Two-photon polymerization 3D printing advances optical fibers into complex lab-on-fiber devices. However, widespread adoption remains bottlenecked by the inherent inefficiencies of sequential, direct-on-fiber printing. To address this, a custom-designed modular platform and a corresponding fiber-decoupled fabrication methodology on planar substrates are presented. This platform features a compliant, spring-like socket that enables passive self-alignment and reversible fiber insertion, paired with a customizable frontal device. The shift to fabrication on planar substrates enables parallel batch processing and allows the substrate to serve as a functional magazine for device mounting. To demonstrate this approach, modular platforms featuring a functional tip are printed, sharpened via post-process plasma etching, metallized, and equipped with an optical aperture using focused ion beam milling, while remaining on the planar substrate. Subsequently, these are used as exchangeable scanning probe microscopy tips mounted in situ within a scanning electron microscope. Simultaneous three-channel correlative imaging (atomic force microscopy topography, secondary electron, and cathodoluminescence) is used to validate the optomechanical stability of the design. Ultimately, by decoupling the delicate optical device's lifespan from the optical fiber, this architecture transforms lab-on-fiber tools into scalable, seamlessly replaceable consumables, offering a highly adaptable pathway for broader applications in photonics, sensing, and microscopy.
Introduction
Optical fibers have evolved from passive light guides into versatile platforms for integration of multifunctional devices [1]. In particular, lab-on-fiber technologies have transformed the fiber tip into a compact site for integration of devices tailored to specific applications [2, 3]. Within this progress, femtosecond-laser Two-Photon Polymerization (TPP) has proven to be a powerful resource for directly fabricating complex micro-optomechanical components on optical fiber facets [4]. TPP provides freeform three-dimensional design capabilities, submicrometer fabrication resolution, and precise alignment with the fiber core. This overcomes the geometric limitations of conventional fiber-end optics and enables comprehensive control of the emerging optical field [5, 6, 7, 8]. These capabilities have been utilized in diverse application-specific fiber-tip devices, including beam-shaping elements, sensors, mechanical grippers, and Scanning Probe Microscopy (SPM) probes [6, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18]. Within the domain of scanning probes, 3D-printed SPM architectures have demonstrated the ability to leverage complex microstructures to tune resonance spectra and tip-sample impact [19, 20]. Furthermore, light-guiding Scanning Near-field Optical Microscopy (SNOM) tips have been introduced for asymmetric nanofocusing [21], high-numerical-aperture mapping, and ultra-sharp tip curvature radii down to 15 nm [22, 23, 24].
Despite these advances, fabricating devices directly on optical fibers introduces severe logistical and physical bottlenecks inherent to the quasi-one-dimensional nature of the fiber substrate. Each fiber must be handled individually, significantly prolonging the manipulation time required for mounting and dismounting during fabrication. This inefficiency is especially pronounced when managing long, bundled fibers, and propagates through all subsequent post-processing steps, including thin-film coating, plasma etching, and pyrolysis. Furthermore, monolithic integration couples the structural integrity of the optical fiber directly to the printed device; damage to either component renders the entire assembly nonfunctional. This coupled risk is especially adverse for short-lifetime or intentionally consumable devices, ultimately limiting the scalability and adoption of 3D-printed on-fiber technologies.
These limitations can be overcome by decoupling device fabrication from the optical fiber and instead printing structures on a planar substrate for subsequent mounting. This shifts manufacturing to a planar wafer-scale approach, facilitating fabrication and processing of structures in batches. A planar substrate streamlines typical post-processing workflows—including curing [25], plasma etching [26], pyrolysis [27], thin-film deposition [28], and surface functionalization [29]—while facilitating a batch-level visual inspection to isolate the highest-performing structures [30, 31]. Decoupled fabrication is highly advantageous for rapid prototyping and consumable applications subject to rapid wear or cross-contamination [32, 33]. However, this paradigm shift is only viable if the subsequent fiber-integration procedure is sufficiently robust and time-efficient [34, 35].
The foundation of decoupled integration has been demonstrated using planar-printed sockets for the passive insertion and self-alignment of micro-optics onto fibers [36]. While this prior architecture provides a proof-of-concept, it is limited by a large form factor; accommodating a standard 125 μm diameter fiber required a socket 470 μm in diameter and 500 μm in length. Such dimensions restrict practical application in domains that require slender, low-profile, or minimally invasive probes, such as SPM. To address this gap, we introduce a compact, modular platform that maintains the scalability of decoupled planar fabrication while minimizing the mechanical footprint. The viability of this platform is validated by a high-stress proof-of-concept application that demonstrates robust optomechanical stability during correlative microscopy consisting of Atomic Force Microscopy (AFM), Scanning Electron Microscopy (SEM), and Cathodoluminescence (CL).
Concept and design of the platform
Here, we propose a modular platform compatible with serial wafer-scale fabrication (Figure 1a), comprising a socket for passive optical fiber integration and a customizable device section

Figure 1. TPP 3D-printed modular platforms enabling fiber-decoupled, wafer-scale fabrication of functional devices. (a) SEM image of a fabrication batch consisting of multiple mounting cells printed on a planar substrate. (b) Colored SEM image of the modular platform highlighting the socket section (blue) for optical fiber integration and the device section (red) in the form of an SPM tip. (c) Proposed versatility of the device section; (i) colored SEM image, (ii–iv) illustrations.
Etching Protocol Optimization
(Figure 1b). Key design parameters prioritize an efficient, reversible fiber-mounting process, mechanical stability, and effective light coupling across the fiber-device interface. This architecture is inherently versatile and can support a wide array of TPP 3D-printed optical fiber devices (Figure 1c). For validation, correlative AFM, SEM, and CL imaging utilizing an integrated SNOM tip as the sensing device was selected as a demanding proof-of-concept application. Consequently, this specific modular platform will be referred to as the exchangeable SPM tip throughout the application-related sections of this work. This high-stress application explicitly tests mechanical stability under shear-force scanning, optical coupling, and structural integrity inside a high-vacuum environment. Rather than optimizing the fundamental optics of the SNOM tip, which has already been established in the literature [22, 24], the tip is used strictly as an optomechanical test to validate the performance and parallel post-processing advantages of the presented modular platform.
The modular platform body consists of the functional device section and a structurally compliant socket section (Figure 2b). The socket serves as a self-locking sleeve that guides and secures the optical fiber. The mechanical design dictates a specific mounting sequence: at the rear of the socket, a guiding cone enables smooth optical fiber insertion. The inner wall of this cone incorporates foldable lamellae featuring a nominal interference fit of at the center that tapers toward the edges. These lamellae permit smooth forward fiber insertion while strongly resisting retraction. During insertion, friction against the lamellae longitudinally compresses the central spring-like body. This compression induces a slight radial expansion of the spring structure, facilitating the continuous advancement of the fiber. The spring body transitions into a rigid, solid-walled front section where the fiber facet is seated flush against the optical base plate. This compliant geometry accommodates common TPP post-fabrication shrinkage and provides tolerance to pre-mounting misalignment while decreasing the overall polymerized volume compared to a solid-walled cylinder, thereby significantly reducing the printing time.

Figure 2. Architecture and mounting methodology of the TPP 3D-printed modular platform. (a) 3D rendering of a single mounting cell on the planar substrate, comprising the modular platform (acting as the exchangeable SPM tip), auxiliary supports, and a guiding block. The sequence illustrates the fiber approach, alignment (highlighted by the colored directional arrows), and engagement. During alignment, the guiding block serves as a solid contact point against which the optical fiber is levered. (b) Cross-sectional design detailing the compliant socket section for fiber integration, the solid internal base plate, and the functional device section (configured here as an SPM tip).
The frontal segment of the platform houses the device section, which in this paper takes the form of an SPM tip for validation (Figure 1c(Figure 1i)). The tip is structured as a cone with a apex angle; this geometry maximizes optical throughput toward the terminal aperture [37] while providing sufficient clearance for unobstructed electron-beam access during correlative SEM imaging.
To fully leverage the aforementioned wafer-scale fabrication capabilities, the mounting cell design embeds auxiliary structures so that the planar substrate can be used as an exchangeable tip magazine (Figure 2a). Each platform is fixed to the substrate via supporting struts equipped with predefined breaking points, allowing a clean mechanical release upon successful fiber engagement. Additionally, a guiding block is printed directly behind each socket. This block pre-aligns the approaching optical fiber with the socket’s longitudinal axis, significantly increasing the reliability and speed of the mounting procedure.
Fabrication and post-processing
Fabrication was performed via TPP using an IQnano3D system (IQS nano) equipped with a nm femtosecond laser source ( fs pulse duration, MHz repetition rate, mW average power) and a microscope immersion objective (NA , Olympus). The mounting cells were fabricated from ResIQ Hybrid (IQS nano), an ORMOCER-type organic-inorganic hybrid photopolymer containing an organically modified silicon-oxygen-based inorganic network integrated within a cross-linked polymer matrix. This material was selected for its compatibility with high-resolution 3D-printing, its mechanical rigidity (Young’s modulus GPa), thermal stability (up to ), and optical properties (refractive index ) [38].
To enable the wafer-scale, fiber-decoupled paradigm, the modular platforms were printed in a horizontal orientation on a planar silicon substrate with the longitudinal axis of the modular platform and the integrated tip oriented approximately parallel to the substrate surface. Consequently, the tip axis was oriented orthogonal to the optical axis of the printing beam (Figure 3a).

Figure 3. Fabrication and characterization of the TPP 3D-printed exchangeable SPM tips and the effect of subsequent etching on the tip sharpness. (a) Schematic representation of the TPP layer-by-layer 3D-printing process in a polymer drop. The insets illustrate a polymerized voxel and a cross-sectional view defining the horizontal () and vertical () tip radii before (yellow, printed) and after (green, etched) the etching process. (b) SEM image of a single TPP 3D-printed mounting cell, with the arrows indicating the viewing angles for the two subsequent panels. (c) Top and (d) side view SEM images comparing the tip morphologies of as-printed (left) and etched (right) structures. The yellow and green stars denote the representative symmetrical tip for the as-printed and etched states, respectively. (e) Schematic defining the tip asymmetry ratio as . Statistical distribution of (f) the horizontal tip radius , and of (g) the vertical tip radius . (h) The calculated asymmetry ratio across three different fabrication batches. While each batch nominally consists of 12 printed samples (with two tips omitted in the second batch due to a printing error), only a subset of tips (1, 2, and 12 tips for the first, second, and third batches, respectively) were fully imaged from the side due to the gradual development of the imaging methodology. The data are compared for as-printed (yellow) versus etched (green) tips and are presented as the average with standard deviation bounds. The star symbols have the same meaning as in (c). The red dashed line in (h) indicates perfect symmetry ().
The mounting cell was imported as a three-dimensional STL model occupying an area of approximately with a total height of . This model was processed using the proprietary IQ Data software with the IQ Slicer module, which converted the model into a sequence of fabrication layers and corresponding exposure points. The STL model was discretized into 792 layers with a vertical layer spacing of 0.25 µm. The lateral voxel-to-voxel spacing in the horizontal plane was set to 0.25 µm.
Before printing, the substrate-photoresist interface was automatically detected at four positions corresponding to the corners of the print area. These measurements were used for automatic leveling and compensation of substrate tilt or local height variations. To ensure reliable attachment of the printed structures to the substrate, the starting layer was embedded by 0.25 µm below the detected substrate-resin interface. The three batches presented in this study were fabricated using an optimized exposure time of 0.5 µs. Under these conditions, the total printing duration for one complete mounting cell was approximately 25 minutes.
Following TPP fabrication, the samples were developed in Propylene Glycol Monomethyl Ether Acetate (PGMEA) for 5 min and then put into a second clean PGMEA bath for an additional 5 min. Subsequently, the samples were transferred into an isopropanol bath for 5 min, rinsed with fresh isopropanol spray, and finally dried using clean dry air or nitrogen. This development sequence was used to remove unpolymerized resin while minimizing contamination and residue formation on the printed structures.
Three batches of 12 exchangeable tips each were printed using this procedure; however, two tips were omitted from the second batch due to a queue error. The horizontal orientation of the exchangeable tip on the substrate, and consequently the orthogonal orientation of the tip to the laser beam (Figure 3a), causes a structural asymmetry at the very apex of the tip. This is an inherent property of the TPP voxel, which exhibits an elongated ellipsoidal geometry along the optical axis, causing the achievable axial feature size to be fundamentally larger than the lateral one [39].
To characterize the fabricated tips, two principal radii were defined and measured: the radius in the horizontal plane ( – measured in top view) and in the vertical plane ( – measured in side view), as detailed in Figure 3a. These dimensions were extracted from SEM micrographs (Figure 3c,Figure 3d) by manually fitting a circle to the tip apex. For structures having a flattened plateau, the fit was adapted across the degraded geometry to estimate the effective macroscopic curvature. To strictly preserve the native tip morphology, all SEM characterization was performed on pristine samples without charge dissipation coatings.
The analysis of the as-printed structures yielded average horizontal radii of = 241 ± 88 nm, 369 ± 186 nm, and 346 ± 94 nm across the three consecutive batches (Figure 3f). Due to the progressive refinement of the imaging methodology, comprehensive side-view characterization was restricted to the third batch, which exhibited an average vertical radius of = 766 ± 157 nm (Figure 3g). Incorporating the limited side-view data from the first (one tip) and second (two tips) batches, the global average tip asymmetry—defined as the ratio (Figure 3e)—was calculated to be = 2.5 ± 0.9 (Figure 3h).
The limitation of spatial resolution inherent to the orientation of the tip relative to the printing laser is especially evident when compared to structures printed directly onto optical fibers parallel to the optical axis, which featured curvature radii of 125 nm [24]. Nevertheless, the optimal as-printed tip reported here achieved a comparable horizontal radius of = 124 nm.
To surpass the resolution limits of TPP 3D-printing, post-fabrication plasma etching was employed. Prior studies have shown significant sharpening of fiber-printed tips using oxygen plasma on SCR500 resin, reducing the radii from 125 nm to 15 nm [22]. The presented planar substrate architecture, which carries the platforms, seamlessly facilitates the parallel application of a similar etching protocol.
The etching parameters were set to a forward power of 100 W, a working pressure of 100 mTorr, and a processing time of 300 s. A flux of 30 sccm O and 30 sccm SF was utilized. This specific ratio was critical for uniformly etching both the organic and inorganic components of the polymerized matrix. Although pure O plasma can enhance tip sharpness, it aggressively and preferentially removes organic compounds, resulting in severe morphological bulging (Figure S7 in Supplement 1).

Figure S7. Top-view SEM image of a single TPP 3D-printed tip demonstrating the bulging effect observed during the etching protocol optimization. The image illustrates the severe structural degradation and bulging resulting from etching the polymer exclusively with plasma (30 sccm) for 5 minutes. This adverse morphological change highlights the necessity of the optimized etching protocol utilized in the main fabrication batches, which instead employs a 1:1 gas mixture of and to achieve uniform tip sharpening without such detrimental artifacts.
Following the plasma treatment, the average horizontal tip radii across the three batches were reduced to nm, nm, and nm (Figure 3f). Concurrently, the average vertical radius in the third batch decreased to nm (Figure 3g). The minimum recorded horizontal radius for a single etched tip was nm. Avoiding charge dissipation coatings for the SEM characterization enabled direct morphological comparisons of each tip before and after etching (Figure 3c,Figure 3d and Figure S1–Figure S6 in Supplement 1). For the third batch, the etching protocol reduced the horizontal and vertical radii by average factors of 3.5 and 1.9, respectively. This anisotropic etch rate inherently increased the average structural asymmetry to (Figure 3h), although two exemplary structures achieved a near-perfect symmetry (). The yield of symmetrical tips could be increased by rigorously optimizing parameters to establish highly anisotropic etching regimes that preferentially target the larger vertical dimension [40].

Figure S1. Top-view morphological characterization of the TPP 3D-printed tips from the first fabrication batch. The SEM images display all 12 printed samples from this batch (labeled t1.1 to t1.12), comparing the apex geometries in the as-printed state (top rows, yellow labels) versus the etched state (bottom rows, green labels). To strictly avoid any additional influence on the tip shape and dimensions, all samples were imaged in their pristine state without applying conductive coatings.

Figure S6. Side-view morphological characterization of the TPP 3D-printed tips from the third fabrication batch. The SEM images illustrate the vertical profiles of all 12 printed samples from this batch (labeled t3.1 to t3.12) in the as-printed (top rows, yellow labels) and etched (bottom rows, green labels) conditions. Similar to the top-view analysis, the samples were imaged in their pristine state without any conductive coatings. Unlike the earlier batches, the imaging methodology was fully developed by this stage of the study, allowing every tip in this batch to be successfully inspected from the side.
Despite these geometric variations, the achieved dimensions meet the requirements for aperture-type SNOM probes, which typically utilize subwavelength apertures ranging from tens to hundreds of nanometers. Because the terminal metal-coated aperture forms the primary optical interface, it fundamentally dictates the local field confinement and coupling behavior. Consequently, the structural asymmetry of the dielectric support is not expected to compromise optical performance, provided the terminal aperture remains well-defined and sufficiently symmetric [37].
Following plasma etching, the whole fabricated batch underwent simultaneous surface metallization without removal from the planar substrate. An Ion Beam Sputtering Deposition (IBSD) system (Figure 4a) was used to deposit a 5 nm titanium adhesion layer followed by a 150 nm aluminum thin film. The process was performed using argon ions at an acceleration voltage of 600 V, at a base pressure of mbar and a working pressure of mbar. The deposition rates were approximately 0.3 Å · s for Ti and 0.5 Å · s for Al.

Figure 4. Batch-level metallization and aperture fabrication of the TPP 3D-printed exchangeable SPM tips. (a) Camera image of the IBSD vacuum chamber used for the deposition of a 5 nm Ti adhesion layer followed by a 150 nm Al film. (b) Detail of the sample holder, illustrating the positioning of the printed exchangeable tips towards the edge; the tips are oriented directly toward the sputtered atoms and rotated during deposition to minimize shadowing. (c) SEM image of the coated mounting cells from the second fabrication batch (with two tips omitted due to a previous printing queue error). (d) Top-view SEM detail of a single tip, showing the morphology of the metallic coating over the etched apex. (e) Front-view FIB Secondary Electron (SE) image demonstrating a 100 nm wide aperture milled with Ga FIB at the apex.
To minimize geometric shadowing, the substrate was mounted at a tilt relative to the atom flux, positioned near the front edge of the sample holder (Figure 4b), and continuously rotated during the deposition. This configuration ensured sufficient metal coverage of the exposed exterior surfaces (Figure 4c,Figure 4d) while intentionally shadowing the socket’s inner optical base plate, preserving its transparency for subsequent light coupling. Finally, a subwavelength optical aperture was fabricated at the tip apex by Ga Focused Ion Beam (FIB) milling (Figure 4e). While FIB milling is inherently a sequential process, retaining the tips on the planar substrate enabled continuous serial milling across the entire batch within a single vacuum cycle, streamlining the fabrication workflow as well as minimizing handling risks.
Fiber mounting
While the presented modular platform was successfully tested directly on bare optical fibers, its versatility is demonstrated here by mounting it onto an optical fiber attached to a Quartz Tuning Fork (QTF) of an SPM module compatible with high vacuum (LiteScope, NenoVision [41]). This SPM configuration was chosen as a proof-of-concept scenario that requires mechanical rigidity against high-frequency shear forces, precise optical alignment for light collection, and vacuum-chamber compatibility.
When the fabrication batch is installed into the custom dual-sample configuration of the SEM/SPM setup, it effectively serves as a tip magazine. This modularity allows for the in situ mounting and replacement of the 3D-printed exchangeable SPM tip directly from its stationary mounting cell onto a long-term installed high-performing QTF probe.
Although 3D-printed polymer tips have demonstrated sufficient durability even under demanding contact-mode scanning [19], they remain inherently more susceptible to mechanical wear than conventional probes. Consequently, this modularity enables the replacement of a tip upon eventual degradation or contamination without dismantling the whole optical fiber probe. Such an in situ exchange is facilitated by the aforementioned LiteScope SPM module. At a SEM stage tilt, the SEM monitors as the SPM probe accesses the horizontally mounted tip magazine. By tilting and rotating the SEM stage, both the probe and tip apex can be continuously observed as they access the region of interest on the vertically mounted target sample.
The high-precision in situ mounting workflow leverages the motorization of the SPM and live visual feedback from the SEM (Figure 5a, bFigure 1–bFigure 5). The fiber insertion procedure consists of three distinct steps:

Figure 5. High-precision in situ and manual benchtop mounting of the TPP 3D-printed exchangeable SPM tips. (a) False-colored SEM overview of the mounting setup, showing an optical fiber (blue) attached to a QTF (red) approaching a guiding block (purple) and an exchangeable SPM tip (green). (b1–b5) SEM image sequence of the mounting workflow. The fiber is aligned, inserted through the guiding block (b1), and pushed into the tip’s spring-like socket (b2). The spring provides visual feedback for fine alignment (b3), and pushing forward a fully engaged fiber (b4) breaks it free from the supporting struts (b5). A continuous recording of the in situ SEM mounting procedure is shown in Visualization 1. (b6) SEM image of the dismounting process, where retracting the fiber along the guiding block mechanically strips the used tip from the facet. (c) Photograph of a simplified benchtop mounting setup utilizing a stereomicroscope and manual micro-positioners. (d1–d5) Optical stereomicroscope image sequence demonstrating the successful tip mounting using the manual setup, facilitated by the socket’s inherent mechanical self-alignment.
Approach and Alignment: The optical fiber is driven toward the magazine and passed through a guiding block. This block mechanically corrects residual tilt and rotation, ensuring strict collinearity between the fiber and the selected tip’s axis (Figure 5bFigure 1).
Engagement: The fiber is advanced into the spring-like socket. The physical compression of the spring provides critical visual feedback, enabling immediate corrections (Figure 5bFigure 2, bFigure 3).
Detachment: Once the optical fiber facet seats against the inner base of the socket, a final forward motion fractures the predetermined breaking points on the supporting struts, leaving the SPM tip securely mounted on the fiber (Figure 5bFigure 4, bFigure 5).
Using this mounting procedure, a 95 % success rate was achieved.
Furthermore, the mounting mechanism is fully reversible, enabling the rapid detachment of worn or contaminated tips (Figure 5bFigure 6). By retracting the optical fiber backward through the rigid guiding block, the used tip is mechanically stripped from the facet. This process leaves the optical fiber pristine and immediately ready for a subsequent mounting cycle without requiring probe removal or manual intervention. It is important to note that while the dismounting process leaves the optical fiber pristine for subsequent mounting cycles, the TPP 3D-printed exchangeable tip itself is designed strictly as a single-use consumable. The physical engagement relies on the intentional deformation of the compliant structure and requires the supporting structures to secure the platform during mounting; thus, a dismounted platform cannot be reused.

Figure 6. Experimental setup and measurement configuration for correlative AFM, SEM, and CL provided by an SNOM tip. (a) Photograph of the LiteScope SPM module integrated within an SEM chamber. The setup adopts a custom dual-sample configuration, featuring a horizontally mounted tip magazine for the in situ tip exchange and a vertically oriented sample for measurement. The custom QTF probe houses an integrated optical fiber enabling simultaneous extraction of the CL signal, generated by the electron beam of the SEM, and AFM sensing of surface morphology. The CL signal is detected by a PMT. (b) Visualization of the custom-designed QTF probe. (c) Macroscopic SEM image showing the QTF probe with the mounted TPP 3D-printed exchangeable tip approaching the vertically oriented sample. (d) Closer SEM view of the mounted TPP 3D-printed exchangeable tip engaged with the sample surface. (e) High-magnification inset detailing the apex of the tip positioned directly over the region of interest.
To evaluate the platform’s dependence on high-precision instrumentation, the mounting procedure was additionally tested using a manual benchtop setup. As shown in Figure 5c and d1–d5, the fiber was mounted under a standard optical stereomicroscope using a manual 3-axis micro-positioner. Despite the mechanical self-alignment provided by the guiding block and spring-like socket, the procedure yielded a 70 % success rate. Experimental observations indicate that this reduced yield is primarily bottlenecked by the limited optical resolution of the stereomicroscope—failing to provide sufficient visual feedback during the critical spring-engagement phase—rather than by the motion-precision constraints of manual micro-positioning. Consequently, while manual benchtop mounting is physically feasible, achieving high reliability requires high-definition monitoring.
Proof-of-concept: validation by SPM application
The experimental setup for correlative AFM, SEM, and CL imaging consists of a LiteScope SPM module (NenoVision) mounted on the stage of an SEM (TESCAN VEGA II). The system utilizes a custom dual-sample configuration, described here in a reference 0° SEM stage tilt position (Figure 6a). In this configuration, the tip magazine carrying the prepared devices is mounted horizontally, and the sample of interest is mounted vertically. The seamless transition between the mounting regime and the measurement regime is facilitated by the SEM stage rotation and tilting, combined with an optimized custom QTF probe design (Figure 6b). The QTF is positioned horizontally, with the optical fiber attached to one of its prongs, ensuring unobstructed access to the tip magazine while preserving the QTF probe’s perpendicular orientation relative to the target sample. To ensure charge dissipation during SEM operation, the probe is equipped with a grounded outer conductive layer. The complete fabrication workflow of the QTF probe is detailed in Supplement 1 (Figure S8). The mechanical quality factor of the finalized probes was typically in the low hundreds, with the best performers exceeding 1300.

Figure S8. Visualization of the QTF probe fabrication process. A1 Optical fiber with partially stripped cladding. A2 Cleaving of the optical fiber after metal sputtering to create a clean facet. B1 Assembly and contacting of the Printed Circuit Board (PCB), QTF, and its holder. B2 Parylene C deposition over a tape mask. B3 Metal sputtering over a new tape mask. 4 Final step of gluing the metallized optical fiber to the metallized probe body.
In the measurement regime, the SEM stage is tilted to 40°, providing an unobstructed view of the tip engaged with the sample (Figure 6c–Figure 6e). Consequently, the relative tilt angle between the electron beam and the sample surface is 50°. The apparatus can acquire up to three distinct signals for post-acquisition spatial correlation. The surface morphology is sensed by a Secondary Electron (SE) detector (SEM), the 3D topography is derived from tip-sample interactions modulating the QTF oscillations (AFM), and the CL distribution is mapped via the photons emitted from the sample upon electron beam irradiation. In the last case, the tip collects the emitted light, couples it into the optical fiber, and directs it to a Photomultiplier Tube (PMT) (Hamamatsu). During scanning, the tip oscillates in a shear mode (amplitude regime, 90 % setpoint), while the electron beam is focused onto the surface with a defined spatial offset relative to the tip apex. The image formation is provided by scanning the sample via a piezo scanner relative to the stationary tip and electron beam.
The mechanical integrity of the modular platform was validated with dual-channel correlative measurements, simultaneously acquiring AFM topography and SE signals. A calibration grid (gold layer on a ruby substrate) featuring circular holes in the thin metal film with a step height of 200 nm was utilized as the sample. As shown in Figure 7a,Figure 7b, the platform successfully resolved the microstructured surface. The spatial correlation of the acquired images is visualized via a 3D overlay combining the two signals (Figure 7c) and through normalized, shift-adjusted line profiles extracted from both data channels (Figure 7d).

Figure 7. Proof-of-concept correlative imaging utilizing the in situ mounted TPP 3D-printed exchangeable SPM tip. The figure demonstrates the mechanical stability of the modular platform and optical coupling capabilities during multimodal scanning probe microscopy. (a) AFM topography of the sample surface. (b) Simultaneously acquired SE image of the same region ( sample tilt). (c) 3D visualization of the correlated overlay, combining the AFM topography and SE signal from the region of interest indicated by the light blue dashed rectangles in (a) and (b). (d) Normalized and shift-adjusted line profiles extracted along the blue and red solid lines in (a) and (b), respectively. (e) Three-channel correlative imaging displaying simultaneously acquired AFM topography (top), SE (middle), and CL signals (bottom). (f) Line profiles extracted along the respective colored lines in (e), presented without shift adjustments. All presented line profiles were acquired as an average across a 10-pixel-wide line.
Following the mechanical validation, a three-channel measurement was conducted to verify the platform’s optomechanical stability. A calibration grid consisting of line trenches in a 388 nm aluminum layer deposited on a Ce:YAP substrate served as the sample. Because Ce:YAP exhibits strong CL emission upon electron excitation, the CL image is expected to display alternating bright stripes corresponding to the exposed substrate, interrupted by dark regions where the aluminum layer blocks photon emission. The acquired three-channel dataset (Figure 7e) demonstrates this periodic spatial modulation across all three signals, as highlighted by the raw, unadjusted line profiles in Figure 7f. Compared to the dual-channel measurement, the CL signal collection required higher electron beam currents, providing demanding operational conditions that induced localized tip and sample charging and image drift. Nevertheless, the successful simultaneous extraction of the CL signal demonstrates the capability of the mounted tip to couple emitted light into the optical fiber.
By design, the modular socket creates an air gap between the optical fiber and the printed polymer component, replacing the direct fiber–polymer interface with separate fiber–air and air–polymer interfaces. This configuration adds extra Fresnel reflections and can lead to higher losses than in structures printed directly onto the fiber. The influence of varying the air gap was experimentally investigated in [36], where a air gap reduced the measured transmittance from 69.35 % for direct contact to 66.5 %. Nevertheless, the present platform is intended for applications in which rapid modularity and consumable batch replacement are prioritized over maximum signal transmission. Furthermore, it is particularly well suited to devices that inherently incorporate an optical gap in their design, as proposed in Figure 1c(ii)–(iv).
Conclusions
Here, we have presented a novel approach to optical fiber devices using fiber-decoupled fabrication in a horizontal orientation. This is facilitated by a TPP 3D-printed modular platform that carries the device on its front and houses the optical fiber in a spring-like socket body. The advantages of fiber-decoupled fabrication are demonstrated through parallel post-processing, enabling batch treatment of devices using standard processes (such as curing, plasma etching, and metallization) while avoiding cumbersome optical fiber bundle management.
The concept is validated through an SPM tip-device application, demonstrating proof-of-concept correlative two- and three-channel SE, AFM, and CL measurements. Admittedly, state-of-the-art SPM applications will require further application-specific optimization. However, the successful extraction of correlative AFM, SEM, and CL data verifies the platform’s optomechanical stability on the optical fiber, even under the high-stress conditions of shear-mode scanning.
Furthermore, this application demonstrates the opportunity for innovation in established fields enabled by fiber-decoupled fabrication in combination with plug-and-play functionality and self-alignment. We successfully implemented the planar substrate carrying the fabricated modular platform (i.e., exchangeable SPM tips) as a tip magazine in an AFM/SEM setup, demonstrating the capability to mount and dismount devices in situ on the optical fiber. Additionally, we demonstrated a complementary manual mounting approach for benchtop environments.
Future work should focus on optimizing the SPM application. Specifically, optimizing the design toward tapping-mode measurements will minimize lateral shear forces and mitigate tip wear. Furthermore, orienting the tip parallel to the printing laser will eliminate its inherent structural asymmetry. Additionally, demonstrating other proposed devices on the platform will showcase the broader versatility of this approach.
Funding This research was supported by Quantum materials for applications in sustainable technologies (QM4ST)–project No. CZ.02.01.01/00/22_008/0004572 under OP JAK, call Excellent Research. L.Z. acknowledges financial support from the Brno Ph.D. Talent Scholarship, funded by the Brno City Municipality.
Acknowledgment CzechNanoLab Research Infrastructure (ID 90251), funded by MEYS CR, is gratefully acknowledged for the financial support of the measurements/sample fabrication.
Disclosures M.M. is an employee of IQS nano s.r.o., and Š.Č. was employed by IQS nano s.r.o. during the course of this research. The other authors declare no conflicts of interest. The authors used Gemini (3.1 Pro and 4 Argon) for grammar refinement and organizational suggestions. The tool was not used to generate scientific claims, references, experimental data, or conclusions.
Data Availability Statement The data that support the findings of this study are openly available in Zenodo at https://doi.org/10.5281/zenodo.23208365.
Supplemental document See Supplement 1 for supporting content.
Supporting Information for: A plug-and-play platform for 3D-printed devices on optical fibers
Lukáš Zezulka; Zdeněk Nováček; Martin Konečný; Milan Matějka; Štěpán Černý; Katarína Rovenská; Jiří Spousta; Tomáš Šikola
This document provides and documents the supplementary information to the main manuscript. Included are individual top- and side-view scanning electron microscopy images of the individual characterized two-photon polymerization 3D-printed tips, details on the influence of gas mixtures during the plasma etching protocol, a step-by-step description of the quartz tuning fork probe assembly, and descriptive text for Visualization 1.
Morphological Characterization of Printed Batches
This section groups the top-view and side-view images for each of the three batches sequentially, allowing the reader to cross-reference the visual evidence with the measured data easily.
Batch 1 Characterization

Figure S2. Side-view morphological characterization of a TPP 3D-printed tip from the first fabrication batch. The SEM images illustrate the vertical profile of tip t1.1 in the as-printed (left, yellow label) and etched (right, green label) conditions. Similar to the top-view analysis, the sample was imaged in its pristine state without any conductive coatings. While this fabrication batch consists of 12 successfully printed samples, only a single tip (t1.1) was fully imaged from the side due to the gradual development of the imaging methodology at this early stage of the study.
Batch 2 Characterization

Figure S3. Top-view morphological characterization of the TPP 3D-printed tips from the second fabrication batch. The SEM images display 10 samples from this batch (labeled t2.1 to t2.4 and t2.7 to t2.12), comparing the apex geometries in the as-printed state (top rows, yellow labels) versus the etched state (bottom rows, green labels). Although a nominal batch consists of 12 printed samples, two tips (t2.5 and t2.6) are missing here because they were skipped in the printing queue due to an error. To strictly avoid any additional influence on the tip shape and dimensions, all samples were imaged in their pristine state without applying conductive coatings.

Figure S4. Side-view morphological characterization of TPP 3D-printed tips from the second fabrication batch. The SEM images illustrate the vertical profiles of tips t2.1 and t2.2 in the as-printed (top row, yellow labels) and etched (bottom row, green labels) conditions. Similar to the top-view analysis, the samples were imaged in their pristine state without any conductive coatings. While 10 samples were successfully printed in this batch, only two tips were fully inspected from the side due to the gradual development of the imaging methodology at this stage of the study.
Batch 3 Characterization

Figure S5. Top-view morphological characterization of the TPP 3D-printed tips from the third fabrication batch. The SEM images display all 12 printed samples from this batch (labeled t3.1 to t3.12), comparing the apex geometries in the as-printed state (top rows, yellow labels) versus the etched state (bottom rows, green labels). To strictly avoid any additional influence on the tip shape and dimensions, all samples were imaged in their pristine state without applying conductive coatings.
Etching Protocol Optimization
This section justifies the specific gas mixture utilized in the final experimental methodology.
Quartz tuning fork probe fabrication
The complete fabrication procedure of the probe is illustrated in Figure S8. The process starts with an FG105UCA multimode optical fiber (Thorlabs) with a core diameter of and a cladding diameter of [42], from which the front section of the cladding is stripped (step A1). The stripped segment is then coated by sputtering of Ti, followed by of Al, using a broad-beam ion source while rotating the fiber (step A2).
Next, the probe body is assembled by gluing the QTF into a 3D-printed holder, which is then attached to the PCB. After mechanical assembly, the QTF is electrically connected to the contact pads on the PCB via two wires (step B1). The contact pads are then partially protected with Kapton tape, and a Parylene C layer is deposited over the entire probe body using an SCS Parylene Deposition System (step B2). This dielectric layer insulates the electrical contacts of the PCB and QTF, preventing short-circuiting during subsequent metallization. Afterward, a bilayer of Ti and Al is deposited on the rotating probe body with a second Kapton tape mask applied (step B3) using the IBSD system. This metallic coating establishes a conductive, grounded outer surface that prevents charging of the tip and probe inside the SEM. Importantly, the two tape masks are designed so that the outer metal layer self-contacts with the central PCB pin, which serves as the grounding point.
Finally, the pre-coated optical fiber (steps A1–A2) is glued onto the tuning fork. Adhesive is applied sparingly at the front of the prong and more generously at the back, reducing disruption of the resonator whilst maintaining mechanical stability (step 4).
Visualization 1
Visualization 1 demonstrates the in situ SEM mounting process of the TPP 3D-printed exchangeable SPM tip onto an optical fiber. While this recording captures a different experimental iteration than the specific sequence shown in Figure 5(bFigure 1–bFigure 5 of the main manuscript, it illustrates the same workflow. The video shows the optical fiber alignment using the guiding block, its insertion into the tip’s spring-like socket through the guiding cone, and the final detachment of the tip from its supporting struts.
Furthermore, the video includes an earlier, now-retired force-mounting step utilizing a second support block; because this step is no longer applied, it is not described in the main text. Please note that the video playback has been accelerated, and static periods corresponding to SEM image acquisition have been edited out for brevity.
For convenience, it can also be viewed online at https://youtu.be/Pwhci0SOXpE.
References
- [1]Cristiano Pendão and Ivo Silva. Optical Fiber Sensors and Sensing Networks: Overview of the Main Principles and Applications. Sensors, 22(19):7554, January 2022. doi:10.3390/s22197554.DOI
- [2]Marco Pisco and Andrea Cusano. Lab-On-Fiber Technology: A Roadmap toward Multifunctional Plug and Play Platforms. Sensors, 20(17):4705, January 2020. doi:10.3390/s20174705.DOI
- [3]Yifeng Xiong and Fei Xu. Multifunctional integration on optical fiber tips: Challenges and opportunities. Advanced Photonics, 2(6):064001, November 2020. doi:10.1117/1.AP.2.6.064001.DOI
- [4]Peng Bian, Zhi-Yong Hu, Ran An, Zhen-Nan Tian, Xue-Qing Liu, and Qi-Dai Chen. Femtosecond Laser 3D Nano-Printing for Functionalization of Optical Fiber Tips. Laser & Photonics Reviews, 18(7):2300957, 2024. doi:10.1002/lpor.202300957.DOI
- [5]Joel Arriaga-Dávila, Cristian Rosero-Arias, Dirk Jonker, Margoth Córdova-Castro, Josua Zscheile, Robert Kirchner, Alan Aguirre-Soto, Robert Boyd, Israel De Leon, Han Gardenniers, and Arturo Susarrey-Arce. From Single to Multi-Material 3D Printing of Glass-Ceramics for Micro-Optics. Small Methods, 9(8):2401809, 2025. doi:10.1002/smtd.202401809.
- [6]Timo Gissibl, Simon Thiele, Alois Herkommer, and Harald Giessen. Sub-micrometre accurate free-form optics by three-dimensional printing on single-mode fibres. Nature Communications, 7(1):11763, June 2016. doi:10.1038/ncomms11763.DOI
- [7]Diana Gonzalez-Hernandez, Simonas Varapnickas, Andrea Bertoncini, Carlo Liberale, and Mangirdas Malinauskas. Micro-Optics 3D Printed via Multi-Photon Laser Lithography. Advanced Optical Materials, 11(1):2201701, 2023. doi:10.1002/adom.202201701.
- [8]Hao Wang, Cheng-Feng Pan, Chi Li, Kishan S Menghrajani, Markus A Schmidt, Aoling Li, Fu Fan, Yu Zhou, Wang Zhang, Hongtao Wang, Parvathi Nair Suseela, John You En Chan, Tomohiro Mori, Yueqiang Hu, Guangwei Hu, Stefan A Maier, Haoran Ren, Huigao Duan, and Joel K W Yang. Two-photon polymerization lithography for imaging optics. International Journal of Extreme Manufacturing, 6(4):042002, April 2024. doi:10.1088/2631-7990/ad35fe.DOI
- [9]Lee-Lun Lai, Po-Han Huang, Göran Stemme, Frank Niklaus, and Kristinn B. Gylfason. 3D Printing of Glass Micro-Optics with Subwavelength Features on Optical Fiber Tips. ACS Nano, 18(16):10788–10797, April 2024. doi:10.1021/acsnano.3c11030.DOI
- [10]Andrea Bertoncini and Carlo Liberale. Polarization Micro-Optics: Circular Polarization From a Fresnel Rhomb 3D Printed on an Optical Fiber. IEEE Photonics Technology Letters, 30(21):1882–1885, November 2018. doi:10.1109/LPT.2018.2871161.DOI
- [11]Simin Cao, Xinggang Shang, Hongyan Yu, Liping Shi, Lei Zhang, Ning Wang, and Min Qiu. Two-photon direct laser writing of micro Fabry-Perot cavity on single-mode fiber for refractive index sensing. Optics Express, 30(14):25536–25543, July 2022. doi:10.1364/OE.464210.DOI
- [12]Mao-qing Chen, Si-yuan Liu, Chi Zhang, and Yong Zhao. Two-photon 3D printing FP microcavity sensor for simultaneous measurement of temperature and non-contact pressure. Optics & Laser Technology, 179:111406, December 2024. doi:10.1016/j.optlastec.2024.111406.DOI
- [13]Jang Ah Kim, Dominic J. Wales, Alex J. Thompson, and Guang-Zhong Yang. Fiber-Optic SERS Probes Fabricated Using Two-Photon Polymerization For Rapid Detection of Bacteria. Advanced Optical Materials, 8(9):1901934, 2020. doi:10.1002/adom.201901934.DOI
- [14]Jiawen Li, Simon Thiele, Bryden C. Quirk, Rodney W. Kirk, Johan W. Verjans, Emma Akers, Christina A. Bursill, Stephen J. Nicholls, Alois M. Herkommer, Harald Giessen, and Robert A. McLaughlin. Ultrathin monolithic 3D printed optical coherence tomography endoscopy for preclinical and clinical use. Light: Science & Applications, 9(1):124, July 2020. doi:10.1038/s41377-020-00365-w.DOI
- [15]Jan Niklas Bauer, Leander Siegle, Claudia Imiolczyk, Pavel Ruchka, and Harald Giessen. Side-looking endoscopic micro-optics: Comparison between state-of-the-art two-photon polymerization printing techniques. Optics Express, 33(16):33473–33482, August 2025. doi:10.1364/OE.569187.DOI
- [16]Chang-Xu Li, Yu-Qing Liu, Dong-Dong Han, Shi-Liang Qu, and Yong-Lai Zhang. A tactile gripper on an optical fiber for perception and actuation. Nature Communications, 16(1):11513, December 2025. doi:10.1038/s41467-025-66575-1.DOI
- [17]Mengqiang Zou, Changrui Liao, Shen Liu, Cong Xiong, Cong Zhao, Jinlai Zhao, Zongsong Gan, Yanping Chen, Kaiming Yang, Dan Liu, Ying Wang, and Yiping Wang. Fiber-tip polymer clamped-beam probe for high-sensitivity nanoforce measurements. Light: Science & Applications, 10(1):171, August 2021. doi:10.1038/s41377-021-00611-9.DOI
- [18]Nourin Alsharif, Anna Burkatovsky, Charles Lissandrello, Keith M. Jones, Alice E. White, and Keith A. Brown. Design and Realization of 3D Printed AFM Probes. Small, 14(19):1800162, 2018. doi:10.1002/smll.201800162.DOI
- [19]Gerald Göring, Philipp-Immanuel Dietrich, Matthias Blaicher, Swati Sharma, Jan G. Korvink, Thomas Schimmel, Christian Koos, and Hendrik Hölscher. Tailored probes for atomic force microscopy fabricated by two-photon polymerization. Applied Physics Letters, 109(6):063101, August 2016. doi:10.1063/1.4960386.DOI
- [20]Liangdong Sun, Hongcheng Gu, Xiaojiang Liu, Haibin Ni, Qiwei Li, Yi Zeng, Ning Chang, Di Zhang, Hongyuan Chen, Zhiyong Li, Xiangwei Zhao, and Zhongze Gu. 3D-printed cellular tips for tuning fork atomic force microscopy in shear mode. Nature Communications, 11(1):5732, November 2020. doi:10.1038/s41467-020-19536-9.DOI
- [21]Liangdong Sun, Haibin Ni, Xiaojianq Liu, Di Zhang, Yi Zeng, Xiaofeng Han, Liyong Jiang, Hongyuan Chen, Xiangwei Zhao, and Zhongze Gu. 3D Printed Asymmetric Nanoprobe for Plasmonic Nanofocusing under Internal Illumination. ACS Photonics, 5(12):4872–4879, December 2018. doi:10.1021/acsphotonics.8b01041.DOI
- [22]Byung Je Jung, Hong Jin Kong, Yong-Hoon Cho, Kyu-Seung Lee, Chung Hyun Park, Dong-Yol Yang, and Kwang-Sup Lee. Fabrication of sharp-needled conical polymer tip on the cross-section of optical fiber via two-photon polymerization for tuning-fork-based atomic force microscopy. Optics Communications, 286:197–203, January 2013. doi:10.1016/j.optcom.2012.09.003.DOI
- [23]Junze Zhou, Arian Gashi, Fabrizio Riminucci, Boyce Chang, Edward Barnard, Stefano Cabrini, Alexander Weber-Bargioni, Adam Schwartzberg, and Keiko Munechika. Sharp, high numerical aperture (NA), nanoimprinted bare pyramid probe for optical mapping. Review of Scientific Instruments, 94(3):033902, March 2023. doi:10.1063/5.0104012.DOI
- [24]Byung Je Jung, Hong Jin Kong, Yong-Hoon Cho, Chung Hyun Park, Min Kwan Kim, Byoung Goo Jeon, Dong-Yol Yang, and Kwang-Sup Lee. Fabrication of 15 nm curvature radius polymer tip probe on an optical fiber via two-photon polymerization and O₂-plasma ashing. Current Applied Physics, 13(9):2064–2069, November 2013. doi:10.1016/j.cap.2013.09.011.DOI
- [25]Julia Purtov, Andreas Verch, Peter Rogin, and René Hensel. Improved development procedure to enhance the stability of microstructures created by two-photon polymerization. Microelectronic Engineering, 194:45–50, July 2018. doi:10.1016/j.mee.2018.03.009.DOI
- [26]Maura Power, Antoine Barbot, Florent Seichepine, and Guang-Zhong Yang. Bistable, Pneumatically Actuated Microgripper Fabricated Using Two-Photon Polymerization and Oxygen Plasma Etching. Advanced Intelligent Systems, 5(4):2200121, 2023. doi:10.1002/aisy.202200121.DOI
- [27]G. Seniutinas, A. Weber, C. Padeste, I. Sakellari, M. Farsari, and C. David. Beyond 100 nm resolution in 3D laser lithography — Post processing solutions. Microelectronic Engineering, 191:25–31, May 2018. doi:10.1016/j.mee.2018.01.018.DOI
- [28]Darija Astrauskytė, Karolis Galvanauskas, Darius Gailevičius, Mantas Drazdys, Mangirdas Malinauskas, and Lina Grinevičiūtė. Anti-Reflective Coatings Produced via Atomic Layer Deposition for Hybrid Polymer 3D Micro-Optics. Nanomaterials, 13(16):2281, January 2023. doi:10.3390/nano13162281.DOI
- [29]Junning Zhang, Haibo Ding, Xiaojiang Liu, Hongcheng Gu, Mengxiao Wei, Xiaoran Li, Shengnan Liu, Sen Li, Xin Du, and Zhongze Gu. Facile Surface Functionalization Strategy for Two-Photon Lithography Microstructures. Small, 17(34):2101048, 2021. doi:10.1002/smll.202101048.DOI
- [30]Koen Vanmol, Al Ameen Abdul Nazar, Hugo Thienpont, Francesco Ferranti, and Jürgen Van Erps. Fabrication of multilevel metalenses using multiphoton lithography: From design to evaluation. Optics Express, 32(6):10190–10203, March 2024. doi:10.1364/OE.514237.DOI
- [31]Leander Siegle, Simon Ristok, and Harald Giessen. Complex aspherical singlet and doublet microoptics by grayscale 3D printing. Optics Express, 31(3):4179–4189, January 2023. doi:10.1364/OE.480472.DOI
- [32]Luigi Rovati, Paola Fabbri, Luca Ferrari, and Francesco Pilati. Construction and evaluation of a disposable pH sensor based on a large core plastic optical fiber. Review of Scientific Instruments, 82(2):023106, February 2011. doi:10.1063/1.3541795.DOI
- [33]Tao Han, Cheng Zhang, Hui Yu, and Jinghong Li. A disposable fiber-optic plasmonic sensor for chemical sensing. Analytical Biochemistry, 696:115672, January 2025. doi:10.1016/j.ab.2024.115672.DOI
- [34]Gligor Djogo, Jianzhao Li, Stephen Ho, Erden Ertorer, and Peter R. Herman. Self-Aligning Sockets for Packaging Multicore Fibers to Photonic Integrated Circuits. Journal of Lightwave Technology, 42(15):5356–5361, August 2024. doi:10.1109/JLT.2024.3391919.DOI
- [35]Yilin Xu, Pascal Maier, Mareike Trappen, Philipp-Immanuel Dietrich, Matthias Blaicher, Rokas Jutas, Achim Weber, Torben Kind, Colin Dankwart, Jens Stephan, Andreas Steffan, Amin Abbasi, Padraic Morrissey, Kamil Gradkowski, Brian Kelly, Peter O’Brien, Wolfgang Freude, and Christian Koos. 3D-printed facet-attached microlenses for advanced photonic system assembly. Light: Advanced Manufacturing, 4(2):77–93, November 2023. doi:10.37188/lam.2023.003.DOI
- [36]Parvathi Nair Suseela, Jonathan Trisno, Hongtao Wang, and Joel K. W. Yang. 3D printed fiber sockets for plug and play micro-optics. International Journal of Extreme Manufacturing, 3(1):015301, November 2020. doi:10.1088/2631-7990/abc674.
- [37]Lukas Novotny and Bert Hecht. Principles of Nano-Optics. Cambridge University Press, Cambridge, 2 edition, 2012. doi:10.1017/CBO9780511794193.
- [38]IQS nano. ResiQ PHOTORESINS. URL: https://iqsnano.com/wp-content/uploads/2025/06/IQS-Nano_Resins.pdf.
- [39]Seán O’Halloran, Abhay Pandit, Andreas Heise, and Andrew Kellett. Two-Photon Polymerization: Fundamentals, Materials, and Chemical Modification Strategies. Advanced Science, 10(7):2204072, 2023. doi:10.1002/advs.202204072.DOI
- [40]Kristian Hagsted Rasmussen, Stephan Sylvest Keller, Flemming Jensen, Anders Michael Jorgensen, and Ole Hansen. SU-8 etching in inductively coupled oxygen plasma. Microelectronic Engineering, 112:35–40, December 2013. doi:10.1016/j.mee.2013.05.011.DOI
- [41]Veronika Novotna, Josef Horak, Martin Konecny, Veronika Hegrova, Ondrej Novotny, Zdenek Novacek, and Jan Neuman. AFM-in-SEM as a Tool for Comprehensive Sample Surface Analysis. Microscopy Today, 28(3):38–46, May 2020. doi:10.1017/S1551929520000875.DOI
- [42]Thorlabs · FG105UCA Multimode Fiber. https://www.thorlabs.com/item/FG105UCA.