Investigation of the Pressure Dependent Physical Properties of MAX Phase Ti2AlX (X = B, C, and N) Compounds: A First-Principles Study

Abstract

The physical properties and their pressure dependence of recently synthesized Ti2AlX (X = B, C, and N) MAX phases are investigated for the very first time applying density functional theory (DFT).

Introduction

The MAX phases are considered as a class of solids with the chemical formula Mn+1AXnM_{n+1}AX_{n} (n=1n = 1-3) belonging to a family of ternary borides, carbides, and nitrides. Here, “M” is an early transition metal, “A” is an A-group element (mainly III A and IV A), and “X” is either the element B or C or N [1, 2, 3]. The MAX phase is classified into three groups based on the n value, viz. 211, 312, and 413. MAX compounds feature an excellent set of properties of both metal and ceramic, which bridges the metal-ceramic gap. The growing interest in the MAX phase over the last few decades is attributed to their alluring properties, including light weight (low density), high melting point, exceptionally damage tolerant behavior at room temperature, excellent conductivity (both thermal and electrical), resistance to thermal shock and chemical attack, high fracture toughness, plastic and high oxidation resistance at high-temperature conditions, self-healing cracks, relatively low thermal expansion coefficient (TEC) of < 10×10−6 ∘C−110\times10^{-6}\,^\circ\mathrm{C}^{-1}, radiation tolerance, and easy machinability [2, 3, 4, 5, 6, 7, 8]. These features make MAX phase materials compatible with a wide range of industrial and technological applications such as in Li-ion batteries, sliding electrical contacts, wear and corrosion-resistant coatings, superconducting materials, spintronics, and the nuclear shielding sector [9, 10].

Ti-based 211 MAX phase compounds such as Ti2AlBTi_2AlB, Ti2AlCTi_2AlC, and Ti2AlNTi_2AlN are reported to have significant potential for applications. Among those, Ti2AlBTi_2AlB is a theoretically predicted new phase [9, 11] that has not yet been experimentally confirmed. Some physical properties of Ti2AlBTi_2AlB, such as mechanical, electronic, acoustic velocities, Debye temperature, minimum thermal conductivity, and phonon dynamics have been studied at ambient and only at a rudimentary level [9, 11]. However, Ti2AlCTi_2AlC and Ti2AlNTi_2AlN have already been experimentally synthesized [7, 12, 13], and some theoretical studies have been reported [11, 14, 15, 16, 17]. Ti2AlCTi_2AlC has already attracted attention from the industry due to its exotic behavior such as it is reported to exhibit excellent oxidation resistance [18], good TBC [3] potential, brittle-to-ductile transition at 1050 °C [18], sufficient damage tolerance to irradiations [19], high yield points and significant plasticity at temperatures as high as 1300°C in air [6]. The TEC of Ti2AlCTi_2AlC and Ti2AlNTi_2AlN are within 8.2×10−68.2\times10^{-6} and 8.8×10−6 ∘C−18.8\times10^{-6}\,^\circ\mathrm{C}^{-1}, respectively, in the temperature range from 25 °C to 1300 °C [5]. The electrical conductivity of Ti2AlCTi_2AlC and Ti2AlNTi_2AlN are 2.7×1062.7\times10^6 and 4×106 (Ωm)−14\times10^6\,(\Omega\mathrm{m})^{-1}, respectively, at room temperature [5, 20]. Some other physical properties of Ti2AlCTi_2AlC and Ti2AlNTi_2AlN have also been studied employing ab-initio calculations in the ground state [11, 14, 16, 20, 21, 22]. Overall, only a few studies on Ti2AlXTi_2AlX (X=BX = B, C, and N) materials have been conducted so far, both experimentally and theoretically [5, 11]. Surprisingly, a combination of physical properties and their responses to pressure and temperature have not been comprehensively explored, either experimentally or theoretically. A systematic study of these materials is therefore necessary. Thus, the prime objective of this article is to explore the physical properties of the Ti-based MAX phase Ti2AlXTi_2AlX (X=BX = B, C, and N) extensively under hydrostatic pressure up to 10 GPa by employing the density functional theory (DFT). Pressure is a clean tuning parameter to alter the physical properties of solids. We have increased the pressure from 0 GPa, in 2 GPa increments, up to 10 GPa. We also studied the effect of temperature on lattice thermal conductivity.

The manipulation of solids through the application of pressure, temperature, electric or magnetic fields, and variations in composition via doping and substitution can bring about significant modifications in the physical properties of these materials. This is particularly important as certain materials require changes in their properties to enhance their suitability for commercial applications. A recent area of research interest involves the investigation of the effects of applying pressure specifically on MAX phases [23, 24, 25]. The general response of MAX phase materials to pressure includes structural, mechanical, electronic, superconducting, and magnetic transitions, as well as increase in the superconducting transition temperature; all of which occurs at specific pressures. Additionally, many other physical parameters such as density, hardness (chemical bonding), machinability, acoustic velocities, melting temperature, Debye temperature, and thermal conductivity vary with pressure. This research, thus, has the potential to uncover new insights and applications for these materials.

The rest of this manuscript proceeds along the following outline: § 2 contains a brief description of the computational methodology. § 3 includes an in-depth investigation of the physical properties of Ti2_2AlX (X = B, C, and N) along with their possible implications. Finally, in § 6, we summarized the key findings and draw conclusions from this work.

Computational scheme

The first-principles calculations were carried out using the density functional theory [26, 27] as contained in the CAmbridge Serial Total Energy Package (CASTEP) code [28]. The electronic valence states for Ti, Al, B, C, and N elements are taken as 3s2 3p6 3d2 4s13s^{2}\ 3p^{6}\ 3d^{2}\ 4s^{1}, 3s2 3p13s^{2}\ 3p^{1}, 2s2 2p12s^{2}\ 2p^{1}, 2s2 2p22s^{2}\ 2p^{2}, and 2s2 2p32s^{2}\ 2p^{3}, respectively. The exchange–correlation energy was evaluated using the functional called generalized gradient approximation (GGA) incorporating the Perdew-Burke-Ernzerhof for solids (PBEsol) scheme [29]. The interaction between the valence electrons and ion cores was modeled with the Vanderbilt-type ultrasoft pseudopotential [30]. The optimized (minimum total energy and internal forces) structure of the studied MAX phases was found by applying the Limited-memory Broyden–Fletcher–Goldfarb–Shanno (LBFGS) minimization algorithm [31]. The plane-wave cut-off energy was set at 550 eV for Ti2_2AlX (X = B, C, and N). The irreducible Brillouin zone was sampled with a 16×16×416 \times16 \times4 kk-grid on the Monkhorst–Pack scheme [32]. Various tolerance parameters, during computations for all three compounds, were set to be 5×10−65 \times10^{-6} eV/atom for energy, maximum lattice point displacement within 5×10−45 \times10^{-4} Å, maximum ionic force within 10−210^{-2} eVÅ−1^{-1}, maximum stress within 0.02 GPa and smearing width of 0.1 eV. A kk-point mesh of 24×24×624 \times24 \times6 was used for the Fermi surface construction since it demands denser kk-mesh. Moreover, the density functional perturbation theory (DFPT) finite displacement method (FDM) [33, 34] has been employed to calculate phonon dispersion spectra (PDS) and total phonon density of states (PHDOS). All the DFT simulations were performed at the default temperature (0 K) and at different hydrostatic pressures in GPa.

The second-order elastic constant (CijC_{ij}) of the studied compounds were obtained employing the stress–strain method [35]. In the case of the hexagonal structure, there are six independent elastic stiffness constants: C11C_{11}, C33C_{33}, C44C_{44}, C12C_{12}, C66C_{66}, and C13C_{13}. Lattice dynamical properties such as phonon dispersion and phonon density of states were calculated with a conventional cell of each system using the finite displacement method. In these calculations, kk-point mesh of 9×9×29 \times9 \times2, 9×9×29 \times9 \times2 (10×10×210 \times10 \times2), and 10×10×210 \times10 \times2 (8×8×28 \times8 \times2) was used for Ti2_2AlB, Ti2_2AlC, and Ti2_2AlN at 0 GPa (10 GPa). A cut-off energy of 350 eV was set for all three compounds.

The frequency-dependent optical spectra are derived from their complex dielectric function given by ε(ω)=ε1(ω)+iε2(ω)\varepsilon(\omega) = \varepsilon_{1}(\omega) + i\varepsilon_{2}(\omega). The imaginary part ε2(ω)\varepsilon_{2}(\omega) has been obtained from the following formula:

ε2(ω)=2e2πΩε0∑k,ν,c∣⟨ψkc∣u^⋅r⃗∣ψkν⟩∣2δ(Ekc−Ekν−E)(1)\varepsilon_{2}(\omega) = \frac{2e^{2}\pi}{\Omega\varepsilon_{0}} \sum_{k,\nu,c} \left|\langle\psi_{k}^{c}|\hat{u}\cdot\vec{r}|\psi_{k}^{\nu}\rangle\right|^{2}\delta(E_{k}^{c}-E_{k}^{\nu}-E) \tag*{(1)}

here, ω\omega is the frequency of the incident photon, Ω\Omega is the unit cell volume, ee is the electronic charge, ε0\varepsilon_0 defines the permittivity of the free space, u^\hat{u} gives the polarization of the incident electric field, and r⃗\vec{r} is the position vector. Besides, Ψkc\Psi_k^c and Ψkv\Psi_k^v refer to the conduction and valence band wave functions at a given wave-vector kk, respectively. This formula needs inputs from the electronic band structure calculations. With the help of Kramers-Kronig relationship, the real part ε1(ω)\varepsilon_1(\omega) has been evaluated from its corresponding imaginary part ε2(ω)\varepsilon_2(\omega) as [36]:

ε1(ω)=1+2πP∫0∞ω′ε2(ω′)ω′2−ω2 dω′(2)\varepsilon_1(\omega)=1+\frac{2}{\pi}P\int_0^\infty\frac{\omega'\varepsilon_2(\omega')}{\omega'^{2}-\omega^2}\,d\omega' \tag*{(2)}

here, PP signifies the principal value of the integral.

Once ε(ω)\varepsilon(\omega) is known, all the other optical parameters, such as refractive index N(ω)N(\omega), reflectivity R(ω)R(\omega), optical conductivity σ(ω)\sigma(\omega), absorption coefficient α(ω)\alpha(\omega), and energy loss-function L(ω)L(\omega) can be deduced from it using standard formulae [37, 38].

Results and analysis

Optimized structure and pressure dependency

Figure 1 displays the optimized unit cell structure of Ti2AlX\mathrm{Ti}_2\mathrm{Al}X (X=BX = \mathrm{B}, C\mathrm{C}, and N\mathrm{N}). An edge-shared octahedral of TiX\mathrm{Ti}X is sandwiched with Al atomic sheets. Like all the MAX phases, Ti2AlX\mathrm{Ti}_2\mathrm{Al}X possesses a hexagonal nanolayered crystal structure with P63/mmcP6_3/mmc (#194) space group symmetry [11]. The unit cell of Ti2AlX\mathrm{Ti}_2\mathrm{Al}X contains a total of eight atoms, including four Ti, two Al, and two XX atoms, corresponding to two formula units. Wyckoff positions for Ti, Al, and XX (B, C, and N) atoms are 4f4f (1/3, 2/3, zz), 2d2d (1/3, 2/3, 3/4), and 2a2a (0, 0, 0), respectively, where zz equals 0.087 [9]. Our simulated lattice parameters, volume, and density for all the studied compounds at ambient pressure are in very good agreement with previous experimental [5, 6, 39] and theoretical studies [9, 11, 40].

Unit cell structure of Ti2AlX MAX phases

Figure 1. The unit cell structure of Ti2AlX\mathrm{Ti}_2\mathrm{Al}X (X=BX = \mathrm{B}, C\mathrm{C}, and N\mathrm{N}) MAX phases.

The pressure-dependent lattice parameters, their ratio (c/ac/a), volume, and density data at 0 K up to 10 GPa with a 2 GPa step are collected and presented in Figure 2. At ambient pressure, lattice constants and volumes decrease as we go from B to N (B→\toC→\toN) in accordance with the mass of the anions, while densities increase. This sequence is maintained under applied pressure. Therefore, as the pressure increases, the bond length shortens and the interaction between the elements (Ti, Al, and X) becomes stronger. The value of the c/ac/a ratio is a significant indicator of whether our materials are kinking nonlinear elastic (KNE) solids or not [41]. The c/ac/a ratio for all the studied compounds is greater than 4. Therefore, we can surmise that our materials are KNE. Ti2_2AlC has been already confirmed as a KNE material through experimental work by B. Poon et al. [42]. The c/ac/a ratio is much higher for Ti2_2AlN than for Ti2_2AlB and Ti2_2AlC. All the compounds are more compressible along cc-axis than aa-axis (see Figure 2a, Figure 2b, and Figure 2c) indicating a decrease in interlayer distance along zz-axis. No evidence of pressure-induced phase transition was found for all the compounds, as confirmed by the monotonous changes in structural parameters under pressure (see Figure 2).

Figure 2. The pressure-dependent lattice parameters (aa and bb), c/ac/a ratio (a-c), volume (d), and density (e).

Mechanical and elastic properties

Information regarding the second-order elastic constants (CijC_{ij}) are important for exploring the mechanical behavior of materials and determining their potential for practical applications [43, 44, 45]. Elastic stiffness constants of solids change with both pressure and temperature. The obtained pressure dependent elastic constants are shown in Figure 3(a, Figure 3b, and Figure 3c). The independent elastic constants for Ti2_2AlX at ambient pressure align well with those reported in the literature [11, 16]. All the compounds meet the Born stability criterion [46]: C11−∣C12∣>0C_{11} - \lvert C_{12} \rvert> 0, (C11+C12)C33−2C132>0(C_{11} + C_{12})C_{33} - 2C_{13}^{2} > 0, C44>0C_{44} > 0, indicating that these MAX compounds are mechanically stable at ambient pressure. Moreover, the mechanical stability criteria for hexagonal crystal under pressure (PP) are as follows [46]:

Variation in the elastic constants and moduli with pressure for Ti2AlB, Ti2AlC, and Ti2AlN MAX phases

Figure 3. Variation in the elastic constants and moduli with pressure for Ti2AlBTi_2AlB (a, d), Ti2AlCTi_2AlC (b, e), and Ti2AlNTi_2AlN (c, f) MAX phases.

C~44>0,C~11>∣C~12∣,C~33(C~11+C~12)>2C~132(3)\widetilde{C}_{44} > 0, \widetilde{C}_{11} > \lvert\widetilde{C}_{12} \rvert, \widetilde{C}_{33}\left(\widetilde{C}_{11} + \widetilde{C}_{12}\right) > 2\widetilde{C}_{13}^{2} \tag*{(3)}

where, C~ii=Cii−P (i=1,3)\widetilde{C}_{ii}=C_{ii}-P\ (i=1,3) and C~1i=C1i+P (i=2,3)\widetilde{C}_{1i}=C_{1i}+P\ (i=2,3)

All the elastic constants of the studied compounds satisfy the stability criteria under pressure. Therefore, all the compounds are mechanically stable up to 10 GPa.

The resistance to linear compression and atomic bonding strength along the [100] and [1] directions is directly related to C11C_{11} and C33C_{33}, respectively [47]. Ti2_2AlN exhibits greater resistance to both the linear compression and atomic bonding strength along the aa- and cc-axis, respectively than Ti2_2AlB and Ti2_2AlC. Unlike Ti2_2AlB, the considerably larger values of C11C_{11} than C33C_{33} for both Ti2_2AlC and Ti2_2AlN indicate that the atomic bonds along [100] are stronger compared to that along [1] direction. On the other hand, the resistance to shape change is represented by C12C_{12}, C13C_{13}, and C44C_{44}. C44C_{44} represents the resistance to shear deformation with respect to tangential stress applied to the (100) plane in the [10] direction of the compound [48]. The value of C44C_{44} is also related to the valence electron density in the material; the higher the valence electron density, the higher the C44C_{44}. The stiffness order of the compounds under pressure is Ti2_2AlN >> Ti2_2AlC >> Ti2_2AlB. Based on the definition of C12C_{12} [44], Ti2_2AlB exhibits greater shear resistance in the (100) plane along the aa-axis than the other two materials. Furthermore, it is evident that CijC_{ij} values for Ti2_2AlX increase almost linearly with applied pressure. However, the rates of increase for C11C_{11} and C33C_{33} are faster than those for C12C_{12}, C13C_{13}, and C44C_{44} (see Figure 3a-Figure 3c). Each of the elastic constant individually influences the properties of the materials, which we will discuss in the next sections.

Different elastic moduli are calculated from the CijC_{ij} via the Voigt–Reuss–Hill (VRH) approximations [49, 50, 51]. The bulk (BVB_V, BRB_R, and BHB_H), shear (GVG_V, GRG_R, and GHG_H), and Young’s (EVE_V, ERE_R, and EHE_H) moduli of the materials were estimated using the VRH formulae [47]. The Bulk modulus (BB), shear modulus (GG), and Young’s modulus (EE) of the Ti2AlXTi_2AlX MAX phases from 0 to 10 GPa pressure range are displayed in Figure 3d-Figure 3f. The BB and GG of the material represent resistance to volume changes (bond length) and plastic deformation (bond angle) under external stress. The lower value of GG compared to BB for all studied materials suggests that plasticity will dominate their mechanical strength up to 10 GPa. The EE value of a material can quantify its stiffness and ability to resist thermal shock [52]. A larger EE value indicates greater stiffness, higher melting temperature, and lower resistance to thermal shock. Therefore, Ti2AlNTi_2AlN is much stiffer and has lower thermal shock resistance than Ti2AlBTi_2AlB and Ti2AlCTi_2AlC MAX phases, making them (Ti2AlBTi_2AlB and Ti2AlCTi_2AlC) more suitable as thermal barrier coating (TBC) system. All the elastic moduli for the compounds at 0 GPa are in good agreement with prior literature [11].

All the elastic moduli increase systematically with pressure and show no anomalies, corresponding to the phase stability of all three materials. Furthermore, a linear increase in moduli with pressure is observable in all the crystals, although their values vary, indicating the absence of any phase transitions. The pressure derivative bulk modulus (B′B') for all three compounds is simulated and displayed in Figure 4a. B′B' increases as we move from B to N of Ti2AlXTi_2AlX (XX = B, C, and N).

Six panels showing the pressure derivate of bulk modulus, machinability, Pugh’s ratio, Poisson’s ratio, elastic Grüneisen parameter, and microhardness of Ti2AlX

Figure 4. The pressure derivate of bulk modulus (a), machinability (b), Pugh’s ratio (c), Poisson’s ratio (d), elastic Grüneisen parameter (e), and microhardness (f) of Ti2_2AlX.

The assessment of the machinability index, a useful performance parameter of materials, has drawn significant interest in the development of manufacturing processes for complex cutting geometries of materials and tools [44]. The machinability index of a material is defined by μM=B/C44\mu_{\mathrm{M}} = B/C_{44} [43]. The pressure-dependent μM\mu_{\mathrm{M}} of Ti2_2AlX is illustrated in Figure 4b. At ambient pressure, the μM\mu_{\mathrm{M}} for Ti2_2AlB is maximum and decreases as we move to a higher atomic number of X (C→\toN), which is also aligned with C44C_{44} value of the compounds. The machinability of the studied compounds increases with pressure. All the compounds possess a medium level of machinability comparable to many other well-known MAX phases [53].

Pugh stated that the ratio of GG and BB (G/BG/B) is a measure of intrinsic ductility and brittleness. Pugh's ratio also addresses the interplay between brittle failure and shear failure within the material. Materials that deform through shear or tension under loading conditions are termed intrinsically ductile or brittle, respectively [54]. For brittle and ductile materials, the value of G/BG/B is higher and lesser than 0.57, respectively. Figure 4c displays that both Ti2_2AlC and Ti2_2AlN are intrinsically brittle, failing under tensile stress, and they also retain their brittleness across a range of pressures considered here. On the contrary, Ti2_2AlB exhibits intrinsic brittleness and shows a brittle-to-ductile transition for pressures above 6 GPa. Although a direct comparison between experimental and theoretical measures of ductility and brittleness is not straightforward, elongation and reduction of area critically depend on several factors, such as temperature, grain size, processing route (e.g., annealed vs. as-fabricated), impurity concentrations, and strain rate. The linear response of the studied materials under applied pressure indicates the absence of any kind of fracture.

Another well-known parameter that characterizes the mechanical behavior (compressibility, brittleness/ductility, and bonding nature/force) of materials is the Poisson’s ratio (ν\nu). This parameter is estimated using the following expression: ν=(3B−2G)/2(3B+G)\nu= (3B - 2G)/2(3B + G) [43]. The values of ν\nu range between −1.0 and 0.5 (viscoelastic) for all elastically stable materials. Materials exhibit brittleness if ν\nu is less than 0.26 and ductility if ν\nu is greater than 0.26 [55]. Moreover, ν\nu represents the lower (0.25) and upper (0.50) limits for central-force solids [47]. The borderline values of ν\nu for covalent and ionic materials are 0.10 and 0.25, respectively [47]. The calculated Poisson’s ratio suggests that all three MAX phase nanolaminates are brittle in the ground state with non-central inter-atomic forces and they are significantly covalently bonded at ambient pressure to up to 8 GPa (see Figure 4d). With a gradual increase in ν\nu as pressure rises, there is an implication of increased plasticity. Additionally, there is a brittle-to-ductile transition of Ti2AlB\mathrm{Ti_2AlB} at approximately 8 GPa. The findings are also consistent with Pugh’s ratio analysis. The lower ν\nu of a material is associated with stronger and more directional covalent bonding and higher hardness (see Figure 4d, and f) [56]. Therefore, Ti2AlC\mathrm{Ti_2AlC} should have the strongest covalent bonding out of all three compounds with a sequence of Ti2AlC>Ti2AlN>Ti2AlB\mathrm{Ti_2AlC} > \mathrm{Ti_2AlN} > \mathrm{Ti_2AlB}.

The Grüneisen parameter for solids is a significant dimensionless thermodynamic parameter that has both pressure and temperature dependencies. This parameter can explain various physical phenomena such as thermal conductivity, thermal expansion, specific heat, elastic properties, and acoustic wave attenuation. Out of five Grüneisen parameters, we have estimated the elastic Grüneisen parameter (γe\gamma_{\mathrm{e}}) for all three compounds using Poisson’s ratio [45, 57]:

γe=3(1+ν)2(2−3ν)\gamma_{\mathrm{e}} = \frac{3(1+\nu)}{2(2-3\nu)}. Figure 4e shows the relationship between γe\gamma_{\mathrm{e}} and applied pressure. The value of γe\gamma_{\mathrm{e}} systematically increases with pressure. The order of γe\gamma_{\mathrm{e}} and kphk_{\mathrm{ph}} (phonon thermal conductivity) for Ti2AlX\mathrm{Ti_2AlX} are in good agreement with the concept presented in an earlier work [47].

Potential materials for applications such as cutting tools, wear-resistant coatings, tribological coatings, solid lubricating coating, and heavy-duty products are chosen based on their hardness [44, 58, 59, 60]. There are several macroscopic models for hardness calculation, and their efficiency depends on the crystal structure. These formulae have been summarized in our previous works [44, 47]. The Vickers micro-hardness of hexagonal Ti2AlX\mathrm{Ti_2AlX} compounds both at ambient and under pressure, is estimated from the elastic moduli using the formula [47, 61]:

H=2(k2G)0.585−3(4)H = 2(k^2G)^{0.585} - 3 \tag*{(4)}

here, k(=G/B)k (= G/B) is the Pugh’s ratio and the moduli are in GPa. The estimated hardness of the compounds is displayed in Figure 4f. The studied materials possess moderate hardness in the order: Ti2AlC>Ti2AlN>Ti2AlB\mathrm{Ti_2AlC} > \mathrm{Ti_2AlN} > \mathrm{Ti_2AlB}. The hardness of Ti2AlX\mathrm{Ti_2AlX} decreases with increasing applied pressure, the decrease rate follows the hardness order, in contrast to their elastic moduli. The reported values here are rough predictions since there are many intrinsic and extrinsic factors that affect the hardness. Furthermore, variety of hardness measures exists giving different values. Solid lubricants are divided into two broad categories based on hardness: soft (H < 10 GPa) and hard (H >10 GPa) [60]. Solid lubricants are critically important for harsh operating conditions where liquid lubricants fail, such as at high vacuum, aerospace, high-speeds, high loads, and at very low or high temperatures.

Cauchy pressure (PCP_{\mathrm{C}}) is another fundamental mechanical parameter that can explain brittleness/ductility and bonding nature. The PCP_{\mathrm{C}} for the studied materials (hexagonal) were estimated using the following expressions [62, 63, 64]:

PCa=(C13−C44) and PCb=(C12−C66)(5)P_C^a = (C_{13} - C_{44}) \text{ and } P_C^b = (C_{12} - C_{66}) \tag*{(5)}

where, PCaP_C^a and PCbP_C^b define the Cauchy pressure for the (100) and (001) planes, respectively. The estimated Cauchy pressures of the compounds are presented in Figure 5(a, Figure 5b). The value of PCP_C is positive for metallic bonding. Besides, materials are expected to exhibit more directionality, bonding immobility, and brittleness if PCP_C is negative [43]. The presence of metallic-like bonding along cc-direction (positive PCbP_C^b) in Ti2_2AlB is an indicator of being more conducting than the other two (see Figure 11d,Figure 11e and 12a). On the other hand, PCaP_C^a is more negative for Ti2_2AlB than Ti2_2AlC and Ti2_2AlN with the sequence: Ti2_2AlC > Ti2_2AlN > Ti2_2AlB. Pettifor stated that the positive and negative PCP_C of a material reflect metallic (non-directional) and angular bonding, respectively [62].

Cauchy pressure and universal anisotropy index of Ti2AlX as a function of pressure

Figure 5. The Cauchy pressure (a, b) and universal anisotropy index (c) of Ti2_2AlX (XX = B, C, and N) as a function of pressure.

Figure 11. (a) Debye temperature, (b) melting temperature, (c) thermal expansion coefficient, and (d,e) minimum thermal conductivity of the materials as a function of hydrostatic pressure.

Studying mechanical anisotropy of materials is crucial for their application potentials in engineering sciences. Mechanical anisotropy controls several physical phenomena in solids (metal, glass, ceramics, etc.), such as micro-crack formation and its motion, the development of plastic deformation, and the relaxation of plasticity in thin-film materials. Therefore, we have studied the mechanical anisotropy of the MAX compounds under applied hydrostatic pressure. The universal anisotropy index (AUA^U), one of the most widely used anisotropy parameter, for the materials can be estimated from the following formula [65]:

AU=5GVGR+BVBR−6≥0(6)A^U = 5\frac{G_V}{G_R} + \frac{B_V}{B_R} - 6 \ge0 \tag*{(6)}

here, BVB_V, GVG_V, BRB_R, and GRG_R represent the Voigt and Reuss approximated elastic moduli [47]. The Voigt (V) and Reuss (R) approximations define the upper and lower limits of BB and GG of a material, respectively. AU=0A^U = 0 for locally isotropic single crystals, whereas the degree of anisotropy extends with the deviation from zero. The AUA^U of Ti2_2AlX as a function of applied pressure is depicted in Figure 5c. At ambient pressure, all the studied compounds are anisotropic with the order: Ti2_2AlB > Ti2_2AlN > Ti2_2AlC. The mechanical anisotropy of Ti2_2AlN increases more rapidly with pressure than Ti2_2AlB and Ti2_2AlC. This implies that the chemical bonding properties are most sensitive to pressure in this compound.

To illustrate the anisotropy of Young’s modulus (EE), compressibility (β\beta), Shear modulus (GG), and Poisson’s ratio (ν\nu) of the crystals at 0 GPa and under 10 GPa, 3D graphical visualization are also studied with the help of ELATE program [66]. The elastic stiffness matrixes, required as input, are estimated using the CASTEP code. Perfectly spherical shape is the manifestation of the isotropic nature of crystals. The 3D graphical representations of EE, β\beta, GG, and ν\nu for the compounds are displayed in Figure 6-Figure 7. The maximum and minimum points of the parameters (GG and ν\nu) are represented by solid transparent blue and green colors, respectively. Ti2_2AlC exhibits the least anisotropy in ν\nu at 0 GPa. The Poisson’s ratio anisotropy of Ti2_2AlB increases more than Ti2_2AlC and Ti2_2AlN under 10 GPa which is also in agreement with the AuA^{u} study (see Figure 5c). All the four parameters exhibit isotropy along [100] direction at both 0 and 10 GPa. We can conclude that the materials possess anisotropy in the following order: β<E<G<ν\beta< E < G < \nu.

Directional dependence of Young’s modulus and shear modulus of Ti2AlX

Figure 6. Directional dependence of Young’s modulus (EE), and shear modulus (GG) of Ti2_2AlX (XX = B, C, and N) at 0 and 10 GPa.

Directional dependence of compressibility and Poisson’s ratio of Ti₂AlX

Figure 7. Directional dependence of compressibility (β\beta), and Poisson’s ratio (ν\nu) of Ti2_2AlX (X=BX = \mathrm{B}, C\mathrm{C}, and N\mathrm{N}) at 0 and 10 GPa.

Electron density difference

The interatomic bonding nature in a material can be explored from the electron density difference (EDD) around the different elements in the material, which displays the accumulation and depletion of charges around the elements. We have calculated EDD for Ti2_2AlX at 0 GPa and 10 GPa, as displayed in Figure 8. The color scale for each compound’s map illustrates the electron density difference. For Ti2_2AlB and Ti2_2AlC, the red and green color indicates high and low charge (electron) density, respectively, whereas vice versa for Ti2_2AlN. Maximum EDD around X atoms for all the studied compounds illustrates that electrons/charges are accepted by this element. On the other hand, the blue color (red for Ti2_2AlN) Ti and Al atoms signify electrons are donated by them. The covalent bonding between Ti-X and Al-X atoms is confirmed. Out of the three compounds, Ti2_2AlC possesses the least EDD value. There is a clear directional dependency of EDD for all the studied compounds.

Electron density difference maps for Ti₂AlB, Ti₂AlC, and Ti₂AlN under 0 GPa and 10 GPa hydrostatic pressures

Figure 8. The electron density difference (A˚−3\mathring{\mathrm{A}}^{-3}) maps for (a) Ti2_2AlB, (b) Ti2_2AlC, and (c) Ti2_2AlN in different planes under 0 GPa and 10 GPa hydrostatic pressures.

Acoustic properties

The transverse (shear), longitudinal, and average sound velocities through the studied materials have been estimated using well-known formulae from the literature [67, 68]. The hydrostatic pressure dependence of the velocities of the acoustic waves propagating through the compounds is also studied, as displayed in Figure 9. In general, the longitudinal sound velocity is greater than the transverse one. Lower values of νt\nu_t compared to νl\nu_l in all the three compounds indicate that the near-surface information will be dominated by transverse wave. Acoustic velocity through a material is directly related to its density, uniaxial compression strength, Young’s modulus, and thermal conduction ability. The longitudinal sound wave velocity increases more rapidly with pressure than the other two wave velocities for all the studied compounds which also correlates with the other parameters’ response with pressure.

The transverse, longitudinal, and average sound velocities for Ti₂AlX compounds

Figure 9. The transverse (vtv_t), longitudinal (vlv_l), and average (vav_a) sound velocities for Ti₂AlX (X=X = B, C, and N) compounds under applied pressure.

Phonon and vibrational analyses

Both the electrons and phonons in a material conduct heat. In solids, acoustic phonon and optical phonon are not independent but interact with each other like, acoustic-acoustic phonon, acoustic-optical phonon, and optical-optical phonon. Figure 10 shows the calculated phonon dispersion with their corresponding total and partial density of states (in the right panel of each diagram) in the BZ of Ti₂AlB, Ti₂AlC, and Ti₂AlN, at ambient and under 10 GPa pressure. The absence of any negative energy phonon branch for the studied compounds ensures their dynamical stability both at 0 and 10 GPa. In fact, we have found dynamical stability at all the pressures up to 10 GPa. A material with NN atoms per unit cell possesses 3 acoustic modes and (3N−3)(3N-3) optical modes. The eight atoms in the unit cell of Ti₂AlX indicates total of 24 vibrational modes, with 3 acoustic and 21 optical branches: 6E1u+3A2u+4E2u+2B1u+4E2g+2B2g+2E1g+A1g6E_{1u} + 3A_{2u} + 4E_{2u} + 2B_{1u} + 4E_{2g} + 2B_{2g} + 2E_{1g} + A_{1g}. The low-frequency region consists of one longitudinal mode (in-plane) and two transverse acoustic modes (one in-plane and one out-of-plane). Acoustic phonon modes dominate the transport of sound and thermal energy in crystals [44]. Coherent vibrations of atoms in a lattice outside their equilibrium position produce acoustic branches. The acoustic vibrational modes of Ti₂AlX correspond to the 2E1u2E_{1u} and A2uA_{2u} modes. Moreover, optical vibrational modes can both be transverse and longitudinal. Out of the 21 optical modes, 6 are infrared (IR)-active and 7 are Raman-active, while the rest are inactive to IR and Raman. These active modes are: 4E1u+2A2u+4E2g+2E1g+A1g4E_{1u} + 2A_{2u} + 4E_{2g} + 2E_{1g} + A_{1g}. The different phonon modes, both active and silent modes, of all the three compounds at ambient pressure are listed in Table 1. These mode frequencies will be useful for the experimental confirmation of the phases later on, especially for Ti₂AlB. The different phonon frequencies of optical branch around Γ\Gamma-point indicate the ionic bonding [22]. The phononic bandgap defines the frequency region where elastic waves through the material are inhibited. The splitting of optical branches (lower and upper) is due to the mass differences among atoms. The overlap/hybridization between acoustic and lower optical branches for all the compounds indicates absence of any phononic bandgap (elastic impedance) between these two branches. Dispersion of phonon modes is related with the bond lengths between atoms in the materials.

Phonon dispersion spectra and phonon density of states of Ti2AlB, Ti2AlC, and Ti2AlN under 0 GPa and 10 GPa hydrostatic pressure

Figure 10. The phonon dispersion spectra (PDS) and phonon density of states (PHDOS) of (a) Ti2AlB\mathrm{Ti}_2\mathrm{AlB}, (b) Ti2AlC\mathrm{Ti}_2\mathrm{AlC}, and (c) Ti2AlN\mathrm{Ti}_2\mathrm{AlN} under 0 GPa and 10 GPa hydrostatic pressure.

Theoretical Mode symmetryActivity (cm−1\mathrm{cm}^{-1})
RamanIR
Ti2AlB\mathrm{Ti}_2\mathrm{AlB}Ti2AlC\mathrm{Ti}_2\mathrm{AlC}Ti2AlN\mathrm{Ti}_2\mathrm{AlN}Ti2AlB\mathrm{Ti}_2\mathrm{AlB}Ti2AlC\mathrm{Ti}_2\mathrm{AlC}Ti2AlN\mathrm{Ti}_2\mathrm{AlN}
E1uE_{1u}––––––
E1uE_{1u}––––––
A2uA_{2u}––––––
E2uE_{2u}––––––
E2uE_{2u}––––––
B1uB_{1u}––––––
E2gE_{2g}139.190147.112147.997–––
E2gE_{2g}139.190147.112147.997–––
E1uE_{1u}–––163.086177.797185.265
E1uE_{1u}–––163.086177.797185.265
B2gB_{2g}––––––
E1gE_{1g}249.225276.293231.403–––
E1gE_{1g}249.225276.293231.403–––
E2gE_{2g}252.453147.112235.393–––
E2gE_{2g}252.453147.112235.393–––
A2uA_{2u}–––282.050317.871344.145
A1gA_{1g}315.822367.656366.615–––
B2gB_{2g}––––––
E2uE_{2u}––––––
E2uE_{2u}––––––
E1uE_{1u}–––578.355684.892614.821
E1uE_{1u}–––578.355684.892614.821
A2uA_{2u}–––592.401640.847559.393
B1uB_{1u}––––––

Table 1. Calculated values of Raman-active and infrared (IR) optical modes at the Γ\Gamma-point of Ti2AlX\mathrm{Ti}_2\mathrm{AlX} (X=BX = \mathrm{B}, C\mathrm{C}, and N\mathrm{N}) at 0 GPa.

Sharp peaks in total phonon density of states (PHDOS) indicate flat phonon dispersion. The total PHDOS in the higher optical branch displays sharp peaks as we move from B to N element. The broad peak in the PHDOS of Ti2AlB\mathrm{Ti}_2\mathrm{AlB} indicates non-localized phonon dispersion compared to the other two compounds. Partial PHDOS for all the compounds confirms that the acoustic and lower optical modes are dominated by vibration of both Ti and Al atoms. Contribution of Ti element is more significant than Al. On the other hand, high frequency optical modes (∼16\sim16 to ∼22\sim22 THz) are mainly generated from the lightest elements such as B, C, and N in the MAX compounds considered. The vibrational frequency of the elements in a material (assuming that the oscillations are harmonic) can be expressed as: ω=k/m\omega= \sqrt{k/m}; where, kk is the bond stiffness and mm is the mass of the element. The strong Ti-X bonding makes the frequency of X atoms much higher than that of the Ti and Al atoms. The heat capacity of a material is proportional to the PHDOS [69].

The phonon frequency for all the compounds increases with pressure. This is because the interaction between atoms becomes stronger as the interatomic distance decreases under pressure, leading to an increase in phonon frequency.

Thermo-physical parameters

The thermal behavior of MAX phases was studied from Debye temperature, melting temperature, lattice thermal conductivity, minimum thermal conductivity, and thermal expansion coefficient. All the thermal parameters of Ti2AlX\mathrm{Ti}_2\mathrm{AlX} (X=CX = \mathrm{C}, B\mathrm{B}, and N\mathrm{N}) studied here have been estimated from well-established formulae summarized elsewhere [43, 47, 67, 70, 71, 72].

Debye temperature

Studying Debye temperature (ΘD\Theta_{\mathrm{D}}) of a solid is important in the material selection process for various applications related to lattice vibrations. The ΘD\Theta_{\mathrm{D}} value reflects many key properties of a solid, such as the bonding strength between elements, vibrational energy (thermal, acoustic, optical), melting temperature, indentation hardness, isothermal compressibility, specific heat capacity, superconducting transition temperature, electron-phonon coupling constant, etc [47]. There are two types of lattice waves: acoustic and optical. The Debye temperatures of Ti2_2AlX (X = B, C, and N) MAX phases have been estimated using Anderson model given in the literature [67, 68]. The Debye temperature versus applied pressure for all three compounds is displayed in Figure 4e. A linear increase in ΘD\Theta_{\mathrm{D}} with applied pressures is observable for all the studied compounds, which is an indicator of thermodynamic stability of structures up to 10 GPa. The ΘD\Theta_{\mathrm{D}} of Ti2_2AlB is much lower than the other two compounds, which makes it more suitable as thermal barrier coating (TBC). The pressure response of ΘD\Theta_{\mathrm{D}} for the studied compounds follows the trend of elastic moduli, melting temperature, minimum thermal conductivity, and acoustic impedance.

Melting temperature

Melting temperature (TmT_{\mathrm{m}}) of solids is crucial for exploring potential materials for various industrial applications [47]. Figure 11b represents the effects of pressure on TmT_{\mathrm{m}} for Ti2_2AlB, Ti2_2AlC, and Ti2_2AlN. It is found that TmT_{\mathrm{m}} for all three compounds are above 1000 ºC and increases monotonically with pressure, which indicates their good thermal stability. Ti2_2AlC and Ti2_2AlN possess higher TmT_{\mathrm{m}} value as compared to Ti2_2AlB which is due to their relatively higher elastic constants and stronger atomic bondings. In addition, a high melting point arises from a high heat of fusion, a low entropy of fusion, or from a combination of both.

Thermal expansion coefficient

Materials go through dimensional (shape, area, and volume) changes under pressure, temperature, magnetic field, etc. Therefore, this has critical implications for materials used in industrial applications. Thermal expansion coefficient (TEC) for a material can quantify many phenomena, such as thermal conductivity, specific heat, entropy, and isothermal compressibility. Studying the TEC of materials is of interest for identifying potential materials for various applications in materials science including automotive, aerospace, railway lines/tracks, communication cables, anti-thermal shock system, electronic packaging, and spintronics [47]. The pressure effect on the TEC of the materials is studied here and displayed in Figure 11c. The order of α\alpha for the materials at ambient pressure is: Ti2_2AlB > Ti2_2AlC > Ti2_2AlN, with Ti2_2AlB exhibiting a much higher TEC than the other two materials. A linear decrease in TEC with increasing pressure has been observed for all three compounds.

Minimum thermal conductivity

The minimum thermal conductivity (kmink_{min}) of materials describe the lowest limit to lattice thermal conductivity at temperature above the Debye temperature. Both the temperature and pressure can manipulate kmink_{min} of a solid. The isotropic kmink_{min} of the studied materials is stimulated from two well-known models [73, 74]:

Cahill’s model: kmin=kB2.48n2/3(νl+2νt)(7)\text{Cahill’s model: } k_{min} = \frac{k_B}{2.48} n^{2/3}(\nu_l + 2\nu_t) \tag*{(7)}
Clarke model: kmin=kBνa(Vatomic)−2/3(8)\text{Clarke model: } k_{min} = k_B \nu_a (V_{atomic})^{-2/3} \tag*{(8)}

here, nn is the number of atoms per unit volume and VatomicV_{atomic} is the cell volume per atom. The estimated values of kmink_{min} as a function of pressure are displayed in Figure 11(d,Figure 11e). Both the models predict that Ti2_2AlB exhibits the lowest kmink_{min} among all three and their values increase with pressure. Similar trend is also found in ΘD\Theta_D and TmT_m. Moreover, Cahill’s model predicts larger kmink_{min} compared to Clarke model which is also observed for other materials [43, 47, 48].

Phonon thermal conductivity

Thermal conductivity in solids is the combination of electron and phonon thermal conductivity (kphk_{ph}). Both high and low phonon thermal conducing materials have industrial importance. Ultrahigh kphk_{ph} materials are reported to exhibit large phonon group velocity, long phonon lifetime and strong bonding [75]. Materials with lower kphk_{ph} show better thermoelectric behavior. For high temperature applications, a material should have a low thermal conductivity at higher operating temperature. Moreover, the decrease in intrinsic/extrinsic resistance to phonon-phonon and electron-phonon interactions in solids indicates decrease in kphk_{ph}. The lower value of kphk_{ph} indicates the presence of softer phonon modes. The kphk_{ph} of Ti2_2AlX (XX = C, B, and N) as function of temperature and pressure is estimated from well-known formulae reported in the literature [44, 71, 72] and displayed in Figure 12.

Pressure and temperature dependence of $k_{ph}$ for Ti$_2$AlB, Ti$_2$AlC, and Ti$_2$AlN MAX phases

Figure 12. The pressure and temperature dependence of kphk_{ph} of (a) Ti2_2AlB, (b) Ti2_2AlC, and (c) Ti2_2AlN MAX phases.

The kphk_{ph} value of the compounds at 0 GPa and 300 KK follows the sequence of Ti2_2AlC > Ti2_2AlN > Ti2_2AlB. The value of kphk_{ph} decreases gradually with increasing pressure and temperature for all three compounds. At ambient pressure and room temperature, Ti2_2AlC has higher kphk_{ph} than Ti2_2AlB and Ti2_2AlN which make it better thermal conductor. The kphk_{ph} of Ti2_2AlC shows the least response to pressure and temperature due to the elevated hardness found in this compound as discussed in mechanical and elastic properties section (see § 3.2). The pressure dependence of kphk_{ph} follows this sequence: Ti2_2AlB < Ti2_2AlC < Ti2_2AlN. Additionally, Ti2_2AlB exhibits stronger pressure dependence than Ti2_2AlC and Ti2_2AlN, which also correlates with the CijC_{ij}, EE, ΘD\Theta_D, and TmT_m of the corresponding compounds. The kphk_{ph} value of all the compounds decreases with temperature in the following order: Ti2_2AlB < Ti2_2AlN < Ti2_2AlC, which correlates with acoustic and dynamic behavior studies. Ti2_2AlB shows the lowest kphk_{ph} and a weaker temperature response than the other two compounds, which may indicate a better heat resistance.

Electronic properties

Band structure and density of states

The calculated pressure-dependent electronic band structure of the studied compounds along the high-symmetry directions in the Brillouin zone is displayed in Figure 13. The horizontal dashed line designates the Fermi level (EFE_F). The overlap of valence and conduction bands at EFE_F for Ti2_2AlB, Ti2_2AlC, and Ti2_2AlN indicates their metallic character. The states close to the Fermi level control the charge transport properties of materials. The anisotropy in electric conductivity of the studied compounds is obvious form the band energy dispersion around the EFE_F. Highly dispersive bands close to the Fermi level is indicative of high mobility of the charge carriers [76]. The most localized bands are along A-H path, whereas the highest band dispersion is observable along K-Γ\Gamma-M path for all the compounds. The bands located along the A-H path indicate that they are less mobile or more tightly bound in that direction, resulting in restricted electron mobility. On the other hand, the high dispersion along the K-Γ\Gamma-M path suggests that the electrons have more freedom and may perform better electrically in that direction. The EFE_F of Ti2_2AlX lies below the valence band maximum near Γ\Gamma-point. The substitution of XX with higher atomic number (B→\toC→\toN) in Ti2_2AlXX, introduces extra valence electrons per atom, leads EFE_{\mathrm{F}} moves to a higher energy level. Therefore, we can say that increase in bonding states near the EFE_{\mathrm{F}}. Strongly hybridized bands consisting of Ti 3dd and Al 3pp orbitals spread over an energy range from −2-2 eV to 2 eV. These bands contribute significantly in formation of chemical bonds and optical properties in the visible region. Bands associated with N are lower in energy than B and C, which is associated with their electrostatic attraction. Consequently, the mechanical strength of the materials also increases with XX (see § 3.2, mechanical behavior). Additionally, all three compounds remain metallic under pressure and the influence of pressure is not pronounced. We have also explored the effects of spin-orbit coupling on the electronic band structure. The overall effect was found insignificant (not shown here).

Figure 13. The electronic band structure of (a) Ti2_2AlB, (b) Ti2_2AlC, and (c) Ti2_2AlN along high symmetry directions of the Brillouin zone under 0 GPa and 10 GPa.

To gain further insights into the electronic responses of the compounds at P = 0 GPa and under hydrostatic pressure, we have studied the electronic density of states of the three MAX phases. The calculated pressure-dependent total density of states (TDOS) as well as partial density of states (PDOS) for Ti2_2AlXX (XX = B, C, and N) are displayed in Figure 14. The vertical dotted line represents Fermi energy (EFE_{\mathrm{F}}). The strong hybridization between Ti 3dd and Al 3pp states is evident for all the compounds. The contribution of XX atoms to TDOS in Ti2_2AlXX around the EFE_{\mathrm{F}} decreases with increasing atomic number. This might be understood this way, compared to lighter elements, heavier elements may have more inner-shell electrons, which are less engaged in bonding and electronic states close to the Fermi level. It is also important to point out that the TDOS below the EFE_{\mathrm{F}} is maximum for Ti2_2AlB due to the lower band energy dispersion E(k)E(k) in this energy range (see Figure 13). Around EFE_{\mathrm{F}}, the contribution of Ti 3d3d orbitals mainly dominates in all the compounds, whereas that of the X elements decreases as we move to heavier elements.

Figure 14. Total and partial electronic density of states (TDOS and PDOS) of (a) Ti₂AlB, (b) Ti₂AlC, and (c) Ti₂AlN under 0 GPa and 10 GPa.

The TDOS value for all the three compounds at EFE_{\mathrm{F}} under pressure is presented in Figure 15a. The TDOS at EFE_{\mathrm{F}} at ambient pressure follow the order of Ti₂AlB > Ti₂AlN > Ti₂AlC which is in good agreement with literature [9, 20]. Therefore, Ti₂AlB is more metallic and the metallicity increases with pressure. On the contrary, metallicity of Ti₂AlC and Ti₂AlN decreases with increasing pressure. In superconductors, transition temperature is connected with their electronic density of states at EFE_{\mathrm{F}} [77].

Total density of states and Coulomb pseudopotential of $\mathrm{Ti_2AlX}$ under pressure

Figure 15. The (a) total density of states and (b) Coulomb pseudopotential of Ti2AlX\mathrm{Ti_2AlX} under pressure.

The Coulomb pseudopotential (μ∗\mu^*), which is electron–electron interaction due to Coulomb force, plays an important role in determining electronic correlations in a system [78]. We have gauged μ∗\mu^* using the following expression [79]:

μ∗=0.26N(EF)1+N(EF)(9)\mu^* = \frac{0.26N(E_F)}{1 + N(E_F)} \tag*{(9)}

The variation in the calculated Coulomb pseudopotential for all three compounds with pressure is displayed Figure 15b. The values of μ∗\mu^* high in the ground state and vary weakly with pressure. The strongest electronic correlations exist in Ti2AlB\mathrm{Ti_2AlB}.

Fermi surface topology

The Fermi surface (FS) is crucial as it can explain several behaviors of a solid such as the electrical, magnetic, thermal, and optical properties. The dynamical properties of an electron on the FS largely depend on the position and shape of the Fermi sheets in the Brillouin zone. The effective mass of the electron is closely correlated with the FS curvature. The effective mass of the electron is smaller in areas where the FS is significantly curved, which can impact the electron's mobility and response to external fields. On the other hand, higher effective masses are associated with flat regions of the FS. The Fermi velocity may be relatively constant if the FS is approximately spherical; but, if it is strongly anisotropic, the velocity may vary dramatically in various directions. Nesting features, or regions on the FS where distinct parts can be superimposed by a certain wave-vector, promotes spin density waves or charge density waves. Anisotropic electrical and thermal conductivities can result from direction-dependent electron mobility in materials whose FS is extended along specific directions [80, 81]. Electrons near the Fermi sheets are actively involved in the superconducting state formation [82]. The electrical characteristics of metallic systems may be inferred from the FS contour with respect to the BZ. Moreover, the dynamical characteristics of an electron on the FS are often location-dependent. The presence of an FS is probably the most important indications of materials containing Fermi liquid quasiparticles. The Fermi surfaces of Ti2AlB\mathrm{Ti_2AlB}, Ti2AlC\mathrm{Ti_2AlC}, and Ti2AlN\mathrm{Ti_2AlN} compounds were constructed from the bands crossing the EFE_F at pressure of 0 and 10 GPa and are depicted in Figure 16-Figure 18. The FS of Ti2AlB\mathrm{Ti_2AlB} has four sheets, while the other two materials contain five sheets.

Figure 16. The Fermi surfaces of Ti2AlB\mathrm{Ti}_{2}\mathrm{AlB} at (a) 0 and (b) 10 GPa.

The Fermi surfaces of Ti₂AlN at (a) 0 and (b) 10 GPa

Figure 18. The Fermi surfaces of Ti₂AlN at (a) 0 and (b) 10 GPa.

For Ti2AlB\mathrm{Ti}_{2}\mathrm{AlB}, all four sheets are central and parallel to the Γ\Gamma–A direction with cylindrical or prismatic-like hexagonal cross section at 0 GPa. These sheets are electron-like and 2D. Under 10 GPa, electron-like spherical FS (for band 28) appears along Γ\Gamma–K path, whereas other Fermi sheets remain identical.

For Ti2AlC\mathrm{Ti}_{2}\mathrm{AlC}, four cylindrical electron-like Fermi sheets are constructed from band numbers 29, 30, 31, and 32 keeping the Γ\Gamma–A direction as their axis. All these sheets exhibit hexagonal cross section as Ti2AlB\mathrm{Ti}_{2}\mathrm{AlB}. For band 33, electron pockets appear around K-point with hexagonal symmetry. The FS topology of Ti2AlC\mathrm{Ti}_{2}\mathrm{AlC} remains unchanged under pressure (10 GPa).

For Ti2AlN\mathrm{Ti}_{2}\mathrm{AlN}, there is an electron-like ring with tinny gap at the center (Γ\Gamma–A direction) and this gap increases as well as the ring breaks up into 4 pieces at 4 GPa (not shown here) which is also visible at 10 GPa. The electron-like FS for band 31 is cylindrical (centered to the Γ\Gamma–A path). For band 32, electron-like sheet (with hexagonal symmetry) is seen around the Γ\Gamma-point. Electron-like sheets appear around at the corner of the Brillouin zone for bands 33 and 34. There are little change observable in FS for bands 31 and 32 under 10 GPa. The FS topologies of Ti2AlX\mathrm{Ti}_{2}\mathrm{AlX} (XX = B, C, and N) at 0 GPa are in complete agreement with the previous studies [40, 83].

Figure 17. The Fermi surfaces of Ti2AlC\mathrm{Ti}_{2}\mathrm{AlC} at (a) 0 and (b) 10 GPa.

Optical properties

In optical properties, we study the response of a material to the irradiation of electromagnetic energy. Unlike semiconductor and insulator, metallic systems require the plasma frequency and Drude damping correction [84, 85]. The calculation of the optical parameters of Ti2_2AlX (XX = B, C, and N) have done using a plasma energy of 5 eV and Drude damping of 0.05 eV with 0.5 eV energy smearing. The optical parameters of the compounds for electric field along the [100] polarization as a function of photon energy up to 25 eV under 0 and 10 GPa were studied to understand their optical response. Results are shown in Figure 19-Figure 20.

Photon energy dependence of dielectric constant and refractive index of Ti2AlX

Figure 19. Photon energy dependence of (a, b) dielectric constant (ε1\varepsilon_{1}, and ε2\varepsilon_{2}), and (c, d) refractive index (nn and kk) of Ti2_{2}AlX (X = B, C, and N) at 0 and 10 GPa.

Photon energy dependence plots for Ti₂AlX compounds

Figure 20. Photon energy dependence of (a) R(ω)R(\omega), (b) α(ω)\alpha(\omega), (c) σ(ω)\sigma(\omega), and (d) L(ω)L(\omega) of Ti₂AlX (X = B, C, and N) compounds at 0 and 10 GPa.

The frequency dependent real (ϵ1\epsilon_1) and imaginary (ϵ2\epsilon_2) parts of the complex dielectric function in the energy range 0–25 eV for the compounds are depicted in Figure 19a-Figure 19b. For a material, ϵ1(ω)\epsilon_1(\omega) elucidates the polarizability and light speed in the system, whereas ϵ2(ω)\epsilon_2(\omega) is related to the band structure and absorptive behavior of the material [47]. The intraband transitions are dominated at low energy in metals and the interband transitions strongly correlates with the electronic band structure. The large negative values of ϵ1\epsilon_1 for all three materials in the low energy region indicate their Drude-like behavior (Figure 19a).

The investigation of complex refractive index of materials is crucial for designing optoelectronic devices. The refractive index n(ω)n(\omega) and extinction coefficient k(ω)k(\omega) of a material are incorporated into complex refractive index as: N(ω)=n(ω)+ik(ω)N(\omega) = n(\omega) + ik(\omega). Figure 19c and 19d represent n(ω)n(\omega) and k(ω)k(\omega) as a function of energy for Ti2_2AlX MAX phases, respectively. The maximum of both n(ω)n(\omega) and k(ω)k(\omega) for all three cases is obtained at 0 eV and decreases with increasing energy. The density of accessible electronic states often drops as one moves further from the Fermi level, which causes the values of n(ω)n(\omega) and k(ω)k(\omega) to fall as energy increases. A compound with a larger value of k(ω)k(\omega) exhibits higher light attenuation ability. Refractive indices of all three MAX compounds are large in the visible region. Thus, these compounds can be used in optoelectronic display devices.

Optical reflectivity [R(ω)R(\omega)] of the materials was studied and presented in Figure 20a. At both 0 and 10 GPa, reflectivity is maximum at zero photon energy and decreases almost linearly around 2 eV for all three compounds. High RR is caused by the interaction of incident light with free electrons in metals. Rmax⁡R_{\max} at zero photon energy predicted shiny nature of the compounds. The value of RR is almost nonselective and remains above 40% in the energy range from 0 to ~14 eV which implies that the studied MAX phase materials can be used as an efficient reflector of solar radiation. A material's electronic band structure is impacted by pressure. The density of states at the Fermi level varies with increasing pressure. These modifications lead to pressure dependent variation in the reflectivity.

The optical absorption [α(ω)\alpha(\omega)] spectra of the compounds at 0 and 10 GPa are shown in Figure 20b. The photon absorption for all the studied compounds begins at 0 eV indicating their metallic nature. This finding is also consistent with the band structure and DOS studies (see § 5.1). The absorption peaks for Ti2_{2}AlB, Ti2_{2}AlC, and Ti2_{2}AlN are observed ~7 eV. Ti, Al, and the other elements (B, C, or N) contribute to the largest absorption peaks, which are connected to their electronic band structures. All three MAX compounds absorb UV radiation efficiently.

Figure 20c displays the photoconductivity, σ(ω)\sigma(\omega), of Ti2_{2}AlX at 0 and 10 GPa. Photoconductivity initiates from zero photon energy for all studied compounds at both pressures, manifesting again the metallic behavior. This is also consistent with the electronic band structure, optical absorption, and dielectric function studies. Several features in the optical conductivity spectrum are related to the bulk plasmon excitations, and caused by valence to conduction band electron transition [37].

The electron energy-loss function [L(ω)][L(\omega)] spectra of the studied materials at 0 and 10 GPa are illustrated in Figure 20d. The electron energy-loss function of a material describes the energy lost by a fast-moving electron traveling through the material. These interactions may include phonon excitation, interband and intraband transitions, plasmon excitations, inner shell ionizations and Cerenkov radiations [37]. The highest peak in energy-loss function spectrum for a material, associated with the plasma resonance, which appears at a specific photon frequency called plasma frequency (ωp\omega_{\mathrm{p}}) of the material [86]. At this specific energy, the charge carriers undergo collective oscillations whose frequency depends on the effective mass and concentration of the electrons. The highest peak of L(ω)L(\omega) for Ti2_2AlB, Ti2_2AlC, and Ti2_2AlN at 0 GPa is about 18.49 eV, 21 eV, and 21.75 eV, respectively. A material becomes transparent and exhibits insulator-like optical features for the incident photon frequency higher than its ωp\omega_{\mathrm{p}}. The peak energy also indicates metallic to dielectric transition; above this point the material shows dielectric features [38]. The plasma frequency is given by the Drude model as ωp=nee2ε0me\omega_{\mathrm{p}} = \sqrt{\frac{n_{\mathrm{e}}e^2}{\varepsilon_0m_{\mathrm{e}}}}, where nen_{\mathrm{e}} is the electron density, ee is the elementary charge, ε0\varepsilon_0 is the the permittivity of free space, and mem_{\mathrm{e}} is the effective mass of the electrons. The basic feature of the connection between free electron density and collective electronic excitations in metals and other conductive materials is this relationship [84, 85].

Overall variation in the optical parameters with pressure is weak (up to 10 GPa). Like many other MAX and MAB phase compounds [87, 88, 89, 90], there is slight optical anisotropy with respect to electric field polarization direction observed in all three MAX compounds under investigation (not shown here).

Theoretical Vickers hardness

The theoretical Vickers hardness (HVH_{\mathrm{V}}) is an important mechanical parameter connected with bond overlap population and bond hardness between the atoms. The theoretical Vickers hardness of the MAX phases was acquired using following equations [91]:

HV=[∏μ(HVμ)nμ]1/∑nμ(10)H_{\mathrm{V}}=\left[\prod_{\mu}\left(H_{\mathrm{V}}^{\mu}\right)^{n^{\mu}}\right]^{1/\sum n^{\mu}} \tag*{(10)}
HVμ=740(Pμ−Pμ′)(Vbμ)−5/3(11)H_{\mathrm{V}}^{\mu}=740\left(P^{\mu}-P^{\mu'}\right)\left(V_{\mathrm{b}}^{\mu}\right)^{-5/3} \tag*{(11)}
Vbμ=(dμ)3∑ν[(dμ)3nμ](12)V_{\mathrm{b}}^{\mu}=\frac{\left(d^{\mu}\right)^3}{\sum_{\nu}\left[\left(d^{\mu}\right)^3 n^{\mu}\right]} \tag*{(12)}

where, dμd^{\mu} and PμP^{\mu} define the Mulliken bond length and bond overlap population of the μ\mu-type bond, respectively. Pμ′P^{\mu'} (=nfree/V=n_{\mathrm{free}}/V) is the metallic population (nfreen_{\mathrm{free}} = number of free electrons), nμn^{\mu} is the number of μ\mu-type bond per unit volume, VbμV_{\mathrm{b}}^{\mu} is the bond volume of μ\mu-type bond, and ∑nμ\sum n^{\mu} represents total number bonds in the unit cell. The constant 740 is a proportionality coefficient. The calculated intrinsic hardness values of Ti₂AlX (X = B, C, and N) are listed in Table 2.

PhasesPressureμ\mu-type bondnμn^{\mu}dμd^{\mu}vbμv_b^{\mu} (Å3^3)PμP^{\mu}Pμ′P^{\mu'}HVμH_V^{\mu} (GPa)HVH_V
Ti2_2AlB0Ti-B42.1868.6331.110.13319.9091.601
Ti-Al42.93920.9850.602.166
10Ti-B42.1498.3201.070.14320.0761.598
Ti-Al42.83819.1720.542.138
Ti2_2AlC0Ti-C42.1087.6221.030.08623.6791.655
Ti-Al42.89619.7720.552.378
10Ti-C42.0787.4081.010.08924.2021.649
Ti-Al42.81218.3670.482.261
Ti2_2AlN0Ti-N42.0837.3490.820.01821.3591.509
Ti-Al42.83718.5610.241.261
10Ti-N42.0567.1350.800.02121.8141.388
Ti-Al42.76717.4010.120.630

Table 2. The calculated μ\mu-type bonds, number of μ\mu-type bond nμn^{\mu}, bond length dμd^{\mu} (Å), bond volume vbμv_b^{\mu} (Å3^3), bond overlap population PμP^{\mu}, metallic population Pμ′P^{\mu'}, bond hardness HVμH_V^{\mu} (GPa), and hardness HVH_V (GPa) of Ti2_2AlX (XX = B, C, and N) at 0 GPa and 10 GPa.

The results indicate that all three compounds are relatively soft, with Ti2_2AlC is comparatively harder among them. The value of PμP^{\mu} for each bond between elements defines the degree of overlap of the electron clouds that form the bond. For all the compounds the longer and smaller values of dμd^{\mu} and PμP^{\mu} for Ti-Al bonds in comparison to Ti-X bonds are a sign of lower bond hardness. This suggests that the bond breaking will start with Ti-Al under pressure or temperature.

Interestingly, the hardness of the materials decreases with pressure which contradicts the general trend of materials being harder under pressure. This comes from decrease in Ti-Al bond hardness under pressure, which results in a lower overall hardness. This decrease in mechanical hardness with pressure also correlates with Pugh’s ratio and micro hardness (see Figure 4). The calculated nfreen_{free} values for Ti2_2AlB, Ti2_2AlC, and Ti2_2AlN at 0 GPa is 15.71, 9.37, and 1.89, respectively. The nfreen_{free} values for Ti2_2AlB and Ti2_2AlC are significantly higher than that of Ti2_2AlN and increases up to 10 GPa. As a consequence, the metallic bonding in the systems also increases under pressure.

Conclusions

We have employed DFT based first-principles calculations to conduct extensive studies of physical properties of Ti2_2AlX (XX = B, C, and N) MAX phases. The (hydrostatic) pressure-dependent structural, mechanical, thermophysical, phonon dynamical behavior, electronic (band, DOS, and FS topology), and optical properties are comprehensively explored for the very first time. The studied compounds possess structural, mechanical, and dynamical stability both at ambient and under pressure. The estimated structural parameters decrease with increasing pressure. Ti2AlB\mathrm{Ti}_{2}\mathrm{AlB} undergoes brittle-ductile transition at about 8 GPa whereas Ti2AlC\mathrm{Ti}_{2}\mathrm{AlC} and Ti2AlN\mathrm{Ti}_{2}\mathrm{AlN} remain brittle up to 10 GPa. The compounds possess a moderate level of mechanical and optical anisotropy. The mixed bonding nature was found in Ti2AlX\mathrm{Ti}_{2}\mathrm{AlX} compounds. All three MAX phases are moderately machinable which increases gradually under pressure. The metallic nature of the compounds is confirmed from their electronic (band structure, DOS, and FS) and optical studies. The FS topologies are studied. A distinct electron-pocket with hexagonal symmetry in the BZ appears in Ti2AlB\mathrm{Ti}_{2}\mathrm{AlB} under 10 GPa. Otherwise, the pressure effect on electronic band structure and FS is small that make the materials alluring for industrial applications under harsh and extreme conditions i.e., conditions involving large pressure changes. The estimated Coulomb pseudopotential implies electronic correlations in the order Ti2AlB>Ti2AlN>Ti2AlC\mathrm{Ti}_{2}\mathrm{AlB} > \mathrm{Ti}_{2}\mathrm{AlN} > \mathrm{Ti}_{2}\mathrm{AlC}. The TDOS and Coulomb pseudopotential of Ti2AlB\mathrm{Ti}_{2}\mathrm{AlB} increases with increasing pressure, while Ti2AlC\mathrm{Ti}_{2}\mathrm{AlC} and Ti2AlN\mathrm{Ti}_{2}\mathrm{AlN} show reverse response. The charge density difference plots reveal direction dependency of atomic bonding. At room temperature, the phonon thermal conductivity of Ti2AlC\mathrm{Ti}_{2}\mathrm{AlC} is significantly higher than other two. All three compounds have some potential as thermal insulation materials [92, 93]. It is predicted that Ti2AlC\mathrm{Ti}_{2}\mathrm{AlC} and Ti2AlN\mathrm{Ti}_{2}\mathrm{AlN} have much higher Debye and melting temperature than Ti2AlB\mathrm{Ti}_{2}\mathrm{AlB}. The optical properties suggest their suitability in some optical applications.

In summary, we have investigated systematically a large number of physical properties of the Ti2AlX\mathrm{Ti}_{2}\mathrm{AlX} (X=B,CX = \mathrm{B}, \mathrm{C}, and N\mathrm{N}) MAX phases in this paper. The studied compounds have considerable potential in thermo-mechanical and optoelectronic applications. We hope that these results will stimulate researchers to investigate these MAX phase nanolaminates in greater detail, both theoretically as well as experimentally in near future.

Acknowledgements

Authors are grateful to the Department of Physics, Chittagong University of Engineering & Technology (CUET), Chattogram-4349, Bangladesh, for providing the computing facilities for this work. This work was also carried out with the aid of a grant (grant number: 21-378 RG/PHYS/AS_G-FR3240319526) from UNESCO-TWAS and the Swedish International Development Cooperation Agency (SIDA). The views expressed herein do not necessarily represent those of UNESCO-TWAS, SIDA, or its Board of Governors.

Data availability

The data sets generated and/or analyzed in this study are available from the corresponding author on reasonable request.

Author Contributions

M. I. Naher: Methodology, Formal analysis, Writing – original draft; M. Montasir: Formal analysis, Writing – original draft; M. Y. H. Khan: Formal analysis, Writing – original draft; M. A. Ali: Formal analysis, Writing – original draft, Validation; M. M. Hossain: Formal analysis, Writing review & editing, Validation; M. M. Uddin: Writing review & editing, Validation; M. Z. Hasan: Writing review & editing, Validation; M. A. Hadi: Writing review & editing, Validation; S. H. Naqib: Conceptualization, Formal analysis, Writing review & editing, Validation, Supervision.

Competing Interests

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

References

  1. [1]Rackl T, Johrendt D. The MAX phase borides Zr₂SB and Hf₂SB. Solid State Sciences 2020;106:106316. https://doi.org/10.1016/j.solidstatesciences.2020.106316
  2. [2]Zhang Z, Duan X, Jia D, Zhou Y, Zwaag SVD. On the formation mechanisms and properties of MAX phases: A review. Journal of the European Ceramic Society 2021;41:3851. https://doi.org/10.1016/j.jeurceramsoc.2021.02.002
  3. [3]Gonzalez-Julian J. Processing of MAX phases: from synthesis to applications. J. Am. Ceram. Soc. 2021;104:659. DOI: 10.1111/jace.17544
  4. [4]Rana MR, Islam S, Hoque K, Biswas GG, Hossain ME, Naqib SH, Ali MA. DFT prediction of the stability and physical properties of M₂GaB (M = Sc, V, Nb, Ta). Journal of Materials Research and Technology 2023;24:7795. https://doi.org/10.1016/j.jmrt.2023.05.008
  5. [5]Barsoum MW, Ali M, El-Raghy T. Processing and characterization of Ti₂AlC, Ti₂AlN, and Ti₂AlC₀.₅N₀.₅. Metall. Mater. Trans. A 2000;31:1857. https://doi.org/10.1007/s11661-006-0243-3
  6. [6]Barsoum MW, Brodkin D, El-Raghy T. Layered machinable ceramics for high temperature applications. Scr. Mater. 1997;36:535. https://doi.org/10.1016/S1359-6462(96)00418-6
  7. [7]Barsoum MW. The Mₙ₊₁AXₙ phases: A new class of solids: Thermodynamically stable nanolaminates. Progress in Solid State Chemistry 2000;28:201. https://doi.org/10.1016/S0079-6786(00)00006-6
  8. [8]Bai Y, Srikanth N, Chua CK, Zhou K. Density functional theory study of Mₙ₊₁AXₙ phases: A review. Critical Reviews in Solid State and Materials Sciences 2019;44:56. https://doi.org/10.1080/10408436.2017.1370577
  9. [9]Surucu G. Investigation of structural, electronic, anisotropic elastic, and lattice dynamical properties of MAX phases borides: An ab-initio study on hypothetical M₂AB (M = Ti, Zr, Hf; A = Al, Ga, In) compounds. Materials Chemistry and Physics 2018;203:106. https://doi.org/10.1016/j.matchemphys.2017.09.050
  10. [10]Ali MA, Qureshi MW. Newly synthesized MAX phase Zr₂SeC: DFT insights into physical properties towards possible applications. RSC Adv. 2021;11:16892. DOI: 10.1039/D1RA02345DDOI
  11. [11]Khazaei M, Arai M, Sasaki T, Estili M, Sakka Y. Trends in electronic structures and structural properties of MAX phases: a first-principles study on M₂AlC (M = Sc, Ti, Cr, Zr, Nb, Mo, Hf, or Ta), M₂AlN, and hypothetical M₂AlB phases. J. Phys.: Condens. Matter 2014;26:505503. DOI: 10.1088/0953-8984/26/50/505503DOI
  12. [12]Sun ZM. Progress in research and development on MAX phases: a family of layered ternary compounds. Int. Mater. Rev. 2011;56(3):143. DOI: 10.1179/1743280410Y.0000000001DOI
  13. [13]Hettinger JD, Lofland SE, Finke P, et al. Electrical transport, thermal transport, and elastic properties of M₂AlC (M = Ti, Cr, Nb, and V). Phys. Rev. B 2005;72:115120. https://doi.org/10.1103/PhysRevB.72.115120
  14. [14]Du YL, Sun ZM, Hashimoto H. First-principles study on phase stability and compression behavior of Ti₂SC and Ti₂AlC. Physica B 2010;405:720. https://doi.org/10.1016/j.physb.2009.09.093
  15. [15]Suna Z, Li S, Ahuja R, Schneider JM. Calculated elastic properties of M₂AlC (M = Ti, V, Cr, Nb and Ta). Solid State Communications 2004;129:589. https://doi.org/10.1016/j.ssc.2003.12.008
  16. [16]Cover MF, Warschkow O, Bilek MMM, McKenzie DR. A comprehensive survey of M₂AX phase elastic properties. J. Phys.: Condens. Matter 2009;21:305403. DOI: 10.1088/0953-8984/21/30/305403DOI
  17. [17]Persson POÅ, Rosén J, McKenzie DR, Bilek MMM. Formation of the MAX-phase oxycarbide Ti₂AlC₁₋ₓOₓ studied via electron energy-loss spectroscopy and first-principles calculations. Phys. Rev. B 2009;80:092102. https://doi.org/10.1103/PhysRevB.80.092102
  18. [18]Wang XH, Zhou YC. High-Temperature oxidation behavior of Ti₂AlC in air. Oxidation of Metals 2003;59:303. https://doi.org/10.1023/A:1023092027697
  19. [19]Low IM. An overview of parameters controlling the decomposition and degradation of Ti-based Mₙ₊₁AXₙ phases. Materials 2019;12(3):473. https://doi.org/10.3390/ma12030473
  20. [20]Hug G, Fries E. Full-potential electronic structure of Ti₂AlC and Ti₂AlN. Phys. Rev. B 2002;65:113104. https://doi.org/10.1103/PhysRevB.65.113104
  21. [21]Dhakal C, Aryal S, Sakidja R, Ching WY. Approximate lattice thermal conductivity of MAX phases at high temperature. Journal of the European Ceramic Society 2015;35:3203. https://doi.org/10.1016/j.jeurceramsoc.2015.04.013
  22. [22]Bai Y, He X, Wang R. Lattice dynamics of Al-containing MAX-phase carbides: a first-principles study. J. Raman Spectrosc. 2015;46:784. https://doi.org/10.1002/jrs.4720
  23. [23]Qureshi MW, Ma X, Tang G, Paudel R. Ab initio predictions of structure and physical properties of the Zr₂GaC and Hf₂GaC MAX phases under pressure. Sci Rep 2021;11:3260. https://doi.org/10.1038/s41598-021-82402-1
  24. [24]Fakhera F, Hossain K, Khanom S, Hossain MK, Ahmed F. Effect of pressure in tuning the physical properties of MAX phase Zr₂AN (A = In, Ga): A DFT scheme. Results in Physics 2023;53:106912. https://doi.org/10.1016/j.rinp.2023.106912
  25. [25]Hossain MS, Jahan N, Hossain MM, Uddin MM, Ali MA, High pressure mediated physical properties of Hf₂AB (A = Pb, Bi) via DFT calculations. Materials Today Communications 2023;34:105147. https://doi.org/10.1016/j.mtcomm.2022.105147
  26. [26]Clark SJ, Segall MD, Pickard CJ, et al. First principles methods using CASTEP. Z. Kristallogr 2005;220:567. https://doi.org/10.1524/zkri.220.5.567.65075.
  27. [27]Parr RG. Density functional theory. Ann Rev Phys Chern 1983;34(1):631. https://doi.org/10.1146/annurev.pc.34.100183.003215
  28. [28]Materials studio CASTEP manual © Accelrys2010. http://www.tcm.phy.cam.ac.uk/castep/documentation/WebHelp/CASTEP.html.
  29. [29]Perdew JP, et al. Restoring the density-gradient expansion for exchange in solids and surfaces. Phys. Rev. Lett. 2008;100:136406. https://doi.org/10.1103/PhysRevLett.100.136406
  30. [30]Vanderbilt D. Soft self-consistent pseudopotentials in a generalized eigenvalue formalism. Phys. Rev. B 1990;41:7892. https://doi.org/10.1103/PhysRevB.41.7892
  31. [31]Packwood D, et al. A universal preconditioner for simulating condensed phase materials. J. Chem. Phys. 2016;144:164109. https://doi.org/10.1063/1.4947024
  32. [32]Monkhorst HJ, Pack JD. Special points for Brillouin-zone integrations. Phys. Rev. B 1976;13:5188. https://doi.org/10.1103/PhysRevB.13.5188
  33. [33]Koukaras EN, Kalosakas G, Galiotis C, Papagelis K. Phonon properties of graphene derived from molecular dynamics simulations. Sci Rep 2015;5:12923. https://doi.org/10.1038/srep12923
  34. [34]Kresse G, Furthmüller J, Hafner J. Ab initio force constant approach to phonon dispersion relations of diamond and graphite. Europhysics Letters 1995;32:729. DOI: 10.1209/0295-5075/32/9/005DOI
  35. [35]Nielsen OH, Martin RM. First-principles calculation of stress. Phys. Rev. Lett. 1983;50:697. https://doi.org/10.1103/PhysRevLett.50.697
  36. [36]Marius G. Kramers-Kronig relations (The Physics of Semiconductors), Springer US, Berlin Heidelberg, 2010.
  37. [37]Naderizadeh S, et al. Electronic and optical properties of Full-Heusler alloy Fe₃−ₓMnₓSi. Eur. Phys. J. B 2012;85:144. https://doi.org/10.1140/epjb/e2012-20919-3
  38. [38]Sun J, Wang HT, He JL, Tian YJ. Ab initio investigations of optical properties of the high-pressure phases of ZnO. Phys. Rev. B 2005;71:125132. https://doi.org/10.1103/PhysRevB.71.125132
  39. [39]Schuster JC, Nowotny H, Vaccaro C. The ternary systems: Cr-Al-C, V-Al-C, and Ti-Al-C and the behavior of H-phases (M₂AlC). Journal of Solid State Chemistry 1980;32:213. https://doi.org/10.1016/0022-4596(80)90569-1
  40. [40]Karaca E, Byrne PJP, Hasnip PJ, Probert MIJ. Prediction of phonon□mediated superconductivity in new Ti□based M₂AX phases. Sci Rep 2022;12:13198. https://doi.org/10.1038/s41598-022-17539-8
  41. [41]Basu S, Barsoum MW, Kalidindi SR. Sapphire: A kinking nonlinear elastic solid. Journal of Applied Physics 2006;99:063501. https://doi.org/10.1063/1.2179974
  42. [42]Poon B, Ponsonn L, Zhao J, Ravichandran G. Damage accumulation and hysteretic behavior of MAX phase materials. Journal of the Mechanics and Physics of Solids 2011;59:2238. https://doi.org/10.1016/j.jmps.2011.03.012
  43. [43]Naher MI, Naqib SH. An ab-initio study on structural, elastic, electronic, bonding, thermal, and optical properties of topological Weyl semimetal TaX (X = P, As). Sci Rep 2021;11:5592. https://doi.org/10.1038/s41598-021-85074-z
  44. [44]Naher MI, Ali MA, Hossain MM, Uddin MM, Naqib SH. A comprehensive ab-initio insights into the pressure dependent mechanical, phonon, bonding, electronic, optical, and thermal properties of CsV₃Sb₅ Kagome compound. Results in Physics 2023;51:106742. https://doi.org/10.1016/j.rinp.2023.106742
  45. [45]Naher MI, Naqib SH. First-principles insights into the mechanical, optoelectronic, thermophysical, and lattice dynamical properties of binary topological semimetal BaGa₂. Results in Physics 2022;37:105507. https://doi.org/10.1016/j.rinp.2022.105507
  46. [46]Born M, Hang K. Dynamical theory and experiments I. Berlin: Springer-Verlag Publishers; 1982.
  47. [47]Naher MI, Naqib SH. Possible applications of Mo₂C in the orthorhombic and hexagonal phases explored via ab-initio investigations of elastic, bonding, optoelectronic and thermophysical properties. Results in Physics 2022;37:105505. https://doi.org/10.1016/j.rinp.2022.105505
  48. [48]Naher MI, Afzal MA, Naqib SH. A comprehensive DFT based insights into the physical properties of tetragonal superconducting Mo₅PB₂. Results in Physics 2021;28:104612. https://doi.org/10.1016/j.rinp.2021.104612
  49. [49]Voigt W. Lehrbuch der Kristallphysik. Leipzig: Taubner; 1928. p. 962.
  50. [50]Reuss A. Berechnung der fließgrenze von mischkrlistallen auf grund der plastizitätsbedingung für einkristalle. Z Angew Math Mech 1929;9:49. https://doi.org/10.1002/zamm.19290090104
  51. [51]Hill R. The elastic behaviour of a crystalline aggregate. Proc. Phys. Soc. A 1952;65:349. DOI: 10.1088/0370-1298/65/5/307DOI
  52. [52]Wang X, Xiang H, Sun X, Liu J, Hou F, Zhou Y. Mechanical properties and damage tolerance of bulk Yb₃Al₅O₁₂ ceramic. Journal of Materials Science & Technology 2015;31:369. https://doi.org/10.1016/j.jmst.2015.01.002
  53. [53]Ali MA, Hossain MM, Uddin MM, Hossain MA, Islam AKMA, Naqib SH. Physical properties of new MAX phase borides M₂SB (M = Zr, Hf and Nb) in comparison with conventional MAX phase carbides M₂SC (M = Zr, Hf and Nb): Comprehensive insights. Journal of Materials Research and Technology 2021;11:1000. https://doi.org/10.1016/j.jmrt.2021.01.068
  54. [54]Jong MD, Winter I, Chrzan DC, Asta M. Ideal strength and ductility in metals from second- and third-order elastic constants. Phys. Rev. B 2017;96:014105. https://doi.org/10.1103/PhysRevB.96.014105
  55. [55]Greaves GN, Greer AL, Lakes RS, Rouxel T. Poisson’s ratio and modern materials. Nat Mater 2011;10:823. https://doi.org/10.1038/nmat3134
  56. [56]Pan Y, Zheng WT, Guan WM, Zhang KH, Fan XF. First-principles study on the structure, elastic properties, hardness and electronic structure of TMB₄ (TM = Cr, Re, Ru and Os) compounds. Journal of Solid State Chemistry 2013;207:29. https://doi.org/10.1016/j.jssc.2013.09.012
  57. [57]Slack GA. The thermal conductivity of nonmetallic crystals. Solid state Physics 1979;34:1. https://doi.org/10.1016/S0081-1947(08)60359-8
  58. [58]Meneve J, Vercammen K, Demkepeneer E, Smeets J. Thin tribological coatings: magic or design? Surf Coat Technol 1997;94–95:476. https://doi.org/10.1016/S0257-8972(97)00430-1
  59. [59]Cheng YT, Page T, Pharr GM, Swain M, Wahl KJ. (Eds.), Fundamentals and applications of instrumented indentation in multidisciplinary research. Journal of Materials Research 2004;19:1.
  60. [60]Donnet C, Erdemir A. Solid lubricant coatings: recent developments and future trends. Tribol Lett 2004;17(3):389. https://doi.org/10.1023/B:TRIL.0000044487.32514.1d
  61. [61]Chen XQ, Niu H, Li D, Li Y. Modeling hardness of polycrystalline materials and bulk metallic glasses. Intermetallics 2011;19:1275. https://doi.org/10.1016/j.intermet.2011.03.026
  62. [62]Pettifor DG. Theoretical predictions of structure and related properties of intermetallics. Mater Sci Technol 1992;8(4):345. DOI: 10.1179/mst.1992.8.4.345DOI
  63. [63]Zeng X, Peng R, Yu Y, Hu Z, Wen Y, Song L. Pressure effect on elastic constants and related properties of Ti3Al intermetallic compound: a first-principles study. Materials 2018;11:2015. https://doi.org/10.3390/ma11102015
  64. [64]Qu D, Li C, Bao L, Kong Z, Duan Y. Structural, electronic, and elastic properties of orthorhombic, hexagonal, and cubic Cu3Sn intermetallic compounds in Sn–Cu lead-free solder. J Phys Chem Solids 2020;138:109253. https://doi.org/10.1016/j.jpcs.2019.109253
  65. [65]Ranganathan SI, Ostoja-Starzewski M. Universal elastic anisotropy index. Phys. Rev. Lett. 2008;101:055504. https://doi.org/10.1103/PhysRevLett.101.055504
  66. [66]Gaillac R, Pullumbi P, Coudert FX. ELATE: an open-source online application for analysis and visualization of elastic tensors. J Phys Condens Matter 2016;28(27):275201. DOI: 10.1088/0953-8984/28/27/275201DOI
  67. [67]Anderson OL. A simplified method for calculating the Debye temperature from elastic constants. J Phys Chem Solids 1963;24(7):909. https://doi.org/10.1016/0022-3697(63)90067-2
  68. [68]Naher MI, Parvin F, Islam AKMA, Naqib SH. Physical properties of niobium-based intermetallics (Nb3B; B = Os, Pt, Au): a DFT-based ab-initio study. Eur Phys J B 2018;91:289. https://doi.org/10.1140/epjb/e2018-90388-9
  69. [69]Cheng L, Yan QB, Hu M. The role of phonon–phonon and electron–phonon scattering in thermal transport in PdCoO2. Phys. Chem. Chem. Phys. 2017;19:21714. DOI: 10.1039/C7CP03667ADOI
  70. [70]Fine ME, Brown LD, Marcus HL. Elastic constants versus melting temperature in metals. Scr Metall 1984;18:951. https://doi.org/10.1016/0036-9748(84)90267-9
  71. [71]Morelli DT, Slack GA. High lattice thermal conductivity solids. In: Shindé SL, Goela JS, editors. High Thermal Conductivity Materials. New York, NY: Springer; 2006. https://doi.org/10.1007/0-387-25100-6_2
  72. [72]Julian CL. Theory of heat conduction in rare-gas crystals. Phys. Rev. 1965;137:A128. https://doi.org/10.1103/PhysRev.137.A128
  73. [73]Clarke DR. Materials selection guidelines for low thermal conductivity thermal barrier coatings. Surf Coat Technol 2003;163-164:67. https://doi.org/10.1016/S0257-8972(02)00593-5
  74. [74]Cahill DG, Pohl RO. Lattice vibrations and heat transport in crystals and glasses. Annu. Rev. Phys. Chem. 1988;39:93.DOI
  75. [75]Shafique A, Shin YH. Ultrahigh and anisotropic thermal transport in the hybridized monolayer (BC₂N) of boron nitride and graphene: a first-principles study. Phys. Chem. Chem. Phys. 2019;21:17306. DOI: 10.1039/C9CP02068CDOI
  76. [76]Whalley LD, Frost JM, Morgan BJ, Walsh A. Impact of nonparabolic electronic band structure on the optical and transport properties of photovoltaic materials. Phys. Rev. B 2019;99:085207. https://doi.org/10.1103/PhysRevB.99.085207
  77. [77]Schlüter M. Effect of high pressure on the electronic density of states of aluminium. phys. stat. sol. (b) 1971;43:141. https://doi.org/10.1002/pssb.2220430115
  78. [78]Kostrzewa M, Szczęśniak R, Kalaga JK, Wrona JA. Anomalously high value of Coulomb pseudopotential for the H₅S₂ superconductor. Sci Rep 2018;8:11957. https://doi.org/10.1038/s41598-018-30391-z
  79. [79]Bennemann KH, Garland JW. Theory for Superconductivity in d band metals. AIP Conf. Proc. 1972;4:103. https://doi.org/10.1063/1.2946179
  80. [80]Hadi MA, Naqib SH, Christopoulos SRG, Chroneos A, Islam AKMA. Mechanical behavior, bonding nature and defect processes of Mo₂ScAlC₂: A new ordered MAX phase. Journal of Alloys and Compounds 2017;724:1167. https://doi.org/10.1016/j.jallcom.2017.07.110
  81. [81]Chowdhury A, Ali MA, Hossain MM, Uddin MM, Naqib SH, Islam AKMA. Predicted MAX phase Sc₂InC: Dynamical stability, vibrational and optical properties. Phys. Status Solidi B 2017;255:1700235. https://doi.org/10.1002/pssb.201700235
  82. [82]Cudazzo P, et al. Ab Initio description of high-temperature superconductivity in dense molecular hydrogen. Phys. Rev. Lett. 2008;100:257001. https://doi.org/10.1103/PhysRevLett.100.257001
  83. [83]Mauchamp V, et al. Anisotropy of the resistivity and charge-carrier sign in nanolaminated Ti₂AlC: Experiment and ab initio calculations. Phys. Rev. B 2013;87:235105. https://doi.org/10.1103/PhysRevB.87.235105
  84. [84]Li S, Ahuja R, Barsoum MW, Jena P, Johansson B. Optical properties of Ti₃SiC₂ and Ti₄AlN₃. Appl. Phys. Lett. 2008;92:221907. https://doi.org/10.1063/1.2938862
  85. [85]Wang H, Chen Y, Kaneta Y, Iwata S. First-principles study on effective doping to improve the optical properties in spinel nitrides. Journal of Alloys and Compounds 2010;491:550. https://doi.org/10.1016/j.jallcom.2009.10.267
  86. [86]Fox M. Optical properties of solids. New York: Academic Press; 1972
  87. [87]Ali MA, Hadi MA, Hossain MM, Naqib SH, Islam AKMA. Theoretical investigation of structural, elastic, and electronic properties of ternary boride MoAlB. Phys. Status Solidi B 2017;254:1700010. https://doi.org/10.1002/pssb.201700010
  88. [88]Ali MA, Hossain MM, Islam AKMA, Naqib SH. Ternary boride Hf₃PB₄: Insights into the physical properties of the hardest possible boride MAX phase. Journal of Alloys and Compounds 2021;857:158264. https://doi.org/10.1016/j.jallcom.2020.158264
  89. [89]Hadi MA, Roknuzzaman M, Nasir MT, Monira U, Naqib SH, Chroneos A, Islam AKMA, Alarco JA, Ostrikov K. Effects of Al substitution by Si in Ti₃AlC₂ nanolaminate. Sci Rep 2021;11:3410. https://doi.org/10.1038/s41598-021-81346-w
  90. [90]Aktar MB, Parvin F, Islam AKMA, Naqib SH. Structural, elastic, electronic, bonding, thermo-mechanical and optical properties of predicted NbAlB MAB phase in comparison to MoAlB: DFT based ab-initio insights. Results in Physics 2023;52:106921. https://doi.org/10.1016/j.rinp.2023.106921
  91. [91]Gao FM. Theoretical model of intrinsic hardness. Phys. Rev. B 2006;73:132104. https://doi.org/10.1103/PhysRevB.73.132104
  92. [92]Barsoum MW, Salama I, El-Raghy T, et al. Thermal and electrical properties of Nb₂AlC, (Ti, Nb)₂AlC and Ti₂AlC. Metallurgical and Materials Transactions A 2002;33:2775. https://doi.org/10.1007/s11661-002-0262-7
  93. [93]Yue SY, Qin G, Zhang X, Sheng X, Su G, Hu M. Thermal transport in novel carbon allotropes with sp² or sp³ hybridization: An ab initio study. Phys. Rev. B 2017;95:085207. https://doi.org/10.1103/PhysRevB.95.085207

Paper details

vlnc:W_h55b5by2
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 10

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy