betaFeedback

WorksPhysics and Astronomy

The rise of 212 MAX phase borides, Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S]: DFT insights into the physical properties for thermo-mechanical applications

Abstract

An interesting class of ternary metallic borides, known as the 212 MAX phase borides, is the recent advancement of the MAX phase family. In this article, results from ab-initio calculations on unexplored Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] are reported wherein Ti2_2PB2_2 along with its 211 boride phase Ti2_2PB are predicted for the first time. The stability was confirmed by calculating the formation energy, phonon dispersion curve, and elastic stiffness constants. The obtained elastic constants, elastic moduli, and Vickers hardness values of Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] were found to be significantly larger than those of their counterparts 211 borides and carbides, in a trend similar to other 212 borides. The studied compounds are brittle like most of the MAX and MAB phases. The electronic band structure and density of states revealed the metallic nature of the titled borides. Several thermal parameters were explored, certifying the suitability of Ti2PB2, Zr2PbB2, and Nb2AB2 [A = P, S] compared to their counterparts, and a similar trend was found for the other 212 borides. The obtained results predict that Ti2PB2, Zr2PbB2, and Nb2AB2 [A = P, S] have significant potential for use as efficient thermal barrier coating materials. The response of Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] to the incident photon was studied by computing the dielectric constant (real and imaginary part), refractive index, absorption coefficient, photoconductivity, reflectivity, and energy loss function. The ability to protect from solar heating was revealed from the studied reflectivity spectra. In this work, we have explored the physical basis of the improved thermo-mechanical properties of 212 MAX phase borides compared to their carbide and boride counterparts.

Introduction

The demand for novel materials with a better demonstration of their performances in various applications is increasing day by day in association with the advancement of technology. One of the best ways to achieve this goal is the prediction and/or synthesis of novel materials in addition to the existing ones that are used in various technological applications. Since the practical use of MAX phase results due to their peculiar physical properties, the prediction, synthesis as well as study of newly synthesized MAX phase materials have received huge interest from both applications as well as basic research points of view [1]. The term MAX represents a layered class of solids in which M is a representative of the transition metal group, A is a representative of the IIIA or IVA group in the periodic table and X is a C/N/B atom [2, 3, 4, 5, 6, 7, 8]. Despite the metallic nature of the MAX phase materials, they are also potential candidates for use as an alternative to high-temperature materials because of their ceramic-like characteristics [1, 4, 5, 9, 10]. A long list of their potential applications can be found elsewhere [1, 5, 11, 12, 13].

However, the main focus for the discovery of a new MAX phase was limited due only to the extension of either the M element or the A element [14, 15, 16, 17, 18, 19, 20, 21, 22, 23] or reporting of the MAX phase alloys by the combination of M, M′M^\prime, and A, A′A^\prime atoms; M, M′M^\prime = Ti, Zr, Hf, Ta, ….; A, A′A^\prime = Al, Ga, Si, Ge, P, … [24, 25, 26, 27, 28, 29, 30, 31, 32, 33]. The atom X was recognized as either C/N for a long time before the groundbreaking work of Khazaei et al. [5] where they have proposed B as an X element. Before this proposal, very few attempts were made to extend the MAX phase family by tuning the X elements in comparison with the attempts taken to extend by choosing the M and/or A element(s) for the same. Both the physical and chemical characteristics of B as well as B-containing compounds convey the prospects of the MAX phase borides by replacing C/N with boron [34].

In recent times such systems have been synthesized and are already listed as promising members of the MAX phases. Significant attention has also been paid to these MAX phase borides [6, 7, 8, 35, 36, 37, 38, 39, 40, 41, 42, 43]. The first report on the hypothetical MAX phase borides [M2AlB\mathrm{M}_2\mathrm{AlB} (M = Sc, Ti, Cr, Zr, Nb, Mo, Hf, or Ta)] was published by Khazaei et al. [6] where the trend in the electronic structures of the phase stability has been investigated. Gencer et al. [36] reported the electronic and vibrational properties of Ti2SiB\mathrm{Ti}_2\mathrm{SiB}. A predictive study of M2AlB\mathrm{M}_2\mathrm{AlB} (M = V, Nb, Ta) borides was performed by Surucu et al. [44]. The first synthesis of the M2SB\mathrm{M}_2\mathrm{SB} (M = Zr, Hf, and Nb) borides phase was carried out by Rackl et al. [7, 40]. Chakraborty et al. [41] predicted the V2AlB\mathrm{V}_2\mathrm{AlB} boride by B substitution in place of C in the V2AlC\mathrm{V}_2\mathrm{AlC}. A DFT study of M2AB\mathrm{M}_2\mathrm{AB} (M = Ti, Zr, Hf; A = Al, Ga, In) compounds was carried out by G. Surucu [42] in which the structural, electronic, elastic anisotropy, and lattice dynamical properties were considered. We have performed a comprehensive investigation of the synthesized borides M2SB\mathrm{M}_2\mathrm{SB} (M = Zr, Hf, and Nb) in our earlier report [43] where the physical properties of borides were compared with those of carbides. Boron substitutional effect on the carbon site in the Nb2SC\mathrm{Nb}_2\mathrm{SC} MAX phase was studied by Mitra et al. [37]. Substitution of C and N in place of the B-site of the first synthesized MAX boride Nb2SB\mathrm{Nb}_2\mathrm{SB} has also been reported [35]. Physical properties of predicted MAX phase borides Hf2AB\mathrm{Hf}_2\mathrm{AB} (A = Pb, Bi) have been reported by Hossain et al. [39]. Only one MAX phase boride belonging to the 413 sub-class has been investigated by A. Gencer [38] so far.

Miao et al. [8] have predicted MAX phase borides Hf2AB\mathrm{Hf}_2\mathrm{AB} (A = Bi, Pb) where they have calculated the formation energy and investigated their dynamical stability. Miao et al. [8] have also predicted another class of MAX phase materials crystallizing with different space groups (S.G.: 187, also called sub-space group of conventional MAX phase [8, 45]) of the hexagonal system. The traditional MAX phases are crystallized in the S.G.: 194 of the hexagonal system. The study [8] predicted six 212 [Ti2InB2\mathrm{Ti}_2\mathrm{InB}_2, Hf2AB2\mathrm{Hf}_2\mathrm{AB}_2 (In, Sn), Zr2AB2\mathrm{Zr}_2\mathrm{AB}_2 (A = In, Tl, Pb)] MAX phases and two 314 [Hf3PB4\mathrm{Hf}_3\mathrm{PB}_4, Zr3CdB4\mathrm{Zr}_3\mathrm{CdB}_4] MAX phases among which Ti2InB2\mathrm{Ti}_2\mathrm{InB}_2 (; No. 187) has already been synthesized [45]. Miao et al. [8] were inspired by the discovery of Ti2InB2\mathrm{Ti}_2\mathrm{InB}_2 [45] and other layered ternary borides known as the MAB phases have been investigated [46, 47, 48] in recent times. Although the B containing 212 and 314 MAX phases have layered structures that crystallize in a hexagonal system, the atomic arrangement in the cell is different from the conventional MAX phases as shown in Figure 1. As evident from the figure, there is a 2D layer of B sandwiched in between two Zr layers that significantly contribute in the enhancement of the structural stability and mechanical strength [49].

Figure 1. The unit cells of (a) Zr2_2PbB2_2 and (b) Zr2_2PbB/Zr2_2PbC MAX compounds.

Li et al. [50] also predicted some MAX phase borides consisting of 212 Nb2AB2\mathrm{Nb}_2\mathrm{AB}_2 [A = P, S] and 211 Nb2AB\mathrm{Nb}_2\mathrm{AB} [A = P, S]. Li et al. [50] have also compared their electronic and transport properties (e.g., the thermal conductivity) with 211 carbides Nb2AC\mathrm{Nb}_2\mathrm{AC} [A = P, S]. The stability of these phases was reported in terms of formation energy and dynamical stability. These compounds there are predicted to possess unusual thermal properties owing to the acoustic and optical contributions; and the anisotropic nature.

Motivated by the study of Miao et al [8] and Li et al [50], we have tried to explore the 212 Ti2PB2\mathrm{Ti}_2\mathrm{PB}_2 and 211 Ti2PB\mathrm{Ti}_2\mathrm{PB} MAX phase borides by the substitutional method. To do this, at first, we created the structure of Nb2PB2\mathrm{Nb}_2\mathrm{PB}_2 and Nb2PB\mathrm{Nb}_2\mathrm{PB} and calculated their physical properties. After then, we substituted the Nb atoms with Ti in both cases. Recently, the substitutional method has also been used by researchers to predict MAX phase borides [38, 41]. Finally, we calculated their formation energy and checked their dynamical and elastic stability.

So far, the physical properties of Ti2InB2\mathrm{Ti}_{2}\mathrm{InB}_{2} [51, 52], Hf2AB2\mathrm{Hf}_{2}\mathrm{AB}_{2} (A = In, Sn) [53], Zr2AB2\mathrm{Zr}_{2}\mathrm{AB}_{2} (A = In, Tl) [49], Hf3PB4\mathrm{Hf}_{3}\mathrm{PB}_{4} [54], and Zr3CdB4\mathrm{Zr}_{3}\mathrm{CdB}_{4} [55] MAX phases have been studied using the density functional theory (DFT) method. For each of the cases, the mechanical properties of B-containing compounds are found to be enhanced remarkably in comparison with their conventional C/N containing 211 MAX phases. The Debye temperature and melting temperature increased for boron-containing 212 phases compared to 211 carbides/nitrides. The minimum thermal conductivity also decreases for the same. The thermal expansion coefficient remains reasonably suitable for coating materials in borides. Thus, the enhanced thermo-mechanical properties of B-containing 212 MAX phases revealed their appropriateness for applications in high-temperature technology compared to the widely used 211 MAX phase carbides. These features of 212 MAX phases are very much motivational and we are interested to study the yet-to-be-investigated stable 212 MAX phase Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}. Though Li et al. [50] studied transport properties, electronic band structure, Fermi surface, etc. of Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] and Nb2AB\mathrm{Nb}_{2}\mathrm{AB}; the mechanical properties and other thermal parameters such as Debye temperature, melting temperature, etc. are not included in their study. Moreover, we have found that Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2} (212) and Ti2PB\mathrm{Ti}_{2}\mathrm{PB} (211) MAX borides are energetically, elastically/mechanically, and dynamically stable.

Therefore, in this study, the thermo-mechanical parameters of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] compounds have been studied employing the DFT method, and the properties are compared with those of other 212 MAX phases as well with their 211 counterpart carbides (Ti2PC\mathrm{Ti}_{2}\mathrm{PC}, Zr2PbC\mathrm{Zr}_{2}\mathrm{PbC}, Nb2AC\mathrm{Nb}_{2}\mathrm{AC} [A = P, S]) and borides (Ti2PB\mathrm{Ti}_{2}\mathrm{PB}, Zr2PbB\mathrm{Zr}_{2}\mathrm{PbB}, Nb2AB\mathrm{Nb}_{2}\mathrm{AB} [A = P, S]). It is noted that the 211 boride, Zr2PdB\mathrm{Zr}_{2}\mathrm{PdB}, has also been predicted in this study following the same procedure mentioned above.

Computational methodology

In this study, the physical properties of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] have been computed by CAmbridge Serial Total Energy Package (CASTEP) code [56, 57] via the plane-wave pseudopotential-based DFT method. The generalized gradient approximation (GGA) of the Perdew–Burke–Ernzerhof (PBE) [58] was used to treat the exchange and correlation functions. The electronic orbitals for B - 2s2 2p12s^{2}\ 2p^{1}, Pb- 6s26p26s^{2}6p^{2}, and Zr - 5s24p6 4d25s^{2}4p^{6}\ 4d^{2} were considered for pseudo-atomic calculations. The cutoff energy and kk-point grids [59] were set to 500 eV and 10×10×410 \times10 \times4. The geometry was relaxed by Broyden Fletcher Goldfarb Shanno’s (BFGS) technique [60] whereas density mixing was selected for the electronic structure calculations. Furthermore, the self-consistent convergence of the total energy was set to 5×10−65 \times10^{-6} eV/atom, and the maximum force per atom was taken as 0.01 eV/Å. A value of 5×10−45 \times10^{-4} Å and 0.02 GPa was fixed for the maximum ionic displacement and maximum stress. The bulk modulus (BB) and shear modulus (GG) were computed using Hill’s approximation [61, 62] which is the average value of the upper limit (Voigt [63]) and lower limit (Reuss [64]) of BB: [B=(BV+BR)/2][B = (B_{V} + B_{R})/2] and GG: [G=(GV+GR)/2][G = (G_{V} + G_{R})/2]. The BVB_{V}, BRB_{R}, GVG_{V}, and GRG_{R} can be expressed as follows: BV=[2(C11+C12)+C33+4C13]/9B_{V} = [2(C_{11} + C_{12}) + C_{33} + 4C_{13}]/9; BR=C2/MB_{R} = C^{2}/M; C2=(C11+C12)C33−2C132C^{2} = (C_{11} + C_{12})C_{33} - 2C_{13}^{2}; M=C11+C12+2C33−4C13M = C_{11} + C_{12} + 2C_{33} - 4C_{13}; GV=[M+12C44+12C66]/30G_{V} = [M + 12C_{44} + 12C_{66}]/30 and GR=(52)[C2C44C66]/[3BVC44C66+C2(C44+C66)]G_{R} = \left(\frac{5}{2}\right)[C^{2}C_{44}C_{66}]/[3B_{V}C_{44}C_{66} + C^{2}(C_{44} + C_{66})]; C66=(C11−C12)/2C_{66} = (C_{11} - C_{12})/2. The Young’s modulus (Y) has been estimated using the equation: Y=9BG/(3B+G)Y = 9BG/(3B + G) [65, 66]. The equation: ν=(3B−Y)/(6B)\nu= (3B - Y)/(6B) [65, 66] was used to compute the Poison’s ratio (ν\nu). The Cauchy pressure (CP) is obtained from the stiffness constants; CP=(C12−C44)CP = (C_{12} - C_{44}).

Results and discussion

Structural properties and stability

The structure of the conventional MAX phase is well known, but the structure of the B-containing 212 MAX phase is less familiar. To distinguish between the structures, the unit cell of both 212 (Zr2_2PbB2_2) and 211 (Zr2_2PbC) phases is presented as a representative in Figure 1. As seen, there is a clear difference in the atomic arrangements in these structures which is responsible for the different physical behaviors concerning mechanical, electronic, and thermal properties. Both 212 (Zr2_2PbB2_2) and 211 (Zr2_2PbB/Zr2_2PbC) are crystallized in the hexagonal system with different space groups. The 212 MAX phase belongs to the space group P6ˉm2\mathrm{P}\bar{6}\mathrm{m}2, (No. 187) [8] while the 211 MAX phase belongs to the space group of P63/mmc (194) [5]. The positions of M, A, and X atoms are different in the 212 and 211 MAX phases. The M (Zr) atoms are positioned at (1/3, 2/3, zMz_{\mathrm{M}}) in the 211 phase, whereas it is at (0.3333, 0.6667, 0.6935) in the 212 phase. The atomic positions of A (Pb) atoms are at (1/3, 2/3, 3/4) and at (0.6667, 0.3333, 0.0), respectively, for the 211 and 212 phases. The most important difference is the positions and contribution of the X atoms in the bulk crystals. The X (C) atoms occupy the corner position (0, 0, 0) in 211 phase while it (B) occupies two positions: (0.6667, 0.3333, 0.5) and (0.0, 0.0, 0.5) forming a 2D layer sandwiched in between the M layers. Within this 2D layer, the B atoms themselves make a strong covalent bond (B-B) that results in a comparatively more stable structure than that of the counterpart 211 MAX phase borides and carbides.

The unit cell of Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] are optimized to obtain the other physical properties. The cell constants calculated for the optimized structures are given in Table 1. A very good consistency is observed between the values obtained in this study and prior results [8, 50]. This reveals the precision of the parameters used for calculations in this work. The lattice constants of 211 borides are presented in Table S1 (in the supplementary document).

Phaseaa (Å)% of deviationcc (Å)% of deviationc/ac/aReference
Ti2_2PB2_23.12186.54572.09This work
Zr2_2PbB2_23.27870.088.42820.152.57This work
Zr2_2PbB2_23.2768.4152.57Ref [8]
Nb2_2PB2_23.19290.536.65170.422.08This work
Nb2_2PB2_23.216.682.08[50]
Nb2_2SB2_23.20250.546.65480.522.07This work
Nb2_2SB2_23.226.692.07[50]

Table 1. The lattice constants (aa and cc) and c/ac/a ratio of Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] MAX phases.

Miao et al. [8] have shown that the predicted 212 phases including Zr2_2PbB2_2 are thermodynamically stable by calculating the enthalpy with respect to the known competing phases. They have also calculated the phonon dispersion curves in which no imaginary frequency branch exists. In the case of Nb2_2AB2_2 [A = P, S], Li et al. [50] have shown their stability in terms of formation energy and phonon dispersion curves. The Ti2_2PB2_2 has been found to be stable because of the negative formation energy, non-existence of the imaginary frequency in the phonon dispersion curves, and fulfillment of the mechanical stability conditions by the calculated CijC_{ij}s. We have also calculated the phonon dispersion curve of Zr2_2PbB2_2 and Nb2_2AB2_2 [A = P, S] in this study wherein no imaginary frequency branch exists as shown in Figure 2a-d). This confirms the dynamical stability of these borides like the other 212 MAX phase borides. The phonon dispersion of corresponding 211 borides is also presented in Figure S1 (in the supplementary document). Moreover, the mechanical stabilities of Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] have also been checked in the following section. It is noted that the formation energy of Ti2_2PB2_2 is calculated from the well-known formula used for the prediction of MAX phase materials [67, 68, 69, 70, 71, 72]: Eform=EMAX−nMEM−nAEA−nXEXnM+nA+nXE_{form} = \frac{E_{MAX}-n_M E_M-n_A E_A-n_X E_X}{n_M+n_A+n_X}. In this case, we have calculated the energy of all the structures of the elements found in the materials projects [tabulated in Table S2] and computed the formation energy for different combinations. The calculated values of EformationE_{\mathrm{formation}} are found to be in the range from -1.03 to -2.38 eV/atom. Thus, it is expected that the predicted Ti2_2PB2_2 will be chemically stable.

Phase ID of TiEnergy of Ti (eV)Phase ID of PEnergy of P (eV)
mp-72-4809.31mp-53-179.58
mp-46-3206.1mp-118-4309.48
mp-6985-1602.97mp-130-359.271
mp-73-1603.02mp-157-718.668
mp-7245-359.269
Phase ID of BEnergy of B (eV)mp-12883-1436.49
mp-160-926.397mp-674158-174.21
mp-1193675-2160.86mp-1014013-718.626
mp-22046-3854.98mp-1094075-1796.33
mp-570316-3697.84mp-1179990-357.596
mp-570602-3848.55mp-1198724-7547.41
mp-632401-923.045
mp-1202723-922.895PhaseEnergy (eV)
mp-1055985-74.4371Ti2_2PB2_2-3545.42

Table S2. Different structures of Ti2_2PB2_2 composing elements.

Phonon dispersion curves of (a) Ti$_2$PB, (b) Zr$_2$PbB, (c) Nb$_2$PB, and (d) Nb$_2$PB MAX phase compounds

Figure S1. Phonon dispersion curves of (a) Ti2_2PB, (b) Zr2_2PbB, (c) Nb2_2PB, and (d) Nb2_2PB MAX phase compounds.

Phonon dispersion curves for Ti2PB2

(a)

Phonon dispersion curves for Zr2PbB2

(b)

Figure 2.

Phonon dispersion curves of Ti2PB2, Zr2PbB2, and Nb2AB2

Figure 2 (PDF p. 8). Phonon dispersion curves of Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S].

Mechanical properties

To bring out the figure of merit of the 212 MAX phases in light, it is necessary to discuss the possible relevant parameters for disclosing the mechanical properties. During the practical use of materials, many of them are subjected to applied forces or loads. Thus, knowledge of the related parameters is essential for the proper selection of the materials, otherwise, crack formation, mechanical failure, fracture introduction or structural deformation may take place. One of the key applications of the MAX phases is as structural components at high temperatures [73]. The constants used to unveil the mechanical behavior of solids are stiffness constants, tensile strength, elastic moduli, hardness, brittleness/ductility, fracture toughness, etc. Thus, the aforementioned parameters of Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] have been estimated and discussed [Table 2]. The first step in the study of mechanical properties is the calculation of single crystal elastic constants from which all the other mechanical parameters can be calculated.

The obtained single crystal elastic constants of the titled borides using the strain-stress method [51, 65, 74, 75, 76] are tabulated in Table 2 along with those of previously reported 212 MAX phases and their corresponding 211 borides and/or carbides phases. The study of mechanical stability is one of the ways for assessing the stability of solids under static stress used in practical applications. For this case, the stabilities of Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] are checked by the well-known stability conditions [77, 78] for hexagonal system as follows: C11>0C_{11} > 0, C11>C12C_{11} > C_{12}, C44>0C_{44} > 0, (C11+C12)C33−2(C13)2>0(C_{11} + C_{12})C_{33} - 2(C_{13})^2 > 0. The titled borides satisfy the above-stated conditions and hence they are predicted to be mechanically stable.

PhaseC11C_{11}C12C_{12}C13C_{13}C33C_{33}C44C_{44}BBGGYYHChenH_{\mathrm{Chen}}HMiaoH_{\mathrm{Miao}}G/BG/Bν\nuCPCPReference
Ti2_2PB2_23689012138318419815236124.7430.790.770.19-94This study
Ti2_2PB2618510532014815811026717.4820.650.700.21-63This study
Ti2_2PC27711913136417118411328214.9619.240.610.24-52This study
Zr2_2PbB2_22975772245761389523215.5517.730.690.22-19This study
Zr2_2PbB201564817758986616211.6112.120.670.22-02This study
Zr2_2PbC2206665216801167819113.0814.280.670.23-14This study
Nb2_2PB2_243811514747621324117943026.3635.490.740.20-98This study
Nb2_2PB35010714139519920714635521.5327.820.710.21-92This study
Nb2_2PC36812316240019422514435518.7225.240.640.23-71This study
Nb2_2SB2_23359013140415519613332619.2024.580.680.22-65This study
Nb2_2SB3268612632815118612831219.0723.860.690.22-65Ref [43]
Nb2_2SC31610815132512419210526712.0216.220.550.27-16Ref [43]
Zr2_2InB2_231546642638213810525119.1121.240.760.20-36Ref [49]
Zr2_2InC2866271248831369523115.8717.940.700.22-14Ref [82]
Zr2_2TlB2_23105261251661359422915.6817.710.700.22-21Ref [49]
Zr2_2TlC2556052207631158019513.9815.060.700.22-03Ref [83]
Hf2_2InB2_234361762789415411427419.4622.560.740.20-33Ref [53]
Hf2_2InC30981802739815210525616.7519.650.690.21-17Ref [82]
Hf2_2SnB2_2353658630611016512429721.0224.840.750.20-45Ref [53]
Hf2_2SnC251711072381011458721812.0014.500.600.25-30Ref [84]
Ti2_2InB2_236447582759414712228723.7226.440.830.17-47Ref [53]
Ti2_2InC28462512428712610023619.5720.920.790.18-25Ref [52]

Table 2. Table 2: The stiffness constants, CijC_{ij} (GPa), elastic moduli [BB, GG, YY] (GPa), hardness parameters, Pugh ratios, G/BG/B, Poisson ratios, ν\nu and Cauchy Pressures, CPCP (GPa) of M2_2AB2_2 (M =Ti, Zr, Hf, Nb; A = P, S, In, Sn, Tl, Pb) together with those of M2_2AC (M =Ti, Zr, Hf, Nb; A = P, S, In, Sn, Tl, Pb) compounds.

As can be seen in Table 2, the C11C_{11} and C33C_{33} values are not only higher for Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A=P,SA = \mathrm{P}, \mathrm{S}] compared to those of the corresponding 211 boride and carbide phases but also higher for other 212 phases compared to their 211 counterpart carbides. In case of C11C_{11}, the values are 41(33)%, 35(47)%, 25(19)%, and 12(16)% higher for Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A=P,SA = \mathrm{P}, \mathrm{S}], respectively than that of the counterpart borides (carbides). In addition, an increase of 10%, 22%, 11%, 40%, and 28% are also observed from the previously reported phases: Zr2InB2\mathrm{Zr}_{2}\mathrm{InB}_{2}, Zr2TlB2\mathrm{Zr}_{2}\mathrm{TlB}_{2}, Hf2InB2\mathrm{Hf}_{2}\mathrm{InB}_{2}, Hf2SnB2\mathrm{Hf}_{2}\mathrm{SnB}_{2}, Ti2InB2\mathrm{Ti}_{2}\mathrm{InB}_{2}, respectively, compared to their corresponding 211 counterparts. Similarly in case of C33C_{33}, the values are 20(5)%, 38(13)%, 20(19)%, and 23(24)% for Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A=P,SA = \mathrm{P}, \mathrm{S}], respectively than that of counterpart borides (carbides). Besides, an increase of 6%, 21%, 2%, 22%, and 14% is noted for Zr2InB2\mathrm{Zr}_{2}\mathrm{InB}_{2}, Zr2TlB2\mathrm{Zr}_{2}\mathrm{TlB}_{2}, Hf2InB2\mathrm{Hf}_{2}\mathrm{InB}_{2}, Hf2SnB2\mathrm{Hf}_{2}\mathrm{SnB}_{2}, and Ti2InB2\mathrm{Ti}_{2}\mathrm{InB}_{2}, respectively, compared to their corresponding 211 phases. It is well known that the C11C_{11} and C33C_{33} measure bonding strength along the aa- and cc-axis. Thus, an increase of C11C_{11} and C33C_{33} implies the increase of bonding strength along the mentioned directions; consequently, the overall bonding strength is expected to be increased for 212 phases which is also reflected in the values of elastic moduli and hardness values presented in Table 2. As we know, the bulk modulus (BB) measures the resistance against the uniform volume-changing hydrostatic pressure whereas the shear modulus (GG) measures the resistance against shape-changing plastic deformation. Comparative stiffness analysis of the solids can be done from the values of Young’s modulus (YY) which give a measure of the resistance against change in the length. In the case of BB, the values are found to be increased by 25(8)%, 41(19)%, 16(07)%, and 5(2)% for Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A=P,SA = \mathrm{P}, \mathrm{S}], respectively, compared to their counterpart borides and carbides. Similarly, shear moduli are observed to be increased by 38(34)%, 44(22)%, 23(24)%, and 4(26)%; and Young’s moduli are noted to be increased by 35(28)%, 43(21)%, 21(21)%, and 4(22)% for Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A=P,SA = \mathrm{P}, \mathrm{S}], respectively, compared to their counterpart borides and carbides. Moreover, for Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, Zr2InB2\mathrm{Zr}_{2}\mathrm{InB}_{2}, Zr2TlB2\mathrm{Zr}_{2}\mathrm{TlB}_{2}, Hf2InB2\mathrm{Hf}_{2}\mathrm{InB}_{2}, Hf2SnB2\mathrm{Hf}_{2}\mathrm{SnB}_{2}, and Ti2InB2\mathrm{Ti}_{2}\mathrm{InB}_{2} phases, the values of B[G(Y)]B[G(Y)] are increased by 1%[11%(9%)], 17%[18%(17%)], 1%[9%(7%)], 14%[43%(36%)], and 17%[22%(22%)] compared to their corresponding 211 phases Zr2InC\mathrm{Zr}_{2}\mathrm{InC}, Zr2TlC\mathrm{Zr}_{2}\mathrm{TlC}, Hf2InC\mathrm{Hf}_{2}\mathrm{InC}, Hf2SnC\mathrm{Hf}_{2}\mathrm{SnC}, and Ti2InC\mathrm{Ti}_{2}\mathrm{InC}, respectively.

Now, we focus our attention on the hardness parameters, HChenH_{\mathrm{Chen}} and HMiaoH_{\mathrm{Miao}}, as calculated using the following equations: HChen=2[(GB)2G]0.585−3H_{\mathrm{Chen}} = 2\left[\left(\frac{G}{B}\right)^2G\right]^{0.585} - 3 [79] and HMiao=(1−2ν)E6(1+ν)H_{\mathrm{Miao}} = \frac{(1-2\nu)E}{6(1+\nu)} [80]. The calculated values are presented in Table 2. Like the elastic moduli, the hardness parameters of 212 MAX phase borides are also higher than those of 211 MAX phase borides and/or carbides. Moreover, the increase of hardness parameters is also significantly larger for Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2PB2_2 while it is small for Nb2_2SB2_2. An increment of 20%(18%), 12%(18%), 16%(15%), 75%(71%), and 21%(26%) for HChenH_{\mathrm{Chen}} (HMiaoH_{\mathrm{Miao}}) is also reported in the cases of Zr2_2AB2_2 (A = In, Tl), Hf2_2AB2_2 (A = In, Sn) and Ti2_2InB2_2, respectively, compared to those of their corresponding 211 MAX phase carbides. Hence, it is evident that the hardness parameters are significantly enhanced for the 212 phases in comparison with the 211 phases. As discussed so far in this section, the mechanical properties of the 212 MAX phase borides are considerably enhanced compared to their counterpart 211 MAX phase borides and/or carbides. The values of C44C_{44} for all the studied phases also indicate a significant enhancement as it is most closely related to the hardness of solids [81]. Thus, a reasonable question is, what features bring about these enhancements in the 212 systems? The possible answer is explored in section 3.5.

The brittleness of Zr2PbB2\mathrm{Zr}_{2}\mathrm{Pb}\mathrm{B}_{2}

Although the MAX phases are metallic, most of them exhibit brittleness like ceramics. In this section, three widely known formalisms are used to predict brittleness/ductility. First of all, the Pugh ratio, (G/B)(G/B) [85] is used to confirm the brittle character of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] [since G/B<0.571G/B < 0.571 for ductile and G/B>0.571G/B > 0.571 for brittle solids]. The Poisson’s ratio (ν\nu) also confirmed the brittle character of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] as ν=0.26\nu= 0.26 is a critical value to identify the brittle and ductile materials, and ν\nu is lower than the critical value for brittle solids, and for ductile solids, the values are higher. In addition, the value of ν\nu also indicates the bonding nature within the solids. For example, it is typically low (0.10) for covalent solids and high (0.33) for metallic solids. For the present case, it (ν\nu) is within the range of 0.19 to 0.23, thus, expecting a mixture of covalent and metallic bonding within the Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] compounds like in other MAX phases. In fact, it agrees well with the existence of the M-X (covalent) bonding and M-A (ionic) bonding within the MAX phase materials. Moreover, Pettifor [86] addressed the Cauchy pressure (CPCP) to determine the chemical bonding and ductile/brittle nature of solids. A negative value of CPCP certifies the covalently bonded brittle solids whereas the positive value indicates the metallic solids. As is evident, Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] belong to the covalently bonded brittle class of solids.

Elastic anisotropy

Complete information regarding the mechanical stability of solids in extreme conditions can be gained from the study of elastic anisotropy. Anisotropy is also related to some other critical processes such as the creation and propagation of microcracks under mechanical stress and anisotropic plastic deformation, etc. Let us look back at the crystal structure again [Fig. 1], the atomic arrangements along the a(b)a(b)- and cc-direction are completely different, consequently, the bond strengths along these directions are also different [for example C11≠C33C_{11} \ne C_{33}]. These lead to elastic anisotropy in the layered hexagonal system [87]. The knowledge of anisotropy also provides a guideline for the enhancement of the mechanical stability of solids under extreme conditions by supplying direction-dependent elastic constants. Thus, the study of the anisotropic nature of elastic properties is compulsory and we have studied the elastic anisotropy of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] by calculating some anisotropy indices using different formalisms. The different anisotropic factors for Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] are computed from elastic constants CijC_{ij} using the following relations [88] and presented in Table 3:

PhasesA1A_1A2A_2A3A_3kc/kak_c/k_aAUA^{\mathrm{U}}
Ti2_2PB2_20.671.320.890.820.14
Ti2_2PB0.641.681.070.630.33
Ti2_2PC0.582.161.270.580.67
Zr2_2PbB2_21.220.630.771.210.45
Zr2_2PbB1.200.800.961.250.06
Zr2_2PbC0.951.040.991.030.34
Nb2_2PB2_20.721.320.950.790.11
Nb2_2PB0.571.640.940.690.34
Nb2_2PC0.551.580.870.700.34
Nb2_2SB2_20.761.270.960.600.11
Nb2_2SB0.621.260.780.790.15
Nb2_2SC0.631.190.750.700.16

Table 3. Table 3: Anisotropy indices, A1A_1, A2A_2, A3A_3, kc/kak_c/k_a, and universal anisotropy index AUA^{\mathrm{U}} of Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] MAX phases along with their counterpart borides and carbides.

A1=16(C11+C12+2C33−4C13)C44A_1 = \frac{\frac{1}{6}(C_{11}+C_{12}+2C_{33}-4C_{13})}{C_{44}}
A2=2C44C11−C12A_2 = \frac{2C_{44}}{C_{11}-C_{12}}
A3=13(C11+C12+2C33−4C13)C11−C12A_3 = \frac{\frac{1}{3}(C_{11}+C_{12}+2C_{33}-4C_{13})}{C_{11}-C_{12}}

The compounds Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] are anisotropic having the non unit (one) values of AiA_is because Ai=1A_i = 1 implies the isotropic nature. The linear compressibility (kk) along the aa and cc-axis are calculated by the equation [89]:

kcka=f=(C11+C12−2C13)/(C33−C13)\frac{k_c}{k_a}=f=(C_{11}+C_{12}-2C_{13})/(C_{33}-C_{13})

The computed values of ff are greater than 1 (f=1f = 1 for isotropic materials) for all the phases considered herein which certify the anisotropic nature of the titled compounds.

The universal anisotropy index AUA^{\mathrm{U}} for Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] is estimated by the following equation [90]:

AU=5GVGR+BVBR−6≥0A^{\mathrm{U}}=5\frac{G_{\mathrm{V}}}{G_{\mathrm{R}}}+\frac{B_{\mathrm{V}}}{B_{\mathrm{R}}}-6\geq0

where BB and GG are bulk and shear modulus; V and R indicate the Voigt and Reuss values. Like other anisotropy indices, AUA^{\mathrm{U}} for Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] is smaller than one (1) that implies the anisotropic nature of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S]. Since the polycrystalline elastic moduli are calculated from the elastic constants CijC_{ij}, thus, it is obvious that the anisotropic behavior will be exhibited by the moduli as well. Similar results have also been reported for some other 211, 212, 314 MAX phases previously [49, 53, 54, 70, 91, 92].

Electronic band structure (EBS) and density of states (DOS)

Figure 3 illustrate the EBS of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] borides in which the electronic paths are shown in the first Brillouin zone. The obtained EBS is similar to the metallic solids due to the overlapping of the valence and conduction bands. These are the characteristics of MAX phase materials that exhibit a good combination of metallic and ceramics properties [43, 53, 93, 94].

Electronic band structures of Ti2PB2, Zr2PbB2, and Nb2AB2 borides

Figure 3.

Figure 3. The electronic band structures of (a) Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, (b) Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, (c) Nb2PB2\mathrm{Nb}_{2}\mathrm{PB}_{2}, and (d) Nb2SB2\mathrm{Nb}_{2}\mathrm{SB}_{2} compounds.

The anisotropic characteristics of the MAX phases are expected due to their layered structure. The EBS also exhibits anisotropy along the basal plane and cc-direction of the crystal. The paths Γ\Gamma-A, H-K, and M-L correspond to the cc-direction while the paths A-H, K-Γ\Gamma, Γ\Gamma-M, and L-H are for the basal plane [95]. It is seen that the energy dispersions along the basal plane and the cc-direction differ significantly, confirming the anisotropic behavior of charge effective masses for these directions, as has been found for other MAX phase nanolaminates [43, 49, 53].

Figure 4 (a) displays the partial and total DOS of Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2} as a representative. These profiles roughly exhibit the usual characteristics of MAX phase materials. The Fermi level is dominantly contributed by the Zr-dd electronic states in association with a very small contribution from the B-pp and Pb-pp electronic states. The most strong orbital hybridization is observed between B-pp states and Zr-dd states that contribute to the formation of strong covalent bonding between them, similar to other MAX phases [12, 70, 96], specially matched with those of Zr2AB2\mathrm{Zr}_{2}\mathrm{AB}_{2} (A = In, Tl) [49]. It is worth stating that the Fermi level of Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2} resides close to the pseudogap in the TDOS profile. This is an indication of a high level of electronic stability. Similar results are also found for other considered compounds [not shown here]. Figure 4 (b) shows the total DOS of the titled phases for a comparative understanding of their nature.

Total and partial DOS of Zr2PbB2 and total DOS of Ti2PB2, Zr2PbB2, and Nb2AB2

Figure 4. The total and partial DOS of (a) Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2} and (b) total DOS of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] compounds.

Thermal Properties

Recently, the high-temperature applications of MAX phases have attracted much attention from both research and application points of view. Some of the thermal parameters of particular interest can be used to assess the suitability of materials for high-temperature applications. In this section, the Debye temperature (ΘD\Theta_{\mathrm{D}}), minimum thermal conductivity (kmin⁡k_{\min}), thermal expansion coefficient, Grüneisen parameter, and melting temperature of Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] compounds have been calculated to assess their potential for thermal applications.

The elastic properties can be correlated with the thermal properties, for example, phonon dynamics, thermal expansion, thermal conductivity, specific heat, and lattice enthalpy are connected to the Debye temperature. The Debye temperature itself depends on the elastic parameters which determine the sound velocity in a material. The details of the calculations can be found elsewhere [49]. The obtained values of ΘD\Theta_{\mathrm{D}} for Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] are 861 K, 434 K, 745 K, and 643 K, much higher than that of the corresponding 211 borides and/or carbides [Table 4]. The ΘD\Theta_{\mathrm{D}} values of Ti2_2PB2_2 and Nb2_2AB2_2 [A = P, S] are also higher than those of prior known 212 phases while ΘD\Theta_{\mathrm{D}} of Zr2_2PbB2_2 is lower than that of Zr2_2InB2_2, Hf2_2SnB2_2, and Ti2_2InB2_2 but greater than those of Zr2_2TlB2_2 and Hf2_2InB2_2. In reality, the obtained values of ΘD\Theta_{\mathrm{D}} for 212 MAX phases are significantly larger compared to those of their B and/or C-containing counterparts belonging to the 211 MAX phases, indicating their higher temperature limits for use because the ΘD\Theta_{\mathrm{D}} limits the normal modes of thermal vibrations within the solids. We can quantify the degree of the increment of Debye temperature as 22.3(22.6)%, 26.3(18.6)%, 17.3(18.8)%, and 8.2(13.8)% for Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S], respectively, compared to their 211 borides (carbides). The ranking of the so far known 212 MAX phases based on the values of ΘD\Theta_{\mathrm{D}} should be as follows: Ti2_2PB2_2 > Nb2_2PB2_2 > Nb2_2SB2_2 > Ti2_2InB2_2 > Zr2_2InB2_2 > Hf2_2SnB2_2 > Zr2_2PbB2_2 > Zr2_2TlB2_2 > Hf2_2InB2_2.

For the assessment of the high-temperature applications, minimum thermal conductivity (kmin⁡k_{\min}) is one of the important parameters. The thermal conductivity attains a constant value (minimum) at high temperatures known as the minimum thermal conductivity [97]. The lower the value of kmin⁡k_{\min}, the more suitable the solid for use in thermal barrier coating applications as it conducts less amount of heat which is one of the main criteria for selecting TBC materials. The kmin⁡k_{\min} is closely associated with the acoustic wave velocity in the materials and can be calculated by the following model due to Clark [97]: Kmin⁡=kBvm(MnρNA)−23K_{\min}=k_{\mathrm{B}}v_{\mathrm{m}}\left(\frac{M}{n\rho N_{\mathrm{A}}}\right)^{-\frac{2}{3}}. The values of kmin⁡k_{\min} are significantly lower for Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] phases compared to those of the corresponding boride and carbide counterparts as seen in Table 4. As also seen in Table 4 that the Kmin⁡K_{\min} of Zr2_2PbB2_2 is the lowest and equal to those of Zr2_2InB2_2 and Hf2_2InB2_2, certifying a very low capability of heat conduction at high temperatures. Actually, the Kmin⁡K_{\min} of 212 phases is lower compared to their 211 counterpart borides and/or carbides, revealing more appropriateness of the 212 phases for the use as TBC materials. However, we can rank [starting from low value] the 212 phases based on the values of Kmin⁡K_{\min} as follows: Zr2_2PbB2_2 = Zr2_2InB2_2 = Hf2_2InB2_2 < Hf2_2SnB2_2 < Zr2_2InB2_2 < Ti2_2InB2_2 < Nb2_2SB2_2 < Nb2_2PB2_2 < Ti2_2PB2_2.

Phaseρ\rho (g/cm3^{3})vlv_l (m/s)vtv_t (m/s)vmv_m (m/s)ΘD\Theta_{\mathrm{D}} (K)Kmin⁡K_{\min} (W/mK)γ\gammaTmT_{\mathrm{m}} (K)Reference
Ti2_2PB2_24.459480583964428611.711.262033This study
Ti2_2PB4.258460508356237042.431.351617This study
Ti2_2PC4.618513494754897022.121.471731This study
Zr2_2PbB2_28.705514330436554340.771.361613This study
Zr2_2PbB8.254748282831313420.881.381338This study
Zr2PbC\mathrm{Zr}_{2}\mathrm{PbC}9.044933293732523660.971.411223This study
Nb2PB2\mathrm{Nb}_{2}\mathrm{PB}_{2}6.748435515356967451.451.292382This study
Nb2PB\mathrm{Nb}_{2}\mathrm{PB}6.72772645951516351.801.341997This study
Nb2PC\mathrm{Nb}_{2}\mathrm{PC}6.987727454150336271.851.442058This study
Nb2SB2\mathrm{Nb}_{2}\mathrm{SB}_{2}6.727449444640216431.391.371965This study
Nb2SB\mathrm{Nb}_{2}\mathrm{SB}6.707294436648315941.141.361824Ref [43]
Nb2SC\mathrm{Nb}_{2}\mathrm{SC}6.317308407945425651.091.401790Ref [43]
Zr2InB2\mathrm{Zr}_{2}\mathrm{InB}_{2}6.876358390743125160.921.281693Ref [49]
Zr2InC\mathrm{Zr}_{2}\mathrm{InC}7.326004361639994591.241.361584Ref [82]
Zr2TlB2\mathrm{Zr}_{2}\mathrm{TlB}_{2}8.715466328436334330.771.361660Ref [49]
Zr2TlC\mathrm{Zr}_{2}\mathrm{TlC}8.924989299333113720.891.361430Ref [83]
Hf2InB2\mathrm{Hf}_{2}\mathrm{InB}_{2}10.865309324035784310.771.291800Ref [53]
Hf2InC\mathrm{Hf}_{2}\mathrm{InC}11.675004299933193831.041.321691Ref [82]
Hf2SnB2\mathrm{Hf}_{2}\mathrm{SnB}_{2}11.085459334436924470.801.281872Ref [53]
Hf2SnC\mathrm{Hf}_{2}\mathrm{SnC}12.065121305033763931.071.491746Ref [101]
Ti2InB2\mathrm{Ti}_{2}\mathrm{InB}_{2}05.907241454550046331.191.191858Ref [53]
Ti2InB2\mathrm{Ti}_{2}\mathrm{InB}_{2}05.917168448749426211.231.201833Ref [52]
Ti2InC\mathrm{Ti}_{2}\mathrm{InC}06.086531405544715341.001.231569Ref [52]
Table 4.

Table 6.

Owing to the close connection of the Grü­neisen parameter (γ\gamma) with the specific heat at constant volume, bulk modulus, and TEC, the calculation of γ\gamma is of scientific interest. It is used to reveal the degree of anharmonic effects present in solids. Thus, γ\gamma has been determined via the relation with the Poisson’s ratio [98]: γ=32(1+ν)(2−3ν)\gamma=\frac{3}{2}\frac{(1+\nu)}{(2-3\nu)}. As seen, the anharmonic effect is low for Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S]. The values remain within the predicted limit [0.85 to 3.53] for polycrystalline solids associated with the limiting value of the Poisson’s ratio [0.05–0.46] [99].

One of the mandatory information for the selection of materials for applications at high-temperature technology is the melting point (TmT_{\mathrm{m}}) which provides an idea of the temperature limit for usage. Owing to the combined ceramic properties of MAX phases with metallic properties, they have been recognized as suitable systems for high-temperature applications since the early days. Hence, the calculation of TmT_{\mathrm{m}} for the MAX phase is important and has been estimated in this study using the equation relating elastic constants as follows [100]: Tm=(3C11+1.5C33+354) KT_{\mathrm{m}}=(3C_{11}+1.5C_{33}+354)\ \mathrm{K}.

Table 4: Debye temperature, ΘD\Theta_{\mathrm{D}}, minimum thermal conductivity, Kmin⁡K_{\min}, Grü­neisen parameter, γ\gamma, and melting temperature, TmT_{\mathrm{m}} of M2_2AB2_2 (M = Ti, Zr, Hf, Nb; A = P, S, In, Sn, Tl, Pb) compounds together with those of M2_2AC (M = Ti, Zr, Hf, Nb; A = P, S, In, Sn, Tl, Pb) compounds.

Like the other 212 MAX phases, the TmT_{\mathrm{m}} of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] values are also larger than their 211 corresponding counterpart borides and/or carbides. On the other hand, TmT_{\mathrm{m}} is the lowest [1613 K] for Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2} in comparison with other 212 MAX phase borides while it is maximum for Nb2PB2\mathrm{Nb}_{2}\mathrm{PB}_{2} [2382 K] (Table 4). In addition, the used formula to calculate the TmT_{\mathrm{m}} contains C11C_{11} and C33C_{33}, which are the measures of the stiffness along the aa- and cc-axis. Thus, a direct relationship between the TmT_{\mathrm{m}} and Young’s modulus [a measure of the stiffness of a polycrystalline solid] is expected which is seen in Table 2 and Table 4. The maximum value of YY is obtained for Nb2PB2\mathrm{Nb}_{2}\mathrm{PB}_{2}, following the ranking as follows: Nb2PB2>Ti2PB2>Nb2SB2>Hf2SnB2>Ti2InB2>Hf2InB2>Zr2InB2>Zr2TlB2>Zr2PbB2\mathrm{Nb}_{2}\mathrm{PB}_{2} > \mathrm{Ti}_{2}\mathrm{PB}_{2} > \mathrm{Nb}_{2}\mathrm{SB}_{2} > \mathrm{Hf}_{2}\mathrm{SnB}_{2} > \mathrm{Ti}_{2}\mathrm{InB}_{2} > \mathrm{Hf}_{2}\mathrm{InB}_{2} > \mathrm{Zr}_{2}\mathrm{InB}_{2} > \mathrm{Zr}_{2}\mathrm{TlB}_{2} > \mathrm{Zr}_{2}\mathrm{PbB}_{2}. This ranking also applies to the melting temperature TmT_{\mathrm{m}} as seen in Table 4. It has been suggested previously that TmT_{\mathrm{m}} will be higher for the solids with higher Young’s modulus and vice versa [102]. Knowledge regarding the decomposition temperature (TdT_{\mathrm{d}}) is also a prerequisite regardless of the value of TmT_{\mathrm{m}}. The MAX phases have a tendency to decompose at a lower temperature than that of TmT_{\mathrm{m}}. Unfortunately, no information regarding TdT_{\mathrm{d}} of the titled borides as well as other 212 phases is present at this moment. An earlier report provided by Cue et al. [103] might be helpful regarding this issue. They have estimated TdT_{\mathrm{d}} and TmT_{\mathrm{m}} of some MAX phases and shown that TdT_{\mathrm{d}} is lower than TmT_{\mathrm{m}}, for some cases TdT_{\mathrm{d}} is close to TmT_{\mathrm{m}} [54], thus, one may expect the same for Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] phases as well.

Why are the thermo-mechanical properties for 212 phases enhanced?

From the analysis of the results obtained so far, it is obvious that the thermo-mechanical properties are significantly upgraded when we go from the 211 MAX phase carbides to the 212 MAX phase borides. Why the properties are get enhanced for the 212 phases? The answer lies in the structure. Though both the 212 and 211 phases belong to the MAX family, their structures are not the same. The 212 phases are crystallized in the space group P-6m2, (No. 187) [8, 45], while the 211 phases are crystallized in the space group P63_3/mmc (No.194) [5, 104] as shown in Figure 1 (a and b). The bonding natures within these two structures are also different. For the 212 phases, there is a very strong covalent bonding among the B atoms by forming a 2D layer and contributing to the 2c-2e type of bonding as shown in Figure 5 (a and b). In addition, there is also strong covalent bonding between M (Zr atoms for Zr2_2PbB2_2) and X (B atoms for Zr2_2PbB2_2) similar to the 211 phases (Zr and B/C are M and X atoms for Zr2_2PbB/Zr2_2PbC). In addition, there is comparatively weak M – A bonding (Pb is the A atom in the case of Zr2_2PbB/Zr2_2PbC). There is no covalent bond among the C atoms in the 211 phase, although strong covalent bonds between M- X atoms are formed as well as the M-A bonds. Owing to the existence of the very strong B-B covalent bonding within the 2D layer of B atoms, the structure becomes more stable, and the overall cohesive energy is enhanced significantly for the 212 phases in comparison with the 211 phases. It is noted that, for 211 MAX phase borides, B-B bonding does not exist [6, 7, 37, 39, 43, 105]. Our statements will be further clarified by the calculation of the Mulliken population analysis given in Table 5. As seen in Table 5, the charge is transferred from Zr to B (0.54/0.55) and Pb (0.01). The charge transfer mechanism confirms the existence of ionic character as observed for the B/C-containing MAX phase Zr2_2PbB/Zr2_2PbC. In this boride/carbide, the charge is transferred from Zr to B (0.77) and Pb (0.00) [Table 5]. Table 5 also shows the bond overlap population (BOP) analysis for both the compounds Zr2_2PbB2_2 and Zr2_2PbB. The value of BOP indicates the nature of bonding/anti-bonding states within the solids depending on the positive/negative values. A negative value of BOP stands for anti-bonding whereas a positive value for bonding states. It is clear from Table 5 that no anti-bonding exists within the considered MAX phases. In addition, the value of BOP is also an indicator of bonding strength, the higher the BOP, the stronger the bonding. As evident from Table 5, the B-B bonding exhibits a much higher BOP value, confirming the very strong covalent bonding formed in the 2c-2e channel. The M (Zr) - X (B) bonding in the Zr2_2PbB is stronger than that of Zr2_2PbB2_2 with the BOP values of 1.25 and 0.24/0.20, respectively. Due to the existence of very strong B-B bonding, the overall bonding strength, as well as mechanical parameters and hardness values, are higher for Zr2PbB2\mathrm{Zr_2PbB_2} compared to Zr2PbB\mathrm{Zr_2PbB}. The results for the other titled compounds are also presented in Table 5. Similar results are also reported for other known 212 phases [49, 51, 53].

Figure 5. Formation of B-B covalent bonding within Zr2PbB2\mathrm{Zr_2PbB_2}.

CompoundAtomsssppddTotalCharge (e)BondBond number nμn^{\mu}Bond length dμd^{\mu} (Å)Bond population PμP^{\mu}
Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}B0.952.620.003.56-0.56B-B11.802422.47
B0.952.610.003.57-0.57Ti-B22.397810.12
Ti2.106.512.7911.390.61Ti-B22.397810.05
P1.583.502.795.080.08Ti-P22.471811.00
Ti2PB\mathrm{Ti}_{2}\mathrm{PB}B1.212.420.003.64-0.64Ti-B42.270171.10
Ti2.216.672.7311.620.38Ti-P42.498430.96
P1.613.520.005.13-0.13
Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}B0.982.580.003.55-0.55B-B11.892982.12
B0.972.570.003.54-0.54Zr-B22.517530.24
Zr2.156.462.8411.450.55Zr-B22.517530.20
Pb1.422.5510.0414.01-0.01
Zr2PbB\mathrm{Zr}_{2}\mathrm{PbB}B1.182.590.003.77-0.77Zr-B42.386331.25
Zr2.286.612.7211.620.38
Pb1.412.5510.0314.000.00
Nb2PB2\mathrm{Nb}_{2}\mathrm{PB}_{2}B0.922.570.003.49-0.49B-B11.843462.22
B0.952.560.003.51-0.51Nb-B22.433780.19
Nb2.156.284.0715.510.49Nb-B22.433780.14
P1.553.430.004.990.01Nb-P22.532791.00
Nb2PB\mathrm{Nb}_{2}\mathrm{PB}B1.142.460.003.60-0.60Nb-B42.290511.15
Nb2.256.414.0212.680.32Nb-P42.561301.06
P1.593.460.005.04-0.04
Nb2SB2\mathrm{Nb}_{2}\mathrm{SB}_{2}B0.922.560.003.47-0.47B-B11.848972.07
B0.932.580.003.51-0.51Nb-B22.403370.20
Nb2.146.274.0412.450.55Nb-B22.403370.19
S1.764.370.006.12-0.12Nb-S22.574880.74
Nb2SB\mathrm{Nb}_{2}\mathrm{SB}B1.112.510.003.62-0.62Nb-B42.265431.12
S1.774.400.006.17-0.17Nb-S42.598170.79
Nb2.246.373.9912.610.39

Table 5. Mulliken atomic and bond overlap populations of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] and Ti2PB\mathrm{Ti}_{2}\mathrm{PB}, Zr2PbB\mathrm{Zr}_{2}\mathrm{PbB}, and Nb2AB\mathrm{Nb}_{2}\mathrm{AB} [A = P, S] MAX compounds.

Now, let us discuss the variation of the mechanical properties [Table 2] among the titled borides in terms of the BOP values as presented in Table 5. We can rank the titled borides based on the values of hardness parameters [Table 2] (HchenH_{\mathrm{chen}}, HmiaoH_{\mathrm{miao}}, and C44C_{44}) as follows: Nb2PB2>Ti2PB2>Nb2SB2>Zr2PbB2\mathrm{Nb_2PB_2} > \mathrm{Ti_2PB_2} > \mathrm{Nb_2SB_2} > \mathrm{Zr_2PbB_2}. The BOP of B-B bonds is 2.22, 2.47, 2.07, and 2.12 for Nb2PB2\mathrm{Nb_2PB_2}, Ti2PB2\mathrm{Ti_2PB_2}, Nb2SB2\mathrm{Nb_2SB_2}, and Zr2PbB2\mathrm{Zr_2PbB_2}, respectively. According to these values, the ranking of borides can be re-ordered. But, for Nb2PB2\mathrm{Nb_2PB_2}, the BOPs of Nb-B are (0.14 and 0.19) higher compared to those of Ti-B (0.05 and 0.12), and the BOP of Nb-P and Ti-P is the same for both compounds. Thus, considering the cumulative contribution from all bonds (BOP), the overall bonding strength is expected to be higher for Nb2PB2\mathrm{Nb_2PB_2} compared to that for Ti2PB2\mathrm{Ti_2PB_2} which is reflected in values of the elastic constants, elastic moduli, and hardness parameters. Again for Nb2SB2\mathrm{Nb_2SB_2} and Zr2PbB2\mathrm{Zr_2PbB_2}, the BOP of the B-B bond is 2.07 and 2.12, respectively. The BOP of Nb-B (0.20 and 0.19) and Zr-B (0.24 and 0.20) are also comparable. But, there is no BOP for Zr-Pb bonding within the considered threshold length (5 Å) whereas the BOP for Nb-S is 0.74. This makes the difference in the overall bonding strength as reflected from values of elastic constants, elastic moduli, and hardness parameters. It is also noted that no BOP of Zr-Pb is found for 211 the Zr2PbB\mathrm{Zr}_{2}\mathrm{PbB} compound [Table 5].

Optical properties

The technologically important optical constants of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] MAX phase compounds are estimated and shown in Figure 6 in the energy range up to 25 eV. The low energy part of the imaginary part of the dielectric function is corrected by introducing a plasma frequency of 3 eV and damping of 0.5 eV owing to the metallic nature of the titled compounds. Besides, we have used a Gaussian smearing 0.5 eV.

Eight-panel plots of dielectric and optical properties

Figure 6. (a) real part, ε1\varepsilon_1, and (b) imaginary part of dielectric function, ε2\varepsilon_2, (c) refractive index, nn, (d) extinction coefficient, kk, (e) absorption coefficient, α\alpha, (f) photoconductivity, σ\sigma, (g) reflectivity, RR and (h) lossfunction, LL as a function of electromagnetic radiation energy.

The real part of the dielectric function, ε1\varepsilon_{1} is shown in Figure 6 (a) exhibiting metallic behavior. Usually, the ε1\varepsilon_{1} exhibit a large negative value in very low energy region for metallic systems. Thus, ε1\varepsilon_{1} spectra of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] agree well with the non-existence of the energy band gap in the electronic band structure. The imaginary part of dielectric function ε2\varepsilon_{2} is depicted in Figure 6 (b) wherein two small peaks are observed for both polarization directions of the electric field vector. The peaks in the ε2\varepsilon_{2} certify that Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] compounds are metal, and the EFE_{\mathrm{F}} [Figure 3] is located at the Ti-3dd states that results in the free electron behavior, consequently, the photon-induced transition between electronic states is possible within the conduction band.

The refractive index (nn) and extinction coefficient (kk) are depicted in Figure 6 (c) and (d), respectively. The n(0)n(0) is found to be 6.4, 7.8, 7.1 and 18.6 for Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S], respectively. The kk for Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] rise progressively in the IR region to its highest values and then decline slowly in the visible and UV regions [Figure 6(d)]. The decline of kk follows the decline of ε2\varepsilon_{2}, as seen in Figure 6 (b) and Figure 6 (d).

The absorption coefficient (α\alpha) of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] is presented in Figure 6 (e). As seen in the figure, it rises almost steadily to attain its maximum value in the UV region. Moreover, α\alpha starts rising from the zero photon energy, indicating once again the metallic nature of the compounds under investigation. In addition, it is found that Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] can be used as good absorbing materials in the visible and UV regions owing to the high values of their absorption coefficients. Figure 6 (f) displays the photoconductivity (σ\sigma) of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] as a function of photon energy. The σ\sigma measures the change in the electrical conductivity of the material when it is subjected to photon irradiation. Like α\alpha, the σ\sigma spectrum also certifies that Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] are metallic compounds.

One of the most important applications of MAX phase materials is as coating materials to reduce solar heating. The potential for this application can be predicted by the study of reflectivity. The reflectivity R(ω)R(\omega) of Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] is presented Figure 6 (g). According to Li et al. [106, 107] the MAX phase materials which have reflectivity greater than 44% are suitable for use as coating materials. As evident from Figure 6 (g), the R(ω)R(\omega) remains always greater than 44% up to ~12 eV for all the considered phases. Though the reflectivity at low energy is highest for Nb2_2SB2_2, the overall performance of Zr2_2PbB2_2 is the best for use as a cover to protect from solar heating. Noted here that the reflectivity spectrum with ~ 53% in the IR, visible, and near UV region (0-5 eV) was almost constant for Zr2_2PbB2_2. Figure 6 (h) shows the energy loss function [L(ω)L(\omega)] spectra of Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] compounds, in which the peaks correspond to plasma frequencies (ωp\omega_{\mathrm{p}}). At this particular frequency the R(ω)R(\omega) exhibits falling a tail, the absorption coefficient falls rapidly and ε1\varepsilon_1 crosses zero from the negative side. It is the characteristic frequency above which the materials behave as transparent to the incident electromagnetic wave.

Conclusions

The thermo-mechanical and optical properties of Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S] are explored via DFT calculations with the intention to shed light on the enhanced thermo-mechanical properties of recently added 212 MAX phase borides in comparison with their 211 boride and carbide counterparts. The titled MAX phases are chemically, dynamically, and mechanically stable. The values of elastic constants and moduli of 212 phases are higher than those of the 211 phase borides and/or carbides. The hardness parameters are also higher for the same. The usual brittleness of the MAX phase is also exhibited by the titled borides. Due to the different atomic arrangements along the aa- and cc-direction, the elastic properties are anisotropic. The metallic character of the studied phases is confirmed by the EBS and DOS. Like the mechanical properties, the thermal parameters are also enhanced significantly for 212 phases compared to their 211 counterparts. For ΘD\Theta_{\mathrm{D}}, the values are increased by 22.3(22.6)%, 26.3(18.6)%, 17.3(18.8)%, and 8.2(13.8)% for Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S], respectively, compared to the corresponding 211 borides (carbides). The melting temperature is also noted to be increased by 26(17)%, 20(32)%, 19(16)%, and 08(10)%. The study of thermo-mechanical properties reveals the more appropriateness of the 212 phase borides compared to their 211 counterparts MAX phases for applications. The existence of very strong B-B bonding contributes to the enhancement of the thermo-mechanical properties of the 212 compounds. The important results concerning the optical constants are found in accord with the electronic band structure results. The dielectric constant, absorption coefficient, and photoconductivity spectra reconfirm the metallic nature of the titled MAX phases. The reflectivity spectra show the suitability of Ti2PB2\mathrm{Ti}_{2}\mathrm{PB}_{2}, Zr2PbB2\mathrm{Zr}_{2}\mathrm{PbB}_{2}, and Nb2AB2\mathrm{Nb}_{2}\mathrm{AB}_{2} [A = P, S] phases for use as shielding materials to protect from solar radiation.

To conclude, we hope, the results presented in this paper will stimulate further research on the 212 MAX phases which exhibit superior characteristics for applications in the thermo-mechanical sectors compared to many other conventional MAX phase nanolaminates.

Conflicts of interest

There are no conflicts of interest to declare.

Acknowledgment

The authors are grateful to the Department of Physics, Chittagong University of Engineering & Technology (CUET), Chattogram-4349, Bangladesh, for providing the computing facility for this work. A part of this work has been done at the ACMRL, Department of Physics, CUET, Bangladesh, where the facility is supported by the research grant from The World Academy of Sciences [No. 21-378 RG/PHYS/AS_G -FR3240319526].

The rise of 212 MAX phase borides, Ti2_2PB2_2, Zr2_2PbB2_2, and Nb2_2AB2_2 [A = P, S]: DFT insights into the physical properties for thermo-mechanical applications

M. A. Ali; M. M. Hossain; M. M. Uddin; A. K. M. A. Islam; S. H. Naqib

Phasea (Å)c (Å)c/aReference
Ti2_2PB3.267411.6044This study
Zr2_2PdB3.502115.1729This study
Nb2_2PB3.340311.6853This study
Nb2_2SB3.538311.6043[1]

Table S1. The lattice constants (aa and cc) and c/ac/a ratio of 211 MAX phase borides.

Electronic band structures of Ti₂PB, Zr₂PbB, Nb₂PB, and Nb₂SB MAX phase compounds

Figure S2. The electronic band structures of (a) Ti2_2PB, (b) Zr2_2PbB, (c) Nb2_2PB, and (d) Nb2_2SB MAX phase compounds.

Total DOS of Ti₂PB, Zr₂PbB, Nb₂PB, and Nb₂SB MAX phase compounds

Figure S3. The total DOS of Ti₂PB, Zr₂PbB, and Nb₂AB [A = P, S] MAX phase compounds.

References

  1. [1]M. Sokol, V. Natu, S. Kota, M.W. Barsoum, On the Chemical Diversity of the MAX Phases, Trends Chem. 1 (2019) 210–223. https://doi.org/10.1016/j.trechm.2019.02.016.
  2. [2]M.W. Barsoum, Physical Properties of the MAX Phases, in: Encycl. Mater. Sci. Technol., Elsevier, 2006: pp. 1–11. https://doi.org/10.1016/B0-08-043152-6/02058-1.
  3. [3]M.W. Barsoum, D. Brodkin, T. El-Raghy, Layered machinable ceramics for high temperature applications, Scr. Mater. 36 (1997) 535–541. https://doi.org/10.1016/S1359-6462 (96) 00418-6.
  4. [4]M.W. Barsoum, The MN+1AXN phases: A new class of solids, Prog. Solid State Chem. 28 (2000) 201–281. https://doi.org/10.1016/S0079-6786(00)00006-6.
  5. [5]M.W. Barsoum, MAX phases: Properties of machinable ternary carbides and nitrides, Wiley-VCH Verlag GmbH & Co. KGaA, Weinheim, Germany, 2013. https://doi.org/10.1002/9783527654581.
  6. [6]M. Khazaei, M. Arai, T. Sasaki, M. Estili, Y. Sakka, Trends in electronic structures and structural properties of MAX phases: a first-principles study on M₂AlC (M = Sc, Ti, Cr, Zr, Nb, Mo, Hf, or Ta), M₂AlN, and hypothetical M₂AlB phases, J. Phys. Condens. Matter. 26 (2014) 505503. https://doi.org/10.1088/0953-8984/26/50/505503.
  7. [7]T. Rackl, L. Eisenburger, R. Niklaus, D. Johrendt, Syntheses and physical properties of the MAX phase boride Nb₂SB and the solid solutions Nb₂SBₓC₁₋ₓ (x=0-1), Phys. Rev. Mater. 3 (2019) 054001. https://doi.org/10.1103/PhysRevMaterials.3.054001.
  8. [8]N. Miao, J. Wang, Y. Gong, J. Wu, H. Niu, S. Wang, K. Li, A.R. Oganov, T. Tada, H. Hosono, Computational Prediction of Boron-Based MAX Phases and MXene Derivatives, Chem. Mater. 32 (2020) 6947–6957. https://doi.org/10.1021/acs.chemmater.0c02139.
  9. [9]M. Naguib, V.N. Mochalin, M.W. Barsoum, Y. Gogotsi, 25th Anniversary Article: MXenes: A New Family of Two-Dimensional Materials, Adv. Mater. 26 (2014) 992–1005. https://doi.org/10.1002/adma.201304138.
  10. [10]W. Jeitschko, H. Nowotny, F. Benesovsky, Carbides of formula T₂MC, J. Less Common Met. 7 (1964) 133–138. https://doi.org/10.1016/0022-5088(64)90055-4.
  11. [11]M.A. Ali, Newly Synthesized Ta-Based MAX Phase (Ta₁₋ₓHfₓ)₄AlC₃ and (Ta₁₋ₓHfₓ)₄Al₀.₅Sn₀.₅C₃ (0 ≤ x ≤ 0.25) Solid Solutions: Unravelling the Mechanical, Electronic, and Thermodynamic Properties, Phys. Status Solidi. 258 (2021) 2000307. https://doi.org/10.1002/pssb.202000307.
  12. [12]M.R. Khatun, M.A. Ali, F. Parvin, A.K.M.A. Islam, Elastic, thermodynamic and optical behavior of V₂AC ( A = Al, Ga) MAX phases, Results Phys. 7 (2017) 3634–3639. https://doi.org/10.1016/j.rinp.2017.09.043.
  13. [13]A.S. Ingason, M. Dahlqvist, J. Rosen, Magnetic MAX phases from theory and experiments; A review, J. Phys. Condens. Matter. (2016). https://doi.org/10.1088/0953-8984/28/43/433003.
  14. [14]T. Lapauw, K. Lambrinou, T. Cabioč’h, J. Halim, J. Lu, A. Pesach, O. Rivin, O. Ozeri, E.N. Caspi, L. Hultman, P. Eklund, J. Rosén, M.W. Barsoum, J. Vleugels, Synthesis of the new MAX phase Zr₂AlC, J. Eur. Ceram. Soc. 36 (2016) 1847–1853. https://doi.org/10.1016/j.jeurceramsoc.2016.02.044.
  15. [15]T. Lapauw, J. Halim, J. Lu, T. Cabioč’h, L. Hultman, M.W. Barsoum, K. Lambrinou, J. Vleugels, Synthesis of the novel Zr₃AlC₂ MAX phase, J. Eur. Ceram. Soc. 36 (2016) 943–947. https://doi.org/10.1016/j.jeurceramsoc.2015.10.011.
  16. [16]M. Dahlqvist, J. Lu, R. Meshkian, Q. Tao, L. Hultman, J. Rosen, Prediction and synthesis of a family of atomic laminate phases with Kagomé-like and in-plane chemical ordering, Sci. Adv. 3 (2017) 1–10. https://doi.org/10.1126/sciadv.1700642.
  17. [17]H. Fashandi, C.C. Lai, M. Dahlqvist, J. Lu, J. Rosen, L. Hultman, G. Greczynski, M. Andersson, A. Lloyd Spetz, P. Eklund, TiAu₂C and Ti₃Au₂C₂ formed by solid state reaction of gold with Ti₂AlC and Ti₃AlC₂, Chem. Commun. 53 (2017) 9554–9557. https://doi.org/10.1039/c7cc04701k.
  18. [18]L. Mian, L. You-Bing, L. Kan, L. Jun, E. Per, P. Per, R. Johanna, H. Lars, D. Shi-Yu, H. Zheng-Ren, H. Qing, Synthesis of Novel MAX Phase Ti₃ZnC₂ via A-site-element-substitution Approach, J. Inorg. Mater. 34 (2019) 60. https://doi.org/10.15541/jim20180377.
  19. [19]T. Lapauw, B. Tunca, T. Cabioć’h, J. Lu, P.O.Å. Persson, K. Lambrinou, J. Vleugels, Synthesis of MAX Phases in the Hf–Al–C System, Inorg. Chem. 55 (2016) 10922–10927. https://doi.org/10.1021/acs.inorgchem.6b01398.
  20. [20]B. Anasori, M. Dahlqvist, J. Halim, E.J. Moon, J. Lu, B.C. Hosler, E.N. Caspi, S.J. May, L. Hultman, P. Eklund, J. Rosén, M.W. Barsoum, Experimental and theoretical characterization of ordered MAX phases Mo₂TiAlC₂ and Mo₂Ti₂AlC₃, J. Appl. Phys. 118 (2015) 094304. https://doi.org/10.1063/1.4929640.
  21. [21]S. Kuchida, T. Muranaka, K. Kawashima, K. Inoue, M. Yoshikawa, J. Akimitsu, Superconductivity in Lu₂SnC, Phys. C Supercond. 494 (2013) 77–79. https://doi.org/10.1016/j.physc.2013.04.050.
  22. [22]Q. Xu, Y. Zhou, H. Zhang, A. Jiang, Q. Tao, J. Lu, J. Rosén, Y. Niu, S. Grasso, C. Hu, Theoretical prediction, synthesis, and crystal structure determination of new MAX phase compound V₂SnC, J. Adv. Ceram. 9 (2020) 481–492. https://doi.org/10.1039/d0ra07730e.
  23. [23]M.S. Ali, M.A. Rayhan, M.A. Ali, R. Parvin, A.K.M.A. Islam, New MAX Phase Compound Mo₂TiAlC₂: First-principles Study, J. Sci. Res. 8 (2016) 109–117. https://doi.org/10.3329/jsr.v8i2.25057.
  24. [24]D. Horlait, S.C. Middleburgh, A. Chroneos, W.E. Lee, Synthesis and DFT investigation of new bismuth-containing MAX phases, Sci. Rep. 6 (2016) 1–9. https://doi.org/10.1038/srep18829.
  25. [25]E. Zapata-Solvas, M.A. Hadi, D. Horlait, D.C. Parfitt, A. Thibaud, A. Chroneos, W.E. Lee, Synthesis and physical properties of (Zr₁−ₓ,Tiₓ)₃AlC₂ MAX phases, J. Am. Ceram. Soc. 100 (2017) 3393–3401. https://doi.org/10.1111/jace.14870.
  26. [26]M. Naguib, G.W. Bentzel, J. Shah, J. Halim, E.N. Caspi, J. Lu, L. Hultman, M.W. Barsoum, New Solid Solution MAX Phases: (Ti₀.₅,V₀.₅)₃AlC₂ , (Nb₀.₅,V₀.₅)₂AlC, (Nb₀.₅,V₀.₅)₄AlC₃ and (Nb₀.₈,Zr₀.₂)₂AlC, Mater. Res. Lett. 2 (2014) 233–240. https://doi.org/10.1080/21663831.2014.932858.
  27. [27]P.A. Burr, D. Horlait, W.E. Lee, Experimental and DFT investigation of (Cr,Ti)₃AlC₂ MAX phases stability, Mater. Res. Lett. 5 (2017) 144–157. https://doi.org/10.1080/21663831.2016.1222598.
  28. [28]B. Tunca, T. Lapauw, O.M. Karakulina, M. Batuk, T. Cabioć’h, J. Hadermann, R. Delville, K. Lambrinou, J. Vleugels, Synthesis of MAX Phases in the Zr-Ti-Al-C System, Inorg. Chem. 56 (2017) 3489–3498. https://doi.org/10.1021/acs.inorgchem.6b03057.
  29. [29]T. Lapauw, B. Tunca, D. Potashnikov, A. Pesach, O. Ozeri, J. Vleugels, K. Lambrinou, The double solid solution (Zr,Nb)₂(Al, Sn)C MAX phase: a steric stability approach, Sci. Rep. 8 (2018) 12801. https://doi.org/10.1038/s41598-018-31271-2.
  30. [30]B. Tunca, T. Lapauw, R. Delville, D.R. Neuville, L. Hennet, D. Thiaudière, T. Ouisse, J. Hadermann, J. Vleugels, K. Lambrinou, Synthesis and Characterization of Double Solid Solution (Zr,Ti)₂(Al,Sn)C MAX Phase Ceramics, Inorg. Chem. 58 (2019) 6669–6683. https://doi.org/10.1021/acs.inorgchem.9b000065.
  31. [31]M. Griseri, B. Tunca, S. Huang, M. Dahlqvist, J. Rosén, J. Lu, P.O.Å. Persson, L. Popescu, J. Vleugels, K. Lambrinou, Journal of the European Ceramic Society Ta-based 413 and 211 MAX phase solid solutions with Hf and Nb, J. Eur. Ceram. Soc. 40 (2020) 1829–1838. https://doi.org/10.1016/j.jeurceramsoc.2019.12.052.
  32. [32]M.A. Ali, M.M. Hossain, M.A. Hossain, M.T. Nasir, M.M. Uddin, M.Z. Hasan, A.K.M.A. Islam, S.H. Naqib, Recently synthesized (Zr₁₋ₓTiₓ)₂AlC (0 ≤ x ≤ 1) solid solutions: Theoretical study of the effects of M mixing on physical properties, J. Alloys Compd. 743 (2018) 146–154. https://doi.org/10.1016/j.jallcom.2018.01.396.
  33. [33]R. Pan, J. Zhu, Y. Liu, Synthesis, microstructure and properties of (Ti₁₋ₓMoₓ)₂AlC phases, Mater. Sci. Technol. 34 (2018) 1064–1069. https://doi.org/10.1080/02670836.2017.1419614.
  34. [34]O.O. Kurakevych, Superhard phases of simple substances and binary compounds of the B-C-N-O system: from diamond to the latest results (a Review), J. Superhard Mater. 31 (2009) 139–157. https://doi.org/10.3103/S1063457609030010.
  35. [35]S.K. Mitro, M.A. Hadi, F. Parvin, R. Majumder, S.H. Naqib, A.K.M.A. Islama, Effect of boron incorporation into the carbon-site in Nb₂SC MAX phase: Insights from DFT, J. Mater. Res. Technol. 11 (2021) 1969–1981. https://doi.org/10.1016/j.jmrt.2021.02.031.
  36. [36]A. Gencer, G. Surucu, Electronic and lattice dynamical properties of Ti₂SiB MAX phase, Mater. Res. Express. 5 (2018) 076303. https://doi.org/10.1088/2053-1591/aace7f.
  37. [37]M.A. Hadi, M. Zahanġir Alam, I. Ahmed, A.M.M. Tanveer Karim, S.H. Naqib, A. Chroneos, A.K.M.A. Islam, A density functional theory approach to the effects of C and N substitution at the B-site of the first boride MAX phase Nb₂SB, Mater. Today Commun. 29 (2021) 102910. https://doi.org/10.1016/J.MTCOMM.2021.102910.
  38. [38]A. GENCER, First Principles Investigations of Ta₄AlX₃ (X= B, C, N) MAX Phase Ceramics, J. Boron. 5 (2020) 115–123. https://doi.org/10.30728/boron.731471.
  39. [39]M.S. Hossain, M.A. Ali, M.M. Hossain, M.M. Uddin, Physical properties of predicted MAX phase borides Hf₂AB (A = Pb, Bi): A DFT insight, Mater. Today Commun. 27 (2021) 102411. https://doi.org/10.1016/j.mtcomm.2021.102411.
  40. [40]T. Rackl, D. Johrendt, The MAX phase borides Zr₂SB and Hf₂SB, Solid State Sci. 106 (2020) 106316. https://doi.org/10.1016/j.solidstatesciences.2020.106316.
  41. [41]P. Chakraborty, A. Chakrabarty, A. Dutta, T. Saha-Dasgupta, Soft MAX phases with boron substitution: A computational prediction, Phys. Rev. Mater. 2 (2018) 103605. https://doi.org/10.1103/PhysRevMaterials.2.103605.
  42. [42]G. Surucu, Investigation of structural, electronic, anisotropic elastic, and lattice dynamical properties of MAX phases borides: An Ab-initio study on hypothetical M₂AB (M = Ti, Zr, Hf; A = Al, Ga, In) compounds, Mater. Chem. Phys. 203 (2018) 106–117. https://doi.org/10.1016/j.matchemphys.2017.09.050.
  43. [43]M.A. Ali, M.M. Hossain, M.M. Uddin, M.A. Hossain, A.K.M.A. Islam, S.H. Naqib, Physical properties of new MAX phase borides M₂SB (M = Zr, Hf and Nb) in comparison with conventional MAX phase carbides M₂SC (M = Zr, Hf and Nb): Comprehensive insights, J. Mater. Res. Technol. 11 (2021) 1000–1018. https://doi.org/10.1016/j.jmrt.2021.01.068.
  44. [44]G. Surucu, A. Gencer, X. Wang, O. Surucu, Lattice dynamical and thermo-elastic properties of M₂AlB (M = V, Nb, Ta) MAX phase borides, J. Alloys Compd. 819 (2020) 153256. https://doi.org/10.1016/j.jallcom.2019.153256.
  45. [45]J. Wang, T.N. Ye, Y. Gong, J. Wu, N. Miao, T. Tada, H. Hosono, Discovery of hexagonal ternary phase Ti₂InB₂ and its evolution to layered boride TiB, Nat. Commun. 10 (2019) 1–8. https://doi.org/10.1038/s41467-019-10297-8.
  46. [46]M. Ade, H. Hillebrecht, Ternary Borides Cr₂AlB₂, Cr₃AlB₄, and Cr₄AlB₆: The First Members of the Series (CrB₂)ₙCrAl with n = 1, 2, 3 and a Unifying Concept for Ternary Borides as MAB-Phases, Inorg. Chem. 54 (2015) 6122–6135. https://doi.org/10.1021/acs.inorgchem.5b00049.
  47. [47]S. Kota, M. Sokol, M.W. Barsoum, A progress report on the MAB phases: atomically laminated, ternary transition metal borides, Int. Mater. Rev. 65 (2020) 226–255. https://doi.org/10.1080/09506608.2019.1637090.
  48. [48]M.A. Ali, M.A. Hadi, M.M. Hossain, S.H. Naqib, A.K.M.A. Islam, Theoretical investigation of structural, elastic, and electronic properties of ternary boride MoAlB, Phys. Status Solidi. 254 (2017) 1700010. https://doi.org/10.1002/pssb.201700010.
  49. [49]M.A. Ali, M.M. Hossain, M.M. Uddin, A.K.M.A. Islam, S.H. Naqib, Understanding the improvement of thermo-mechanical and optical properties of 212 MAX phase borides Zr₂AB₂ (A = In, Tl), J. Mater. Res. Technol. 15 (2021) 2227–2241. https://doi.org/10.1016/j.jmrt.2021.09.042.
  50. [50]S. Li, W. Sun, Y. Luo, J. Yu, L. Sun, B.-T. Wang, J.-X. Liu, G.-J. Zhang, I. Di Marco, Pushing the limit of thermal conductivity of MAX borides and MABs, J. Mater. Sci. Technol. 97 (2022) 79–88. https://doi.org/10.1016/J.JMST.2021.05.006.
  51. [51]Y.X. Wang, Z.X. Yan, W. Liu, G.L. Zhou, Structure stability, mechanical properties and thermal conductivity of the new hexagonal ternary phase Ti₂InB₂ under pressure, Philos. Mag. 100 (2020) 2054–2067. https://doi.org/10.1080/14786435.2020.1754485.
  52. [52]M.M. Ali, M.A. Hadi, I. Ahmed, A.F.M.Y. Haider, A.K.M.. Islam, Physical properties of a novel boron-based ternary compound Ti₂InB₂, Mater. Today Commun. 25 (2020) 101600. https://doi.org/10.1016/j.mtcomm.2020.101600.
  53. [53]M.A. Ali, M.M. Hossain, M.M. Uddin, A.K.M.A. Islam, D. Jana, S.H. Naqib, DFT insights into new B-containing 212 MAX phases: Hf₂AB₂ (A = In, Sn), J. Alloys Compd. 860 (2021) 158408. https://doi.org/10.1016/j.jallcom.2020.158408.
  54. [54]M.A. Ali, M.M. Hossain, A.K.M.A. Islam, S.H. Naqib, Ternary boride Hf₃PB₄: Insights into the physical properties of the hardest possible boride MAX phase, J. Alloys Compd. 857 (2021) 158264. https://doi.org/10.1016/j.jallcom.2020.158264.
  55. [55]M.W. Qureshi, M.A. Ali, Y. Ma, Screen the thermomechanical and optical properties of the new ductile 314 MAX phase boride Zr₃CdB₄: A DFT insight, J. Alloys Compd. 877 (2021) 160248. https://doi.org/10.1016/j.jallcom.2021.160248.
  56. [56]M.D. Segall, P.J.D. Lindan, M.J. Probert, C.J. Pickard, P.J. Hasnip, S.J. Clark, M.C. Payne, First-principles simulation: ideas, illustrations and the CASTEP code, J. Phys. Condens. Matter. 14 (2002) 2717–2744. https://doi.org/10.1088/0953-8984/14/11/301.
  57. [57]S.J. Clark, M.D. Segall, C.J. Pickard, P.J. Hasnip, M.I.J. Probert, K. Refson, M.C. Payne, First principles methods using CASTEP, Zeitschrift Für Krist. - Cryst. Mater. 220 (2005). https://doi.org/10.1524/zkri.220.5.567.65075.
  58. [58]J.P. Perdew, K. Burke, M. Ernzerhof, Generalized Gradient Approximation Made Simple, Phys. Rev. Lett. 77 (1996) 3865–3868. https://doi.org/10.1103/PhysRevLett.77.3865.
  59. [59]H.J. Monkhorst, J.D. Pack, Special points for Brillouin-zone integrations, Phys. Rev. B. 13 (1976) 5188–5192. https://doi.org/10.1103/PhysRevB.13.5188.
  60. [60]T.H. Fischer, J. Almlof, General methods for geometry and wave function optimization, J. Phys. Chem. 96 (1992) 9768–9774. https://doi.org/10.1021/j100203a036.
  61. [61]R. Hill, The Elastic Behaviour of a Crystalline Aggregate, Proc. Phys. Soc. Sect. A. 65 (1952) 349–354. https://doi.org/10.1088/0370-1298/65/5/307.
  62. [62]M.A. Ali, A.K.M.A. Islam, M.S. Ali, Ni-rich Nitrides ANNi₃ (A = Pt, Ag, Pd) in Comparison with Superconducting ZnNNi₃, J. Sci. Res. 4 (2011) 1. https://doi.org/10.3329/jsr.v4i1.9026.
  63. [63]W. Voigt, Lehrbuch der Kristallphysik, Vieweg+Teubner Verlag, Wiesbaden, 1966. https://doi.org/10.1007/978-3-663-15884-4.
  64. [64]A. Reuss, Berechnung der Fließgrenze von Mischkristallen auf Grund der Plastizitätsbedingung für Einkristalle ., ZAMM - J. Appl. Math. Mech. / Zeitschrift Für Angew. Math. Und Mech. 9 (1929) 49–58. https://doi.org/10.1002/zamm.19290090104.
  65. [65]M.A. Ali, M. Roknuzzaman, M.T. Nasir, A.K.M.A. Islam, S.H. Naqib, Structural, elastic, electronic and optical properties of Cu₃MTe₄ (M = Nb, Ta) sulvanites — An ab initio study, Int. J. Mod. Phys. B. 30 (2016) 1650089. https://doi.org/10.1142/S0217979216500892.
  66. [66]M.A. Ali, M. Anwar Hossain, M.A. Rayhan, M.M. Hossain, M.M. Uddin, M. Roknuzzaman, K. Ostrikov, A.K.M.A. Islam, S.H. Naqib, First-principles study of elastic, electronic, optical and thermoelectric properties of newly synthesized K₂Cu₂GeS₄ chalcogenide, J. Alloys Compd. 781 (2018) 37–46. https://doi.org/10.1016/j.jallcom.2018.12.035.
  67. [67]Q. Chen, X. Li, B. Ye, L. Xiong, First-Principle Prediction of Phase Stability, Electronic and Elastic Properties Study of the Mₙ₊₁ANₙ (A = Al, Si, M = Ti, Zr, Hf), J. Phase Equilibria Diffus. 41 (2020) 883–890. https://doi.org/10.1007/s11669-020-00851-z.
  68. [68]R. Khaledialidusti, M. Khazaei, S. Khazaei, K. Ohno, High-throughput computational discovery of ternary-layered MAX phases and prediction of their exfoliation for formation of 2D MXenes, Nanoscale. 13 (2021) 7294–7307. https://doi.org/10.1039/d0nr08791b.
  69. [69]D. Ohmer, G. Qiang, I. Opahle, H.K. Singh, H. Zhang, High-throughput design of 211- M₂AX compounds, Phys. Rev. Mater. 3 (2019). https://doi.org/10.1103/PhysRevMaterials.3.053803.
  70. [70]M.W. Qureshi, M.A. Ali, X. Ma, G. Tang, M.U. Javed, D. Paudyal, Verification of stability and unraveling the electronic and physical properties of bulk and (001)-surfaces of newly synthesized Ti₂ZnX (X = C, N) MAX phases, Surfaces and Interfaces. 31 (2022) 102032. https://doi.org/10.1016/j.surfin.2022.102032.
  71. [71]M.W. Qureshi, X. Ma, G. Tang, R. Paudel, Ab initio predictions of structure and physical properties of the Zr₂GaC and Hf₂GaC MAX- phases under pressure, Sci. Reports |. 11 (2021) 1–23. https://doi.org/10.1038/s41598-021-82402-1.
  72. [72]M. Dahlqvist, B. Alling, J. Rosén, Stability trends of MAX phases from first principles, Phys. Rev. B - Condens. Matter Mater. Phys. (2010). https://doi.org/10.1103/PhysRevB.81.220102.
  73. [73]N. Atazadeh, M. Saeedi Heydari, H.R. Baharvandi, N. Ehsani, Reviewing the effects of different additives on the synthesis of the Ti₃SiC₂ MAX phase by mechanical alloying technique, Int. J. Refract. Met. Hard Mater. 61 (2016) 67–78. https://doi.org/10.1016/j.ijrmhm.2016.08.003.
  74. [74]M.A. Ali, A.K.M.A. Islam, Sn₁−xBiₓO₂ and Sn₁−xTaₓO₂ (0≤x≤0.75): A first-principles study, Phys. B Condens. Matter. 407 (2012) 1020–1026. https://doi.org/10.1016/j.physb.2012.01.002.
  75. [75]M.A. Ali, A.K.M.A. Islam, N. Jahan, S. Karimunnesa, First-principles study of SnO under high pressure, Int. J. Mod. Phys. B. 30 (2016) 1650228. https://doi.org/10.1142/S0217979216502283.
  76. [76]M.A. Ali, N. Jahan, A.K.M.A. Islam, Sulvanite Compounds Cu₃TMS₄ (TM = V, Nb and Ta): Elastic, Electronic, Optical and Thermal Properties using First-principles Method, J. Sci. Res. 6 (2014) 407–419. https://doi.org/10.3329/jsr.v6i3.19191.
  77. [77]M. Born, On the stability of crystal lattices. I, Math. Proc. Cambridge Philos. Soc. 36 (1940) 160–172. https://doi.org/10.1017/S0305004100017138.
  78. [78]F. Mouhat, F.X. Coudert, Necessary and sufficient elastic stability conditions in various crystal systems, Phys. Rev. B - Condens. Matter Mater. Phys. 90 (2014) 224104. https://doi.org/10.1103/PhysRevB.90.224104.
  79. [79]X.-Q. Chen, H. Niu, D. Li, Y. Li, Modeling hardness of polycrystalline materials and bulk metallic glasses, Intermetallics. 19 (2011) 1275–1281. https://doi.org/10.1016/j.intermet.2011.03.026.
  80. [80]N. Miao, B. Sa, J. Zhou, Z. Sun, Theoretical investigation on the transition-metal borides with Ta₃B₄-type structure: A class of hard and refractory materials, Comput. Mater. Sci. 50 (2011) 1559–1566. https://doi.org/10.1016/J.COMMATSCI.2010.12.015.
  81. [81]S.H. Jhi, J. Ihm, S.G. Louie, M.L. Cohen, Electronic mechanism of hardness enhancement in transition-metal carbonitrides, Nature. 399 (1999) 132–134. https://doi.org/10.1038/20148.
  82. [82]A. Bouhemadou, Calculated structural and elastic properties of M₂InC (M = Sc, Ti, V, Zr, Nb, Hf, Ta), Mod. Phys. Lett. B. 22 (2008) 2063–2076. https://doi.org/10.1142/S0217984908016807.
  83. [83]A. Bouhemadou, Structural, electronic and elastic properties of Ti₂TiC, Zr₂TiC and Hf₂TiC, Cent. Eur. J. Phys. 7 (2009) 753–761. https://doi.org/10.2478/s11534-009-0022-z.
  84. [84]M.A. Hadi, N. Kelaidis, S.H. Naqib, A. Chroneos, A.K.M.A. Islam, Mechanical behaviors, lattice thermal conductivity and vibrational properties of a new MAX phase Lu₂SnC, J. Phys. Chem. Solids. 129 (2019) 162–171. https://doi.org/10.1016/j.jpcs.2019.01.009.
  85. [85]S.F. Pugh, XCII. Relations between the elastic moduli and the plastic properties of polycrystalline pure metals, London, Edinburgh, Dublin Philos. Mag. J. Sci. 45 (1954) 823–843. https://doi.org/10.1080/14786440808520496.
  86. [86]D.G. Pettifor, Theoretical predictions of structure and related properties of intermetallics, Mater. Sci. Technol. 8 (1992) 345–349. https://doi.org/10.1179/026708392790170801.
  87. [87]M.A. Hadi, S.R.G. Christopoulos, S.H. Naqib, A. Chroneos, M.E. Fitzpatrick, A.K.M.A. Islam, Physical properties and defect processes of M₃SnC₂ (M = Ti, Zr, Hf) MAX phases: Effect of M-elements, J. Alloys Compd. 748 (2018) 804–813. https://doi.org/10.1016/j.jallcom.2018.03.182.
  88. [88]H.M. Ledbetter, Elastic properties of zinc: A compilation and a review, J. Phys. Chem. Ref. Data. 6 (1977) 1181–1203. https://doi.org/10.1063/1.555564.
  89. [89]J. Wang, Y. Zhou, T. Liao, Z. Lin, First-principles prediction of low shear-strain resistance of Al₃BC₃: A metal borocarbide containing short linear BC₂ units, Appl. Phys. Lett. 89 (2006) 021917. https://doi.org/10.1063/1.2220549.
  90. [90]S.I. Ranganathan, M. Ostoja-Starzewski, Universal Elastic Anisotropy Index, Phys. Rev. Lett. 101 (2008) 055504. https://doi.org/10.1103/PhysRevLett.101.055504.
  91. [91]M.A. Ali, M.W. Qureshi, DFT insights into the new Hf-based chalcogenide MAX phase Hf₂SeC, Vacuum. 201 (2022) 111072. https://doi.org/10.1016/j.vacuum.2022.111072.
  92. [92]M.A. Ali, M.W. Qureshi, Newly synthesized MAX phase Zr₂SeC: DFT insights into physical properties towards possible applications, RSC Adv. 11 (2021) 16892–16905. https://doi.org/10.1039/d1ra02345d.
  93. [93]M.A. Ali, M.M. Hossain, N. Jahan, A.K.M.A. Islam, S.H. Naqib, Newly synthesized Zr₂AlC, Zr₂(Al₀.₅₈Bi₀.₄₂)C, Zr₂(Al₀.₂Sn₀.₈)C, and Zr₂(Al₀.₃Sb₀.₇)C MAX phases: A DFT based first-principles study, Comput. Mater. Sci. 131 (2017) 139–145. https://doi.org/10.1016/j.commatsci.2017.01.048.
  94. [94]M.A. Ali, S.H. Naqib, Recently synthesized (Ti₁−xMoₓ)₂AlC (0 ≤ x ≤ 0.20) solid solutions: deciphering the structural, electronic, mechanical and thermodynamic properties via ab initio simulations, RSC Adv. 10 (2020) 31535–31546. https://doi.org/10.1039/D0RA06435A.
  95. [95]Y. Zhou, Z. Sun, Electronic structure and bonding properties of layered machinable and ceramics, Phys. Rev. B - Condens. Matter Mater. Phys. 61 (2000) 12570–12573. https://doi.org/10.1103/PhysRevB.61.12570.
  96. [96]M.A. Ali, M.W. Qureshi, DFT insights into the new Hf-based chalcogenide MAX phase Hf₂SeC, Vacuum. 201 (2022) 111072. https://doi.org/10.1016/j.vacuum.2022.111072.
  97. [97]D.R. Clarke, Materials selection guidelines for low thermal conductivity thermal barrier coatings, Surf. Coatings Technol. 163–164 (2003) 67–74. https://doi.org/10.1016/S0257-8972(02)00593-5.
  98. [98]V.N. Belomestnykh, E.P. Tesleva, Interrelation between anharmonicity and lateral strain in quasi-isotropic polycrystalline solids, Tech. Phys. 49 (2004) 1098–1100. https://doi.org/10.1134/1.1787679.
  99. [99]S.I. Mikitishin, Interrelationship of Poisson’s ratio with other characteristics of pure metals, Sov. Mater. Sci. 18 (1982) 262–265. https://doi.org/10.1007/BF01150837.
  100. [100]M.E. Fine, L.D. Brown, H.L. Marcus, Elastic constants versus melting temperature in metals, Scr. Metall. 18 (1984) 951–956. https://doi.org/10.1016/0036-9748(84)90267-9.
  101. [101]A. Bouhemadou, Prediction study of structural and elastic properties under pressure effect of M₂SnC (M = Ti, Zr, Nb, Hf), Phys. B Condens. Matter. 403 (2008) 2707–2713. https://doi.org/10.1016/j.physb.2008.02.014.
  102. [102]D. Salamon, Advanced Ceramics, in: Adv. Ceram. Dent., Elsevier Inc., 2014: pp. 103–122. https://doi.org/10.1016/B978-0-12-394619-5.00006-7.
  103. [103]B. Cui, W.E. Lee, B. Cui, W.E. Lee, High-temperature Oxidation Behaviour of MAX Phase Ceramics, Refract. Worldforum. 5 (2013) 105–112.
  104. [104]M. Barsoum, T. El-Raghy, The MAX Phases: Unique New Carbide and Nitride Materials, Am. Sci. 89 (2001) 334. https://doi.org/10.1511/2001.4.334.
  105. [105]S. Aydin, A. Tatar, Y.O. Ciftci, Some new members of MAX family including light-elements: Nanolayered Hf₂XY (X= Al, Si, P and Y Combining double low line B, C, N), Solid State Sci. 53 (2016) 44–55. https://doi.org/10.1016/j.solidstatesciences.2015.10.010.
  106. [106]S. Li, R. Ahuja, M.W. Barsoum, P. Jena, B. Johansson, Optical properties of Ti₃SiC₂ and Ti₄AlN₃, Appl. Phys. Lett. 92 (2008) 221907. https://doi.org/10.1063/1.2938862.
  107. [107]M.A. Ali, M.S. Ali, M.M. Uddin, Structural, elastic, electronic and optical properties of metastable MAX phase Ti₅SiC₄ compound, Indian J. Pure Appl. Phys. 54 (2016) 386–390.

Paper details

vlnc:W_jwu3499r
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents