Doping Tunable CDW Phase Transition in Bulk 1T-ZrSe2_2

Abstract

Tuneable electronic properties in transition metal dichalcogenides (TMDs) are essential to further their use in device applications. Here, we present a comprehensive scanning tunnelling microscopy and spectroscopy study of a doping-induced charge density wave (CDW) in semiconducting bulk 1T-ZrSe2_2. We find that atomic impurities which locally shift the Fermi level (EFE_F) into the conduction band trigger a CDW reconstruction concomitantly to the opening of a gap at EFE_F. Our findings shed new light on earlier photoemission spectroscopy and theoretical studies of bulk 1T-ZrSe2_2, and provide a local understanding of the electron-doping mediated CDW transition observed in semiconducting TMDs.

Since the discovery of graphene, extensive theoretical and experimental efforts have been devoted to two-dimensional (2D) and quasi-2D systems. The investigations into their intriguing physical properties have generated numerous highly influential contributions to the field of material physics, including 2D superconductivity,[1] heterostructure devices,[2] moiré physics,[3] topology,[4] spin and charge density waves,[5] and many more. However, even though our understanding of these systems has grown massively in recent years, with both theoretical and experimental advances, individual pieces of the puzzle remain undiscovered or elusive. Here, we focus on the charge density wave (CDW) phase in a quasi-2D system, which is of particular interest because of the many open questions concerning its formation mechanism and its interplay with other electronic phases such as superconductivity.[6, 7, 8]

The CDW formation in one dimension is well-established: a metallic chain of atoms distorts into a gapped state concomitant to a modulated charge distribution due to Fermi surface nesting (FSN). However, the underlying mechanism of the CDW phase transition in 2D and quasi-2D compounds remains to be fully understood. In certain systems, FSN is proposed as the driving force,[9, 10, 11, 12] while in others, Jahn-Teller-like electron-phonon coupling is considered the primary candidate.[13, 14, 15, 16, 17, 18, 19]

We use scanning tunnelling microscopy (STM) and spectroscopy (STS) in ultra-high vacuum to investigate in-situ cleaved surfaces of bulk 1T1\mathrm{T}-ZrSe2\mathrm{ZrSe}_2 (hereafter ZrSe2_2) at 4.5 Kelvin. Depending on scanning bias voltage, we find dispersing and non-dispersing periodic charge modulations. At small negative tunnelling biases, we observe non-dispersing charge modulations akin to the 2a×2a2a \times2a modulation observed at the semiconductor-to-metal transition in few-layer thin ZrSe2_2 flakes grown by molecular beam epitaxy on graphitized SiC(0001).[20] A well-defined non-dispersing q\mathbf{q}-vector and contrast inversion across the CDW gap at the Fermi level (EFE_{\mathrm{F}}) underline the CDW nature of this modulation.[21] At a tunneling bias of +100 meV or higher above EFE_{\mathrm{F}}, we find dispersive charge modulations with a wavelength that increases with energy. These modulations are clearly quasiparticle interference (QPI) patterns incompatible with a CDW. They are associated with a large density of state (DOS) in the conduction band and only observed above EFE_{\mathrm F}.

The scanning probe data discussed here provide compelling evidence that the onset of the CDW phase transition in bulk ZrSe2\mathrm{ZrSe_2} is associated with a shift of the Fermi level into the conduction band due to local electron doping by impurities. A doping-induced CDW concomitant to a semiconductor-to-metal phase transition has previously been reported in few-layers thin ZrSe2\mathrm{ZrSe_2} grown on graphene. [20] However, in contrast to these previous experiments, we can unambiguously attribute the CDW’s origin to doping, excluding any measurable strain or reduced dimensionality. Our data reveal a remarkable correlation between the shift of the Fermi level into the conduction band and the appearance of a CDW with the opening of a gap at EFE_{\mathrm F}. ZrSe2\mathrm{ZrSe_2} is the second system after potassium doped MoS2\mathrm{MoS_2} where a doping-dependent CDW reconstruction is observed, [22] demonstrating doping as a possible tuning parameter of the CDW ground state in semiconductor TMD systems.

Single crystals of 1T1T-ZrSe2\mathrm{ZrSe_2} were grown by the chemical vapour transport (CVT) method, using ZrCl4\mathrm{ZrCl_4} as a transport agent. The use of ZrCl4\mathrm{ZrCl_4} is beneficial for the growth of high-quality crystals, compared to the more common use of iodine as a transport agent. Adding low amounts of the transition metal chloride to the precursors, instead of pure iodine, was reported to favour the fast and reproducible growth of pure crystals of many other TMDs. [23] We started from 99.9%-pure Zr lumps, 99.5%-pure ZrCl4\mathrm{ZrCl_4} powder and 99.999%-pure Se shots, according to the following reaction equation 0.9 Zr+0.1 ZrCl4+2 Se⟶ZrSe2+0.2 Cl20.9\,\mathrm{Zr}+0.1\,\mathrm{ZrCl_4}+2\,\mathrm{Se}\mathbin{\longrightarrow}\mathrm{ZrSe_2}+0.2\,\mathrm{Cl_2}. The precursors were weighed and mixed inside a glove box under Ar(6N) atmosphere, then sealed under vacuum in a quartz tube of internal diameter 8 mm and length ≃12\simeq12 cm. A total mass of 0.3 g was introduced into each ampule. The ampule was annealed in a tubular furnace under a T-gradient (Thot=830∘CT_{\mathrm{hot}}=830^\circ\mathrm{C}, Tcold=750∘CT_{\mathrm{cold}}=750^\circ\mathrm{C}) for 120 h, then quickly pulled out to room temperature. An almost complete transport of the material from the hot to the cold end was achieved under these conditions, and grey-greenish platelets with a metallic lustre were found to crystallise at the cold end. X-ray diffraction measurements, performed in a Philips X’Pert four-circle diffractometer using CuKα\mathrm{CuK}_{\alpha} radiation, confirmed the 1T1T-ZrSe2\mathrm{ZrSe_2} crystal structure (P3ˉm1P\bar{3}m_{1} space group, CdI2_2 structure type) and the [00ll] orientation of the plate-like crystals. Careful analyses of the crystal composition were carried out by Energy Dispersive X-ray Spectroscopy (EDS) in a LEO438VTP scanning electron microscope coupled to a Noran Pioneer X-ray detector. All crystals exhibited a little excess of Zr and Se vacancies (average composition Zr1.08_{1.08}Se1.92_{1.92}), locally varying from ZrSe2_2 to Zr1.15_{1.15}Se1.85_{1.85}, in agreement with previous reports.[24] No traces of Cl and ZrSe3_3 were found within the resolution of the EDS probe. The intrinsic and non-homogeneous off-stoichiometry of ZrSe2_2 is of primary importance in understanding the electronic properties of this material. The equilibrium Zr-Se phase diagram has not been assessed; however, it is reasonable to expect that it exhibits a broad miscibility range like the similar systems Ti-Se, Zr-S and Zr-Te, and we expect some level of self-intercalated Zr. The crystals were cleaved in-situ shortly before inserting into the STM head.

We carried out STM and STS measurements using etched tungsten tips in a SPECS JT-STM setup operated at ≈4.4\approx4.4 Kelvin at a base pressure around 4×10−114 \times10^{-11} mbar. STM measurements were performed in constant current mode, applying a bias voltage to the sample. We have added a small windowing to smooth the edges of all images, resulting in cleaner Fourier transforms. STS conductance maps were acquired using a standard lock-in technique with a 5 mV AC modulation. CITS maps were taken on a 170×170170 \times170 grid in a 30×3030 \times30 nm2^{2} window. Each spectrum consists of 183 equally spaced points between −300-300 mV and +50+50 mV and is low-pass filtered using a moving average over five points. The CITS maps are normalized by dividing the dI/dV(V)dI/dV(V) signal by (I/V)(I/V). The Fourier components were isolated using soft 21-by-21-pixel Gaussian windows centred on the Fourier peaks.

In Figure 1, we present three constant-current STM topography images acquired at different biases over the same area of an in-situ cleaved ZrSe2_2 surface at 4.4 Kelvin. Positive bias images reveal very sharp atomic resolution with different atomic impurity features (Figure 1a). Reducing the bias to small negative voltages (Figure 1b), we still resolve the atomic lattice, albeit less sharply, but we no longer see most of the atomic defects resolved at positive bias. The most remarkable aspect of small negative bias images is the appearance of static 2a2a charge modulations aligned with the atomic lattice, where aa is the atomic lattice constant. These modulations are only resolved for bias voltages between −800 mV and +50 mV. At larger negative bias (< −900 mV), STM images reveal nm-sized bright and dark spots on a homogeneous background, with no atomic-scale resolution (Figure 1c). We associate these spots with the charge inhomogeneities observed at small negative bias in Figure 1b, but with opposite contrast. This change, in contrast, is a direct consequence of the semiconducting gap,[25] as explained below.

30 × 30 nm² STM topography of ZrSe₂ with panels (a)–(f)

Figure 1. 30 × 30 nm² STM topography of the same region of ZrSe₂ measured at (a) +400 mV, (b) −400 mV and (c) −1.1 V bias. The insets show the corresponding Fourier transforms. (d) Topography in (a) with overlaid inverse Fourier transforms restricted to the blue and red areas of the FTs in (a) and (b). (e) Trace from the Γ–point to the Bragg peaks as a function of energy averaged along the dashed lines in the FTs (no data is available near EFE_{\mathrm{F}}). The green dashed line marks the Bragg peak, the blue one marks the CDW peak, and the red dotted lines mark two dispersing QPI features. (f) Topography in (c) with overlaid inverse Fourier transforms restricted to the blue and red areas of the FTs in (a) and (b). The white arrows indicate selected hole-doping defects.

The periodic modulations observed in the topographic and spectroscopic images can be easily isolated by Fourier transform (FT), with distinct features observed in the positive and negative bias images of ZrSe2\mathrm{ZrSe}_2. The crisp atomic lattice resolved at positive bias yields well-defined Bragg peaks at qBq_{\mathrm{B}} outlined in green in the inset of Figure 1a. At negative bias, the Bragg peaks are weaker and significantly more diffuse (inset in Figure 1b). The focus of this study is on the Fourier components near q1/2=12qBq_{1/2} = \frac{1}{2}q_{\mathrm{B}} present at both polarities but with very different bias dependencies (Figure 1e). FTs of positive bias images show very weak peaks near q1/2q_{1/2} outlined in red in Figure 1a. Their centre of mass shifts towards smaller qq-values with increasing imaging voltage (Figure 1e) while becoming more and more diffuse. Higher positive bias images show finite scattering amplitude in the entire hexagonal region defined by the six Bragg peaks. In contrast, the FTs of negative bias images reveal more defined peaks at q1/2q_{1/2} outlined in blue in Figure 1b. These peaks do not shift as a function of tunnelling bias (Figure 1e), and no additional diffuse amplitude covers the hexagonal region defined by the Bragg peaks.

The spatial distribution and amplitude of the dispersing and non-dispersing modulations introduced above can be obtained through the inverse FT of the components outlined in blue and in red in Figure 1a,Figure 1b. The composite images obtained by overlaying these spatial distributions on the topographic images in Figure 1d,Figure 1f clearly show that the dispersing (red) and non-dispersing (blue) components originate in different regions on the surface.

The dispersing modulations develop in the immediate vicinity of the sharp atomic defects observed in positive bias topographic images and rapidly decay with distance from them. In contrast, the non-dispersing components are primarily located in between them. As demonstrated below, the dispersing charge modulations observed above +100 mV are the result of quasiparticle interference, whereas the non-dispersing modulations with periodicity 2a2a observed between −800 mV and +50 mV are CDWs. The latter appear only in regions where local electron doping shifts the Fermi level into the conduction band.

The periodic modulations observed near q1/2q_{1/2} at positive and negative bias are of a very different nature. The dispersing q\mathbf{q}-vector as a function of tunnelling bias (Figure 1e) and the absence of contrast inversion clearly identify the modulations observed at positive bias above +100 mV as quasiparticle interference. They are associated with the sharp rise of the tunnelling conductance with bias above the semiconducting gap, corresponding to a large density of states available for scattering. Many bands contribute to this DOS, with many possible scattering vectors which ultimately cover the entire phase space inside the hexagon defined by the Bragg peaks (see inset in Figure 1a). Note that the Bragg peaks are very sharp, indicating that they are not affected by higher-order components that would be expected if the peaks near q1/2q_{1/2} were a CDW. On the other hand, the periodic modulations observed between −800 mV and +50 mV correspond to well-defined q\mathbf{q}-vectors (Figure 1e) and comply with all the criteria expected for a CDW: their q\mathbf{q}-vector of q1/2=12qBq_{1/2} = \frac{1}{2}q_B does not depend on the imaging voltage, they appear alongside a gap in the local DOS at the Fermi level, and their contrast is inverting across this gap in topographic and spectroscopic images. [21] The broad q1/2q_{1/2} components reflect the lack of long-range order and limited size of the CDW domains. Here, the Bragg peaks are similarly diffuse, consistent with a commensurate CDW at q1/2q_{1/2} whose higher-order components will coincide with and affect the peaks at qBq_B.

As seen in the conductance map in Figure 2a, the CDW revealed here by STM in bulk ZrSe2_2 is a 2a×2a2a \times2a charge modulation with different strengths of its three characteristic q\mathbf{q}-vectors, giving it a 1Q, 2Q or 3Q character[26] depending on location on the surface. The stripy character of the CDW in some regions has been reported previously on other TMD compounds. The associated suppression of some of the q\mathbf{q}-vectors has been explained in terms of strain[27, 28, 29] or local doping.[30] Here, we find no clear experimental evidence for local strain in the 1Q and 2Q regions, although we cannot exclude that some of the dopant atoms might induce local strain. On the other hand, we find that the conduction band minimum is closer to EFE_F in these regions, indicating a lower degree of electron doping compared to the 3Q regions. The CDW contrast inversion across the gap near EFE_F is seen in Figure 2b, where we plot the conductance averaged along YY as a function of position XX and energy in the 1Q region outlined by the white box in Figure 2a.

Figure 2. (a) Normalized STS map at −9-9 mV revealing CDW modulations. (b) dI/dV(V)dI/dV(V) map as a function of position and energy averaged along the YY direction at each position XX over the white rectangle in (a), showing the CDW contrast inversion across EFE_F.

Most relevant for the present study is that the CDW primarily develops in regions where local impurities induce electron doping. This is exemplified by the strong correlation between the dark defects seen at large negative bias in Figure 1c and the blue regions corresponding to finite CDW amplitudes in Figure 1f. These dark defects correspond to electron doping by subsurface defects. The bright defects identified by arrows in Figure 1c,Figure 1f correspond to local hole doping by other subsurface defects. They shift the Fermi level below the conduction band edge, leading to a suppression of the CDW amplitude. One may realise that the contrast in Figure 1b is opposite to the above defect analysis, with the CDW developing in the bright regions. This apparent contradiction is a direct consequence of the setpoint dependence of the tunnelling current in the presence of a semiconducting gap. Indeed, for a large negative bias setpoint outside the semiconducting gap shown in Figure 3a, the integrated DOS available for tunnelling is reduced as the Fermi level is shifting into the conduction band (i.e. for electron doping), and the tip will have to move closer to the surface to maintain a constant tunnelling current. Hence, electron doping defects appear as depressions (i.e. dark Figure 1c). The opposite is true when tunnelling at a small negative setpoint voltage within the semiconducting gap (Figure 3b). In this case, the integrated DOS available for tunnelling is larger when the Fermi level is shifted higher into the conduction band. Consequently, the tip has to be retracted to maintain a constant tunnelling current and the corresponding surface region appears high (i.e. bright in Figure 1b).

Figure 3. Two averaged dI/dV(V)dI/dV(V) spectra on a log scale from a grid with different setpoint bias, −300-300 mV and +600+600 mV for (a) and (b), respectively. The small inserts in each graph show conceptual sketches of the corresponding tip-sample distance.

The direct link between electron doping and the emergence of a CDW reconstruction is very explicit in Figure 4. Figure 4a shows the amplitude of the CDW Fourier component as a function of position along the trace displayed in the inset. In Figure 4b, we present a grey-scale plot of the tunnelling conductance as a function of energy and position along the same trace. The minimum of the conduction band edge is at the Fermi level –highlighted by a red dashed line– in the regions devoid of any CDW modulations. Remarkably, we measure a finite CDW amplitude wherever the conduction band edge shifts below EFE_F, with the appearance of a slight depression in the conductance near EFE_F corresponding to the CDW gap. To emphasise these characteristic spectral features, we consider the dI/dV(V)dI/dV(V) curves in three selected boxes outlined in Figure 4b and plot their average in the corresponding colour in Figure 4c. The semiconducting gap extends to the Fermi level (yellow spectrum in Figure 4c) in the central region where no CDW modulation is detected (yellow box). Conversely, in regions where a finite CDW amplitude is detected, the edge of the conductance band is significantly below EFE_F, with a gap appearing at EFE_F (red and blue spectra in Figure 4c). Note that the gap is more pronounced in the region outlined in red, where the CDW Fourier component is stronger compared to the region outlined in blue.

Figure 4. CDW modulation amplitude versus spectroscopic signal near EFE_F. (a) CDW modulation amplitude along the black line in the inset CITS map. (b) Grey-scale plot of the dI/dV(V)dI/dV(V) spectra measured along the same line as panel (a). (c) Normalized dI/dV(V)dI/dV(V) spectra averaged over the boxes with corresponding colour in panel (b).

Band structure calculations [31] suggest that the CDW and QPI feature we observe on ZrSe2_2 originate in different electronic bands. The CDW lives in the lowest available conduction band, whose minimum lies at the MM–point. The next band above EFE_F is a few hundred meV higher, with a minimum at the Γ\Gamma–point. States at Γ\Gamma (i.e with small k∥k_\parallel) decay slower into the vacuum and thus contribute more to the tunnelling current than states at the MM–point with a large parallel momentum to the surface in a 2D crystal. [32] Therefore, the bottom of the conduction band at the MM–point can only be measured at low bias when the tip is close to the surface and when only the lowest energy states are sampled in the tunnelling process.

By increasing the tunnelling bias, we probe deeper into the conduction band, resulting in the tunnelling current being dominated by the states at the Γ\Gamma–point, which are not involved in the CDW reconstruction but contribute to QPI. This explains the different nature of the periodic modulations resolved above and below Vbias=+100V_{\mathrm{bias}} = +100 meV.

Angle-resolved photoemission spectroscopy (ARPES) of alkali metal and copper intercalated ZrSe2_2 [33, 34, 35] further support our data analysis. These experiments clearly show that electron doping from the intercalated atoms shifts EFE_F into the conduction band and forms electron pockets at the MM–point. The q1/2q_{1/2} CDW modulation is associated with nesting vectors connecting these pockets. [20] We do not introduce intentional dopant atoms into our crystals. However, stoichiometric ZrSe2_2 single crystals are challenging to grow, and the dopant atoms in our case are most likely self-intercalated excess Zr atoms, [36] which are expected to electron dope the system.

In summary, analysing scanning tunnelling conductance maps as a function of energy, we find that intrinsic doping induces a 2a×2a2a \times2a CDW modulation at the cleaved surface of bulk ZrSe2_2. Electron doping causes the Fermi level to shift into the conduction band whose minimum sits at the MM–point, which triggers the formation of a CDW reconstruction and the opening of a gap at the Fermi level. STS, ARPES and theoretical band structure calculations explain the set-point-specific differences in spectroscopy and topography images in terms of momentum selectivity in the STM tunnelling process. Our study unambiguously demonstrates the ability to tune the CDW phase transition by means of electron doping in a semiconducting bulk TMD. In addition to paving the way for applications exploiting tuneable CDW ground states, these results enable further studies to understand the CDW formation mechanism. Of particular interest is quasiparticle interference imaging as a function of non-local doping using field effect or space charge doping to map the band structure in the vicinity of the Fermi level in the presence or absence of a CDW over the same area.

Acknowledgement

We thank A. Guipet and G. Manfrini for their technical assistance with the scanning probe instruments. This work was supported by the Swiss National Science Foundation (Division II Grant No. 182652).

References

  1. [1]Saito, Y.; Nojima, T.; Iwasa, Y. Highly crystalline 2D superconductors. Nature Reviews Materials 2016, 2, 1–18.DOI
  2. [2]Novoselov, K. S.; Mishchenko, A.; Carvalho, A.; Castro Neto, A. H. 2D materials and van der Waals heterostructures. Science 2016, 353, aac9439.DOI
  3. [3]He, F.; Zhou, Y.; Ye, Z.; Cho, S.-H.; Jeong, J.; Meng, X.; Wang, Y. Moiré patterns in 2D materials: A review. ACS nano 2021, 15, 5944–5958.DOI
  4. [4]Kou, L.; Ma, Y.; Sun, Z.; Heine, T.; Chen, C. Two-dimensional topological insulators: Progress and prospects. The journal of physical chemistry letters 2017, 8, 1905–1919.DOI
  5. [5]Hwang, J.; Ruan, W.; Chen, Y.; Tang, S.; Crommie, M. F.; Shen, Z.-X.; Mo, S.-K. Charge density waves in two-dimensional transition metal dichalcogenides. Reports on Progress in Physics 2024, 87, 044502.DOI
  6. [6]Morosan, E.; Zandbergen, H. W.; Dennis, B.; Bos, J.; Onose, Y.; Klimczuk, T.; Ramirez, A.; Ong, N.; Cava, R. J. Superconductivity in CuₓTiSe₂. Nature Physics 2006, 2, 544–550.DOI
  7. [7]Chang, J.; Blackburn, E.; Holmes, A.; Christensen, N. B.; Larsen, J.; Mesot, J.; Liang, R.; Bonn, D.; Hardy, W.; Watenphul, A., et al. Direct observation of competition between superconductivity and charge density wave order in YBa₂Cu₃O₆.₆₇. Nature Physics 2012, 8, 871–876.
  8. [8]Singh, Y.; Nirmala, R.; Ramakrishnan, S.; Malik, S. K. Competition between superconductivity and charge-density-wave ordering in the Lu₃Ir₄(Si₁₋ₓGeₓ)₁₀ alloy system. Physical Review B 2005, 72, 045106.
  9. [9]Borisenko, S. V.; Kordyuk, A. A.; Zabolotnyy, V. B.; Inosov, D. S.; Evtushinsky, D.; Büchner, B.; Yaresko, A. N.; Varykhalov, A.; Follath, R.; Eberhardt, W., et al. Two energy gaps and Fermi-surface “arcs” in NbSe₂. Physical review letters 2009, 102, 166402.DOI
  10. [10]Bosak, A.; Souliou, S.-M.; Faugeras, C.; Heid, R.; Molas, M. R.; Chen, R.-Y.; Wang, N.-L.; Potemski, M.; Le Tacon, M. Evidence for nesting-driven charge density wave instabilities in the quasi-two-dimensional material LaAgSb₂. Physical Review Research 2021, 3, 033020.DOI
  11. [11]Strocov, V. N.; Shi, M.; Kobayashi, M.; Monney, C.; Wang, X.; Krempasky, J.; Schmitt, T.; Patthey, L.; Berger, H.; Blaha, P. Three-dimensional electron realm in VSe₂ by soft-x-ray photoelectron spectroscopy: Origin of charge-density waves. Physical Review Letters 2012, 109, 086401.pubmed.ncbi.nlm.nih.gov/23002761
  12. [12]Giambattista, B.; Slough, C. G.; McNairy, W. W.; Coleman, R. V. Scanning tunneling microscopy of atoms and charge-density waves in 1T-TaS₂, 1T-TaSe₂, and 1T-VSe₂. Physical Review B 1990, 41, 10082.pubmed.ncbi.nlm.nih.gov/9993392
  13. [13]Johannes, M. D.; Mazin, I. I. Fermi surface nesting and the origin of charge density waves in metals. Physical Review B 2008, 77, 165135.DOI
  14. [14]Zhu, X.; Cao, Y.; Zhang, J.; Plummer, E.; Guo, J. Classification of charge density waves based on their nature. Proceedings of the National Academy of Sciences 2015, 112, 2367–2371.DOI
  15. [15]Valla, T.; Fedorov, A. V.; Johnson, P. D.; Glans, P. A.; McGuinness, C.; Smith, K. E.; Andrei, E. Y.; Berger, H. Quasiparticle Spectra, Charge-Density Waves, Superconduc- tivity, and Electron-Phonon Coupling in 2H-NbSe₂. Physical review letters 2004, 92, 086401.
  16. [16]Xie, Y.; Li, Y.; Bourges, P.; Ivanov, A.; Ye, Z.; Yin, J.-X.; Hasan, M. Z.; Luo, A.; Yao, Y.; Wang, Z., et al. Electron-phonon coupling in the charge density wave state of CsV₃Sb₅. Physical Review B 2022, 105, L140501.DOI
  17. [17]Weber, F.; Rosenkranz, S.; Castellan, J.-P.; Osborn, R.; Karapetrov, G.; Hott, R.; Heid, R.; Bohnen, K.-P.; Alatas, A. Electron-phonon coupling and the soft phonon mode in TiSe₂. Physical review letters 2011, 107, 266401.pubmed.ncbi.nlm.nih.gov/22243169
  18. [18]Otto, M. R.; Pö hls, J.-H.; René de Cotret, L. P.; Stern, M. J.; Sutton, M.; Siwick, B. J. Mechanisms of electron-phonon coupling unraveled in momentum and time: The case of soft phonons in TiSe₂. Science Advances 2021, 7, eabf2810.DOI
  19. [19]Si, J. G.; Lu, W. J.; Wu, H. Y.; Lv, H. Y.; Liang, X.; Li, Q. J.; Sun, Y. P. Origin of the multiple charge density wave order in 1T-VSe₂. Physical Review B 2020, 101, 235405.DOI
  20. [20]Ren, M.-Q.; Han, S.; Fan, J.-Q.; Wang, L.; Wang, P.; Ren, W.; Peng, K.; Li, S.; Wang, S.-Z.; Zheng, F.-W., et al. Semiconductor–Metal Phase Transition and Emergent Charge Density Waves in 1T–ZrX₂ (X = Se, Te) at the Two-Dimensional Limit. Nano Letters 2022, 22, 476–484.DOI
  21. [21]Spera, M.; Scarfato, A.; Pásztor, Á.; Giannini, E.; Bowler, D. R.; Renner, Ch. Insight into the Charge Density Wave Gap from Contrast Inversion in Topographic STM Images. Physical Review Letters 2020, 125, 267603.DOI
  22. [22]Bin Subhan, M. K.; Suleman, A.; Moore, G.; Phu, P.; Hoesch, M.; Kurebayashi, H.; Howard, C. A.; Schofield, S. R. Charge density waves in electron-doped molybdenum disulfide. Nano letters 2021, 21, 5516–5521.DOI
  23. [23]Ubaldini, A.; Jacimovic, J.; Ubrig, N.; ; Giannini, E. Chloride-Driven Chemical Vapor Transport Method for Crystal Growth of Transition Metal Dichalcogenides. Crystal Growth and Design 2013, 13, 4453.DOI
  24. [24]Whitehouse, C. R.; Balchin, A. A. Non-stoichiometry in ZrS₂ and ZrSe₂. Physica Status Solidi A 1978, 47, K173.
  25. [25]Quang, T. L.; Nogajewski, K.; Potemski, M.; Dau, M. T.; Jamet, M.; Mallet, P.; Veuillen, J.-Y. Band-bending induced by charged defects and edges of atomically thin transition metal dichalcogenide films. 2D Materials 2018, 5, 035034.DOI
  26. [26]McMillan, W. L. Theory of discommensurations and the commensurate-incommensurate charge-density-wave phase transition. Physical Review B 1976, 14, 1496–1502.DOI
  27. [27]Soumyanarayanan, A.; Yee, M. M.; He, Y.; Van Wezel, J.; Rahn, D. J.; Rossnagel, K.; Hudson, E.; Norman, M. R.; Hoffman, J. E. Quantum phase transition from triangular to stripe charge order in NbSe₂. Proceedings of the National Academy of Sciences 2013, 110, 1623–1627.DOI
  28. [28]Rahnejat, K.; Howard, C.; Shuttleworth, N.; Schofield, S.; Iwaya, K.; Hirjibehedin, C.; Renner, Ch.; Aeppli, G.; Ellerby, M. Charge density waves in the graphene sheets of the superconductor CaC₆. Nature communications 2011, 2, 558.DOI
  29. [29]Cossu, F.; Palotás, K.; Sarkar, S.; Di Marco, I.; Akbari, A. Strain-induced stripe phase in charge-ordered single layer NbSe₂. NPG Asia Materials 2020, 12, 24.DOI
  30. [30]Novello, A. M.; Spera, M.; Scarfato, A.; Ubaldini, A.; Giannini, E.; Bowler, D. R.; Renner, Ch. Stripe and Short Range Order in the Charge Density Wave of 1T-CuₓTiSe₂. Physical review letters 2017, 118, 017002.DOI
  31. [31]Zhao, Q.; Guo, Y.; Si, K.; Ren, Z.; Bai, J.; Xu, X. Elastic, electronic, and dielectric properties of bulk and monolayer ZrS₂, ZrSe₂, HfS₂, HfSe₂ from van der Waals density-functional theory. physica status solidi (b) 2017, 254, 1700033.
  32. [32]Wiesendanger, R.; Güntherodt, H.-J. Scanning tunneling microscopy III: theory of STM and related scanning probe methods; Springer Science & Business Media, 2013; Vol. 29.
  33. [33]Muhammad, Z.; Mu, K.; Lv, H.; Wu, C.; ur Rehman, Z.; Habib, M.; Sun, Z.; Wu, X.; Song, L. Electron doping induced semiconductor to metal transitions in ZrSe₂ layers via copper atomic intercalation. Nano research 2018, 11, 4914–4922.arxiv.org/abs/1803.08242
  34. [34]Muhammad, Z.; Li, Y.; Ullah, S.; Khan, F.; Alarfaij, S. S.; Alanazi, A. M.; Sun, Z.; Alshahrani, T.; Zhang, Y.; Zhao, W. Extrinsic n-type semiconductor transition in ZrSe₂ with the metallic character through hafnium substitution. Journal of Alloys and Compounds 2024, 980, 173616.DOI
  35. [35]Wang, S.; Lawan, M. A.; Zareen, S.; Moses, O. A.; Zhu, W.; Wu, X.; Sun, Z.; Song, L., et al. Band structure tailoring in ZrSe₂ single crystal via trace rhenium intercalation. Applied Physics Letters 2019, 115.DOI
  36. [36]Brauer, H. E.; Starnberg, H. I.; Holleboom, L. J.; Hughes, H. P. The electronic structure of ZrSe₂ and CsₓZrSe₂ studied by angle-resolved photoelectron spectroscopy. Journal of Physics: Condensed Matter 1995, 7, 7741.

Paper details

vlnc:W_gqgn3tpm
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents