Ultralow Thermal Conductivity and Thermoelectric Properties of Bi4GeTe7 with an Intrinsic van der Waal Heterostructure

Abstract

Ternary chalcogenides, having large crystalline unit cell and van der Waal stacking of layers, are expected to be poor thermal conductors and good thermoelectric (TE) materials. We are reporting that layered Bi4GeTe7, with alternating quintuplet-septuplet layers of Bi2Te3 and Bi2GeTe4, has an ultralow thermal conductivity, \k{appa}total 0.42 Wm-1K-1 because of high degree of anharmonicity as estimated from large Gruneisen parameter (γ 4.07) and low Debye temperature (θd 135 K). The electron dominated charge transport has been realized from the Seebeck coefficient, S - 82 uV/K, at 380 K, and Hall carrier concentration of ne ~ 9.8 x 1019 cm-3 at 300 K. Observation of weak antilocalization (WAL), due to spin-orbit coupling (SOC) of heavy Bi and Te, advocate Bi4GeTe7 to be a topological quantum material also. The cross-sectional transmission electron microscopy images show the inherent stacking of hetero-layers, which are leading to a large anharmonicity for poor phonon propagation. Thus, being a poor thermal conductor with a TE figure of merit, ZT ~ 0.24, at 380 K, the Bi4GeTe7 is a good material for TE applications.

Thermoelectric materials are important for harvesting waste thermal energy by directly converting heat into useful electricity.[1] The efficiency of TE materials are governed by the dimensionless figure of merit, ZT=S2σκtotalTZT = \frac{S^{2}\sigma}{\kappa_{total}}T, where SS is Seebeck coefficient, σ\sigma is electrical conductivity, TT is absolute temperature and κtotal\kappa_{total} denotes the total thermal conductivity which has contribution from electrons (κe\kappa_{e}) as well as lattice (κl\kappa_{l}).[1] The involved physical parameters, except κl\kappa_{l}, are intricately interdependent and thus limiting the usage of TE materials for commercial applications. After understanding the challenges of optimizing the charge carriers in TE research, recently, materials with intrinsically ultralow κl\kappa_{l} have grabbed the scientific attention since it allows to modulate the σ\sigma with negligible rise in κe\kappa_{e}, independently.[2, 3, 4, 5] In general, materials having high degree of anharmonicity shows ultralow κl\kappa_{l} due to damping effects of phonon-phonon interactions, which plays an important role in engineering of their thermal properties.[5]

In TE materials with large unit cells, complex and layered crystal structures, the presence of large number of defects give a high degree of crystal anharmonicity hence reducing κtotal\kappa_{total}.[6, 3, 5] By adopting various methodologies such as nanostructuring, second phase nanoinclusions, mass contrast, soft phonons and phonon-glass/liquid-electron-crystal (PGEC or PLEC), a further reduction of κl\kappa_{l} can also be achieved.[3, 7, 8, 9, 10, 11, 12, 13] In addition, the heterostructured TE materials have shown a promise for significant enhancement in ZTZT through (i) reduction of κtotal\kappa_{total} from enhanced phonon scattering and (ii) enhancement of SS from selective filtering of low energy charge carriers, simultaneously.[14] In literature, a ZT∼2.4ZT \sim2.4 has been reported in the thin film heterostructure of Bi2_{2}Te3_{3}/Sb2_{2}Te3_{3} through controlled manipulation of electrons and phonons.[15] A significant enhancement of the SS through low energy charge carrier filtering have been reported for Bi2_{2}Te3_{3}/Te heterostructured thin films.[16] However, all these heterostructured TE compounds are artificially grown or chemical modified, thus required expensive and tedious ways for large scale productions.

Owing to their layered crystal structure and high degree of anharmonicity, the ternary chalcogenides, such as Bi2Se2Te\mathrm{Bi_2Se_2Te}, Bi2Te2(Se/S)\mathrm{Bi_2Te_2(Se/S)}, Bi2GeTe4\mathrm{Bi_2GeTe_4}, Bi4PbTe7\mathrm{Bi_4PbTe_7}, Bi4SnTe7\mathrm{Bi_4SnTe_7}, and Pb2Bi2Se5\mathrm{Pb_2Bi_2Se_5} possesses ultralow κtotal\kappa_{\mathrm{total}}. [5, 17, 18]With the narrow band gaps and layered crystal structures, the family of (Bi/Sb)2(Te/Se/S)3(\mathrm{Bi/Sb})_2(\mathrm{Te/Se/S})_3 chalcogenides is known for the excellent TETE properties and first generation topological insulators (TITI) also. [1, 7] The exotic surface states are arising because of the involvement of SOC of heavier metal like Bi/Sb/Pb/Sn, and Te. [19, 20, 21, 22] In this regard, Bi4GeTe7\mathrm{Bi_4GeTe_7} is an important TETE as well as TITI material with inherent alternate repeating quintuplet-septuplet heterostructured crystal structure. While, the magneto transport studies show the presence of WALWAL (T≤5KT \le5\mathrm{K}) and supports possibility of topological surface states, the existence of high degree of crystal anharmonicity and large Grün­eisen parameter, γ∼4.07\gamma\sim4.07, leading to an ultralow value of κtotal∼0.42\kappa_{\mathrm{total}} \sim0.42 W m−1 K−1\mathrm{W\,m^{-1}\,K^{-1}} at 380 K. Our results provide subtle understanding of the structural aspects for Bi4GeTe7\mathrm{Bi_4GeTe_7} as a potential TETE material.

Polycrystalline Bi4GeTe7\mathrm{Bi_4GeTe_7} was grown by a solid-state melting route using high purity chunks of Bi (99.99 %), Ge (99.999%) and Te (99.99%) in the stoichiometric ratio. The vacuum sealed (∼10−5\sim10^{-5} mbar) quartz tube, with pure elements, was heated to ∼1123\sim1123 K for ∼24\sim24 h followed by water quenching. The obtained ingot was finely ground and pelletized into a ∼10\sim10 mm dia. pellet, which was further vacuum sealed and subjected to an annealing at ∼773\sim773 K for ∼100\sim100 h. The annealing was done to improve the consolidation and homogenization of the compound. The annealed pellet was cut into a rectangular bar (2×2×10 mm32 \times2 \times10\ \mathrm{mm^3}) for thermoelectric transport measurements.

Structural and phase analysis of the powder was carried out with a rotating anode Rigaku Smartlab X-ray diffractometer using CuKαCuK_{\alpha} radiation. High resolution transmission electron microscopy (HRTEM) was done using FEI make Tecnai G2 20 S-TWIN transmission electron microscope. Morphology and elemental mapping were identified using field-emission scanning electron microscopy (FESEM, Nova Nano SEM 450). Temperature dependent thermoelectric and magnetotransport properties were performed in a physical properties measurement system (PPMS, DynaCool, Quantum Design).

X-ray diffraction pattern of the finely ground powder of the annealed Bi4GeTe7\mathrm{Bi}_{4}\mathrm{Ge}\mathrm{Te}_{7} (Fig. 1(a)) have been indexed to Rhombohedral geometry (space group P3ˉm1P\bar{3}m1, 164).[23] Rietveld refinement confirms Bi4GeTe7\mathrm{Bi}_{4}\mathrm{Ge}\mathrm{Te}_{7} as the primary phase (∼96.5%\sim96.5\%) with the inherent Bi2GeTe4\mathrm{Bi}_{2}\mathrm{GeTe}_{4} is identified as the secondary phase (∼3.5%\sim3.5\%).[24] The observation of secondary phase is quite likely due to the shorter annealing time during the synthesis.[25, 26] The refined lattice parameters for Bi4GeTe7\mathrm{Bi}_{4}\mathrm{Ge}\mathrm{Te}_{7} are a=b=4.36a=b=4.36 Å and c=23.92c=23.92 Å and the corresponding unit cell volume, V∼393.64V\sim393.64 Å3^{3}.[27] A schematic in Fig. 1(b), depicts the natural arrangements of alternating quintuplets (TeI−Bi−TeII−Bi−TeI\mathrm{Te}^{\mathrm{I}}\mathrm{-Bi}\mathrm{-Te}^{\mathrm{II}}\mathrm{-Bi}\mathrm{-Te}^{\mathrm{I}}) and septuplets (TeI−Bi−TeII−Ge−TeII−Bi−TeI\mathrm{Te}^{\mathrm{I}}\mathrm{-Bi}\mathrm{-Te}^{\mathrm{II}}\mathrm{-Ge}\mathrm{-Te}^{\mathrm{II}}\mathrm{-Bi}\mathrm{-Te}^{\mathrm{I}}), which are separated by van der Waal gaps. The cross sectional HRTEM image in Fig. 1(c) clearly showcase the quintuplet-septuplet heterostructure arrangements in Bi4GeTe7\mathrm{Bi}_{4}\mathrm{GeTe}_{7}. The global layered nature and hierarchical layered stacking is shown in SEM image (Fig. 1(d)).[5, 13] Elemental mapping performed on polished surface of the pellet (Figure 2), suggests absence of isolated secondary phase of Bi2GeTe4\mathrm{Bi}_{2}\mathrm{GeTe}_{4} in Bi4GeTe7\mathrm{Bi}_{4}\mathrm{GeTe}_{7}.

FESEM image of top view of the pellet and elemental mapping

Figure 2. (a) FESEM image of top view of the pellet, and (b-f) the homogenous distribution of various elements observed in the mapping performed on polished surface of pellet.

The large unit cell Bi4GeTe7\mathrm{Bi}_{4}\mathrm{GeTe}_{7} is also a topological quantum material because of the presence of heavy elements like Bi and Te, which provides adequate spin-orbit-coupling for observation of signature metallic surface states in magnetotransport studies.[19] Hall analysis suggest electrons as the dominating charge carriers with a concentration, ne∼9.8×1019 cm−3n_e\sim9.8\times10^{19}\ \mathrm{cm}^{-3} at 300 K. The magnetoresistivity, ρxx(B)\rho_{xx}(B), is shown in Figure 3(a), where a sharp dip near the zero-field region providing a clue for SOC driven WAL, below 5K.[20, 28, 29, 30, 31] To understand further, we fitted the the magnetoconductivity data with Hikami-Larkin-Nagaoka (HLN) equation,

Magnetic field and temperature dependence of magnetoresistivity, magnetoconductivity, and thermopower

Figure 3. Magnetic field dependence of (a) longitudinal magnetoresistivity (ρxx\rho_{xx}), and (b) HLN fitted magnetoconductivity, and temperature dependence of (c) ρxx(T)\rho_{xx}(T), (d) S(T)S(T) and (Inset S2σS^{2}\sigma).

Δσ=σ(B)−σ(0)=−αe22π2ℏ[ln⁡(ℏ4eℓϕ2B)−ψ(12+ℏ4eℓϕ2B)]+cB2,\Delta\sigma=\sigma(B)-\sigma(0)=-\frac{\alpha e^{2}}{2\pi^{2}\hbar}\left[\ln\left(\frac{\hbar}{4e\ell_{\phi}^{2}B}\right)-\psi\left(\frac{1}{2}+\frac{\hbar}{4e\ell_{\phi}^{2}B}\right)\right]+cB^{2},

where ee is electronic charge, α\alpha is a dimensionless fitting parameter called prefactor, BB is applied magnetic field, lϕl_{\phi} is phase coherence length and Ψ\Psi represents digamma function.[32, 33] From the fitting (Figure 3(b)), the estimated phase coherence length lϕl_{\phi} decreases from ~ 161 nm (2.5 K) to ~ 67 nm (10 K), which suggest the inelastic scattering of electrons from phonons. Generally, single conducting surface channel correspond to the α∼−0.5\alpha\sim-0.5,[34] however a significant contribution of bulk conductivity reduces prefactor, α\alpha from ~ - 22 (at 2.5 K) to ~ - 0.11 (at 10 K). Thus, the observation of WAL provides an evidence of involvement of bulk as well as topological surface states in Bi4GeTe7\mathrm{Bi}_{4}\mathrm{Ge}\mathrm{Te}_{7}.

To understand the potential for TE applications, temperature dependence of the involved physical parameters, for ZT, have been studied in detail. The positive temperature coefficient of resistivity in ρxx(T)\rho_{xx}(T), indicates a metallic behavior or a narrow band gap degenerate nature of semiconductors, (Figure 3(c)), with a residual resistivity ratio (RRRRRR) of ~ 1.87.[13] A relatively higher ρxx\rho_{xx} for Bi4GeTe7\mathrm{Bi}_{4}\mathrm{Ge}\mathrm{Te}_{7}, in comparison with ternary chalcogenides shows a higher crystal complexity involved and an additional resistance to the electron flow in the material.[5, 35] The S(T)S(T), in Figure 3(d), further confirms the electron dominated charge transport with S∼−82S \sim-82 µV/K and correspondingly, the power factor (inset of Figure 3(d)), PF∼2.65×10−4PF \sim2.65 \times10^{-4} Wm−1^{-1}K−2^{-2} at 380 K, has been determined.

The κtotal\kappa_{\mathrm{total}} shows ultralow values, throughout the temperature range, with a κtotal∼0.42\kappa_{\mathrm{total}} \sim0.42 Wm−1^{-1}K−1^{-1} at 380 K (Figure 4(a)), which assures that Bi4GeTe7\mathrm{Bi}_{4}\mathrm{Ge}\mathrm{Te}_{7} has a potential for better TE material. The contribution of κe\kappa_e and κl\kappa_l in κtotal\kappa_{\mathrm{total}}, is estimated using the modified Wiedemann Franz law: κe=[1.5+exp⁡[−∣α∣116]]σT\kappa_e = \left[1.5 + \exp\left[-\frac{|\alpha|}{116}\right]\right]\sigma T.[5, 36] Thus κe∼0.29\kappa_e \sim0.29 Wm−1^{-1}K−1^{-1} and κl∼0.13\kappa_l \sim0.13 Wm−1^{-1}K−1^{-1}, at 380 K, are extracted from temperature dependence of the Lorenz number, LL as shown in the inset of Figure 4(a). Here the interesting crystal structure of Bi4GeTe7\mathrm{Bi}_{4}\mathrm{Ge}\mathrm{Te}_{7}, with quintuplet-septuplet heterostructure having van der Waal’s gaps, has sufficient hindrance for phonon propagation as reflected from the ultralow values of κl\kappa_l. The room temperature comparison of ultralow values of κl\kappa_l of various layered chalcogenides such as Bi2Te3\mathrm{Bi_2Te_3}, Bi2GeTe4\mathrm{Bi_2GeTe_4}, GeBi3SbTe7\mathrm{GeBi_3SbTe_7}, GeBi2Sb2Te7\mathrm{GeBi_2Sb_2Te_7}, GeBiSb3Te7\mathrm{GeBiSb_3Te_7} and Sb4GeTe7\mathrm{Sb_4GeTe_7} is shown in Figure 4(b), which showcases the importance of structural complexities of quintuplet-septuplet heterostructure in Bi4GeTe7\mathrm{Bi_4GeTe_7}. [5, 13, 35]

Temperature dependence and comparative thermal and thermoelectric properties

Figure 4. (a) Temperature dependence of κtotal\kappa_{\mathrm{total}}, κel\kappa_{\mathrm{el}}, κl\kappa_l, and inset shows L(T)L(T)), and (b) comparative graph for κtotal\kappa_{\mathrm{total}}, κel\kappa_{\mathrm{el}} and κl\kappa_l of various layered chalcogenides.[5, 13, 35] Temperature dependence of (c) CpC_p (Inset: Cp/TC_p/T vs T2T^2) and (d) ZTZT.

In TE materials, the higher crystalline anharmonicity drives phonon relaxation processes by damping the exchange of energy between thermal and mechanical vibrations, and thus resulting in ultralow κl\kappa_l. [5, 6, 37] In order to understand the origin of ultralow κl\kappa_l, the anharmonicity can be assessed from the heat capacity data by estimating the Debye temperature (θd\theta_d) and the Gruneisen parameter (γ\gamma), of the materials. The low temperature heat capacity (CpC_p) data is shown in Figure 4(c), and the linear fit (inset of Figure 4(c)), of Cp/T=A+BT2C_p/T = A + BT^2, [38] gives the characteristic constants AA (~ 1.81×10−3 J mol−1 K−21.81 \times10^{-3}\,\mathrm{J\,mol^{-1}\,K^{-2}}) related to electronic contributions and BB (~ 9.31×10−3 J mol−1 K−49.31 \times10^{-3}\,\mathrm{J\,mol^{-1}\,K^{-4}}) related to lattice contributions in Bi4GeTe7\mathrm{Bi_4GeTe_7}. The θd\theta_d ~ 135.7 K has been estimated using, θd=(12π4pR5B)1/3\theta_d = \left(\frac{12\pi^4 pR}{5B}\right)^{1/3}, where pp is the number of atoms per formula unit and RR is the molar gas constant. [17] The Grüneisen parameter, γ\gamma, is calculated using the relation: κl=PM‾δθd3γ2N2/3T\kappa_l = \frac{P\overline{M}\delta\theta_d^3}{\gamma^2N^{2/3}T}, where M‾\overline{M} is the averaged mass of atoms of the material, δ3\delta^3 is the volume per atom, NN represents the total number of atoms in the primitive unit cell and P=3.1×10−6P = 3.1 \times10^{-6} is a constant (the units of δ\delta is in Å, κl\kappa_l is in Wm−1K−1\mathrm{Wm^{-1}K^{-1}} and M‾\overline{M} is in amu). [5, 17, 39] Here, Bi4GeTe7\mathrm{Bi_4GeTe_7} possesses a high value of γ\gamma ~ 4.07 (at 380 K), which is better than champion Bi2Te3\mathrm{Bi_2Te_3} and comparable to the TE materials known for ultralow thermal conductivity, such as Bi2GeTe4\mathrm{Bi_2GeTe_4}, Ag8SnSe6\mathrm{Ag_8SnSe_6} and Ag8GeSe6\mathrm{Ag_8GeSe_6}. [3, 5] The low θd\theta_d and large γ\gamma signify that Bi4GeTe7\mathrm{Bi_4GeTe_7} has a high degree of anharmonicity. An additional insight on the nature of phonon propagation in Bi4GeTe7\mathrm{Bi_4GeTe_7} can be drawn from the calculation of average phonon velocity, (vavgv_{avg}). In general, materials with stiffer bonds tends to have higher vavgv_{avg} and hence higher κtotal\kappa_{total}, whereas smaller vavgv_{avg} corresponds to lower κtotal\kappa_{total}. For Bi4_4GeTe7_7, νavg∼1.49\nu_{avg} \sim1.49 km s−1^{-1}, has been estimated using the equation νavg=2πkBθd(6π2nv)1/3h\nu_{avg} = \frac{2\pi k_B\theta_d}{(6\pi^2 n_v)^{1/3}h}, where kBk_B and h represents Boltzmann constant and Planck’s constant, respectively, while nvn_v denotes number of atoms per unit volume of the material. The νavg\nu_{avg} for Bi4_4GeTe7_7 is considerably smaller when compared to ultralow κtotal\kappa_{total} materials such as Bi2_2GeTe4_4 (νavg∼1.54\nu_{avg} \sim1.54 km s−1^{-1}) and Bi2_2Te3_3 (νavg∼1.78\nu_{avg} \sim1.78 km s−1^{-1}).[5, 17] Therefore, intrinsically ultralow κtotal\kappa_{total} in Bi4_4GeTe7_7 can be understood as a result of anharmonicity arising due to large unit cell, intrinsic heterostructures, presence of heavy Bi atoms, large γ\gamma and small νavg\nu_{avg}. Furthermore, the calculated ZTZT at 380 K is ∼0.24\sim0.24 (Figure 4(d)), which is relatively higher than the similar ternary layered chalcogenides.[5, 35] The results establish that Bi4_4GeTe7_7 has potential for good TE Material. Moreover, other members of Bi based ternary layered chalcogenides with higher structural complexities such as (Bi/Pb)6_6GeTe10_{10}, (Bi/Pb)2_2GeTe5_5 and (Bi/Pb)2_2Ge3_3Te6_6 can be expected to show ultralow κtotal\kappa_{total} and host topological surface states which upon proper tuning of the electrical properties can be good TEs and TIs.

In summary, the structural aspects of Bi4_4GeTe7_7 has been discussed for its magneto transport, TE transport properties. Here, the possibility of topological surface states have been understood by the lϕ∼161l_{\phi} \sim161 nm (2.5 K) and an existence of WAL in magneto transport studies. With S∼−82S \sim-82 µV/K at 380 K, and ne∼9.8×1019n_e \sim9.8 \times10^{19} cm−3^{-3} at 300 K, the Bi4_4GeTe7_7 has an electron dominated charge transport like degenerate semiconductors. The intrinsic van der Waal heterostructure of quintuplet-septuplet layers provide a large anharmonicity and phonon scattering for an ultralow κl∼0.13\kappa_l \sim0.13 Wm−1^{-1}K−1^{-1} at 380 K. Hence, Bi4_4GeTe7_7 is an important topological quantum material and promising TE material with high γ∼4.07\gamma\sim4.07 and an overall ZT∼0.24ZT \sim0.24 at 380 K.

NKS would like to acknowledge CSIR-SRF and AK acknowledges SERB for providing the fellowship. AS would like to acknowledge DST-SERB (Grant No. CRG/2018/002197). Authors thank IIT Mandi for the research facilities.

Rietveld refinement, schematic hetero-structure, cross-sectional TEM image, and SEM image

Figure 1. (a) Rietveld refinement of powder XRD pattern, (b) Schematic of the quintuplet-septuplet hetero-structure with vdW gaps of Bi4GeTe7Bi_{4}GeTe_{7}, (c) cross-sectional TEM image showcasing the

Image not extracted

Figure 1 (PDF p. 12). stacked layers at atomic scales, and (d) FESEM image of fractured crystal showcasing global pictures of the layers.

References

  1. [1]D. M. Rowe, Thermoelectrics Handbook : Macro to Nano (CRC/Taylor & Francis, 2005).
  2. [2]P. Acharyya, T. Ghosh, K. Pal, K. Kundu, K. Singh Rana, J. Pandey, A. Soni, U. V. Waghmare and K. Biswas, Journal of the American Chemical Society 142 (36), 15595-15603 (2020).
  3. [3]S. Acharya, J. Pandey and A. Soni, ACS Applied Energy Materials 2 (1), 654-660 (2019).
  4. [4]J. Pandey, S. Mukherjee, D. Rawat, S. Athar, K. S. Rana, R. C. Mallik and A. Soni, ACS Applied Energy Materials 3 (3), 2175-2181 (2020).
  5. [5]N. K. Singh and A. Soni, Applied Physics Letters 117 (12), 123901 (2020).
  6. [6]J. P. Heremans, Nature Physics 11 (12), 990-991 (2015).
  7. [7]G. S. Nolas, J. Sharp and H. J. Goldsmid, Thermoelectrics: Basic Principles and New Materials Developments. (Springer, 2001).
  8. [8]M. G. Kanatzidis, Chem Mater 22 (3), 648-659 (2010).
  9. [9]S. Bathula, M. Jayasimhadri, B. Gahtori, N. K. Singh, K. Tyagi, A. K. Srivastava and A. Dhar, Nanoscale 7 (29), 12474-12483 (2015).
  10. [10]A. Soni, Y. Shen, M. Yin, Y. Zhao, L. Yu, X. Hu, Z. Dong, K. A. Khor, M. S. Dresselhaus and Q. Xiong, Nano Letters 12 (8), 4305 (2012).
  11. [11]A. Soni, Z. Yanyuan, Y. Ligen, M. K. K. Aik, M. S. Dresselhaus and Q. Xiong, Nano Letters 12 (3), 1203 (2012).
  12. [12]N. K. Singh, S. Bathula, B. Gahtori, K. Tyagi, D.Haranath and A. Dhar, Journal of Alloys and Compounds 668, 152-158 (2016).
  13. [13]N. K. Singh, J. Pandey, S. Acharya and A. Soni, Journal of Alloys and Compounds 746, 350-355 (2018).
  14. [14]Y. Zhang and G. D. Stucky, Chem Mater 26 (1), 837-848 (2014).
  15. [15]R. Venkatasubramanian, E. Siivola, T. Colpitts and B. O'Quinn, Nature 413 (6856), 597-602 (2001).
  16. [16]H.-J. Shang, F.-Z. Ding, Y. Deng, H. Zhang, Z.-B. Dong, W.-J. Xu, D.-X. Huang, H.-W. Gu and Z.-G. Chen, Nanoscale 10 (43), 20189-20195 (2018).
  17. [17]Q. Guo, J.-B. Vaney, R. Virtudazo, R. Minami, Y. Michiue, Y. Yamabe-Mitarai and T. Mori, Inorganic Chemistry 57 (9), 5258-5266 (2018).
  18. [18]C. Shekhar, C. E. ViolBarbosa, B. Yan, S. Ouardi, W. Schnelle, G. H. Fecher and C. Felser, Physical Review B 90 (16), 165140 (2014).
  19. [19]C. Fu, Y. Sun and C. Felser, Apl Mater 8 (4), 040913 (2020).
  20. [20]M. Neupane, S.-Y. Xu, L. A. Wray, Petersen, R. Shankar, N. Alidoust, Chang Liu, A. Fedorov, H. Ji, J. M. Allred, Y. S. Hor, T.-R. Chang, H.-T. Jeng, H. Lin, A. Bansil, R. J. Cava and a. M. Z. Hasan, Physical Review B 85, 235406 (2012).
  21. [21]E. Papalazarou, L. Khalil, M. Caputo, L. Perfetti, N. Nilforoushan, H. Deng, Z. Chen, S. Zhao, A. Taleb-Ibrahimi, M. Konczykowski, A. Hruban, A. Wołos, A. Materna, L. Krusin-Elbaum and M. Marsi, Physical Review Materials 2 (10), 104202 (2018).
  22. [22]V. L. Kuznetsov, L. A. Kuznetsova and D. M. Rowe, Journal of Physics D: Applied Physics 34 (5), 700 (2001).
  23. [23]V. L. Kuznetsov, L. A. Kuznetsova and D. M. Rowe, Journal of Applied Physics 85 (6), 3207-3210 (1999).
  24. [24]J. Rodríguez-Carvajal, Physica B: Condensed Matter 192 (1), 55-69 (1993).
  25. [25]L. A. Kuznetsova, V. L. Kuznetsov and D. M. Rowe, Journal of Physics and Chemistry of Solids 61 (8), 1269-1274 (2000).
  26. [26]P. P. Konstantinov, L. E. Shelimova, E. S. Avilov, M. A. Kretova and J. P. Fleurial, Journal of Solid State Chemistry 146 (2), 305-312 (1999).
  27. [27]O. G. Karpinsky, L. E. Shelimova, M. A. Kretova and J. P. Fleurial, Journal of Alloys and Compounds 265 (1), 170-175 (1998).
  28. [28]J. Chen, X. Y. He, K. H. Wu, Z. Q. Ji, L. Lu, J. R. Shi, J. H. Smet and Y. Q. Li, Physical Review B 83 (24), 241304 (2011).
  29. [29]S.-P. Chiu and J.-J. Lin, Physical Review B 87 (3), 035122 (2013).
  30. [30]L. Fu, C. L. Kane and E. J. Mele, Physical Review Letters 98 (10), 106803 (2007).
  31. [31]B. Bhattacharyya, B. Singh, R. P. Aloysius, R. Yadav, C. Su, H. Lin, S. Auluck, A. Gupta, T. D. Senguttuvan and S. Husale, Scientific Reports 9 (1), 7836 (2019).
  32. [32]S. Hikami, A. I. Larkin and Y. Nagaoka, Progress of Theoretical Physics 63 (2), 707-710 (1980).
  33. [33]N. K. Singh, D. Rawat, D. Dey, A. Elsukova, P. O. Å. Persson, P. Eklund, A. Taraphder and A. Soni, arXiv:2110.06587 [cond-mat.mtrl-sci] (2021).DOI
  34. [34]P. Sahu, J.-Y. Chen, J. C. Myers and J.-P. Wang, Applied Physics Letters 112 (12), 122402 (2018).
  35. [35]F. von Rohr, A. Schilling and R. J. Cava, Journal of Physics: Condensed Matter 25 (7), 075804 (2013).
  36. [36]H. S. Kim, Z. M. Gibbs, Y. L. Tang, H. Wang and G. J. Snyder, Apl Mater 3 (4), 041506 (2015).
  37. [37]C. W. Li, J. Hong, A. F. May, D. Bansal, S. Chi, T. Hong, G. Ehlers and O. Delaire, Nature Physics 11 (12), 1063-1069 (2015).
  38. [38]E. S. R. Gopal, Specific Heats at Low Temperatures. (Plenum Press, 1966).DOI
  39. [39]D. Bessas, I. Sergueev, H. C. Wille, J. Perßon, D. Ebling and R. P. Hermann, Physical Review B 86 (22), 224301 (2012).

Paper details

vlnc:W_k59svret
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 2

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents