Predicting local electric field in Alx_xGa1−x_{1-x}N p-i-n photodiodes using exciton Franz-Keldysh photocurrent spectroscopy

Abstract

In AlGaN p-i-n photodiodes, reverse bias redshifts and broadens the sub-bandgap photocurrent responsivity through the eXciton Franz-Keldysh (XFK) effect, and this spectral line shape encodes the local electric field inside the device. Fitting the photocurrent spectra of two such photodiodes, with 5% and 40% Al, to an XFK absorption model at each bias yields the local voltage, VlV_l, a single parameter that sets the line shape and uniquely determines the electric-field profile inside the device. In both devices, VlV_l varies linearly with the applied bias (R2=0.994R^2 = 0.994 and 0.9980.998) but changes far more slowly than the bias itself, revealing a strong local reduction of the electric field that points to non-uniform electrostatics. The slopes show that only 12.4% of the applied bias in the 5% Al device, and 45.8% in the 40% Al device, drops across the junction at the probed location. Extrapolated to zero bias, VlV_l gives built-in voltages of 3.39 and 4.29 V, within 0.02 V of the 3.41 and 4.28 V obtained from technology computer-aided design (TCAD) simulation, which validates the extracted local voltages at equilibrium. These results extend sub-bandgap photocurrent spectroscopy to AlGaN devices as an optical probe of local electrostatics, relevant to ultraviolet photodetectors and high-voltage electronics.

Alx_xGa1−x_{1-x}N is a direct-bandgap III-nitride alloy whose bandgap can be tuned from 3.4 eV (GaN) to 6.2 eV (AlN) through the Al content xx, placing the absorption edge anywhere from the near to the deep ultraviolet (UV).[1, 2, 3] For x≳0.4x \gtrsim0.4 the edge falls below the 280-nm solar-blind cutoff,[3] enabling intrinsically solar-blind detection without the bulky optical filters needed by Si-based detectors.[4, 5] AlGaN has thus yielded solar-blind photodiodes,[6, 7] including low-noise pp–ii–nn devices with very low dark current,[4] and avalanche photodiodes (APDs) with high gain,[3, 8] exceeding 10510^5 in Al0.05_{0.05}Ga0.95_{0.95}N APDs on GaN substrates.[5] Because the critical electric field rises steeply with bandgap, AlGaN is also an ultrawide-bandgap platform for high-voltage electronics.[9] In both device classes, the internal field governs carrier collection, gain, dark current, and breakdown.

Yet the field inside an operating device is rarely measured. Designers instead rely on simulations that usually assume laterally uniform, one-dimensional (1D) electrostatics.[10] In vertical GaN pp–nn diodes, the field peaks at the outer mesa edge, where destructive breakdown usually starts, so edge terminations such as guard rings are needed to relieve field crowding.[11] In AlGaN APDs, dislocations and dry-etched sidewall features disturb the field distribution and trigger premature microplasma breakdown.[3, 5] In solar-blind AlGaN photodiodes, two-dimensional simulations indicate possible field crowding beneath the pp contact, and the resistive Al-rich pp-type layer makes the transient response depend on the illumination position.[4] Electroreflectance and photoreflectance spectroscopy quantify built-in fields in nitride layers and heterostructures,[12, 13] but their oscillations decay at high fields and their analysis assumes a homogeneous field.[10] Electric-field-induced second-harmonic generation maps fields in GaN devices with submicrometer resolution and shows that devices with similar terminal characteristics can have very different internal fields, with crowding wherever the edge-termination charge is uneven.[14, 15] Directly mapping the field inside an active device region thus remains challenging,[14] and a local field probe for operating AlGaN devices is needed.

Photocurrent spectroscopy offers such a probe through the Franz–Keldysh (FK) effect. An electric field tilts the band edges, so the electron and hole wave functions overlap inside the gap and photons below the bandgap are absorbed, and the absorption edge redshifts and broadens as the field grows.[16, 17, 18] In wide-bandgap semiconductors, the electron–hole Coulomb interaction strongly enhances this sub-bandgap absorption and changes its field dependence. This eXciton Franz–Keldysh (XFK) effect[19, 20, 21, 22] has been observed in the electroabsorption of GaN.[23] Because the sub-bandgap absorption follows the local field, the bias-dependent responsivity of a reverse-biased junction encodes the field where the light is absorbed. FK photocurrent has been modeled in GaN pp–nn diodes[24] and β\beta-Ga2_2O3_3 Schottky diodes[25] under high reverse bias and used to extract built-in fields in an AlGaN/GaN heterostructure,[26] and Li et al. attributed the bias-induced redshift of an Al0.4_{0.4}Ga0.6_{0.6}N photodiode to the FK effect, assuming a uniform field.[4] Myers and co-workers developed the XFK effect into a quantitative local probe.[10, 27, 28] Verma et al. showed that the XFK line shape of the responsivity of a GaN pp–nn diode is fit with a single parameter, the local voltage VlV_l, which fixes the field profile at the illuminated position, and found a large local field reduction that they attributed to electrostatic non-uniformity.[10] Adnan et al. then identified the onset of dielectric breakdown in β\beta-Ga2_2O3_3 Schottky diodes, near 6 MV/cm, from the saturation of the XFK redshift,[27] and Verma et al. resolved the anisotropic excitonic photocurrent of β\beta-Ga2_2O3_3.[28]

Here, we extend XFK photocurrent spectroscopy to AlGaN and establish an XFK-based model of the internal electric-field profile of AlGaN pp–ii–nn photodiodes. Two changes are needed. First, the bandgap, exciton binding energy, Bohr radius, and permittivity in the XFK model depend on Al content. Second, practical AlGaN photodiodes are pp–ii–nn structures with an unintentionally doped (UID) absorber, so the field profile is trapezoidal rather than the triangular profile of an abrupt pp–nn junction. We apply the model to the published responsivity spectra of two previously fabricated photodiodes, with 5% and 40% Al, validate it against technology computer-aided design (TCAD) simulation at zero bias, and show that the field at the probed location under reverse bias is far smaller than the 1D simulation predicts. To our knowledge, this is the first use of the XFK line shape to determine local fields in AlGaN devices. Because the method needs only the spectral responsivity, which is routinely measured for UV photodetectors, it can be applied across the AlGaN composition range.

The sub-bandgap photocurrent spectra of the two AlGaN pp–ii–nn photodiodes shown in Figure 1 were reported by Kim et al.⁵ and Sood et al.²⁹ (Device 1) and by Li et al.⁴,⁷ (Device 2) Here they are reanalyzed with the XFK model generalized to the pp–ii–nn field profile, from which the local voltage is obtained at each bias. Device 1 [Figure 1(a)] is a top-illuminated Al0.05_{0.05}Ga0.95_{0.95}N pp–ii–nn avalanche photodiode grown by metalorganic chemical vapor deposition (MOCVD) on a free-standing nn-GaN substrate. Its 300-nm UID absorber lies between a 100-nm pp-Al0.05_{0.05}Ga0.95_{0.95}N:Mg layer (hole concentration ∼5×1017 cm−3\sim5 \times10^{17}\ \mathrm{cm}^{-3}), capped by 20 nm of p+p^{+}-Al0.05_{0.05}Ga0.95_{0.95}N ([Mg] ∼1×1020 cm−3\sim1 \times10^{20}\ \mathrm{cm}^{-3}), and a 150-nm nn-Al0.02_{0.02}Ga0.98_{0.98}N:Si layer (∼4×1018 cm−3\sim4 \times10^{18}\ \mathrm{cm}^{-3}). The mesas were formed by inductively coupled plasma etching, with Ni/Ag/Ni/Au anodes and Ti/Al/Ti/Au cathodes. Device 2 [Figure 1(c)] is a back-illuminated Al0.4_{0.4}Ga0.6_{0.6}N/Al0.6_{0.6}Ga0.4_{0.4}N solar-blind pp–ii–nn photodiode grown by low-pressure MOCVD on double-polished sapphire. Its 150-nm UID absorber lies between a 200-nm nn-Al0.4_{0.4}Ga0.6_{0.6}N layer and a 200-nm pp-Al0.4_{0.4}Ga0.6_{0.6}N:Mg layer. The pp layer is topped by a 10-nm compositionally graded layer of the kind used for polarization-induced hole doping³⁰ and a 10-nm p+p^{+}-GaN contact layer, and a 700-nm Al0.6_{0.6}Ga0.4_{0.4}N layer below the nn side serves as the optical window. Its mesas were defined by reactive ion etching, with Ni/Au anodes and Ti/Al cathodes. The zero-bias band diagrams [Figure 1(b) and Figure 1(d)] were computed with Silvaco ATLAS³¹ and give built-in voltages Vbi=3.41V_{\mathrm{bi}} = 3.41 V (Device 1) and 4.28 V (Device 2).

Figure 1. Device structures and equilibrium band diagrams. (a) Device 1: p+p^{+}-Al0.05_{0.05}Ga0.95_{0.95}N:Mg (20 nm)/pp-Al0.05_{0.05}Ga0.95_{0.95}N:Mg (100 nm)/UID Al0.05_{0.05}Ga0.95_{0.95}N:Mg (300 nm)/nn-Al0.02_{0.02}Ga0.98_{0.98}N:Si (150 nm)/GaN:Si (450 nm) on bulk GaN, with Ni/Ag/Ni/Au anode and Ti/Al/Ti/Au cathode. (b) Simulated zero-bias band diagram of Device 1 (qVbi=3.41qV_{\mathrm{bi}} = 3.41 eV). (c) Device 2: p+p^{+}-GaN:Mg (10 nm)/pp-Alx_{x}Ga1−x_{1-x}N:Mg graded from x=0x = 0 to 0.4 (10 nm)/pp-Al0.4_{0.4}Ga0.6_{0.6}N:Mg (200 nm)/UID Al0.4_{0.4}Ga0.6_{0.6}N:Mg (150 nm)/nn-Al0.4_{0.4}Ga0.6_{0.6}N:Si (200 nm)/Alx_{x}Ga1−x_{1-x}N graded from x=0.4x = 0.4 to 0.6 (36 nm)/Al0.6_{0.6}Ga0.4_{0.4}N (700 nm)/AlN (20 nm) on sapphire, with Ni/Au anode and Ti/Al cathode. (d) Simulated zero-bias band diagram of Device 2 (qVbi=4.28qV_{\mathrm{bi}} = 4.28 eV). ECE_{\mathrm{C}}, EVE_{\mathrm{V}}, and EFE_{\mathrm{F}} are the conduction-band edge, valence-band edge, and Fermi level. The shaded bars mark the pp, ii, and nn regions.

The responsivity spectra R(Eph)R(E_{\mathrm{ph}}) were acquired with a xenon lamp, a monochromator, and lock-in detection. For Device 1, the spectra are those of a 70-µm-diameter mesa under front-side illumination.²⁹,³² For Device 2, a ∼25\sim25-µm beam was focused through the sapphire substrate onto the center of the mesa.⁴ Spectra are analyzed at reverse biases from −10 to −90 V for Device 1 and −10 to −60 V for Device 2, in −10 V steps, together with the zero-bias spectrum of each device.

The pp–nn photocurrent responsivity model¹⁰ is generalized to pp–ii–nn structures:

R=q(1−r)Eph[1−apne−∫−Wpd+Wnα(F(z)) dz],(1)R = \frac{q(1-r)}{E_{\mathrm{ph}}}\left[1-a_{pn}e^{-\int_{-W_p}^{d+W_n}\alpha(F(z))\,\mathrm{d}z}\right], \tag*{(1)}

where qq is the elementary charge, rr the surface reflectance, EphE_{\mathrm{ph}} the photon energy, apn=e−(αpLp+αnLn)a_{pn}=e^{-(\alpha_pL_p+\alpha_nL_n)} the transmittance of the undepleted pp and nn portions of the collection region, of widths LpL_p and LnL_n and field-independent absorption coefficients αp\alpha_p and αn\alpha_n. The layer-by-layer attenuation of the incident flux for the front-illuminated Device 1 and the back-illuminated Device 2 is given in Sec. S1 of the supplementary material.

Here, α(F(z))\alpha(F(z)) is the field-dependent absorption coefficient of the depleted material, whose integral gives the total sub-bandgap attenuation along the optical path. The integral spans the depleted stack: WpW_p on the pp side, the UID layer of thickness dd, and WnW_n on the nn side, with the depletion widths (Wp,Wn)(W_p,W_n) given by Eq. (5).

Because the band-to-band Franz–Keldysh–Aspnes model¹⁸ underestimates absorption within a few exciton binding energies of the gap,¹⁰,¹⁹,²⁰ the XFK absorption coefficient of Merkulov²² was used,

α(F(z))=Cξπ2(δ2ξ2+1),δ=Δ−1−9f22,\alpha(F(z))=\frac{C\xi}{\pi^2(\delta^2\xi^2+1)},\qquad\delta=\Delta-1-\frac{9f^2}{2},
ξ=8fexp⁡[−4Δ3/23f−2Δln⁡(8Δ3/2f)],\xi=\frac{8}{f}\exp\left[-\frac{4\Delta^{3/2}}{3f}-\frac{2}{\sqrt{\Delta}}\ln\left(\frac{8\Delta^{3/2}}{f}\right)\right],
f=q∣F(z)∣aEX,Δ=Eg−EphEX,(2)f=\frac{q|F(z)|a}{E_X},\qquad\Delta=\frac{E_g-E_{\mathrm{ph}}}{E_X}, \tag*{(2)}

where CC is the exciton wave-function normalization coefficient, ff is the field in dimensionless units, aa is the exciton Bohr radius, and EX=EX0+bF(z)2E_X=E_X^0+bF(z)^2 is the Stark-shifted exciton binding energy with polarizability b=9q2a2/(8EX0)b=9q^2a^2/(8E_X^0).³³ Bandgaps of Eg=3.50E_g=3.50 eV and 4.40 eV were used for Device 1 and Device 2, respectively, taken from reported values.⁴,²⁹ The static dielectric constant and the electron and hole masses are interpolated linearly between GaN and AlN.³⁴–³⁷ The exciton Bohr radius a=4πεsℏ2/(μq2)a=4\pi\varepsilon_s\hbar^2/(\mu q^2), with μ\mu the reduced mass,³⁸ and the binding energy EX0=ℏ2/(2μa2)E_X^0=\hbar^2/(2\mu a^2) then follow from the same hydrogenic model, so that aa and EX0E_X^0 are mutually consistent. The coefficient CC is obtained from a two-parameter fit of CC and VlV_l to the highest-bias spectrum of each device and is then held fixed. Table I lists the values, and the supplementary material (Sec. S3) gives the interpolation formulas.

The field enters Eq. (1) through F(z)F(z). We take z=0z=0 at the pp/UID interface and z=dz=d at the UID/nn interface, with dd the UID thickness. Integrating Poisson’s equation from the pp-side depletion edge gives

F(z)=qεs∫−WpzN(z′) dz′,(3)F(z)=\frac{q}{\varepsilon_s}\int_{-W_p}^{z}N(z')\,\mathrm{d}z', \tag*{(3)}

for −Wp≤z≤d+Wn-W_p\le z\le d+W_n, where N(z)N(z) is the net ionized dopant density. The depletion edges follow from charge neutrality and from the requirement that the field integrates to the local voltage.

∫−Wpd+WnN(z) dz=0,∫−Wpd+WnF(z) dz=Vl.(4)\int_{-W_p}^{d+W_n}N(z)\,\mathrm{d}z=0,\qquad \int_{-W_p}^{d+W_n}F(z)\,\mathrm{d}z=V_l. \tag*{(4)}

For uniform acceptor density NAN_A in the pp layer, net density NiN_i in the UID layer, and donor density NDN_D in the nn layer, Eqs. (3) and (4) give

Wp=Q−NAd(ND−Ni)NA(NA+ND),Wn=NAWp−NidND,W_p=\frac{\sqrt{Q}-N_Ad(N_D-N_i)}{N_A(N_A+N_D)},\qquad W_n=\frac{N_AW_p-N_id}{N_D},
Q=NAND[d2(ND−Ni)(NA+Ni)−2εs(NA+ND)Vlq].(5)Q=N_AN_D\left[d^2(N_D-N_i)(N_A+N_i)-\frac{2\varepsilon_s(N_A+N_D)V_l}{q}\right]. \tag*{(5)}

At the doping levels of both devices the UID layer is fully depleted at zero bias, so the field profile is trapezoidal at all biases considered and the integral in Eq. (1) spans the whole UID thickness. Equation (5) further assumes depletion edges inside the pp and nn layers. In practice we solve Eq. (4) numerically for the interface field, which reproduces Eq. (5) and also covers full depletion of the pp or nn layer. In that case the layer is taken as depleted across its whole thickness, with the residual field terminating in the adjacent, more heavily doped layer. The doping densities are listed in Table I. With the doping fixed, VlV_l uniquely sets WpW_p, WnW_n, and F(z)F(z).

Neither the surface reflectance nor the absolute photon flux is known independently, and both vary with position on the device. Both are removed by dividing each spectrum by the zero-bias responsivity at a reference energy ErefE_{\mathrm{ref}} above the gap, where αL≫1\alpha L \gg1 and essentially all light entering the collection region is absorbed. The same zero-bias spectrum also fixes apna_{pn} at every photon energy, since the field-dependent absorption integral is negligible at V=0V = 0 over the fitting range, leaving VlV_l as the only free parameter. This gives the normalized responsivity,[10] which is derived step by step in Sec. S2 of the supplementary material,

RN(Eph)=ErefEph[1−apne−∫α(F(z)) dz].(6)R^{N}(E_{\mathrm{ph}})=\frac{E_{\mathrm{ref}}}{E_{\mathrm{ph}}}\left[1-a_{pn}e^{-\int\alpha(F(z))\,\mathrm{d}z}\right]. \tag*{(6)}

Because the field-dependent absorption is taken as negligible at zero bias, the zero-bias spectrum then fixes

apn(Eph)=1−EphErefRN(Eph;V=0).(7)a_{pn}(E_{\mathrm{ph}})=1-\frac{E_{\mathrm{ph}}}{E_{\mathrm{ref}}}R^{N}(E_{\mathrm{ph}};V=0). \tag*{(7)}

We use Eref=4.40E_{\mathrm{ref}} = 4.40 eV for Device 1 and 4.60 eV for Device 2. Figure 2(a) and Figure 2(c) show the responsivity spectra. In both devices, the sub-bandgap absorption edge shifts to lower photon energy and broadens as the reverse bias increases, the signature of field-assisted absorption. With CC fixed, each spectrum is fit to Eq. (6) by minimizing the mean squared difference between the measured and modeled log⁡10RN\log_{10}R^{N}, with VlV_l as the only parameter that controls the line shape. Excellent agreement between the fitted and measured line shapes is obtained across the energy and bias ranges studied, with R2>0.99R^{2}>0.99.

Figure 2. Photocurrent responsivity spectra and extracted local voltages. (a) Responsivity RR of Device 1 versus photon energy EphE_{\mathrm{ph}} for reverse biases VR=−10V_{\mathrm{R}}=-10 to −90-90 V in −10-10 V steps (symbols), with XFK fits (dashed lines). (b) Local voltage VlV_{\mathrm{l}} of Device 1 versus applied voltage VappV_{\mathrm{app}}, with the linear fit Vl=0.124Vapp−3.391V_{\mathrm{l}}=0.124V_{\mathrm{app}}-3.391 V (R2=0.994R^{2}=0.994) as a dashed line. (c) Same as (a) for Device 2, VR=−10V_{\mathrm{R}}=-10 to −60-60 V. (d) Same as (b) for Device 2, with Vl=0.458Vapp−4.289V_{\mathrm{l}}=0.458V_{\mathrm{app}}-4.289 V (R2=0.998R^{2}=0.998). Arrows indicate increasing reverse bias.

Figure 2(b) and Figure 2(d) plot the extracted VlV_{\mathrm{l}} against the applied voltage. Both devices follow the empirical relation,[10]

Vl=clVapp−Vbi,(8)V_{\mathrm{l}}=c_{\mathrm{l}}V_{\mathrm{app}}-V_{\mathrm{bi}}, \tag*{(8)}

where clc_{\mathrm{l}} is the fraction of the applied bias that appears across the junction at the probed location. Linear fits give cl=0.124c_{\mathrm{l}}=0.124 and Vbi=3.391V_{\mathrm{bi}}=3.391 V for Device 1 (R2=0.994R^{2}=0.994), and cl=0.458c_{\mathrm{l}}=0.458 and Vbi=4.289V_{\mathrm{bi}}=4.289 V for Device 2 (R2=0.998R^{2}=0.998). The extrapolated built-in voltages agree with the TCAD values of 3.41 and 4.28 V to within 0.019 and 0.009 V, respectively.

Figure 3 compares the field profiles reconstructed from the fitted VlV_{\mathrm{l}} with the 1D TCAD profiles. At zero bias the two coincide in both devices [Figure 3(a) and Figure 3(d)]. The local voltages extrapolated to zero bias with Eq. (8), Vl=−3.39V_{\mathrm{l}}=-3.39 and −4.29-4.29 V, equal −Vbi-V_{\mathrm{bi}}, and the peak fields of about 0.2 and 0.28 MV/cm match TCAD. This agreement in equilibrium, where no external current flows, is consistent with the material parameters used in Eq. (2) and the electrostatic model of Eqs. (3)–(5). The trapezoidal shape of the profiles reflects the residual charge in the UID layer. The field decreases toward the nn side in Device 1 and increases toward it in Device 2, corresponding to net positive and net negative space charge, respectively, in the electrostatic model. In Device 2 the low ionized acceptor density of pp-Al0.4_{0.4}Ga0.6_{0.6}N, a consequence of the deep Mg acceptor level in Al-rich AlGaN,[39] lets the depletion region extend deep into the pp layer.

Figure 3. Vertical electric-field profiles ∣F(z)∣|F(z)| at the probed location. The blue curves are 1D TCAD simulations and the orange curves are profiles reconstructed from the XFK fit through Eqs. (3)–(5). Panels (a)–(c) show Device 1 at VR=0V_R = 0, −40-40, and −90-90 V, and panels (d)–(f) show Device 2 at VR=0V_R = 0, −30-30, and −60-60 V. The TCAD labels give ∣VR∣|V_R| (and VbiV_{\mathrm{bi}} at VR=0V_R = 0). The XFK labels give the fitted total local voltage ∣Vl∣|V_l|, extrapolated with Eq. (8) at VR=0V_R = 0. Dotted lines mark the pp/UID and UID/nn interfaces.

Device 1Device 2
Al fraction (pp and UID layers)0.050.40
UID thickness dd (nm)300150
NAN_{\mathrm{A}}, pp layer (cm−3^{-3})5×10175 \times10^{17}1×10171 \times10^{17}
NiN_{\mathrm{i}}, UID layer (cm−3^{-3})+4×1016+4 \times10^{16}−3.5×1016-3.5 \times10^{16}
NDN_{\mathrm{D}}, nn layer (cm−3^{-3})4×10184 \times10^{18}1×10191 \times10^{19}
EgE_{\mathrm{g}} (eV)3.504.40
εs/ε0\varepsilon_{\mathrm{s}}/\varepsilon_{0}10.319.64
μ/m0\mu/m_{0}0.180.22
aa (nm)3.012.28
EX0E_{\mathrm{X}}^{0} (meV)23.2232.71
CC4.4×1084.4 \times10^{8}5×1085 \times10^{8}
VbiV_{\mathrm{bi}}, TCAD (V)3.414.28
VbiV_{\mathrm{bi}}, XFK intercept (V)3.3914.289
Bias fraction clc_{\mathrm{l}}0.1240.458
R2R^{2} of Eq. (8)0.9940.998
Peak ∣F∣\lvert F\rvert, XFK/TCAD (MV/cm)a^{\mathrm{a}}0.52/2.431.08/2.00

Table 1. Model inputs and extracted parameters.

Under reverse bias the profiles diverge. For Device 1, the local peak field is about 0.36 MV/cm at −40-40 V and 0.52 MV/cm at −90-90 V, compared with 1.25 and 2.43 MV/cm from TCAD [Figure 3(b) and Figure 3(c)]. For Device 2, it is about 0.69 and 1.08 MV/cm at −30-30 and −60-60 V, compared with 1.17 and 2.00 MV/cm [Figure 3(e) and Figure 3(f)]. The 1D simulation therefore overestimates the peak field at the probed location by factors of about 4.7 and 1.9 at the highest biases. The local peak field remains well below the TCAD peak field at every bias (Sec. S4 of the supplementary material). A similar reduction, corresponding to cl≈0.23c_l \approx0.23, can be inferred from the local voltage and built-in voltage reported for a GaN pp–nn diode,[10] where it was attributed to electrostatic non-uniformity associated with the electrode geometry.

Several mechanisms can make cl<1c_l < 1 at a given location. Field fringing near the contact and mesa edges redistributes the applied bias. Lateral current flow through the resistive pp-type AlGaN can drop part of the bias between the contact and the illuminated region. Li et al. attributed the strong position dependence of the pulse response of Device 2 to the high resistivity of its pp-Al0.4_{0.4}Ga0.6_{0.6}N layer.[4] Charge trapped at the surface or mesa sidewall can also screen part of the applied field. Measuring VlV_l as a function of distance from the anode edge, for several contact geometries and temperatures, would separate these contributions. Whatever the mechanism, the result has practical consequences. In photodetectors, the XFK tail sets a bias-dependent long-wavelength cutoff, so the field actually present in the absorber determines the out-of-band rejection. In high-voltage devices, local fields that differ several-fold from 1D predictions mean that breakdown hot spots cannot be located from simulation alone.

In summary, we extended exciton Franz–Keldysh photocurrent spectroscopy from GaN pp–nn diodes to two previously reported AlGaN pp–ii–nn photodiodes with 5% and 40% Al. A closed-form pp–ii–nn electrostatic model lets each respective spectrum be fit with the local voltage as the only parameter that controls the line shape. The extracted local voltage is linear in bias, its zero-bias intercept reproduces the built-in voltage within 0.02 V, and at zero bias the reconstructed field matches TCAD. Under reverse bias, only 12.4% and 45.8% of the applied bias acts at the probed location, and at the highest biases the local peak field is about 2–5 times below the 1D estimate. Sub-bandgap photocurrent spectroscopy therefore offers a contactless way to map electric fields in AlGaN devices and to test electrostatic designs.

Supplementary Material

See the supplementary material for the layer-by-layer photon-flux chains of both devices, the step-by-step normalization of the photocurrent spectra, the exciton binding energy and Bohr radius as functions of Al content, and the relation between the extracted local peak field and the TCAD peak field.

Acknowledgments

The authors gratefully acknowledge Bangladesh University of Engineering and Technology (BUET) for supporting this work.

Author Declarations

Conflict of Interest

The authors have no conflicts to disclose.

Author Contributions

Himel Kundu Utsha: Formal analysis (equal); Methodology (equal); Software (equal); Visualization (equal); Writing – original draft (equal); Writing – review & editing (equal).

Manjur Muntasir: Formal analysis (equal); Methodology (equal); Software (equal); Visualization (equal); Writing – original draft (equal); Writing – review & editing (equal).

Md. Mohsinur Rahman Adnan: Conceptualization (lead); Supervision (lead); Writing – review & editing (equal).

Data Availability

The data that support the findings of this study are available from the corresponding author upon reasonable request.

References

  1. [1]M. Razeghi and A. Rogalski, J. Appl. Phys. 79, 7433 (1996).
  2. [2]E. Monroy, F. Omnès, and F. Calle, Semicond. Sci. Technol. 18, R33 (2003).
  3. [3]Q. Cai, H. You, H. Guo, J. Wang, B. Liu, Z. Xie, D. Chen, H. Lu, Y. Zheng, and R. Zhang, Light Sci. Appl. 10, 94 (2021).
  4. [4]T. Li, D. J. H. Lambert, M. M. Wong, C. J. Collins, B. Yang, A. L. Beck, U. Chowdhury, R. D. Dupuis, and J. C. Campbell, IEEE J. Quantum Electron. 37, 538 (2001).
  5. [5]J. Kim, M.-H. Ji, T. Detchprohm, J.-H. Ryou, R. D. Dupuis, A. K. Sood, and N. K. Dhar, IEEE Photonics Technol. Lett. 27, 642 (2015).
  6. [6]D. Walker, V. Kumar, K. Mi, P. Sandvik, P. Kung, X. H. Zhang, and M. Razeghi, Appl. Phys. Lett. 76, 403 (2000).
  7. [7]D. J. H. Lambert, M. M. Wong, U. Chowdhury, C. Collins, T. Li, H. K. Kwon, B. S. Shelton, T. G. Zhu, J. C. Campbell, and R. D. Dupuis, Appl. Phys. Lett. 77, 1900 (2000).
  8. [8]Z. G. Shao, D. J. Chen, H. Lu, R. Zhang, D. P. Cao, W. J. Luo, Y. D. Zheng, L. Li, and Z. H. Li, IEEE Electron Device Lett. 35, 372 (2014).
  9. [9]Y. I. Tsao et al., Adv. Electron. Mater. 4, 1600501 (2018).
  10. [10]D. Verma, M. M. R. Adnan, M. W. Rahman, S. Rajan, and R. C. Myers, Appl. Phys. Lett. 116, 202102 (2020).
  11. [11]H. Ohta, K. Hayashi, F. Horikiri, M. Yoshino, T. Nakamura, and T. Mishima, Jpn. J. Appl. Phys. 57, 04FG09 (2018).
  12. [12]C. Wetzel, T. Takeuchi, H. Amano, and I. Akasaki, J. Appl. Phys. 85, 3786 (1999).
  13. [13]L. Janicki, M. S. Mohajerani, J. Hartmann, E. Zdanowicz, H.-H. Wehmann, A. Waag, and R. Kudrawiec, Appl. Phys. Lett. 113, 032109 (2018).
  14. [14]Y. Cao, J. W. Pomeroy, M. J. Uren, F. Yang, and M. Kuball, Nat. Electron. 4, 478 (2021).
  15. [15]Y. Cao, J. W. Pomeroy, M. J. Uren, F. Yang, J. Wang, P. Fay, and M. Kuball, Appl. Phys. Lett. 120, 242106 (2022).
  16. [16]W. Franz, Z. Naturforsch. A 13, 484 (1958).
  17. [17]V. V. Keldysh, Sov. Phys. JETP 7, 788 (1958).
  18. [18]D. E. Aspnes, Phys. Rev. 147, 554 (1966).
  19. [19]J. D. Dow and D. Redfield, Phys. Rev. B 1, 3358 (1970).
  20. [20]D. F. Blossey, Phys. Rev. B 2, 3976 (1970).
  21. [21]D. F. Blossey, Phys. Rev. B 3, 1382 (1971).
  22. [22]A. A. Merkulov, Sov. Phys. JETP 39, 1140 (1974). [Zh. Eksp. Teor. Fiz. extbf66, 2314 (1974)].
  23. [23]J. Y. Binet, J. Y. Duboz, E. Rosencher, F. Scholz, and V. Härle, Phys. Rev. B 54, 8116 (1996).
  24. [24]T. Maeda, T. Narita, M. Kanechika, T. Uesugi, T. Kachi, T. Kimoto, M. Horita, and J. Suda, Appl. Phys. Lett. 112, 252104 (2018).
  25. [25]T. Maeda, K. Ema, and K. Sasaki, Appl. Phys. Express 17, 124001 (2024).
  26. [26]Y. Turkulets and I. Shalish, J. Appl. Phys. 124, 075102 (2018).
  27. [27]M. M. R. Adnan, D. Verma, Z. Xia, N. K. Kalarickal, S. Rajan, and R. C. Myers, Phys. Rev. Appl. 16, 034011 (2021).
  28. [28]D. Verma, M. M. R. Adnan, S. Dhara, C. Sturm, S. Rajan, and R. C. Myers, Phys. Rev. Mater. 7, L061601 (2023).
  29. [39]K. B. Nam, M. L. Nakarmi, J. Li, J. Y. Lin, and H. X. Jiang, Appl. Phys. Lett. 83, 878 (2003).

Paper details

vlnc:W_j253w67w
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents