betaFeedback

WorksPhysics and Astronomy

Good Practices for Measuring the Interfacial Dzyaloshinskii-Moriya Interaction by Brillouin Light Scattering and Magneto-Optical Kerr Effect

Abstract

The interfacial Dzyaloshinskii-Moriya interaction (iDMI) is a key ingredient for stabilizing chiral magnetic states, such as skyrmions and chiral domain walls, which are key building blocks for next-generation spintronic technologies. Despite its importance, the quantitative determination of the iDMI constant, DD, is often plagued by significant discrepancies. This paper establishes a set of good practices for measuring iDMI using two primary techniques: Brillouin Light Scattering (BLS) and the Magneto-Optical Kerr Effect (MOKE). Through the analysis of Co/Pt-based heterostructures, this work provides a comprehensive roadmap for measurement procedures, data evaluation, and uncertainty analysis. Our analysis highlights the crucial role of magnetic parameters used to extract the iDMI constant and propagation of their uncertainties, and the measurement model for enhancing measurement reliability. The proposed methodology provides a practical framework for improving the consistency and reproducibility of iDMI measurements across different laboratories and experimental techniques.

Introduction

The development of next-generation spintronic technologies, such as racetrack memory and logic-in-memory architectures, relies on the energy-efficient manipulation of chiral magnetic states like chiral domain walls (DWs) and skyrmions [1, 2]. These textures are particularly attractive as information carriers because electric currents can drive them with high efficiency. A fundamental requirement for stabilizing these topological spin structures is the Dzyaloshinskii-Moriya interaction (DMI).

Originally proposed in the 1950s to explain weak ferromagnetism in bulk antiferromagnets like α\alpha-Fe2_2O3_3 [3, 4], the DMI is a key ingredient for non-collinear or helical magnetic states in various systems, including spin glasses, orthoferrites, manganites, and superconducting cuprates [5, 6, 7, 8]. While the DMI often cancels out in bulk materials due to crystal inversion symmetry, a finite contribution emerges when this symmetry is broken. In thin-film heterostructures, symmetry breaking occurs at the interface between a ferromagnet (FM) and a heavy metal (HM) with strong spin-orbit coupling [9]. In these systems, the interaction becomes interfacial in nature (iDMI), therefore its strength DD is inversely proportional to the magnetic layer thickness [9, 10]. The iDMI is crucial for stabilizing Néel-type domain walls with a fixed chirality [11, 12], which are energetically favored over traditional Bloch walls and enable fast current-driven dynamics [13, 14].

However, despite its technological importance, quantitatively determining the iDMI constant DD remains challenging. Recent literature, including our review [15, 16, 17, 18] and our international interlaboratory round-robin comparison conducted across European, US, and Asian metrology and research institutes [19], reports notable discrepancies in DD values for nominally identical material systems, particularly when evaluated using different experimental techniques.

To address these inconsistencies, this work aims to establish concrete, step-by-step measurement protocols and good practices that minimize uncertainty and maximize interlaboratory reproducibility for measuring iDMI. We focus on two of the most prevalent techniques in the field [18], which were already employed in the round-robin comparison: Brillouin Light Scattering (BLS) and the Magneto-Optical Kerr Effect (MOKE). While BLS relies on the non-reciprocity of spin-wave dispersion [10, 20, 21, 22, 23, 24, 25, 26], MOKE characterizes iDMI through domain wall dynamics within the thermally activated creep regime [27, 28, 29, 30, 31, 32]. While we leave the detailed discussion of quantitative discrepancies between the two methods [19] for future work, here we focus on overcoming common pitfalls in the measurement procedures, data evaluation and uncertainty analysis. Particular key roles are attributed to the magnetic field reversal for BLS and minimum bubble size for MOKE. Furthermore, we determine spatial iDMI statistics, assess their impact on uncertainty, and correlate the results with sample homogeneity, a factor often neglected due to the substantial laboratory time required. Overall, the proposed protocols ensure reliable and reproducible results for both methods and offer a practical roadmap toward the standardized characterization of iDMI in chiral magnetic systems.

Determination of iDMI by Brillouin Light Scattering

Physical Principle: Spin-Wave Non-reciprocity

Brillouin light scattering (BLS) is a widely used technique for probing spin-wave (SW) dispersion and non-reciprocity. In a typical BLS experiment, a monochromatic laser beam is focused onto the sample surface, and the backscattered light is collected by the same objective and analyzed in frequency by a high-resolution spectrometer. During the scattering process, magnons can be either created (Stokes process) or annihilated (anti-Stokes process), resulting in a redshift or blueshift of the scattered light relative to the incident beam. In wave-vector space, Stokes and anti-Stokes processes correspond to magnons with opposite wave vectors. Because BLS probes thermally populated spin waves, it provides a non-destructive method to investigate spin dynamics without requiring external microwave excitation.

Numerous studies over the past decade have determined the iDMI constant DD using BLS, particularly in heavy-metal/ferromagnet (HM/FM) systems typically consisting of Co or CoFeB in contact with heavy metals such as Pt, W, or Ta [18]. The method exploits the fact that, in the presence of iDMI, counterpropagating spin waves exhibit different frequencies—i.e., the dispersion becomes non-reciprocal. To measure iDMI in thin films or multilayers, the Damon–Eshbach (DE) geometry is typically employed. In this configuration, the film is magnetized in-plane by a sufficiently large external magnetic field HH, while the spin-wave wave vector kk lies perpendicular to the magnetization. In the presence of iDMI, this geometry produces a non-reciprocal spin-wave dispersion. The magnitude of the SW wave vector is determined by the angle of incidence θ\theta through conservation of in-plane momentum:

k=2kilightsin⁡θ(1)k = 2k_i^{\mathrm{light}} \sin\theta \tag*{(1)}

The iDMI contribution introduces a linear frequency shift:

fDMI=γDπMsk(2)f_{\mathrm{DMI}} = \frac{\gamma D}{\pi M_s} k \tag*{(2)}

where γ\gamma is the gyromagnetic ratio and MsM_s is the saturation magnetization. Therefore, the frequency difference between counterpropagating spin waves is directly proportional to both the wave vector kk and the iDMI constant DD.

For an FM/HM bilayer, the sign of DD determines the favored magnetic chirality and depends on the Hamiltonian convention adopted; here, we use the plus-sign convention, where positive DD corresponds to Néel domain walls with right-handed (clockwise) chirality (↑→↓\uparrow\to\downarrow or ↓←↑\downarrow\leftarrow\uparrow), while negative DD corresponds to left-handed (anticlockwise) chirality (↑←↓\uparrow\leftarrow\downarrow or ↓→↑\downarrow\to\uparrow) [18]. As shown in the lower panels of Figure 1, a negative (positive) value of DD produces a negative (positive) frequency shift fDMIf_{\mathrm{DMI}}, resulting in a rigid relative displacement of the Stokes and anti-Stokes peaks.

Schematic diagram of the BLS interaction geometry

Figure 1. Schematic diagram of the BLS interaction geometry. The bottom panel shows a typical BLS spectrum in the absence of iDMI (dashed line) and with iDMI (solid line) for negative and positive values of DD, respectively. Here kilightk_i^{\mathrm{light}} denotes the incident light wave numbers, while HH and MM are the applied in-plane field and magnetization, respectively.

Measurement Protocol

Brillouin light scattering measurements were performed using a monochromatic light source (λ=532\lambda= 532 nm) provided by a single-mode diode-pumped solid-state laser. The optical path utilized a camera objective with a focal length of 50 mm and a numerical aperture of 0.25. Analysis of the backscattered light was conducted via a Sandercock-type (3+3)-pass tandem Fabry–Perot interferometer. The magnitude of the in-plane wave vector kk is defined by the incidence angle θ\theta and wavelength λ\lambda through k=4πsin⁡θλk = \frac{4\pi\sin\theta}{\lambda} (here k=1.67×107k = 1.67 \times10^7 rad/m at θ=45∘\theta= 45^\circ). The sample was mounted on a rotary non-magnetic stage between the poles of an electromagnet capable of generating fields up to 1.5 T.

Reversing the direction of the applied magnetic field, and thus the sign of fDMIf_{\mathrm{DMI}}, is essential for obtaining a reliable value of DD. The presence of iDMI is not the sole cause of a rigid frequency shift: even in a symmetric spectrum, minor optical alignment differences between the scattered light and the stabilization reference beam can introduce an instrumental asymmetry, typically on the order of 0.1–0.3 GHz. In conventional BLS measurements, this effect is negligible because the spin-wave frequency can be extracted by averaging the Stokes and anti-Stokes peaks. However, when probing systems with iDMI, this physical asymmetry combines with the instrumental offset, biasing fDMIf_{\mathrm{DMI}}.

In our experimental protocol, the two spectra under opposite field directions are acquired sequentially, immediately one after the other, on the exact same position on the sample. This back-to-back experimental protocol effectively minimizes any time-dependent thermal or mechanical drifts of the optical setup, making any temporal variation in the field-independent frequency offset negligible. Furthermore, because reversing the external magnetic field does not require any mechanical adjustment of the sample stage or optical alignment, it guarantees that the probed micro-scale volume remains identical for both field directions, preserving spatial reproducibility. The iDMI-induced frequency shift is then extracted as:

fDMI=(f+k(+H)+f−k(+H))−(f+k(−H)+f−k(−H))4(3)f_{\mathrm{DMI}}=\frac{\left(f_{+k}(+H)+f_{-k}(+H)\right)-\left(f_{+k}(-H)+f_{-k}(-H)\right)}{4} \tag*{(3)}

The uncertainty in fDMIf_{\mathrm{DMI}} is calculated using the law of propagation.

From Eq. (2), fDMIf_{\mathrm{DMI}} is proportional to the spin-wave wave vector kk, which is selected by adjusting the incidence angle θ\theta. Choosing θ\theta involves a trade-off: larger angles increase the frequency asymmetry (improving resolution), but reduce the optical signal-to-noise ratio. A fixed incidence angle of θ=45∘\theta=45^\circ represents an optimized experimental compromise for our setup: it achieves a wave vector kk large enough to yield an fDMIf_{\mathrm{DMI}} shift well above the experimental uncertainty and avoiding the sharp drop in the BLS scattering cross-section that occurs at higher angles, thus keeping the total measurement time manageable for systematic spatial mapping.

Evaluation of D from BLS Data

Evaluating DD requires fitting the Stokes and anti-Stokes peaks (typically using Lorentzian functions) to extract the resonance frequencies f±k(±H)f_{\pm k}(\pm H). As an example, Figure 2 shows two BLS spectra measured on a Ta(5 nm)/Pt(3 nm)/Co(0.8 nm)/Ir(1 nm)/Ta(3 nm) (Pt/Co/Ir) multilayer sample. This sample is part of the original series of round robin samples prepared at the University of Leeds [19]. Spectra were recorded for opposite magnetic field directions (H=±1.1H = \pm1.1 T) at an incidence angle of θ=45∘\theta= 45^\circ. From the fitted peak positions and Eq. (3), the DMI frequency and its combined standard uncertainty1 is obtained, fDMI=−0.59±0.08f_{\mathrm{DMI}} = -0.59 \pm0.08 GHz.

BLS spectra for opposite applied magnetic field directions

Figure 2. BLS spectra measured at a fixed incidence angle of θ=45∘\theta= 45^\circ for a Pt(3 nm)/Co(0.8 nm)/Ir(1 nm) sample under opposite applied magnetic field directions (H=±1.1H = \pm1.1 T). Red curves represent Lorentzian fits.

To extract the iDMI constant DD, Eq. (2) is inverted while propagating the uncertainties of all constituent parameters:

D=πMsγfDMIk(4)D = \frac{\pi M_{\mathrm{s}}}{\gamma}\frac{f_{\mathrm{DMI}}}{k} \tag*{(4)}

The uncertainty in kk (set by the incidence angle) is typically around 1%. The gyromagnetic ratio γ\gamma can be measured with an accuracy of 2–3% using ferromagnetic resonance (FMR) or field-dependent BLS measurements. Aside from fDMIf_{\mathrm{DMI}}, the largest uncertainty contribution usually stems from MsM_{\mathrm{s}}, which is commonly measured by VSM or SQUID magnetometry with an uncertainty of 5–10%. As emphasized in [19], accounting for dead layers or proximity effects is essential to accurately determine the effective magnetic volume and magnetization; neglecting these can introduce errors of 30–40%.

Laser heating must also be considered. Focused laser powers up to 200 mW can increase the local temperature in the probed region, altering temperature-dependent properties including DD. On semiconductor substrates like Si, thermal dissipation limits this temperature rise to ≈20\approx20–30 K (where variations in MsM_{\mathrm{s}} remain within experimental uncertainty), whereas insulating glass substrates can experience heating of several hundred degrees, risking sample damage.

Using the measured values (with their respective standard uncertainty (type B)) Ms=1.20±0.09 MA/mM_s = 1.20 \pm0.09\ \mathrm{MA/m} (corrected for proximity effects [19]), γ=194±4 GHz/T\gamma= 194 \pm4\ \mathrm{GHz/T}, and k=16.7±0.2 rad/μmk = 16.7 \pm0.2\ \mathrm{rad/\mu m}, we obtain D=−0.68±0.11 mJ/m2D = -0.68 \pm0.11\ \mathrm{mJ/m^2}. The relative combined standard uncertainty in DD is derived by applying the root-sum-square method to the independent physical parameters, yielding a value of about 15%. Although individual Lorentzian peak positions can be fitted with low standard uncertainty (1–5% in Figure 2), fDMIf_{\mathrm{DMI}} depends on small frequency differences, expanding the relative error. Keeping the total number of parameters low is therefore critical to minimize uncertainty propagation.

To improve statistical accuracy – an aspect that was not considered in the previous round-robin comparison – measurements were repeated at different locations across the sample surface separated by several millimeters (Figure 3). For the Pt/Co/Ir sample (Figure 3a), spatial averaging reduced the relative uncertainty from ≈20%\approx20\% for a single measurement to ≈10%\approx10\% for the relative combined standard uncertainty of the weighted mean. The black markers represent DD values obtained at five locations, while the red marker indicates the weighted average and its combined uncertainty. The spatial consistency confirms good overall sample uniformity despite minor local fluctuations.

Measured D values at various surface locations for Pt/Co/Ir, Pt/Co, continuous as-grown HZO/Co/Pt, and patterned HZO/Co/Pt pads

Figure 3. Measured DD values at various surface locations (black) and weighted averages (red) for (a) Pt/Co/Ir, (b) Pt/Co, (c) continuous as-grown HZO/Co/Pt, and (d) patterned HZO/Co/Pt pads.

An identical spatial analysis was performed on a Ta(5 nm)/Pt(3 nm)/Co(0.8 nm)/Ta(3 nm) (Pt/Co) sample, which lacks the top Ir layer (Figure 3b). As expected [18], omitting Ir increases the interfacial iDMI constant by roughly 50% (D=−0.98±0.05 mJ/m2D = -0.98 \pm0.05\ \mathrm{mJ/m^2}). While single-point combined standard uncertainties are comparable to the Pt/Co/Ir stack, the lower scatter across points indicates superior spatial uniformity, suggesting that the top Ir interface introduces additional spatial variation.

Finally, we investigated CMOS-compatible heterostructures consisting of Co/Pt deposited on a ferroelectric Hafnium Zirconium Oxide (HZO) layer: as-grown HZO(10 nm)/Co(0.7 nm)/Pt(6 nm)2. Measurements were carried out both on continuous films (seven locations) and on 400 μm×400 μm400\ \mu\mathrm{m} \times400\ \mu\mathrm{m} square pads patterned by optical lithography and ion beam etching (five locations) (Figure 3c,Figure 3d). Spectra for the continuous film required 3–4 hours of integration per spectrum due to broader linewidths and lower signal-to-noise ratios, resulting in slightly higher individual combined standard uncertainties, with a weighted average of D=0.75±0.07 mJ/m2D = 0.75 \pm0.07\ \mathrm{mJ/m^2}. The patterned pads yielded a slightly higher relative combined standard uncertainty of 15–20%, while maintaining the same weighted average DD value as the continuous film. Repeating measurements at multiple pads constrained the final relative uncertainty to 15%. Notably, DD is positive in the HZO/Co/Pt stack because the Pt layer lies above the ferromagnetic Co layer, reversing the interface symmetry relative to the Pt/Co stacks.

Determination of iDMI by Magneto-Optic Kerr Effect

Physical Principle: Creep Theory

The MOKE-based determination of iDMI exploits its influence on field-driven domain wall (DW) motion. In ultrathin magnetic films with perpendicular magnetic anisotropy (PMA), iDMI acts as an internal effective field, HDH_D, which favors chiral Néel walls over Bloch configurations. Measurements in the thermally activated creep regime [27] require low driving fields and long pulse durations, allowing DW motion to be resolved by standard magneto-optical imaging at room temperature [19, 29, 31, 32]. Expanding magnetic bubble domains provide access to the angular velocity profile, v(θ)v(\theta), around the full bubble circumference, from which the iDMI constant DD can be extracted. Under an out-of-plane driving field HzH_z and a static in-plane (IP) field HxH_x, the creep velocity is described by

v(θ,Hz)=v0exp⁡[−α0(χ(Hx,θ)μ0Hz)1/4].(5)v(\theta,H_z) = v_0 \exp\left[-\alpha_0\left(\frac{\chi(H_x,\theta)}{\mu_0 H_z}\right)^{1/4}\right]. \tag*{(5)}

Here, v0v_0 and α0\alpha_0 are experimentally determined scaling parameters, while χ(Hx,θ)\chi(H_x,\theta) is a dimensionless factor describing the IP-field and angular dependence of the activation barrier, normalized to unity at Hx=0H_x = 0. Different models of DW creep relate this factor to the equilibrium DW energy or to the DW stiffness. The energy-based model introduced by Je et al. [28] associates this dependence with changes in the equilibrium DW energy density. For an IP field applied along xx, the DW surface energy density is [33]

σ‾DW(Hx,θ,ϕ)=4AKeff−πMsΔμ0[HDcos⁡(θ−ϕ)+Hxcos⁡(ϕ)]+ln⁡(2)πδμ0Ms2cos⁡2(θ−ϕ).(6)\overline{\sigma}_{\mathrm{DW}}(H_x,\theta,\phi) = 4\sqrt{A K_{\mathrm{eff}}} - \pi M_s \Delta\mu_0 \left[H_D \cos(\theta-\phi) + H_x \cos(\phi)\right] + \frac{\ln(2)}{\pi}\delta\mu_0 M_s^2 \cos^2(\theta-\phi). \tag*{(6)}

AA is the exchange stiffness, KeffK_{\mathrm{eff}} is the effective anisotropy, MsM_s is the saturation magnetization, Δ=A/Keff\Delta= \sqrt{A/K_{\mathrm{eff}}} is the DW width, and δ\delta is the magnetic film thickness. The angles θ\theta and ϕ\phi specify the DW normal and the internal DW magnetization, respectively, relative to the xx axis. The equilibrium DW energy density follows by minimizing over ϕ\phi:

E‾DW(Hx,θ)=min⁡ϕ∈[0,2π)σ‾DW(Hx,θ,ϕ).(7)\overline{\mathcal{E}}_{\mathrm{DW}}(H_x,\theta) = \min_{\phi\in[0,2\pi)} \overline{\sigma}_{\mathrm{DW}}(H_x,\theta,\phi). \tag*{(7)}

In this model, the factor entering Eq. (5) is χ(Hx,θ)=E‾DW(Hx,θ)/E‾DW(0,θ)\chi(H_x,\theta) = \overline{\mathcal{E}}_{\mathrm{DW}}(H_x,\theta)/\overline{\mathcal{E}}_{\mathrm{DW}}(0,\theta). Although this approximation describes creep velocities in some systems, its applicability is limited when the anisotropic elastic response of the DW becomes significant. We therefore compare this model with the stiffness-based description introduced by Pellegren, Lau, and Sokalski [34]

σ~DW(Hx,θ)=E‾DW(Hx,θ)+σθθ,(8)\widetilde{\sigma}_{\mathrm{DW}}(H_x,\theta) = \overline{\mathcal{E}}_{\mathrm{DW}}(H_x,\theta) + \sigma_{\theta\theta}, \tag*{(8)}

where σθθ\sigma_{\theta\theta} is the second partial derivative of the unminimized DW energy density with respect to θ\theta, taken at fixed internal angle ϕ\phi and evaluated at the equilibrium angle that minimizes the DW energy (Eq. (7)). In this version of the model, χ(Hx,θ)=σ~DW(Hx,θ)/σ~DW(0,θ)\chi(H_x,\theta) = \widetilde{\sigma}_{\mathrm{DW}}(H_x,\theta)/\widetilde{\sigma}_{\mathrm{DW}}(0,\theta) [35].

Measurement Protocol

To measure asymmetric bubble expansion, a standard wide-field MOKE microscope is used, configured to apply simultaneous in-plane (IP) and out-of-plane (OOP) magnetic fields. In our setup, a commercial EVICO MOKE system was equipped with flat-pole electromagnet pieces capable of IP fields up to 150 mT, alongside an OOP coil generating up to 100 mT. Post-processing of polar Kerr images to extract DW velocities was performed using custom Python-based software [32].

To ensure the entire field of view remains in sharp focus, precise sample-stage tilt control is required. Strict planarity is critical: any angle misalignment causes the strong IP field to project a parasitic OOP field component onto the sample, which artificially biases the measured DW velocity.

The measurement sequence follows three standardized steps: saturation, nucleation, and expansion.

  1. Saturation: The sample is magnetized to a uniform state using a high-amplitude HzH_z pulse.

  1. Nucleation: A initial domain (magnetic bubble) is nucleated using a square out-of-plane field pulse, HznucH_z^{\mathrm{nuc}}. A reference Kerr image, I(Hznuc)I(H_z^{\mathrm{nuc}}), is captured to record the initial bubble size.

Expansion

A propagation field pulse, HzpropH_z^{\mathrm{prop}}, is applied to drive domain expansion. The expanded state is recorded in image I(Hzprop)I(H_z^{\mathrm{prop}}).

Calculating the differential image ΔI=I(Hzprop)−I(Hznuc)\Delta I=I(H_z^{\mathrm{prop}})-I(H_z^{\mathrm{nuc}}) subtracts background optical artifacts. As shown in Figure 4, the initial bubble domain appears as a central light region, while the newly expanded area appears dark. This differential technique cleanly isolates the starting and ending DW boundaries, significantly improving spatial accuracy.

Nucleated magnetic bubble and expanded domain difference image

Figure 4. Nucleated magnetic bubble I(Hznuc)I(H_z^{\mathrm{nuc}}) imaged at 100× magnification to highlight initial DW boundary roughness (left; scale bar: 50 μ\mum). Expanded domain difference image I(Hzprop)−I(Hznuc)I(H_z^{\mathrm{prop}})-I(H_z^{\mathrm{nuc}}) captured at 20× magnification (right; scale bar: 200 μ\mum). Applied field pulse parameters: Hznuc=27H_z^{\mathrm{nuc}}=27 mT, Hzprop=20H_z^{\mathrm{prop}}=20 mT. Sample: HZO/Co/Pt (see Table 1).

Before data collection, the system is calibrated to ensure the planarity of the sample surface with respect to the IP field. The DW velocity is obtained by the time duration of the field pulse and by a measure of the bubble displacement along the xx axis. This displacement Δx\Delta x is caused by the HzH_z pulse produced by the OOP coil, under a (generally non-zero) IP field HxH_x. In the presence of a slight tilt α\alpha of the sample with respect to the HxH_x direction, an additional Hxsin⁡αH_x\sin\alpha field is generated, accelerating or slowing the DW motion depending on its sign. A simple solution is the acquisition of two expanded bubble images under opposing HxH_x field. By tuning a tilting stage holder the condition is reached in which Δx+Hx=Δx−Hx\Delta x_{+H_x}=\Delta x_{-H_x}, within pixel resolution (at 50× magnification, 1 px ≈\approx 235 nm), confirming the elimination of stray OOP components.

After calibration, the creep scaling parameters v0v_0 and α0\alpha_0 are determined by measuring the DW velocity v(Hz)v(H_z) at zero IP field across various OOP pulse amplitudes (HzH_z) and fitting the response to the creep power law. Pulses typically use a duration of Δt=100\Delta t=100 μ\mus, with multiple pulses applied if larger displacements are required.

A known challenge in MOKE-based iDMI determination is that the domain expansion characteristics varies from bubble to bubble, which can increase measurement uncertainty. As shown in our recent work [32], this variation stems from a dependence of DW expansion velocity on the initial bubble domain radius. Small initial radii introduce a negative curvature-induced pressure (analogous to Laplace pressure in liquid droplets) that acts like a demagnetizing field, hindering domain expansion. To eliminate this systematic effect, a preliminary calibration is performed to identify the minimum radius, Rbmin⁡R_b^{\min}, above which velocity becomes independent of initial domain size. All subsequent measurements acquiring v(θ,Hx,Hz,Rb)v(\theta, H_x, H_z, R_b) are conducted for Rb>Rbmin⁡R_b > R_b^{\min}. The effective iDMI field HDH_D is then extracted using either field-dependent velocity profiling or single-image anisotropic mapping.

Evaluation of D from MOKE Data

Once domain expansion images are acquired, the effective iDMI field HDH_D (and the corresponding iDMI constant DD) can be extracted through two primary approaches:

IP-Field Dependent Velocity Profiling

The most widespread method determines HDH_D by measuring DW velocity vv as a function of an applied IP field HxH_x swept along fixed angular directions (typically along the field axis, θ=0\theta= 0 and θ=π\theta= \pi). Fitting the resulting v(Hx)v(H_x) velocity profiles against Eq. (5) yields HDH_D.

The primary strength of field-dependent profiling lies in its experimental robustness: HDH_D is directly identified by the shift in the minimum of the v(Hx)v(H_x) curve. In the absence of iDMI, domain wall velocity is symmetric around Hx=0H_x = 0; an internal iDMI field shifts this velocity minimum to Hx,min⁡=±HDH_{x,\min} = \pm H_D, corresponding to the IP field that exactly compensates HDH_D. Because this approach relies directly on measured velocity-field curves, it minimizes dependence on auxiliary parameters and their associated uncertainties [19]. However, acquiring velocity profiles across many field points is time-consuming and less suited for rapid screening or constrained geometries.

Single-Image Method

Alternatively, HDH_D can be extracted by mapping the full angular velocity profile v(θ)v(\theta) from a single asymmetric expansion event. Fitting this profile numerically to Eq. (5) yields HDH_D (Figure 5) [33].

Figure 5. (a) Predicted anisotropic velocity profiles v(θ)v(\theta) for different values of μ0HD\mu_{0}H_{D}. (b) Schematic representation of asymmetric bubble expansion under simultaneous IP (HxH_{x}) and OOP (HzH_{z}) magnetic fields. The cartoon shows a positive DMI (D>0D > 0) bubble expansion with an OOP applied field HzH_{z}.

The single-image method significantly increases throughput, making it well-suited for collecting large statistical datasets or characterizing spatially confined micro-patterned samples where domain expansion distance is constrained. However, because an analytical expression for the minimized energy density (Eq. (7)) cannot be written in closed form, the fit relies on numerical minimization. This demands precise, independent measurement of all auxiliary material parameters prior to fitting, including saturation magnetization (MsM_s), exchange stiffness (AA), effective anisotropy (KeffK_{\mathrm{eff}}), film thickness (δ\delta), and creep parameters (v0,α0v_0, \alpha_0).

The overall multiplicative prefactor v0v_0 can be eliminated as a fitting parameter by normalizing each angular velocity profile to its peak value. Care is required, however, because fluctuations in the normalization reference affect the entire profile and can influence the fit-[12]

ted HDH_D. We therefore normalize each profile by the arithmetic mean of the four measured velocities nearest the reference peak direction, which yields more stable HDH_D estimates than normalization by a single measured value.

A fundamental challenge for both MOKE evaluation techniques is the absence of a single, universally accepted analytical model for chiral DW dynamics in the creep regime [31, 34]. Consequently, model selection must be carefully evaluated for each specific material system.

Experimental Results

A detailed analysis of asymmetric expansion by MOKE in the Pt/Co/Ir and Pt/Co round-robin samples using field-dependent velocity profiling was previously reported by the authors, noting that MOKE evaluations often yield systematically lower DD values than BLS on those systems [19]. Here, we focus instead on the HZO/Co/Pt sample stack and analyze the uncertainty of the high-throughput single-image method.

Eight measurements were performed on three different 400 μm×400 μm400\,\mu\mathrm{m} \times400\,\mu\mathrm{m} patterned pads of the as-grown HZO/Co/Pt stack, labeled 4A, 6B, and 10D in Figure 6. The anisotropic velocity profiles v(θ)v(\theta), recorded at μ0Hx=±130 mT\mu_0 H_x = \pm130\,\mathrm{mT} and μ0Hz=19.4 mT\mu_0 H_z = 19.4\,\mathrm{mT}, are shown in the same figure. For each measurement, HDH_D was extracted by fitting Eq. (5). We tested two creep models: one in which χ(Hx,θ)\chi(H_x,\theta) depends on the domain wall energy density [28, 33] – this is the model more commonly used in literature; and a second in which χ(Hx,θ)\chi(H_x,\theta) depends on the domain wall stiffness [34, 35]. The creep coefficient α0\alpha_0 was fixed at its independently determined value. The other auxiliary parameters used in the model are reported in Table 1. MsM_s, and KeffK_{\mathrm{eff}} were were obtained from the independent magnetometry [19] and fixed at their nominal values. The Co thickness used in the model was obtained from the independent X-ray characterization. The exchange stiffness was not measured directly. We used a nominal value of A=20 pJ m−1A = 20\,\mathrm{pJ}\,\mathrm{m}^{-1} and assigned a uniform interval of 1515-25 pJ m−125\,\mathrm{pJ}\,\mathrm{m}^{-1}, based on values reported for comparable ultrathin Co films [36, 37, 38]. This interval corresponds to a standard uncertainty u(A)=5 pJ m−1u(A) = 5\,\mathrm{pJ}\,\mathrm{m}^{-1}. Uncertainties in AA, MsM_s, and KeffK_{\mathrm{eff}} were propagated using numerical sensitivity coefficients following JCGM 100:2008, Sec. 5.1.3, Note 2. For each input q∈{A,Ms,Keff}q \in\{A, M_s, K_{\mathrm{eff}}\}, the complete velocity-profile fit was repeated at q0−u(q)q_0-u(q) and q0+u(q)q_0+u(q), while the other inputs were held at their nominal values. At each perturbed value, DD was recalculated as

ParameterSymbolValueUnit
Co Thicknessδ\delta0.68±0.030.68 \pm0.03nm
Saturation magnetizationMsM_{\mathrm{s}}1.42±0.021.42 \pm0.02MA m−1\mathrm{m}^{-1}
Effective anisotropyKeffK_{\mathrm{eff}}0.67±0.020.67 \pm0.02MJ m−3\mathrm{m}^{-3}
Exchange stiffnessAA20±5∗20 \pm5^{*}pJ m−1\mathrm{m}^{-1}

Table 1. Material Parameters for As-Grown HZO/Co/Pt. All parameters, except AA, were obtained from independent measurements with combined standard uncertainties (type B). *Literature value. [36, 37, 38]

Figure 6. Normalized Anisotropic velocity profiles vnormv_{\mathrm{norm}} measured across 8 distinct measurements performed on 3 pads of the as-grown HZO/Co/Pt sample. The label "rep." indicates an independent measurement on the same sample pad.

D=μ0MsAKeffHD.(9)D = \mu_0 M_s \sqrt{\frac{A}{K_{\mathrm{eff}}}} H_D. \tag*{(9)}

The sensitivity coefficient and corresponding standard uncertainty contribution were evaluated as

cq≃D[q0+u(q)]−D[q0−u(q)]2u(q),uq(D)=∣cq∣u(q).(10)c_q \simeq\frac{D[q_0+u(q)]-D[q_0-u(q)]}{2u(q)}, \qquad u_q(D)=\lvert c_q\rvert u(q). \tag*{(10)}

Assuming uncorrelated inputs, the combined standard uncertainty of each determination was calculated as

uc(D)=ufit2(D)+uA2(D)+uMs2(D)+uKeff2(D).(11)u_c(D)=\sqrt{u_{\mathrm{fit}}^2(D)+u_A^2(D)+u_{M_s}^2(D)+u_{K_{\mathrm{eff}}}^2(D)}. \tag*{(11)}

where ufit(D)u_{\mathrm{fit}}(D) is the standard uncertainty obtained from the nominal fit. The individual DD estimates obtained from the fit and the above stated uncertainty estimation are show in Figure 7. The individual determinations are compatible within their combined standard uncertainties. The overall DD value is calculated as their inverse-variance weighted mean, treating all measurements as independent. Its error bar represents the combined standard uncertainty of the weighted mean.

Figure 7. iDMI constant values (D) obtained by fitting the measured v(θ)v(\theta) profiles shown in Figure 6. The black triangles are the values obtained by fitting the energy only model [28, 33] (Eq. (7)) and the red circles are the values obtained from the DW stiffness [34, 35] (Eq. (8)). The values separated by the dashed line are the average (weighted mean) values. The black star is the iDMI value obtained from BLS measurements.

Discussion

The BLS method provides a reliable framework for determining the iDMI constant DD, exploiting the non-reciprocal dispersion of Damon–Eshbach spin waves and modeling the response with a limited number of free parameters. This simplicity inherently minimizes the impact of error propagation compared to more complex models. An essential experimental protocol identified here is the implementation of field reversal, which is mandatory to decouple iDMI-induced non-reciprocity from inherent instrumental asymmetries within the interferometer. To address spatial inhomogeneities, we utilized multi-point spatial sampling across the sample surface. This practice significantly reduces statistical uncertainty through weighted averaging and serves as a diagnostic tool for verifying sample uniformity and interface quality. While BLS precision is sensitive to the signal-to-noise ratio and linewidth of the spectra, sometimes requiring acquisition times of 4–8 hours per spectrum, we demonstrate that rigorous statistical sampling can constrain uncertainty to 15–20%, even in samples with low spectrum quality.

In contrast, creep-regime MOKE microscopy provides a faster and more accessible route to iDMI characterization, making the single-image method particularly suitable for high-throughput screening. Quantitative extraction nevertheless requires independent knowledge of parameters such as MsM_{\mathrm{s}}, KeffK_{\mathrm{eff}} and AA entering Eq. (6), some of which, particularly AA, are difficult to determine accurately. The analysis must also account for the dependence of DW velocity on the bubble radius, which otherwise introduces a systematic bias in the extracted effective iDMI field.

A more fundamental limitation is the absence of a universally accepted model of chiral DW dynamics in the creep regime [31, 34]. Although the energy-only model can adequately describe some material systems, including that studied by Pakam et al., for the present HZO/Co/Pt dataset it gives Denergy=0.46±0.02D_{\mathrm{energy}} = 0.46 \pm0.02 mJ/m2^2, approximately 38% below the BLS result of 0.75±0.070.75 \pm0.07 mJ/m2^2. Together with the measurement-to-measurement scatter in Figure 7, this suggests that the energy-only model does not capture all contributions to the velocity profiles. Including DW elasticity through the field-dependent DW stiffness [35] instead brings the MOKE-derived value (Dstiffness=0.86±0.05D_{\mathrm{stiffness}} = 0.86 \pm0.05 mJ/m2^2) into agreement with BLS.

Since no independent criterion currently determines which creep model is appropriate for a given material system, model selection remains the principal limitation of quantitative MOKE characterization. MOKE and BLS can nevertheless be used complementarily: BLS can provide a reference DD value to constrain multi-parameter creep-model fits [35], after which the faster MOKE method can screen similar samples or patterned structures. In this approach, however, the BLS result acts as a calibration constraint rather than an independent validation of the creep model.

Conclusions

In this work, we establish a comprehensive set of good practices for the reliable determination of the iDMI constant, DD, using either BLS spectroscopy or MOKE microscopy. By investigating various heavy-metal/ferromagnet heterostructures, specifically Pt/Co/Ir, Pt/Co, and HZO/Co/Pt stacks, we identify primary sources of uncertainty and provide robust methodologies for their mitigation. Our analysis reveals that BLS inherently yields lower uncertainties due to the reduced number of independent parameters required to evaluate DD. However, this technique remains highly sensitive to sample quality and may necessitate long measurement times to achieve sufficient signal-to-noise ratios. Conversely, MOKE microscopy offers the advantages of wider accessibility and high throughput, yet the determination of DD is complicated by a larger parameter space, including creep coefficients, which can propagate significant measurement error. Furthermore, the selection of an appropriate measurement model is critical and must be tailored to the specific magnetic properties of the sample. We recommend that researchers carefully weigh these experimental trade-offs to ensure a reliable determination of the iDMI constant. Adhering to the protocols established herein, incorporating field reversal symmetry, domain wall curvature corrections, and rigorous statistical sampling, is essential for achieving the reproducible iDMI values necessary to advance next-generation chiral spintronic devices.

Acknowledgment

The work was supported by the MetroSpin project, funded by PRIN2022 SAYARY (CUP E53D2300183 0006) financed by the European Union - Next Generation EU and MUR (Ministero dell’Universita e della Ricerca). C.R. and G.G. acknowledge the project Spin-ORBit Effects in Two-dimensional magnets (SORBET) – ID 2022ZY8HJY - CUP D53D23002500006 financed by EU – Next Generation EU - “PNRR - M4C2, investimento 1.1 - “Fondo PRIN 2022”. We thank E. Darwin and A. Huxtable for the growth of the round robin multilayers at the University of Leeds.

References

  1. [1]B. Dieny, I. L. Prejbeanu, K. Garello, P. Gambardella, P. Freitas, R. Lehndorff, W. Raberg, U. Ebels, S. O. Demokritov, J. Akerman, A. Deac, P. Pirro, C. Adelmann, A. Anane, A. V. Chumak, A. Hirohata, S. Mangin, S. O. Valenzuela, M. C. Onbaşlı, M. d’Aquino, G. Prenat, G. Finochio, L. Lopez-Diaz, R. Chantrell, O. Chubykalo-Fesenko, and P. Bortolotti, “Opportunities and challenges for spintronics in the micro-electronics industry,” Nature Electronics, vol. 3, no. 8, pp. 446–459, 2020.
  2. [2]S. Parkin and S.-H. Yang, “Memory on the racetrack,” Nature Nanotechnology, vol. 10, no. 3, pp. 195–198, 2015.DOI
  3. [3]I. E. Dzyaloshinskii, “Thermodynamic theory of “Weak” ferromagnetism in antiferromagnetic substances,” Sov. Phys. JETP, vol. 5, no. 6, p. 1259, 1957.
  4. [4]T. Moriya, “Anisotropic superexchange interaction and weak ferromagnetism,” Phys. Rev., vol. 120, no. 6, p. 91, 1960.DOI
  5. [5]A. Fert and P. M. Levy, “Role of anisotropic exchange interactions in determining the properties of spin-glasses,” Phys. Rev. Lett., vol. 44, no. 23, pp. 1538–1541, 1980.DOI
  6. [6]H. M. Luo, Y. Y. Hsu, B. N. Lin, Y. P. Chi, T. J. Lee, and H. C. Ku, “Correlation between weak ferromagnetism and crystal symmetry in Gd₂CuO₄-type cuprates,” Phys. Rev. B, vol. 60, no. 18, pp. 13 119–13 124, 1999.DOI
  7. [7]A. N. Bogdanov, U. K. Rößler, M. Wolf, and K.-H. Müller, “Magnetic structures and reorientation transitions in noncentrosymmetric uniaxial antiferromagnets,” Phys. Rev. B, vol. 66, no. 21, p. 214410, 2002.DOI
  8. [8]D. Coffey, T. M. Rice, and F. C. Zhang, “Dzyaloshinskii-Moriya interaction in the cuprates,” Phys. Rev. B, vol. 44, no. 18, pp. 10 112–10 116, 1991.pubmed.ncbi.nlm.nih.gov/9999014
  9. [9]F. Hellman, A. Hoffmann, Y. Tserkovnyak, G. S. D. Beach, E. E. Fullerton, C. Leighton, A. H. Macdonald, D. C. Ralph, D. A. Arena, H. A. Dürr, P. Fischer, J. Grollier, J. P. Heremans, T. Jungwirth, A. V. Kimel, B. Koopmans, I. N. Krivorotov, S. J. May, A. K. Petford-Long, J. M. Rondinelli, N. Samarth, I. K. Schuller, A. N. Slavin, M. D. Stiles, O. Tchernyshyov, A. Thiaville, and B. L. Zink, “Interface-induced phenomena in magnetism,” Rev. Mod. Phys., vol. 89, no. 2, p. 025006, 2017.
  10. [10]J.-H. Moon, S.-M. Seo, K.-J. Lee, K.-W. Kim, J. Ryu, H.-W. Lee, R. D. McMichael, and M. D. Stiles, “Spin-wave propagation in the presence of interfacial Dzyaloshinskii-Moriya interaction,” Phys. Rev. B, vol. 88, no. 18, p. 184404, 2013.
  11. [11]M. Heide, G. Bihlmayer, and S. Blügel, “Dzyaloshinskii-Moriya interaction accounting for the orientation of magnetic domains in ultrathin films: Fe/W(110),” Phys. Rev. B, vol. 78, no. 14, p. 140403, 2008.DOI
  12. [12]A. Thiaville, S. Rohart, É. Jué, V. Cros, and A. Fert, “Dynamics of Dzyaloshinskii domain walls in ultrathin magnetic films,” EPL, vol. 100, no. 5, p. 57002, 2012.DOI
  13. [13]S. Emori, U. Bauer, S.-M. Ahn, E. Martinez, and G. S. D. Beach, “Current-driven dynamics of chiral ferromagnetic domain walls,” Nat. Mater., vol. 12, pp. 611–616, 2013.DOI
  14. [14]K.-S. Ryu, L. Thomas, S.-H. Yang, and S. Parkin, “Chiral spin torque at magnetic domain walls,” Nat. Nanotechnol., vol. 8, pp. 527–533, 2013.DOI
  15. [15]R. Soucaille, M. Belmeguenai, J. Torrejon, J.-V. Kim, T. Devolder, Y. Roussigne, S.-M. Chérif, A. A. Stashkevich, M. Hayashi, and J.-P. Adam, “Probing the Dzyaloshinskii-Moriya interaction in CoFeB ultrathin films using domain wall creep and Brillouin light spectroscopy,” Phys. Rev. B, vol. 94, no. 10, p. 104431, 2016.DOI
  16. [16]K. Shahbazi, J.-V. Kim, H. T. Nembach, J. M. Shaw, A. Bischof, M. D. Rossell, V. Jeudy, T. A. Moore, and C. H. Marrows, “Domain-wall motion and interfacial Dzyaloshinskii-Moriya interactions in Pt/Co/Ir({tIr})/Ta multilayers,” Phys. Rev. B, vol. 99, no. 9, p. 94409, Mar. 2019.DOI
  17. [17]L. Herrera Diez, Y. T. Liu, D. A. Gilbert, M. Belmeguenai, J. Vogel, S. Pizzini, E. Martinez, A. Lamperti, J. B. Mohammedi, A. Laborieux, Y. Roussigne, A. J. Grutter, E. Arenholtz, P. Quarterman, B. Maranville, S. Ono, M. S. E. Hadri, R. Tolley, E. E. Fullerton, L. Sanchez-Tejerina, A. Stashkevich, S. M. Chérif, A. D. Kent, D. Querlioz, J. Langer, B. Ocker, and D. Ravelosona, “Nonvolatile Ionic Modification of the Dzyaloshinskii-Moriya Interaction,” Physical Review Applied, vol. 12, no. 3, p. 1, 2019. [Online]. Available: https://doi.org/10.1103/PhysRevApplied.12.034005
  18. [18]M. Kuepferling, A. Casiraghi, G. Soares, G. Durin, F. Garcia-Sanchez, L. Chen, C. H. Back, C. H. Marrows, S. Tacchi, and G. Carlotti, “Measuring interfacial Dzyaloshinskii-Moriya interaction in ultra-thin magnetic films,” Rev. Mod. Phys., vol. 95, no. 1, p. 015003, 2023.
  19. [19]A. Magni, G. Carlotti, A. Casiraghi, E. Darwin, G. Durin, L. H. Diez, B. J. Hickey, A. Huxtable, C. Y. Hwang, G. Jakob, C. Kim, M. Kläui, J. Langer, C. H. Marrows, H. T. Nembach, D. Ravelosona, G. A. Riley, J. M. Shaw, V. Sokalski, S. Tacchi, and M. Kuepferling, “Key points in the determination of the interfacial Dzyaloshinskii-Moriya interaction from asymmetric bubble domain expansion,” IEEE Transactions on Magnetics, vol. 58, no. 12, pp. 1–16, 2022.DOI
  20. [20]L. Udvardi and L. Szunyogh, “Chiral asymmetry of the spin-wave spectra in ultrathin magnetic films,” Phys. Rev. Lett., vol. 102, no. 20, p. 207204, 2009.pubmed.ncbi.nlm.nih.gov/19519069
  21. [21]M. Kostylev, “Non-reciprocity of dipole-exchange spin waves in thin ferromagnetic films,” J. Appl. Phys., vol. 113, no. 5, p. 053901, 2013.DOI
  22. [22]D. Cortés-Ortuño and P. Landeros, “Influence of the Dzyaloshinskii-Moriya interaction on the spin-wave spectra of thin films,” J. Phys. Condens. Matter, vol. 25, no. 15, p. 156001, 2013.
  23. [23]H. T. Nembach, J. M. Shaw, M. Weiler, E. Jué, and T. J. Silva, “Linear relation between Heisenberg exchange and interfacial Dzyaloshinskii-Moriya interaction in metal films,” Nature Physics, vol. 11, no. 10, pp. 825–829, 2015.DOI
  24. [24]K. Di, V. L. Zhang, H. S. Lim, S. C. Ng, M. H. Kuok, J. Yu, J. Yoon, X. Qiu, and H. Yang, “Direct Observation of the Dzyaloshinskii-Moriya Interaction in a Pt/Co/Ni Film,” Phys. Rev. Lett., vol. 114, no. 4, p. 47201, Jan. 2015. [Online]. Available: https://link.aps.org/doi/10.1103/PhysRevLett.114.047201DOI
  25. [25]X. Ma, G. Yu, S. A. Razavi, S. S. Sasaki, X. Li, K. Hao, S. H. Tolbert, K. L. Wang, and X. Li, “Dzyaloshinskii-Moriya Interaction across an Antiferromagnet-Ferromagnet Interface,” Phys. Rev. Lett., vol. 119, no. 2, p. 27202, Jul. 2017.DOI
  26. [26]W. Lin, B. Yang, A. P. Chen, X. Wu, R. Guo, S. Chen, L. Liu, Q. Xie, X. Shu, Y. Hui, G. M. Chow, Y. Feng, G. Carlotti, S. Tacchi, H. Yang, and J. Chen, “Perpendicular Magnetic Anisotropy and Dzyaloshinskii-Moriya Interaction at an Oxide/Ferromagnetic Metal Interface,” 2020.
  27. [27]S. Lemerle, J. Ferré, C. Chappert, V. Mathet, T. Giamarchi, and P. Le Doussal, “Domain wall creep in an Ising ultrathin magnetic film,” Phys. Rev. Lett., vol. 80, no. 4, pp. 849–852, 1998.DOI
  28. [28]S.-G. Je, D.-H. Kim, S.-C. Yoo, B.-C. Min, K.-J. Lee, and S.-B. Choe, “Asymmetric magnetic domain-wall motion by the Dzyaloshinskii-Moriya interaction,” Phys. Rev. B, vol. 88, no. 21, p. 214401, 2013.DOI
  29. [29]M. Vaňatka, J.-C. Rojas-Sánchez, J. Vogel, M. Bonfim, M. Belmeguenai, Y. Roussigne, A. Stashkevich, A. Thiaville, and S. Pizzini, “Velocity asymmetry of Dzyaloshinskii domain walls in the creep and flow regimes,” J. Phys.: Condens. Matter, vol. 27, no. 32, p. 326002, 2015.DOI
  30. [30]A. Hrabec, N. A. Porter, A. Wells, M. J. Benitez, G. Burnell, S. McVitie, D. Mc-Grouther, T. A. Moore, and C. H. Marrows, “Measuring and tailoring the Dzyaloshinskii-Moriya interaction in perpendicularly magnetized thin films,” Phys. Rev. B, vol. 90, no. 2, p. 020402(R), 2014.DOI
  31. [31]D. M. F. Hartmann, R. A. Duine, M. J. Meijer, H. J. M. Swagten, and R. Lavrijsen, “Creep of chiral domain walls,” Phys. Rev. B, vol. 100, no. 9, p. 094417, 2019.DOI
  32. [32]A. Di Pietro, A. Magni, G. Durin, M. Kuepferling, G. Carlotti, M. Madami, C. Marrows, A. Huxtable, B. Hickey, S. Tacchi, and E. Darwin, “Effect of magnetic domain-wall curvature on velocity in the creep regime,” Phys. Rev. Appl., vol. 24, no. 2, p. 024044, 2025.arxiv.org/abs/2503.19811
  33. [33]T. Pakam, A. A. Adjanoh, S. D. M. Afenyiveh, J. Vogel, S. Pizzini, and L. Ranno, “Anisotropic creep velocity of Dzyaloshinskii domain walls,” Appl. Phys. Lett., vol. 124, no. 9, p. 092403, 2024.DOI
  34. [34]J. P. Pellegren, D. Lau, and V. Sokalski, “Dispersive stiffness of Dzyaloshinskii domain walls,” Phys. Rev. Lett., vol. 119, no. 2, p. 027203, 2017.DOI
  35. [35]A. D. Pietro, A. Magni, S. Pizzini, F. Dörr, Y. Shokr, G. Durin, S. Tacchi, M. Madami, G. Carlotti, E. Darwin, A. J. Huxtable, C. H. Marrows, B. J. Hickey, and M. Kuepferling, “Anisotropic domain wall velocity profiles in the creep regime: the interplay of chiral damping, stiffness and Dzyaloshinskii-Moriya interaction,” arXiv preprint arXiv:2607.25470 [cond-mat.mes-hall], 2026. [Online]. Available: https://arxiv.org/abs/2607.25470
  36. [36]B. Zimmermann, G. Bihlmayer, M. Böttcher, M. Bouhassoune, S. Lounis, J. Sinova, S. Heinze, S. Blügel, and B. Dupé, “Comparison of first-principles methods to extract magnetic parameters in ultrathin films: Co/pt(111),” Physical Review B, 2019.DOI
  37. [37]T. Böttcher, T. S. Suraj, X.-Y. Chen, B. Sinha, H. Tan, H. K. Tan, R. Laskowski, B. Hillebrands, M. Kostylev, K. Khoo, A. Soumyanarayanan, and P. Pirro, “Quantifying symmetric exchange in ultrathin ferromagnetic films with chirality,” Physical Review B, 2021.DOI
  38. [38]T. Devolder, J.-V. Kim, L. Nistor, R. Sousa, B. Rodmacq, and B. Dieny, “Exchange stiffness in ultrathin perpendicularly magnetized cof eb layers determined using the spectroscopy of electrically excited spin waves,” Journal of Applied Physics, vol. 120, p. 183902, 2016.DOI

Paper details

vlnc:W_k32jvge3
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 13

downloads · 1

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…