betaFeedback

WorksPhysics and Astronomy

Fast Fabrication of WS2/Bi2Se3 Heterostructures for High Performance Photodetection

Abstract

Two-dimensional (2D) material heterostructures have attracted considerable attention owing to their interesting and novel physical properties, which expand the possibilities for future optoelectronic, photovoltaic, and nanoelectronic applications. A portable, fast, and deterministic transfer technique is highly needed for the fabrication of heterostructures. Herein, we report a fast half wet poly(dimethylsiloxane) (PDMS) transfer process utilizing the change of adhesion energy with the help of micron-sized water droplets. Using this method, a vertical stacking of the WS2/Bi2Se3 heterostructure with a straddling band configuration is successfully assembled on a fluorophlogopite substrate. Thanks to the complementary band gaps and high efficiency of interfacial charge transfer, the photodetector based on the heterostructure exhibits a superior responsivity of 109.9 A/W for a visible incident light at 473 nm and 26.7 A/W for a 1064 nm near-infrared illumination. Such high photoresponsivity of the heterostructure demonstrates that our transfer method not only owns time efficiency but also ensures high quality of the heterointerface. Our study may open new pathways to the fast and massive fabrication of various vertical 2D heterostructures for applications in twistronics/valleytronics and other band engineering devices.

Introduction

Van der Waals (vdW) heterostructures based on vertically stacked two-dimensional (2D) materials have been widely studied owing to their synergistic role that improving the functional characteristics.[1, 2] New functionalities can arise from the interface between dissimilar 2D materials, or from the differences of their electronic structures, lattice constants and Young’s modulus, creating quantum wells, twisted superlattices, strong light-matter interaction and superior optoelectronic properties.[3, 4, 5, 6]

There have been extensive reports on methods of producing 2D heterostructures, which can be divided into two directions: in situ direct growth and multistep mechanical transfer.

In situ direct growth means direct growth of different layers sequentially. The general techniques, such as molecular beam epitaxy (MBE), physical vapor deposition (PVD), pulsed laser deposition (PLD), and chemical vapor deposition (CVD) for monolayer growth, can be slightly modified to realize the direct fabrication of heterostructures. [7, 8, 9, 10] MBE potentially allows precise control over elemental deposition rates and easy switching from one material to another, enabling the fabrication of the heterostructures on wafer-scales. Several kinds of heterostructures have been reported, like MoTe2_2/MoS2_2, MoSe2_2/HfSe2_2 and Bi2_2Se3_3/graphene, via one-step growth or in situ growth on the bottom material. [11, 12, 13, 14] PVD offers many advantages such as selective and large-area growth, high growth rate and low cost. WS2_2/MoS2_2 heterojunction can be assembled via reactive sputtering deposition (RSD), which is one type of PVD. [9] Moreover, PLD is also a type of PVD methods, which is precursor free and provides controllable growth rate and sample thickness via changing the energy fluence of the pulsed laser. A few reports demonstrate this large-area growth technology, WS2_2/Bi2_2Te3_3 heterostructure and WS2_2/WSe2_2/WS2_2 tri-layer heterostructure have been fabricated and demonstrate great performance in photodetection and quantum well, respectively. [8, 15] CVD is an efficient and scalable method in the preparation of monolayer and bilayer 2D materials, which is also an alternative choice for the fabrication of heterostructures. [16] Gong et al. achieved direct growth of MoS2_2/WS2_2 heterostructures on SiO2_2/Si substrate. [7] Several other van der Waals heterostructures, such as MoS2_2/WSe2_2, MoS2_2/CdS, WSe2_2/SnS2_2 have been successfully synthesized by the CVD method. [17, 18, 19] Although in situ growth technology has plenty of advantages, like large scale, considerable productivity and low cost, it is still confronted with certain challenges. Firstly, the constructure of the heterostructures, like the twist angle between two layers, is fixed by the self-assembly process. [10] Furthermore, the random position growth leads to low reproducibility. Secondly, it is hard to satisfy the growth conditions of the two target materials simultaneously, such as growth temperature and gas atmosphere, which limits the categories of heterostructures that in situ direct growth can achieve. [20]

As a result, traditional mechanical transfer methods still have irreplaceable advantages. The pick-drop process has almost no restrictions on the categories of the target samples. In some degree, every two types of thin film materials could be combined and form a heterostructure. Moreover, this technique provides controllable precise stacking alignment, which makes nearzero twisted heterostructures possible.[4] One of the most commonly reported methods is the polymethylmethacrylate (PMMA) film based wet transfer, which uses a PMMA film spin-coated on substrates as an adhesion layer and support.[21] Utilizing the contrast between hydrophilic and hydrophobic of PMMA and growth substrate or using corrosive solvent (like NaOH or HF aqueous solution) to separate substrates and PMMA adhered with target material. The whole PMMA film can be placed onto another target substrate and after dissolving PMMA, the target material remains on the substrate and the transfer finishes.[22] However, the PMMA is hard to be dissolved completely and the residue remaining on the sample degrades its device performance and limits its potential applications. Moreover, the wrinkling of the PMMA film cannot be avoided, which makes precise placement challenging and brings unwanted deformation of the sample. Another general method via the viscosity of polydimethylsiloxane (PDMS) can easily pick up mechanically exfoliated flakes and release the flakes by stronger van der Waals force between flakes and the bottom substrate or sample.[23] Nevertheless, it’s hard for PDMS to pick up samples grown by CVD because of the robust adhesion between samples and the rigid grown substrate. Other effective transfer methods have been reported such as using a polypropylene carbonate (PPC) coated PDMS block as the transfer support or polymer support/Graphene/target substrate roll-to roll transfer.[24, 25] These methods either involve residues or have difficulty on picking up CVD grown flakes. Due to current status, there is still urgent need to develop a clean, fast and easy aligning transfer method to fabrication of vdW heterostructures exploiting the massively CVD grown materials.

Herein, we report a fast half-wet PDMS transfer method that utilizes the change of adhesion energy with the help of hot water vapor and compare the complexity of different grown substrates. In previous reports, X. Ma et al. explored the assisted effect of capillary force induced by water vapor and successfully transferred graphene and MoS2_2 domains grown on SiO2_2/Si wafer. But they didn’t explore the applicability of this method in other substrate, such as sapphire and mica. Also, it lacks fine control of material placement in an in situ manner and more precise transfer manipulation is needed for large scale monolayer.[26] Lee et al. achieved high quality graphene transfer from an Al2_2O3_3 substrate via deionized (DI) water, while Y. Hou et al. utilized similar method to fabricate twisted bilayer graphene.[27, 28] However, they both focused on mechanical exfoliated graphene and a pretreated step was needed, while samples grown by CVD were still neglected. S. Dong et al. expanded the transfer method to transition metal dichalcogenides (TMD) grown by CVD via assistance of hot DI water, which was induced by pipette or directly dipping PDMS/sample in water.[29] In this process, plenty of water was needed, resulting in long time to dry PDMS and large area of monolayer was unable to be transferred because of the wrinkles caused by water. J. Cai et al. also used trapezoid PDMS and water droplets to transfer WS2_2 flakes, while the size of the transferred flakes was limited to a few microns.[30] Compared to previously reported methods, our method not only combines their advantages, but also explores the applicability to different substrates (such as sapphire and mica) and realizes the transfer of large-area single monolayer flakes. With the assistance of micro sized water droplets instead of spraying or immersion in water, PDMS can be switched from wet to dry in seconds, which promotes the efficiency of transfer and maintaining the original flatness of large monolayer. The whole transfer process can be accompanished in a few minutes.

Furthermore, we fabricate a WS2_2/Bi2_2Se3_3 heterostructure for photodetection via our new method and CVD/PVD grown flakes. The heterostructure with a type-I band alignment shows an excellent photodetection performance from visible to near-infrared illumination. The response parameters of the resultant device are superior to that of the previous reports. For example, the responsivity of our device is 74.5 AW−1^{-1} at visible 532 nm light illumination, which is 10310^3 higher than MoS2_2/WS2_2 heterostructure, while the responsivity at near-infrared 1064 nm is nearly 2.7×1042.7 \times10^4 higher than WS2_2/Bi2_2O2_2Se device.[10, 31] Besides, the on/off ratio of 1.06×1061.06 \times10^6 and 7.2×1047.2 \times10^4 at 473 nm and 1064 nm respectively, is 1.7×1031.7 \times10^3 higher than that of reported WSe2_2/Bi2_2O2_2Se structure.[32] The response speed at visible illumination of our device is 18 times faster than previous WS2_2/Bi2_2Se3_3 heterostructure grown by PVD.[33] such outstanding performance manifests that our methodology has potential applications in fast and massive fabrications for high quality functional heterostructure devices and twistronics/valleytronics.

Results and discussion

Fast half-wet transfer process

The heterostructure is assembled by a fast half-wet transfer process as mentioned above. The basic procedure of the transfer process is illustrated in Figure 1. The setup is developed consisting of a glass slide mounted on a micromanipulator, a bottom stage with translation capability and an optical microscope for visualization. First, a small piece of PDMS is cut and stuck onto a glass slide for adhesion and support. A flask filled with hot water (80 °C) is placed below PDMS and kept for about 10 seconds. The hot vapor condenses on PDMS and forms micro droplets. Then fresh monolayer WS2\mathrm{WS}_{2} grown on a sapphire substrate is moved to the bottom of PDMS by the translation stage and a suitable WS2\mathrm{WS}_{2} sample is selected by the microscope. After achieving contact between PDMS and the sapphire by lifting off the glass slide, the droplets penetrate into the interface and decrease the adhesion energy of WS2\mathrm{WS}_{2} on the sapphire, which make it easier for PDMS to pick WS2\mathrm{WS}_{2} up. The PDMS moves up with picked WS2\mathrm{WS}_{2}, the sapphire is replaced by the target mica with PVD grown Bi2Se3\mathrm{Bi}_{2}\mathrm{Se}_{3} flakes. By employing the microscope imaging and 3-axis micromanipulator stage, monolayer WS2\mathrm{WS}_{2} is moved to the aligned location and dropped onto the Bi2Se3\mathrm{Bi}_{2}\mathrm{Se}_{3} slowly and softly. Finally, by careful manipulation through the zz-motion of the glass slide-carrying stage, PDMS is peeled off from the mica and monolayer WS2\mathrm{WS}_{2} remains on Bi2Se3\mathrm{Bi}_{2}\mathrm{Se}_{3} because of van der Waals attracting force. The optical images of the corresponding transfer steps are shown in Figure S1 and S2. In order to tightly combine these two materials, the heterostructure is put into the glove box and annealed at 150 °C for 30 minutes. The final fabrication of WS2\mathrm{WS}_{2}/Bi2Se3\mathrm{Bi}_{2}\mathrm{Se}_{3} heterostructure device is completed via standard electron-beam lithography, with the 5/75 nm Cr/Au electrodes deposited by thermal evaporation.

Schematic diagram of the transfer and construction processes of WS$_2$/Bi$_2$Se$_3$ heterostructure

Figure 1. Schematic diagram of the transfer and construction processes of WS2_2/Bi2_2Se3_3 heterostructure, inset: optical image of the fabricated heterostructure (scale bar 10 μ\mum).

Optical images of the half-wet transfer process and photodetection device

Figure S1. Optical image of half-wet transfer process from SiO2_2/Si to mica. (a) Monolayer WS2_2 grown on SiO2_2/Si. (b) The water droplets liquified on PDMS from hot DI water vapour. (c) WS2_2 lifted on PDMS. (d) The WS2_2/Bi2_2Se3_3 heterostructure. (e) PL mapping of the heterostructure. (f) The photodetection device.

During the transfer process, the micron sized droplets evaporate quickly, making it easier to precisely drop WS2\mathrm{WS}_{2} and avoiding wrinkling of the monolayer flake. As a result, no additional steps to dry PDMS are needed, which not only saves time, but also simplifies manipulation and avoids possible folding of monolayer WS2\mathrm{WS}_{2}. In the present setup, only the chosen area of WS2\mathrm{WS}_{2} is taken up by the transfer process, while the rest of the substrate area remains intact and is preserved for next transfer process, leading to efficient utilization of WS2\mathrm{WS}_{2}. Overall, we compared the half-wet transfer method to several reported transfer techniques with an emphasis on the optimization of the potential limitations of those methods, as shown in Table 1.

WorkTransfer processTime consumptionStacking precisionSample retainingUtilization efficiency
Evaluation
WorkTransfer processTime consumptionStacking precisionSample retainingUtilization efficiency
C. R. Dean et al. [21]PMMA support film with acetone etchingOvernight soaking to remove PMMAHard to locate monolayer on pleated PMMASome solvent (like HF) may etch monolayerSelective transfer of a picked region is not feasible
Q. Fu et al. [22]PMMA support film with acetone etchingOvernight soaking to remove PMMAHard to locate monolayer on pleated PMMASome solvent (like HF) may etch monolayerSelective transfer of a picked region is not feasible
A. C.-Gomez et al. [23]All-dry viscoelastic stamping via GelfilmIn a few minutesPrecise alignment via optical microscopeNo residual inducedOnly for mechanically exfoliated materials
F. Pizzocchero et al. [24]PPC coated PDMS block as transfer supportIn a few minutesPrecise alignment via optical microscopeHeating (over 100 °C) in atmosphere results in oxidationOnly for mechanically exfoliated materials
Z. Juang et al. [25]Roll-to-roll transfer from Ni foil to viscous polymer support filmRolling speed does not contribute to the transfer resultsNot consideredHeating (over 150 °C) in atmosphere results in oxidation and curling produces foldsSelective transfer of a picked region is not feasible and targeted sample is finite
X. Ma et al. [26]Capillary-force-assisted transferIn a few minutesAbsence of fine control of sample placement in an in situ mannerNo additional pollutionAbsence of flexibility in controlling area sizes
Lee et al. [27]; Y. Hou et al. [28]Pre-treated substrate and PDMS transferIn a few minutesPrecise alignment via optical microscopeNo additional pollutionOnly for mechanically exfoliated materials

Table 1. Transfer performance comparison of this work with previously reported techniques

and the size of transferred sample is less than 30 μ\mum
S. Dong et al.[29]Hot water infiltration assisted PDMS transferA certain amount of time needed to immerse and evaporate waterPrecise alignment via optical microscopeNo additional pollutionThe size of transferred materials is a few tens of micrometers
J. Cai et al.[30]
This workHalf-wet transfer methodIn a few minutesPrecise alignment via optical microscopeNo additional pollutionGood versatility for various types of 2D materials grown on various substrates; flexibility in selecting specific samples and the transferred size up to nearly hundred micrometers

It is worth noting that, compared with other reported transfer results, our half-wet transfer process can pick up single monolayer flake with larger size, up to ∼\sim100 μ\mum (shown in Figure S3). A. Kozbial et al. theoretically calculated the surface wettability of MoS2_2 on SiO2_2/Si and found the changes in hydrophilicity of MoS2_2 with hydrocarbon absorption. S. Dong et al.[34] compared the surface energies of TMDCs and SiO2_2 exposed to water with ambient atmosphere and found water-driven separation of TMDC-SiO2_2 more energetically favorable. J. Cai et al.[29] proposed the water transport model between two surfaces based on the Young-Laplace equation. The mechanism of water-assisted transfer should have been unambiguous and universal. However, the results based on previous theories showed limited transfer area, which is inconsistent with ours, meaning extra analysis is needed. We propose that the intercalation of water molecule between WS2_2 and sapphire plays an important role in changing adhesion energy. Though direct evidence can be hardly derived for the intercalating process in current stage, the size of water molecule and crystal structure of WS2_2 make it comprehensible. According to the previous reported work by Y. Gao et al., the crystal structure of monolayer WS2_2 was shown via high-resolution transmission electron microscopy (HRTEM) and the distance between W and S atom is about 3 Å, which form periodic hexagons.[35] The size and geometry of water molecule has been widely studied and the length of 2.7 Å is convictive.[36] These results suggest that water molecule is small enough to go through atomic gap of crystal lattice of WS2_2.[37]After water intercalation and wetting the WS2_2/sapphire interface, a large scale monolayer flake can be picked up and the picking speed does not change with the size of transferred flake. Furthermore, we apply half-wet transfer method for different growth substrates, including SiO2_2/Si, sapphire and mica, and find that the successful transfer rate for the samples on sapphire is the highest, up to almost 100%.

Optical images and PL spectrum of WS$_2$ transfer process

Figure S3. Optical image of half-wet transfer process from sapphire to SiO2_2/Si. (a) Monolayer WS2_2 grown on sapphire. (b) WS2_2 lifted on PDMS. (c) WS2_2 dropped onto SiO2_2/Si. (d) PL spectra of WS2_2 with high efficiency.

Characterization of WS2_2/Bi2_2Se3_3 Heterostructure

fig:2a demonstrates the 3D schematic structure of the WS2_2/Bi2_2Se3_3 heterostructure for photodetection, and an optical microscopic image of the device is provided in Figure 2b. Atomic force microscopy (AFM) confirms the thickness across the heterostructure and each individual flake region as shown in Figure S4. The thickness line profile implies 1 nm thickness of WS2_2 and 8 nm thickness of Bi2_2Se3_3. With a theoretical thickness of monolayer WS2_2 of 0.7 nm and monolayer Bi2_2Se3_3 of 0.955 nm, this result confirms that our WS2_2 flake is monolayer and Bi2_2Se3_3 flake is about 8-layers.[38, 39] In order to confirm the interfacial coupling effect, room temperature photoluminescence (PL) spectra and mapping were collected from the WS2_2/Bi2_2Se3_3 heterostructure (Figure 2c, Figure 2d). The results indicate that the WS2_2 exhibits a strong PL emission peak at 2.01 eV (616 nm), which is comparable to a previously reported value of monolayer WS2_2.[40] The heterostructure region demonstrates an apparent PL quenching effect, as the PL intensity of WS2_2 decays to 21% of the pristine and remains only 7% compared with the original after annealing at 150 °C. The evolution of PL change as a function of annealing temperature is shown in Figure S5. This suggests the photoexcited carriers are primarily transferred between the WS2_2 and Bi2_2Se3_3 interface, rather than emitting from the individual WS2_2 band edges.[41] For the Bi2_2Se3_3, long-time exposure to air makes its surface oxidation, resulting in the band bending and the change of photodetection performance. Utilizing our fast half-wet transfer method, the time for heterostructure stacking is shortened, just a few minutes. As a result, air exposure time for the whole period of device fabrication can be restricted within 4 hours, meaning that the heterostructure maintains natural properties. Raman spectra of Bi2_2Se3_3 after fabricating demonstrates three distinct Raman peak positions at 69, 126, and 173 cm−1^{-1}, corresponding to the A1g1^{1}_{1g}, Eg2^{2}_{g} and A1g2^{2}_{1g} modes, respectively, which are in accordance with the previous reports (Figure 2e).[14] The in-plane and out-of-plane vibration modes for the individual and overlap region of WS2_2 at 355 and 420 cm−1^{-1}, respectively, are also shown in Figure 2e. The ratio of the intensities of the A1g_{1g} and E2g1^{1}_{2g} peaks is less than 0.5, which also indicates its monolayer thickness.[42] The WS2_2 and Bi2_2Se3_3 characteristic peaks show no shift in the heterostructure, demonstrating that the lattice property of WS2_2 and Bi2_2Se3_3 are not changed after half-wet transfer and thermal annealing.

Device structure and optical characterizations

Figure 2. Device structure and optical characterizations. (a) Schematic diagram and (b) Optical image of WS2_2/Bi2_2Se3_3 heterostructure device. The monolayer WS2_2 is stacked on the top of the Bi2_2Se3_3 flake. (c) PL mapping of the region surrounded by red dashed lines in Figure 2b. (d) PL spectra measured for WS2_2 and the heterostructure. (e) Raman spectra of individual Bi2_2Se3_3 and WS2_2/Bi2_2Se3_3 heterostructure after device fabrication.

AFM mapping and height profile of the WS$_2$/Bi$_2$Se$_3$ heterostructure

Figure S4. AFM of the WS2_2/Bi2_2Se3_3 heterostructure. (a) AFM mapping of the WS2_2/Bi2_2Se3_3

Optical image, PL mapping, and PL relative intensity of a WS2/Bi2Se3 heterostructure at different annealing temperatures

Figure S5. The evolution of PL intensity as a function of annealing temperature. (a) Optical image of selected WS2/Bi2Se3\mathrm{WS_2/Bi_2Se_3} heterostructure, marked by red dotted rectangular. (b) PL mapping of selected region after annealing at different temperature. (c) PL relative intensity after annealing at different temperature.

Electronic Characteristics of WS2_2/Bi2_2Se3_3 Heterostructure

The electric transport characteristics of the heterostructure device were studied to understand the interaction in the overlapped heterojunction region. All results are acquired by applying a drain voltage (VdsV_{\mathrm{ds}}) on Bi2_2Se3_3 with WS2_2 being ground. Figure 3a presents the current-voltage (II-VV) curves of the WS2_2/Bi2_2Se3_3 heterostructure in logarithmic (black) and linear (red) scale with the source/drain bias range of -4 to 4 V in the dark. This device shows a rectification behavior with a calculated rectification factor reaching up to 250. To comprehend the carrier transport behavior of the device, the electronic band alignment of the WS2_2/Bi2_2Se3_3 heterostructure is established as shown in Figure 3b. According to the previously reported measurement results and our PL spectrum, the conduction band minimum (EcE_\mathrm{c}), valence band maximum (EvE_\mathrm{v}) and Fermi level (EfE_\mathrm{f}) of the WS2_2 (Bi2_2Se3_3) locate at ~-3.87 eV (-4.91 eV), -5.88 eV (-5.21 eV) and -4.81 eV (-4.61 eV), respectively.[42, 43] From the electronic band before contact, the Fermi level of Bi2_2Se3_3 is higher than that of WS2_2. To prove the band difference, Kelvin probe force microscopy (KPFM) is performed to measure the surface potential of the heterostructure, as shown in Figure S6. Since larger surface potential corresponds to lower work function and thus higher Fermi level, the surface potential of Bi2_2Se3_3 is higher than that of WS2_2 by 0.2 eV, which proves the difference of Fermi level between WS2_2 and Bi2_2Se3_3.[44] Under the reverse bias condition, the external bias voltage breaks the unified Fermi level, elevating the energy band on Bi2_2Se3_3 side and descending the WS2_2 side as shown in Figure 3c. When a small negative VdsV_\mathrm{ds} is applied, the electrons in the Bi2_2Se3_3 are prevented to drift or tunnel to the conduction band of WS2_2 because of the existence of potential barrier. With the increasing of bias, the energy band of WS2_2 is further descended, the electrons have the possibility to directly tunnel to WS2_2. Nevertheless, the amount of tunneling electrons is limited due to the degenerated Bi2_2Se3_3 and the light doped of WS2_2. Tunneling current cannot be significantly higher than the thermionic current, which resulting in a stably low bias current ≈6×10−12\approx6 \times10^{-12} A at -4 V condition In opposite, the energy band of WS2_2 is elevated under forward bias voltage as shown in Figure 3d, which allows the electrons transfer freely from WS2_2 to Bi2_2Se3_3, resulting in a relatively high current.[45] Because of the unavoidable surface oxidation of Bi2_2Se3_3, there exists a barrier between the interface, leading the “open” voltage slightly shifts. Above all, the WS2_2/Bi2_2Se3_3 heterostructure device with a type-I band alignment configuration shows a diode characteristics obviously, indicating that our transfer method ensures high quality of the heterointerface.

Electronic characteristics of WS$_2$/Bi$_2$Se$_3$ heterostructure

Figure 3. Electronic characteristics of WS2_2/Bi2_2Se3_3 heterostructure. (a) II-VV curves of the heterostructure in dark. (b) Energy band diagram of WS2_2/Bi2_2Se3_3 heterostructure before contact and after contact. (c) and (d) Energy band alignment of WS2_2/Bi2_2Se3_3 heterostructure under different bias voltage VdsV_{\mathrm{ds}}.

Image not extracted

Figure S6. KPFM surface potential of the WS2_2/Bi2_2Se3_3 heterostructure. (a) The surface potential mapping of the heterostructure and individual Bi2_2Se3_3. (b) The surface potential profile across the sample corresponding to the dashed line in panel (a).

Photoresponse Properties of WS2_2/Bi2_2Se3_3 Heterostructure

Considering the complementary bandgaps of monolayer WS2_2 (2.01 eV) and few-layer Bi2_2Se3_3 (0.3 eV), their heterostructure may exhibit excellent photoresponse performances in both visible and near-infrared regions. [31, 46] Figure 4a shows the II-VV curves of the device under dark and different wavelength focused laser illumination with fixed incident power (0.5 mW). Under different condition, the WS2_2/Bi2_2Se3_3 heterostructure shows significant response, demonstrating that the device has a potential in terms of broadband photodetection. Figure 4b, Figure 4c, Figure 4d present the output characteristics of the device under 473, 532 and 1064 nm laser light with different power density, respectively. The currents in both forward and reverse biases show increasement with the increase of power density under different laser illumination. In order to evaluate the photodetection performance of the device, the responsivity (RR) and specific detectivity (D∗D^{*}) are calculated. The RR value can be calculated by the equation of R=Iph/(P⋅Seff)R=I_{\mathrm{ph}}/(P\cdot S_{\mathrm{eff}}), where IphI_{\mathrm{ph}}, PP and SeffS_{\mathrm{eff}} are the photocurrent, incident power density and effective areas of the device, respectively. D∗D^{*} can be extracted by D∗=R⋅Seff/2eIdarkD^{*}=R\cdot\sqrt{S_{\mathrm{eff}}}/\sqrt{2eI_{\mathrm{dark}}}, where IdarkI_{\mathrm{dark}} represents the dark current.[47] Figure 4e, f demonstrate the calculated RR and D∗D^{*} under different laser illumination at different excitation power density, respectively. For visible light of 473 nm, the responsivity reaches up to 109.9 A W−1^{-1} and the detectivity can get to 3.2×10123.2 \times10^{12} Jones at the power density of 4.527 mW cm−2^{-2} at Vds=4V_{\mathrm{ds}}=4 V, while the near-infrared responsivity is up to 26.7 A W−1^{-1} and detectivity is 7.76×10117.76 \times10^{11} Jones, which is superior to most reported near-infrared photodetectors.[31, 48]

Photoelectric characteristics of WS2/Bi2Se3 heterostructure

Figure 4. Photoelectric characteristics of WS2_2/Bi2_2Se3_3 heterostructure. (a) Broadband response of the device under different wavelength laser illumination at fixed laser power. (b), (c) and (d) Power depended IdsI_{\mathrm{ds}}-VdsV_{\mathrm{ds}} curves under 473, 532 and 1064 nm laser illumination, respectively. (e) and (f) Power depended RR and D∗D^{*} of the device under different wavelength laser illumination at VdsV_{\mathrm{ds}}=4 V.

To understand the photocurrent generation mechanism, we further studied the response of the device under reverse and forward bias separately. When the device worked at reverse biases voltage, we found that the IdsI_{ds}-VdsV_{ds} characteristics could be modeled by the direct tunneling mechanism with linear relationship between ln⁡(∣Ids∣/Vds2)\ln(\lvert I_{ds}\rvert/V_{ds}^{2}) and ln⁡(1/∣Vds∣)\ln(1/\lvert V_{ds}\rvert) as shown in Figure 5a. This indicates that the photocarriers generated in the WS2/Bi2Se3\mathrm{WS}_{2}/\mathrm{Bi}_{2}\mathrm{Se}_{3} heterostructure are dominated by the tunneling mechanism driven by the external reverse electric field. Under visible laser illumination, both WS2\mathrm{WS}_{2} and Bi2Se3\mathrm{Bi}_{2}\mathrm{Se}_{3} produce photon-generated electron-hole pairs. The barrier height of the heterojunction region becomes smaller, and the electrons can overcome the barrier or direct tunnel, consequently forming considerable photocurrent (Figure 5b). The carriers are generated only in Bi2Se3\mathrm{Bi}_{2}\mathrm{Se}_{3} when illuminated by 1064 nm laser as shown in Figure 5c. The photogenerated holes would enter the circuit, while the photo-generated electrons would accumulate at the interface and tunnel into the conduction band of WS2\mathrm{WS}_{2}, which exhibits a near-infrared photoresponse. From the linear relationship shown in Figure 5a, a formula like ln⁡(∣Ids∣Vds2)=kln⁡(1Vds)+b\ln\left(\frac{\lvert I_{ds}\rvert}{V_{ds}^{2}}\right)=k\ln\left(\frac{1}{V_{ds}}\right)+b can be extracted, where kk and bb are the slope and y-axial offset of the linear fitting line, which is relating to the probability of tunneling. [49, 50] Then the relationship between photogenerated current and bias voltage can be described as Ids=eb⋅Vds2−kI_{ds}=e^{b}\cdot V_{ds}^{2-k}. From the fitting curves, kvisiblek_{\mathrm{visible}} is smaller than kNIRk_{\mathrm{NIR}} while bvisibleb_{\mathrm{visible}} is larger than bNIRb_{\mathrm{NIR}}, meaning a higher photogenerated current under visible illumination, which is consistent with the observed phenomena. By fitting the incident power density (PP) dependent current (IphI_{\mathrm{ph}}) through the equation of Iph∝PαI_{\mathrm{ph}}\propto P^{\alpha} (Figure 5d), it was found that all the power exponent α\alpha values are smaller than 1 under forward bias. This deviation from the ideal value of α=1\alpha=1 suggests a complex process, which relates to the trap states caused by the defects or impurities present in WS2\mathrm{WS}_{2} or Bi2Se3\mathrm{Bi}_{2}\mathrm{Se}_{3}, or the absorbed molecules at WS2/Bi2Se3\mathrm{WS}_{2}/\mathrm{Bi}_{2}\mathrm{Se}_{3} interface and slight oxidation on Bi2Se3\mathrm{Bi}_{2}\mathrm{Se}_{3} surface. These factors can trap the photogenerated charges, so that the absorbed photons cannot be completely converted into photocurrent, resulting in the nonlinear photocurrent response. [51, 52] It can also explain why RR and D∗D^{*} decrease with power density increasing, that is, a drop in the recombination possibility occurs as the photogenerated electrons are captured by the trap states under lower PP. The transfer processes of visible and near-infrared photo-generated carriers under forward bias are shown in Figure 5e, Figure 5f. Moreover, the value of external quantum efficiency (EQE) is another parameter of photodetectors, defined by the ratio of the number of electrons collected to the number of incident photons. The calculation and the dependence on power density of EQE are shown in Figure S7[53]. The WS2_2/Bi2_2Se3_3 heterostructure shows an EQE up to 288.6%, corresponding to the photoconductive gain effect caused by interface trapped states.

Photocurrent generated mechanism of WS2/Bi2Se3 heterostructure

Figure 5. Photocurrent generated mechanism of WS2_2/Bi2_2Se3_3 heterostructure. (a) DT fitting of the device at reverse bias voltage. (b) and (c) Energy band diagram of the heterostructure under reverse bias. (d) The photocurrent dependence of laser power density at Vds=4V_{\mathrm{ds}}=4 V. (e) and (f) Energy band diagram of the heterostructure under forward bias.

EQE of the WS$_2$/Bi$_2$Se$_3$ heterostructure device

Figure S7. EQE of the WS2_2/Bi2_2Se3_3 heterostructure device.

Apart from responsivity, specific detectivity and EQE, response rate and light on/off ratio are also two important parameters for photodetectors. As shown in Figure 6a, the WS2_2/Bi2_2Se3_3 heterostructure exhibits well-reproducible photo switching characteristics under different wavelength laser modulation at Vds=4V_{\mathrm{ds}}=4 V and fixed laser power 0.5 W. Furthermore, the light on/off ratio was obtained by comparing the IdsI_{\mathrm{ds}} under illumination and dark. The dependence of light on/off ratio on the bias voltage is shown in Figure 6b. Consequently, we obtained the maximum on/off ratio of ∼1.06×106\sim1.06 \times10^{6} for 473 nm @ 118.307 mW cm−2118.307\ \mathrm{mW\,cm^{-2}}, 6.3×1056.3 \times10^{5} for 532 nm @ 127.32 mW cm−2127.32\ \mathrm{mW}\,\mathrm{cm}^{-2} and 7.2×1047.2 \times10^{4} for 1064 nm @ 102.342 mW cm−2102.342\ \mathrm{mW}\,\mathrm{cm}^{-2} at Vds=−3V_{\mathrm{ds}}=-3 V. In order to evaluate the ability of charge separation and diffusion, Figure 6c and Figure S8 extracts the rise time (τ1\tau_{1}) and fall time (τ2\tau_{2}) of the WS2/Bi2Se3\mathrm{WS}_{2}/\mathrm{Bi}_{2}\mathrm{Se}_{3} heterostructure, which are usually defined as the time requirement of the photocurrent increasing from 10% to 90% and decreasing from 90% to 10%, respectively. For 473 nm laser illumination, the rise time and fall time are estimated to be 7 and 3 ms. Moreover, for 1064 nm photoresponse, the rise time of ∼\sim13 ms and decay time of ∼\sim7 ms are a bit slower than previous reports. The trap state in CVD grown WS2\mathrm{WS}_{2} and slightly unavoidable oxidation on the surface of Bi2Se3\mathrm{Bi}_{2}\mathrm{Se}_{3} reduce the recombination rate of photogenerated carriers and prolong the life of carriers.43

Photoresponse characteristics of the WS2/Bi2Se3 heterostructure

Figure 6. Photoresponse characteristics of the WS2/Bi2Se3\mathrm{WS}_{2}/\mathrm{Bi}_{2}\mathrm{Se}_{3} heterostructure. (a) Long-cycle stability measurement of the heterostructure device under different wavelength laser illumination. (b) Light on/off ratio as a function of bias voltage under 473 nm@118.307 mW cm−2118.307\ \mathrm{mW}\,\mathrm{cm}^{-2}, 532 nm@127.32 mW cm−2127.32\ \mathrm{mW}\,\mathrm{cm}^{-2} and 1064 nm@102.342 mW cm−2102.342\ \mathrm{mW}\,\mathrm{cm}^{-2}. (c) Response time curve of the heterostructure under 473 nm laser illumination.

Response time curve of the heterostructure under 1064 nm laser illumination

Figure S8. Response time curve of the heterostructure under 1064 nm laser illumination.

Finally, we make a comparison of our device with similar vdW heterostructures recently reported on the performances of photodetection, as shown in Table 2. There are some other photodetection devices we have fabricated performing similarly, as shown in Figure S9 and Figure S10. One can observe that our WS2/Bi2Se3\mathrm{WS}_{2}/\mathrm{Bi}_{2}\mathrm{Se}_{3} heterostructure is highly comparable to the state-of-the-art previously reported photodetection materials, suggesting that our transfer method is a promising way for the future fast and massive fabrication of multifunctional heterostructures.

Device structureFabrication methodWavelength [nm]Bias [V]Responsivity [A W−1^{-1}]Detectivity [Jones]Response rateOn/off ratio
MoS2_2/WS2_2[10]CVD growth53210.068—35/36 ms—
Bi2_2Se3_3/graphene[14]MBE growth5201.51.4——/114.94 ms—
Bi2_2O2_2Se/WS2_2[31]PSb^{\mathrm{b}} wet transfer53250.6289.5×1089.5 \times10^{8}33/38 ms160
Bi2_2O2_2Se/WS2_2[31]PSb^{\mathrm{b}} wet transfer135050.001———
Bi2_2O2_2Se/WSe2_2[32]PVA dry transfer6351443.0×10133.0 \times10^{13}20/20 ms1.2×1041.2 \times10^{4}
Bi2_2O2_2Se/WSe2_2[32]PVA dry transfer106410.012×1082 \times10^{8}——
WS2_2/Bi2_2Se3_3[33]PVD growth5321 (Vg=−20V_{\mathrm{g}}=-20)——126/162 ms—
Bi2_2Se3_3/WSe2_2[43]PDMS dry transfer532−594.267.9×10127.9 \times10^{12}1.5/0.11 ms7.5×1057.5 \times10^{5}
Bi2_2Se3_3/WSe2_2[43]PDMS dry transfer1456−532.2×10102.2 \times10^{10}4/4 ms3.5×1043.5 \times10^{4}
Bi2_2O2_2Se/BP[48]PDMS dry transfer700−15002.8×10112.8 \times10^{11}—/9 ms—
Bi2_2O2_2Se/BP[48]PDMS dry transfer1310−14.32.4×1092.4 \times10^{9}——
WS2_2[51]PVAa^{\mathrm{a}} dry transfer405−23.45—31.78/19.81 ms—
WSe2_2/Bi2_2O2_2Se[54]PDMS dry transfer5325443.83—2.4/2.6 μ\mus1.48
WSe2_2/Bi2_2O2_2Se[54]PDMS dry transfer532−50.638——618
Bi2_2O2_2Se/MoSe2_2[55]PMMA wet transfer78020.41313.7×10113.7 \times10^{11}0.79/0.49 s—
GaSe/graphene[56]MBE growth532−2983.1×10123.1 \times10^{12}3/3 ms10
WS2_2/Bi2_2Se3_3 (this work)half-wet transfer4734109.93.2×10123.2 \times10^{12}7/3 ms1.06×1061.06 \times10^{6}
WS2_2/Bi2_2Se3_3 (this work)half-wet transfer1064426.77.7×10117.7 \times10^{11}13/7 ms7.2×1047.2 \times10^{4}

Table 2. Photodetection performance comparison of this work with similar devices

Optical image, PL mapping, and broadband response of the WS₂/Bi₂Se₃ heterostructure device

Figure S9. Optical image of the WS2/Bi2Se3WS_{2}/Bi_{2}Se_{3} heterostructure device and its photodetection performance. (a) Optical image of the heterostructure. (b) PL mapping of the region surrounded by red dashed lines in (a). (c) Broadband response of the device under different wavelength laser illumination at fixed laser power.

Optical image and broadband response of the WS₂/Bi₂Se₃ heterostructure device

Figure S10. Optical image of the WS2/Bi2Se3WS_{2}/Bi_{2}Se_{3} heterostructure device and its photodetection performance. (a) Optical image of the heterostructure. (b) Broadband response of the device under different wavelength laser illumination at fixed laser power.

Conclusion

In summary, our study presents a novel 2D material transfer method. By utilizing PDMS and DI water as transfer substrate and lubricant, we successfully realize convenient and fast pick-and-drop process of monolayer WS2_2. The size of single transferred monolayer piece is up to hundred-micron scale, which is an order of magnitude higher than the original report. To prove the clean and nondestructive transfer process, we fabricate a high quality WS2_2/Bi2_2Se3_3 heterostructure for photodetection. Our heterostructure with type-I band alignment demonstrates wide spectrum response from visible light to near-infrared band (from 405 to 1064 nm). The critical parameters of our heterostructures such as responsivity of 109.9 and 26.7 A W−1^{-1}, light on/off ratio of 1.06×1061.06 \times10^{6} and 7.2×1047.2 \times10^{4} with a fast response time of 7 and 13 ms are obtained at both visible 473 and near-infrared 1064 nm, respectively. Such superior performance demonstrates that our new transfer method may pave a unique avenue to fabricate manifold 2D heterostructures fast and massively.

Experimental Section

Fabrication of Bi2_2Se3_3/WS2_2 heterostructure: First, monolayer WS2_2 was grown on Si/SiO2_2 (300 nm) substrates or sapphire (C-plane) by using confined-space chemical vapor deposition at atmospheric pressure.3 A quartz tube was placed in the center of a horizontal tube furnace (BTF-1200C, Anhui Best Equipment Ltd, China) equipped with an assistant substrate facing upward. The WO3_3 power was sprinkled on the surface of the assistant substrate while a target growth substrate was placed on the surface of the quartz tube facing down to the assistant substrate. The distance between the assistant substrate and the target growth substrate was about 1 mm. The sulfur power was put into another quartz tube in the center of another furnace upstream. The distance between W and S source was kept as 40 cm. The temperature of W source was first gradually raised up to 600 °C in 60 min, then it was increased to 830 °C with a rate of 10 °C/min and kept at 830 °C for 10 min. When the temperature of W source reached 780 °C, the sulfur power was heated to 200 °C in 5 min and was kept at 200 °C for 10 min for the growth of monolayer WS2_2. Finally, the tube furnace was naturally cooled down to room temperature. Ar was used as the carrier and protective gas at a flow rate of 50 sccm during the whole growth process.

Then, 2D Bi2_2Se3_3 flakes were grown on flurophlogopite mica substrate by low pressure physical vapor deposition.4 The Bi2_2Se3_3 power was placed in the center of the furnace equipped with a quartz tube and the flurophlogopite mica substrates were placed in the downstream 8-11 cm away from center. The temperature of Bi2_2Se3_3 was first raised up to 590 °C in 30 min and kept at this temperature for 20 min with Ar carrier gas flow of 100 sccm. The pressure of the furnace was kept at 100 Torr. Finally, the furnace was naturally cooled down to room temperature with a flowing Ar gas.

Next, the monolayer WS2\mathrm{WS}_2 was transferred onto the Bi2Se3\mathrm{Bi}_2\mathrm{Se}_3 flake via a piece of PDMS as the supporting membrane and DI water as lubricant. The transfer details of picking and dropping were discussed in Results and Discussion. The alignment process is shown as follows: We selected one Bi2Se3\mathrm{Bi}_2\mathrm{Se}_3 as bottom material and marked its location on the camera screen as we did with WS2\mathrm{WS}_2. When both WS2\mathrm{WS}_2 and Bi2Se3\mathrm{Bi}_2\mathrm{Se}_3 were settled, by employing the microscope imaging and 3-axis micromanipulator stage, monolayer WS2\mathrm{WS}_2 was moved to the aligned location and started to drop onto the Bi2Se3\mathrm{Bi}_2\mathrm{Se}_3. With the slide going down, we checked the position of Bi2Se3\mathrm{Bi}_2\mathrm{Se}_3 from time to time, in order to make sure it still stays at the original position we marked. As distance decreasing, we could see the two materials in the screen till they contacted with each other. Last but not least, by careful manually manipulation through the z-motion of the glass slide-carrying stage, PDMS was peeled off from the mica and monolayer WS2\mathrm{WS}_2 remained on Bi2Se3\mathrm{Bi}_2\mathrm{Se}_3 because of van der Waals force. Finally, electrode patterns were defined by typical electron beam lithography (Nova Nanosem 450) and deposited by thermally evaporating 5/75 nm Cr/Au (K.J.Lesker Nano 36 Thermal Evaporator).

Characterizations: Optical microscope (Nikon ECLIPSE LV1SON) and AFM (Park NX-10) were utilized to characterize the morphology of the heterostructure. Raman and PL were investigated by a confocal microscope spectrometer (Alpha300R-2018model, WITech Ltd.) together with 532 laser source. EFM test cantilever (PPP-NCSTAu 3M) was used to measure the surface potential to obtain the difference of Fermi levels. The electronic and photoelectronic measurements of the Bi2Se3/WS2\mathrm{Bi}_2\mathrm{Se}_3/\mathrm{WS}_2 heterostructure were performed by using a Keithley 2450 sourcemeter. Power fixed 405-nm laser and power adjustable 473-, 532- and 1064 nm lasers (Changchun New Industries Optoelectronics Technology Ltd.) were used to record the photoelectric response of the heterostructure. The radius of laser spot in visible waveband was about 1 mm, and the radius of laser spot in 1064 nm was approximately 1.2 mm.

Supporting Information

Additional characterization results, including optical image characterization, PL mapping characterization, AFM characterization, KPFM characterization and photodetection performance of additional devices.

Acknowledgements

L. J. Li acknowledges the funding from the state key program (91950205), National Key R&D Program of China (2019YFA0308602), and the general program (12174336) of National Science Foundation of China, the Zhejiang Provincial Natural Science Foundation of China (LR20A040002).

Conflict of Interest

The authors declare no conflict of interest.

Data Availability Statement

The data that support the findings of this study are available from the corresponding author upon reasonable request.

Received:

Revised:

Published online:

References

Fast fabrication of WS2_2/Bi2_2Se3_3 heterostructure for high-performance photodetection

Fan Li; Jialin Li; Junsheng Zheng; Yuanbiao Tong; Huanfeng Zhu; Pan Wang; Linjun Li

Support Information

Optical images of the half-wet transfer process

Figure S2. Optical image of half-wet transfer process from sapphire to mica. (a) Monolayer WS2WS_{2} grown on sapphire. (b) WS2WS_{2} lifted on PDMS. (c) The WS2WS_{2}/Bi2Se3Bi_{2}Se_{3} heterostructure. (d) PL mapping of the region surrounded by red dashed lines in (c).

heterostructure and individual Bi2Se3\mathrm{Bi_2Se_3}. (b) Height profile of the WS2/Bi2Se3\mathrm{WS_2/Bi_2Se_3} heterostructure in (a) white dotted line.

Scanning probe image and potential profile of a heterostructure

Figure 7.

References

  1. [1]Ohno, Y.; Young, D. K.; Beschoten, B.; Matsukura, F.; Ohno, H.; Awschalom, D. D., Electrical Spin Injection in a Ferromagnetic Semiconductor Heterostructure. Nature 1999, 402, 790-792.DOI
  2. [2]Geim, A. K.; Grigorieva, I. V., Van der Waals Heterostructures. Nature 2013, 499 (7459), 419-425.DOI
  3. [3]Pasqu​al Rivera; Kyle L. Seyler; Hongyi Yu; John R. Schaibley; Jiaqiang Yan; David G. Mandrus; Wang Yao; Xu, X., Valley-Polarized Exciton Dynamics in a 2D Semiconductor Heterostructure. Science 2016, 351 (6274), 688-691.
  4. [4]Cao, Y.; Fatemi, V.; Fang, S.; Watanabe, K.; Taniguchi, T.; Kaxiras, E.; Jarillo-Herrero, P., Unconventional Superconductivity in Magic-Angle Graphene Superlattices. Nature 2018, 556 (7699), 43-50.DOI
  5. [5]Alexeev, E. M.; Ruiz-Tijerina, D. A.; Danovich, M.; Hamer, M. J.; Terry, D. J.; Nayak, P. K.; Ahn, S.; Pak, S.; Lee, J.; Sohn, J. I.; Molas, M. R.; Koperski, M.; Watanabe, K.; Taniguchi, T.; Novoselov, K. S.; Gorbachev, R. V.; Shin, H. S.; Fal'ko, V. I.; Tartakovskii, A. I., Resonantly Hybridized Excitons in Moire Superlattices in van der Waals Heterostructures. Nature 2019, 567 (7746), 81-86.DOI
  6. [6]Forg, M.; Colombier, L.; Patel, R. K.; Lindlau, J.; Mohite, A. D.; Yamaguchi, H.; Glazov, M. M.; Hunger, D.; Hogele, A., Cavity-Control of Interlayer Excitons in van der Waals Heterostructures. Nat Commun 2019, 10 (1), 3697.
  7. [7]Gong, Y.; Lin, J.; Wang, X.; Shi, G.; Lei, S.; Lin, Z.; Zou, X.; Ye, G.; Vajtai, R.; Yakobson, B. I.; Terrones, H.; Terrones, M.; Tay, B. K.; Lou, J.; Pantelides, S. T.; Liu, Z.; Zhou, W.; Ajayan, P. M., Vertical and in-plane Heterostructures from WS₂/MoS₂ Monolayers. Nat Mater 2014, 13 (12), 1135-42.DOI
  8. [8]Yao, J.; Zheng, Z.; Yang, G., Layered-Material WS₂/Topological Insulator Bi₂Te₃ Heterostructure Photodetector with Ultrahigh Responsivity in the Range from 370 to 1550 nm. Journal of Materials Chemistry C 2016, 4 (33), 7831-7840.DOI
  9. [9]Yang, W.; Kawai, H.; Bosman, M.; Tang, B.; Chai, J.; Tay, W. L.; Yang, J.; Seng, H. L.; Zhu, H.; Gong, H.; Liu, H.; Goh, K. E. J.; Wang, S.; Chi, D., Interlayer Interactions in 2D WS₂/MoS₂ Heterostructures Monolithically Grown by in situ Physical Vapor Deposition. Nanoscale 2018, 10 (48), 22927-22936.DOI
  10. [10]Zhang, X.; Huangfu, L.; Gu, Z.; Xiao, S.; Zhou, J.; Nan, H.; Gu, X.; Ostrikov, K. K., Controllable Epitaxial Growth of Large-Area MoS₂/WS₂ Vertical Heterostructures by Confined-Space Chemical Vapor Deposition. Small 2021, 17 (18), 2007312.DOI
  11. [11]Aretouli, K. E.; Tsipas, P.; Tsoutsou, D.; Marquez-Velasco, J.; Xenogiannopoulou, E.; Giamini, S. A.; Vassalou, E.; Kelaidis, N.; Dimoulas, A., Two-Dimensional Semiconductor HfSe₂ and MoSe₂/HfSe₂ van der Waals Heterostructures by Molecular Beam Epitaxy. Applied Physics Letters 2015, 106 (14).
  12. [12]Diaz, H. C.; Chaghi, R.; Ma, Y.; Batzill, M., Molecular Beam Epitaxy of the van der Waals Heterostructure MoTe₂ on MoS₂: Phase, Thermal, and Chemical Stability. 2D Materials 2015, 2 (4).DOI
  13. [13]Hinkle, C., van der Waals Heterostructures Grown by MBE. the MAR16 Meeting of the American Physical Society 2015.
  14. [14]Chae, J.; Hong, S.-B.; Kim, D.; Kim, D.-K.; Kim, J.; Jeong, K.; Park, S. H.; Cho, M.-H., Enhancement of Photoresponse in Bi₂Se₃/Graphene Heterostructures by Effective Electron–Hole Separation through Internal Band Bending. Applied Surface Science 2021, 554.DOI
  15. [15]Zatko, V.; Dubois, S. M.; Godel, F.; Carretero, C.; Sander, A.; Collin, S.; Galbiati, M.; Peiro, J.; Panciera, F.; Patriarche, G.; Brus, P.; Servet, B.; Charlier, J. C.; Martin, M. B.; Dlubak, B.; Seneor, P., Band-Gap Landscape Engineering in Large-Scale 2D Semiconductor van der Waals Heterostructures. ACS Nano 2021, 15 (4), 7279-7289.DOI
  16. [16]Zhou, J.; Lin, J.; Huang, X.; Zhou, Y.; Chen, Y.; Xia, J.; Wang, H.; Xie, Y.; Yu, H.; Lei, J.; Wu, D.; Liu, F.; Fu, Q.; Zeng, Q.; Hsu, C. H.; Yang, C.; Lu, L.; Yu, T.; Shen, Z.; Lin, H.; Yakobson, B. I.; Liu, Q.; Suenaga, K.; Liu, G.; Liu, Z., A Library of Atomically Thin Metal Chalcogenides. Nature 2018, 556 (7701), 355-359.DOI
  17. [17]Yu, J. H.; Lee, H. R.; Hong, S. S.; Kong, D.; Lee, H. W.; Wang, H.; Xiong, F.; Wang, S.; Cui, Y., Vertical Heterostructure of Two-Dimensional MoS₂ and WSe₂ with Vertically Aligned Layers. Nano Lett 2015, 15 (2), 1031-5.DOI
  18. [18]Yang, T.; Zheng, B.; Wang, Z.; Xu, T.; Pan, C.; Zou, J.; Zhang, X.; Qi, Z.; Liu, H.; Feng, Y.; Hu, W.; Miao, F.; Sun, L.; Duan, X.; Pan, A., Van der Waals Epitaxial Growth and Optoelectronics of Large-Scale WSe₂/SnS₂ Vertical Bilayer p-n Junctions. Nat Commun 2017, 8 (1), 1906.DOI
  19. [19]Weixia Gu; Fan Yang; Chen Wu; Yi Zhang; Shi, M.; Ma, X., Fabrication and Investigation of the Optoelectrical Properties of MoS₂/CdS Heterojunction Solar Cells. Nanoscale Research Letters 2014, 9 (662).DOI
  20. [20]Castellanos-Gomez, A.; Duan, X.; Fei, Z.; Gutierrez, H. R.; Huang, Y.; Huang, X.; Quereda, J.; Qian, Q.; Sutter, E.; Sutter, P., Van der Waals Heterostructures. Nature Reviews Methods Primers 2022, 2 (1).
  21. [21]Dean, C. R.; Young, A. F.; Meric, I.; Lee, C.; Wang, L.; Sorgenfrei, S.; Watanabe, K.; Taniguchi, T.; Kim, P.; Shepard, K. L.; Hone, J., Boron Nitride Substrates for High-Quality Graphene Electronics. Nat Nanotechnol 2010, 5 (10), 722-6.DOI
  22. [22]Fu, Q.; Zhu, C.; Zhao, X.; Wang, X.; Chaturvedi, A.; Zhu, C.; Wang, X.; Zeng, Q.; Zhou, J.; Liu, F.; Tay, B. K.; Zhang, H.; Pennycook, S. J.; Liu, Z., Ultrasensitive 2D Bi₂O₂Se Phototransistors on Silicon Substrates. Adv Mater 2019, 31 (1), 1804945.DOI
  23. [23]Andres Castellanos-Gomez; Michele Buscema; Rianda Molenaar; Vibhor Singh; Laurens Janssen; Zant, H. S. J. v. d.; Steele, G. A., Deterministic Transfer of Two-Dimensional Materials by All-Dry Viscoelastic Stamping. 2D Materials 2014, 1 (1).
  24. [24]Pizzocchero, F.; Gammelgaard, L.; Jessen, B. S.; Caridad, J. M.; Wang, L.; Hone, J.; Boggild, P.; Booth, T. J., The Hot Pick-up Technique for Batch Assembly of van der Waals Heterostructures. Nat Commun 2016, 7, 11894.DOI
  25. [25]Juang, Z.-Y.; Wu, C.-Y.; Lu, A.-Y.; Su, C.-Y.; Leou, K.-C.; Chen, F.-R.; Tsai, C.-H., Graphene Synthesis by Chemical Vapor Deposition and Transfer by a Roll-to-Roll Process. Carbon 2010, 48 (11), 3169-3174.arxiv.org/abs/1005.1510
  26. [26]Ma, X.; Liu, Q.; Xu, D.; Zhu, Y.; Kim, S.; Cui, Y.; Zhong, L.; Liu, M., Capillary-Force-Assisted Clean-Stamp Transfer of Two-Dimensional Materials. Nano Lett 2017, 17 (11), 6961-6967.DOI
  27. [27]Jun-Ho Lee; Han-Byeol Lee; Nae Bong Jeong; Do-Hyun Park; Inchul Choi; Chung, H.-J., High-Speed Residue-Free Transfer of Two-Dimensional Materials Using PDMS Stamp and Water Infiltration. Current Applied Physics 2020, 20 (10), 1190-1194.DOI
  28. [28]Hou, Y.; Ren, X.; Fan, J.; Wang, G.; Dai, Z.; Jin, C.; Wang, W.; Zhu, Y.; Zhang, S.; Liu, L.; Zhang, Z., Preparation of Twisted Bilayer Graphene via the Wetting Transfer Method. ACS Appl Mater Interfaces 2020, 12 (36), 40958-40967.DOI
  29. [29]Dong, S.; Zhang, X.; Nathamgari, S. S. P.; Krayev, A.; Zhang, X.; Hwang, J. W.; Ajayan, P. M.; Espinosa, H. D., Facile Fabrication of 2D Material Multilayers and vdW Heterostructures with Multimodal Microscopy and AFM Characterization. Materials Today 2022, 52, 31-42.DOI
  30. [30]Cai, J.; Chen, H.; Ke, Y.; Deng, S., A Capillary-Force-Assisted Transfer for Monolayer Transition-Metal-Dichalcogenide Crystals with High Utilization. ACS Nano 2022, 16 (9), 15016-15025.
  31. [31]Fang, C.; Han, J.; Yu, M.; Liu, W.; Gao, S.; Huang, K., WS₂/Bi₂O₂Se van der Waals Heterostructure with Straddling Band Configuration for High Performances and Broadband Photodetector. Advanced Materials Interfaces 2022, 9 (9).DOI
  32. [32]Tao, L.; Li, S.; Yao, B.; Xia, M.; Gao, W.; Yang, Y.; Wang, X.; Huo, N., Raman Anisotropy and Polarization-Sensitive Photodetection in 2D Bi₂O₂Se-WSe₂ Heterostructure. ACS Omega 2021, 6 (50), 34763-34770.
  33. [33]She, Y.; Wu, Z.; You, S.; Du, Q.; Chu, X.; Niu, L.; Ding, C.; Zhang, K.; Zhang, L.; Huang, S., Multiple-Dimensionally Controllable Nucleation Sites of Two-Dimensional WS₂/Bi₂Se₃ Heterojunctions Based on Vapor Growth. ACS Appl Mater Interfaces 2021, 13 (13), 15518-15524.DOI
  34. [34]Kozbial, A.; Gong, X.; Liu, H.; Li, L., Understanding the Intrinsic Water Wettability of Molybdenum Disulfide (MoS₂). Langmuir 2015, 31 (30), 8429-35.
  35. [35]Gao, Y.; Liu, Z.; Sun, D. M.; Huang, L.; Ma, L. P.; Yin, L. C.; Ma, T.; Zhang, Z.; Ma, X. L.; Peng, L. M.; Cheng, H. M.; Ren, W., Large-Area Synthesis of High-Quality and Uniform Monolayer WS₂ on Reusable Au Foils. Nat Commun 2015, 6, 8569.DOI
  36. [36]Huang, Y.; Zhang, X.; Ma, Z.; Li, W.; Zhou, Y.; Zhou, J.; Zheng, W.; Sun, C. Q., Size, Separation, Structural Order, and Mass Density of Molecules Packing in Water and Ice. Sci Rep 2013, 3, 3005.DOI
  37. [37]Kausar, A.; Taherian, R., Electrical Conductivity Behavior of Polymer Nanocomposite with Carbon Nanofillers. In Electrical Conductivity in Polymer-Based Composites: Experiments, Modelling and Applications, 2019; pp 41-72.DOI
  38. [38]Weijie Zhao; Zohreh Ghorannevis; Leiqiang Chu; Minglin Toh; Christian Kloc; Ping-Heng Tan; Eda, G., Evolution of Electronic Structure in Atomically Thin Sheets of WS₂ and WSe₂. ACS Nano 2013, 7 (1), 791-797.DOI
  39. [39]Wang, F.; Li, L.; Huang, W.; Li, L.; Jin, B.; Li, H.; Zhai, T., Submillimeter 2D Bi₂Se₃ Flakes toward High-Performance Infrared Photodetection at Optical Communication Wavelength. Advanced Functional Materials 2018, 28 (33).DOI
  40. [40]Yu Zhang; Yanfeng Zhang; Qingqing Ji; Jing Ju; Hongtao Yuan; Donglin Ma; Mengxi Liu; Yubin Chen; Xiuju Song; Harold Y. Hwang; Jianping Shi; Teng Gao; Yi Cui; Liu, Z., Controlled Growth of High-Quality Monolayer WS₂ Layers on Sapphire and Imaging Its Grain Boundary. ACS Nano 2013, 7 (10), 8963-8971.DOI
  41. [41]Yu, Y.; Hu, S.; Su, L.; Huang, L.; Liu, Y.; Jin, Z.; Purezky, A. A.; Geohegan, D. B.; Kim, K. W.; Zhang, Y.; Cao, L., Equally Efficient Interlayer Exciton Relaxation and Improved Absorption in Epitaxial and Nonepitaxial MoS₂/WS₂ Heterostructures. Nano Lett 2015, 15 (1), 486-91.DOI
  42. [42]Liu, S.; He, D.; Tan, C.; Fu, S.; Han, X.; Huang, M.; Miao, Q.; Zhang, X.; Wang, Y.; Peng, H.; Zhao, H., Charge Transfer Properties of Heterostructures Formed by Bi₂O₂Se and Transition Metal Dichalcogenide Monolayers. Small 2022, 18 (7), e2106078.DOI
  43. [43]Wang, F.; Luo, P.; Zhang, Y.; Huang, Y.; Zhang, Q.; Li, Y.; Zhai, T., Band Structure Engineered Tunneling Heterostructures for High-Performance Visible and near-Infrared Photodetection. Science China Materials 2020, 63 (8), 1537-1547.DOI
  44. [44]Kun Chen; Xi Wan; Jinxiu Wen; Weiguang Xie; Zhiwen Kang; Xiaoliang Zeng; Huanjun Chen; Xu, J.-B., Electronic Properties of MoS₂/WS₂ Heterostructures Synthesized with Two-Step Lateral Epitaxial Strategy. ACS Nano 2015, 9 (10), 9868–9876.DOI
  45. [45]Yu, M.; Fang, C.; Han, J.; Liu, W.; Gao, S.; Huang, K., Construction of Bi₂O₂Se/Bi₂Se₃ Van Der Waals Heterostructures for Self-Powered and Broadband Photodetectors. ACS Appl Mater Interfaces 2022, 14 (11), 13507-13515.DOI
  46. [46]Luo, M.; Lu, C.; Liu, Y.; Han, T.; Ge, Y.; Zhou, Y.; Xu, X., Band Alignment of Type-I SnS₂/Bi₂Se₃ and Type-II SnS₂/Bi₂Te₃ van der Waals Heterostructures for Highly Enhanced Photoelectric Responses. Science China Materials 2021, 65 (4), 1000-1011.DOI
  47. [47]Xing Zhou; Lin Gan; Wenming Tian; Qi Zhang; Shengye Jin; Huiqiao Li; Yoshio Bando; Dmitri Golberg; Zhai, T., Ultrathin SnSe₂ Flakes Grown by Chemical Vapor Deposition for High-Performance Photodetectors. Adv Mater 2015, 27 (48), 8035-8041.DOI
  48. [48]Liu, X.; Wang, W.; Yang, F.; Feng, S.; Hu, Z.; Lu, J.; Ni, Z., Bi₂O₂Se/BP van der Waals Heterojunction for High Performance Broadband Photodetector. Science China Information Sciences 2021, 64 (4).DOI
  49. [49]Simmons, J. G., Generalized Formula for the Electric Tunnel Effect between Similar Electrodes Separated by a Thin Insulating Film. Journal of Applied Physics 1963, 34 (6), 1793-1803.DOI
  50. [50]Ma, Q.; Andersen, T. I.; Nair, N. L.; Gabor, N. M.; Massicotte, M.; Lui, C. H.; Young, A. F.; Fang, W.; Watanabe, K.; Taniguchi, T.; Kong, J.; Gedik, N.; Koppens, F. H. L.; Jarillo-Herrero, P., Tuning Ultrafast Electron Thermalization Pathways in a van der Waals Heterostructure. Nature Physics 2016, 12 (5), 455-459.arxiv.org/abs/1601.02265
  51. [51]Wei Gao; Shuai Zhang; Feng Zhang; Peiting Wen; Li Zhang; Yiming Sun; Hongyu Chen; Zhaoqiang Zheng; Mengmeng Yang; Dongxiang Luo; Nengjie Huo; Li, J., 2D WS₂ Based Asymmetric Schottky Photodetector with High Performance. Advanced Electronic Materials 2020, 7 (7).DOI
  52. [52]Wenjing Zhang; Jing-Kai Huang; Chang-Hsiao Chen; Yung-Huang Chang; Yuh-Jen Cheng; Li, L.-J., High-Gain Phototransistors Based on a CVD MoS₂ Monolayer. Adv Mater 2013, 25 (25), 3456-3461.DOI
  53. [53]Koppens, F. H.; Mueller, T.; Avouris, P.; Ferrari, A. C.; Vitiello, M. S.; Polini, M., Photodetectors Based on Graphene, Other Two-Dimensional Materials and Hybrid Systems. Nat Nanotechnol 2014, 9 (10), 780-93.DOI
  54. [54]Luo, P.; Wang, F.; Qu, J.; Liu, K.; Hu, X.; Liu, K.; Zhai, T., Self-Driven WSe₂/Bi₂O₂Se Van der Waals Heterostructure Photodetectors with High Light on/Off Ratio and Fast Response. Advanced Functional Materials 2020, 31 (8).
  55. [55]Yang, T.; Yang, X.; Li, X.; Wang, L.; Liao, L.; Liu, Y.; Chen, K.; Dong, L.; Shan, C.-X., Broadband Photodetection of 2D Bi₂O₂Se–MoSe₂ Heterostructure. Journal of Materials Science 2019, 54 (24), 14742-14751.DOI
  56. [56]Saroj, R. K.; Guha, P.; Lee, S.; Yoo, D.; Lee, E.; Lee, J.; Kim, M.; Yi, G. C., Photodetector Arrays Based on MBE-Grown GaSe/Graphene Heterostructure. Advanced Optical Materials 2022.DOI

Paper details

vlnc:W_jmx5c9mu
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents