Investigation of the timing performance of double-sided pp-type 3D silicon sensors produced by CNM

Abstract

We investigate the timing performance and spatial uniformity of double-sided pp-type 3D silicon sensors produced by the Centro Nacional de Microelectrónica (CNM). Three sensor layouts are studied: hexagonal and square geometries with an inter-electrode spacing of \SI{30}{\micro\meter}, and a hexagonal geometry with an inter-electrode spacing of \SI{50}{\micro\meter}. The sensors are characterized using a \SI{1064}{\nano\meter} infrared laser and a custom two-stage wide-band readout. Measurements with a 90^{90}Sr source are used to establish a minimum-ionizing-particle-like reference for the laser signal. The timing resolution improves with increasing bias voltage for all three layouts. Two-dimensional laser scans are used to study the position dependence of the timing response and to quantify its uniformity. Among the investigated devices, the square \SI{30}{\micro\meter} geometry shows the best overall timing performance at the highest measured bias voltage.

Prepared for submission to JINST

Introduction

The High-Luminosity Large Hadron Collider (HL-LHC) will operate under challenging conditions, with a nominal bunch-crossing frequency of 40 MHz and up to approximately 200 proton–proton interactions per bunch crossing. The high pileup environment presents significant challenges for event reconstruction, while the accumulated radiation exposure requires silicon tracking detectors to exhibit high radiation hardness. Although precise timing information is not a baseline requirement for the inner tracking detectors, it could provide additional benefits for pileup mitigation and event reconstruction. Therefore, radiation-tolerant silicon sensors with fast timing capabilities are of interest for future tracking applications.

Low Gain Avalanche Detectors (LGADs) [1, 2, 3] can achieve timing resolutions below 50 ps, but their performance degrades under irradiation due to damage to the gain layer, despite mitigation techniques such as carbon co-implantation [4].

3D silicon detectors offer an alternative [5] by decoupling the electrode spacing from the sensor thickness, providing excellent radiation hardness. Their short inter-electrode distance also enables fast charge collection. These devices can operate at fluences beyond Φeq=1×1016 cm−2\Phi_{\mathrm{eq}} = 1 \times10^{16}\ \mathrm{cm}^{-2} and have demonstrated promising timing performance [6].

In this work, we investigate the timing performance and spatial uniformity of double-sided pp-type 3D silicon sensors using a 90Sr{}^{90}\mathrm{Sr} source and a 1064 nm infrared laser. Three layouts with different electrode geometries and inter-electrode spacings are compared to evaluate how these design parameters influence the timing response and its spatial uniformity.

Sensors

The investigated sensors were manufactured by the Centro Nacional de Microelectrónica (CNM) [7] using a double-sided 3D fabrication process. Unlike single-sided 3D sensors, in which both electrode types are etched from the same surface, the n+n^{+} and p+p^{+} electrode columns are etched from opposite sides of the pp-type silicon substrate, as illustrated in Figure 1(a). The sensors have a thickness of approximately 230 μm\mu\mathrm{m}, with column depths of approximately 210 μm\mu\mathrm{m}. Further details of the fabrication process can be found in Ref. [7].

Schematic and optical images of the investigated double-sided 3D silicon sensors

Figure 1. (a) Schematic of the double-sided 3D sensor. (b) Hexagonal, 30 μm\mu\mathrm{m}. (c) Square, 30 μm\mu\mathrm{m}. (d) Hexagonal, 50 μm\mu\mathrm{m}.

Figure 1: Schematic illustration and optical images of the investigated double-sided 3D silicon sensors. (a) Cross-sectional structure and electrode arrangements. (b)–(d) Optical images of the three electrode geometries, with red boxes indicating the laser-scanned regions.

The electrode geometry and inter-electrode spacing influence the electric-field distribution and charge-collection characteristics, which may affect the timing response and its spatial uniformity. To investigate these effects, three layouts are compared: a hexagonal geometry with 30 μm\mu\mathrm{m} inter-electrode spacing, a square geometry with 30 μm\mu\mathrm{m} spacing, and a hexagonal geometry with 50 μm\mu\mathrm{m} spacing. Optical images of the three layouts are shown in Figure 1, with red boxes indicating the laser-scanned regions.

Experimental setup and readout

The transient response of the sensors was studied at room temperature using a 90Sr{}^{90}\mathrm{Sr} source to establish a MIP-like reference signal [8], followed by measurements with a 1064 nm infrared laser focused to a spot of approximately 2 μm×2 μm\mu\mathrm{m}\times2\,\mu\mathrm{m} [9]. A custom two-stage wide-band front-end was used to record the fast detector signal. The readout and biasing scheme is shown in Figure 2(a). Further details of the readout and timing measurements can be found in Ref. [8].

Readout and biasing scheme and measured leakage current

Figure 2. (a) Readout and biasing scheme. (b) Measured leakage current.

Figure 2: Readout system and electrical behavior of the investigated sensors.

The detector bias is supplied through two 1 MΩ\Omega series resistors, as shown in the biasing circuit for the 3D sensors (Figure 2(a)). Consequently, the voltage drop produced by the detector leakage current must be taken into account when determining the effective sensor bias. Figure 2(b) shows the measured leakage current as a function of applied voltage for the three sensor layouts, which is used to correct the bias voltage.

Laser calibration and timing measurements

Laser calibration and timing measurements

The example calibration distributions, laser timing distributions, and spatial timing-resolution maps were obtained at an applied voltage of 50 V (corresponding to an effective sensor bias of approximately 40 V after correcting for leakage-current voltage drops). The 90Sr{}^{90}\mathrm{Sr} measurement was used to obtain a MIP-like reference signal. Approximately 10410^{4} waveforms were recorded using an 8 GHz LeCroy WavePro 804HD oscilloscope. For each event, the waveform was integrated within ±2\pm2 ns around the pulse minimum. The resulting distribution was fitted with a Gaussian function for the electronic-noise component and a Landau distribution for the β\beta-particle signal [10]. The most probable value (MPV) of the Landau distribution was used as the reference for calibrating the laser intensity. Representative 90Sr{}^{90}\mathrm{Sr} waveforms and the corresponding integrated-signal distribution for the square 30 µm sensor are shown in Figure 3. Because the trigger threshold affects the low-amplitude part of the Landau distribution, the laser intensity was conservatively adjusted to a mean integrated signal approximately 15 % below the 90Sr{}^{90}\mathrm{Sr} Landau MPV. The resulting timing resolution therefore provides a conservative estimate for a MIP-like signal.

Representative 90Sr waveforms

(a) Representative 90Sr{}^{90}\mathrm{Sr} waveforms.

(b) Gaussian and Landau fit.

Figure 3. 90Sr{}^{90}\mathrm{Sr} calibration used to define the MIP-like reference signal.

Figure 4 illustrates the laser-signal calibration and timing-resolution extraction. For each recorded laser waveform, the signal was integrated within the same time window used for the 90Sr{}^{90}\mathrm{Sr} analysis. The resulting integrated-signal distribution was fitted with a Gaussian function, as shown in Figure 4(a). The fitted mean was used to set the laser intensity relative to the 90Sr{}^{90}\mathrm{Sr} reference. For the timing analysis, the threshold-crossing time was extracted from the leading edge of each waveform at 40 % of its pulse amplitude. The crossing-time distribution was fitted with a Gaussian function, as shown in Figure 4(b). The fitted width σ\sigma was taken as the timing resolution.

Laser-signal calibration and timing-resolution extraction

Figure 4. Laser-signal calibration and timing-resolution extraction. (a) Integrated laser-signal distribution with Gaussian fit; the fitted mean is used for calibration to the 90Sr{}^{90}\mathrm{Sr} reference. (b) Threshold-crossing-time distribution with Gaussian fit; the fitted width σ\sigma defines the measured timing resolution.

Figure 5 compares the final position-dependent timing-resolution maps for the square 30 µm and hexagonal 50 µm sensors. The scan steps were 5 µm and 10 µm, respectively. The measured timing resolution is indicated at each laser-scan position, illustrating the spatial variation within the sensor cells.

Position-dependent timing-resolution maps for square and hexagonal sensors

Figure 5. Position-dependent timing-resolution maps measured with the infrared laser for (a) the square 30 μ\mum sensor and (b) the hexagonal 50 μ\mum sensor. The numerical values indicate the timing resolution at the scanned positions.

To compare the three layouts, the timing resolution was averaged over the measured scan positions. The resulting mean timing resolution is shown as a function of bias voltage in Figure 6(a). All three layouts improve with increasing bias voltage. The hexagonal 50 µm sensor shows a particularly strong improvement between the lowest bias points, while the two 30 µm layouts provide better timing at low bias. At the highest measured bias, the square 30 μ\mum sensor reaches the best average timing resolution, below 50 ps.

Figure 6. (a) Mean timing resolution. (b) Relative spatial spread Δσ/σˉ\Delta\sigma/\bar{\sigma}. Summary of the timing performance as a function of bias voltage for investigated sensors.

The spatial uniformity is quantified by the relative spread U=Δσ/σˉU = \Delta\sigma/\bar{\sigma}, where σˉ\bar{\sigma} is the mean timing resolution over the scan and Δσ\Delta\sigma is the standard deviation of the position-dependent timing-resolution values. As shown in Figure 6(b), the two 30 μ\mum layouts remain at approximately U≃0.17U \simeq0.17–0.200.20 over the measured bias range. The hexagonal 50 μ\mum geometry is substantially less uniform at the lowest bias, but its uniformity improves rapidly with increasing voltage and becomes comparable to, or better than, the 30 μ\mum layouts at the highest measured bias. This comparison may be partly influenced by the coarser 10 μ\mum scan step used for the hexagonal 50 μ\mum geometry.

Conclusion

The timing performance and spatial uniformity of three double-sided pp-type 3D silicon sensor layouts produced by CNM were investigated using a 1064 nm infrared laser. A 90Sr{}^{90}\mathrm{Sr} source was used to calibrate the laser signal to a MIP-like reference.

The timing resolution improves with increasing bias voltage for all three geometries. The hexagonal 50 μ\mum sensor shows the strongest bias dependence, while at the highest measured bias the square 30 μ\mum geometry provides the best average timing resolution, below 50 ps. Due to the uncertainty associated with the Landau tail in the 90Sr{}^{90}\mathrm{Sr} calibration, the infrared-laser signal used in this measurement was set approximately 15 % below the 90Sr{}^{90}\mathrm{Sr} reference signal. A timing resolution of approximately 30 ps was obtained in our previous measurement [9] using a laser signal approximately 15 % larger.

The spatial laser scans show a clear position dependence of the timing response within the 3D cell. The relative spread of the local timing resolution is approximately 0.17–0.20 for the 30 μ\mum layouts over the measured bias range. The 50 μ\mum hexagonal geometry shows substantially larger non-uniformity at low bias, which decreases with increasing bias voltage.

References

  1. [1]H. F.-W. Sadrozinski et al., Nucl. Instrum. Meth. A 730 (2013) 226–231.
  2. [2]N. Cartiglia et al., Nucl. Instrum. Meth. A 796 (2015) 141–148.
  3. [3]G. Pellegrini et al., Nucl. Instrum. Meth. A 765 (2014) 12–16.
  4. [4]G. Kramberger et al., JINST 10 (2015) P07006.
  5. [5]S. I. Parker and C. J. Kenney, Nucl. Instrum. Meth. A 395 (1997) 328–343.
  6. [6]C. Betancourt et al., Sensors 19 (2019) 2041.
  7. [7]G. Pellegrini et al., Nucl. Instrum. Meth. A 699 (2013) 27–30.
  8. [8]C. Liao et al., 3rd DRD3 Week on Solid State Detectors R&D, Nikhef, Amsterdam, (2025).
  9. [9]C. Liao et al., 5th DRD3 Week on Solid State Detectors R&D, Bucharest, Romania (2026).
  10. [10]L. Landau, J. Phys. (USSR) 8 (1944) 201–205.

Paper details

vlnc:W_je9qu9ns
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC0-1.0
Usage

views · 10

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents