and red solid circles represent La, Ni, and O atoms, respectively. b, The temperature-dependent resistivity for two typical films of La₃Ni₂O₇₋δ; the dashed line represents the resistivity measurement of a La₃Ni₂O₇ single crystal in ref. [8] and is rescaled for clarity. c, Reciprocal space map of the position of the resonant diffraction peaks in La₃Ni₂O₇. d, A schematic of the RXS scattering geometry. e, Representative momentum scans across the wave vector measured at K and eV with polarized (red open circle) and polarized (blue open circle) incident photons. The solid lines fit the data using the Lorentz profiles and a linear background.
Figure 1c and Figure 1d illustrate the scattering geometry of the RXS experiments. We use a pseudo-cubic notation in defining the unit cell and use reciprocal lattice units (r. l. u.) for the reciprocal space (, , ) components, which are given in units of . At K, the in-plane lattice constants are Å, and the out-of-plane lattice constant is Å. We have observed superlattice reflections at with photon energy tuned near the Ni absorption edge. This reflection exhibits strong photon polarization dependence, as shown in Figure 1e. It appears much stronger in - than in - polarized incidence geometry, consistent with the recent report on bulk crystal LaNiO [54]. Such a photon polarization dependence suggests that the resonant reflection might be magnetic [54, 63].
In Figure 2a, we present the X-ray absorption spectra (XAS) for both films at the O -edge and the corresponding X-ray linear dichroism (XLD) to uncover the orbital configurations of the Ni ions and the influence of oxygen ligands. According to the Zaanen-Sawatzky-Allen (ZSA) scheme, which classifies insulators into Mott-Hubbard and charge-transfer types, the role of ligands in determining the smallest energy gap of the charge excitations becomes evident [62]. The charge-transfer nature manifests as a pre-edge peak in the oxygen -edge XAS [64]. We observe clear pre-edge peaks in O -edge XAS in both films around a photon energy of eV. They exhibit apparent polarization dependence: a sharp peak with in-plane polarization and two broad peaks with out-of-plane polarization. This indicates that the oxygen ligands significantly influence the electronic ground state of Ni cations. Notably, the XLD analysis of the difference of pre-edge peaks with different polarization enables us to deduce the Ni orbital configurations through - hybridization within the NiO bilayers. As shown in Figure 2a, the main peak at ~528 eV with the in-plane polarization shows little sample dependence, consistent with Zhang-Rice singlet state in cuprate. Intriguingly, the two dips flanking the main peak with the out-of-plane polarization exhibit slight sample dependence, reflecting the strong hybridization of the inner apical O and the Ni orbital and the formation of an out-of-plane Zhang-Rice singlet state in bilayer nickelates. The energy difference of ~1.2 eV between the two dips is approximately two times that for the interlayer hopping of the orbitals revealed from the density functional calculations [8, 65, 66]. Thus, these two dips correspond to the interlayer bonding and antibonding states, as illustrated in Figure 2b. This contrasts with the recent angle-resolved photoemission spectroscopy (ARPES) measurements on a bulk crystal , where the correlation effects were proposed to push the bonding states derived from the orbitals downward by about 50 meV below the Fermi level [66]. Such discrepancy may arise from the variance in oxygen concentration and its impact on covalency (mainly through the apical oxygen) and/or the Fermi level position and the external pressure from substrates. As shown in Figure 2a, the energy of the bonding states from the orbitals appears to be more sensitive to the possible oxygen variation compared with the antibonding state from the orbitals and the bands from the [67], consistent with the observed prominent inner apical oxygen vacancy [43].

Figure 2. X-ray absorption spectra (XAS), and energy profiles of the resonant reflections in LaNiO. a, The X-ray absorption spectra (XAS) and X-ray linear dichroism (XLD) near the O-K edge for Film 1 (red color) and Film 2 (blue color). The XAS are offset for clarity. b, Schematic density of states of LaNiO and the corresponding bonding and antibonding orbitals. c, Energy profiles of the resonant reflection at near the Ni- absorption edge with - and - polarizations, and the peak intensity is maximized at eV. d, Energy scans at constant wavevector on and off the using different photon polarizations for two LaNiO films. The solid lines corresponds to the energy scans on , while the dashed lines correspond to that off the . The curves are offset for clarity.
We conducted momentum scans along high symmetry directions in momentum space for a comprehensive search of translational symmetry-breaking signatures. This led us to the observation of a superlattice peak (SP) at the wave vector in our films, as shown in Figure 2c. To further understand the nature of this reflection, we performed momentum scans across the with various photon energies. The results, depicted in Figure 2c, demonstrate the resonant enhancement of the scattering signals, with a more pronounced increase in the scattered signal when using -polarized incident photons, suggesting the magnetic nature of the reflection. In Figure 2d, we present the energy scans with wave vectors fixed at , which reproduce the energy profiles in Figure 2c. To provide a reference, we also repeated the energy scans slightly off this wave vector to characterize the scattering background under an identical geometry. The spectra taken slightly off the exhibit much weaker signals (primarily resulting from fluorescence) than those measured at the wave vector, confirming the electronic nature of the reflection at .
Figure 3a and Figure 3b summarize the temperature dependence of the scattered intensity of the reflection at with - and -polarized incident photons, respectively. Figure 3a reveals a clear transition at K for both films. Figure 3c-Figure 3d show the representative scans using -polarized incident photons at various temperatures, confirming vanishing intensity above 150 K. This transition at K aligns with the earlier studies [42, 52, 53, 54, 55], suggesting the transition from magnetic ordering. However, surprisingly, the measurements with -polarized incident photons show different characteristics. The temperature dependence of the scattered signals takes an entirely different turn, exhibiting three characteristic temperatures near K, 150 K, and 110 K, respectively. The corresponding representative scans in Figure 3e-Figure 3f show the vanishing intensity near K. This unexpected behavior is a fascinating twist in our understanding. While the transition at K likely mirrors the same transition as revealed in the channel, the transition at K suggests a different type of order with the same wave vector that already occurs about 50 K above the proposed magnetic order at K. Furthermore, the peak intensity starts decreasing at K as decreasing temperature, in sharp contrast to that measured in the channel.

Figure 3. Temperature dependence of the intensity of the resonant peak at . a, b, The diffraction peak intensity as a function of temperature taken with (a) and (b) polarized incident light at 852.2 eV for the films. The dashed lines mark the transition temperature. c, d (e, f), Representative momentum scans across the wave vector for Film 1 and Film 2 measured with () polarization at various temperatures. The circle and triangle correspond to Film 1 and Film 2, respectively.
The discrepancy in the measurements of the scattering intensity versus temperature using the - and -polarized incident photons indicates that the superlattice reflection at may contain multiple components. Therefore, we conducted a symmetry-restricted tensorial examination of the azimuthal angle dependence of the scattered intensity to resolve the electronic texture underlying the superlattice reflection.
The scattered intensity of the resonant reflection is given below [68, 69, 70],
where represents the polarization of incoming (outgoing) photons, and stands for the wave vector of the incoming (outgoing) photons. and stand for the position of the atom and its scattering tensor, respectively. The polarization of the incident photons is resolved between the σ- and π-channel in the measurements, while outgoing photons are not polarization resolved. Therefore, we measured when using π-polarized incoming photons, and when using σ-polarized incoming photons.
We propose different ordered electronic motifs with an in-plane wavevector (1/4, 1/4) aligned with the wavevector revealed in the measurements. In Figure 4a, we enforce the antiparallel alignment of next-nearest-neighboring spins while allowing the nearest-neighboring spins to align randomly except for being antiparallel; this comprises both collinear (double spin stripe) and non-collinear antiferromagnetism. In Figure 4b, we propose a spin-charge stripe pattern that enforces the antiparallel alignment of next-nearest-neighboring spins with spinless charge domains; this would imply charge order with an in-plane wavevector (1/2, 1/2), double that of spin order. Figure 4c shows the measurements for the scattering intensity ratio π/σ as a function of the azimuthal angle. It turns out that the model of the spin-charge stripe cannot give a satisfactory fit to the measurements. The dashed curve represents the modeling of the spin-charge stripe with the magnetic moment pointing along the (1 -1 0) direction, as illustrated in Figure 4b. This model substantially deviates from the measurements. We then explore a model with the spin textures as illustrated in Figure 4a, and find both the non-collinear magnetic structures and double spin stripe yield a better agreement with the data, as indicated by the solid red curve from the fit to the data (see the Supplementary materials for further information). However, it still significantly deviates from the observed intensity ratios. Considering that the models of both collinear and complex magnetic spin textures cannot give a satisfactory fit to the data, we expect the likely presence of an anisotropic charge distribution that further lowers the symmetry on the spinless sublattices, as illustrated with green ellipses in Figure 4b. A fit using the model that consists of both charge anisotropy and collinear antiferromagnetic spin order is given by the solid light blue curve in Figure 4c, exhibiting a significantly improved agreement to the measurement, yielding the collinear antiferromagnetic spin ordering with spin moment primarily pointing along the orientation (see the Supplementary Materials for details).

Figure 4. Azimuthal angle dependence of the resonant reflection at (1/4, 1/4, 1.9) in LaNiO. a, b, A schematic of spin configuration illustrating the magnetic structure in real space. a shows spin configuration that can be both non-collinear antiferromagnetism (NCM) and collinear antiferromagnetism (CM). b shows spin-charge stripe configurations with charge anisotropy on the spinless sublattices (CM + charge anisotropy). The blue and red solid circles represent the spin and charge sublattices, respectively; brown arrows denote the spin momentum directions. The green shaded areas indicate the presence of charge anisotropy lowering the local symmetry on the spinless sublattices. c, Azimuthal dependence of the integrated intensity of the reflection (1/4, 1/4, 1.9) at 20 K (where not shown, the error bars are within the symbol size). The azimuthal angle corresponds to a sample orientation where the (1 1 0) orientation lies within the scattering plane. The solid blue lines represent the best fit for a model illustrated in (b), while the solid red line corresponds to the best fit illustrated in (a) corresponding to noncollinear spin configurations. The model of the spin-charge stripe without charge anisotropy does not seem to converge in the fit regardless of the initial parameters; the dashed line represents the simulation of the spin-charge stripe with the spin momentum direction fixed to the (1 -1 0)
The discovery of two components contributing to the resonant reflection at from the symmetry-restricted tensorial analysis naturally explains the remarkable differences in the scattering intensity measurements versus temperature when using - and -polarized incident photons. In particular, the scattering tensor for the charge anisotropy contains only the diagonal components dominating the - channel. The scattering intensity versus temperature measured using the -polarized incoming light mainly reflects the presence of charge anisotropy that emerges around K, followed by the collinear spin ordering at K. Notably, the transition at K agrees with earlier studies using various experimental techniques [42, 52, 53, 54, 55, 57]. The sudden decrease in scattering intensity at K coincides with the characteristic temperature of the anomaly observed in various measurements [42, 51], which is proposed to originate from a density wave intimately linked to the orbital-derived Fermi surface topology [51].
In summary, we have revealed the electronic motif and the corresponding thermal dynamics in oxygen-varying films of using X-ray absorption spectroscopy and resonant X-ray scattering. We have uncovered the pivotal role of oxygen ligands, which hybridize with the Ni orbitals, forming the ZhangRice-like bands. However, unlike cuprates in which only the hybridization between O-2p and Cu dominates the lower energy physics, in our LaNiO films, both the Ni and hybridize with the in-plane O- orbitals, and apical O- orbitals, as manifested by the pre-edge peak at the O edge XAS, suggesting both the Ni- and play essential roles in the low-energy physics in LaNiO[8, 17, 19, 20, 21, 31].
The revelation of the possible spin ordering at at K in our film samples aligns with the recent studies on the bulk crystals [54]. More subtly, our azimuthal angle measurements, along with the symmetry-restricted tensorial analysis, suggest the presence of an aspherical charge distribution at the sublattices of the spinless sites in the spin-charge model resulting in two components in the reflection at . The ordering due to the charge anisotropy exhibits two characteristic temperatures at K and K. Note that our symmetry-restricted tensorial analysis cannot pinpoint the source accounting for the transition at K since any ordering of charge-like anisotropy would assume a similar format of a diagonal matric tensor. One possibility is that an ordered Jahn-Teller effect may exist on the spinless sublattices [71], leading to charge anisotropy. Another possibility is the presence of a magnetic quadrupole ordering on the spinless sites, which is compatible with our symmetry analysis (see the supplementary materials for further information).
Studying the electronic ground state of LaNiO films with varying oxygen concentrations could have important implications for understanding the superconductivity discovered under pressurized conditions. In unconventional superconductors, various orderings, such as spin order, charge order, and spin-charge stripe, often appear to compete with superconductivity. Perturbations such as applying strain, pressure, or magnetic field can disrupt the balance between the superconducting phase and other competing orders. This scenario may also apply to LaNiO, where high pressure could suppress the spin-charge stripe while enhancing superconductivity. Notably, the resonant reflection at in the film grown at lower oxygen pressure exhibits a much higher intensity than that in the film grown at higher oxygen pressure. The resistivity versus temperature in the high oxygenated film resembles that of the bulk samples which become superconducting under pressure. Variations in oxygen levels may have already suppressed the spin-charge ordering to some extent, thereby aiding pressure in eliminating it and enabling the full emergence of superconductivity.
orientation. The inset in c shows a schematic of the scattering geometry of azimuthal angle-dependent measurements.
Methods
Sample preparation. Thin films of the precursor phase with a thickness of nm were prepared using pulsed laser deposition (PLD) on (001)-oriented substrates with a 248-nm KrF excimer laser. The substrate was kept at during growth under an oxygen partial pressure of 150 mTorr. After deposition, the films were cooled to room temperature at per minute in the oxygen partial pressure of 100 Torr.
XAS and RXS measurements. The X-ray absorption spectroscopy (XAS) and resonant x-ray scattering (RXS) measurements at the Ni -edge and O- edge were performed at the REIXS (10ID-2) beamline of the Canadian Light Source (CLS). At these photon energy ranges, the beamline provides a photon flux of about photons per second with energy resolution . An in-vacuum 4-circle diffractometer hosts the endstation under an ultra-high vacuum (UHV) condition below mbar. The XAS spectra were collected in both total fluorescence yield (TFY) and total electron yield (TEY) modes at 20 K with linear vertical () and horizontal () light polarizations. The XAS spectra are normalized to the incident photon flux. The RXS spectra are extracted after a Lorentzian fitting with a linear background.
Acknowledgment
This work was supported in part by the National Key Research and Development Program of China (Grant No. 2022YFA1403900 and 2021YFA1401800), the National Natural Science Foundation of China (Grant No. 12074411), the Strategic Priority Research Program (B) of the Chinese Academy of Sciences (Grant No. XDB25000000), and the Synergetic Extreme Condition User Facility (SECUF).
Part of the research described in this paper was performed at the Canadian Light Source, a national research facility of the University of Saskatchewan, which is supported by the Canada Foundation for Innovation (CFI), the Natural Sciences and Engineering Research Council (NSERC), the Canadian Institutes of Health Research (CIHR), the Government of Saskatchewan, and the University of Saskatchewan.
Author contributions: Z.H.Z. and X.J.Z. conceived the research. X.L.R. prepared and characterized the film samples. X.L.R., R.S., and Z.H.Z. performed the RXS experiments. X.L.R., Z.H.Z, R.C., and H.H. analyzed the experimental data. T.X., J.P.H., X.X.W., and J.F.Z. provided theoretical guidance with DFT calculations. X.L.R. and Z.H.Z. wrote the manuscript with the input of all co-authors.
Supplementary Material for Resolving the electronic ground state of LaNiO films
Xiaolin Ren; Ronny Sutarto; Xianxin Wu; Jianfeng Zhang; Hai Huang; Tao Xiang; Jiangping Hu; Riccardo Comin; X. J. Zhou; Zhihai Zhu
Film Growth and Characterizations
The films with a thickness of about 30 nm were grown by the PLD using a 248-nm KrF excimer laser (COMPex 201, Coherent). During growth, the substrate temperature was maintained at 750 °C, and the oxygen partial pressure was 150 mTorr for Film 1 and 200 mTorr for Film 2, respectively. After deposition, the films were cooled to room temperature at a rate of 5 °C/min with an oxygen partial pressure of 100 Torr. The pulse-to-pulse repetition rate was set to 4 Hz, and the pulse laser energy was set to 500 mJ. The laser target is a chemically measured mixture containing (Alfa Aesar, 99.99%) and NiO (Sigma Aldrict-Chemie GmbH, 99.995%) prepared by a solid-state reaction, the pellets were heated in air at three °C/min to 1100 °C and held for 12 h.
Figure S1 shows a - scan of the out-of-plane XRD patterns for two typical films grown on (001) substrates, identifying the right structural phase, i.e., Ruddlesden–Popper (RP) perovskites of . Film 1 has a smaller lattice constant (20.3126 Å) than Film 2 (21.1105 Å). Figure S1 and Figure 1c show the reciprocal space map (RSM) around the (1 0 17) peaks of Film 1 and Film 2, respectively, confirming that the films are epitaxially grown on substrates and coherently strained by the substrates. Figure S2 shows the resistivity versus temperature under various magnetic fields for Film 2. A metal-to-insulator transition occurs around 80 K, but it does not show any response to the applied magnetic field. It suggests the meal-to-insulator transition likely arises from the disorder.

Figure S1. Epitaxial growth of high-quality LaNiO films on LaAlO (001) substrates. a, The out-of-plane X-ray diffraction (XRD) patterns for two LaNiO films. b, c, Reciprocal space maps (RSM) of the (1 0 17) reflection for Film 1 and Film 2, respectively.

Figure S2. Resistivity versus temperature under various magnetic fields of a typical LaNiO sample.
STEM Characterizations
In the scanning transmission electron microscopy (STEM) images in Figure S3, the distinction between atoms of different brightness, based on the difference in atomic number, is evident. The interface between the substrate and the two films is clearly visible. By comparing the high-angle annular dark field (HAADF) STEM images shown in Figure S3 and 3c and Annular Bright Field (ABF) STEM images shown in Figure S3 and S3d, we find that the perovskite structure of the substrate and the RP structure of the film are orderly arranged along the -axis without any noticeable defects or other phases. Despite the different growth oxygen partial pressure along with the difference in transport measurements on the two films, no discernible difference in microstructure is observed. However, we seem to have a poorer resolution, which does not allow us to detect the likely presence of oxygen defects as reported in bulk samples [1].

Figure S3. Scanning transmission electron microscopy (STEM) images for two LaNiO films. a (c), b (d), The high-angle annular dark field (HAADF) STEM and the annular bright field (ABF) STEM images of Flm1 (Film 2), respectively. e, The schematics of the crystal structures of the LaNiO films.
X-ray absorption spectra collected at the La -edge and Ni -edge on LaNiO films
Figure S4 shows the normalized X-ray absorption spectra (XAS) collected via the total electron yield (TEY) mode at the La -edge and the Ni -edge for Film 1 and Film 2, the same films studied in the main text. The salient peaks at 833 eV and 850 eV correspond to the La () and the La () absorption edges, respectively, while the relatively weaker peaks at 852 eV and 870 eV correspond to the Ni () and the Ni () absorption edges, respectively. The energy difference between the peak maximum of the XAS at the La and the Ni is about 2 eV. The superlattice peak at the wave vector in LaNiO appears only at the Ni absorption edge, in sharp contrast to the infinite-layer nickelates in which superlattice peaks show up at both the Ni edges and the rare earth (La, Nd, and Pr) edges [2, 3, 4, 5, 6]. The double-peak feature at the Ni absorption edge resembles that measured from the bulk crystal [7]. In analogous to the cuprates, the double peaks may be ascribed to different final states of the Ni ions: Ni- and Ni-, where denotes the oxygen ligands. By performing X-ray linear dichroism (XLD) analysis, we find that the out-of-plane XAS peak has a higher intensity than that of in-plane XAS at 852.2 eV, which indicates that the holes primarily occupy the orbital. In contrast, the out-of-plane XAS peak shows a lower intensity than the in-plane XAS peak at eV, suggesting the holes primarily occupy the orbital when the oxygen ligands are at play.

Figure S4. XAS of LaNiO films collected at the La- edge and the Ni- edge via total electron yield (TEY) mode. The XAS at the La edge and the Ni edge of two LaNiO films with the linear photon polarization perpendicular () and parallel () to the films’ axis. The inset shows an enlarged view of XAS near the Ni- absorption edge along with the XLD analysis.
Overall, the XAS for two LaNiO films appears similar, implying a nearly identical electronic configuration of the Ni orbital configurations for the two films.
Density of States of bulk LaNiO
Figure S5 shows the orbital-resolved density of states (DOS) for bulk LaNiO. It is apparent that the low-energy physics is dominated by the and orbitals and they exhibit strong hybridization with O and orbitals. The strong interlayer coupling between orbital through the inner apical oxygen generates bonding and antibonding states. The bonding state is almost fully filled, while the antibonding state is empty. These orbital characteristics and hybridization can account for the pre-edge XAS peaks at the O-K edge shown in Figure 2a.

Figure S5. Orbital-resolved DOS for bulk LaNiO. The d (d) denotes the interlayer bonding (antibonding) state. The Ni orbital shows strong hybridization with O orbitals, while Ni exhibits strong hybridization with O orbital.
dependence of the charge order in LaNiO films
In Figure S6, we show the dependence of the scattering intensity across the wavevector in the LaNiO films. The measurements were taken at K with the incident photons being polarized and the energy eV. Figure S6 represents the momentum scans across the wave vector for Film 1 (red) and Film 2 (blue). For both films, the superlattice peak exhibits weak but definite dependence with a maximum at . In Figure S6, we also show the momentum scan along for Film 1, exhibiting a similar weak dependence of the peak intensity.

Figure S6. dependence of the superlattice peak at in LaNiO films. a, dependence of the scattering intensity measured at 20 K for LaNiO films with the -polarized incident photons of energy eV (near the Ni edge); the fitting to the data using the Gaussian profile is given by the black solid line. b, The momentum scans across the wavevector with a series of values. The spectra are shifted vertically for clarity.
By fitting the data with the Gaussian profile (black solid line), we obtain the correlation length Å along , suggesting a quasi-2D nature of the reflection at .
Symmetry-restricted tensorial analysis.
As illustrated in Figure 4a and 4b in the main text, we can define structure factors as , where labels the atomic sites on the square lattice. Here, we do not consider the ordering pattern normal to the - plane since the reflections are observed at the wave vector . The structure factor at can be written as . In the model, as illustrated in Figure 4a, we assume , , and . These restrictions cover three typical spin patterns: spin-charge stripe, double spin stripe, and non-collinear spin ordering. We can label the structure factors , , , and , respectively, at the atomic positions , , , and . The total structure factor is calculated as , which can be simplified to with , . The atomic scattering tensor can be written as
where represents the coefficient for the pure magnetic term and depends on the photon energy.
In Figure 4b, we introduce charge anisotropy in the spinless sublattices. The scattering tensor for the anisotropic charge distribution can be written as
where coefficient is a function of photon energy and a real value. This diagonal tensor can represent the anisotropic charge distribution arising from magnetic quadrupolar contribution. The total structural factor is written as
where we have assumed that symmetry breaking occurs primarily in the ab-plane by setting .
We can define the magnetic momentum by spherical coordinates,
, where represents the magnitude of the spin moment, and and represents angles of the spin moment relative to the crystallographic axes and , respectively. The light polarization is defined in the crystallographic coordinate frame involving the scattering vector and a second arbitrary vector that must be perpendicular to , named as . We have the following formula for the vectors and photon polarizations and [8]:
Where presents the angle between and , and is the azimuthal angle. The scattered intensity of the resonant reflection is given:
Where represents the photon polarizations whose formulas are given in eq. (5).
The spin-charge stripe does not fit the data well, so we explored the complex magnetic structure, double spin stripe, and a combination of spin-charge stripe and charge-like anisotropy. We found that selecting different initial parameters in our fitting process resulted in a good fit in two different regions of the parameter spaces, corresponding to two typical spin textures of noncollinear antiferromagnetism and double spin stripe (shown in Figure S7, Figure S7). The best-fit results for these two spin textures are shown in Figure S7 as the solid and dashed lines. The fitting parameters (, , ) for the spin moments are and for the solid line in Figure S7, and and for the dashed line in Figure S7. However, these fitting parameters may vary depending on the initial parameters chosen in the nonlinear fit. After numerous attempts, we found that using non-collinear antiferromagnetic and double spin stripe spin models did not improve the fit shown in Figure S7. While they fit the data better than the spin-charge stripe model, they still substantially deviate from the measurements. The fit using a combination of spin-charge stripe and charge-like anisotropy significantly improved the agreement with the data, as shown in Figure 4c. In the best fit to the data set, as shown by the solid blue curve in Figure 4c in the main text, we found is approximately -0.72, with the spin momentum pointing dominantly along the (1 -1 0) orientation, with the out-of-plane canting of 15°. It is worth noting that this model has one less fitting parameter than noncollinear antiferromagnetism and double spin stripe models. One possible explanation for this anisotropic scattering is that an ordered Jahn-Teller effect may exist on the spinless sublattices[9] that can naturally introduce the tensor with the formula shown in eq. (3) and is compatible with the negative value of . Another possibility is that magnetic quadrupole order in the spinless sublattices leads to the anisotropic scattering from the mixture of dipole-quadrupole in eq. (4). If we only consider the spherical symmetry and assume that the local momentum is mainly pointing in the crystallographic plane, we can define the direction of the local moment as . The scattering tensor for the quadrupole terms can be written as:

Figure S7. Azimuthal angle dependence of the scattered intensity of resonant reflection at . a, b, Schematics of non-collinear antiferromagnetism (NCM) and double stripe in real space. c, The dashed and solid lines represent the best fit to the measurement, corresponding to the non-collinear antiferromagnetism and double stripe spin texture, respectively.
where describes magnetic linear dichroism and is a real value [8]. It is possible that the slight change in the magnetic quadrupole moments further lowers the local symmetry on the spinless sites.
For example, consider that for , and for , where , one finds that
By comparing the second term in eq. (4) and eq. (8), one finds that , which is close to the value of -0.72 from our fitting.
DFT calculation method and results
The spin order and characteristic wave vector of system in ambient Amam phase was further studied by the Density Functional Theory (DFT) [10, 11] calculation as implemented in the Vienna ab initio Simulation Package (VASP) [12, 13]. The calculations were carried out within the orthorhombic convention cell of the Amam phase as shown in Figure 1a. The generalized gradient approximation (GGA) of Perdew-Burke-Ernzerhof (PBE) [14] type was adopted for the exchange-correlation functional. The kinetic energy cutoff of plane-wave basis was set to be 500 eV. The Gaussian smearing method with a width of 50 meV was employed for the Fermi surface broadening.
The lattice constants and internal atomic positions were fixed at our relaxed results in non-magnetism calculation ( Å, Å, Å). An -point mesh was used for the Brillouin zone (BZ) sampling of this orthorhombic conventional cell and will be proportionally reduced in other magnetism supercell calculations.
Plentiful collinear spin configurations within the bilayer square lattice were studied. By analysis of our calculation results, we found the spin exchange between two Ni-O layers in this bilayer system consistently favors anti-ferromagnetic. This suggests the stable interlayered antiferromagnetic ground state. Therefore, in our subsequent discussions, we will solely concentrate on the spin configurations within a single layer while fixing the interlayered spin configuration at anti-ferromagnetic. Some typical single layered spin configurations in our calculations were exhibited in Figure S8 a-h and their related energy differences can be found in Table S1. Here the energy reference was set to the energy of non-magnetic state. In Table S1, the Double Stripe2 configuration proposed in [7] exhibits the lowest energy, indicating the magnetic ground state of in the Amam phase. The corresponding wave vector is (1/4, 1/4), consistent with our observation on . This result also implies that the PBE functional [14] without other corrections can also capture the partial spin-wave character of this system. Nevertheless, we also carried out the Dudarev-type DFT+ calculations [15]. When we set eV, we found the magnetism ground state of the system will change to a typical G-AFM state with a characteristic wave vector of (1/2, 1/2). This suggests that the DFT+ strategy might excessively correct the correlation effect on Ni electrons, potentially overshadowing other crucial factors. Notably, similar results were also reported in a recent first-principles calculation study on for its Fmmm phase [16].

Figure S8. FIG. S8: Colinear spin configurations within single Ni-O layer. a-h, The interlayered spin configuration was fixed at anti-ferromagnetic. The red and blue dots signed the Ni atoms with opposite spin directions. The grey dots in panel (g) signed the non-magnetic Ni atoms. The green dotted lines frame out their spin superlattice and the corresponded characteristic wave-vector were also denoted below.
| Magnetism | Energy | Wave vector | Moment |
| NM | 0.0 | (0, 0) | 0.0 |
| FM | -4.21 | (0, 0) | 0.175 |
| Neel | -20.98 | (1/2, 1/2) | 0.563 |
| Stripe | -32.91 | (1/2, 0) | 0.748 |
| Dimer Stripe | -26.77 | (1/4, 1/2) | 0.748 |
| Dimer | -41.78 | (1/4, 1/2) | 0.713 |
| Cluster | -40.27 | (±1/4, ±1/4) | 0.755 |
| Double Stripe1 | *, -27.69 | (1/4, 1/4) | *, 0.854 |
| Double Stripe2 | -51.87, -42.60 | (1/4, 1/4) | 0.788, 0.754 |
Table S1. TABLE S1: The energy comparison (in units of meV/Ni) between different spin configurations in Figure S7. The third and fourth column are their characteristic wave-vectors and average magnetic moments (in units of ). The two values in Double Stripe1 and Double Stripe2 configurations respectively correspond to two vertical stripy directions, whose degeneration was broken in the Amam phase of $\mathrm{La}_{3}\mathrm{Ni}_{2}\mathrm{O}_{7} at ambient pressure. The asterisk in Double Stripe1 denotes the calculation doesn’t converge to our specified spin configuration.
References
- [1]Keimer, B., Kivelson, S. A., Norman, M. R., Uchida, S. & Zaanen, J. From quantum matter to high-temperature superconductivity in copper oxides. Nature 518, 179-186 (2015).
- [2]Moodenbaugh, A., Xu, Y., Suenaga, M., Folkerts, T. & Shelton, R. Superconducting properties of La₂−ₓBaₓCuO₄. Physical Review B 38, 4596 (1988).
- [3]Tranquada, J., Sternlieb, B., Axe, J., Nakamura, Y. & Uchida, S.-i. Evidence for stripe correlations of spins and holes in copper oxide superconductors. Nature 375, 561-563 (1995).
- [4]Choi, J. et al. Unveiling unequivocal charge stripe order in a prototypical cuprate superconductor. Physical Review Letters 128, 207002 (2022).
- [5]Fisher, I. R., Degiorgi, L. & Shen, Z. In-plane electronic anisotropy of underdoped ‘122’Fe-arsenide superconductors revealed by measurements of detwinned single crystals. Reports on progress in Physics 74, 124506 (2011).
- [6]Chu, J.-H., Kuo, H.-H., Analytis, J. G. & Fisher, I. R. Divergent nematic susceptibility in an iron arsenide superconductor. Science 337, 710-712 (2012).
- [7]Kasahara, S. et al. Electronic nematicity above the structural and superconducting transition in BaFe₂(As₁−ₓPₓ)₂. Nature 486, 382-385 (2012).
- [8]Sun, H. et al. Signatures of superconductivity near 80 K in a nickelate under high pressure. Nature 621, 493-498 (2023).
- [9]Jun, H. et al. Emergence of High-Temperature Superconducting Phase in Pressurized La₃Ni₂O₇ Crystals. Chinese Physics Letters 40, 117302 (2023).
- [10]Zhang, Y. et al. High-temperature superconductivity with zero-resistance and strange metal behavior in La₃Ni₂O₇. arXiv preprint arXiv:2307.14819 (2023).
- [11]Wang, G. et al. Pressure-induced superconductivity in polycrystalline La₃Ni₂O₇. arXiv preprint arXiv:2309.17378 (2023).
- [12]Zhou, Y. et al. Evidence of filamentary superconductivity in pressurized La₃Ni₂O₇ single crystals. arXiv preprint arXiv:2311.12361 (2023).
- [13]Puphal, P. et al. Unconventional crystal structure of the high-pressure superconductor La₃Ni₂O₇. arXiv preprint arXiv:2312.07341 (2023).
- [14]Chen, X. et al. Polymorphism in the Ruddlesden–Popper Nickelate La₃Ni₂O₇: Discovery of a Hidden Phase with Distinctive Layer Stacking. Journal of the American Chemical Society 146, 3640-3645 (2024).
- [15]Wang, H., Chen, L., Rutherford, A., Zhou, H. & Xie, W. Long-range structural order in a hidden phase of Ruddlesden–Popper bilayer nickelate La₃Ni₂O₇. Inorganic Chemistry 63, 5020-5026 (2024).
- [16]Abadi, S. N. et al. Electronic structure of the alternating monolayer-trilayer phase of La₃Ni₂O₇. arXiv preprint arXiv:2402.07143 (2024).
- [17]Luo, Z., Hu, X., Wang, M., Wú, W. & Yao, D.-X. Bilayer Two-Orbital Model of La₃Ni₂O₇ under Pressure. Physical Review Letters 131, 126001 (2023).
- [18]Zhang, Y., Lin, L.-F., Moreo, A. & Dagotto, E. Electronic structure, dimer physics, orbital-selective behavior, and magnetic tendencies in the bilayer nickelate superconductor La₃Ni₂O₇ under pressure. Physical Review B 108, L180510 (2023).
- [19]Yang, Q.-G., Wang, D. & Wang, Q.-H. Possible s±-wave superconductivity in La₃Ni₂O₇. Physical Review B 108, L140505 (2023).
- [20]Lechermann, F., Gondolf, J., Bötzel, S. & Eremin, I. M. Electronic correlations and superconducting instability in La₃Ni₂O₇ under high pressure. Physical Review B 108, L201121 (2023).
- [21]Gu, Y., Le, C., Yang, Z., Wu, X. & Hu, J. Effective model and pairing tendency in bilayer Ni-based superconductor La₃Ni₂O₇. arXiv preprint arXiv:2306.07275 (2023).
- [22]Shen, Y., Qin, M. & Zhang, G.-M. Effective Bi-Layer Model Hamiltonian and Density-Matrix Renormalization Group Study for the High-Tc Superconductivity in La₃Ni₂O₇ under High Pressure. Chinese Physics Letters 40, 127401 (2023).
- [23]Sakakibara, H., Kitamine, N., Ochi, M. & Kuroki, K. Possible High Tc Superconductivity in La₃Ni₂O₇ under High Pressure through Manifestation of a Nearly Half-Filled Bilayer Hubbard Model. Physical Review Letters 132, 106002 (2024).DOI
- [24]Shilenko, D. & Leonov, I. Correlated electronic structure, orbital-selective behavior, and magnetic correlations in double-layer La₃Ni₂O₇ under pressure. Physical Review B 108, 125105 (2023).DOI
- [25]Lu, C., Pan, Z., Yang, F. & Wu, C. Interlayer-coupling-driven high-temperature superconductivity in La₃Ni₂O₇ under pressure. Physical Review Letters 132, 146002 (2024).
- [26]Liao, Z. et al. Electron correlations and superconductivity in La₃Ni₂O₇ under pressure tuning. Physical Review B 108, 214522 (2023).
- [27]Qu, X.-Z. et al. Bilayer t−J⊥ Model and Magnetically Mediated Pairing in the Pressurized Nickelate La₃Ni₂O₇. Physical Review Letters 132, 036502 (2024).DOI
- [28]Yang, Y.-f., Zhang, G.-M. & Zhang, F.-C. Interlayer valence bonds and two-component theory for high-Tc superconductivity of La₃Ni₂O₇ under pressure. Physical Review B 108, L201108 (2023).
- [29]Tian, Y.-H., Chen, Y., Wang, J.-M., He, R.-Q. & Lu, Z.-Y. Correlation effects and concomitant two-orbital s±-wave superconductivity in La₃Ni₂O₇ under high pressure. Physical Review B 109, 165154 (2024).DOI
- [30]Wú, W., Luo, Z., Yao, D.-X. & Wang, M. Superexchange and charge transfer in the nickelate superconductor La₃Ni₂O₇ under pressure. Science China Physics, Mechanics & Astronomy 67, 117402 (2024).DOI
- [31]Liu, Y.-B., Mei, J.-W., Ye, F., Chen, W.-Q. & Yang, F. s±-Wave Pairing and the Destructive Role of Apical-Oxygen Deficiencies in La₃Ni₂O₇ under Pressure. Physical Review Letters 131, 236002 (2023).DOI
- [32]Huang, J., Wang, Z. & Zhou, T. Impurity and vortex states in the bilayer high-temperature superconductor La₃Ni₂O₇. Physical Review B 108, 174501 (2023).
- [33]Jiang, K., Wang, Z. & Zhang, F.-C. High-temperature superconductivity in La₃Ni₂O₇. Chinese Physics Letters 41, 017402 (2024).
- [34]Cao, Y. & Yang, Y.-f. Flat bands promoted by Hund's rule coupling in the candidate double-layer high-temperature superconductor La₃Ni₂O₇ under high pressure. Physical Review B 109, L081105 (2024).DOI
- [35]Qin, Q. & Yang, Y.-f. High-Tc superconductivity by mobilizing local spin singlets and possible route to higher Tc in pressurized La₃Ni₂O₇. Physical Review B 108, L140504 (2023).
- [36]Chen, X., Jiang, P., Li, J., Zhong, Z. & Lu, Y. Critical charge and spin instabilities in superconducting La₃Ni₂O₇. arXiv preprint arXiv:2307.07154 (2023).
- [37]Jiang, R., Hou, J., Fan, Z., Lang, Z.-J. & Ku, W. Pressure driven fractionalization of ionic spins results in cupratelike high-Tc superconductivity in La₃Ni₂O₇. Physical Review Letters 132, 126503 (2024).
- [38]Christiansson, V., Petocchi, F. & Werner, P. Correlated electronic structure of La₃Ni₂O₇ under pressure. Physical Review Letters 131, 206501 (2023).
- [39]Lu, D.-C. et al. Superconductivity from Doping Symmetric Mass Generation Insulators: Application to La₃Ni₂O₇ under Pressure. arXiv preprint arXiv:2308.11195 (2023).DOI
- [40]Zhang, Z., Greenblatt, M. & Goodenough, J. B. Synthesis, Structure, and Properties of the Layered Perovskite La₃Ni₂O₇-δ. Journal of Solid State Chemistry 108, 402-409 (1994).DOI
- [41]Taniguchi, S. et al. Transport, Magnetic and Thermal Properties of La₃Ni₂O₇-δ. Journal of the Physical Society of Japan 64, 1644-1650 (1995).
- [42]Liu, Z. et al. Evidence for charge and spin density waves in single crystals of La₃Ni₂O₇ and La₃Ni₂O₆. Science China Physics, Mechanics & Astronomy 66, 217411 (2023).DOI
- [43]Dong, Z. et al. Visualization of Oxygen Vacancies and Self-doped Ligand Holes in La₃Ni₂O₇-δ. Nature 630, 847-852 (2024).DOI
- [44]Lee, K. W. & Pickett, W. E. Infinite-layer LaNiO₂: Ni¹⁺ is not Cu²⁺. Physical Review B 70, 165109 (2004).DOI
- [45]Botana, A. S. & Norman, M. R. Similarities and Differences between LaNiO₂ and CaCuO₂ and Implications for Superconductivity. Physical Review X 10, 011024 (2020).DOI
- [46]Hepting, M. et al. Electronic structure of the parent compound of superconducting infinite-layer nickelates. Nature Materials 19, 381-385 (2020).
- [47]Goodge, B. H. et al. Doping evolution of the Mott–Hubbard landscape in infinite-layer nickelates. Proceedings of the National Academy of Sciences 118, e2007683118 (2021).DOI
- [48]Ren, X. et al. Possible strain-induced enhancement of the superconducting onset transition temperature in infinite-layer nickelates. Communications Physics 6, 341, doi:10.1038/s42005-023-01464-x (2023).DOI
- [49]Gao, Q. et al. Magnetic excitations in strained infinite-layer nickelate PrNiO₂ films. Nature Communications 15, 5576 (2024).DOI
- [50]Ling, C. D., Argyrıou, D. N., Wu, G. & Neumeier, J. J. Neutron Diffraction Study of La₃Ni₂O₇: Structural Relationships Among n=1, 2, and 3 Phases Laₙ₊₁NiₙO₃ₙ₊₁. Journal of Solid State Chemistry 152, 517-525 (2000).DOI
- [51]Liu, Z. et al. Electronic correlations and energy gap in the bilayer nickelate La₃Ni₂O₇. arXiv preprint arXiv:2307.02950 (2023).
- [52]Chen, K. et al. Evidence of Spin Density Waves in La₃Ni₂O₇-δ. Physical Review Letters 132, 256503 (2024).
- [53]Khasanov, R. et al. Pressure-Induced Split of the Density Wave Transitions in La₃Ni₂O₇-δ. arXiv preprint arXiv:2402.10485 (2024).
- [54]Zhou, K.-J. et al. Electronic and magnetic excitations in La₃Ni₂O₇. arXiv preprint arXiv:2401.12657 (2024).
- [55]Dan, Z. et al. Spin-density-wave transition in double-layer nickelate La₃Ni₂O₇. arXiv preprint arXiv:2402.03952 (2024).
- [56]Xie, T. et al. Neutron Scattering Studies on the High-Tc Superconductor La₃Ni₂O₇-δ at Ambient Pressure. arXiv preprint arXiv:2401.12635 (2024).
- [57]Meng, Y. et al. Density-wave-like gap evolution in La₃Ni₂O₇ under high pressure revealed by ultrafast optical spectroscopy. arXiv preprint arXiv:2404.19678 (2024).DOI
- [58]Greenblat, M., Zhang, Z. & Whangbo, M. H. Electronic properties of La₃Ni₂O₇ and Ln₄Ni₃O₁₀, Ln=La, Pr and Nd. Synthetic Metals 85, 1451-1452 (1997).
- [59]Li, Z. et al. Epitaxial growth and electronic structure of Ruddlesden–Popper nickelates (Laₙ₊₁NiₙO₃ₙ₊₁, n=1–5). APL Materials 8, 091112 (2020).DOI
- [60]Cui, T. et al. Strain-mediated phase crossover in Ruddlesden–Popper nickelates. Communications Materials 5, 32 (2024).arxiv.org/abs/2311.13228
- [61]Wang, G. et al. Pressure-Induced Superconductivity In Polycrystalline La₃Ni₂O₇-δ. Physical Review X 14, 011040 (2024).
- [62]Zaanen, J., Sawatzky, G. A. & Allen, J. W. Band gaps and electronic structure of transition-metal compounds. Physical Review Letters 55, 418-421 (1985).pubmed.ncbi.nlm.nih.gov/10032345
- [63]Hill, J. & McMorrow, D. Resonant exchange scattering: polarization dependence and correlation function. Acta Crystallographica Section A: Foundations of Crystallography 52, 236-244 (1996).
- [64]64 Chen, C. et al. Electronic states in La₂−ₓSrₓCuO₄+δ probed by soft-x-ray absorption. Physical Review Letters 66, 104 (1991).pubmed.ncbi.nlm.nih.gov/10043153
- [65]65 Zhang, Y., Lin, L.-F., Moreo, A., Maier, T. A. & Dagotto, E. Structural phase transition, s±-wave pairing, and magnetic stripe order in bilayered superconductor La₃Ni₂O₇ under pressure. Nature Communications 15, 2470 (2024).
- [66]66 Yang, J. et al. Orbital-dependent electron correlation in double-layer nickelate La₃Ni₂O₇. Nature Communications 15, 4373 (2024).
- [67]67 Sui, X. et al. Electronic properties of the bilayer nickelates R₃Ni₂O₇ with oxygen vacancies (R=La or Ce). Physical Review B 109, 205156 (2024).
- [68]68 Haverkort, M., Hollmann, N., Krug, I. & Tanaka, A. Symmetry analysis of magneto-optical effects: The case of x-ray diffraction and x-ray absorption at the transition metal L₂,₃ edge. Physical Review B 82, 094403 (2010).DOI
- [69]69 Frano, A. et al. Orbital control of noncollinear magnetic order in nickel oxide heterostructures. Physical Review Letters 111, 106804 (2013).DOI
- [70]70 Hepting, M. et al. Complex magnetic order in nickelate slabs. Nature Physics 14, 1097-1102 (2018).
- [71]71 Kim, W. J. et al. Geometric frustration of Jahn–Teller order in the infinite-layer lattice. Nature 615, 237-243 (2023).