Surface properties of alkali silicate glasses: Influence of the modifiers

Abstract

Using large-scale molecular dynamics simulations, we investigate the surface properties of lithium, sodium, and potassium silicate glasses containing 25 mole % of alkali oxide. The comparison of two types of surfaces, a melt-formed surface (MS) and a fracture surface (FS), demonstrates that the influence of the alkali modifier on the surface properties depends strongly on the nature of the surface. The FS exhibits a monotonic increase of modifier concentration with increasing alkali size while the MS shows a saturation of alkali concentration when going from Na to K glasses, indicating the presence of two competing mechanism that influence the properties of a MS. For the FS, we find that larger alkali ions reduce the concentration of under-coordinated Si atoms and increase the fraction of two-membered rings, implying an enhanced chemical reactivity of the surface. For both types of surfaces, the roughness is found to increase with alkali size, with the effect being more pronounced for the FS than for the MS. The height-height correlation functions of the surfaces show a scaling behavior that is independent of the alkali species considered: The ones for the MS are compatible with the prediction of the frozen capillary wave theory while the ones for the FS show a logarithmic growth, i.e., on the nanoscale these surfaces are not self-affine fractals. The influence of the modifier on the surface properties are rationalized in terms of the interplay between multiple factors involving the size of the ions, bond strength, and charge balance on the surface.

I Introduction

Controlling the properties of the surface, such as composition, local structure, and roughness on intermediate length scales is crucial for many practical application of silicate glasses. For instance, some structural units that are uniquely present on the surface are know to control its reactivity and thus to influence the chemical stability and corrosion resistance of the surface, properties that are of great importance for biomedical and pharmaceutical usages of glasses [1, 2, 3, 4, 5, 6, 7]. Surface morphology is another characteristic of high relevance since it has been shown to play a key role in many functional properties of glasses such as friction and adhesion [8, 9, 10, 11, 12]. In addition, morphological investigations of glass fracture surfaces, via techniques such as atomic force microscopy (AFM), have allowed to obtain a better understanding of the failure mechanisms of glasses, documenting the importance of the surface for the mechanical properties of glasses [13, 14, 15, 16, 17, 18, 19, 20, 21].

Significant progress in our understanding of the surface properties of glasses has been made by using a combination of experimental techniques such as low-energy ion scattering (LEIS) spectroscopy and AFM [22, 23, 24, 25, 26, 27, 28, 29], as well as molecular dynamics (MD) computer simulations [7, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40]. Regarding the chemical composition of silicate glass surfaces, it is well established that on surfaces the concentration of oxygen and modifiers, e.g., sodium, are usually higher than in the bulk, resulting that the one of silicon atoms is lower [22, 38, 39]. This compositional difference between the surface and the bulk is related to their different geometry: Due to the presence of the vacuum, glass surfaces have a higher concentration of non-bridging oxygen (NBO) which in turn requires more positively charged modifiers in their vicinity for the sake of charge neutrality [22]. Also the production history of the surface influences the composition and structure on the surface: The melt-formed surfaces (MS) of sodium silicate glasses have been found to be more enriched in Na and NBO than the fracture surfaces (FS), whereas the latter have more structural defects such as two-membered (2M) rings (i.e., closed loops of two oxygen and two silicon atoms) and under-coordinated Si [38, 39]. This dependence has been attributed to the different mechanisms that govern the formation of these two types of surfaces: The MS is created in the liquid state, which allows more Na to diffuse to the surface and thus to reorganize the surface structure. The FS, by contrast, is generated by creating a surface at room temperature, and therefore, one can expect that only very little reconstruction of the fracture surface has occurred once the crack has passed [38].

A further consequence of the different production history is that for silicate glasses the FS is rougher than the one of MS and also shows a stronger dependence on composition [13, 40]. Moreover, experiments and simulations find that the geometrical features of the topography of the MS is described well by the theory of capillary waves that freeze in at the glass transition [13, 15, 40]. In contrast to this, early experiments indicated that the structure of the FS is given by a self-affine fractal down to the nanometer scale [16, 41]. However, this conclusion could be flawed due to the limitation in the lateral resolution of surface measurement [42, 43, 44]. In fact, a recent large-scale MD simulation study of the FS of sodium silicate glasses with atomic resolution has demonstrated that the FS is not a self-affine fractal on length scales below 10 nm [40]. However, it remains to be confirmed whether or not this conclusion also holds when the glass composition is changed, e.g., glasses containing other alkali oxides.

Alkali oxides are a key component for modifying the properties of silicate glasses. Previous experimental and theoretical studies of alkali silicate glasses have mainly focused on their structural properties in the bulk [45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57], and the correlations between structure and various physical properties, such as density [58, 59], phase separation and transformation [60, 61, 62], transport coefficients [63, 64, 65], and elastic behavior [66, 67, 68]. The observed influence of the alkali species on the various glass properties were frequently associated with the difference in cation field strength (i.e., the ratio between the charge and ionic radius of the cation) which is 1.69, 1.00 and 0.66 eA˚−1e\mathrm{\AA}^{-1} for Li, Na, and K ions, respectively [69]. It has been suggested that some anomalies of lithium silicate glasses, such as the increase of medium range order [54, 55, 56] and elastic moduli [67, 70] with increasing alkali concentration, are directly related to the high field strength of lithium ions (and thus a high strength of the Li-O bond), since the other alkali silicate glasses show the opposite trend. In contrast to this, a recent ab initio molecular dynamics study indicates that the trends observed in the various physical properties of bulk alkali-silicate glasses are related to a complex interplay between multiple competing factors such as bond strength, bond length, and the local environments [57]. Also relevant for the present study is the observation that the surface tension of molten alkali silicates decreases with increasing alkali radius [71] (for a given temperature and composition), which is expected to affect the properties of the glass surfaces, although so far this dependence has not been clarified. Thus, despite these previous studies, there are at present still many important open questions on how the chemical nature of the alkali modifiers affects the surface properties of silicate glasses, and the goal of the present work is to advance our understanding on this subject.

The main objective of this work is to investigate how the surface properties of binary alkali silicate glasses are influenced by the alkali type. Specifically, we will elucidate the effects of the modifiers on the composition, structure and topographical properties of the MS and FS. To this aim we consider the alkali species Li, Na, and K since they are among the most widely used additives for the production of commercial silicate glasses and are also the key components for chemical strengthening of glasses via ion-exchange at the glass surface [72, 73]. Our results are thus not only of practical relevance for the design of novel glasses with new/improved properties but also useful for obtaining a deeper understanding of the fracture behavior of these glasses.

The rest of the paper is organized as follows. In Section II we introduce the simulation methods which consist of the preparation of the glass using MD and the identification of the outermost surface layer using a geometric approach. Next, in § 0.3 we present and discuss the main results regarding the properties of the MS and FS. Finally, we summary and conclude this work in § 0.4.

Simulations

Preparation of the glass samples

The glass samples we investigate have the nominal composition A2O\mathrm{A}_2\mathrm{O}-3SiO2\mathrm{SiO}_2 (hereafter denoted as AS3, with A=Li\mathrm{A} = \mathrm{Li}, Na\mathrm{Na}, or K\mathrm{K}), and are produced by means of classical MD simulations. The interaction between the atoms are given by a pairwise effective potential (named SHIK) [74], which has been found to give a good quantitative description of the density, structure and mechanical properties of bulk silica and alkali (Li\mathrm{Li}, Na\mathrm{Na}, K\mathrm{K}) silicate glasses [68, 75]. Its functional form is given by

V(rij)=qiqje24πϵ0rij+Aijexp⁡(−rij/Bij)−Cijrij6,(1)V(r_{ij}) = \frac{q_iq_je^2}{4\pi\epsilon_0r_{ij}} + A_{ij}\exp(-r_{ij}/B_{ij}) - \frac{C_{ij}}{r_{ij}^{6}}, \tag*{(1)}

where rijr_{ij} is the distance between two atoms of species ii and jj. In order to attain a high computational efficiency, the long-range interactions given by the Coulomb term in Eq. (1) are evaluated using the method proposed by Wolf et al. [76] where the long-range cutoff is set to 10 Å; more details of this implementation can be found in Refs. [74, 77]. A previous study [75] has shown that this treatment of the long range forces has negligible influence on various properties of the silica and sodium silicate systems while allowing for a significantly improved computational efficiency, and thus large-scale simulations can be performed.

The values of the potential parameters AijA_{ij}, BijB_{ij}, CijC_{ij} are given in Ref. [74]. The effective charges for Li, Na, K, and Si are 0.5727ee, 0.6018ee, 0.6849ee and 1.7755ee, respectively. We note that these charges are compatible with those of the partial charges reported in first-principles simulations of similar glass compositions [57]. The charge for oxygen is composition-dependent in order to maintain overall charge neutrality [74]. Our recent MD studies have shown that the SHIK potential also allows to obtain reliable results on the surface properties of silica and sodium silicate glasses [38, 40]. The present work is the first study that uses this interaction potential for simulating the surface properties of Li and K containing silicate glasses, thus allowing to investigate how these alkali atoms modify the properties of the glass surface and how these modifications depend on the alkali type.

For each composition, approximately 2,300,000 atoms were placed randomly in a simulation box with a volume given by the experimental value of the glass density at room temperature [78]. The box dimensions were roughly 20 nm, 30 nm, and 50 nm in the xx, yy, and zz directions, respectively. Previous studies have shown that such large samples are needed to allow for an accurate determination of the surface properties and the mitigation of finite size effects for the fracture process [38, 40]. Using periodic boundary conditions in three dimensions, these samples were equilibrated at 6000 K for 80 ps in the canonical ensemble (NVTNVT) and then cooled and equilibrated at a lower temperature T1T_1 (still in the liquid state) for another 160 ps. This temperature T1T_1 was 2000 K, 2000 K and 2200 K for LS3 and NS3 and KS3, respectively. (The higher T1T_1 for KS3 is to take into account the slower dynamics of the sample due to the large alkali ions.) Subsequently we cut the sample orthogonal to the zz−axis and inserted an empty space, thus creating two free surfaces, i.e., the sample has the geometry of a slab. Periodic boundary conditions were applied in all three directions. In order to ensure that the two free surfaces do not interact with each other, the thickness of the vacuum layer was chosen to be 14 nm. These samples were equilibrated at T1T_1 for 1.6 ns, a time span that is sufficiently long to allow the reconstruction of the surfaces and the equilibration of the interior of the samples. Subsequently the samples were cooled via a two-stage quenching: A cooling rate of γ1=0.125\gamma_1 = 0.125 K/ps was used to quench the samples from T1T_1 to a temperature T2T_2 and a faster cooling rate γ2=0.375\gamma_2 = 0.375 K/ps to cool them from T2T_2 to 300 K. Finally, the samples were annealed at 300 K for 800 ps. The temperature T2T_2 at which the cooling rate is changed was chosen to be 1200 K which is well below the simulation glass transition temperature TgT_g (around 1400 K). (Note that the determination of the TgT_g for the sample with free surfaces is more difficult than for the bulk sample since the faster dynamics of the surface regions blurs the transition from liquid to glass.) At T2T_2, we also switched the simulation ensemble from NVTNVT to NPTNPT (at zero pressure) so that the generated glass samples were not under macroscopic stress at room temperature. The so obtained samples had thus two surfaces and were used to determine the properties of the MS.

After preparation of the glass samples we introduced on one of its free surfaces a linear “scratch” in the form of a triangular notch spanning the sample in the xx direction of width and depth of 3 nm and 2 nm, respectively. Subsequently we applied to the sample a strain in the yy direction, using a constant rate of 0.5 ns−1^{-1}, until it broke. (Note that this rate is sufficiently low so that the fracture behavior [79, 80], as well as the properties of the resulting fracture surface do not depend on it in a significant manner [38, 40].) Due to the presence of the notch, the place at which the fracture initiated could be changed at will, thus allowing to reuse the undamaged glass sample for several fracture processes.

Temperature and pressure were controlled using a Nosé-Hoover thermostat and barostat [81, 82, 83]. All simulations were carried out using the Large-scale Atomic/Molecular Massively Parallel Simulator software (LAMMPS) [84, 85] with a time step of 1.6 fs.

The results presented in the following correspond to one melt-quench sample for each composition. However, we emphasize that the system size considered are sufficiently large to make sample-to-sample fluctuations negligible [79]. For the MS, the results for the two surfaces on the top and bottom sides of the glass sample were averaged. For the FS, we averaged the results over six surfaces, resulting from three independent fracture (by changing the location of the notch). The error bars were estimated as the standard error of the mean of the samples.

Identifying the surface

In order to have a reliable description of the surface one needs a method that allows to map the positions of the atoms onto a well-defined mathematical surface. The algorithm that we used for constructing this surface mesh is based on the alpha-shape method of Edelsbrunner and Mücke [86]. It starts with the Delaunay tetrahedrization of the set of input points, i.e., the atoms in the sample. For each of the resulting tetrahedra one evaluates its circumsphere and compares it to a reference probe sphere that has a radius RαR_{\alpha}. The elements with circumsphere radius RR which satisfy R<RαR < R_{\alpha} are classified as solid, and the union of all solid Delaunay elements defines the geometric shape of the atomistic solid. A robust realization of this algorithm is implemented in OVITO [87].

It is important to mention that the probe sphere radius RαR_{\alpha} is the length scale which determines how many details and small features of the solid’s geometric shape are resolved. To construct the geometric surfaces for the glass samples we use Rα=3.2R_{\alpha} = 3.2 Å, i.e., the typical distance between neighboring Si atoms. This choice allows to resolve fine surface features but avoids the creation of artificial holes in the constructed surfaces. We note, however, that a small change of RαR_{\alpha} (e.g. by ±0.5\pm0.5 Å) will not alter significantly the results presented in the the following (see Refs. [38, 79] for details). Note that, by definition, the surfaces are two-dimensional objects. Finally, we point out that for the FS we have not considered the parts of the surface that are closer than ≈5\approx5 nm to the top/bottom MS in order to avoid the influence of these surfaces onto the properties of the FS.

Once the geometric surface is constructed, i.e., the mesh points of the surface are identified, we first fit a plane to the set of mesh points using a least squares fitting procedure, and defined this plane to be z=0z = 0. Finally, a linear interpolation is applied to the triangular mesh to obtain a uniform quadratic grid which is subsequently used to determine the morphology and roughness of the surface. Recent studies that used similar simulation protocols and surface analysis strategies have demonstrated that this approach does indeed allow to determine the surface characteristics of silica and sodium silicate glasses [38, 40, 79].

Results and discussion

Composition and structure of the surface

In this subsection we present how the composition and local structure of the surface depends on the alkali type and how the presence of the surface affects the structural properties of the sub-surface layer.

Figure 1 shows how the surface composition and the major structural quantities depend on alkali and surface type. Overall, we note that the influence of the modifiers are more complex than the simple monotonic dependence that one might expect, in that several quantities saturate or show even a non-monotonic behavior as a function of the alkali type, indicating the presence of competing mechanisms. The differences between the two types of surfaces can be attributed to their production history which affects the thermodynamics and kinetics of their formation (see below for a more detailed discussion). Panels (a) and (b) show that, with respect to the bulk, both kinds of surfaces are significantly enriched in alkali and oxygen and that this enrichment in alkali is more pronounced for the MS, results that agree with a previous simulation study on sodium silicate glass surfaces [38]. Consequently the two surfaces are strongly depleted of Si relative to the bulk, panel (c), and this depletion is more pronounced for the MS. The compositional difference between the MS and the FS can be related to the fact that the MS was created in the liquid state, which allows more alkali ions to diffuse to the surface, resulting in a more pronounced change of composition with respect to the bulk. In contrast to this, the FS was generated by dynamic fracture (i.e., with a crack velocity on the order of 10310^{3} m/s) [79, 80] at room temperature, and thus the atomic diffusion is very limited, resulting that the compositional change at the FS is smaller than the one of the MS [38]. Furthermore, one notices that the compositional difference depends not only on the surface type but also on alkali species: With increasing alkali size, the composition of the FS changes monotonically, while the MS shows a notable change of

Figure 1. Surface composition and structure. (a)-(c) Elemental concentration of O, alkali (A), and Si, respectively, for the two types of surfaces and the bulk (dashed line). (d) Fraction of bridging and non-bridging oxygen atoms, BO and NBO, respectively. The fractions are with respect to the total number of surface (bulk) atoms. (e) Fraction of the most abundant types of QnQ^n species on the surfaces. (f)-(g) Fraction of edge-sharing Si (esSi) and three-fold coordinated Si (Si3\mathrm{Si}^{3}), respectively. Note that in panels (e)-(g) the fractions are relative to the total number of Si on the surface. Error bars smaller than the symbol size are not shown. (h) Coordination number of the modifiers. The cutoff distances for determining the coordination number of the alkali are 2.5, 3.0, and 3.6 Å for Li, Na, and K, respectively, corresponding to the locations of the first minimum in gAO(r)g_{\mathrm{AO}}(r).

surface composition from LS3 to NS3, but basically no difference between NS3 and KS3, implying a possible saturation of the modifier effect. The monotonic change of composition from LS3 to KS3 for the FS can be rationalized by considering the difference in the A-O bond strength: The force constants inferred from the frequency of the characteristic vibrational modes of the A-NBO interaction have been reported to be 347 cm−1^{-1}, 180 cm−1^{-1}, and 113 cm−1^{-1} for Li-O, Na-O, and K-O, respectively [88]. Therefore, Li atoms are bound more strongly to the matrix than the two other alkali atoms and hence their thermodynamic driving force for migration to the surface is smaller. For the FS, the saturation of composition from NS3 to KS3 might be attributed to the delicate balance between two trends, i.e., the aforementioned bond strength and ionic size, with the latter resulting in a decreasing mobility of the large alkali ions.

The deviation of the surface composition from the bulk has the consequence that the net charge on the surface is not zero. We find that the MS as well as the FS are negatively charged and the negativity (per atom) is more pronounced for the MS than for the FS. This imbalance of surface charge weakens with increasing alkali size since larger alkali ions have a larger positive effective charge [74]. We also mention that this charge imbalance decreases quickly with distance from the surface and thus charge neutrality is restored within a few nm below the surface, see below for details.

Next, we show that not only the surface composition, but also the network connectivity is influenced by the alkali type. This is reflected in the fraction of bridging oxygen (BO), i.e., oxygen that is bonded to two Si, and thefraction of non-bridging oxygen (NBO), i.e., oxygen that is bonded to a single Si and thus forms a dangling SiO−^{-} bond, Figure 1d. Firstly, we note that in the bulk the alkali type does not affect the network connectivity, in agreement with previous findings [67, 68]. Secondly, one observes that both the MS and the FS are significantly more depolymerized than the bulk structure and the depolymerization is more prominent for the MS (i.e., higher fraction of NBO). This result is directly related to the fact that the MS is more enriched in modifiers, panel (b), and one sees that these two quantities do indeed track each other very closely. In fact, one finds that the ratio NBO/alkali is around 1.0 (bulk), 1.2 (MS), and 1.1 (FS) and depends only weakly on alkali type.

To characterize the network connectivity on length scales larger than the nearest neighbor distance, one can probe the concentration of the so-called QnQ^n units, where nn denotes the number of BO in a [SiO4_4] tetrahedron. Panel (e) shows the fraction of the two most abundant QnQ^n units for the surfaces as well as the bulk and one recognizes that the bulk sample is mainly composed of Q4Q^4 and Q3Q^3 units, demonstrating that the Si-O network is highly cross-linked, independent of the alkali type considered. These QnQ^n values for the bulk are in good agreement with the ones reported in a previous simulation study of the structure of alkali silicate glasses [56], but are about 20% off the values given by NMR [49]. This discrepancy is likely a consequence of the high cooling rates typically used in MD simulations which exceed by orders of magnitude the ones of experiments [89, 90]. In comparison with the bulk, the surface structures are significantly less connected, favoring the formation of less-polymerized units in that the MS has no longer Q4Q^{4} units but is instead mainly composed of Q3Q^{3} and Q2Q^{2} structures (the latter are presents in the bulk only with a small concentration) and for the FS one finds more Q3Q^{3} units than Q4Q^{4}, opposite to the case in the bulk (see also the snapshots in Figure 2).

Snapshots of the representative atomic configuration near the MS (a) and the FS (b) of the NS3 glass

Figure 2. Snapshots of the representative atomic configuration near the MS (a) and the FS (b) of the NS3 glass. O, Si and Na are represented by spheres in red, blue and green, respectively. The Si-O bonds that are shorter than 0.2 nm are denoted by solid sticks. The interactions between a Na and its nearest neighbor oxygens are indicated by dashed lines. The two [SiO4][\mathrm{SiO}_4] tetrahedra that are interacting with the Na are shaded light blue and are labeled by their QnQ^n type. Bridging oxygen (BO), non-bridging oxygen (NBO), and edge-sharing (es) atoms in the neighborhood of the Na are also labeled.

Figure 1(f) and (Figure 1g) demonstrate that the nature of the modifier influences also the concentration of the defect structures in the network and that this effect is particularly pronounced for the FS since this surface was generated from a highly non-equilibrium dynamic fracture process. Panel (f) shows that over 60% of Si atoms on the FS are edge-sharing (esSi), i.e., forming two-membered (2M) ring structures (see the snapshot in Figure 2b), and that this probability grows with increasing alkali size. (Note that basically no 2M rings are found in the bulk since these structures are energetically very unfavorable.) This finding can be linked to the dependence of the medium range order on alkali type: A recent simulation study, using the same potential as in the present work, has demonstrated that in (bulk) alkali silicate glasses with 20% alkali oxide, the fraction of small sized rings (less than 5 Si-O linkages) increases as the alkali varies from Li to K [74]. These small rings, which are likely to be broken during fracture because of their high internal stress, are favourable structures for the formation of 2M rings since the creation of larger rings, although energetically more favorable than short rings, takes much more time because it requires an atomic rearrangement on larger length scale [38]. Panel (f) also shows that for the MS the concentration of 2M rings is very small and, panel (g), that also the fraction of Si3\mathrm{Si}^{3} is basically zero (for the FS the latter concentration is significantly higher). These low concentrations can be attributed to the fact that for the MS the high temperature at its creation as well as the long time for the cooling allows the surface structure to reorganize and thus to eliminate these energetically unfavorable structural units.

Panel (g) shows that for the FS the fraction of three-fold under-coordinated Si, Si3\mathrm{Si}^{3}, although small in absolute value, is reduced by a factor of five when increasing the alkali size from Li to K. This strong dependence is likely due to the above mentioned fact that the alkali-NBO energy decreases significantly with increasing alkali radius, thus making it easier for a under-coordinated Si atom to pick up an additional oxygen atom. However, it cannot be excluded that some other aspects of the fracture process or the relaxation of the local structure shortly after the fracture depend on the alkali species, thus giving rise to the observed dependence of the Si3\mathrm{Si}^{3} concentration.

Finally, we demonstrate that also the local environment of the modifiers on the surface is different from the one in the bulk and that it depends on the alkali type. To quantify this dependence, we have determined the coordination numbers, ZA−OZ_{\mathrm{A-O}} and ZA−NBOZ_{\mathrm{A-NBO}}, of the modifiers by counting the number of oxygen and NBO atoms, respectively, up to the first minimum in the pair distribution function of A-O, gAO(r)g_{\mathrm{A O}}(r). Panel (h) shows that for the bulk the mean ZA−OZ_{\mathrm{A-O}} are respectively 3.4, 5.0, 7.2, for Li, Na, and K, comparable with the values reported in previous simulation works for the same glass compositions but using different interaction potentials [56, 67]. The coordination numbers of the alkali ions on the surfaces are smaller relative to the bulk values: For the MS, the mean ZA−OZ_{\mathrm{A-O}} are 2.7, 3.9, and 5.3 for Li, Na, and K, respectively and the corresponding values for the FS are only slightly smaller. This considerably reduced coordination number of the modifiers on the surface is due to the fact that the modifiers are located at the outermost atomic layer and thus have no oxygen atoms on the vacuum side to be bonded to. For the MS the coordination number between a modifier and a NBO is basically the same as in the bulk, i.e, the reduction of the coordination number found in ZA−OZ_{\mathrm{A-O}} is not seen. This implies that the decrease in ZA−OZ_{\mathrm{A-O}} at the surface is because the modifier reduces the number bridging oxygen atoms but not NBO, since the latter can be more easily accommodated at the surface, in agreement with panels (d) and (e). The value of ZA−NBOZ_{\mathrm{A-NBO}} is around 2.5 and slightly increasing with increasing alkali size. This value can be related to the fact that the most abundant QnQ^n units on the MS are Q3Q^3 and Q2Q^2, contributing respectively one and two NBOs for potential bonding with the alkali on the surface, see panel (e). By contrast, the FS is primarily composed of Q3Q^3 and Q4Q^4 and consequently the number of candidate NBOs for bonding with the modifier is significantly less, resulting in a considerably smaller mean coordination number ZA−NBOZ_{\mathrm{A-NBO}} around 0.5, a value that increases slightly with increasing alkali size. The snapshots of the two surfaces of the NS3 glass, Figure 2, illustrate the representative atomic structures and coordination environments near the surfaces. The bulk (although it is more polymerized than the surfaces) has a ZA−NBOZ_{\mathrm{A-NBO}} comparable to that of the MS which can be ascribed to the presence of NBOs in all directions around the modifier, contrasting the situation on a surface. Finally, we note that the modifier effect is reflected by the fact that the ZA−NBOZ_{\mathrm{A-NBO}} generally increases with increasing alkali size.

In addition to the properties of the surface monolayer, we have also investigated how the composition evolves with increasing distance rr from the surface. Here we define this distance as the length of the shortest path from a given atom below the surface to any atom on the surface, and thus r=0r = 0 represents the surface monolayer. Figure 3(a)–(Figure 3c) show that for r≤0.1r \le0.1 nm, the fractions of O and Na decrease very rapidly with rr, while the Si concentration increases steeply, indicating that the top-most surface layer is strongly enriched in O and alkali and is followed by a layer that is mainly composed of Si atoms. This layered arrangement of different atomic species propagates towards the interior of the glass, although the fluctuations of the composition gradually decay with increasing rr. For the Si concentration the details of this layering effect are found to depend on the type of alkali atom in that larger modifiers give rise to more pronounced peaks in the region close to the surface, i.e., less than 0.7 nm, see panel (c), and at the same time the location of the peaks shifts to slightly larger distances. These effects can be directly ascribed to the size of the alkali ions since their presence at the surface will push the Si atoms to larger rr. From panel (b), one observes that the fluctuation of the alkali concentration seems to decay faster

Figure 3. (a)–(c) Depth profiles of elemental concentrations with respect to the surfaces. For better visibility the data for the FS are shifted upward by 0.2. In practice, the composition at distance rr is the mean over a layer with thickness 0.11 nm. The triangles on the right ordinate axis indicate the corresponding bulk values. (d)–(f) Double-logarithmic plots of the absolute value of the atomic charge QQ as a function of distance from the surface. The black solid lines are power-laws with exponent −2-2 that help to distinguish the decay behavior of QQ. For the sake of comparison we include in (d) also the data for the FS of silica glass [38].

than that of the Si and O, reaching the bulk value (indicated by the triangles on the right ordinate) already at r≈1r \approx1 nm. This observation can be attributed to the higher mobility and thus higher flexibility of the alkali ions relative to the Si and O [38].

To quantify the decay of the compositional fluctuation with increasing distance from the surface, we use the per-atom atomic charge as a overall structural indicator, defined by Q(r)=∑αqαfα(r)Q(r) = \sum_{\alpha} q_{\alpha} f_{\alpha}(r), where qαq_{\alpha} and fαf_{\alpha} are, respectively, the charge and fraction of atomic species α\alpha. Figure 3 (d)-(Figure 3f) show the rr-dependence of the absolute value of the charge QQ in a double-logarithmic representation. For LS3, one recognizes that the decay of QQ is described well by a power-law with an exponent -2. Surprisingly we find that this rr-dependence as well as the value of the exponent are very similar to those found for the behavior of Q(r)Q(r) in pure silica [38], included in the graph as well. Our results are thus coherent with the view that Li acts as a pseudo-network former which enhances the cohesion of the Si-O network structure [67]. In contrast to LS3, the decay of QQ with rr for NS3 and KS3 can no longer be described by a power-law but is rather exponential-like with a decay rate that is larger for KS3 than for NS3, panels (e) and (f). These results can be attributed to the fact that silica and LS3 can be considered as structures that are relatively homogeneous and therefore the elastic response of the medium due to a defect (here the surface) decays algebraically with distance. In contrast to this, Na and K are strongly modifying the network resulting in pronounced structural heterogeneities, making that the perturbation by the surface is damped out much quicker, i.e., exponential-like.

Topography of the surface

In this subsection we discuss the structure of the surface on large scales and probe how it depends on the alkali type and the preparation protocol.

To get a first idea on the topographical features of the surfaces we present in Figure 4 a map of the height of the MS and FS, top and bottom panels, respectively. (The z=0z = 0 level has been determined such that the average height is zero). Overall, we note that the MS are smoother than the FS and that the roughness of the MS seems to be independent of the alkali type, while the one for the FS increases with alkali size. In order to makes these statements more precise we will in the following quantify the roughness and the symmetric property of the surfaces.

Topography of the surface. Melt-formed surfaces (a)–(c) and fracture surfaces (d)–(f) for the AS3 glasses

Figure 4. Topography of the surface. Melt-formed surfaces (a)–(c) and fracture surfaces (d)–(f) for the AS3 glasses. For the FS, the crack propagates in the negative yy-direction and the crack front is parallel to the xx-direction. The mean surface height is equal to zero.

Figure 5 shows the distribution of the surface height zz for the three glasses (MS and FS, panels (a) and (b), respectively). We recognize that these distributions have a Gaussian-like shape and that the one for the MS depends only weakly on the alkali type while for the FS this dependence is more pronounced. This observation reflects thus again the fact that the MS has a structure that has been well equilibrated while the one of the FS is strongly affected by dynamical processes that do not allow the structure to relax.

Figure 5. (a-b) Distribution of surface height for MS and FS, respectively. The data are shown for surfaces with an area of 20 nm×30 nm20\ \mathrm{nm} \times30\ \mathrm{nm}, corresponding to Figure 4. The mean surface height is equal to zero. (c-d) Compositional dependence of the roughness and the skewness γ1\gamma_1 of the surface height distribution, respectively. The dashed line with open symbols is a theoretical prediction of the intrinsic roughness of melt-quenched surfaces. For the sake of comparison, we note that the roughness for the MS and FS of a silica glass is 0.25 nm0.25\ \mathrm{nm} and 0.42 nm0.42\ \mathrm{nm}, respectively [40].

The standard deviation of the height distribution defines the roughness σ\sigma of the surface. Panel (c) shows that for the MS this roughness has a value of ≈0.2\approx0.2 nm and increases weakly with increasing alkali size. This result can be rationalized by recalling the concept of a frozen liquid interface [91, 92], which predicts that the intrinsic roughness of a MS is determined by the freezing of the capillary waves at a temperature T0T_0 during cooling, i.e., σ≈kBT0/γ\sigma\approx\sqrt{k_{\mathrm{B}}T_0/\gamma}, where kBk_{\mathrm{B}} is Boltzmann’s constant and γ\gamma is the surface tension at T0T_0. Previous studies have shown that this theory works well if one uses for T0T_0 the glass transition temperature TgT_{\mathrm{g}} [13, 15, 40, 93]. Making the assumption that Tg=1400T_{\mathrm{g}} = 1400 K is independent of glass composition and using the surface tension data of the corresponding alkali silicate melts [94] (γ\gamma is 0.312, 0.278, and 0.218 J/m2^2 for LS3, NS3, and KS3, respectively), allows to predict how the intrinsic roughness of the MS depends on the alkali species. Panel (c) shows that this theoretical prediction (open symbols) follows the same compositional dependence as the simulation results, although the values are about 20% higher. This overestimation is likely related to the fact that the surface can relax to some extent even for temperatures below TgT_{\mathrm{g}}, thus decreasing its roughness. On overall the good agreement between the predicted and measured values of σ\sigma gives thus support to the view that surface tension is the controlling factor in determining the roughness of MS. Also of interest is the fact that these values of the roughness are smaller than the one found for the MS of silica, which is σ=0.25\sigma=0.25 [40]. This shows that the presence of the alkali atoms leads to a flattening of the surface because of the enhanced mobility of these ions with respect to the one of the network.

The roughness of the FS is more than three times higher than the one of the MS, demonstrating that the formation process has a significant impact on its topography. The roughness increases by about 20% when lithium is replaced by sodium, and below we discuss this trend in more detail. If sodium is replaced by potassium, the amplitude of these fluctuations does, however, not increase further, in line with the remarks made in context of Figure 1(b) that for Na and K the increased mobility due to the decreasing bonding strength is compensated by an increasing ion size that hinders the migration of the atoms and as a result the geometrical properties of the surface do not change significantly. We are not aware of any experimental data for the surface roughness of AS3 glasses and therefore cannot compare our predictions with real data. However, for the case of silica such a comparison has shown that the prediction of the simulation is accurate to within 10% [40], giving credibility to the results presented here.

The trend that the roughness increases with alkali size can be related to the fact that with increasing alkali size the bonds with the network become weaker, thus allowing for larger fluctuations in the surface height. A further mechanism that enhances this dependence is related to the observation that the glass becomes increasingly ductile when changing from Li-silicate to K-silicate glasses [57]. This increased ductility originates from the enhanced structural heterogeneities, particularly the medium range order [74]: With increasing alkali size, the ring size distribution becomes broader (the frequency of the small- as well as large-sized rings increases while the one for intermediate-sized rings decreases). This leads to a larger variety of structures along the fracture path and thus a fracture surface that is rougher. This trend is also in line with the fact that for silica, which has a relatively narrow ring size distribution, the roughness of the FS is found to be around 0.42 nm [40], thus a value that is significantly smaller than the ones found for the AS3 glasses.

A further question of interest is whether or not the two sides of the surface (facing the vacuum or facing the glass) are statistically equivalent. For this, we have investigated the symmetry of the surfaces by quantifying the skewness, γ1=⟨z3⟩/⟨z2⟩3/2\gamma_1 = \langle z^3 \rangle/ \langle z^2 \rangle^{3/2}, of the surface height distribution. Figure 5(d) shows that both surfaces are asymmetric: The MS are more likely to have deep holes than high protrusions on the surface side facing the vacuum (γ1\gamma_1 is negative), whereas the FS shows the opposite, which is directly related to the fact that during the fracture process the breaking of Si-O-Si bridges or chain-like structures gives rise to a spiky surface [40]. The influence of the modifier is clearly seen for the FS in that larger alkali ions give rise to more asymmetric surface, whereas the influence of alkali type on the symmetry property of the MS is not evident. Finally we note that a non-vanishing γ1\gamma_1 indicates that the capillary wave theory cannot be valid in a strict sense since this approach predicts γ1=0\gamma_1 = 0 [40].

To characterize the topography of the surfaces on larger length scales it is useful to look at the height-height correlations. For this we define the normalized surface height autocorrelation function

C(r)=⟨z(r0)⋅z(r0+r)⟩−⟨z(r0)⟩⟨z(r0+r)⟩⟨z2(r0)⟩−⟨z(r0)⟩2(2)C(r) = \frac{\langle z(r_0) \cdot z(r_0 + r)\rangle- \langle z(r_0)\rangle\langle z(r_0 + r)\rangle}{\langle z^2(r_0)\rangle- \langle z(r_0)\rangle^2} \tag*{(2)}

where z(r0)z(r_0) is the surface height at a reference position r0r_0, and z(r0+r)z(r_0 + r) is the height at a distance rr from the reference point. The brackets ⟨…⟩\langle\ldots\rangle denote the average over the position r0r_0 and the different realizations of the surfaces. Since by construction of the surface we have that ⟨z(r0)⟩=0\langle z(r_0)\rangle= 0 and ⟨z2(r0)⟩−⟨z(r0)⟩2\langle z^2(r_0)\rangle- \langle z(r_0)\rangle^2 is equal to σ2\sigma^2, the above expression can be simplified to

C(r)=⟨z(r0)⋅z(r0+r)⟩σ2(3)C(r) = \frac{\langle z(r_0) \cdot z(r_0 + r)\rangle}{\sigma^2} \tag*{(3)}

(Note that the MS is statistically isotropic and hence C(r)C(r) depends only on the distance rr. For the FS this is not quite true, since the propagation direction of the crack front gives rise to an anisotropy. It is found, however, that this effect is relatively mild [40], and hence here we have averaged over all directions.) From Figure 6(a) one recognizes that for all investigated cases C(r)C(r) exhibits an exponential decay and that for the FS this decay is slower than the one for the MS. We determine the decay length ξ\xi by fitting C(r)C(r) in the range 0.5≤r≤1.80.5 \le r \le1.8 nm by the functional form C(r)=Aexp⁡(−r/ξ)C(r) = A\exp(-r/\xi). Figure 6(b) shows that ξMS\xi_{\mathrm{MS}} and ξFS\xi_{\mathrm{FS}} have a value of ≈1.3\approx1.3 nm and ≈2.5\approx2.5 nm, respectively, and depend only mildly on the alkali type.

Figure 6. (a) Normalized surface height autocorrelation function C(r)C(r), see Eq. (3), for the AS3 glass surfaces. (b) The decay length ξ\xi estimated by fitting C(r)C(r) by the expression C(r)=Aexp⁡(−r/ξ)C(r) = A\exp(-r/\xi).

A further possibility to characterize the topography of the surface is to consider the one-dimensional height-height correlation function

Δz(r)=⟨[z(r+x)−z(x)]2⟩x,(4)\Delta z(r) = \sqrt{\left\langle[z(r+x)-z(x)]^2 \right\rangle_x}, \tag*{(4)}

which measures the variance of the height difference between two points separated by a distance rr along a direction xx [21, 40, 41, 95, 96]. Figure 7(a) shows (Δz)2(\Delta z)^2 as a function of rr for the MS and, for the sake of comparison, we have included in this graph also the data for the MS of silica glass [40]. One sees that, for length scales less than ≈4\approx4 nm, Δz(r)\Delta z(r) increases logarithmically with rr, in accordance with the prediction of the frozen capillary wave theory, i.e., (Δz)2∝ln⁡r(\Delta z)^2 \propto\ln r [91, 92]. For larger length scales the curves become flat, most likely because of finite size effects which prevent the fluctuations to grow beyond a level that is dictated by the linear extension of the sample. For a fixed distance rr the value of Δz\Delta z increases with increasing alkali size and one also notices that the curve for silica is the highest one. This dependence of Δz(r)\Delta z(r) on the composition is thus in harmony with the one of the roughness σ\sigma presented in Figure 5(c) and which shows the same ordering.

Figure 7. Height-height correlation function Δz(r)\Delta z(r), see Eq. (4), (linear-log scale) for the MS (a) and FS (b). In (b) the curves are for the direction of crack propagation. The data for a silica glass [40] are included for comparison.

For the FS, experimental studies have reported a power-law dependence of Δz(r)\Delta z(r) (no square!) on rr which indicates that the FS is a self-affine fractal [16, 41, 97]. However, the validity of this description down to the nanometer is questionable, since at such small scales the reliability of the experimental data can be severely restricted by the spatial resolution of the measurements that use techniques such as AFM [42, 43, 44]. In fact, theoretical and numerical studies of the FS of heterogenous materials [95, 98] have reported a logarithmic dependence of Δz(r)\Delta z(r) on rr, but it was only very recently that computer simulations of realistic oxide glasses demonstrated that the FS of silica glass does indeed show such a logarithmic rr-dependence of Δz(r)\Delta z(r), demonstrating that on length scales less than 10 nm the surface is not a fractal object [40]. In Figure 7(b) we show that this logarithmic dependence also holds for the FS of alkali silicate glasses and that this dependence is unaffected by varying the alkali species. We mention that this scaling property is found in both the direction of crack propagation as well as the direction parallel to the crack front (not shown). Finally, we note that also here the flattening of the curves at large rr is most likely related to the fact that the sample is finite and hence fluctuations are bounded. However, for small-to-intermediate rr these finite size effects are small and the observed scaling behavior is stable.

Figure 8 shows the (not normalized) height-autocorrelation function ⟨z(r0)⋅z(r0+r)⟩\langle z(r_0) \cdot z(r_0+r) \rangle (in contrast to the normalized one in Eq. (3)). By its definition, this quantity contains thus information about the surface height fluctuations and their spatial correlations. Specifically, the value of these curves at r=0r=0 is given by the surface roughness, thus following the same order as σ\sigma presented in Figure 5. Comparing panels (a) and (b) demonstrates that the curves for the MS, notably the AS3 ones, decay faster than the FS curves, consistent with the difference in decay length as measured from the normalized correlation function C(r)C(r) (see Figure 6). Furthermore one notes that on the length scales displayed in these panels, the decay can be described reasonably well by an exponential law, although we have seen in the context of Figure 7 that this is not the case, at least not at small distances. One thus concludes that high quality data is needed in order to be able to identify reliably the rr-dependence of the fluctuations. Furthermore the graphs also show that the different curves do not cross each other which implies that the relative roughness is independent of the length scale considered. All together, Figure 5 to Figure 8 present in a comprehensive and coherent manner the topographical features of the surfaces.

Figure 8. Height autocorrelation function (log-linear scale) for the MS (a) and FS (b).

Conclusions and outlook

In this work, we have performed large scale MD simulations in order to investigate systematically how the properties of alkali glass surfaces depend on the chemical nature of the alkali species and the surface type, i.e., surface formed by a melt-quench process (MS) or by a dynamic fracture process (FS). The main conclusions are:

  • (i) The MS is more enriched in alkali and more depolymerized than the FS, while the elemental concentrations on the FS show a stronger dependence on the alkali type than the MS.

  • (ii) Larger alkali ions facilitate the restoration of undercoordinated Si defects, whereas the two-membered rings created by the violent fracture process can hardly be annealed away at room temperature.

  • (iii) The presence of the surface induces a gradient in composition in the regions beneath the surface. Larger alkali ions lead to a stronger deviation of the surface composition from the nominal bulk composition (in particular Si concentration) in the first few atomic layers below the surface, as well as a faster decay of the compositional fluctuation. However, the zone in which the surface influences the composition extents only over 2-3 nm while beyond this distance one recovers the bulk composition to within 1%.

  • (iv) The roughness of the MS increases with increasing alkali size, a trend that can be attributed to the reduced surface tension, and the prediction of the theory of frozen

capillary waves. The FS is found to be significantly rougher than the MS. That this roughness increases with increasing alkali size can be related to the enhanced heterogeneity in medium-range structure of the glass as well as the weakening of the bonding between the alkali atoms and the network.

(v) The decay length of surface height fluctuations of the FS (2.5 nm) is about twice the value for the MS, suggesting a more heterogeneous structure near the FS than the MS. The scaling property of the MS is consistent with the prediction of the capillary wave theory, whereas we find that the FS are not self-affine fractals on the nanoscale. This conclusion is unaffected by the variation of alkali species.

As a final remark, we note that the surface properties of glasses are intriguing yet challenging to probe in experiments and rationalize on a microscopic level because of the disordered nature of the glass structure. The present work provides an atomistic understanding on how/why the alkali modifiers influence the surface properties of silicate glasses which is of practical relevance for the design of glasses with functional properties. In addition, the set of tools developed in this work (and our recent studies [38, 39, 40]) will be useful for future investigation of the surface properties of network-forming amorphous materials.

Acknowledgments

W.K. is a senior member of the Institut Universitaire de France. The simulations were performed using the HPC resources of CINES under the allocations (Grant Nos. A0050907572 and A0070907572) attributed by GENCI (Grand Equipement National de Calcul Intensif), as well as the computing resources at Xi’an Jiaotong University.

References

References

  1. [1]L. Hench and D. E. Clark, Physical chemistry of glass surfaces, J. Non-Cryst. Solids 28, 83 (1978).
  2. [2]C. G. Pantano, Glass surfaces, Rev. Solid State Sci. 3, 379 (1989).
  3. [3]L. H. Dubois and B. R. Zegarski, Bonding of alkoxysilanes to dehydroxylated silica surfaces: A new adhesion mechanism, J. Phys. Chem. 97, 1665 (1993).DOI
  4. [4]A. Grabbe, T. Michalske, and W. Smith, Strained siloxane rings on the surface on silica: their reaction with organosiloxanes, organosilanes, and water, J. Phys. Chem. 99, 4648 (1995).DOI
  5. [5]J. P. Hamilton and C. G. Pantano, Effects of glass structure on the corrosion behavior of sodium-aluminosilicate glasses, J. Non-Cryst. Solids 222, 167 (1997).DOI
  6. [6]K. Zheng, M. Kapp, and A. R. Boccaccini, Protein interactions with bioactive glass surfaces: A review, Appl. Mater. Today 15, 350 (2019).DOI
  7. [7]A. Rimola, D. Costa, M. Sodupе, J.-F. Lambert, and P. Ugliengo, Silica Surface Features and Their Role in the Adsorption of Biomolecules: Computational Modeling and Experiments, Chem. Rev. 113, 4216 (2013).pubmed.ncbi.nlm.nih.gov/23289428
  8. [8]S. Derler, L.-C. Gerhardt, A. Lenz, E. Bertaux, and M. Hadad, Friction of human skin against smooth and rough glass as a function of the contact pressure, Tribol. Int. 42, 1565 (2009).DOI
  9. [9]N. Belkhir, T. Aliouane, and D. Bouzid, Correlation between contact surface and friction during the optical glass polishing, Appl. Surf. Sci. 288, 208 (2014).DOI
  10. [10]M. L. Rahaman, L. Zhang, M. Liu, and W. Liu, Surface roughness effect on the friction and wear of bulk metallic glasses, Wear 332, 1231 (2015).DOI
  11. [11]B. Li and B. E. Logan, Bacterial adhesion to glass and metal-oxide surfaces, Colloids Surf. B 36, 81 (2004).pubmed.ncbi.nlm.nih.gov/15261011
  12. [12]S. Biggs, R. G. Cain, R. R. Dagastine, and N. W. Page, Direct measurements of the adhesion between a glass particle and a glass surface in a humid atmosphere, J. Adhes. Sci. Technol. 16, 869 (2002).DOI
  13. [13]P. K. Gupta, D. Inniss, C. R. Kurkjian, and Q. Zhong, Nanoscale roughness of oxide glass surfaces, J. Non-Cryst. Solids 262, 200 (2000).DOI
  14. [14]M. Ciccotti, Stress-corrosion mechanisms in silicate glasses, J. Phys. D 42, 214006 (2009).DOI
  15. [15]T. Sarlat, A. Lelarge, E. Søndergård, and D. Vandembroucq, Frozen capillary waves on glass surfaces: An AFM study, Eur. Phys. J. B 54, 121 (2006).DOI
  16. [16]L. Ponson, D. Bonamy, and E. Bouchaud, Two-dimensional scaling properties of experimental fracture surfaces, Phys. Rev. Lett. 96, 035506 (2006).DOI
  17. [17]D. Bonamy, L. Ponson, S. Prades, E. Bouchaud, and C. Guillot, Scaling Exponents for Fracture Surfaces in Homogeneous Glass and Glassy Ceramics, Phys. Rev. Lett. 97, 135504 (2006).pubmed.ncbi.nlm.nih.gov/17026045
  18. [18]J.-P. Guin and S. Wiederhorn, Fracture of Silicate Glasses: Ductile or Brittle?, Phys. Rev. Lett. 92, 215502 (2004).pubmed.ncbi.nlm.nih.gov/15245288
  19. [19]S. M. Wiederhorn, J.-P. Guin, and T. Fett, The Use of Atomic Force Microscopy to Study Crack Tips in Glass, Metall. Mater. Trans. A 42, 267 (2011).DOI
  20. [20]M. Ciccotti and M. George, in Handbook of Materials Modeling: Applications: Current and Emerging Materials, edited by W. Andreoni and S. Yip (Springer International Publishing, Cham, 2018) pp. 1–37.
  21. [21]S. M. Wiederhorn, J. M. López-Cepero, J. Wallace, J.-P. Guin, and T. Fett, Roughness of glass surfaces formed by sub-critical crack growth, J. Non-Cryst. Solids 353, 1582 (2007).DOI
  22. [22]J. F. Kelso, C. G. Pantano, and S. H. Garofalini, A comparison of ion scattering spectra and molecular dynamics simulations at the surface of silicate glasses, Surf. Sci. Lett. 134, L543 (1983).
  23. [23]R. M. Almeida, R. Hickey, H. Jain, and C. G. Pantano, Low-Energy Ion Scattering spectroscopy of silicate glass surfaces, J. Non-Cryst. Solids 385, 124 (2014).DOI
  24. [24]R. M. Almeida, H. Jain, and C. G. Pantano, Low-Energy Ion-Scattering Spectroscopy of Modified Silicate Glasses, J. Am. Ceram. Soc. 99, 1259 (2016).DOI
  25. [25]C. V. Cushman, P. Brüner, J. Zakel, C. Dahlquist, B. Sturgell, T. Grehl, B. M. Lunt, J. Banerjee, N. J. Smith, and M. R. Linford, Low energy ion scattering (LEIS) of as-formed and chemically modified display glass and peak-fitting of the Al/Si LEIS peak envelope, Appl. Surf. Sci. 455, 18 (2018).DOI
  26. [26]E. Rädlein and G. H. Frischat, Atomic force microscopy as a tool to correlate nanostructure to properties of glasses, J. Non-Cryst. Solids 222, 69 (1997).DOI
  27. [27]J.-F. Poggemann, A. Goss, G. Heide, E. Rädlein, and G. Frischat, Direct view of the structure of a silica glass fracture surface, J. Non-Cryst. Solids 281, 221 (2001).DOI
  28. [28]J.-F. Poggemann, G. Heide, and G. Frischat, Direct view of the structure of different glass fracture surfaces by atomic force microscopy, J. Non-Cryst. Solids 326, 15 (2003).DOI
  29. [29]G. Frischat, J.-F. Poggemann, and G. Heide, Nanostructure and atomic structure of glass seen by atomic force microscopy, J. Non-Cryst. Solids 345, 197 (2004).DOI
  30. [30]B. Feuston and S. Garofalini, Topological and bonding defects in vitreous silica surfaces, J. Chem. Phys. 91, 564 (1989).DOI
  31. [31]A. Roder, W. Kob, and K. Binder, Structure and dynamics of amorphous silica surfaces, J. Chem. Phys. 114, 7602 (2001).DOI
  32. [32]D. Ceresoli, M. Bernasconi, S. Iarlori, M. Parrinello, and E. Tosatti, Two-membered silicon rings on the dehydroxylated surface of silica, Phys. Rev. Lett. 84, 3887 (2000).pubmed.ncbi.nlm.nih.gov/11019231
  33. [33]M. Rarivomanantsoa, P. Jund, and R. Jullien, Classical molecular dynamics simulations of amorphous silica surfaces, J. Phys. Condens. Matter 13, 6707 (2001).DOI
  34. [34]J. Du and A. N. Cormack, Molecular dynamics simulation of the structure and hydroxylation of silica glass surfaces, J. Am. Ceram. Soc. 88, 2532 (2005).
  35. [35]S. H. Garofalini, Molecular dynamics computer simulations of silica surface structure and adsorption of water molecules, J. Non-Cryst. Solids 120, 1 (1990).DOI
  36. [36]M. Ren, L. Deng, and J. Du, Bulk, surface structures and properties of sodium borosilicate and boroaluminosilicate nuclear waste glasses from molecular dynamics simulations, J. Non-Cryst. Solids 476, 87 (2017).DOI
  37. [37]T. S. Mahadevan and J. Du, Hydration and reaction mechanisms on sodium silicate glass surfaces from molecular dynamics simulations with reactive force fields, J. Am. Ceram. Soc. 103, 3676 (2020).DOI
  38. [38]Z. Zhang, S. Ispas, and W. Kob, Structure and vibrational properties of sodium silicate glass surfaces, J. Chem. Phys. 153, 124503 (2020).DOI
  39. [39]Z. Zhang, W. Kob, and S. Ispas, First-principles study of the surface of silica and sodium silicate glasses, Phys. Rev. B 103, 184201 (2021).DOI
  40. [40]Z. Zhang, S. Ispas, and W. Kob, Roughness and scaling properties of oxide glass surfaces at the nanoscale, Phys. Rev. Lett. 126, 066101 (2021).DOI
  41. [41]G. Pallares, F. Lechenault, M. George, E. Bouchaud, C. Ottina, C. L. Rountree, and M. Ciccotti, Roughness of oxide glass subcritical fracture surfaces, J. Am. Ceram. Soc. 101, 1279 (2018).DOI
  42. [42]J. Schmittbuhl, J.-P. Vilotte, and S. Roux, Reliability of self-affine measurements, Phys. Rev. E 51, 131 (1995).pubmed.ncbi.nlm.nih.gov/9962626
  43. [43]P.-E. Mazeran, L. Odoni, and J.-L. Loubet, Curvature radius analysis for scanning probe microscopy, Surf. Sci. 585, 25 (2005).DOI
  44. [44]F. Lechenault, G. Pallares, M. George, C. Rountree, E. Bouchaud, and M. Ciccotti, Effects of finite probe size on self-affine roughness measurements, Phys. Rev. Lett. 104, 025502 (2010).DOI
  45. [45]S. A. Brawer and W. B. White, Raman spectroscopic investigation of the structure of silicate glasses. i. The binary alkali silicates, J. Chem. Phys. 63, 2421 (1975).DOI
  46. [46]D. W. Matson, S. K. Sharma, and J. A. Philpotts, The structure of high-silica alkali-silicate glasses. a raman spectroscopic investigation, J. Non-Cryst. Solids 58, 323 (1983).DOI
  47. [47]R. Dupree, D. Holland, and D. Williams, The structure of binary alkali silicate glasses, J. Non-Cryst. Solids 81, 185 (1986).
  48. [48]C. Huang and A. Cormack, Structural differences and phase separation in alkali silicate glasses, J. Chem. Phys. 95, 3634 (1991).DOI
  49. [49]H. Maekawa, T. Maekawa, K. Kawamura, and T. Yokokawa, The structural groups of alkali silicate glasses determined from 29Si MAS-NMR, J. Non-Cryst. Solids 127, 53 (1991).DOI
  50. [50]A. C. Hannon, B. Vessal, and J. M. Parker, The structure of alkali silicate glasses, J. Non-Cryst. Solids 150, 97 (1992).DOI
  51. [51]J. F. Stebbins, I. Farnan, and X. Xue, The structure and dynamics of alkali silicate liquids: A view from NMR spectroscopy, Chem. Geol. 96, 371 (1992).DOI
  52. [52]B. O. Mysen and J. D. Frantz, Structure and properties of alkali silicate melts at magmatic temperatures, Eur. J. Mineral. 5, 393 (1993).DOI
  53. [53]T. Maehara, T. Yano, S. Shibata, and M. Yamane, Structure and phase transformation of alkali silicate melts analysed by Raman spectroscopy, Philos. Mag. 84, 3085 (2004).
  54. [54]H. Uhlig, M. J. Hoffmann, H.-P. Lamparter, F. Aldinger, R. Bellissent, and S. Steeb, Short-range and medium-range order in lithium silicate glasses, Part i: Diffraction experiments and results, J. Am. Ceram. Soc. 79, 2833 (1996).
  55. [55]H. Uhlig, M. J. Hoffmann, H.-P. Lamparter, F. Aldinger, R. Bellissent, and S. Steeb, Short-range and medium-range order in lithium silicate glasses, Part ii: Simulation of the structure by the reverse Monte Carlo method, J. Am. Ceram. Soc. 79, 2839 (1996).
  56. [56]J. Du and L. R. Corrales, Compositional dependence of the first sharp diffraction peaks in alkali silicate glasses: A molecular dynamics study, J. Non-Cryst. Solids 352, 3255 (2006).DOI
  57. [57]K. Baral, A. Li, and W.-Y. Ching, Ab initio modeling of structure and properties of single and mixed alkali silicate glasses, J. Phys. Chem. A 121, 7697 (2017).DOI
  58. [58]L. Shartsis, S. Spinner, and W. Capps, Density, expansivity, and viscosity of molten alkali silicates, J. Am. Ceram. Soc. 35, 155 (1952).DOI
  59. [59]H. Doweidar, The density of alkali silicate glasses in relation to the microstructure, J. Non-Cryst. Solids 194, 155 (1996).DOI
  60. [60]J. E. Shelby, Property/morphology relations in alkali silicate glasses, J. Am. Ceram. Soc. 66, 754 (1983).DOI
  61. [61]N. Kitamura, K. Fukumi, H. Mizoguchi, M. Makihara, A. Higuchi, N. Ohno, and T. Fukunaga, High pressure densification of lithium silicate glasses, J. Non-Cryst. Solids 274, 244 (2000).DOI
  62. [62]D. Uhlmann, Densification of alkali silicate glasses at high pressure, J. Non-Cryst. Solids 13, 89 (1973).DOI
  63. [63]W. M. MacDonald, A. Anderson, and J. Schroeder, Low-temperature behavior of potassium and sodium silicate glasses, Phys. Rev. B 31, 1090 (1985).pubmed.ncbi.nlm.nih.gov/9935858
  64. [64]W. Beier and G. H. Frischat, Transport mechanisms in alkali silicate glasses, J. Non-Cryst. Solids 73, 113 (1985).DOI
  65. [65]T. F. Soules and R. F. Busbey, Sodium diffusion in alkali silicate glass by molecular dynamics, J. Chem. Phys. 75, 969 (1981).DOI
  66. [66]Y. Vaills, Y. Luspin, and G. Hauret, Two opposite effects of sodium on elastic constants of silicate binary glasses, Mater. Sci. Eng. B 40, 199 (1996).DOI
  67. [67]A. Pedone, G. Malavasi, A. N. Cormack, U. Segre, and M. C. Menziani, Insight into Elastic Properties of Binary Alkali Silicate Glasses; Prediction and Interpretation through Atomistic Simulation Techniques, Chem. Mater. 19, 3144 (2007).DOI
  68. [68]Z. Zhang, S. Ispas, and W. Kob, Origin of the non-linear elastic behavior of silicate glasses, Acta Mater. 231, 117855 (2022).arxiv.org/abs/2111.09549
  69. [69]R. T. Shannon and C. T. Prewitt, Effective ionic radii in oxides and fluorides, Acta. Crystallogr. B. Struct. Sci. Cryst. Eng. Mater. 25, 925 (1969).DOI
  70. [70]M. R. DeGuire and S. Brown, Dependence of Young’s modulus on volume and structure in alkali silicate and alkali aluminosilicate glasses, J. Am. Ceram. Soc. 67, 270 (1984).DOI
  71. [71]L. Shartsis and S. Spinner, Surface tension of molten alkali silicates, J. Res. Natl. Bur. Stand. 38, 385 (1951).
  72. [72]R. Gy, Ion exchange for glass strengthening, Mater. Sci. Eng. B 149, 159 (2008).
  73. [73]A. K. Varshneya, Chemical strengthening of glass: Lessons learned and yet to be learned, Int. J. Appl. Glass Sci. 1, 131 (2010).DOI
  74. [74]S. Sundararaman, L. Huang, S. Ispas, and W. Kob, New interaction potentials for alkali and alkaline-earth aluminosilicate glasses, J. Chem. Phys. 150, 154505 (2019).DOI
  75. [75]Z. Zhang, S. Ispas, and W. Kob, The critical role of the interaction potential and simulation protocol for the structural and mechanical properties of sodosilicate glasses, J. Non-Cryst. Solids 632, 119895 (2020).DOI
  76. [76]D. Wolf, P. Keblinski, S. R. Phillpot, and J. Eggebrecht, Exact method for the simulation of Coulombic systems by spherically truncated, pairwise r-1 summation, J. Chem. Phys. 110, 8254 (1999).DOI
  77. [77]S. Sundararaman, L. Huang, S. Ispas, and W. Kob, New optimization scheme to obtain interaction potentials for oxide glasses, J. Chem. Phys. 148, 194504 (2018).DOI
  78. [78]N. P. Bansal and R. H. Doremus, Handbook of glass properties (Orlando: Academic Press, 1986).
  79. [79]Z. Zhang, Fracture, surface, and structure of silicate glasses: Insights from atomistic computer simulations, Doctoral dissertation, University of Montpellier, hal.science/tel-02902601 (2020).
  80. [80]Z. Zhang, S. Ispas, and W. Kob, Fracture of silicate glasses: Microcavities and correlations between atomic-level properties, Phys. Rev. Mater. 6, 085601 (2022).arxiv.org/abs/2205.02461
  81. [81]S. Nosé, A unified formulation of the constant temperature molecular dynamics methods, J. Chem. Phys. 81, 511 (1984).DOI
  82. [82]W. G. Hoover, Canonical dynamics: Equilibrium phase-space distributions, Phys. Rev. A 31, 1695 (1985).pubmed.ncbi.nlm.nih.gov/9895674
  83. [83]W. G. Hoover, Constant-pressure equations of motion, Phys. Rev. A 34, 2499 (1986).pubmed.ncbi.nlm.nih.gov/9897546
  84. [84]S. Plimpton, Fast parallel algorithms for short-range molecular dynamics, J. Comput. Phys. 117, 1 (1995).
  85. [85]A. P. Thompson, H. M. Aktulga, R. Berger, D. S. Bolintineanu, W. M. Brown, P. S. Crozier, P. J. in’t Veld, A. Kohlmeyer, S. G. Moore, T. D. Nguyen, et al., LAMMPS-a flexible simulation tool for particle-based materials modeling at the atomic, meso, and continuum scales, Computer Physics Communications 271, 108171 (2022).
  86. [86]H. Edelsbrunner and E. P. Mücke, Three-dimensional alpha shapes, ACM Trans. Graph. 13, 43 (1994).arxiv.org/abs/math/9410208
  87. [87]A. Stukowski, Computational analysis methods in atomistic modeling of crystals, JOM 66, 399 (2014).DOI
  88. [88]G. Hauret, Y. Vaills, T. Parot-Rajaona, F. Gervais, D. Mas, and Y. Luspin, Dynamic behaviour of (1 − x) SiO₂ − 0.5xM₂O glasses (M = Na, Li) investigated by infrared and Brillouin spectroscopies, J. Non-Cryst. Solids 191, 85 (1995).DOI
  89. [89]K. Vollmayr, W. Kob, and K. Binder, Cooling-rate effects in amorphous silica: A computer-simulation study, Phys. Rev. B 54, 15808 (1996).DOI
  90. [90]X. Li, W. Song, K. Yang, N. M. A. Krishnan, B. Wang, M. M. Smedskjaer, J. C. Mauro, G. Sant, M. Balonis, and M. Bauch y, Cooling rate effects in sodium silicate glasses: Bridging the gap between molecular dynamics simulations and experiments, J. Chem. Phys. 147, 074501 (2017).DOI
  91. [91]J. Jäckle and K. Kawasaki, Intrinsic roughness of glass surfaces, J. Phys. Condens. Matter 7, 4351 (1995).DOI
  92. [92]T. Seydel, M. Tolan, B. M. Ocko, O. H. Seeck, R. Weber, E. DiMasi, and W. Press, Freezing of capillary waves at the glass transition, Phys. Rev. B 65, 184207 (2002).DOI
  93. [93]P. Roberts, F. Couny, H. Sabert, B. Mangan, D. Williams, L. Farr, M. Mason, A. Tomlinson, T. Birks, J. Knight, and P. S. Russell, Ultimate low loss of hollow-core photonic crystal fibres, Opt. Express 13, 236 (2005).pubmed.ncbi.nlm.nih.gov/19488348
  94. [94]L. Shartsis and S. Spinner, Surface tension of molten alkali silicates, J. Res. Natl. Bur. Stand. 46, 385 (1951).
  95. [95]J. Barés, M. Barlet, C. L. Rountree, L. Barbier, and D. Bonamy, Nominally brittle cracks in inhomogeneous solids: From microstructural disorder to continuum-level scale, Front. Phys. 2, 70 (2014).DOI
  96. [96]R. L. C. Vink, J. Horbach, and K. Binder, Capillary waves in a colloid-polymer interface, J. Chem. Phys. 122, 134905 (2005).pubmed.ncbi.nlm.nih.gov/15847500
  97. [97]B. B. Mandelbrot, D. E. Passoja, and A. J. Paullay, Fractal character of fracture surfaces of metals, Nature 308, 721 (1984).DOI
  98. [98]S. Ramanathan, D. Ertaş, and D. S. Fisher, Quasistatic crack propagation in heterogeneous media, Phys. Rev. Lett. 79, 873 (1997).DOI

Paper details

vlnc:W_hr5b5s89
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents