Structural Trends and Itinerant Magnetism of the New Cage-structured Compound HfMn2_{2}Zn20_{20}

Abstract

A new cage-structured compound - HfMn2_{2}Zn20_{20} - belonging to the AB2_{2}C20_{20} (A, B = transition or rare earth metals, and C = Al, Zn, or Cd) family of structures has been synthesized via the self-flux method. The new compound crystallizes in the space group Fd-3m with lattice parameter a = 14.0543(2) Å (Z = 8) and exhibits non-stoichiometry due to Mn/Zn mixing on the Mn-site and an underoccupied Hf-site. The structure refines to Hf0.93_{0.93}Mn1.63_{1.63}Zn20.37_{20.37} and follows lattice size trends when compared to other HfM2_{2}Zn20_{20} (M = Fe, Co, and Ni) structures. The magnetic measurements show that this compound displays a modified Curie-Weiss behavior with a transition temperature around 22 K. The magnetization shows no saturation, a small magnetic moment, and near negligible hysteresis, all signs of the itinerant magnetism. The Rhodes-Wohlfarth ratio and the spin fluctuation parameters ratio both confirm the itinerant nature of the magnetism in HfMn2_{2}Zn20_{20}.

Introduction

The large family of isostructural ternary intermetallic compounds with formula AB2C20AB_2C_{20} (AA, BB = transition and/or rare earth metals, and CC = Al, Zn, or Cd) crystallize in the CeCr2_2Al20_{20}-type structure [1] with space group Fd3ˉmFd\bar{3}m and exhibit “cages” formed by the element CC which contain the loosely-bound elements AA and BB [2, 3, 4, 5]. Even though over a hundred compounds in this 1-2-20 family have been discovered, new ones are still being found and many of them have been explored for various properties. For example, some of the AB2C20AB_2C_{20} compounds exhibit superconductivity, mainly among the CC = Al compounds [6, 7, 8, 9, 10, 11, 12] although it has also been observed in CC = Zn compounds [13, 14]. The superconductivity has been explored in terms of enhanced TC_C due to the rattling of the heavier AA and BB elements within the cages. The rattling of the AA and BB elements was also the focus for the most recent surge of interest in the AB2C20AB_2C_{20} compounds: enhanced low-temperature thermoelectricity [15, 16, 17]. This was first explored in Yb-comprising Zn compounds, i.e., YbB2Zn20\mathrm{YbB}_{2}\mathrm{Zn}_{20} where BB is a transition metal [15, 16] but more recently in site-mixed Yb/Ce/Sm [17].

Many more compounds in the AB2C20\mathrm{AB}_{2}\mathrm{C}_{20} family have naturally been explored for their magnetic properties since the elements AA and BB are transition metals and/or rare earth metals that exhibit magnetism. The vast majority of them comprise a rare earth element (lanthanide or actinide) as the AA element [4, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38]. Very few have a transition metal as the AA element; only with zirconium [39] and hafnium [5]. A few compounds have yttrium as the AA element [19, 40, 41], however, Y is generally considered a rare earth element. The BB element, on the other hand, is always a transition metal. The compounds which have manganese as the BB element, i.e., the AMn2Zn20\mathrm{AMn}_{2}\mathrm{Zn}_{20} compounds, have been shown to exhibit itinerant magnetism [28, 39, 40, 41, 42]. Interestingly, they have all been reported as non-stoichiometric: while Al or In was added to the AMn2Zn20\mathrm{AMn}_{2}\mathrm{Zn}_{20} (AA = Y, Ce, Pr, Nd, Sm, Gd, Dy, Er, Yb) resulting in Al/Zn or In/Zn mixing [40, 41, 43], the ZrMn2Zn20\mathrm{ZrMn}_{2}\mathrm{Zn}_{20} exhibits a mixed Mn/Zn site [39], i.e., Zn mixing with Mn in its site residing within a cage.

Itinerant magnetism arises due to the itinerancy – or movement – of electrons, resulting in a magnetic behavior governed by the collective motion of electrons throughout the lattice instead of localized magnetic moments associated with individual ions. The magnetic moments in such materials come from the spins of the itinerant electrons aligning, therefore, lowering the effective magnetic moment (when compared to that from localized magnetism) since the moments are determined by the collective behavior of the electrons and not exclusively by the individual, localized ions.

In this work, we report on the discovery, single crystal growth, and magnetic properties of a new compound in this family, HfMn2Zn20\mathrm{HfMn}_{2}\mathrm{Zn}_{20}, which, similar to its Zr analog, exhibits Mn/Zn mixing. We show that the structure of this new compound follows the expected lattice size trend when compared to the existing HfM2Zn20\mathrm{HfM}_{2}\mathrm{Zn}_{20} (MM = Fe, Co, and Ni) [5] with deviations that can be explained by the Mn/Zn mixing. In addition, our magnetic study confirms the itinerant nature of this compound.

Methods

Synthesis. Single crystals of HfMn2Zn20\mathrm{HfMn}_{2}\mathrm{Zn}_{20} were grown via the self-flux method. Elements (>99.9%>99.9\%) were measured in atomic ratio of 1:2:60 Hf:Mn:Zn and loaded in a 2 ml alumina crucible, where the excess zinc acts as flux and provides enough reaction bath despite its boil-off at higher temperatures. A second alumina crucible was filled with quartz wool and put as a cap on the top of the reaction crucible. The two crucibles were then placed in a quartz ampoule. To ensure inert conditions of the reaction, the entire assembly was done inside an argon-filled glovebox. The quartz ampoule was subsequently sealed under vacuum using an oxygen-hydrogen torch and put inside a muffle furnace. The reaction was heated up at 800°C at a rate of 80°C/h, maintained at 800°C for 20 hours, and then slowly cooled to 550°C at a rate of 3°C/h. After completion of the temperature cycle, the quartz ampoule was rapidly taken out of the furnace, flipped upside down, and centrifuged to segregate the crystal from excess molten flux. After centrifuging and cooling, the quartz was broken to extract the crystals from inside the crucible. The extracted crystals had a layer of extra flux on their surface which was etched away with highly dilute HCl solution which attack elemental zinc at a higher rate than the crystals.

Energy dispersion spectroscopy. For energy dispersive spectroscopy (EDS)-based elemental analysis, a FEI QUANTA 200 FEG scanning electron microscope (SEM) equipped with an Oxford Instruments Ultim Max EDS detector was used. Several crystals of different sizes and shapes were picked to confirm the stoichiometry of the compound. All the crystals were fixed on copper tape so that a flat surface faced up.

Single crystal X-ray diffraction. Single-crystal X-ray diffraction was performed with a Rigaku-Oxford Diffraction XtaLAB Synergy-S diffractometer equipped with a HyPix-6000HE Hybrid Photon Counting detector and dual PhotonJet-S Mo/Cu 50W Microfocus X-ray sources. Data were collected at room temperature with Mo KαK\alpha radiation (λ=0.71073\lambda= 0.71073 Å) using ω\omega scans with 0.5° frame widths to a resolution of 0.5 Å, equivalent to 2θ≈90∘2\theta\approx90^\circ. Reflections were recorded, indexed, and corrected for absorption using Rigaku Oxford Diffraction CrysAlisPro [44]. The structure refinement was done with CRYSTALS [45], employing the charge-flipping software SUPERFLIP [46] to solve the structure. The data quality permitted an unconstrained full matrix refinement against F2F^2 (the square of the structure factors which are directly proportional to the scattered intensities) with anisotropic displacement parameters for all atoms. A CIF has been deposited with the Cambridge Crystallographic Data Center (CSD #2212294) [47].

Powder X-ray diffraction. Powder X-ray diffraction was performed with a Bruker Discover D8 in a Bragg-Brentano geometry, operating at 40 kV and 40 mA. A pattern was collected at room temperature with Cu KαK\alpha radiation (λ=1.541\lambda= 1.541 Å) in approximately 0.02° steps from 10° to 90° in 2θ2\theta. The sample comprised several clean crystals that were finely ground and deposited on a glass slide. The pattern was refined with the Rietveld method using the Bruker software TOPAS [48].

Magnetization. Magnetic measurements were done in a Quantum Design MPMS-3 system at the Cornell Center for Materials Research. Magnetization as a function of temperature was obtained at an applied field of 0.1 T and the temperature was swept at a rate of approximately 0.1 K/s from 1.8 K to 300 K. Magnetization as a function of field was obtained at temperatures 1.8 K and 300 K and the field was swept at a rate of approximately 50 Oe/s. All measurements were done on a zero field-cooled single crystal of approximately 14.6 mg.

Result and discussion

Structure

Several crystals of various sizes were grown out of the flux. The crystals exhibit in general an octahedral morphology (double pyramid shape), with the largest crystal approximately 1.5 mm long. Single crystal X-ray diffraction reveals that this compound crystallizes in the cubic space group Fd3ˉm\mathit{Fd}\bar{3}m (Z=8Z = 8), isostructural with all other members of the AB2C20AB_{2}C_{20} family [3, 5], comprising of one Hf site, one Mn site, and three distinct Zn sites. The unit cell comprises large cages (“voids”) of Zn with Hf in the center of a 16-atom coordinated Frank-Kasper polyhedron formed by twelve Zn1 and four Zn3, and Mn in the center of a 12-coordinated icosahedron formed by six Zn1 and six Zn2. All cages are corner-shared via Zn atoms. The Hf-centered Frank-Kasper polyhedra are corner-shared with each other via the Zn3 atoms, the Mn-centered icosahedra are corner-shared with each other via the Zn2 atoms, and the two different polyhedra are corner-shared with each other via the Zn1 atoms. This results in a Hf–Hf distance of 6.086 Å, a Mn–Mn distance of 4.969 Å, and a Hf–Mn distance of 5.827 Å. These structures have also been previously described in detail [3, 5, 16, 39]. Figure 1(a) shows the unit cell along [110] with the Frank-Kasper polyhedra in blue and the icosahedra in purple. Figure 1(b) shows an image of the crystal, obtained with a scanning electron microscope in backscatter mode. Figure 2 displays the two polyhedra along [111].

Unit cell of HfMn₂Zn₂₀ and SEM image of a crystal

Figure 1. (a) Unit cell of HfMn₂Zn₂₀ viewed along [110]. The structure image was generated with CrystalMaker [49]. (b) SEM image of a crystal of HfMn₂Zn₂₀ in backscatter mode.

Figure 2. View along [111] of (a) the Frank-Kasper polyhedron with Hf in the center and (b) the icosahedron with Mn/Zn in the center. Colors are the same as in Figure 1.

The initial structural refinement based on the stoichiometric ratios resulted in good residuals (R1=0.0273R_1 = 0.0273 and wR2=0.0723wR_2 = 0.0723), however, the elemental composition as obtained via EDS deviated enough from the stoichiometric 1:2:20 of HfMn2_2Zn20_{20} to raise concerns, despite the fairly large error margin of EDS. Furthermore, Svanidze et al. [39] reported off-stoichiometry in the Zr-analog, ZrMn1.78_{1.78}Zn20.22_{20.22}, which exhibited Mn/Zn site mixing on the 16d site (the Mn site). We performed EDS measurements on several spots and areas on multiple crystals, and the average results are summarized in Table 1 together with calculated standard error of the mean. As can be seen, the Hf average value is within the ideal value. Mn, on the other hand, is lacking, and Zn is in excess. The EDS thus indicates a composition of Hf1.03±0.05_{1.03\pm0.05}Mn1.75±0.03_{1.75\pm0.03}Zn20.21±0.04_{20.21\pm0.04}.

ElementsAtomic percentageIdeal ratios
Hf4.5±0.24.5 \pm0.24.3494.349
Mn7.6±0.17.6 \pm0.18.6968.696
Zn87.9±0.287.9 \pm0.286.9686.96
CompositionHf1.03±0.05_{1.03\pm0.05}Mn1.75±0.03_{1.75\pm0.03}Zn20.21±0.04_{20.21\pm0.04}HfMn2_2Zn20_{20}

Table 1. Averages of the EDS results obtained on multiple crystals together with ratios based on the ideal 1:2:20 composition.

Further refinement on the X-ray diffraction data revealed indeed a Mn/Zn mixing on the 16d site. Unlike the Zr-analog, however, we also observe an underoccupied 8a site (the Hf site). It is not uncommon to observe Zr mixing in Hf sites since there is typically a nominal amount of Zr in Hf chemicals. EDS, however, revealed no Zr. It is not clear why the Hf site is underoccupied as there is no clear reason for Zn to site-mix with Hf. Nevertheless, the residuals improved remarkably and all the crystal data and crystallographic parameters resulting from the single-crystal X-ray diffraction are summarized in Table 2. The final composition refined to Hf0.93_{0.93}Mn1.63_{1.63}Zn20.37_{20.37} (Hf1−δ_{1-\delta}Mn2−_{2-} xZn20+xx\mathrm{Zn}_{20+x}, δ=0.07\delta= 0.07, x=0.37x = 0.37) which is fairly close to the composition found via EDS. For clarity, however, this compound will still be referred to as HfMn2_2Zn20_{20}. Table 3 lists the atomic coordinates.

ParametersHfMn2_2Zn20_{20}
Actual stoichiometryHf0.93_{0.93}Mn1.63_{1.63}Zn20.37_{20.37} (Hf1−δ_{1-\delta}Mn2−x_{2-x}Zn20+x_{20+x}, δ=0.07\delta= 0.07, x=0.37x = 0.37)
Molecular weight (g/mol)1587.61
Space groupFd3ˉmFd\bar{3}m (#227)
aa (Å)14.0543(2) [14.0496]
VV (Å3^3)2776.03(9) [2773.26]
ZZ8
ρcalc\rho_{\mathrm{calc}} (g/cm3^3)7.597 [7.664]
Absorption coefficient μ\mu (mm−1^{-1})42.744
Absorption corrections Tmin⁡T_{\min}, Tmax⁡T_{\max}0.22, 0.30
Crystal size (mm3^3)0.028 x 0.041 x 0.050
Data collection range (°)2.510 < θ\theta < 44.778
hh range−19≤h≤27-19 \le h \le27
kk range−27≤k≤16-27 \le k \le16
ll range−27≤l≤19-27 \le l \le19
Reflections collected5375
Independent reflections587
Parameters refined18
Restraints6
Residual electron density Δρmin⁡\Delta\rho_{\min}, Δρmax⁡\Delta\rho_{\max} (e/Å3^3)-6.36, 3.01
RintR_{\mathrm{int}}0.023
R1(F)R_1(F) for all dataa^{\mathrm{a}}0.0176 [0.0277]
wR2(FO2)bwR_2(F_{\mathrm{O}}^2)^{\mathrm{b}}0.0305 [0.0404]
Goodness-of-fit on F2F^21.0000 [1.67]
CSD #2212294

Table 2. Single crystal X-ray diffraction data and parameters for HfMn2_2Zn20_{20}, collected at room temperature. The values in square brackets are powder X-ray diffraction data from the Rietveld refinement of crushed single crystals.

Table 3. Atomic coordinates, and equivalent displacement parameters of HfMn2_2Zn20_{20}.

AtomSiteSOFxyzUeqU_{\mathrm{eq}} (Å2^2)
Hf8a0.932(2)1/81/81/80.0063(5)
Mn1116d0.816(9)1/21/21/20.0056(4)
Zn1216d0.184(9)1/21/21/20.0056(4)
Zn196g10.06010(2)0.06010(2)0.32312(2)0.0132(9)
Zn248f10.48833(2)1/81/80.0090(1)
Zn316c10000.0148(1)

Table 3.

Figure 3 displays the powder X-ray diffraction pattern obtained after grounding several clean crystals. The red line is a Rietveld refinement of the experimental data and guided by the lattice parameters obtained from the single-crystal X-ray diffraction refinement. All the observed peaks match well with the structure obtained from single-crystal X-ray diffraction refinement and only one spurious peak, belonging to residual zinc, was observed, indicating a single-phase compound. In other words, there were no magnetic impurity compounds present: if there were any such present, their amount was too small to be observed in the powder x-ray diffraction.

Powder X-ray diffraction pattern of ground HfMn2Zn20 crystals

Figure 3. Powder X-ray diffraction pattern of ground HfMn2_2Zn20_{20} crystals. The fit in red matches well with the pattern which indicates no major

impurities. Only a small additional peak indicating residual zinc was observed.

Gross et al. [5] compared the structural parameters of several HfM2Zn20\mathrm{HfM}_{2}\mathrm{Zn}_{20} compounds including M=FeM = \mathrm{Fe}, Co\mathrm{Co}, and Ni\mathrm{Ni} where they showed a lattice constant and unit cell volume reduction consistent with the metallic radius trend of the transition metals [50]. We extend the trend with the addition of HfMn2Zn20\mathrm{HfMn}_{2}\mathrm{Zn}_{20}. Figure 4 displays the trend in lattice parameter and unit cell volume of HfM2Zn20\mathrm{HfM}_{2}\mathrm{Zn}_{20} for M=MnM = \mathrm{Mn}, Fe\mathrm{Fe}, Co\mathrm{Co}, and Ni\mathrm{Ni}. While the metallic radius increases linearly from 1.24 Å for Ni to 1.27 Å for Mn [50], the lattice parameter and the unit cell volume are larger for our HfMn2Zn20\mathrm{HfMn}_{2}\mathrm{Zn}_{20} compound than expected from the linear trend. The reason for this deviation could be due to the Mn/Zn site mixing: the metallic radius of Zn is 1.34 Å, approximately 8.1% larger than the metallic radius of Mn, so that the inclusion of Zn on the Mn-site enlarges the overall unit cell of HfMn2Zn20\mathrm{HfMn}_{2}\mathrm{Zn}_{20} more than expected.

Lattice constant and unit cell volume comparison for HfM2Zn20

Figure 4. Lattice constant (upper panel) and unit cell volume (lower panel) comparison for HfM2Zn20\mathrm{HfM}_{2}\mathrm{Zn}_{20} (red circles) across M=MnM = \mathrm{Mn}, Fe\mathrm{Fe}, Co\mathrm{Co}, and Ni\mathrm{Ni}. The metallic radii are shown on the right axis of the upper panel (open, red diamonds) [50]. Data for the M=FeM = \mathrm{Fe}, Co\mathrm{Co}, and Ni\mathrm{Ni} compounds are taken from Ref. [5]. All error bars are within symbols.

In fact, looking at the volumes of the two polyhedra, we can observe the deviation of the Mn/Zn-containing icosahedron from the linear trend (upper panel in Figure 5). The Frank-Kasper polyhedron containing Hf, on the other hand, shrinks when MM goes from Fe to Mn (lower panel in Figure 5). One reason could be the underoccupied Hf-site, although it is more likely that the overall structure is the real reason: a Frank-Kasper polyhedron is corner-shared with 12 MM-containing icosahedra and only four other Frank-Kasper polyhedra. The Frank-Kasper polyhedron is therefore affected strongly by the relatively larger expansion of the surrounding icosahedra; hence, it is compressed.

Volume of the icosahedron that contains the M atom and volume of the Frank-Kasper polyhedron that contains Hf

Figure 5. Volume of the icosahedron that contains the MM atom (upper panel) and volume of the Frank-Kasper polyhedron that contains Hf (lower panel) across HfM2Zn20\mathrm{HfM}_{2}\mathrm{Zn}_{20} with M=Mn,Fe,Co,M = \mathrm{Mn}, \mathrm{Fe}, \mathrm{Co}, and Ni\mathrm{Ni}. Data for the M=Fe,Co,M = \mathrm{Fe}, \mathrm{Co}, and Ni\mathrm{Ni} compounds are taken from Ref. [5]. All error bars are within symbols.

Magnetic properties

Figure 6 displays the zero field-cooled magnetic susceptibility as a function of temperature at an applied field of 0.1 T. This field was chosen since low magnetization was expected due to the nature of the structure: Mn ions completely surrounded by non-magnetic Zn ions and with a large Mn–Mn distance of 4.969 Å. The derivative (solid line) indicates two transitions: one at approximately 22.3 K and one at approximately 8.7 K. A similar low-temperature transition was observed in the analogous ZrMn2Zn20\mathrm{ZrMn}_{2}\mathrm{Zn}_{20} [39] at approximately 10 K which was attributed to ferromagnetic impurities. The transition appearing at 8.7 K in the derivative curve is likely due to the onset of saturation of the susceptibility, which is onsetting at approximately 16 K. Saturation of susceptibility is expected to take place in ferromagnets [51]. The saturation, however, is interrupted by a small upturn in susceptibility at approximately 3 K. This upturn is hard to explain: while a majority of the literature with magnetic measurements tends to explain such small upturns with the presence of small ferromagnetic impurities, our powder x-ray diffraction (Figure 3), indicated no presence of secondary phases. If any such impurities resulted from the synthesis, they must be incredibly small to not appear in the powder x-ray diffraction, and therefore contribute very little to the overall magnetization of this sample. Another reason for this upturn could be due to the appearance of a low-field saturation of the magnetization, discussed below. The magnetization behavior is clearly non-Curie-Weiss as can be seen by the inverse susceptibility as a function of temperature (inset to Figure 6). The lack of Curie-Weiss behavior together with two transitions were also observed in the ZrMn2_2Zn20_{20} analog [39] where it was also noted that these behaviors were reminiscent of other compounds containing Mn [52]. The susceptibility, in fact, seems to follow the modified Curie-Weiss behavior [53]

Zero field-cooled magnetic susceptibility as a function of temperature

Figure 6. Zero field-cooled magnetic susceptibility as a function of temperature from 1.8 K to 300 K (although only up to 100 K is shown), obtained at an applied field of 0.1 T. The red solid line (right axis) is the derivative of the susceptibility. Inset: inverse susceptibility as a function of temperature. The green solid line is a fit to the modified Curie-Weiss law.

χ=CT−θ+χ0(1)\chi= \frac{C}{T-\theta}+\chi_0 \tag*{(1)}

in the region above the transition temperature. Here, θ\theta is a Curie-Weiss temperature, χ0\chi_0 is a temperature-independent term, and CC is the Curie constant and is related to the effective moment μeff\mu_{\mathrm{eff}} via

C=NAμB2μeff23kB.(2)C = \frac{N_{\mathrm{A}}\mu_{\mathrm{B}}^2\mu_{\mathrm{eff}}^2}{3k_{\mathrm{B}}}. \tag*{(2)}

The susceptibility data above the transition temperature fits Eqs. (1) and (2) moderately well with the fit displayed in the large inset to Figure 6 as a green, solid line. The fit yields the effective moment μeff≈0.222(2) μB/f.u.\mu_{\mathrm{eff}} \approx0.222(2)\ \mu_{\mathrm{B}}/\mathrm{f.u.}, the Curie-Weiss temperature θ≈21.8(2) K\theta\approx21.8(2)\ \mathrm{K}, and χ0≈3.73(8) μB/f.u.\chi_0 \approx3.73(8)\ \mu_{\mathrm{B}}/\mathrm{f.u.}, although the error margins are likely larger due to uncertainty in the sample mass. Nevertheless, the positive Curie-Weiss temperature indicates that the transition is possibly of a ferromagnetic nature with a TC≈22.3 KT_{\mathrm{C}} \approx22.3\ \mathrm{K} as obtained from the derivative. Since the magnetic ion is manganese, the effective moment can be written μeff≈0.111(2) μB/Mn\mu_{\mathrm{eff}} \approx0.111(2)\ \mu_{\mathrm{B}}/\mathrm{Mn} if assuming stoichiometric HfMn2_2Zn20_{20} or μeff≈0.137(2) μB/Mn\mu_{\mathrm{eff}} \approx0.137(2)\ \mu_{\mathrm{B}}/\mathrm{Mn} if assuming Hf0.93_{0.93}Mn1.63_{1.63}Zn20.37_{20.37}. In any case, we note that the effective moment is quite small for Mn.

Figure 7 displays the magnetization as a function of applied field at 1.8 K and at 300 K. No high-field saturation is observed even at the lowest temperature (1.8 K) and highest applied field (6 T); the moment at 1.8 K and 6 T is quite small, approximately 9.9⋅10−39.9 \cdot10^{-3} μB\mu_{\mathrm{B}}/f.u. In addition, hysteresis in the 1.8 K isotherm is very small, essentially negligible (upper inset to Figure 7). All of these features – no saturation, small magnetic moment, and lack of hysteresis – have been taken as evidence for itinerant magnetism in the analogous ZrMn2_2Zn20_{20} compound [39, 42]. HfMn2_2Zn20_{20} is, therefore, also a likely candidate for itinerant ferromagnetism.

Image not extracted

Figure 7. Magnetization as a function of applied field, obtained at 1.8 K (black circles) and 300 K (red diamonds). Upper inset: Close-up around zero field showing the low-field saturation and the near-negligible hysteresis at 1.8 K. Lower inset: Magnetization curve above zero applied field. The solid green line is a fit to Eq. (3) (see main text).

The isotherm at 1.8 K experiences a small but steep rise (upper inset to Figure 7) before a so-called low-field saturation (the bend in the isotherm) sets in at approximately 0.015 T. A spontaneous magnetization at 1.8 K, i.e., MSP=M(H=0)M_{\mathrm{SP}} = M(H = 0), can be obtained by fitting M(H)M(H) above the low-field saturation to the expression [54, 55]

M(H)=MSP+aH+χhfH,(3)M(H) = M_{\mathrm{SP}} + a\sqrt{H} + \chi_{\mathrm{hf}}H, \tag*{(3)}

where the middle term is related to the field-suppression of spin waves and χhf\chi_{\mathrm{hf}} is the high-field susceptibility. The fit is displayed in the lower inset to Figure 7 as a green, solid line with parameters MSP≈2.84(5)⋅10−4 μB/f.u.M_{\mathrm{SP}} \approx2.84(5)\cdot10^{-4}\,\mu_{\mathrm{B}}/\mathrm{f.u.}, a≈2.08(7)⋅10−3 μB/f.u.⋅T1/2a \approx2.08(7)\cdot10^{-3}\,\mu_{\mathrm{B}}/\mathrm{f.u.}\cdot\mathrm{T}^{1/2}, and χhf≈7.45(3)⋅10−4 μB/f.u.⋅T\chi_{\mathrm{hf}} \approx7.45(3)\cdot10^{-4}\,\mu_{\mathrm{B}}/\mathrm{f.u.}\cdot\mathrm{T}. In these units, MSPM_{\mathrm{SP}} is the spontaneous magnetic moment: μSP≈2.84(5)⋅10−4 μB/f.u.\mu_{\mathrm{SP}} \approx2.84(5)\cdot10^{-4}\,\mu_{\mathrm{B}}/\mathrm{f.u.}. This spontaneous magnetic moment is very small, as can also be seen in the upper inset to Figure 7. Extending the magnetization just above the initial bend linearly to zero field yields low values.

The nature of the magnetism can be probed further with the so-called Rhodes-Wohlfarth ratio μC/μS\mu_C/\mu_S where μC\mu_C is the number of magnetic carriers in the paramagnetic state (i.e., at high temperatures) and μS\mu_S is the number of magnetic carriers in the ordered state (i.e., at low temperatures) [42, 56]. The Rhodes-Wohlfarth ratio shows how the number of magnetic carriers changes from high to low temperature. For local magnetism, μC/μS=1\mu_C/\mu_S = 1, while for itinerant magnetism, μC/μS≫1\mu_C/\mu_S \gg1. The μC\mu_C is related to the paramagnetic moment and therefore the effective magnetic moment that was obtained in Eqns. (1) and (2). The relation can be expressed as [42, 56, 57]

μeff2=μC(μC+2)(4)\mu_{\mathrm{eff}}^{2} = \mu_C(\mu_C + 2) \tag*{(4)}

and yields μC≈0.0244 μB\mu_C \approx0.0244\ \mu_B/f.u. The μS\mu_S is related to the saturated magnetic moment via

μsat=2μS(5)\mu_{\mathrm{sat}} = 2\mu_S \tag*{(5)}

and can be obtained at low temperatures and high fields. This is not the spontaneous magnetic moment that was obtained via Eqn. (3) since that value is related to the steep rise and low-field saturation. We, as stated above, do not observe an actual saturation of the magnetization (see Figure 7), a situation similar to the itinerant compound ZrMn2_2Zn20_{20} [39]. Instead, we estimate by using the magnetization value at the highest field and lowest temperature we noted earlier: 0.03496 emu/g, corresponding to a “saturation” magnetic moment of 0.00994 μB\mu_B/f.u. This then yields μS≈0.00497 μB\mu_S \approx0.00497\ \mu_B/f.u. With these values, we obtain the Rhodes-Wohlfarth ratio μC/μS≈4.91\mu_C/\mu_S \approx4.91, which is reasonably large and clearly shows that the magnetism in HfMn2_2Zn20_{20} is of itinerant nature. This value is added to the Rhodes-Wohlfarth plot of μC/μS\mu_C/\mu_S vs. TCT_C [57] depicted in Figure 8(a), comparing several itinerant magnetism compounds.

Rhodes-Wohlfarth and Deguchi-Takahashi plots

Figure 8. (a) Rhodes-Wohlfarth plot of μC/μS\mu_C/\mu_S vs. TCT_C for various compounds with our compound as a red square. The plot was obtained from Ref. [57]. (b) Deguchi-Takahashi plot of μeff/μS\mu_{\mathrm{eff}}/\mu_S vs. TC/T0T_C/T_0 for various compounds with our compound as a red square. The plot was obtained from Ref. [66]. Note that the authors in both references use the letter pp to denote magnetic moment while we employ the more commonly used μ\mu.

The itinerant magnetism of this sample can be probed further with the spin fluctuation theories developed by Takahashi and Moriya [57, 58, 59, 60, 61, 62, 63, 64] which built on the earlier Stoner criterion [65]. These theories have been explored in detail for several itinerant compounds [55, 57, 62, 63, 64, 66, 67, 68, 69, 70, 71, 72]. Starting from minimization of the Landau expansion of the free energy, a relation is found between the magnetization and the applied field,

H=F1NA3(2μB)4M(M2−MSP2),(6)H = \frac{F_1}{N_A^3(2\mu_B)^4}M(M^2-M_{SP}^2), \tag*{(6)}

where MSPM_{SP} is the spontaneous magnetization and F1F_1 is a mode-mode coupling term and expressed in terms of spin fluctuation parameters T0T_0 and TAT_A [57, 62, 64]. Here, T0T_0 represents the energy width of the dynamical spin fluctuation spectrum and TAT_A the dispersion of the static magnetic susceptibility in wave vector space. Importantly, F1F_1 can be evaluated experimentally via

F1=NA3(2μB)4kBζ,(7)F_1 = \frac{N_A^3(2\mu_B)^4}{k_B\zeta}, \tag*{(7)}

where ζ≈6.83⋅10−9 (μB/f.u.)3/T\zeta\approx6.83 \cdot10^{-9}\,(\mu_B/\mathrm{f.u.})^3/\mathrm{T} is the slope of the Arrott plot M2M^2 vs. H/MH/M [73] (not shown). The spin fluctuation parameters can then be expressed in terms of TCT_C, MSPM_{SP}, and F1F_1 as [57, 62, 64]

(TCT0)5/6=MSP240C4/3(15F1TC)1/2(8)\left(\frac{T_C}{T_0}\right)^{5/6} = \frac{M_{SP}^2}{40C_{4/3}}\left(\frac{15F_1}{T_C}\right)^{1/2} \tag*{(8)}
(TCTA)5/3=MSP220C4/3(4TC15F1)1/3(9)\left(\frac{T_C}{T_A}\right)^{5/3} = \frac{M_{SP}^2}{20C_{4/3}}\left(\frac{4T_C}{15F_1}\right)^{1/3} \tag*{(9)}

where C4/3≈1.006089C_{4/3} \approx1.006089 is a constant. With these expressions, Takahashi [57] showed that the degree of localization or itinerancy can be characterized by the ratio TC/T0T_C/T_0: if the ratio is equal to unity, the compound has local magnetism while if TC/T0≪1T_C/T_0 \ll1, the compound has itinerant magnetism. Using Eqns. (7) and (8), together with the TCT_C found from Figure 6 and the MSPM_{SP} obtained via Eqn. (3), we obtain the ratio TC/T0≈0.0043T_C/T_0 \approx0.0043, thus, again proving that HfMn2_2Zn20_{20} experiences itinerant magnetism. Furthermore, a generalized Rhodes-Wohlfarth plot – a Deguchi-Takahashi plot – was constructed out of experimental data showing the relation [57]

μeffμS≈1.4(TCT0)−2/3.(10)\frac{\mu_{\mathrm{eff}}}{\mu_S} \approx1.4\left(\frac{T_C}{T_0}\right)^{-2/3}. \tag*{(10)}

Using the calculated ratio of TC/T0T_C/T_0, we obtain μeff/μS≈53\mu_{\mathrm{eff}}/\mu_S \approx53 and using the previously calculated μeff\mu_{\mathrm{eff}} and μS\mu_S, we obtain μeff/μS≈45\mu_{\mathrm{eff}}/\mu_S \approx45, in fairly good agreement with each other. The Deguchi-Takahashi plot [57, 66] is shown in Figure 8(b) with our value added.

Conclusion

In conclusion, we have discovered a new member of the AB2C20\mathrm{AB}_2\mathrm{C}_{20} family: HfMn2Zn20\mathrm{HfMn}_2\mathrm{Zn}_{20}. Due to Mn/Zn mixing on the Mn-site and an underoccupied Hf-site, the final stoichiometry is Hf0.93Mn1.63Zn20.37\mathrm{Hf}_{0.93}\mathrm{Mn}_{1.63}\mathrm{Zn}_{20.37} (Hf1−δMn2−xZn20+x\mathrm{Hf}_{1-\delta}\mathrm{Mn}_{2-x}\mathrm{Zn}_{20+x}, δ=0.07\delta= 0.07, x=0.37x = 0.37). This Mn-site mixing was also observed in the Zr-analog. The structure of the new compound follows expected lattice size trends when compared to existing isostructures with Hf and first-row transition metals. The magnetic susceptibility follows the modified Curie-Weiss law with a transition temperature around 22 K. The magnetization as a function of applied field shows no saturation, a small magnetic moment, and near negligible hysteresis, all signs of itinerant magnetism. The Rhodes-Wohlfarth ratio μC/μS\mu_C/\mu_S is approximately 4.91 and the spin fluctuation parameters ratio TC/T0T_C/T_0 approximately 0.0043, both of these confirming the itinerant nature of the magnetism in HfMn2Zn20\mathrm{HfMn}_2\mathrm{Zn}_{20}.

Acknowledgement

The authors acknowledge the NSF MRI program that funded the purchase of the Synergy-S X-ray diffractometer via award CHE-2117129. This work made use of a Quantum Design MPMS-3 supported by NSF (DMR-1920086) and the Cornell Center for Materials Research Shared Facilities which are supported through the NSF MRSEC program (DMR-1719875). T.B. also acknowledges financial support provided by Missouri State University’s new faculty startup fund.

References

  1. [1]P. I. Kripyakevich and O. S. Zarechnuyk, "RCr₂Al₂₀ Compounds in Systems of Rare Earth Metals and Calcium, and their Crystal Structures" Dopov. Akad. Nauk Ukr. RSR, Ser. A 30 364-367 (1968).
  2. [2]S. Niemann and W. Jeitschko, "Ternary Aluminides AT₂Al₂₀ (A = Rare Earth Elements and Uranium; T = Ti, Nb, Ta, Mo, and W) with CeCr₂Al₂₀-type Structure" J. Solid State Chem. 114 337-341 (1995).DOI
  3. [3]T. Nasch, W. Jeitschko, and U. C. Rodewald, "Ternary Rare Earth Transition Metal Zinc Compounds RT₂Zn₂₀ with T = Fe, Ru, Co, Rh, and Ni" Z. Naturforsch. B 52 1023-1030 (1997).DOI
  4. [4]V. M. T. Thiede, W. Jeitschko, S. Niemann, and T. Ebel, "EuTa₂Al₂₀, Ca₆W₄Al₄₃ and Other Compounds with CeCr₂Al₂₀ and Ho₆Mo₄Al₄₃ Type Structures and Some Magnetic Properties of These Compounds" J. Alloy. Comp. 267 23-31 (1998).DOI
  5. [5]N. Gross, T. Nasch, and W. Jeitschko, "Ternary Intermetallics with High Zinc Content: TT′₂Zn₂₀ (T = Zr, Hf, Nb; T′ = Mn, Fe, Ru, Co, Rh, Ni) with CeCr₂Al₂₀-type Structure" J. Solid State Chem. 161 288-293 (2001), 10.1006/jssc.2001.9311.
  6. [6]N. Nakamura, R. Higashinaka, Y. Aoki, H. Sato, and T. D. Matsuda, "Superconducting Properties of Cage Compounds YbTr₂Al₂₀ with Tr = Mo and Ta" Solid State Commun. 363 (2023), 10.1016/j.ssc.2023.115098.DOI
  7. [7]M. J. Winiarski, B. Wiendlocha, M. Sternik, P. Wiśniewski, J. R. O’Brien, D. Kaczorowski, and T. Klimczuk, "Rattling-enhanced Superconductivity in MV₂Al₂₀ (M = Sc, Lu, Y) Intermetallic Cage Compounds" Phys. Rev. B 93 (2016), 10.1103/PhysRevB.93.134507.DOI
  8. [8]Z. Hiroi, A. Onosaka, Y. Okamoto, J. Yamaura, and H. Harima, "Rattling and Superconducting Properties of the Cage Compound GaₓV₂Al₂₀" J. Phys. Soc. Jpn. 81 (2012), 10.1143/jpsj.81.124707.DOI
  9. [9]A. Onosaka, Y. Okamoto, J.-i. Yamaura, and Z. Hiroi, "Superconductivity in the Einstein Solid AₓV₂Al₂₀ (A = Al and Ga)" J. Phys. Soc. Jpn. 81 (2012), 10.1143/JPSJ.81.023703.DOI
  10. [10]T. Klimczuk, M. Szlawska, D. Kaczorowski, J. R. O’Brien, and D. J. Safarik, "Superconductivity in the Einstein Solid VAl₁₀.₁" J. Phys.: Condens. Matter 24 (2012), 10.1088/0953-8984/24/36/365701.DOI
  11. [11]D. J. Safarik, T. Klimczuk, A. Llobet, D. D. Byler, J. C. Lashley, J. R. O’Brien, and N. R. Dilley, "Localized Anharmonic Rattling of Al Atoms in VAl₁₀.₁" Phys. Rev. B 85 (2012), 10.1103/PhysRevB.85.014103.DOI
  12. [12]A. Sakai, K. Kuga, and S. Nakatsuji, "Superconductivity in the Ferroquadrupolar State in the Quadrupolar Kondo Lattice PrTi₂Al₂₀" J. Phys. Soc. Jpn. 81 (2012), 10.1143/JPSJ.81.083702.DOI
  13. [13]T. Onimaru et al., "Superconductivity and Structural Phase Transitions in Caged Compounds RT₂Zn₂₀ (R = La, Pr, T = Ru, Ir)" J. Phys. Soc. Jpn. 79 (2010), 10.1143/jpsj.79.033704.
  14. [14]T. Onimaru, N. Nagasawa, K. T. Matsumoto, K. Wakiya, K. Umeo, S. Kittaka, T. Sakakibara, Y. Matsushita, and T. Takabatake, "Simultaneous Superconducting and Antiferroquadrupolar Transitions in PrRh₂Zn₂₀” Phys. Rev. B 86 (2012), 10.1103/PhysRevB.86.184426.
  15. [15]E. D. Mun, S. Jia, S. L. Bud'ko, and P. C. Canfield, ”Thermoelectric Power of the YbₓT₂Zn₂₀ (T = Fe, Ru, Os, Ir, Rh, and Co) Heavy Fermions” Phys. Rev. B 86 (2012), 10.1103/PhysRevB.86.115110.DOI
  16. [16]K. Wei, J. N. Neu, Y. Lai, K.-W. Chen, D. Hobbis, G. S. Nolas, D. E. Graf, T. Siegrist, and R. E. Baumbach, ”Enhanced Thermoelectric Performance of Heavy-fermion Compounds YbₓTM₂Zn₂₀ (TM = Co, Rh, Ir) at Low Temperatures” Sci. Adv. 5 (2019), 10.1126/sciadv.aaw6183.DOI
  17. [17]J. R. Galeano-Cabral et al., ”Enhanced Thermoelectric Properties of Heavy-fermion Compounds YbₓCeᵧSm𝓏Ir₂Zn₂₀ (x + y + z = 1)” Phys. Rev. Mater. 7 (2023), 10.1103/PhysRevMaterials.7.025406.
  18. [18]E. D. Bauer, A. D. Christianson, J. S. Gardner, V. A. Sidorov, J. D. Thompson, J. L. Sarrao, and M. F. Hundley, ”Physical Properties of the Ferromagnetic Heavy-fermion Compound UIr₂Zn₂₀” Phys. Rev. B 74 (2006), 10.1103/PhysRevB.74.155118.DOI
  19. [19]S. Jia, S. L. Bud’ko, G. D. Samolyuk, and P. C. Canfield, ”Nearly Ferromagnetic Fermi-liquid Behaviour in YFe₂Zn₂₀ and High-temperature Ferromagnetism of GdFe₂Zn₂₀” Nature Phys. 3 334-338 (2007), 10.1038/nphys568.DOI
  20. [20]S. Jia, N. Ni, S. L. Bud’ko, and P. C. Canfield, ”Magnetic Properties of GdₓY₁₋ₓFe₂Zn₂₀: Dilute, Large-S Moments in a Nearly Ferromagnetic Fermi Liquid” Phys. Rev. B 76 (2007), 10.1103/PhysRevB.76.184410.DOI
  21. [21]Y. Verbovytsky, K. Łątka, and K. Tomala, ”The Crystal Structure and Magnetic Properties of the GdV₂Al₂₀ and GdCr₂Al₂₀ Ternary Compounds” J. Alloy. Comp. 442 334-336 (2007), 10.1016/j.jallcom.2006.07.148.
  22. [22]S. Jia, N. Ni, G. D. Samolyuk, A. Safa-Sefat, K. Dennis, H. Ko, G. J. Miller, S. L. Bud’ko, and P. C. Canfield, ”Variation of the Magnetic Ordering in GdT₂Zn₂₀ (T=Fe, Ru, Os, Co, Rh and Ir) and Its Correlation with the Electronic Structure of Isostructural YT₂Zn₂₀” Phys. Rev. B 77 (2008), 10.1103/PhysRevB.77.104408.DOI
  23. [23]P. C. Canfield, S. Jia, E. D. Mun, S. L. Bud’ko, G. D. Samolyuk, and M. S. Torikachvili, ”Myriad of Correlated Electron Effects Found in the RT₂Zn₂₀ Family” Phys. B: Condens. Matter 403 844-846 (2008), 10.1016/j.physb.2007.10.234.
  24. [24]S. Jia, N. Ni, S. L. Bud’ko, and P. C. Canfield, ”Magnetic Properties of RFe₂Zn₂₀ and RCo₂Zn₂₀ (R=Y, Nd, Sm, Gd-Lu)” Phys. Rev. B 80 (2009), 10.1103/PhysRevB.80.104403.DOI
  25. [25]S. Yoshiuchi et al., ”Heavy Fermion State in YbIr₂Zn₂₀” J. Phys. Soc. Jpn. 78 (2009), 10.1143/jpsj.78.123711.DOI
  26. [26]W. Tian, A. D. Christianson, J. L. Zarestky, S. Jia, S. L. Bud’ko, P. C. Canfield, P. M. B. Piccoli, and A. J. Schultz, ”Magnetic Order in TbCo₂Zn₂₀ and TbFe₂Zn₂₀” Phys. Rev. B 81 (2010), 10.1103/PhysRevB.81.144409.DOI
  27. [27]C. H. Wang et al., ”Neutron Scattering and Scaling Behavior in URu₂Zn₂₀ and YbFe₂Zn₂₀” Phys. Rev. B 82 (2010), 10.1103/PhysRevB.82.184407.DOI
  28. [28]C. H. Wang et al., ”Unusual Signatures of the Ferromagnetic Transition in the Heavy Fermion Compound UMn₂Al₂₀” Phys. Rev. B 82 (2010), 10.1103/PhysRevB.82.094406.DOI
  29. [29]Y. Hirose et al., ”Metamagnetic Transition in Heavy Fermion Compounds YbTb₂Zn₂₀ (T : Co, Rh, Ir)” J. Phys.: Conf. Ser. 273 (2011), 10.1088/1742-6596/273/1/012003.DOI
  30. [30]A. Sakai and S. Nakatsuji, ”Strong valence fluctuation effects in SmTr₂Al₂₀ (Tr=Ti, V, Cr)” Phys. Rev. B 84 (2011), 10.1103/PhysRevB.84.201106.DOI
  31. [31]M. J. Kangas, D. C. Schmitt, A. Sakai, S. Nakatsuji, and J. Y. Chan, ”Structure and Physical Properties of Single Crystal PrCr₂Al₂₀ and CeM₂Al₂₀ (M=V, Cr): A Comparison of Compounds Sdopting the CeCr₂Al₂₀ Structure Type” J. Solid State Chem. 196 274-281 (2012), 10.1016/j.jssc.2012.06.035.
  32. [32]P. Swatek and D. Kaczorowski, ”Magnetic and Electrical Properties of UCr₂Al₂₀ Single Crystals” J. Solid State Chem. 191 191-194 (2012), 10.1016/j.jssc.2012.03.018.DOI
  33. [33]N. Kase, Y. Shimura, S. Kittaka, T. Sakakibara, S. Nakatsuji, T. Nakano, N. Takeda, and J. Akimitsu, ”Antiferromagnetic Transition of the Caged Compound TmTi₂Al₂₀” J. Phys.: Conf. Ser. 592 (2015), 10.1088/1742-6596/592/1/012052.DOI
  34. [34]K. Wakiya, K. T. Matsumoto, T. Onimaru, K. Umeo, and T. Takabatake, ”Ferromagnetic Transition in a Caged Compound NdOs₂Zn₂₀” Phys. Procedia 75 511-515 (2015), 10.1016/j.phpro.2015.12.064.DOI
  35. [35]Y. Hirose, H. Doto, F. Honda, D. Li, D. Aoki, Y. Haga, and R. Settai, ”New Heavy-fermion Antiferromagnet UPd₂Cd₂₀” J. Phys.: Condens. Matter 28 (2016), 10.1088/0953-8984/28/42/425601.DOI
  36. [36]M. J. Winiarski, J. C. Griveau, E. Colineau, K. Wochowski, P. Wiśniewski, D. Kaczorowski, R. Caciuffo, and T. Klimczuk, ”Synthesis and properties of AxV₂Al₂₀ (A = Th, U, Np, Pu) ternary actinide aluminides” J. Alloy. Comp. 696 1113-1119 (2017), 10.1016/j.jallcom.2016.12.033.DOI
  37. [37]M. J. Winiarski and T. Klimczuk, ”Synthesis and properties of HoT₂Al₂₀ (T = Ti, V, Cr) intermetallic cage compounds” Intermetallics 85 103-109 (2017), 10.1016/j.intermet.2017.02.005.DOI
  38. [38]M. J. Winiarski and T. Klimczuk, ”Crystal structure and low-energy Einstein mode in ErV₂Al₂₀ intermetallic cage compound” J. Solid State Chem. 245 10-16 (2017), 10.1016/j.jssc.2016.09.029.DOI
  39. [39]E. Svanidze, M. Kindy II, C. Georgen, B. W. Fulfer, S. H. Lapidus, J. Y. Chan, and E. Morosan, ”Magnetic and Crystallographic Properties of ZrM₂-dZn₂₀+d (M = Cr-Cu)” J. Magn. Magn. Mater. 416 401-407 (2016), 10.1016/j.jmmm.2016.04.082.
  40. [40]Y. Okamoto, T. Shimizu, J.-i. Yamaura, Y. Kiuchi, and Z. Hiroi, ”Itinerant-electron Magnet of the Pyrochlore Lattice: Indium-doped YMn₂Zn₂₀” J. Phys. Soc. Jpn. 79 (2010), 10.1143/JPSJ.79.093712.DOI
  41. [41]Y. Okamoto, T. Shimizu, J. Yamaura, and Z. Hiroi, ”Crystal Chemistry and Magnetic Properties of Manganese Zinc Alloy “YMn₂Zn₂₀” Comprising a Mn Pyrochlore Lattice” J. Solid State Chem. 191 246-256 (2012), 10.1016/j.jssc.2012.03.038.DOI
  42. [42]J. M. Santiago, C. L. Huang, and E. Morosan, ”Itinerant Magnetic Metals” J. Phys.: Condens. Matter 29 (2017), 10.1088/1361-648X/aa7889.DOI
  43. [43]E. M. Benbow and S. E. Lattuner, ”Mixed-metal Flux Synthesis of Quaternary RMn₂₋ₓTrₓZn₂₀₋ₓ Compounds with Tr=Al, In” J. Solid State Chem. 179 3989-3996 (2006), 10.1016/j.jssc.2006.09.001.
  44. [44]Rigaku Oxford Diffraction CrysAlisPro, Rigaku Corporation, 2022.
  45. [45]P. W. Betteridge, J. R. Carruthers, R. I. Cooper, K. Prout, and D. J. Watkin, ”CRYSTALS version 12: Software for Guided Crystal Structure Analysis” J. Appl. Crystallogr. 36 1487 (2003), 10.1107/S0021889803021800.DOI
  46. [46]L. Palatinus and G. Chapuis, ”SUPERFLIP - a Computer Program for the Solution of Crystal Structures by Charge Flipping in Arbitrary Dimensions” J. Appl. Crystallogr. 40 786-790 (2007), 10.1107/S0021889807029238.DOI
  47. [47]C. R. Groom, I. J. Bruno, M. P. Lightfoot, and S. C. Ward, ”The Cambridge Structural Database” Acta Crystallographica B 72 171-179 (2016), 10.1107/S2052520616003954.DOI
  48. [48]TOPAS, Bruker, 2009.
  49. [49]CrystalMaker, CrystalMaker Software Ltd, 2023.
  50. [50]J. C. Slater, ”Atomic Radii in Crystals” J. Chem. Phys. 41 3199-3204 (1964), 10.1063/1.1725697.DOI
  51. [51]S. Mugiraneza and A. M. Hallas, ”Tutorial: a beginner’s guide to interpreting magnetic susceptibility data with the Curie-Weiss law” Commun. Phys. 5 95 (2022), 10.1038/s42005-022-00853-y.DOI
  52. [52]M. Shiga, H. Wada, K. Yoshimura, and Y. Nakamura, ”Transition from Itinerant Electron to Local Moment System in Y(Mn₁₋ₓAlₓ)₂” J. Magn. Magn. Mater. 54-57 1073-1074 (1986), 10.1016/0304-8853(86)90387-2.DOI
  53. [53]S. Mugiraneza and A. M. Hallas, ”Tutorial: a Beginner’s Guide to Interpreting Magnetic Susceptibility Data with the Curie-Weiss Law” Commun. Phys. 5 (2022), 10.1038/s42005-022-00853-y.DOI
  54. [54]A. Semwal and S. N. Kaul, ”Magnetic Properties of the Weak Itinerant-electron Ferromagnet Ni₇₅Al₂₅: I. The Effect of Site Disorder” J. Phys.: Condens. Matter 16 (2004), 10.1088/0953-8984/16/47/019.DOI
  55. [55]D. Patra, S. Vishvakarma, P. D. Babu, and S. Veeturi, ”Weak Itinerant Magnetic Behaviour in Al Substituted Ni₉₂Cr₈ Alloys” AIP Adv. 13 (2023), 10.1063/9.0000541.DOI
  56. [56]P. Rhodes and E. P. Wohlfarth, ”The Effective Curie-Weiss Constant of Ferromagnetic Metals and Alloys” Proc. R. Soc. A 273 247-258 (1963), 10.1098/rspa.1963.0086.
  57. [57]Y. Takahashi, Spin Fluctuation Theory of Itinerant Electron Magnetism (Springer-Verlag, Berlin Heidelberg, Germany, 2013), Springer Tracts in Modern Physics, 253.
  58. [58]T. Moriya and A. Kawabata, ”Effect of Spin Fluctuations on Itinerant Electron Ferromagnetism” J. Phys. Soc. Jpn. 34 639-651 (1973), 10.1143/JPSJ.34.639.DOI
  59. [59]T. Moriya and A. Kawabata, ”Effect of Spin Fluctuations on Itinerant Electron Ferromagnetism. II” J. Phys. Soc. Jpn. 35 669-676 (1973), 10.1143/JPSJ.35.669.DOI
  60. [60]T. Moriya and Y. Takahashi, ”Spin Fluctuation Theory of Itinerant Electron Ferromagnetism –A Unified Picture” J. Phys. Soc. Jpn. 45 397-408 (1978), 10.1143/JPSJ.45.397.DOI
  61. [61]T. Moriya, Spin Fluctuations in Itinerant Electron Magnetism (Springer-Verlag, Berlin Heidelberg, Germany, 1985), Vol. 56, Springer Series in Solid-State Sciences.
  62. [62]Y. Takahashi, ”On the Origin of the Curie-Weiss Law of the Magnetic Susceptibility in Itinerant Electron Ferromagnetism” J. Phys. Soc. Jpn. 55 3553-3573 (1986), 10.1143/JPSJ.55.3553.DOI
  63. [63]Y. Takahashi, ”Theoretical Development in Itinerant Electron Ferromagnetism” J. Phys.: Conf. Ser. 868 012002 (2017), 10.1088/1742-6596/868/1/012002.DOI
  64. [64]Y. Takahashi, ”Quantum Spin Fluctuation Theory of the Magnetic Equation of State of Weak Itinerant-electron Ferromagnets” J. Phys.: Condens. Matter 13 (2001), 10.1088/0953-8984/13/29/305.DOI
  65. [65]E. C. Stoner, ”Collective electron ferromagnetism” Proc. R. Soc. A 165 372-414 (1938), 10.1098/rspa.1938.0066.DOI
  66. [66]H. K. Dara, D. Patra, G. P. Moharana, S. N. Sarangi, and D. Samal, ”Evidence of Weak Itinerant Ferromagnetism and Griffiths Like Phase in MnFeGe” J. Phys.: Condens. Matter 35 (2023), 10.1088/1361-648X/ace0ac.DOI
  67. [67]T. Sakon et al., ”Investigation of the Itinerant Electron Ferromagnetism of Ni₂₊ₓMnGa₁₋ₓ and Co₂VGa Heusler Alloys” Materials 12 (2019), 10.3390/ma12040575.DOI
  68. [68]H. Masumitsu, S. Yoshinaga, Y. Mitsui, R. Y. Umetsu, M. Hiroi, Y. Uwatoko, and K. Koyama, ”Weak Itinerant-electron Ferromagnetism of CrAlGe Modified by 3d Transition Metal” J. Magn. Magn. Mater. 492 (2019), 10.1016/j.jmmm.2019.165677.DOI
  69. [69]N. Tateiwa, J. Pospíšil, Y. Haga, H. Sakai, T. D. Matsuda, and E. Yamamoto, ”Itinerant Ferromagnetism in Actinide 5f-electron Systems: Phenomenological Analysis with Spin Fluctuation Theory” Phys. Rev. B 96 (2017), 10.1103/PhysRevB.96.035125.DOI
  70. [70]T. Waki, S. Terazawa, Y. Tabata, K. Sato, A. Kondo, K. Kindo, and H. Nakamura, ”Observation of Two Ferromagnetic Phases in Fe₃Mo₃N” Phys. Rev. B 90 (2014), 10.1103/PhysRevB.90.014416.DOI
  71. [71]J. Yang, B. Chen, H. Ohta, C. Michioka, K. Yoshimura, H. Wang, and M. Fang, ”Spin Fluctuations on the Verge of a Ferromagnetic Quantum Phase Transition in Ni₃Al₁₋ₓGaₓ” Phys. Rev. B 83 (2011), 10.1103/PhysRevB.83.134433.DOI
  72. [72]H. Ohta and K. Yoshimura, ”Anomalous Magnetization in the Layered Itinerant Ferromagnet LaCoAsO” Phys. Rev. B 79 (2009), 10.1103/PhysRevB.79.184407.DOI
  73. [73]A. Arrott and J. E. Noakes, ”Approximate Equation of State For Nickel Near its Critical Temperature” Physical Review Letters 19 786-789 (1967), 10.1103/PhysRevLett.19.786.DOI

Paper details

vlnc:W_jnvzjcp3
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents