First-Principles Investigation of Irida-Graphane: A Wide-Band-Gap Semiconductor Derived from Irida-Graphene

Abstract

Opening a band gap in metallic two-dimensional carbon allotropes is an important step toward their use in electronic and optoelectronic devices, and full hydrogenation has proven to be an effective route to achieve it. Here, we propose irida-graphane, the fully hydrogenated derivative of the irida-graphene, a monolayer composed of three-, six-, and eight-membered rings, and investigate its structural, mechanical, electronic, and optical properties using density functional theory (DFT) at the PBE and HSE06 levels combined with phonon and ab initio molecular dynamics (AIMD) simulations. All carbon atoms adopt sp3sp^3 hybridization, with the hydrogen atoms of the three- and six-membered rings bonded to opposite sides of a buckled carbon framework, and the lattice parameter contracts by 4.3% with respect to irida-graphene. The hydrogenation energy of −0.53-0.53 eV/H indicates that the hydrogenation of irida-graphene from molecular hydrogen is exothermic. The absence of imaginary phonon frequencies confirms the dynamical stability of irida-graphane, and AIMD simulations show that its structure remains intact at temperatures up to 2000 K. Irida-graphane is mechanically isotropic, with an in-plane stiffness of approximately 156 N/m, a Poisson's ratio of approximately 0.1, and critical strains of approximately 20%. Hydrogenation transforms the metallic parent structure into a semiconductor with an indirect band gap of 4.68 eV (PBE) and 6.0 eV (HSE06). Irida-graphane is transparent in the visible range, with reflectivity below 0.3%, and absorbs strongly in the deep ultraviolet, with absorption coefficients of the order of 105−10610^{5} - 10^{6} cm−1^{-1}. These results suggest irida-graphane as a candidate wide-gap material for ultraviolet optoelectronics and transparent coatings.

Introduction

Two-dimensional (2D) materials have attracted considerable attention over the past two decades owing to their combination of structural, mechanical, electronic, and optical properties that differ substantially from those of their bulk counterparts.[1, 2, 3] The isolation of graphene in 2004[4] marked a turning point in materials science, revealing a material with high carrier mobility, remarkable mechanical strength, and high thermal conductivity.[5, 6, 7, 8] However, the absence of a band gap in graphene limits its direct use in transistors and digital logic,[9] which has motivated intensive efforts to design carbon-based 2D materials with tunable electronic properties.

One of the most fruitful directions in this effort has been the exploration of 2D carbon allotropes with non-hexagonal ring topologies. Graphdiyne was synthesized in 2010,[10] and the subsequent years saw the theoretical prediction of penta-graphene,[11] phagraphene,[12] and ψ\psi-graphene,[13] among many others. The synthesis of the biphenylene network in 2021[14] and of the monolayer fullerene network in 2022[15] demonstrated that 2D carbon networks beyond graphene are experimentally accessible, and renewed the interest in the theoretical design of new members of this family.

In this context, irida-graphene, a planar all-sp2sp^{2} carbon allotrope composed of fused three-, six-, and eight-membered rings,[16, 17] was fully characterized in 2023, crystallizing in the hexagonal P6/mmmP6/mmm space group with a lattice parameter of 6.34 Å and a formation energy of −6.96-6.96 eV/atom.[17] Irida-graphene was shown to be dynamically stable and to preserve its planar structure in AIMD simulations up to 1000 K, and it is a nonmagnetic metal with a Dirac cone above the Fermi level and an elastic modulus of approximately 396 GPa.[17] Since then, irida-graphene has attracted considerable attention. Its porous network has been explored for hydrogen storage upon decoration with transition, alkali, and alkaline-earth metals,[18, 19, 20, 21, 22, 23, 24] and for electrochemical energy storage as an anode for metal-ion batteries,[25, 26, 27, 28, 29] an anchoring material for lithium-sulfur batteries,[30] and an electrode for supercapacitors.[31] Its fracture behavior[32] and phonon thermal transport[33] have also been investigated, and its topology has inspired related carbon structures[34, 36] [35] as well as boron nitride[37] and silicon[38] analogues. Notably, the metallic character of irida-graphene, which favors its use in electrochemical energy storage,

which was predicted in 2007,[40] and experimental evidence for its formation through the reversible hydrogenation of graphene was reported in 2009.[41] In graphane, the conversion of all carbon atoms to sp3sp^{3} hybridization removes the π\pi states and opens a direct band gap of approximately 3.5 eV at the PBE level,[40, 42] which increases to 5.4 eV within the GW approximation.[42] Fluorination of graphene similarly yields a wide-gap insulator.[43] This strategy has been extended to other 2D carbon allotropes. The hydrogenation of penta-graphene widens its band gap,[44] while the hydrogenation of the metallic biphenylene network[45] and ψ\psi-graphene[46] opens band gaps whose magnitude depends on the hydrogen coverage.[46]

Despite the growing body of work on irida-graphene, its hydrogenated counterpart remains unexplored. To the best of our knowledge, no previous study has addressed whether the full hydrogenation of irida-graphene yields a stable monolayer, nor how its three-membered rings, which are highly strained in the sp2sp^{2} lattice, accommodate the conversion to sp3sp^{3} hybridization. These questions are relevant because the strain stored in the parent lattice may favor hydrogenation energetically, while the coexistence of rings of different sizes may lead to a buckling pattern and to physical properties distinct from those of graphane.

In this work, we investigate the structural, mechanical, electronic, and optical properties of irida-graphane, the fully hydrogenated derivative of irida-graphene, using density functional theory (DFT) calculations at the PBE and HSE06 levels, complemented by phonon calculations and ab initio molecular dynamics (AIMD) simulations. We show that irida-graphane is dynamically stable, remains structurally intact at temperatures up to 2000 K, energetically favored with respect to irida-graphene and molecular hydrogen, mechanically isotropic, and a wide-gap semiconductor that is transparent in the visible range and absorbs strongly in the deep ultraviolet.

Methodology

First-principles calculations were performed using the SIESTA code,[47, 48] which is based on the DFT formalism.[49, 50] The exchange-correlation effects were described using the generalized gradient approximation (GGA) with the Perdew-Burke-Ernzerhof (PBE) functional.[51] Given that GGA/PBE systematically underestimates the electronic band gap, additional calculations of the electronic and optical properties were carried out using the hybrid Heyd-Scuseria-Ernzerhof (HSE06) functional[52] as implemented in the HONPAS package.[53, 54] The electron-ion interactions were described by Troullier-Martins norm-conserving pseudopotentials[55] in the Kleinman-Bylander factored form,[56] with valence electron configurations of 2s22p22s^2 2p^2 and 1s11s^1 for C and H atoms, respectively. A mesh cutoff of 800 Ry and a double-ζ\zeta polarized (DZP) basis set composed of numerical atomic orbitals with finite range were employed in all calculations. The Brillouin zone of the unit cell was sampled using a 40×40×140 \times40 \times1 Monkhorst-Pack kk-point mesh.[57] In the structural optimization, both the lattice vectors and atomic positions were fully relaxed until the maximum force acting on each atom was less than 10−310^{-3} eV/Å and the difference in total energy was less than 10−510^{-5} eV. A simulation cell length of 30 Å was adopted along the direction perpendicular to the monolayer, which corresponds to a vacuum region of approximately 27 Å and prevents spurious interactions between periodic images.

Phonon dispersion calculations were performed to assess the dynamical stability of the irida-graphane monolayer. A 3×3×13 \times3 \times1 supercell was employed with an energy convergence criterion of 10−510^{-5} eV, a force convergence criterion of 0.001 eV/Å, and a mesh cutoff of 800 Ry. The acoustic sum rule was applied to the vibrational frequencies at the Γ\Gamma point. Additionally, AIMD simulations were performed using a 2×2×12 \times2 \times1 supercell containing 96 atoms to assess the thermal stability of irida-graphane at 300, 1000, and 2000 K. The simulations were performed within the NVT ensemble with a 10×10×110 \times10 \times1 kk-point mesh, using a time step of 1.0 fs and a Nosé-Hoover thermostat for temperature regulation,[58, 59] and the system was evolved for 10 ps at each temperature.[60, 61, 62]

The mechanical response was evaluated by applying uniaxial and biaxial tensile strains to a 2×2×12 \times2 \times1 supercell in increments of 0.5% up to structural failure. Uniaxial strain was applied independently along the xx- and yy-directions, while the supercell was allowed to relax along the direction perpendicular to the loading. The effective thickness of the monolayer, required to express the two-dimensional mechanical quantities in three-dimensional units, was obtained from the interlayer distance of stacked irida-graphane layers, and the calculations for bilayer, trilayer, and periodically stacked systems consistently yielded 5.50 Å. Finally, the optical properties were computed for unpolarized light incident along the direction normal to the monolayer, so that the electric field lies in the basal plane and the response corresponds to an average over the in-plane directions, using a 10×10×110 \times10 \times1 kk-point mesh and a Gaussian broadening of 0.05 eV.

Results and Discussion

Full hydrogenation transforms all carbon atoms of the parent lattice from sp2sp^2 to sp3sp^3 hybridization, and the way in which the three-, six-, and eight-membered rings accommodate this conversion determines the geometry of the resulting monolayer. The optimized structure of irida-graphane is shown in Figure 1. Its hexagonal unit cell contains 24 atoms (12 C and 12 H) and has an optimized lattice parameter of 6.081 Å, which is 4.3% smaller than the value of 6.357 Å obtained for pristine iridagraphene calculated using the same computational setup, in close agreement with the value of 6.34 Å reported previously.[17] Each carbon atom is bonded to three carbon atoms and one hydrogen atom, confirming the complete conversion to sp3sp^3 hybridization in the lattice. The hydrogen atoms bonded to the carbon atoms of the three-membered rings point toward one side of the monolayer, while those bonded to the carbon atoms of the six-membered rings point toward the opposite side. This arrangement induces, the carbon framework becomes buckled, resulting in a vertical separation of 1.122 Å between the two carbon sublayers and a total thickness of 3.077 Å measured between the outermost hydrogen atoms.

Atomic structure of the irida-graphane monolayer

Figure 1. Atomic structure of the irida-graphane monolayer. The main panel shows the top view of an extended sheet, the inset shows the unit cell, and the side panels show views along the xx- and yy-directions. Gray and white spheres represent C and H atoms, respectively.

This arrangement is reflected in the C–C bond lengths. Within the three-membered rings, the C–C bonds connect carbon atoms whose hydrogen atoms lie on the same side of the monolayer and measure 1.521 Å. The bonds connecting the three- and six-membered rings, where the bonded carbon atoms bear hydrogen atoms on opposite sides of the sheet, are slightly longer, measuring 1.529–1.530 Å. Within the six-membered rings, the C–C bonds reach 1.593 Å, with the hydrogen atoms again lying on the same side of the monolayer. Thus, along the carbon framework, the hydrogen atoms alternate in pairs rather than individually. This pattern combines chair-like arrangements between the rings with boat-like arrangements within them, in contrast to the uniform chair conformation of graphane.[40]

All these C–C bonds are longer than those calculated for pristine irida-graphane, for which we obtain 1.417 Å within the three-membered rings and 1.408–1.444 Å for the remaining bonds. The resulting bond lengths are broadly consistent with single C–C bonds, whose characteristic length is approximately 1.54 Å in diamond.[63] Notably, the C–C bond length within the three-membered rings is close to the equilibrium value of 1.503 Å reported for cyclopropane,[64] suggesting that the triangular motifs of the parent lattice are retained as saturated, cyclopropane-like units. In contrast, the longer C–C bonds within the six-membered rings may be associated with steric repulsion between hydrogen atoms attached to adjacent carbon atoms on the same side of the monolayer. These hydrogen atoms may experience enhanced repulsion because of their eclipsed arrangement, imposed by the ring geometry.

The C–H bond lengths range from 1.103 to 1.110 Å. The bond angles around the carbon atoms span 104.6–126.1°, excluding the 60° angles within the three-membered rings. This broad angular range indicates a substantial distortion of the local tetrahedral geometry associated with the sp3sp^3-hybridized carbon atoms.

Interestingly, the lattice parameter contracts upon hydrogenation despite the elongation of all C–C bonds: by 7.3% within the three-membered rings, 8.6% between the three- and six-membered rings, and 10.3% within the six-membered rings. This apparent contradiction can be explained by the buckling of the carbon framework, which tilts the bonds out of the basal plane and thereby reduces their in-plane projections. This behavior contrasts with that of graphene, whose calculated lattice parameter increases from 2.46 Å to approximately 2.52–2.54 Å upon full hydrogenation to chair graphane.[40, 65]

The energetic favorability of hydrogenation provides a further criterion for assessing the feasibility of obtaining irida-graphane from iridagraphene. To quantify this contribution, we calculated the hydrogenation energy per hydrogen atom relative to molecular hydrogen, defined as

EH=EIGH−EIG−nH2EH2nH(1)E_{\mathrm{H}} = \frac{E_{\mathrm{IGH}} - E_{\mathrm{IG}} - \frac{n_{\mathrm{H}}}{2}E_{\mathrm{H}_2}}{n_{\mathrm{H}}} \tag*{(1)}

where EIGHE_{\mathrm{IGH}} and EIGE_{\mathrm{IG}} are the total energies of the irida-graphane and irida-graphene unit cells, respectively, EH2E_{\mathrm{H}_2} is the total energy of an isolated H2\mathrm{H}_2 molecule, and nH=12n_{\mathrm{H}} = 12 is the number of hydrogen atoms in the unit cell. We obtain EH=−0.53E_{\mathrm{H}} = -0.53 eV/H, indicating that hydrogenation is exothermic with respect to irida-graphene and molecular hydrogen at the level of theory employed. This value is more negative than the corresponding value of approximately −0.19-0.19 eV/H inferred from the PBE formation energy of −0.097-0.097 eV/atom reported for chair graphane relative to graphene and H2\mathrm{H}_2.[65] The greater exothermicity found for irida-graphane may be associated with the release of strain in the sp2sp^2-bonded three-membered rings of the parent lattice as they transform into saturated, cyclopropane-like units.

A favorable hydrogenation energy, however, does not ensure that the resulting lattice is stable against small atomic displacements. To assess its dynamical stability, we have calculated the phonon dispersion of irida-graphane along the Γ\Gamma-M\mathrm{M}-K\mathrm{K}-M\mathrm{M}-Γ\Gamma path of the first Brillouin zone, as presented in Figure 2. The 24 atoms of the unit cell give rise to 72 phonon branches, of which three are acoustic and 69 are optical. We observe no imaginary frequencies along the sampled path, supporting the dynamical stability of the monolayer. As shown in the inset, the longitudinal and transverse acoustic branches exhibit linear dispersion from the Γ\Gamma point, while the out-of-plane acoustic branch exhibits the quadratic dispersion characteristic of the flexural mode of two-dimensional materials. No pronounced softening is observed near the zone center, and the lowest optical mode at Γ\Gamma lies at 212 cm−1\mathrm{cm}^{-1}.

Phonon dispersion of the irida-graphane monolayer

Figure 2. Phonon dispersion of the irida-graphane monolayer along the Γ\Gamma-M\mathrm{M}-K\mathrm{K}-M\mathrm{M}-Γ\Gamma path. The inset shows the low-frequency region and the first Brillouin zone.

At higher frequencies, the vibrational spectrum splits into well-separated groups of modes, with three main frequency gaps at 366–408 cm−1\mathrm{cm}^{-1}, 1311–1426 cm−1\mathrm{cm}^{-1}, and 1436–2987 cm−1\mathrm{cm}^{-1}. The widest one, of approximately 1550 cm−1\mathrm{cm}^{-1}, isolates the C-H stretching modes,

which form a narrow group of bands between 2987 and 3115 cm−1\mathrm{cm}^{-1}. These modes are nearly dispersionless, as expected for localized vibrations of the light hydrogen atoms against the much heavier carbon framework. A similarly wide gap separating the C-H stretching modes from the framework modes is present in the phonon dispersion of graphane, whose C-H stretching frequencies at the Γ\Gamma point were calculated at 2739 and 2783 cm−1\mathrm{cm}^{-1}.[66] Below approximately 1440 cm−1\mathrm{cm}^{-1}, the modes involve the vibrations of the carbon framework coupled to the C-H bending motions.

Dynamical stability at zero temperature, in turn, does not guarantee that the lattice survives thermal fluctuations, particularly in a hydrogenated structure in which hydrogen desorption or ring reconstruction could be thermally activated. For this reason, the thermal stability of irida-graphane was evaluated through AIMD simulations at 300, 1000, and 2000 K, as presented in Figure 3. At 300 K, the temperature fluctuates around an average value of 300.0±\pm60.4 K, and the Kohn-Sham total energy fluctuates around −88.966±0.009-88.966 \pm0.009 eV/atom with no systematic drift over the 10 ps trajectory. A similar behavior is observed at 1000 and 2000 K, in which the energy oscillates around constant mean values after the initial thermalization, with larger fluctuation amplitudes that follow the increase in temperature. The snapshots at the end of the simulations show that the carbon framework retains its three-, six-, and eight-membered rings at all temperatures, with thermal fluctuations of the atomic positions that increase with temperature and no evidence of bond breaking, ring reconstruction, or hydrogen desorption. Together with the phonon results, these simulations indicate that irida-graphane is dynamically stable and thermally robust up to at least 2000 K within the simulated time scale.

AIMD simulations of irida-graphane at 300 K, 1000 K, and 2000 K, showing top and side views and the time evolution of temperature and total energy per atom

Figure 3. AIMD simulations of irida-graphane at (a) 300 K, (b) 1000 K, and (c) 2000 K. The top row shows the final snapshots (top and side views), and the middle and bottom rows show the time evolution of the temperature and of the total energy per atom, respectively.

Once its stability is established, a natural question is how the conversion of the sp2sp^{2} network into a buckled sp3sp^{3} network with longer bonds affects the response of the lattice to in-plane loading. We have addressed it by applying uniaxial strain along the xx- and yy-directions and biaxial strain along both directions simultaneously, and the resulting strain energy curves are presented in Figure 4. The curves for uniaxial strain along the xx- and yy-directions are practically superimposed over the entire strain range, which reflects the in-plane mechanical isotropy expected for a lattice with hexagonal symmetry. Since the strain energy is stored in both directions simultaneously, the biaxial curve rises more steeply and reaches 34.6 eV per supercell at 20% strain, compared with approximately 19.2 eV for uniaxial strain.

Strain energy of the irida-graphane supercell as a function of strain, with structures under corresponding strains

Figure 4. Strain energy of the irida-graphane supercell as a function of uniaxial strain along the xx- and yy-directions and of biaxial strain (xyxy). The critical strains are indicated, and the right panels show the structures under the corresponding strains.

From the quadratic region of these curves, we have extracted the in-plane stiffness [67, 68]

C=1A×(∂2ES∂ε2)∣ε=0,(2)C = \frac{1}{A} \times\left(\frac{\partial^{2} E_{S}}{\partial\varepsilon^{2}}\right)\bigg|_{\varepsilon=0}, \tag*{(2)}

where AA is the area of the optimized supercell, ε=Δl/l0\varepsilon= \Delta l/l_{0} is the uniaxial strain with l0l_{0} being the equilibrium supercell length and Δl=l−l0\Delta l = l-l_{0}, and ESE_{S} is the strain energy obtained by subtracting the equilibrium total energy from the total energy under strain, as well as the in-plane bulk modulus [69, 70]

B=A×(∂2ES∂A2)∣A0,(3)B = A \times\left(\frac{\partial^{2} E_{S}}{\partial A^{2}}\right)\bigg|_{A_{0}}, \tag*{(3)}

where A0A_{0} and AA represent the supercell area at equilibrium and under biaxial strain, respectively. We obtain an in-plane stiffness of approximately 156 N/m along both the xx- and yy-directions and an in-plane bulk modulus of 77 N/m.

Using the effective thickness of 5.50 Å, the in-plane stiffness corresponds to a Young’s modulus of approximately 284 GPa. These values are considerably lower than the in-plane stiffness of 340 N/m for graphene[8] and of 243–246 N/m for graphane[68, 71], which is consistent with the lower areal density of bonds in a lattice containing eight-membered rings and with the replacement of sp2sp^{2} bonds by longer sp3sp^{3} single bonds. In contrast, the elastic modulus of approximately 396 GPa reported for irida-graphene from reactive molecular dynamics simulations[17] corresponds to approximately 133 N/m for a thickness of 3.35 Å, which indicates that, despite the longer bonds, the full hydrogenation does not reduce the in-plane stiffness of the parent lattice and may even increase it slightly. We note that this comparison is made in terms of two-dimensional quantities, since the values in GPa depend on the thickness adopted for each monolayer. This behavior may be attributed to the additional rigidity introduced by the buckled sp3sp^{3} framework, although a quantitative comparison is limited by the different levels of theory employed in the two studies. The lateral response was quantified through the Poisson’s ratio[72]

ν=−εtransεaxial,(4)\nu= -\frac{\varepsilon_{\mathrm{trans}}}{\varepsilon_{\mathrm{axial}}}, \tag*{(4)}

obtained from the ratio of the transverse strain (εtrans\varepsilon_{\mathrm{trans}}) to the axial strain (εaxial\varepsilon_{\mathrm{axial}}) at small strains, which yields νx=0.08\nu_{x}=0.08 and νy=0.11\nu_{y}=0.11 for strain applied along the xx- and yy-directions, respectively. Such small values are comparable to the values of 0.07–0.08 reported for graphene[68, 71] and indicate that the transverse contraction under uniaxial tension is weak, which may be attributed to the buckled sp3sp^{3} framework, in which the applied strain is accommodated mainly by the flattening of the buckled carbon sublayers and the opening of the bond angles rather than by a lateral contraction of the lattice.

Beyond the elastic regime, the in-plane stress, obtained from the stress tensor and converted into a two-dimensional quantity by multiplying it by the length of the simulation cell normal to the monolayer, increases monotonically with strain up to the critical strain, which we identify as the strain at which the stress reaches its maximum value. The critical strains are approximately 20% for uniaxial strain along both directions and for biaxial strain, as indicated in Figure 4, and the corresponding ultimate strengths are 17.5 N/m along the xx-direction, 16.7 N/m along the yy-direction, and 15.1 N/m for biaxial strain, which correspond to 31.8, 30.4, and 27.5 GPa, respectively. Under biaxial strain, the stress collapses immediately beyond the critical strain, at 21%, signaling the simultaneous rupture of C-C bonds and the structural failure of the monolayer. Under uniaxial strain, in contrast, the stress decreases slowly up to 21.5%, drops by approximately 20% between 21.5 and 22%, declines gradually to approximately 6–7 N/m at 24.5%, and only then collapses at 25%, which suggests that the lattice accommodates the deformation through successive local bond ruptures before complete failure. Although these ultimate strengths are well below the intrinsic strength of 42 N/m measured for graphene,[8] the critical strains of approximately 20% indicate that the hydrogenated irida-graphene lattice combines a reduced stiffness with a considerable tolerance to tensile deformation, which suggests that irida-graphane could withstand the deformations involved in flexible device architectures without loss of structural integrity.

The same saturation of the carbon framework that softens the lattice has an even more pronounced effect on its electronic structure. In graphene, hydrogenation removes the delocalized π\pi states and converts a semimetal into a wide-gap insulator,[40, 41, 42] and an analogous transformation is expected for the metallic irida-graphene.[17] The electronic band structure and the density of states (DOS) of iridagraphane calculated at the PBE and HSE06 levels are presented in Figure 5. We observe that irida-graphane is a semiconductor with an indirect band gap, with the valence band maximum (VBM) located at the M point and the conduction band minimum (CBM) located at the Γ\Gamma point. The band gap is 4.68 eV at the PBE level and 6.0 eV with the HSE06 functional, and the smallest direct gap, located at the Γ\Gamma point, is 5.39 eV at the PBE level.

Electronic band structure and density of states of irida-graphane calculated at the PBE and HSE06 levels

Figure 5. (a) Electronic band structure and (b) density of states of irida-graphane calculated at the PBE (black) and HSE06 (green) levels. The Fermi level is set to zero.

This wide band gap is a direct consequence of the complete sp3sp^{3} hybridization of the carbon framework. In pristine irida-graphene, the partially filled π\pi bands derived from the pzp_{z} orbitals give rise to its metallic character.[17] Upon hydrogenation, each pzp_{z} orbital forms a σ\sigma bond with a hydrogen atom, and the band edges become determined by the bonding and antibonding σ\sigma states, which are separated by a much larger energy. The band gaps of irida-graphane are larger than those reported for chair graphane, namely approximately 3.5 eV at the PBE level[40, 42] and 4.5–4.6 eV with the HSE06 functional,[73] which may be related to the longer C-C bonds and to the reduced orbital

overlap in the strained ring network. Regarding the band dispersion, the conduction band is strongly dispersive around the Γ\Gamma point, with an energy increase of approximately 1.7 eV between Γ\Gamma and K, whereas the topmost valence band varies by approximately 0.7 eV along the path, which is reflected in the steep increase of the DOS at the valence band edge. The HSE06 functional increases the band gap by approximately 1.3 eV, as expected from the partial incorporation of screened exact exchange, which reduces the band gap underestimation of semilocal functionals, [74, 75] while preserving the overall dispersion of the bands. A band gap of this magnitude places irida-graphane among the wide-gap two-dimensional materials and is relevant for dielectric and ultraviolet optoelectronic applications.

Such a wide gap also implies that the optical activity of irida-graphane is confined to the ultraviolet region. To quantify this behavior, we have computed the dielectric function of the monolayer. Its imaginary part, which accounts for the interband optical transitions between the valence band (VB) and the conduction band (CB), is given by Fermi’s golden rule[76]

ϵ2(ω)=4π2Ωω2∑i∈VB∑j∈CB∑kWk∣ρij∣2δ(ϵkj−ϵki−ℏω)(5)\epsilon_{2}(\omega)=\frac{4\pi^{2}}{\Omega\omega^{2}}\sum_{i\in\mathrm{VB}}\sum_{j\in\mathrm{CB}}\sum_{k}W_{k}\lvert\rho_{ij}\rvert^{2}\delta(\epsilon_{kj}-\epsilon_{ki}-\hbar\omega) \tag*{(5)}

where ω\omega represents the photon frequency, ∣ρij∣\lvert\rho_{ij}\rvert is the dipole transition matrix element, WkW_{k} is the weight of the respective kk-point in reciprocal space, and Ω\Omega is the system volume, while its real part follows from the Kramers–Kronig relation[77, 78]

ϵ1(ω)=1+1πP∫0∞dω′ω′ϵ2(ω′)ω′2−ω2(6)\epsilon_{1}(\omega)=1+\frac{1}{\pi}P\int_{0}^{\infty}d\omega'\frac{\omega'\epsilon_{2}(\omega')}{\omega'^{2}-\omega^{2}} \tag*{(6)}

where PP denotes the principal value of the integral over ω′\omega'. From ϵ1\epsilon_{1} and ϵ2\epsilon_{2}, we have obtained the absorption coefficient (α\alpha), reflectivity (RR), and refractive index (η\eta)

α(ω)=2ω[(ϵ12(ω)+ϵ22(ω))1/2−ϵ1(ω)]1/2(7)\alpha(\omega)=\sqrt{2}\omega\left[\left(\epsilon_{1}^{2}(\omega)+\epsilon_{2}^{2}(\omega)\right)^{1/2}-\epsilon_{1}(\omega)\right]^{1/2} \tag*{(7)}
R(ω)=[(ϵ1(ω)+iϵ2(ω))1/2−1(ϵ1(ω)+iϵ2(ω))1/2+1]2(8)R(\omega)=\left[\frac{\left(\epsilon_{1}(\omega)+i\epsilon_{2}(\omega)\right)^{1/2}-1}{\left(\epsilon_{1}(\omega)+i\epsilon_{2}(\omega)\right)^{1/2}+1}\right]^{2} \tag*{(8)}

and

η(ω)=12[(ϵ12(ω)+ϵ22(ω))1/2+ϵ1(ω)]1/2(9)\eta(\omega)=\frac{1}{\sqrt{2}}\left[\left(\epsilon_{1}^{2}(\omega)+\epsilon_{2}^{2}(\omega)\right)^{1/2}+\epsilon_{1}(\omega)\right]^{1/2} \tag*{(9)}

which are presented in Figure 6 for in-plane polarized light at the PBE and HSE06 levels, where the shaded region indicates the visible range.

Absorption coefficient, refractive index, and reflectivity of irida-graphane at the PBE and HSE06 levels

Figure 6. (a) Absorption coefficient, (b) refractive index, and (c) reflectivity of irida-graphane at the PBE (black) and HSE06 (green) levels. The shaded region indicates the visible range.

As anticipated from the band gap, irida-graphane does not absorb in the infrared and visible ranges, as shown in Figure 6(a). At the PBE level, the absorption begins at approximately 5.6 eV, which is close to the direct gap at the Γ\Gamma point and above the indirect gap, since the indirect transitions do not contribute to Eq. (5). The absorption coefficient exceeds 105 cm−110^{5}\ \mathrm{cm}^{-1} at 7.2 eV, exhibits a pronounced peak of 8.8×105 cm−18.8\times10^{5}\ \mathrm{cm}^{-1} at 8.25 eV, and rises again to 1.1×106 cm−11.1\times10^{6}\ \mathrm{cm}^{-1} at the upper limit of the computed spectrum. With the HSE06 functional, the absorption onset shifts to approximately 6.7 eV, the absorption coefficient exceeds 105 cm−110^{5}\ \mathrm{cm}^{-1} only at 9.0 eV, and the strongest absorption occurs at the upper limit of the computed spectrum, consistent with the blue shift of the band edges discussed above.

In the visible range, the refractive index shown in Figure 6(b) remains nearly constant, between 1.09 and 1.10 at the PBE level, with static values of 1.09 (PBE) and 1.02 (HSE06). At the PBE level, it increases in the ultraviolet up to a maximum of 1.65 at 8.20 eV, just below the absorption peak at 8.25 eV, and then decreases, which is the typical dispersion behavior near a strong absorption band. Likewise, the reflectivity shown in Figure 6(c) remains below 0.3% in the visible range at both levels of theory and reaches 19% at 8.26 eV at the PBE level, following the absorption peak, before rising steeply toward the upper limit of the spectrum. The combination of negligible absorption and reflectivity in the visible range with strong absorption in the deep ultraviolet suggests that irida-graphene may be suitable for transparent coatings and ultraviolet-filtering applications.

Conclusions

In summary, we have performed a first-principles investigation of the structural, mechanical, electronic, and optical properties of irida-graphane, the fully hydrogenated derivative of irida-graphene. Full hydrogenation converts the carbon atoms from sp2sp^{2} to sp3sp^{3} hybridization and produces a buckled framework in which the hydrogen atoms attached to the three- and six-membered rings lie on opposite sides of the monolayer. The three-membered rings retain saturated, cyclopropane-like configurations, while the buckling of the carbon framework reduces the in-plane projections of the C–C bonds, leading to lattice contraction despite their elongation. The calculated hydrogenation energy indicates an exothermic process relative to pristine irida-graphene and molecular hydrogen. Furthermore, the phonon dispersion exhibits no imaginary frequencies along the investigated high-symmetry path, and ab initio molecular dynamics simulations show that the structure retains its integrity over 10 ps at temperatures up to 2000 K under the simulated conditions.

Our calculations also reveal a wide indirect band gap, transforming metallic irida-graphene into a semiconductor with band gaps of 4.68 eV at the PBE level and 6.0 eV with the HSE06 functional. These values exceed those reported for chair graphane. The calculated mechanical response indicates that irida-graphene can sustain substantial tensile deformation, although its mechanical properties warrant further comparative analysis. The optical spectra predict negligible absorption and reflectivity in the visible range, together with strong absorption in the deep ultraviolet. Overall, these findings establish hydrogenation as a promising strategy for tailoring the structural and electronic properties of irida-graphene and identify irida-graphane as a candidate material for ultraviolet optoelectronics and transparent coatings. They also motivate further investigations into its experimental synthesis and the controlled hydrogenation of this carbon allotrope.

Author Contributions

D.S.G.: Data Curation, Investigation, Software, Writing - Original Draft. I.M.F.: Investigation, Formal Analysis, Visualization, Writing - Original Draft. M.L.P.J.: Conceptualization, Methodology, Formal Analysis, Validation, Resources, Supervision, Project Administration, Funding Acquisition, Writing - Review & Editing. All authors reviewed the manuscript.

Declaration of Competing Interests

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

Data Availability

The data that support the findings of this study are available from the corresponding author upon reasonable request.

Acknowledgments

D.S.G. acknowledges financial support from the Coordenação de Aperfeiçoamento de Pessoal de Nível Superior (CAPES). M.L.P.J. acknowledges financial support from FAPDF (grant 00193-00001807/2023-16), CNPq (grants 444921/2024-9 and 308222/2025-3), and CAPES (grant 88887.005164/2024-00).

References

  1. [1]Butler, S. Z. et al. Progress, Challenges, and Opportunities in Two-Dimensional Materials Beyond Graphene. ACS Nano 2013, 7, 2898–2926.DOI
  2. [2]Bhimanapati, G. R. et al. Recent Advances in Two-Dimensional Materials beyond Graphene. ACS Nano 2015, 9, 11509–11539.DOI
  3. [3]Novoselov, K. S.; Mishchenko, A.; Carvalho, A.; Castro Neto, A. H. 2D Materials and van der Waals Heterostructures. Science 2016, 353, aac9439.DOI
  4. [4]Novoselov, K. S.; Geim, A. K.; Morozov, S. V.; Jiang, D.; Zhang, Y.; Dubonos, S. V.; Grigorieva, I. V.; Firsov, A. A. Electric Field Effect in Atomically Thin Carbon Films. Science 2004, 306, 666–669.pubmed.ncbi.nlm.nih.gov/15499015
  5. [5]Geim, A. K.; Novoselov, K. S. The rise of graphene. Nat. Mater. 2007, 6, 183–191.
  6. [6]Castro Neto, A. H.; Guinea, F.; Peres, N. M. R.; Novoselov, K. S.; Geim, A. K. The electronic properties of graphene. Rev. Mod. Phys. 2009, 81, 109–162.DOI
  7. [7]Balandin, A. A.; Ghosh, S.; Bao, W.; Calizo, I.; Teweldebrhan, D.; Miao, F.; Lau, C. N. Superior Thermal Conductivity of Single-Layer Graphene. Nano Lett. 2008, 8, 902–907.DOI
  8. [8]Lee, C.; Wei, X.; Kysar, J. W.; Hone, J. Measurement of the Elastic Properties and Intrinsic Strength of Monolayer Graphene. Science 2008, 321, 385–388.
  9. [9]Schwierz, F. Graphene transistors. Nat. Nanotechnol. 2010, 5, 487–496.DOI
  10. [10]Li, G.; Li, Y.; Liu, H.; Guo, Y.; Li, Y.; Zhu, D. Architecture of graphidyne nanoscale films. Chem. Commun. 2010, 46, 3256–3258.DOI
  11. [11]Zhang, S.; Zhou, J.; Wang, Q.; Chen, X.; Kawazoe, Y.; Jena, P. Penta-graphene: A new carbon allotrope. Proc. Natl. Acad. Sci. U.S.A. 2015, 112, 2372–2377.
  12. [12]Wang, Z.; Zhou, X.-F.; Zhang, X.; Zhu, Q.; Dong, H.; Zhao, M.; Oganov, A. R. Phagraphene: A Low-Energy Graphene Allotrope Composed of 5–6–7 Carbon Rings with Distorted Dirac Cones. Nano Lett. 2015, 15, 6182–6186.DOI
  13. [13]Li, X.; Wang, Q.; Jena, P. ψ-Graphene: A New Metallic Allotrope of Planar Carbon with Potential Applications as Anode Materials for Lithium-Ion Batteries. J. Phys. Chem. Lett. 2017, 8, 3234–3241.DOI
  14. [14]Fan, Q.; Yan, L.; Tripp, M. W.; Krejčí, O.; Dimosthenous, S.; Kachel, S. R.; Chen, M.; Foster, A. S.; Koert, U.; Liljeroth, P.; Gottfried, J. M. Biphenylene network: A nonbenzenoid carbon allotrope. Science 2021, 372, 852–856.DOI
  15. [15]Hou, L.; Cui, X.; Guan, B.; Wang, S.; Li, R.; Liu, Y.; Zhu, D.; Zheng, J. Synthesis of a monolayer fullerene network. Nature 2022, 606, 507–510.DOI
  16. [16]Lu, H.; Li, S.-D. Two-dimensional carbon allotropes from graphene to graphyne. J. Mater. Chem. C 2013, 1, 3677–3680.DOI
  17. [17]Pereira Júnior, M.; da Cunha, W.; Giozza, W.; de Sousa Junior, R.; Ribeiro Junior, L. Irida-graphene: A new 2D carbon allotrope. FlatChem 2023, 37, 100469.DOI
  18. [18]Tan, Y.; Tao, X.; Ouyang, Y.; Peng, Q. Stable and 7.7 wt% hydrogen storage capacity of Ti decorated Irida-Graphene from first-principles calculations. Int. J. Hydrogen Energy 2024, 50, 738–748.DOI
  19. [19]Bhat, C. P.; Bandyopadhyay, D. Insights into the reversible hydrogen storage mechanism of transition metal-decorated Irida-graphene: A DFT study. Int. J. Hydrogen Energy 2025, 137, 750–761.DOI
  20. [20]Yuan, L.; Shi, M.; Su, J.; Wang, D.; Zhang, H.; Gong, J.; Ma, J. First-principles investigation of Irida-graphene decorated with alkali metal for reversible hydrogen storage. Comput. Theor. Chem. 2024, 1239, 114756.DOI
  21. [21]Zhang, Y.-F.; Guo, J. Li-decorated 2D Irida-graphene as a potential hydrogen storage material: A dispersion-corrected density functional theory calculations. Int. J. Hydrogen Energy 2024, 50, 1004–1014.DOI
  22. [22]Sun, Y.; Chen, Y.; Yang, M.; Zhou, K.; Sun, J.; Zhao, K.; Xu, L. First-principles study of the hydrogen storage properties of Irida-graphene. Phys. Chem. Chem. Phys. 2025, 27, 915–929.DOI
  23. [23]Duan, Z.; Shi, S.; Yao, C.; Liu, X.; Diao, K.; Lei, D.; Liu, Y. Reversible hydrogen storage with Na-modified Irida-Graphene: A density functional theory study. Int. J. Hydrogen Energy 2024, 85, 1–11.DOI
  24. [24]Zhang, Y.; Liu, Z.; Guo, J.; Cao, Z.; Wang, J. Ca-decorated 2D Irida-graphene as a promising hydrogen storage material: A combination of DFT and AIMD study. Int. J. Hydrogen Energy 2024, 91, 118–126.DOI
  25. [25]Xiong, X.; Cao, H.-B.; Lu, Z.; Liu, C.-S.; Ye, X.-J. Theoretical prediction on Irida-graphene monolayer as promising anode material for lithium-ion batteries. Comput. Mater. Sci. 2024, 244, 113225.DOI
  26. [26]Martins, N. F.; Laranjeira, J. A.; Fabris, G. S.; Denis, P. A.; Sambrano, J. R. Irida-graphene as a high-performance anode for sodium batteries. J. Energy Storage 2024, 104, 114637.DOI
  27. [27]Kaur, M.; Duhan, N.; Dhilip Kumar, T. Irida-graphene: A new two-dimensional electrode material for sodium-ion batteries. J. Energy Storage 2024, 104, 114456.DOI
  28. [28]Wei, Y.; Zhang, X.; Fu, G.; Yang, B.; Zhang, L. C₆₃: A promising alkali-ion battery anode material. Diam. Relat. Mater. 2024, 148, 111528.DOI
  29. [29]Rusho, M. A.; Ahmed, A. T.; Jasim, A. S.; Kanjariva, P.; Rajiv, A.; Shankhyan, A.; Bhakuni, P. N.; Elshafie, H. A new type of two-dimensional carbon-based monolayers namely irida-graphene as an anode material for magnesium-ion batteries. J. Mol. Graph. Model. 2025, 135, 108934.DOI
  30. [30]Martins, N. F.; Abdullah, Y. Z.; Laranjeira, J. A.; Sambrano, J. R. Exploring Irida-graphene as an efficient anchoring material for lithium-sulfur batteries: A DFT study. Surf. Interfaces 2025, 72, 107193.DOI
  31. [31]Rodrigues, H. X.; Silva, I. A.; Ribeiro Jr., L. A.; Pereira Jr., M. L.; Siqueira, L. J. A. Irida-Silicene as promising electrode material for supercapacitors. A comparative study by means of molecular dynamics. J. Energy Storage 2026, 154, 121121.DOI
  32. [32]Li, J.; Han, M.; Zhao, S.; Li, T.; Yu, T.; Zhang, Y.; Tang, H.-K.; Peng, Q. Mechanics and Crack Analysis of Irida Graphene Bilayer Composite: A Molecular Dynamics Study. J. Compos. Sci. 2023, 7, 490.DOI
  33. [33]Felix, I. M.; Tromer, R. M.; Machado, L. D.; Galvão, D. S.; Ribeiro, L. A.; Pereira, M. L. Irida-graphene phonon thermal transport via non-equilibrium molecular dynamics simulations. Nanoscale 2024, 16, 16430–16438.DOI
  34. [34]Majidi, R. Irida-graphyne: A promising material for optoelectronic applications. Mater. Today Commun. 2024, 38, 107641. Majidi, R.; Ayesh, A. I. Twin Irida Graphene: A Carbon Material with Optoelectronic Features. Adv. Theory Simul. 2024, 7, 2400131.DOI
  35. [36]Felix, I. M.; de Oliveira, R. B.; Ribeiro, L. A.; Galvão, D. S.; Pereira, M. L.; Tromer, R. M. 3D Carbon Nanostructures Derived from 2D Irida-Graphene: Insights into Structural, Mechanical, Electronic, and Optical Properties. ACS Omega 2025, 10, 38985–38994.DOI
  36. [37]Pereira, M. L.; da S. Gomes, D.; Lima, K. A. L.; Nze, G. D. A.; Mendonça, F. L. L.; Ribeiro, L. A. Two-dimensional boron nitride allotrope Irida-B₁₂N₁₂ with 3-6-8 membered rings and wide-bandgap semiconducting properties. Sci. Rep. 2024, 14, 28892.DOI
  37. [38]Gomes, D. d. S.; Ribeiro, L. A.; Pereira, M. L. Predicting Irida-Silicene: A Novel 2D Silicon Allotrope. ACS Omega 2024, 9, 50570–50578.DOI
  38. [40]Sofo, J. O.; Chaudhari, A. S.; Barber, G. D. Graphene: A two-dimensional hydrocarbon. Phys. Rev. B 2007, 75, 153401.
  39. [41]Elias, D. C.; Nair, R. R.; Mohiuddin, T. M. G.; Morozov, S. V.; Blake, P.; Halsall, M. P.; Ferrari, A. C.; Boukhvalov, D. W.; Katsnelson, M. I.; Geim, A. K.; Novoselov, K. S. Control of Graphene’s Properties by Reversible Hydrogenation: Evidence for Graphane. Science 2009, 323, 610–613.DOI
  40. [42]Lebègue, S.; Klintenberg, M.; Eriksson, O.; Katsnelson, M. I. Accurate electronic band gap of pure and functionalized graphene from GW calculations. Phys. Rev. B 2009, 79, 245117.DOI
  41. [43]Nair, R. R. et al. Fluorographene: A Two-Dimensional Counterpart of Teflon. Small 2010, 6, 2877–2884.DOI
  42. [44]Li, X.; Zhang, S.; Wang, F. Q.; Guo, Y.; Liu, J.; Wang, Q. Tuning the electronic and mechanical properties of pentagraphene via hydrogenation and fluorination. Phys. Chem. Chem. Phys. 2016, 18, 14191–14197.DOI
  43. [45]Demirci, S.; Gorkan, T.; Çallıoğlu, Ş.; Özçelik, V. O.; Barth, J. V.; Aktürk, E.; Ciraci, S. Hydrogenated Carbon Monolayer in Biphenylene Network Offers a Potential Paradigm for Nanoelectronic Devices. J. Phys. Chem. C 2022, 126, 15491–15500.DOI
  44. [46]Huang, X.; Ma, M.; Cheng, L.; Liu, L. Hydrogenated ψ-graphene: Band gap engineering and optical properties. Phys. E: Low-Dimens. Syst. Nanostruct. 2020, 115, 113701.DOI
  45. [47]Soler, J. M.; Artacho, E.; Gale, J. D.; García, A.; Junquera, J.; Ordejón, P.; Sánchez-Portal, D. The SIESTA method for ab initio order-N materials simulation. J. Phys.: Condens. Matter 2002, 14, 2745–2779.DOI
  46. [48]García, A. et al. SIESTA: Recent developments and applications. J. Chem. Phys. 2020, 152, 204108.
  47. [49]Kohn, W.; Sham, L. J. Self-Consistent Equations Including Exchange and Correlation Effects. Phys. Rev. 1965, 140, A1133–A1138.DOI
  48. [50]Sánchez-Portal, D.; Ordejón, P.; Artacho, E.; Soler, J. M. Density-functional method for very large systems with LCAO basis sets. Int. J. Quantum Chem. 1997, 65, 453–461.
  49. [51]Perdew, J. P.; Burke, K.; Ernzerhof, M. Generalized Gradient Approximation Made Simple. Phys. Rev. Lett. 1996, 77, 3865–3868.pubmed.ncbi.nlm.nih.gov/10062328
  50. [52]Heyd, J.; Scuseria, G. E.; Ernzerhof, M. Hybrid functionals based on a screened Coulomb potential. J. Chem. Phys. 2003, 118, 8207–8215.DOI
  51. [53]Qin, X.; Shang, H.; Xiang, H.; Li, Z.; Yang, J. HONPAS: A linear scaling open-source solution for large system simulations. Int. J. Quantum Chem. 2015, 115, 647–655.DOI
  52. [54]Shang, H.; Xu, L.; Wu, B.; Qin, X.; Zhang, Y.; Yang, J. The dynamic parallel distribution algorithm for hybrid density-functional calculations in HONPAS package. Comput. Phys. Commun. 2020, 254, 107204.DOI
  53. [55]Troullier, N.; Martins, J. L. Efficient pseudopotentials for plane-wave calculations. Phys. Rev. B 1991, 43, 1993–2006.pubmed.ncbi.nlm.nih.gov/9997467
  54. [56]Kleinman, L.; Bylander, D. M. Efficacious Form for Model Pseudopotentials. Phys. Rev. Lett. 1982, 48, 1425–1428.DOI
  55. [57]Monkhorst, H. J.; Pack, J. D. Special points for Brillouin-zone integrations. Phys. Rev. B 1976, 13, 5188–5192.DOI
  56. [58]Nosé, S. A unified formulation of the constant temperature molecular dynamics methods. J. Chem. Phys. 1984, 81, 511–519.DOI
  57. [59]Hoover, W. G. Canonical dynamics: Equilibrium phase-space distributions. Phys. Rev. A 1985, 31, 1695–1697.pubmed.ncbi.nlm.nih.gov/9895674
  58. [60]Tromer, R. M.; Freitas, A.; Felix, I. M.; Mortazavi, B.; Machado, L.; Azevedo, S.; Pereira, L. F. C. Electronic, optical and thermoelectric properties of boron-doped nitrogenated holey graphene. Phys. Chem. Chem. Phys. 2020, 22, 21147–21157.DOI
  59. [61]Montes, E.; Schwingenschlögl, U. Nanotubes based on monolayer blue phosphorus. Phys. Rev. B 2016, 94, 035412.DOI
  60. [62]Silva, D.; Azevedo, S.; Kaschny, J. Structural and electronic properties of fluorinated boron nitride monolayers. Eur. Phys. J. B 2021, 94, 1–11.
  61. [63]Straumanis, M. E.; Aka, E. Z. Precision Determination of Lattice Parameter, Coefficient of Thermal Expansion and Atomic Weight of Carbon in Diamond. J. Am. Chem. Soc. 1951, 73, 5643–5646.
  62. [64]Gauss, J.; Cremer, D.; Stanton, J. F. The rₑ Structure of Cyclopropane. J. Phys. Chem. A 2000, 104, 1319–1324.
  63. [65]Leenaerts, O.; Peelaers, H.; Hernández-Nieves, A. D.; Partoens, B.; Peeters, F. M. First-principles investigation of graphene fluoride and graphane. Phys. Rev. B 2010, 82, 195436.DOI
  64. [66]Peelaers, H.; Hernández-Nieves, A. D.; Leenaerts, O.; Partoens, B.; Peeters, F. M. Vibrational properties of graphene fluoride and graphane. Appl. Phys. Lett. 2011, 98, 051914.
  65. [67]Özçelik, V. O.; Ciraci, S. Size Dependence in the Stabilities and Electronic Properties of α-Graphyne and Its Boron Nitride Analogue. J. Phys. Chem. C 2013, 117, 2175–2182.
  66. [68]Topsakal, M.; Cahangirov, S.; Ciraci, S. The response of mechanical and electronic properties of graphene to the elastic strain. Appl. Phys. Lett. 2010, 96, 091912.DOI
  67. [69]Majidi, R. Mechanical properties of novel forms of graphyne under strain: A density functional theory study. Phys. E: Low-Dimens. Syst. Nanostruct. 2017, 90, 189–193.DOI
  68. [70]Asadpour, M.; Malakpour, S.; Faghihnasiri, M.; Taghipour, B. Mechanical properties of two-dimensional graphyne sheet, analogous system of BN sheet and graphyne-like BN sheet. Solid State Commun. 2015, 212, 46–52.
  69. [71]Cadelano, E.; Palla, P. L.; Giordano, S.; Colombo, L. Elastic properties of hydrogenated graphene. Phys. Rev. B 2010, 82, 235414.DOI
  70. [72]Kang, J.; Li, J.; Wu, F.; Li, S. S.; Xia, J. B. Elastic, electronic, and optical properties of two-dimensional graphyne sheet. J. Phys. Chem. C 2011, 115, 20466–20470.DOI
  71. [73]Karlický, F.; Zbořil, R.; Otyepka, M. Band gaps and structural properties of graphene halides and their derivatives: A hybrid functional study with localized orbital basis sets. J. Chem. Phys. 2012, 137, 034709.DOI
  72. [74]Heyd, J.; Peralta, J. E.; Scuseria, G. E.; Martin, R. L. Energy band gaps and lattice parameters evaluated with the Heyd-Scuseria-Ernzerhof screened hybrid functional. J. Chem. Phys. 2005, 123, 174101.pubmed.ncbi.nlm.nih.gov/16375511
  73. [75]Krukau, A. V.; Vydrov, O. A.; Izmaylov, A. F.; Scuseria, G. E. Influence of the exchange screening parameter on the performance of screened hybrid functionals. J. Chem. Phys. 2006, 125, 224106.pubmed.ncbi.nlm.nih.gov/17176133
  74. [76]Tignon, J.; Voisin, P.; Delalande, C.; Voos, M.; Houdré, R.; Oesterle, U.; Stanley, R. From Fermi’s golden rule to the vacuum Rabi splitting: Magnetopolaritons in a semiconductor optical microcavity. Phys. Rev. Lett. 1995, 74, 3967.pubmed.ncbi.nlm.nih.gov/10058379
  75. [77]Kramers, H. A. La diffusion de la lumiere par les atomes. Atti del Congresso Internazionale dei Fisici. Como, Italy, 1927; pp 1–13.
  76. [78]Kronig, R. d. L. On the theory of dispersion of X-rays. J. Opt. Soc. Am. 1926, 12, 547–557.

Paper details

vlnc:W_jcartnkh
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 1

downloads · 2

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents