Controlling nitrogen incorporation in (Eu,Ba,Ca)TiO3_3-derived perovskite-type oxynitrides through Fermi Level Engineering

Abstract

Defect states directly influence not only functional properties, but also oxynitride formation during ammonolysis. Along with structural stability and charge balance, these defects can cause non-uniform nitrogen incorporation. To address this, the recently proposed Fermi Level Engineering concept provides a powerful alternative of rationalising oxynitride synthesis. By using the electron chemical potential, i.e., the Fermi level, as a unique descriptor, this approach can predict, understand, and manipulate defect formation enthalpies and charge transition levels, subsequently allowing to incorporate defect-property correlations to the concept. This work combines theoretical modelling and experimental characterisation of barium titanium oxynitrides to explain an intrinsic, self-limiting nitridation process. Progressive nitrogen incorporation causes a Fermi level downward shift, leaving further nitrogen substitution on oxygen sites energetically unfavourable, up to 0.03 N per unit formula. We demonstrate that A-site cation substitution in Eu1−x_{1-x}Bax_xTiO3_3- and Eu1−x_{1-x}Cax_xTiO3_3-derived oxynitrides can be applied to control compensation of the additional negative charge from N3−^{3-} and keep the Fermi level high. The Eu2+/3+^{2+/3+} redox couple enables substitution of oxygen by nitrogen through pinning of the Fermi level at the europium charge transition level, at ∼\sim 2.9 eV above the VBM. This allows for higher nitrogen uptake of up to 0.65 per formula unit (taken from hot gas extraction) through a more controlled process. Further incorporation is then limited by an intra-Ti(O,N)6_6 octahedra distortion due to internal bond-angle variance. These findings demonstrate that Fermi Level Engineering provides a pathway to predict and overcome intrinsic synthetic and thermodynamic limitations in oxynitride synthesis.

Keywords

Perovskites, Oxynitrides, Fermi Level Engineering, Charge Transition Level, Defect Chemistry, Defect Modelling, XPS

Introduction

Oxynitride materials attract considerable attention given their ability to combine the structural robustness of oxides with the favourable electronic properties introduced by nitrogen. In most cases, substituting O2−^{2-} by N3−^{3-} raises the valence band maximum due to the higher-energy N 2p states, narrowing the bandgap and improving visible light absorption compared to oxide materials [1, 2]. An exception are Eu-containing titanates, that exhibit a widening of the bandgap after ammonolysis due to the involvement of the Eu 4f states [3]. Perovskite-type oxynitrides are especially promising due to versatile cation substitutions that permit tuning of the optical, electronic, and defect-related properties [4]. They are therefore interesting for solar water splitting (SWS), which requires efficient light absorption, suitable bandgaps, and favourable band edge positions for the water redox reactions [4, 5, 6]. Most bulk or powdered oxynitrides are currently synthesised by thermal ammonolysis of oxide precursors under flowing ammonia gas at high temperatures [7, 8], and the compositional choice is guided typically by crystallographic stability and charge compensation strategies derived from the final products. However, ammonolysis is heavily influenced by topotactical reaction kinetics, often resulting in non-uniform nitrogen incorporation and a high concentration of defects such as anion vacancies/deficiencies and reduced transition-metal cations such as Ti3+^{3+} [5]. This reduction and consequent charged defects affect the electronic structure, e.g., by moving the Fermi level (EFE_\mathrm{F}) and increasing charge carrier recombination, which can significantly hinder the photocatalytic activity even when the bandgap seems suitable [5].

Cation substitution has served often as a tool for charge compensation and structure stabilisation, rather than as an intentional strategy to control defect equilibria. Recently, a more targeted (co-)substitution methodology for better control of oxynitride formation was introduced: the concept of Fermi Level Engineering (FLE) [9]. The Fermi level represents the electron chemical potential and is directly related to the defect concentration in a material and its defect chemistry. FLE takes the Fermi level as a common descriptor for the different charge compensation mechanisms that occur during synthesis and material treatments. This generalisation is possible based on the interdependence of defect concentrations and charge neutrality, governed by the Fermi level position: EFE_\mathrm{F} is determined by the concentration of charged defects and their associated energy levels. In addition, defect concentrations themselves are also closely linked to the Fermi level, since their formation enthalpies vary as a function of the EFE_\mathrm{F} position within the band structure [9]. Hence, the formation enthalpies of charged point defects such as oxygen vacancies, cation vacancies, reduced transition-metal species, and nitrogen dopants all depend on the Fermi level. Therefore, the EFE_\mathrm{F} directly governs which charge compensation mechanisms are thermodynamically favoured. During ammonolysis of oxides, for instance, acceptor doping by N3−^{3-} downshifts the Fermi level, lowering the formation enthalpy of charge compensating donor defects such as oxygen vacancies and reduced cations. In turn, these defects can limit the downward movement of the EFE_{\mathrm{F}}. These shifts influence the incorporation of nitrogen in the anionic sublattice. Charge transition levels (CTLs) are the values of the electron chemical potential at which defects shift charge states. By mapping CTLs and adjusting the formation enthalpies of relevant defects through different synthesis conditions and substitution [9], Fermi Level Engineering offers a unifying, predictive concept that connects synthesis conditions, defect thermodynamics, and functional properties, which can be applied to oxynitride materials as photoabsorbers.

Within a FLE perspective, BaTiO3_3 (BTO) serves as an ideal model system. It maintains the perovskite-type structure over wide temperature ranges, benefits from extensive available literature on defect properties, and shows commercial and technological relevance [10, 11, 12]. Upon ammonolysis of pristine BaTiO3_3, the available charge compensation mechanism for N3−^{3-} acceptor doping is the formation of oxygen vacancies. Perovskite-type materials generally remain stable against transformation into lower-coordination phases (e.g., brownmillerite) up to an anion-deficiency of δ≈0.5\delta\approx0.5 [13]. Theoretically, this stability window would allow up to one nitride ion per unit formula, leading to BaTiO3−3δ_{3-3\delta}N2δ_{2\delta} (0<δ<0.50 < \delta< 0.5). In practice, however, reported N contents in pristine BaTiO3_3 are below 0.1 N per formula unit [14, 15]. While higher nitrogen contents (up to 0.4) have been observed, they require different starting materials, for instance, reduced BaTi(O3−x_{3-x}Hx_x) oxyhydride [16, 17] or Ta-substituted BaTiO3_3 [18].

In this study, direct ammonolysis of pristine BaTiO3_3 was deliberately chosen to keep a single-step synthesis that avoided intermediates, co-dopants, or additional chemical processes. This choice could minimise the environmental footprint which is typical of oxynitride synthesis routes [19], while preserving a simple baseline system. From an FLE standpoint, nitrogen incorporation in pristine BTO might drive excessive EFE_{\mathrm{F}} downward shifts, possibly beyond favourable energetic values. Introducing heterovalent cations such as Eu on the A-site bypasses such excessive shifts by introducing another charge compensation mechanism. In EuTiO3_3, which preserves the perovskite-type structure across both the oxide and resulting oxynitride configuration, the Eu2+^{2+}/Ti4+^{4+} base state allows oxidation of Eu2+^{2+} to Eu3+^{3+} to balance N3−^{3-} uptake [3, 20]. This modifies defect formation enthalpies and drives the EFE_{\mathrm{F}} stabilisation mechanism away from being strictly vacancy-based. Furthermore, to allow even further nitrogen incorporation, isovalent substitution of Ba2+^{2+} for smaller Ca2+^{2+} changes lattice strain and electronic structure, thereby influencing the density of states of the Eu 4f4f levels [21, 22].

To bridge these gaps and investigate the thermodynamic limitations preventing stoichiometric nitrogen incorporation, this work combines Density Functional Theory (DFT) modelling with experimental synthesis of BaTiO3_3 and its oxynitride to map defect energetics and Fermi level shifts. Building on this reference system, we extend our investigation to Eu1−x_{1-x}Bax_xTiO3_3 and Eu1−x_{1-x}Cax_xTiO3_3 and corresponding oxynitrides to deliberately manipulate the EFE_{\mathrm{F}} position through the Eu2+^{2+}/3+ charge transition level. By using complementary structural and spectroscopic tools such as neutron diffraction, hot gas extraction (HGE), UV Visible Spectroscopy, X-Ray Photoelectron Spectroscopy (XPS) and reductive and oxidative in situ treatments, we established a direct correlation between defect chemistry, crystal and electronic structure, and nitrogen incorporation. This correlation paves the way towards a more complete design of functional oxynitrides through simultaneous engineering of their structural and electronic properties.

Results and Discussion

Ammonolysis of pristine BaTiO3_3

Effect of defect formation energies on incorporation of nitrogen

DFT calculations were performed on rhombohedral BaTiO3_3 using the Python package pynter [23]. The defect model includes oxygen vacancies νO\nu_{\mathrm{O}} with charge states q=0,+1,+2q = 0, +1, +2, and nitrogen substitution on the oxygen sites NO_{\mathrm{O}} with charge states q=−2,−1,0,+1q = -2, -1, 0, +1. Here, qq denotes the net defect charge and should not be interpreted as the formal oxidation state of N. Defect formation energies were calculated according to Equation S1, using the chemical potentials corresponding to point X in the stability diagram (Figure S 1.1). Charged-defects finite-size corrections were applied using the scheme proposed by Kumagai et al. [24]. The relevant charge states and charge transition levels (CTLs, Equation S3) were included in the charge-neutrality condition together with electrons and holes. Electronic carrier concentrations were determined from the bulk density of states. Under the conditions considered here, the hole concentration is negligible.

Stability diagram of the ternary Ba-Ti-O system

Figure S 1.1. Stability diagram of the ternary Ba-Ti-O system, as derived from the data in Table S 1.1. The defect formation energies are discussed in terms of the chemical potentials at points A to D and point X, as reported in Table S 1.2.

The data analysis was performed with the Python package defermi [25]. We first investigate the electronic response to nitrogen incorporation by treating the total nitrogen concentration [N][\mathrm{N}] as an externally imposed quantity. For each imposed [N][\mathrm{N}], the charge-neutrality condition was solved self-consistently for the Fermi level. Increasing [N][\mathrm{N}] shifts EFE_{\mathrm{F}} toward lower energies (Figure 1a), suggesting the feedback mechanism illustrated in Figure 1b: nitrogen incorporation lowers EFE_{\mathrm{F}}, which in turn affects the thermodynamic driving force for further NO_{\mathrm{O}} formation.

Self-limiting nitrogen incorporation mechanism

Figure 1. a. Self-consistent Fermi level EFE_{\mathrm{F}} obtained from the charge-neutrality condition as a function of imposed nitrogen concentration [N][\mathrm{N}] at T=1073T = 1073 K. b. Schematic representation of the proposed self-limiting feedback mechanism: nitrogen incorporation lowers EFE_{\mathrm{F}}, thereby increasing the formation energy of NO_{\mathrm{O}} and suppressing further nitrogen incorporation. c.

This behaviour can be explained by the defect formation energies in Figure 1c, evaluated at fixed chemical potentials corresponding to the selected experimental conditions and plotted with transposed axes. The horizontal dashed lines in Figure 1a and Figure 1c indicate two representative Fermi level positions (2.95 and 2.55 eV above the valence-band maximum) and serve as guides to the eye, illustrating how the shift in EFE_{\mathrm{F}} affects the formation energies of NO_{\mathrm{O}} and νO\nu_{\mathrm{O}}. The stars represent the CTLs, while the crossing point between the formation energies of NO_{\mathrm{O}} and νO\nu_{\mathrm{O}} marks the Fermi level at which the two defects become energetically equivalent. Above this crossing, NO_{\mathrm{O}} has the lower formation energy, whereas below it, νO\nu_{\mathrm{O}} becomes energetically more favourable. As the imposed nitrogen concentration increases (Figure 1a), the Fermi level shifts toward lower energies, moving further below the crossing point. This increases the formation energy of NO_{\mathrm{O}}, making further nitrogen incorporation less favourable. Figure 1a describes the response to an imposed nitrogen concentration rather than the equilibrium nitrogen uptake at fixed nitrogen partial pressure.

Formation energies of NO\mathrm{N}_{\mathrm{O}} and VO\mathrm{V}_{\mathrm{O}} as a function of EFE_{\mathrm{F}}, plotted with transposed axes. The horizontal dashed lines in Figure 1a and 1c. mark two Fermi level positions and serve as guides to the eye for visualizing the effect of the Fermi-level shift on defect formation energies. Stars indicate the corresponding charge transition levels, and the marked crossing point indicates equal formation energies of NO\mathrm{N}_{\mathrm{O}} and VO\mathrm{V}_{\mathrm{O}}. Formation energies were determined at T=1073T = 1073 K and pO2=10−27p_{\mathrm{O}_2} = 10^{-27} atm, with the nitrogen chemical potential corresponding to an ideal-gas N2\mathrm{N}_2 reservoir with pN2=0.25p_{\mathrm{N}_2} = 0.25 atm, estimated assuming complete NH3\mathrm{NH}_3 dissociation at a total pressure of 1 atm.

The model therefore identifies an electronic negative-feedback mechanism that can contribute to self-limiting nitridation: incorporation of NO\mathrm{N}_{\mathrm{O}} lowers the Fermi level, which raises the formation energy of nitrogen on oxygen and reduces the driving force for further incorporation.

Crystal and electronic structure invariance in BaTi(O,N)3\mathrm{BaTi(O,N)_3} vs BaTiO3\mathrm{BaTiO_3}

Thermal ammonolysis of BaTiO3\mathrm{BaTiO_3} was performed. The refinements of the XRD data of the oxide and resulting oxynitride can be seen in Figure 2. As expected, the diffractogram remains essentially unchanged from that of the parent oxide, in the tetragonal P4mmP4mm space group, and the lattice parameters remain very similar. The refinements of BaTi(O,N)3\mathrm{BaTi(O,N)_3} prepared at T=973T = 973 K and further details are found in Figure S2.1 and Table S2.1.

Refined XRD patterns of BaTiO3 and BaTi(O,N)3

Figure 2. Refined XRD (λ=0.70932\lambda= 0.70932 Å) patterns of a. BaTiO3\mathrm{BaTiO_3}, and b. BaTi(O,N)3\mathrm{BaTi(O,N)_3} synthesised at T=1073T = 1073 K, using the tetragonal P4mmP4mm space group model. The red dots represent the experimental data, the black line the calculated pattern, and the blue line the difference curve. The green hash marks represent the indexed reflections of the model.

Figure S2.1. Refined XRD (λ=0.70932\lambda= 0.70932 Å) pattern of BaTi(O,N)3_3 synthesised at T=973T = 973 K, using the tetragonal P4mmP4mm space group model. The red dots represent the experimental data, the black line the calculated pattern, and the blue line the difference curve. The green hash marks represent the indexed reflections of the model.

BaTiO3_3BaTi(O,N)3_3 973 KBaTi(O,N)3_3 1073 K
Measurement typeXRDXRDXRD
Wavelength λ\lambda (Å)0.709320.709320.70932
Measurement range5∘≤2θ≤47∘5^\circ\le2\theta\le47^\circ5∘≤2θ≤47∘5^\circ\le2\theta\le47^\circ5∘≤2θ≤47∘5^\circ\le2\theta\le47^\circ
Space groupP4mmP4mmP4mmP4mmP4mmP4mm
aa (Å)3.99753(2)3.99861(2)3.99838(3)
bb (Å)= aa= aa= aa
cc (Å)4.03683(3)4.03814(4)4.03658(4)
VV (Å3^3)64.509(1)64.565(1)64.533(1)
Overall BisoB_{\mathrm{iso}} (Å2^2)0.32(3)0.24(3)0.25(3)
RpR_{\mathrm{p}} (%)9.929.8710.2
RwpR_{\mathrm{wp}} (%)15.114.715.2
RBraggR_{\mathrm{Bragg}} (%)4.004.264.07
χ2\chi^242.721.323.3

Table S2.1. Summary of measurement conditions, unit cell parameters, and goodness of fit values for BaTiO3_3 and BaTi(O,N)3_3 synthesised at T=973T = 973 K and T=1073T = 1073 K.

The oxygen and nitrogen contents, displayed in Table 1, demonstrate that the nitrogen incorporation in pristine BaTiO3\mathrm{BaTiO_3} is exceptionally low, at a maximum of N ≈0.033\approx0.033 atoms per formula unit. This is lower than values observed in literature [15, 26], and confirms the predictions made by density functional theory.

SampleComposition
BaTiO3\mathrm{BaTiO_3}BaTiO3.06±0.05\mathrm{BaTiO_{3.06 \pm0.05}}
BaTi(O,N)3\mathrm{BaTi(O,N)_3} (973 K)BaTiO2.99±0.02N0.015±0.003\mathrm{BaTiO_{2.99 \pm0.02}N_{0.015 \pm0.003}}
BaTi(O,N)3\mathrm{BaTi(O,N)_3} (1073 K)BaTiO2.967±0.001N0.033±0.001\mathrm{BaTiO_{2.967 \pm0.001}N_{0.033 \pm0.001}}

Table 1. Oxygen and nitrogen contents of BaTiO3\mathrm{BaTiO_3} and resulting oxynitrides, determined by hot gas extraction (HGE).

The optical properties of the samples were measured through UV-Visible spectroscopy (Figure S3.1). As expected, the optical bandgap of both oxynitrides remains identical to the bandgap of BaTiO3_3, with Eg=3.2E_{\mathrm{g}} = 3.2 eV for the parent oxide and both oxynitrides. This provides further evidence that the introduction of nitrogen is very low, keeping the electronic band structure essentially unchanged. A smaller feature can be observed at 2.5 eV. However, rather than representing a true band-to-band transition, this sub-bandgap absorption tail is likely induced by isolated, in-gap N 2p2p states situated just above the VB.

UV-Vis diffuse reflectance spectra for BaTiO3 and resulting oxynitrides

Figure S3.1. UV-Vis Diffuse Reflectance Spectra, plotted in K-M vs Energy, for BaTiO3_3 and resulting oxynitrides.

XPS was performed (results seen in Figure S4.1); however, given the low nitrogen content in the ammonolysed materials, the system maintains the electronic characteristics of BaTiO3_3, which has very poor electrical conductivity. Consequently, significant charging effects were observed during the XPS measurements. Because an electron flood gun was used to compensate for surface charging, the resulting shifts and manual treatment of the data compromised the determination of the EFE_{\mathrm{F}}.

X-ray photoelectron spectra of BaTiO3 and BaTi(O,N)

Figure S4.1. X-ray photoelectron spectra of a. the survey scans and b. corresponding Ti 2p2p and c. N 1s1s core levels of BaTiO3_3 and BaTi(O,N) measured at DAISY-FUN. Charge compensation with an electron flood gun was applied.

Ultimately, the low nitrogen incorporation observed in pristine BaTiO3_3 is dictated by defect thermodynamics. Our DFT calculations reveal that the substitution of oxygen by nitrogen (NO_{\mathrm{O}}) becomes energetically favourable only at high Fermi levels. Keeping the EFE_{\mathrm{F}} high is therefore a defining factor to allow higher nitrogen incorporation.

Cationic substitution improves nitrogen incorporation: Eu1−x_{1-x}Bax_xTi(O,N)3_3 and Eu1−x_{1-x}Cax_xTi(O,N)3_3 (x=0.2x = 0.2, 0.8)

Guided by the predictions from the electrochemical series for solid materials [27], we performed A-site substitution with europium to maintain the Fermi level high, closer to the CBM. We use the Eu2+/3+^{2+/3+} redox pair to ideally keep defect formation energies favourable for higher nitrogen incorporation. In addition, Ca2+^{2+} substitution was applied on the A-site to induce lattice strain, serving as a complementary pathway to promote higher nitrogen contents [3].

Accurately describing the influence of the localised Eu 4f4f states is challenging for semi-local density functional approximations [28, 29]. Similar difficulties are encountered by DFT+UU or hybrid-functional approaches [30, 31]. Therefore, within the PBE-level framework used in this work, we restrict the quantitative charge-transition-level analysis to NO_{\mathrm{O}} and vOv_{\mathrm{O}}.

Facilitation of nitrogen uptake by lower symmetry

The Powder Neutron Diffraction (PND) data refinements, shown in Figure 3, confirm that Eu0.2_{0.2}Ba0.8_{0.8}Ti(O,N)3_3 crystallises in a P4mmP4mm tetragonal structure, maintaining the symmetry of the parent oxide, as shown in Figure S5.1. It contains a minor secondary phase of titanium nitride (space group Fm3ˉmFm\bar{3}m). This is not unexpected, as it is a classic by-product of the strongly reducing ammonolysis environment, leading to local reduction of Ti [3].

Refined neutron diffraction patterns of four Eu-containing oxynitrides

Figure 3. Refined neutron diffraction (λ\lambda = 1.120148(1) Å) patterns of a. Eu0.2_{0.2}Ba0.8_{0.8}Ti(O,N)3_3, using the tetragonal P4mmP4mm space group model; and b. Eu0.8_{0.8}Ba0.2_{0.2}Ti(O,N)3_3, c. Eu0.2_{0.2}Ca0.8_{0.8}Ti(O,N)3_3, and d. Eu0.8_{0.8}Ca0.2_{0.2}Ti(O,N)3_3, using the orthorhombic PnmaPnma space group model. The red dots represent the experimental data, the black line the calculated pattern, and the blue line the difference curve. The green hash marks represent the indexed reflections of the respective P4mmP4mm and PnmaPnma models, the purple ones the vanadium can reflections, and the yellow ones the reflections of TiN. The * also represents vanadium can reflections.

Rietveld refinements of high-resolution synchrotron XRD data

Figure S5.1. Rietveld refinements of the high-resolution synchrotron XRD data of a. Eu0.2Ba0.8TiO3\mathrm{Eu}_{0.2}\mathrm{Ba}_{0.8}\mathrm{TiO}_{3} in the P4mm\mathit{P4mm} space group, and b. Eu0.8Ba0.2TiO3\mathrm{Eu}_{0.8}\mathrm{Ba}_{0.2}\mathrm{TiO}_{3} in the Pm3ˉm\mathit{Pm\bar{3}m} space group. The red dots represent the experimental data, the black line the calculated pattern, and the blue line the difference curve. The green hash marks in a. represent the indexed reflections of the P4mm\mathit{P4mm} model, and the different coloured marks in b. represent 5 different cubic models.

Eu0.8_{0.8}Ba0.2_{0.2}Ti(O,N)3_3, however, undergoes loss of translational symmetry, with superstructure reflections indicative of the orthorhombic space group PnmaPnma. The multi-cubic-phased parent oxide (Figure S5.1), Eu0.8_{0.8}Ba0.2_{0.2}TiO3_3, likely contains localised microstrain gradients and compositional inhomogeneity [32], which are likely to be driven by the presence of mixed-valence states (Eu2+^{2+}/Eu3+^{3+}). Remarkably, no indication for such inhomogeneity from reflection profiles was indicated for the oxynitride phase.

From the refinements of the Ba-containing oxides, the Eu:Ba ratios were 0.216(1):0.784(1) and 0.810(1):0.190(1). The refined O/N occupancies on the resulting oxynitrides led to Eu0.2_{0.2}Ba0.8_{0.8}TiO2.528(1)_{2.528(1)}N0.184(1)_{0.184(1)}□0.288(1)_{0.288(1)} and Eu0.8_{0.8}Ba0.2_{0.2}TiO2.8(1)_{2.8(1)}N0.1(1)_{0.1(1)}□0.0(1)_{0.0(1)}.

The PND confirms that both Ca-containing oxynitrides show an orthorhombic PnmaPnma perovskite-type structure. While the Eu-poor sample mainly maintains the structure from its parent oxide (Figure S5.2), Eu0.8_{0.8}Ca0.2_{0.2}Ti(O,N)3_3 undergoes slight structural transition. Eu0.8_{0.8}Ca0.2_{0.2}TiO3_3 (Figure S5.2) was modelled using the PnmaPnma space group, as a tetragonal symmetry alone was insufficient to refine it. However, the pattern shows lack of certain reflections predicted by the orthorhombic symmetry. This might arise due to a local-scale competition between PnmaPnma and I4/mcmI4/mcm domains, similar to structural fluctuations previously reported [33, 34]. While this Eu-rich oxynitride shows no secondary phases in PND, for Eu0.2_{0.2}Ca0.8_{0.8}Ti(O,N)3_3, there is a small impurity phase of TiN, suggesting minor decomposition during the ammonolysis, which is in accordance with previous findings [3]. Further 3D Electron Diffraction (3DED) analysis of Eu0.2_{0.2}Ca0.8_{0.8}Ti(O,N)3_3 revealed, in addition to the Ca-rich PnmaPnma majority phase previously obtained from PND and HR synchrotron XRD, a minority cubic phase with P213P2_{1}3 symmetry. Dynamical refinements of the PnmaPnma phase (R=13.80R = 13.80 %) gives an Eu:Ca ratio of 17:83, in good agreement with the bulk composition (20:80), whereas dynamical refinement of the P213P2_{1}3 phase (R=25.99R = 25.99 %) yields nearly equimolar Eu/Ca occupancies, demonstrating its compositionally distinct character. Additionally, the minority phase inclusion in the structural model accounts for a series of very weak reflections close to the detection limit in the HR synchrotron pattern of Eu0.2Ca0.8TiO3Eu_{0.2}Ca_{0.8}TiO_{3} indicating that the P213P2_{1}3 phase is likely an oxide. The crystallographic details derived from 3DED are summarized in Table S 5.10. Complementary Electron Energy-Loss Spectroscopy (EELS) measurements reveal Ti-rich nanoscale domains, consistent with the presence of TiN at the nanoscale (Figure S6.1).

Figure S5.2. Rietveld refinements of the high-resolution synchrotron XRD data of a. Eu0.2Ca0.8TiO3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{TiO}_{3}, and b. Eu0.8Ca0.2TiO3\mathrm{Eu}_{0.8}\mathrm{Ca}_{0.2}\mathrm{TiO}_{3} in the Pnma\mathit{Pnma} space group. The red dots represent the experimental data, the black line the calculated pattern, and the blue line the difference curve. The green hash marks represent the indexed reflections of the Pnma\mathit{Pnma} model.

Eu0.2Ca0.8Ti(O,N)3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{Ti(O,N)}_{3}
PhasePnma\mathit{Pnma}P213\mathit{P2}_{1}3
Measurement type3D electron diffraction (3DED), dynamical refinements
Radiation/ λ\lambda (Å)Electrons, λ=0.02508\lambda= 0.02508
InstrumentThermo Scientific Talos FEG TEM (200 kV)
Volume (Å)213.0(1)430.5(2)
Calculated density (g cm−3\mathrm{g\ cm^{-3}})4.8345.721
Unit cell contentEu0.17Ca0.83TiO3\mathrm{Eu}_{0.17}\mathrm{Ca}_{0.83}\mathrm{TiO}_{3}Eu0.44Ca0.56TiO3\mathrm{Eu}_{0.44}\mathrm{Ca}_{0.56}\mathrm{TiO}_{3}
Unique reflections22502917
Observed reflections (I>2σII > 2\sigma I)21791603
aa (Å)5.352(1)7.551(1)
bb (Å)7.523(1)=a= a
cc (Å)5.289(1)=a= a
R1R1 (obs) (%)13.8025.99
wRwR (obs) (%)16.9125.65
GOF (obs)10.536.82

Table S 5.10. Table S 5.10. 3DED crystallographic parameters of the Pnma\mathit{Pnma} and P213\mathit{P2}_{1}3 phases of Eu0.2Ca0.8Ti(O,N)3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{Ti(O,N)}_{3}.

STEM-EDS and STEM-EELS elemental maps of Eu$_{0.2}$Ca$_{0.8}$Ti(O,N)$_3$

Figure S6.1. STEM-EDS (top row) and STEM-EELS (bottom row) elemental maps of Eu0.2_{0.2}Ca0.8_{0.8}Ti(O,N)3_3, showing Eu, Ca, Ti, O, and N distributions. In the EELS maps, coloured points highlight four representative nanoscale regions identified through post-processing and classified by nitrogen content: N-rich (red), N-medium-rich (blue), N-poor (green), and N-non-existent (yellow). The N-rich point shows the highest N/Ti and lowest O/Ti ratio among the regions analysed and is co-located with a locally elevated Ti and N signal, consistent with a Ti- and N-enriched local environment resembling TiN.

From the precursor oxides high resolution XRD data (Table S5.7., Table S 5.8., and Table S 5.9.), the refined ratios of Eu:Ca led to 0.192(1):0.808(1) and 0.796(2):0.204(2). These are close to the results obtained by SEM-EDX, which show Eu:Ca ratios of 0.23(2):0.82(3) and 0.79(4):0.21(2). The refinements of the O/N ratios led to Eu0.2Ca0.8TiO2.55(2)N0.36(2)□0.09(2)Eu_{0.2}Ca_{0.8}TiO_{2.55(2)}N_{0.36(2)}\square_{0.09(2)} and Eu0.8Ca0.2TiO2.20(4)N0.59(4)□0.21(4)Eu_{0.8}Ca_{0.2}TiO_{2.20(4)}N_{0.59(4)}\square_{0.21(4)}, similar to the results obtained by hot gas extraction.

Eu0.2Ca0.8TiO3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{TiO}_{3}Eu0.8Ca0.2TiO3\mathrm{Eu}_{0.8}\mathrm{Ca}_{0.2}\mathrm{TiO}_{3}
Measurement typeHR-XRDHR-XRD
Wavelength λ\lambda (Å)0.354432(9)0.354432(9)
Measurement range0∘≤2θ≤47∘0^\circ\le2\theta\le47^\circ0∘≤2θ≤47∘0^\circ\le2\theta\le47^\circ
Space groupPnma\mathit{Pnma}Pnma\mathit{Pnma}
aa (Å)5.45182(1)5.50386(8)
bb (Å)7.68172(1)7.80520(2)
cc (Å)5.42061(1)5.50277(8)
VV (Å3^3)227.011(1)236.392(5)
Overall BisoB_{\mathrm{iso}} (Å2^2)0.383(4)0.477(6)
RpR_{\mathrm{p}} (%)7.5811.7
RwpR_{\mathrm{wp}} (%)10.116.0
RBraggR_{\mathrm{Bragg}} (%)9.945.65
χ2\chi^216.446.0

Table S5.7. Structural data from the Rietveld refinements of the high-resolution synchrotron XRD patterns of Eu0.2Ca0.8TiO3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{TiO}_{3} and Eu0.8Ca0.2TiO3\mathrm{Eu}_{0.8}\mathrm{Ca}_{0.2}\mathrm{TiO}_{3}.

Table S 5.8. Atomic positions data from the Rietveld refinements of the high-resolution synchrotron pattern of Eu0.2_{0.2}Ca0.8_{0.8}TiO3_3. The atomic positions and occupancy of Ti were kept fixed at nominal values. The occupancies of O(1) and O(2) were fixed at nominal values. O(1) occupies the 4c Wyckoff position, and O(2) occupies the 8d position.

xxyyzzocc
Eu/Ca0.5233(1)14\frac{1}{4}0.0051(1)0.192/0.808(1)
Ti0001
O(1)0.4885(3)14\frac{1}{4}0.5672(4)1.028(4)
O(2)0.2845(2)0.0318(2)0.2158(3)1.009(2)

Table S 5.8.

Table S 5.9. Atomic positions data from the Rietveld refinement of the high-resolution synchrotron pattern of Eu0.8_{0.8}Ca0.2_{0.2}TiO3_3. The atomic positions and occupancy of Ti were kept fixed at nominal values. The occupancies of O(1) and O(2) were fixed at nominal values. O(1) occupies the 4c Wyckoff position, and O(2) occupies the 8d position.

xxyyzzocc
Eu/Ca0.5033(7)14\frac{1}{4}0.0023(2)0.796/0.204(2)
Ti0001
O(1)0.518(7)14\frac{1}{4}0.539(2)1
O(2)0.207(7)0.011(2)0.251(6)1

Table S 5.9.

In all our oxynitrides, N showed preference for the axial 4c4c sites compared to the equatorial 8d8d sites, indicating partial site-selective anion ordering. While many oxynitrides favour equatorial positioning via local cis-octahedral configurations [35], there is indication in literature of the possibility of some B=TiB = \mathrm{Ti} oxynitrides favouring a local trans-configuration [36].

The oxygen and nitrogen contents were measured by hot gas extraction and can be seen in Table 2, where a trend of less to most N content is revealed: Ba0.8<Ca0.8<Ba0.2<Ca0.2Ba_{0.8} < Ca_{0.8} < Ba_{0.2} < Ca_{0.2}.

SampleComposition
Eu0.2Ba0.8Ti(O,N)3Eu_{0.2}Ba_{0.8}Ti(O,N)_{3}Eu0.2Ba0.8TiO2.63±0.02N0.14±0.01□0.23±0.02Eu_{0.2}Ba_{0.8}TiO_{2.63\pm0.02}N_{0.14\pm0.01}\square_{0.23\pm0.02}
Eu0.8Ba0.2Ti(O,N)3Eu_{0.8}Ba_{0.2}Ti(O,N)_{3}Eu0.8Ba0.2TiO2.34±0.07N0.44±0.01□0.22±0.07Eu_{0.8}Ba_{0.2}TiO_{2.34\pm0.07}N_{0.44\pm0.01}\square_{0.22\pm0.07}
Eu0.2Ca0.8Ti(O,N)3Eu_{0.2}Ca_{0.8}Ti(O,N)_{3}Eu0.2Ca0.8TiO2.78±0.04N0.21±0.01□0.01±0.04Eu_{0.2}Ca_{0.8}TiO_{2.78\pm0.04}N_{0.21\pm0.01}\square_{0.01\pm0.04}
Eu0.8Ca0.2Ti(O,N)3Eu_{0.8}Ca_{0.2}Ti(O,N)_{3}Eu0.8Ca0.2TiO2.21±0.01N0.65±0.01□0.14±0.01Eu_{0.8}Ca_{0.2}TiO_{2.21\pm0.01}N_{0.65\pm0.01}\square_{0.14\pm0.01}

Table 2. Oxygen and nitrogen contents measured by HGE of Eu1−xBaxTi(O,N)3Eu_{1-x}Ba_{x}Ti(O,N)_{3} and Eu1−xCaxTi(O,N)3Eu_{1-x}Ca_{x}Ti(O,N)_{3} (x=0.2x = 0.2, 0.8).

While pure BaTiO3BaTiO_{3} resists nitridation, with [N] < 0.1 per formula unit, the introduction of europium acts as an electronic buffer that enables higher nitrogen content across all samples. Given that europium is mainly in the 3+ state in the oxynitrides (as discussed in § 4.ii. ahead), the defect chemistry is consistent with Eu3+/N3−Eu^{3+}/N^{3-} charge compensation.

Despite the shared electronic stabilisation, the calcium series achieves higher nitrogen uptake than the barium series due to differences in lattice flexibility and local distortion. For Eu1−xBaxTi(O,N)3Eu_{1-x}Ba_{x}Ti(O,N)_{3}, at high Ba content the larger ionic radius of Ba2+Ba^{2+} (ri=1.61r_i = 1.61 Å) with Eu substitution takes the lattice framework into a rigid, non-tilted tetragonal P4mmP4mm space group, as verified by neutron diffraction. Because the P4mmP4mm structure does not distort to relieve the strain, forcing N3−N^{3-} into this tightly packed lattice leads to structural limits at N ≈ 0.14 (x=0.8x = 0.8), favouring the formation of oxygen vacancies to stabilise the system. In contrast, at high Eu content the system relaxes into an orthorhombic structure (space group PnmaPnma) allowing to relieve lattice strain by using the a+b−b−a^{+}b^{-}b^{-} tilting pattern. However, the size mismatch between Ba2+Ba^{2+} and Eu3+Eu^{3+} induces a larger distortion of the Ti(O,N)6Ti(O,N)_{6} octahedra by ca. 38% compared to Eu0.8Ca0.2Ti(O,N)3Eu_{0.8}Ca_{0.2}Ti(O,N)_{3} (Table S5.4.), limiting the N content to about 0.44.

Eu0.8Ba0.2Ti(O,N)3\mathrm{Eu}_{0.8}\mathrm{Ba}_{0.2}\mathrm{Ti}(\mathrm{O},\mathrm{N})_{3}Eu0.8Ca0.2Ti(O,N)3\mathrm{Eu}_{0.8}\mathrm{Ca}_{0.2}\mathrm{Ti}(\mathrm{O},\mathrm{N})_{3}Eu0.2Ca0.8Ti(O,N)3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{Ti}(\mathrm{O},\mathrm{N})_{3}
∠(B−X(1)−B)\angle(B-X(1)-B) (°)158.76(1)168.70(1)158.23(1)
∠(B−X(2)−B)\angle(B-X(2)-B) (°)169.7(9)158.8(2)158.82(1)
d(B−X(1))d(B-X(1)) (Å)1.995(3)1.9491(3)1.9515(3)
d(B−X(2))d(B-X(2)) (Å)1.92(1)1.996(4)1.949(1)
Δd\Delta d (%)3.762.350.13

Table S5.4. Bond angles and lengths in all three Pnma\mathit{Pnma} oxynitrides; X(1) is located on the Wyckoff site 4c4c and X(2) on 8d8d, respectively.

The calcium series makes use of the structural flexibility given by the lower symmetry, orthorhombic Pnma space group. The smaller radius of Ca2+\mathrm{Ca}^{2+} (ri=1.34r_i = 1.34 Å) allows for TiO6\mathrm{TiO}_6 octahedral tilting, and this counteracts the strain introduced by the N3−\mathrm{N}^{3-} ions. Consequently, the measured nitrogen content of Eu0.2Ca0.8Ti(O,N)3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{Ti(O,N)}_3 (N ≈\approx 0.21) closely matches the Eu concentration measured in SEM-EDX and refined by HR-XRD, indicating a stoichiometric incorporation of N, without the need for significant oxygen vacancy formation. While the Eu-rich sample would ideally lead to an approximate N content of 0.8, the measured nitrogen content of Eu0.8Ca0.2Ti(O,N)3\mathrm{Eu}_{0.8}\mathrm{Ca}_{0.2}\mathrm{Ti(O,N)}_3 is N = 0.65, slightly higher than what was previously observed [3]. Ultimately, the europium’s charge transition level allows for more controlled nitrogen incorporation and higher N contents. However, the perovskite-type lattice reaches a nitrogen incorporation limit, arising from increasing lattice strain, anion-site instability, and the lower thermodynamic stability against reductive decomposition at high nitrogen concentrations.

As the europium content is increased from 0.2 to 0.8, the UV-Vis absorption edges (Figure S7.1) shift slightly towards lower energies, with the extrapolated absorption maximum around 1.3 eV from the first absorption edge. However, low reflectance from the dark powders distorts the curves, which leads to large absorption tails caused likely by in-gap states, such as the Eu 4f4f states near the valence band. Therefore, it is likely that the extrapolations of the UV-Vis spectra are measuring transitions starting from these occupied states up to the CB, rather than revealing the true fundamental bandgap from the VB.

UV-Vis diffuse reflectance spectra plotted in K-M versus energy

Figure S7.1. UV-Vis Diffuse Reflectance Spectra, plotted in K-M vs Energy, for Eu1−x_{1-x}Bax_xTi(O,N)3_3 and Eu1−x_{1-x}Cax_xTi(O,N)3_3, (x=0.2x = 0.2, 0.8).

Importance of the charge transition level on higher nitrogen incorporation

To investigate the electronic structure and chemical states of the samples, synchrotron-based XPS was conducted. An analysis of the Eu 4d4d core-level spectra before and after ammonolysis reveals the co-existence of both Eu2+\mathrm{Eu}^{2+} and Eu3+\mathrm{Eu}^{3+} valence states in the initial oxides (Figure 4). To enable the direct comparison between different Eu concentrations, the oxynitride spectra were scaled so that the intensity around 124 eV to 126 eV and 146 eV to 150 eV aligned with the oxide.

Synchrotron-based X-ray photoelectron spectra of the Eu 4d core levels for perovskite-type oxides and their corresponding ammonolysed oxynitride counterparts

Figure 4. Synchrotron-based X-ray photoelectron spectra of the Eu 4d4d core levels for the perovskite-type oxides and their corresponding ammonolysed oxynitride counterparts, with a. and c. Eu1−x_{1-x}Bax_xTi(O,N)3_3, and b. and d. Eu1−x_{1-x}Cax_xTi(O,N)3_3. The spin-orbit split multiplets for Eu3+^{3+} (4d5/24d_{5/2} and 4d3/24d_{3/2}) are indicated, alongside the characteristic low-binding-energy shoulder (~134 eV) and broad multi-peak feature (127–132 eV), associated with the screened final states of the Eu2+^{2+} valence fraction. The oxynitride spectra were scaled so that the intensity around 146 eV to 150 eV aligned with the oxide. Measured at SoLiAS@OPUS at BESSY II with an excitation energy of hν=786h\nu= 786 eV (Ekin=∼650E_{\mathrm{kin}} = \sim650 eV).

The spin-orbit split multiplets of Eu3+\mathrm{Eu}^{3+} (Eu 4d5/24d_{5/2} and 4d3/24d_{3/2}) are clearly distinguished at approximately 136 eV and 142 eV, respectively. The spectroscopic identification of Eu2+\mathrm{Eu}^{2+} is more subtle; its 4d3/24d_{3/2} component appears as a distinct shoulder on the lower binding energy side of the Eu3+\mathrm{Eu}^{3+} 4d5/24d_{5/2} peak (around 134 eV). However, the corresponding Eu2+\mathrm{Eu}^{2+} Eu 4d5/24d_{5/2} primary peak is split up into a broad feature spanning from 127 eV to 132 eV. This distinct configuration aligns with previous studies, which state that the intensity of this feature scales with the Eu2+\mathrm{Eu}^{2+} concentration and is fundamentally driven by complex final state effects [37, 38]. Benefiting from the high resolution of the synchrotron source, a characteristic fine structure within this region was successfully resolved, as previously seen in literature [38, 39]. For further analysis, this complex structure is explicitly assigned to the Eu2+\mathrm{Eu}^{2+} electronic states.

Elemental ON analysis shows a clear trend in nitrogen incorporation: Eu0.8_{0.8}Ca0.2_{0.2} > Eu0.8_{0.8}Ba0.2_{0.2} > Eu0.2_{0.2}Ca0.8_{0.8} > Eu0.2_{0.2}Ba0.8_{0.8}, while no major contribution of oxygen vacancies is measured. The Ti 2p2p synchrotron XPS data shows a related trend of titanium atoms in a mixed oxynitride coordination environment (see Figure S8.1 for the N 1s1s spectra, Figure S 8.2 for the Ti 2p2p spectra). Due to the low nitrogen incorporation in the Eu0.2_{0.2}Ba0.8_{0.8}Ti(O,N)3_3 sample, and it’s low conductivity leading to significant surface charging, the Eu0.2_{0.2}Ba0.8_{0.8}TiO3_3 and Eu0.2_{0.2}Ba0.8_{0.8}Ti(O,N)3_3 samples were excluded during further discussion.

Synchrotron-based X-ray photoelectron spectra of the N 1s core level for the perovskite oxynitrides

Figure S8.1. Synchrotron-based X-ray photoelectron spectra of the N 1s core level for the perovskite oxynitrides. Measured at SoLiAS@OPUS at BESSY II with an excitation energy of hν=1046h\nu= 1046 eV (Ekin∼650E_{\mathrm{kin}} \sim650 eV).

Synchrotron-based X-ray photoelectron spectra and NEXAFS spectra

Figure S 8.2. Synchrotron-based X-ray photoelectron spectra of the Ti 2p3/22p_{3/2} core level of the a.-c. oxide and d.-f. oxynitride samples, fitted using Gaussian–Lorentzian line shapes. The intensity of each oxide and oxynitride with the same composition is shown in the same scale. In order to compare the binding energy shift a vertical line was drawn from the oxide to the oxynitride (in purple). Measured at SoLiAS@OPUS at BESSY II with an excitation energy of hν=1108h\nu= 1108 eV (Ekin∼650E_{\mathrm{kin}} \sim650 eV). g.-i. Near-Edge X-ray Absorption Fine Structure (NEXAFS) spectra recorded at the Ti L2,3L_{2,3}-edge for the Ca- and Ba-containing samples before and after ammonolysis. NEXAFS was recorded in Auger electron yield (AEY) mode. The NEXAFS data was normalised according to the edge jump.

A comparison between the oxide and oxynitride spectra confirms that the Eu2+^{2+} to Eu3+^{3+} oxidation reaction is the primary charge compensation mechanism during ammonolysis [20]. Upon ammonolysis, Eu2+^{2+} nearly completely converts into Eu3+^{3+} for Eu0.8_{0.8}Ca0.2_{0.2}TiO3_3. In contrast, Eu0.8_{0.8}Ba0.2_{0.2}TiO3_3 shows an incomplete transition, retaining a significant amount of residual Eu2+^{2+}, as indicated by the persistently prominent feature around 127 eV to 132 eV and the lower N content. For the Eu-poor Eu0.2_{0.2}Ca0.8_{0.8}TiO3_3 sample, while nearly all available Eu2+^{2+} ions are successfully oxidised to Eu3+^{3+}, the lower europium concentration intrinsically limits the total capacity for nitrogen uptake.

Binding energy shifts were monitored by relating the shift of the Fermi level relative to the VBM, and comparing them to the shift of the O 1s, and Ti 2p core levels to track electronic variations using a methodology adapted from Chaoudhary et al. [40], where the onsets of the valence band spectra are directly read off from the measured valence band spectra, and the shifts of the core levels are indirectly compared by subtracting one fixed value for each core level, as shown in the graph (see Figure 5). This is done to evaluate whether the core level binding energy shift can be related to the Fermi level shift. To be able to do this, we need to ensure that all materials are sufficiently conductive (to mitigate charging effects) and that the valence band maximum does not change shape. The subtracted value was chosen by subtracting the VBM position from the O 1s or Ti 2p peak position of Eu0.2Ca0.8TiO3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{TiO}_{3} and extrapolating this to all other compounds to achieve a common scale. The Ti 2p spectra can be found in Figure S 8.2, while the O 1s and VB spectra are compiled in Figure S8.3. The measured shifts can be seen in Table S8.1.

Fermi level shifts determined from valence band maximum and core levels

Figure 5. Fermi level shifts, determined from the valence band maximum (VBM) positions and indirectly from representative core levels (O 1s, Ti 2p), tracking the electronic variations upon ammonolysis, with errors of ± 0.1 eV. All determined core level values were subtracted by the values given in the legend. The lines connecting the oxide and oxynitride values are for visual guidance only. Measured at SoLiAS@OPUS at BESSY II, the detail spectra can be found in Figure S8.2 and Figure S8.3.

Synchrotron-based X-ray photoelectron spectra of the valence band and O 1s detail spectra

Figure S8.3. Synchrotron-based X-ray photoelectron spectra of the valence band (a.-c.) and O 1s (d.-f.) detail spectra for the perovskite-type oxides and their corresponding ammonolysed oxynitride counterparts. Measured at SoLiAS@OPUS at BESSY II with an excitation energy of hνh\nu = 650 eV (EkinE_{\mathrm{kin}} = ~650 eV), for the VB, and hνh\nu = 1180 eV (EkinE_{\mathrm{kin}} = ~650 eV), for O 1s. The spectra were normalised from minimum to maximum to account for intensity differences between the oxide and oxynitride samples.

Binding energy in eVEu0.2Ca0.8TiO3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{TiO}_{3}Eu0.2Ca0.8Ti(O,N)3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{Ti(O,N)}_{3}Eu0.8Ba0.2TiO3\mathrm{Eu}_{0.8}\mathrm{Ba}_{0.2}\mathrm{TiO}_{3}Eu0.8Ba0.2Ti(O,N)3\mathrm{Eu}_{0.8}\mathrm{Ba}_{0.2}\mathrm{Ti(O,N)}_{3}Eu0.8Ca0.2TiO3\mathrm{Eu}_{0.8}\mathrm{Ca}_{0.2}\mathrm{TiO}_{3}Eu0.8Ca0.2Ti(O,N)3\mathrm{Eu}_{0.8}\mathrm{Ca}_{0.2}\mathrm{Ti(O,N)}_{3}
O 1s1s530.38530.07 (-0.31)530.19530.18 (-0.01)530.23530.02 (-0.21)
Ti 2p2p458.87458.59 (-0.28)458.74458.68 (-0.06)458.74458.35 (-0.39)
Ca 2p2p347.35347.09 (-0.26)347.40347.15 (-0.25)
VBM3.052.75 (-0.30)2.902.90 (0)2.952.70 (-0.25)

Table S8.1. Peak positions for the perovskite-type oxide and corresponding ammonolysed oxynitride counterparts, extracted from the synchrotron-based X-ray photoelectron spectra, for O 1s1s, Ti 2p2p, Ca 2p2p or Ba 3d3d, and the valence band maximum. In brackets, the change in binding energy from oxide to oxynitride is shown.

The Eu 4d level was excluded from this tracking due to its active participation in charge compensation, while N 1s, Ca 2p, and Ba 3d were omitted because they are not universally present across all samples. The survey scans of all samples, as well as the Ca 2p, Ba 3d, and C 1s spectra can be found in Figure S 8.4 and Figure S8.5, and display similar shifts. Upon ammonolysis, a distinct downshift of the Fermi level to 2.75 eV (± 0.1 eV) above the VBM is observed for the Ca-containing samples, which is followed by the core levels. In contrast, the Fermi level of the Ba-containing system remains rigid within an experimental uncertainty of ± 0.1 eV. The incomplete Eu2+/Eu3+\mathrm{Eu}^{2+}/\mathrm{Eu}^{3+} transition in the Ba-containing oxynitride suggests that the Fermi level remains electronically pinned at the Eu2+/Eu3+\mathrm{Eu}^{2+}/\mathrm{Eu}^{3+} CTL, while the Ca-containing samples can complete the charge transition and unpin the Fermi level again. This locates the CTL of Eu2+/Eu3+\mathrm{Eu}^{2+}/\mathrm{Eu}^{3+} at around 2.9 eV (± 0.1 eV) above the VBM.

Synchrotron-based X-ray photoelectron survey spectra for the perovskite oxides and their corresponding ammonolysed oxynitride counterparts

Figure S 8.4. Synchrotron-based X-ray photoelectron survey spectra for the perovskite oxides and their corresponding ammonolysed oxynitride counterparts. Measured at SoLiAS@OPUS at BESSY II with an excitation energy of hν=1200h\nu= 1200 eV. The plots were shifted along the y-axis for easier comparison.

Synchrotron-based X-ray photoelectron spectra of the Ca 2p, Ba 3d and C 1s detail spectra

Figure S8.5. Synchrotron-based X-ray photoelectron spectra of the Ca 2p2p (a. and c.), Ba 3d3d (b.) and C 1s1s (d.-f.) detail spectra for the perovskite-type oxides and their corresponding ammonolysed oxynitride counterparts. Measured at SoLiAS@OPUS at BESSY II with an excitation energy of hν=997h\nu= 997 eV (Ekin∼650E_{\mathrm{kin}} \mathrel{\sim} 650 eV) for Ca 2p2p, hν=1430h\nu= 1430 eV (Ekin∼650E_{\mathrm{kin}} \mathrel{\sim} 650 eV) for Ba 3d3d and hν=935h\nu= 935 eV (Ekin∼650E_{\mathrm{kin}} \mathrel{\sim} 650 eV) for C 1s1s. The spectra were normalised from minimum to maximum to account for intensity differences between the oxide and oxynitride samples.

A significant discrepancy was detected in the Ti 2p binding energy position, specifically for the Eu0.8Ca0.2Ti(O,N)3\mathrm{Eu}_{0.8}\mathrm{Ca}_{0.2}\mathrm{Ti(O,N)}_{3} sample. While all other elemental core levels moved in parallel, the anomalous downshift of the Ti 2p doublet by an additional 0.2 eV implies a distinct modification of the local coordination environment around the central titanium cation, which has been repeatedly observed in literature upon ammonolysis or substitution [2, 3, 20, 41]. Further analysis of this shift was performed by fitting the Ti 2p spectra, as well as complementing the data with Near-Edge X-ray Absorption Fine Structure (NEXAFS) spectroscopy at the Ti L-edge (see Figure S 8.2 and the additional discussion in S8.1).

To probe the dynamic behaviour of the electronic states and assess whether the Fermi level remains rigidly pinned or responds to external chemical potentials, a series of in situ oxidising and reducing thermal treatments was performed on the Eu0.2Ca0.8Ti(O,N)3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{Ti(O,N)}_{3} oxynitride. The sample was heated to T=573T = 573 K under alternating atmospheres of molecular oxygen (5×10−45 \times10^{-4} mbar O2\mathrm{O}_{2}) or in ultra-high vacuum (UHV, 5×10−95 \times10^{-9} mbar), and the Eu 4d4d and valence band spectra can be found in Figure 6.

X-ray photoelectron spectra of the Eu 4d core levels and corresponding valence band

Figure 6. X-ray photoelectron spectra of a. the Eu 4d4d core levels and b. corresponding valence band for Eu0.2Ca0.8Ti(O,N)3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{Ti(O,N)}_{3} during cyclic redox testing after annealing in vacuum (1×10−81 \times10^{-8} mbar during heating) or in oxygen partial pressure (backfilling the vacuum chamber with 5×10−45 \times10^{-4} mbar O2\mathrm{O}_{2}) at T=573T = 573 K and cooling down to room temperature, measured at DAISY-FUN with Al Kα_{\alpha} radiation. The spectra were normalised minimum to maximum.

Consistent with previous observations, the as-synthesized oxynitride surface is oxidised, with almost complete conversion of Eu2+\mathrm{Eu}^{2+} to Eu3+\mathrm{Eu}^{3+}. Subsequent in situ annealing under reducing UHV conditions triggers a reduction of the surface, marked by a small intensity increase in both the Eu2+\mathrm{Eu}^{2+} 4d4d final-state multiplet features (127–132 eV) and the characteristic Eu2+\mathrm{Eu}^{2+}-derived states located near the top of the valence band (≈ 2 eV below the Fermi level). Cyclic exposure to alternating oxidising and reducing atmospheres demonstrates that this low-temperature redox behaviour is fully reversible. No Fermi level shift is visible, suggesting either that, after the ammonolysis, the Fermi level is still pinned at the CTL of Eu2+\mathrm{Eu}^{2+}/Eu3+\mathrm{Eu}^{3+} (around 2.9 eV ± 0.1 eV), or that the magnitude of these shifts fell within the baseline experimental uncertainty of the measurements.

The interaction of water with photocatalytic surfaces governs the water-splitting mechanism. Within this interaction, the direction of surface charge transfer, i.e. whether water acts as a local reducing or oxidizing agent, depends strongly on the material’s electronic structure. To probe whether the Eu2+/3+\mathrm{Eu}^{2+/3+} CTL remains electrochemically active under conditions relevant to water splitting, we exposed the calcium-containing oxynitride surfaces to 1 mbar water vapour at room temperature within a Near-Ambient Pressure XPS (NAP-XPS) system (see Figure S 8.6 and Figure S 8.7). We observe that the introduction of water vapour induces a surface oxidation, driving the conversion of Eu2+\mathrm{Eu}^{2+} to Eu3+\mathrm{Eu}^{3+}, as indicated by the attenuation of the Eu2+\mathrm{Eu}^{2+} features in both the Eu 4d4d core levels and the valence band. This behaviour contrasts with observations from Hermans et al. on BiVO4_{4}, where room-temperature water exposure raised the Fermi level and reduced surface metal ions (V5+^{5+} to V4+^{4+} and Bi3+^{3+} to Bi0^{0}) via reductive water dissociation [42]. This contrasting surface response reflects the different electronic structure of the two materials. In BiVO4_{4}, the Fermi level position makes the surface susceptible to reduction by dissociative water adsorption, whereas in the oxynitride, the Fermi level, pinned at the Eu2+/3+\mathrm{Eu}^{2+/3+} charge transition level, seems to favour Eu2+\mathrm{Eu}^{2+} oxidation instead. This observation indicates that similar to influencing nitrogen incorporation in the bulk, the Eu2+/3+\mathrm{Eu^{2+/3+}} charge transition level at the surface also seems to govern surface charge exchange within a water vapour environment.

X-ray photoelectron spectra of the Eu 4d, O 1s and valence band levels

Figure S 8.6. X-ray photoelectron spectra of a.+ d. the Eu 4d4d core levels, b.+ e. O 1s1s core levels and c.+ f. valence band spectra for the oxynitride Eu1−xCaxTi(O,N)3\mathrm{Eu}_{1-x}\mathrm{Ca}_{x}\mathrm{Ti}(\mathrm{O},\mathrm{N})_{3} systems. The surfaces were exposed to 1 mbar water vapour at room temperature utilising Near-Ambient pressure XPS (NAP-XPS), measured at TUM with Al Kα\alpha radiation.

X-ray photoelectron spectra of the Ti 2p, Ca 2p and C 1s core levels

Figure S 8.7. X-ray photoelectron spectra of a.+ d. the Ti 2p2p core levels, b.+ e. Ca 2p2p core levels and c.+ f. C 1s1s core level for the oxynitride Eu1−xCaxTi(O,N)3\mathrm{Eu}_{1-x}\mathrm{Ca}_{x}\mathrm{Ti}(\mathrm{O},\mathrm{N})_{3} systems. The surfaces were exposed to 1 mbar water vapour at room temperature utilising Near-Ambient pressure XPS (NAP-XPS), measured at TUM with Al Kα\alpha radiation.

Fermi Level Engineering as a tool for oxynitride design

Combining synchrotron XRD, neutron diffraction, 3D electron diffraction, and synchrotron-based XPS reveals that nitrogen incorporation in perovskite-type oxides is regulated by an interplay of the Fermi level position and crystal symmetry. DFT calculations on pristine BaTiO3\mathrm{BaTiO_3} show that the incorporation of nitrogen is only energetically favourable at high EFE_{\mathrm{F}}. Introducing europium adds an active redox centre through the Eu2+/3+\mathrm{Eu^{2+/3+}} charge transition level, which lies high in the bandgap [27] and pins the Fermi level to accommodate higher nitrogen incorporation. Nevertheless, the rigid, high-symmetry tetragonal structure of Eu0.2Ba0.8Ti(O,N)3\mathrm{Eu_{0.2}Ba_{0.8}Ti(O,N)_3} results in a lower saturation limit, stopping the reaction before the Eu2+\mathrm{Eu^{2+}} reservoir can be fully utilised. The structural rigidity dictated by the large ionic radius of Ba2+\mathrm{Ba^{2+}} (ri=1.61r_{\mathrm{i}} = 1.61 Å) [43] prevents lattice adaptation to volume changes during oxidation of Eu2+\mathrm{Eu^{2+}} to Eu3+\mathrm{Eu^{3+}} (ri=1.46r_{\mathrm{i}} = 1.46 Å to 1.281.28 Å) [44] and N3−\mathrm{N^{3-}} incorporation (ri=1.47r_{\mathrm{i}} = 1.47 Å) [45]. Even though Eu0.8Ba0.2Ti(O,N)3\mathrm{Eu_{0.8}Ba_{0.2}Ti(O,N)_3} relaxes into an orthorhombic symmetry, the size mismatch between Ba2+\mathrm{Ba^{2+}} and Eu3+\mathrm{Eu^{3+}} induces massive Ti(O,N)6\mathrm{Ti(O,N)_6} octahedra internal distortion, which limits the nitrogen content at roughly N=0.44\mathrm{N} = 0.44 per unit formula.

The orthorhombic Ca-containing samples operate within a more flexible and compliant framework due to the smaller ionic radius of Ca2+\mathrm{Ca^{2+}} (ri=1.34r_{\mathrm{i}} = 1.34 Å) [43], which aligns with the ionic radius of the newly formed Eu3+\mathrm{Eu^{3+}}. This decreases atomic strain and enables the Ti(O,N)6\mathrm{Ti(O,N)_6} octahedra to tilt and rotate to accommodate the larger N3−\mathrm{N^{3-}} anions. In Eu0.2Ca0.8TiO3\mathrm{Eu_{0.2}Ca_{0.8}TiO_3}, the pre-existing distorted orthorhombic oxide minimises the substitution energy barrier upon ammonolysis, enabling stoichiometric nitrogen incorporation (N=0.2\mathrm{N} = 0.2). For Eu0.8Ca0.2TiO3\mathrm{Eu_{0.8}Ca_{0.2}TiO_3}, ammonolysis drives a transition to an orthorhombic oxynitride that restructures the metal-anion orbital overlap and the electronic density of states. The flexible octahedral tilting allows the system to unpin the EFE_{\mathrm{F}} from the charge transition level, leading to high nitrogen incorporation and a complete Eu2+\mathrm{Eu^{2+}} to Eu3+\mathrm{Eu^{3+}} oxidation without phase segregation.

Our study deliberately initially focuses on pristine BaTiO3\mathrm{BaTiO_3}-based systems to explore a direct, potentially less environmentally hazardous ammonolysis route. However, the unified concept of Fermi Level Engineering provides a broader viewpoint from which other successful synthetic pathways can be understood. In oxynitride intermediate precursors (BaTiO3−xHx\mathrm{BaTiO_{3-x}H_x}) [16], the reducing synthesis conditions raise the EFE_{\mathrm{F}} until titanium reveals mixed Ti4+/Ti3+\mathrm{Ti^{4+}/Ti^{3+}} valence [27], pinning the EFE_{\mathrm{F}} at this charge transition level to aid controlled nitrogen substitution. Similarly, partial Ta5+\mathrm{Ta^{5+}} substitution on the BB-site in BTO [18] shifts the EFE_{\mathrm{F}} toward the CBM prior to nitridation, potentially driving the Fermi level towards a range of more favourable formation energies of nitrogen on oxygen substitution. Viewing distinct experimental approaches through an FLE perspective highlights its potential as a transferable, predictive design tool for effective nitrogen incorporation in perovskites, complementing the classical crystal-chemical guidelines.

Conclusion

A self-limiting nitridation process in pristine BaTiO3\mathrm{BaTiO_3} is revealed, driven by electronic limitations, aligning closely with the concept of Fermi Level Engineering in oxide (electro)ceramics. Increasing nitrogen incorporation shifts the EFE_{\mathrm{F}} downward, taking it well below the crossing point of acceptor and donor defect formation energies, and making further nitrogen incorporation energetically unfavourable. Consequently, our findings reveal that higher incorporation of nitrogen can be successfully achieved by keeping the EFE_{\mathrm{F}} at high levels.

We demonstrated that AA-site cationic co-substitution with Eu and Ca successfully alters the governing defect chemistry. The Eu2+/3+\mathrm{Eu^{2+/3+}} redox couple acts as an electronic buffer that pins the Fermi level at its charge transition level, which lies closer to the CBM. This stabilisation effectively evades the self-limiting process, enabling a more controlled introduction of nitrogen and significantly higher nitrogen concentrations. Therefore, cationic co-substitution shifts the limiting constraints of nitridation from energetic to structural ones, which depend on the symmetry of the crystal structure.

In Eu1−xBaxTi(O,N)3\mathrm{Eu}_{1-x}\mathrm{Ba}_{x}\mathrm{Ti(O,N)}_{3}, the crystal structure is either rigid, as the tetragonal P4mmP4mm symmetry at high Ba content cannot easily accommodate strain, or the size mismatch between Ba2+\mathrm{Ba}^{2+} and Eu3+\mathrm{Eu}^{3+} induces octahedral distortion in the Ti(O,N)6\mathrm{Ti(O,N)}_{6} polyhedra. As a result, the introduction of the larger N3−\mathrm{N}^{3-} ion is structurally constrained, limiting the nitrogen content to N≈0.14\mathrm{N} \approx0.14 (x=0.8x = 0.8) and N≈0.44\mathrm{N} \approx0.44 (x=0.2x = 0.2), instead of the expected stoichiometric values. Contrarily, Eu1−xCaxTi(O,N)3\mathrm{Eu}_{1-x}\mathrm{Ca}_{x}\mathrm{Ti(O,N)}_{3} benefits from a more flexible, orthorhombic structure. The structural tolerance allows for higher lattice distortions minimising that of the Ti(O,N)6\mathrm{Ti(O,N)}_{6} octahedra to accommodate the larger N3−\mathrm{N}^{3-} anions, leading to higher nitrogen contents of N≈0.21\mathrm{N} \approx0.21 (x=0.8x = 0.8) and N≈0.65\mathrm{N} \approx0.65 (x=0.2x = 0.2), and showing the possibility to reach near-stoichiometric oxynitride phases.

Ultimately, the combination of structural and electronic structure characterisation established a clear correlation between nitrogen incorporation, Fermi level positioning, and crystal symmetry. This work’s insights provide a predictive framework for future improvements in designing functional oxynitrides via coupled electronic and structural engineering.

Acknowledgements

We kindly acknowledge the financial support provided by the German Research Foundation (DFG) via the CRC 1548 – FLAIR (Projektnummer: 463184206). The authors deeply appreciate the granted beam time by the Institut Laue-Langevin (ILL), Grenoble, France; and the European Synchrotron Radiation Facility (ESRF), Grenoble, France, and the financial support received during the experiments. Our sincere thanks to Dr. Thomas Hansen (ILL), and Dr. Catherine Dejoie (ESRF) for their kind support during the sample preparation and the neutron diffraction and high-resolution XRD experiments. We are very grateful to the Helmholtz-Zentrum Berlin für Materialien und Energie (HZB, BESSY II) for the allocation of synchrotron radiation beamtime and the technical support of Dr. Ronny Golnak and Dr. Jie Xiao at SoLiAS@OPUS. JPH and PZ acknowledge financial support from the Federal Ministry of Research, Technology and Space (BMFTR), Germany in the framework of ErUM-Pro 05K25RD3. The authors gratefully acknowledge the computing time provided to them at the NHR Center NHR4CES at TU Darmstadt (project number p0023194). This is funded by the Federal Ministry of Research, Technology, and Space, and the state governments participating on the basis of the resolutions of the GWK for national high-performance computing at universities (www.nhr-verein.de/unsere-partner). We would like to thank Dr. Jochen Rohrer, Dr. Lorenzo Villa, and Dr. Sabrina Sicolo (TU Darmstadt) for helpful discussions and advice. Our deep thanks to Dr. Harol Moreno Fernández (Technical University of Darmstadt) for the technical support, assistance with NAP-XPS measurements, and valuable discussions. The authors thank LNNano - Laboratório Nacional de Nanotecnologia for access to the TEM equipment (project no. 20254354; Characterization of Challenging Structures by Total Scattering and Pair Distribution Function (PDF)). We acknowledge the support of João Batista Souza Junior (LNNano, Brazilian Center for Research in Energy and Materials, CNPEM) for the assistance with the TEM measurements and data analysis. We thank Vishnu Mogili for support with the 3DED measurements. NAP-XPS measurements were funded by the Deutsche Forschungsgemeinschaft (DFG, German Research Foundation) under Germany’s Excellence Strategy – EXC 2089/2 – 390776260. VS acknowledges financial support from the German Federal Ministry of Research, Technology and Space (BMFTR, Germany), project SINATRA:CO2UPLED/033RC034.

Supporting Information

Experimental

Commercial BaTiO3\mathrm{BaTiO_3} (Alfa Aesar, 99%) was annealed at T=1423T = 1423 K for 12 h. For the oxynitride synthesis, the annealed BaTiO3\mathrm{BaTiO_3} was then introduced in a tube furnace to undergo thermal ammonolysis at ambient pressure under flowing ammonia (Westfalen, ≥99.98\ge99.98%) at T=973T = 973 K and T=1073T = 1073 K for 4 h using a gas flow rate of 100 mL ⋅\cdot min−1^{-1}.

The parent oxides, with general formula Eu1−xBaxTiO3\mathrm{Eu_{1-x}Ba_xTiO_3} and Eu1−xCaxTiO3\mathrm{Eu_{1-x}Ca_xTiO_3} (x=0.2x = 0.2, 0.8), were synthesised via a soft chemistry route and subsequent annealing in forming gas. Stoichiometric amounts of europium(III) oxide (Alfa Aesar, 99.9%), titanium(IV)bis(ammonium dilactato)dihydroxide (Sigma Aldrich, 50 wt.% solution in water), barium acetate (Sigma Aldrich, ≥99\ge99%) and calcium acetate monohydrate (Thermo Scientific, 99%) were used to produce the samples. Citric acid (ROTH, ≥99.5\ge99.5%) and ethylene glycol (Merck, ≥99.5\ge99.5%) were used as complexing and gelling agent, respectively. More detailed information regarding synthesis can be found in Xiao et al. [1, 2]. After calcination at T=723T = 723 K for 6 h, the white powders were treated in flowing forming gas (AirLiquide, 95 vol.% Ar, 5 vol.% H2_2; >99.999> 99.999%) at a flow rate of 300 mL ⋅\cdot min−1^{-1}, at T=1473T = 1473 K for 12 h. The oxynitrides were synthesised via thermal ammonolysis of the black parent oxides, using a tube furnace under flowing ammonia (Westfalen, ≥99.98\ge99.98%) at ambient pressure and T=1073T = 1073 K for 10 h using a gas flow rate of 100 mL ⋅\cdot min−1^{-1}.

A STOE STADI MP diffractometer was used to perform the powder X-ray diffraction (XRD) at room temperature in transmission geometry. The instrument utilises a Ge (111) monochromator and Mo-Kα1\alpha_1 radiation.

Neutron diffraction (ND) experiments were performed using the D20 high-resolution powder diffractometer [3, 4] of the Institut Laue-Langevin (ILL) in Grenoble, France, utilising an incident wavelength of 1.120148(1) Å at a take-off angle of 90°, determined by Rietveld refinements of the Na2Ca3Al2F14\mathrm{Na_2Ca_3Al_2F_{14}} (NAC) standard sample. The wavelength was chosen to balance neutron flux at the sample and the wavelength-dependent neutron absorption behaviour of Eu [5]. The samples [6] were measured in 5 mm diameter vanadium cans at room temperature.

High-resolution XRD data [7] were collected at the high-flux high-resolution powder X-ray diffractometer using the ID22 beamline of the European Synchrotron Radiation Facility (ESRF) in Grenoble, France, with a wavelength of 0.354432(9) Å [8].

Most of the XRD and ND patterns obtained were refined by the Rietveld method [9, 10], using the Fullprof.2k software (version 7.40) [11], taking into account XRD refinements done in previous work [12]. For the refinements, pseudo-Voigt profile functions were used with the Caglioti formula for the full width at half maximum (FWHM) determination. One specific oxide sample’s synchrotron XRD data refinements (Eu0.8Ba0.2TiO3\mathrm{Eu_{0.8}Ba_{0.2}TiO_3}) were performed using the Rietveld method with the TOPAS6.0 program [13, 14] over the full measured 2θ2\theta range. Instrumental parameters were determined from a reference standard measurement (Si/LaB6\mathrm{Si/LaB_6}) and incorporated into the refinements. The microstructural parameters (crystallite size and strain broadening) were refined to account for the observed peak shapes. Isotropic atomic displacement parameters were constrained where appropriate to minimise parameter correlations and improve refinement stability.

Oxygen and nitrogen contents of all samples were determined via hot gas extraction (HGE) using an Eltra Verder ELEMENTRAC ONH-p2 analyser operated in the ON mode. About 5 mg of each sample was weighed into a nickel capsule and introduced into a nickel basket, used as flux. The capsule was dropped into a graphite crucible containing 50 mg of graphite, promoting complete fusion. The impulse furnace power was 5500 W during the outgassing phase. High-purity helium (99.996 %) was used as carrier gas. Before every measurement, the furnace atmosphere was thoroughly purged with helium to eliminate residual gases and moisture. Calibration was done using certified reference metal samples with well-defined oxygen and nitrogen contents, as follows. Eltra GmbH: Steel 921G, 91100-1003, 0.0036 ± 0.0002 %O, 0.0228 ± 0.0009 %N; Steel 1121R, 91100-1002, 0.0034 %O, 0.0069 %N; Steel 1221S, 91100-1005, 0.0031 ± 0.0003 %O, 0.0537 ± 0.0008 %N; Steel 1022P, 91100-1010, 0.0033 ± 0.0003 %O, 0.155 ± 0.002 %N; Copper 322F, 91000-1003, 0.0251 ± 0.0003 %O; Sigma-Aldrich: ZrO2_2, 99%, 25.97 %O; Thermo Scientific: Si3_3N4_4, 99.9%, 39.94 %N. Each sample was measured at least three times to ensure reproducibility.

Ultra-high vacuum (UHV) X-ray photoelectron spectroscopy (XPS) measurements were performed inside the DAISY-FUN (Darmstadt Integrated Systems for FUNdamental research) cluster tool, which has a measurement base pressure of approximately 1×10−91 \times10^{-9} mbar. The measurements used a monochromated Al Kα_\alpha X-ray source (XR 50M by SPECS, with hν=h\nu= 1486.74 eV, operating at 12.5 kV), coupled with a Focus 500 monochromator and a PHOIBOS 150 analyser by SPECS. Survey spectra were measured with 20 eV pass energy (step size 0.5 eV) and detail spectra with 10 eV (step size 0.05 eV). The spot size was around 2 mm × 2 mm. The spectrometer’s binding energy was calibrated using a sputter-cleaned silver film. Inside the cluster tool, it was possible to heat the samples without air contact. For heating of the samples in O2_2 partial pressure and ultra-high vacuum, a laser heating system from PREVAC (laser wavelength 976 nm) was used, where the samples were heated from the backside, and a thermocouple contact was fixed at the top of the sample. The laser power was controlled with a PID controller, and liquid nitrogen cooling was used to achieve a stable heating rate (1 K/s). The chosen temperature was then held for 10 minutes, and afterward, the sample cooled down to room temperature.

The near-ambient pressure (NAP)-XPS measurements were performed at the Technical University of Munich. The XPS measurements were performed using a lab-based near-ambient pressure X-ray photoelectron spectroscopy setup (NAP-XPS, Specs Surface Nano Analysis GmbH) in a chamber with a base pressure below 5×10−95 \times10^{-9} mbar. A monochromatic Al Kα_\alpha X-ray source (50 W, 120 μm spot size) provided the excitation. The analyser was calibrated using sputter-cleaned copper, silver, and gold foils, positioning the Au 4f7/24f_{7/2}, Ag 3d5/23d_{5/2}, and Cu 2p3/22p_{3/2} core-level peaks at 84.0 eV, 368.3 eV, and 932.6 eV, respectively. All spectra were acquired in fixed analyser transmission (FAT) mode with a 0.05 eV step size, 300 ms dwell time, and 30 eV pass energy, achieving a resolution of 0.5 eV. High-resolution spectra for each core level were collected over a minimum of five scans in cyclic mode, each peak scan interleaved with sequential scans of the others. This approach minimised the effect of temporal X-ray power fluctuations on our quantitative analysis. For near-ambient measurements, water vapour was dosed via a mass flow controller (MFC) at a maximum flow rate of 10 ml/min, with chamber pressure held at 1 mbar and regulated by the MFC. All measurements were performed at room temperature.

Synchrotron based XPS and NEXAFS measurements were performed at SoLiAS@OPUS (UE51_PGM-1) at the BESSY II electron storage ring, operated by Helmholtz-Zentrum Berlin für Materialien und Energie. The measurements took place at the SoLiAS endstation, which has a base pressure of approximately 1.5×10−101.5 \times10^{-10} mbar [15]. The system is equipped with a PHOIBOS 150 analyser by SPECS, featuring a 1D DLD detector. The spectrometer's binding energy was calibrated using a sputter-cleaned gold film. Survey spectra were measured with 20 eV pass energy (step size 0.5 eV) and detail spectra with 10 eV (step size 0.05 eV). The spot size was around 100 μm × 150 μm. The incident photon energy was systematically adjusted for all core levels to maintain a consistent kinetic energy of approximately 650 eV for the emitted photoelectrons. This energy was chosen, since it ensures a steady inelastic mean free path (IMFP) throughout all measurements, providing a uniform, surface-sensitive probing depth. Additionally, selecting a kinetic energy of 650 eV effectively reduces spectral overlap with Auger lines and prevents contributions from higher-order harmonics generated by the beamline monochromator. The IMFP for this kinetic energy, calculated for BaTiO3_3, with the Tanuma-Powell-Penn formula (TPP-2M) [16], is ~1.4 nm, providing an information depth (d95%d_{95\%}) of ~4.2 nm, which is expected to be similar for the other compounds. The oxides samples exhibited sufficient intrinsic conductivity to prevent detectable charging effects. In contrast, surface charging was observed during the measurement of the semiconducting oxynitride samples. Therefore, the incident photon flux was intentionally decreased by closing the apertures of the beamline to remove charging artefacts. Furthermore, all core levels exhibited uniform binding energy shifts (see Table S8.1) despite being measured at different photon energies resulting in different incident photon fluxes indicating a successful removal of surface charging. Despite these optimization efforts, there is still a small residual uncertainty in the absolute binding energies of the oxynitrides. XAS spectra were recorded in Auger electron yield (AEY) mode at kinetic energies of 240 eV for the Ti L2,3_{2,3}-edge.

All XPS data were analysed using CasaXPS version 2.3.25. The spectra were fitted with a combination of Gaussian-Lorentzian curve (GL(30)), and Shirley background was applied [17].

The SEM-EDX mapping for Eu, Ca, and Ti was performed on a Tescan Mira 3 SEM and an METEK EDAX detector, using an accelerating voltage of 15 kV and beam intensity of 15.

Continuous-rotation three-dimensional electron diffraction (3DED) [18, 19] data were collected on a Thermo Scientific Talos Transmission Electron Microscope (TEM) equipped with a field emission gun (FEG) and operated at an accelerating voltage of 200 kV (wavelength λ=0.025082\lambda= 0.025082 Å). Powder samples of Eu0.2_{0.2}Ca0.8_{0.8}Ti(O,N)3_3 were gently crushed in an agate mortar and dispersed in ethanol p.a., and a droplet of the resulting suspension was deposited onto a lacey carbon-coated copper grid. Diffraction patterns were recorded during continuous rotation using a Thermo Scientific Ceta 16M CMOS camera (4096 × 4096 pixels, used here with 2×2 binning, giving an effective frame size of 2048 × 2048 pixels and a pixel size of 0.028 mm) at a spot size of 6, with data acquisition controlled using the EPU-D (Thermo Scientific) software. Frames were acquired over a total tilt range of 120° (from -60° to +60°) at a tilt speed of 2°/s, with a tilt increment of 1° per frame and an exposure time of 0.5 s per frame, at a camera length of 656.4 mm.

Data reduction was performed with PETS2 [20] (calibration constant 0.001701 Å−1^{-1}/pixel), with reflections integrated to a resolution of 0.71 Å (d=1.4d = 1.4 Å−1^{-1}) using kinematical and dynamical approximations. The structure was solved by direct/dual-space methods using SHELXT [21] and SIR2014 [22], as implemented in Jana2020 [23], and refined using the dynamical refinement procedure in Jana2020.

EDS analyses were carried out using an Oxford SDD X-Max 80 mm2^2 windowless detector, and the results were verified by EELS measurements performed with a Gatan GIF Tridiem 863 on a JEOL JEM-2100F.

Ultra-violet–visible diffuse reflectance spectroscopy (UV–Vis DRS) data were recorded at room temperature over a wavelength range of 240–2000 nm (5.2–0.6 eV) using a J&M TIDAS UV–Vis–NIR spectrophotometer equipped with a reflection measuring head. A BaSO4_4 standard was used as a reference. Further details regarding the method used for the estimation of the optical bandgap can be found in § 12.

Computational details

Density functional theory (DFT) calculations were performed using the Vienna Ab Initio Simulation Package (VASP) [24, 25, 26]. The projector-augmented wave (PAW) scheme [27, 28] described the electron-ion interaction. For the valence electron configuration, Ba was considered with 5s25p65d0.016s1.995s^{2}5p^{6}5d^{0.01}6s^{1.99}, Ti with 3s23p63d34s13s^{2}3p^{6}3d^{3}4s^{1}, O with 2s22p42s^{2}2p^{4}.

Calculations with hybrid functionals were performed to obtain an accurate reference band gap for the 0 K-stable trigonal rhombohedral phase of BaTiO3_3 (R3m, space group No. 160). The band structure was calculated using the Heyd-Scuseria-Ernzerhof (HSE06) functional [29, 30], with a mixing of 16% and a screening parameter of 0.2 Å−1^{-1}, employing a 5-atom unit cell. The wave functions were expanded into plane waves up to an energy cutoff of 750 eV. The Brillouin zone was sampled using a Γ-centered 6×6×66 \times6 \times6 kk mesh. The atomic positions were relaxed until the Hellmann-Feynman forces acting on each atom were below 0.05 eV/Å.

For the defect calculations, the electron exchange and correlation effects were treated within the generalised gradient approximation (GGA) using the Perdew-Burke-Ernzerhof (PBE) [31] functional, using a 3×3×33 \times3 \times3 supercell containing 135 atoms. The same plane-wave cutoff and relaxation criterion were used as for the HSE06 reference calculations; however, the Brillouin zone was sampled using a Γ-centered 2×2×22 \times2 \times2 kk mesh for the supercell.

The lattice parameters and energy gaps calculated using both functionals are reported in Table S 1.

aa (Å)α\alpha (°)EgE_g (eV)
PBE4.075389.7482.29
HSE064.044089.7023.55
Exp. [34]4.0036089.839–

Table S 1. Values of lattice constant aa (Å), angle α\alpha (°), and band gap EgE_g of rhombohedral BaTiO3_3 (R3m, space group No. 160), computed with the PBE [27] and HSE06 [32, 33] exchange-correlation functionals and confronted with experimental data from Kwei et al. [34]. A measured band gap for this phase was not established from the references examined.

The defect thermodynamics applied in this work can be found down below, in § 10.

Density Functional Theory (DFT)

Defect Thermodynamics

The formation energy ΔEDf\Delta E_D^f of a defect DD with charge qq can be written as [35]:

ΔEDf=ED−EP+q(EVBM+μe)+Ecorr−∑iΔniμi(1)\Delta E_D^f = E_D - E_P + q(E_{\mathrm{VBM}} + \mu_e) + E_{\mathrm{corr}} - \sum_i \Delta n_i\mu_i \tag*{(1)}

where EDE_D is the total energy of the system with defect DD and charge qq, and EPE_P is the energy of the pristine reference cell. The third term describes the dependence of the formation energy on the electron chemical potential μe\mu_e, while the position of the valence band maximum (VBM) EVBME_{\mathrm{VBM}} is taken as its reference. EcorrE_{\mathrm{corr}} describes the applied energy corrections. The spurious electrostatic interactions between periodic images of charged defects, which arise due to the finite size of the supercell, are corrected using the scheme proposed by Kumagai et al. [32]. It is well known that semi-local functionals, such as PBE, severely underestimate the band gap and can, in some cases, introduce uncertainties in calculated defect energetics [35]. To account for this, the band gap is corrected by rigidly shifting the valence band maximum (VBM) and the conduction band minimum (CBM) as obtained from PBE calculations to the respective values obtained by HSE06 [29, 30] calculations. The correction energy is then given by:

ΔEbg=neΔECBM+nhΔEVBM,(2)\Delta E_{bg} = n_e \Delta E_{\mathrm{CBM}} + n_h \Delta E_{\mathrm{VBM}}, \tag*{(2)}

where nen_e and nhn_h are the number of electrons introduced in the conduction band and the number of holes introduced in the valence band, respectively. ΔECBM\Delta E_{\mathrm{CBM}} and ΔEVBM\Delta E_{\mathrm{VBM}} are the shifts in the CBM and VBM between HSE06 and PBE. Here, donor defects follow the energy correction of the CBM, while acceptor defects follow the correction of the VBM. Since the VBM is shifted downward, EVBME_{\mathrm{VBM}} is also shifted by:

EVBM=EVBMPBE−ΔEVBM.(3)E_{\mathrm{VBM}} = E_{\mathrm{VBM}}^{\mathrm{PBE}} - \Delta E_{\mathrm{VBM}}. \tag*{(3)}

Finally, the last term accounts for the dependence of the formation energy on the chemical potentials of the constituent elements. Here, Δni\Delta n_i is the difference between the number of atoms of species ii in the defective and bulk systems. The chemical potential μi\mu_i of element ii can be rewritten as:

μi=μiref+Δμi,(4)\mu_i = \mu_i^{\mathrm{ref}} + \Delta\mu_i, \tag*{(4)}

where μiref\mu_i^{\mathrm{ref}} is the chemical potential of the element ii in its stable elemental phase.

The Density Functional Theory data used to generate the phase stability diagram for rhombohedral BaTiO3_3 were obtained from the Materials Project (MP) database (PYMATGEN implementation, version 2025.5.2) [33, 36, 37], which uses consistent computational parameters with respect to our defect calculations. It is well known that semi-local DFT (e.g., LDA or GGA) exhibits an overbinding error in the O2_2 and N2_2 molecule [38, 39, 40]. To account for this effect, all entries used to construct the phase diagram were processed using the Materials Project compatibility corrections as implemented in PYMATGEN (class MaterialsProjectCompatibility). These corrections do not address the O2_2 molecule directly. Instead, they apply a correction to oxygen-containing compounds (with distinct values for oxide, peroxides, and superoxides, depending on the oxygen bonding environment) [41].

A charge transition level (CTL), ε\varepsilon, is the electron chemical potential at which the formation energy of a given defect in two different charge states (q1q_1 and q2q_2) becomes equal. It is given by:

ε=−ΔEDF(q1,μe=0)−ΔEDF(q2,μe=0)q1−q2,(5)\varepsilon= -\frac{\Delta E_D^F(q_1,\mu_e = 0) - \Delta E_D^F(q_2,\mu_e = 0)}{q_1 - q_2}, \tag*{(5)}

where ΔEDF(q1,μe=0)\Delta E_D^F(q_1,\mu_e = 0) and ΔEDF(q2,μe=0)\Delta E_D^F(q_2,\mu_e = 0) are the defect formation energies at charge states q1q_1 and q2q_2, respectively, when the electron chemical potential μe\mu_e is at the VBM.

At thermodynamic equilibrium, the concentration of a defect DD in charge state qq is given by:

[Dq]=Nsitesexp⁡(−ΔEq,Df(μe)kBT),(6)[D_q] = N_{\mathrm{sites}} \exp\left(-\frac{\Delta E_{q,D}^{\mathrm{f}}(\mu_e)}{k_B T}\right), \tag*{(6)}

where qq represents the defect charge, NsitesN_{\mathrm{sites}} the concentration of the corresponding lattice sites, TT the absolute temperature, and kBk_B the Boltzmann constant.

It is important to stress that the electron chemical potential μe\mu_e is not a free parameter. It is rather determined by the charge neutrality condition:

ne+nA=nh+nD,(7)n_e + n_A = n_h + n_D, \tag*{(7)}

in which nen_e and nhn_h are the electron and hole carrier concentrations, respectively, while nDn_D and nAn_A are the donor and acceptor concentrations, respectively.

Considering all defect species DD in their different charge states qq, (7) can be reformulated as:

∑q,Dq⋅[Dq]−ne+nh=0.(8)\sum_{q,D} q \cdot[D_q] - n_e + n_h = 0. \tag*{(8)}

Intrinsic carrier concentrations are computed by integrating the number of unoccupied states up to the VBM (EVBME_{\mathrm{VBM}}) for holes,

nh=∫−∞EVBMD(ε)[1−f(ε)]dε,(9)n_h = \int_{-\infty}^{E_{\mathrm{VBM}}} D(\varepsilon)[1-f(\varepsilon)]\mathrm{d}\varepsilon, \tag*{(9)}

and the number of occupied states from the conduction band minimum (CBM) (ECBME_{\mathrm{CBM}}) for electrons,

ne=∫ECBM+∞D(ε)f(ε)dε,(10)n_e = \int_{E_{\mathrm{CBM}}}^{+\infty} D(\varepsilon)f(\varepsilon)\mathrm{d}\varepsilon, \tag*{(10)}

where f(ε,μe)=[exp⁡((ε−μe)/kBT)]−1f(\varepsilon,\mu_e) = [\exp((\varepsilon-\mu_e)/k_B T)]^{-1} is the Fermi-Dirac distribution.

In this study, the integrals in Equation S9 and S10 were computed as Riemann sums over the energies in the calculated density of states, following the method delineated by PYMATGEN [36, 37]. Subsequently, the equilibrium electron chemical potential μe\mu_e was determined self-consistently by solving the charge neutrality condition for μe\mu_e at a given temperature.

Oxygen and nitrogen chemical potentials

Defect formation energies depend on the chemical potential of the reservoir. For oxygen, μO\mu_{\mathrm{O}} varies with its partial pressure pO2p_{\mathrm{O}_2} and can be expressed via the ideal gas law as:

μO(T,pO2)=μO(T,p0)+12kBTln⁡(pO2p0).(11)\mu_{\mathrm{O}}(T,p_{\mathrm{O}_2}) = \mu_{\mathrm{O}}(T,p^0) + \frac{1}{2}k_B T \ln\left(\frac{p_{\mathrm{O}_2}}{p^0}\right). \tag*{(11)}

Here, kBk_B is the Boltzmann constant, TT the temperature, μO\mu_{\mathrm{O}} the oxygen chemical potential, and p0p^0 the reference pressure.

The computed energy of the O2_2 molecule at 0 K μO(0 K,p0)=−4.95\mu_{\mathrm{O}}(0\ \mathrm{K},p^0) = -4.95 eV serves as the reference. The temperature dependence μO(T,p0)\mu_{\mathrm{O}}(T,p^0) was calculated following Reuter and Scheffler's methodology [42], using the thermochemical tables in [43]. This procedure enables a mapping between the experimentally controlled variables, such as temperature and oxygen partial pressures, and the oxygen chemical potential used in our defect-thermodynamic model. For nitrogen, the 0 K reference was taken from the legacy Materials Project MaterialsProjectCompatibility scheme, where the μN(0 K,p0)=−7.95 eV\mu_{\mathrm{N}}(0\ \mathrm{K},p^{0})=-7.95\ \mathrm{eV} reference is fitted to experimental formation energies of various nitrides. Although nitrogen is experimentally introduced by annealing in an ammonia-containing atmosphere, the high treatment temperatures considered here are assumed to be sufficient for ammonia to decompose and equilibrate with molecular nitrogen and hydrogen [44]. Therefore, the nitrogen chemical potential was referenced to N2\mathrm{N}_{2}, rather than directly to NH3\mathrm{NH}_{3}.

Using this mapping, defect concentrations and the electron chemical potential can be evaluated as functions of the gas partial pressures within a consistent theoretical framework, facilitating comparison of defect-chemistry trends with experiment. We note that additional finite-temperature contributions to the free energies are neglected. Therefore, absolute concentrations should be interpreted with appropriate caution at high temperature.

To define the thermodynamic reservoirs, we constructed the semigrand canonical phase diagram, which maps the stability regions as a function of the chemical potentials of the constituents. The list of stable phases is reported in Table S 1.1.

CompositionStructureΔEf\Delta E^{f} (eV/atom)
BaCubic (Im3ˉmIm\bar{3}m)0.00
Ba2_{2}Ti13_{13}O22_{22}Orthorhombic (CmceCmce)-3.38
Ba2_{2}Ti6_{6}O13_{13}Monoclinic (C2/mC2/m)-3.50
Ba2_{2}TiO4_{4}Monoclinic (P21/cP2_{1}/c)-3.41
Ba3_{3}Ti20_{20}O40_{40}Monoclinic (C2/mC2/m)-3.49
Ba4_{4}Ti13_{13}O30_{30}Orthorhombic (CmceCmce)-3.54
BaOCubic (Fm3ˉmFm\bar{3}m)-2.83
BaO2_{2}Tetragonal (I4/mmmI4/mmm)-2.17
BaTiO5_{5}Orthorhombic (PnmaP nma)-3.54
BaTi8_{8}O16_{16}Monoclinic (C2C2)-3.49
BaTiO3_{3}Trigonal (R3mR3m)-3.50
O2_{2}Monoclinic (C2/mC2/m)0.00
TiHexagonal (P63/mmcP6_{3}/mmc)0.00
Ti2_{2}OTrigonal (P3ˉm1P\bar{3}m1)-2.04
Ti2_{2}O3_{3}Trigonal (R3ˉcR\bar{3}c)-3.31
Ti3_{3}OTrigonal (P3ˉ1cP\bar{3}1c)-1.57
Ti3_{3}O5_{5}Monoclinic (C2/mC2/m)-3.39
Ti6_{6}OTrigonal (P3ˉ1cP\bar{3}1c)-0.92
TiOHexagonal (P622P6_{2}2)-2.92
TiO2_{2}Monoclinic (C2/mC2/m)-3.51

Table S 1.1. Formation energy per atom for all the materials used to compute the stability diagram. The data is taken from the Materials Project database (PYMATGEN implementation, version 2025.5.2) [33, 36, 37].

The resulting stability diagram, obtained from these formation energies, is shown in Figure S 1.1. The allowed range of chemical potential is constrained by the condition that their sum must be equal to the formation enthalpy of BaTiO3\mathrm{BaTiO}_{3}:

ΔμBa+ΔμTi+3ΔμO=ΔHf[BaTiO3](12)\Delta\mu_{\mathrm{Ba}}+\Delta\mu_{\mathrm{Ti}}+3\Delta\mu_{\mathrm{O}}=\Delta H_{f}[\mathrm{BaTiO}_{3}] \tag*{(12)}

For a fixed sum of ΔμBa+ΔμTi\Delta\mu_{\mathrm{Ba}}+\Delta\mu_{\mathrm{Ti}}, the oxygen chemical potential ΔμO\Delta\mu_{\mathrm{O}} is determined by this condition. The stability region of BaTiO3\mathrm{BaTiO}_{3} is further limited by the presence of competing phases and is represented by the area delimited by points A to D, in Figure S 1.1. More specifically, given a generic competing phase of composition BaiTijOk\mathrm{Ba}_{i}\mathrm{Ti}_{j}\mathrm{O}_{k}, the chemical potentials must satisfy the condition:

iΔμBa+jΔμTi+kΔμO≤ΔHf[BaiTijOk].(13)i\Delta\mu_{\mathrm{Ba}} + j\Delta\mu_{\mathrm{Ti}} + k\Delta\mu_{\mathrm{O}} \le\Delta H_{\mathrm{f}}[\mathrm{Ba}_{i}\mathrm{Ti}_{j}\mathrm{O}_{k}]. \tag*{(13)}

The defect formation energies were calculated for different thermodynamic reservoirs, represented in Figure S 1.1 by the labels from A to D and X. Regions A-D span from O-rich conditions (points C and D) to Ba-rich and Ti-rich conditions (points A and B).

We also evaluated the formation energies using a thermodynamic reservoir that represents the experimental conditions. In particular, we fix the oxygen chemical potential (ΔμO\Delta\mu_{\mathrm{O}}) to its value under the conditions of temperature and partial pressure of the nitridation process (T=1073T = 1073 K, pO2=10−27p_{\mathrm{O}_{2}} = 10^{-27} atm). At these finite-temperature conditions, the 0 K-stability diagram is kept fixed, and temperature/pressure enter only through Equation (9), which details the calculation of this quantity. With this procedure, we obtained ΔμO=−4.04\Delta\mu_{\mathrm{O}} = -4.04 eV, which is indicated by the point X in Figure S 1.1.

For each oxygen partial pressure, we first determined μO\mu_{\mathrm{O}}. The remaining cation chemical potentials were then constrained by BaTiO3\mathrm{BaTiO}_{3} phase stability in the Ba-Ti-O system of Figure S 1.1: at fixed μO\mu_{\mathrm{O}}, the allowed μBa\mu_{\mathrm{Ba}} and μTi\mu_{\mathrm{Ti}} values form a line segment given by the intersection of the constant μO\mu_{\mathrm{O}} line with the BaTiO3\mathrm{BaTiO}_{3} stability region. The endpoints of this segment correspond to the limiting equilibria BaTiO3+BaTi2O5\mathrm{BaTiO}_{3} + \mathrm{BaTi}_{2}\mathrm{O}_{5} (Ti-rich limit) and BaTiO3+Ba2Ti2O4\mathrm{BaTiO}_{3} + \mathrm{Ba}_{2}\mathrm{Ti}_{2}\mathrm{O}_{4} (Ba-rich limit). We adopted a representative condition defined as the midpoint between these endpoints for each μO\mu_{\mathrm{O}}, and used the resulting set to compute defect formation energies and solve the charge-neutrality condition.

Assuming complete decomposition of NH3\mathrm{NH}_3 according to 2NH3→N2+3H22\mathrm{NH}_3 \rightarrow\mathrm{N}_2 + 3\mathrm{H}_2, the stoichiometric product gas contains a mole fraction xN2=0.25x_{\mathrm{N}_2} = 0.25. At a total pressure of 1 atm, this corresponds to pN2=0.25p_{\mathrm{N}_2} = 0.25 atm. We therefore use N2\mathrm{N}_2 as an effective nitrogen reservoir, with ΔμN=−1.18\Delta\mu_{\mathrm{N}} = -1.18 eV.

Since the range of stability varies for every compound, we evaluated the chemical potential of the elements in O-poor and O-rich regions, assigning the former to reservoirs A and B and the latter to reservoirs C and D. In region X, the values were taken from the center of the stability region, having fixed ΔμO\Delta\mu_{\mathrm{O}} to −4.04-4.04 eV. This procedure was employed to compare the formation energies of intrinsic defects. The chemical potential values associated with the labelled regions in the stability diagram are reported in Table S 1.2.

ReservoirΔμBa\Delta\mu_{\mathrm{Ba}}ΔμTi\Delta\mu_{\mathrm{Ti}}ΔμO\Delta\mu_{\mathrm{O}}ΔμN\Delta\mu_{\mathrm{N}}
A-1.84-1.14-4.84-1.18
B-1.02-0.50-5.33-1.18
C-6.68-10.830.00-1.18
D-6.18-10.83-0.17-1.18
X-2.47-2.91-4.04-1.18

Table S 1.2. Values in eV of the chemical potentials of the individual elements for each of the labelled regions in the stability diagram Figure S 1.1.

To assess the contribution of different point defects to the defect chemistry of BaTiO3\mathrm{BaTiO}_3 under the investigated conditions, we compared the equilibrium defect concentrations obtained from the full defect model with those calculated considering only NO\mathrm{N}_{\mathrm{O}} and vO\mathrm{v}_{\mathrm{O}} (Figure S 1.2). The full model includes NO\mathrm{N}_{\mathrm{O}}, vO\mathrm{v}_{\mathrm{O}}, vBa\mathrm{v}_{\mathrm{Ba}}, and vTi\mathrm{v}_{\mathrm{Ti}}. As illustrated by the formation energies in Figure S 1.2.c, the cation vacancies exhibit comparatively high formation energies, resulting in negligible equilibrium concentrations. Consequently, their exclusion from the charge-neutrality calculation is expected to have little influence on the concentrations of the dominant defects.

Concentrations of defect species and formation energies

Figure S1.2. a. Concentrations of all considered defect species as a function of imposed nitrogen concentration [N][\mathrm{N}], obtained from the charge-neutrality condition at T=1073T = 1073 K. b. Corresponding defect concentrations recalculated considering only NO\mathrm{N}_{\mathrm{O}} and vO\mathrm{v}_{\mathrm{O}}. c. Formation energies of all considered point defects as a function of EFE_{\mathrm{F}}, plotted with transposed axes. Stars indicate the corresponding charge transition levels, and the marked crossing point indicates equal formation energies of NO\mathrm{N}_{\mathrm{O}} and vO\mathrm{v}_{\mathrm{O}}. The high formation energies and low concentrations of vBa\mathrm{v}_{\mathrm{Ba}} and vTi\mathrm{v}_{\mathrm{Ti}} under these conditions motivate their exclusion from the reduced defect model discussed in the main text. Formation energies were determined at T=1073T = 1073 K and pO2=10−27p_{\mathrm{O}_2} = 10^{-27} atm, with the nitrogen chemical potential corresponding to an ideal-gas N2\mathrm{N}_2 reservoir with pN2=0.25p_{\mathrm{N}_2} = 0.25 atm, estimated assuming complete NH3\mathrm{NH}_3 dissociation at a total pressure of 1 atm.

Crystallography Data – BaTi(O,N)3_3

Optical Properties – BaTi(O,N)3_3

The optical response was assessed by calculating apparent absorbance as:

A=−log⁡(R)(14)A = -\log(R) \tag*{(14)}

where AA is absorbance and RR is reflectance, and by plotting the Kubelka–Munk (K–M) function F(R∞)F(R^\infty) directly against wavelength. The optical bandgaps of the samples were estimated using the K–M function [45], which transforms diffuse reflectance data into absorbance-like values suitable for powdered samples [46]. The reflectance of an optically thick sample (R∞R^\infty) was converted using the relation:

F(R∞)=(1−R∞)22R∞(15)F(R^\infty) = \frac{(1 - R^\infty)^2}{2R^\infty} \tag*{(15)}

where F(R∞)F(R^\infty) approximates the absorbance. Kubelka–Munk-transformed spectra F(R∞)F(R^\infty) were plotted as a function of photon energy for the entire sample series without normalisation in order to retain absolute differences in reflectance-derived absorption intensity.

In this study, band gaps were determined by plotting photon energy (hνh\nu) directly against the Kubelka–Munk absorbance function F(R∞)F(R^\infty), i.e., ‘energy vs absorbance’ plot, and estimating the onset of absorption from the inflection point or linear rise of the absorption edge of the raw, non-normalized spectra. Direct and indirect optical transitions were further evaluated using Tauc plots constructed from Kubelka–Munk-transformed diffuse reflectance data, with normalisation applied only for visual comparison of spectral features. Bandgap onset energies were extracted from the linear absorption edge of the raw Kubelka–Munk spectra, while normalised spectra were used exclusively for comparison of spectral shapes and absorption-edge evolution.

Electronic Structure Data – BaTi(O,N)3_3

Crystallography Data – Eu1−x_{1-x}Bax_xTi(O,N)3_3 / Eu1−x_{1-x}Cax_xTi(O,N)3_3

Neutron Diffraction Refinements

For all oxynitrides, the thermal atomic displacement parameters were refined as an overall value, and not as independent values. The atomic positions were kept fixed at the values obtained from the refinements of the synchrotron XRD data of the precursor oxides. The Ti occupancies were kept at nominal values, and Eu, Ba, and Ca occupancies were kept at the values refined from the parent oxides. Finally, for Eu0.8_{0.8}Ba0.2_{0.2}Ti(O,N)3_3, given the very low signal-to-noise ratio of the data due to the neutron absorption of Eu, symmetry lowering, and large reflection broadening, the atomic positions were kept fixed at the nominal values. This was done in order to avoid strong parameter correlation.

Table S 5.1. Structural data from Rietveld refinements of the neutron diffraction patterns of Eu0.2Ba0.8Ti(O,N)3\mathrm{Eu}_{0.2}\mathrm{Ba}_{0.8}\mathrm{Ti(O,N)}_{3} and Eu0.8Ba0.2Ti(O,N)3\mathrm{Eu}_{0.8}\mathrm{Ba}_{0.2}\mathrm{Ti(O,N)}_{3}. A secondary phase (TiN) is observed for the first. The atomic positions were kept fixed at theoretical and at the values obtained from the refinements of the synchrotron XRD data of the precursor oxide, seen in Table S 5.6. The Ti, and Eu, Ba occupancies were kept at nominal and at the values refined from the parent oxides, respectively. For Eu0.8Ba0.2Ti(O,N)3\mathrm{Eu}_{0.8}\mathrm{Ba}_{0.2}\mathrm{Ti(O,N)}_{3}, given the very low signal-to-noise ratio of the data due to the neutron absorption of Eu, the atomic positions were kept fixed at the nominal values. Occ = occupancy. For the P4mmP4mm structure, (O1)/N(1) occupy the 1b Wyckoff position, and O(2)/N(2) occupy the 2c position. For the PnmaPnma structure, O(1)/N(1) occupy the 4c Wyckoff position, and O(2)/N(2) occupy the 8d position.

Eu0.2Ba0.8Ti(O,N)3\mathrm{Eu}_{0.2}\mathrm{Ba}_{0.8}\mathrm{Ti(O,N)}_{3}Eu0.8Ba0.2Ti(O,N)3\mathrm{Eu}_{0.8}\mathrm{Ba}_{0.2}\mathrm{Ti(O,N)}_{3}
PhaseoxynitrideTiNoxynitride
Measurement typePNDPND
Wavelength λ\lambda (Å)1.120148(1)1.120148(1)
Measurement range0∘≤2θ≤153∘0^\circ\le2\theta\le153^\circ0∘≤2θ≤153∘0^\circ\le2\theta\le153^\circ
Space groupP4mmP4mmFm3ˉmFm\bar{3}mPnmaPnma
Fraction (wt.%)98.8(2)1.2(2)100
aa (Å)3.9785(2)4.167(2)5.538(3)
bb (Å)3.9785(2)= aa7.842(4)
cc (Å)3.9756(5)= aa5.480(4)
VV (Å3^{3})62.927(9)72.33(5)238.0(3)
Overall BisoB_{\mathrm{iso}} (Å2^{2})0.57(2)--0.2(1)
Occ((O1)/(N1))0.680/0.136(1)0.89/0.11(9)
Occ((O2)/(N2))0.924/0.024(1)1.00/0.00(5)
RpR_{\mathrm{p}} (%)1.636.69
RwpR_{\mathrm{wp}} (%)2.079.65
RBraggR_{\mathrm{Bragg}} (%)19.142.01.97
χ2\chi^{2}2.171.27

Table S 5.2. Structural data from Rietveld refinements of the neutron diffraction patterns of Eu0.2_{0.2}Ca0.8_{0.8}Ti(O,N)3_3 and Eu0.8_{0.8}Ca0.2_{0.2}Ti(O,N)3_3. A secondary phase (TiN) is observed for the first. The atomic positions were kept fixed at the values obtained from the refinements of the synchrotron XRD data of the precursor oxides, seen in Table S 5.8 and Table S 5.9. The Ti occupancies were kept at nominal values, and Eu and Ca occupancies were kept at the values refined from the parent oxides, respectively. Occ = occupancy. For both Pnma structures, O(1)/N(1) occupy the 4c Wyckoff position, and O(2)/N(2) occupy the 8d position.

Eu0.2_{0.2}Ca0.8_{0.8}Ti(O,N)3_3Eu0.8_{0.8}Ca0.2_{0.2}Ti(O,N)3_3
PhaseoxynitrideTiNoxynitride
Measurement typePNDPNDPND
Wavelength λ\lambda (Å)1.120148(1)1.120148(1)1.120148(1)
Measurement range0∘≤2θ≤153∘0^\circ\le2\theta\le153^\circ0∘≤2θ≤153∘0^\circ\le2\theta\le153^\circ0∘≤2θ≤153∘0^\circ\le2\theta\le153^\circ
Space groupPnmaFm3ˉ\bar{3}mPnma
Fraction (wt.%)98(1)1.7(1)100
aa (Å)5.4497(1)4.2174(4)5.5020(3)
bb (Å)7.6654(2)= aa7.7585(4)
cc (Å)5.4049(1)= aa5.4850(4)
VV (Å3^3)225.79(1)75.01(1)234.14(3)
Overall BisoB_{\mathrm{iso}} (Å2^2)0.56(2)--0.53(3)
Occ((O1)/(N1))0.79/0.14(1)0.682/0.304(1)
Occ((O2)/(N2))0.88/0.11(1)0.760/0.142(1)
RpR_p (%)3.043.042.57
RwpR_{\mathrm{wp}} (%)3.983.983.24
RBraggR_{\mathrm{Bragg}} (%)8.9110.112.8
χ2\chi^211.211.210.4

Table S 5.2.

Table S 5.3. Atomic positions data from the Rietveld refinements of the neutron diffraction pattern of Eu0.2_{0.2}Ca0.8_{0.8}Ti(O,N)3_3.

xxyyzz
Eu/Ca0.5133(8)14\frac{1}{4}-0.001(2)
Ti000
O(1)/N(1)0.500(1)14\frac{1}{4}0.5350(6)
O(2)/N(2)0.2773(6)0.0359(3)0.2173(7)

Table S 5.3.

High Resolution Synchrotron XRD Refinements

Table S5.5. Structural data from the Rietveld refinements of the high-resolution synchrotron XRD patterns of Eu0.2Ba0.8TiO3\mathrm{Eu}_{0.2}\mathrm{Ba}_{0.8}\mathrm{TiO}_{3} and Eu0.8Ba0.2TiO3\mathrm{Eu}_{0.8}\mathrm{Ba}_{0.2}\mathrm{TiO}_{3}. The atomic positions of Eu0.8Ba0.2TiO3\mathrm{Eu}_{0.8}\mathrm{Ba}_{0.2}\mathrm{TiO}_{3} were kept fixed at theoretical values.

Eu0.2Ba0.8TiO3\mathrm{Eu}_{0.2}\mathrm{Ba}_{0.8}\mathrm{TiO}_{3}Eu0.8Ba0.2TiO3\mathrm{Eu}_{0.8}\mathrm{Ba}_{0.2}\mathrm{TiO}_{3}1
Measurement typeHR-XRDHR-XRD
Wavelength λ\lambda (Å)0.354432(9)0.354432(9)
Measurement range0∘≤2θ≤47∘0^\circ\le2\theta\le47^\circ0∘≤2θ≤47∘0^\circ\le2\theta\le47^\circ
Space groupP4mmP4mmPm3ˉmPm\bar{3}m
aa (Å)3.98615(1)3.92(1)
bb (Å)=a=a=a=a
cc (Å)3.98775(1)=a=a
VV (ų)63.363(1)60.4(7)
Overall BisoB_{\mathrm{iso}} (Ų)0.507(5)--
Biso(Eu)/(Ba)B_{\mathrm{iso}}(\mathrm{Eu})/(\mathrm{Ba})--0.687
Biso(Ti)/(O1)B_{\mathrm{iso}}(\mathrm{Ti})/(\mathrm{O1})--0.298
RpR_{\mathrm{p}} (%)5.434.34
RwpR_{\mathrm{wp}} (%)8.896.86
RBraggR_{\mathrm{Bragg}} (%)1.96--
χ2\chi^230.72.53

Table S5.6. Atomic positions data from the Rietveld refinements of the high-resolution synchrotron XRD pattern of Eu0.2Ba0.8TiO3\mathrm{Eu}_{0.2}\mathrm{Ba}_{0.8}\mathrm{TiO}_{3}. The atomic positions and occupancy of Ti were kept fixed on the nominal values. O(1) occupies the 1b Wyckoff position, and O(2) occupies the 2c position.

xxyyzzOccupancy (occ)
Eu/Ba00-0.000(1)0.216/0.784(1)
Ti12\frac{1}{2}12\frac{1}{2}12\frac{1}{2}1
O(1)12\frac{1}{2}12\frac{1}{2}-0.021(4)1.00(2)
O(2)12\frac{1}{2}00.464(2)1.09(1)

3D Electron Diffraction

For the orthorhombic PnmaPnma majority phase of Eu0.2_{0.2}Ca0.8_{0.8}Ti(O,N)3_3, the AA-site was refined as a mixed Eu/Ca position with constrained occupancies, giving occ(Eu) = 0.170(8) and occ(Ca) = 0.830(8). For the cubic P213P2_13 minority phase in the same Eu0.2_{0.2}Ca0.8_{0.8}Ti(O,N)3_3 sample, two crystallographically distinct AA-sites were refined. The first site shows occ(Eu1) = 0.494(8) and occ(Ca1′) = 0.506(8), while the second site refines to occ(Ca2) = 0.611(12) and occ(Eu2′) = 0.389(12). These occupancies indicate a more Eu-rich AA-site environment compared to the PnmaPnma phase.

All atoms in both refinements were treated with isotropic displacement parameters. Occupancies were constrained such that occ(Eu) + occ(Ca) = 1 for each AA-site. Nitrogen could not be refined reliably in the 3DED datasets and is therefore omitted from both structural models.

Electron Energy-Loss Spectroscopy (EELS) and Energy Dispersive Spectroscopy (EDS) of Eu0.2Ca0.8Ti(O,N)3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{Ti(O,N)}_{3}

Elemental distributions of Eu, Ca, Ti, O, and N were mapped by both STEM-EDS and STEM-EELS (Figure S 6.1). For the EELS data, the N-K, O-K, and Ti-L edges were each integrated over a 30 eV window. Because absolute EELS intensities scale with local sample thickness, the N-K and O-K signals were normalised to the Ti-L edge, which served as the internal thickness reference, as Ti is present throughout the structure and exhibits a strong edge signal. Negative N-K integrals indicate nitrogen below the detection limit and were excluded from further quantitative analysis.

Four representative regions were classified by nitrogen content as N-rich, N-medium-rich, N-poor, and N-non-existent, and the corresponding N/Ti and O/Ti ratios were quantified for each (Figure S 6.1). The N-rich region showed the highest N/Ti and lowest O/Ti ratio among the regions analysed, and is co-located with a locally elevated Ti and N signal, consistent with a Ti- and N-enriched local environment resembling TiN.

Optical properties – Eu1−x_{1-x}Bax_xTi(O,N)3_3 / Eu1−x_{1-x}Cax_xTi(O,N)3_3

Electronic structure – Eu1−xBaxTi(O,N)3\mathrm{Eu}_{1-x}\mathrm{Ba}_{x}\mathrm{Ti(O,N)}_{3} / Eu1−xCaxTi(O,N)3\mathrm{Eu}_{1-x}\mathrm{Ca}_{x}\mathrm{Ti(O,N)}_{3}

Discussion Ti 2p and Ti L-edge and TiN

The Ti 2p3/22p_{3/2} core level spectra were fit with a Shirley background and deconvoluted using Gaussian-Lorentzian fits (GL(30)) to elucidate the local chemical environment and oxidation states of titanium. For the oxide samples, one main peak was observed, assigned to the Ti4+^{4+} state, corresponding to the standard tetravalent configuration of the titanium BB-site cation in the ideal ABO3AB\mathrm{O}_{3} perovskite-type lattice [47]. Additionally, a minor component may be present at a lower binding energy, approximately 1.5 eV below the Ti4+^{4+} main peak. This feature is attributed to a minor contribution of reduced Ti3+^{3+} species, which is typically associated with oxygen vacancies formed during processing under reducing conditions. However, because the contribution is small, this component was not fitted to avoid overparameterization.

When the samples were fit with a single peak after ammonolysis, all oxynitrides showed a higher Ti 2p3/22p_{3/2} FWHM. This led to the conclusion that another component, likely titanium atoms in a mixed oxynitride coordination environment (TiO6−xNx\mathrm{TiO}_{6-x}\mathrm{N}_{x}), is present, which shows the largest impact for the highest nitrogen incorporation in Eu0.8Ca0.2Ti(O,N)3\mathrm{Eu}_{0.8}\mathrm{Ca}_{0.2}\mathrm{Ti(O,N)}_{3}. Due to this, another component was added to the fit, while keeping the FWHM of the oxide fixed. This TiON4+\mathrm{Ti}^{4+}_{\mathrm{ON}} component was implemented with a FWHM of 1.2 times that of the oxide and a binding energy shift of 0.8 eV. Since it is assumed that, due to the Eu2+/3+\mathrm{Eu}^{2+/3+} charge transition, oxygen vacancy formation is hindered, little additional Ti3+\mathrm{Ti}^{3+} is expected, which is why it was not taken into consideration in the fit.

However, even after isolating the discrete TiON4+\mathrm{Ti}^{4+}_{\mathrm{ON}} coordination environments, the primary oxide-like Ti4+\mathrm{Ti}^{4+} peak of Eu0.8Ca0.2Ti(O,N)3\mathrm{Eu}_{0.8}\mathrm{Ca}_{0.2}\mathrm{Ti(O,N)}_{3} still exhibits a downward shift in binding energy greater than what can be accounted for by the Fermi level shift alone. While the TiON4+\mathrm{Ti}^{4+}_{\mathrm{ON}} peak captures the effects of the first coordination sphere, this overarching shift of the entire lattice network seems to be additionally driven by global changes in covalency. This additional chemical shift is probably observed because nitrogen (3.04) is less electronegative than oxygen (3.44) on the Pauling scale, the replacement of O2−\mathrm{O}^{2-} by N3−\mathrm{N}^{3-} reduces the overall ionic character of the extended anion network.

For Eu0.2Ca0.8Ti(O,N)3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{Ti(O,N)}_{3}, a third distinct component was required to accurately fit the spectra. This additional feature is located at a significant downward shift of approximately 3.0 eV relative to the Ti4+\mathrm{Ti}^{4+} position, which is characteristic of titanium nitride (TiN\mathrm{TiN}) [47,48]. TiN\mathrm{TiN} has previously been discussed as forming for higher Ca contents in Eu1−xCaxTi(O,N)3\mathrm{Eu}_{1-x}\mathrm{Ca}_{x}\mathrm{Ti(O,N)}_{3} by Widenmeyer et al. [12]. This peak assignment is fully corroborated by the neutron diffraction data refinements and can also clearly be distinguished in the N 1s spectrum in Figure S8.1. This selective phase segregation provides compelling evidence for a saturation-controlled reaction mechanism during high-temperature ammonolysis. Exposure to the reducing and nitriding ammonia atmosphere no longer alters the bulk composition; instead, it induces a localised structural decomposition, driving the exsolution of titanium to form secondary TiN\mathrm{TiN} once the sample reaches its limit for nitrogen incorporation, when the Eu2+/3+\mathrm{Eu}^{2+/3+} charge transition is complete.

The analysis of the Ti L-edge NEXAFS of the Ca-containing samples reveals another difference. While the Eu0.8Ba0.2Ti(O,N)3\mathrm{Eu}_{0.8}\mathrm{Ba}_{0.2}\mathrm{Ti(O,N)}_{3} shows only minor differences to its oxide counterpart, Eu0.2Ca0.8Ti(O,N)3\mathrm{Eu}_{0.2}\mathrm{Ca}_{0.8}\mathrm{Ti(O,N)}_{3} already shows larger differences around 456 eV to 458 eV photon energy. The Eu0.8Ca0.2Ti(O,N)3\mathrm{Eu}_{0.8}\mathrm{Ca}_{0.2}\mathrm{Ti(O,N)}_{3} sample shows an even larger difference, even showing a splitting of the t2gt_{2g} feature. This behaviour is well rationalised by the crystal-field multiplet calculations by de Groot et al., which demonstrate that lowering the local coordination symmetry from a perfect octahedron breaks the degeneracy of the t2gt_{2g} subbands, resulting in distinct peak splitting or multi-peak profiles that reflect severe local polyhedral distortions [49].

References

References

  1. [1]Y. Bao, C. Li, K. Domen, F. Zhang, Strategies and Methods of Modulating Nitrogen-Incorporated Oxide Photocatalysts for Promoted Water Splitting, Accounts of Materials Research 3 (2022) 449–460. https://doi.org/10.1021/accountsmr.1c00271.
  2. [2]M. Pichler, J. Szlachetko, I.E. Castelli, N. Marzari, M. Döbeli, A. Wokoun, D. Pergolesi, T. Lippert, Determination of Conduction and Valence Band Electronic Structure of LaTiOₓNᵧ Thin Film, ChemSusChem 10 (2017) 2099–2106. https://doi.org/10.1002/cssc.201601632.
  3. [3]M. Widenmeyer, T. Kohler, M. Samolis, A.T. de Denko, X. Xiao, W. Xie, F.E. Osterloh, A. Weidenkaff, Band Gap Adjustment in Perovskite-type Eu₁₋ₓCaₓTiO₃ via Ammonolysis, Zeitschrift für Physikalische Chemie 234 (2020) 887–909. https://doi.org/10.1515/zpch-2019-1429.
  4. [4]K. Maeda, K. Domen, New Non-Oxide Photocatalysts Designed for Overall Water Splitting under Visible Light, The Journal of Physical Chemistry C 111 (2007) 7851–7861. https://doi.org/10.1021/jp070911w.
  5. [5]T. Takata, C. Pan, K. Domen, Recent progress in oxynitride photocatalysts for visible-light-driven water splitting, Science and technology of advanced materials 16 (2015) 33506. https://doi.org/10.1088/1468-6996/16/3/033506.
  6. [6]K. Maeda, K. Domen, Oxynitride materials for solar water splitting, MRS Bulletin 36 (2011) 25–31. https://doi.org/10.1557/mrs.2010.4.
  7. [7]A. Fuertes, Synthetic approaches in oxynitride chemistry, Progress in Solid State Chemistry 51 (2018) 63–70. https://doi.org/10.1016/j.progsolidstchem.2017.11.001.
  8. [8]S. Jiang, Y. Liu, J. Xu, Rare earth oxynitrides: promising visible-light-driven photocatalysts for water splitting, Materials Advances 2 (2021) 1190–1203. https://doi.org/10.1039/D0MA00867B.
  9. [9]A. Klein, K. Albe, N. Bein, O. Clemens, K.A. Creutz, P. Erhart, M. Frericks, E. Ghorbani, J.P. Hofmann, B. Huang, B. Kaiser, U. Kolb, J. Koruza, C. Kübel, K.N.S. Lohaus, J. Rödel, J. Rohrer, W. Rheinheimer, R.A. de Souza, V. Streibel, A. Weidenkaff, M. Widenmeyer, B.-X. Xu, H. Zhang, The Fermi energy as common parameter to describe charge compensation mechanisms: A path to Fermi level engineering of oxide electroceramics, Journal of Electroceramics 51 (2023) 147–177. https://doi.org/10.1007/s10832-023-00324-y.
  10. [10]H.-I. Yoo, C.-R. Song, D.-K. Lee, BaTiO₃₋δ: Defect Structure, Electrical Conductivity, Chemical Diffusivity, Thermoelectric Power, and Oxygen Nonstoichiometry, Journal of Electroceramics 8 (2002) 5–36. https://doi.org/10.1023/A:1015570717935.
  11. [11]J. Nowotny, Defect chemistry of BaTiO₃, Solid State Ionics 49 (1991) 135–154. https://doi.org/10.1016/0167-2738(91)90079-Q.
  12. [12]E. Erdem, P. Jakes, R.-A. Eichel, D.C. Sinclair, M. Pasha, I.M. Reaney, Formation of defect dipoles in BaTiO₃ ceramics heat-treated under reduced oxygen partial-pressure, Functional Materials Letters 3 (2010) 65–68. https://doi.org/10.1142/S1793604710000956.
  13. [13]Y. Takeda, K. Kanno, T. Takada, O. Yamamoto, M. Takano, N. Nakayama, Y. Bando, Phase relation in the oxygen nonstoichiometric system, SrFeOₓ (2.5 ≤ x ≤ 3.0), Journal of Solid State Chemistry 63 (1986) 237–249. https://doi.org/10.1016/0022-4596(86)90174-X.
  14. [14]H. Guo, A. Jaworski, Z. Chen, C. Lu, A. Slabon, U. Häussermann, Barium Titanium Oxynitride from Ammonia-Free Nitridation of Reduced BaTiO₃, Inorganics 9 (2021) 62. https://doi.org/10.3390/inorganics9080062.
  15. [15]S. Yoon, K. Son, S.G. Ebbinghaus, M. Widenmeyer, A. Weidenkaff, Ferromagnetism in nitrogen and fluorine substituted BaTiO₃, Journal of Alloys and Compounds 749 (2018) 628–633. https://doi.org/10.1016/j.jallcom.2018.03.221.
  16. [16]M. Miyazaki, H. Saito, K. Ogasawara, M. Kitano, H. Hosono, BaTiO₃-xNᵧ: Highly Basic Oxide Catalyst Exhibiting Coupling of Electrons at Oxygen Vacancies with Substituted Nitride Ions, Journal of the American Chemical Society 145 (2023) 25976–25982. https://doi.org/10.1021/jacs.3c10727.
  17. [17]T. Yajima, F. Takeiri, K. Akamatsu, K. Fujita, W. Yoshimune, M. Ohkura, S. Lei, V. Gopalan, K. Tanaka, C.M. Brown, M.A. Green, T. Yamamoto, Y. Kobayashi, H. Kageyama, A labile hydride strategy for the synthesis of heavily nitridized BaTiO₃, Nature Chem 7 (2015) 1017–1023. https://doi.org/10.1038/nchem.2370.
  18. [18]T. Müller, T. Großmann, H.-P. Abicht, Nitrogen containing barium titanate: Preparation and characterisation, Journal of Physics and Chemistry of Solids 70 (2009) 1093–1097. https://doi.org/10.1016/j.jpcs.2009.06.003.
  19. [19]M. Barroso, A. Nazneen, M. Hackner, W. Xie, A. Weidenkaff, M. Widenmeyer, Environmental evaluation of oxynitride synthesis pathways using Life Cycle Assessment, Solid State Sciences 174 (2026) 108233. https://doi.org/10.1016/j.solidstatesciences.2026.108233.
  20. [20]L. Sagarna, K.Z. Rushchanskii, A. Maegli, S. Yoon, S. Populoh, A. Shkabko, S. Pokrant, M. Ležaić, R. Waser, A. Weidenkaff, Structure and thermoelectric properties of EuTi(O,N)₃±δ, Journal of Applied Physics 114 (2013) 33701. https://doi.org/10.1063/1.4813098.
  21. [21]T.-C. Lin, X. Qi, Cation Valences and Multiferroic Properties of EuTiO₃ Co-Doped with Ba and Transition Metals of Co/Ni, Materials 15 (2022) 6652. https://doi.org/10.3390/ma15196652.
  22. [22]P. Serna-Gallén, H. Beltrán-Mir, E. Cordoncillo, A.R. West, R. Balda, J. Fernández, Site-selective symmetries of Eu³⁺-doped BaTiO₃ ceramics: a structural elucidation by optical spectroscopy, Journal of Materials Chemistry C 7 (2019) 13976–13985. https://doi.org/10.1039/C9TC03987B.
  23. [23]L. Villa, Impact of doping conditions on the Fermi level in lead-free antiferroelectrics. PhD Thesis, Universitäts- und Landesbibliothek Darmstadt, 2023. https://doi.org/10.26083/tuprints-00024481.
  24. [24]Y. Kumagai, F. Oba, Electrostatics-based finite-size corrections for first-principles point defect calculations, Physical Review B 89 (2014) 195205. https://doi.org/10.1103/PhysRevB.89.195205.
  25. [25]L. Villa, K. Albe, defermi: A tool for computing and visualizing point-defect equilibria, bridging computational and experimental users, The Journal of Chemical Physics 165 (2026). https://doi.org/10.1063/5.0344236.
  26. [26]M. Widenmeyer, J. Häcker, C. Bubeck, S. Yoon, O. Clemens, A. Weidenkaff, Sequential double anionic substitution through synthesis of perovskite-type AB(O,N,F)₃ with A = Ca, Sr, Ba and B = Ti, Zr, Solid State Sciences 146 (2023) 107376. https://doi.org/10.1016/j.solidstatesciences.2023.107376.
  27. [27]T. Mueller, J. Montoya, W. Ye, X. Lei, L. Hung, J. Hummels­høj, M. Puzon, D. Martinez, C. Fajardo, R. Abela, An electrochemical series for materials, Proceedings of the National Academy of Sciences of the United States of America 121 (2024) e2320134121. https://doi.org/10.1073/pnas.2320134121.
  28. [28]R. Gillen, S.J. Clark, J. Robertson, Nature of the electronic band gap in lanthanide oxides, Physical Review B 87 (2013) 125116. https://doi.org/10.1103/PhysRevB.87.125116.
  29. [29]B. Huang, 4f fine-structure levels as the dominant error in the electronic structures of binary lanthanide oxides., Journal of Computational Chemistry 37 (2016) 825–835. https://doi.org/10.1002/jcc.24272.
  30. [30]A.P. Aslla-Quispe, R.H. Miwa, J. Guerra, Role of the rare-earth doping on the multiferroic properties of BaTiO3: First-principles calculation, Physica B: Condensed Matter 615 (2021) 413107. https://doi.org/10.1016/j.physb.2021.413107.
  31. [31]S. Xu, Y. Gu, X. Wu, Structural, electronic and magnetic properties of a ferromagnetic metal: Nb-doped EuTiO3, Journal of Magnetism and Magnetic Materials 497 (2020) 166077. https://doi.org/10.1016/j.jmmm.2019.166077.
  32. [32]V.K. Pecharsky, P.Y. Zavalii, Fundamentals of Powder Diffraction and Structural Characterization of Materials, Springer US, Boston, MA, 2009.
  33. [33]X. Xiao, M. Widenmeyer, K. Mueller, M. Scavini, S. Cecchia, C. Castellano, D. Ma, S. Yoon, W. Xie, U. Starke, K. Zakharchuk, A. Kovalevsky, A. Weidenkaff, A squeeze on the perovskite structure improves the thermoelectric performance of Europium Calcium Titanates, Materials Today Physics 7 (2018) 96–105. https://doi.org/10.1016/j.mtphys.2018.11.009.
  34. [34]M. Widenmeyer, S. Cecchia, X. Xiao, M. Scavini, A. Weidenkaff, Effects of Nanodomains on Local and Long-Range Phase Transitions in Perovskite-Type Eu₀.₈Ca₀.₂TiO₃-δ, Nanomaterials 10 (2020) 769. https://doi.org/10.3390/nano10040769.
  35. [35]M. Yang, J. Oró-Solé, J.A. Rodgers, A.B. Jorge, A. Fuertes, J.P. Attfield, Anion order in perovskite oxynitrides, Nature Chemistry 3 (2011) 47–52. https://doi.org/10.1038/nchem.908.
  36. [36]N. Vonrüti, U. Aschauer, Anion Order and Spontaneous Polarization in LaTiO₂N Oxynitride Thin Films, Physical review letters 120 (2018) 46001. https://doi.org/10.1103/PhysRevLett.120.046001.
  37. [37]C. Laubschat, B. Perscheid, W.-D. Schneider, Final-state effects and surface valence in Eu-transition-metal compounds, Physical review. B, Condensed matter 28 (1983) 4342–4348. https://doi.org/10.1103/PhysRevB.28.4342.
  38. [38]S.P. Kowalczyk, N. Edelstein, F.R. McFeely, L. Ley, D.A. Shirley, X-ray photoemission spectra of the 4d levels in rare-earth metals, Chemical Physics Letters 29 (1974) 491–495. https://doi.org/10.1016/0009-2614(74)85076-1.
  39. [39]R. Vercaemst, D. Poelman, L. Fiermans, R.L. van Meirhaeghe, W.H. Laflère, F. Cardon, A detailed XPS study of the rare earth compounds EuS and EuF₃, Journal of Electron Spectroscopy and Related Phenomena 74 (1995) 45–56. https://doi.org/10.1016/0368-2048(95)02349-6.
  40. [40]S. Chaoudhary, L. Nguyen, X. Xiao, A. Weidenkaff, A. Klein, M. Widenmeyer, Uncovering the Electronic Effects of Cr Doping in Ba₂In₂O₅, Chemistry of Materials 37 (2025) 1621–1628. https://doi.org/10.1021/acs.chemmater.4c03240.
  41. [41]R. Mikita, T. Aharen, T. Yamamoto, F. Takeiri, T. Ya, W. Yoshimune, K. Fujita, S. Yoshida, K. Tanaka, D. Batuk, A.M. Abakumov, C.M. Brown, Y. Kobayashi, H. Kageyama, Topochemical Nitridation with Anion Vacancy-Assisted N³⁻/O²⁻ Exchange, Journal of the American Chemical Society 138 (2016) 3211–3217. https://doi.org/10.1021/jacs.6b00088.
  42. [42]Y. Hermans, S. Murcia-López, A. Klein, W. Jaegermann, BiVO₄ Surface Reduction upon Water Exposure, ACS Energy Letters 4 (2019) 2522–2528. https://doi.org/10.1021/acsenergylett.9b01667.
  43. [43]R.D. Shannon, Revised effective ionic radii and systematic studies of interatomic distances in halides and chalcogenides, Acta Crystallographica Section A: Crystal Physics, Diffraction, Theoretical and General Crystallography 32 (1976) 751–767. https://doi.org/10.1107/S0567739476001551.
  44. [44]Y.Q. Jia, Crystal radii and effective ionic radii of the rare earth ions, Journal of Solid State Chemistry 95 (1991) 184–187. https://doi.org/10.1016/0022-4596(91)90388-X.
  45. [45]F.C. Hawthorne, O.C. Gagné, New ion radii for oxides and oxysalts, fluorides, chlorides and nitrides, Acta Crystallographica Section B: Structural Science, Crystal Engineering and Materials 80 (2024) 326–339. https://doi.org/10.1107/S2052520624005080.

Paper details

vlnc:W_gx4zpee4
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 1

downloads · 2

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents