betaFeedback

WorksPhysics and Astronomy

Anomalous Hall effect from inter-superlattice scattering in a noncollinear antiferromagnet

Abstract

Superlattice formation dictates the physical properties of many materials, including the nature of the ground state in magnetic materials. Chemical composition is commonly considered to be the primary determinant of superlattice identity, especially in intercalation compounds. Here, we find that, contrary to this conventional wisdom, kinetic control of superlattice growth leads to the coexistence of disparate domains within a compositionally "perfect" single crystal. We demonstrate that Cr1/4_{1/4}TaS2_2 is a bulk noncollinear antiferromagnet in which scattering between bulk and minority superlattice domains engenders complex magnetotransport below the Néel temperature, including an anomalous Hall effect. We characterize the magnetic phases in different domains, image their nanoscale morphology, and propose a mechanism for nucleation and growth. These results provide a blueprint for the deliberate engineering of macroscopic transport responses via microscopic patterning of magnetic exchange interactions in superlattice domains.

Introduction

Superlattices impart emergent properties to many materials, including metal alloys,[1] semiconductors,[2] and ceramics.[3] The periodicity and symmetry of the long-range order determine the underlying many-body physics, with especially profound implications for quantum materials. Moiré superlattices, for example, host a plethora of emergent electronic phenomena, such as unconventional superconductivity,[4] correlated insulating states,5,6 and the quantum anomalous Hall effect.7,8 In magnetic materials, superlattices of the spin-bearing centers can dictate the distances between them, strongly influencing the microscopic magnetic exchange interactions and hence the ground state.9–11

The link between superlattice identity and magnetic ordering is especially apparent in transition metal dichalcogenides (TMDs) intercalated with first-row transition metals.12–14 In this family of materials, many types of magnetism can be accessed by varying the host lattice, intercalant, and stoichiometry, including hard ferromagnetism,15–17 noncollinear antiferromagnetism,18–20 and spin glass phases.21,22 Although off-stoichiometry and structural disorder are known to modify their magnetotransport properties,23–25 composition is generally treated as a proxy for the periodicity of the intercalant superlattice. Assuming a formula of TxMCh2T_xMCh_2, where TT is a first-row transition metal, MM is Nb or Ta, and ChCh is S or Se, it is typically assumed that x=1/4x = 1/4 results in a 2×22 \times2 superlattice, x=1/3x = 1/3 results in a (3×3)R30∘(\sqrt{3} \times\sqrt{3})R30^\circ superlattice, and intermediate compositions result in defective, disordered, or mixed superlattices.24,26–30 Nevertheless, since the magnetism of these materials is highly sensitive to the intercalant superlattice,26,31,32 precise control over atomic-scale ordering is necessary to realize transport signatures associated with specific magnetic phases, including noncollinear textures and altermagnetism.32–36

In this work, we synthesize the new material Cr1/4TaS2Cr_{1/4}TaS_2 and find that it is a bulk noncollinear antiferromagnet with a well-ordered 2×22 \times2 superlattice of Cr. Below the Néel temperature (TNT_\mathrm{N}) of 145 K, it exhibits an anomalous Hall response, which is inconsistent with the symmetry of the magnetic structure. Detailed characterization of the nanoscale atomic structure reveals minority domains with different superlattice ordering, even in high-quality, stoichiometric single crystals. We propose a mechanism for kinetically arrested growth of disparate superlattice domains and show that the complex magnetotransport originates from scattering between domains. The results show how variation of local ordering can be leveraged to tune magnetotransport in an antiferromagnet, with implications for designing transport responses via deliberate superlattice engineering without changes in chemical composition.

Results

We initially targeted the compound Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2} with the hypothesis that Cr3+\mathrm{Cr}^{3+} (S=3/2S = 3/2) is a promising intercalant for targeting a noncollinear ground state: it has a largely quenched orbital moment37 and strong easy-plane anisotropy,38 which can lead to predictable interplay between second-order perturbations and Heisenberg exchange. For example, in Cr1/3NbS2\mathrm{Cr}_{1/3}\mathrm{NbS}_{2} and Cr1/3TaS2\mathrm{Cr}_{1/3}\mathrm{TaS}_{2}, the Dzyaloshinskii–Moriya interaction arising from broken inversion symmetry competes with ferromagnetic coupling, resulting in chiral helimagnetism.39–41 We thus surmised that putting Cr3+\mathrm{Cr}^{3+} on a geometrically frustrated triangular lattice with antiferromagnetic (AFM) coupling would favor a noncollinear ground state to relieve the frustration (Figure 1a), potentially yielding an anomalous Hall response.18–20,42–44

Figure 1. Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2 is a noncollinear antiferromagnet. (a) Local dd-orbital splitting for Cr3+\mathrm{Cr}^{3+}, and design principle for noncollinear antiferromagnetism. (b) Structure of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2 from single-crystal X-ray diffraction. The unit cell (2×2×12 \times2 \times1 relative to 2H2H-TaS2\mathrm{TaS}_2) is indicated in black and the triangular lattice is emphasized in purple. (c) Heat capacity (CpC_p) vs. TT normalized to the formula CrTa4S8\mathrm{CrTa}_4\mathrm{S}_8. (d) Single-crystal neutron diffraction data: Integrated intensities of the (1/3,1/3,2)(1/3, 1/3, 2) peak vs. TT, and the (1/3,1/3,2)(1/3, 1/3, 2) peak at different temperatures (solid lines indicate Gaussian fits), associated with the propagation vector k=(1/3,1/3,0)\mathbf{k} = (1/3, 1/3, 0). (e) 120∘120^\circ antiferromagnetic structure as obtained from neutron diffraction (Γ6\Gamma_6 representation). The (3×3)R30∘×1(\sqrt{3} \times\sqrt{3})R30^\circ\times1 magnetic unit cell (relative to the 2×2×12 \times2 \times1 Cr superlattice) is shown in light blue, and the nuclear unit cell is shown in black. The magnetic structure is invariant with respect to the three mirror planes perpendicular to the magnetic moments (dotted black lines).

Single crystals of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2} were grown from the constituent elements using chemical vapor transport with iodine as a transport agent. We found that Cr crystallographic disorder was minimized in a two-zone furnace with the hot zone at 1100 °C and the cold (growth) zone at 1000 °C, and a cooling rate of 20 °C/hour. The structure, as determined by single-crystal X-ray diffraction (SCXRD), consists of 2H2H-TaS2\mathrm{TaS}_{2} layers with 1/4 of the pseudo-octahedral sites in the van der Waals gap occupied by Cr, forming a 2×22 \times2 superlattice (Figure 1b; more details of the refinement in Table S1 and Table S2). Within the sensitivity limits of a laboratory diffractometer, we detect no evidence of Cr deficiency on the 2a2a site, electron density on the 6g6g site, or additional reflections corresponding to the (3×3)R30∘(\sqrt{3} \times\sqrt{3})\mathrm{R}30^\circ superlattice (Figure S1). Unless otherwise indicated, all experiments were carried out on crystals from two batches with “perfect” (within experimental error) 2×22 \times2 Cr stoichiometries of x=0.252(3)x = 0.252(3) as determined by energy dispersive X-ray spectroscopy (EDS, Figure S2), and a fully occupied 2×22 \times2 superlattice as determined by SCXRD (see the Supplementary Information for more details on crystal growth and compositional characterization).

Empirical formulaCrTa4S8\mathrm{CrTa}_{4}\mathrm{S}_{8}
Formula weight (g/mol)1032.27
Temperature (K)293(2)
Wavelength (Å)0.71073
Crystal systemHexagonal
Space groupP63/mmcP6_{3}/mmc
aa (Å)6.5959(3)
cc (Å)12.0391(7)
Volume (Å−3^{-3})453.60(5)
ZZ2
Density (calculated) (g/cm3^{3})7.558
Absorption coefficient (mm−1^{-1})50.985
FF(000)888
Crystal size (mm3^{3})0.031 × 0.023 × 0.015
θ\theta (°)3.384 to 29.622
Index ranges−9≤h≤8-9 \le h \le8
−8≤k≤9-8 \le k \le9
−16≤l≤16-16 \le l \le16
Reflections collected18880
Independent reflections272
Completeness to θfull\theta_{\mathrm{full}}0.975
Absorption correctionSemi-empirical from equivalents
Refinement methodFull-matrix least-squares on F2F^{2}
Data / restraints / parameters272 / 0 / 18
Goodness-of-fit on F2F^{2}1.331
Final RR indices [I>2σ(I)I > 2\sigma(I)]R1=0.0404R_{1} = 0.0404, wR2=0.1430wR_{2} = 0.1430
RR indices (all data)R1=0.0438R_{1} = 0.0438, wR2=0.1450wR_{2} = 0.1450
Largest diff. peak and hole (e Å−3^{-3})4.46 and −4.24

Table S1. Crystal data and refinement details for Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2} from single-crystal X-ray diffraction.

Atom LabelxxyyzzSiteUisoU_{\mathrm{iso}}
Cr1001/21/22a0.0121(13)
Ta2001/41/42b0.0064(5)
Ta30.49435(7)0.50565(7)1/41/46h0.0063(4)
S40.1667(3)0.3334(5)0.3809(3)12k0.0074(8)
S52/32/31/31/30.1188(5)4f0.0076(11)

Table S2. Atomic coordinates, Wyckoff positions, and equivalent isotropic displacement parameters for Cr1/4Ta2\mathrm{Cr}_{1/4}\mathrm{Ta}_2 from single-crystal X-ray diffraction.

Reconstructed (HK0), (H0L), and (HHL) scattering planes

Figure S1. Reconstructed (HK0)(HK0), (H0L)(H0L), and (HHL)(HHL) scattering planes from single-crystal X-ray diffraction of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2}. Bragg peaks associated with the 2H2H-TaS2\mathrm{TaS}_{2} host lattice and 2×22 \times2 Cr superlattice are circled in light blue and navy, respectively.

Figure S2. Representative energy dispersive X-ray spectroscopy data for a single crystal of Cr1/4_{1/4}TaS2_2, with peaks corresponding to Cr, Ta, S, and C labeled. The atomic ratio determined by fitting the Cr Kα1\alpha_{1}, Ta Mα1\alpha_{1}, and S Kα1\alpha_{1} peaks yields a formula of Cr0.252(3)_{0.252(3)}TaS1.78(5)_{1.78(5)} for this crystal.

Heat capacity and neutron diffraction measurements establish that Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2 is a bulk antiferromagnet with TN=145T_N = 145 K. A single λ\lambda anomaly in the heat capacity (CpC_p) is observed at 145 K (Figure 1c and inset), indicating a bulk phase transition at this temperature. Using single-crystal neutron diffraction in the (HHL)(HHL) scattering plane, we observe satellite peaks below 150 K consistent with the magnetic propagation vector k=(1/3,1/3,0)\mathbf{k} = (1/3, 1/3, 0), corresponding to the onset of AFM ordering (Figure 1d). (Due to crystal size requirements, we measured a slightly Cr-deficient crystal with x=0.226(6)x = 0.226(6).) Representation analysis of the observed kk using SARAh45 indicates that the magnetic representation Γmag\Gamma_{\mathrm{mag}} can be decomposed into six irreducible representations (Γmag=Γ1+Γ2+Γ3+Γ4+2Γ5+2Γ6\Gamma_{\mathrm{mag}} = \Gamma_1 + \Gamma_2 + \Gamma_3 + \Gamma_4 + 2\Gamma_5 + 2\Gamma_6), of which Γ5\Gamma_5 and Γ6\Gamma_6 are consistent with the easy-plane anisotropy. The only stable refinement of data collected at 1.5 K is obtained with Γ6\Gamma_6, which corresponds to an in-plane cycloidal structure with parallel orientation of moments along cc. When an equal moment constraint is applied, the value refines to 2.07(8) μB/Cr2.07(8)\,\mu\mathrm{B}/\mathrm{Cr}, with the spins oriented along the ⟨100⟩\langle100\rangle directions, i.e. a 120° AFM structure (Figure 1e). The lower-than-expected moments (compared to the theoretical 3 μB/Cr3+3\,\mu\mathrm{B}/\mathrm{Cr}^{3+}) could be a consequence of itinerant magnetism, which has been observed in related materials.35,36,46 Additional details of the refinement are available in the Supplementary Information (Table S3–Table S5). Altogether, the heat capacity and neutron diffraction data unambiguously point to a single bulk AFM transition in Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2 at 145 K.

Table S3: Refinement details for the nuclear structure of Cr0.226(6)TaS2\mathrm{Cr}_{0.226(6)}\mathrm{TaS}_2 from single-crystal neutron diffraction.

ParameterValue
Crystal mass (mg)16.0
Temperature (K)1.5
Wavelength (Å)1.486
Space groupP63/mmcP6_3/mmc
aa (Å)6.619(5)
cc (Å)11.961(9)
Volume (Å−3^{-3})453.8(6)
RF2R_F^24.64
RwF2R_{wF}^26.36
RFR_F5.05
χ2(I)\chi^2(I)5.87
NeffN_{\mathrm{eff}} reflections58 [I>2σI > 2\sigma]
Scale factor693(12)

Table S3.

ParameterValue
Crystal mass (mg)16.0
Temperature (K)1.5
Wavelength (Å)1.486
RepresentationΓ6\Gamma_{6}
k1\mathbf{k}_{1}(+1/3,+1/3,0)(+1/3, +1/3, 0)
k2\mathbf{k}_{2}(−1/3,−1/3,0)(-1/3, -1/3, 0)
RF2R_{F}^{2}19.8
RwF2R_{wF}^{2}30.8
RFR_{F}10.2
χ2(I)\chi^{2}(I)3.22
NeffN_{\mathrm{eff}} reflections19 [I>2σ][I > 2\sigma]
Cr1 moment (μB\mu_{\mathrm{B}})2.07(8)

Table S5. Refinement details for the magnetic structure of Cr0.226(6)TaS2\mathrm{Cr}_{0.226(6)}\mathrm{TaS}_{2} from single-crystal neutron diffraction.

Electrical transport measurements on bulk single crystals of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2 reveal metallic behavior from the in-plane longitudinal resistivity (ρxx\rho_{xx}) (Figure 2a). A sharp drop at TN=145T_{\mathrm{N}} = 145 K is consistent with reduced carrier scattering upon bulk AFM ordering. The residual resistivity ratio, RRR=ρ300K/ρ2.5KRRR = \rho_{300\mathrm{K}}/\rho_{2.5\mathrm{K}}, is about 10, indicating good crystal quality. The in-plane Hall resistivity (ρxy\rho_{xy}) is dominated by the ordinary Hall effect (Figure 2b). An anomalous Hall contribution, evidenced by jumps in ρxy\rho_{xy} centered at zero field, is present below TNT_{\mathrm{N}} (Figure 2c,Figure 2d). We fit ρxy\rho_{xy} for fields smaller than 5 T to a single-band model comprising an ordinary Hall component and a small component from an anomalous Hall effect (AHE), ρxy=1neμ0H+ρAHE\rho_{xy} = \frac{1}{ne}\mu_0 H + \rho_{\mathrm{AHE}}. From the ordinary Hall component, we extract carrier concentrations (nhn_{\mathrm{h}}) for the dominant hole carriers on the order of 1021 cm−310^{21}\,\mathrm{cm}^{-3}, and carrier mobilities (μh\mu_{\mathrm{h}}) up to 138 cm2 V−1s−1138\,\mathrm{cm}^2\,\mathrm{V}^{-1}\mathrm{s}^{-1} at 2.5 K (Figure 2e), reasonable values for an electron-doped intercalation compound of 2H-TaS2_2.16 The faster decrease in nhn_{\mathrm{h}} below 150 K may correspond to Fermi surface reconstruction as a result of AFM ordering.47

Magnetotransport properties of Cr$_{1/4}$TaS$_2$

Figure 2. Magnetotransport properties of Cr1/4_{1/4}TaS2_2. (a) In-plane longitudinal resistivity (ρxx\rho_{xx}) and dρxx/dTd\rho_{xx}/dT vs. TT. (b) In-plane Hall resistivity (ρxy\rho_{xy}) vs. μ0H\mu_0 H, and schematic of the measurement configuration. Colors indicate temperatures as labeled in (C). (c) Anomalous Hall resistivity (ρAHE\rho_{\mathrm{AHE}}) vs. μ0H\mu_0 H at different temperatures. Translucent lines are the raw data; opaque lines are denoised. (d) The saturation values of ρAHE\rho_{\mathrm{AHE}} vs. TT. (e) Charge carrier concentration (nhn_h) and carrier mobility (μh\mu_h) vs. TT, as derived from the ordinary Hall component of ρxy\rho_{xy}. (f) Magnetoresistance (MR) vs. μ0H\mu_0 H at different temperatures. Colors indicate temperatures as labeled in (C). (g) MR at 12 T vs. TT.

Several interesting features are observed in the temperature dependence of ρAHE\rho_{\mathrm{AHE}} (Figure 2c,Figure 2d). Below 40 K, ρAHE\rho_{\mathrm{AHE}} is negligible. Between 40 to 100 K, ρAHE\rho_{\mathrm{AHE}} is positive in sign and exhibits a small zero-field hysteresis of less than 1 T up to 80 K. The saturation magnitude of ρAHE\rho_{\mathrm{AHE}} increases with increasing TT in this regime. At 110 K, the circulation of ρAHE\rho_{\mathrm{AHE}} changes sign while retaining a similar magnitude. ρAHE\rho_{\mathrm{AHE}} then approaches zero with increasing temperature and vanishes above TNT_{\mathrm{N}}. The anomalous Hall conductivity, σAHE=ρAHE(ρAHE)2+(ρxx)2\sigma_{\mathrm{AHE}} = \frac{\rho_{\mathrm{AHE}}}{(\rho_{\mathrm{AHE}})^2+(\rho_{xx})^2}, has a maximum magnitude of about 9 Ω−1 cm−1\Omega^{-1}\,\mathrm{cm}^{-1} at 50 K.

The magnetoresistance (MR), defined as Δρxx(T,H)/ρxx(T,0)\Delta\rho_{xx}(T,H)/\rho_{xx}(T,0), also exhibits a complex temperature dependence (Figure 2f,Figure 2g). At 10 K and below, the MR is positive and approximately quadratic with respect to field. Above 10 K, the MR decreases quickly with increasing TT. The high-field MR becomes negative at 60 K and increases gradually in magnitude until 100 K. There is a significant decrease in the magnitude of the negative MR between 100 and 110 K. At intermediate temperatures in the positive and negative MR regimes, cusps are observed around zero field (Figure 2f inset). At 150 K and above, i.e. above TNT_{\mathrm{N}}, the MR becomes uniformly quadratic in field and remains negative.

The fact that a non-zero ρAHE\rho_{\mathrm{AHE}} and complex temperature-dependent MR are observed only below TNT_{\mathrm{N}} indicates that these magnetotransport phenomena are tied to the bulk AFM order.

The intrinsic anomalous Hall conductivity (AHC) can be evaluated from the integral of Berry curvature over the Brillouin zone within linear response theory. However, symmetry analysis of the magnetic structure shows that it is invariant with respect to the mirror planes perpendicular to the magnetic moments, as indicated by the dashed lines in Figure 1e. The Berry curvature is odd under these mirror symmetry transformations. Therefore, the intrinsic AHC sums to zero across the Brillouin zone.48 Hence, we sought to investigate mechanisms for an extrinsic, scattering-mediated AHE that could also explain the rich MR behavior.

Considering the nature of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2 as an intercalation compound, we used more sensitive probes of local symmetry to study possible intercalant disorder as a source of magnetic scattering. In confocal Raman microscopy (with a laser spot size of approximately 1 μm21\,\mathrm{\mu m}^{2}), we observe a sharp, intense phonon mode at 157 cm−1157\,\mathrm{cm}^{-1}, which we attribute to the 2×22 \times2 Cr superlattice (Figure 3a,Figure 3b).49,50 A small but sharp feature at 148 cm−1148\,\mathrm{cm}^{-1} is also present, which matches the 3×3\sqrt{3} \times\sqrt{3} superlattice mode observed in the compound Cr1/3TaS2\mathrm{Cr}_{1/3}\mathrm{TaS}_2.51 This suggests that a small amount of 3×3\sqrt{3} \times\sqrt{3} ordering with sub-micron in-plane domain sizes is present in bulk crystals of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2, and that these 3×3\sqrt{3} \times\sqrt{3}-containing domains coexist with the dominant 2×22 \times2 superlattice.

Evidence for $\sqrt{3}\times\sqrt{3}$ domains in $\mathrm{Cr}_{1/4}\mathrm{TaS}_2$, including crystal structures, Raman spectra, electron diffraction, 4D-STEM images, magnetic susceptibility, magnetization, and an Arrott plot

Figure 3. Evidence for 3×3\sqrt{3}\times\sqrt{3} domains in Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2. (a) Structures of 2H2H-TaS2\mathrm{TaS}_2, Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2, and Cr1/3TaS2\mathrm{Cr}_{1/3}\mathrm{TaS}_2, with 1×11\times1, 2×22\times2, and 3×3\sqrt{3}\times\sqrt{3} unit cells. (b) Raman spectra of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2, Cr1/3TaS2\mathrm{Cr}_{1/3}\mathrm{TaS}_2, and 2H2H-TaS2\mathrm{TaS}_2, with Cr superlattice phonon modes highlighted. (c) Selected area electron diffraction of an exfoliated flake of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2, with primitive and superlattice reflections indicated. (d) Virtual dark-field images from four-dimensional scanning transmission electron microscopy (4D-STEM) reconstructed using the intensities of 2×22\times2 and 3×3\sqrt{3}\times\sqrt{3} Bragg disks. (e) 4D-STEM diffraction patterns from the regions indicated in (d). (f) Field-cooled (FC) and zero-field-cooled (ZFC) DC magnetic susceptibility (χDC\chi_{\mathrm{DC}}) vs. TT, measured with a 100 Oe field parallel and perpendicular to cc. (g) Real part of the AC susceptibility (χAC′\chi'_{\mathrm{AC}}) vs. TT, measured with an in-plane AC field of 10 Oe. (h) Isothermal magnetization (MM) vs. μ0H⊥c\mu_0H\perp c. (i) Arrott plot with linear fit to the 98 K trace.

Electron diffraction studies on Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2 unambiguously confirm the existence of ordered 3×3\sqrt{3} \times\sqrt{3}-containing domains, and furthermore demonstrate nanoscale domains of different superlattices. Selected area electron diffraction (SAED) of a mechanically exfoliated flake in a circular region with a radius of ∼700 nm\sim700\,\mathrm{nm} shows 2×22 \times2 superlattice reflections, as well as significantly weaker but sharp 3×3\sqrt{3} \times\sqrt{3} reflections (Figure 3c). To investigate the spatial distribution of superlattice domains, we used four-dimensional scanning transmission electron microscopy (4D-STEM). In 4D-STEM, a converged electron beam (∼6 nm\sim6\,\mathrm{nm} under our experimental conditions) is scanned across a two-dimensional (2D) area of the sample, and 2D diffraction data is collected at each probe position.52 Virtual dark-field images reconstructed using the intensities of 2×22 \times2 and 3×3\sqrt{3} \times\sqrt{3} Bragg disks reveal in-plane spatial separation of superlattices (Figure 3d). The 2×22 \times2 superlattice is dominant over the entire area except for two small regions that resemble pinched triangles. These 2×22 \times2-deficient regions precisely

correspond to the brightest regions in the 3×3\sqrt{3} \times\sqrt{3} map. Individual electron diffraction patterns shown in Figure 3e illustrate the evolution of superlattice order over a 100 nm length scale, showing mixed superlattices with maximal 3×3\sqrt{3} \times\sqrt{3} order, weaker 3×3\sqrt{3} \times\sqrt{3} order, and exclusive 2×22 \times2 order in moving from a triangular 3×3\sqrt{3} \times\sqrt{3}-containing region to a 2×22 \times2 region.

The presence of 3×3\sqrt{3} \times\sqrt{3} order offers a clue for interpreting bulk magnetometry data on Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2, which are inconsistent in several respects with the fully compensated AFM structure associated with the 2×22 \times2 Cr superlattice. A sharp rise in the field-cooled DC magnetic susceptibility (χDC\chi_{\mathrm{DC}}) below 100 K, along with marked bifurcation between zero-field-cooled and field-cooled traces, is suggestive of a minority ferromagnetic (FM) transition (Figure 3f). The larger χDC\chi_{\mathrm{DC}} with the magnetic field applied in-plane is consistent with the expected easy-plane behavior. Fitting χDC−1\chi_{\mathrm{DC}}^{-1} to the Curie–Weiss law, χ−1=(T−θCW)/C\chi^{-1} = (T-\theta_{\mathrm{CW}})/C, yields C=1.77(4)C = 1.77(4) emu K (mol Cr)−1^{-1} and θCW=32(1)\theta_{\mathrm{CW}} = 32(1) K (Figure S3). We then obtain μeff=8C=3.76(8) μB/Cr\mu_{\mathrm{eff}} = \sqrt{8C} = 3.76(8)\,\mu_{\mathrm{B}}/\mathrm{Cr}, close to the theoretical spin-only value of 3.87 μB/Cr3.87\,\mu_{\mathrm{B}}/\mathrm{Cr} for Cr3+\mathrm{Cr}^{3+} (S=3/2S = 3/2). The value of θCW\theta_{\mathrm{CW}} is positive but considerably smaller than the temperature of the upturn in χDC\chi_{\mathrm{DC}}, suggesting the coexistence of AFM and FM coupling.53

Figure S3. Fitting of inverse DC susceptibility data vs. TT to the Curie–Weiss law, χ−1=(T−θCW)/C\chi^{-1} = (T-\theta_{\mathrm{CW}})/C, for a 1 T magnetic field perpendicular to cc.

The real part of the AC magnetic susceptibility (χAC′\chi_{\mathrm{AC}}^{\prime}) shows a cusp below 100 K, as well as a broader and more prominent feature with a maximum at about 40 K with a modest frequency dependence (Figure 3g and Figure S4). The peak at 40 K is especially pronounced in the imaginary part of the AC susceptibility (Figure S5). These observations suggest magnetic irreversibility at lower temperatures. We tentatively propose a reentrant spin glass (SG) state below 40 K that is driven by spin disorder arising from competition between AFM and FM exchange interactions.22,23 This interpretation is corroborated by the slow relaxation dynamics observed in thermoremanent magnetization measurements (Figure S6 and Table S6).54

Real part of the AC susceptibility measured at different frequencies

Figure S4. Real part of the AC susceptibility (χAC′\chi'_{\mathrm{AC}}), measured with an in-plane AC driving field of 10 Oe, fitted to a univariate spline in the vicinity of the spin glass transition temperature.

Plot of imaginary AC susceptibility versus temperature, with curves for frequencies 10 Hz, 27 Hz, 72 Hz, 193 Hz, 519 Hz, 1389 Hz, 3725 Hz, and 9984 Hz

Figure S5. Imaginary part of the AC susceptibility (χAC′′\chi^{\prime\prime}_{\mathrm{AC}}), measured with an in-plane AC driving field of 10 Oe.

Image not extracted

Figure S6. Thermoremanent magnetization curves obtained by field-cooling in a field of 1 T, removing the field, then measuring the magnetization as a function of time. Open circles represent the data, while solid lines represent fits to stretched exponential functions for 2 K, 15 K, 50 K, and 80 K.

TT (K)M0M_0 (μB\mu_{\mathrm{B}}/Cr)M1M_1 (μB\mu_{\mathrm{B}}/Cr)τ\tau (s)nn
20.28768(2)0.003641(6)1224.4(4)0.6541(7)
150.25815(2)0.007156(6)1231.3(2)0.6274(4)
500.18978(5)0.009451(9)2315.6(5)0.6586(4)
800.07196(3)0.01006(7)1425.8(2)0.6399(3)

Table S6. Parameters for fitting thermoremanent magnetization data to a stretched exponential function, M(t)=M0+M1exp⁡[−(tτ)1−n]M(t) = M_0 + M_1 \exp\left[-\left(\frac{t}{\tau}\right)^{1-n}\right], where M(t)M(t) is the total magnetization, tt is the time, M0M_0 is the constant magnetization, M1M_1 is the glassy component of the magnetization, τ\tau is the characteristic relaxation time, and nn is a stretching exponent.

Partial FM ordering in a minority of the sample is also supported by the isothermal magnetization (MM) vs. field traces (Figure 3h). At 4 K, MM with μ0H⊥c\mu_{0}H \perp c shows a small zero-field hysteresis of 400 Oe (Figure 3h inset). A detectable hysteresis persists up to 94 K (Figure S7), above which a slight “S”-shape remains below 150 K. The magnetization is non-saturating up to fields of 12 T, reaching a maximum value of 0.55 μB\mu_{\mathrm{B}}/Cr at 4 K, which is reasonable for compensated AFM ordering in the majority of the sample. An Arrott plot indicates a first-order FM transition with TCT_{\mathrm{C}} = 98 K (Figure 3i), 55 in agreement with the AC and DC susceptibility results.

Image not extracted

Figure S7. Isothermal magnetization curves with H⊥cH \perp c, showing zero-field hysteresis at 94 K and below.

It is known that the fully occupied 3×3\sqrt{3} \times\sqrt{3} Cr superlattice in Cr1/3TaS2\mathrm{Cr}_{1/3}\mathrm{TaS}_{2} exhibits local FM coupling both in- and out-of-plane, with chiral helimagnetic order developing below 140 K because of competition between FM Heisenberg exchange and the Dzyaloshinskii–Moriya (DM) interaction. 40,41 The introduction of vacancies on the 3×3\sqrt{3} \times\sqrt{3} Cr superlattice in the closely related material Cr1/3NbS2\mathrm{Cr}_{1/3}\mathrm{NbS}_{2} lowers TCT_{\mathrm{C}} markedly and suppresses the DM interaction, resulting in bulk FM behavior. 26,28 Hence, we attribute the partial FM ordering observed in Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2} to the minority 3×3\sqrt{3} \times\sqrt{3}-containing structural domains. The lower TCT_{\mathrm{C}} of 98 K observed in our samples compared to the reported TCT_{\mathrm{C}} of Cr1/3TaS2\mathrm{Cr}_{1/3}\mathrm{TaS}_{2} is consistent with a defective 3×3\sqrt{3} \times\sqrt{3} Cr superlattice in the minority FM domains of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2}, which is expected from the average stoichiometry of our samples.

To investigate the effects of Cr intercalation and superlattice ordering on the electronic structure of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2}, we first consider the symmetry of the 120∘120^{\circ} AFM and the dominant 2×22 \times2 structural superlattice relative to the host lattice of 2H2H-TaS2\mathrm{TaS}_{2}. The 2D Brillouin zone (BZ) for the 120∘120^{\circ} AFM BZ is scaled down by 1/31/\sqrt{3} and rotated by 30∘30^{\circ} relative to the 2×22 \times2 structural BZ, which is itself scaled down by 1/21/2 relative to the 1×11 \times1 host lattice BZ (Figure 4a). As a result, extensive zone folding is expected in-plane. For the three-dimensional (3D) BZ, the out-of-plane reciprocal lattice vector remains unchanged.

Figure 4. Electronic structure of Cr1/4_{1/4}TaS2_{2}. (a) Two-dimensional Brillouin zone (BZ) for 120° AFM, 2×22 \times2 superlattice, and 1×11 \times1 host lattice, and three-dimensional BZ for 120° AFM, with high-symmetry points labeled. (b) Experimental Fermi surfaces from angle-resolved photoemission spectroscopy measured with linear horizontal (LH) and linear vertical (LV) polarization. Dotted lines indicate the 1×11 \times1 host lattice BZ. (c) Energy vs. k∥k_{\parallel} dispersion along M0M_{0}–Γ0\Gamma_{0}–K0K_{0}–M0M_{0}. Overlay: density functional theory (DFT) band structure of 2H-TaS2_{2} shifted down by 0.2 eV. Purple arrows indicate replica bands from folding that cross EFE_{\mathrm{F}}. (d) DFT band structure for Cr1/4_{1/4}TaS2_{2} in the 120° AFM phase. (e) Energy vs. kzk_{z} dispersion at kx=0k_{x} = 0 from the photon energy dependence. (f) Energy vs. kxk_{x} dispersions from constant kzk_{z} cuts centered at A and Γ\Gamma. Overlays: DFT band structures along the K0K_{0}–Γ\Gamma–K0K_{0} direction with kz=π/ck_{z} = \pi/c and kz=0k_{z} = 0 for A and Γ\Gamma, respectively. All ARPES data were measured at 10 K with 80 eV, LH-polarized photons unless otherwise indicated.

Using angle-resolved photoemission spectroscopy (ARPES), we find that the experimental Fermi surfaces show clear evidence of 2×22 \times2 reconstruction (Figure 4b). With linear horizontal (LH) polarized photons (80 eV), we see replica hole pockets at M0\mathrm{M}_{0} that are folded from Γ0\Gamma_{0}. In linear vertical (LV) polarization, we also observe duplication of the hole pockets from K0\mathrm{K}_{0} at the corners of the 2×22 \times2 BZ. By fitting the main hole pocket around Γ0\Gamma_{0} from the LH data, we obtain kF=0.38k_{\mathrm{F}} = 0.38 Å−1^{-1} along Γ0\Gamma_{0}–K0K_{0} (Figure S8), which is intermediate between 2H-TaS2_{2} and Cr1/3_{1/3}TaS2_{2}.51,56

Image not extracted

Figure S8. Momentum distribution curve for E−EF=0E - E_{\mathrm{F}} = 0 eV and ky=0k_y = 0 Å−1^{-1}, fitted to multiple Lorentzian peaks.

The ARPES energy vs. momentum dispersion shows further evidence for superlattice-induced electronic reconstruction. As expected, the most prominent bands are consistent with the overlaid density functional theory (DFT) band structure for 2H-TaS2_{2} with the Fermi level (EFE_{\mathrm{F}}) shifted down by 0.2 eV (Figure 4c).57 However, clear replica bands are present throughout the BZ that do not correspond to any bands from the unfolded host lattice (indicated by purple arrows in Figure 4c and Figure S9). The DFT band structure calculated for the 120° AFM structure of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2 indicates that the magnetic and structural folding results in several bands crossing EFE_{\mathrm{F}} (Figure 4d).

Image not extracted

Figure S9. Increasing cell size and the folding of the bandstructure (yellow, shifted down by 0.2 eV) of 2H2H-TaS2_2 in the reciprocal space in comparison with the ARPES experiment. (a) 1×1×11 \times1 \times1, (b) 2×2×12 \times2 \times1, (c) 23×23×12\sqrt{3} \times2\sqrt{3} \times1 unit cells of 2H2H-TaS2_2. The calculated bandstructure of (d) 1×1×11 \times1 \times1, (e) 2×2×12 \times2 \times1, (f) 23×23×12\sqrt{3} \times2\sqrt{3} \times1 unit cells of 2H2H-TaS2_2.

We observe a marked kzk_z dispersion of bands near EFE_{\mathrm{F}}, as shown in Figure 4e, consistent with the Γ\Gamma–A dispersion from DFT (Figure 4d). Constant kzk_z cuts from the high-symmetry points qualitatively match the DFT band structures for kz=0k_z = 0 and kz=π/ck_z = \pi/c, respectively (Figure 4f and Figure S10). This constitutes additional evidence that the Cr superlattice and 120° AFM structure strongly modulate the electronic structure beyond the rigid band picture in a manner consistent with other intercalated TMDs.51,58–61 More broadly, the ARPES experiments further confirm that the 2×22 \times2 superlattice is dominant, as we do not observe evidence of electronic reconstruction associated with minority 3×3\sqrt{3} \times\sqrt{3}-containing structural domains.

Image not extracted

Figure S10. (a) Band structures of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2 with U=0 (red) and U=4 (blue) eV. (b) Band structures of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2 with kz=0k_z = 0 (red), kz=0.4k_z = 0.4 (blue), and kz=0.5k_z = 0.5 (green).

Discussion

From the magnetometry data and geometry of domains observed in 4D-STEM, we propose the following simplified scheme for Cr ordering during crystal growth and the subsequent cooling process (Figure 5a). At high temperatures, a defective 3×3\sqrt{3} \times\sqrt{3} superlattice, which has higher configurational entropy, is more stable. At intermediate temperatures, enthalpically favored 2×22 \times2 domains nucleate and grow. At lower temperatures, Cr intercalants become immobile due to insufficient thermal energy, thus freezing the superlattice domain configurations at room temperature and below. This implies that if 2×22 \times2 domains are not given enough time to grow during cooling, defective 3×3\sqrt{3} \times\sqrt{3}-containing domains will persist between them. The spatial separation of superlattices revealed by 4D-STEM suggests that despite cooling at the relatively slow rate of 20 °C/hour and being within experimental error of the perfect Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2 stoichiometry, growth of pure 2×22 \times2 domains appears to be kinetically limited in our best samples. This picture explains how 3×3\sqrt{3} \times\sqrt{3} order can be present in samples with compositions that should favor a 2×22 \times2 superlattice from purely thermodynamic considerations,32 consistent with computational predictions.62

Schematic illustration of growth and ordering of Cr intercalant domains, proposed magnetic phases, and inelastic scattering between domains.

Figure 5. In-plane superlattice domain formation and magnetic phases in Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2}. (a) Schematic illustration of growth and ordering of Cr intercalant domains at elevated temperatures. Gray dots indicate possible interstitial sites, blue dots indicate Cr, light green shaded regions indicate local 3×3\sqrt{3} \times\sqrt{3} order, and light blue shaded regions indicate 2×22 \times2 order. (b) Proposed magnetic phases in 2×22 \times2 and 3×3\sqrt{3} \times\sqrt{3} structural domains at 145 K and below, comprising antiferromagnetic (AFM), ferromagnetic (FM), paramagnetic (PM), and spin glass (SG) phases. (c) Schematic illustration of inelastic scattering of spin-up and spin-down carriers between AFM 2×22 \times2 domains and minority domains or domain walls.

Accordingly, we propose the following coexistence of magnetic phases in Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2} based on the transition temperatures for the AFM, FM, and SG phases established previously (Figure 5b). Below 145 K, the majority 2×22 \times2 domains exhibit 120∘120^\circ AFM order, while the minority 3×3\sqrt{3} \times\sqrt{3}-containing domains remain paramagnetic (PM). Below 98 K and above 40 K, the 3×3\sqrt{3} \times\sqrt{3}-containing domains exhibit FM order, and below 40 K, they enter an SG state. We note that our proposed scheme for superlattice domain formation considers only in-plane ordering. From the 4D-STEM data, the 3×3\sqrt{3} \times\sqrt{3}-containing domains also show 2×22 \times2 reflections (Figure 3e), implying that some mixing of superlattices occurs in the out-of-plane direction. It is possible that the structural proximity of superlattices with FM vs. AFM coupling both in- and out-of-plane is responsible for the observed SG behavior.

The magnetic transition temperatures correlate well with changes observed in the AHE. A nonzero AHE emerges below 145 K, coinciding with the onset of AFM ordering. We attribute the negative sign between 100 and 145 K to an extrinsic AHE from inelastic scattering, specifically from spin defects at domain walls between AFM domains and PM minority superlattice domains (Figure 5c).16,63 The AHE is positive between 40 and 100 K, which corresponds with FM ordering in the minority domains. The complex scaling between the anomalous Hall conductivity (σAHE\sigma_{\mathrm{AHE}}) and the longitudinal conductivity (σxx\sigma_{xx}) suggests that different mechanisms are responsible in different temperature regimes (Figure S11). No clear signature of AHE is observed below 40 K, reminiscent of the disappearance of some components of the AHE in the cluster glass phase of the kagome 120∘120^\circ AFM Mn3_3Sn.42

Image not extracted

Figure S11. Plot of the longitudinal conductivity (σxx\sigma_{xx}) vs. the anomalous Hall conductivity (σAHE\sigma_{\mathrm{AHE}}).

These temperature regimes are further supported by the MR behavior, which is generally consistent with disparate magnetic phases coexisting on the nanoscale. The crossover between positive and negative MR and low-field cusps at intermediate temperatures are reminiscent of dilute magnetic semiconductors and magnetically doped topological insulators with clustering of the magnetic species.64,65 We note also that Cr1/3_{1/3}NbS2_2 likewise exhibits complex field dependence of the MR and a sign change in the AHE, which have been attributed to field evolution of noncoplanar spin textures.66,67 In Cr1/4_{1/4}TaS2_2, although the minority 3×3\sqrt{3} \times\sqrt{3}-containing domains are defective, local DM interactions or domain wall effects may still lead to spin canting or chiral textures that influence the transport behavior.

To test our proposed mechanisms, we carried out an analogous set of magnetometry and transport experiments on Cr-deficient crystals with the composition Cr0.23_{0.23}TaS2_2. The Cr-deficient material clearly shows an AFM transition at 145 K, with no second transition at 98 K. It exhibits a negative θCW\theta_{\mathrm{CW}} and a small, linear MM vs. μ0H\mu_0H, indicating the absence of FM/SG domains (Figure S12). The Raman spectrum does not show a well-defined 3×3\sqrt{3} \times\sqrt{3} peak, and the 2×22 \times2 superlattice mode is slightly broadened and red-shifted, consistent with a defective superlattice (Figure S13). Critically, we observe zero detectable AHE at 200 K and below (Figure S14). The Cr-deficient material has a RRR\mathit{RRR} value of 1.6, almost an order of magnitude lower than Cr1/4_{1/4}TaS2_2, which we attribute to increased scattering off of defects in the Cr superlattice. We also observe higher carrier concentration, lower mobility, and lower MR, which are additionally consistent with lower crystal quality and the absence of FM/SG domains. These findings indicate that the combined presence of a well-ordered and fully occupied 2×22 \times2 Cr superlattice and minority 3×3\sqrt{3} \times\sqrt{3}-containing domains is required for the rich magnetotransport behavior observed in Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2.

Image not extracted

Figure S12. Magnetometry of Cr0.23_{0.23}TaS2_2. (a) Zero-field-cooled (ZFC) DC magnetic susceptibility (χDC\chi_{\mathrm{DC}}) vs. TT, measured with a 1 T magnetic field perpendicular to cc. (b) Fitting of inverse DC susceptibility data vs. TT to the Curie–Weiss law, χ−1=(T−θCW)/C\chi^{-1} = (T - \theta_{\mathrm{CW}})/C. (c) Isothermal magnetization (MM) vs. μ0H⊥c\mu_0 H \perp c.

Image not extracted

Figure S13. Raman spectra of Cr0.23TaS2\mathrm{Cr}_{0.23}\mathrm{TaS}_{2} and Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2}, with 3×3\sqrt{3} \times\sqrt{3} and 2×22 \times2 superlattice peak regions highlighted for Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2}.

Image not extracted

Figure S14. Magnetotransport properties of Cr0.23TaS2\mathrm{Cr}_{0.23}\mathrm{TaS}_{2}. (a) In-plane longitudinal resistivity (ρxx\rho_{xx}) vs. TT. (b) In-plane Hall resistivity (ρxy\rho_{xy}) vs. μ0H\mu_{0}H. (c) Charge carrier concentration (nhn_{h}) and carrier mobility (μh\mu_{h}) vs. TT, as derived from the ordinary Hall component of ρxy\rho_{xy}. (d) Anomalous Hall resistivity (ρAHE\rho_{\mathrm{AHE}}) vs. μ0H\mu_{0}H at different temperatures, obtained by subtracting the ordinary Hall component of ρxy\rho_{xy}. (e) Magnetoresistance (MR) vs. μ0H\mu_{0}H at different temperatures. (f) MR at 12 T vs. TT.

Conclusions

Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_2 is a metallic antiferromagnet with a noncollinear 120∘120^\circ AFM ground state. High-quality crystals with a well-ordered 2×22 \times2 Cr superlattice nevertheless also contain minority domains with local 3×3\sqrt{3} \times\sqrt{3} order. These samples host complex magnetotransport phenomena below the AFM TNT_{\mathrm{N}}, including temperature-dependent sign changes in AHE and MR. Interactions between the majority AFM phase and minority PM/FM/SG domains engender the observed transport responses through scattering between the disparate superlattices. Altogether, this work shows that growth conditions (in addition to composition) must be taken into account to determine superlattice identity and microstructure. Our results corroborate a growing body of literature indicating that subtle differences in crystallographic order in intercalated TMDs can be harnessed towards realizing a wide array of magnetic and electronic properties.24,25,28,31,68–70

The possibility of engineering disparate magnetic phases by controlling the geometry of superlattice domains, as well as the topology of domain walls, is an intriguing prospect and worthy of further exploration.71,72 In addition, intercalated TMDs might be promising platforms to study analogues of the three- and four-state Potts universality classes (corresponding to 2D 2×22 \times2 and 3×3\sqrt{3} \times\sqrt{3} ordering, respectively) in three dimensions.73 More generally, our work points to the importance of using sensitive and local probes to investigate the possibility of disorder or inhomogeneity in intercalation compounds with more than one stable superlattice. Further tailoring of scattering interactions via optimization of superlattice nucleation and growth may lead to the development of new materials exhibiting electrical transport responses relevant to spintronic devices.

Materials and Methods

Single crystals of Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2} were grown from Cr (powder, 99.97%, Alfa Aesar), Ta (powder, 99.98%, Alfa Aesar, and S (powder, 99.999%, Acros Organics) using I2\mathrm{I}_{2} (99.999%, Spectrum Chemicals) as a transport agent. The constituent elements in a 0.33:1:2.05 molar ratio were sealed in an evacuated fused quartz ampoule (14 mm inner diameter, 1 mm wall thickness, 25 cm long) along with 2 mg/cm3^{3} of I2\mathrm{I}_{2}. The ampoule was placed in a two-zone furnace with the hot zone maintained at 1100 °C and the cold (growth) zone maintained at 1000 °C for 200 hours, after which both zones were cooled down to room temperature over the course of 50 hours (about 20 °C/hour). Hexagonal plate-shaped crystals were obtained, with lateral dimensions of several mm and thicknesses of 1–2 mm. Single crystals of Cr0.23TaS2\mathrm{Cr}_{0.23}\mathrm{TaS}_{2} were grown in an analogous fashion using a 0.30:1:2.02 molar ratio, 2.3 mg/cm3^{3} of I2\mathrm{I}_{2}, and a 1100 °C hot zone and 950 °C cold zone.

Single-crystal X-ray diffraction data were collected on a Rigaku XtaLAB P200 with Mo Kα\alpha radiation at 295 K. Data reduction and scaling and empirical absorption correction were performed in CrysAlis Pro. Structures were solved by direct methods using SHELXT74 and refined against F2F^{2} on all data by full-matrix least squares with SHELXL75 using the ShelXle graphical user interface.76 Reconstructed scattering planes were generated from the frames in CrysAlis Pro. Energy dispersive X-ray spectroscopy data were acquired on a FEI Quanta 3D FEG scanning electron microscope with an accelerating voltage of 20 kV.

Single-crystal neutron diffraction measurements were conducted on WAND2^{2} at the High Flux Isotope Reactor (Oak Ridge National Laboratory) with an incident wavelength of 1.486 Å. A single crystal was mounted on an aluminum rod with GE Varnish in the HHLHHL scattering geometry. The data were integrated using Mantid Workbench.77 Representational analysis was carried out using SARAh,45 and structural refinement was performed using FullProf.78

Heat capacity, electrical transport, and magnetometry measurements were carried out in a Quantum Design Physical Property Measurement System Dynacool equipped with a 12 T magnet. For heat capacity measurements, single crystals were affixed to the stage using Apiezon N grease. For electrical transport measurements, cleaved single crystals with thicknesses of 30 μm\mu\mathrm{m} or less were affixed using GE Varnish and contacted using silver paint and gold wire. Measurements were conducted using Stanford Research Systems SR830 lock-in amplifiers by applying a 5 mA AC current (17.777 Hz) and measuring the transverse and longitudinal voltages in typical four-probe or Hall configurations. ρxx\rho_{xx} and ρxy\rho_{xy} data were symmetrized and antisymmetrized, respectively. ρAHE\rho_{\mathrm{AHE}} and MR data were denoised with a Savitzky–Golay filter; a notch filter was applied to MR data to remove low-frequency noise on the order of 0.001 Hz. Magnetometry measurements were performed using the Vibrating Sample Magnetometer option for DC measurements, and the AC Measurement System II option for AC measurements, with crystals affixed to quartz paddles or brass holders using GE Varnish.

Confocal Raman microscopy data were collected on a Horiba LabRAM HR Evolution with an ultra-low frequency filter using 633 nm laser excitation and powers between 1 and 8 mW.

Plan-view transmission electron microscopy (TEM) imaging of a ∼50\sim50 nm-thick Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2} flake was performed using an FEI TitanX operating at 80 keV. Selected area electron diffraction (SAED) and four-dimensional scanning transmission electron microscopy (4D-STEM) were acquired in the same sample region. Samples were prepared via a dry transfer method utilizing a poly(bisphenol A carbonate)/polydimethylsiloxane polymer stamp.17 In this process, Cr1/4TaS2\mathrm{Cr}_{1/4}\mathrm{TaS}_{2} flakes were mechanically exfoliated using Kapton tape onto SiO2\mathrm{SiO}_{2}/Si, and were then transferred onto a 200 nm silicon nitride holey TEM grid (Norcada) that had been treated with O2\mathrm{O}_{2} plasma for 5 minutes immediately prior to stacking. For the SAED experiments, a 40 μm\mu\mathrm{m} diameter aperture was used, defining a selected diameter of ∼720\sim720 nm. On the other hand, 4D-STEM was acquired with a 0.55 indicated convergence semi-angle yielding a ∼6\sim6 nm converged electron probe size. The acquired 4D-STEM data were analyzed using the py4DSTEM Python package.79 Peak detection algorithms identified the HH–TaS2\mathrm{TaS}_{2} Bragg peaks, which were used to calculate the reciprocal lattice vectors of the HH–TaS2\mathrm{TaS}_{2} structure. Based on their symmetry relations to these vectors, the 2×22 \times2 and 3×3\sqrt{3} \times\sqrt{3} Cr superlattice reciprocal vectors were determined. Virtual apertures were then constructed separately. for each superlattice by masking all regions of the diffraction patterns except for the corresponding Cr superlattice peak areas. These apertures were applied to the 4D-STEM data to extract the integrated intensities of the two distinct superlattices at each probe position.

Angle-resolved photoemission (ARPES) measurements were carried out on beamline 4.0.3 (MERLIN) of the Advanced Light Source (Lawrence Berkeley National Laboratory) equipped with a Scienta Omicron R8000 hemispherical electron analyzer. Crystals were cleaved in situ under high vacuum (base pressures of 5×10−115 \times10^{-11} Torr or less) by carefully knocking off alumina posts affixed to the top surface using silver epoxy. Photon energy-dependent measurements were conducted between 30 and 124 eV, and momentum conversion was carried out using an inner potential (V0V_0) of 8 eV. The primary datasets were collected at hν=80h\nu= 80 eV, close to Γ0\Gamma_0 as determined by the photon energy dependence. Data analysis was carried out using the PyARPES software package.80

First-principles calculations based on density functional theory (DFT) were performed using the Vienna Ab Initio Simulation Package (VASP)81,82 and the open source plane-wave code QuantumEspresso (QE).83 The projector-augmented wave (PAW) methods84 implemented in VASP was used with a kinetic energy cutoff of 400 eV. The optimized norm-conserving Vanderbilt (ONCV) pseudopotentials from the PseudoDojo project85,86 were applied for calculations using QE with a kinetic energy cutoff of 86 Ry. The lattice constants (a=6.584(2)a = 6.584(2) Å, c=12.015(2)c = 12.015(2) Å) of Cr1/4_{1/4}TaS2_2 were taken from a single-crystal X-ray diffraction measurement at 100 K. A Γ\Gamma-center 2×2×22 \times2 \times2 k-mesh was used to sample the Brillouin zone for Cr1/4_{1/4}TaS2_2, and 8×8×28 \times8 \times2 k-mesh was used for TaS2_2. The exchange-correlation interaction was described by the Perdew-Burke-Ernzerhof (PBE) functional.87 An effective on-site Coulomb interaction of 4 eV on Cr atom was employed within DFT+UU of the Dudarev scheme.88 The magnetic ordering in Cr1/4_{1/4}TaS2_2 was taken as the 120° noncollinear antiferromagnetic structure using a magnetic unit cell shown in Figure 1e. VASP was used for the calculations of band structure and magnetic properties in Cr1/4_{1/4}TaS2_2, and QE was used for the calculation of band structure in TaS2_2.

Acknowledgments

We thank Sae Hee Ryu for assistance with ARPES measurements. A portion of this research used resources at the High Flux Isotope Reactor, a DOE Office of Science User Facility operated by the Oak Ridge National Laboratory. The beam time was allocated to WAND2^{2} on proposal number IPTS-30492.1. This research used resources of the Advanced Light Source, which is a DOE Office of Science User Facility under contract no. DE-AC02-05CH11231. Work at the Molecular Foundry, LBNL, was supported by the Office of Science, Office of Basic Energy Sciences, the U.S. Department of Energy under Contract no. DE-AC02-05CH11231. Computational work in this paper used the Lux Supercomputer at UC Santa Cruz, funded by NSF MRI Grant No. AST 1828315. L.S.X. acknowledges support from the Arnold and Mabel Beckman Foundation through an Arnold O. Beckman Postdoctoral Fellowship (award no. 51532). B.H.G. was supported by the University of California Presidential Postdoctoral Fellowship Program (UC PPFP), Schmidt Science Fellows in partnership with the Rhodes Trust, and the Max Planck Society. O.G. acknowledges support from a NSF Graduate Research Fellowship Grant DGE 1752814. S.H. acknowledges support from the Blavatnik Innovation Fellowship.

Author Contributions

L.S.X. and D.K.B. conceived of the study. L.S.X. synthesized samples and carried out transport and EDS experiments. L.S.X., O.G., and S.S.F. collected and analyzed SCXRD data. M.D.F., S.S.F., and L.S.X. collected and analyzed neutron diffraction data. W.F. and K.L. carried out symmetry analysis and first-principles DFT calculations. L.S.X., M.P.E., and C.M. collected and analyzed Raman data. S.H. collected and analyzed electron diffraction data; B.H.G. and I.M.C. provided analysis and interpretation. C.M., L.S.X., and S.S.F. collected and analyzed magnetometry and heat capacity data. L.S.X., J.P.D., S.S.F., and M.P.E. collected and analyzed ARPES data. D.K.B. and Y.P. supervised the project. L.S.X. wrote the manuscript with input from all authors.

Competing Interests

The authors declare no competing interests.

Single-Crystal X-ray Diffraction

Energy-Dispersive X-ray Spectroscopy

Single-Crystal Neutron Diffraction

Table S4: Atomic coordinates, Wyckoff positions, isotropic displacement parameters, and occupancies for the nuclear structure of Cr0.226(6)TaS2\mathrm{Cr}_{0.226(6)}\mathrm{TaS}_2 from single-crystal neutron diffraction.

Atom LabelxxyyzzSiteBisoB_{\mathrm{iso}}Occupancy
Cr1011/22a1.73(7)0.848(26)
Ta2011/42b1.73(7)1
Ta30.495(1)0.989(2)1/46h1.73(7)1
S40.1670(9)0.8330(9)0.3802(5)12k1.73(7)1
S5−1/3-1/31/30.118(1)4f1.73(7)1

Table S4.

Magnetometry

To extract the maximum of the real part of χAC′\chi'_{\mathrm{AC}}, corresponding to the spin glass freezing temperature (TfT_{\mathrm{f}}) at each frequency, we fit the data to a univariate spline and take the root of the derivative. We then quantify the frequency dependence of TfT_{\mathrm{f}} by calculating the Mydosh parameter (KK), according to the formula K=ΔTfTflog⁡(Δf)K = \frac{\Delta T_{\mathrm{f}}}{T_{\mathrm{f}}\log(\Delta f)} at different frequencies (ff). We obtain K=0.011(4)K = 0.011(4), which is somewhat larger than typical values for canonical spin glasses (e.g. 0.0045 for AuMn),[1] and in line with expected values for cluster spin glasses.[2, 3, 4]

The obtained values for τ\tau and nn are consistent with those expected for a spin glass.[2] The persistence of thermoremanent magnetization above Tf=40T_f = 40 K and below TC=98T_C = 98 K suggests that the FM state also exhibits some glassy characteristics.

Angle-Resolved Photoemission Spectroscopy

Density Functional Theory Calculations

In Figure S9a–c, we show different unit cells of 2H2H-TaS2_2 from 1×1×11 \times1 \times1, 2×2×12 \times2 \times1, to 23×23×12\sqrt{3} \times2\sqrt{3} \times1. One effect of increasing the unit cell size is the folding of the band structure in the reciprocal space, as seen in Figure S9d–f. In spite of the band folding, the calculated band structure of 2H2H-TaS2_2 always contains the key features that are measured from the ARPES experiment. The position of the key features in DFT calculation differs by 0.2 eV with respect to the experiment. The comparison indicates that the main contribution to ARPES measurement is from 2H2H-TaS2_2, and that the intercalated Cr shifts the Fermi level by introducing extra electrons.

In Figure S10a, we compare the band structures of Cr1/4_{1/4}TaS2_2 with U=0U = 0 and U=4U = 4 eV. Including Hubbard interaction moves the bands upward, which brings the agreement between DFT band structures and ARPES measurements closer. It also increases the magnetic moment on Cr from 2.5 μB2.5\,\mu_{\mathrm{B}} to 3.2 μB3.2\,\mu_{\mathrm{B}}, which makes it close to the theoretical spin-only value of 3.87 μB3.87\,\mu_{\mathrm{B}}/Cr for Cr3+^{3+} (S=3/2S = 3/2). In Figure S10b, we compare the band structures of Cr1/4_{1/4}TaS2_2 with different kzk_z. Increasing kzk_z makes many bands degenerate. Overall, including Hubbard UU with a kz=0.5k_z = 0.5 gives the best agreement between DFT band structures and the main ARPES dataset collected with hν=80h\nu= 80 eV.

Magnetotransport of Cr1/4_{1/4}TaS2_2

Characterization of Cr0.23_{0.23}TaS2_2

References

  1. [1]Mulder, C. A. M., van Duynneveldt, A. J. & Mydosh, J. A. Frequency and field dependence of the ac susceptibility of the AuMn spin-glass. Phys. Rev. B 25, 515–518 (1982).
  2. [2]Mydosh, J. A. Spin Glasses: An Experimental Introduction (CRC Press, 1993).
  3. [3]Anand, V. K., Adroja, D. T. & Hillier, A. D. Ferromagnetic cluster spin-glass behavior in PrRhSn₃. Phys. Rev. B 85, 014418 (2012).
  4. [4]Bag, P., Baral, P. R. & Nath, R. Cluster spin-glass behavior and memory effect in Cr₀.₅Fe₀.₅Ga. Phys. Rev. B 98, 144436 (2018).

Paper details

vlnc:W_gqgqpxuv
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…