WorksPhysics and Astronomy
EuCdAs: a magnetic semiconductor
Abstract
EuCdAs is now widely accepted as a topological semimetal in which a Weyl phase is induced by an external magnetic field. We challenge this view through firm experimental evidence using a combination of electronic transport, optical spectroscopy and excited-state photoemission spectroscopy. We show that the EuCdAs is in fact a semiconductor with a gap of 0.77 eV. We show that the externally applied magnetic field has a profound impact on the electronic band structure of this system. This is manifested by a huge decrease of the observed band gap, as large as 125~meV at 2~T, and consequently, by a giant redshift of the interband absorption edge. However, the semiconductor nature of the material remains preserved. EuCdAs is therefore a magnetic semiconductor rather than a Dirac or Weyl semimetal, as suggested by ab initio computations carried out within the local spin-density approximation.
Magnetic Weyl semimetals have harboured the great hope of bringing spintronics and topology together, unfortunately, to a great extent only in theory. Candidate materials where the magnetic Weyl phase might come to fruition are scarce, and their solid experimental confirmations are even scarcer [1, 2, 3, 4, 5]. EuCdAs has been seen as one of a few rare magnetic Weyl semimetals stable under ambient conditions, with large Eu spins positioned on a frustrated triangular lattice. The interplay of frustrated magnetism with topological bands made EuCdAs into a hopeful playground for a broad range of exciting phenomena [6, 7]. Through an extreme sensitivity of valence and conduction bands to Eu magnetism, external fields would then modify the band structure [8]. This compound has up to this point been proposed and interpreted as a Weyl semimetal, based upon ab initio band structure calculations, electronic transport and photoemission measurements [6, 8, 9, 10].
In this work, we study ultraclean EuCdAs crystals. Electronic transport measurements indicate an extremely low hole concentration. Accordingly, optical conductivity shows no detectable Drude component, and a strong Reststrahlen phonon mode. Our pump-probe photoemission measurement points to a clear band gap, and a carrier lifetime in the picosecond time scale. These experiments, together with extensive optical measurements,
provide decisive proof that EuCdAs is a semiconductor, and not a topological semimetal as previously thought [6, 9, 10, 11, 12, 13]. We deduce a band gap of 770 meV. Our results underline the need for more adapted band structure calculations. Moreover, our results demonstrate that the band structure of EuCdAs changes dramatically in an external magnetic field, due to an intimate coupling to localized Eu spins. All of these effects persist up to high temperatures, deep within the paramagnetic phase. We understand this through a strong exchange coupling of Eu localized spins to the band states originating from Eu , and orbitals.
Single crystals of EuCdAs were prepared by the Sn-flux method [6]. Details of sample synthesis, X-ray and electron probe microanalysis are described in Supplemental Material (SM) [14]. Carrier density was changed through controlling the purity of the starting materials. To increase the crystal size and quality, a two-step process was employed, where the crystals from the first growth were used as a seed material for the final growth. The layered trigonal lattice of EuCdAs, shown in the inset of Figure 1(a), results in triangular and hexagonally shaped crystals. The flux-growth of single crystals leads to an optically isotropic (001) surface. Blocks of CdAs are sandwiched between the Eu planes, with similar distances to binary semiconducting CdAs [15]. We have determined infrared reflectance and transmission [16, 17], complemented by infrared measurements in magnetic fields up to 16 T, for details see SM [14]. Time-resolved photoemission (tr-ARPES) experiments were carried out at the EPFL LACUS, at the ASTRA end station [18] of the Harmonium beamline [19], with details described in SM [14].

Figure 1. (a) Resistivity as a function of temperature for an insulating and a metallic sample. Inset shows the structure of EuCdAs, with Eu atoms shown in green, Cd atoms in yellow, and As atoms in purple. Magnetic properties, (b) dc susceptibility, and (c) magnetization at 4 K, are shown for the same two sample batches. (d) Static ARPES band map. (e) Pump-probe ARPES experiment results at a delay of 200 fs, where red means increased count rate after the pump-pulse excitation. (f) Time traces of the intensity integrated at different energies above the Fermi level. The integration is done for a 200 meV window around the indicated energy. (g) Infrared reflectance at different temperatures, for the insulating sample batch. (h) Transmission and reflectance at 5 K, and their multilayer modelling, which results in (i) the real part of the optical conductivity, .
Through a controlled crystal synthesis, we obtained insulating samples of EuCdAs, which have not been reported before. Figure 1(a) shows the resistivity of an insulating sample, resulting from a higher-purity synthesis, compared to a metallic sample, made through a standard purity synthesis. The resistivity of a high-purity sample is thermally activated above , with an activation energy of meV, flattening above 170 K. Given the Hall coefficient sign, this indicates that thermal activation from the acceptor states is present up to 170 K and valence band transport above. A strong activation energy decrease in a magnetic field, and the corresponding colossal negative magnetoresistance, is expected for magnetic semiconductors in a paramagnetic phase [20, 21], in agreement with our resistivity in magnetic fields [14].
The standard synthesis results in metallic behavior above 50 K, consistent with previous reports. Interestingly, in both samples the resistivity peak at K coincides with a sharp, symmetric peak in the magnetic susceptibility, in Figure 1(b), and an antiferromagnetic (AFM) ordering [9]. The susceptibility in both metallic and insulating samples shows no difference between the zero-cooled and field-cooled (measured in 10 mT) values above 3.5 K [14], excluding a possible ferromagnetic phase above [22]. The magnetization is measured with the field applied along the axis, perpendicular to the Eu planes. first steeply and linearly increases up to 0.8 T, followed by a kink at 1.8 T, reaching a saturated value of /Eu atom. This corresponds to the divalent Eu with half filled orbitals, like in EuTe [23]. The initial steep slope of is consistent with a ferromagnetic structure within each layer, and a relatively weak magnetic anisotropy expected for atoms with a half-filled orbital. Despite a strong difference in the resistivity, the susceptibility and magnetization are very similar in both samples, implying a weak effect of residual doping on magnetic properties. Both samples are insulating or at the localization boundary, meaning there are insufficient band carriers at low temperatures to change by the RKKY mechanism.
The resistivity of the sample with lower residual doping strongly disagrees with the widely accepted notion that EuCdAs is a semimetal, and instead suggests it is a semiconductor. To confirm this, we turn to photoemission measurements of the more resistive samples. Figure 1(d) shows a static ARPES band map, where the band structure agrees with the published spectra [6, 8, 9]. A strong band is centered around 1.3 eV below the Fermi level, and the valence band is near the Fermi level. The results of a pump-probe experiment in Figure 1(e) show the conduction band minimum around 800 meV above the Fermi level. No further states are seen in the band gap under these conditions. The conduction band shows extremely high intensity and is visible without any data treatment. Time traces of the intensity integrated at different energies above the Fermi level are shown in Figure 1(f). The valence band maximum at meV, and the conduction band away from the minimum, both show a time delay of around 1 ps. In contrast, the conduction band minimum ( eV) shows hardly any decay within the full observed time range of 10 ps. The long recombination time implies an energy barrier, and confirms there is a band gap of meV. Similar results are obtained on a metallic sample [14].
The infrared properties of EuCdAs are shown in Figure 1(g-Figure 1i), determined for the insulating sample. Far-infrared reflectance, shown at several different temperatures in Figure 1(g), is dominated by two strong in-plane, Eu phonon modes, at 86 and 165 cm [24]. The higher frequency mode is an unscreened Reststrahlen mode, since there are no free carriers to screen it. The weak temperature dependence of the reflectance is typical of semiconductors. Moreover, the value of reflectance at low photon energies is far below unity, contrasting the behaviour of metals and semimetals. To obtain the precise value of the semiconducting band gap, we determine transmission through a thin EuCdAs sample. Transmission and reflectance are modelled using a multilayer model of the dielectric response [25]. Kramers-Kronig analysis of reflectance is unreliable as the sample is highly transparent in the mid-infrared range. The obtained optical conductivity, , is shown in Figure 1(i). The onset of absorption coincides with a sudden drop in transmission at 770 meV (6200 cm). No Drude component appears in the optical conductivity, in line with our resistivity measurement. Metallic samples [14] show screened phonons, in agreement with previous optical studies [24, 26]. In metallic and insulating samples, the infrared phonons appear at the same frequencies, and there is a strong increase of the optical conductivity above 1 eV. In both cases, the Drude contribution, if at all present, is minor. Based on the experimental evidence outlined thus far, we assert that EuCdAs is a semiconductor—in our case with a light -type doping—whose carrier density depends on the starting material purity and the crystal synthesis. The steep slope of the interband absorption edge at 770 meV is typical of a direct band gap [27]. This is consistent with the ARPES data in Figure 1(e), showing the accumulation of both photo excited electrons and holes at the point.
The electronic band structure of EuCdAs is remarkably tunable even with a small magnetic field. First, let us focus on the interband absorption edge, evident from magneto-transmission. In Figure 2a, transmission spectra taken at 4 K are shown at photon energies around the onset, as the magnetic field is increased in 50 mT steps up to 1 T. Relative magneto-transmission in a broader energy and magnetic field range is shown in color plots in Figure 2(b-Figure 2d), where in (d) we show the energy-derivative of the magneto-transmission. Stacked plots of relative transmission are shown in the Supplemental Material [14]. The sharp zero-field step at 770 meV transforms into a double-step feature already at the lowest fields. Below 0.5 T, the lower energy step shifts down in energy, and the higher energy step moves up in energy. The steps split by 160 meV/T, giving an effective factor with an extremely high value of [28]. This large splitting originates from exchange interaction rather than Zeeman splitting. Above 0.5 T, the higher energy step also begins to redshift. The splitting between the two steps saturates at about 50 meV. This is a signature of spin polarized bands, which differently absorb light with opposite circular polarization. The weak oscillations of the signal below the gap, Figure 2(d), are assigned to giant Faraday rotation induced in our gapped system, with spin-split electronic bands, due to interband absorption of light that differs for opposite circular polarizations [14, 29, 30]. Remarkably, the band gap decreases by meV under 2 T of applied field, reaching a plateau above 5 T.

Figure 2. (a) Near infrared transmission showing the interband absorption edge at low fields, T. (b) Color plot of relative magneto-transmission, , in a broad energy range, and up to 2 T. (c) Magneto-transmission and (d) its first energy-derivative, , in a broad energy and magnetic field range.
While the gap is strongly reduced, it never closes in field, and no band inversion is seen. Instead, the strong redshift of the band gap in Figure 2(b-Figure 2d), is proportional to Eu spin magnetization , similarly to EuTe [31]. This means that the molecular field approximation is valid, and can be written as:
where is an effective exchange energy between band carriers and Eu spins, , and is saturated Eu spin magnetization. Highly localized electrons will weakly hybridize with band states, and originates mainly from the intraatomic potential exchange interaction. This interaction is ferromagnetic. According to optical spectra of free Eu ions in the orbital momentum state (no spin-orbit coupling), , and meV [32, 33], in accord with measured trends of – exchange energies determined for rare earths in solids [34]. Applying the above expression to our data, we obtain meV. Therefore, we propose that the bands undergo a large splitting via – exchange coupling to Eu spins. Overall, our results provide a clear indication that the Eu magnetic sublattice controls the electronic band structure of the compound via a strong Eu onsite exchange interaction.
The natural question that follows is whether the observed effects are limited to the low-temperature AFM phase. Figure 3 shows a series of magneto-reflectivity color plots taken up to 16 T, at temperatures ranging from 4 to 140 K. In the magneto-reflectivity, we see the same kind of features as in the magneto-transmission: the band edge redshifting as magnetic field is applied, and a splitting between the upper and lower band gap edge. The zero-field band gap increases first, then decreases with increasing temperature. The splitting can be described by an effective factor, which drops from 1500 at 4 K to 80 at 140 K [14]. At all the temperatures up to 100 K, we see that the bands become polarized in high magnetic field, even deep within the paramagnetic phase. This shows that EuCdAs is a strong paramagnet, and that qualitatively there is no difference in its response whether the zero-field state is an AFM or a paramagnet. Interestingly, at all temperatures, the extracted band edge as a function of external magnetic field behaves qualitatively very similar to magnetization, see Figure 3(m-Figure 3n). This means that the Eq. (1) remains valid for all temperatures and all magnetic fields.

Figure 3. (a–l) Colorplots of relative infrared magneto-reflectivity, . Each panel represents a different temperature, going from the AFM phase below 9.5 K, deep into the paramagnetic phase. (m) Magnetization as a function of magnetic field, at the same set of temperatures where magneto-reflectivity is shown. (n) Onset of absorption extracted from the magneto-reflectivity color plots, at the same set of temperatures as in (m).
In conclusion, with the full weight of the experimental evidence presented in this Letter, we show decisively that EuCdAs is not a topological semimetal, but rather a semiconductor with a band gap of 770 meV. This finding was verified on a number of specimens originating in five different syntheses. The absorption onset dependence on the magnetic field mimics the shape of magnetization. The band gap strongly decreases in magnetic fields, but it never becomes inverted, and the semiconductor nature of the material remains preserved. These results show that more accurate ab initio studies are desired, scrutinizing in detail all the complexities of correlated electron physics in Eu-based compounds [35]. Nonetheless, the local Eu magnetic moments are responsible for band structure changes, through strong 4 exchange coupling to valence and conduction states.
We thank B. Fauqué, M. Müller, D. van der Marel, N. Schröter, A. Grushin, F. de san Juan, Iurii Timrov and Luca Binci for enriching conversations. We are grateful to N. Miller for the helpful comments. A.A. acknowledges funding from the Swiss National Science Foundation through project PP00P2 202661. This research was supported by the NCCR MARVEL, a National Centre of Competence in Research, funded by the Swiss National Science Foundation (grant number 205602). F.G. and J.H.D. acknowledge the funding through SNSF grant 200021_200362. M.N. and N.B. acknowledge the support of CeNIKS project co-financed by the Croatian Government and the EU through the European Regional Development Fund Competitiveness and Cohesion Operational Program (Grant No. KK.01.1.1.02.0013). This work has been supported by the ANR DIRAC3D. We acknowledge the support of LNCMI-CNRS, a member of the European Magnetic Field Laboratory (EMFL). This work was supported by the Foundation for Polish Science through the International Research Agendas program co-financed by the European Union within the Smart Growth Operational Programme. The work at the TU Wien was supported by the European Research Council (ERC Consolidator Grant No 725521).
References
[1] D. F. Liu, A. J. Liang, E. K. Liu, Q. N. Xu, Y. W. Li, C. Chen, D. Pei, W. J. Shi, S. K. Mo, P. Dudin, T. Kim, C. Cacho, G. Li, Y. Sun, L. X. Yang, Z. K. Liu, S. P. Parkin, C. Felser, and Y. L. Chen, Science 365, 1282 (2019).
[2] N. Morali, R. Batabyal, P. K. Nag, E. Liu, Q. Xu, Y. Sun, B. Yan, C. Felser, N. Avraham, and H. Beidenkopf, Science 365, 1286 (2019).
[3] S. Nie, T. Hashimoto, and F. B. Prinz, Physical Review Letters 128, 176401 (2022).
[4] J.-F. Wang, Q.-Z. Dong, Z.-P. Guo, M. Lv, Y.-F. Huang, J.-S. Xiang, Z.-A. Ren, Z.-J. Wang, P.-J. Sun, G. Li, and G.-F. Chen, Physical Review B 105, 144435 (2022).
[5] M. Kanagaraj, J. Ning, and L. He, Reviews in Physics 8, 100072 (2022).
[6] J. Z. Ma, S. M. Nie, C. J. Yi, J. Jandke, T. Shang, M. Y. Yao, M. Naumann, L. Q. Yan, Y. Sun, A. Chikina, V. N. Strocov, M. Medarde, M. Song, Y. M. Xiong, G. Xu, W. Wulfhekel, J. Mesot, M. Reticcioli, C. Franchini, C. Mudry, M. Müller, Y. G. Shi, T. Qian, H. Ding, and M. Shi, Science Advances 5, eaaw4718 (2019).
[7] Y. Xu, L. Das, J. Z. Ma, C. J. Yi, S. M. Nie, Y. G. Shi, A. Tiwari, S. S. Tsirkin, T. Neupert, M. Medarde, M. Shi, J. Chang, and T. Shang, Physical Review Letters 126, 076602 (2021).
[8] J. R. Soh, F. de Juan, M. G. Vergniory, N. B. M. Schröter, M. C. Rahn, D. Y. Yan, J. Jiang, M. Bristow, P. Reiss, J. N. Blandy, Y. F. Guo, Y. G. Shi, T. K. Kim, A. McCollam, S. H. Simon, Y. Chen, A. I. Coldea, and A. T. Boothroyd, Physical Review B 100, 201102(R) (2019).
[9] N. H. Jo, B. Kuthanazhi, Y. Wu, E. Timmons, T.-H. Kim, L. Zhou, L.-L. Wang, B. G. Ueland, A. Palasyuk, D. H. Rauh, R. J. McQueeney, K. Lee, B. Schrunk, A. A. Burkov, R. Prozorov, S. L. Bud’ko, A. Kaminski, and P. C. Canfield, Physical Review B 101, 140402(R) (2020).
[10] K. M. Taddei, L. Yin, L. D. Sanjeewa, Y. Li, J. Xing, C. dela Cruz, D. Phelan, A. S. Sefat, and D. S. Parker, Physical Review B 105, 124401 (2022).
[11] J. Ma, H. Wang, S. Nie, C. Yi, Y. Xu, H. Li, J. Jandke, W. Wulfhekel, Y. Huang, D. West, P. Richard, A. Chikina, V. N. Strocov, J. Mesot, H. Weng, S. Zhang, Y. Shi, T. Qian, M. Shi, and H. Ding, Advanced Materials 32, 1907565 (2020).
[12] J. R. Soh, C. Donnerer, K. M. Hughes, E. Schierle, E. Wesche, D. Prabhakaran, and A. T. Boothroyd, Physical Review B 98, 064419 (2018).
[13] J. R. Soh, E. Schierle, D. Y. Yan, H. Su, D. Prabhakaran, E. Wesche, Y. F. Guo, Y. G. Shi, and A. T. Boothroyd, Physical Review B 102, 014408 (2020).
[14] See Supplemental Material at http://link.aps.org/supplemental/xxxx for more information and data on sample synthesis and characterization; zero-field reflectance of metallic and insulating samples; expected temperature dependence of the Drude component in a semimetal; pump-probe ARPES measurement of a metallic sample; Faraday rotation; energy gap and the effective Landé factor; stacked plots of transmission and reflectivity in a magnetic field; resistivity in magnetic fields. The Supplemental Material includes the additional Refs. [27, 29, 36–40].
Supplemental Material for “EuCdAs: a magnetic semiconductor”
D. Santos-Cottin; I. Mohelský; J. Wyzula; F. le Mardelé; I. Kapon; S. Nasrallah; N. Barišić; I. Živković; J.R. Soh; F. Guo; K. Rigaux; M. Puppin; J.H. Dil; B. Gudac; Z. Rukelj; M. Novak; A.B. Kuzmenko; C. C. Homes; Tomasz Dietl; M. Orlita; Ana Akrap
In the Supplemental Materials, we describe the sample synthesis in more detail, and show X-ray diffraction (XRD) and Electron Probe Microanalysis (EPMA) characterization. We provide information on zero-field optical properties for metallic samples in comparison to the insulating sample, presented in the main text. We show that the behavior expected for a semimetal, in particular the Drude component, is not observed in our samples. For a metallic sample, we show the time-resolved ARPES data, similar to the data for the insulating sample which are presented in the main text. We show Faraday rotation in a high magnetic field. Next, we show the temperature dependence of the band gap, and the effective factor, extracted from the magneto-optical data in the main text. We also show that the band gap remains the same for samples made in different synthesis batches. Finally, we show the temperature dependence of the resistivity in magnetic fields.
Sample Synthesis and Characterization
Our single crystals of EuCdAs were prepared by the Sn-flux method [1]. Starting materials were mixed in the ratio Eu:Cd:As:Sns = 1:2:2:10. Carrier density was changed through controlling the purity of the starting materials. Metallic samples were obtained by using lower purity (2N) Eu pieces packed under mineral oil. Insulating samples were obtained in a two-step process where the crystals from the initial growth were used as feeding material for the second (final) growth, while paying attention to Eu purity. The used Eu pieces were 4N purity, packed under Ar, and had a shiny metallic luster prior to being used. A similar synthesis was recently performed by another group [2]. Single crystals of EuCdAs were characterized by powder
X-ray diffraction and Electron Probe Microanalysis (EPMA).
For the powder X-ray diffraction, a few well-shaped crystals with no visible traces of Sn flux on the surface were selected from the metallic and insulating batch. The diffraction pattern in both cases was recorded in the range of 10-120 degrees, and the collected data were analyzed by the Rietveld refinement using Profex 5.2.0 software interface [3]. The analysis confirmed that the samples’ structure belongs to the trigonal crystal system, with space group P-3m1 (no. 164), see Figure S1. No visible traces of secondary phases were detected. The parameters of the refinement are given in Table I and Table II.

Figure S1. Powder X-ray diffraction pattern of EuCdAs from the (a) metallic and (b) insulating batch. In both cases, the diffraction pattern confirms the structure of the trigonal crystal system with space group P-3m1 (no. 164). No traces of secondary phase or Sn flux have been detected.
| Atom | |||
| Eu | 0 | 0 | 0 |
| Cd1 | 1/3 | 2/3 | 0.6327(2) |
| Cd2 | 1/3 | 2/3 | -0.6327(2) |
| As1 | 1/3 | 2/3 | 0.2483(3) |
| As2 | 1/3 | 2/3 | -0.2483(3) |
Table I. Atomic positions for the metallic sample obtained from XRD powder refinement.
| Atom | |||
| Eu | 0 | 0 | 0 |
| Cd1 | 1/3 | 2/3 | 0.6317(2) |
| Cd2 | 1/3 | 2/3 | -0.6317(2) |
| As1 | 1/3 | 2/3 | 0.2556(3) |
| As2 | 1/3 | 2/3 | -0.2556(3) |
Table II. Atomic positions for the insulating sample obtained from XRD powder refinement.
For the insulating sample, we obtained the following lattice parameters: Å and Å. For the metallic sample, we obtained: Å and Å.
Most importantly, there is no change in the X-ray peak arrangement between the samples from the metallic and insulating batch.
The EPMA was done on the as-synthesized metallic sample, as shown in Figure S2. The composition was checked on multiple points on the sample surface, and it gave a good agreement with the stoichiometric ratio of Eu:Cd:As = 1:2:2. A small amount of Sn flux was detected on the sample’s surface. This small amount of Sn flux results in a feature at 3.5 K in the magnetic susceptibility , which is due to the superconducting transition of Sn.

Figure S2. Electron Probe Microanalysis (EPMA) of a metallic EuCdAs single crystal. The analysis is done at several points on the crystal surface designated by numbers 1 to 5.
INFRARED SPECTROSCOPY, MAGNETO-TRANSMISSION AND MAGNETO-REFLECTIVITY EXPERIMENTS
Infrared reflectance and transmission were measured using a Bruker Vertex 80v spectrometer, at temperatures from 5 K to room temperature, with in situ gold evaporation [4]. High energy reflectance was complemented by ellipsometry and X-ray data [5]. The magneto-transmission and magneto-reflectivity were measured in the Faraday configuration, in magnetic fields up to @page 8/15 starts_mid=1 ends_mid=1 16 T, and at temperatures from 4 K to 140 K. The light wave vector propagated parallel to the external magnetic field, aligned with the crystallographic axis. A Bruker Vertex 80v interferometer using an infrared source was coupled to the experiment using light-pipe optics. The sample was located in a superconducting coil and surrounded by the helium exchange gas.
TIME-RESOLVED PHOTOEMISSION EXPERIMENTS
Time-resolved photoemission (tr-ARPES) experiments were carried out at the EPFL LACUS, at the ASTRA end station [6] of the Harmonium beamline [7]. A single -polarized harmonic at an energy of 37 eV was selected by a time-preserving monochromator. The in situ cleaved sample was excited by an -polarized pump pulse at a fluence of 0.5 mJ/cm. The measurements were carried out at 80 K, with a temporal resolution better than 150 fs, an energy resolution of 150 meV, and an angular resolution of .
ZERO-FIELD REFLECTANCE OF METALLIC AND INSULATING SAMPLES
The optical reflectance at 5 K is shown for the metallic and insulating samples of EuCdAs in Figure S3. In both cases, the dominant feature are the two infrared active phonons of symmetry, at 86 and 165 cm, the latter forming a characteristic Reststrahlen band typical of semiconductors [9]. These frequencies agree well with the previous optical studies of EuCdAs [8]. The metallic sample shows a low-energy reflectance upturn, where as , and is similar to the previous results [8]. This low-energy upturn is indicative of a weak Drude contribution in the metallic samples. Figure S3 shows the reflectance of the metallic sample at various temperatures, again consistent with the previous results [8]. We note that the low-energy reflectance decreases with temperature . This is at odds with the expected semimetallic behavior, as we discuss below.

Figure S3. (a) Reflectance of an insulating and a metallic sample at 5 K, and (b) reflectance of a metallic sample at various temperatures. The arrows in (a) point to the two infrared-active phonon modes. Those modes are observed at the same frequencies, 86 and 165 cm, in both of our samples, and agree well with the previous work on a metallic sample [8].
PUMP-PROBE ARPES MEASUREMENT OF A METALLIC SAMPLE
For a metallic sample, in Figure S6 we show the static and pump-probe ARPES data. The data was taken in the same way as the data for the insulating sample, described and shown in the main text.

Figure S6. Faraday rotation measured at 4 K and 2 T.
The chemical potential is now deeper inside the valence band, in agreement with the metallic resistivity shown in the main text, in Figure 1(a). The bottom of the conduction band can be clearly resolved in the pump-probe spectra. Most important information is that, within the error bar, the band gap is the same as in the insulating sample, 0.7 0.1 eV.
The gap is determined from the distance between the valence band maximum and the conduction band minimum and the error bars are based on the experimental energy resolution.

Figure S4. (a) Static ARPES map of a metallic sample of EuCdAs. (b) Pump-probe ARPES spectrum on the same metallic sample, showing the conduction band, separated from the valence band by a sizeable gap.
TEMPERATURE DEPENDENCE OF THE DRUDE COMPONENT IN A SEMIMETAL
In a semimetal, the Drude component is expected to increase with , contrary to what is seen in the previously published work on EuCdAs [8], as well as in our data.
To illustrate the expected semimetallic behavior, we provide readers with a quantitative estimate of the Drude contribution to optical conductivity, and its temperature dependence, in an ideal Weyl semimetal with two cones. For simplicity, we consider a full electron-hole symmetry and the Fermi level that crosses the Weyl nodes. The latter condition implies that the Drude weight vanishes at low temperatures. The optical conductivity at can then be calculated using the expression by Ashby and Carbotte [10], which only reflects interband excitations:
Here, is the valley degeneracy, is the velocity parameter, and is the photon frequency. At higher temperatures, the above expression has to be complemented by the occupation factor, , where stands for the Fermi-Dirac distribution.
The result is shown in Figure S5 and (Figure S5) at , 100, 200 and 300 K and for two different velocity parameters, and m/s. These two values represent velocity parameters typical of Weyl semimetals. With increasing , the occupation factor – plotted separately in Figure S5 and (Figure S5), for clarity – gradually suppresses the strength of interband excitations at low photon energies. This is due to a simple occupation effect that reflects electrons excited thermally from the valence to the conduction band. The thermally excited charge carries, both electrons and holes, give rise to a Drude-type part of optical conductivity, whose strength equals the thermally suppressed contribution of interband excitations. The resulting real part of optical conductivity, comprising both the Drude and interband excitations, is plotted in Figure S5 and (Figure S5). Here we assumed the characteristic broadening of 10 meV for the Drude peak.

Figure S5. Panels (a) and (e) show the interband optical conductivity calculated for two different Fermi velocities, and m/s. In (b) and (f) we show the occupational factor. Panels (c) and (g) show the total optical conductivity, which is a sum of the Drude term and the interband contribution. In (d) and (h) we show the calculated reflectance for the Drude part alone, showing the plasma edge which shifts to higher energies as the temperature increases.
To estimate the impact of the thermally-induced Drude component on the overall optical response at low photon energies, we have calculated the corresponding reflectivity spectra, again as a function of and for two characteristic values of the velocity parameter, see Figure S5 and (Figure S5). To simplify our calculations, we have only included the Drude contribution, complemented by a background dielectric constant (). We see that the thermally excited carriers give rise to a pronounced plasma-edge feature in the calculated reflectivity spectra. Hence, even though it is absent at low temperatures, the Drude contribution becomes relevant at higher temperatures and it is expected to impact profoundly the optical response at K.
Let us note that this behavior – quantitatively evaluated for the case of an ideal Weyl semimetal – should be characteristic of any gapless phase, or even of weakly gapped systems, provided that the gap is significantly smaller than . The thermally induced Drude contribution should always be present at higher , with the weight that reflects the particular profile of the (joint) density of states at low energies. On the other hand, the thermally-activated Drude component should stay negligible in systems with the energy band gap that is significantly larger than . This latter scenario is consistent with our data and also with the previous work on EuCdAs [8]. We observe neither a temperature increase in the Drude component, nor a development and increase of a plasma edge.
Faraday Rotation
In the main text, the magneto-transmission shows weak oscillations below the band gap, see Figure 2(d) of the main text. These
oscillations are related to the Faraday rotation. Faraday rotation measures how much polarization of the incident beam is rotated by the sample in a magnetic field.
EuCdAs is a gapped system, which becomes spin-polarized in a magnetic field. The two circular polarizations of light are absorbed differently. These two polarizations are mixed in our magneto-transmission measurements, but are separate in the measurement of Faraday rotation, shown in Figure S6. We see that the Faraday rotation shows strong oscillations below the band gap, similar to [11]. Hence, the left and right circularly polarized light is not equally absorbed, which manifests as oscillations in the magneto-transmission.
ENERGY BAND GAP AND THE EFFECTIVE FACTOR
The effective factor and band gap can be extracted from the temperature dependent magneto-optical reflectivity, shown in the Figure 3(a–Figure 3l) of the main text. The resulting values are shown in Figure S7. The large drop of the effective factor takes place as the magnitude of magnetization at given magnetic field decreases rapidly with temperature above . From 4 to 40 K, the band gap increases as the temperature increases. Above 40 K, the band gap decreases as the temperature grows.

Figure S7. (a) Effective factor and (b) band gap, both as a function of temperature, extracted from the temperature-dependent relative magneto-reflectance.
STACKED PLOTS OF TRANSMISSION AND REFLECTIVITY IN A MAGNETIC FIELD
In the main text, we show color plots of relative magneto-transmission (Figure 2b–Figure 2d) and magneto-reflectance (Figure 3a–Figure 3l). Below, in Figure S8 and Figure S9 we show the same data as a series of stacked plot made out of individual curves. For clarity, some of the data is omitted.

Figure S8. Relative magneto-transmission shown up to the field of (a) 2 T and (b) 16 T, as a function of incident photon energy. Magneto-transmission is normalized by a field-average in (a) and by zero-field transmission .

Figure S9. Relative magneto-reflectivity, normalized by the zero-field reflectivity , and shown up to the field of 16 T for a series of different temperatures.
COMPARISON OF MAGNETO-OPTICAL DATA FOR DIFFERENT SAMPLES
The same band gap is present in all the samples we have measured. In Figure S10 we show results of magneto-optical measurements performed on six samples coming from five different single crystal syntheses. Samples (c-f) are from the same synthesis batch. Sample (a-b) is discussed in the main text. In all the measurements, there is a clear and strong feature near 0.77 eV (or 6200 ) for the field T. This feature corresponds to the band gap. The band gap changes very similarly in all the measured samples, strongly decreasing in field.

Figure S10. (a,c,e,g,i,k) Magneto-transmission and (b,d,f,h,j,l) its first energy-derivative, , shown in a broad energy up to magnetic field of 4 T.
RESISTIVITY IN MAGNETIC FIELDS
In the main text, we show the resistivity of an insulating and a metallic sample. Figure S11 shows the Arrhenius plot for the resistivity of an insulating sample, with the activation energy of 26 meV, in the temperature range 25 – 175 K. In a magnetic field, Figure S11, the resistivity drops several orders of magnitude, but remains activated at low temperature, without becoming metallic. Interestingly, a similar profound drop in the resistivity, spanning several orders of magnitude, was observed in a magnetic field in other insulating (gapped) magnetic systems, e.g., based on europium [12] or manganese [13].

Figure S11. (a) Resistivity showing activated behavior, with activation of 26 meV. (b) Resistivity in different magnetic fields, up to 7 T.
References
- [1]J. Z. Ma, S. M. Nie, C. J. Yi, J. Jandke, T. Shang, M. Y. Yao, M. Naamneh, L. Q. Yan, Y. Sun, A. Chikina, V. N. Strocov, M. Medarde, M. Song, Y. M. Xiong, G. Xu, W. Wulfhekel, J. Mesot, M. Reticcioli, C. Franchini, C. Mudry, M. Müller, Y. G. Shi, T. Qian, H. Ding, and M. Shi, Science Advances 5, eaaw4718 (2019).
- [2]B. Kuthanazhi, K. R. Joshi, S. Ghimire, E. Timmons, L.-L. Wang, E. Gati, L. Xiang, R. Prozorov, S. L. Bud’ko, and P. C. Canfield, Physical Review Materials 7, 034402 (2023).
- [3]N. Doebelin and R. Kleberg, Journal of Applied Crystallography 48, 1573 (2015).
- [4]C. C. Homes, M. Reedyk, D. A. Cradles, and T. Timusk, Applied Optics 32, 2976 (1993).
- [5]D. B. Tanner, Physical Review B 91, 035123 (2015).
- [6]A. Crepaldi, M. Chergui, H. Berger, A. Magez, P. Bugnon, F. van Mourik, J. Ojeda, C. A. Arrell, G. Gatti, S. Roth, and M. Grioni, CHIMIA 71, 273 (2017).
- [7]J. Ojeda, C. A. Arrell, J. Grilj, F. Frassetto, L. Mewes, H. Zhang, F. van Mourik, L. Poletto, and M. Chergui, Structural Dynamics 3, 023602 (2015).
- [8]H. P. Wang, D. S. Wu, Y. G. Shi, and N. L. Wang, Physical Review B 94, 045112 (2016).
- [9]P. Y. Yu and M. Cardona, Fundamentals of Semiconductors (Springer, Berlin Heidelberg, 2010).
- [10]P. E. C. Ashby and J. P. Carbotte, Phys. Rev. B 89, 245121 (2014).
- [11]L. Ohnoutek, M. Hakl, M. Veis, B. A. Piot, C. Faugeras, G. Martinez, M. V. Yakushev, R. W. Martin, Č. Draśar, A. Materna, G. Strzelecka, A. Hruban, M. Potemski, and M. Orlita, Scientific Reports 6, 19087 (2016).
- [12]S. Von Molnar and S. Methfessel, Journal of Applied Physics 38, 959 (1967).
- [13]Y. Tokura, Reports on Progress in Physics 69, 797 (2006).