WorksPhysics and Astronomy
Nanoparticles of NbC produced by laser ablation in liquid: a study of structural, magnetic and superconductivity properties
Abstract
Niobium carbide (NbC) is a high-field Type II superconductor with a critical temperature () of 11.1 K, just above that of pure Nb ( K). Downsizing NbC to the nanoparticle scale introduces significant alterations in its critical field and/or the superconducting temperature. Here we report on superconducting NbC nanoparticles with 10 K synthesized by laser ablation in acetone, using the lens-target distance (laser fluence) and centrifugation as control parameters of the particle size. X-ray diffraction analyses certified the cubic NbC phase and electron microscopy images revealed spherical particles with average size near 8 nm, with no apparent size dependence on fluence. Besides, magnetization curves exhibited magnetic loops featuring a saturation magnetization around /molecule along with a small and typical superconducting loop for all investigated samples. We also observed a suppression of the diamagnetic behavior below upon decreasing laser fluence. Moreover, all samples exhibited a weak electron spin resonance (ESR) Curie-like signal at probably associated with localized defects in the particle's surface. The intriguing coexistence of superconductivity and magnetism in nanoparticles has recently garnered significant research attention. This complex scenario and unique properties are due to the substantial increase of surface-to-volume ratio in these superconducting NbC nanoparticles and further investigation would be crucial to unveil novel material properties and shed new light on our understanding of the superconducting phenomenon in this new morphology.
Abstract
Introduction
Niobium carbide (), a representative transition metal carbide, possesses distinctive physical properties featuring a simple -type cubic lattice, an elevated melting point (), remarkable hardness, high thermal and electrical conductivity, superior wear resistance, and chemical stability[1]. Such a versatile combination renders suitable for various applications, including cutting and grinding tools[2, 3], wear protection of surfaces[4, 5], catalysis[6], super-capacitors and hybrid ion capacitors[7]. As a Type II superconductor, is considered a key player in high-field superconductor applications, boasting excellent critical superconducting properties. Notably, within the realm of low-temperature superconductors, stands out with a relatively high superconducting transition temperature of K, just above that of pure Nb ( K), coupled with an impressive critical magnetic field () exceeding 4 T[8, 9, 10].
Despite extensive research since its discovery in 1964[11], considerable attention has been devoted to understand the superconducting properties of . Investigations have explored alterations in carbon vacancy density, varied production routes, and diverse synthesis techniques[12]. Additionally, numerous studies have probed the superconducting properties of in low-dimensional forms, such as thin films, nanofibers, and nanoparticles, exhibiting different morphologies[8, 13, 14]. However, challenges persist in the production of bulk or nanosystems based on with specific functionalities, primarily due to the high temperatures required. Nevertheless, the physical top-down synthesis method namely pulsed laser ablation have demonstrated capability of producing nanomaterials and it stands out as a “green” technique enabling the preparation of a substantial quantity of materials at room temperature[15, 16, 17, 18]. This process involves focusing a high-power pulsed laser on the Nb target surface, leading to the production of nanoparticles in organic solvents (such as acetone or ethanol). Interestingly, these particles are surrounded by a thin porous graphite layer, enhancing the chemical stability of the solution.[15]
Regardless of the substantial body of research on niobium carbide, there is a notable gap in data exploring the coexistence of magnetic and superconducting properties of nanoparticles produced through laser ablation. Therefore, in this work, we dedicated our efforts to the production and a detailed characterization of using laser ablation in acetone. By varying the laser fluence at the Nb target surface, we examined changes in the
Material and methods
The NbC nanoparticles were synthesized through pulsed laser ablation (LA) using a Nb target immersed in acetone. The LA process employed a Nd:Yag laser (1064 nm) with a 10 ns pulse duration and a 20 Hz repetition rate. Focused with a 50 mm lens, the laser was directed onto a freshly polished (sanded) surface of a Nb target (99.9% of purity) vertically positioned and submerged in 75 ml of acetone. The laser path through the liquid spanned a distance of 2 cm.
The ablation process continued for 20 minutes, resulting in a uniformly dark and stable solution. Initially, the NbC nanoparticles were synthesized under a laser fluency of . The resultant sample underwent centrifugation at 1000 RCF for 10 minutes, separating the supernatant (S1) from the sediment (P1). Subsequently, three additional samples were produced with laser fluencies of , , and , each of them subjected to the same procedure aforementioned. The resulting supernatant samples were named S2, S3, and S4, respectively. Finally, the powder samples investigated here were obtained from evaporating the acetone at room temperature.
Total reflection X-ray fluorescence (TXRF) elemental analysis of the samples revealed an exceptional purity level of 99.5% following the entire experimental procedure. The remaining 0.5 % primarily comprises iron contaminants, presumably coming from the sanding paper. The X-ray diffraction (XRD) measurements of the samples were performed in a Phaser D2 diffractometer (Bruker). Transmission electron microscopy (TEM) images were taken in a Talos F200X G2 equipment equipped with a field emission gun (FEG-X) source operating at 200 kV and in JEOL JEM-2100F also with a FEG gun source operating at 200 kV. TEM samples were prepared by dropping the acetone solution containing the nanoparticles on a copper grid with an ultra-thin hollow carbon film. The -dependent -magnetic susceptibility measurements of the powdered samples were carried out in a SQUID (Quantum Design, MPMS 3) magnetometer. The ESR experiments were carried out in a Bruker ELEXYS 500 ESR spectrometer at GHz (X-band), using an appropriate TE102 resonator coupled to an Oxford -controller helium gas flow system varying the temperature in the range of K K. Colloidal NPs and powdered bulk samples were dispersed in high purity paraffin for the ESR experiments.
Results and Discussion
Figure 1 illustrates the X-ray diffraction (XRD) patterns for the samples. All discernible diffraction patterns agree well with a cubic NbC structure (COD database code: 1011323). The diffraction peaks exhibit notable broadening beyond the instrumental resolution, indicative of a finite-size effect. Notably, the peak broadening observed in the P1 sample is less pronounced compared to the Si samples, suggesting a larger crystal size for P1. The determined lattice parameter for all nanoparticles samples is Å, in close proximity to the expected value for stoichiometric NbC ( Å)[1]. This suggests a negligible presence of carbon vacancies in the nanoparticles generated through laser ablation.[1] Additionally, certain samples exhibit peaks associated with hexagonal graphite (COD database code: 9014004).
Figure 2 displays representative transmission electron microscopy (TEM) images of P1, S2, and S3 samples, all exhibiting a similar spherical morphology with a broad size distribution, which was determined by counting nearly thousand particles in each specimen, as shown in Figure 2 (d). The associated size histograms were fitted with a log-normal function defined by and, thus, and were estimated. Therefore, the mean diameter and standard deviation were calculated.
Figure 2. Representative TEM images of P1 (a), S3 (b) and S2 (c) samples. The sample size distributions are presented in (d). The red lines are the best fit with a log-normal: the mean diameter () and the standard deviation () are displayed.

Figure 1. XRD patterns of samples P1, S1, S2, S3 and S4. The stars on the figure represent the cubic NbC diffraction pattern (COD: 9008682) and the circles the hexagonal graphite pattern (COD: 9014004).
It is noteworthy that the sedimented sample particles are considerably larger than those in the supernatant. In the former, the ablation process is broadly categorized as fragmentation, involving the detachment of hot atoms, vapors, and liquid drops out of thermodynamic equilibrium[17]. Specifically, the P1 particles are formed by the melt expulsion of the target during the ablation process. Conversely, in the supernatant (Si) samples, the nanoparticles are generated after the detachment of hot atoms and vapors. Notably, the and for Si samples do not substantially change with fluency and all of them exhibited nearly 8.5(5) nm size.
High-resolution TEM images reveal crystalline planes of NbC, as illustrated in Figure 2(c) for the (111) and (200) planes in two different particles. Additionally, a carbon shell is evident on the particle surface. Clear lattice fringes with an inter-planar spacing of 0.34 nm align precisely with the typical (002) plane of graphite carbon. In all S samples, 3 to 6 layers of graphite surround the NbC nanoparticles, whereas for the P1 sample, 9 to 20 carbon layers cap the NbC particles. Similar carbon encapsulated metals are obtained by the ablation of Ti, V, Nb, Cr, Mo, W, Zr, Ni and Co[15, 16, 19, 20].
Raman spectroscopy was employed to validate the presence of carbon and its crystalline structure in the carbon-encapsulated NbC samples. The Raman spectra of all five samples, as depicted in Figure 3, reveal two prominent bands at approximately (D band) and 1600 (G band). These bands correspond to the vibrations of carbon atoms with dangling bonds in the in-plane terminations of disordered graphite (D) and the vibrations in -bonded carbon atoms in a 2D hexagonal lattice (G), respectively, as established by Emanich et al.[21]. The relative intensity ratio varies across the sample regions, ranging from 0.89 to 2.89 for all samples. Although a precise value for cannot be unequivocally determined, the consistent elevated values suggest the presence of numerous structural defects in the synthesized carbon shells. This observation is in accordance with other carbon-encapsulated nanoparticles produced by laser ablation[15, 16].
Figure 3. Room temperature Raman spectra for all carbon-encapsulated NbC samples.
Magnetic measurements are presented in Figure 4 (a). The zero-field cooled (ZFC) magnetization as function of temperature revealed the onset of the superconducting critical temperature at K. This value is slightly smaller than that of stoichiometric bulk NbC ( K)[22], but aligns with reported values for NbC nanoparticles obtained through other methods[8]. Besides, no dependence of with the laser fluency employed in the ablation process was observed.
Figure 4. Zero field cooled magnetization at 20 Oe for all samples. Inset displays the zooming out of these measurements.
Moreover, a positive magnetization was observed for the S samples above , attributed to a paramagnetic contribution of C defects on the NbC surface nanoparticles. Interestingly, the magnetization was nearly zero for the P1 sample, within the accuracy of the equipment.
Below the critical temperature (), a notable decrease in the superconducting volume was observed when comparing the P1 sample with the S samples. Below in a bulk type II superconductor, the magnetic field is completely expelled from the sample volume, except for a surface layer with a thickness denoted by known as the London penetration length. Under ideal conditions, the magnetic susceptibility below is expected to be . For bulk NbC, is determined as 140 nm[23], meaning that the magnetic field only penetrates into the P1 particles partially, whereas it penetrates into the S particles completely. This results in a significant reduction of the Meissner effect when comparing with the bulk material, and it can be accounted by the following equation[24, 25]:
where represents the particle diameter and nm is the coherence length for NbC[23]. For particles with 8 nm diameter, eq. 1 leads to a diamagnetic susceptibility of emu/cmOe, consistent with the observations for the sample S4. However, a reduction of the Meissner susceptibility is noted upon decreasing the laser fluency (from S4 to S1 samples), which is attributed to an increase of defects other than C vacancies (i.e. NbC). On the other hand, emu/cmOe for the P1 particles, which have an average size larger than . This value is also smaller than the expected value for bulk NbC, . The observed value for P1 suggests a particle size more akin to 22 nm, way smaller than the average particle size estimated ( nm) and suggests the presence of numerous reminiscent defects in the crystalline structure, ultimately leading to a reduced superconducting volume. It is worth highlighting that the fabrication of nanoparticles through laser ablation in a liquid involves the detachment of hot atoms, vapors, and liquid drops followed by a rapid quenching of the material upon its interaction with the liquid[17]. This intricate process has the potential to generate a substantial amount of crystalline defects within the particle system.
The isothermal magnetization as function of magnetic field at 2K and 300K for the NbC samples are shown in Figure 5. The magnetization data was obtained after subtracting the diamagnetic contribution from the sample holder. Two distinct magnetic contribution are observed: a positive component and a superconducting loop at low temperature and low fields. The positive component, which is present even at room temperature, exhibits a larger magnetization for the P1 sample, decreasing with reduced fluency for the S samples. This positive magnetization with values on the order of emu/g and a coercitive field around 100 Oe at room temperature has been reported for materials reduced to a nanometric scale[26, 27, 28, 29, 30, 31, 32]. Surface ferromagnetism is suggested to be a universal feature in almost all nanoparticles of otherwise nonmagnetic inorganic materials, arising from surface cation or anion vacancies leading to ferromagnetic spin polarizations[26]. Moreover, since our P1 sample does not show any ESR signal (see the Figure 6) we conclude that this ferromagnetic signal is ESR silent. Furthermore, the coexistence of superconductivity and ferromagnetism at low temperature has been observed in NPs of metal[27, 28, 29], oxides[30, 31] and nitrides[32], but for the first time we report in carbides. However, it is acknowledged that this ferromagnetic signal may have originated from iron contamination in the synthesis process.

Figure 5. Magnetic hysteresis loops at 2K (a) and 300K (b). The insets in (a) provide a closer look at these curves at low field for the P1 sample (upper left) and S samples (lower right). Meanwhile, the inset in (b) is a magnified view at low field aimed at revealing the coercive field () of the order of 100 Oe at 300 K for this samples.
Figure 6. (a) Electron spin resonance (ESR) spectra at 300 K for P1, S1, S2, and S3 samples. In (b), ESR spectra for the S2 sample are presented at various temperatures. And in (c) the Normalized intensity of the S2 samples as function of . The red dashed line in (c) represent a Curie-like curve and inset the line width and resonance field at low .
The electron spin resonance (ESR) experiments shown in Figure 6(a) present narrow resonances of line width G and a -value at only for the S samples. These resonances are often attributed to localized spins present in the samples and can not be attributed to the iron contamination. A quantification of the amount of spins against a standard sample indicated that there are only 1 spin every 10 to 20 nanoparticles for the
S samples. However, within the accuracy of the ESR experiment the P1 sample does not present this ESR signal. This result indicates that this localized spin may be in the particles surface once the surface/volume rations for the S samples are about fifty times greater than that of the P1 sample.
The -dependence of the ESR spectra for the sample S2 is shown in the Figure 6 (b). By lowering the temperature the signal do not change much, however below 10 K the signal starts to broaden, shift toward higher fields and its intensity increase. Figure 6 (c) depicts the temperature dependence of the relative ESR intensity, . An illustrative Curie-like behavior reveals that the signal intensity displays an increase beyond this -dependence. Futhermore, as highlighted in the inset of Figure 6 (c), below , the linewidth increases, and a small resonance shift toward higher fields is observed. Similar phenomena, including increased and below , have been reported in bulk Type-II superconductors.[33] The line broadening is attributed to the field distribution within the superconducting vortex state, while the resonance shift is linked to the diamagnetism in the superconducting state. These results suggest that, in our samples, the localized spins on the particles’ surfaces are being influenced by the diamagnetism of the superconducting vortex state in NbC particles, presumably through proximity superconducting effects.[34]
Conclusions
In conclusion, our study successfully demonstrated the synthesis of superconducting NbC nanoparticles through low-temperature laser ablation in acetone. Notably, varying the laser fluence showed negligible impact on the average size of the resulting NbC nanoparticles, which exhibited a broad size distribution. Some particles displayed surface features indicative of graphite or amorphous material, potentially porous amorphous carbon. The elevation in laser fluence at syntheses process increase the volume of the superconducting fraction. Additionally, a paramagnetic contribution was evident across all samples, even in the sedimented sample. Particularly noteworthy was the observation that this magnetic moment increased with rising fluence, especially notable in the supernatant sample at lower temperatures. These findings contribute valuable insights into the synthesis and properties of NbC nanoparticles, offering avenues for further exploration and application in superconductivity research.
Acknowledgments
This study was mainly supported and performed under the auspices of the São Paulo Research Foundation (FAPESP) through Grant No. 2017/10581-1 (Thematic). F.F. acknowledges his postdoc FAPESP Grant No. 2019/13678-1. R.R.U also acknowledges the National Council for Scientific and Technological Development (CNPq) for support through Grant No. 314587/2021-7. This research used facilities of the Brazilian Nanotechnology National Laboratory (LNNano), part of the Brazilian Centre for Research in Energy and Materials (CNPEM), a private non-profit organization under the supervision of the Brazilian Ministry for Science, Technology, and Innovations (MCTI). The electronic microscopy staff is acknowledged for the assistance during the experiments (proposal number: 20230481).
References
- [1]M. G. D. V. Cuppari and S. F. Santos, “Physical properties of the nbc carbide,” Metals 6 (2016), 10.3390/met6100250.
- [2]E. Uhlmann, P. Meier, and D. Hinzmann, “Application of niobium carbide based cutting materials for peripheral milling of cfrp,” Procedia CIRP 85, 108–113 (2019).DOI
- [3]P. Montenegro, J. Gomes, R. Rego, and A. Borille, “Potential of niobium carbide application as the hard phase in cutting tool substrate,” International Journal of Refractory Metals and Hard Materials 70, 116–123 (2018).DOI
- [4]M. Woydt, H. Mohrbacher, J. Vleugels, and S. Huang, “Niobium carbide for wear protection – tailoring its properties by processing and stoichiometry,” Metal Powder Report 71, 265–272 (2016).DOI
- [5]M. Woydt and H. Mohrbacher, “Friction and wear of binder-less niobium carbide,” Wear 306, 126–130 (2013).DOI
- [6]S. Alhowity, K. Balogun, A. Ganesan, C. J. Lund, O. Omolere, Q. Adesope, P. Chukwunenye, S. C. Amagbor, F. Anwar, M. K. Altafi, F. D’Souza, T. R. Cundari, and J. A. Kelber, “Niobium carbide and tantalum carbide as nitrogen reduction electrocatalysts: Catalytic activity, carbophilicity, and the importance of intermediate oxidation states,” ACS Applied Materials & Interfaces 16, 2180–2192 (2024).DOI
- [7]G. Yang, X. Zhao, F. Liao, Q. Cheng, L. Mao, H. Fa, and L. Chen, “Recent progress and applications of niobium-based nanomaterials and their composites for supercapacitors and hybrid ion capacitors,” Sustainable Energy Fuels 5, 3039–3083 (2021).DOI
- [8]K. Bhattacharjee, S. P. Pati, and A. Maity, “High critical field nbc superconductor on carbon spheres,” Phys. Chem. Chem. Phys. 18, 15218–15222 (2016).DOI
- [9]G. Zou, H. Luo, S. Baily, Y. Zhang, N. Haberkorn, J. Xiong, E. Bauer, T. McCleskey, A. Burrell, L. Civale, et al., “Highly aligned carbon nanotube forests coated by superconducting nbc,” Nature Communications 2, 428 (2011).DOI
- [10]Y. Zhang, F. Ronning, K. Gofryk, N. A. Mara, N. Haberkorn, G. Zou, H. Wang, J. H. Lee, E. Bauer, T. M. McCleskey, A. K. Burrell, L. Civale, Y. T. Zhu, and Q. Jia, “Aligned carbon nanotubes sandwiched in epitaxial nbc film for enhanced superconductivity,” Nanoscale 4, 2268–2271 (2012).DOI
- [11]M. Wells, M. Pickus, K. Kennedy, and V. Zackay, “Superconductivity of solid solutions of tac and nbc,” Phys. Rev. Lett. 12, 536–538 (1964).DOI
- [12]A. I. Gusev and A. A. Rempel, “Superconductivity in disordered and ordered niobium carbide,” physica status solidi (b) 151, 211–224 (1989).DOI
- [13]D. Li, W. F. Li, S. Ma, and Z. D. Zhang, “Electronic transport properties of nbc(c)-c nanocomposites,” Phys. Rev. B 73, 193402 (2006).DOI
- [14]A. Fukunaga, S. Chu, and M. E. McHenry, “Synthesis, structure, and superconducting properties of tantalum carbide nanorods and nanoparticles,” Journal of Materials Research 13, 2465–2471 (1998).DOI
- [15]D. Zhang, C. Zhang, J. Liu, Q. Chen, X. Zhu, and C. Liang, “Carbon-encapsulated metal/metal carbide/metal oxide core–shell nanostructures generated by laser ablation of metals in organic solvents,” ACS Applied Nano Materials 2, 28–39 (2019).DOI
- [16]H. Zhang, J. Liu, Z. Tian, Y. Ye, Y. Cai, C. Liang, and K. Terabe, “A general strategy toward transition metal carbide/carbon core/shell nanospheres and their application for supercapacitor electrode,” Carbon 100, 590–599 (2016).DOI
- [17]V. Amendola and M. Meneghetti, “What controls the composition and the structure of nanomaterials generated by laser ablation in liquid solution?” Phys. Chem. Chem. Phys. 15, 3027–3046 (2013).DOI
- [18]L. M. Frias Batista, A. Nag, V. K. Meader, and K. M. Tibbetts, “Generation of nano-materials by reactive laser-synthesis in liquid,” Science China: Physics, Mechanics and Astronomy 65 (2022), 10.1007/s11433-021-1835-x.
- [19]H. Zhang, C. Liang, J. Liu, Z. Tian, and G. Shao, “The formation of onion-like carbon-encapsulated cobalt carbide core/shell nanoparticles by the laser ablation of metallic cobalt in acetone,” Carbon 55, 108–115 (2013).DOI
- [20]D. B. A, C. M, S. A, G. A, and T. R., “Transition metal carbide core/shell nanoparticles by ultra-short laser ablation in liquid.” Nanomaterials 14, 145) (2020).
- [21]R. J. Nemanich and S. A. Solin, “First- and second-order raman scattering from finite-size crystals of graphite,” Phys. Rev. B 20, 392–401 (1979).DOI
- [22]A. L. Giorgi, E. G. Szkl ar z, E. K. Storms, A. L. Bowman, and B. T. Matthias, “Effect of composition on the superconducting transition temperature of tantalum carbide and niobium carbide,” Phys. Rev. 125, 837–838 (1962).DOI
- [23]T. Shang, J. Z. Zhao, D. J. Gawryluk, M. Shi, M. Medarde, E. Pomjakushina, and T. Shiroka, “Superconductivity and topological aspects of the rocksalt carbides nbc and tac,” Phys. Rev. B 101, 214518 (2020).DOI
- [24]M. Tinkham, Introduction to superconductivity (Courier Corporation, 2004).
- [25]P. Zolotavin and P. Guyot-Sionnest, “Meissner effect in colloidal pb nanoparticles,” ACS Nano 4, 5599–5608 (2010).DOI
- [26]A. Sundaresan and C. Rao, “Ferromagnetism as a universal feature of inorganic nanoparticles,” Nano Today 4, 96–106 (2009).DOI
- [27]W.-H. Li, C.-W. Wang, C.-Y. Li, C. K. Hsu, C. C. Yang, and C.-M. Wu, “Coexistence of ferromagnetism and superconductivity in sn nanoparticles,” Phys. Rev. B 77, 094508 (2008).DOI
- [28]S. Bose, P. Raychaudhuri, R. Banerjee, P. Vasa, and P. Ayyub, “Mechanism of the size dependence of the superconducting transition of nanostructured nb,” Phys. Rev. Lett. 95, 147003 (2005).pubmed.ncbi.nlm.nih.gov/16241688
- [29]M.-H. Ma, E. Batsaikhan, H.-N. Chen, T.-Y. Chen, C.-H. Lee, W.-H. Li, C.-M. Wu, and C.-W. Wang, “Non-conventional superconductivity in magnetic in and sn nanoparticles,” Scientific Reports 12, 775 (2022).DOI
- [30]Z. Zhu, D. Gao, C. Dong, G. Yang, J. Zhang, J. Zhang, Z. Shi, H. Gao, H. Luo, and D. Xue, “Coexistence of ferromagnetism and superconductivity in ybco nanoparticles,” Phys. Chem. Chem. Phys. 14, 3859–3863 (2012).DOI
- [31]31M. Jirsa, M. Rames, and T. Wolf, “Interplay of paramagnetic signal with superconductive environment in a (nd,eu,gd)bacuo single crystal,” Journal of Physics: Conference Series 400, 022039 (2012).DOI
- [32]32R. Shipra, N. Kumar, and A. Sundaresan, “Surface ferromagnetism and superconducting properties of nanocrystalline niobium nitride,” Materials Chemistry and Physics 139, 500–505 (2013).DOI
- [33]33R. R. Urbano, P. G. Pagliuso, C. Rettori, Y. Kopelevich, N. O. Moreno, and J. L. Sarrao, “Field distribution and flux-line depinning in MgB₂,” Phys. Rev. Lett. 89, 087602 (2002).
- [34]34R. Holm and W. Meissner, “Messungen mit hilfe von flüssigem helium. xiii: Kontaktwider-stand zwischen supraleitern und nichtsupraleitern,” Zeitschrift für Physik 74, 715–735 (1932).DOI