betaFeedback

WorksPhysics and Astronomy

Capping Layer Effects on Sb2S3Sb_{2}S_{3}-based Reconfigurable Photonic Devices

Abstract

Capping layers are essential for protecting phase change materials (PCMs) used in non-volatile photonics technologies. This work demonstrates how (ZnS)0.8−(SiO2)0.2(ZnS)_{0.8}-(SiO_2)_{0.2} caps radically influence the performance of Sb2S3Sb_{2}S_{3} and Ag-doped Sb2S3Sb_{2}S_{3} integrated photonic devices. We found that at least 30 nm of capping material is necessary to protect the material from Sulfur loss. However, adding this cap affects the crystallization temperatures of the two PCMs in different ways. The crystallization temperature of Sb2S3Sb_{2}S_{3} and Ag-doped Sb2S3Sb_{2}S_{3} increased and decreased respectively, which is attributed to interfacial energy differences. Capped and uncapped Ag-doped Sb2S3Sb_{2}S_{3} microring resonator (MRR) devices were fabricated and measured to understand how the cap affects the device performance. Surprisingly, the resonant frequency of the MRR exhibited a larger red-shift upon crystallization for the capped PCMs. This effect was due to the cap increasing the modal overlap with the PCM layer. Caps can, therefore, be used to provide a greater optical phase shift per unit length, thus reducing the overall footprint of these programmable devices. Overall, we conclude that caps on PCMs are not just useful for stabilizing the PCM layer, but can also be used to tune the PCM crystallization temperature and reduce device footprint. Moreover, the capping layer can be exploited to enhance light-matter interactions with the PCM element.

Capping_Layer

Introduction

Programmable photonic devices are essential for realizing many next-generation photonic integrated circuit (PIC) technologies. Current PIC technologies are mostly application-specific and consist of repetitive simple circuitry designs [1, 2]. Moreover, developing them involves a slow and costly iterative process, which hinders photonic innovations [1]. Having programmable PIC components allows sophisticated circuit designs to be developed efficiently. In the short term, more advanced and complex circuitry can be developed, which will inevitably generate a wider range of novel photonic devices and enhance application-specific systems like optical networks [3, 4] and sensors [5, 6]. In effect, programmable PIC chips will be analogous to electronic field-programmable gate arrays (FPGAs) [7]. We anticipate photonic FPGAs to become accessible to mainstream users, offering an inexpensive and efficient way to design and prototype new photonic systems.

Controlling amplitude and phase of light are important features in a programmable PIC. To this end, various tuning mechanisms such as thermo-optic [8, 9, 10], electro-optic [11, 12], and free-carrier dispersion effects [13, 14, 15] have been explored. However, these mechanisms are volatile, which requires a constant power supply to hold an optical state. In addition, the refractive index changes are small and implementing them requires large footprint [16]. With the lack of non-volatile tuning devices in current PIC platforms, photonic systems can become inefficient and have limited device scalability. For instance, in application-specific Optical Neural Networks, each electro-optic/thermo-optic tuned weighting component requires a 10 mW power supply to sustain an optical state [17]. Moreover, for photonic FPGAs to have comparable performance to their electrical counterparts, the programmable logic unit must also consist of non-volatile memory. Hence developing non-volatile programmable photonic devices is one of the key design criteria for next-generation PIC technologies.

Phase change materials (PCMs) have drawn interest from the photonics community in recent years due to their non-volatile switching characteristics [18, 19]. Incorporating PCMs into conventional photonic structures can bring us a step closer to programmable PIC technologies. PCMs can be easily integrated with PIC devices by depositing tens of nanometer thick PCM films above the waveguide using standard complementary metal-oxide-semiconductor (CMOS) processes [16]. The mode index of the waveguide, neffn_{eff}, can then be effectively tuned when the PCM is switched between the amorphous and crystalline structural states [20, 21, 22].

In recent years, PIC devices that are tuned by PCMs have been developed and extensively studied. These studies ranged from the design and fabrication of conventional photonic structures that incorporate conventional data storage PCMs [20, 22, 23, 24, 25] to developing sophisticated PCM switching operations with on-chip heaters [26, 27, 28, 29]. The plethora of advantages offered by PCMs over other tuning mechanisms are clear, however, the common data storage PCMs are lossy at visible and near-infrared frequencies. Recently, therefore, state-of-the-art PCM-tuned photonic devices using low-loss PCMs, like Sb2_2S3_3 and Sb2_2Se3_3, have been proposed as better PCM alternatives to the data storage PCM, Ge2_2Sb2_2Te5_5 [30, 31]. The introduction of wide band gap PCMs has led to the rapid development of low-loss PCM based photonic devices [26, 27, 32, 33, 34, 35] [36].

As low-loss PCMs are becoming popular choices for developing tunable photonic devices, further understanding of their properties and limitations is required for better device integration. One important area of study involves the capping layer, which is needed to protect low-loss PCMs from the atmosphere. Whilst the influence of capping layers on well-known PCMs like Ag4_4In3_3Sb67_{67}Te26_{26} [37] or those on the GeTe-Sb2_2Te3_3 pseudobinary tie-line [38, 39, 40, 41, 42, 43] have been extensively studied, understanding how capping layers influence the material, crystallization and optical properties of low-loss PCMs is still nascent. As such, capping layers were mainly considered for PCM protection purposes, and a wide range of capping layer thicknesses were used to justify material loss prevention during the structural phase transition heating process [26, 31, 32, 35, 44, 45]. This ranged from 10 nm [26, 32] to the hundreds of nanometers [31, 45]. Inadequate capping thickness can affect photonic device performance [32]. Moreover, capping layers can affect the PCM crystallization temperature [37, 38, 39, 40, 41, 42] and neffn_{eff} of the photonic device. These changes will influence the PCM switching parameters and the photonic device design.

Herein, we describe the influence of (ZnS)0.8_{0.8}-(SiO2_2)0.2_{0.2} capping layers on the structural phase transition and optical properties of two related low-loss PCMs, Sb2_2S3_3 and Ag-doped Sb2_2S3_3. These properties can influence the device design and switching operations. We chose to focus on Sb2S3\mathrm{Sb_2S_3} as it exhibits the lowest optical loss amongst the four PCMs, Ge2Sb2Te5\mathrm{Ge_2Sb_2Te_5}, Ge2Sb2Se4Te1\mathrm{Ge_2Sb_2Se_4Te_1}, Sb2Se3\mathrm{Sb_2Se_3} and Sb2S3\mathrm{Sb_2S_3} [36], and consequently it is of particular interest for tuning a wide range of photonic devices [19, 32, 34, 35, 44, 46, 47] [36]. Previously [48, 49], we showed that lightly doping Sb2S3\mathrm{Sb_2S_3} with Ag can lower the crystallization temperature and produce smaller crystallites. The melting point for lightly Ag-doped Sb2S3\mathrm{Sb_2S_3} (below 12.5 %) along the Sb2S3\mathrm{Sb_2S_3} – Ag2S\mathrm{Ag_2S} tie line is also lower [50], suggesting a lower amorphization temperature. For these reasons, we believe that Ag-doped Sb2S3\mathrm{Sb_2S_3} has potential applications in tunable photonic devices. (ZnS)0.8(\mathrm{ZnS})_{0.8}-(SiO2)0.2(\mathrm{SiO_2})_{0.2}, a capping material widely used in phase change rewriteable devices, was chosen to cap the low-loss PCMs. This material can withstand high temperature phase transition processes [31, 40, 41, 51, 52] and has negligible optical losses in the visible and near infrared spectrum [53].

The capping layer should not be neglected when designing and developing low-loss PCM devices. Through thermogravimetric analysis (TGA) and film thickness measurements, we observed material loss during the heating process. Capping thickness of more than 30 nm were necessary to preserve the material. The crystallization behavior of capped Sb2S3\mathrm{Sb_2S_3} and Ag-doped Sb2S3\mathrm{Sb_2S_3} were also altered. Cap-PCM interface stumped crystal growth and altered nucleation behavior, which in turn caused the crystallization temperature of Sb2S3\mathrm{Sb_2S_3} and Ag-doped Sb2S3\mathrm{Sb_2S_3} to increase and decrease, respectively. This finding suggests that the device switching parameters of differently capped PCMs will vary. By incorporating Ag-doped Sb2S3\mathrm{Sb_2S_3} into a microring resonator (MRR) device, we found that the capping layer caused a larger red-shift than its uncapped form. Counterintuitively, the optical losses were also greater despite the capping material being transparent to the near infrared light. The larger red-shift and higher optical loss were due to an upward modal shift from the waveguide to the PCM layer. The greater mode confinement on the PCM layer suggests that overall device footprints can be reduced, thus mitigating the large footprint issue reported in low-loss PCM devices due to their smaller Δneff\Delta n_{eff} [31, 32] [36]. Future low-loss PCM device designs should optimize capping layer parameters to enhance both device and system performance.

Methods

PCM TGA Measurements

A thermogravimetric analyzer (TA-Instruments Q-50) was used to conduct TGA on the three PCMs: Sb2S3\mathrm{Sb_2S_3}, (Ag)0.1(\mathrm{Ag})_{0.1}-(Sb2S3)0.9(\mathrm{Sb_2S_3})_{0.9} and Ge2Sb2Te5\mathrm{Ge_2Sb_2Te_5}. PCM dust residuals were collected by scrapping the surface of sputtering targets of 99.99% purity. The dust was then transferred into Al2O3\mathrm{Al_2O_3} crucibles for heating in the thermogravimetric analyzer furnace. The samples were heated to 600 °C with a heating rate of 5 °C/min. To prevent material oxidation, N2\mathrm{N_2} gas was supplied at 40 ml/min to the heating chamber.

Thin Film Deposition and Characterization

Amorphous Sb2S3\mathrm{Sb_2S_3}, Ag2.4Sb42.2S55.4\mathrm{Ag_{2.4}Sb_{42.2}S_{55.4}}, and (ZnS)0.8(\mathrm{ZnS})_{0.8}-(SiO2)0.2(\mathrm{SiO_2})_{0.2} (simplified as ZnS-SiO2_2 in the remaining text) thin films were deposited on SiO2_2 substrates using radio frequency confocal magnetron sputtering system, AJA Orion 5, at room temperature. All films were deposited from commercially available targets of 50.8 mm diameter and 99.99% purity. The Ag2.4Sb42.2S55.4\mathrm{Ag_{2.4}Sb_{42.2}S_{55.4}} (simplified as Ag-SbS in the remaining text) films came from a (Ag)0.1(\mathrm{Ag})_{0.1}-(Sb2S3)0.9(\mathrm{Sb_2S_3})_{0.9} target. We confirmed the thin film composition with scanning electron microscope-energy dispersive X-Ray (SEM-EDX). The EDX results can be found in the main supporting information document, Table S1. All depositions were done at a process pressure of 0.5 Pa, with a base pressure below 6.7×10−56.7 \times10^{-5} Pa. The deposition power for Sb2S3\mathrm{Sb_2S_3}, Ag-SbS, and ZnS-SiO2_2 were 30 W, 40 W and 100 W respectively, and their corresponding deposition rates were 0.69 Å/s, 0.55 Å/s and 0.76 Å/s. The thicknesses of the films were confirmed with profilometry scans using an atomic force microscope (AFM), Asylum Research MFP-3D Origin.

RegionAtomic PercentageAtomic PercentageAtomic Percentage
AgSbS
12.5143.0054.49
23.1242.2554.63
32.2941.4456.27
42.1941.6856.13
52.8541.7955.36
61.0843.3255.60
72.2541.6956.06
82.3242.7354.95
92.7642.0155.23
Average2.3742.2155.41
Standard deviation0.580.660.65

Table S1. EDX measurements of Ag-doped Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3} film

To determine whether the film thickness changes during thermal annealing, step profilometry of films were also conducted with the AFM before and after crystallization. The AFM scan areas were 40 μ\mum by 40 μ\mum wide and contained 512 scanning lines. An example of the AFM scan and film thickness derivation can be found in the main supporting information document, Figure S1. The film thickness is represented as the average thickness across seven different regions of the wafer sample. Sb2_2S3_3 and Ag-SbS films of different capping thicknesses were crystallized at 320 °C and 280 °C respectively in a heating furnace (Linkam T95-HT), with a ramp rate of 5 °C/min and then held at their corresponding crystallization temperatures to ensure complete PCM crystallization. The hold time typically took between 20 to 30 min. To prevent film oxidation, the furnace chamber was purged with Ar gas at 4 sccm during the experiment.

Camera images and histogram plots showing the thickness of a capped Sb2S3 film before and after crystallization

Figure S1. Camera image of the 55 nm-thick cap on Sb2S3\mathrm{Sb_2S_3} sample (a) before and (b) after crystallization. The corresponding (c) amorphous and (d) crystalline thickness values were derived through subtracting the z height values (x-axis) of the two distinct peaks in the histograms.

To compare the crystallization temperature of capped and uncapped PCMs, the samples were also heated in the Linkam furnace at 5 °C/min from room temperature to 350 °C. Similarly, the chamber was purged with Ar gas at 4 sccm. The Linkam microscope furnace was attached to a microscope-camera setup and a spectrometer (Ocean Optics flame). The spectrometer was used to measure the spectrum of a light source (Olympus TH4 200), which was reflected from the thin film samples during heating. The light source wavelength ranged from 500 nm to 700 nm. In this experiment, a microscope image and reflectivity reading of the film were taken for every 1 °C rise in temperature. The spectra and images were then analyzed to find the non-isothermal crystallization behavior of the films.

Ellipsometry of films was conducted using the Accurion EP4 system to extract the material optical constants. Delta, Δ\Delta, and Psi, Ψ\Psi, measurements were taken across the 400 nm to 900 nm spectral band. The data was then fitted with Tauc Lorentz and Lorentz oscillator models [54] [36]. The complex refractive indices (n+ikn+ik) for the 400nm<λ<1600nm400nm < \lambda< 1600nm wavelength range were found by curve-fitting. The nn and kk values from 900 nm to 1600 nm were extrapolated based on the fitted model. These extrapolations were valid as previous ellipsometry measurements at near infrared wavelengths show the fitting models converging asymptotically towards a single nn and kk value after the material bandgap wavelength, which is located in the visible wavelength range [32, 34, 53] [36].

Waveguide Mode Simulations

Finite difference eigenmode (FDE) solver from Lumerical MODE [55] was used to solve Maxwell’s equations for the electromagnetic wave distribution within the PCM-deposited waveguide model. Hence, the neffn_{eff} and loss values of the waveguide structure can be obtained. In the simulation model, optical constants of the low-loss PCMs and cap were obtained from ellipsometry measurements described above, whilst Si3_3N4_4 and SiO2_2 were obtained from literature [56, 57].

Ag-SbS-tuned MRR Device Fabrication and Characterization

MRR devices were fabricated by a Si photonic foundry. The devices were made of Si3_3N4_4 waveguides that were 1.5 μ\mum wide, 200 nm thick, and were embedded in a 2 μ\mum thick SiO2_2 cladding. The top SiO2_2 cladding at the coupling region was removed to expose the waveguide for PCM deposition. The removal process involved immersing the chips in 10 % HF solution for 3 min followed by a deionized water stop bath. Upon removing the top SiO2\mathrm{SiO}_2 cladding, PCM patches (40 μm40\,\mu\mathrm{m} by 40 μm40\,\mu\mathrm{m}) were patterned on the devices using maskless photolithography (Nanyte BEAM). Ag-SbS and the corresponding ZnS-SiO2\mathrm{SiO}_2 capping material were then deposited as described above, followed by a lift-off process which involved sonicating the chips at low power in acetone followed by isopropyl alcohol for 20 s each. The chips were then measured using a tunable laser source-photodetector system (Keysight 8164B), with the laser source being attached to a polarization controller (Thorlabs FPC 562). Afterwards, the Linkam furnace was used to crystallize the PCM patch for the crystalline PCM MRR device measurements. The annealing process for the capped and uncapped samples involved heating the furnace to 280 ∘C280\,^\circ\mathrm{C} and 300 ∘C300\,^\circ\mathrm{C} respectively at 5 ∘C5\,^\circ\mathrm{C}/min and holding it for 30 min. The chamber was also purged with Ar gas at a flowrate of 4 sccm to prevent oxidation of the films.

Results and Discussion

The thermal stabilities of the two low-loss PCMs were found to be lower than Ge2Sb2Te5\mathrm{Ge}_2\mathrm{Sb}_2\mathrm{Te}_5, which highlights the importance of a capping layer in low-loss PCM tuned photonic devices. The TGA measurements in Figure 1 show that the mass loss for Sb2S3\mathrm{Sb}_2\mathrm{S}_3 and (Ag)0.1(\mathrm{Ag})_{0.1}-(Sb2S3)0.9({\mathrm{Sb}_2\mathrm{S}_3})_{0.9} occurred at a lower temperature than Ge2Sb2Te5\mathrm{Ge}_2\mathrm{Sb}_2\mathrm{Te}_5. We noticed an accumulated 4.5% mass loss in Sb2S3\mathrm{Sb}_2\mathrm{S}_3 between 150 ∘C150\,^\circ\mathrm{C} to 270 ∘C270\,^\circ\mathrm{C} followed by rapid mass loss starting from 500 ∘C500\,^\circ\mathrm{C}, which is near the melting point of Sb2S3\mathrm{Sb}_2\mathrm{S}_3 [50]. A similar trend was also reported in previous literature [58]. The accumulated 4.5% mass loss between 150 ∘C150\,^\circ\mathrm{C} to 270 ∘C270\,^\circ\mathrm{C} was due to small amounts of Sulfur evaporating. The rapid mass loss at 500 ∘C500\,^\circ\mathrm{C} was due to Sb2S3\mathrm{Sb}_2\mathrm{S}_3 melting and evaporating.

TGA measurements of Sb₂S₃, 10% Ag-doped Sb₂S₃ and Ge₂Sb₂Te₅

Figure 1. TGA measurements of Sb₂S₃, 10% Ag-doped Sb₂S₃ and Ge₂Sb₂Te₅.

Doping the Sb2S3\mathrm{Sb}_2\mathrm{S}_3 compound with Ag helps to prevent Sulfur loss, thereby improving its thermal stability. We observed that the onset peak mass loss in (Ag)0.1(\mathrm{Ag})_{0.1}-(Sb2S3)0.9(\mathrm{Sb}_2\mathrm{S}_3)_{0.9} shifted from 260 ∘C260\,^\circ\mathrm{C} to the higher temperature of 450 ∘C450\,^\circ\mathrm{C}. Note, the mass loss was also less severe than the pure Sb2S3\mathrm{Sb}_2\mathrm{S}_3 due to the formation of AgSbS2\mathrm{AgSbS}_2, Sb2S3\mathrm{Sb}_2\mathrm{S}_3 and Sb compounds upon doping [50]. The melting point of AgSbS2\mathrm{AgSbS}_2 was found to be 450 ∘C450\,^\circ\mathrm{C}, which accounts for this slight mass loss. Similarly, the compound experienced a rapid mass loss at temperatures close to the melting point of Sb2S3\mathrm{Sb}_2\mathrm{S}_3, indicating liquid Sb2S3\mathrm{Sb}_2\mathrm{S}_3 evaporating. The residual Sb did not contribute to the mass loss because the melting point of Sb is above 600 ∘C600\,^\circ\mathrm{C} [50]. In the remaining studies, the Ag concentration was approximately 2 at.%, which is substantially lower than that of the TGA-studied sputtering target dust. We infer that the thermal stability of the thin film will be better than that of Sb2S3\mathrm{Sb}_2\mathrm{S}_3 but lower than the 10% Ag-doped target dust. Hence, adding a capping layer is important in preserving the Ag-Sb films.

Fine tuning the Ag concentration is important for optimizing Ag-SbS photonic devices. Introducing Ag into Sb2S3\mathrm{Sb}_2\mathrm{S}_3 helps to prevent Sulfur vaporization due to the formation of AgSbS2\mathrm{AgSbS}_2, Sb2S3\mathrm{Sb}_2\mathrm{S}_3 and Sb compounds. Sulfur residuals seem to result in poor thermal stability, which is likely due to its low melting point [50]. Ag seems to help improve the thermal stability of Sb2S3\mathrm{Sb}_2\mathrm{S}_3, however, adding more than 8 at. % Ag will cause AgSbS2\mathrm{AgSbS}_2 and Sb2S3\mathrm{Sb}_2\mathrm{S}_3 compounds to phase separate upon crystallisation [48, 49]. Moreover, Ag nanoparticles will emerge, which will absorb photons strongly and substantially reduce optical intensity through local plasmonic resonances [59, 60]. The 2% Ag-doped films, which were used in this work, do not show any evidence of Ag nanoparticulate precipitation. However, our future works will further optimize the Ag concentration to fine tune the crystallization kinetics and optical properties.

With Sulfur loss occurring within the phase transition temperature range, the optimal capping layer thicknesses for the two low-loss PCMs were investigated. Sb₂S₃ and Ag-SbS films of various capping thickness were measured with AFM before and after crystallization. We associate the change in overall film thickness from the crystallization of PCM films [61, 62]. Note, ZnS-SiO₂ exhibits minimal thickness change upon thermal annealing [63], which was also verified in this work. The corresponding ZnS-SiO₂ thickness change measurements can be found in the main supporting information document, Table S2.

Before Annealing (nm)After Annealing (nm)
39.9±0.339.9 \pm0.340.5±0.340.5 \pm0.3
70.1±0.370.1 \pm0.370.2±0.270.2 \pm0.2

Table S2. Thickness change of ZnS−SiO2\mathrm{ZnS-SiO_2} thin films before and after thermal annealing

We first studied the thermal stability of the Sb₂S₃ and Ag-SbS PCM layers, as shown in Figure 2a, which gives the PCM thickness reduction for different capping layer thicknesses upon thermal annealing. The thicknesses of the PCM materials were chosen as 33 nm for Sb₂S₃ and 30 nm for Ag-SbS because they are similar to the typical PCM thicknesses used to control photonic devices [21, 23, 26, 32, 34, 35] [36].

Capping layer thickness optimization

Figure 2. Capping layer thickness optimization. (a) Thickness reduction of both PCMs upon crystallization for different capping layer thicknesses. (b) Optical microscope images of crystalline PCM films with different cap thickness. (i) to (vi) show the corresponding cap thickness indicated in (a). Images were taken under the same lighting conditions and lens magnification.

The PCM layer thickness shrunk by approximately 10% for the thickest caps. Indeed, the shrinking effect saturates for cap thicknesses of > 30 nm in Figure 2a. Thus, we conclude that at least 30 nm of ZnS-SiO₂ is needed to prevent Sb₂S₃ and Ag-SbS films from material degradation. This 10% thickness change represents an increase in the PCM density upon crystallization, which was also previously reported [61, 62]. A larger thickness change was seen for films with capping layers thinner than 30 nm. This larger change is likely due to cap fracturing, which allows the Sulfur atoms in both PCMs to escape. We observed distinct dark circular rings appearing at the nucleation sites of both uncapped crystalline films as shown in Figure 2b(Figure 2i) and Figure 2b(iv). After depositing a cap on the PCM films, the rings disappeared during annealing as can be seen in Figure 2b(iii) and 2b(vi). These rings could be signs of the PCM degrading. The uncapped Sb₂S₃ experienced a 30% thickness reduction, which was also reported in earlier works of uncapped films [30]. A lower thickness reduction was seen in the uncapped Ag-SbS films as Sulfur vaporization was mitigated. Based on these results, we recommend the use of at least 30 nm ZnS-SiO₂ to protect low-loss PCM-tuned photonic devices. For the rest of this work, the following capped samples were used in our analysis: (1) Sb₂S₃: 55 nm ZnS-SiO₂ cap on 33 nm Sb₂S₃ (2) Ag-SbS: 60 nm ZnS-SiO₂ cap on 30 nm Ag-SbS.

The crystallization behaviors of capped and uncapped low-loss PCM films were investigated. Capped and uncapped Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3} and Ag-SbS were deposited on Si substrates and heated under the same heating conditions (see methods section). We note that in previous works [37, 39, 40, 41], the samples used to investigate the capping layer influence were symmetrical, where the PCM was sandwiched between the capping materials. However, the films in this work were deposited directly on Si substrates because in programmable Si photonic devices, the PCM should ideally be in direct contact with the Si waveguide to maximize its interaction with the optical mode. The crystallization temperature is seen as an abrupt change in reflectivity [41, 64]. The changes in reflectivity of the capped and uncapped PCMs, and their corresponding microscope images at different temperatures during the annealing process, are presented in Figure 3. Whilst the reflectance of chalcogenide PCMs is known to increase upon crystallization [64, 65], we note that adding the ZnS-SiO2_{2} layer caused interference effects and the reflectivity readings of the capped samples decreased upon crystallization, as seen in Figure 3b and Figure 3d. This trend was confirmed by the calculated reflectivity spectrum using the transfer matrix method on OpenFilters [66]. The reflectivity values of the amorphous capped samples were mainly higher than its crystalline form within the light source wavelength range. The simulated reflectivity spectrum of the four samples can be found in the main supporting information document, Figure S2.

Crystallization profiles of capped and uncapped $\mathrm{Sb_2S_3}$ and Ag-SbS

Figure 3. Crystallization profiles of capped and uncapped Sb2S3\mathrm{Sb_2S_3} and Ag-SbS. Reflectivity measurements of (a) uncapped and (b) capped Sb2S3\mathrm{Sb_2S_3}, and (c) uncapped and (d) capped Ag-SbS with respect to temperature. Optical microscope images of (e) Sb2S3\mathrm{Sb_2S_3} and (f) Ag-SbS films during the crystallization process. (i) to (v) show the crystals nucleating and growing as the temperature increases.

Simulated reflectance spectra of uncapped and capped Sb₂S₃ and Ag-SbS films

Figure S2. Simulated reflectance spectrum of the (a) uncapped and (b) capped Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3} films and (c) uncapped and (d) capped Ag-SbS films. Figure insets show the corresponding simulation structure.

The capping layer was found to influence the crystallization behavior of the low-loss PCMs. Based on the reflectivity measurements and microscope images in Figure 3, we make the following observations: (1) The reflectivity curve for capped Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3} in Figure 3b experienced a more gradual change in reflectivity upon crystallization when compared to its uncapped form in Figure 3a. Conversely, the capped Ag-SbS in Figure 3d shows a sharper change in reflectivity when compared to its uncapped form in Figure 3c. (2) The presence of a cap impeded Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3} and Ag-SbS crystal growth as can be seen in Figure 3e(iii) and 3f(iii).

The aforementioned differences in crystallization behavior can be attributed to the PCM-cap interfacial energy affecting the two crystallization mechanisms in a crystallization process: nucleation and growth [39, 41, 67]. Introducing an extra layer of material above the PCM changes the surface energy of the PCM by creating new chemical bonds and also mechanical stresses, which in turn affect the crystallization kinetics. The first observation shows the effect of capping layer on PCM nucleation. In capped Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3}, we observed a more gradual decrease in reflectivity during crystallization than its uncapped form. The gradual decrease was also observed in certain capped materials on Ge1Sb2Te4\mathrm{Ge}_{1}\mathrm{Sb}_{2}\mathrm{Te}_{4} previously, which was caused by a larger surface energy difference between the PCM and cap [41]. Video 1 in the supporting information section shows the crystal matrix expanding outwards over a large temperature range. For the capped Ag-SbS, we observed a sharper decrease in reflectivity than when it is uncapped, which indicates the two mechanisms occurring concurrently. This result suggests that Ag-SbS has a similar interface energy to the ZnS-SiO2_{2} cap. Video 2 in the supporting information section shows the crystal nucleating and growing over a small temperature range. For the second observation, we compared the interfacial energies of PCM-cap with respect to the PCM structural states. The interfacial energy difference of crystalline PCM-amorphous cap is generally higher than amorphous PCM-amorphous cap [39]. As smaller interfacial energy differences are preferred, the cap prevents the Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3} and Ag-SbS crystallites from radially growing, as shown in Figure 3e(iii) and 3f(iii), i.e. crystal growth of the two low-loss PCMs appears to be impeded by the capping layer. However, the films can still nucleate new seeds from which the crystal can grow. Consequentially, we observed a high density of small nuclei in the capped samples. We note that in this work, the capped Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3} and Ag-SbS led to higher and lower crystallization temperatures respectively when compared to their uncapped forms. These results indicate that a cap can alter the PCM crystallization temperature and affect the switching energy used for structural phase transition. This effect is also important because Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3} films are known to crystallize into large birefringent grains [47], but if the correct choice of cap can reduce the size of these grains such that they are substantially smaller than the wavelength of the optical signal, then polycrystalline films with an average isotropic refractive index tensor will result.

To design PCM-tuned photonic devices, we first obtained the complex refractive index of the PCMs and their capping layers from ellipsometry measurements. Figure 4a shows the extracted (n,k)(n, k) values for Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3} and Ag-SbS PCMs in their crystalline and amorphous states, while Figure 4b shows the extracted (n,k)(n, k) for the 70-nm thick ZnS-SiO2_2 capping layer. The refractive index data shown in Figure 4 can be found in the second supporting information document (Supporting Information 2) for the interested readers. Extracting the optical constants of the crystalline PCMs with caps were non-trivial because a double-layer fitting model was required. Therefore, a single-layer ZnS-SiO2_2 film was first measured and then incorporated into the double-layer film model. In this characterization, the single layer ZnS-SiO2_2 film was also annealed at the 320 ℃ crystallization temperature to observe for any changes in the (n,k)(n, k) values during annealing. As shown in Figure 4b, we found the (n,k)(n, k) values to be consistent before and after annealing. Small changes in the refractive index were also observed in thicker films [63], which is consistent with our measurements.

Optical constants of low-loss PCMs and ZnS-SiO2 capping layer

Figure 4. (a) Optical constants of low-loss PCMs Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3} and Ag-SbS in the amorphous and crystalline states, with (i) and (ii) corresponding to the real and imaginary components respectively. Figure inset in (ii) shows the magnified kk data from 1200 nm to 1600 nm wavelength. (b) Optical constants of 70 nm ZnS-SiO2_2 before and after annealing.

Owing to its higher thermal stability and lower crystallization temperature, we integrated Ag-SbS into Si3N4\mathrm{Si}_{3}\mathrm{N}_{4} MRR devices (125 μ\mum radius). The Si3N4\mathrm{Si}_{3}\mathrm{N}_{4} devices were fabricated by a standard Si photonic foundry. As the pristine Si3N4\mathrm{Si}_{3}\mathrm{N}_{4} MRR devices were by default embedded in 2μ\mum SiO2_2 cladding, the cladding was first removed by HF wet etching to expose the waveguide for PCM deposition. However, due to fabrication limitations, the etching rate at the ring-bus coupling region was faster than the other regions, as shown in the Transmission Electron Microscopy (TEM) images in Figure 5a. For this reason, the PCM had to be deposited at the coupling region. Note, the SiO2_2 top cladding outside the coupling region appeared uniform across the long bus waveguide. Hence the device outside the coupling region was protected by the unetched top SiO2_2 cladding, and mode propagation was consistent throughout the device. The TEM cross section images of the etched device taken at different regions can be found in the main supporting information document, Figure S3.

Comparison of uncapped and capped Ag-SbS MRR devices

Figure 5. Comparison of uncapped and capped Ag-SbS MRR devices. (a) Microscope image of a MRR device with Ag-SbS patch deposited in the coupling region. (i) and (ii) show the TEM images of a separate MRR device after HF etching but before the PCM deposition step. Note, the TEM measurement locations correspond to the red boxes on the microscope image. Moreover, the device was coated with a conductive layer to address charging effects. (b) FDE simulation of PCM-deposited coupling regions of the MRR device (c) PCM-tuned MRR device spectra with various capping conditions, shown in (i) to (iv). The schematic illustrations of the devices are not drawn to scale.

MRR device structure schematic and TEM cross-section images

Figure S3. MRR device structure. (a) Top view schematic of the etched device. Labelled regions correspond to the TEM cross section measurements shown in (i) to (v). (b) Pristine device cross section before HF etching.

With the ZnS-SiO2_2 capping layer, the change in optical properties of the PCM layer upon crystallisation was amplified. This loading effect caused the optical mode to shift towards the PCM and experienced more spatial overlap with it. The ZnS-SiO2_2 cap led to a higher neffn_{eff} and, counterintuitively, a higher associated optical loss upon PCM crystallization. Figure 5b shows the Transverse Electric (TE) mode profile of the coupling region deposited with capped and uncapped Ag-SbS, together with their corresponding neffn_{eff} and loss values. There was a higher mode spatial overlap with the PCM layer for the capped case as we see the mode pattern shifting towards the capping layer. This upward modal shift resulted in a higher Δneff\Delta n_{eff} (by ~4x) and losses (by ~2x) as the PCM crystallizes. Note, the crystalline Ag-SbS layer undergoes thickness reduction in a similar manner to that shown in Figure 2b. Based on these findings, the capping layer provides an additional degree of freedom in the design of PCM-tuned photonic devices, whereby its thickness and optical properties can optimize Δneff\Delta n_{eff} and loss to desired values.

Such a large change in neffn_{eff} results in a red-shift in the MRR resonant wavelength. Moreover, the change in both neffn_{eff} and loss led to different coupling conditions between the microring and the single waveguide channel. Coupling condition is dependent on the (1) mode spatial overlap between the two coupled waveguides and (2) amplitude cavity loss in the microring. These two parameters are denoted as the self-coupling coefficient, rr, and cavity loss coefficient in the microring, aa, respectively [68]. Indeed, the former is associated with the coupling strength of the paired waveguide and thus neffn_{eff}, whilst the latter is inversely related to the optical losses. The coupling condition depends on the matching between the coupling strength and cavity roundtrip loss. The system is in under-coupled situation when the roundtrip loss is greater than the amount of light coupled into the cavity, while the system is in over-coupled situation when the coupling strength is greater than the roundtrip loss. The system is in critically-coupled condition when the coupling strength is equal to the cavity loss (r=ar = a), which corresponds to the highest transmission contrast due to optimized interference condition at the output port. With a change in both rr and aa in our devices, the coupling conditions changed from over-coupled to near critically-coupled or under-coupled upon crystallizing, as illustrated in the comparison of amorphous and crystalline transmission spectra of the various MRRs in Figure 5c.

To further study the effects of the cap on resonance shift, we tracked the MRR device azimuthal mode number [68], mm, of the four devices, labelled as (i) to (iv) in Figure 5c. mm represents the integer multiple of wavelengths that fit the cavity length (ring circumference) at resonance wavelength. With an increase (decrease) in neffn_{eff}, the optical pathlength increases (decreases) and longer (shorter) wavelengths are required to interfere constructively during resonance under the same mm multiple. This causes the resonance peak to shift to a longer (shorter) wavelength. The mm value approximations of the devices can be found in the main supporting information document, Table S3 to Table S6. The analysis focused on the resonant peaks near the 1550 nm wavelength.

Parameterλres\lambda_{res} (nm)FSRFSR (nm)ng(exp)n_g^{(exp)}ng(sim)n_g^{(sim)}AAneff(corrected)n_{eff}^{(corrected)}mm
Value1549.7251.7151.7831.776-0.18451.497759

Table S3. mm value approximation of device in Figure 5c(i)

Parameterλres\lambda_{res} (nm)neff(waveguide)n_{eff}^{(waveguide)}neff(PCM)n_{eff}^{(PCM)}mm
Amorphous1550.23751.4971.672763
Crystalline1550.141.4971.715764

Table S6. mm value approximation of device in Figure 5c(iv)

The corresponding mm values of the resonance peak near the 1550 nm wavelength are shown in Figure 5c. The MRR device without the PCM layer corresponds to m=759m = 759. Upon amorphous Ag-SbS deposition, the optical path length increased as a section of the ring has a higher neffn_{eff}. Hence for the same mm multiple, longer wavelengths were required to fit the entire ring circumference. For this reason, the resonance peak of m=759m = 759 shifted to a longer wavelength as shown in Figure 5c(ii). Under the influence of a cap, the optical pathlength further increased and the shift becomes more pronounced. The amorphous mm value near the 1550 nm wavelength increased to m=761m = 761 as shown in Figure 5c(iii). There was also a further increase in mm when the PCM layer thickness increased to 60 nm as shown in Figure 5c(iv). Within the device itself, we also observed a larger resonance peak shift for the capped PCM devices upon crystallization. With a cap on the PCM, the spectrum exhibited close to 2π2\pi phase shift (or close to ~FSR), as shown in Figure 5c(iii) and 5c(iv). By contrast, the uncapped PCM in Figure 5c(ii) showed a phase shift of less than π\pi (or less than 0.5 FSR). We note that the smaller phase shift could also be partly due to material degradation [32]. With a larger phase shift, the capped PCM length can be shortened to reduce the phase shift down to π\pi. A shorter PCM length could mitigate the large footprint limitation reported in low-loss PCM photonic devices [31, 32] [36] as they have a smaller Δneff\Delta n_{\mathrm{eff}} when compared to the data storage PCM alloys along the GeTe−Sb2Te3GeTe-Sb_{2}Te_{3} pseudobinary tie-line.

Next, we analysed the effects of optical loss on the waveguide coupling condition. Our analysis focused on the change in coupling condition within a single device upon structural phase transition as the optical losses across all devices in the amorphous state were negligible. As mentioned, the device coupling condition is determined by the matching between rr and aa [68]. rr is related to the coupling strength of the ring-bus waveguide, which corresponds to the difference between the even and odd modes of the coupled waveguide pair. aa is inversely related to the optical loss. For devices 5c(ii) and 5c(iii), rr was approximated to be consistent in both PCM structural states, whilst for device 5c(iv), rr was higher upon crystallization due to weaker coupling of the waveguide pair. These observations were based on the odd and even mode values from the simulated ring-bus coupling regions. The values can be found in the main supporting information document, Figure S4 and Table S7. Our devices started off by being over-coupled and moved towards critical-coupling or under-coupling conditions. This observation was supported by the fact that crystalline PCMs have a higher optical loss than its amorphous state, which increase the cavity roundtrip loss (or decrease in aa). Given that the coupling strength is relatively unchanged, this leads to the shift of coupling condition from over-coupled (r<ar < a) to under-coupled (r>ar > a) [68]. In Figure 5c(ii), the device moved towards critical coupling when the PCM patch crystallizes as we see a narrower linewidth and sharper resonance contrast. However, in Figure 5c(iii), the device was slightly under-coupled as the loss in the crystalline state is greater by almost two-fold, based on Figure 5b. We observed that with a thicker PCM in Figure 5c(iv), the loss increased further and together with a further increase in rr, the extent of under-coupling becomes larger. The FDE simulation of the capped 60 nm PCM single waveguide and its corresponding loss values can also be found in the main supporting information document, Figure S4.

Deviceneven−noddn_{even} - n_{odd} (amorphous)neven−noddn_{even} - n_{odd} (crystalline)
(ii) uncapped 30 nm Ag-SbS0.0150.016
(iii) 60 nm ZnS-SiO₂ on 30 nm Ag-SbS0.0400.041
(iv) 60 nm ZnS-SiO₂ on 60 nm Ag-SbS0.0850.078

Table S7. neven−noddn_{even} - n_{odd} for the various devices

Simulated mode profiles for amorphous and crystalline tuned MRR devices

Figure S4. Simulated mode profile and corresponding neffn_{\mathrm{eff}} and loss values of (a) 30 nm Ag-SbS, (b) 60 nm ZnS-SiO2_2 on 30 nm Ag-SbS and (c) 60 nm ZnS-SiO2_2 on 60 nm Ag-SbS - tuned MRR devices at 1550 nm wavelength.

Based on the ∼2π\sim2\pi phase shift for the capped PCM with a fixed length, it is possible to reduce the cavity length by half, such that the free spectral range (FSR) doubles [68]. This would correspond to a phase shift of ∼π\sim\pi, thereby changing the detuning from a resonance to an anti-resonance upon Ag-SbS structural phase transition. In addition, this π\pi phase shift maximizes extinction ratio, thereby improving switching resolution when multi-level switching functionalities are introduced [35]. Changing the cavity length will cause the Q-factor to decrease proportionally. To improve the Q-factor of smaller rings, the coupling gap between the ring and bus can be optimized to increase the cavity finesse [68]. Alternatively, the PCM strip length can be proportionally reduced to shorten the optical path length. Future works should investigate how the phase shift varies with various capped PCM strip lengths and cap thicknesses, similar to the experimental works in previous literature [32].

Conclusion

It is essential that capping layers are used to protect both Sb2_2S3_3 and Ag-SbS-tuned photonic devices. Moreover, the impact of capping layers must be considered when designing Sb2_2S3_3-based programmable devices. The caps clearly influence the device switching operations and optical performance. We recommend using at least a 30 nm thick ZnS-SiO2_2 capping layer to protect Sb2_2S3_3 and Ag-SbS. Other caps [27, 32, 44, 45] could be considered, but both the interfacial energy and stress effects on the PCM structural phase transition needs to be carefully studied. Surprisingly, adding the lower refractive index ZnS-SiO2_2 cap to Ag-SbS increased the effect of Ag-SbS on the transmitted light. The effect was due to increased mode confinement in the PCM, leading to a greater change in neffn_{\mathrm{eff}} as the PCM crystallizes. This effect implies that capped couplers and MRRs can be designed to have a smaller footprint than their uncapped counterparts. This work shows that caps on PCMs are not just useful for stabilizing the PCM layer, but can also be used to tune the PCM crystallization temperature and reduce device footprint. Moreover, the capping layer can be exploited to enhance light-matter interactions with the PCM element. Future PCM-tuned photonic device designs should consider optimizing the capping layer to enhance device performance.

Author Contribution

T.Y.T, N. L., L.Y.T.L. and R.E.S. conceived the idea. All experiments and simulations were done by T.Y.T. after consulting: (a) R.E.S. and N. L. for the overall experimental design and execution and (b) A.S.K.T. and D.K.T.N. for top SiO2_2 cladding etching. L.Y.M.T. helped with the MRR device calculation and analysis. Z.R. and C.L. assisted with the waveguide measurements. T.Y.T. wrote the manuscript with all authors contributing to it.

Funding

This work was funded by the Agency for Science, Technology and Research (A*STAR) grants A18A7b0058 and C220415015, and Ministry of Education (MOE) Singapore Tier 2 project (MOE-T2EP50220-0014).

Notes

The authors declare no conflict of interest.

Acknowledgements

We would like to thank Dr Yuyu Jiang (SUTD) for fruitful discussions, Mr Chern Chia Ser (SUTD) for conducting the HF etching training session, and Mr Zhonghua Gu (A*STAR IME) for the TEM measurements.

Supporting Information

The main supporting information document consists of the following: (1) EDX measurement of Ag-SbS film (2) Film thickness measurement method of the PCM crystallization thickness study in Figure 2 (3) Thickness measurements of ZnS-SiO2_2 before and after annealing (4) Simulated reflectivity spectrum of uncapped and capped Sb2_2S3_3 and Ag-SbS (5) TEM cross section images of an etched MRR device (6) MRR azimuthal mode number derivation for devices in fig:5c (7) Coupling condition analysis and FDE simulation of the various MRR devices in fig:5c.

The second supporting information document consists of the raw data in Figure 4.

Videos 1 and 2 show the crystallization process of capped Sb2_2S3_3 and Ag-SbS respectively.

Capping Layer Effects on Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3}-based Reconfigurable Photonic Devices: Supporting Information

Ting Yu Teo; Nanxi Li; Landobasa Y. M. Tobing; Amy S. K. Tong; Doris K. T. Ng; Zhihao Ren; Chengkuo Lee; Lennon Y. T. Lee; Robert Edward Simpson

Supporting_Information

Energy Dispersive X-ray (EDX) Measurements of Ag-doped Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3} films

We measured the Ag-doped Sb2S3\mathrm{Sb}_{2}\mathrm{S}_{3} thin film composition with EDX across 9 different regions on the sample wafer of dimension 1cm by 1cm. The measured compositions are shown in Table S1.

Atomic Force Microscope (AFM) Film Thickness Measurement

AFM was used to measure capped Sb2S3\mathrm{Sb_2S_3} film thicknesses before and after crystallization. Figure S1 and Figure S1 show the camera image of a 55 nm-thick cap on Sb2S3\mathrm{Sb_2S_3} sample scan area before and after crystallization respectively. To extract the film thicknesses, z-height of the scanned areas were represented as histogram plots shown in Figure S1 and Figure S1. The distinct step on the sample caused the histogram to form two distinct peaks, which correspond to the film thickness.

ZnS-SiO₂ Cap Thickness Before and After Thermal Annealing

The thickness of ZnS−SiO2\mathrm{ZnS-SiO_2} films before and after thermal annealing are shown in Table S2. The measurement method was identical to the capped phase change material (PCM) thickness study in Figure 2. The single ZnS−SiO2\mathrm{ZnS-SiO_2} films were annealed at 320 ∘C320\,^\circ\mathrm{C} for 30 min. The heating parameters were chosen to match the conditions used to crystallize the Sb2S3\mathrm{Sb_2S_3} films.

Reflectivity Spectrum of PCM Thin Films

Through solving Fresnel’s equation with the transfer matrix method on OpenFilters [1], we obtained the reflectivity spectrum of the film stacks shown in Figure S2. In the simulation model, optical constants of the PCM and ZnS−SiO2\mathrm{ZnS}-\mathrm{SiO}_{2} cap were from ellipsometry measurements while the Si substrate was from the OpenFilters built-in library. The gray region in the graphs represents the light source wavelength range. The reflectance readings of the capped crystalline films were generally lower than capped amorphous films in the light source wavelength range. Hence in Figure 3b and Figure 3d, the film reflectance decreased upon crystallization.

Transmission Electron Microscopy (TEM) Cross Section Image of Microring Resonator (MRR) Device

To verify that the HF etching process gives a uniform surface, TEM images were taken at different regions of the etched device as shown in Figure S3. We observed that the top cladding oxide had consistent thickness throughout, except at the coupling region (Figure S3(iii)) where the waveguides were exposed for PCM deposition. Figure S3 shows the cross-section of the pristine device.

Value Approximations

The azimuthal mode number, mm, is related to the optical path length by eq (1) [2]:

mλres=neffLcav(1)m\lambda_{res} = n_{eff}L_{cav} \tag*{(1)}

where λres\lambda_{res} is the resonant wavelength, neffn_{eff} is the effective refractive index and LcavL_{cav} is the resonating cavity length.

For devices with uniform effective medium, neffn_{eff} can be derived through an iterative calculation between the empirical group index, ng(exp)n_g^{(exp)}, and simulated group index, ng(sim)n_g^{(sim)}, as shown in Eqs. (2) and (3). Eq. 3 was derived from the dispersion relation between neffn_{eff} and ngn_g found in reference [2].

ng(exp)=λres2FSR×Lcav,(2)n_g^{(exp)} = \frac{\lambda_{res}^{2}}{FSR \times L_{cav}}, \tag*{(2)}

where FSRFSR represents the free spectral range.

neff=Aλ+ng(sim)(λres)(3)n_{eff} = A\lambda+ n_g^{(sim)}(\lambda_{res}) \tag*{(3)}

The gradient, AA, and intercept, ng(sim)n_g^{(sim)}, gives a linear relationship between λ\lambda and neffn_{eff}. AA and ng(sim)n_g^{(sim)} can be obtained by solving Maxwell’s equation of the waveguide stack across a wavelength range with Lumerical Eigenmode solver. For small λ\lambda approximations around λres\lambda_{res}, ng(sim)n_g^{(sim)} can be corrected with ng(exp)n_g^{(exp)} so that the resultant neffn_{eff} value, neff(corrected)n_{eff}^{(corrected)}, is closer to its true value. Hence mm is approximated as such:

mλres=neff(corrected)Lcav(4)m\lambda_{res} = n_{eff}^{(corrected)}L_{cav} \tag*{(4)}

The mm value for the device without the PCM and capping layer (Figure 5c(Figure 5i)) was approximated using eqs (2) – (4). Table S3 shows the mm value approximation near the 1550 nm wavelength. Note, the resonating cavity has a 125 μ\mum radius. We observed that ng(exp)n_g^{(exp)} and ng(sim)n_g^{(sim)} were not far off from each other, based on Table S3.

For PCM-deposited MRR, mm is related to the optical path length as shown [3]:

mλres=neff(waveguide)(Lcav−LPCM)+neff(PCM)(LPCM)(5)m\lambda_{res} = n_{eff}^{(waveguide)}(L_{cav} - L_{PCM}) + n_{eff}^{(PCM)}(L_{PCM}) \tag*{(5)}

mm of Figure 5c(ii) to Figure 5c(iv) were approximated using AA and ng(exp)n_g^{(exp)} from Table S3 to derive neff(waveguide)n_{eff}^{(waveguide)}. Moreover, neff(PCM)n_{eff}^{(PCM)} values were obtained from the single waveguide mode simulation shown in Figure S4. Table S4 to Table S6 show the mm value approximation of the three devices in Figure 5c(ii) to Figure 5c(iv). Note, LPCML_{PCM} is 40 μ\mum long. Moreover, λres\lambda_{res} corresponds to the resonant peak nearest to 1550 nm. As the capped devices have a phase shift close to 2π2\pi, the nearest 1550 nm crystalline resonant peaks in Table S5 and Table S6 corresponds to the next mode number. Hence, we see a greater mm value than the amorphous peaks.

Parameterλres\lambda_{res} (nm)neff(waveguide)n_{eff}^{(waveguide)}neff(PCM)n_{eff}^{(PCM)}mm
Amorphous1550.4531.4971.531759
Crystalline1551.1251.4971.535759

Table S4. mm value approximation of device in Figure 5c(ii)

Parameterλres\lambda_{res} (nm)neff(waveguide)n_{eff}^{(waveguide)}neff(PCM)n_{eff}^{(PCM)}mm
Amorphous1549.691.4971.594761
Crystalline1549.5081.4971.610762

Table S5. mm value approximation of device in Figure 5c(iii)

2D Mode Simulation of Coupling Region

The mode pattern and neffn_{eff} values of the MRR coupling region for various devices were obtained by solving Maxwell’s equation with Lumerical Eigenmode solver. Figure S4 shows the corresponding mode profile of the 3 devices, together with their neffn_{eff} and loss values. The coupling strength is denoted by the difference between the even and odd modes, neven−noddn_{even} - n_{odd}. A greater difference gives a stronger coupling strength and smaller self-coupling coefficient, rr. Table S7 shows neven−noddn_{even} - n_{odd} for each device. We observed that the coupling strength remained consistent for both capped and uncapped 30 nm Ag-SbS whilst the coupling strength is weaker (greater rr) for the capped 60 nm Ag-SbS upon crystallization. Hence, all devices will tend towards under-coupling conditions as they experienced a greater optical loss with the crystalline PCM layer.

  1. S. Larouche and L. Martinu, "OpenFilters: open-source software for the design, optimization, and synthesis of optical filters," Applied Optics 47, C219-C230 (2008).

  1. W. Bogaerts, P. De Heyn, T. Van Vaerenbergh, K. De Vos, S. Kumar Selvaraja, T. Claes, P. Dumon, P. Bienstman, D. Van Thourhout, and R. Baets, "Silicon microring resonators," Laser & Photonics Reviews 6, 47-73 (2012).

  1. T. Y. Teo, X. Ma, E. Pastor, H. Wang, J. K. George, J. K. W. Yang, S. Wall, M. Miscuglio, R. E. Simpson, and V. J. Sorger, "Programmable chalcogenide-based all-optical deep neural networks," Nanophotonics 11, 4073-4088 (2022).

References

  1. [1]W. Bogaerts and A. Rahim, "Programmable Photonics: An Opportunity for an Accessible Large-Volume PIC Ecosystem," IEEE Journal of Selected Topics in Quantum Electronics 26, 1-17 (2020).DOI
  2. [2]A. Khanna, Y. Chen, A. Novack, Y. Liu, R. Ding, T. Baehr-Jones, and M. Hochberg, "Complexity scaling in silicon photonics," in 2017 Optical Fiber Communications Conference and Exhibition (OFC), 2017), 1-3.DOI
  3. [3]Y. Shen, N. C. Harris, S. Skirlo, M. Prabhu, T. Baehr-Jones, M. Hochberg, X. Sun, S. Zhao, H. Larochelle, D. Englund, and M. Soljačić, "Deep learning with coherent nanophotonic circuits," Nature Photonics 11, 441-446 (2017).
  4. [4]M. Yang, W. M. J. Green, S. Assefa, J. Van Campenhout, B. G. Lee, C. V. Jahnes, F. E. Doany, C. L. Schow, J. A. Kash, and Y. A. Vlasov, "Non-Blocking 4×4 Electro-Optic Silicon Switch for On-Chip Photonic Networks," Opt. Express 19, 47-54 (2011).
  5. [5]C. V. Poulton, M. J. Byrd, P. Russo, E. Timurdogan, M. Khandaker, D. Vermeulen, and M. R. Watts, "Long-Range LiDAR and Free-Space Data Communication With High-Performance Optical Phased Arrays," IEEE Journal of Selected Topics in Quantum Electronics 25, 1-8 (2019).DOI
  6. [6]M. Dong, G. Clark, A. J. Leenheer, M. Zimmermann, D. Dominguez, A. J. Menssen, D. Heim, G. Gilbert, D. Englund, and M. Eichenfield, "High-speed programmable photonic circuits in a cryogenically compatible, visible–near-infrared 200 mm CMOS architecture," Nature Photonics 16, 59-65 (2022).
  7. [7]W. Bogaerts, D. Pérez, J. Capmany, D. A. B. Miller, J. Poon, D. Englund, F. Morichetti, and A. Melloni, "Programmable photonic circuits," Nature 586, 207-216 (2020).
  8. [8]K. Liu, C. Zhang, S. Mu, S. Wang, and V. J. Sorger, "Two-dimensional design and analysis of trench-coupler based Silicon Mach-Zehnder thermo-optic switch," Opt. Express 24, 15845-15853 (2016).DOI
  9. [9]J. Joo, J. Park, and G. Kim, "Cost-Effective 2 X 2 Silicon Nitride Mach-Zehnder Interferometric (MZI) Thermo-Optic Switch," IEEE Photonics Technology Letters 30, 740-743 (2018).DOI
  10. [10]M. R. Watts, J. Sun, C. DeRose, D. C. Trotter, R. W. Young, and G. N. Nielson, "Adiabatic thermo-optic Mach-Zehnder switch," Opt. Lett. 38, 733-735 (2013).DOI
  11. [11]C. Wang, M. Zhang, B. Stern, M. Lipson, and M. Lončar, "Nanophotonic lithium niobate electro-optic modulators," Opt. Express 26, 1547-1555 (2018).DOI
  12. [12]L. Chen, Q. Xu, M. G. Wood, and R. M. Reano, "Hybrid silicon and lithium niobate electro-optical ring modulator," Optica 1, 112-118 (2014).DOI
  13. [13]A. Liu, R. Jones, L. Liao, D. Samara-Rubio, D. Rubin, O. Cohen, R. Nicolaescu, and M. Paniccia, "A high-speed silicon optical modulator based on a metal–oxide–semiconductor capacitor," Nature 427, 615-618 (2004).pubmed.ncbi.nlm.nih.gov/14961115
  14. [14]R. Soref and J. Lorenzo, "All-silicon active and passive guided-wave components for λ = 1.3 and 1.6 μm," IEEE Journal of Quantum Electronics 22, 873-879 (1986).DOI
  15. [15]R. Soref and B. Bennett, "Electrooptical effects in silicon," IEEE Journal of Quantum Electronics 23, 123-129 (1987).DOI
  16. [16]R. Chen, Z. Fang, F. Miller, H. Rarick, J. E. Fröch, and A. Majumdar, "Opportunities and Challenges for Large-Scale Phase-Change Material Integrated Electro-Photonics," ACS Photonics 9, 3181-3195 (2022).DOI
  17. [17]Q. Zhang, H. Yu, M. Barbiero, B. Wang, and M. Gu, "Artificial neural networks enabled by nanophotonics," Light: Science & Applications 8, 42 (2019).DOI
  18. [18]M. Wuttig, H. Bhaskaran, and T. Taubner, "Phase-change materials for non-volatile photonic applications," Nature Photonics 11, 465 (2017).DOI
  19. [19]R. E. Simpson, J. K. W. Yang, and J. Hu, "Are phase change materials ideal for programmable photonics?: opinion," Opt. Mater. Express 12, 2368-2373 (2022).DOI
  20. [20]P. Xu, J. Zheng, J. K. Doylend, and A. Majumdar, "Low-Loss and Broadband Nonvolatile Phase-Change Directional Coupler Switches," ACS Photonics 6, 553-557 (2019).DOI
  21. [21]Q. Zhang, Y. Zhang, J. Li, R. Soref, T. Gu, and J. Hu, "Broadband nonvolatile photonic switching based on optical phase change materials: beyond the classical figure-of-merit," Opt. Lett. 43, 94-97 (2018).DOI
  22. [22]C. Ríos, M. Stegmaier, P. Hosseini, D. Wang, T. Scherer, C. D. Wright, H. Bhaskaran, and W. H. P. Pernice, "Integrated all-photonic non-volatile multi-level memory," Nature Photonics 9, 725-732 (2015).DOI
  23. [23]M. Rudé, J. Pello, R. E. Simpson, J. Osmond, G. RoelKens, J. J. G. M. van der Tol, and V. Pruneri, "Optical switching at 1.55 μm in silicon racetrack resonators using phase change materials," Applied Physics Letters 103, 141119 (2013).DOI
  24. [24]J. Faneca, T. D. Bucio, F. Y. Gardes, and A. Baldycheva, "O-band N-rich silicon nitride MZI based on GST," Applied Physics Letters 116, 093502 (2020).DOI
  25. [25]J. Feldmann, N. Youngblood, C. D. Wright, H. Bhaskaran, and W. H. P. Pernice, "All-optical spiking neurosynaptic networks with self-learning capabilities," Nature 569, 208-214 (2019).DOI
  26. [26]C. Ríos, Q. Du, Y. Zhang, C.-C. Popescu, M. Y. Shalaginov, P. Miller, C. Roberts, M. Kang, K. A. Richardson, T. Gu, S. A. Vitale, and J. Hu, "Ultra-compact nonvolatile phase shifter based on electrically reprogrammable transparent phase change materials," Photonix 3, 26 (2022).arxiv.org/abs/2105.06010
  27. [27]R. Chen, Z. Fang, J. E. Fröch, P. Xu, J. Zheng, and A. Majumdar, "Broadband Nonvolatile Electrically Controlled Programmable Units in Silicon Photonics," ACS Photonics 9, 2142-2150 (2022).DOI
  28. [28]Z. Fang, R. Chen, J. Zheng, A. I. Khan, K. M. Neilson, S. J. Geiger, D. M. Callahan, M. G. Moebius, A. Saxena, M. E. Chen, C. Rios, J. Hu, E. Pop, and A. Majumdar, "Ultra-low-energy programmable non-volatile silicon photonics based on phase-change materials with graphene heaters," Nature Nanotechnology 17, 842-848 (2022).
  29. [29]J. Zheng, Z. Fang, C. Wu, S. Zhu, P. Xu, J. K. Doylend, S. Deshmukh, E. Pop, S. Dunham, M. Li, and A. Majumdar, "Nonvolatile Electrically Reconfigurable Integrated Photonic Switch Enabled by a Silicon PIN Diode Heater," Advanced Materials 32, 2001218 (2020).DOI
  30. [30]W. Dong, H. Liu, J. K. Behera, L. Lu, R. J. H. Ng, K. V. Sreekanth, X. Zhou, J. K. W. Yang, and R. E. Simpson, "Wide Bandgap Phase Change Material Tuned Visible Photonics," Advanced Functional Materials 29, 1806181 (2019).DOI
  31. [31]M. Delaney, I. Zeimpekis, D. Lawson, D. W. Hewak, and O. L. Muskens, "A New Family of Ultralow Loss Reversible Phase-Change Materials for Photonic Integrated Circuits: Sb2S3 and Sb2Se3," Advanced Functional Materials 30, 2002447 (2020).DOI
  32. [32]Z. Fang, J. Zheng, A. Saxena, J. Whitehead, Y. Chen, and A. Majumdar, "Non-Volatile Reconfigurable Integrated Photonics Enabled by Broadband Low-Loss Phase Change Material," Advanced Optical Materials 9, 2002049 (2021).DOI
  33. [33]M. Delaney, I. Zeimpekis, H. Du, X. Yan, M. Banakar, J. Thomson David, W. Hewak Daniel, and L. Muskens Otto, "Nonvolatile programmable silicon photonics using an ultralow-loss Sb2Se3 phase change material," Science Advances 7, eabg3500.DOI
  34. [34]L. Lu, S. F. G. Reniers, Y. Wang, Y. Jiao, and R. E. Simpson, "Reconfigurable InP waveguide components using the Sb2S3 phase change material," Journal of Optics 24, 094001 (2022).DOI
  35. [35]R. Chen, Z. Fang, C. Perez, F. Miller, K. Kumari, A. Saxena, J. Zheng, S. J. Geiger, K. E. Goodson, and A. Majumdar, "Non-volatile electrically programmable integrated photonics with a 5-bit operation," in 2023, T. Y. Teo, M. Krbal, J. Mistrik, J. Prikryl, L. Lu, and R. E. Simpson, "Comparison and analysis of phase change materials-based reconfigurable silicon photonic directional couplers," Opt. Mater. Express 12, 606-621 (2022).
  36. [37]W. K. Njoroge, H. Dieker, and M. Wuttig, "Influence of dielectric capping layers on the crystallization kinetics of Ag5In6Sb59Te30 films," Journal of Applied Physics 96, 2624-2627 (2004).DOI
  37. [38]I. Friedrich, V. Weidenhof, W. Njoroge, P. Franz, and M. Wuttig, "Structural transformations of Ge2Sb2Te5 films studied by electrical resistance measurements," Journal of Applied Physics 87, 4130-4134 (2000).DOI
  38. [39]R. Pandian, B. J. Kooi, J. T. M. De Hosson, and A. Pauza, "Influence of capping layers on the crystallization of doped SbxTe fast-growth phase-change films," Journal of Applied Physics 100, 123511 (2006).DOI
  39. [40]J. Tominaga, T. Nakano, and N. Atoda, "Double Optical Phase Transition of GeSbTe Thin Films Sandwiched between Two SiN Layers," Japanese Journal of Applied Physics 37, 1852 (1998).DOI
  40. [41]N. Ohshima, "Crystallization of germanium–antimony–tellurium amorphous thin film sandwiched between various dielectric protective films," Journal of Applied Physics 79, 8357-8363 (1996).DOI
  41. [42]R. E. Simpson, M. Krbal, P. Fons, A. V. Kolobov, J. Tominaga, T. Uruga, and H. Tanida, "Toward the Ultimate Limit of Phase Change in Ge2Sb2Te5," Nano Letters 10, 414-419 (2010).DOI
  42. [43]L. Liu, W. Dong, J. K. Behera, L. Chew, and R. E. Simpson, "Inter-diffusion of plasmonic metals and phase change materials," Journal of Materials Science 54, 2814-2823 (2019).
  43. [44]L. Liu, Z. Dong, F. Tjiptoharsono, R. J. H. Ng, H. Wang, S. D. Rezaei, Y. Wang, H. S. Leong, P. C. Lim, J. K. W. Yang, and R. E. Simpson, "Reversible Tuning of Mie Resonances in the Visible Spectrum," ACS Nano 15, 19722-19732 (2021).
  44. [45]P. Moitra, Y. Wang, X. Liang, L. Lu, A. Poh, T. W. W. Mass, R. E. Simpson, A. I. Kuznetsov, and R. Paniagua-Dominguez, "Programmable Wavefront Control in the Visible Spectrum Using Low-Loss Chalcogenide Phase-Change Metasurfaces," Advanced Materials n/a, 2205367 (2022).DOI
  45. [46]T. Y. Teo, X. Ma, E. Pastor, H. Wang, J. K. George, J. K. W. Yang, S. Wall, M. Miscuglio, R. E. Simpson, and V. J. Sorger, "Programmable chalcogenide-based all-optical deep neural networks," Nanophotonics 11, 4073-4088 (2022).DOI
  46. [47]H. Liu, W. Dong, H. Wang, L. Lu, Q. Ruan, Y. S. Tan, R. E. Simpson, and J. K. W. Yang, "Rewritable color nanoprints in antimony trisulfide films," Science Advances 6, eabb7171 (2020).DOI
  47. [48]W. Dong and R. Simpson, "Application of phase change materials in photonic devices," (Singapore University of Technology and Design, Singapore, 2019).
  48. [49]W. Dong, M. Krbal, J. Kalikka, X. Y. Chin, B. Gholipour, C. Soci, P. J. Fons, K. V. Mitrofanov, L. Chen, and R. E. Simpson, "Enhanced Sb2S3 crystallisation by electric field induced silver doping," Thin Solid Films 616, 80-85 (2016).DOI
  49. [50]C. W. Wigh and R. M. Honea, "The system Ag-Sb-S from 600°C to 200°C," Mineralium Deposita 4, 153-171 (1969).
  50. [51]S. Abdollahramezani, O. Hemmatyar, H. Taghinejad, A. Krasnok, Y. Kiarashinejad, M. Zandehshahvar, A. Alù, and A. Adibi, "Tunable nanophotonics enabled by chalcogenide phase-change materials," 9, 1189-1241 (2020).
  51. [52]M. Kuwahara, O. Suzuki, Y. Yamakawa, N. Taketoshi, T. Yagi, P. Fons, T. Fukaya, J. Tominaga, and T. Baba, "Temperature Dependence of the Thermal Properties of Optical Memory Materials," Japanese Journal of Applied Physics 46, 3909-3911 (2007).DOI
  52. [53]M. Kuwahara, O. Suzuki, T. Yagi, and N. Taketoshi, "Complex Refractive Index, Specific Heat Capacity, and Thermal Conductivity for Crystalline Sb–Te Alloys and ZnS–SiO2 with Various Compositions at High Temperatures," Japanese Journal of Applied Physics 52, 128003 (2013).DOI
  53. [54]C. Wang, C. Ma, J. He, W. Liu, X. Zhu, S. Fang, and R. Zhang, "Optical properties of Sub-30 nm-thick ZnS films studied by spectroscopic ellipsometry," Materials Science in Semiconductor Processing 142, 106454 (2022).DOI
  54. [55]L. Inc., https://www.lumerical.com/products/.
  55. [56]H. R. Philipp, "Silicon Dioxide (SiO2) (Glass)," in Handbook of Optical Constants of Solids, E. D. Palik, ed. (Academic Press, Boston, 1985), pp. 749-763.
  56. [57]Filmetrics, "Refractive Index of Si3N4, Silicon Nitride, SiN, SiON" (2022), retrieved 7 May, 2021 https://www.filmetrics.com/refractive-index-database/Si3N4/Silicon-Nitride-SiN-SiON.
  57. [58]C. Lan, G. Liang, H. Lan, H. Peng, Z. Su, D. Zhang, H. Sun, J. Luo, and P. Fan, "Microstructural and Optical Properties of Sb2S3 Film Thermally Evaporated from Antimony Pentasulfide and Efficient Planar Solar Cells," physica status solidi (RRL) – Rapid Research Letters 12, 1800025 (2018).DOI
  58. [59]W. Dong, T. Cao, K. Liu, and R. E. Simpson, "Flexible omnidirectional and polarisation-insensitive broadband plasmon-enhanced absorber," Nano Energy 54, 272-279 (2018).DOI
  59. [60]K. V. Sreekanth, W. Dong, Q. Ouyang, S. Sreejith, M. Elkabbash, C. T. Lim, G. Strangi, K.-T. Yong, R. E. Simpson, and R. Singh, "Large-Area Silver–Stibnite Nanoporous Plasmonic Films for Label-Free Biosensing," ACS Applied Materials & Interfaces 10, 34991-34999 (2018).DOI
  60. [61]K. Gao, K. Du, S. Tian, H. Wang, L. Zhang, Y. Guo, B. Luo, W. Zhang, and T. Mei, "Intermediate Phase-Change States with Improved Cycling Durability of Sb2S3 by Femtosecond Multi-Pulse Laser Irradiation," Advanced Functional Materials 31, 2103327 (2021).
  61. [62]W. K. Njoroge, H.-W. Wöltgens, and M. Wuttig, "Density changes upon crystallization of Ge2Sb2.04Te4.74 films," Journal of Vacuum Science & Technology A 20, 230-233 (2002).DOI
  62. [63]D. V. Tsu and T. Ohta, "Mechanism of Properties of Noble ZnS–SiO2 Protection Layer for Phase Change Optical Disk Media," Japanese Journal of Applied Physics 45, 6294-6307 (2006).DOI
  63. [64]N. Yamada, E. Ohno, K. Nishiuchi, N. Akahira, and M. Takao, "Rapid-phase transitions of GeTe-Sb2Te3 pseudobinary amorphous thin films for an optical disk memory," Journal of Applied Physics 69, 2849-2856 (1991).DOI
  64. [65]C. D. Wright, Y. Liu, K. I. Kohary, M. M. Aziz, and R. J. Hicken, "Arithmetic and Biologically-Inspired Computing Using Phase-Change Materials," Advanced Materials 23, 3408-3413 (2011).DOI
  65. [66]S. Larouche and L. Martinu, "OpenFilters: open-source software for the design, optimization, and synthesis of optical filters," Applied Optics 47, C219-C230 (2008).pubmed.ncbi.nlm.nih.gov/18449250
  66. [67]W. Zhang, R. Mazzarello, M. Wuttig, and E. Ma, "Designing crystallization in phase-change materials for universal memory and neuro-inspired computing," Nature Reviews Materials 4, 150-168 (2019).DOI
  67. [68]W. Bogaerts, P. De Heyn, T. Van Vaerenbergh, K. De Vos, S. Kumar Selvaraja, T. Claes, P. Dumon, P. Bienstman, D. Van Thourhout, and R. Baets, "Silicon microring resonators," Laser & Photonics Reviews 6, 47-73 (2012).DOI

Paper details

vlnc:W_j5bcq274
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents