WorksPhysics and Astronomy
Enhanced Ionic Conductivity of confined Ionic-Liquid in Angstrom-scale 2D channels
Abstract
Understanding ion-transport under molecular confinement is essential for developing next-generation energy technologies, where ionic motion often occurs within nanoscale or angstrom-scale channels. In this study, we use the model system of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide ([EMIM]+[TFSI]-) confined within angstrom-scale slit-shaped 2D channels fabricated via van der Waals assembly to exemplify a broader class of confined ionic liquids.This system provides a well-defined platform to unravel generic features of ion transport under extreme confinement. By systematically varying the channel height h, we demonstrate a non-monotonic conductivity dependence on confinement, with a maximum 26.7 S/m at confining height, 1.02 nm, over 30 times of the bulk value for these ionic liquids. The variation of conductivity with confinement arises from structural rearrangements of ionic layers in the slit channel. Enhanced values of conductivity occur under confinements that promote the breakup of ion pairs and larger clusters, thereby increasing the number of free ions. Stronger confinement (h, 0.68 nm) also leads to steric hindrance, lowering conductivity below bulk values. Furthermore, introducing co-solvents with a higher dielectric constant and lower viscosity, such as acetonitrile (ACN), amplifies conductivity to ~145 S/m. Comparative studies using ACN, dimethyl carbonate and diethyl carbonate highlight that both large dielectric constant and low viscosity critically govern ion transport under confinement, as also supported by molecular dynamics simulations. Overall, this work establishes confined [EMIM]+[TFSI]- as a representative system for probing mechanisms of nano- and angstrom-scale ion transport, demonstrating how nanoconfinement and the solvent environment can be systematically tuned to manipulate ionic conductivity at the molecular level.
#
Equally contributed
*Correspondence to: [email protected] and [email protected]
Introduction
Room-temperature ionic liquids (ILs), liquids composed entirely of cations and anions, have emerged as a distinctive class of electrolytes in both practical applications and fundamental research.[1] Their unique physicochemical properties such as non-volatility, high thermal and chemical stability, low flammability, and broad electrochemical windows, make them particularly attractive for energy-related technologies. ILs are considered promising candidates for use as electrolytes or additives in electrochemical double-layer capacitors (EDLCs) and have garnered significant attention in the broader field of energy storage. Although extensive research has studied the bulk properties of ILs including conductivity, electrochemical stability, transport properties, supramolecular structure, self-assembled solvent organization, and the free and bound states of ions;[1, 2, 3] their behaviour under nanoscale confinement has only recently emerged as a focus of study.[4, 5, 6, 7] Over the past two decades, EDLCs based on nanoporous materials have attracted increasing interest due to remarkable improvements in energy density under strong confinement.[8, 9, 10] A growing research focus is on understanding how nanoscale confinement influences the transport properties of room-temperature ILs.[11] Although their bulk properties such as viscosity, diffusion, and ionic conductivity are well characterized,[1, 2, 3] the behaviour of ILs under nanoscale confinement in systems such as conical nanopores,[12, 13] porous membranes,[14, 15, 16] and carbon-based matrices[17, 18] reveal the effects of different pore geometry and surface chemistry of the pore walls. This opens an exciting and highly promising direction for both experimental and theoretical investigation, as understanding ionic motion within nanoscale or Å-scale channels is becoming essential for the development of next-generation iontronic technologies, including energy storage devices.
Recent advances in van der Waals (vdW) assembly techniques now enable the fabrication of Å-scale slit-shaped 2D channels with precisely tunable dimensions.[19, 20] These platforms with Å-scale confinement present a unique opportunity to investigate ion transport in regimes dominated by molecular-scale packing, ion-wall interactions, strong Coulomb correlations, and steric effects. In such extreme confinements, classical continuum models often fail, giving rise to novel and unique transport phenomena such as ultra-fast water transport[19] and charge- and size-selective ion transport,[21, 22] enabling ionic memristors,[23] molecular sensing,[24] and advanced spectroscopy.[25]
In this study, we systematically explore how Å-scale confinement and solvent environment affect the conductivity of a room temperature IL, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl) imide ([EMIM][TFSI]), a well-studied one and known, in particular, for its excellent electrochemical stability. Using 2D channels with tunable ranging from sub-nm to 66 nm, we first examine of the pure IL, revealing a non-monotonic dependence of on confinement with a pronounced peak at ∼10.2 Å, suggesting enhanced ion mobility under optimal confinement. Beyond confinement effects, the introduction of co-solvents offers an additional tool to modulate ionic transport. Solvents of high dielectric constant () facilitate dissociation of ion pairs and higher order ion clusters, while low viscosity () ones enhance ion mobility. Complex interplay between confinement-induced structural ordering and solvent-mediated screening, largely unexplored earlier in concentrated ionic systems such as ILs, will be studied in this paper.
Materials and methods
Fabrication of slit shaped 2D channels
2.1. Fabrication of slit shaped 2D channels: The slit-shaped 2D channels were fabricated by van der Waals (vdW) assembly of three layers of 2D materials, viz., top, bottom and spacers following our previously reported method.[19, 20] Briefly, the bottom layer, the spacers, and the top layers are subsequently transferred onto a pre-made SiN hole, followed by etching from the hole side to expose the channels, as shown in fig:S1A. The top and bottom are 2D layers of hexagonal boron nitride (hBN), while the spacers were parallel strips (Fig. S1B, representative AFM image) of graphene layers. The number of layers is chosen depending on the requirements of the devices. A microscopic image of a trilayer stack is shown in fig:S1C. A Cr(5nm)/Au(50nm) layer is deposited on top of the trilayer stack to enhance the adhesion of the channels with the SiN substrate and to define the channel length (). The height () of the 2D channels were determined by the number of graphene layers in the spacer flake (= 3.4 × number of graphene layers). The width () of the channels is defined by the space between the parallel array of spacers, generally 100 to 150 nm. The number of channels () for the devices are in the range of 200 ± 20.
Synthesis of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl) imide ([EMIM][TFSI])
The ([EMIM][TFSI]) was synthesized following a procedure we previously reported.[26] Briefly, 75 g (0.5115 mol) 1-ethyl-3-methylimidazolium chloride and 154 g (0.54 mol) of lithium bis(trifluoromethanesulfonyl)imide were dissolved separately in 100 mL water. The two solutions were then mixed and stirred continuously at 40 °C overnight. The resulting mixture was transferred to a separating funnel and allowed to rest until two distinct phases formed. The bottom phase, consisting predominantly of the ionic liquid, was collected, while the top aqueous phase containing LiCl impurities was discarded. The collected ionic liquid phase was washed repeatedly with deionized (DI) water (at least twice the volume of the ionic liquid per wash). After thorough mixing, the mixture was transferred back to the separating funnel, and the ionic liquid phase was collected again. This washing process was repeated at least 10 times to ensure complete removal of LiCl impurities. Finally, the purified IL was dried under vacuum (<6 × 10 bar) at 70 °C for 3 days to remove residual water.
Electrochemical cell setup and measurement protocol
The electrochemical cell, constructed from polyether ether ketone (PEEK), features two small reservoirs designed to hold solutions and accommodate 2D channel devices. The devices are clamped between the reservoirs with the aid of two O-rings for sealing. Each reservoir has a capacity of ~0.4 mL and includes slots for electrode insertion. Prior to each measurement, the cell and O-rings were thoroughly cleaned using DI water and dried with a nitrogen gas flow. Once the 2D channel device was placed in the cell, either pure organic solvents or DI water, depending on the solution being tested, were injected into the cell to wash and wet both the cell and 2D channel devices. The voltage-dependent-current () characteristics were measured using a Biologic potentiostat (SP-300) equipped with an ultra-low current cable booster, offering a base current range from 1 μA to 1 pA. The potentiostat low current resolution can reach 80 aA within the 1 pA range, as specified in the instructions. Data observed from the potentiostat were analysed using EClab software. Freshly prepared Ag/AgCl electrodes were used for each - measurement using two-electrode configuration where the reference and counter-electrode were connected to one Ag/AgCl electrode and the working electrode was connected to the other. The voltage scan rate was set at 40 mV s and when necessary, it was lowered to avoid capacitive effects that could mask the resulting current. All experiments were conducted at room temperature (293 K) inside a faraday cage.
Channel height () dependent - measurements through slit-shaped 2D channels device
The effect of molecular confinement on the of [EMIM][TFSI] was investigated by measuring the characteristics in slit-shape 2D channels of different values of . These 2D channels were fabricated by vdW assembly of 2D materials, primarily using hBN as the top and bottom walls, sandwiching layers of graphene strips as parallel spacers (schematic shown in fig:S1).[19, 20] The resulting trilayer stack was then placed over a pre-made micro-hole, forming the confined fluidic devices; schematic and microscopic images are in fig:1A and fig:1B, respectively. These devices offer excellent tuning of the channel dimensions even at the Å-scale level: length (), width () and channels number () through nano-lithography process and determined by the selection of the number of graphene layers () in the spacers, following the relation Å. The - curves were recorded by sandwiching the device between two electrolyte reservoirs containing custom-made Ag/AgCl electrodes connected to a potentiostat (schematic represented in fig:S5).
2.5. Conductivity and conductance relationships: The conductance of a 2D channel device is given by: where is conductivity, is channel width, is channel height, is channel length, and is the number of channels in the device.[21, 27] The channel resistance is on the Gigaohm (G) scale, which is much larger than the entry-exit resistance of the channel. Consequently, the conductance of ions is dominated by ion diffusion within the channel.
2.6. Molecular dynamics (MD) simulations: The MD simulations of the [EMIM][TFSI] inside the slit-shaped 2D channels are executed using the experimental setup represented in Figure 2A. The channel size was defined as the slit height (), following the experimental convention, and ranged from 3.3 Å to ~40 Å. The channel and reservoir lengths were set to 7 nm and 10 nm, respectively. Periodic boundary conditions were applied in all three directions. The channel walls (hBN surfaces in our case) were treated as rigid in all simulations, and B and N atoms were described using a Lennard-Jones potential[28], while the ionic liquid [EMIM][TFSI] was represented with an all-atom model.[29] The partial charges of cation and anion were scaled to 0.8 to account for the polarization. All simulations were carried out using the GROMACS software package.[30] In electrostatic interactions between charges representing ions and their interaction with hBN-walls, image forces due to dielectric polarizability of the hBN walls were not taken into account. The temperature of the IL was maintained at 300 K using the velocity-rescale thermostat within the canonical ensemble, where the number of particles (N), volume (V), and temperature (T) of the system are kept constant (NVT). Electrostatic interactions were computed using the particle mesh Ewald (PME) method[31, 32], with a fast Fourier transform (FFT) grid spacing of 1 Å and a real-space cutoff of 1.2 nm. The systems were initially annealed from 400 K to 300 K over 5 ns, followed by an additional 15 ns of NVT simulation to achieve equilibrium. Subsequently, a further 10 ns of NVT simulation was performed for static property analysis. To improve statistical reliability, three independent simulations were conducted for each channel size.

Figure 2. Molecular dynamics (MD) simulations. (A) Schematics of MD simulation system setup. (B) dependent enhancement of estimated based on Green-Kubo equation, relative to the . (C) Ion number distribution along the of the channels. represents the central plane between the channels’ walls and the grey shaded areas, which represent the individual walls. Schematic of effect on the ion distribution; (D) 3.3 Å, (E) 10 Å, and (F) 23.3 Å.
The Green–Kubo (GK) equation has been used to estimate the as it accounts for all interactions in dense ionic systems and provides a more reliable estimate than the Nernst–Einstein equation, which tends to overestimate the of concentrated electrolytes.[3] The slit is confined along (~7 nm, i.e. length) but unbounded in under periodic boundary conditions, and the conductivity is anisotropic. Therefore, the reported reflects in-plane transport and allows direct comparison with experiments. Thus, from the GK-equation:
where is the slit-volume, is the Boltzmann constant, and is the temperature, denotes the component of the electric current along the -direction at time (Figure 2A). For each case, a 3 ns production simulation was performed, with trajectories saved every 0.05 ps for current autocorrelation function analysis. To improve statistical accuracy, fifteen independent simulations were carried out for each system, starting from different equilibrium configurations.
Results and discussions
Considering the ionic size of the [EMIM] and [TFSI] ion[33] (Figure 1C), 2D channels with ranging from ~ 6.8 Å to 660 Å are used to investigate the confinement effect on the transport of the pure [EMIM][TFSI]. The IVs through these 2D channels are linear, however slopes varied depending on (with other dimensions being constant), Figure 1D. The bulk of pure [EMIM][TFSI] varies depending on factors such as water content, temperature, and measurement methods, typically ranging between 0.5 and 1 S.m.[34, 35] We obtained a S.m for pure liquid when measured using: (i) standard conductivity meter and (ii) measured through a micro-hole (25 m 2.5 m 500 nm). For the 2D channels with Å, is comparable to the bulk value. Increasing the confinement by reducing enhances to a maximum of 26.7 at Å (Figure 1E). However, further confinement to Å results in . In contrast, these 2D channels with aqueous electrolytes exhibit suppressed values regardless of the type of ions used.[21, 22, 36] Thus, the confinement induced enhancement in demonstrates the tunability of of with confinement, providing a route to manipulate ionic transport by precisely controlling at the atomic scale.
!Confinement effect on [EMIM]+[TFSI]− conductivity bbox=0.15,0.18,0.88,0.55
Figure 1. Confinement effect on conductivity (). (A) Schematic of the slit-shaped 2D channels on top of a micro-hole. Inset shows the cross-section view of a 2D channel. (B) Microscopic image showing the top-view of slit-shaped 2D channels device, where the spacers and 2D channels are sandwiched between the top and bottom layers. (C) Molecular structure and effective size of and ions. Comparison of (D) the voltage-dependent-current (-) curves of 2D channel devices with channel heights () of 6.8 Å, 10.2 Å and 13.6 Å. (normalized channels dimensions: length () = 1 μm, width () = 100 nm and number of channels () = 200) and (E) the dependent of different channels, with the and using ionic liquid as the electrolyte. In (D), the 6.8 Å plot is multiplied by 10 times for better comparison. The dotted line in (E) is a guide to the eye.
We continue with describing the MD simulations results of the behaviour in the slit-shaped 2D channels to understand this confinement-enhanced of . The calculated (estimated by Green–Kubo relation, detailed in methods section) exhibits a non-monotonic dependence on , with a maximum at Å (Figure 2B), consistent with the experimental findings (Figure 1E). Although the maximum occurs at the same height, it is less pronounced than in the experiments. Nevertheless, the similar qualitative trend suggests that the experimentally observed enhancement originates from intrinsic ion dynamics under nanoscale confinement. To understand this behaviour, we first examined the in-channel ion structure by analysing number-density distributions (Figure 2C), since the local organization of confined IL strongly influences their dynamics.[37] At Å, only a single mixed layer forms near the channel midplane. At Å, however, the ions reorganize into three distinct layers: cations preferentially located near the hBN walls due to stronger interactions between the imidazolium ring and the surface, while an additional cation layer emerges at the centre, and anions populate a layer in between the two cation layers. As increases further, the central region becomes increasingly bulk-like. 2D number-density maps confirm that the emergence of this three-layer structure in the 10 Å-channel disrupts crystal-like ordering in the narrowest channel (Figure 3), thereby enhancing ionic dynamics.

Figure 3. The 2D number density of and inside the slit-shaped 2D channels (A) in the first interfacial layer, close to the wall and (B) in the middle region.
The confinement also affects the rotational degrees of freedom of the ions (fig:S7). The confinement elicits a channel-size dependent reorientation of both ions. In the narrowest slit ( Å), there is only one layer, where cations are predominantly perpendicular to the hBN plane and anions align in-plane. At intermediate (10 Å to 13.2 Å), the ring of interfacial cations reorient toward parallel to the plane, while anions develop a robust tilted subpopulation; The center at Å mirrors this motif. Wider slits exhibit increasingly random, bulk-like orientations in the middle region, alongside a partial rebound of edge-on cations at the interface and a decline of tilted-anion fraction. Notably, the face-on (parallel) configuration at 10 Å is expected to weaken cation-anion interlocking and reduce electrostatic caging, thereby promoting ionic mobility and potentially enhancing the conductivity by enhanced in-plane motion.[10, 37]
Further insight into the confinement-dependent conductivity is obtained from the free-ion population inside the channels. In IL, conductivity arises from the fraction of the free ions, while the majority of the cations and anions readily form ion pairs.[3] The in-channel number density of free ions increases from 2.08 nm at Å to 2.30 nm at Å, then gradually decreases toward the stable value (fig:S9A), displaying a nonmonotonic dependence on , peaking at Å (19%). In addition, the diffusion coefficients (simulated for free ions via Green-Kubo relation) show an oscillatory dependence on , reaching a maximum at Å for both cations and anions (fig:S9B). Thus, at Å originates from a cooperative structural and dynamical transition. In the narrowest slit, strong confinement enforces a single mixed layer with crystal-like ordering and the resulting steric hindrance severely limits ion transport and mobility. At Å, the system reorganizes into a three-layer (cation-anion-cation) arrangement, with ions adopting predominantly parallel orientations relative to the channel walls. This configuration weakens cation-anion interlocking, reduces electrostatic caging and steric constraints, and enhances free-ion diffusivity along the unconfined direction. Together with the peak in free-ion fraction, these effects account for the observed conductivity enhancement compared with other nano-channels.
In IL-solvent mixtures, the of an electrolyte depends on several factors including , , , diffusion coefficient and, critically the population of actual mobile charge carriers. The characteristics of the solvents used to prepare the electrolyte play a substantial role in determining its electrochemical properties. Solvents with higher promotes more ion dissociation, increasing the number of free charge carriers and thereby increasing . The capacitance, , and of ILs in different organic solvents vary with dilutions.[38, 39] To investigate the effect of confinement on at different dilutions, we select ACN as a solvent, which has a higher of 37.5, as compared to 12 of pure [EMIM]+[TFSI]−, and its strong dipole–dipole interactions, which promote preferential head-to-tail, antiparallel molecular arrangements and weak hydrogen bonding with .[39, 40, 41, 42, 43] For a 2D slit-channel device with Å, the addition of ACN initially enhances increasing from S.m to a maximum of S.m upon diluting the IL from 3.88 M (i.e., pure concentration) to 1.5 M. Beyond this concentration, however, decreases with further dilution, Figure 4B. This trend in with dilution is also observed but with a different magnitude (20 to 47 times, depending on the dilutions) (Figure 4B). Furthermore, we have investigated this dilution-dependent of under different degrees of confinement within the 2D channels, viz., (Å) = 6.8, 13.6, 23.8, 30.6 and 660. The dependence of as a function of exhibited similar behaviour for all confinement conditions, as shown in fig:S11. However, the measured at each followed the same trend as the confinement-dependent- of pure ; at each , increases as the confinement decreases, reaching a maximum at 10.2 Å and then decreases with further confinement, Figure 4C. This behaviour indicates the existence of an optimal confinement, arising from a balance between confinement-induced ordering and excessive steric restriction. To evaluate the influence of on , we then used dimethyl carbonate (DMC) as a solvent to dilute . DMC has a very low of 0.629 cP, significantly lower (55 times) than that of pure (35 cP).[44] When is diluted with DMC (), initially increases from 24 to 28.1 S.m for 2D channel device with Å as decreases from 3.88 to 2 M. Below 2 M, begins to decrease with further dilution, Figure 5A. A similar trend is observed in the micro-hole, though the overall values are lower. This difference in emphasizes the additional impact of geometric confinement on ion-transport of these electrolytic solutions, where slit channels provide more favourable conditions for directional and ordered ion migration compared to micro-hole slits. To further probe the role of solvent and properties, we also studied diluted in diethyl carbonate (DEC), which has a cP and . The profile in DEC follows a similar trend as in DMC: down to M, increases but then declines with further dilution (Figure 5B). However, the maximum values in DEC (Figure 5B) are some 1.7 times smaller than those in DMC (Figure 5A) under comparable confinement (partially due to slightly lower and higher ; the difference in those values, however, is not that significant to entirely explain that effect).
!Effect of acetonitrile on conductivity of [EMIM]+[TFSI]− bbox=0.10,0.52,0.90,0.72
Figure 4. Effect of acetonitrile on . (A) Concentration dependent - curves of a Å slit-shape 2D channels device (channels dimensions: m, nm and ). Comparison of the in ACN (B) of Å slit-shaped 2D channels and a micro-hole, and (C) of slit-shape 2D channels of various with mM, 1.5 M and 2.94 M in ACN as electrolytes. The dotted lines in (B) and (C) are guides to the eye.
Figure 5. Effect of solvent on . Concentration dependent of Å slit-shaped 2D channels and a micro-hole with different solvents: (A) dimethyl carbonate (DMC) and (B) diethyl carbonate (DEC). (C) -dependent of slit-shaped 2D channels for 1.5 M in ACN, DMC and DEC as solvents. The dotted lines in (B) and (C) are guides to the eye.
To understand the solvent-dependent of , MD simulations were performed with ACN, DMC, and DEC at various concentrations under bulk conditions. For the pure IL (3.88 M), the fraction of free ions is low (15.4%) due to strong Coulombic interactions promoting ion pairing.[3] Dilution increases the free ion fraction (Fig. S14A) as solvent molecules partially screen these interactions. ACN shows the most pronounced increase, reaching 81.3% at 0.1 M, whereas DMC and DEC remain relatively low (25% to 35%) across the concentration range, reflecting their limited dielectric screening. Consequently, ACN also exhibits the highest free ion density (Fig. S14B), DMC intermediate, and DEC the lowest, subject to their dielectric constants. Diffusion coefficients of both cations and anions increase with dilution as crowding and electrostatic correlations weaken. IL dissolved in ACN presents the highest mobility, followed by in DMC and DEC (fig:S14C). The resulting ionic conductivity reflects the combined effects of free ion density and mobility: rises with initial dilution, peaks at intermediate concentrations, and then decreases at very low concentrations due to the limited number of charge carriers. ACN exhibits the highest owing to its high dielectric constant and low viscosity, DMC shows intermediate values, and DEC the lowest, dominated by higher viscosity and weaker dielectric screening. These bulk trends provide a baseline for understanding confinement effects, as the same interplay of ion dissociation, mobility, and solvent properties govern in 2D channels, where additional geometric restrictions can further enhance or modulate conductivity.
fig:5c presents the variation of with slit channel height at a fixed [EMIM][TFSI] C of 1.5 M across the three solvents: ACN, DMC, and DEC. In all cases, is highest at Å and gradually decreases as increases. At the smallest confinement of 6.8 Å, conductivity drops below the level observed in bulk conditions because the space becomes too tight for ions to move freely due to steric hindrance. This observation confirms that molecular confinement plays a critical role in determining ion transport. Among the solvents, [EMIM][TFSI] in ACN exhibits the highest across all , while DMC shows intermediate and DEC yields the lowest values. This trend may arise because ACN combines a high (37.5) with (0.334 cp), promoting efficient ion dissociation and high ionic mobility, whereas DMC has relatively low (0.629 cp) and moderate (3.1), and DEC has a (0.75 cp) and lower (2.8). However, further studies are required to understand the complex interplay of ionic liquids diluted in different solvents under confinement, since confining solvents in Å-scale channels can suppress the .[25] Nevertheless, ACN reinforces its role as an effective molecular ‘lubricant,’ easing ion motion in room temperature Ils– whether in the bulk or in nanoconfinement.
Conclusion
This study demonstrates how Å-scale confinement and organic solvent additives influence the of [EMIM][TFSI]. Confining the ionic liquid within 2D channels leads to a remarkable enhancement in , peaking at of Å due to confinement-induced mobility enhancement. However, when approaches the ionic diameter, steric hindrance reduces . Further modulation of is achieved by introducing solvents such as ACN, DMC, and DEC, which affect ion dissociation and mobility through their and . Among them, ACN achieves the highest values due to its favourable combination of high , which suppresses clustering of ions in IL, as well as low . These findings highlight the effects of precise control over nanoscale geometry of the ion channels and electrolyte composition. By combining experiment and MD simulations, we established that the conductivity maximum originates from a confinement-driven transition in ion layering and orientation, which enhances free-ion fraction and in-plane diffusivity.
Acknowledgements
B.R. acknowledges funding from the Royal Society University Research Fellowship URF\R\231008, Philip Leverhulme Prize PLP-2021-262, European Union’s H2020 Framework Programme/ERC Starting Grant 852674 - AngstroCAP, EPSRC new horizons grant EP/X019225/1, Leverhulme Trust grant No. RPG-2025-136. A.K. acknowledges Royal Society grant ICA\R1\231014 and the Leverhulme Trust grant No. RPG-2026-190. B.R and A.K acknowledge EPSRC strategic equipment grant EP/W006502/1. R.A.W.D acknowledges EPSRC grant EP/V049925/1. A.A.K acknowledges the grant of EU Underwrite - Innovate UK EXANST PSP764 and the Leverhulme Trust grant No. RPG 2022-142. M.C and A.A.K acknowledge Prof. Guang Feng of Huazhong University of Science and Technology for useful discussions.
Contributions
B. R. designed and directed the project; B.R., A.A.K, R.A.W.D and A.K. provided the overall supervision; J.Y. perfomed the ion transport measurements with help from A.I.; R.K.G., J.Y., A.I., analysed the ion transport measurements. L.A.M. led the 2D channels fabrication with help of H.J. A.K, K.V.S, R.Q and R.S.; C.M. and A.A.K. performed all the MD simulations; R.K.G and B.R. wrote the manuscript with J.Y., C.M. and A.A.K. All the authors contributed to the discussions
Data availability
The data that support the findings of this study are available from the authors upon reasonable request.
Conflict of interest
The authors declare no conflict of interest.
References
- [1]Fedorov, M.V., and Kornyshev, A.A. (2014). Ionic Liquids at Electrified Interfaces. Chem. Rev. 114, 2978-3036. 10.1021/cr400374x.
- [2]Hayes, R., Warr, G.G., and Atkin, R. (2015). Structure and Nanostructure in Ionic Liquids. Chem. Rev. 115, 6357-6426. 10.1021/cr500411q.
- [3]Feng, G., Chen, M., Bi, S., Goodwin, Z.A.H., Postnikov, E.B., Brilliantov, N., Urbach, M., and Kornyshev, A.A. (2019). Free and Bound States of Ions in Ionic Liquids, Conductivity, and Underscreening Paradox. Phys. Rev. X 9, 021024. 10.1103/PhysRevX.9.021024.DOI
- [4]Marion, S., Davis, S.J., Wu, Z.-Q., and Radenovic, A. (2020). Nanocapillary confinement of imidazolium based ionic liquids. Nanoscale 12, 8867-8874. 10.1039/D0NR01164A.
- [5]Lahrar, E.H., Belhboub, A., Simon, P., and Merlet, C. (2020). Ionic Liquids under Confinement: From Systematic Variations of the Ion and Pore Sizes toward an Understanding of the Structure and Dynamics in Complex Porous Carbons. ACS Appl. Mater. Interfaces 12, 1789-1798. 10.1021/acsami.9b16740.
- [6]Zhang, Z., Li, C., Chandresh, A., and Heinke, L. (2022). Conductivity measurement of ionic liquids confined in the nanopores of metal–organic frameworks: a case study for [BMIM][TFSI] in HKUST-1. Ionics 28, 487-494. 10.1007/s11581-021-04249-w.DOI
- [7]Filippov, A., Rudakova, M., Archipov, V.P., and Shah, F.U. (2024). Nanoconfinement effects on the dynamics of an ionic liquid-based electrolyte probed by multinuclear NMR. Soft Matter 20, 8436-8445. 10.1039/D4SM01058B.DOI
- [8]Chmiola, J., Yushin, G., Gogotsi, Y., Portet, C., Simon, P., and Taberna, P.L. (2006). Anomalous Increase in Carbon Capacitance at Pore Sizes Less Than 1 Nanometer. Science 313, 1760-1763. doi:10.1126/science.1132195.DOI
- [9]Largeot, C., Portet, C., Chmiola, J., Taberna, P.-L., Gogotsi, Y., and Simon, P. (2008). Relation between the Ion Size and Pore Size for an Electric Double-Layer Capacitor. J. Am. Chem. Soc. 130, 2730-2731. 10.1021/ja7106178.DOI
- [10]Futamura, R., Iiyama, T., Takasaki, Y., Gogotsi, Y., Biggs, M.J., Salanne, M., Ségalini, J., Simon, P., and Kaneko, K. (2017). Partial breaking of the Coulombic ordering of ionic liquids confined in carbon nanopores. Nat. Mater. 16, 1225-1232. 10.1038/nmat4974.DOI
- [11]Kondrat, S., Feng, G., Bresme, F., Urbahk, M., and Kornyshev, A.A. (2023). Theory and Simulations of Ionic Liquids in Nanoconfinement. Chem. Rev. 123, 6668-6715. 10.1021/acs.chemrev.2c00728.
- [12]Davenport, M., Rodriguez, A., Shea, K.J., and Siwy, Z.S. (2009). Squeezing Ionic Liquids through Nanopores. Nano Lett. 9, 2125-2128. 10.1021/nl900630z.DOI
- [13]Tasserit, C., Koutsoubas, A., Lairez, D., Zalcer, G., and Clochard, M.C. (2010). Pink Noise of Ionic Conductance through Single Artificial Nanopores Revisited. Phys. Rev. Lett. 105, 260602. 10.1103/PhysRevLett.105.260602.
- [14]Jacob, C., Sangoro, J.R., Papadopoulos, P., Schubert, T., Naumov, S., Valiullin, R., Kärger, J., and Kremer, F. (2010). Charge transport and diffusion of ionic liquids in nanoporous silica membranes. Phys. Chem. Chem. Phys. 12, 13798-13803. 10.1039/C004546B.
- [15]Jacob, C., Sangoro, J.R., Kipnusu, W.K., Valiullin, R., Kärger, J., and Kremer, F. (2012). Enhanced charge transport in nano-confined ionic liquids. Soft Matter 8, 289-293. 10.1039/C1SM06581E.
- [16]Dong, Y., Steinhart, M., Butt, H.-J., and Floudas, G. (2023). Conductivity of Ionic Liquids in the Bulk and during Infiltration in Nanopores. J. Phys. Chem. B 127, 6958-6968. 10.1021/acs.jpcb.3c01216.DOI
- [17]Chathoth, S.M., Mamontov, E., Dai, S., Wang, X., Fulvio, P.F., and Wesolowski, D.J. (2012). Fast diffusion in a room temperature ionic liquid confined in mesoporous carbon. Europhys. Lett. 97, 66004. 10.1209/0295-5075/97/66004.
- [18]Chathoth, S.M., Mamontov, E., Fulvio, P.F., Wang, X., Baker, G.A., Dai, S., and Wesolowski, D.J. (2013). An unusual slowdown of fast diffusion in a room temperature ionic liquid confined in mesoporous carbon. Europhys. Lett. 102, 16004. 10.1209/0295-5075/102/16004.
- [19]Radha, B., Esfandiar, A., Wang, F.C., Rooney, A.P., Gopinadhan, K., Keerthi, A., Mishchenko, A., Janardanan, A., Blake, P., Fumagalli, L., et al. (2016). Molecular transport through capillaries made with atomic-scale precision. Nature 538, 222-225. 10.1038/nature19363.DOI
- [20]Bhardwaj, A., Surmani Martins, M.V., You, Y., Sajja, R., Rimmer, M., Goutham, S., Qi, R., Abbas Dar, S., Radha, B., and Keerthi, A. (2024). Fabrication of angstrom-scale two-dimensional channels for mass transport. Nat. Protoc. 19, 240-280. 10.1038/s41596-023-00911-x.
- [21]Esfandiar, A., Radha, B., Wang, F.C., Yang, Q., Hu, S., Garaj, S., Nair, R.R., Geim, A.K., and Gopinadhan, K. (2017). Size effect in ion transport through angstrom-scale slits. Science 358, 511-513. doi:10.1126/science.aan5275.DOI
- [22]Goutham, S., Keerthi, A., Ismail, A., Bhardwaj, A., Jalali, H., You, Y., Li, Y., Hassani, N., Peng, H., Martins, M.V.S., et al. (2023). Beyond steric selectivity of ions using ångström-scale capillaries. Nat. Nanotechnol. 18, 596-601. 10.1038/s41565-023-01337-y.
- [23]Robin, P., Emmerich, T., Ismail, A., Niguès, A., You, Y., Nam, G.-H., Keerthi, A., Siria, A., Geim, A.K., Radha, B., and Bocquet, L. (2023). Long-term memory and synapse-like dynamics in two-dimensional nanofluidic channels. Science 379, 161-167. doi:10.1126/science.adc9931.DOI
- [24]Yang, W., Radha, B., Choudhary, A., You, Y., Mettela, G., Geim, A.K., Aksimentiev, A., Keerthi, A., and Dekker, C. (2021). Translocation of DNA through Ultrathin Nanoslits. Adv. Mater. 33, 2007682. https://doi.org/10.1002/adma.202007682.
- [25]Ronceray, N., You, Y., Glushkov, E., Lihter, M., Rehl, B., Chen, T.-H., Nam, G.-H., Borza, F., Watanabe, K., Taniguchi, T., et al. (2023). Liquid-activated quantum emission from pristine hexagonal boron nitride for nanofluidic sensing. Nat. Mater. 22, 1236-1242. 10.1038/s41563-023-01658-2.DOI
- [26]Yang, J., Papaderakis, A.A., Roh, J.S., Keerthi, A., Adams, R.W., Bissett, M.A., Radha, B., and Dryfe, R.A.W. (2024). Measuring the Capacitance of Carbon in Ionic Liquids: From Graphite to Graphene. J. Phys. Chem. C 128, 3674-3684. 10.1021/acs.jpcc.3c08269.DOI
- [27]Goutham, S., Gogoi, R.K., Jyothilal, H., Nam, G.-H., Ismail, A., Pandey, S.V., Keerthi, A., and Radha, B. (2025). Electric Field Mediated Unclogging of Angstrom-Scale Channels. Small Methods 9, 2400961. https://doi.org/10.1002/smtd.202400961.
- [28]Mukhopadhyay, T.K., and Datta, A. (2017). Deciphering the Role of Solvents in the Liquid Phase Exfoliation of Hexagonal Boron Nitride: A Molecular Dynamics Simulation Study. J. Phys. Chem. C 121, 811-822. 10.1021/acs.jpcc.6b09446.
- [29]Canongia Lopes, J.N., Pádua, A.A.H., and Shimizu, K. (2008). Molecular Force Field for Ionic Liquids IV: Trialkylimidazolium and Alkoxycarbonyl-Imidazolium Cations; Alkylsulfonate and Alkylsulfate Anions. J. Phys. Chem. B 112, 5039-5046. 10.1021/jp800281e.DOI
- [30]Hess, B., Kutzner, C., van der Spoel, D., and Lindahl, E. (2008). GROMACS 4: Algorithms for Highly Efficient, Load-Balanced, and Scalable Molecular Simulation. J. Chem. Theory Comput. 4, 435-447. 10.1021/ct700301q.
- [31]Darden, T., York, D., and Pedersen, L. (1993). Particle mesh Ewald: An N·log(N) method for Ewald sums in large systems. J. Chem. Phys. 98, 10089-10092. 10.1063/1.464397.
- [32]Essmann, U., Perera, L., Berkowitz, M.L., Darden, T., Lee, H., and Pedersen, L.G. (1995). A smooth particle mesh Ewald method. J. Chem. Phys. 103, 8577-8593. 10.1063/1.470117.
- [33]Elbourne, A., McDonald, S., Voichovsky, K., Endres, F., Warr, G.G., and Atkin, R. (2015). Nanostructure of the Ionic Liquid–Graphite Stern Layer. ACS Nano 9, 7608-7620. 10.1021/acsnano.5b02921.
- [34]Widegren, J.A., Sauer, E.M., Marsh, K.N., and Magee, J.W. (2005). Electrolytic conductivity of four imidazolium-based room-temperature ionic liquids and the effect of a water impurity. J. Chem. Thermodyn. 37, 569-575. https://doi.org/10.1016/j.jct.2005.04.009.
- [35]Widegren, J.A., Laesecke, A., and Magee, J.W. (2005). The effect of dissolved water on the viscosities of hydrophobic room-temperature ionic liquids. Chem. Commun., 1610-1612. 10.1039/B417348A.
- [36]Gopinadhan, K., Hu, S., Esfandiar, A., Lozada-Hidalgo, M., Wang, F.C., Yang, Q., Tyurnina, A.V., Keerthi, A., Radha, B., and Geim, A.K. (2019). Complete steric exclusion of ions and proton transport through confined monolayer water. Science 363, 145-148. doi:10.1126/science.aau6771.DOI
- [37]Mo, T., Bi, S., Zhang, Y., Presser, V., Wang, X., Gogotsi, Y., and Feng, G. (2020). Ion Structure Transition Enhances Charging Dynamics in Subnanometer Pores. ACS Nano 14, 2395-2403. 10.1021/acsnano.9b09648.
- [38]Bożym, D.J., Uralcan, B., Limmer, D.T., Pope, M.A., Szamreta, N.J., Debenedetti, P.G., and Aksay, I.A. (2015). Anomalous Capacitance Maximum of the Glassy Carbon–Ionic Liquid Interface through Dilution with Organic Solvents. J. Phys. Chem. Lett. 6, 2644-2648. 10.1021/acs.jpclett.5b00899.
- [39]Pivnic, K., Bresme, F., Kornyshev, A.A., and Urbahk, M. (2020). Electrotunable Friction in Diluted Room Temperature Ionic Liquids: Implications for Nanotribology. ACS Appl. Nano Mater. 3, 10708-10719. 10.1021/acsanm.0c01946.
- [40]Jitvisate, M., and Seddon, J.R.T. (2018). Direct Measurement of the Differential Capacitance of Solvent-Free and Dilute Ionic Liquids. J. Phys. Chem. Lett. 9, 126-131. 10.1021/acs.jpclett.7b02946.
- [41]Mata, R.A., and Costa Cabral, B.J. (2004). Structural, energetic, and electronic properties of (CH3CN)2–8 clusters by density functional theory. J. Mol. Struct. THEOCHEM 673, 155-164. https://doi.org/10.1016/j.theochem.2003.12.011.
- [42]Jadżyn, J., and Świergiel, J. (2011). On Intermolecular Dipolar Coupling in Two Strongly Polar Liquids: Dimethyl Sulfoxide and Acetonitrile. J. Phys. Chem. B 115, 6623-6628. 10.1021/jp2013336.
- [43]Marekha, B.A., Kalugin, O.N., Bria, M., and Idrissi, A. (2015). Probing structural patterns of ion association and solvation in mixtures of imidazolium ionic liquids with acetonitrile by means of relative 1H and 13C NMR chemical shifts. Phys. Chem. Chem. Phys. 17, 23183-23194. 10.1039/C5CP02748A.
- [44]Rotnicki, K., Sterczyńska, A., Fojud, Z., Jażdżewska, M., Beskrovnyi, A., Waliszewski, J., and Śliwińska-Bartkowiak, M. (2020). Phase transitions, molecular dynamics and structural properties of 1-Ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide ionic liquid. J. Mol. Liq. 313, 113535. https://doi.org/10.1016/j.molliq.2020.113535.