Atomic Layer Molecular Beam Epitaxy of Kagome Magnet RMnSn (R = Er, Tb) Thin Films
Abstract
Kagome lattices have garnered substantial interest because their band structure consists of topological flat bands and Dirac cones. The RMnSn (R = rare earth) compounds are particularly interesting because of the existence of large intrinsic anomalous Hall effect (AHE) which originates from the gapped Dirac cones near the Fermi level. This makes RMnSn an outstanding candidate for realizing the high-temperature quantum anomalous Hall effect. The growth of RMnSn thin films is beneficial for both fundamental research and potential applications. However, most of the studies on RMnSn have focused on bulk crystals so far, and the synthesis of RMnSn thin films has not been reported so far. Here we report the atomic layer molecular beam epitaxy growth, structural and magnetic characterizations, and transport properties of ErMnSn and TbMnSn thin films. It is especially noteworthy that TbMnSn thin films have out-of-plane magnetic anisotropy, which is important for realizing the quantum anomalous Hall effect. Our work paves the avenue toward the control of the AHE using devices patterned from RMnSn thin films.
Materials with layered kagome structures provide an ideal platform for studying the interplay between band structure and magnetism. In momentum space, a two-dimensional kagome lattice manifests Dirac cones at the K points[1, 2], saddle points at the M points[3, 4], and a flat band across the Brillouin zone[5, 6]. The introduction of magnetism and spin-orbital coupling further opens a gap at the band touching points, leading to topologically non-trivial electronic states[7, 8, 9]. In real space, non-trivial spin textures (e.g. magnetic skyrmions) have been observed in kagome magnets[10, 11].
Recently, RMn₆Sn₆ (R = rare earth) compounds have emerged as a new family of topological kagome magnets[12, 13]. The Mn atoms in RMn₆Sn₆ form Mn₃ kagome layers and the spin ordering of the Mn₃ layers is largely affected by the R atoms. Previous studies on bulk crystals report that R = Gd, Tb, Dy, and Ho give rise to ferromagnetic coupling of Mn spins, while R = Er, Tm, and Lu lead to antiferromagnetic coupling of Mn spins at zero field[14, 15, 16]. Rare earth elements in RMn₆Sn₆ compounds also provide one additional knob for tuning the magnetocrystalline anisotropy (MCA) which is connected to the Dirac gap opening[17]. Large Berry-curvature-induced intrinsic anomalous Hall effect (AHE) may originate from the gapped Dirac cones close to the Fermi level, because the intrinsic anomalous Hall conductivity (AHC) is connected to the Dirac gap opening and the Dirac cone position through[18]:
Notably, TbMn₆Sn₆ bulk crystals exhibit out-of-plane magnetic anisotropy, which leads to a 34 meV Dirac gap opening at 130 meV above the Fermi level[12], and band structure calculations predict the quantum anomalous Hall effect (QAHE) if the Fermi level could be tuned into the gap. Experimentally, the observation of a giant intrinsic AHC of per kagome layer in TbMn₆Sn₆ bulk crystals[12] makes the RMn₆Sn₆ family of materials attractive for QAHE. To this end, the growth of RMn₆Sn₆ thin films provides opportunities for tuning the band structure and Fermi level through epitaxial strain, chemical doping, or voltage gating. However, all of the reported works have focused on bulk crystals of RMn₆Sn₆, while studies on their thin film counterparts have been missing. Therefore, the development of epitaxial RMn₆Sn₆ thin films is highly desired.
In this paper, we report the growth of (0001)-oriented thin films of ErMn₆Sn₆ and TbMn₆Sn₆ using atomic layer molecular beam epitaxy (AL-MBE) and characterize their magnetic and transport properties. The films are grown on Pt(111) buffer layers on Al₂O₃ (0001) substrates. Various methods are employed to characterize the structure of our samples, including in-situ reflection high energy electron diffraction (RHEED), X-ray diffraction (XRD), and atomic force microscopy (AFM). We demonstrate that the magnetic properties of RMn₆Sn₆ thin films can be tuned through the selection of rare earth element . ErMn₆Sn₆ thin films favor in-plane (IP) magnetization, while TbMn₆Sn₆ thin films undergo an out-of-plane (OOP) to IP spin-reorientation transition (SRT) as the temperature increases above 300 K. Lastly, we find that the longitudinal resistance of RMn₆Sn₆/Pt bilayers do not follow a simple parallel resistor model but instead depends on the electron mean free path and can be explained qualitatively by the Fuchs-Sondheimer model.
The crystal structure of RMn₆Sn₆ is displayed in Figure 1, featuring a hexagonal lattice (space group , lattice constants Å and Å) with atomic layers stacked along the c-axis[19]. In each unit cell, there are two kagome Mn₃ layers closely neighboured by two Sn₁ layers, with one honeycomb Sn₂ layer inserted between two Sn₁ layers, and one RSn₂ layer inserted between Mn₃ kagome layers. Inspired by this stacking sequence, we develop an AL-MBE recipe to grow ErMn6Sn6 and TbMn6Sn6 thin films on epitaxial Pt(111) buffer layers on Al2O3(0001) substrates. In AL-MBE, atomic layers are grown sequentially by opening and closing the appropriate MBE source shutters with precise timing. A similar growth strategy allowed us to synthesize thin films of another kagome magnet, Fe3Sn2, which also has a hexagonal layered lattice structure[20].
Figure 1. AL-MBE Growth of RMn6Sn6 thin films. (a). Lattice structure of RMn6Sn6 viewed from the side. In each unit cell, RMn6Sn6 consists of alternating stacking of RSn2, Mn3, Sn1, Sn2, Sn1, Mn3 layers (from bottom to top) along c-axis. (b). In-plane lattice structure of kagome Mn3 (top left), triangular Sn1 (top right), honeycomb Sn2 (bottom left), and RSn2 (bottom right) layers. (c, d). in-situ RHEED pattern of 20 nm ErMn6Sn6 sample grown on Pt(111) buffer layer on Al2O3(0001) substrate. (d). in-situ RHEED pattern of 20 nm TbMn6Sn6 sample grown on Pt(111) buffer layer on Al2O3(0001) substrate.
The base pressure of the growth chamber is Torr. The Al2O3(0001) substrates (MTI corporation) are annealed in air at 1000 °C for 3 hours, then degassed in-situ at 500 °C for 30 minutes to prepare a flat and clean surface. A 5 nm epitaxial Pt(111) buffer layer is subsequently grown on Al2O3(0001) following the recipe described in our previous work[20]. The ErMn6Sn6(0001) and TbMn6Sn6(0001) thin films are grown on Pt(111) buffer layers at 100 °C and 80 °C, respectively using the AL-MBE recipe described below. First, the kagome Mn3 layer and hexagonal Sn1 layer are co-deposited with flux ratio Mn:Sn = 3:1, then the honeycomb RSn2 is deposited with flux ratio Er:Sn (or Tb:Sn) = 2:1, then another hexagonal Sn1 layer and kagome Mn3 layer are co-deposited, then one Sn2 layer is deposited. The aforementioned shutter growth sequence is repeated until the desired thickness (typically 20 nm) of RMn6Sn6 is achieved. Typical deposition rates are 1.6 Å/min, 1.6 Å/min, 3.9 Å/min, and 2.8 Å/min for Er, Tb, Mn, and Sn, respectively. After growth, a 5 nm CaF2 layer is deposited to prevent sample oxidation.
The in-situ RHEED patterns of ErMn6Sn6 and TbMn6Sn6 are monitored during the growths. The RHEED patterns of a 20 nm ErMn6Sn6 thin film and a 20 nm TbMn6Sn6 thin film along Al2O3[] direction are shown in Figure 1c and Figure 1d, respectively. The RHEED patterns are generally streaky, suggesting the morphology of our RMn6Sn6 thin films is dominated by two-dimensional terraces with finite sizes, although some three-dimensional features also exist as spots. The RHEED pattern suggests the in-plane lattice constants for our samples are Å, and Å, respectively, and the in-plane epitaxial relationship is RMn6Sn6[]‖Pt[]‖Al2O3[].
We perform XRD measurements to confirm the crystallographic structures of ErMn6Sn6 and TbMn6Sn6 thin films. The X-ray is from the Cu-Kα radiation, with a wavelength of 1.5406 Å. Figure 2a shows the XRD data of a 20 nm ErMn6Sn6 thin film. Next to the substrate peaks at 41.57° and 90.60°, two major peaks are found at 39.78° and 85.46°, respectively. These peaks are attributed to Pt(111) and Pt(222) peaks because their angles convert to out-of-plane lattice constants of 2.275 Å and 2.270 Å, respectively. These values are close to the out-of-plane lattice constant of Pt along (111) direction ( Å = 2.265 Å)[21]. ErMn6Sn6(0004) and ErMn6Sn6(0008) peaks appear as nearby shoulder peaks at 40.36° and 87.63°, respectively. The out-of-plane lattice constant of ErMn6Sn6 extracted from (0004) peak is 8.93 Å, which is close to but slightly smaller than the reported bulk value of 9.0006 Å[22].
Figure 2. Structural characterizations of RMn6Sn6 thin films. (a). XRD data of ErMn6Sn6(20 nm)/Pt(5 nm) sample. (b). AFM image of ErMn6Sn6(20 nm)/Pt(5 nm) sample. (c). XRD data of TbMn6Sn6(25 nm)/Pt(5 nm) sample. (d). AFM image of TbMn6Sn6(25 nm)/Pt(5 nm) sample.
For TbMn6Sn6 thin film, the general characteristics of the XRD data are similar to ErMn6Sn6. To the right of Pt(111) peak which is at 39.88°, the TbMn6Sn6(0004) peak is found as a shoulder peak (see Figure 2c). A double Gaussian peak fitting yields TbMn6Sn6(0004) peak position of , which corresponds to an out-of-plane lattice of . This is also smaller than the reported bulk value of [22].
We characterize the surface morphology of ErMnSn and TbMnSn thin films using AFM. Figure 2b shows the AFM image of a 20 nm ErMnSn sample grown at C. The film has a continuous and flat surface with sub-micron grain size. The root-mean-square (rms) roughness of the 20 nm ErMnSn sample is 1.02 nm. Figure 2b shows the AFM image of a 20 nm TbMnSn sample grown at C. The rms roughness of the 20 nm TbMnSn sample is 1.45 nm.
To investigate the magnetic properties of the RMnSn thin films, we perform SQUID magnetometer measurements. Figure 3a shows the IP (blue) and OOP (red) hysteresis loops of a 20 nm ErMnSn thin film. The IP hysteresis loop has a smaller saturation field of 0.2 Tesla, while the OOP hysteresis loop has a larger saturation field of 1.7 Tesla, indicating ErMnSn has easy-plane
Figure 3. Magnetic properties of ErMn₆Sn₆ and TbMn₆Sn₆ thin films. (a - c). Magnetic properties of 20 nm ErMn₆Sn₆ thin film measured with out-of-plane (OOP, red) and in-plane (IP, blue) geometries. (a). M vs. H hysteresis loops measured at T=300 K. (b). M vs. H hysteresis loop measured at T=5 K. (c). M vs. T curve. (d - f). Magnetic properties of 20 nm TbMn₆Sn₆ thin film measured with out-of-plane (OOP, red) and in-plane (IP, blue) geometries. (d). M vs. H hysteresis loops measured at T=300 K. (e). M vs. H hysteresis loop measured at T=5 K. (f). M vs. T curve, showing uniaxial anisotropy for T<300 and an OOP-to-IP spin reorientation at T=300 K.
anisotropy at room temperature. The saturation magnetization of ErMnSn thin film is (212 kA/m) at room temperature. The IP and OOP hysteresis loops of ErMnSn at K are shown in Figure 3b. At K, both IP and OOP hysteresis loops show much larger coercive fields and larger saturation fields, while the saturation field of the OOP hysteresis loop is still larger than the IP hysteresis loop. The IP loop exhibits a sharper switching behavior, with the coercive field of 0.47 Tesla. Meanwhile, the OOP hysteresis loop becomes narrower near zero field and wider at higher fields. The coercive field of the OOP hysteresis loop is 0.30 Tesla.
We also measure the temperature-dependence of remanence magnetization of the ErMnSn thin film, as shown in Figure 3c. For both OOP (the red curve) and IP (the blue curve) measurements, the sample is cooled down under 7 Tesla applied field, and measured at low field while heating up. A 30 mT field is applied to set the polarity of the magnetization. From the temperature-dependent magnetization curve, the Curie temperature of the 20 nm ErMn₆Sn₆ thin film is determined to be 353 K, signified by a drop of magnetization to zero. This Curie temperature is consistent with the reported value of 350 K on ErMn₆Sn₆ bulk crystals[16].
Compared to ErMn₆Sn₆ thin films, TbMn₆Sn₆ thin films show different magnetic properties. Figure 3d and Figure 3e show the hysteresis loops of a 25 nm TbMn₆Sn₆ thin film at 300 K and 5 K, respectively. At K, the OOP (red) and IP (blue) hysteresis loops of TbMn₆Sn₆ are almost identical, with a saturation field of 0.6 Tesla (see Figure 3d). The saturation magnetization of TbMn₆Sn₆ is 3.9 /f.u. (154 kA/m) at room temperature. While cooling down to K, the OOP hysteresis loop of TbMn₆Sn₆ exhibits a square shape, with tails extended to 5 Tesla, as shown in Figure 3e. Meanwhile, the IP hysteresis loop shows a gradual switching behavior. At zero field, the OOP remanence magnetization is much larger than the IP remanence magnetization, suggesting that TbMn₆Sn₆ favors OOP at K.
The perpendicular magnetic anisotropy is highly unusual for epitaxial kagome magnet thin films, as most of the previously reported kagome magnet thin films have easy-plane anisotropy[20, 23, 24, 25, 26, 27]. Even for epitaxial Fe₃Sn₂ whose bulk form has MCA along the c-axis, the MCA is overcome by the magnetic shape anisotropy (MSA) which favors easy-plane anisotropy. As a result, both
MBE-grown and sputtered Fe₃Sn₂ thin films manifest easy-plane anisotropy[20, 25]. However, in TbMn₆Sn₆ thin films, the MCA is strong enough to overcome the MSA and leads to an easy-axis anisotropy at low temperatures. It is noteworthy that such large magnetocrystalline anisotropy along the c-axis opens a gap at the Dirac cone, leading to a large intrinsic AHE[12, 13].
The perpendicular magnetic anisotropy of the TbMn₆Sn₆ thin film sample at low temperatures is further confirmed by the temperature-dependent SQUID measurements, as shown in Figure 3f. A 20 mT field is applied to set the polarity of the magnetization. Below 300 K, the OOP magnetization (red curve) is always larger than the IP magnetization (blue curve). A crossover between IP and OOP magnetization happens at K above which the IP magnetization becomes larger than the OOP magnetization. This crossover suggests an OOP-to-IP SRT as the temperature increases above 300 K. A similar temperature-induced SRT has been reported at 310 K in TbMn₆Sn₆ bulk crystals[16] and is reported to be related to the formation of magnetic skyrmions[11]. Both IP and OOP magnetization eventually disappears above the Curie temperature which is determined to be 380 K. This Curie temperature is lower than the reported value of 423 K on TbMn₆Sn₆ bulk crystals[14].
We next discuss the transport properties of ErMn₆Sn₆/Pt and TbMn₆Sn₆/Pt thin films. The transport measurements are performed using Quantum Design Physical Property Measurement System (PPMS) on 300 µm×100 µm Hall bar devices patterned from ErMn₆Sn₆/Pt and TbMn₆Sn₆/Pt thin films. The longitudinal resistance of the Hall bar devices at
zero field is shown in Figure 4a. Comparing between TbMn₆Sn₆(25 nm)/Pt(5 nm) bilayer (the red curve) and Pt(5 nm) single layer (the black dashed curve), the bilayer resistance is lower than the Pt single layer resistance for higher temperatures (T>200 K). This is consistent with the parallel resistor model in which the TbMn₆Sn₆ and Pt layers are modeled as two resistors connected in parallel and therefore have smaller resistance than the Pt layer alone. The parallel resistor model has been widely used to extract the resistivity of kagome material thin films grown on metallic buffer layers[24, 25, 26, 28]. However, at low temperatures (T<150 K), the resistance of the TbMn₆Sn₆(25 nm)/Pt(5 nm) bilayer is larger than that of the Pt(5 nm) single layer. This is the opposite of what one would expect from the parallel resistor model. The comparison between ErMn₆Sn₆(20 nm)/Pt(5 nm) bilayer (the green curve) and Pt(5 nm) single layer shows a similar trend that the bilayer resistance is smaller than the Pt single layer resistance for T>200 K and larger than the Pt single layer resistance for T<100 K. The deviation from the parallel resistor model is more pronounced for the bilayers with smaller kagome layer thicknesses. For example, for TbMn₆Sn₆(5 nm)/Pt(5 nm) bilayer (the blue curve), the resistance is larger than Pt(5 nm) single layer from T=5 K up to T=300 K.
Figure 4. Transport measurements of ErMn₆Sn₆/Pt and TbMn₆Sn₆/Pt bilayers. (a). Resistance of 300 µm×100 µm devices patterned from TbMn₆Sn₆(25 nm)/Pt(5 nm) bilayer (red), TbMn₆Sn₆(5 nm)/Pt(5 nm) bilayer (blue), ErMn₆Sn₆(20 nm)/Pt(5 nm) bilayer, and 5 nm Pt single layer (black, dashed), respectively. (b). Anomalous Hall resistivity of ErMn₆Sn₆(20 nm)/Pt(5 nm) bilayer measured at different temperatures ranging from 2 K to 300 K. (c). Anomalous Hall resistivity of TbMn₆Sn₆(25 nm)/Pt(5 nm) bilayer measured at different temperatures ranging from 2 K to 300 K.
The deviation from the parallel resistor model can be explained by Fuchs-Sondheimer theory, in which the resistance of bilayers depends not only on the bulk resistance of two materials but also the mean free path of electrons in them[29, 30]. In the Fuchs-Sondheimer model, when the electron mean free path is much smaller than the thickness of each layer, the bilayer resistance is smaller than the resistance of individual layers. In this case, the Fuchs-Sondheimer model converges to the parallel resistor model. However, when the electron mean free path is much larger than the thickness of each layer, the bilayer resistance is larger than the resistance of individual layers, which is more similar to the series resistor model. Especially in an infinite superlattice consisting of alternating stacking of two materials with the same thickness, in the thin layer limit and under the assumption that the electron densities in two materials are identical, the averaged resistivity of the superlattice is exactly equal to the average value of the bulk resistivity of the two materials[31]. In our RMn₆Sn₆/Pt bilayer samples, the scattering length is shorter than the individual layer thickness at high temperatures, therefore the bilayer resistance is smaller than the resistance of Pt layer, similar to the parallel resistor model. Meanwhile, at low temperatures or with smaller thicknesses, the mean free path becomes longer than the individual layer thickness, and the bilayer resistance is larger than the resistance of Pt layer, similar to the series resistor model. Due to the complexity of data analysis, extracting the intrinsic longitudinal resistivity of ErMn₆Sn₆ and TbMn₆Sn₆ from bilayer resistance is outside the scope of this paper.
We also measured the anomalous Hall effect (AHE) of ErMnSn(20 nm)/Pt(5 nm) and TbMnSn(25 nm)/Pt(5 nm) bilayers, as shown in Figure 4b and Figure 4c, respectively. Here, the anomalous Hall resistivity is calculated by multiplying the anomalous Hall resistance by the thickness of the RMnSn layer. For ErMnSn, the AHE hysteresis loop at K has a large remanence, a low-field opening (with the coercive field of T) and a large saturation field ( T). The opening of the hysteresis loop decreases quickly as the temperature increases, and almost disappears before the temperature reaches 100 K. For TbMnSn, the AHE hysteresis loops are relatively square, with the coercive field decreasing as temperature increases. For both materials, as temperature increases from 2 K to 300 K, the amplitude of AHE first increases, reaches the maximum value between 200 K and 250 K, and then decreases. This behavior is understood as follows. The anomalous Hall resistivity scales with where is between 1 and 2. The intrinsic and side-jump contributions yield and skew-scattering yields .[32] Since increases with temperature (Figure 4a), this scaling explains the enhancement of with temperature as observed below 200 K. On the other hand, the reduction of AHE resistivity at higher temperatures can be attributed to the decrease in magnetization as the temperature approaches the Curie temperature.
In conclusion, this study demonstrates the synthesis of c-plane ErMnSn and TbMnSn thin films using atomic layer molecular beam epitaxy. A combination of RHEED, XRD, and AFM confirms the structure of the samples. Magnetization measurements show that ErMnSn has easy-plane anisotropy from 5 K to room temperature, while TbMnSn has perpendicular magnetic anisotropy at low temperature and an OOP-to-IP spin reorientation as the temperature increases above 300 K. Transport measurements at low temperatures show that the longitudinal resistance of the RMnSn/Pt bilayer is larger than that of the Pt layer alone, which is inconsistent with the parallel resistance model. On the other hand, such behavior is qualitatively explained by the Fuchs-Sondheimer model. Lastly, since both ErMnSn and TbMnSn are synthesized under similar conditions, other members of the RMnSn family could likely be grown using similar AL-MBE recipes. These results create a solid foundation for future research and applications based on RMnSn thin films.
Acknowledgments
We acknowledge Daniel Halbing, Katherine Robinson, and Xueshi Gao for their assistance in the construction of the evaporation cells. S.C. was supported by NSF Grant No. CHE-1935885. I.L. was supported by the Center for Emergent Materials, an NSF MRSEC, under Grant No. DMR-2011876. W.Z. was supported by AFOSR MURI 2D MAGIC Grant No. FA9550-19-1-0390 and the US Department of Energy Grant No. DE-SC0016379.
Author Declarations
Conflict of Interest
The authors declare no conflicts of interest to disclose.
Data Availability Statement
The data that support the findings of this study are available from the corresponding author upon reasonable request.
References
- [1]K. Kuroda, T. Tomita, M.-T. Suzuki, C. Bareille, A. Nugroho, P. Goswami, M. Ochi, M. Ikhlas, M. Nakayama, S. Akebi, R. Noguchi, R. Ishii, N. Inami, K. Ono, H. Kumigashira, A. Varykhalov, T. Muro, T. Koretsune, R. Arita, S. Shin, T. Kondo, and S. Nakatsuji, “Evidence for magnetic Weyl fermions in a correlated metal,” Nature materials 16, 1090–1095 (2017).
- [2]L. Ye, M. Kang, J. Liu, F. Von Cube, C. R. Wicker, T. Suzuki, C. Jozwiak, A. Bostwick, E. Rotenberg, D. C. Bell, L. Fu, R. Comin, and J. G. Checkelsky, “Massive Dirac fermions in a ferromagnetic kagome metal,” Nature 555, 638–642 (2018).
- [3]M. Kang, S. Fang, J.-K. Kim, R. R. Ortiz, S. H. Ryu, J. Kim, J. Yoo, G. Sangiovanni, D. Di Sante, B.-G. Park, C. Jozwiak, A. Bostwick, E. Rotenberg, E. Kaxiras, S. D. Wilson, J.-H. Park, and R. Comin, “Magnetic Weyl points, Fermi arcs, and origin of charge order in topological kagome superconductor CsV3Sb5,” Nature Physics 18, 301–308 (2022).
- [4]X. Teng, J. S. Oh, H. Tan, L. Chen, J. Huang, B. Gao, J.-X. Yin, J.-H. Chu, M. Hashimoto, D. Lu, C. Jozwiak, A. Bostwick, E. Rotenberg, G. E. Granroth, B. Yan, R. J. Birgeneau, P. Dai, and M. Yi, “Magnetism and charge density wave order in kagome FeGe,” Nature Physics 1–9 (2023).DOI
- [5]M. Kang, S. Fang, L. Ye, H. C. Po, J. Denlinger, C. Jozwiak, A. Bostwick, E. Rotenberg, E. Kaxiras, J. G. Checkelsky, and R. Comin, “Topological flat bands in frustrated kagome lattice CoSn,” Nature communications 11, 4004 (2020).
- [6]M. Kang, L. Ye, S. Fang, J.-S. You, A. Levitan, M. Han, J. I. Facio, C. Jozwiak, A. Bostwick, E. Rotenberg, M.-K. Chan, R. D. McDonald, D. Graf, K. Kaznatcheev, E. Vescovo, D. C. Bell, E. Kaxiras, J. van den Brink, M. Richter, M. P. Ghimire, C. J. G., and R. Comin, “Dirac fermions and flat bands in the ideal kagome metal FeSn,” Nature materials 19, 163–169 (2020).DOI
- [7]K. Sun, Z. Gu, H. Katsura, and S. D. Sarma, “Nearly flatbands with nontrivial topology,” Physical Review Letters 106, 236803 (2011).pubmed.ncbi.nlm.nih.gov/21770533
- [8]H.-M. Guo and M. Franz, “Topological insulator on the kagome lattice,” Physical Review B 80, 113102 (2009).DOI
- [9]A. Bolens and N. A. Nagaosa, “Topological states on the breathing kagome lattice,” Physical Review B 99, 165141 (2019).DOI
- [10]Z. Hou, W. Ren, B. Ding, G. Xu, Y. Wang, B. Yang, Q. Zhang, Y. Zhang, E. Liu, F. Xu, W. Wang, G. Wu, X. Zhang, B. Shen, and Z. Zhang, “Observation of various and spontaneous magnetic skyrmionic bubbles at room temperature in a frustrated kagome magnet with uniaxial magnetic anisotropy,” Advanced Materials 29, 1701144 (2017).
- [11]Z. Li, Q. Yin, Y. Jiang, Z. Zhu, Y. Gao, S. Wang, J. Shen, T. Zhao, J. Cai, H. Lei, S.-Z. Lin, Y. Zhang, and B. Shen, “Discovery of topological magnetic textures near room temperature in quantum magnet TbMn₆Sn₆,” Advanced Materials, 2211164 (2023).DOI
- [12]J.-X. Yin, W. Ma, T. A. Cochran, X. Xu, S. S. Zhang, H.-J. Tien, N. Shumiya, G. Cheng, K. Jiang, B. Lian, Z. Song, G. Chang, I. Belopolski, D. Multer, M. Litskevich, Z.-J. Cheng, X. P. Yang, B. Svidler, H. Zhou, H. Lin, T. Neupert, Z. Wang, N. Yao, T.-R. Chang, S. Jia, and M. Z. Hasan, “Quantum-limit Chern topological magnetism in TbMn₆Sn₆,” Nature 583, 533–536 (2020).DOI
- [13]W. Ma, X. Xu, J.-X. Yin, H. Yang, H. Zhou, Z.-J. Cheng, Y. Huang, Z. Qu, F. Wang, M. Z. Hasan, and S. Jia, “Rare earth engineering in RMn₆Sn₆ (R = Gd - Tm, Lu) topological kagome magnets,” Physical review letters 126, 246602 (2021).DOI
- [14]G. Venturini, B. C. El Idrissi, and B. Malaman, “Magnetic properties of RMn₆Sn₆ (R= Sc, Y, Gd–Tm, Lu) compounds with HfFe₆Ge₆ type structure,” Journal of magnetism and magnetic materials 94, 35–42 (1991).DOI
- [15]B. Malaman, G. Venturini, R. Welter, J. Sanchez, P. Vulliet, and E. Ressouche, “Magnetic properties of RMn₆Sn₆ (R= Gd–Er) compounds from neutron diffraction and Mössbauer measurements,” Journal of magnetism and magnetic materials 202, 519–534 (1999).DOI
- [16]D. Clatterbuck and K. Gschneidner Jr., “Magnetic properties of RMn₆Sn₆ (R= Tb, Ho, Er, Tm, Lu) single crystals,” Journal of magnetism and magnetic materials 207, 78–94 (1999).DOI
- [17]Z.-J. Cheng, I. Belopolski, H.-J. Tien, T. A. Cochran, X. P. Yang, W. Ma, J.-X. Yin, D. Chen, J. Zhang, C. Jozwiak, et al., “Visualization of tunable Weyl line in A–A stacking kagome magnets,” Advanced Materials 35, 2205927 (2023).DOI
- [18]N. Sinitsyn, A. MacDonald, T. Jungwirth, V. Dugaev, and J. Sinova, “Anomalous Hall effect in a two-dimensional Dirac band: The link between the Kubo-Streda formula and the semi-classical Boltzmann equation approach,” Physical Review B 75, 045315 (2007).
- [19]B. Malaman, G. Venturini, and B. Roques, “New ternary stannides: MMn₆Sn₆ (M = Sc, Y, Sm, Gd-Tm, Lu) AND ScFe₆Sn₆,” Materials research bulletin 23, 1629–1633 (1988).
- [20]S. Cheng, B. Wang, I. Lyalín, N. Bagués, A. J. Bishop, D. W. McComb, and R. K. Kawakami, “Atomic layer epitaxy of kagome magnet Fe₃Sn₂ and Sn-modulated heterostructures,” APL Materials 10, 061112 (2022).DOI
- [21]H. Rooksby and B. Lewis, “Relations between the structures of phases in the system platinum-molybdenum,” Journal of the Less Common Metals 6, 451–460 (1964).DOI
- [22]D. Clatterbuck, R. Lange, and K. Gschneidner Jr, “Magneto-optical properties of RMn₆Sn₆ (R= Gd, Tb, Dy, Ho, Er, Tm, Lu) single crystals,” Journal of magnetism and magnetic materials 195, 639–645 (1999).DOI
- [23]J. M. Taylor, A. Markou, E. Lesne, P. K. Sivakumar, C. Luo, F. Radu, P. Werner, C. Felser, and S. S. Parkin, “Anomalous and topological Hall effects in epitaxial thin films of the noncollinear antiferromagnet Mn₃Sn,” Physical Review B 101, 094404 (2020).DOI
- [24]D. Hong, N. Anand, C. Liu, H. Liu, I. Arslan, J. E. Pearson, A. Bhattacharya, and J. Jiang, “Large anomalous nernst and inverse spin-hall effects in epitaxial thin films of kagome semimetal Mn₃Ge,” Physical Review Materials 4, 094201 (2020).DOI
- [25]D. Khadka, T. Thapaliya, S. H. Parra, J. Wen, R. Need, J. M. Kikkawa, and S. Huang, “Anomalous Hall and Nernst effects in epitaxial films of topological kagome magnet Fe₃Sn₂,” Physical review materials 4, 084203 (2020).DOI
- [26]Y. Cheng, S. Yu, M. Zhu, J. Hwang, and F. Yang, “Tunable topological Hall effects in noncollinear antiferromagnet Mn₃Sn/Pt bilayers,” APL Materials 9, 051121 (2021).DOI
- [27]K. Fujiwara, Y. Kato, H. Abe, S. Noguchi, J. Shiogai, Y. Niwa, H. Kumigashira, Y. Motome, and A. Tsukazaki, “Curvature contributions of kagome-lattice fragments in amorphous Fe–Sn thin films,” Nature Communications 14, 3399 (2023).DOI
- [28]T. Thapaliya, T. Yoo, S. Hurtado, N. D. Arndt, R. Need, J. M. Kikkawa, H. Kim, and S. Huang, “High-quality epitaxial thin films of topological kagome metal CoSn by magnetron sputtering,” Applied Physics Letters 119, 201902 (2021).DOI
- [29]K. Fuchs, “The conductivity of thin metallic films according to the electron theory of metals,” in Mathematical Proceedings of the Cambridge Philosophical Society, Vol. 34 (Cambridge University Press, 1938) pp. 100–108.DOI
- [30]E. Sondheimer, “The mean free path of electrons in metals,” Advances in Physics 1, 1–42 (1952).
- [31]A. Misra, M. Hundley, D. Hristova, H. Kung, T. Mitchell, M. Nastasi, and J. Embury, “Electrical resistivity of sputtered Cu/Cr multilayered thin films,” Journal of Applied Physics 85, 302–309 (1999).DOI
- [32]Y. Tian, L. Ye, and X. Jin, “Proper scaling of the anomalous Hall effect,” Physical review letters 103, 087206 (2009).DOI