Abstract

CoFe2O4/Co-Fe magnetic composites are usually prepared through partial reduction of CoFe2O4, which often yields monoxides (i.e., FeO, CoO) as secondary phases. Since these compounds are paramagnetic at ambient conditions, the presence of a small amount of monoxide is generally downplayed in the literature, and the possible effects on the magnetic properties are simply ignored. However, the present study shows that even a low concentration of monoxide results in decoupling of the soft and hard magnetic phases, which inevitably leads to a deterioration of the magnetic properties. Additionally, it is confirmed that a partial reduction of CoFe2O4 is a suitable method to produce CoFe2O4/Co-Fe nanocomposites, provided that the treatment is well controlled with respect to duration, temperature and flow of reductant. A monoxide-free nanocomposite was produced and its magnetic properties evaluated both at room and low temperature. Our model system exemplifies the potential of exchange-coupling (and decoupling) as a tool to tune the magnetic properties of a material within a relatively wide range of values, thus widening its spectrum of potential applications.

Introduction

Magnetic nanoparticles (MNPs) have undoubtedly been one of the hot research topics of the 21st century.[1] Intensive research on the subject has yielded notable advances in a wide range of technologies and disciplines. For instance, MNPs have been a great aid in medical diagnosis and treatment of diseases.[2] Among other cutting-edge medical applications, MNPs are integral components of drug carriers for magnetic drug delivery,[3, 4] heat mediators in cancer therapy by magnetic fluid hyperthermia (MFH),[5] or contrast agents for magnetic resonance imaging (MRI).[6] MNPs are also highly relevant in matter of sensors and biosensors aimed to diverse analytes,[7] e.g., food contaminants,[8, 9] environmental pollutants,[10] antibodies,[11] etc.

The actual application determines the required magnetic properties. Very often, the stability and longevity of the devices rely on a strong resistance to demagnetization (i.e. hard magnetic material, with large coercivity, HcH_\mathrm{c}). Other times, the crucial parameter that ensures compliance with the specific task is the ability of the material to become magnetized up to a high value (i.e. high saturation magnetization, MsM_\mathrm{s}). Most of the available materials show either a large HcH_\mathrm{c} and a moderate MsM_\mathrm{s} or vice versa.[12] Consequently, if relatively high values of both HcH_\mathrm{c} and MsM_\mathrm{s} are necessary, fabrication of composite materials should be addressed. According to the exchange-spring theory, the MsM_\mathrm{s} of a hard magnetic material can be enhanced by adding a controlled amount of a large-MsM_\mathrm{s} material (generally soft), and the cost in HcH_\mathrm{c} will be low provided that the two materials are effectively exchange-coupled.[13]

Ferrites are among the most used magnetic materials, owing to their good magnetic properties, chemical and mechanical stability, and the availability of elements they are based on. Especially interesting are the spinel ferrites (SFs), as they allow easy tunability of the magnetic properties with small changes on the chemical composition,[14, 15, 16] thus increasing their versatility towards different applications. SFs have been widely used in the electronic industry, for high-density data storage and spintronic devices.[17] [18] Their utilization for biomedical applications has increased significantly over the last years, especially in the fields of drug delivery19 and biosensors.20,21 In addition to their applications as magnetic materials, it is worth mentioning that SFs are widely used for other purposes, e.g., as catalysts for very varied chemical processes,22,23 advanced battery electrodes,24,25 electrochemical supercapacitors in energy storage systems,26 etc.

SFs have the general formula M2+(Fe3+)2O4\mathrm{M}^{2+}(\mathrm{Fe}^{3+})_{2}\mathrm{O}_{4}, with M = Mg, Mn, Fe, Co, Ni, Cu, Zn.[17] Out of all them, only Co-spinel shows hard magnetic properties, while the rest are soft magnetic species.27 Moreover, CoFe2O4\mathrm{CoFe}_{2}\mathrm{O}_{4} can be easily reduced to a Co–Fe alloy in the presence of a small concentration of H2\mathrm{H}_{2} gas and moderate temperatures (≈300\approx300 °C).28 Both facts make this compound interesting, as an incomplete CoFe2O4\mathrm{CoFe}_{2}\mathrm{O}_{4} reduction directly leads to coexistence of hard (CoFe2O4\mathrm{CoFe}_{2}\mathrm{O}_{4}) and soft (Co–Fe) magnetic phases. This is an excellent tool from the material science viewpoint, as it offers the potential to fine tuning the soft/hard magnetic behavior of the produced material by means of controlling the composite composition.

For the above reasons, numerous studies on the CoFe2O4\mathrm{CoFe}_{2}\mathrm{O}_{4} (hard)/Co–Fe (soft) composite are found in the literature, including composites prepared as powders,29 dense pellets,30 or thin films.31 Some works have set the main focus on the preparation process (in situ studies),28,32 while others have taken care of an in-depth structural characterization of the produced composites using spectroscopic techniques such as Raman33 or Mössbauer spectroscopy.34,35 Others have put great efforts on studying the inter-particle coupling from different perspectives, both using transmission electron microscopy (TEM), and measuring δm\delta m curves (Henkel plots).35,36 Recently, micromagnetic calculations on these systems have also been reported.37 However, a successful exchange-coupling of these two magnetic phases has proven rather challenging to achieve, the reason behind it often remaining unclear. In the present work, the origin of magnetic decoupling in CoFe2O4\mathrm{CoFe}_{2}\mathrm{O}_{4}/Co–Fe nanocomposites is addressed. Composites covering a range of compositions are prepared, and their crystalline and atomic structures are studied using high-resolution powder X-ray diffraction. Physical characterization of the magnetic properties is carried out both at room and low temperature, and coupling/decoupling of the system is evaluated in terms of the phases present in the sample and their average crystallite sizes.

Experimental

Sample preparation

Magnetic CoFe2O4\mathrm{CoFe}_{2}\mathrm{O}_{4}/Co–Fe nanocomposites were prepared by means of a controlled reduction of CoFe2O4\mathrm{CoFe}_{2}\mathrm{O}_{4} nanoparticles. The starting CoFe2O4\mathrm{CoFe}_{2}\mathrm{O}_{4} material was hydrothermally synthesized following the procedure described in a previous work,38 and had a volume-averaged crystallite size of 14.4(1) nm. 0.20 g of the as-synthesized powders were spread on an Al2O3\mathrm{Al}_{2}\mathrm{O}_{3} crucible with approximate dimensions 60×40 mm260 \times40\ \mathrm{mm}^{2}. The crucible was placed at the hot spot of a tubular furnace (C.H.E.S.A. Ovens). The furnace was sealed at both ends and purged down to a pressure of ≈1×10−2\approx1 \times10^{-2} mbar using a vacuum pump connected to the furnace outlet. Gas mixture 10% H2\mathrm{H}_{2}/90% N2\mathrm{N}_{2} was fed through the furnace inlet, regulating the flow until the pressure inside the furnace stabilized at 20 mbar. Finally, the thermal treatment was initiated. An initial heating ramp of 100 °C min−1^{-1} drove the temperature up to the set point (300–600 °C), at which the system was maintained during 2–8 hours (see heating profiles in Fig. S1, ESI†). Subsequently, the sample was left to cool down inside the furnace, while maintaining the flow of reducing gas. The sample was removed from the furnace once the temperature was below 75 °C. All samples were stable in air.

Characterization

Powder X-ray diffraction (PXRD)

PXRD data were collected on all the samples in a Bragg-Brentano θ/θ\theta/\theta configuration using Cu Kα1,2\mathrm{K}\alpha_{1,2} radiation (λ1=1.540593\lambda_{1} = 1.540593 Å, λ2=1.544427\lambda_{2} = 1.544427 Å) at a laboratory Rigaku SmartLab® diffractometer operated at 40 kV and 180 mA. The incident slit (IS) choice was different depending on the amount of sample available for the measurement. Further details on IS and 2θ2\theta range may be found in the ESI.† A diffracted beam monochromator (DBM) was installed on the receiving optics to suppress the fluorescence contribution to the background and the data were collected with a D/teX Ultra detector.

Rietveld analysis of the PXRD data was performed using the FullProf Suite.39 In the Rietveld model, the oxides were described assuming a Co : Fe stoichiometry of 1 : 2 (i.e., CoFe2O4\mathrm{CoFe}_{2}\mathrm{O}_{4}, Co0.33Fe0.67O\mathrm{Co}_{0.33}\mathrm{Fe}_{0.67}\mathrm{O}) and a random distribution of the two cations among the equivalent crystallographic sites. The elemental composition of the alloy in the model varied depending on the sample. A detailed crystallographic description of all the Rietveld phases may be found on Tables S1–S5 in the ESI.†

Data were also collected on a NIST 660B LaB6_{6} calibrant in the different experimental configurations, and these data were modelled (LeBail fit) to estimate the instrumental contribution to the peak broadening. The instrument contribution was deconvoluted from the samples data, and the remaining profile broadening, originating from the sample, was modelled as Lorentzian isotropic size-broadening using the Thompson–Cox–Hastings formulation of the pseudo-Voigt function.40

Magnetic properties

About 10 mg of the nano-powders, measured with a precision of 0.001 mg, were gently compressed into thin cylindrical pellets (diameter = 3.00 mm, thickness = 0.50–0.60 mm). Magnetization as a function of an externally applied magnetic field was measured using a Quantum Design Physical Property Measurement System (PPMS®) equipped with a vibrating sample magnetometer (VSM). After field-cooling in 50 kOe (i.e., 3979 kA m−1^{-1}) down to 10 K, the magnetization was measured while varying the applied field in the range ±50 kOe. Subsequently, the sample was heated up to 300 K, and the magnetization was measured in the field range ±20 kOe (1591 kA m−1^{-1}). For the starting material, the LT measurement was done after cooling in absence of an external field.

Prior to the measurements described above, the room temperature magnetization of the samples was measured in a smaller field range ±4 kOe (318 kA m−1^{-1}) using a home-built VSM setup.41

Results and discussion

Composition and crystallite size from Rietveld analysis

Reduction treatments of variable duration and temperature yielded five different samples. Henceforth, tags in the form {time@temperature} are used to refer to the samples. Sample composition and sizes obtained from Rietveld analysis of the PXRD data collected on those samples are displayed in Figure 1 and Table 1. A representative example of a Rietveld model fitted to the PXRD data is shown in Figure 2(a). The Rietveld models fitted to the PXRD data collected for the remaining samples may be found on Fig. S5 in the ESI.†

Image not extracted

Figure 1. (a) Sample composition and (b) crystallite size of the constituent phases extracted from Rietveld analysis of the PXRD data measured on the starting material and the five different nanocomposites. The magnetic properties of the samples highlighted with a green/red/blue square are represented in Fig. 4 and 5 using the same color-code.

SampleCoFe2_2O4_4 wt%CoFe2_2O4_4 ⟨D⟩\langle D\rangle (nm)CoFe2_2O4_4 aa (Å)Co0.33_{0.33}Fe0.67_{0.67}O wt%Co0.33_{0.33}Fe0.67_{0.67}O ⟨D⟩\langle D\rangle (nm)Co0.33_{0.33}Fe0.67_{0.67}O aa (Å)Metallic alloy wt%Metallic alloy phaseMetallic alloy ⟨D⟩\langle D\rangle (nm)Metallic alloy aa (Å)
Starting material100.0(3)14.4(1)8.3929(1)———————
{2h@300°C}63.8(3)21.5(1)8.3889(1)15.7(2)10.1(2)4.2695(2)20.5(1)CoFe28.9(3)2.85645(4)
{4h@300°C}52.7(3)19.5(1)8.3886(1)8.5(2)8.3(3)4.2680(4)38.9(2)CoFe26.0(2)2.85877(4)
{8h@300°C}19.1(4)10.6(3)8.3904(5)———80.9(4)CoFe30.4(2)2.86141(4)
{2h@400°C}56.1(4)52.9(4)8.38952(7)6.2(2)11.9(6)4.2860(4)37.8(7)Co2_2Fe16.9(3)2.84639(3)
{2h@400°C}——————CoFe46.3(8)2.85434(3)
{2h@600°C}——————100(4)CoFe64(2)2.85954(6)
{2h@600°C}——————Co2_2Fe3_3139(5)2.86405(3)

Table 1. Results from Rietveld refinements for the three phases, i.e., weight fraction, wt%, volume-averaged crystallite size, ⟨D⟩\langle D\rangle, unit cell parameter, aa. The uncertainties specified along with the refined wt% and the values are the standard deviations calculated from the refinement software (FullProf).39 For the refined ⟨D⟩\langle D\rangle, the uncertainties are calculated by propagation of error

Image not extracted

Figure 2. (a) PXRD data and corresponding Rietveld model of the phases present in sample {2h@300°C}. (b) Selected 2θ2\theta-region of data and models for {2h@300°C}, (c) {4h@300°C}, and (d) {8h@300°C}.

From the series of experiments at 300 °C with variable duration (2–8 h), it is clear that as time increases, the amount of CoFe2_2O4_4 decreases, at the expense of the appearance of reduced phases: a monoxide phase (Co0.33_{0.33}Fe0.67_{0.67}O) and a metallic alloy phase (CoFe). The monoxide seems to play the role of a reaction intermediate, as it disappears as the reduction advances. Thus, while 2 and 4 h at 300 °C produced composites with 16.1(2)% and 8.6(3)% monoxide, respectively, a monoxide-free composite with an 80.9(4)% metallic content was obtained after 8 h. Figure 2(b–Figure 2d) show selected 2θ2\theta-regions of the PXRD data and models corresponding to these three samples. The distinct Rietveld phases are highlighted to illustrate the appearance/disappearance of the different phases as dwell time increases.

At 300 °C, the growth of the soft phase crystallites remains relatively controlled (≤30.4(2)\leq30.4(2) nm) regardless of the dwell time. Increasing the treatment temperature accelerates the reduction process,28 thus, 2 h at 400 °C led to lower CoFe2_2O4_4 content than 2 h at 300 °C. The monoxide content also decreased substantially at 400 °C. At 600 °C, 2 hours were sufficient to completely reduce the starting material to pure metallic phases. However, increasing the temperature entails a significant growth of the alloy crystallites.

Figure 3(a) shows the evolution of the most intense reflections of the alloy phase as a function of the reduction temperature. While the diffraction data collected for the {2h@300°C} nanocomposite can be modelled with a single metallic phase (CoFe), at least two metallic phases are clearly present in the {2h@400°C} and {2h@600°C} samples. The refined unit cell parameters for the individual phases are displayed in Table 1 and plotted in Figure 3(b) as a function of the treatment temperature. The dissimilar distribution of cell parameters suggests different elemental compositions of the alloys. Unfortunately, the Co : Fe ratio could not be extracted from the refinements, because Co and Fe are next-neighbors in the periodic table and therefore, practically indistinguishable using X-rays (see ESI in ref. 28).

Image not extracted

Figure 3. (a) Selected 2θ2\theta-regions of the PXRD data collected after 2 h reduction treatment at 300, 400, and 600 °C, and Rietveld models of the different metallic phases, i.e., Co2_2Fe3_3, CoFe, and Co2_2Fe. (b) Refined unit cell parameters of the phases as a function of the treatment temperature, circles and crosses representing the time and temperature series, respectively. The error bars lie within the size of the symbols.

The unit cell dimensions of Co–Fe alloys increase with an increasing Fe content.42 This allows an estimate of the elemental composition based on the lattice parameter. The empirical chemical compositions shown in Table 1 and Figure 3 were assessed by substituting the refined unit cell parameters in the equation obtained by Ohnuma et al. for ordered body-centered-cubic

(bcc) structures.42 For the mildest reduction, {2h@300°C}, the calculated alloy composition is CoFe. This indicates surplus Co on the alloy, compared to the Co: Fe stoichiometry of 1: 2 presumed for the starting spinel material. This observation is in agreement with previous in situ investigations on this system, where the reduced phases were observed to appear in a Co-rich form, to later incorporate Fe and evolve towards Co: Fe = 1: 2.28 At the higher temperatures, CoFe coexists with other alloy phases, i.e., Co2_2Fe in {2h@400°C} and Co2_2Fe3_3 in {2h@600°C}, showing that the Fe-content increases as the temperature rises. A similar phase segregation may be occurring at 300 °C, although the effect remains hidden under the broader diffraction peaks derived from the smaller crystallite sizes at this temperature, and in that case, the refined unit cell parameter should be understood as the weighted average of all the phases present. The cell dimensions increase slightly with dwell time, again indicating a late incorporation of the Fe in the alloy structure.

The influence of the amount of H2_2 inside the furnace was also investigated (see Fig. S6 in the ESI†). The gas pressure was increased up to 100 and 300 mbar, and no significant changes were observed neither on the sample composition nor the crystallite sizes, compared to the experiments at 20 mbar. This suggests that, for the amounts of sample used here, an H2_2 excess is ensured even at the lowest pressure, and as long as there is enough H2_2 available, the gas pressure does not seem to have a major influence on the process.

To evaluate whether the crystallite size of the starting material plays a role, an additional time series of experiments were carried out at 300 °C using CoFe2_2O4_4 powders with an average size of 8.2(1) nm (see Fig. S7 in the ESI†). Comparing these results with those represented in Figure 1 (mean size starting material 14.4(1) nm), it is concluded that the smaller the size of the starting CoFe2_2O4_4, the faster the reduction occurs, i.e., the shorter the time required to achieve a certain reduction stage.

Magnetic properties

Magnetization at room temperature (RT). Magnetic hysteresis loops measured at 300 K are displayed in Fig. S8 (ESI†) and saturation magnetization, MsM_\mathrm{s}, remanence, MrM_\mathrm{r}, and coercivity, HcH_\mathrm{c}, obtained from those curves are compiled in Table 2 and plotted in Figure 4 as a function of the alloy content. MsM_\mathrm{s} was calculated from the loops using the law of approach to saturation.43 MrM_\mathrm{r} and HcH_\mathrm{c} were extracted from linear fits including 5 data points on each side of the yy- and the xx-intercept, respectively.

SampleMsM_{\mathrm{s}} (A m2^{2} kg−1^{-1})MrM_{\mathrm{r}} (A m2^{2} kg−1^{-1})HcH_{\mathrm{c}} (kA m−1^{-1})a^{a}HcH_{\mathrm{c}} (kOe)a^{a}
Starting material73.9(4)19.7(1)83(2)1.04(2)
{2h@300°C}86.3(1)29.5(1)115(1)1.44(2)
{4h@300°C}115.6(1)30.4(2)90(1)1.13(2)
{8h@300°C}185.1(1)27.0(2)60.4(9)0.76(1)
{2h@400°C}125.6(1)13.8(2)44.3(6)0.557(7)
{2h@600°C}229.7(2)1.7(2)3.23(2)0.0406(2)

Table 2. Saturation magnetization, MsM_{\mathrm{s}}, remanence, MrM_{\mathrm{r}}, and coercivity, HcH_{\mathrm{c}}, extracted from magnetic hysteresis measured at 300 K. The errors on the values are calculated from the uncertainties on the linear fits.

Image not extracted

Figure 4. Room temperature MsM_{\mathrm{s}}, MrM_{\mathrm{r}}, and HcH_{\mathrm{c}} as a function of the weight fraction of metallic alloy. The green, open squares correspond to the starting material, the rest of the squares represent the time series of experiments (at 300 °C), and the open circles the two high-temperature experiments (400 and 600 °C). The crystallite sizes indicated in the figure are relevant for the discussion of results in the text. The gray, solid circles correspond to a reference/blank sample fabricated from the same starting material, in a 2 h-long treatment in vacuum at 400 °C. The drawn lines are intended as a guide to the eye.

In order to discriminate the influence of the temperature from the effect of the actual reduction process, a 2 h long treatment in vacuum at 400 °C was carried out. No significant changes were observed in the magnetic properties after this treatment (see solid, gray circles in Figure 4). Therefore, in the following, the starting CoFe2_2O4_4 powders will continue to be used as reference to evaluate the magnetic properties of the nanocomposites.

MsM_{\mathrm{s}} follows the expected linear increase with the amount of alloy present in the sample. The trends exhibited by MrM_{\mathrm{r}} and HcH_{\mathrm{c}} are slightly more complex. A mild reduction, such as {2h@300°C} (in red color) yields a significant enhancement of both parameters; the composite with a 20.5(1) wt% alloy has a 50% higher MrM_{\mathrm{r}} and a 39% larger HcH_{\mathrm{c}} than the starting material. This is understood as a consequence of the temperature which causes a moderate growth of the CoFe2_2O4_4 nanoparticles, from 14.4(1) to 21.5(1) nm, and has very likely induced a betterment of the crystallinity as well.

As the alloy wt% increases, both MrM_{\mathrm{r}} and HcH_{\mathrm{c}} decrease, but the decrease is much more pronounced for the temperature series (circles) than for the time series (squares). For instance, the {4h@300°C} nanocomposite has a Mr=30.4(2)M_{\mathrm{r}} = 30.4(2) A m2^{2} kg−1^{-1} and a Hc=90(1)H_{\mathrm{c}} = 90(1) kA m−1^{-1}, and these parameters are reduced by more than half for the sample with approximately the same composition fabricated at 400 °C for 2 h (Mr=13.8(2)M_{\mathrm{r}} = 13.8(2) A m2^{2} kg−1^{-1}, Hc=44.3(6)H_{\mathrm{c}} = 44.3(6) kA m−1^{-1}). Despite the similarity in composition between these two samples, the crystallite sizes of both hard and soft phases are much larger for the composite prepared at the higher temperature, which can explain the deterioration of the magnetic properties: (i) the 52.9(4) nm refined for the hard phase in {2h@400°C} is above the critical stable single-domain size (SSD) for CoFe2_2O4_4 (≈40\approx40 nm), which explains the collapse in HcH_{\mathrm{c}} observed for this sample. (ii) The alloy also grows well beyond typical SSD values, and formation of domains in the soft phase eases spontaneous demagnetization of the hard when both phases are coupled.

Magnetization at low temperature (LT). Magnetization versus applied field measured at 10 K is shown in Figure 5(a) for selected samples: starting CoFe2_2O4_4 powders in green, {2h@300°C} in red, and {8h@300°C} in blue. The rest of the 10 K curves and the MsM_{\mathrm{s}}, MrM_{\mathrm{r}}, and HcH_{\mathrm{c}} values extracted may be found in Fig. S6 and Table S6 of the ESI, respectively. LT magnetization measurements help understanding whether or not the hard and soft phases are linked through inter-particle exchange-coupling. Although the average reversal fields of CoFe2_2O4_4 and Co–Fe are similar at RT, they radically draw apart when lowering the temperature, as the anisotropy of the hard magnetic phase is significantly larger at LT. This is clearly seen on our samples, with the HcH_{\mathrm{c}} of the hard phase being roughly 10 times larger at 10 K than at 300 K, while the HcH_{\mathrm{c}} of the soft phase {2h@600°C} is of the same order of magnitude at both temperatures (compare values from Table 2 and Table S6, ESI). A discontinuous hysteresis loop is expected for uncoupled systems, as the hard and soft phases are independently demagnetized (two-step magnetization reversal). Oppositely, a smooth curve is expected for exchange-coupled systems, where a joint reversal of both phases takes place (1-step or single-phase reversal). The correlation single-/two-step LT hysteresis ↔\leftrightarrow coupling/decoupling, respectively, is not always as simple as described above, but the statement is valid for the CoFe2_2O4_4/Co–Fe composite (see specific section in the ESI).

Image not extracted

Figure 5. (a) Low temperature magnetic hysteresis loops for selected samples and (b) corresponding first derivative normalized. The samples represented in green, red and blue color in this figure are highlighted with the same colors in Fig. 1 and 4.

The number of reversal or switching events is readily revealed by the maxima in the first derivative curve of the magnetization data. First derivatives of the MM–HH data from all samples are displayed in Figure 5(b). The starting material shows the single-step behavior expected for a pure phase, with a single switching field, HswH_{\mathrm{sw}}, at ≈940\approx940 kA m−1^{-1}. The same is observed for the fully-reduced sample {2h@600°C} but with a nearly zero HswH_{\mathrm{sw}}. Note the shape of the peaks here is much more Lorentzian than for the starting material. This shape can result from the convolution of several independent contributions from distinct phases (rather than a single-phase), all of them having a very similar, nearly-null magnetic anisotropy. This is in agreement with the two bcc species with different Co : Fe ratios visible in the PXRD data.

Two very distinct HswH_{\mathrm{sw}} are detected for {2h@300°C} (red), which is an indicative of weakly exchanged soft–hard inter-phases. On the contrary, {8h@300°C} (blue) presents a single-step reversal, which in this case is attributed to an effective of exchange-coupling between the soft and hard phases. Independent magnetization reversal of the magnetic phases is visible for {4h@300°C}, although the peak defined by the larger HswH_{\mathrm{sw}} is much less intense compared to the 2 h experiment at the same temperature (red curve). The dM/dHdM/dH curve for {2h@400°C} is maximized at a single HswH_{\mathrm{sw}} value. However, the peaks here are not symmetric and the peak tails do not coincide, suggesting some degree of decoupling of the two magnetic phases.

To summarize, the only composite showing LT exchange-coupling behavior is the monoxide-free sample {8h@300°C} (blue color). We believe this observation is far from coincidental, considering the correlation between the monoxide concentration and the degree of decoupling shown by our data (see plots on the right from Figure 5(b)). The present study demonstrates how avoiding the monoxide is imperative for producing effectively exchange-coupled CoFe2_2O4_4/Co–Fe nanocomposites. This observation is consistent with and may help explain previous literature on the subject. Several studies report decoupling at RT in monoxide-containing samples29,45–48 Some decoupled “monoxide-free” examples are also found.49–53 However, we consider it possible that the monoxide was overlooked in those works. The proximity in 2θ2\theta of the monoxide and the spinel Bragg positions (see Figure 2) makes it difficult to separate the contribution from these two phases unless the PXRD data has high enough resolution and the subsequent data analysis is appropriate.

Based on a joint interpretation of the RT and LT magnetization data, we understand that our monoxide-free, exchange-coupled sample {8h@300°C} is far from reaching the best magnetic properties the CoFe2_2O4_4/Co–Fe system allows. Samples with a lower alloy content, such as {2h@300°C} and {4h@300°C}, appear significantly more promising, owing to their higher MrM_{\mathrm{r}} and HcH_{\mathrm{c}} values at RT (see Figure 4), despite the presence of monoxide hindering the optimal magnetic performance of these samples. Therefore, we believe that monoxide-free composites with an alloy content ≲40\lesssim40 wt% may lead to effectively exchange-coupled CoFe2_2O4_4/Co–Fe composites with superior magnetic properties, and should thus be pursued in future work.

Conclusions

CoFe2_2O4_4 (hard)/Co–Fe (soft) magnetic nanocomposites have been prepared through controlled partial reduction of CoFe2_2O4_4 nanoparticles, obtaining samples with several compositions and crystallite sizes. An additional monoxide phase was found in some of the samples, although this phase disappeared for long reaction times. Magnetization curves at room and low temperature reveal that an increasing monoxide concentration deteriorates inter-phase magnetic exchange-coupling. In fact, the only composite showing an effective exchange-coupling was monoxide-free. Thus, minimizing/avoiding the formation of the monoxide is crucial for producing effectively exchange-coupled CoFe2_2O4_4/Co–Fe nanocomposites.

Once the chemistry behind the process is understood, partial reduction of CoFe2_2O4_4 is a very strong method for synthesizing CoFe2_2O4_4/Co–Fe nanocomposites with controlled magnetic properties. Adjusting each of the reduction parameters (temperature, time, partial H2_2 pressure, crystallite size of the starting CoFe2_2O4_4 powders) has a very specific impact on the composition and crystallite sizes of the obtained nanocomposite, which, in turn, directly determines its magnetic behavior. The present work reveals exchange-coupling to be an excellent tool to further expand the range within which the magnetic properties of spinel ferrites can be tuned, extending the scope of this family of compounds. The method described here using CoFe2_2O4_4/Co–Fe as an example may in principle be applicable to other ferrite systems, including hard hexaferrites or other spinel ferrites (soft), and allows multiple combinations of magnetic compounds.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

C. G.-M. and A. Q. have contributed equally to this work. The authors would like to thank financial support from the European Commission through the AMPHIBIAN project (H2020-NMBP-2016-720853), the Danish National Research Foundation (Center for Materials Crystallography, DNRF-93), and the Spanish Ministerio de Ciencia, Innovación y Universidades (RTI2018-095303-A-C52). C. G.-M. acknowledges financial support from the Spanish Ministerio de Ciencia, Innovación y Universidades through the Juan de la Cierva Program (FJC2018-035532-I). Authors from Aarhus University gratefully acknowledge affiliation with the Center for Integrated Materials Research (iMAT) at Aarhus University. We acknowledge support of the publication fee by the CSIC Open Access Publication Support Initiative through its Unit of Information Resources for Research (URICI).

References

  1. [1]1 D. L. Andrews, R. H. Lipson and T. Nann, Comprehensive Nanoscience and Nanotechnology, Elsevier B.V., 2019.
  2. [2]2 H. M. Williams, The application of magnetic nanoparticles in the treatment and monitoring of cancer and infectious diseases, Biosci. Horizons Int. J. Student Res., 2017, 10, 1–10.DOI
  3. [3]3 Y.-L. Liu, D. Chen, P. Shang and D.-C. Yin, A review of magnet systems for targeted drug delivery, J. Controlled Release, 2019, 302, 90–104.DOI
  4. [4]4 P. Dong, K. P. Rakesh, H. M. Manukumar, Y. H. E. Mohammed, C. S. Karthik, S. Sumathi, P. Mallu and H. L. Qin, Innovative nano-carriers in anticancer drug delivery-a comprehensive review, Bioorg. Chem., 2019, 85, 325–336.DOI
  5. [5]5 D. Chang, M. Lim, J. A. C. M. Goos, R. Qiao, Y. Y. Ng, F. M. Mansfeld, M. Jackson, T. P. Davis and M. Kavallaris, Biologically Targeted Magnetic Hyperthermia: Potential and Limitations, Front. Pharmacol., 2018, 9, 831.DOI
  6. [6]6 K. Wu, D. Su, R. Saha, D. Wong and J.-P. Wang, Magnetic particle spectroscopy-based bioassays: methods, applications, advances, and future opportunities, J. Phys. D: Appl. Phys., 2019, 52, 173001.DOI
  7. [7]7 T. A. P. Rocha-Santos, Sensors and biosensors based on magnetic nanoparticles, TrAC, Trends Anal. Chem., 2014, 62, 28–36.
  8. [8]8 G. Bülbül, A. Hayat and S. Andreescu, Portable Nanoparticle-Based Sensors for Food Safety Assessment, Sensors, 2015, 15, 30736–30758.DOI
  9. [9]9 Y. Li, Z. Wang, L. Sun, L. Liu, C. Xu and H. Kuang, Nanoparticle-based sensors for food contaminants, TrAC, Trends Anal. Chem., 2019, 113, 74–83.DOI
  10. [10]10 D. Song, R. Yang, F. Long and A. Zhu, Applications of magnetic nanoparticles in surface-enhanced Raman scattering (SERS) detection of environmental pollutants, J. Environ. Sci., 2019, 80, 14–34.DOI
  11. [11]11 M. Pastucha, Z. Farka, K. Lacina, Z. Mikušová and P. Skládal, Magnetic nanoparticles for smart electrochemical immunoassays: a review on recent developments, Microchim. Acta, 2019, 186, 312.DOI
  12. [12]12 J. M. Soares, V. B. Galdino and F. L. A. Machado, Exchange-bias and exchange-spring coupling in magnetic core–shell nanoparticles, J. Magn. Magn. Mater., 2014, 350, 69–72.DOI
  13. [13]13 E. F. Kneller and R. Hawig, The exchange-spring magnet: a new material principle for permanent magnets, IEEE Trans. Magn., 1991, 27, 3588–3600.DOI
  14. [14]14 G. Muscas, N. Yacoub, G. Concas, F. Sayed, R. Sayed Hassan, J. M. Grenèche, C. Cannas, A. Musinu, V. Foglietti, S. Casciardi, C. Sangregorio and D. Peddis, Evolution of the magnetic structure with chemical composition in spinel iron oxide nanoparticles, Nanoscale, 2015, 7, 13576–13585.DOI
  15. [15]15 H. L. Andersen, M. Saura-Múzquiz, C. Granados-Miralles, E. Canévet, N. Lock and M. Christensen, Crystalline and magnetic structure–property relationship in spinel ferrite nanoparticles, Nanoscale, 2018, 10, 14902–14914.DOI
  16. [16]16 H. L. Andersen, C. Granados-Miralles, M. Saura-Múzquiz, M. Stringaci, J. Larsen, F. Søndergaard-Pedersen, J. V. Ahlburg, L. Keller, C. Frandsen and M. Christensen, Enhanced intrinsic saturation magnetization of ZnₓCo₁−ₓFe₂O₄ nanocrystallites with metastable spinel inversion, Mater. Chem. Front., 2019, 3, 668–679.
  17. [17]17 T. Tatarchuk, M. Boudinina, J. J. Vijaya and L. J. Kennedy, in Nanophysics, Nanomaterials, Interface Studies, and Applications,

Paper details

vlnc:W_gctg4r5r
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 10

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents