Abstract

Group IV color centers in diamond – silicon, germanium, tin, and lead-vacancy centers – are a promising platform for quantum networking. Typical Group-IV creation utilizes ion implantation during diamond growth that leaves the color centers with a broad depth distribution and damage-induced strain inhomogeneity. Deterministic placement and damage reduction in Group IV generation are essential for improving this platform. In this letter, we report on the localization of germanium-vacancy (GeV−^-) to a << 10 nm layer via the timed injection of GeH4_4 during microwave plasma chemical vapor deposition. In this layer we have realized 17 ppm of Ge and a strain-free environment for the GeV−^-. Subsequent electron irradiation and annealing have generated a sheet density of 0.12 GeV−^-/μμm2^2. The minimal damage from color center generation mitigates spectral inhomogeneity and allows spectral resolution of isotopic clusters, with the best cluster having an inhomogeneous distribution of 2.14 GHz and an average linewidth of 47±1147 \pm 11 MHz. Our study gives insight into formation dynamics of GeV−^- in delta-doped systems and estimates our vacancy to GeV−^- yield to be ≥\geq 90%, establishing an athermal nearest-neighbor formation model. We further characterized the spin T2∗T_2^* and set a lower bound of 730 ns, limited by a paramagnetic defect.

Introduction

Group IV color centers in diamond have coherent spin and optical interfaces that are utilized in quantum network architectures and in investigations of many-body physics. These color centers are insensitive to first-order electric field noise and have demonstrated excellent single qubit properties in nanophotonic and strained devices[1, 2, 3] [4]. Moreover, entangled two qubit and blind computing has been demonstrated with Group IVs, enabled by quantum frequency conversion5–7. In parallel, heterogeneous integration with χ(2)\chi^{(2)} materials such as lithium niobate has been used to demonstrate phononic and photonic control and explore transduction schemes8,9. More recently, two-dimensional arrays of Group-IV centers in diamond were investigated as a platform to engineer compact optics10,11, and could be extended to enable emergent cooperative effects12, or squeezed spin13,14 in large identical ensembles.

Current synthesis typically relies on ion implantation, where dopant-lattice collisions generate Frenkel pairs and strain-inducing vacancy clusters. Due to the large strain susceptibility of group IV color center, this heterogeneity causes significant spectral inhomogeneity[1] [15] and other electrostatic issues16. Additionally, for device integration, deterministic spatial localization is key for achieving desired performance17. However, implanted ions present an inherent straggle on the order of tens-of-nm (scaling with the implantation energy)17–19. High pressure high temperature (HPHT) annealing techniques, in which the diamond lattice is brought to thermodynamic regimes that promote sp3\mathrm{sp}^{3} stability, can reduce inhomogeneity to desireably gigahertz (GHz) levels20–23 but does not address depth localization. Shallow implantation with subsequent overgrowth, demonstrated to generate SnV ensembles with a straggle under 3 nm24, can provide excellent depth localization but with significant 100 GHz inhomogeneity.

Alternatively, growth-based doping can yield precise control over depth localization while sidestepping ion-implantation-induced lattice damage. Growth-based doping methods such as HPHT25–28 and chemical vapor deposition (CVD)15,29–37 have been used to generate optically homogeneous Group-IV color centers38 with spin properties that surpass implantation-derived results. By further leveraging intrinsic control over precursor residency times and slow growth rates, depth-localization of color centers (i.e. δ\delta-doping39) with accuracies of ≈1.6\approx1.6 nm was shown to be possible15,29,34,40,41.

In this work, we report on the in-situ synthesis of delta-doped germanium vacancy centers in isotopically purified diamond. We investigate in-situ germanium incorporation and depth localization, followed by subsequent conversion into GeV−\mathrm{GeV}^{-} centers through post-processing. Our approach allows us to decouple key formation pathways by quantitatively studying vacancy conversion efficiencies, providing insight into defect formation dynamics. Photoluminescence spectra of the GeV−\mathrm{GeV}^{-} reveal minimal strain in the doped layer and isotopic resolution of the GeV−\mathrm{GeV}^{-} phonon lines. We observe excellent optical homogeneity within each isotopic grouping. Finally, all-optical measurements of spin coherence reveal coherence times comparable to implantation-created GeV, likely limited by an unknown paramagnetic species.

Diamond Growth and Processing

Diamond overgrowth was performed on a strain released42 2x2x0.5 mm substrate (EL grade, ElementSix) in a microwave plasma chemical vapor deposition (MPCVD) chamber, using a ≥99.95\ge99.95 at.% iso-purified 12CH4{}^{12}\mathrm{CH}_{4} carbon precursor with a 0.1:100 ratio of 12CH4:H2{}^{12}\mathrm{CH}_{4}:{\mathrm{H}}_{2} (≈14.2\approx14.2 nm/h growth rate). Growth was performed at an on-substrate temperature in the range of 800–875 °C as measured via optical pyrometer and a plasma power density of ≈24\approx24 W/cm3^{3}, at a pressure of 25 Torr. Ge doping was achieved by introducing diluted germane, with a total dilution of GeH4:H2\mathrm{GeH}_{4}:{\mathrm{H}}_{2} of 1.75:1000. The sample geometry is schematized in the inset of figure 1b, with the associated Secondary Ion Mass Spectroscopy (SIMS) depth profile showed in figure 1a and b, for the Ge and 12C:13C{}^{12}\mathrm{C}:{}^{13}\mathrm{C} ratios, respectively. After growth, the substrate was degassed at ≈550\approx550 °C for 14 hours in high-vacuum (≤2×10−7\le2 \times10^{-7} Torr) to minimize undesirable hydrogen related defect formation in subsequent processing steps16.

SIMS characterization confirms at 40 nm deep, a 17 ppm Ge layer with a 9 nm FWHM, with an achievable lower bound based on precursor residency times of around 2 nm41. Integrating over the layer yields a sheet density of 33,000 Ge/μ\mum2^{2}. To achieve a similar amount of germanium incorporation with ion implantation at this depth would require a dose of around 101310^{13} ions/cm2^{2}, but the distribution43 would be over 20 nm and create a peak density of vacancies around 10,000 ppm, see SI figure 1. This vacancy density is approaching diamond’s amorphization threshold of 50,000 ppm44 and would cause extreme inhomogeneity within the diamond.

No Nitrogen was measured in the sample to a detection limit of 17 ppb, likewise with no oxygen down to the detection limit of 0.6 ppm, see SI figure 2. Moreover, the isotope of 13C{}^{13}\mathrm{C} at the Ge layer is measured to be on the order of 10−310^{-3} % - down two to three orders of magnitude from natural abundance, see figure 1b. We observe an irregularity in 13C{}^{13}\mathrm{C} incorporation in the first ≈15\approx15 nm of growth. This is being investigated and it remains unclear if this arises as a SIMS artifact (re-sputtering of natural abundance) or is an actually true growth anomaly (e.g. natural abundance carbon contamination). Critically, this anomaly stops at the Ge doping layer.

Defect activation is achieved with electron irradiation at 2 MeV with a dose of 2×10142 \times10^{14} e−^{-}/cm2^{2}, resulting in an expected vacancy density of ≈0.25\approx0.25 ppm45,46. A subsequent vacuum annealing regimen is then performed at 850 °C and 1400 °C16.

Formation Dynamics

Unlike ion implanted samples, Ge atoms are incorporated during growth predominately to the substitutional site, due to the nature of CVD thermodynamics47. We intentionally maintain a low growth rate15,29 to maximize crystal quality and minimize the in-situ formation of vacancies and other undesirable species. Therefore, ex-situ vacancy creation is necessary to generate GeV−^{-}s. Using electron irradiation and subsequent annealing, we generate a 0.12 GeV−^{-}/µm2^{2} sheet density, see figure 2a. We consider two parallel mechanisms for GeV−^{-} creation16: the ejection of a carbon adjacent to the germanium substitutional site, an athermal process, and/or delocalized vacancy creation and migration to the germanium site. In ion implantation studies with Sn48 and Ge49, beta decay is experimentally used to suggest the ejection of a neighboring site is likely.

Annealing serves only to clean the lattice via migration of vacancies and easily disassociated clusters but overall hinders XV formation (where X is a generic substitutional dopant larger than the C atom). Other NV studies align with this and suggest that the adjacent C-atom ejection is the energetically favorable, and therefore most likely route50 compared to the migrating and combining vacancy picture. However, NV studies using spatially localized vacancies51 suggest that migration could still be the dominant mechanism under other circumstances.

At annealing temperatures of ≥850\ge850 °C, vacancy diffusivity reaches ≈2\approx2 nm2^{2}/s52, driving competing defect recombination, surface loss, and trapping processes53,54. Mobile vacancies recombine with carbon self-interstitials53,55,56 and annihilate at surfaces and interfaces, creating a vacancy-depleted layer near the sample surface or any other significant interface57. Concurrently, vacancies can be captured by substitutional impurities (e.g. N, Ge) or secondary vacancies to form XV color centers and multivacancy complexes47,58,59. At high local vacancy concentrations, mobile divacancies (V2_2) can also migrate directly to Ge impurities to form GeV centers22.

Here, the GeV−^{-} yield remains invariant between the 850 °C and 1400 °C anneals (SI figure 3). While the emergence of GeV−^{-} centers after 850 °C does not inherently distinguish athermal creation during irradiation from thermally activated vacancy mobilization/capture, the yield saturation by 850 °C indicates the governing formation process is complete at or below this temperature. This temperature invariance establishes two main considerations on the vacancy kinetics: (1) divacancy (V2_2) migration to Ge impurities is negligible in this regime22, and (2) the mobile monovacancy pool is fully exhausted by 850 °C. Furthermore, the thermal stability of GeV−^{-} centers up to 1400 °C agrees with their high calculated dissociation energy47,59. The absence of GeV−^{-} annihilation at elevated temperatures—despite exceeding the thermal activation barrier for carbon self-interstitial mobility—further points to a negligible residual interstitial concentration16,59.

These results demonstrate that GeV creation is predominantly driven by athermal processes, specifically the direct displacement of a carbon atom neighboring a substitutional germanium site (Ges_{\mathrm{s}}) during electron irradiation. For a Ges_{\mathrm{s}} center coordinated by four nearest-neighbor (NN) carbon atoms, each carbon has an ejection probability of ≥0.25\ge0.25 ppm, for this irradiation45,46,50, facilitated by local strain and Ge – C bond weakening relative to bulk sp3^{3} C – C bonds. Summing over the four NN sites yields a direct vacancy-generation probability of ≥1.0\ge1.0 ppm at the Ges_{\mathrm{s}} atom, corresponding to an estimated GeV density of 0.033 GeV−^{-}/μm2^{2}. Following DFT arguments, vacancies created at the 12 next-nearest-neighbor (NNN) sites likely spontaneously capture into Ges_{\mathrm{s}} due to local strain field gradients59,60, and as such remain an athermal process. Summing over all 16 NN and NNN candidate sites increases the predicted yield to ≈0.13\approx0.13 GeV−^{-}/μm2^{2}, in agreement with our experimentally observed 0.12 GeV−^{-}/μm2^{2} (Figure 2). Although only a small percentage, 36×10−5%36 \times10^{-5}\%, of Ge are converted to GeV−^{-}, 90% of NN and NNN vacancies are converted to GeV−^{-}.

Computational arguments suggest that the unavoidable contamination of nitrogen donors will likely incorporate near group IV dopants during growth61. This is advantageous, as the nearby donor likely stabilizes the charge of GeV to the negative state. In this context, we propose that annealing at ≥850\ge850 °C is critical for mobilizing and removing residual, non-complexed vacancies, which would otherwise act as competing electron traps that would destabilize this charge state. However, dense ensemble creation of GeV−\mathrm{GeV}^{-} will still require deliberate Fermi-level engineering62,63. Systematic dose-dependent irradiation studies across a broader thermal activation range are required to further decouple secondary defect pathways.

Optical

Using off resonant excitation, we measure GeV−\mathrm{GeV}^{-} photoluminescence spectra, shown in Figure 2b. From the spectra, we extract the zero-phonon line (ZPL) and generate a histogram of five distinct clusters that are agnostic of polarization. We hypothesize these clusters to originate from the Germane gas’ isotope distribution causing a shift in the emission. This emission can be understood as a change in the vibronic structure due to the different Ge masses64, see table 1. We identify the bluest cluster to be 70Ge{}^{70}\mathrm{Ge}, and the reddest 76Ge{}^{76}\mathrm{Ge}. We then use the 70Ge{}^{70}\mathrm{Ge} and 76Ge{}^{76}\mathrm{Ge} clusters to estimate where 72Ge{}^{72}\mathrm{Ge}, 73Ge{}^{73}\mathrm{Ge}, and 74Ge{}^{74}\mathrm{Ge} clusters should be from their expected shifts to the optical spectra. This estimate and subsequent population quantification is portrayed in figure 2c. The width of the shaded boxes (7.5 GHz) are identical and bounded by the observed and isolated 76Ge{}^{76}\mathrm{Ge} cluster. We approximate that all of the populations will have similar inhomogeneous broadening effects. From figure 2c we can see that the proposed boxes for 72Ge{}^{72}\mathrm{Ge}, 73Ge{}^{73}\mathrm{Ge}, and 74Ge{}^{74}\mathrm{Ge} are in good agreement with the observed clustering. Furthermore, we observe that the trend matches well with the expected natural abundance of the precursor gases, see table 1. We note that there is likely overlap between the 72–74Ge{}^{72\text{--}74}\mathrm{Ge} distributions, making it a challenge to unambiguously assign each isotope. Color centers that are not unambiguously within a cluster are marked as ??Ge.

Additionally, 87% of the observed color centers exhibit an orbital splitting of 160±8160 \pm8 GHz, closely matching the theoretical unstrained value for GeV centers65 (Figure 2d). Because defect centers occupying different crystallographic orientations sample distinct components of the local strain tensor[1], this uniform distribution confirms negligible strain within the GeV−\mathrm{GeV}^{-}-doped layer. Comparing the orbital splitting and ZPL histograms reveal that in this low-strain regime, inhomogeneous broadening is sufficiently suppressed such that secondary effects from isotopic variation, to govern the observed ZPL distribution.

To further resolve the optical spectra and isotopic sub-populations, we perform photoluminescent excitation (PLE), to investigate with MHz resolution the linewidth and ZPL. In these experiments, we keep the resonant power around 2–5 nW to avoid power broadening effects, and scan over a 1.5 GHz range for 10 minutes. Representative color centers, from the 322 observed, were randomly down-selected from each cluster due to experimental time constraints, with PLE measured successfully with a ratio of 70:13. Of these 70 individual color centers: about 49 of them have stable PLE with 1 exhibiting stable emission but two distinct peaks, see SI figure 11. In the remaining 20: 5 of them required resonant excitation greater than 10 nW, 9 were slightly unstable (see SI) and 6 had linewidths greater than 400 MHz. We attribute the instability to a nearby defect, either a divacancy or nearby other color centers (e.g. NV), and hypothesize that a gated PLE scheme could reduce this66. In the following analysis, we exclude the 6 broad and the 5 high resonant power color centers as their signals were immeasurable in typical experimental conditions. A representative stable GeV is given in figure 3d, showing no signs of hopping or spectral instability67,68. However, stable color centers still undergo self ionization69, but recover immediately, see SI.

In figure 3a, we plot the linewidth versus ZPL for each color center, while maintaining the same groupings as figure 2. We find that within each cluster the ZPLs are distributed within <10< 10 GHz of each other, see Table 2. This is within range of demonstrated strain or stark tuning devices to tune zero-phonon line emission and realize identicality[1, 2] [70, 71]. Additionally, the 74Ge{}^{74}\mathrm{Ge} group hosts excellent color centers with the measured color centers being within 2 GHz of each, and an average linewidth of 47 MHz; this sub-group of PLE is plotted in figure 3b. In contrast, the 73Ge{}^{73}\mathrm{Ge} group has broader PLE, illustrated in figure 3c. This is in agreement with the zerofield splitting of the spin 9/2 system of the 73Ge{}^{73}\mathrm{Ge} nucleus72. Excluding this ”naturally” broadened 73Ge{}^{73}\mathrm{Ge} contribution, our doping scheme results the linewidth average to be 73 MHz, and around 50% of the measured color centers to have linewidths less than 50 MHz (3.12 ns) see figure 3a, demonstrating that nonradiative decay is minimized.

IsotopeCountLinewidth [MHz]ZPL Range [GHz]
70Ge^{70}\mathrm{Ge}20/5888±5488 \pm547.66
72Ge^{72}\mathrm{Ge}15/5867±3067 \pm304.12
73Ge^{73}\mathrm{Ge}5/58181±36181 \pm362.52
74Ge^{74}\mathrm{Ge}13/5847±1147 \pm112.14
??Ge^{??}\mathrm{Ge}5/5898±6498 \pm64

Table 2. Summary statistics of the PLE clusters.

Spin

Focusing on characterizing the electronic spin of our delta-doped GeVs, we employ coherent population trapping (CPT)73,74, an all optical technique that creates a lambda system to address the GeV−\mathrm{GeV}^{-} spin directly. A schematic of group IV electronics and the lambda scheme is given in SI Figure 19. Here, all optical control is advantageous to microwave control because the low transverse strain prevents the qubit levels from exhibiting a large spatial overlap[3] [75]. In addition, the low transverse strain enables decoherence pathways between the orbital manifolds, therefore milikelvin temperature operation is critical to suppress phononic decoherence pathways76,77.

Figure 19. Schematic of the group IV electronic diagram, and the selected levels to form a lambda system for optical control.

Using this lambda scheme, we demonstrate a characteristic CPT dip and use a quadratic model to fit the PLE background and a Lorentzian for the dip (see SI). At 70 nW we extract a linewidth of 1195 ±\pm 334 kHz (T2∗=133±37T_2^* = 133 \pm37 ns), see Figure 4a. Furthermore, we repeat this process across many optical powers to determine the linewidth as a function of power. This broadening will depend linearly as a function of power, and fitting it to a linear model sets a lower bound to the T2∗T_2^*. The fitted model extracts an intercept of 0±2180 \pm218 kHz with an R2=0.93R^2 = 0.93. From this we set the lower bound of T2∗T_2^* to be 730 ns, see Figure 4b. This value is lower than anticipated compared to previous CPT measurements under similar conditions (T2∗=1.43 μsT_2^* = 1.43\ \mu\mathrm{s}78) or strained SnV−^{-} at 4 K (T2∗=2.7 μsT_2^* = 2.7\ \mu\mathrm{s}[3]). We attribute this reduction in T2∗T_2^* to spectral diffusion caused by a nearby charging paramagnetic defect, which induces a temporal drift in the spin resonance frequency (Figure 4c). Off-resonant photoexcitation with a green or blue laser resets this frequency shift to zero, after which the resonance climbs steadily at a rate of ∼20\sim20 kHz/min (SI Figure 15). To understand this defect we employed electron spin resonance and found a weak g factor of around 2 within the diamond, see SI Figure 17. This measurement did not help elucidate the source of paramagnetism, as many defects in diamond have a similar g factor79–81 (details in SI). Subsequent experiments are planned to elucidate the origin of this defect.

Figure 15. Change of the CPT transition under no excitation, and blue excitation.

Figure 17. EPR signal at 4.5 K

Additionally, future studies will move away from bulk material into a diamond membrane platform42,82, enabling longer T2∗T_2^* coherence times for single spin qubits through the application of transverse strain[3] [77] while giving us more latitude to isolate the cause of this paramagnetic defect species.

Conclusion

In summary, we have demonstrated the synthesis of low-strain delta-doped germanium in diamond via chemical vapor deposition (CVD). SIMS measurements confirm a high Ge incorporation density approaching the kinetic solubility limit of < 60 ppm15,83. Optical spectroscopy of the resulting germanium-vacancy (GeV−^{-}) centers confirms a low-strain environment enabling isotope-resolved optical transitions and narrow linewidths. In addition, electron irradiation was used to propose a refinement on their formation mechanisms in the diamond lattice. However, these results are observed alongside an unidentified paramagnetic defect that warrants further investigations. This growth process is readily compatible with thin diamond membranes42,82, establishing a scalable platform for strain-engineered quantum devices, integrated photonic/phononic resonators, and heterogeneous integration with nonlinear optical media.

Methods

Optical Experiments

Optical measurements were taken at 4 K, in a Montana CryoAdvance 100 with a 0.9 NA cryoobjective. Color centers were addressed with a home-built confocal microscope. Off resonant photoluminesence measures used a 532 nm laser with around 3 mW of power. PL maps were obtained using a tilted narrowband filter (Alluxa 607.7-1.6). Color center spectra was characterized via a Horiba IHR550 spectrometer, equipped with a 2400 g/mm grating and a Synapse Plus 2048 Camera. For PLE, we used an M Squared SolsTIS laser and sum frequency generation (AdvR)42,67 to obtain the orange light. The phonon sideband was collected with a Semrock 647/57 bandpass filter and sent to an Excelitas avalanche photodiode. Measurement software was developed using the nspyre84 package.

Spin Measurements

The sample was mounted in a Bluefors dilution refrigerator (LD400) and cooled down to 20 mK. Optical excitation and signal collection were carried out by a home-built confocal microscope with a high NA objective (Olympus MPLFLN100x, NA = 0.9, working distance = 1 mm). The resonant excitation laser was generated by sum-frequency generation (SFG) of 1550 nm (Toptica CTL1550) and 984 nm (Moglabs LDX) lasers in a Periodically Poled Lithium Niobate (PPLN) crystal (HCP photonics). The 1550 nm laser was first sent through an amplitude Electro-Optic Modulator (EOM, Exail) and subsequently amplified by an erbium-doped fiber amplifier (Thorlabs EDFA100P) before entering the PPLN. The EOM was driven by a microwave source (Windfreak SynthHD v2) at the frequency of the GeV−^{-} electron-spin resonance, resulting in the two phase coherent sidebands that were used for coherent population trapping. The 602 nm, 445 nm, and 532 nm lasers pulses were generated using acousto-optic modulator (AA Optoelectronic) in their respective optical paths, with pulse timing controlled by a digital signal generator (Swabian Instruments). The phonon-sideband emission is collected and measured with a single-photon counting module (Excelitas), and the resulting electrical pulses were recorded by a time-tagging module (Swabian Instruments).

Figures and Tables

IsotopeNatural AbundanceMeasured Abundance (N=322N = 322)
70Ge^{70}\mathrm{Ge}20.5%18.01% (58)
72Ge^{72}\mathrm{Ge}27.4%27.02% (87)
73Ge^{73}\mathrm{Ge}7.76%6.52% (21)
74Ge^{74}\mathrm{Ge}36.5%30.75% (99)
76Ge^{76}\mathrm{Ge}7.75%4.97% (16)
??Ge^{??}\mathrm{Ge}-12.73% (41)

Table 1. Measured Abundance of each isotope

Secondary Ion Mass Spectroscopy plots of germanium and carbon isotopes

Figure 1. Secondary Ion Mass Spectroscopy (SIMS) of a) Germanium and b) Carbon Isotopes: 12 and 13 as a function of depth. Detection limit of Ge is given as the dashed line at 4 ppb. a inset) A schematic illustrating the diamond overgrowth stack with approximate thicknesses.

Figure 2. a) PL map of the diamond with a narrowband filter in place. b) Representative spectra of the GeV−\mathrm{GeV}^{-}. The left most peak is referred to as the ZPL, the distance between the two peaks is the orbital splitting. c) Distribution of GeV−\mathrm{GeV}^{-} ZPLs resolved by the spectrometer, distinguished by polarization. The two polarizations are stacked for clarity. Proposed isotopic grouping is overlayed. Group width is estimated by the 76Ge^{76}\mathrm{Ge} cluster and is 7.5 GHz wide d) Distribution of orbital splitting, distinguished by polarization.

Figure 3. a) Distribution of GeV−^{-} ZPLs resolved by PLE, distinguished by polarization. Proposed isotopic grouping is overlayed. The span of each grouping is 7.5 GHz and determined from the 76Ge{}^{76}\mathrm{Ge} Spectra. b) PLE scans of the 74Ge{}^{74}\mathrm{Ge} group. c) PLE scan of a 73Ge{}^{73}\mathrm{Ge}. d) 10 minute PLE scan of the highlighted color center in figure 3b, showcasing the optical stability under resonant excitation.

Acknowledgments

This research was primarily supported by the U.S. Department of Energy, Office of Science; Basic Energy Sciences, Materials Sciences, and Engineering Division (M.W.N.N., B.P., D.D.A., F.J.H., and N.D.). This work was supported by the Laboratory Directed Research and Development (LDRD) Program at Argonne National Laboratory (Project No. 2020-0204), supported by the U.S. Department of Energy, Office of Science, under Contract No. DE-AC02-06CH11357. I.N.H. acknowledges support from the Quantum Leap Challenge Institute for Hybrid Quantum Architectures and Networks (HQAN) (NSF OMA-2016136) and NSF award AM-2240399. A.A.H. acknowledges additional support from Q-NEXT, a U.S. Department of Energy Office of Science National Quantum Information Science Research Centers under Award Number DE-FOA-0002253. A.W.W. acknowledges support by NSF QuBBE QLCI (NSF OMA-2121044). The spin measurements at JILA was supported by the National Science Foundation (NSF) (2326628 and 2443684). S.S. acknowledges support from the Sloan Research Fellowship.

Supplemental Information

SRIM Calculation

Figure 1 (PDF p. 18). SRIM computation for 74Ge^{74}\mathrm{Ge} implanted into diamond at an angle of 7∘7^\circ and 98 keV. The blue line is the dopant profile, and red line is the Vacancy profile. Profiles have been scaled to reflect a 1013 ions/cm210^{13}\,\mathrm{ions}/\mathrm{cm}^2 dose.

Growth and SIMS

SIMS characterization plots for nitrogen and oxygen with diamond overgrowth stack schematic inset

Figure 2 (PDF p. 19). SIMS characterization for a) Nitrogen and b) Oxygen. Detection limits are given with the dashed line at 17 ppb and 570 ppb, respectively. The large surface signal is a SIMS artifact. inset) A schematic illustrating the diamond overgrowth stack with approximate thicknesses.

Annealing PL Map

Figure 3 (PDF p. 20). a) PL map after 850 °C Anneal. 118 GeVs were observed in an 900 μm2\mu\mathrm{m}^{2} area. b) PL map after 1400 °C Anneal. 104 GeVs were observed in an 900 μm2\mu\mathrm{m}^{2} area. There is no significant change in GeV−^{-} density (Poisson test verification).

PLE

In this section, examples of the PLE scans are shared. Most of the color centers are stable with some ionization events, but recover immediately: figure 4, 5, 6, 7, 8, 9. The double peaked GeV−^{-} is given in figure 10. A detailed example of a 73Ge{}^{73}\mathrm{Ge} PLE is given in figure 11. Moreover, other color centers have an instability with bursts of luminescence or irregular lineshapes: figure 12, 13, and 14.

Stable PLE

In the following section PLE time traces are given for selected stable GeV−^{-}. These color centers recover well against self ionization. Figure 4, 5, 6 are from the 70Ge{}^{70}\mathrm{Ge} subset with the first two being polarized along [11ˉ0][1\bar{1}0] and the last along [110][110]. Figure 7 and 8 are from the 72Ge{}^{72}\mathrm{Ge} subset polarized along the [110][110] and [11ˉ0][1\bar{1}0]. Lastly, Figure 9 is the 74Ge{}^{74}\mathrm{Ge} featured in the main text.

CPT dip for GeV− at our lowest power

(a)

Change of CPT linewidth with incident laser power

(b)

Change of the CPT resonance over time

(c)

Figure 4. a) CPT dip for GeV−^{-} at our lowest power, 70 nW. Fitted line is given in grey. See SI for further fit details. b) Change of CPT linewidth with incident laser power. Fitted line is given in black, with the extrapolation to 0 power in grey. c) Change of the CPT resonance over time.

Figure 7. a-e) Time trace of the PLE with a broken axis to highlight the PLE transition. f) Histogram of the PLE. g) PL Spectra. This color center is polarized along the [110], with a 160 GHz orbital splitting. The average power during PLE is around 5 nW. The fitted linewidth is 38 MHz. This color center is with the 72Ge^{72}\mathrm{Ge} isotope.

Figure 9. a-e) Time trace of the PLE with a broken axis to highlight the PLE transition. f) Histogram of the PLE. g) PL Spectra. This color center is polarized along the [110], with a 160 GHz orbital splitting. The average power during PLE is around 3 nW. The fitted linewidth is 40 MHz. This color center is with the 74Ge{}^{74}\mathrm{Ge} isotope and is featured in the main text.

Figure 4 (PDF p. 21). a-e) Time trace of the PLE with a broken axis to highlight the PLE transition. f) Histogram of the PLE. g) PL Spectra. This color center is polarized along the [1̄10], with a 160 GHz orbital splitting. The average power during PLE is around 4 nW. The fitted linewidth is 47 MHz. This color center is with the 70^{70}Ge isotope.

Figure 5. a-e) Time trace of the PLE with a broken axis to highlight the PLE transition. f) Histogram of the PLE. g) PL Spectra. This color center is polarized along the [11ˉ0][1\bar{1}0], with a 160 GHz orbital splitting. The average power during PLE is around 4 nW. The fitted linewidth is 45 MHz. This color center is with the 70Ge^{70}\mathrm{Ge} isotope.

Figure 6. a-e) Time trace of the PLE with a broken axis to highlight the PLE transition. f) Histogram of the PLE. g) PL Spectra. This color center is polarized along the [110], with a 160 GHz orbital splitting. The average power during PLE is around 3.5 nW. The fitted linewidth is 41 MHz. This color center is with the 70Ge^{70}\mathrm{Ge} isotope.

Figure 8. a-e) Time trace of the PLE with a broken axis to highlight the PLE transition. f) Histogram of the PLE. g) PL Spectra. This color center is polarized along the [11ˉ0]\left[1\bar{1}0\right], with a 160 GHz orbital splitting. The average power during PLE is around 4 nW. The fitted linewidth is 42 MHz. This color center is with the 72Ge^{72}\mathrm{Ge} isotope.

Double Peak PLE

Figure 10 features the double peaked GeV−^{-}. We estimate the splitting to be 152 MHz. Noticeably from the PLE we donot see a hopping behavior1. Additionally, the self ionization events of the peaks seem slightly correlated. The second order correlation function was not acquired to determine if this is a single emitter or two.

Figure 10. a-e) Time trace of the PLE with a broken axis to highlight the PLE transition. f) Histogram of the PLE. g) PL Spectra. This color center is polarized along the [110], with a 160 GHz orbital splitting. The average power during PLE is around 3 nW. Both peaks are fitted to a linewidth of 42 MHz, their splitting is 152 MHz. This color center is with the 74Ge^{74}\mathrm{Ge} isotope.

73Ge{}^{73}\mathrm{Ge} PLE

Figure 11. a-e) Time trace of the PLE with a broken axis to highlight the PLE transition. f) Histogram of the PLE. g) PL Spectra. This color center is polarized along the [110], with a 160 GHz orbital splitting. The average power during PLE is around 3 nW. The fitted linewidth is around 208 MHz. This color center is with the 73Ge{}^{73}\mathrm{Ge} isotope.

Unstable PLE

Figure 12. a-e) Time trace of the PLE with a broken axis to highlight the PLE transition. f) Histogram of the PLE. g) PL Spectra. This color center is polarized along the [11ˉ0][1\bar{1}0], with a 160 GHz orbital splitting. The average power during PLE is around 3 nW. The fitted linewidth is around 60 MHz. This color is with the 70Ge isotope.

Figure 13. a-e) Time trace of the PLE with a broken axis to highlight the PLE transition. f) Histogram of the PLE. g) PL Spectra. This color center is polarized along the [110], with a 160 GHz orbital splitting. The average power during PLE is around 3.5 nW. The fitted linewidth is around 50 MHz. This color center is with the 70Ge{}^{70}\mathrm{Ge} isotope.

Figure 14. a-e) Time trace of the PLE with a broken axis to highlight the PLE transition. f) Histogram of the PLE. g) PL Spectra. This color center is polarized along the [110], with a 160 GHz orbital splitting. The average power during PLE is around 4 nW. The fitted linewidth is around 50 MHz. This color center is with the 70Ge^{70}\mathrm{Ge} isotope.

Unknown Paramagnetic Defect

Observation in CPT

Figure 16. Change of the CPT transition under resonant excitation over the course of 21 hours. We observe a drift around 80 MHz (3 mT). Fitting to an exponential decay, the time constant is around 3 hours.

Observation in ESR

We performed continuous wave (CW) EPR measurement on the delta doped GeV−^{-} sample to gain insight into the GeV−^{-}’s spin properties and presence of any other paramagnetic defects. Measurements were conducted using an X-band (9.36 GHz) Bruker ELEXSYS II E500 EPR spectrometer, equipped with a TE102 rectangular EPR resonator. The sample was maintained at cryogenic temperatures around 4.7 K with magnetic field parallel to the diamond sample surface. Figure 17 shows the measured EPR spectrum over a magnetic field range of 2000-4000 G, using a 1 G B-field modulation. This range corresponds to g-factors from approximately 1.6 to 3.4 and covers the well-known region for defects in diamond[2]. As shown in the left panel, only a resonance at g ≈ 2 is observed. The resonance has a narrow linewidth of 32 MHz, as shown in the zoomed in plot on the right. This resonance is most likely the associated with GeV−^{-} centers containing predominately the even Ge isotope (70^{70}Ge, 72^{72}Ge, 74^{74}Ge and 76^{76}Ge). No additional resonance were detected. The concentration of any possible co-existing paragenetic defects in the sample is likely below the EPR detection limit.

Discussion

We can use a few magneto-static models to estimate the concentration of this defect. To summarize the experimental results: We observe a shift of 80 MHz of the GeV−^{-} spin transition, see SI figure 16. This shift corresponds to a field change of around 3 mT. The applied field in this experiment is 330 mT along the diamond’s ⟨100⟩\langle100\rangle, we note that the shift is observed for multiple field directions, however due to experimental constraints were unable to determine if the maximum shift depended on applied field direction or intensity.

We can use Curie’s Law in the fully saturated regime to estimate the required density to generate a 3 mT field under an applied 330 mT at 20 mK, see equation (1) and 2. We take μBμ0≈1.165×10−20 mT/cm3\mu_{\mathrm{B}}\mu_{0} \approx1.165 \times10^{-20}\ \mathrm{mT/cm^{3}}. Assuming a magnetic moment of approximately μB\mu_{\mathrm{B}} for a system of g factor 2 and spin 1/2, we estimate a density of 1500 ppm. This density is very unexpected and does not corroborate with any typical defect that could be created throughout the processing. To recall, we had nominally 17 ppm of Ge at the delta doped layer’s peak, a background detection limit of 17 ppb for Nitrogen, and an initial irradiated density of 0.25 ppm of vacancies.

Furthermore, we can estimate the probability to find a magnetic defect close enough to our GeV−^{-} to generate such a field. We use the largest magnetic field from a single electron, see equation 3, and find that at a distance, r<8.5 A˚r < 8.5\ \mathring{\mathrm{A}} the magnetic field, B≥3mTB \geq3\mathrm{mT}. This distance corresponds to about 5 to 6 bond lengths. We then use the probability to find a defect within a radius of a GeV−^{-}, see equation 4. Taking ρD\rho_{D} to be diamond density, and nXn_{X} to be defect concentration we plot probabilities for different concentrations as a function of distance, see figure 18. We find again, that the concentrations required to have this be probable are unreasonable given the material processing and analysis we have done. This suggests the presence of an unknown impurity with a significantly lower density and high magnetic moment or an impurity that preferentially incorporates near the germanium during CVD growth. Per the discussion in the main text, the ionized Ns_{s}, commonly referred to as the P1 center, is a potential candidate. If it is indeed the P1 center, this poses an interesting caveat with Fermi engineering: the codopants have to be readily ionized and cannot possess paramagnetic properties. If it is the P1 center, a potential solution is to use a higher working temperature, achieved by transverse strain2 to leave the P1 in a mixed state. We also suspect it could be a contaminant in the germane gas, or it is from the parent substrate. Further experiments will reuse this gas in the membrane platform to deconvolve these effects.

δB≈μ0M=μ0μn(1)\delta B \approx\mu_{0}\mathbf{M} = \mu_{0}\mu n \tag*{(1)}
μ=gSμB(2)\mu= gS\mu_{\mathrm{B}} \tag*{(2)}
Bdip(r)=μ04π2μ∣r∣3(3)\mathbf{B}_{\mathrm{dip}}(\mathbf{r}) = \frac{\mu_{0}}{4\pi}\frac{2\mu}{\lvert\mathbf{r}\rvert^{3}} \tag*{(3)}
P(X<r∣GeV−)=1−exp⁡(−4π3r3ρDnX)(4)\mathrm{P}(X < r \mid\mathrm{GeV}^{-}) = 1 - \exp\left(-\frac{4\pi}{3}r^{3}\rho_{D}n_{X}\right) \tag*{(4)}

Figure 18. Log plot of probability to find a defect, XX, at a distance ≤r\le r for different concentrations of XX (nXn_X). Dashed grey line is at 8.5 A˚8.5\,\mathring{A}: the distance in which a single defect can produce a 3 mT field.

CPT Details

Schematic

Fit Details

To fit the coherent population trapping, we use a Lorentzian dip on a PLE lorentzian. Since we sampled with the zero order of the laser slightly detuned from the spin transition we observe some asymmetry in our CPT scans. To accurately model this, we need to include the contribution from the PLE dome, see equation (5). However, since we only scanned over a narrowband we can use a Taylor expansion on the PLE dome around the CPT transition: Δ=Δ0\Delta= \Delta_{0} and find equation (6).

VariableDefinition
S(Δ)S(\Delta)Experimental Luminescence
Δ\DeltaTwo photon detuning of the lasers
Δ0\Delta_0Spin Transition
Δ′\Delta'Detuning of the PLE dome from the Spin Transition
γCPT\gamma_{CPT}Spin Transition Linewidth
γPLE\gamma_{PLE}Linewidth of the PLE dome
AAPLE Dome amplitude
rrratio of CPT dip to PLE dome
BBbackground counts

Table 1 (PDF p. 37). Definition of variables in equation 5.

S(Δ)=−rA1+4(Δ−Δ0γCPT)2+A1+4(Δ−(Δ0−Δ′)γPLE)2+B(5)S(\Delta) = \frac{-rA}{1 + 4\left(\frac{\Delta-\Delta_0}{\gamma_{CPT}}\right)^2} + \frac{A}{1 + 4\left(\frac{\Delta-(\Delta_0-\Delta')}{\gamma_{PLE}}\right)^2} + B \tag*{(5)}
A1+4(Δ−(Δ0−Δ′)γPLE)2≈C2(Δ−Δ0)2+C1(Δ−Δ0)+C0(6)\frac{A}{1 + 4\left(\frac{\Delta-(\Delta_0-\Delta')}{\gamma_{PLE}}\right)^2} \approx C_2(\Delta-\Delta_0)^2 + C_1(\Delta-\Delta_0) + C_0 \tag*{(6)}
C2=−4γPLE2AγPLE2−12Δ′2(4Δ′2+γPLE2)3(7)C_2 = -4\gamma_{PLE}^2 A \frac{\gamma_{PLE}^2 - 12\Delta'^2}{(4\Delta'^2+\gamma_{PLE}^2)^3} \tag*{(7)}
C1=−8γPLE2AΔ′(4Δ′2+γPLE2)2(8)C_1 = -8\gamma_{PLE}^2 A \frac{\Delta'}{(4\Delta'^2+\gamma_{PLE}^2)^2} \tag*{(8)}
C0=A11+4(Δ′γPLE)2(9)C_0 = A \frac{1}{1 + 4\left(\frac{\Delta'}{\gamma_{PLE}}\right)^2} \tag*{(9)}

Supplementary References

References

References

  1. [1]Z. Li, et al., Nature Photonics 18, 1113 (2024).
  2. [2]J. A. v. Wyk, Journal of Physics: Condensed Matter 6, 801 (1994).
  3. [3]X. Guo, et al., Physical Review X 13, 041037 (2023).

Paper details

vlnc:W_hcgr5phz
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 9

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents