Emergent interlayer magnetic order via strain-induced orthorhombic distortion in the 5d Mott insulator Sr2IrO4

Abstract

We report a La2CuO4-like interlayer antiferromagnetic order in Sr2IrO4 films with large orthorhombic distortion (> 1.5%). The biaxial lattice strain in epitaxial heterostructures of Sr2IrO4/Ca3Ru2O7 lowers the crystal symmetry of Sr2IrO4 from tetragonal (C4) to orthorhombic (C2), guiding the Ir 5d Jeff = 1/2 pseudospin moment parallel to the elongated b-axis via magnetic anisotropy. From resonant X-ray scattering experiments, we observed an antiferromagnetic order in the orthorhombic Sr2IrO4 film whose interlayer stacking pattern is inverted from that of the tetragonal Sr2IrO4 crystal. This interlayer stacking is similar to that of the orthorhombic La2CuO4, implying that the asymmetric interlayer exchange interaction along a and b-directions exceeds the anisotropic interlayer pseudo-dipolar interaction. Our result suggests that strain-induced distortion can provide a delicate knob for tuning the long-range magnetic order in quasi-two-dimensional systems by evoking the competition between the interlayer exchange coupling and the pseudo-dipolar interaction.

Transition metal oxides are a featured condensed matter system for realizing emergent electronic and magnetic phases due to competing interactions and strong electron correlation. Layered oxides with the quasi-two-dimensional K2_2NiF4_4-type structure are of particular interest since they include superconducting high-TcT_c cuprates [1, 2], spin/charge/orbital ordered manganates [3], spin-orbit coupled iridates [4, 5], and so forth. Despite their diverse physical properties, the spin Hamiltonian of the system is commonly described by

Hij=Jij Si⋅Sj+Dij⋅Si×Sj+Si⋅Γij⋅Sj(1)H_{ij} = J_{ij}\,\mathbf{S}_i \cdot\mathbf{S}_j + \mathbf{D}_{ij} \cdot\mathbf{S}_i \times\mathbf{S}_j + \mathbf{S}_i \cdot\mathbf{\Gamma}_{ij} \cdot\mathbf{S}_j \tag*{(1)}

, where the first term is the Heisenberg exchange interaction, the second term is the Dzyaloshinskii-Moriya (DM) interaction, and the third term is the pseudo-dipolar interaction, respectively, between two sites ii and jj [6]. Because of the quasi-two-dimensional nature of the layered oxides, only in-plane interactions are often considered important in theoretical models [7]. This approximation is justified because the Heisenberg exchange interaction within the basal plane is a few orders of magnitude stronger than any interlayer interactions. Nevertheless, it is noteworthy that many layered-oxides exhibit long-range magnetic order with well-defined Néel temperature (TNT_N), which is not allowed in an ideal two-dimensional (2D) Heisenberg spin system with continuous symmetry according to the Mermin-Wagner theorem [8]. The interlayer-long-range magnetic order is determined by interlayer Hamiltonian defined as:

H⟨i,j⟩//a=Jouta(Si⋅Sj)+Γouta(SiaSja−SibSjb)H_{\langle i,j\rangle// a} = J_{\mathrm{out}}^{a} \left(\mathbf{S}_i \cdot\mathbf{S}_j\right) + \Gamma_{\mathrm{out}}^{a} \left(S_i^{a}S_j^{a} - S_i^{b}S_j^{b}\right)
H⟨i,j⟩//b=Joutb(Si⋅Sj)+Γoutb(SibSjb−SiaSja)(2)H_{\langle i,j\rangle// b} = J_{\mathrm{out}}^{b} \left(\mathbf{S}_i \cdot\mathbf{S}_j\right) + \Gamma_{\mathrm{out}}^{b} \left(S_i^{b}S_j^{b} - S_i^{a}S_j^{a}\right) \tag*{(2)}

where JoutaJ_{\mathrm{out}}^{a} and JoutbJ_{\mathrm{out}}^{b} are the nearest interlayer exchange interactions and Γouta\Gamma_{\mathrm{out}}^{a} and Γoutb\Gamma_{\mathrm{out}}^{b} are the anisotropic interlayer pseudo-dipolar interactions along the crystallographic aa- and bb-directions, respectively, as shown in Figure 1(a). We define jcj_c and δc\delta_c as the energies from the nearest interlayer exchange interaction and the anisotropic interlayer pseudo-dipolar interaction, respectively:

Crystal structure of layered oxides and two antiferromagnetic stacking patterns

Figure 1. (a) Crystal structure of layered oxides with the distorted K2_2NiF4_4 structure. The interlayer exchange interactions JoutaJ_{\mathrm{out}}^{a} and JoutbJ_{\mathrm{out}}^{b} share the same interaction paths with interlayer pseudo-dipolar interactions Γouta\Gamma_{\mathrm{out}}^{a} and Γoutb\Gamma_{\mathrm{out}}^{b}, respectively. (b) Schematic diagrams of two different long-range antiferromagnetic stacking patterns in K2_2NiF4_4 type oxides. AFM-1 type is observed in Sr2_2IrO4_4 and La2_2NiO4_4 whereas AFM-2 is observed in La2_2CuO4_4.

jc=Jouta(Si⋅Sj)+Joutb(Si⋅Sj)j_c = J_{\mathrm{out}}^{a} \left(\mathbf{S}_i \cdot\mathbf{S}_j\right) + J_{\mathrm{out}}^{b} \left(\mathbf{S}_i \cdot\mathbf{S}_j\right)
δc=Γouta(SiaSja−SibSjb)+Γoutb(SibSjb−SiaSja)(3)\delta_c = \Gamma_{\mathrm{out}}^{a} \left(S_i^{a}S_j^{a} - S_i^{b}S_j^{b}\right) + \Gamma_{\mathrm{out}}^{b} \left(S_i^{b}S_j^{b} - S_i^{a}S_j^{a}\right) \tag*{(3)}

Two distinct antiferromagnetic (AFM) interlayer stacking patterns are found in the K2_2NiF4_4-type oxides depending on jcj_c and δc\delta_c. For example, tetragonal La2_2NiO4_4 and Sr2_2IrO4_4 crystals show the AFM-1 type [9, 10, 11, 12] whereas orthorhombic La2_2CuO4_4 crystals exhibit the AFM-2 type [13, 14, 15, 16], as shown in Figure 1(b). La2_2CoO4_4 crystals present both types depending upon their phase transitions between tetragonal and orthorhombic structures [17].

One may conjecture that the AFM stacking order is correlated with the crystal structure since the AFM-1 (i.e., δc<0\delta_c < 0) and AFM-2 (i.e., δc>0\delta_c > 0) type patterns seem to appear in tetragonal and orthorhombic structures, respectively. One way to check is to see if the AFM-2 type order is induced when orthorhombic distortion is applied in a tetragonal system. However, recent experiments by Kim et al. [18] showed that the AFM-1 type order remained in the Sr2_2IrO4_4 crystals even under orthorhombic distortion using a piezoelectric strain device [18]. Hence, the interlayer AFM stacking order would be irrelevant to the crystal structure or the magnitude of the orthorhombic distortion (∼0.03%\sim0.03\%) was not large enough to stabilize the AFM-2 type stacking pattern in the Sr2_2IrO4_4 crystals. It is formidable to figure out which one is correct because conventional strain/stress device approaches using bulk crystals cannot exert much larger external pressure than the magnitude used in the studies of Ref. [18].

In this Letter, we report that the long-range AFM-2 stacking order emerges in the layered iridate Sr2_2IrO4_4 thin films when substantially large (>1.5%> 1.5\%) orthorhombic distortion is applied by biaxial strain. Such a large magnitude of orthorhombic distortion is realized by constructing epitaxial thin-film heterostructures of Sr2_2IrO4_4/Ca3_3Ru2_2O7_7 with excellent structural coherence and atomically sharp interfaces. We observed clear magnetic Bragg reflections from the Ir L-edge resonant X-ray scattering (RXS) experiments, indicating that the AFM-2 type stacking order is stabilized when ∣jc∣|j_c| exceeds ∣δc∣|\delta_c|. Our result confirms that the long-range AFM stacking order of the quasi-two-dimensional oxides is correlated with their crystal structures. It is noteworthy that our experimental finding provides a useful approach for enhancing the magnetic frustrations (i.e., magnetic quantum fluctuations) of various two-dimensional magnetic systems via utilizing the subtle competition between the interlayer exchange interaction and the pseudo-dipolar interaction.

We conceived Sr2_2IrO4_4/Ca3_3Ru2_2O7_7 heterostructures to study the effect of orthorhombic distortion to the AFM order because of the large anisotropic lattice mismatch between the tetragonal Sr2_2IrO4_4 and the orthorhombic Ca3_3Ru2_2O7_7, i.e., −2.22%-2.22\% and +0.45%+0.45\% along the aa- and bb-directions, respectively, as shown in Figure 2(a). The heterostructure samples were synthesized by depositing 24-nm-thick Sr2_2IrO4_4 epitaxial thin-films on Ca3_3Ru2_2O7_7 (001) single crystals with

Sr2IrO4/Ca3Ru2O7 heterostructure schematic, X-ray diffraction scan, and STEM images

Figure 2. (a) A schematic diagram of a Sr2_2IrO4_4/Ca3_3Ru2_2O7_7 heterostructure. The red and blue arrows represent compressive and tensile strain directions and magnitudes. (b) X-ray diffraction (0 0 L) scan of a Sr2_2IrO4_4/Ca3_3Ru2_2O7_7 heterostructure. The (0 0 12) and (0 0 18) peaks from the Sr2_2IrO4_4 thin film are visible. The asterisks [*] indicate the peaks from the Ca3_3Ru2_2O7_7 single crystal substrate. (c) High-resolution Z-contrast STEM images of a Sr2_2IrO4_4/Ca3_3Ru2_2O7_7 heterostructure for two different cross-sectional directions. The red triangles mark the atomically sharp interface between Sr2_2IrO4_4 and Ca3_3Ru2_2O7_7. The scale bar is 1 nm.

cleaved surfaces using pulsed laser deposition (PLD). The PLD conditions are a laser fluence of 1.2 J/cm2^2, a substrate temperature of 700°C, and an oxygen partial pressure of 10 mTorr, which are consistent with Ref. [19]. Figure 2(b) shows X-ray diffraction with well-defined (0 0 l)(0\ 0\ l) peaks and Kiessig fringes from a Sr2_2IrO4_4/Ca3_3Ru2_2O7_7 heterostructure, indicating a high-quality thin film with a thickness of ∼\sim24 nm. The structural coherence length of ∼\sim29 nm, obtained from the FWHM of the (0 0 20)(0\ 0\ 20) peak is comparable to the thickness of the Sr2_2IrO4_4 thin film (Figure S1). The H and K scans near (2 0 20)(2\ 0\ 20) and (0 2 20)(0\ 2\ 20)-reflections show that the Sr2_2IrO4_4 thin films are fully strained along both in-plane directions (Figure S1 and (Figure S1)). Large in-plane anisotropy with -2.22% compressive strain along the aa-axis and +0.45% tensile strain along the bb-axis is observed in these thin films (Table I) which correspond to the significantly large orthorhombic distortion (α≡(b−a)/(b+a)\alpha\equiv(b-a)/(b+a)) of +1.58% at low temperature (6 K). Considering Young’s modulus of ∼\sim130 GPa of Sr2_2IrO4_4 crystals [20], this compressive strain corresponds to an effective uniaxial pressure of ∼\sim2.9 GPa along the aa-axis, which is far above the accessible range of conventional strain/stress approaches [21]. This anisotropic strain is expected to lower the crystal symmetry of Sr2_2IrO4_4 from tetragonal to orthorhombic, as shown in Figure 2(a). Structural Bragg peaks of (1 2 19)(1\ 2\ 19) and (1 2 21)(1\ 2\ 21) that are relevant to the octahedral rotation along the cc-axis [22, 23] were not observed from our samples (Figure S1), implying that the octahedral rotational pattern is substantially modified in these Sr2_2IrO4_4/Ca3_3Ru2_2O7_7 heterostructures presumably due to the large orthorhombic distortion. Figure 2(c) shows high-resolution Z-contrast scanning transmission electron microscopy (STEM) data of the cross-sections of the heterostructures. Note that an atomically sharp interface between Sr2_2IrO4_4 and Ca3_3Ru2_2O7_7 is observed without any noticeable misfit dislocations or atomic inter-mixing even under such a large orthorhombic distortion.

Epitaxial Sr2_2IrO4_4 thin film on Ca3_3Ru2_2O7_7aa (Å)bb (Å)cc (Å)α\alpha (%)a^{\mathrm{a}}εaa\varepsilon_{aa} (%)εbb\varepsilon_{bb} (%)εcc\varepsilon_{cc} (%)VV (Å3^3)
6 K5.364(4)5.536(4)25.92(2)+1.58-2.21(7)+0.93(7)+0.47(8)769.9
296 K5.378(4)5.523(4)25.94(2)+1.33-2.22(9)+0.44(8)+0.61(8)770.5

Table I. Lattice constants and strain values of Sr2_2IrO4_4 (001) thin films grown epitaxially on Ca3_3Ru2_2O7_7 (001) single crystals. a^{\mathrm{a}} Values are obtained using α≡{(b−a)/(b+a)}×100(%)\alpha\equiv\{(b-a)/(b+a)\}\times100(\%).

Four-panel scans of Cr₃Ru₂O₇ substrates and Sr₂IrO₄ thin films

Figure S1. (a) HH scan of Cr3Ru2O7\mathrm{Cr}_3\mathrm{Ru}_2\mathrm{O}_7 substrate and Sr2IrO4\mathrm{Sr}_2\mathrm{IrO}_4 thin film measured around the (2 0 16) and (2 0 20) Bragg's reflections, respectively. (b) KK scan of Cr3Ru2O7\mathrm{Cr}_3\mathrm{Ru}_2\mathrm{O}_7 substrate and Sr2IrO4\mathrm{Sr}_2\mathrm{IrO}_4 thin film measured around the (0 2 16) and (and (0 2 20) Bragg's reflections, respectively. (c) The LL scan of Sr2IrO4\mathrm{Sr}_2\mathrm{IrO}_4 thin film around (0 0 20) structural Bragg’s reflection used to measure the coherence length (ξc\xi_c) along cc-direction. The correlation length was obtained to be 28.6 nm, comparable to the entire 24 nm thickness of Sr2IrO4\mathrm{Sr}_2\mathrm{IrO}_4 thin film. (d) (1 2 LL) scan of Sr2IrO4\mathrm{Sr}_2\mathrm{IrO}_4 / Ca3Ru2O7\mathrm{Ca}_3\mathrm{Ru}_2\mathrm{O}_7 thin film showing no (1 2 odd) peak of Sr2IrO4\mathrm{Sr}_2\mathrm{IrO}_4 thin films. The asterisk [⁎] indicates a peak from the Ca3Ru2O7\mathrm{Ca}_3\mathrm{Ru}_2\mathrm{O}_7 single crystal substrate.

Resonant X-ray scattering experiments reveal an unprecedented AFM-2 stacking order, which has not been observed from any Sr2_2IrO4_4 crystals or thin films. Using resonant X-ray near the Ir L3_3 edge (ℏω=11.217\hbar\omega= 11.217 keV), we observed a clear (1 0 24)(1\ 0\ 24) magnetic Bragg peak at 6 K with a magnetic coherence length of ∼\sim26 nm along the out-of-plane direction (Figure S3), comparable to the out-of-plane structural coherence length of ∼\sim29 nm (Figure S1). Figure 3(a) shows the azimuthal angle (Ψ\Psi) dependence of the (1 0 24)(1\ 0\ 24) magnetic Bragg peak (see Figure S4) in which the sample is rotated about the scattering vector with Ψ=0\Psi= 0 defined such that the crystallographic aa-axis lies in the scattering plane as shown in Figure 3(b). We used the σ\sigma-π\pi polarization channel of the incoming and outgoing X-rays because the magnetic Bragg

Normalized integrated intensities of magnetic Bragg peaks and temperature dependence

Figure 3. (a) Normalized integrated intensities of the Ir L-edge (1 0 24)(1\ 0\ 24) magnetic Bragg peaks of a Sr2_2IrO4_4/Ca3_3Ru2_2O7_7 heterostructure as a function of azimuthal angle (Ψ\Psi) with σ\sigma-π\pi polarization channel. The solid (red) line represents a theoretical calculation for the Jeff=12J_{\mathrm{eff}} = \frac{1}{2} pseudospin magnetic moment (m⃗\vec{m}) parallel to the crystallographic bb-axis, as shown in the schematic diagram. Ψ=0\Psi= 0 is defined as the crystallographic aa-axis lies in the scattering plane. The inset shows the same magnetic Bragg peak intensities at selected azimuthal angles. (b) Normalized integrated intensities of the (1 0 24)(1\ 0\ 24) magnetic Bragg peaks as a function of temperature. The solid (red) line is power law fit using equation I∝[1−TTN]2βI \propto\left[1-\frac{T}{T_N}\right]^{2\beta}, where TNT_N and β\beta are the Néel temperature (∼\sim222 K) and the critical exponent, respectively. (Inset) Normalized integrated intensity vs. the reduced temperature (1−TTN)\left(1-\frac{T}{T_N}\right) in the logarithmic scale. The estimated critical exponent β=0.22\beta= 0.22 is below 0.23 that corresponds to the 2D XY4_4 universality model [30, 31].

L scan of the (1 0 24) magnetic Bragg reflection and schematic diagram of scattering geometry

Figure S3. (a) The L scan of the (1 0 24) magnetic Bragg reflection. The out-of-plane direction coherence length (ξc\xi_c) is obtained to be around 26 nm, comparable to the structural coherence length (Figure 1S(c)). (b) Schematic diagram of scattering geometry. σ\sigma - π\pi polarization channel of the incoming and outgoing X-rays defined by the wave vectors κ\kappa and κ′\kappa', respectively. Ψ\Psi represent the azimuthal angle rotated about the scattering vector where Ψ=0\Psi= 0 is defined as the crystallographic aa-axis lies in the scattering plane.

L-scans of the (1 0 24) magnetic Bragg peaks

Figure S4. The L-scans of the (1 0 24) magnetic Bragg peaks (a) for various azimuthal angles (Ψ\Psi) at 6 K and (b) as a function of temperature at Ψ=90∘\Psi= 90^\circ.

peak intensities follow the relation I∝∣m⃗⋅(σi×σo′)∣2I \propto|\vec{m}\cdot(\sigma_i \times\sigma'_o)|^2, where σi\sigma_i and σo′\sigma'_o are the incoming and outgoing polarizations of photons and m⃗\vec{m} is the Jeff=1/2J_{\mathrm{eff}} = 1/2 pseudo-spin magnetic moment [24, 25]. We observed that the azimuthal angle dependence of the integrated peak intensity, obtained by fitting the Gaussian peak shape of LL-scans, follows the theoretical calculation for m⃗∥b⃗\vec{m} \parallel\vec{b}. This observation indicates that the magnetic moment is along the crystallographic bb-axis without any secondary magnetic domains of m⃗∥a⃗\vec{m} \parallel\vec{a}. Note that this observation of m⃗∥b⃗\vec{m} \parallel\vec{b} is consistent with the result of Ref. [18], in which the orthorhombic distortion of ∼0.03%\sim0.03\% is applied using uniaxial compressive strain along the aa-axis of a Sr2_2IrO4_4 single crystal. These two results confirm that the uniaxial anisotropy due to orthorhombic distortion is crucial in determining the direction of the magnetic moment with respect to the crystallographic axis [26].

Figure 3(b) shows that the integrated intensity of the magnetic Bragg peak (see Figure S4) decreases with increasing temperature, suggesting the long-range AFM order below TN=222T_{\mathrm{N}} = 222 K. Note that this value of TNT_{\mathrm{N}} is comparable to that of Sr2_2IrO4_4 single crystals (<230< 230 K) [27, 28, 29] despite the orthorhombic distortion. The integrated intensity follows the power-law scaling function I(t)≈∣t∣2βI(t) \approx|t|^{2\beta} with the critical exponent β=0.22\beta= 0.22, where t≡1−TTNt \equiv1 - \frac{T}{T_{\mathrm{N}}} is the reduced temperature, as shown in the inset of Figure 3(b). The critical exponent (0.22), corresponding to the 2D XYh4_{h4} universality class, seems reasonable for this quasi-2D system with weak interlayer coupling [30, 31, 32].

Full (0 1 LL) and (1 0 LL) scans over the wide range of LL from 15 to 25 reciprocal lattice units show clear (1 0 4nn) and (0 1 4nn+2) magnetic Bragg peaks with n=4n = 4, 5, and 6, as shown in Figure 4(a). Additional strong structural Bragg reflections from the Ca3_3Ru2_2O7_7 crystal are indicated by asterisks (*). Note that these magnetic Bragg peaks, i.e., (1 0 4nn) and (0 1 4nn+2) with m⃗∥b⃗\vec{m} \parallel\vec{b}, are the ones expected in the AFM-2 type stacking order, which is observed in orthorhombic systems such as La2_2CuO4_4. In tetragonal Sr2_2IrO4_4 crystals, the AFM-2 type stacking is energetically 2∣δc∣2|\delta_c| higher than the AFM-1 type stacking, i.e., (1 0 4nn+2) and (0 1 4nn) with m⃗∥b⃗\vec{m} \parallel\vec{b}.

L scans and schematic diagram of AFM phases

Figure 4. (a) Ir LL-edge X-ray (1 0 LL) and (0 1 LL) scans of a Sr2_2IrO4_4/Ca3_3Ru2_2O7_7 heterostructure at 6 K. (1 0 16), (1 0 20), (1 0 24), (0 1 18), and (0 1 22) magnetic Bragg peaks are observed. The asterisks [*] indicate the peaks from the Ca3_3Ru2_2O7_7 single crystal substrate. (b) Schematic diagram of AFM phases of Sr2_2IrO4_4 as a function of orthorhombic distortion.

Our experimentally finding not only confirms that the interlayer AFM order is correlated with crystal symmetry but also leads us to further understand that the competition between jcj_c and δc\delta_c in determining the long-range AFM order in the system, as schematically shown in Figure 4(b):

  1. The orthorhombic distortion (α\alpha) = 0, tetragonal Sr2_2IrO4_4 crystals have isotropic JoutJ_{\mathrm{out}}, i.e., Jouta=JoutbJ_{\mathrm{out}}^a = J_{\mathrm{out}}^b, resulting in jc=0j_c = 0 for a G-type AFM order. Two equivalent AFM domains with the AFM-1 type stacking order with m⃗∥a⃗\vec{m} \parallel\vec{a} and m⃗∥b⃗\vec{m} \parallel\vec{b} are stabilized with the energy of δc<0\delta_c < 0. They correspond to uudduudd and lrlrlrlr stacking order discussed in Ref. [12].

  2. 0<α<αc0 < \alpha< \alpha_c, where αc\alpha_c is a critical value, as the tetragonal structure of Sr2_2IrO4_4 becomes an orthorhombic structure, the AFM-1 type order with m⃗∥b⃗\vec{m} \parallel\vec{b} is stabilized over the other phase with m⃗∥a⃗\vec{m} \parallel\vec{a} due to the pseudospin-lattice interaction within the IrO2_2 basal planes. This transition was experimentally observed with α≈0.03%\alpha\approx0.03\% [18]. JoutJ_{\mathrm{out}} is no longer isotropic, i.e., Jouta>JoutbJ_{\mathrm{out}}^a > J_{\mathrm{out}}^b, resulting in non-zero jcj_c.

Nevertheless, the interlayer pseudo-dipolar interaction remains dominant since ∣jc∣<∣δc∣|j_c| < |\delta_c|.

  1. α>αc\alpha> \alpha_c, the interlayer exchange interaction becomes dominant over the pseudo-dipolar interaction, i.e., jc+δc<0j_c + \delta_c < 0, with ∣jc∣>∣δc∣|j_c| > |\delta_c|, making the AFM-2 type stacking order stabilized. Using the tight-binding approximation, we can estimate the value of jcj_c to be around −0.9 μ-0.9\ \mueV (α=1.6%\alpha= 1.6\%), whose magnitude is larger than the estimated value of δc=0.3 μ\delta_c = 0.3\ \mueV.

  2. α≈αc\alpha\approx\alpha_c, both AFM-1 and AFM-2 type stacking orders can coexist due to ∣jc∣≈∣δc∣|j_c| \approx|\delta_c|, meaning that the system has a large interlayer magnetic frustration and consequently enhances the magnetic quantum fluctuation. By assuming δc=0.3 μ\delta_c = 0.3\ \mueV (Ref. [12]) and linear extrapolation between our experimental values, αc\alpha_c is estimated to be around +0.7%+0.7\%. It would be a formidable task to experimentally study the interlayer magnetic frustration near the critical value. However, applying a gradual strain to obtain continuous orthorhombic distortion in freestanding nanomembranes [33] could provide an accessible approach.

Our result suggests that the competition between interlayer exchange interaction and pseudo-dipolar interaction provides an intriguing tuning parameter to stabilize the long-range magnetic stacking order in quasi-2D systems. We have observed a distinct La2CuO4\mathrm{La}_2\mathrm{CuO}_4-like AFM stacking order in Sr2IrO4\mathrm{Sr}_2\mathrm{IrO}_4 by enhancing ∣jc∣|j_c| over ∣δc∣|\delta_c| via large orthorhombic distortion. In addition to opening exciting questions on the detailed nature of the competition between interlayer interactions, these results raise the prospects of tuning the anisotropic coupling between spins into exotic quantum phases.

Acknowledgments

We acknowledge the support of National Science Foundation Grants No. DMR-1454200, DMR-2011876, and DMR-2104296 for sample synthesis and characterization. This research used resources of the Advanced Photon Source, a U.S. Department of Energy (DOE) Office of Science User Facility, operated for the DOE Office of Science by Argonne National Laboratory under Contract No. DE-AC02-06CH11357. Electron microscopy was performed at the Center for Electron Microscopy and Analysis at the Ohio State University. B.K. acknowledges financial support from the Deutsche Forschungsgemeinschaft (DFG, German Research Foundation) – Projektnummer 107745057 - TRR 80.

Emergent interlayer magnetic order via strain-induced orthorhombic distortion in the 5d5d Mott insulator Sr2IrO4\mathrm{Sr}_2\mathrm{IrO}_4

S. Shrestha; M. Krautloher; M. Zhu; J. Kim; J. Hwang; J. Kim; J.-W. Kim; B. Keimer; A. Seo

Figure S2. High-resolution Z-contrast STEM images of a Sr2IrO4/Ca3Ru2O7\mathrm{Sr}_{2}\mathrm{IrO}_{4}/\mathrm{Ca}_{3}\mathrm{Ru}_{2}\mathrm{O}_{7} heterostructure along both [1 0 0] and [1 1 0] directions.

References

  1. [1]P. M. Grant, S. S. Parkin, V. Y. Lee, E. M. Engler, M. L. Ramirez, J. E. Vazquez, G. Lim, R. D. Jacowitz, and R. L. Greene, Phys. Rev. Lett. 58, 2482 (1987).
  2. [2]J. Orenstein and A. J. Millis, Science 288, 468 (2000).
  3. [3]M. Imada, A. Fujimori, and Y. Tokura, Rev. Mod. Phys. 70, 1039 (1998).
  4. [4]B. J. Kim, H. Ohshumi, T. Komesu, S. Sakai, T. Morita, H. Takagi, and T. Arima, Science 323, 1329 (2009).
  5. [5]B. J. Kim et al., Phys. Rev. Lett. 101, 076402 (2008).
  6. [6]V. M. Katukuri, V. Yushankhai, L. Siurakshina, J. van den Brink, L. Hozoi, and I. Rousochatzakis, Phys. Rev. X 4, 021051 (2014).
  7. [7]P. A. Lee, N. Nagaosa, and X.-G. Wen, Rev. Mod. Phys. 78, 17 (2006).
  8. [8]N. D. Mermin and H. Wagner, Phys. Rev. Lett. 17, 1133 (1966).
  9. [9]J. Rodriguez-Carvajal, M. T. Fernandez-Diaz, and J. L. Martinez, J. Phys. Condens. Matter 3, 3215 (1991).
  10. [10]T. M. Brill, G. Hampel, F. Mertens, R. Schurmann, W. Assmus, and B. Luthi, Phys. Rev. B 43, 10548 (1991).
  11. [11]C. Dhital, T. Hogan, Z. Yamani, C. de la Cruz, X. Chen, S. Khadka, Z. Ren, and S. D. Wilson, Phys. Rev. B 87, 144405 (2013).
  12. [12]J. Porras et al., Phys. Rev. B 99, 085125 (2019).
  13. [13]D. Vaknin, S. K. Sinha, D. E. Moncton, D. C. Johnston, J. M. Newsam, C. R. Safinya, and H. E. King, Jr., Phys. Rev. Lett. 58, 2802 (1987).
  14. [14]T. Freltoft, J. P. Remeika, D. E. Moncton, A. S. Cooper, J. E. Fischer, D. R. Harshman, G. Shirane, S. K. Sinha, and D. Vaknin, Phys. Rev. B 36, 826 (1987).
  15. [15]M. Ree huis, C. Ulrich, K. Prokes, A. Gozar, G. Blumberg, S. Komiya, Y. Ando, P. Pattison, and B. Keimer, Phys. Rev. B 73, 144513 (2006).
  16. [16]Y. S. Lee, R. J. Birgeneau, M. A. Kastner, Y. Endoh, S. Wakimoto, K. Yamada, R. W. Erwin, S. H. Lee, and G. Shirane, Phys. Rev. B 60, 3643 (1999).
  17. [17]K. Yamada, M. Matsuda, Y. Endoh, B. Keimer, R. J. Birgeneau, S. Onodera, J. Mizusaki, T. Matsuura, and G. Shirane, Phys. Rev. B 39, 2336 (1989).
  18. [18]J.-W. Kim, S. H. Chun, Y. Choi, B. J. Kim, M. H. Upton, and P. J. Ryan, Phys. Rev. B 102, 054420 (2020).
  19. [19]S. S. A. Seo, J. Nichols, J. Hwang, T. Jerzic, J. H. Gruenewald, M. Souri, J. Thompson, J. G. Connell, and G. Cao, Appl. Phys. Lett. 109, 201901 (2016).
  20. [20]A. Jain et al., APL Mater. 1, 011002 (2013).
  21. [21]J. Park et al., Rev. Sci. Instrum. 91, 083902 (2020).
  22. [22]M. K. Crawford, M. A. Subramanian, R. L. Harlow, J. A. Fernandez-Baca, Z. R. Wang, and D. C. Johnston, Phys. Rev. B 49, 9198 (1994).
  23. [23]S. Geprags et al., Phys. Rev. B 102, 214402 (2020).
  24. [24]J. P. Hill and D. F. McMorrow, Acta Cryst. A 52, 236 (1996).
  25. [25]M. Moretti Sala, S. Boseggia, D. F. McMorrow, and G. Monaco, Phys. Rev. Lett. 112, 026403 (2014).
  26. [26]H. Zhang et al., Adv. Mater. 32, 2002451 (2020).
  27. [27]H. Wang, C. Lu, J. Chen, Y. Liu, S. L. Yuan, S. W. Cheong, S. Dong, and J. M. Liu, Nat. Commun. 10, 2280 (2019).
  28. [28]M. Ge, T. F. Qi, O. B. Korneta, D. E. De Long, P. Schlottmann, W. P. Crummett, and G. Cao, Phys. Rev. B 84, 100402(R) (2011).
  29. [29]G. Cao, J. Bolivar, S. McCall, J. E. Crow, and R. P. Guertin, Phys. Rev. B 57, R11039 (1998).
  30. [30]A. Taroni, S. T. Bramwell, and P. C. Holdsworth, J. Phys. Condens. Matter 20, 275233 (2008).
  31. [31]S. T. Bramwell and P. C. W. Holdsworth, J. Phys. Condens. Matter 5, 53 (1993).
  32. [32]J. G. Vale et al., Physical Review B 92, 020406(R) (2015).
  33. [33]S. Shrestha et al., ACS Appl. Nano Mater. 3, 6310 (2020).

Paper details

vlnc:W_gvvjcpy4
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents