Direct imaging of plasmonic coupling between gold nanoparticles and one-dimensional van der Waals materials

Abstract

Hybrids of plasmonic metals and van der Waals (vdW) materials combine electromagnetic field enhancement with the electronic properties of the vdW component, but the studies reported so far concern two-dimensional layers, and the near field at the metal/vdW interface is generally inferred from far-field measurements. Here we report the plasmonic coupling between Au nanoparticles and a one-dimensional (1D) vdW material, NbS3, and measure the near field at the Au-NbS3 contact directly. NbS3 nanowires and nanoribbons were grown by salt-assisted vapor-liquid-solid growth on graphene-covered TEM grids, and atomic-resolution electron microscopy shows atomically sharp Au/NbS3 interfaces. Photon-induced near-field electron microscopy at 1030 nm shows that an Au particle in contact with NbS3 produces a near field of higher intensity and larger extent than an isolated particle of similar size, and that the hot spot at a contact is excited only when the incident polarization is parallel to the particle-NbS3 axis. Finite-difference time-domain simulations reproduce these observations and quantify the dependence of the coupling on the particle-NbS3 gap, the NbS3 thickness, and the dimension ratio of the NbS3 structure. Size-specific Au nanoparticles on NbS3 nanowires enhance the Raman scattering of rhodamine 6G by a factor of 1.8-4.2 relative to Au nanoparticles alone, with a detection limit of 10^-7 M. These results extend plasmonic metal/vdW hybrids to 1D vdW crystals and establish a multimodal approach that correlates the atomic structure of a metal/vdW interface with its nanoscale plasmonic response.

: These authors contributed equally to this work

*Corresponding Authors: [email protected], [email protected]

Introduction

Transition metal trichalcogenides (TMTs), MX3MX_{3} (MM = Ti, Zr, Hf, Nb, Ta; XX = S, Se, Te), are quasi-one-dimensional (1D) van der Waals (vdW) materials in which MX6MX_{6} trigonal prisms share faces to form infinite chains along the [10] axis[1, 2, 3]. Bonding is covalent within a chain and vdW between chains. This structural anisotropy results in direction-dependent electrical and optical properties[2, 4]. Among TMTs, NbS3NbS_{3} crystallizes in several polymorphs[5, 6] whose electronic structure ranges from semiconducting (phases I and IV) to metallic (phases II, III, and V). The metallic phase II has been synthesized as nanowires and nanoribbons by salt-assisted vapor-liquid-solid (VLS) growth with Au-based catalysts and by catalyst-free vapor–solid (VS) growth[7, 8]. The optical response of these nanostructures, and in particular their interaction with plasmonic metals, has not been investigated.

Localized surface plasmon resonances (LSPRs) of noble metal nanoparticles confine optical fields to dimensions well below the wavelength of light[9, 10]. The resulting near-field enhancement is the basis of surface-enhanced Raman scattering (SERS), in which the electromagnetic enhancement factor scales approximately with the fourth power of the local field and reaches 10410^{4}-10810^{8} for noble metal substrates[11]. VdW materials can also enhance Raman scattering, mainly by charge transfer to the adsorbed molecule, but the enhancement factors are typically limited to 10210^{2}-10310^{3}[11]. Combining a plasmonic metal with a vdW material therefore provides both electromagnetic and chemical enhancement[11, 12, 13]. Reported examples include Au nanoparticles on MoWS2MoWS_{2}, with a detection limit of 10−1110^{-11} M for rhodamine 6G (R6G)[11], and 1T′1T'-WS2WS_{2} monolayers on 4H-Au nanowires, with a detection limit of 10−1810^{-18} M[14]. In these hybrids, the enhancement is determined by the near field at the metal/vdW interface. This near field is generally inferred from far-field Raman spectra and from electromagnetic simulations rather than measured[15, 16]. Furthermore, the vdW components investigated to date are two-dimensional (2D) layers.

Photon-induced near-field electron microscopy (PINEM), a mode of ultrafast electron microscopy (UEM), provides a direct measurement of optically excited near fields in real space[17, 18]. A femtosecond laser pulse excites the specimen, and a synchronized electron pulse traversing the evanescent field gains or loses integer multiples of the photon energy. An image formed from the electrons that gained energy maps the field component along the electron trajectory with nanometer spatial resolution and sub-picosecond temporal resolution[15, 16]. Because the excitation wavelength and polarization are defined, PINEM measures the response that governs plasmon-enhanced spectroscopy. PINEM has been applied to the fields at graphene steps[19] and to coupled metal nanoparticles[15, 16, 20]. It has not been applied to a metal nanoparticle in contact with a 1D vdW crystal.

Here, we report the plasmonic coupling between Au nanoparticles and NbS3NbS_{3} nanowires and nanoribbons, measured by PINEM and applied to the Raman detection of R6G. For PINEM, NbS3NbS_{3} was grown by salt-assisted VLS on graphene-covered TEM grids. Au particles in contact with NbS3NbS_{3} and isolated Au particles on the same support were therefore imaged under identical excitation conditions. Atomic-resolution TEM shows an atomically sharp Au/NbS3NbS_{3} interface. PINEM at 1030 nm shows that an Au particle in contact with NbS3NbS_{3} produces a near field of higher intensity and larger spatial extent than an isolated Au particle with similar radius, and that the near field at a given contact is excited only when the incident polarization is parallel to the particle-NbS3NbS_{3} axis. Finite-difference time-domain (FDTD) simulations reproduce these observations and quantify the dependence of the coupling on the particle-NbS3_3 separation, the dimension ratio of the NbS3_3 structure, and its thickness. Finally, colloidal Au nanoparticles (10, 20, and 40 nm) deposited on catalyst-free NbS3_3 nanowires increase the Raman intensity of R6G at 1362 cm−1^{-1} by a factor of 3.2 ±\pm 1.4 relative to Au nanoparticles alone, with a detection limit of 10−7^{-7} M. These results extend plasmonic metal/vdW hybrids from 2D layers to a 1D vdW material and relate the measured near-field distribution at the Au-NbS3_3 contact to the Raman enhancement.

Results and Discussion

Salt-assisted VLS growth of NbS3_3 nanowires and nanoribbons

Figure 1a shows the crystal structure of NbS3_3, in which NbS6_6 trigonal prisms share faces to form chains along the [10] (b) axis. NbS3_3 nanowires and nanoribbons were synthesized by salt-assisted VLS growth in a horizontal tube furnace (Figure 1b), following our previous procedure[7]. The synthesis parameters are given in the Methods section. Au films of 1-25 nm thickness were deposited by electron-beam evaporation on SiO2_2/Si and c-sapphire substrates (Figure 1b, top) and on few-layer graphene transferred onto holey SiN TEM grids (Figure 1b, bottom). On heating, the films dewet into particles that serve as the VLS catalysts. A mixture of Nb powder and NaCl was used as the metal source, with the substrate placed face down above it. S was introduced from upstream after the substrate reached the growth temperature of 725-775 °C, with Ar (100-250 sccm) as the carrier gas. Growth on TEM grids allows the Au-NbS3_3 contacts to be characterized by TEM, STEM, and PINEM in the as-grown state, without transfer.

Synthesis of Au-NbS3 nanostructures

Figure 1. Synthesis of Au-NbS3_3 nanostructures. (a) Crystal structure of NbS3_3 (Nb, green; S, yellow). The chain direction b is indicated. (b) Schematic of the CVD setup for salt-assisted

Figure 1c and Figure 1d show SEM images of growths on SiO2_2/Si with initial Au film thicknesses of 5 and 15 nm, respectively (see also Fig. SI1). For Au films thinner than about 5 nm, the dewetted particles are too small to sustain VLS growth. NbS3_3 then grows by the VS mechanism, and the Au particles decorate its surface (Figure 1c). For Au films of 10-25 nm, VLS growth produces nanowires with a square cross-section that grow along the chain direction [10], and nanoribbons with a rectangular cross-section that grow along [100] (Figure 1d), as reported previously[7]. The catalyst particle remains at one end of each structure. The initial Au thickness determines the NbS3_3 morphology, the size of the Au particles, and whether the particles are located at the tip (VLS) or on the surface (VS) of the NbS3_3 structure. Both configurations of Au-NbS3_3 contact are examined below.

VLS growth on bulk substrates (SiO2\mathrm{SiO}_{2}/Si, c-sapphire; top) and on graphene/SiN TEM grids (bottom). (c, d) SEM images of NbS3\mathrm{NbS}_{3} grown on SiO2\mathrm{SiO}_{2}/Si from Au films with initial thicknesses of 5 nm (c) and 15 nm (d).

Structure of the Au-NbS3\mathrm{NbS}_{3} junctions

Figure 2a shows a TEM image of NbS3\mathrm{NbS}_{3} nanostructures grown on a graphene/SiN TEM grid (see also Fig. SI2). Nanowires and nanoribbons lie on the suspended graphene together with dewetted Au particles with diameters from about 15 to 220 nm. Most 1D structures terminate in an Au particle at one end, which is the signature of VLS growth[7, 21], and smaller Au particles are attached to the sidewalls of several structures. Three configurations of Au are therefore present in the same specimen: catalyst particles at the tips of the 1D structures, particles on their sidewalls, and isolated particles on the graphene. STEM-EDS mapping of a nanowire and its catalyst particle (Figure 2b) shows that Au is confined to the particle, while Nb and S are confined to the nanowire.

Image not extracted

Figure 2. Structure of Au-NbS3_3 contacts. (a) TEM image of NbS3_3 nanowires and nanoribbons grown on a graphene/SiN TEM grid, with Au catalyst particles at their tips, Au particles on their sidewalls, and isolated Au particles. (b) STEM-EDS maps of Au, Nb, and S for a nanowire with its catalyst particle. (c) Atomic-resolution TEM image of the junction between an Au catalyst particle and a NbS3_3 nanowire. (d) Inverse FFT image of the region marked in (c), reconstructed from the Au (orange) and NbS3_3 (blue) reflections. Insets: FFTs of the Au particle (top) and of the NbS3_3 nanowire (bottom) with indexed reflections. (e) HAADF-STEM image of a NbS3_3 nanoribbon with Au particles at its ends and on its sidewalls. (f) HAADF-STEM image showing atomically-sharp interface between an Au particle and NbS3_3.

Figure 2c shows an atomic-resolution TEM image of the junction between a catalyst particle and a nanowire. The particle is faceted, and the lattice fringes of NbS3\mathrm{NbS}_{3} continue to a flat interface with the particle. Figure 2d shows the interface region marked in Figure 2c together with the FFTs of the particle and of the nanowire. The FFT of the nanowire is indexed to monoclinic NbS3\mathrm{NbS}_{3}-II along the [201][201] zone axis, with d010=3.3±0.1d_{010} = 3.3 \pm0.1 Å and d−204=3.8±0.1d_{-204} = 3.8 \pm0.1 Å consistent with the lattice parameters of NbS3\mathrm{NbS}_{3}-II[7]. The FFT of the particle is indexed to face-centered cubic Au along [111][111]. The two FFTs give the orientation relationship NbS3\mathrm{NbS}_{3} [201]∥[201] \parallel Au [111][111] and NbS3\mathrm{NbS}_{3} (010)∥(010) \parallel Au (22ˉ0)(2\bar{2}0). An inverse FFT image reconstructed from the Au and NbS3\mathrm{NbS}_{3} reflections (Figure 2d) shows an atomically sharp interface without an intermediate layer.

Figures 2e and 2f display HAADF-STEM images of Au particles on the surface of a NbS3\mathrm{NbS}_{3} nanoribbon, the configuration obtained with thin Au films (Figure 1c, see also Figs. SI2b-c). The nanoribbon in Figure 2e is about 43 nm wide and is in contact with four Au particles, two at its ends and two on its sidewalls, with diameters between about 10 and 40 nm. Figure 2f shows one sidewall particle at higher magnification. The particle has the shape of a truncated sphere with a flat contact face on NbS3\mathrm{NbS}_{3}, and its {111}\{111\} lattice planes, with a spacing of 2.4 Å, are parallel to the interface. The image resolves the atomic columns of Au and NbS3\mathrm{NbS}_{3} up to the interface, which is atomically sharp, as found for the catalyst junction in Figure 2d. The truncated-sphere shape and the flat contact face suggest that the particle was liquid, or had high atomic mobility, when it attached to the NbS3\mathrm{NbS}_{3} surface, consistent with the Au-NaCl alloy catalyst proposed for salt-assisted VLS growth[7]. In both configurations, at the tip and on the sidewall, the Au particle is in direct contact with NbS3\mathrm{NbS}_{3} across a flat crystalline interface. These contacts are the subject of the near-field measurements in § 3.3.

Six-panel electron microscopy and elemental mapping images

Figure 6.

Real-space imaging of Au-NbS3_3 near fields

To investigate the electromagnetic coupling in the Au-NbS3_3 heterostructures, we performed PINEM measurements with the configuration illustrated in Figure 3a. The optical pump and the electron probe are derived from the same femtosecond (fs) laser, and a motorized delay stage sets the delay between them. Electrons that pass through the optically excited near field exchange energy with it in multiples of the photon energy ℏω\hbar\omega, so that the electron energy spectrum shows sidebands separated by ℏω\hbar\omega on both sides of the zero-loss peak[17, 18]. PINEM images are formed with an energy-selecting slit that passes only the electrons that gained energy. Further details are given in the Methods section. The coexistence of Au particles in contact with NbS3_3 and isolated Au particles on the same support allows both to be recorded in one image under the same pump fluence, electron dose, and alignment.

Polarization-dependent near-field localization in Au-NbS$_3$ heterostructures

Figure 3. Polarization-dependent near-field localization in Au-NbS3_3 heterostructures. (a) Schematic of the PINEM experiment. (b) Bright-field TEM image of NbS3_3 nanoribbons and

nanowires decorated with Au particles. The two areas analyzed in the text are marked (Area 1, red; Area 2, green), and the arrows indicate the particles discussed. (c,d) PINEM images for linear polarization at −78∘-78^{\circ} (c) and 22∘22^{\circ} (d), indicated by the white arrows. The crescent-shaped contrast at the periphery arises from the edge of the SiN membrane. (e) PINEM intensity profiles along Line 1 (isolated Au particle) and Line 2 (Au particle in contact with a NbS3\mathrm{NbS}_{3} nanowire) in (d). Scale bars: 200 nm. Pump wavelength: 1030 nm; delay: 0 ps.

Figure 3b shows a bright-field TEM image of the analyzed region, which contains NbS3\mathrm{NbS}_{3} nanoribbons and nanowires of different width and thickness decorated with Au particles with radii of 20–75 nm. Particles with radii of about 50 and 75 nm are in direct contact with NbS3\mathrm{NbS}_{3}. Since these radii are much smaller than the excitation wavelength of 1030 nm, the quasi-static approximation gives a first-order estimate of the optical response of the Au particles. In this limit, an isolated Au sphere is described by an induced electric dipole,

p=4πε0εmr3εAu(ω)−εmεAu(ω)+2εmEloc\mathbf{p}=4\pi\varepsilon_{0}\varepsilon_{m}r^{3}\frac{\varepsilon_{\mathrm{Au}}(\omega)-\varepsilon_{m}}{\varepsilon_{\mathrm{Au}}(\omega)+2\varepsilon_{m}}\mathbf{E}_{\mathrm{loc}}

where rr is the nanoparticle radius, εm\varepsilon_{m} is the permittivity of the surrounding medium, εAu(ω)\varepsilon_{\mathrm{Au}}(\omega) is the frequency-dependent permittivity of gold, and is Eloc\mathbf{E}_{\mathrm{loc}} the local optical field driving the particle[22]. The dipole moment scales with the particle volume, and the dipolar localized surface plasmon resonance (LSPR) occurs near the Fröhlich condition Re⁡[εAu(ω)]=−2εm\operatorname{Re}[\varepsilon_{\mathrm{Au}}(\omega)]=-2\varepsilon_{m} [22], which for gold lies in the visible range[23]. Two consequences follow for the present experiment. First, at 1030 nm the Au particles are excited far from their dipolar LSPR. Second, larger Au particles possess larger effective polarizabilities and can therefore generate stronger and more spatially extended near fields.

To examine how the Au–NbS3\mathrm{NbS}_{3} heterostructure geometry modifies this picture, we focus on two areas marked in Figure 3b, Area 1 (red) and Area 2 (green). PINEM images were acquired at zero delay for two polarization angles, −78∘-78^{\circ} and 22∘22^{\circ} (Figure 3c and Figure 3d). The strong crescent-shaped contrast at the periphery of both images originates from the edge of the SiN membrane, and all analyses below concern structures far from this edge. The PINEM maps reveal that the near-field localization is not simply confined to individual nanoparticles but emerges as a collective phenomenon, with dipolar hot spots forming across the NbS3\mathrm{NbS}_{3}–Au heterostructures. In the NbS3\mathrm{NbS}_{3}–Au heterostructure, the Au nanospheres are strongly coupled to lossy NbS3\mathrm{NbS}_{3} nanowires/nanoribbons, so that both the local driving field and the effective plasmonic response are modified by the presence of the anisotropic, absorbing NbS3\mathrm{NbS}_{3} host. Furthermore, the larger Au spheres approach a size regime where finite-size effects, including retardation and radiative damping, become non-negligible and can alter both the resonance frequency and the spatial distribution of the near-fields. To account for these effects, we performed full-wave finite-difference time-domain (FDTD) simulations of the imaged geometry, which allow direct comparison with the PINEM maps. Simulations of Area 1 with the Au particles removed and with the NbS3\mathrm{NbS}_{3} structures removed are given in Fig. S13 and separate the contributions of the two components.

A more detailed analysis of individual nanoparticles within the heterostructure provides direct evidence of the anisotropic nature of the coupling. We first consider a nanoparticle located in Area 2, indicated by the green arrow (Figure 3b), which is in contact with the NbS3\mathrm{NbS}_{3} structure from below. The axis defined by this nanoparticle–NbS3\mathrm{NbS}_{3} contact is oriented approximately along the −78° direction. Consistent with this alignment, a pronounced PINEM hot spot is observed around this nanoparticle when the incident polarization is set to −78° (Figure 3c), whereas the same region exhibits negligible enhancement when the polarization is rotated to 22° (Figure 3d). Conversely, the particle marked by the red arrow in Area 1 (Figure 3b) is in contact with the tip of a NbS3\mathrm{NbS}_{3} nanowire, and its contact axis is nearly parallel to 22° polarization. In this case, a strong, localized hot spot is observed under 22° excitation (Figure 3d), while no discernible enhancement appears under the orthogonal −78° polarization (Figure 3c). The excellent agreement between these experimental PINEM observations and the FDTD simulations (Fig. SI3) confirms that the near-field enhancement at a given junction is governed by the relative orientation of the incident electric field with respect to the particle-NbS3\mathrm{NbS}_{3} contact axis. In other words, the activation of a specific hot spot is highly polarization-selective, underscoring the pronounced anisotropy of the hybrid coupling.

To quantify the impact of NbS3\mathrm{NbS}_{3} coupling on the near-field distribution, we extracted intensity line profiles along the induced dipole direction for two representative Au nanospheres: one that is effectively isolated and one that is coupled to a NbS3\mathrm{NbS}_{3} nanowire (Figure 3d). According to the quasi-static model, the larger isolated sphere (radius 60 nm) should exhibit a stronger near-field response than the smaller coupled sphere (radius 50 nm), due to its larger volume and, hence, larger polarizability. Contrary to this expectation, the PINEM line profiles in Figure 3e reveal that the coupled nanoparticle exhibits both higher peak intensity (∼\sim1.5 times) and a more spatially extended near-field region compared to the larger isolated nanoparticle. This behavior indicates that the NbS3\mathrm{NbS}_{3} nanowire does not simply act as a passive dielectric environment but actively participates in shaping and enhancing the local fields. The enhanced localization observed in the coupled configuration is consistent with the formation of NbS3\mathrm{NbS}_{3}-Au modes.

Comparison of the areas in Figure 3 and of the additional heterostructures in Fig. SI4 indicates that the dimensions (length, width and thickness) of the NbS3\mathrm{NbS}_{3} structure might influence the field localization, but the number of configurations in the present samples is too small to extract a quantitative dependence. We therefore examine these parameters by simulation, varying the particle-NbS3\mathrm{NbS}_{3} gap, the dimension ratio (defined as width/length or w/l) of the NbS3\mathrm{NbS}_{3} structure, and the NbS3\mathrm{NbS}_{3} thickness as illustrated in Figure 4.

Dependence of the Au-NbS3 coupling on the NbS3 geometry

Figure 4. Dependence of the Au-NbS3_3 coupling on the NbS3_3 geometry (FDTD). (a) Model: a rectangular NbS3_3 structure of length ll, width ww, and thickness hh at a gap gg from an Au sphere of radius 50 nm. Two regions of interest (ROIs; width 40 nm, height 100 nm) around the sphere are used for parallel (0°) and perpendicular (90°) polarization relative to the NbS3_3-sphere axis, and the integrated ∣Ez∣2\lvert E_z\rvert^2 in each ROI is the coupling metric. Nominal values: ll = 330 nm, ww = 110 nm, hh = 50 nm, gg = 20 nm and rr = 50 nm. (b-d) Integrated ∣Ez∣2\lvert E_z\rvert^2 as a function of (b) the gap gg, (c) the structure’s dimension ratio (w/lw/l) and (d) the NbS3_3 thickness hh. ROI width (WROIW_{\mathrm{ROI}}) is 40 nm and height (HROIH_{\mathrm{ROI}}) is 100 nm. Excitation: 1030 nm, normal incidence.

Dependence of the coupling on the NbS3_3 geometry

We modeled a single NbS3_3 structure, a rectangular prism of length ll, width ww, and thickness hh, separated by a gap gg from an Au sphere of radius rr = 50 nm (Figure 4a). Unless stated otherwise, ll = 330 nm, ww = 110 nm, hh = 50 nm, and gg = 20 nm. The structure is illuminated at normal incidence at 1030 nm, and the polarization angle is defined relative to the NbS3_3-sphere axis, the line connecting the centers of the NbS3_3 structure and the sphere. In this configuration, dipolar localized surface plasmons on the Au nanosphere are generated along the incident polarization direction according to the quasi-static description and the PINEM observations in Figure 3. Therefore, two three-dimensional regions of interest (ROIs) around the sphere, corresponding to parallel (0∘0^\circ) and perpendicular (90∘90^\circ) polarizations, are used to compute the integrated out-of-plane field intensity ∫∣Ez∣2 dV\int|E_z|^2 \,dV as a measure of coupling strength. g=20g = 20 nm is chosen for the base calculation so that ROI boxes do not overlap with NbS3_3 region to avoid effects merely arise due to NbS3_3. Further simulation details are provided in the Methods section.

We first examined the dependence of the coupling on the sphere-NbS3_3 gap gg, sweeping from 10 nm to 200 nm (Figure 4b). Under parallel polarization, the integrated EzE_z intensity exhibits a strong inverse relationship with the gap. For small separations (10-20 nm), the field intensity is significantly enhanced, indicating strong hybridization between the NbS3_3 structure and sphere modes. As the gap increases, the coupling progressively weakens and the integrated field converges towards a constant value characteristic of an effectively isolated nanosphere. In contrast, under perpendicular polarization, the integrated EzE_z shows only a weak dependence on the gap and only for the smallest separations (10-20 nm). Beyond this range, the integrated field remains nearly constant, indicating that the NbS3_3-sphere pair is essentially uncoupled when the incident polarization is orthogonal to the NbS3_3 structure-sphere axis.

We next varied the dimension ratio (w/lw/l) of the NbS3_3 structure (Figure 4c). For parallel polarization, the integrated field reaches a maximum at an intermediate dimension ratio l/w=1.25l/w = 1.25 and decreases on either side. Simulations of the NbS3_3 structure alone (Fig. SI5) show the same trend, with a maximum of the extinction efficiency at the same dimension ratio. The dependence of the coupled system therefore follows the intrinsic scattering of the NbS3_3 structure, which is transferred to the sphere by coupling. We attribute this apparent contradiction to the lossy character of NbS3_3. As seen from the gap-dependence analysis, the ribbon-sphere system is only weakly coupled under perpendicular polarization, so the enhancement contributed by hybridization is small. At the same time, the increasing absorption efficiency and effective area of the NbS3_3 ribbon with larger dimension ratio provide an efficient loss channel for the localized fields. The ribbon thus acts mainly as an absorber in close proximity to the sphere, draining energy from the near-field region and reducing the integrated field at the ROI despite the increased scattering and absorption of the ribbon itself.

Finally, varying the NbS3_3 thickness from 10 to 100 nm (Figure 4d) gives an approximately linear increase of the integrated field with thickness for parallel polarization, consistent with stronger hybridization as the optical cross-section of the NbS3_3 structure increases. For perpendicular polarization, the integrated field decreases slightly with thickness, again because absorption dominates in the weakly coupled geometry. In summary, the coupling between the Au particle and NbS3_3 is strongest for small gaps, thick NbS3_3, and polarization along the particle-NbS3_3 axis, which is the configuration realized by the catalyst and sidewall particles in Section 2.2.

Plasmon-enhanced Raman detection of R6G

The PINEM measurements and simulations show that the near field of an Au particle is enhanced by contact with NbS3_3. We tested whether this enhancement increases the Raman scattering of molecules adsorbed at the Au-NbS3_3 contact, using R6G as the probe molecule (Figure 5 and Fig. SI6). R6G has well-assigned vibrational bands, and its Raman cross section is resonantly enhanced at 532 nm excitation [11, 24]. For this experiment, colloidal Au nanoparticles with diameters of 10, 20, and 40 nm were deposited from solution onto NbS3_3 nanowires grown on c-sapphire without a catalyst [8]. The Raman intensity of R6G on Au-NbS3_3 showed no systematic dependence on particle size within the measurement uncertainty (Fig. SI7), and the 40 nm particles were used for the comparison between samples because their size is closest to the particles imaged by PINEM and modeled by FDTD (radii of 20 to 75 nm and 50 nm, respectively) and because 40 nm Au spheres are near their dipolar resonance at the 532 nm excitation wavelength. Colloidal particles were used instead of dewetted Au films because of their narrower size distribution. Four samples were compared: (i) bare c-sapphire, (ii) Au nanoparticles on c-sapphire, (iii) NbS3_3 nanowires on c-sapphire, and (iv) Au nanoparticles on NbS3_3 nanowires. R6G was deposited from aqueous solutions with concentrations of 10−710^{-7} to 10−410^{-4} M (about 25 μ\muL per sample), followed by drying at 80 °C. Raman spectra were acquired at 532 nm with 5 mW laser power through a 100× objective. Each spectrum is the sum of 10 acquisitions of 10 s.

Raman spectra and intensity of R6G on Au–NbS3

Figure 5. Raman detection of R6G on Au–NbS3_3. (a) Raman spectra of R6G (10−710^{-7} M) on NbS3_3 nanowires, on 40 nm Au nanoparticles, and on 40 nm Au nanoparticles deposited on NbS3_3 nanowires, all on c-sapphire. (b) Raman spectra of R6G on 40 nm Au nanoparticles on NbS3_3 for concentrations from 10−410^{-4} to 10−710^{-7} M. (c) Intensity of the 1362 cm−1^{-1} band as a function of R6G concentration for the four samples. Inset: NbS3_3 and bare c-sapphire on an expanded scale. Error bars are the standard deviation over 3–10 spots.

fig:5a compares the Raman spectra of R6G at 10−710^{-7} M on NbS3_3 nanowires, on 40 nm Au nanoparticles, and on 40 nm Au nanoparticles deposited on NbS3_3 nanowires. R6G bands are present on both Au-containing samples and absent on NbS3_3 alone, and the intensities are higher on Au-NbS3_3 than on Au. fig:5b shows the spectra on Au-NbS3_3 for R6G concentrations from 10−410^{-4} to 10−710^{-7} M. At 10−410^{-4} M, the characteristic bands of R6G at 1183, 1310, 1362, 1508, 1573, and 1651 cm−1^{-1} are resolved [24]. As the concentration decreases, the bands broaden and partially merge, but their positions coincide with the resolved bands at 10−410^{-4} M. At 10−710^{-7} M, the peak intensities of the 1310, 1362, and 1573 cm−1^{-1} bands are about 10–20 times the baseline level between the bands, and we take this concentration as the detection limit under these acquisition conditions. fig:5c plots the intensity of the 1362 cm−1^{-1} band as a function of R6G concentration for the four samples. On Au\mathrm{Au}-NbS3\mathrm{NbS}_{3}, the intensity is 3.2±1.43.2 \pm1.4 times that on Au\mathrm{Au} nanoparticles alone over the whole concentration range. On NbS3\mathrm{NbS}_{3} alone and on bare c-sapphire, the intensity is at the noise level (Figure 5c, inset).

Two mechanisms can contribute to the higher signal on Au\mathrm{Au}-NbS3\mathrm{NbS}_{3}[11]. The electromagnetic mechanism arises from the plasmonic near field of the Au\mathrm{Au} particle, which is enhanced by contact with NbS3\mathrm{NbS}_{3} as shown by PINEM (§ 3.3) and FDTD simulations (§ 3.4). Because the SERS enhancement scales approximately as ∣E/E0∣4\lvert E/E_0\rvert^4, an increase of the near-field intensity ∣E∣2\lvert E\rvert^2 at the contact by a factor of ∼1.5\sim1.5-22 is sufficient to account for the observed Raman enhancement of 3.2±1.43.2 \pm1.4. The chemical mechanism requires charge transfer between R6G and the substrate. The absence of a measurable signal on NbS3\mathrm{NbS}_{3} alone (Figure 5c, inset) indicates that charge transfer to NbS3\mathrm{NbS}_{3} does not contribute significantly under these conditions. The enhancement on Au\mathrm{Au}-NbS3\mathrm{NbS}_{3} relative to Au\mathrm{Au} is therefore attributed to the electromagnetic near field at the Au\mathrm{Au}-NbS3\mathrm{NbS}_{3} contact.

The detection limit of 10−7 M10^{-7}\ \mathrm{M} does not reach the values reported for optimized metal/2D-material SERS substrates, 10−11 M10^{-11}\ \mathrm{M} for Au\mathrm{Au} nanoparticles on MoWS2\mathrm{MoWS}_{2}[11] and 10−18 M10^{-18}\ \mathrm{M} for 4H-Au@1T′\mathrm{Au}@1\mathrm{T}^{\prime}-WS2\mathrm{WS}_{2} nanowires[14], which contain a high density of hot spots within the laser spot. The present samples were not designed for this purpose. The aim of this work is to connect the structure of the Au\mathrm{Au}-NbS3\mathrm{NbS}_{3} contact to its optical response across length scales. Atomic-resolution TEM and STEM resolve the interface (Section 2.2), PINEM images and quantifies the near field at the interface (§ 3.3 and § 3.4), and Raman spectroscopy measures the resulting enhancement over an ensemble of contacts (this section). This combination of methods identifies the Au\mathrm{Au}-NbS3\mathrm{NbS}_{3} contact as a plasmonic hot spot in a metal/1D vdW hybrid and provides the basis for substrates with a higher density of such contacts.

Summary

We have studied the plasmonic coupling between Au\mathrm{Au} nanoparticles and NbS3\mathrm{NbS}_{3} nanowires and nanoribbons, a 1D vdW material. Salt-assisted VLS growth on graphene-covered TEM grids produced atomically sharp Au\mathrm{Au}–NbS3\mathrm{NbS}_{3} contacts. PINEM at 1030 nm shows that an Au\mathrm{Au} particle in contact with NbS3\mathrm{NbS}_{3} produces a near field of higher intensity and larger extent than an isolated particle of similar size, and that the hot spot at a contact is excited only when the incident polarization is parallel to the particle-NbS3\mathrm{NbS}_{3} axis. FDTD simulations reproduce these observations and show that the coupling increases with decreasing gap and increasing NbS3\mathrm{NbS}_{3} thickness, and depends on the dimension ratio of the NbS3\mathrm{NbS}_{3} structure. Colloidal Au\mathrm{Au} nanoparticles deposited on catalyst-free NbS3\mathrm{NbS}_{3} nanowires enhance the Raman scattering of R6G by a factor of 3.2±1.43.2 \pm1.4 relative to Au\mathrm{Au} nanoparticles alone, with a detection limit of 10−7 M10^{-7}\ \mathrm{M}, whereas NbS3\mathrm{NbS}_{3} alone gives no measurable enhancement.

To the best of our knowledge, this work is the first observation of the plasmonic interaction between a noble metal and a 1D vdW material, obtained by combining atomic-resolution TEM and STEM of the interface, PINEM imaging of the near field at the same interface, FDTD simulations, and Raman spectroscopy of an ensemble of contacts. The coupling is anisotropic and is set by the orientation of the particle-NbS3\mathrm{NbS}_{3} axis relative to the incident polarization. We believe the same multimodal approach can be applied to other metal/vdW systems in which the near field at the interface has so far been inferred rather than measured. The 0D/1D heterostructure studied here is the simplest case. Heterostructures of 1D vdW crystals with each other (1D/1D) and with 2D layers (1D/2D), whose contacts can be defined during growth, offer additional control over the direction and position of field confinement, and the intrinsic anisotropy of the 1D crystal may add to the geometric anisotropy observed here. We anticipate that such dimensionally hybrid systems with growth-defined, atomically sharp interfaces are of interest for polarization-sensitive photodetection[25], nanoscale heat generation[26] and the coupling of plasmons to the collective electronic states of 1D vdW crystals[27].

Methods

VLS Au-NbS3_3 synthesis: SiO2_2/Si and c-sapphire substrates were cleaned with acetone, isopropanol, and deionized water, followed by oxygen plasma (150 mTorr, 3-5 min). For TEM-compatible growth, few-layer graphene was mechanically exfoliated and transferred onto holey SiN TEM grids. Au films with thicknesses of 1-25 nm were deposited on the substrates by electron-beam evaporation. Au-NbS was grown in 30 minutes by salt-assisted VLS in a horizontal tube furnace as illustrated in Figure 1b with 50 mg Nb, 25 mg NaCl, 100-150 mg S at 725-775°C, 350-760 torr and 100-250 sccm Ar carrier gas flow. All chemicals were purchased from Sigma-Aldrich.

VS NbS3_3 synthesis: NbS3_3 nanowires for the Raman experiments were grown on c-sapphire without Au by salt-assisted chemical vapor deposition. The synthesis parameters are the same as VLS Au-NbS3_3 synthesis listed above except the Au thin film deposition step.

Materials Characterization: SEM images were acquired at 5-15 kV on an FEI Helios Nanolab 600 and a Helios 5 UC. TEM and STEM were performed on a Thermo Fisher Scientific Themis Z and JEOL NEOARM operated at 200 kV. Aberration-corrected HAADF-STEM images were recorded with a semi-convergence angle of 25 mrad and a probe current of 80 pA. FFT analysis, inverse-FFT filtering (Figure 2d), and EDS processing were carried out with Gatan Microscopy Suite and Velox software.

PINEM: PINEM measurements were performed on the ultrafast electron microscope at the Center for Nanoscale Materials, Argonne National Laboratory, a JEOL JEM-2100 Plus modified for ultrafast operation and operated at 200 kV. The output of a femtosecond laser central wavelength 1030 nm, pulse duration 280 fs, repetition rate 250 kHz was split into two beams. One beam was frequency-quadrupled to 257 nm wavelength and directed to the photocathode to generate the probe electron pulses. The other beam (1030 nm) was directed onto the specimen as the pump. Its linear polarization was set by a half-wave plate placed after a linear polarizer. The delay between pump and probe was controlled by a motorized delay stage, and time zero was determined from time-resolved PINEM spectra. PINEM images were recorded at zero delay with a Gatan Imaging Filter, using an energy-selecting slit (10 eV slit width) placed on the energy-gain side of the zero-loss peak. The Au-NbS3 heterostructures were imaged on the graphene/SiN grids on which they were grown, without further preparation.

Electromagnetic Simulations: Electromagnetic simulations of far-field spectra and the near-field distributions were performed using commercial software Ansys Lumerical FDTD. The optical constants of NbS3_3 and gold (Au) were obtained from Dusabe et al.[28] and Johnson and Christy's dataset[23], respectively. The geometries and dimensions are extracted from TEM images. Thickness values are obtained through Energy Filtered TEM (EFTEM) thickness mapping. A total-field-scattered-field (TSFS) source was positioned above the structures on the +z side. Perfectly matched layer (PML) boundary conditions were applied along all directions (±z\pm z, ±x\pm x, ±y\pm y). A 3D near-field field and power monitor were placed to encompass the structures and capture the fields. PINEM fields are calculated as F(x,y)=∫Ez(x,y,z)e−i(ω/v)zdzF(x,y) = \int E_z(x,y,z)e^{-i(\omega/v)z}\mathrm{d}z though numerical integration of simulated EzE_z field, where vv, the speed of the electron, is assumed 0.7c0.7c for our system[18, 20]. Additional box monitors are positioned around the structure to record the extinction efficiency.

Raman Spectroscopy: Colloidal Au nanoparticles with diameters of 10, 20, and 40 nm suspended in a citrate buffer solution (150 μ\muL) purchased from Sigma Aldrich were drop-cast onto bare c-sapphire and onto c-sapphire with VS-grown NbS3_3 nanowires. R6G (Sigma Albrich) was dissolved in deionized water at concentrations of 10−710^{-7} to 10−410^{-4} M, and about 25 μ\muL of solution was drop-cast onto each sample and dried at 80 °C on a hot plate. Raman spectra were acquired on a confocal XploRA PLUS Raman microscope with 532 nm excitation, a laser power of 5 mW, and a 100X objective. Each spectrum is the sum of 10 acquisitions of 10 s. Band intensities were determined after baseline subtraction, and the values reported in Figure 5c are the mean and standard deviation over 5-20 spots per sample.

Acknowledgements: The authors acknowledge Frances Ross (MIT) for initiating the collaboration. AN acknowledges the support from ICTAS’s Graduate Student Fellowship. Work performed at the Center for Nanoscale Materials, a U.S. Department of Energy Office of Science User Facility, was supported by the U.S. DOE, Office of Basic Energy Sciences, under Contract No. DE-AC02-06CH11357. This work used shared facilities at the Nanoscale Characterization and Fabrication Laboratory, which is funded and managed by Virginia Tech’s Institute for Critical Technology and Applied Science. Additional support is provided by the Virginia Tech National Center for Earth and Environmental Nanotechnology Infrastructure (NanoEarth), a member of the National Nanotechnology Coordinated Infrastructure (NNCI), supported by NSF (ECCS 1542100 and ECCS 2025151).

References

  1. [1]Balandin, A. A.; Kargar, F.; Salguero, T. T.; Lake, R. K. One-Dimensional van Der Waals Quantum Materials. Mater. Today 2022, 55, 74–91. https://doi.org/10.1016/J.MATTOD.2022.03.015
  2. [2]Island, J. O.; Molina-Mendoza, A. J.; Barawi, M.; Biele, R.; Flores, E.; Clamagirand, J. M.; Ares, J. R.; Sánchez, C.; Van Der Zant, H. S. J.; D’Agosta, R.; Ferrer, I. J.; Castellanos-Gomez, A. Electronics and Optoelectronics of Quasi-1D Layered Transition Metal Trichalcogenides. 2D Mater. 2017, 4 (2), 022003. https://doi.org/10.1088/2053-1583/AA6CA6
  3. [3]Patra, A.; Rout, C. S. Anisotropic Quasi-One-Dimensional Layered Transition-Metal Trichalcogenides: Synthesis, Properties and Applications. RSC Adv. 2020, 10 (60), 36413–36438. https://doi.org/10.1039/D0RA07160A
  4. [4]Ly, T.; Huang, X.; Zhang, W.; Deng, C.; Chen, F.; Wang, Y.; Long, J.; Gao, H.; Deng, L.; Ye, L.; Xiong, W. High-Responsivity Multiband and Polarization-Sensitive Photodetector Based on TiS3/MoS2 Heterojunction. ACS Appl. Mater. Interfaces 2022, 14 (43), 48812–48820. https://doi.org/10.1021/ACSAMI.2C12332/ASSET/IMAGES/LARGE/AM2C12332_0005.JPEG
  5. [5]Conejeros, S.; Guster, B.; Alemany, P.; Pouget, J. P.; Canadell, E. Rich Polymorphism of Layered NbS3. Chem. Mater. 2021, 33 (14), 5449–5463. https://doi.org/10.1021/ACS.CHEMMATER.1C01417/SUPPL_FILE/CM1C01417_SI_002.PDF
  6. [6]Bloodgood, M. A.; Wei, P.; Aytan, E.; Bozhilov, K. N.; Balandin, A. A.; Salguero, T. T. Monoclinic Structures of Niobium Trisulfide. APL Mater. 2017, 6 (2), 026602. https://doi.org/10.1063/1.5005813
  7. [7]Pham, T.; Reidy, K.; Thomsen, J. D.; Wang, B.; Deshmukh, N.; Filler, M. A.; Ross, F. M. Salt-Assisted Vapor–Liquid–Solid Growth of 1D van Der Waals Materials. Adv. Mater. 2024, 36 (24), 2309360. https://doi.org/10.1002/adma.202309360
  8. [8]Pham, T.; Nag, A.; Reidy, K.; Filler, M. A.; Ross, F. M. Synthesis and Guided Assembly of Niobium Trisulfide Nanowires and Nanowire Chains by Chemical Vapor Deposition. arXiv February 3, 2026. https://doi.org/10.48550/arXiv.2602.03971
  9. [9]Gramotnev, D. K.; Bozhevolnyi, S. I. Plasmonics beyond the Diffraction Limit. Nat. Photonics 2010, 4 (2), 83–91. https://doi.org/10.1038/nphoton.2009.282
  10. [10]Schuller, J. A.; Barnard, E. S.; Cai, W.; Jun, Y. C.; White, J. S.; Brongersma, M. L. Plasmonics for Extreme Light Concentration and Manipulation. Nat. Mater. 2010, 9 (3), 193–204. https://doi.org/10.1038/nmat2630
  11. [11]Thakur, A.; Singh, R.; Yadav, V.; Siddhanta, S.; Jayaramulu, K. Advancing SERS Applications of 2D Materials through the Interplay of Rational Design and Structure-Property Relationships. Small Methods 2025, 9 (8), 2402056. https://doi.org/10.1002/smtd.202402056
  12. [12]Li, X.; Zhu, J.; Wei, B. Hybrid Nanostructures of Metal/Two-Dimensional Nanomaterials for Plasmon-Enhanced Applications. Chem. Soc. Rev. 2016, 45 (11), 3145–3187. https://doi.org/10.1039/c6cs00195e
  13. [13]Xu, W.; Ling, X.; Xiao, J.; Dresselhaus, M. S.; Kong, J.; Xu, H.; Liu, Z.; Zhang, J. Surface Enhanced Raman Spectroscopy on a Flat Graphene Surface. Proc. Natl. Acad. Sci. 2012, 109 (24), 9281–9286. https://doi.org/10.1073/pnas.1205478109
  14. [14]Li, Z.; Zhai, L.; Zhang, Q.; Zhai, W.; Li, P.; Chen, B.; Chen, C.; Yao, Y.; Ge, Y.; Yang, H.; Qiao, P.; Kang, J.; Shi, Z.; Zhang, A.; Wang, H.; Liang, J.; Liu, J.; Guan, Z.; Liao, L.; Neacșu, V. A.; Ma, C.; Chen, Y.; Zhu, Y.; Lee, C.-S.; Ma, L.; Du, Y.; Gu, L.; Li, J.-F.; Tian, Z.-Q.; Ding, F.; Zhang, H. 1T-Transition Metal Dichalcogenide Monolayers Stabilized on 4H-Au Nanowires for Ultrasensitive SERS Detection. Nat. Mater. 2024, 23 (10), 1355–1362. https://doi.org/10.1038/s41563-024-01860-w
  15. [15]Liu, H.; Gage, T. E.; Singh, P.; Jaiswal, A.; Schaller, R. D.; Tang, J.; Park, S. T.; Gray, S. K.; Arslan, I. Visualization of Plasmonic Couplings Using Ultrafast Electron Microscopy. Nano Lett. 2021, 21 (13), 5842–5849. https://doi.org/10.1021/acs.nanolett.1c01824
  16. [16]Tanriover, J.; Li, Y.; Gage, T. E.; Arslan, I.; Liu, H.; Mirkin, C. A.; Aydin, K. Unveiling Spatial and Temporal Dynamics of Plasmon-Enhanced Localized Fields in Metallic Nanoframes through Ultrafast Electron Microscopy. ACS Nano 2024, 18 (41), 28258–28267. https://doi.org/10.1021/ACS NANO.4C08875/ASSET/IMAGES/LARGE/NN4C08875_0006.JPEG
  17. [17]Barwick, B.; Flannigan, D. J.; Zewail, A. H. Photon-Induced near-Field Electron Microscopy. Nature 2009, 462 (7275), 902–906. https://doi.org/10.1038/nature08662
  18. [18]Park, S. T.; Lin, M.; Zewail, A. H. Photon-Induced near-Field Electron Microscopy (PINEM): Theoretical and Experimental. New J. Phys. 2010, 12 (12), 123028. https://doi.org/10.1088/1367-2630/12/12/123028
  19. [19]Park, S. T.; Yurtsever, A.; Baskin, J. S.; Zewail, A. H. Graphene-Layered Steps and Their Fields Visualized by 4D Electron Microscopy. Proc. Natl. Acad. Sci. 2013, 110 (23), 9277–9282. https://doi.org/10.1073/pnas.1306661110
  20. [20]Yurtsever, A.; Baskin, J. S.; Zewail, A. H. Entangled Nanoparticles: Discovery by Visualization in 4D Electron Microscopy. Nano Lett. 2012, 12 (9), 5027–5032. https://doi.org/10.1021/nl302824f
  21. [21]Pham, T.; Nag, A. Vapor–Liquid–Solid Growth of Unconventional Nanowires. Chem. Mater. 2026. https://doi.org/10.1021/acs.chemmater.6c01372
  22. [22]Saleh, B.; Teich, M. Fundamentals of Photonics; John Wiley & Sons, Inc., 1991.
  23. [23]Johnson, P. B.; Christy, R. W. Optical Constants of the Noble Metals. Phys. Rev. B 1972, 6 (12), 4370–4379. https://doi.org/10.1103/PhysRevB.6.4370
  24. [24]Guthmuller, J.; Champagne, B. Resonance Raman Spectra and Raman Excitation Profiles of Rhodamine 6G from Time-Dependent Density Functional Theory. ChemPhysChem 2008, 9 (12), 1667–1669. https://doi.org/10.1002/cphc.200800253
  25. [25]Talib, M.; Tripathi, N.; Manzoor, S.; Sharma, P.; Pavelyev, V.; Volkov, V. S.; Arsenin, A. V.; Novikov, S. M.; Mishra, P. TiS3 Nanoribbons: A Novel Material for Ultra-Sensitive Photodetection across Extreme Temperature Ranges. Sensors 2023, 23 (10), 4948. https://doi.org/10.3390/s23104948
  26. [26]Pan, Z.; Lu, G.; Li, X.; McBride, J. R.; Juneja, R.; Long, M.; Lindsay, L.; Caldwell, J. D.; Li, D. Remarkable Heat Conduction Mediated by Non-Equilibrium Phonon Polaritons. Nature 2023, 623 (7986), 307–312. https://doi.org/10.1038/s41586-023-06598-0
  27. [27]Song, C.; Yuan, X.; Huang, C.; Huang, S.; Xing, Q.; Wang, C.; Zhang, C.; Xie, Y.; Lei, Y.; Wang, F.; Mu, L.; Zhang, J.; Xiu, F.; Yan, H. Plasmons in the van Der Waals Charge-Density-Wave Material 2H-TaSe2. Nat. Commun. 2021, 12 (1), 386. https://doi.org/10.1038/s41467-020-20720-0
  28. [28]Dusabe, B.; Dongho-Nguimdo, G. M.; Joubert, D. P. Pressure Effect on Structural Stability and Optical Absorption of Triclinic NbS3 from DFT and Many-Body Perturbation Calculations. Eur. Phys. J. B 2020, 93 (7), 122. https://doi.org/10.1140/epjb/e2020-10060-3

Paper details

vlnc:W_jpnxg5ch
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 3

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents