Dynamic evolution of internal stress, grain growth, and crystallographic texture in arc-evaporated AlTiN thin films using in-situ synchrotron x-ray diffraction

Abstract

Understanding the nucleation and growth of polycrystalline thin films is a long-standing goal. Polycrystalline films have many grains with different orientations that affect thin-film properties. Numerous studies have been done to determine these grain size and their preferred crystallographic orientation as well as stress in films. However most past studies have either employed an ex-situ methodology or only monitor the development of macroscopic stress in real-time. There has never been any research done on the simultaneous determination of crystallographic texture, grain size, and microscopic stress in polycrystalline thin films. In this study, we simultaneously monitored the generation and temporal evolution of texture, grain size, and internal stress in cathodic arc evaporated Al0.50Ti0.50N thin films using a bespoke deposition apparatus designed for use with 2-dimensional synchrotron x-ray diffraction technique. The influence of the substrate temperature is investigated in terms of the emergence and development of texture, grain size and stress evolution. A dynamic evolution of the crystallographic texture is observed as the overall film thickness varies. We clearly resolved two regime of films growth based on stress evolution. Beyond a threshold grain size (~ 14 nm), the stress scales inversely to the average grain sizes, and as the film thickness increases, immediate compressive stress relaxation was seen. An extensive ex-situ evaluation of thin films using electron microscopies and electron diffraction was performed to support the in-situ x-ray diffraction results.

Introduction

Transition metal nitrides (TMNs), especially AlN-alloyed TiN (Alx_xTi1−x_{1-x}N)-based thin films, show extraordinary physical, mechanical, and tribological properties, e.g., high mechanical hardness, high melting temperature, thermodynamic stability at elevated temperature, and oxidation resistance [1, 2]. Owing to these characteristics, thin films of Alx_xTi1−x_{1-x}N are preferred as protective films that extend the life of cutting tools and inhibit corrosion. In practice, polycrystalline thin films of Alx_xTi1−x_{1-x}N are deposited on top of a rigid substrate (e.g., cutting tools) by physical vapour deposition (PVD), such as magnetron sputtering or cathodic arc evaporation, or chemical vapour deposition (CVD) techniques. Typical PVD deposited films possess nanocolumnar and/or nanocrystalline morphologies [3] with preferred orientation of certain crystallographic planes along the growth direction (known as crystallographic texture). As the PVD deposition involves non-equilibrium processes and the formation of high-energy ions, as-deposited films are also often in a state of residual stress. These inherent stresses (usually compressive stresses) in PVD coated thin films play a vital role in the overall performance and efficiency of the films. During mechanical operations, the stress due to external mechanical loads adds to the pre-existing stress. A high pre-existing stress may lead to the complete failure of the coating, including its delamination from the substrate. At the same time the smaller values of residual stress and low values of mechanical hardness correlate with each other[4, 5]. Thus, optimizing the stress in thin films is important and it is required for industry to realize their full potential. In this regard understanding the mechanisms of thin film nucleation and growth has been an important aspect of research for the community, since these factors are essential in determining the properties of films and their practical significance.

It has already been established that many process parameters in PVD can be used to tune the film’s stress level. For example, application of a negative substrate bias voltage (VsV_{\mathrm{s}}) leads to the formation of finer grains and an increase in residual stress [6, 7, 8, 9]. At the same time, higher VsV_{\mathrm{s}} also helps in the deposition of dense or compact films and leads to high mechanical hardness. The partial pressure of N2\mathrm{N}_{2} in the total growth pressure (Ar+N2\mathrm{Ar}+\mathrm{N}_{2}) influences the composition, roughness, grain size, and microstructure of the films. The non-stoichiometric films, resulting from different Ar+N2\mathrm{Ar}+\mathrm{N}_{2} combinations, show poor mechanical hardness [10, 11, 12, 13]. Machet et al. [14] examined the effect of substrate temperature (varying from 100 °C to 450 °C) on the elemental composition, surface morphology, and mechanical hardness properties of magnetron sputtered TiN films. They found that for a given N2\mathrm{N}_{2} partial pressure, the development of crystallographic texture is greatly influenced by the substrate temperature. At low growth temperatures (below 300 °C), 111 crystallographic texture of the face-centered-cubic (FCC) TiN phase forms in the growth direction (GD), while at higher temperature a 200 and/or 220 texture of FCC-TiN are developed along GD. Machet et al. characterized the mechanical properties of the films and claimed that TiN films with a crystallographic texture of 111 possess a hardness of 20 GPa, but exhibit poorer wear resistance than films with a crystallographic texture of 200, which have a hardness of 25 GPa along with a good wear resistance [15]. A similar observation was made by Wang et al. [16] in (Ti, Al)N films deposited with cathode discharge deposition process. Kalss et al. investigated the interdependence of stress and crystallographic texture in (Al, Ti)N films deposited with cathodic arc evaporations [17] and argued that the formation of high index crystallographic plane’s texture (e.g., 113 and 115) leads to residual stress relaxation and reduction in film density, contrary to Beckers et al. [18] and Greene et al [19].

Most of the above-mentioned reports determined residual stress (or simply stress), crystallographic texture, and grain size after the film’s deposition and after cooling down from growth to room temperature. Little is known about the real-time formation and evolution of stress and microstructure of AlxTi1−xN\mathrm{Al}_{x}\mathrm{Ti}_{1-x}\mathrm{N} thin films, particularly when deposited with the industry-preferred arc evaporation technique. Recently, by utilizing a home designed cathodic arc evaporation chamber [20], adapted for in-situ synchrotron radiation studies, we recorded the evolution of stress/strain and microstructure of polycrystalline AlxTi1−xN\mathrm{Al}_{x}\mathrm{Ti}_{1-x}\mathrm{N} (x=0x = 0, 0.25, 0.5, and 0.67) thin films under different substrate bias voltage (VsV_{\mathrm{s}}) [21]. In this report, we examine the formation and evolution of biaxial stress, crystallographic texture, and grain size in Al0.50Ti0.50N\mathrm{Al}_{0.50}\mathrm{Ti}_{0.50}\mathrm{N} films deposited by varying substrate temperatures, while maintaining a constant substrate electrical bias of -40 V.

Experimental Details

To deposit Al0.50Ti0.50N\mathrm{Al}_{0.50}\mathrm{Ti}_{0.50}\mathrm{N} films on the 100 surface of a Si substrate, a reactive cathodic arc evaporation technique was used. A 63 mm diameter Al0.50Ti0.50\mathrm{Al}_{0.50}\mathrm{Ti}_{0.50} metallic cathode (FK Grade, PLANSEE-Germany) was used at a fixed arc current of 75 Amperes. The angle formed by the surface normal of the cathode and the normal of the substrate was 35°. A substrate rotation speed of 5 rotations per minute was maintained. The details of the experimental setup were previously discussed [20, 21]. The pure N2\mathrm{N}_{2} (99.9995 %) pressure was kept constant at 40 mTorr during depositions. The substrate was heated using an 808 nm infrared laser diode-based heating unit. In this study, four different substrate temperatures (TsT_{\mathrm{s}}) were used for thin film deposition: 250, 450, 600, and 750 °C. A DC power supply was used to electrically bias the substrate with a fixed voltage of -40 V.

The deposition system was placed at the P07 beamline (DESY, Germany) for in situ x-ray diffraction (XRD) during growth. The deposition system was aligned such that the x-ray beam travelled through the growing coating, parallel to the substrate surface. The x-ray energy was 73.79 keV and the beam size was defined by slits to 100×600 μm². A 2D flat panel detector with a 2048×2048-pixel resolution was used to record the diffractograms (PerkinElmer XRD 1622). Each exposure was 0.2 seconds, and ten exposures were superimposed to create the final diffractogram. The diffractogram of NIST standard LaB6\mathrm{LaB}_{6} powder was used to measure the distance between the substrate and the detector. The detector was placed to capture one quadrant of the diffraction pattern to maximize resolution. The 2D diffractograms were converted into 1D-line profiles using pyFAI [22], a Python-based program that integrates the intensities using 5∘5^\circ wide azimuthal bins (Δφ\Delta\varphi). To obtain the peak positions and peak widths of the diffraction peaks, the intensity vs. 2θ2\theta data was fitted with a pseudo-Voigt function. The biaxial stress was determined by the well-known sin⁡2ψ\sin^{2}\psi method. The unstrained interplanar spacing (dhkl0d^{0}_{hkl}) was determined from the dhkld_{hkl} vs. sin⁡2ψ\sin^{2}\psi plot and is corresponding to dhkld_{hkl} value at the corresponding invariant tilt angle ψ∗\psi^{*}, i.e., dhkl0=dhkl(ψ=ψ∗)d^{0}_{hkl}=d_{hkl}(\psi=\psi^{*}). The ψ∗\psi^{*} was determined by the relation: sin⁡2ψ∗=2νhkl1+νhkl\sin^{2}\psi^{*}=\frac{2\nu_{hkl}}{1+\nu_{hkl}}, here νhkl\nu_{hkl} is the Poisson ratio for the hklhkl orientation of the films. The 111-diffraction peak was used to determine the high biaxial stress. High temperature elastic constants of FCC-Al0.50Ti0.50N\mathrm{Al}_{0.50}\mathrm{Ti}_{0.50}\mathrm{N} from the work of Shulumba et al. [23] were used to estimate strain and stress and are tabulated in Table 1.

TsT_{\mathrm{s}} (°C)C11C_{11} (GPa)C12C_{12} (GPa)C44C_{44} (GPa)E111E_{111} (GPa)ν111\nu_{111}ψ∗\psi^{*} (°)
250410134178422.90.18832.5
450394130171406.670.18932.5
600382127166394.90.18932.6
750369123161382.790.188732.5

Table 1. Temperature dependent elastic coefficients of FCC- Al0.50Ti0.50N\mathrm{Al}_{0.50}\mathrm{Ti}_{0.50}\mathrm{N} used in determination of biaxial stress in thin films. The values are obtained from the work of Shulumba et al. [23].

The average grain size ⟨Dhkl⟩\langle D_{hkl}\rangle, which is averaged over the Debye-Scherrer rings, at a given instant during the deposition is estimated using Debye-Scherrer method [24] and is given by:

⟨Dhkl⟩=1N(Δϕi)∑Δϕi=1N0.9×λβ(Δϕi)×cos⁡θ(Δϕi)(1)\langle D_{hkl}\rangle= \frac{1}{N(\Delta\phi_i)} \sum_{\Delta\phi_i=1}^{N} \frac{0.9 \times\lambda}{\beta(\Delta\phi_i) \times\cos\theta(\Delta\phi_i)} \tag*{(1)}

N(Δϕi)N(\Delta\phi_i) is the number of azimuthal bins. β(Δϕi)\beta(\Delta\phi_i) is the full width at half maximum of the pattern of individual intensity vs. 2θ2\theta plots for a given value of Δϕi\Delta\phi_i and θ\theta is the corresponding half of the scattering angle (2θ2\theta). λ\lambda is the wavelength of the x-ray beam and is 0.168 Å for this study.

The ex-situ characterization of the films was carried out by using scanning electron microscopy (SEM, Leo 1550 Gemini with an electron acceleration voltage of 4-5 kV), transmission (TEM) and scanning transmission (STEM) electron microscopy (both performed on a FEI Tecnai G2 microscope operated at 200 kV). STEM was combined with both high angle annular dark field (HAADF) and energy dispersive x-ray spectroscopy (EDS) detectors. Prior to analysis by (S)TEM suitable thin specimens were prepared by using a cross beam focussed ion beam (FIB) instrument (Zeiss EsB 1540) using the standard lift out approach[25]. Mechanical properties of the films such as hardness, and elastic recovery was obtained with a nanoindenter equipped with Berkovich diamond tip. The maximum load of the nanoindentations was set to 10 mN so the indentation depth is less than 10% of the total film thicknesses. The hardness values were quantified by the method proposed by Oliver and Pharr [26]. At least 30 indents were used to calculate the mean values of hardness and their standard deviation.

Results and Discussion

Fractured cross-section SEM micrographs of the films are presented in Figure 1. A typical nano-columnar thin film morphology is seen for samples deposited below 750 °C whereas the film deposited at Ts=750T_{\mathrm{s}} = 750 °C has a nanocrystalline like morphology (Figure 1(d)). The Al0.50Ti0.50N\mathrm{Al}_{0.50}\mathrm{Ti}_{0.50}\mathrm{N} thin film deposited at Ts=250T_{\mathrm{s}} = 250 °C shows a variation in film thickness across the film (Figure 1 (a)) indicating a cohesive failure of the film during its deposition. A plan view SEM inspection of the films confirms the delamination of the film from the substrate. From the visual inspection of the SEM images, the width of the nanocolumns is maximum for film deposited at Ts=450T_{\mathrm{s}} = 450 °C, and minimum for film deposited at Ts=750T_{\mathrm{s}} = 750 °C.

Image not extracted

Figure 1. Figure 1 shows the fractured cross-sectional FESEM micrographs of Al0.50_{0.50}Ti0.50_{0.50}N films deposited at substrate temperatures of 250 °C (a), 450 °C (b), 600 °C (c), and 750 °C (d). The yellow-coloured arrow-marked region in figure (a) shows a cohesive failure region in the film.

The 2D x-ray diffractograms reveal that for all the TsT_{\mathrm{s}} that are discussed here, the Al0.50_{0.50}Ti0.50_{0.50}N films crystallized in an FCC structure (see Figure 2). It can be clearly seen from Figure 2 that in the films deposited with Ts=250T_{\mathrm{s}} = 250 °C, there is a preferred c-200 orientation in the growth direction (GD), while the c-111 orientation is preferred at ϕ≈35∘\phi\approx35^\circ (see Figure 2 (a)). With increase in TsT_{\mathrm{s}} to 450 °C and 600 °C, the diffraction signal from c-111 is more randomly distributed in ϕ\phi. The diffraction pattern recorded for the Al0.50_{0.50}Ti0.50_{0.50}N film deposited at Ts=750T_{\mathrm{s}}=750 °C differs from the others. Firstly, the diffraction intensity recorded from the sample is relatively low despite using the same geometry and x-ray flux. The diffraction pattern shows that both c-111 and c-200 are weakly textured. However, the most intense diffracted intensity is seen at ϕ≈54∘\phi\approx54^\circ for c-111 and ϕ≈47∘\phi\approx47^\circ for c-200.

Image not extracted

Figure 2. Figure 2 shows the polar transformed 2D x-ray diffractograms of Al0.50_{0.50}Ti0.50_{0.50}N films deposited at a substrate temperature of 250 °C (a), 450 °C (b), 600 °C (c), and 750 °C (d) at the end of their depositions. For φ=90∘\varphi= 90^\circ and 0∘0^\circ, the growth direction (GD) and in-plane (IP) directions are assigned.

TEM micrographs of the films deposited at Ts=450T_{\mathrm{s}} = 450 °C and 750 °C are shown in Figure 3. Figure 3 (aFigure 1 shows a bright field TEM micrograph of the film deposited at Ts=450T_{\mathrm{s}} = 450 °C. The micrograph reveals 50-100 nm wide nanocolumns with no evidence of voids or under-dense grain boundaries. For the first ≈300\approx300 nm of deposition, a larger number of narrower columns are seen, consistent with our previous observations [21] and a result of competitive grain growth. SAED patterns were recorded at four different locations along the GD and marked as coloured circles in Figure 3 (aFigure 1. The SAED pattern recorded at the bottom of the film (green circle, Figure 3 aFigure 6) show a preferential c-200 orientation along the GD. There is however an azimuthal spread of the c-200 diffraction signal, indicating small grains with a mosaicity along the GD. The SAED pattern recorded at the top of the film (see orange coloured circle in Figure 3 (aFigure 1 and Figure 3 (aFigure 3) shows a spotty diffraction pattern, indicating larger grain sizes with film growth. To verify that the diffraction pattern is representative of the film structure, we recorded SAED patterns from multiple locations on the top part of the film and found that all patterns were consistent. The intense diffraction spots corresponding to c-200 are slightly tilted away from the GD, agreeing well with our in-situ XRD data (see Figure 2 (b)). In this case, a combination of 111 and 113 crystal planes from FCC-Al0.50_{0.50}Ti0.50_{0.50}N appear to be preferred along the GD. Similar observations are made from the SAED pattern recorded from the middle of the films (see Figure 3 (aFigure 4).

TEM micrographs and SAED patterns of Al0.50Ti0.50N thin films

Figure 3. Figure 3 shows TEM micrographs of the Al0.50_{0.50}Ti0.50_{0.50}N thin films deposited with TsT_\mathrm{s} of 450 °C (a1-a6) and 750 °C (b1-b6). Figures a1, b1 are BF-TEM micrographs; a2, b2 are STEM micrographs and corresponding EDS maps, and a3-a6, b3-b6 are the SAED patterns recorded at various locations (shown as dotted-coloured circles at Figure a1, b1). The diffraction signal present on the circumference of circles marked as 1, 2, 3, and 4 on Figures a3-a6 and b3-b6 are identified as 111, 200, 220, and 113 crystal planes of FCC-(Al, Ti)N. The green arrows in a3-a6 and b3-b6 represent the growth direction. The red arrows in Figures b3-b6 show diffraction from the 0002 planes of HCP-(Al,Ti)N.

Evolution of texture of 200 crystal planes of FCC-(Al,Ti)N along the azimuthal angle

Figure 4. Figure 4 shows the evolution of texture of 200 crystal planes of FCC-(Al,Ti)N along the azimuthal angle (φ)(\varphi) for film deposited with a substrate temperature, TsT_s, of 250 °C (a), 450 °C (b), 600 °C (c), and 750 °C (d). The dotted lines in (b) and (c) are guided lines for change in Φ\Phi as tft_f increases.

Figure 6. Figure 6 is the HRTEM image (a) and Fast Fourier Transformation (FFT) pattern (b) of the interface region of the Al0.50_{0.50}Ti0.50_{0.50}N thin film grown on Si (100) substrate deposited at Ts=750T_{\mathrm{s}} = 750 °C.

Figure 3 (bFigure 1 represents bright field TEM images of the film deposited with Ts=750T_{\mathrm{s}} = 750 °C and reveal a densely packed nanocrystalline-like morphology. The SAED patterns recorded at different film thickness (see coloured circle in Figure 3 (bFigure 1) are presented as Figure 3 (bFigure 3-bFigure 6. At the top of the film, the pattern consists of defined arcs rather than discrete spots as for the Ts=450T_{\mathrm{s}} = 450 °C film. This indicates that the film is composed of smaller. Irrespective of the film thickness, the c-220 crystal planes of FCC-(Al, Ti)N are predominantly textured along the GD, while c-111, and c-200 crystal planes textured close to 35-45° tilted away from the GD (see Figure 3 (bFigure 3-bFigure 6), in agreement with our in-situ XRD findings (see Figure 2 (d)). It was also observed that diffractograms from both c-111 and c-200 planes appeared very close to each other in azimuthal angle, φ\varphi. This suggests that there was some coherency between both c-111 and c-200 oriented grains in the film. Besides the diffraction pattern from FCC-(Al, Ti)N, we observed a faint diffraction signal from 0002 crystal planes (h-0002) of hexagonal-closed-packed (HCP)-(Al, Ti)N (see the red coloured arrow marked in Figure 3 (bFigure 3-bFigure 6). We also note that the diffraction from c-111 and h-0002 have the same azimuthal angle (Figure 3 (bFigure 3-bFigure 6), suggesting that the c-111 and h-0002 crystal planes share the same orientation. STEM-EDS mapping of Si, Al, Ti, and N, shown as Figure 3 (aFigure 2 and (b2) respectively, did not reveal any measurable compositional modulation in the films, and Al, Ti, and N form a uniform solid solution over the film thickness.

Figure 4 shows the texture evolution of c-200 planes of (Al, Ti)N thin films deposited at different TsT_\mathrm{s}. The film deposited at Ts=250T_\mathrm{s} = 250 °C shows that c-200 crystal planes are aligned along the GD (φ=90\varphi=90°) throughout the film thickness, tft_\mathrm{f} (see Figure 4 (a)). Contrary to this, as mentioned previously, film deposited at Ts=450T_\mathrm{s} = 450 °C and 600 °C show that c-200 crystal planes are textured at a certain tilt angle to the GD. Interestingly, as the tft_\mathrm{f} increases, the tilt angle of the c-200 texture also increases. The change in tilt angle as the tft_\mathrm{f} increases from 300 nm to ~1450 nm is estimated to 7° and 10° for film deposited with Ts=450T_\mathrm{s} = 450 and 600 °C respectively (see (b-c)). The results agree well with the SAED pattern recorded from thin film deposited with Ts=450T_\mathrm{s} = 450°C (see Figure 4 (aFigure 3-aFigure 6). The c-200 of the film that was deposited at Ts=750T_\mathrm{s} = 750 °C have a texture that is relatively broad along φ\varphi, but the intense spots only occur at φ≈45\varphi\approx45° and stay consistent throughout the thickness of the film (see Figure 2 (d)). Thus, two important observations are made from ex-situ data:

  1. In polycrystalline thin films of (Al,Ti)N, if c-200 crystal planes are tilted away from the GD, a mixed of c-111+c-113 textures develops along the GD.

  2. There is a consistent increase in the tilt angle of c-200 planes of grains that are formed far from the interface of the films compared to towards the interface of the films.

The texture formation of c-200 crystal planes along the GD is well documented in the literature, and is often attributed to the minimization of surface energy, strain energy, and the channelling effect of ions at lower substrate bias voltages (e.g., -40 V) that are observed in films deposited at Ts=250T_\mathrm{s} = 250 °C. However, the microscopic origin of the off-axis tilt of 200 crystal planes away from the GD has been debated throughout the literature. Rafaja et al. [27] attribute the inclined preferred orientation in AlTiN deposited by arc evaporation to the geometry of the deposition system with a non-rotating substrate. Wahlström et al. [28] argued the tilted texture of magnetron sputtered AlTiN films is due to the oblique path between the substrate and magnetron targets. Je et al. [29] attributed the ±5∘\pm5^\circ tilt of the 002 planes in TiN to competitive growth of 111 and 200 oriented grains, and to maintain the overall growth direction of 111 oriented grains close to the surface normal, the 200 oriented grains are tilted away. The inclined texture of nanostructured Al1−xTixN\mathrm{Al}_{1-x}\mathrm{Ti}_x\mathrm{N} is attributed to twin faults developed in the lattice by Kalss et al. [30]. Falub et al. argued an interdependence of texture and stress in arc evaporated AlTiN thin films and suggested stress can influence the texture formation, and the tilt angle increases with an increase in the level of stress in the films [17]. A similar interpretation is made for CrN [31, 32, 33], and Ti0.67Al0.33N\mathrm{Ti}_{0.67}\mathrm{Al}_{0.33}\mathrm{N} [34] thin films, where the transition of texture from c-200 to c-113 is attributed to a decrease in stress and film density. Karimi et al. suggest that competitive growth promotes the formation of c-111-oriented grains, and to accommodate growth of this c-111-oriented grain, the c-200-oriented grains are tilted away from the GD [35]. It was observed that with an increase in substrate temperature, the tilt angle of c-200 reduces owing to an increase in adatom mobility at higher substrate temperatures [35].

In our study, the off-axis tilt of c-200 texture cannot be attributed to the oblique incidence of metal vapours toward the substrate, as previously argued [27, 28, 36], because perfect alignment of c-200 texture along the GD is observed with film deposited at the same geometrical configuration (i.e., 35∘35^\circ inclination angle), but at a relatively lower TsT_s of 250250 °C. Our in-situ stress analysis (see Figure 5 (a-Figure 5d)) revealed that the stress level in films is also not responsible for the tilt of the c-200 texture as proposed by Falub et al. [17] and Karimi et al. [34]. The Al0.50Ti0.50N\mathrm{Al}_{0.50}\mathrm{Ti}_{0.50}\mathrm{N} thin film deposited at Ts=250T_s = 250 °C shows high stress state (see Figure 5 (a)), but the c-200 planes are perfectly textured along the GD. Between films deposited at Ts=450T_s = 450 °C and 600600 °C, the latter shows a lower stress (Figure 5 (b-Figure 5c)) and a higher off-axis tilt angle of c-200 than the former ones, contradicting the predictions by Falub et al.[17] and Karimi et al. [34]. A consistent increase in tilt angle with an increase in substrate temperature is also in contradiction to the model proposed by Karimi et al [34]. We propose that in these samples, along with the competitive growth mechanisms, other factors such as that which causes film surface roughening (e.g., the shadowing effect) during deposition [37] are together responsible for the off-axis tilt of c-200 in films deposited with Ts=450T_s = 450 °C and 600600 °C.

Evolution of biaxial stress and average crystallite size for Al$_{0.50}$Ti$_{0.50}$N films

Figure 5. (a-d) shows the evolution of biaxial stress ⟨σ111⟩\langle\sigma_{111}\rangle as a function of film thickness, tft_{\mathrm{f}}, of Al0.50_{0.50}Ti0.50_{0.50}N at a substrate temperature of 250 °C, 450 °C, 600 °C and 750 °C respectively. Figure (e-h) shows the temporal evolution of the average crystallite size ⟨D111⟩\langle D_{111}\rangle of the films deposited at a substrate temperature of 250 °C, 450 °C, 600 °C, and 750 °C, respectively.

To the best of our knowledge, there is no report on the dynamics of texture evolution that are determined in real time during the film depositions. The literature has never documented a constant rise in off-axis tilt with film thickness except observations made by Kubec et al. [38][37] in a multi-layered TiN and SiOx_x thin film and was attributed to the difference in nucleation nature between the substrate and SiOx_x buffer layer and between two TiN layers. At this point, our hypothesis is that the consistency of the off-axis tilt of the 002 texture of Ti0.50Al0.50N\mathrm{Ti}_{0.50}\mathrm{Al}_{0.50}\mathrm{N} thin films deposited at TsT_s of 450450 °C and 600600 °C is controlled by the rise in surface roughness [35][34] and/or formation of twinned crystallites with the film thickness.

The formation of c-220 texture, as seen in the film deposited with a TsT_{\mathrm{s}} of 750 °C, in TMNs' thin films deposited with PVD and CVD is seen previously. Often in PVD deposition process, the c-220 textured was seen, when depositions were carried out with high energetics ions [39, 40, 41] as <220> direction has the high degree of channelling effect in FCC lattice. While in CVD-deposited thin films, the formation of c-220 texture is attributed to the formation of twinned crystallites at temperatures lower than 1200 °C [42], and the formation of twinned crystallites is attributed to the lower adatom mobility. To gain a microscopic insight into the c-220 texture formation in Al0.50_{0.50}Ti0.50_{0.50}N film with TsT_{\mathrm{s}} = 750 °C, we probed the atomic scale crystal using HR-TEM. As the c-220 textured from at the very initial stages of depositions (as seen from the SAED pattern, see Figure 3 (bFigure 6) towards the interface of the film and substrate. Below a film thickness of 5 nm, the lattice planes could not be clearly resolved (see Figure 6(a)). However, beyond that, the formation of specific crystalline grains is seen. The formed grains are found to be faceted (see the yellow dotted lines in Figure 6 (a) and the angle between the normal of the crystal facets and the normal of the film/substrate interface varies from 35° to 45°. The FFT pattern (see Figure 6 (b)) also showed that the strongest intensity of the c-111 lattice planes was tilted away from the GD, along with a lower intensity of both c-111 and c-200 crystal planes being aligned along the GD. This established formation of c-111 crystal facets at very initial stages of depositions (tf≈15t_{\mathrm{f}} \approx15 nm) starts. A similar analysis for the film deposited with TsT_{\mathrm{s}} = 450 °C showed an intense texture of c-200 along the GD. The formation of these crystal facets could be driven by the change in supersaturation of Al in Al0.50_{0.50}Ti0.50_{0.50}N at this high temperature (TsT_{\mathrm{s}} = 750 °C) [43]. These newly formed facets are responsible for the further nucleation of tilted, 111-oriented grains. And since the angle between c-111 and c-220 crystal planes in the FCC lattice is 35.3°, the c-220 planes are textured along the GD in this case. The frequent re-nucleation induced nanocrystalline surface morphology, relatively higher growth rate, and formation of minute HCP-Alx_xTi1−x_{1-x}N in this film suggest the film is grown under high supersaturation [44, 45]. The appearance of the diffraction pattern of h-0002 crystal planes of HCP-Alx_xTi1−x_{1-x}N and c-111 of FCC-Al0.50_{0.50}Ti0.50_{0.50}N along the same azimuthal angle (as seen in Figure 3 (bFigure 3-bFigure 6) is commensurate with the symmetry and low lattice mismatch between these planes [46].

Figure 5 shows the evolution of biaxial stress (⟨σ111⟩\langle\sigma_{111} \rangle) and average grain/domain size (⟨D111⟩\langle D_{111} \rangle) as a function of tft_{\mathrm{f}}. Because of the low intensity of the diffraction signal, data could not be extracted below film thicknesses of ∼300\sim300 nm. For the film deposited with Ts=250T_{\mathrm{s}} = 250 °C, ⟨σ111⟩\langle\sigma_{111} \rangle increases consistently until tf≈800t_{\mathrm{f}} \approx800 nm, but at higher tft_{\mathrm{f}} the ⟨σ111⟩\langle\sigma_{111} \rangle decreases as tft_{\mathrm{f}} increases (see Figure 5 (a)) suggesting a compressive stress relaxation with film thickness. The films deposited at Ts=450T_{\mathrm{s}} = 450 °C and 600 °C show a clear power-law like relaxation of ⟨σ111⟩\langle\sigma_{111} \rangle with tft_{\mathrm{f}} (see Figure 5 (b,Figure 5c)). The power law fitting reveals that the σ0\sigma_{0}, cc and γ\gamma are -1.91 GPa, -27.13 GPa nmγ^{\gamma}, and 0.49, respectively for Ts=450T_{\mathrm{s}} = 450 °C and -1.62 GPa, -4.675 GPa nmγ^{\gamma} and 0.37, respectively for Ts=600T_{\mathrm{s}} = 600 °C. The evolution of ⟨σ111⟩\langle\sigma_{111} \rangle with tft_{\mathrm{f}} for the film deposited with Ts=750T_{\mathrm{s}} = 750 °C is different than Ts=450T_{\mathrm{s}} = 450 and 600 °C the previously discussed ones. Between tf≈300t_{\mathrm{f}} \approx300 nm and tf≈750t_{\mathrm{f}} \approx750 nm the ⟨σ111⟩\langle\sigma_{111} \rangle increases, while at larger tft_{\mathrm{f}} a consistent relaxation of ⟨σ111⟩\langle\sigma_{111} \rangle is observed (see Figure 5 (d)).

The evolution of average grain/domain size ⟨Dhkl⟩\langle D_{hkl} \rangle as a function of tft_{\mathrm{f}} is shown in Figure 5 (e-Figure 5h). The film deposited with Ts=250T_{\mathrm{s}} = 250 °C shows a consistent increase in ⟨D111⟩\langle D_{111} \rangle, reaching 18.2 nm at tf=1250t_{\mathrm{f}} = 1250 nm, beyond which a scattered value of ⟨D111⟩\langle D_{111} \rangle is seen (see Figure 5 (e)). When TsT_{\mathrm{s}} is raised to 450 °C, the estimated ⟨D111⟩\langle D_{111} \rangle increases with thickness to 25.2 nm at tf=1485t_{\mathrm{f}} = 1485 nm (see Figure 5 (f)). For the coatings grown at 600 °C, the maximum grain size of 22.2 nm is reached already at tf=620t_{\mathrm{f}} = 620 nm, beyond which it remains approximately constant (see Figure 5 (g)). At TsT_{\mathrm{s}} of 750 °C, the change in ⟨D111⟩\langle D_{111} \rangle is very small, and it increases from 11.5 nm to a maximum of 14.6 nm, as tft_{\mathrm{f}} increases from 300 nm to 1540 nm (see Figure 5 (h)).

The generation of compressive stress in polycrystalline thin films is widely reported in the literature and is attributed to densification of grain boundaries and the generation of defects in the bulk by high energy ions [47, 48]. The generation of compressive stress in our films agrees with the literature, as the films are deposited with a -40 V of substrate bias. However, the stress relaxation associated with an increase in total film thickness, tft_{\mathrm{f}}, needs to be explained. Also, the microscopic origin of anomalies in the ⟨σ111⟩\langle\sigma_{111} \rangle evolution in films deposited at Ts=250T_{\mathrm{s}} = 250 °C and 750 °C needs to be examined. The relaxation of compressive stress in films with an increase in film thickness indicates that a tensile component is being generated, often due to grain growth or larger average domain sizes. Since the deposition temperatures are well below the melting point of AlTiN (∼2949\sim2949 °C (Toth, n.d.)[48]) it is unlikely the grain growth due to bulk diffusion. Thus, we suggest the larger average grain sizes with increase in tft_{\mathrm{f}} originates from the kinetics effect (see Figure 5). The contribution from the tensile component of grain growth or increase in average grain size and the compressive component due to grain boundaries and adatom attachment to 2D islands formed at the surfaces of grains, were deconvoluted by Thompson et al. (Yu & Thompson, 2014)[49]. The instantaneous tensile stress due to grain growth (σingg\sigma_{\mathrm{in}}^{\mathrm{gg}}) is given by;

σingg(d)=E1−νΔad(11+(E1−ν)Δad1σy)(2)\sigma_{in}^{gg}(d)=\frac{E}{1-\nu}\frac{\Delta a}{d}\left(\frac{1}{1+\left(\frac{E}{1-\nu}\right)\frac{\Delta a}{d}\frac{1}{\sigma_y}}\right) \tag*{(2)}

where EE, and ν\nu are Young's modulus and Poisson’s ratio, respectively. The dd, Δa\Delta a, and σy\sigma_y represent the average grain size, excess free volume associated with grain boundaries, and biaxial tensile stress yield limit respectively. The authors [51] further argued that the instantaneous stress generated by the newly deposited surface layer (σ∗(t)\sigma^*(t)) is the ratio of the capture probability of adatoms to the grain boundary (Nadatoms−GB_{\mathrm{adatoms-GB}}) and to the newly formed 2D islands (Nadatoms−2Disland_{\mathrm{adatoms-2Disland}}). Thus, the compressive component of instantaneous stress is;

σincomp=−E1−ν2pδd(3)\sigma_{in}^{comp}=-\frac{E}{1-\nu}\frac{2p\delta}{d} \tag*{(3)}

where pp is the capture probability of the adatoms by the grain boundary, and δ\delta is the average distance between the 2D islands and the grain boundaries. In the smaller grain limit of d<Lislandd < L_{\mathrm{island}}, LislandL_{\mathrm{island}} being the 2D island spacing, the σincomp\sigma_{in}^{comp} is independent of grain size, dd. The transition of σincomp\sigma_{in}^{comp} being independent of dd to its inverse dependence to dd occurs at d=Lislandd = L_{\mathrm{island}}. We applied the model to the evolution of ⟨σ111⟩\langle\sigma_{111}\rangle with increasing film thickness tft_f. The instantaneous compressive stress was calculated through σincomp=⟨σ111⟩−σingg(d)\sigma_{in}^{comp} = \langle\sigma_{111}\rangle-\sigma_{in}^{gg}(d) for all four films. Even though the growth temperatures used for this study were relatively low for bulk diffusion that results into grain growth, for completeness of the model we estimate σingg(d)\sigma_{in}^{gg}(d) in following way. σingg(d)\sigma_{in}^{gg}(d) (mentioned as σ111gg\sigma_{111}^{gg} in Figure 7) was calculated using Δa=1\Delta a = 1 Å, and σy=830\sigma_y=830 MPa (the maximum converged tensile stress recorded from a similar study [21]) in Eqn. (2). The instantaneous dd was approximated to ⟨D111⟩\langle D_{111}\rangle. Thus, the estimated σingg(d)\sigma_{in}^{gg}(d) represent the maximum tensile stress generated by grain growth. For EE and ν\nu, the high temperature values of E111E_{111} and ν111\nu_{111} were used.

Instantaneous compressive stress as a function of inverse grain size

Figure 7. Figure 7 shows instantaneous compressive stress (σ111−σingg(d)\sigma_{111}-\sigma_{in}^{gg}(d) as a function of inverse of grain size (⟨D111⟩\langle D_{111}\rangle). The dashed/solid lines over experimental scatter data points shows linear fitting of the experimental σ111−σingg(d)\sigma_{111}-\sigma_{in}^{gg}(d) vs inverse of ⟨D111⟩\langle D_{111}\rangle.

The estimated σincomp\sigma_{in}^{comp} vs 1d\frac{1}{d} (or 1⟨D111⟩\frac{1}{\langle D_{111}\rangle}) is shown in Figure 7. At 1⟨D111⟩=0.072\frac{1}{\langle D_{111}\rangle}=0.072 nm−1^{-1} the behaviour changes. At values lower than 0.072 nm−1^{-1}, there is a linear dependence of σincomp\sigma_{in}^{comp} on 1⟨D111⟩\frac{1}{\langle D_{111}\rangle}, whereas for larger values, σincomp\sigma_{in}^{comp} is independent of 1⟨D111⟩\frac{1}{\langle D_{111}\rangle}. Thompson et al. [50] proposed that the transition from inverse dependence to independence of σincomp\sigma_{in}^{comp} occurs at d=Lislandd = L_{\mathrm{island}}. Thus, we identify the LislandL_{\mathrm{island}} to 1/0.0721/0.072 nm−1^{-1}=13.9 nm. We also estimated σingg(d)\sigma_{in}^{gg}(d) by varying Δa\Delta a from 0.5 Å to 1 Å and σy\sigma_y from 500 MPa to 1.0 GPa and analysed the dependence of σincomp\sigma_{in}^{comp} to 1⟨D111⟩\frac{1}{\langle D_{111}\rangle}. The obtained results are similar as discussed above. As a result, we suggest that, for grain sizes smaller than 13.9 nm, the compressive stress, ⟨σ111⟩\langle\sigma_{111}\rangle, does not relax with increasing in film thickness, despite an increase in grain size with film thickness. In this grain size regime, the capture probability of adatoms at the grain boundary is higher than that of the 2D islands formed on top of grains, leading to the generation of compressive stress. With grain size larger than 13.8 nm, the effect is reversed, and the capture probability of adatoms on 2D islands increases as grain size increases, leading to a reduction in the magnitude of compressive stress and hence a small stress relaxation observed in our films. The calculated LislandL_{\mathrm{island}} is in close agreement with our earlier predictions of the mean grain size (Do=13.4±3.6D_{\mathrm{o}} = 13.4 \pm3.6 nm) at which discrete islands shift to continuous films in Alx_xTi1−x_{1-x}N coatings [21]. The computed LislandL_{\mathrm{island}} and DoD_{\mathrm{o}} are within the range of 2D island spacing anticipated by classical nucleation theory [52].

The relatively smaller grain size in film deposited at Ts=250T_{\mathrm{s}} = 250 and 750750 °C compared to Ts=450T_{\mathrm{s}} = 450 and 600600 °C can be understood as follows:

  • (i) Because of the lower substrate temperature, TsT_{\mathrm{s}}, the adatom mobility as well as the grain boundary mobility are smaller, and hence the rate of increment of average grain size due to growth kinetics is lower. This leads to a smaller average grain size and, consequently, relatively narrow nanocolumns and an intercolumnar gap (as seen in Figure 1 (a)).

  • (ii) Adatom mobility and grain boundary mobility both rise as the substrate temperature rises to 450450 and 600600 °C, causing increase in average grain sizes as film thickness increases and the emergence of wider and denser nanocolumns (as seen in Figure 1 (b-Figure 1c) and Figure 3(aFigure 1).

  • (iii) At Ts=750T_{\mathrm{s}} = 750 °C, the development of smaller grain size is a little trickier. The nanocrystalline microstructure shows that during thin film growth, grain nucleation occurs frequently. It is possible that the formation of hexagonal Alx_xTi1−x_{1-x}N at grain boundaries driven by thermodynamics, as previously observed, is what limits kinetics induced grain growth, as suggested by the occurrence of a faint diffraction from HCP-Alx_xTi1−x_{1-x}N 0002 planes.

In Al0.50_{0.50}Ti0.50_{0.50}N thin films deposited at Ts=250T_{\mathrm{s}} = 250 °C, the evolution of ⟨σ111⟩\langle\sigma_{111} \rangle deviates from power-law after a total film thickness of 1250 nm, and the evolution of ⟨D111⟩\langle D_{111} \rangle becomes scattered (see Figure 5 (a) and (Figure 5e)). We also observe a discontinuity at the same tft_{\mathrm{f}} in the evolution of the integrated intensity of diffraction patterns from crystal planes c-111 and c-200. The SEM also demonstrates the film's lack of coherence (see Figure 1 (a)). Our earlier work made a similar set of observations, which we attribute to cohesive failure of films due to high stress fields. The critical stress (σcr.\sigma_{\mathrm{cr.}}) and critical film thickness (hcr.h_{\mathrm{cr.}}) values, which correspond to the point(s) of discontinuity in the graph of ⟨σ111⟩\langle\sigma_{111} \rangle vs tft_{\mathrm{f}}, can be used to calculate the plain strain fracture toughness (KICK_{\mathrm{IC}}) [21, 53, 54]. The KICK_{\mathrm{IC}} is estimated to be 4.45 ±\pm 0.4 MPa.m1/2^{1/2} for an approximate σcr.=σ111\sigma_{\mathrm{cr.}} = \sigma_{111}(at tf=1250t_{\mathrm{f}} = 1250 nm) and hcr.=1250h_{\mathrm{cr.}} = 1250 nm. This estimate is very similar to the Al0.50_{0.50}Ti0.50_{0.50}N films deposited at a relatively higher bias voltage (-80 V), but it is slightly higher than previously reported values for Al0.60_{0.60}Ti0.40_{0.40}N [1] and Al0.46_{0.46}Ti0.54_{0.54}N [55].

To characterize the effect of different microstructures to the mechanical properties of Al0.50_{0.50}Ti0.50_{0.50}N films, we measured the mechanical hardness and elastic recovery from thin films deposited with Ts=450T_{\mathrm{s}} = 450, 600, and 750 °C. The recorded hardness values are 30.4 ±\pm 1.4, 32.7 ±\pm 0.9, and 30.9 ±\pm 1.4 GPa. The elastic recovery is measured with a load of 10 mN and is found to be 43.7%, 47.6%, and 43.8% for film deposited at Ts=450T_{\mathrm{s}} = 450, 600, and 750 °C, respectively. As the uncertainty in the estimation of hardness is larger than the difference between samples, a definitive conclusion on the effect of microstructures on the mechanical hardness of Al0.50_{0.50}Ti0.50_{0.50}N thin film deposited with cathodic arc evaporation could not be drawn conclusively.

Summary

We used in-situ 2D synchrotron x-ray diffraction to investigate the impact of substrate temperature on the in-situ internal stress, crystallographic texture, and grain/crystallite sizes of Al0.50_{0.50}Ti0.50_{0.50}N thin films deposited on 100 surface of silicon using the reactive cathodic arc evaporation method. The thin films exhibited a single-phase FCC crystal structure and a nanocolumnar morphology, when they were formed at a substrate temperature of less than 750 °C. Small amounts of HCP phased Alx_xTi1−x_{1-x}N formed at substrate temperature of 750 °C, along with the dominating FCC phase, resulting in a nanocrystalline-like morphology. We discovered that the temperature of the substrate has a significant influence on the development of crystallographic textures. The 200 crystal planes are oriented parallel to the film-substrate interface at low substrate temperature (250 °C). The 200 crystal planes are tilted away from the direction perpendicular to the normal of the film/substrate interface as the substrate temperature rises to 450–600 °C, and a combination of 111 and 113 crystallographic texture is generated along the growth direction. When the substrate temperature reaches 750 °C, a 220 crystallographic texture begins to form. We also see that the off-axis tilt of 200 crystal planes increases between 7°–10° as the film thickness increases from ∼\sim250 nm to ∼\sim1400 nm. In conjunction with an increase in average grain size with an increase in overall film thickness, we observe a power-law-like behaviour of biaxial stress relaxation with increasing film thickness for films grown at 450–600 °C. Our investigation showed that the biaxial compressive stress is independent of grain size up to a certain size (determined as ∼\sim14 nm for Al0.50_{0.50}Ti0.50_{0.50}N), after which the stress level scales with the inverse of average grain sizes. The highest degree of biaxial compressive stress, which leads to film cohesive failure, is seen in the thin film of Al0.50Ti0.50N\mathrm{Al}_{0.50}\mathrm{Ti}_{0.50}\mathrm{N} formed at a substrate temperature of 250 °C. The plain strain fracture toughness of Al0.50Ti0.50N\mathrm{Al}_{0.50}\mathrm{Ti}_{0.50}\mathrm{N} is estimated to be 4.45 ± 0.4 MPa·m1/2^{1/2}, which is in good agreement with our earlier estimates.

Acknowledgments

The synchrotron experiments were conducted at DESY under the proposal I-20210060EC. We acknowledge the financial support from the Swedish Research Council (grant no 2017-06701) via the Röntgen Ångström Cluster (RÅC) Frame Program, the competence center FunMat-II supported by Vinnova (grant no 2022-03071), and the Swedish government strategic research area grant AFM (SFO Mat LiU, grant no 2009-00971)

References

  1. [1]M. Bartosik, C. Rumeau, R. Hahn, Z.L. Zhang, P.H. Mayrhofer, Fracture toughness and structural evolution in the TiAlN system upon annealing, Sci Rep. 7 (2017) 16476.DOI
  2. [2]N. Norrby, M.P. Johansson, R. M’Säoubi, M. Odén, Pressure and temperature effects on the decomposition of arc evaporated Ti₀.₆Al₀.₄N coatings in continuous turning, Surf Coat Technol. 209 (2012) 203–207. https://doi.org/10.1016/j.surfcoat.2012.08.068.
  3. [3]L. Hultman, G. Håkansson, U. Wahlström, J.E. Sundgren, I. Petrov, F. Adibi, J.E. Greene, Transmission electron microscopy studies of microstructural evolution, defect structure, and phase transitions in polycrystalline and epitaxial Ti₁-xAlₓN and TiN films grown by reactive magnetron sputter deposition, Thin Solid Films. 205 (1991) 153–164. https://doi.org/10.1016/0040-6090(91)90297-B.
  4. [4]G. Skordaris, K.D. Bouzakis, T. Kotsanis, P. Charalampous, E. Bouzakis, B. Breidenstein, B. Bergmann, B. Denkena, Effect of PVD film’s residual stresses on their mechanical properties, brittleness, adhesion and cutting performance of coated tools, CIRP J Manuf Sci Technol. 18 (2017) 145–151. https://doi.org/10.1016/j.cirpj.2016.11.003.
  5. [5]M. Abdoos, B. Bose, S. Rawal, A.F.M. Arif, S.C. Veldhuis, The influence of residual stress on the properties and performance of thick TiAlN multilayer coating during dry turning of compacted graphite iron, Wear. 454–455 (2020) 203342. https://doi.org/10.1016/j.wear.2020.203342.
  6. [6]N. Schalk, C. Mitterer, J. Keckes, M. Penoy, C. Michotte, Influence of residual stresses and grain size on the spinodal decomposition of metastable Ti₁-xAlₓN coatings, Surf Coat Technol. 209 (2012) 190–196. https://doi.org/10.1016/j.surfcoat.2012.08.052.
  7. [7]C. Wüstefeld, D. Rafaja, V. Klemm, C. Michotte, M. Kathrein, Effect of the aluminium content and the bias voltage on the microstructure formation in Ti₁-xAlₓN protective coatings grown by cathodic arc evaporation, Surf Coat Technol. 205 (2010) 1345–1349. https://doi.org/10.1016/j.surfcoat.2010.07.057.
  8. [8]F. Lomello, F. Sanchette, F. Schuster, M. Tabarant, A. Billard, Influence of bias voltage on properties of AlCrN coatings prepared by cathodic arc deposition, Surf Coat Technol. 224 (2013) 77–81. https://doi.org/10.1016/j.surfcoat.2013.02.051.
  9. [9]P. Patsalas, C. Charitidis, S. Logothetidis, The effect of substrate temperature and biasing on the mechanical properties and structure of sputtered titanium nitride thin films, Surf Coat Technol. 125 (2000) 335–340.DOI
  10. [10]J. Bujak, J. Walkowicz, J. Kusiński, Influence of the nitrogen pressure on the structure and properties of (Ti,Al)N coatings deposited by cathodic vacuum arc PVD process, Surf Coat Technol. 180–181 (2004) 150–157. https://doi.org/10.1016/j.surfcoat.2003.10.058.
  11. [11]K.M. Calamba, J. Salamania, M.P.J. Jõesaar, L.J.S. Johnson, R. Boyd, J.F. Pierson, M.A. Sortica, D. Primetzhofer, M. Odén, Effect of nitrogen vacancies on the growth, dislocation structure, and decomposition of single crystal epitaxial (Ti₁-xAlₓ)Nᵧ thin films, Acta Mater. 203 (2021) 116509. https://doi.org/10.1016/j.actamat.2020.116509.
  12. [12]R. Wuhrer, W.Y. Yeung, A comparative study of magnetron co-sputtered nanocrystalline titanium aluminium and chromium aluminium nitride coatings, Scr Mater. 50 (2004) 1461–1466. https://doi.org/10.1016/j.scriptamat.2004.03.007.
  13. [13]B.Y. Shew, J.L. Huang, The effects of nitrogen flow on reactively sputtered TiAlN films, Surf Coat Technol. 71 (1995) 30–36. https://doi.org/10.1016/0257-8972(94)02300-F.
  14. [14]L. Combadiere, J. Machet, Reactive magnetron sputtering deposition of TiN films. I. Influence of the substrate temperature on structure, composition and morphology of the films Laurette, Surf Coat Technol. 88 (1996) 17–27.DOI
  15. [15]L. Combadiere, J. Machet, Reactive magnetron sputtering deposition of TiN films. II. Influence of substrate temperature on the mechanical properties of the films, Surf Coat Technol. 88 (1997) 28–37. https://doi.org/10.1016/S0257-8972(96)02870-8.
  16. [16]Y.K. Wang, X.Y. Cheng, W.M. Wang, X.H. Gu, L.F. Xia, T.C. Lei, W.H. Liu, Microstructure and properties of (Ti, Al) N coating on high speed steel, Surf Coat Technol. 72 (1995) 71–77. https://doi.org/10.1016/0257-8972(94)02331-J.
  17. [17]C. V Falub, A. Karimi, M. Ante, W. Kalss, Interdependence between stress and texture in arc evaporated Ti--Al--N thin films, Surf Coat Technol. 201 (2007) 5891–5898.DOI
  18. [18]M. Beckers, N. Schell, R.M.S. Martins, A. Mücklich, W. Möller, The influence of the growth rate on the preferred orientation of magnetron-sputtered Ti-Al-N thin films studied by in situ x-ray diffraction, J Appl Phys. 98 (2005). https://doi.org/10.1063/1.1999829.
  19. [19]J.E. Greene, J.-E. Sundgren, L. Hultman, I. Petrov, D.B. Bergstrom, Development of preferred orientation in polycrystalline TiN layers grown by ultrahigh vacuum reactive magnetron sputtering, Appl Phys Lett. 67 (1995) 2928–2930.DOI
  20. [20]J.L. Schroeder, W. Thomson, B. Howard, N. Schell, L. Näslund, L. Rogström, M.P. Johansson-Jõesaar, N. Ghafoor, M. Odén, E. Nothnage, A. Shepard, J. Greer, J. Birch, Industry-relevant magnetron sputtering and cathodic arc ultra-high vacuum deposition system for in situ x-ray diffraction studies of thin film growth using high energy synchrotron radiation, Review of Scientific Instruments. 86 (2015) 95113.DOI
  21. [21]S. Nayak, T.-W. Hsu, L. Rogström, M. Moreno, J.M. Andersson, M.P. Johansson-Jöesaar, R. Boyd, N. Schell, J. Gimbmeier, J. Birch, and M. Odén, In-situ real-time evolution of intrinsic stresses and microstructure during growth of cathodic arc deposited (Al,Ti)N coatings, Unpublished. (2022).arxiv.org/abs/2301.03935
  22. [22]J. Kieffer, V. Valls, N. Blanc, C. Hennig, New tools for calibrating diffraction setups, J Synchrotron Radiat. 27 (2020) 558–566. https://doi.org/10.1107/S1600575200000776.
  23. [23]N. Shulumba, O. Hellman, L. Rogström, Z. Raza, F. Tasnádi, I.A. Abrikosov, M. Odén, Temperature-dependent elastic properties of Ti1- x Al x N alloys, Appl Phys Lett. 107 (2015) 231901.DOI
  24. [24]A.L. Patterson, The Scherrer formula for X-ray particle size determination, Physical Review. 56 (1939) 978.DOI
  25. [25]L.A. Giannuzzi, A Tutorial of the Fib Lift-Out Technique for TEM Specimen Preparation, Microscopy and Microanalysis. 5 (1999) 516–517. https://doi.org/10.1017/S1431927600015907.
  26. [26]W.C. Oliver, G.M. Pharr, Measurement of hardness and elastic modulus by instrumented indentation: Advances in understanding and refinements to methodology, J Mater Res. 19 (2004) 3–20. https://doi.org/10.1557/jmr.2004.19.1.3.
  27. [27]D. Rafaja, M. Šíma, V. Klemm, G. Schreiber, D. Heger, L. Havela, R. Kužel, X-ray diffraction on nanocrystalline Ti1- xAlxN thin films, J Alloys Compd. 378 (2004) 107–111.DOI
  28. [28]U. Wahlström, L. Hultman, J.E. Sundgren, F. Adibi, I. Petrov, J.E. Greene, Crystal growth and microstructure of polycrystalline Ti1-xAlxN alloy films deposited by ultra-high-vacuum dual-target magnetron sputtering, Thin Solid Films. 235 (1993) 62–70. https://doi.org/10.1016/0040-6090(93)90244-J.
  29. [29]J.H. Je, D.Y. Noh, H.K. Kim, K.S. Liang, Preferred orientation of TiN films studied by a real time synchrotron x-ray scattering, J Appl Phys. 81 (1997) 6126–6133. https://doi.org/10.1063/1.364394.
  30. [30]A. Karimi, W. Kalss, Off-axis texture in nanostructured Ti1 - xAlxN thin films, Surf Coat Technol. 202 (2008) 2241–2246. https://doi.org/10.1016/j.surfcoat.2007.08.074.
  31. [31]L. Chekour, C. Nouveau, A. Chala, C. Labidi, N. Rouag, M.A. Djouadi, Growth mechanism for chromium nitride films deposited by magnetron and triode sputtering methods, Surf Coat Technol. 200 (2005) 241–244. https://doi.org/10.1016/j.surfcoat.2005.02.062.
  32. [32]M.A. Djouadi, C. Nouveau, O. Banakh, R. Sanjinés, F. Lévy, G. Nouet, Stress profiles and thermal stability of CrxNy films deposited by magnetron sputtering, Surf Coat Technol. 151–152 (2002) 510–514. https://doi.org/10.1016/S0257-8972(01)01635-8.
  33. [33]C. Nouveau, M.A. Djouadi, M.A. Djouadi, O. Banakh, R. Sanjinés, F. Lévy, Stress and structure profiles for chromium nitride coatings deposited by r.f. magnetron sputtering, Thin Solid Films. 398 (2001) 490–495. https://doi.org/10.1016/S0040-6090(01)01435-3.
  34. [34]A.R. Shetty, A. Karimi, Formation of (113) texture in fcc nitride thin films and its influence on the film properties, Thin Solid Films. 528 (2013) 255–262. https://doi.org/10.1016/j.tsf.2012.08.062.
  35. [35]A.R. Shetty, A. Karimi, Texture change through film thickness and off-axis accommodation of (0 0 2) planes, Appl Surf Sci. 258 (2011) 1630–1638. https://doi.org/10.1016/j.apsusc.2011.10.037.
  36. [36]Y.H. Sohn, R.R. Biederman, R.D. Sisson, Microstructural development in physical vapour-deposited partially stabilized zirconia thermal barrier coatings, Thin Solid Films. 250 (1994) 1–7. https://doi.org/10.1016/0040-6090(94)90155-4.
  37. [37]Y. Zhao, Y. Qian, W. Yu, Z. Chen, Surface roughness of alumina films deposited by reactive r.f. sputtering, Thin Solid Films. 286 (1996) 45–48. https://doi.org/10.1016/S0040-6090(95)08514-9.
  38. [38]J. Keckes, R. Daniel, J. Todt, J. Zalesak, B. Sartory, S. Braun, J. Gluch, M. Rosenthal, M. Burghammer, C. Mitterer, S. Niese, A. Kubec, 30 nm X-ray focusing correlates oscillatory stress, texture and structural defect gradients across multilayered TiN-SiOx thin film, Acta Mater. 144 (2018) 862–873. https://doi.org/10.1016/j.actamat.2017.11.049.
  39. [39]Y.H. Cheng, B.K. Tay, Development of texture in TiN films deposited by filtered cathodic vacuum arc, J Cryst Growth. 252 (2003) 257–264. https://doi.org/10.1016/S0022-0248(03)00871-6.
  40. [40]H.S. Park, D.H. Jung, H.D. Na, J.H. Joo, J.J. Lee, The properties of (Ti,Al) N coatings deposited by inductively coupled plasma assisted d.c. magnetron sputtering, Surf Coat Technol. 142–144 (2001) 999–1004. https://doi.org/10.1016/S0257-8972(01)01217-8.
  41. [41]T. Hurkmans, D.B. Lewis, H. Paritong, J.S. Brooks, W.D. Münz, Influence of ion bombardment on structure and properties of unbalanced magnetron grown CrNx coatings, Surf Coat Technol. 114 (1999) 52–59. https://doi.org/10.1016/S0257-8972(99)00031-6.
  42. [42]H.E. Cheng, M.H. Hon, Texture formation in titanium nitride films prepared by chemical vapor deposition, J Appl Phys. 79 (1996) 8047–8053. https://doi.org/10.1063/1.362358.
  43. [43]H.X. Lin, Z.C. Lei, Z.Y. Jiang, C.P. Hou, D.Y. Liu, M.M. Xu, Z.Q. Tian, Z.X. Xie, Supersaturation-dependent surface structure evolution: From ionic, molecular to metallic micro/nanocrystals, J Am Chem Soc. 135 (2013) 9311–9314. https://doi.org/10.1021/ja404371k.
  44. [44]D.G. Vlachos, Growth of elongated nanostructures, Materials Science and Engineering A. 204 (1995) 90–95. https://doi.org/10.1016/0921-5093(95)09943-3.
  45. [45]J. Nyvlt, Kinetics of nucleation in solutions, J Cryst Growth. 3 (1968) 377–383. https://doi.org/10.1016/0022-0248(81)90380-8.
  46. [46]D. Rafaja, C. Wüstefeld, M. Dopita, M. Motylenko, C. Baeh tz, C. Michotte, M. Kathrein, Crystallography of phase transitions in metastable titanium aluminium nitride nanocomposites, Surf Coat Technol. 257 (2014) 26–37. https://doi.org/10.1016/j.surfcoat.2014.01.039.
  47. [47]E. Chason, B.W. Sheldon, L.B. Freund, J.A. Floro, S.J. Hearne, Origin of Compressive Residual Stress in Polycrystalline Thin Films, Phys Rev Lett. 88 (2002) 4. https://doi.org/10.1103/PhysRevLett.88.156103.
  48. [48]E. Chason, P.R. Guduru, Tutorial: Understanding residual stress in polycrystalline thin films through real-time measurements and physical models, J Appl Phys. 119 (2016) 191101. https://doi.org/10.1063/1.4949263.
  49. [49]L.E. Toth, Transition Metal Carbides and Nitrides (Academic Press, New York, 1971)., (n.d.).
  50. [50]H.Z. Yu, C. V. Thompson, Grain growth and complex stress evolution during Volmer-Weber growth of polycrystalline thin films, Acta Mater. 67 (2014) 189–198. https://doi.org/10.1016/j.actamat.2013.12.031.
  51. [51]H.Z. Yu, C. V. Thompson, Grain growth and complex stress evolution during Volmer-Weber growth of polycrystalline thin films, Acta Mater. 67 (2014) 189–198. https://doi.org/10.1016/j.actamat.2013.12.031.
  52. [52]T. Michely, J. Krug, Islands, mounds and atoms, Springer Science \& Business Media, 2012.
  53. [53]J.H. Huang, Y.H. Chen, A.N. Wang, G.P. Yu, H. Chen, Evaluation of fracture toughness of ZrN hard coatings by internal energy induced cracking method, Surf Coat Technol. 258 (2014) 211–218. https://doi.org/10.1016/j.surfcoat.2014.09.026.
  54. [54]A.-N. Wang, G.-P. Yu, J.-H. Huang, Fracture toughness measurement on TiN hard coatings using internal energy induced cracking, Surf Coat Technol. 239 (2014) 20–27.DOI
  55. [55]W.M. Seidl, M. Bartosik, S. Kolozsvári, H. Bolvardi, P.H. Mayrhofer, Influence of Ta on the fracture toughness of arc evaporated Ti-Al-N, Vacuum. 150 (2018) 24–28.

Paper details

vlnc:W_hrsbau5e
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper