betaFeedback

WorksPhysics and Astronomy

Magnetic Susceptibility of Superconducting Films in the Meissner-London Regime

Abstract

Extracting the London penetration depth, λ(T)λ(T), from the measured magnetic susceptibility, χ(T)χ(T), of a superconducting platelet in a perpendicular magnetic field requires knowing the function χ(λ)χ(λ) computed for the actual sample geometry. Thin films are increasingly important in quantum computing and superconducting electronics, most of which operate at ultra-low excitation fields in the vortex-free regime. Understanding their electromagnetic response in the Meissner–London (finite-λλ, no vortices) state is therefore essential for extracting intrinsic properties such as the London penetration depth and superfluid phase stiffness. While numerous prior works have addressed different aspects of this problem, here we focus on providing an analytical semi-empirical representation of χ(λ)χ(λ) based on the 2D sheet-current model and establishing the limits of its applicability using two independent full 3D numerical solutions: finite-element modeling and a volume-current integral equation. As a result, we provide χ(λ)χ(λ) for a disc of radius aa and thickness dd in closed form, valid for all λλ and for aspect ratios δ≡d/(2a)≤0.05δ\equiv d/(2a)\le0.05, and accurate to 0.1%0.1\%. The two-dimensional sheet description with Pearl length Λ=2λ2/dΛ=2λ^2/d is adequate for δ≲10−4δ\lesssim10^{-4} and λ≳4dλ\gtrsim 4d. Thicker films require the full closed form, which includes the three-dimensional corrections. Using the same numerical analysis, we provide an empirical formula that maps rectangular samples—the geometry most commonly used in experiments—onto a disc with an ``effective radius'' for subsequent calculation of χ(λ)χ(λ), and formulate a complete calibration protocol for whole-sample susceptibility measurements.

Introduction

Small-amplitude (vortex-free) Meissner–London susceptibility in a perpendicular magnetic field is an established probe for extracting the London penetration depth, λ\lambda, and thus the superfluid density [1]. We consider a thin disc of radius aa and thickness dd, placed in a uniform applied magnetic field, H=Hz^\mathbf{H} = H\hat{\mathbf{z}}. In the London gauge, the vector potential A\mathbf{A} satisfies ∇×∇×A+A/λ2=0\nabla\times\nabla\times\mathbf{A} + \mathbf{A}/\lambda^2 = 0 inside the sample and ∇×∇×A=0\nabla\times\nabla\times\mathbf{A} = 0 outside. We focus on linear magnetic susceptibility, χ=m/(VH)\chi= m/(VH), where mm is the total magnetic moment and V=πa2dV = \pi a^2d is the sample volume, and we characterize the geometry by the aspect ratio, defined as the full thickness over the diameter, δ≡d/(2a)\delta\equiv d/(2a). Radial positions are given in units of the radius, x=r/ax = r/a.

Two classes of experiments use perpendicular-field susceptibility, and each poses a distinct electromagnetic problem.

In a conventional whole-sample measurement, the entire sample is placed in a nearly uniform magnetic field, and the measured signal is proportional to its total magnetic moment, mm [1, 2, 3, 4]. In thin films, this response is governed by the demagnetizing factor, dominated by the sample edges, and controlled by the competition between the Pearl screening length Λ=2λ2/d\Lambda= 2\lambda^2/d [5] and the lateral sample size aa.

The other class of χ\chi measurements frequently used for thin films comprises two-coil mutual-inductance [6, 7, 8, 9, 10, 11, 12] and miniature scanning SQUID susceptibility [13, 14, 15, 16, 17, 18], where a film much larger than the pickup/drive coils is excited locally. Unless the film is comparable in size to the coils [11], the lateral sample dimensions drop out, the relevant screening length competes with the coil radius and probe height, and the analysis laterally assumes an infinite film.

This paper addresses the whole-sample problem, in which a measurement returns a quantity proportional to χ(T)\chi(T) with an unknown apparatus calibration constant GG. Extracting the intrinsic London penetration depth, λ(T)\lambda(T), then requires knowing the function χ(λ,d,a)\chi(\lambda,d,a) for the actual sample geometry.

This problem has been examined in many previous works from different perspectives and under various approximations. Most treatments rely on the 2D sheet-current approximation, in which the film is replaced by an infinitely thin sheet carrying the thickness-integrated current density, with Pearl’s screening length derived for a current uniform across the thickness dd. Here, we use two independent full 3D solutions to test and establish the validity bounds of these assumptions.

When λ→0\lambda\to0 and δ→0\delta\to0, the diamagnetic susceptibility of a thin disc is analytic, with magnitude χ0≡∣χ(λ→0,δ→0)∣=8a/(3πd)=4/(3πδ)\chi_0 \equiv|\chi(\lambda\to0,\delta\to0)| = 8a/(3\pi d) = 4/(3\pi\delta) [19, 20]. Brandt’s treatment of the general linear response of thin discs [21, 22] provides the strong-screening asymptote and a tabulated pole expansion, although it was formulated for ac losses and, to our knowledge, has not been systematically used to invert vortex-free London penetration depth data. Square and rectangular sheets were treated by Brandt in subsequent works [23, 24]. Chen et al. computed the ideal (λ=0\lambda= 0) magnetic susceptibility of rectangular films of arbitrary aspect ratio [25, 26], solved the thin strip at finite Λ\Lambda [27], and inverted the square-film response to obtain λ(T)\lambda(T) [28]. Their low-Λ\Lambda empirical law for the strip, 1−∣χ∣/χ0≈5.2Λ/w1 - |\chi|/\chi_0 \approx5.2\Lambda/w (ww being the half-width), omits the logarithmic factor produced by the edge singularity: first-order perturbation in the kinetic energy gives the same functional form as for the disc, (2/π)(Λ/w)ln⁡(Cw/Λ)(2/\pi)(\Lambda/w)\ln(Cw/\Lambda), and a strip version of our sheet solver gives C≃5.3C \simeq5.3. The same law, with C=16.2/π=5.16C = 16.2/\pi= 5.16, is contained in Brandt’s high-frequency asymptote for the Ohmic strip [29] continued to the London regime, exactly as for the disc. The purely linear law is therefore adequate near Λ/w=10−3\Lambda/w = 10^{-3}, where it was fitted (within 4%), but underestimates the susceptibility deficit by 25% at Λ/w=10−4\Lambda/w = 10^{-4} and by 38% at 10−510^{-5}. For thicker samples, the ideal (λ=0\lambda= 0) limit is known for arbitrary aspect ratios [30, 31, 32]. For thick London cylinders, finite-λ\lambda empirical formulas based on full 3D numerical solutions are given in our previous work [33].

In this work, we provide a closed-form expression for ∣χ(λ,d,a)∣|\chi(\lambda,d,a)| of a circular disc valid for all λ\lambda and across the full range of practical film thicknesses used in modern experiments (δ≤0.05\delta\leq0.05). We use two independent full 3D Meissner–London solvers to determine its accuracy and the boundaries of the 2D sheet regime.

Three-Dimensional Solutions

The full 3D axisymmetric Meissner–London problem was solved by two independent numerical methods:

  1. Finite-element analysis using COMSOL Multiphysics in an axisymmetric formulation for a disc of radius a=3a = 3 mm and thicknesses ranging from d=4d = 4 nm to 300 μ\mum (δ=6.7×10−7\delta= 6.7 \times10^{-7} to 0.05). The adaptive mesh was refined near the rim and sample surfaces to fully resolve the spatial distributions of magnetic fields and supercurrents inside and around the disc.

Figure 1 shows the cross-sectional distribution of axial magnetic induction Bz(r,z)B_z(r,z) in a thin film (d=10d = 10 nm, a=3a = 3 mm) for four values of the London penetration depth λ\lambda indicated in the panels. To make the variation across the 10 nm thickness visible alongside the radial penetration from the film’s edge, the vertical zz-scale is expanded by a factor of 10510^5 relative to the radial rr-scale. The minimum of BzB_z at the midplane reflects the cosh⁡(z/λ)\cosh(z/\lambda) profile of the vector potential and of the current across the film (Sec. IV).

Cross-sectional distribution of the z-component of the magnetic induction near the rim of a superconducting disc

Figure 1. Cross-sectional distribution of the zz-component of the magnetic induction, BzB_z (in G, for an applied field μ0H=1\mu_0H = 1 G), near the rim of a d=10d = 10 nm, a=3a = 3 mm superconducting disc for four values of the London penetration depth λ\lambda indicated in the panels. To visually resolve the distribution across the thickness, the vertical zz-axis is stretched by a factor of 10510^5 relative to the radial rr-axis.

To verify the numerical accuracy, we integrated the azimuthal current density over the film thickness to obtain the sheet current density, js(x)=∫−d/2d/2j(x,z) dzj_s(x) = \int_{-d/2}^{d/2} j(x,z)\,dz. In the 2D ideal-screening limit (d→0d \to0, λ→0\lambda\to0), the magnitude of the sheet current is analytic, js(x)=(4H/π)x/1−x2j_s(x) = (4H/\pi)x/\sqrt{1-x^2} [19, 20, 21], so that its initial slope at the center is (djs/dx)x→0=4H/π(dj_s/dx)_{x\to0} = 4H/\pi. Figure 2 compares a set of numerically computed js(x,λ)j_s(x,\lambda) curves against this analytic profile (green curve). Our smallest penetration depth calculation, λ=5\lambda= 5 nm (purple dashed curve), lies directly on top of the λ=0\lambda= 0 analytic curve. With increasing λ\lambda, screening weakens and js(x,λ)j_s(x,\lambda) rounds off near the rim as x→1x \to1 as expected. While λ\lambda cannot be set identically to zero inside the finite-λ\lambda London PDE solver in COMSOL, an independent perfect-shielding boundary-value problem (B⋅n^=0\mathbf{B}\cdot\hat{\mathbf{n}} = 0 on the sample surface, which is numerically much simpler) was solved on the identical mesh for every geometry to verify that the λ→0\lambda\to0 extrapolation of the London solution always converges to the exact λ=0\lambda= 0 limit.

Thickness-integrated sheet current density near the rim of a superconducting disc

Figure 2. Thickness-integrated sheet current density, js(x)j_s(x), normalized by the central slope of the ideal profile, (djs/dx)x→0=4H/π(dj_s/dx)_{x\to0} = 4H/\pi, as a function of x=r/ax = r/a near the rim of a d=10d = 10 nm, a=3a = 3 mm disc; the curves end at x=0.9999x = 0.9999. For λ→0\lambda\to0 (λ=0.005 μ\lambda= 0.005\,\mum, dashed blue), the numerical solution coincides with the exact 2D ideal-screening profile x/1−x2x/\sqrt{1-x^2} [19, 20, 21] (solid green curve).

  1. The second, independent 3D method solves the volume-current integral equation for j(r,z)j(r,z) directly [31]: the rr–zz cross-section of the disc is partitioned into Nr×NzN_r \times N_z coaxial rectangular rings of uniform current den-

sity, coupled via ring–ring mutual inductances computed from the coaxial-filament formula integrated over the ring cross-sections [31, 34], with the mesh graded geometrically toward the rim r=ar=a and both surfaces z=±d/2z=\pm d/2. No exterior air mesh is required. Across 30 benchmark (λ,d)(\lambda,d) parameter points spanning the full regime of interest, the two 3D methods agree to better than 0.07%.

Having established two mutually consistent 3D solutions, we use them as the exact reference to quantify when the 2D sheet-current approximation breaks down and to constrain our closed-form model across all λ\lambda and δ≤0.05\delta\leq0.05.

Effect of sharp edges. Mikitik [35] recently suggested that sharp corners of a sample with rectangular cross-section add a singular contribution ∝λ2/3\propto\lambda^{2/3} to the low-λ\lambda susceptibility deficit, which would dominate the standard linear-in-λ\lambda term in thin samples. Our rim-resolved 3D solutions do not show such a term. At a right-angle, the ideal (λ=0)(\lambda=0) surface magnetic field diverges as ρ−1/3\rho^{-1/3} with distance ρ\rho from the corner; consequently, the surface integral ∮Ht2 dS\oint H_t^2\,dS that determines the first-order (∝λ)(\propto\lambda) London correction converges, and the corner region ρ≲λ\rho\lesssim\lambda where the Meissner singular field is cut off contributes only at order ∫0λρ−2/3ρ dρ∝λ4/3\int_0^\lambda\rho^{-2/3}\rho\,d\rho\propto\lambda^{4/3}. Direct fits of ∣χ∣=∣χ0∣−Aλ+Bλp|\chi|=|\chi_0|-A\lambda+B\lambda^p to our 3D results for a disc with δ=0.05\delta=0.05 return p≃1.5p\simeq1.5. Forcing p=2/3p=2/3 degrades the fit residuals fifteen-fold, and evaluating the λ2/3\lambda^{2/3} term with the coefficients quoted in Ref. [35] would exceed the total numerically observed deficit tenfold. We attribute the spurious λ2/3\lambda^{2/3} term in Ref. [35] to the sharp spatial cut-off imposed there. In addition, we explored filleted corners and found no difference, provided the fillet radius is much smaller than the film thickness.

The two-dimensional sheet current model

When the film is much thinner than the lateral length scales on which the current varies, only the thickness-integrated sheet current, js(r)=∫−d/2d/2j(r,z) dzj_s(r)=\int_{-d/2}^{d/2}j(r,z)\,dz, enters the exterior field problem. Integrating London’s equation μ0λ2j=−A\mu_0\lambda^2\mathbf{j}=-\mathbf{A} over the thickness under the assumption that A\mathbf{A} is uniform across dd (d≪λ)(d\ll\lambda) yields the local constitutive law of a Pearl sheet [5],

js=−2μ0ΛA,Λ=2λ2d,(1)j_s=-\frac{2}{\mu_0\Lambda}A,\qquad\Lambda=\frac{2\lambda^2}{d}, \tag*{(1)}

where A=Aa+AjsA=A_a+A_{j_s} is the total azimuthal vector potential Aϕ(r,z=0)A_\phi(r,z=0) in the film plane, comprising the applied-field potential Aa=μ0Hr/2A_a=\mu_0Hr/2 and the self-field potential AjsA_{j_s} generated by the sheet current itself. The self-field term follows from the mutual inductance of two coaxial circular filaments [36],

Ajs(r)=12πr∫0aM(r,r′)js(r′) dr′,A_{j_s}(r)=\frac{1}{2\pi r}\int_0^a\mathcal{M}(r,r')j_s(r')\,dr',
M(r,r′)=μ0rr′[(2k−k)K(k)−2kE(k)],(2)\mathcal{M}(r,r')=\mu_0\sqrt{rr'}\left[\left(\frac{2}{k}-k\right)K(k)-\frac{2}{k}E(k)\right], \tag*{(2)}

with k2=4rr′/(r+r′)2k^2=4rr'/(r+r')^2 and K(k)K(k), E(k)E(k) the complete elliptic integrals of the first and second kind. Combining Eqs. (1) and (2) yields a linear Fredholm integral equation of the second kind for js(r)j_s(r),

μ0Λ2js(r)+12πr∫0aM(r,r′)js(r′) dr′=−μ0Hr2.(3)\frac{\mu_0\Lambda}{2}j_s(r)+\frac{1}{2\pi r}\int_0^a\mathcal{M}(r,r')j_s(r')\,dr'=-\frac{\mu_0Hr}{2}. \tag*{(3)}

(3) is the Euler–Lagrange condition minimizing the London free energy functional of the film in the applied field,

G[js]=12∫0a∫0ajs(r)M(r,r′)js(r′) dr dr′+μ0Λ4∫js2 dA+∫jsAa dA.(4)\mathcal{G}[j_s]=\frac{1}{2}\int_0^a\int_0^a j_s(r)\mathcal{M}(r,r')j_s(r')\,dr\,dr' +\frac{\mu_0\Lambda}{4}\int j_s^2\,dA+\int j_sA_a\,dA. \tag*{(4)}

with area element dA=2πr drdA=2\pi r\,dr. The three terms represent the magnetic energy of the self-field in all space, the kinetic energy of the supercurrent (∫12μ0λ2j2 dV(\int\frac{1}{2}\mu_0\lambda^2j^2\,dV for a current uniform across dd), and the coupling to the applied field. Setting the first variation of G\mathcal{G} with respect to js(r)j_s(r) to zero yields Eq. (3). Because G\mathcal{G} is a positive-definite quadratic functional plus a linear driving term, its stationary point is a unique global minimum. Note that Eq. (3) is the purely inductive (Meissner–London) limit of Brandt’s integral equation for a thin disc in an ac field [21, 22, 29].

The magnetic moment is m=πa3∫01x2js(x) dxm=\pi a^3\int_0^1x^2j_s(x)\,dx, giving susceptibility magnitude ∣χ∣=∣m∣/(πa2dH)|\chi|=|m|/(\pi a^2dH). Because all radial lengths scale with aa, the normalized sheet susceptibility depends only on the single dimensionless parameter ϵ=Λ/a\epsilon=\Lambda/a:

∣χ∣χ0=F(ϵ),χ0=8a3πd=43πδ,\frac{|\chi|}{\chi_0}=F(\epsilon),\qquad\chi_0=\frac{8a}{3\pi d}=\frac{4}{3\pi\delta},

where χ0\chi_0 follows from the ideal (ϵ=0)(\epsilon=0) sheet current, of magnitude js0(x)=(4H/π)x/1−x2j_{s0}(x)=(4H/\pi)x/\sqrt{1-x^2} [19, 20].

We solve Eq. (3) numerically by the Galerkin method [37]: js(r)j_s(r) is approximated as piecewise constant on concentric rings Ri−1<r<RiR_{i-1}<r<R_i of width wiw_i and mid-radius rir_i, graded geometrically toward the rim r=ar=a (with the outermost ring width 10−7a10^{-7}a–10−9a10^{-9}a so that the edge boundary layer of width ∼Λ\sim\Lambda is fully resolved), and the equation is imposed on the flux averaged over each ring. For the ring currents Ii=js(ri)wiI_i=j_s(r_i)w_i this gives

(M+L)I=−Φa,(5)(\mathbf{M}+\mathbf{L})\mathbf{I}=-\boldsymbol{\Phi}_a, \tag*{(5)}

where MijM_{ij} is the mutual inductance of rings ii and jj (the double average of M\mathcal{M} over their widths), Lii=L_{ii}= μ0λ22πri/(wid)\mu_0\lambda^2 2\pi r_i/(w_i d) is the kinetic inductance of ring ii, and Φa,i=μ0Hπ⟨r2⟩i\Phi_{a,i}=\mu_0 H\pi\langle r^2\rangle_i is the applied flux through it; each row states fluxoid conservation in one ring, and the solution minimizes the discretized energy G\mathcal{G}, Eq. (4). The ring–ring inductances are evaluated by Gauss–Legendre quadrature [38]: three quadrature points per ring for well-separated rings, and six for adjacent rings or rings near the r=0r=0 axis whose width is comparable to their radius. For self- and adjacent-ring integrals, the logarithmic singularity M(r,r′)≃−μ0rr′ln⁡∣r−r′∣M(r,r^\prime)\simeq-\mu_0\sqrt{rr^\prime}\ln\lvert r-r^\prime\rvert is subtracted and integrated analytically over the ring widths [39]. Since LL is proportional to Λ\Lambda, L=ϵDL=\epsilon D with Dii=μ0πari/wiD_{ii}=\mu_0\pi a r_i/w_i, a single generalized eigenvalue problem Mvk=μkDvkMv_k=\mu_kDv_k yields F(ϵ)F(\epsilon) for all ϵ\epsilon simultaneously as a spectral sum of poles,

F(ϵ)=∑kak1+ϵ/μk,∑kak=1,(6)F(\epsilon)=\sum_k\frac{a_k}{1+\epsilon/\mu_k},\qquad\sum_k a_k=1, \tag*{(6)}

with ak∝(vkTΦa)2/μk>0a_k\propto(v_k^{T}\Phi_a)^2/\mu_k>0 for vkTDvk=1v_k^{T}Dv_k=1. This has the structure of Brandt’s mode expansion [22], here evaluated with ∼103\sim10^3 eigenmodes rather than 20. The solver reproduces the ideal moment ∣m(λ=0)∣=83a3H\lvert m(\lambda=0)\rvert=\frac{8}{3}a^3H to 10−810^{-8} and the weak-screening limit F(ϵ)→3π/(32ϵ)F(\epsilon)\to3\pi/(32\epsilon) to 10−610^{-6}, and agrees with Brandt’s tabulated values [22] to their stated precision of 2×10−42\times10^{-4}; mesh refinement changes the screening deficit 1−F(ϵ)1-F(\epsilon) by less than 0.1%0.1\% for all ϵ≥5×10−8\epsilon\ge5\times10^{-8}.

In the pure 2D sheet model, the thickness dd enters only through Pearl’s Λ=2λ2/d\Lambda=2\lambda^2/d and the prefactor χ0∝1/d\chi_0\propto1/d. As we show next, replacing 2λ2/d2\lambda^2/d by the effective length Λeff\Lambda_{\mathrm{eff}} of Eq. (7) makes the sheet reproduce the exterior field of a film of finite thickness away from the rim. Rectangular films (§ 6) are solved similarly by expressing the divergence-free sheet current via a stream function, js=∇×(gz^)\mathbf{j}_s=\nabla\times(g\hat{\mathbf{z}}), and minimizing the London energy on a 2D Cartesian mesh graded toward all four edges [23, 24].

A SEMI-EMPIRICAL CLOSED-FORM SUSCEPTIBILITY

Our primary practical motivation is to construct a fast, easy to implement, yet accurate closed-form representation of χ(λ,d,a)\chi(\lambda,d,a) that can be inverted directly by experimentalists to extract λ(T)\lambda(T) from whole-sample susceptibility measurements across all realistic film thicknesses and penetration depths.

Finite thickness dd modifies the 2D sheet response through three distinct physical mechanisms:

(a) Through-thickness variation of the current and vector potential not too close to the rim. Locally, the film behaves as an infinite parallel slab, ∣z∣<d/2\lvert z\rvert<d/2, whose top and bottom surfaces experience tangential self-fields of equal magnitude and opposite sign, ±Ht=±js/2\pm H_t=\pm j_s/2, while the uniform perpendicular applied field contributes no tangential component. The tangential magnetic field inside the slab is therefore antisymmetric across the midplane,

Hr(z)=Htsinh⁡(z/λ)/sinh⁡(d/2λ)H_r(z)=H_t\sinh(z/\lambda)/\sinh(d/2\lambda), vanishing at z=0z=0, while the diametral current density jϕ(z)∝cosh⁡(z/λ)j_\phi(z)\propto\cosh(z/\lambda) flows in the same direction across the entire thickness. Integrating across z∈[−d/2,d/2]z\in[-d/2,d/2] gives js=2Htj_s=2H_t and a surface vector potential Aϕ(±d/2)=−μ0Htcoth⁡(d/2λ)A_\phi(\pm d/2)=-\mu_0H_t\coth(d/2\lambda). Outside the slab (∣z∣>d/2\lvert z\rvert>d/2), the magnetic field is identical to that of a zero-thickness current sheet at the midplane z=0z=0 carrying the same total sheet current jsj_s. Analytically continuing the exterior vector potential from the physical surfaces ∣z∣=d/2\lvert z\rvert=d/2 to the equivalent sheet plane z=0z=0 via ∂Aϕ/∂z∣=−μ0Ht\partial A_\phi/\partial z\lvert=-\mu_0H_t adds +μ0Htd/2+\mu_0H_t d/2, yielding Pearl’s law js=−(2/μ0Λeff)Aϕ(z=0)j_s=-(2/\mu_0\Lambda_{\mathrm{eff}})A_\phi(z=0) with Λ\Lambda replaced by the effective screening length

Λeff=λ[coth⁡d2λ−d2λ]=2λ2d[1−d26λ2−d4720λ4−⋯ ](d<2πλ)=λ−d2+O(e−d/λ)(d≫λ).(7)\begin{aligned} \Lambda_{\mathrm{eff}}=\lambda\left[\coth\frac{d}{2\lambda}-\frac{d}{2\lambda}\right] \\ &=\frac{2\lambda^2}{d}\left[1-\frac{d^2}{6\lambda^2}-\frac{d^4}{720\lambda^4}-\cdots\right]\qquad(d<2\pi\lambda) \\ &=\lambda-\frac{d}{2}+O\left(e^{-d/\lambda}\right)\qquad(d\gg\lambda). \tag*{(7)} \end{aligned}

The expansion parameter for thin films is (d/λ)2(d/\lambda)^2. Pearl’s Λ=2λ2/d\Lambda=2\lambda^2/d is the leading term; it corresponds to the thickness average of AA. The value of AA at the surface exceeds this average because of the cosh⁡(z/λ)\cosh(z/\lambda) profile, which adds +d/6+d/6, and continuing the exterior potential to the midplane subtracts d/2d/2. The net leading finite-thickness shift is Λeff−Λ≃−d/3\Lambda_{\mathrm{eff}}-\Lambda\simeq-d/3, which reduces Λ\Lambda by 1% at λ=4d\lambda=4d. Notably, Λeff\Lambda_{\mathrm{eff}} passes through zero at d/λ=2.39936d/\lambda=2.39936 (d≃2.40λd\simeq2.40\lambda) and becomes negative for thicker films (d>2.40λd>2.40\lambda), where supercurrents flow within skin layers of thickness ∼λ\sim\lambda near the top and bottom faces located at distance d/2d/2 from the midplane. We use the exact closed form on the first line of Eq. (7) for all calculations, never the truncated series.

(b) Finite-thickness correction to the ideal (λ=0\lambda=0) limit. At λ=0\lambda=0, a disc of finite thickness has ∣χ∣=(8a/3πd)E(δ)\lvert\chi\rvert=(8a/3\pi d)E(\delta) with E>1E>1. Its magnetic moment exceeds the thin-disc value 83a3H\frac{8}{3}a^3H because the excluded flux must go around a rim of finite height dd, and the edge singularity of the sheet current is cut off at a distance ∼d\sim d from the rim. To leading order, E≃1+(3/π)δln⁡(3.55/δ)E\simeq1+(3/\pi)\delta\ln(3.55/\delta), which is equivalent to enlarging the disc radius by (d/2)ln⁡(3.55/δ)(d/2)\ln(3.55/\delta). The total ∣χ∣∝E/d\lvert\chi\rvert\propto E/d still decreases with dd; only its ratio to 8a/3πd8a/3\pi d grows.

(c) Three-dimensional current redistribution at the rim. Within a radial distance ∼d\sim d of the edge r=ar=a, the current distribution is genuinely three-dimensional rather than a sheet current, producing a rim correction of relative order δ\delta.

Combining these three ingredients, we express the susceptibility magnitude ∣χ(λ,d,a)∣\lvert\chi(\lambda,d,a)\rvert in factored form,

∣χ(λ,d,a)∣=8a3πd F[1−2δh(λ/d)],F={F′(Λeff/a),Λeff>0,E(∣Λeff∣/a),Λeff≤0,(8)\lvert\chi(\lambda,d,a)\rvert=\frac{8a}{3\pi d}\,\mathcal{F}\left[1-2\delta h(\lambda/d)\right], \qquad \mathcal{F}= \begin{cases} F^\prime(\Lambda_{\mathrm{eff}}/a), & \Lambda_{\mathrm{eff}}>0,\\ E(\lvert\Lambda_{\mathrm{eff}}\rvert/a), & \Lambda_{\mathrm{eff}}\le0, \end{cases} \tag*{(8)}

and determine its empirical parameters by fitting to the full 3D numerical solutions of § 2. Exact analytical asymptotes fix the functional structure at both ends, while the intermediate crossover constants are fitted.

Sheet function F(ϵ)F(\epsilon): the normalized susceptibility of a zero-thickness disc as a function of ϵ=Λ/a\epsilon= \Lambda/a, evaluated in Eq. (8) at ϵ=Λeff/a\epsilon= \Lambda_{\mathrm{eff}}/a, is represented across all ϵ>0\epsilon> 0 by

1F(ϵ)−1=ϵ[3πln⁡(1+c2ϵ)+323π+c31+c4ϵ+c5ϵ(1+c6ϵ)2](9)\frac{1}{F(\epsilon)} - 1 = \epsilon\left[\frac{3}{\pi}\ln\left(1+\frac{c_{2}}{\epsilon}\right)+\frac{32}{3\pi}+\frac{c_{3}}{1+c_{4}\epsilon}+\frac{c_{5}\epsilon}{(1+c_{6}\epsilon)^{2}}\right] \tag*{(9)}

with c2=0.0401744c_{2}=0.0401744, c3=0.8898535c_{3}=0.8898535, c4=8.093975c_{4}=8.093975, c5=20.06212c_{5}=20.06212, and c6=94.44745c_{6}=94.44745. (9) reproduces the exact weak-screening asymptote F(ϵ)→3π/(32ϵ)F(\epsilon)\to3\pi/(32\epsilon) as ϵ→∞\epsilon\to\infty and the strong-screening logarithmic law 1−F(ϵ)≃(3/π)ϵln⁡(3.571/ϵ)1-F(\epsilon)\simeq(3/\pi)\epsilon\ln(3.571/\epsilon) as ϵ→0\epsilon\to0, whose coefficient 3/π3/\pi follows from first-order perturbation in the kinetic energy and agrees with Brandt’s numerical asymptote [21]; the matched asymptotics of Ref. [40] give the same form with the coefficient 22/π2\sqrt{2}/\pi, 6% lower. Equation (9) is accurate to 0.02% in FF and 0.15% in the deficit 1−F1-F over 2×10−7≤ϵ≤2002\times10^{-7}\leq\epsilon\leq200, and remains asymptotically exact beyond both ends.

Effective length Λeff\Lambda_{\mathrm{eff}}, Eq. (7): for λ<d/2.3994\lambda<d/2.3994, Λeff≤0\Lambda_{\mathrm{eff}}\leq0; in this thick-film regime, the top and bottom skin layers screen like an ideal disc of effective thickness deff=2∣Λeff∣≃d−2λd_{\mathrm{eff}}=2|\Lambda_{\mathrm{eff}}|\simeq d-2\lambda, which enters the second branch of FF through the effective aspect ratio δeff=deff/(2a)=∣Λeff∣/a\delta_{\mathrm{eff}}=d_{\mathrm{eff}}/(2a)=|\Lambda_{\mathrm{eff}}|/a.

Finite-thickness ideal limit E(δ)=∣χ0(d)∣/(8a/3πd)E(\delta)=|\chi_{0}(d)|/(8a/3\pi d):

E(δ)=3π4(δ+q),q=43π+23π×tanh⁡[6πδln⁡(1+0.17760δ)+1.00822δ](10)E(\delta)=\frac{3\pi}{4}(\delta+q), \qquad q=\frac{4}{3\pi}+\frac{2}{3\pi}\times\tanh\left[\frac{6}{\pi}\delta\ln\left(1+\frac{0.17760}{\delta}\right)+1.00822\delta\right] \tag*{(10)}

which follows the functional form proposed by Brandt [32] and is accurate to 0.05% for δ≤0.017\delta\leq0.017 and 0.3% up to δ=0.25\delta=0.25. For thin discs (δ≪1\delta\ll1), Eq. (10) expands as E(δ)≃1+(3/π)δln⁡(3.55/δ)E(\delta)\simeq1+(3/\pi)\delta\ln(3.55/\delta); the finite-thickness enhancement E−1E-1 reaches 1.1% at δ=1.5×10−3\delta=1.5\times10^{-3} and 8.8% at δ=0.017\delta=0.017. In Eq. (8), EE is evaluated at δeff=∣Λeff∣/a\delta_{\mathrm{eff}}=|\Lambda_{\mathrm{eff}}|/a, which reduces to the geometric aspect ratio δ=d/(2a)\delta=d/(2a) at λ=0\lambda=0 (Λeff=−d/2\Lambda_{\mathrm{eff}}=-d/2) and smoothly approaches E(0)=1=F(0)E(0)=1=F(0) as Λeff→0\Lambda_{\mathrm{eff}}\to0.

Rim function h(λ/d)h(\lambda/d), universal for δ≤0.05\delta\leq0.05: defining the reduced variable w=2.3994λ/dw=2.3994\lambda/d (so that w=1w=1 at Λeff=0\Lambda_{\mathrm{eff}}=0) and v=w−1v=w-1,

h={w(1.15083−0.26951w)1+0.50433w7.3113,w<1,0.557981+2.11811v0.84584+0.59756v1.75785,w≥1,(11)h=\begin{cases} \dfrac{w(1.15083-0.26951w)}{1+0.50433w^{7.3113}}, & w<1,\\[6pt] \dfrac{0.55798}{1+2.11811v^{0.84584}+0.59756v^{1.75785}}, & w\geq1, \end{cases} \tag*{(11)}

where the two branches are bridged by linear interpolation over ∣v∣<0.04|v|<0.04 (0.96<w<1.040.96<w<1.04). At small λ/d\lambda/d, hh grows linearly as h≃2.761λ/dh\simeq2.761\lambda/d (corresponding to radial flux penetration shrinking the effective rim radius by ∝λ\propto\lambda), reaches a maximum of 0.682 near λ/d=0.34\lambda/d=0.34, and falls off as v−1.76v^{-1.76} (approximating the ∼(d/λ)2\sim(d/\lambda)^2 decay over the fitted range) for λ≫d\lambda\gg d.

Overall accuracy. Benchmarked against the full 3D numerical solutions across the entire range of λ\lambda, Eq. (8) is accurate to 0.07% for δ≤1.7×10−3\delta\leq1.7\times10^{-3}, 0.08% at δ=0.017\delta=0.017, and 0.11% at δ=0.05\delta=0.05. Where higher precision is required, the sheet integral equation or 3D problem can be solved directly.

When is a film two-dimensional?

For a superconducting film in a perpendicular magnetic field, “two-dimensional” has (at least) three distinct physical meanings, governed by three different length-scale ratios:

  1. Electrodynamic 2D regime (sheet vs. volume current). The 2D sheet approximation requires the current distribution to vary laterally on scales much larger than dd, so that locally the film acts as a planar slab with tangential fields ±Ht\pm H_t on its faces and the exterior field senses only the integrated sheet current jsj_s. Figure 3 compares the pure 2D sheet model (using the unshifted Pearl length Λ=2λ2/d\Lambda=2\lambda^2/d, normalized to its λ=0\lambda=0 limit) against the full 3D COMSOL finite-element solutions for a disc of radius a=3a=3 mm and four thicknesses. For δ=d/(2a)≤1.7×10−5\delta=d/(2a)\leq1.7\times10^{-5} (d≤100d\leq100 nm), the 2D sheet and 3D curves are virtually indistinguishable over λ≲3 μm\lambda\lesssim3\,\mu\mathrm{m}. At δ=1.7×10−4\delta=1.7\times10^{-4} (d=1 μmd=1\,\mu\mathrm{m}), they separate visibly, and at δ=3.3×10−4\delta=3.3\times10^{-4} (d=2 μmd=2\,\mu\mathrm{m}) the pure sheet model misses ∼8%\sim8\% of the susceptibility deficit 1−∣χ∣/∣χ(λ=0)∣1-|\chi|/|\chi(\lambda=0)| at λ=3 μm\lambda=3\,\mu\mathrm{m} and ∼30%\sim30\% of it at λ=1 μm\lambda=1\,\mu\mathrm{m}. Because Λ(T)\Lambda(T) in experiments is extracted directly from this deficit, the error in λ\lambda is substantial when the pure 2D sheet formula is applied to micro-scale films. We conclude that the bare 2D Pearl sheet model is quantitatively reliable for δ≲10−4\delta\lesssim10^{-4} and λ≳4d\lambda\gtrsim4d.

Normalized susceptibility curves for discs with varying thicknesses

Figure 3. Normalized susceptibility χ/χ(λ=0)\chi/\chi(\lambda= 0) of a disc with a=3a = 3 mm as a function of λ\lambda: pure 2D sheet-current model with Λ=2λ2/d\Lambda= 2\lambda^2/d (black curves) vs. full 3D finite-element solution (COMSOL, orange curves) for d=10d = 10 nm, 100 nm, 1 μ\mum, and 2 μ\mum (δ=d/(2a)=1.7×10−6\delta= d/(2a) = 1.7 \times10^{-6} to 3.3×10−43.3 \times10^{-4}).

  1. Screening crossover (Pearl length vs. lateral sample size). The ratio ϵ=Λ/a\epsilon=\Lambda/a separates strong diamagnetic screening (Λ≪a\Lambda\ll a, where 1−F(ϵ)∝ϵln⁡(C/ϵ)1-F(\epsilon)\propto\epsilon\ln(C/\epsilon) is controlled by the edge peak) from weak screening (Λ≫a\Lambda\gg a). In the weak-screening limit, F(ϵ)→3π/(32ϵ)F(\epsilon)\to3\pi/(32\epsilon) so that ∣χ∣→a2/(8λ2)|\chi|\to a^{2}/(8\lambda^{2}), which measures λ−2\lambda^{-2} directly and is independent of both the film thickness dd and the ideal-screening normalization χ0\chi_{0}.

  1. Thermodynamic 2D regime (thickness vs. coherence length). When d≲ξ(T)d\lesssim\xi(T), the superconducting order parameter is uniform across the thickness and thermal phase fluctuations become two-dimensional. This modifies the physical penetration depth λ(T)\lambda(T) itself—through surface scattering, thickness-induced TcT_c suppression, and the Berezinskii-Kosterlitz-Thouless (BKT) renormalization of the 2D superfluid stiffness Λ−1(T)\Lambda^{-1}(T) by bound vortex–antivortex pairs [41, 42, 43, 44, 45, 46, 47]—but it does not alter the macroscopic Maxwell–London electrodynamics: Eq. (8)

remains valid with whatever renormalized λ(T)\lambda(T) the film possesses, provided the current–field relation remains local (i.e., Pippard coherence length ξ0≪λ\xi_0 \ll\lambda or mean free path ℓ≪λ\ell\ll\lambda).

Rectangular Samples

Most experimental thin-film samples are rectangular platelets rather than circular discs. To make our closed-form disc model directly applicable to realistic sample shapes, we solved the 2D sheet-current integral equation numerically for rectangular films of lateral dimensions w×lw \times l (w≤lw \le l) and thickness dd on a 2D mesh graded toward the edges [23, 24], covering aspect ratios 1≤l/w≤161 \le l/w \le16 and the full range of Λ\Lambda. We then fitted the normalized rectangular response ∣χ(Λ)∣/∣χ(0)∣|\chi(\Lambda)|/|\chi(0)| to the normalized disc sheet function F(Λ/ar)F(\Lambda/a_r) of Eq. (9) using a single effective disc radius ar(w,l)a_r(w,l) as the mapping parameter, obtaining

ar=w[0.735−0.222(wl)1.32],w≤l.(12)a_r = w\left[0.735 - 0.222\left(\frac{w}{l}\right)^{1.32}\right], \qquad w \le l. \tag*{(12)}

At each aspect ratio l/wl/w, ara_r was chosen to minimize the maximum relative error in the inverted λ\lambda across the experimentally relevant window 10−4≤Λ/w≤310^{-4} \le\Lambda/w \le3, and Eq. (12) reproduces these optimal radii to within 0.5%. Using ara_r in F(Λ/ar)F(\Lambda/a_r), the error in the extracted λ\lambda remains within ±1.1%\pm1.1\% over six decades of screening, 10−5≤Λ/w≤3010^{-5} \le\Lambda/w \le30. For a square film (w=lw = l), Eq. (12) gives ar=0.513wa_r = 0.513w; for a long strip (w/l→0w/l \to0), ar→0.735wa_r \to0.735w; for a typical 3×43 \times4 mm2^2 rectangular substrate (w=3w = 3 mm, l=4l = 4 mm) [4], ar=1.75a_r = 1.75 mm.

Other common choices for mapping a rectangle onto a disc perform significantly worse: using the inscribed radius w/2w/2, the equal-area radius (wl/π)1/2(wl/\pi)^{1/2}, or the radius of equal ideal susceptibility produces errors in the inverted λ\lambda of 2%, 6%, and 3% for a square (l/w=1l/w = 1), and 16%, 27%, and 8% for an elongated rectangle with l/w=4l/w = 4. Naturally, no single effective radius can be exact for all Λ/w\Lambda/w, because the weak-screening limit (Λ≫w\Lambda\gg w) is governed by the global bulk current circulation whereas the strong-screening limit (Λ≪w\Lambda\ll w) is governed by the perimeter edges and corners.

Importantly, the mapping a→ara \to a_r transfers the normalized shape ∣χ(λ)∣/∣χ(0)∣|\chi(\lambda)|/|\chi(0)| of the response, not its absolute amplitude. The ideal (λ=0\lambda= 0, δ→0\delta\to0) susceptibility of a rectangular film is ∣χ0rect∣=∣m0∣/(wldH)|\chi_0^{\mathrm{rect}}| = |m_0|/(wldH) with

∣m0∣=π4w2lH[1−0.548wl+0.126(wl)2]|m_0| = \frac{\pi}{4}w^2lH\left[1 - 0.548\frac{w}{l} + 0.126\left(\frac{w}{l}\right)^2\right]

(accurate to 0.15%), or as given by the empirical fit of Chen et al. [26] (accurate to 0.1%), rather than 8ar/(3πd)8a_r/(3\pi d). One should also bear in mind that Eq. (12) was derived within the 2D sheet model and has been established only for d/(2ar)≲10−4d/(2a_r) \lesssim10^{-4}. Within that range, the largest error in λ\lambda, 1.0%, occurs for the square, and it is at most 0.5% for 2≤l/w≤42 \le l/w \le4.

Calibration of Whole-Sample Measurements

Finally, we formulate the practical calibration procedure for whole-sample susceptibility measurements, such as frequency-domain tunnel-diode resonator (fTDR), microwave cavity perturbation, or global ac susceptometry. If the raw measured signal is S(T)S(T) (for example, the resonator frequency f(T)f(T)), the shift measured from the transition temperature TcT_c, ΔS(T)=S(Tc)−S(T)\Delta S(T) = S(T_c) - S(T), is directly proportional to the susceptibility magnitude (since χ(Tc)=0\chi(T_c) = 0),

ΔS(T)=G∣χ(T)∣,(13)\Delta S(T) = G|\chi(T)|, \tag*{(13)}

with an unknown apparatus calibration constant GG.

In bulk crystals where λ(0)\lambda(0) is much smaller than the effective sample dimension ReffR_{\mathrm{eff}} [33, 48], (1−N)χ(T→0)≃1−λ(0)/Reff≃1(1 - N)\chi(T \to0) \simeq1 - \lambda(0)/R_{\mathrm{eff}} \simeq1, so normalizing ΔS(T)\Delta S(T) by its base-temperature value ΔS(0)\Delta S(0) directly yields ∣χ(T)∣/χ0|\chi(T)|/\chi_0, and low-temperature changes Δλ(T)=λ(T)−λ(0)\Delta\lambda(T) = \lambda(T) - \lambda(0) are proportional to S(T)−S(0)S(T) - S(0) without requiring precise knowledge of λ(0)\lambda(0).

In thin and ultrathin films in a perpendicular field, by contrast, the Pearl length Λ(0)=2λ2(0)/d\Lambda(0) = 2\lambda^2(0)/d can be a substantial fraction of the lateral size aa even at T→0T \to0. Consequently, the base-temperature susceptibility ∣χ(0)∣|\chi(0)| is significantly smaller than the ideal value ∣χ(λ=0)∣|\chi(\lambda= 0)| (for example, ∣χ(λ(0))∣/∣χ(0)∣≈0.62|\chi(\lambda(0))|/|\chi(0)| \approx0.62 for a d=10d = 10 nm film with λ(0)≈1.14\lambda(0) \approx1.14 μ\mum and ar=1.75a_r = 1.75 mm [4]), and the curve χ(λ)\chi(\lambda) is strongly nonlinear. Dividing ΔS(T)\Delta S(T) by its extrapolated zero-temperature value ΔS(T→0)=S(Tc)−S(T→0)\Delta S(T \to0) = S(T_c) - S(T \to0) eliminates the unknown instrumental constant GG:

ΔS(T)ΔS(T→0)=χ(T)χ(T→0)=χ(λ(T))χ(λ(0)).(14)\frac{\Delta S(T)}{\Delta S(T \to0)} = \frac{\chi(T)}{\chi(T \to0)} = \frac{\chi(\lambda(T))}{\chi(\lambda(0))}. \tag*{(14)}

To invert the nonlinear function χ~(λ)≡∣χ(λ,d,a)∣/∣χ(0;d,a)∣\widetilde{\chi}(\lambda) \equiv|\chi(\lambda,d,a)|/|\chi(0;d,a)| calculated from Eq. (8) (using a=ara=a_r from Eq. (12) for a rectangular film), the experimental ratio in Eq. (14) is multiplied by the calculated base-temperature deficit factor χ~(λ(0))\widetilde{\chi}(\lambda(0)), where λ(0)\lambda(0) is taken from an independent measurement or estimate (such as aluminium coating [49], optical/transport Drude weight, or μ\muSR):

χ~exp(T)≡ΔS(T)ΔS(T→0)χ~(λ(0))=χ~(λ(T)).(15)\widetilde{\chi}_{\mathrm{exp}}(T) \equiv\frac{\Delta S(T)}{\Delta S(T \to0)}\widetilde{\chi}(\lambda(0)) = \widetilde{\chi}(\lambda(T)). \tag*{(15)}

Numerically inverting χ~(λ)=χ~exp(T)\widetilde{\chi}(\lambda)=\widetilde{\chi}_{\mathrm{exp}}(T) at each temperature TT then directly yields the intrinsic λ(T)\lambda(T) and the normalized superfluid density ρs(T)=[λ(0)/λ(T)]2\rho_s(T)=[\lambda(0)/\lambda(T)]^2 [3, 4].

Notice that in the 2D sheet regime (δ≲10−4\delta\lesssim10^{-4}, λ≳4d\lambda\gtrsim4d), where χ~=F(Λ/a)\widetilde{\chi}=F(\Lambda/a) depends on λ\lambda and dd solely through Λ=2λ2/d\Lambda=2\lambda^2/d, the measurement determines Λ(T)\Lambda(T) once Λ(0)\Lambda(0) is fixed. If the reference is Λ(0)\Lambda(0) itself (for example, from a two-coil measurement), the film thickness drops out of ρs(T)=Λ(0)/Λ(T)\rho_s(T)=\Lambda(0)/\Lambda(T) entirely and is needed only to convert Λ\Lambda into λ\lambda. If instead λ(0)\lambda(0) is the reference, an error in dd enters through Λ(0)=2λ2(0)/d\Lambda(0)=2\lambda^2(0)/d and propagates into ρs(T)\rho_s(T).

Conclusions

In conclusion, two independent full 3D Meissner–London numerical solutions for a superconducting disc in a perpendicular magnetic field were used to establish the quantitative range of validity of the 2D Pearl sheet-current model: δ=d/(2a)≲10−4\delta=d/(2a)\lesssim10^{-4} and λ≳4d\lambda\gtrsim4d. To eliminate the need for tedious 3D numerical calculations in data analysis, we constructed a semi-empirical closed-form expression for ∣χ(λ,d,a)∣|\chi(\lambda,d,a)|, Eq. (8), constrained by exact analytical limits and accurate to 0.1% for all λ\lambda and aspect ratios d/(2a)≤0.05d/(2a)\leq0.05. For rectangular films, we determined a phenomenological effective disc radius ar(w,l)a_r(w,l), Eq. (12), that maps the normalized rectangular sheet response onto the disc curve to within 1.1% in the extracted λ\lambda across six decades of Λ/w\Lambda/w. Finally, we formulated the complete whole-sample calibration protocol, Eqs. (14)–(15), enabling reliable extraction of the intrinsic London penetration depth λ(T)\lambda(T) and superfluid density ρs(T)\rho_s(T) from global susceptibility measurements such as conventional ac susceptometry, microwave cavity perturbation, and planar frequency-domain tunnel-diode resonator (fTDR) techniques.

Acknowledgments

This work was supported by the U.S. Department of Energy, Office of Science, National Quantum Information Science Research Centers, Superconducting Quantum Materials and Systems Center (SQMS), under Contract No. 89243024CSC000002, and by DOE BES, Materials Science and Engineering Division. Ames Laboratory is operated for the U.S. DOE by Iowa State University under contract DE-AC02-07CH11358.

References

  1. [1]C. V. Topping and S. J. Blundell, AC susceptibility as a probe of low-frequency magnetic dynamics, J. Phys.: Condens. Matter 31, 013001 (2019).DOI
  2. [2]R. Prozorov and R. W. Giannetta, Magnetic penetration depth in unconventional superconductors, Supercond. Sci. Technol. 19, R41 (2006).DOI
  3. [3]B. S. Moirangthem, K. R. Joshi, A. P. McFadden, J.-S. Oh, A. Datta, M. A. Tanatar, F. Lecocq, R. W. Simmonds, L. Zhou, M. J. Kramer, and R. Prozorov, Quasiparticle spectroscopy in tantalum films with different Ta/sapphire interfaces, Quantum Sci. Technol. 11, 03LТ01 (2026), arXiv:2603.06802.arxiv.org/abs/2603.06802
  4. [4]B. S. Moirangthem, K. R. Joshi, Z.-J. Yan, P. Xiao, L.-K. Lai, M. A. Tanatar, C.-Z. Chang, and R. Prozorov, Anisotropic interface-confined superconductivity in FeTe-based heterostructures, arXiv:2609.38148 10.48550/arXiv.2609.38148 (2026).arxiv.org/abs/2609.38148
  5. [5]J. Pearl, Current distribution in superconducting films carrying quantized fluxoids, Appl. Phys. Lett. 5, 65 (1964).DOI
  6. [6]A. T. Fiory, A. F. Hebard, P. M. Mankiewich, and R. E. Howard, Penetration depths of high-Tc films measured by two-coil mutual inductances, Appl. Phys. Lett. 52, 2165 (1988).DOI
  7. [7]S. J. Turneaure, E. R. Ulm, and T. R. Lemberger, Numerical modeling of a two-coil apparatus for measuring the magnetic penetration depth in superconducting films and arrays, J. Appl. Phys. 79, 4221 (1996).
  8. [8]J. H. Claassen, M. L. Wilson, J. M. Byers, and S. Adrian, Optimizing the two-coil mutual inductance measurement of the superconducting penetration depth in thin films, J. Appl. Phys. 82, 3028 (1997).DOI
  9. [9]S. J. Turneaure, A. A. Pesetskii, and T. R. Lemberger, Numerical modeling and experimental considerations for a two-coil apparatus to measure the complex conductivity of superconducting films, J. Appl. Phys. 83, 4334 (1998).DOI
  10. [10]T. R. Lemberger, I. Hetel, J. W. Knepper, and F. Yang, Superfluid density of YBa₂Cu₃O₇−δ ultrathin films, Phys. Rev. B 76, 094515 (2007).
  11. [11]B. Zhang, M. Qin, L. Zhang, L. You, C. Dong, P. Sha, Q. Chen, J. Yuan, and K. Jin, Determining the absolute value of magnetic penetration depth in small-sized superconducting films, Supercond. Sci. Technol. 34, 085022 (2021).DOI
  12. [12]S. P. Harvey, B. Y. Wang, J. Fowlie, M. Osada, K. Lee, Y. S. Lee, D. Li, and H. Y. Hwang, Evidence for nodal superconductivity in infinite-layer nickelates, Proc. Natl. Acad. Sci. U.S.A. 122, e2427243122 (2025).DOI
  13. [13]V. G. Kogan, Meissner response of anisotropic superconductors, Phys. Rev. B 68, 104511 (2003).DOI
  14. [14]M. E. Huber, N. C. Koshnick, H. Bluhm, L. J. Archuleta, T. Azua, P. G. Björnsson, B. W. Gardner, S. T. Hal- loran, E. A. Lucero, and K. A. Moler, Gradimetric micro-SQUID susceptometer for scanning measurements of mesoscopic samples, Rev. Sci. Instrum. 79, 053704 (2008).DOI
  15. [15]J. A. Bert, B. Kalisky, C. Bell, M. Kim, Y. Hikita, H. Y. Hwang, and K. A. Moler, Direct imaging of the coexistence of ferromagnetism and superconductivity at the LaAlO₃/SrTiO₃ interface, Nat. Phys. 7, 767 (2011).DOI
  16. [16]J. R. Kirtley, B. Kalisky, J. A. Bert, C. Bell, M. Kim, Y. Hikita, H. Y. Hwang, J. H. Ngai, Y. Segal, F. J. Walker, C. H. Ahn, and K. A. Moler, Scanning SQUID susceptometry of a paramagnetic superconductor, Phys. Rev. B 85, 224518 (2012).DOI
  17. [17]J. A. Bert, K. C. Nowack, B. Kalisky, H. Noad, M. Kim, C. Bell, Y. Hikita, H. Y. Hwang, and K. A. Moler, Gate-tuned superfluid density at the superconducting LaAlO₃/SrTiO₃ interface, Phys. Rev. B 86, 060503 (2012).
  18. [18]D. Low, G. M. Ferguson, A. Jarjour, B. T. Schaefer, M. D. Bachmann, P. J. W. Moll, and K. C. Nowack, Scanning SQUID microscopy in a cryogen-free dilution refrigerator, Rev. Sci. Instrum. 92, 083704 (2021).DOI
  19. [19]P. N. Mikheenkо and Yu. E. Kuzovlev, Inductance measurements of HTSC films with high critical currents, Physica C 204, 229 (1993).
  20. [20]J. R. Clem and A. Sanchez, Hysteretic ac losses and susceptibility of thin superconducting disks, Phys. Rev. B 50, 9355 (1994).pubmed.ncbi.nlm.nih.gov/9974983
  21. [21]E. H. Brandt, Thin superconductors in a perpendicular magnetic ac field. II. Circular disk, Phys. Rev. B 50, 4034 (1994).pubmed.ncbi.nlm.nih.gov/9976684
  22. [22]E. H. Brandt, Transverse ac susceptibility of strips and disks with complex linear resistivity, Phys. Rev. B 50, 13833 (1994).pubmed.ncbi.nlm.nih.gov/9975593
  23. [23]E. H. Brandt, Square and rectangular thin superconductors in a transverse magnetic field, Phys. Rev. Lett. 74, 3025 (1995).pubmed.ncbi.nlm.nih.gov/10058084
  24. [24]E. H. Brandt, Thin superconductors and SQUIDs in perpendicular magnetic field, Phys. Rev. B 72, 024529 (2005).DOI
  25. [25]D.-X. Chen, C. Navau, N. Del-Valle, and A. Sanchez, Perpendicular critical-state susceptibility of square superconducting films, Appl. Phys. Lett. 92, 202503 (2008).DOI
  26. [26]D.-X. Chen, C. Navau, N. Del-Valle, and A. Sanchez, Analytical expressions for critical-state ac susceptibility of rectangular superconducting films in perpendicular magnetic field, Physica C 470, 89 (2010).DOI
  27. [27]D.-X. Chen, C. Navau, N. Del-Valle, and A. Sanchez, Effective penetration depths of a thin type-II superconducting strip, Supercond. Sci. Technol. 21, 105010 (2008).DOI
  28. [28]D.-X. Chen, C. Navau, N. Del-Valle, and A. Sanchez, Determination of London penetration depth from ac susceptibility measurements of a square superconducting thin film, Physica C 500, 9 (2014).DOI
  29. [29]E. H. Brandt, Thin superconductors in a perpendicular magnetic ac field: General formulation and strip geometry, Phys. Rev. B 49, 9024 (1994).pubmed.ncbi.nlm.nih.gov/10009682
  30. [30]E. H. Brandt, Superconductors of finite thickness in a perpendicular magnetic field: Strips and slabs, Phys. Rev. B 54, 4246 (1996).pubmed.ncbi.nlm.nih.gov/9986329
  31. [31]E. H. Brandt, Superconductor disks and cylinders in an axial magnetic field: II. Nonlinear and linear ac susceptibilities, Phys. Rev. B 58, 6523 (1998).DOI
  32. [32]E. H. Brandt, Theory of type-II superconductors with finite London penetration depth, Phys. Rev. B 64, 024505 (2001).DOI
  33. [33]R. Prozorov, Meissner-London susceptibility of superconducting right circular cylinders in an axial magnetic field, Phys. Rev. Appl. 16, 024014 (2021).DOI
  34. [34]F. W. Grover, Inductance Calculations (Van Nostrand, New York, 1946) reprinted by Dover, 2004.
  35. [35]G. P. Mikitik, Determination of the London penetration depth with the tunnel diode oscillator technique, Phys. Rev. B 111, 024511 (2025).
  36. [36]J. D. Jackson, Classical Electrodynamics, 3rd ed. (Wiley, New York, 1999) Sec. 5.5.
  37. [37]K. E. Atkinson, The Numerical Solution of Integral Equations of the Second Kind (Cambridge University Press, Cambridge, 1997).DOI
  38. [38]M. Abramowitz and I. A. Stegun, Handbook of Mathematical Functions (National Bureau of Standards, Washington, 1964) Sec. 25.4, Eq. (25.4.29) and Table 25.4.
  39. [39]P. J. Davis and P. Rabinowitz, Methods of Numerical Integration, 2nd ed. (Academic Press, Orlando, 1984).
  40. [40]A. T. Dorsey, Linear response of thin superconductors in perpendicular magnetic fields: An asymptotic analysis, Phys. Rev. B 51, 15329 (1995).DOI
  41. [41]V. L. Berezinskii, Destruction of long-range order in one-dimensional and two-dimensional systems possessing a continuous symmetry group. II. Quantum systems, Zh. Eksp. Teor. Fiz. 61, 1144 (1971), [Sov. Phys. JETP 34, 610 (1972)].
  42. [42]J. M. Kosterlitz and D. J. Thouless, Ordering, metastability and phase transitions in two-dimensional systems, J. Phys. C 6, 1181 (1973).
  43. [43]D. R. Nelson and J. M. Kosterlitz, Universal jump in the superfluid density of two-dimensional superfluids, Phys. Rev. Lett. 39, 1201 (1977).DOI
  44. [44]M. R. Beasley, J. E. Mooij, and T. P. Orlando, Possibility of vortex-antivortex pair dissociation in two-dimensional superconductors, Phys. Rev. Lett. 42, 1165 (1979).DOI
  45. [45]B. I. Halperin and D. R. Nelson, Resistive transition in superconducting films, J. Low Temp. Phys. 36, 599 (1979).DOI
  46. [46]A. F. Hebard and A. T. Fiory, Evidence for the Kosterlitz-Thouless transition in thin superconducting aluminum films, Phys. Rev. Lett. 44, 291 (1980).
  47. [47]V. Ambegaokar, B. I. Halperin, D. R. Nelson, and E. D. Siggia, Dynamics of superfluid films, Phys. Rev. B 21, 1806 (1980).DOI
  48. [48]R. Prozorov, R. W. Giannetta, A. Carrington, and F. M. Araujo-Moreira, Meissner-London state in superconductors of rectangular cross section in a perpendicular magnetic field, Phys. Rev. B 62, 115 (2000).DOI
  49. [49]Prozorov, R. W., Giannetta, A. K., Carrington, A. P. Fournier, R. L. Greene, P. Guptrasarma, D. G. Hinks, and A. R. Banks, Measurements of the absolute value of the penetration depth in high-Tc superconductors using a low-Tc, superconductive coating, Appl. Phys. Lett. 77, 4202 (2000).DOI

Paper details

vlnc:W_j8n37jbd
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 11

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents