Unravelling the oxygen influence in cubic bixbyite In2_2O3_3 on Raman active phonon modes by isotope studies

Abstract

In this study, we performed comprehensive investigations on the Raman active phonon modes in cubic bixbyite In2_2O3_3, an important oxide based, wide-bandgap semiconductor. Fundamental insights into the lattice dynamics are revealed, by determining the atomistic contribution to all modes and their frequencies by density functional perturbation theory calculations. Those simulations were performed for different compositions of 16^{16}O and 18^{18}O isotope ratios, including their pure states. An increasing red-shift of the mode frequencies with increasing 18^{18}O content for all modes, due to the increased atomic mass, is revealed. For the seven lowest energy modes, this relative shift is below 1%, whereas for the remaining 15 higher energetic modes a shift of about 5.5% was identified. All modes have energy contributions of both indium and oxygen lattice sites, except for one, which corresponds to a pure oxygen vibrational state. Applying Raman spectroscopy, those results could be verified experimentally with excellent agreement. Investigated samples consisted of a bulk single crystal with 16^{16}O isotopes and a MBE grown thin film as the 18^{18}O sample. Time-of-flight secondary ion mass spectrometry confirms the purity of the oxygen isotope in the sample. These isotopologue studies allow for a direct experimental access to fundamental material properties in cubic In2_2O3_3 by means of Raman spectroscopy. For example, we speculate, that the presence of oxygen vacancies in In2_2O3_3 would result in a shift of modes that are dominated by O-vibrations, e. g., Eg(4)E_{g}^{(4)} or Ag(4)A_{g}^{(4)}, towards lower frequencies.

Introduction

The sesquioxide In2_2O3_3 is a wide-bandgap material with a fundamental bandgap in the range of 2.7 to 2.9 eV[2, 4] [1, 3], but a strong onset of optical absorption only occurring at 3.8 eV5, making it a promising material for transparent electronics[6, 8] [7]. In2_2O3_3 is observed in two different polymorphs, a stable body centered cubic bixbyite and a meta-stable rhombohedral structure. Latter one is only observed when grown under special conditions9 and will be disregarded for our discussion here. The bixbyite structure has space group Ia3‾Ia\overline{3} (206) (Ia3‾Ia\overline{3}), a lattice parameter of a=10.117a = 10.117 Å and a cubic unit cell containing 16 formula units,[10] making a total of 80 atoms, illustrated in Figure 1. Widespread applications of In2_2O3_3 include heavily Sn doped (ITO) crystals with nn-type conductivity[12] [11, 13] and conductometric gas sensors[14]. For both applications, low quality crystals suffice. However, low crystal quality in In2_2O3_3 e. g. comes with a considerable high unintentionally doped (UID) nn-type conductivity or surface electron accumulation layer (SEAL), directly impacting the gas sensing properties of In2_2O3_3 and restricting the material’s usecases.[14] [15] In recent years, sesquioxides attracted focused efforts towards more advanced semiconductor applications, such as power electronics[16] or heterostructures, stacking several different oxides.17 Photon detection in the ultraviolet regime would benefit greatly by a tailored absorption edge in the active material. A combination of In2_2O3_3 with Ga2_2O3_3 in the form of an (In,Ga)2_2O3_3 alloy[18, 20, 22] [19, 21, 23] promises such a bandgap engineering up to the 4.8 eV[24] [25] of pristine Ga2_2O3_3. Along with such applications, semiconductor-grade crystal qualities are demanded. Inherently, a detailed understanding of the underlying fundamental mechanics of In2_2O3_3 is required and needs more studies to facilitate the rise in quality standards. A comprehensive understanding of phonon modes in In2_2O3_3 is integral to key material properties including mechanical strain, disorder, thermal and electrical dynamics as well as phonon-mediated optical processes. Hence, insights into vibrational properties facilitate improved crystal synthesis and offer critical input for both fundamental material characterization and applied studies, driving advances in both theoretical modelling and practical implementations of In2_2O3_3-based technologies.

Unit cell of cubic bixbyite In2O3

Figure 1. Unit cell of cubic bixbyite In2_2O3_3, having space group Ia3‾Ia\overline{3} (206). It comprises of 48 oxygen and 32 indium atoms, a lattice parameters of a=b=c=10.117a = b = c = 10.117 Å and α=β=γ=90∘\alpha= \beta= \gamma= 90^\circ. The image was created using VESTA.[26]

The aim of the present work is to provide valuable insights into the fundamental mechanics of the lattice vibrations of cubic bixbyite In2O3\mathrm{In_2O_3} and the contribution of individual lattice sites to those. Raman spectroscopy is a powerful, experimental method for the investigation of the vibrational properties of In2O3\mathrm{In_2O_3}.[27, 28, 29, 30] [19] Aside from experimental approaches, theoretical methods, e. g. based on density functional theory frameworks, have been successfully applied to predict the Raman active phonon mode frequencies in In2O3\mathrm{In_2O_3}[29] or for calculations on the fundamental bandgap of In2O3\mathrm{In_2O_3}[31] In the case of In2O3\mathrm{In_2O_3}, vibrational modes could originate solely from indium or oxygen lattice sites, or a combination of those. Discrimination of a mode against these types of origin poses challenges, hence making an identification of the role of oxygen atoms in the phonon mode spectrum challenging. In our study, we combine confocal Raman spectroscopy experiments with complementary density functional perturbation theory (DFPT) studies, both with the novel approach for In2O3\mathrm{In_2O_3} of using different oxygen isotopes. As Raman vibrations are quantized oscillations between atoms of the crystal lattice, exchanging an 16O{}^{16}\mathrm{O} with its 18O{}^{18}\mathrm{O} isotope does not affect the electronic structure and preserves the crystal structure and phonon modes, but changes the frequencies of phonon modes, involving an oxygen lattice site, due to the change in mass. Given the relative low mass of oxygen atoms, the 18O{}^{18}\mathrm{O} isotope has a significant relative mass increase of 12.5% over the 16O{}^{16}\mathrm{O} isotope. Therefore, using different oxygen isotopologues renders an excellent option to study isotope effects on phonon modes via theoretical calculations and Raman spectroscopy. This has been demonstrated for TiO2\mathrm{TiO_2}[32, 33], where modes without oxygen contribution could be identified. A recent study by Janzen et al. (see Ref. 34) successfully applies DFPT calculations and Raman spectroscopy on β\beta-Ga2O3\mathrm{Ga_2O_3} with 16O{}^{16}\mathrm{O} and 18O{}^{18}\mathrm{O} isotopologues, assigning the energy contribution of each lattice site to the vibrational modes. By extending this method to In2O3\mathrm{In_2O_3}, our study aims on gaining valuable insights into the lattice dynamics of bixbyite In2O3\mathrm{In_2O_3} beyond the symmetry and frequencies of the Raman active phonon modes,[29, 30] by providing quantitative insights into the element specific energy contribution to those lattice vibrations.

EXPERIMENTAL METHODS

The investigated 0.5 μ\mum thin In218O3\mathrm{In_2^{18}O_3} film was grown homoepitaxially on the (1 1 1) surface of an In2O3\mathrm{In_2O_3} substrate by plasma-assisted molecular beam epitaxy (PA-MBE) at a growth temperature of 750 °C, with the oxygen-plasma source running at 300 W. As oxygen source, a nominally 97.39% enriched 18O2{}^{18}\mathrm{O_2} isotope source was employed, with an oxygen flux of 0.3 sccm during the film deposition. For the homoepitaxial growth, a high quality single crystal bulk In2O3\mathrm{In_2O_3}, with a thickness of 500 μ\mum, was used. In2O3\mathrm{In_2O_3} substrates for homoepitaxy were prepared from bulk single crystals grown directly from the melt at the Leibniz-Institut für Kristallzüchtung, Berlin, using a novel crystal growth technique under the name Levitation-Assisted Self-Seeding Crystal Growth Method.[35]

Structural characterization of the deposited film succeeded by XRD measurements (PANalytical X’Pert Pro MRD equipped with a four-axis goniometer and using well-collimated and monochromatic Cu Kα1\alpha_1 radiation). Symmetric, out-of-plane 2Θ−ω2\Theta-\omega-scans and ω\omega-rocking curves of the In2O3\mathrm{In_2O_3} 2 2 2 reflex were performed to investigate the out-of-plane lattice parameter as well as the strain relaxation of the layer. The out-of-plane lattice parameters were additionally measured by high-resolution XRD (HRXRD).

ModeExperiment x=1x=1 (cm−1^{-1})Experiment x=0x=0 (cm−1^{-1})Theory x=1x=1 (cm−1^{-1})Theory x=0.75x=0.75 (cm−1^{-1})Theory x=0.5x=0.5 (cm−1^{-1})Theory x=0.25x=0.25 (cm−1^{-1})Theory x=0x=0 (cm−1^{-1})Experiment Δω\Delta\omega (cm−1^{-1})Experiment Δω\Delta\omega (%)Theory Δω\Delta\omega (cm−1^{-1})Theory Δω\Delta\omega (%)
Fg(1)F_g^{(1)}112.3111.6106.5106.4106.3106.2106.10.70.620.40.38
Fg(2)F_g^{(2)}121.5120.5115.3115.2115.1114.9114.81.00.820.50.43
Ag(1)A_g^{(1)}135.3134.1129.9129.7129.5129.3129.11.20.890.80.62
Fg(3)F_g^{(3)}156.5155.5150.6150.5150.3150.1150.01.00.640.60.40
Eg(1)E_g^{(1)}172.7171.7167.4167.2166.9166.7166.51.00.580.90.54
Fg(4)F_g^{(4)}209.8208.6203.3203.0202.7202.4202.01.20.571.30.64
Fg(5)F_g^{(5)}215.6214.4208.2208.1207.9207.7207.51.20.560.70.34
Fg(6)F_g^{(6)}303.4287.1305.1300.7296.4292.3288.416.35.3716.75.47
Ag(2)A_g^{(2)}309.4293.1306.8302.4298.2294.1290.316.35.2716.55.38
Ag(2)A_g^{(2)}313.3297.0313.4308.7304.2299.8295.716.35.2017.75.65
Fg(7)F_g^{(7)}318.0302.2316.6311.8307.3303.0298.815.84.9717.85.62
Fg(8)F_g^{(8)}369.2349.3362.8357.5352.6347.9343.319.95.3919.55.37
Fg(9)F_g^{(9)}392.1371.2385.1379.6374.3369.3364.420.95.3320.75.38
Eg(3)E_g^{(3)}396.0374.2390.9385.3380.0374.9370.121.85.5120.85.32
Fg(10)F_g^{(10)}455.1431.2442.0435.5429.3423.4417.823.95.2524.25.48
Fg(11)F_g^{(11)}468.9444.8454.7448.2442.0436.1430.524.15.1424.25.32
Ag(3)A_g^{(3)}497.2472.6481.7474.5467.7461.2455.024.64.9526.75.54
Fg(12)F_g^{(12)}518.0-506.4498.7491.5484.5477.9--28.55.63
Fg(13)F_g^{(13)}546.9-529.4521.6514.1506.8500.0--29.45.63
Eg(4)E_g^{(4)}595.3562.7587.4578.6570.1562.0554.332.65.4832.95.71
Ag(4)A_g^{(4)}608.9575.5575.9567.1558.7550.7543.033.45.4933.15.64
Fg(14)F_g^{(14)}631.8597.7611.9602.8594.2585.9578.034.15.4033.95.54

Table 1. TABLE I. Experimentally and theoretically determined phonon mode frequencies of all Raman-active phonons in cubic bixbyite In2_2O3_3. The table lists frequencies for different oxygen isotope compositions In216_2{}^{16}O3x18_{3x}{}^{18}O3(1−x)_{3(1-x)} as a function of xx. Experimentally, two samples with a pure isotope composition of either 100% 16{}^{16}O or 18{}^{18}O were investigated. Theoretical modeling additionally considered three mixed isotope configurations. The right section of the table presents the absolute and relative Raman mode frequency shifts Δω\Delta\omega for the fully substituted 16{}^{16}O and 18{}^{18}O samples, based on both experimental and theoretical wavenumbers.

For the determination of the actual incorporated 18{}^{18}O isotope ratio into the film’s In2_2O3_3 matrix, time-of-flight secondary ion mass spectrometry (ToF-SIMS) was performed on a ToF-SIMS IV machine (IONTOF GmbH, Münster, Germany) equipped with a ToF-SIMS V analyser and an extended dynamic range (EDR) unit. A high energy Ga+^+ primary ion gun, operated at 25 keV and in spectrometry mode, was rastered on an area of 100 μ\mum ×\times 100 μ\mum to produce secondary ions for ToF analysis. Negative secondary ions were collected with a cycle time of 50 μ\mus. The EDR was used for the 16{}^{16}O−^- and 18{}^{18}O−^- species to prevent overloading the detector. A low energy Cs+^+ ion gun, operated at 2 keV, was used to sputter etch the sample over an area of 400 μ\mum ×\times 400 μ\mum. Charge compensation was achieved by using a low energy (<20<20 eV) electron flood gun. The crater depths were measured post analysis, using an Interference Microscope (NT1100, Veeco Instruments Inc., NY, USA).

Raman spectroscopic measurements were performed in backscattering geometry with optical excitations at the 325-nm (3.81 eV) line of a He-Cd laser. For polarization-dependent mode symmetry identification, a second setup with an excitation wavelength of 473 nm (2.62 eV) of a solid-state laser was used. In both cases, the incident laser light was focused by a microscope objective onto the sample surface.

The backscattered light was collected by the same objective, spectrally dispersed by a 80-cm spectrograph (LabRam HR, Horiba/Jobin Yvon) and detected by a liquid-nitrogen-cooled charge-coupled device (CCD). Calibrating the Raman spectra was carried out by a reference Hg gas-discharge lamp (3.81 eV spectra) and a silicon reference sample (2.62 eV spectra). All spectra were acquired at room-temperature. Polarization dependent Raman spectra were recorded with the utilization of a λ/2\lambda/2 waveplates and polarization analysers. Using the Porto notation,[36] the z(xx)zˉz(x x)\bar{z} and z(xy)zˉz(x y)\bar{z} scattering geometries were applied, where zz denotes the direction normal to the sample surface and xx, yy spanning the surface plane, perpendicular to each other. For cubic bixbyite In2_2O3_3 in [?] orientation, it is known, that a z(xy)zˉz(x y)\bar{z} configuration leads to an extinction of modes with AgA_g symmetry, while the z(xx)zˉz(x x)\bar{z} setting reduces the FgF_g modes intensity by a third.[30] For the determination of phonon mode frequencies, the Raman spectra were analysed by line-fittings with Voigt functions resulting in an accuracy of 0.1 cm−1^{-1} for the peak positions.

THEORETICAL METHODS

Simulations of the lattice vibrations were performed within the frame of density functional perturbation theory (DFPT) on the level of the Perdew-Burke-Ernzerhof exchange-correlation approximation for solids (PBEsol) as implemented into the Quantum Espresso computational package.[37] The In (5s,5p,4d) and the O (2s,2p) states were treated as valence electrons using multi-projector optimized norm-conserving Vanderbildt (ONCV) pseudopotentials[38] from the Pseudo Dojo repository[39] and described by a planewave basis set using a cutoff energy of 180 Ry (2450 eV). All reciprocal space integrations were performed by a discrete kk-point sampling of 6×6×66 \times6 \times6 points in the Brillouin zone. We fully optimized the atomic positions and cell parameters of the primitive cell cubic In2_2O3_3 the residual forces between atoms and the cell stress were smaller than 0.0025 eVÅ−1^{-1} and 0.01 GPa, respectively. The threshold for the total energy was set to 10−1410^{-14} Ry, which ensured tightly converged interatomic forces for the geometry optimization and of the ground state density and wavefunctions for the DFPT calculations. We obtain a lattice constant of a=10.17a = 10.17 Å, i.e. an underbinding of 0.5% compared to the experimental lattice constant (aexp=10.119a^{\mathrm{exp}} = 10.119 Å) and a corresponding systematic underestimation of the simulated Raman shifts. Using the obtained phonon mode frequencies and displacement patterns, we then computed the relative energy contributions of indium and oxygen atoms to the Raman active lattice vibrations for In2_2O3_3 systems containing 16^{16}O and 18^{18}O isotopes using the method outlined in Ref. [34].

RESULTS and DISCUSSION

Density functional perturbation theory

Cubic bixbyite In2_2O3_3 contains 24 oxygen and 16 indium atoms per primitive unit cell. Group theory predicts for the given space group 206 (Ia3‾Ia\overline{3}) a total of 120 vibrational modes.[29, 40] Regarding only the gerade (g) modes, which are Raman active, a total of 22 modes remain, which can be represented at the Γ-point as following:

Γg=4Ag+4Eg+14Fg,(1)\Gamma_g = 4A_g + 4E_g + 14F_g, \tag*{(1)}

where EgE_g modes are double and FgF_g modes triple degenerated.[41] The resulting energy contribution of In and O atoms to AgA_g, EgE_g and FgF_g modes can be seen in Figure 2 (a)-(c). A notable finding is that, for all mode symmetries, there is at least one low-energy mode with approximately 10% of the total mode energy stemming from the oxygen lattice sites. Conversely, several high-energy modes exhibit over 90% of their vibrational energy originating from oxygen related vibrations. Most strikingly, when plotted as a function of mode frequency, these two distinct contribution regimes form two plateaus, characterized by a step-like behaviour, with no gradual redistribution occurring for modes with intermediate energy. Mode Eg(4)E_g^{(4)} stands out compared to the rest of the 21 phonon active modes, since it is the only mode, where only one element (oxygen) is contributing to the vibration, see Figure 2 (b). All other modes are a combination of In–O vibrations. A large oxygen related energy contribution translates into a strong sensitivity in terms of mode frequency and intensity with respect to changes in physical properties, correlated with oxygen lattice sites. No significant change in element specific energy contribution to the modes can be found for a crystal with 18^{18}O instead of 16^{16}O. In the same approach, a prediction of the absolute wavenumber of the modes were calculated for pure 18^{18}O and 16^{16}O crystals as well as of mixed isotope compositions (incremental steps of 25% of relative isotope contents). Table I lists the absolute wavenumbers of all phonon modes for both experimental and theoretical results, along with the absolute and relative frequency shifts (Δω\Delta\omega) between the two isotope variants. The relative shifts are referenced to 16^{16}O. As one of the most relevant results of our calculations, a clear monotonic shift towards lower mode frequencies with increasing 18^{18}O content is revealed.

Figure 2. Theoretical predictions for the relative energy contributions of indium (black) or oxygen, distinguished by isotope variants 16O{}^{16}\mathrm{O} (red) and 18O{}^{18}\mathrm{O} (purple), to the Raman-active lattice vibrations are presented. The analysed modes exhibit are modes with (a) AgA_g, (b) EgE_g and (c) FgF_g symmetry. The relative energy contribution of each element is represented by the height of the corresponding coloured column. All modes consist of vibrations involving both elements present in the crystal, with the exception of mode Eg(4)E_g^{(4)}, which is purely oxygen-driven.

ToF-SIMS and XRD

An essential experiment for the entire discussion is the determination of the successful incorporation of the 18^{18}O isotope into the homoepitaxially grown In2_2O3_3 film. From our Raman experiments independent verification and quantification comes from ToF-SIMS experiments. The quantity of interest is the 18^{18}O isotope fraction n∗n^*, which is directly reflected by the isotope intensities

n∗=I18OI16O+I18O.(2)n^* = \frac{I_{^{18}\mathrm{O}}}{I_{^{16}\mathrm{O}} + I_{^{18}\mathrm{O}}}. \tag*{(2)}

Throughout the 18^{18}O layer, a constant 18^{18}O isotope fraction of 96.5% could be determined. After approximately 0.5 μm, n∗n^* drops below 7%. This steep drop represents the film-substrate interface. These results allow for the assumption of a homogeneous and almost pure 18^{18}O presence for the Raman spectroscopic probing depth at 3.81 eV. The corresponding ToF-SIMS scan can be found in Figure S1 in the supplementary material.

Figure S1. Symmetric out-of-plane XRD analysis of the 500 nm-thick In218O3\mathrm{In}_2{}^{18}\mathrm{O}_3 layer on the In2O3\mathrm{In}_2\mathrm{O}_3 substrate. (a) Wide range 2Θ−ω2\Theta-\omega-scan with logarithmic intensity scale, (b) ω\omega-rocking curve of the 2 2 2 reflex with linear intensity scale, and (c) high-resolution XRD 2Θ−ω2\Theta-\omega-scan of the 2 2 2 reflex with logarithmic intensity scale. The horizontal line shows a lower bound estimate for the intensity contribution of the layer.

XRD analysis of the 18^{18}O thin film on In2_2O3_3(1 1 1) substrate (see Fig. S1 and related discussion in the supplementary material) indicates the exclusive presence of (1 1 1) oriented In2_2O3_3 lattice planes with a cubic lattice parameter of a=10.119a = 10.119 Å (within 0.02% of that given in [10]). A narrow ω\omega-rocking curve (full width at half maximum 0.014 deg) indicates excellent crystal quality. The out-of-plane lattice mismatch of the film to the substrate is estimated to be within ±0.035 %, translating into a negligible in-plane strain state for the thin film. Due to the negligible lattice strain and the overall high quality of the film, no impact of the growth conditions on the phonon mode structure and the Raman selection rules are expected for the 18^{18}O containing sample.[29, 42]

Raman spectra

All theoretically predicted 22 Raman active phonon modes could be identified for the 16O{}^{16}\mathrm{O} bulk-like substrate, while for the 18O{}^{18}\mathrm{O} homoepitaxially grown film, a total of 20 Raman active modes were successfully identified. Thereby, we took advantage of the optical excitation at 2.62 eV, for which the optical probing depth (αi+αs)−1(\alpha_i+\alpha_s)^{-1} in In2_2O3_3[30] is much larger than the film thickness, leading to an excellent signal-to-noise ratio. In particular, our bulk sample provides enough interaction volume and a resulting signal strength sufficient to detect the complete set of cubic bixbyite In2_2O3_3 phonon modes. Figure 3 displays the corresponding Raman spectra of the 16O{}^{16}\mathrm{O} bulk sample measured with two different polarization configurations. The utilization of excitation in the transparent regime together with polarization-dependent measurements has been particularly beneficial for disentangling the Raman signal at around 310 cm−1^{-1}, a superposition of four Raman modes, Fg(6)F_g^{(6)}, Ag(2)A_g^{(2)}, Eg(2)E_g^{(2)} and Fg(7)F_g^{(7)}. Assuming a negligible contribution of the Eg(2)E_g^{(2)} mode for excitation at 2.62 eV,[30] a detailed line-fitting analysis of the Raman spectra measured with different scattering geometries allowed us to unambiguously attribute the central peak as well as a red and blue shifted shoulder peaks to the Fg(6)F_g^{(6)} mode at 303.4 cm−1^{-1}, the Ag(2)A_g^{(2)} at 309.4 cm−1^{-1} and the Fg(7)F_g^{(7)} one at 318.0 cm−1^{-1}, respectively. With the knowledge of these mode frequencies, the Eg(2)E_g^{(2)} mode was determined with a wavenumber of 313.3 cm−1^{-1} by a line-fitting analysis of Raman spectra excited at 3.81 eV, in excellent agreement with the numerical predictions and with unambiguously identifiable 16O{}^{16}\mathrm{O} modes in the study by Kranert et al. 30, cf. Table I. Such a disentanglement of the superimposed Raman peaks at 310 cm−1^{-1} has not been possible in previous reports based on the investigation of thin films[30] and is described in more detail in the supplementary material.

Figure 3. Raman spectra of the 16O{}^{16}\mathrm{O} In2_2O3_3 sample, acquired at room temperature, 2.62 eV excitation photon energy and for two different polarization states, z(xx)zˉz(xx)\bar{z} and z(xy)zˉz(xy)\bar{z} following the Porto notation. As the AgA_g modes intensity is highly dependent on the polarization state of the scattered Raman photon, this dependence can be applied for an unambiguous mode identification.

In order to exclude any contribution from the substrate to the Raman signal when investigating the homoepitaxially grown 18O{}^{18}\mathrm{O} film, using an excitation energy above the bandgap is necessary. With an approximate film thickness of 0.5 μ\mum and an excitation energy of 3.81 eV, which results in the small optical probing depth of 80 nm,5 any contribution of the In2_2O3_3 substrate to the spectra, which would be present at an excitation at 2.62 eV, can be excluded. Since our calculations predict a phonon mode specific, monotonic decrease of the phonon mode frequencies with increasing 18O{}^{18}\mathrm{O} content (see Table I), the mode assignment for the 18O{}^{18}\mathrm{O} containing film could be derived in a straightforward manner from the spectrum of the 16O{}^{16}\mathrm{O} bulk sample.

Discussion of isotopic Raman shifts

The experimentally acquired Raman spectra, shown in Figure 4, were recorded at room-temperature and with an excitation photon energy of 3.81 eV, whereby the probing volume is constrained within the MBE grown 18O{}^{18}\mathrm{O} containing film.

Figure 4. Room temperature Raman spectra, acquired with an excitation photon energy of 3.81 eV, of the investigated cubic bixbyite In2_2O3_3 samples with natural, predominantly 16O{}^{16}\mathrm{O} and 96.5% enriched 18O{}^{18}\mathrm{O} oxygen abundance, depicted in black and purple, respectively. The two spectra have an artificial offset, for a clearer optical distinguishability. Except for the Fg(12)F_g^{(12)} and Fg(13)F_g^{(13)} ones (light grey), all Raman active phonon modes could be identified for both spectra. A clear red-shift for the modes stemming from the heavier oxygen isotope is apparent for frequencies above 300 cm−1^{-1}.

Comparing the two In2_2O3_3 crystals with either 16O{}^{16}\mathrm{O} or 18O{}^{18}\mathrm{O} isotopologues, a striking effect of the increased oxygen mass is the red-shift of phonon modes with wavenumbers higher than approximately 300 cm−1^{-1}. Phonon modes with wavenumbers below 300 cm−1^{-1} show a negligible dependence on the type of the oxygen isotope. Other aspects of the spectrum, such as the mode intensities and line-shape, do not differ with respect to the 16O^{16}\mathrm{O} grown crystal. Therefore, the experimental results support our theoretical predictions, indicating that oxygen vibrations contribute only a minor fraction - approximately 10% - to the total mode energy of the first seven lowest-energy modes, see Figure 2 (a) – (Figure 2c).

The Raman mode frequencies of the epitaxial In2_2O3_3 film obtained by line-fitting are shown in Figure 5 as a function of the 18O^{18}\mathrm{O} content. Our prediction of a monotonic, linear decrease of the phonon mode frequencies with increasing 18O^{18}\mathrm{O} content could be confirmed for all resolved phonon modes, i. e. all but the Fg(12)F_g^{(12)} and Fg(13)F_g^{(13)} modes. Raman features observed in the corresponding range of 520 – 580 cm−1^{-1} for excitation energy of 3.81 eV are predominantly attributed to higher-order Raman scattering processes involving phonon modes with AgA_g symmetry.[30]

Figure 5. Visualization of the Raman active phonon mode frequencies as a function of the 18O^{18}\mathrm{O} isotope content. AgA_g modes are symbolized by rectangles, EgE_g modes by circles and FgF_g modes by squares. Compared are experimentally (red) determined wavenumbers with theoretically calculated (purple) values. The theoretical results underestimate the phonon mode wavenumbers slightly compared to the experimental results. However, both methods reveal the behaviour of a decrease in mode energy with rising 18O^{18}\mathrm{O} content for modes above 300 cm−1^{-1} contrasting the almost constant behaviour below that threshold.

The simple linear dependence of the mode frequencies on the isotope ratio could, for example, be utilized to study the fundamental MBE growth dynamics for bixbyite-type oxide systems when two different oxygen sources are used simultaneously.[43] Supplying different oxygen isotopes by the two sources, their relative incorporation efficiencies can be determined by ex-situ Raman experiments by analyzing the phonon mode frequencies.

Table I provides a detailed breakdown of the absolute and relative mode shifts for the two isotope variants based on experimental and theoretical results. Overall, the DFPT results underestimate the experimental mode frequencies by about 4%, which is well within the typical accuracy of DFT simulations for phonons in oxides.[44] The slight ’softening’ of lattice vibrations is a known property of the PBEsol exchange-correlation functional used in our simulations and might indicate a somewhat overestimated screening of long-range interactions between atoms. For modes in the frequency range around 300 cm−1^{-1} (Fg(6)F_g^{(6)}, Ag(2)A_g^{(2)}, Eg(2)E_g^{(2)} and Fg(7)F_g^{(7)}), however, a reduced discrepancy between experimental and theoretical values is found. However, we note that the reliable experimental determination of the superimposed modes in this frequency range is challenging.

The absolute frequency shifts, comparing both isotopologues, increase almost monotonically for both, the experimental and theoretical results, with increasing mode frequency. The range of experimentally observed shifts reaches from 0.7 cm−1^{-1} to 34 cm−1^{-1}.

The most striking observation, however, concerns the two plateaus in the relative frequency shifts ((16O^{16}\mathrm{O} − 18O^{18}\mathrm{O}) / 16O^{16}\mathrm{O}). For modes with frequencies up to 215 cm−1^{-1} (Fg(5)F_g^{(5)}), the relative frequency shifts remain on the order of 1%, whereas for modes with higher frequencies, a values of 5% and higher are found both experimentally and theoretically. Figure 6 illustrates this behaviour including the excellent agreement between experiment and theory. Note, that no influence of the mode-symmetries on the relative frequency shifts could be identified. The two-plateau behaviour, however, corresponds exactly to the result of our calculations shown in Figure 2 and is, thus, explained by the jump in the relative energy contribution of oxygen for modes with higher frequencies than mode Fg(5)F_g^{(5)}.

Figure 6. Relative frequency shift of the Raman active phonon modes of the 16O{}^{16}\mathrm{O} to the 18O{}^{18}\mathrm{O} isotope sample, with the 16O{}^{16}\mathrm{O} values treated as the reference system. Both, experimental (red) and theoretical (purple) results are in great agreement with each other. Experimental values for modes Fg(12)F_g^{(12)} and Fg(13)F_g^{(13)} are missing, due to difficulties in their analysis. For modes with frequencies up to the value of the Fg(5)F_g^{(5)} mode, show a very low oxygen isotope dependence of sub 1% in relative frequency shift. In contrast, modes with higher frequencies show an almost constant relative shift of greater than 5%.

Regarding the suitability to study oxygen related phenomena, Klein et al. estimated a maximum concentration of oxygen vacancies of 3⋅10203 \cdot10^{20} for In2_2O3_3,[45] translating into vacant oxygen-sites of approximately 1%. In Wurtzite-type ZnO, such oxygen vacancy concentrations resulted in 1.6% lower mode frequency for a mode associated with the vibration of the oxygen system.[46] Assuming a similar influence on the bixbyite In2_2O3_3 system and a line-fitting accuracy of 0.1 cm−1^{-1}, an analysable oxygen vacancy concentration down to 0.02% could be resolved. Further research is necessary to investigate this potential usecase. The phonon mode Eg(4)E_g^{(4)} cm−1^{-1} appears to be most sensitive from a theoretical point of view, given the fact that only oxygen atoms contribute to this mode. Experimentally, however, the analysis of the Eg(4)E_g^{(4)} mode is impracticable due to its extremely low intensity in real-world experiments. Similar arguments can be applied to mode Eg(2)E_g^{(2)} and Ag(4)A_g^{(4)}, with only 1% of the mode’s energy contributed by indium lattice sites. Our recommendation for experimental probing of oxygen lattice site related effects, fall towards mode Fg(14)F_g^{(14)}. This mode has a relative small In contribution of 3% and shows the largest occurring absolute shift in our isotopologues experiments, while having negligible overlap with other spectral features.

Summary and conclusion

We conducted a comprehensive theoretical and experimental investigation of phonon modes in cubic bixbyite In2_2O3_3 with varying oxygen isotopic compositions. Using DFPT simulations, we analysed crystals with pure 16O{}^{16}\mathrm{O} and 18O{}^{18}\mathrm{O} isotopes, as well as three intermediate mixtures, and confirmed these results with Raman spectroscopy measurements on a nearly pure 18O{}^{18}\mathrm{O} In2_2O3_3 thin film and a bulk 16O{}^{16}\mathrm{O} reference sample. The DFPT simulations yielded several key findings. Except for a single pure oxygen vibration, all Raman-active phonon modes involve coupled indium-oxygen vibrations, with no indium-only vibrational modes observed. Most notably, two different plateaus in the relative isotopic mode shift are found for low-frequency and high-frequency phonon modes, respectively. This behaviour is explained by step-like increase in the energy contribution of oxygen to phonon modes with frequencies above 215 cm−1^{-1}. Furthermore, the substitution of 16O{}^{16}\mathrm{O} with 18O{}^{18}\mathrm{O} leads to a linear decrease of a mode’s Raman shift. The experimental Raman spectra align closely with theoretical predictions, affirming the accuracy of the DFPT model, though with a slight underestimation of mode energies in the calculations. Our study establishes a clear linear relationship between the oxygen isotope ratio and phonon mode energies, highlighting the utility of Raman spectroscopy as a precise method for examining isotopic effects in cubic bixbyite crystals. Future research can leverage this approach to explore fundamental properties of In2_2O3_3 and to gain insights into crystal growth dynamics through controlled isotopic variation.

Conflicts of Interest

There are no conflicts of interest to declare.

Acknowledgements

We thank Tobias Schulz and Hans Tornatzky for a critical reading of the manuscript. This work was performed in the framework of GraFOx, a Leibniz-ScienceCampus partially funded by the Leibniz association. J. F. gratefully acknowledges the financial support of the Leibniz Association. The authors gratefully acknowledge the scientific support and HPC resources provided by the Erlangen National High Performance Computing Center (NHR@FAU) of the Friedrich-Alexander-Universität Erlangen-Nürnberg (FAU) under the NHR project b181dc. NHR funding is provided by federal and Bavarian state authorities. NHR@FAU hardware is partially funded by the German Research Foundation (DFG) 440719683.

Supplemental Material: Unravelling the oxygen influence in cubic bixbyite In2O3\mathrm{In}_2\mathrm{O}_3 on Raman active phonon modes by isotope studies

Johannes Feldl; Roland Gillen; Janina Maultzsch; Alexandra Papadogianni; Joe Kler; Zbigniew Galazka; Oliver Bierwagen; Manfred Ramsteiner

Supplemental Material: Unravelling the oxygen influence in cubic bixbyite In2O3\mathrm{In}_2\mathrm{O}_3 on Raman active phonon modes by isotope studies

Figure S1 shows the symmetric out-of-plane XRD analysis of the 500 nm-thick homoepitaxial In218O3\mathrm{In}_2{}^{18}\mathrm{O}_3 layer. The wide-range 2Θ−ω2\Theta-\omega-scan (Figure S1) shows the presence of two diffraction orders of the In2O3\mathrm{In}_2\mathrm{O}_3 (1 1 1) planes and the absence of other orientations or secondary phases, thus indicating epitaxial match of the film to the substrate. The narrow ω\omega-rocking curve (Figure S1) with full-widths at half maximum of 0.014 deg is confirms a high crystal quality of substrate and film. The high-resolution XRD (Figure S1) indicates the 2 2 2 reflex at 2Θ=30.5802\Theta= 30.580 deg, corresponding to a cubic lattice parameter of 1.0119 nm. The 2 2 2 reflex intensity measured on an In218O3\mathrm{In}_2{}^{18}\mathrm{O}_3 layer with same thickness grown in the same growth run on a co-loaded c-plane sapphire substrate was found to be ≈5%\approx5\% that of the homoepitaxial layer. Thus, the reflex of the homoepitaxial layer may be dominated by the substrate contribution yet the layer should still contribute ≥5%\ge5\%. At this intensity level (indicated by the horizontal dashed line) the reflex looks symmetric with a widths of only 0.04 deg, suggesting the potential layer reflex to deviate no more than 0.01 deg from the substrate reflex (corresponding to a lattice mismatch or layer strain of ≤0.035%\le0.035\%).

For our experimental investigation of the influence of the oxygen isotope mass on the phonon mode frequency, it is crucial to have confirmation of the actual successfully incorporated oxygen isotopologue in the MBE grown thin film. For this purpose, we conducted an experiment independent of our Raman spectroscopic analysis tool by applying time-of-flight secondary ion mass spectrometry (ToF-SIMS). ToF-SIMS provides a quantitative depth profile of the isotope fraction of, in our case, oxygen ions. The data used for the analysis presented in the main article can be found in Figure S2. The sharp drop in 18O{}^{18}\mathrm{O} intensity is an indication of interface quality, with minimized diffusion despite elevated temperatures during growth. The drop occurs within a range of several tens of nanometers once the layer depth exceeds approximately 0.5 μm\mu\mathrm{m}. An almost constant 18O{}^{18}\mathrm{O} isotope fraction of 96.5% was found throughout the film depth.

Figure S2. ToF-SIMS depth profile of our 18O{}^{18}\mathrm{O} isotope MBE grown thin film on a 16O{}^{16}\mathrm{O} substrate, showing a 96.5% 18O{}^{18}\mathrm{O} isotope fraction at the surface of the film, estimated by a linear fit (black line). The steep drop in 18O{}^{18}\mathrm{O} isotope fraction marks the film thickness at approximately 0.5 μm\mu\mathrm{m}.

To disentangle the Raman signal around 310 cm−1^{-1}, which arises from the superposition of four Raman modes (Fg(6)F_g^{(6)}, Ag(2)A_g^{(2)}, Eg(2)E_g^{(2)} and Fg(7)F_g^{(7)}), we first analyzed the Raman spectrum of the 16O{}^{16}\mathrm{O} bulk sample using a 2.62 eV laser excitation. Under this excitation condition, Raman modes with EgE_g symmetry exhibit significantly lower intensities due to their reduced scattering cross-section. Consequently, the measured spectrum primarily comprises contributions from the Fg(6)F_g^{(6)}, Ag(2)A_g^{(2)} and Fg(7)F_g^{(7)} modes.

Further discrimination of these modes was achieved through polarization optics, which enable symmetry-dependent intensity variations, allowing for an unambiguous assignment of the Raman peaks. The extracted peak positions are 303.4 cm−1^{-1} for the Fg(6)F_g^{(6)} mode, 309.4 cm−1^{-1} for the Ag(2)A_g^{(2)} and 318.0 cm−1^{-1} for the Fg(7)F_g^{(7)} mode. These positions were determined by fitting the spectrum with Voigt functions.

At an excitation photon energy of 3.81 eV, the analysis must also account for the Eg(2)E_g^{(2)} mode, as its scattering cross-section is significantly enhanced and the experimental setup does not allow for symmetry induced suppression by polarization optics at this energy. To isolate the contribution of Eg(2)E_g^{(2)}, we performed spectral fitting while keeping the frequencies of the Fg(6)F_g^{(6)}, Ag(2)A_g^{(2)}, Eg(2)E_g^{(2)} and Fg(7)F_g^{(7)} modes fixed, with a correction applied for a setup specific offset. An additional Voigt function was introduced without constraints, allowing us to identify the Eg(2)E_g^{(2)} mode at 313.3 cm−1^{-1}. The detailed fitting procedure is shown in Figure S3.

Figure S3. Section of the 16O^{16}\mathrm{O} bulk sample Raman signal at 3.81 eV excitation energies, showing the superposition of Fg(6)F_g^{(6)}, Ag(2)A_g^{(2)}, Eg(2)E_g^{(2)} and Fg(7)F_g^{(7)} modes and their respective Voigt functions, derived by fitting procedures.

References

References

  1. [2]V. Scherer, C. Janowitz, A. Krapf, H. Dwelk, D. Braun and R. Manzke, Applied Physics Letters, 2012, 100, 212108.
  2. [4]P. D. C. King, T. D. Veal, F. Fuchs, Ch. Y. Wang, D. J. Payne, R. Bourlange, H. Zhang, G. R. Bell, W. Cimalla, O. Ambacher, R. G. Egdell, F. Bechstedt and C. F. McConville, Phys. Rev. B, 2009, 79, 205211.
  3. [6]O. Bierwagen, Semicond. Sci. Technol., 2015, 30, 024001.
  4. [8]H. Von Wenckstern, Adv Electron Materials, 2017, 3, 1600350.
  5. [10]M. Marezio, Acta Cryst, 1966, 20, 723–728.
  6. [12]A. N. Tiwari, G. Khrypunov, G. Kurdzesau, D. L. Bätzner, A. Romeo and H. Zogg, Progress in Photovoltaics, 2004, 12, 33–38.
  7. [14]14 N. Barsan and U. Weimar, Journal of Electroceramics, 2001, 7, 143–167.
  8. [16]16 M. Higashiwaki, K. Sasaki, A. Kuramata, T. Masui and S. Yamakoshi, Physica Status Solidi (a), 2014, 211, 21–26.
  9. [18]18 H. V. Wenckstern, D. Splith, M. Purfürst, Z. Zhang, C. Kranert, S. Müller, M. Lorenz and M. Grundmann, Semicond. Sci. Technol., 2015, 30, 024005.
  10. [20]20 R. Hill, J. Phys. C: Solid State Phys., 1974, 7, 521–526.
  11. [22]22 J. E. N. Swallow, R. G. Palgrave, P. A. E. Murgatroyd, A. Regoutz, M. Lorenz, A. Hassa, M. Grundmann, H. Von Wenckstern, J. B. Varley and T. D. Veal, ACS Appl. Mater. Interfaces, 2021, 13, 2807–2819.
  12. [24]24 N. Ueda, H. Hosono, R. Waseda and H. Kawazoe, Applied Physics Letters, 1997, 71, 933–935.
  13. [26]26 K. Momma and F. Izumi, J Appl Crystallogr, 2011, 44, 1272–1276.
  14. [27]27 M. H. Carvalho, M. Rizzo Piton, O. M. Lemine, M. Bououdina, H. V. A. Galeti, S. Souto, E. C. Pereira, Y. Galvão Gobato and A. J. A. De Oliveira, Mater. Res. Express, 2018, 6, 025017.
  15. [28]28 A. Regoutz, R. Egdell, D. Morgan, R. Palgrave, H. Téllez, S. Skinner, D. Payne, G. Watson and D. Scanlon, Applied Surface Science, 2015, 349, 970–982.
  16. [29]29 B. Garcia-Domene, H. M. Ortiz, O. Gomis, J. A. Sans, F. J. Manjón, A. Muñoz, P. Rodríguez-Hernández, S. N. Achary, D. Errandonea, D. Martínez-García, A. H. Romero, A. Singhal and A. K. Tyagi, Journal of Applied Physics, 2012, 112, 123511.
  17. [30]Kranert et al. [bibliographic details not printed on this page]
  18. [31]31 H. Peelaers, D. Steiauf, J. B. Varley, A. Janotti and C. G. Van De Walle, Phys. Rev. B, 2015, 92, 085206.
  19. [32]32 L. Kavan, M. Zukalova, M. Ferus, J. Kürti, J. Koltai and S. Civiš, Phys. Chem. Chem. Phys., 2011, 13, 11583.
  20. [33]33 O. Frank, M. Zukalova, B. Laskova, J. Kürti, J. Koltai and L. Kavan, Phys. Chem. Chem. Phys., 2012, 14, 14567.
  21. [34]34 B. Manzen, P. Mazzolini, R. GIllen, A. Falkenstein, M. Martin, H. Tornatzky, J. Maultzsch, O. Bierwagen and M. R. Wagner, J. Mater. Chem. C, 2021, 9, 2311–2320.
  22. [35]35 Z. Galazka, R. Uecker and R. Fornari, Journal of Crystal Growth, 2014, 388, 61–69.
  23. [36]36 T. C. Damen, S. P. S. Porto and B. Tell, Phys. Rev., 1966, 142, 570–574.
  24. [37]37 P. Giannozzi, S. Baroni, N. Bonini, M. Calandra, R. Car, C. Cavazzoni, D. Ceresoli, G. L. Chiarotti, M. Cococcioni, A. Dabo, A. Dal Corso, S. De Gironcoli, S. Fabris, G. Fratesi, R. Gebauer, U. Gerstmann, C. Gougoussis, A. Kokalj, M. Lazzeri, L. Martin-Samos, N. Marzari, F. Mauri, R. Mazzarello, S. Paolini, A. Pasquarello, L. Paulatto, C. Sbraccia, S. Scandolo, G. Sclauzero, A. P. Seit­sonen, A. Smogunov, P. Umari and R. M. Wentzcovitch, J. Phys.: Condens. Matter, 2009, 21, 395502.
  25. [38]38 D. R. Hamann, Phys. Rev. B, 2013, 88, 085117.
  26. [39]39 M. Van Setten, M. Giantomassi, E. Bousquet, M. Verstraete, D. Hamann, X. Gonze and G.-M. Rignanese, Computer Physics Communications, 2018, 226, 39–54.
  27. [40]40 W. B. White and V. G. Keramidas, Spectrochimica Acta Part A: Molecular Spectroscopy, 1972, 28, 501–509.
  28. [41]41 M. Stokey, R. Korlacki, S. Knight, A. Ruder, M. Hilfiker, Z. Galazka, K. Irmscher, Y. Zhang, H. Zhao, V. Darakchieva and M. Schubert, Journal of Applied Physics, 2021, 129, 225102.
  29. [42]42 D. Liu, W. W. Lei, B. Zou, S. D. Yu, J. Hao, K. Wang, B. L. Liu, Q. L. Cui and G. T. Zou, Journal of Applied Physics, 2008, 104, 083506.
  30. [43]43 G. Hoffmann, M. Budde, P. Mazzolini and O. Bierwagen, APL Materials, 2020, 8, 031110.
  31. [44]44 L. He, F. Liu, G. Gautier, M. J. T. Oliveira, M. A. L. Marques, F. D. Vila, J. J. Rehr, G.-M. Rignanese and A. Zhou, Phys. Rev. B, 2014, 89, 064305.
  32. [45]45 A. Klein, A. Frebel, K. A. Creutz and B. Huang, Phys. Rev. Materials, 2024, 8, 044601.
  33. [46]46 H. Fukushima, T. Kou, H. Shima, H. Funakubo, H. Uchida, T. Katoda and K. Nishida, 2015 Joint IEEE International Symposium on the Applications of Ferroelectric (ISAF), International Symposium on Integrated Functionalities (ISIF), and Piezoelectric Force Microscopy Workshop (PFM), Singapore, Singapore, 2015, pp. 28–31.

Paper details

vlnc:W_h5764dvj
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents