betaFeedback

WorksPhysics and Astronomy

Oxygens breathe, electrons jump

Abstract

Electronic transport in polyanionic battery cathodes proceeds through small-polaron hopping between transition-metal sites and is commonly assumed to be tightly coupled to the motion of charge-compensating mobile ions. Using olivine Lix_xMnPO4_4 as a prototypical platform, we use first-principles molecular dynamics with extended Hubbard functionals to follow, in real time and at finite temperature, the adiabatic evolution of Mn oxidation states and atomic sublattices. We find that polaron hopping and cation migration are dynamically decoupled: Mn2+^{2+}/Mn3+^{3+} valence exchanges occur frequently while the intercalated ions remain confined to their sites, and hopping is gated by the local oxygen framework. Freezing the six oxygen atoms of an individual MnO6_6 octahedron excludes that site from the hopping network, while increasing the fictitious oxygen mass slows down electronic transport. Each valence exchange coincides with a concerted breathing of the donor and acceptor octahedra (ΔV≃2ΔV \simeq 2 A˚3Å^3), with their volume asymmetry crossing zero at the transition, consistent with the Holstein-Marcus coincidence condition. The hopping rate yields an activation energy of Ea=0.20±0.03E_a = 0.20 \pm 0.03 eV, closely matching the elastic energy scale of the two coordination cages (λV/4≈0.20λ_V/4 \approx 0.20 eV). These results identify the oxygen coordination cage, not the mobile cation sublattice, as the dynamical gate for small-polaron transport: a site can accept the electron only if its cage can breathe, and the barrier is governed by cage elasticity. Selective constraints and mass scaling applied to first-principles dynamics provide a general route to link electronic and lattice degrees of freedom in redox-active materials, opening the door to framework engineering in intercalation and mixed ionic-electronic conductors.

Introduction

The concept of oxidation state (OS) is ubiquitous in physics and chemistry [1], and its evolution in time underlies the functioning of rechargeable batteries, in which redox reactions on the transition-metal (TM) ions of the cathode accompany the insertion and removal of lithium. Olivine phosphates LiMPO4\mathrm{Li}M\mathrm{PO}_{4} (M=Fe,MnM = \mathrm{Fe}, \mathrm{Mn}) are prototypical intercalation cathodes [2, 3]: their strong P–O covalent bonds confer thermal and chemical stability, and LiMnPO4\mathrm{LiMnPO}_{4} is particularly attractive because of its higher redox potential (∼\sim4.1 V vs Li/Li+^{+}) compared with LiFePO4\mathrm{LiFePO}_{4} [2, 4]. Its practical use, however, has long been hampered by sluggish kinetics, which have been ascribed to an extremely low intrinsic electronic conductivity, lower than that of LiFePO4\mathrm{LiFePO}_{4} by several orders of magnitude [4, 5], combined with one-dimensional lithium diffusion along the bb channels [6, 7].

In olivines, the extra electrons (or holes) introduced upon (de)lithiation do not delocalize in a band but self-trap on individual TM sites, together with a local distortion of the surrounding oxygen cage, forming small polarons [8, 9, 10, 11]. Electronic transport then occurs through thermally activated hops between neighbouring TM sites [9, 12]. A central and still debated question is the extent to which these hops are coupled to the motion of the charge-compensating Li+\mathrm{Li}^{+} ions. Static first-principles calculations at zero temperature predict a sizeable electrostatic binding between polarons and Li ions or vacancies [13, 14], which raises the calculated hopping barrier of a bound polaron with respect to a free one [14]; on the other hand, Mössbauer spectroscopy on LixFePO4\mathrm{Li}_{x}\mathrm{FePO}_{4} solid solutions has been interpreted in terms of coupled lithium-ion and electron mobility [15]. In this coupled picture, the Li sublattice would effectively control electronic transport, and the polaron and the Li ion would migrate as a correlated pair.

Static calculations, such as nudged-elastic-band estimates of hopping barriers along predefined pathways [13, 14, 16], cannot by themselves resolve whether this binding governs finite-temperature transport. What is required is a description in which electrons, lithium ions and the oxygen framework evolve dynamically together at finite temperature, and in which the OS of every TM ion can be followed unambiguously in time. First-principles molecular dynamics (FPMD) [17] offers such a description, provided the electronic-structure method localizes the excess charges correctly. Standard (semi)local functionals fail in this respect because of self-interaction errors, delocalizing the extra electrons over all TM sites and producing “unchemical” fractional OSs [18, 19]. Hybrid functionals [20] correct this, but are typically unaffordable for FPMD simulations long enough to yield meaningful statistics. Extended Hubbard functionals (DFT +U+V+ U + V) [21], with on-site UU and inter-site VV parameters computed from first principles [22, 23, 24], provide accurate electronic structures and intercalation voltages for olivines [18, 25], and DFT +U+V+ U + V-FPMD captures sharp, “digital” changes of the Mn OS during the adiabatic dynamics of LixMnPO4\mathrm{Li}_{x}\mathrm{MnPO}_{4} [19].

Here, we exploit this capability to analyze the microscopic mechanism of polaron hopping in LixMnPO4\mathrm{Li}_{x}\mathrm{MnPO}_{4}. By combining unconstrained and selectively constrained FPMD, fictitious isotope substitution, analysis of the electron–lattice coupling and the temperature dependence of the hopping rate, we show that (i) polaron hopping is dynamically decoupled from lithium motion, proceeding on timescales much shorter than those of lithium migration, (ii) it is gated by the local oxygen cage of each Mn site, (iii) the donor–acceptor volume asymmetry crosses zero at the instant of transfer through a geometrically symmetric coincidence transition state, and (iv) the resulting activation energy (Ea=0.20±0.03E_{\mathrm{a}} = 0.20 \pm0.03 eV) is quantitatively consistent with the elastic reorganization energy of two breathing cages (∼0.20\sim0.20 eV) and matches the barrier of a free electron polaron. The oxygen framework thus emerges as the controlling degree of freedom for electronic transport in these polyanionic cathodes.

Results

Following oxidation states in time

In LixMnPO4\mathrm{Li}_{x}\mathrm{MnPO}_{4} (orthorhombic, space group PnmaPnma), each Mn ion sits at the centre of a distorted MnO6\mathrm{MnO}_{6} octahedron; the octahedra share corners in the bcbc plane and are linked by PO4\mathrm{PO}_{4} tetrahedra, while Li+\mathrm{Li}^{+} ions occupy one-dimensional channels along bb [2, 6]. Each Li inserted in MnPO4\mathrm{MnPO}_{4} brings one Li+\mathrm{Li}^{+} ion and one electron, which reduces one Mn3+\mathrm{Mn}^{3+} ion to Mn2+\mathrm{Mn}^{2+}. Following the approach of Ref. 26, we determine the OS of each Mn from the eigenvalues of its 3d3d occupation matrix, and use as a compact descriptor the Löwdin occupation nn, i.e. the sum of the 3d3d occupation eigenvalues in both spin channels [19, 27]. We emphasize that nn is a hybridized Löwdin occupation: the contrast of Δn≈0.20 e\Delta n \approx0.20\ e between Mn3+^{3+} (n≃5.00n \simeq5.00) and Mn2+^{2+} (n≃5.20n \simeq5.20) in DFT +U+V+ U + V [19] reflects covalent hybridization with coordinating oxygen 2p2p states, while the integer change in oxidation state is unambiguously defined by the occupation-matrix eigenvalues [19, 26]. Thermal motion makes nn fluctuate around these two values; we therefore define two intervals, n<5.05n < 5.05 (Mn3+^{3+}) and n>5.15n > 5.15 (Mn2+^{2+}), separated by a hysteresis band that suppresses spurious recrossings, and count an OS change (“hop”) only when the occupation enters the opposite interval and remains there for at least a dwell time tdwellt_{\mathrm{dwell}} (Methods). We underscore that the transitions observed in DFT +U+V+ U + V-FPMD are adiabatic changes of the electronic ground state driven by the evolving atomic configuration [19]; we do not attempt to describe non-adiabatic tunnelling [28, 29], which would take place on the same configurations but with an electronically reduced transmission probability.

Polaron hopping proceeds while lithium stays put

Figure 1 shows a 10 ps DFT +U+V+ U + V-FPMD trajectory of Li0.5_{0.5}MnPO4_4 at T=900T = 900 K, in a unit cell of 26 atoms containing two Li+^+ ions and two extra electrons. The two Li ions (Figure 1a) never leave their sites: their displacements ∣ΔR(t)∣=∣R(t)−R(0)∣|\Delta\mathbf{R}(t)| = |\mathbf{R}(t) - \mathbf{R}(0)| remain below 1 Å (with a single transient excursion below 2 Å), far from the distance between nearest-neighbour Li sites, dLi−Li=3.03d_{\mathrm{Li-Li}} = 3.03 Å. Over the same time window, the Löwdin occupations of the four Mn sites (Figure 1b) switch repeatedly and sharply between the Mn3+^{3+} and Mn2+^{2+} basins, with electrons always conserved (two Mn2+^{2+} and two Mn3+^{3+} at any time outside the short transition windows). Polaron hopping is therefore active on the picosecond timescale even when the Li sublattice is completely static (i.e., oscillating at equilibrium and not hopping). The high temperature is chosen to obtain sufficient hopping statistics within a single trajectory. On the full 38 ps of this run the two Li ions perform only three site changes, and none occurs in the 600 and 700 K trajectories used below (32.7 and 41.7 ps), whereas the polaron keeps hopping at all temperatures. Hence, the hopping does not require Li migration.

Figure 1. Decoupling of lithium motion and small-polaron dynamics in Li0.5_{0.5}MnPO4_4. a, Displacements ∣R(t)−R(0)∣|\mathbf{R}(t) - \mathbf{R}(0)| of the two Li+^+ ions (Li1_1, Li2_2) during a 10 ps DFT +U+V+ U + V-FPMD trajectory at T=900T = 900 K (unit cell of 26 atoms, with two Li+^+ ions and two extra electrons). Faint lines: raw data; solid lines: 0.1 ps running average. The dashed line marks the distance between nearest-neighbour Li sites, dLi−Li=3.03d_{\mathrm{Li-Li}} = 3.03 Å. Both ions only vibrate within their sites. b, Löwdin 3d occupations of the four Mn sites over the same time window (δt=4\delta t = 4 fs). Shaded bands indicate the Mn2+^{2+} (n>5.15n > 5.15) and Mn3+^{3+} (n<5.05n < 5.05) basins, dashed lines the corresponding thresholds. Faint lines: raw data; solid lines: median filter over a 20 fs (5-frame) window. The Mn oxidation states change continuously through polaron hops while the Li sublattice is static.

To test whether the polaron is pinned to the Li+^+ ion, we analysed two trajectories with a single Li+^+ ion and a single polaron at 900 K: the Li0.25_{0.25}MnPO4_4 unit cell of 25 atoms (27.8 ps) and a 1×1×21 \times1 \times2 Li1/8_{1/8}MnPO4_4 supercell of 49 atoms (33.3 ps). For every Mn site we evaluated the distribution of instantaneous Li–Mn distances under the minimum-image convention (MIC, i.e., taking the shortest distance across periodic–boundary conditions), separately for the frames in which that site is Mn2+^{2+} and for those in which it is Mn3+^{3+}. In the unit cell (Supplementary Fig. S1), the Li+^+ ion jumps six times between nearest-neighbour Li sites. Every Mn site lies within the first coordination shell of the Li (2.35–4.73 Å), and both oxidation states occupy the full distance range at every site. The supercell (Figure 2) adds two Mn sites (Mn4, Mn6) at ≈5.5 Å from the Li, the second-shell distance at which static calculations place the largest part of the Li+^+–polaron binding [13]. The polaron also visits these sites, and their Mn2+^{2+} and Mn3+^{3+} distributions overlap. This already holds in the first 11.5 ps, before the Li+^+ ion leaves its initial site (shaded window in Figure 2a; dashed profiles in Figure 2b): during this stage the polaron visits all eight Mn sites, including Mn4 and Mn6.

Figure 2. Li migration and polaron hopping in the Li1/8_{1/8}MnPO4_4 supercell at 900 K. 1 × 1 × 2 supercell (49 atoms: 8 Mn, 8 P, 32 O, 1 Li; a×b×c≈9.94×6.03×9.63a \times b \times c \approx9.94 \times6.03 \times9.63 Å) with one Li+^+ ion and one polaron, 33.3 ps (8,314 frames, δt=4\delta t = 4 fs). a, Displacement of the Li+^+ ion. The plateaus at ≈\approx0, 3.1 and 6.0 Å correspond to two successive jumps between nearest-neighbour Li sites (≈\approx3 Å each). The shaded window (t≤11.5t \le11.5 ps) marks the pre-diffusion stage, before the first Li jump. Faint line: raw data; solid line: 100 fs running average. b, Split-violin distributions of the instantaneous Li–Mn distance under the minimum-image convention (MIC, range 2.41–6.21 Å) for each Mn site, conditioned on the oxidation state of that site: Mn2+^{2+} (orange, n>5.137n > 5.137) and Mn3+^{3+} (blue, n<5.035n < 5.035), with thresholds set by the same convention as in the unit cell (Methods). Filled violins: full trajectory; dashed lines: contribution of the pre-diffusion stage (dark red, Mn2+^{2+}; dark blue, Mn3+^{3+}), scaled by its share of the frames. Grey bands: second-shell sites (Mn4, Mn6). Horizontal dashed line: largest Li–Mn MIC distance in the unit cell (4.73 Å; Supplementary Fig. S1).

The local oxygen cage gates the hopping

The results above show that Li motion is not required for polaron hopping; we now ask which degrees of freedom are required. To this end we performed two FPMD simulations, at T=900T = 900 K and for 13.46 ps each, of a 1×1×21 \times1 \times2 supercell (49 atoms: eight Mn, eight P, 32 O and one Li, i.e. Li1/8_{1/8}MnPO4_4 with a single polaron). In the first, all atoms are free; in the second, the six oxygen atoms forming the octahedron of one Mn site (Mn2) are frozen at their initial positions, while all other atoms, including Mn2 itself, evolve freely (Methods).

In the unconstrained run (Figure 3a,Figure 3c), the Li+^+ ion vibrates within its site for ∼11.4\sim11.4 ps before performing a single jump; during the quiescent window highlighted in Figure 3 (6.0–10.4 ps), the polaron hops continuously among all eight Mn sites, including Mn2. Over the whole trajectory we count 154 OS transitions (tdwell≥12t_{\mathrm{dwell}} \ge12 fs), i.e. 77 polaron hops, with Mn2 participating in 25 of them. When the Mn2_2O6_6 cage is frozen (Figure 3b,Figure 3d), Mn2 remains Mn3+^{3+} throughout the entire trajectory, with zero transitions and strongly reduced occupation fluctuations, whereas the polaron keeps hopping among the other seven sites; the total number of transitions (146) is essentially unchanged. Freezing a single coordination cage is therefore sufficient to remove the corresponding site from the hopping network, without perturbing hopping elsewhere.

Figure 3. Site-selective freezing of the oxygen cage. DFT +U+V+ U + V-FPMD of Li1/8_{1/8}MnPO4_4 (1×1×21 \times1 \times2 supercell, 49 atoms: 8 Mn, 8 P, 32 O, 1 Li; a×b×c≈9.94×6.03×9.63a \times b \times c \approx9.94 \times6.03 \times9.63 Å, one Li+^+ ion and one polaron) at T=900T = 900 K, 13.46 ps, δt=4\delta t = 4 fs. a, Li+^+ displacement with all atoms free (faint: raw data; solid: 0.4 ps running average). The Li ion vibrates within its site until t≈11.4t \approx11.4 ps, when it jumps to a neighbouring site. The grey band (6.0–10.4 ps) marks the window shown in c and d. b, Same as a with the six oxygen atoms of the Mn2_2O6_6 octahedron frozen at their initial positions. c, Löwdin occupations of the eight Mn sites with all atoms free, in the window 6.0–10.4 ps. Blue and red bands indicate the Mn3+^{3+} and Mn2+^{2+} basins. The polaron hops among all sites, including Mn2 (framed). d, Same as c with the Mn2_2O6_6 cage frozen: Mn2 (framed) remains Mn3+^{3+} for the entire trajectory, while hopping continues among the other seven sites at an unchanged overall rate.

Because the frozen cage retains the geometry of the initial Mn3+^{3+} configuration (V≈11.2V \approx11.2 Å3^3), this result demonstrates that a site can host the polaron only if its oxygen cage can expand to accommodate the larger Mn2+^{2+} ion (V≈13.0V \approx13.0 Å3^3, see below). Freezing a cage in the expanded Mn2+^{2+} geometry would be the complementary test; we expect it to stabilize the polaron on that site and suppress hopping away from it, since the coincidence condition could then be met only through large expansions of a neighbouring cage. We note that the Li ion did not jump in the constrained run; given that only a single jump was observed in the unconstrained one, we refrain from drawing conclusions on Li mobility from this comparison.

A complementary probe of the role of the oxygen framework is provided by fictitious isotope substitution. In classical molecular dynamics on an electronic Born–Oppenheimer potential energy surface, altering the atomic masses leaves the potential energy landscape and all static activation barriers strictly invariant; any variation in the hopping rate thus isolates the purely dynamical effect of framework inertia. We note that this classical dynamical effect is physically distinct from the quantum polaronic isotope effect observed in perovskite manganites [30], where oxygen substitution (16^{16}O →\to 18^{18}O) renormalizes the electronic bandwidth and polaronic binding through zero-point lattice fluctuations. Here we isolate framework inertia by setting the fictitious oxygen mass mOm_{\mathrm{O}} to 19 (F), 32 (S) and 79 u (Se).

Figure 4a shows the polaron hopping rate ⟨Γ⟩\langle\Gamma\rangle for Li0.5_{0.5}MnPO4_4 at 900 K (trajectories of 26.0–38.0 ps). The rate at mO=19m_{\mathrm{O}} = 19 u (1.68 ± 0.18 ps−1^{-1}) is comparable within statistical uncertainty to that at 16 u (1.49 ± 0.14 ps−1^{-1}), whereas heavier oxygen masses lower it, down to 1.08 ± 0.14 ps−1^{-1} at 79 u, a reduction of ∼25–35%. At 79 u all four Mn sites hop more slowly than at 16 and 19 u, and the decrease is found for all dwell-time criteria (Figure 4b), excluding artefacts of the counting procedure. Figure 4 thus indicates that polaron hopping kinetics is slowed down by the inertia of the oxygen framework.

Figure 4. Fictitious oxygen-isotope effect on polaron hopping. DFT + U+VU + V-FPMD of Li0.5_{0.5}MnPO4_4 (unit cell, 26 atoms: 4 Mn, 4 P, 16 O, 2 Li; a×b×c≈10.15×6.07×4.81a \times b \times c \approx10.15 \times6.07 \times4.81 Å) at T=900T = 900 K with oxygen mass mO=16m_{\mathrm{O}} = 16 (O), 19 (F), 32 (S) and 79 u (Se), on an unchanged Born–Oppenheimer potential-energy surface (trajectories of 26.0–38.0 ps, δt=4\delta t = 4 fs). a, Polaron hopping rate as a function of mOm_{\mathrm{O}}. Large symbols: four-site average ⟨Γ⟩=14∑iNi/ttot\langle\Gamma\rangle= \frac{1}{4}\sum_i N_i/t_{\mathrm{tot}} (tdwell≥12t_{\mathrm{dwell}} \ge12 fs), with Poisson uncertainties ⟨Γ⟩/Nhop\langle\Gamma\rangle/\sqrt{N_{\mathrm{hop}}}, where Nhop=Ntot/2N_{\mathrm{hop}} = N_{\mathrm{tot}}/2 is the number of hops; small symbols: individual Mn sites. b, Hopping rate ⟨Γ⟩\langle\Gamma\rangle evaluated for dwell-time thresholds tdwell≥4t_{\mathrm{dwell}} \ge4, 8 and 12 fs.

Concerted electron–lattice dynamics and Marcus coincidence

Figure 5 resolves individual hopping events in Li0.25_{0.25}MnPO4_4 at 900 K. The overview heatmaps (Figure 5a) show that the Mn OS pattern (top) is mirrored by the MnO6_6 octahedral volumes (middle), whereas no corresponding pattern is visible in the Li–Mn distances (bottom). The zooms on two representative events (Figure 5b,Figure 5c) display the anatomy of a hop: within a few tens of femtoseconds, the occupation of the donor site drops from ∼5.18 to ∼5.00 while that of the acceptor rises from ∼5.00 to ∼5.18; at the same time, the donor octahedron contracts and the acceptor octahedron expands by ∼2 Å3^3, while the Li–Mn distances remain essentially unaffected. Adiabatic electron

Figure 5. Structural fingerprint of polaron hops in Li0.25_{0.25}MnPO4_4 at T=900T = 900 K. Unit cell, 25 atoms: 4 Mn, 4 P, 16 O, 1 Li; a×b×c≈9.93×6.04×4.84a \times b \times c \approx9.93 \times6.04 \times4.84 Å, one Li+^+ ion and one polaron. a, Heatmaps over 8 ps of the Mn Löwdin occupations (top), MnO6_6 octahedral volumes from convex-hull tessellation (middle) and Li–Mn distances (minimum-image convention; bottom). Shaded windows mark the two events shown in b and c. b, Zoom on jump 1 (t=0.08t = 0.08–0.340.34 ps): Löwdin occupations of the four Mn sites (left), with the polaron transferred from Mn4 to Mn1, octahedral volumes (centre) and Li–Mn distances (right). c, Same for jump 2 (t=1.36t = 1.36–1.561.56 ps), with the polaron transferred from Mn3 to Mn4. In both events the donor cage contracts and the acceptor cage expands by ∼2\sim2 Å3^3 in step with the electronic transition, while the Li–Mn distances do not change appreciably.

transfer and cage breathing thus occur as a single concerted event, involving the donor–acceptor pair of octahedra; of course, the matrix element between diabatic states [29, 31] would ultimately renormalize the reaction rate and forbid long-distance tunnelling.

This concerted behaviour is quantified in Figure 6 for Li0.5_{0.5}MnPO4_4 at 900 K (6 ps, 1,500 frames). The instantaneous octahedral volume and the Löwdin occupation are strongly correlated on every site (Pearson r=0.77r = 0.77–0.79; Figure 6a), with average volumes of ∼11.2\sim11.2 Å3^3 for Mn3+^{3+} and ∼13.0\sim13.0 Å3^3 for Mn2+^{2+}; the larger, Jahn–Teller-inactive high-spin Mn2+^{2+} ion requires a larger and more regular cage than the Jahn–Teller-active Mn3+^{3+} [32]. The normalized cross-correlation C(τ)C(\tau) between the two time series (Figure 6b) peaks within ±8\pm8 fs (two time steps) of zero lag for all sites, with C(0)C(0) within 0.002 of the maximum; on the timescale of cage reorganization (Figure 6e) the lag between the two series is therefore zero within resolution.

Figure 6. Concerted electron–lattice dynamics and Holstein–Marcus coincidence in Li0.5_{0.5}MnPO4_4 at T=900T = 900 K. Unit cell, 26 atoms: 4 Mn, 4 P, 16 O, 2 Li; a×b×c≈10.15×6.07×4.81a \times b \times c \approx10.15 \times6.07 \times4.81 Å, two Li+^+ ions and two polarons. a, MnO6_6 volume versus Löwdin occupation for the four Mn sites (6 ps, 1,500 frames), showing bimodal clustering for Mn3+^{3+} (blue) and Mn2+^{2+} (orange) and linear regression fits (dashed black lines, Pearson r=0.77r = 0.77–0.790.79). b, Normalized cross-correlation C(τ)C(\tau) between volume and occupation; the maximum (red dot) lies within ±8 fs of τ=0\tau= 0 for all sites, with C(0)C(0) within 0.002 of the peak value, confirming that octahedral breathing tracks the electronic state without appreciable phase lag. c, Hop-aligned donor (VDV_D) and acceptor (VAV_A) octahedral volumes over [−150, +150] fs (δt=0.5\delta t = 0.5 fs resolution, N=16N = 16 hops), crossing at the transition-state volume V‡≈12.12V^{\ddagger} \approx12.12 Å3^3 at t=0t = 0. d, Event-averaged cage volume asymmetry ΔV(t)=VD(t)−VA(t)\Delta V(t) = V_D(t) - V_A(t) approaching zero near the electronic switch (ΔV(0)=−0.11±0.15\Delta V(0) = -0.11 \pm0.15 Å3^3, mean ± standard error over N=16N = 16 hops; shaded band: ±1σ\sigma, σ=0.61\sigma= 0.61 Å3^3), consistent with the Holstein–Marcus coincidence condition. e, Simultaneous electronic transfer: Löwdin occupation difference Δn(t)=nD−nA\Delta n(t) = n_D - n_A (dotted line; Δn=0\Delta n = 0 defines t=0t = 0) and bond-valence sum mismatch ΔBVS(t)=BVSD−BVSA\Delta\mathrm{BVS}(t) = \mathrm{BVS}_D - \mathrm{BVS}_A (dashed line) crossing zero at t=0t = 0.

In Born–Oppenheimer dynamics, the electronic ground state is an instantaneous functional of the nuclear coordinates. Therefore, a vanishing phase lag between n(t)n(t) and V(t)V(t) is physically expected for any structural descriptor that captures the reaction coordinate; its significance is that the MnO6_6 octahedral volume, and even more closely the bond-valence sum (Supplementary Figure S2–S4), directly tracks the electronic coordinate rather than a delayed structural relaxation (i.e., when the oxygens breathe, the electron jumps). To test the microscopic transfer mechanism, we aligned all transitions at the instant of electron transfer and averaged them over a trajectory with a shorter time step (δt=0.5\delta t = 0.5 fs, 10,216 frames, 5.11 ps; Figure 6c–Figure 6e). Aligning the trajectories at the transfer time (t=0t = 0), the donor and acceptor cage volumes VD(t)V_{\mathrm{D}}(t) and VA(t)V_{\mathrm{A}}(t) evolve symmetrically towards each other, crossing at a transition-state volume V‡≈12.12V^{\ddagger} \approx12.12 Å3^3 midway between the Mn3+^{3+} and Mn2+^{2+} cages (Figure 6c). The donor–acceptor volume asymmetry coordinate:

Figure S2. Octahedral volume versus Löwdin occupation at δt=0.5\delta t = 0.5 fs. Li0.5_{0.5}MnPO4_4 at T=900T = 900 K, unit cell, 26 atoms: 4 Mn, 4 P, 16 O, 2 Li; a×b×c≈10.15×6.07×4.81a \times b \times c \approx10.15 \times6.07 \times4.81 Å. a, Scatter plots for the four Mn sites (r=0.82r = 0.82, 0.770.77, 0.770.77, 0.820.82; ⟨r⟩≃0.80\langle r \rangle\simeq0.80). b, Cross-correlations CV,n(τ)C_{V,n}(\tau): the maxima lie at +2.5+2.5, 0.00.0, −7.0-7.0 and −2.5-2.5 fs for Mn1–Mn4 (site average −1.75-1.75 fs), with C(0)C(0) differing from Cmax⁡C_{\max} by at most 0.0050.005. Peak positions are read on the 0.50.5 fs time grid; a parabolic interpolation shifts them by less than 0.30.3 fs.

ΔV(t)=VD(t)−VA(t)(1)\Delta V(t) = V_{\mathrm{D}}(t) - V_{\mathrm{A}}(t) \tag*{(1)}

approaches zero near the electronic switch (ΔV(0)=−0.11±0.15\Delta V(0) = -0.11 \pm0.15 Å3^{3}, averaged over N=16N = 16 hops; Figure 6d). In the event average, the donor and acceptor cage volumes become nearly equal near the electronic switch, consistent with a predominantly breathing reaction coordinate and the Holstein–Marcus coincidence condition[8, 33], with the two cages reorganizing concertedly. While the electronic occupation crossing (Δn(0)=0\Delta n(0) = 0) defines the temporal origin t=0t = 0, the crucial physical finding is the simultaneous vanishing of the purely geometric asymmetries ΔV(0)=−0.11±0.15\Delta V(0) = -0.11 \pm0.15 Å3^{3} and ΔBVS(0)≈0\Delta\mathrm{BVS}(0) \approx0, accompanied by the strictly symmetric, ∼±50\sim\pm50 fs concerted reorganization of both cages around the transfer (Figure 6e). This shows that the electron transfers through a geometrically symmetric configuration, consistent with the coincidence state required for adiabatic polaronic transport. In the language of Marcus theory, the hop takes place where the diabatic free-energy curves of the electron localized on donor and acceptor cross; the electronic coupling between the two sites splits these curves, and in the adiabatic limit followed here the electron transfers with unit probability whenever the crossing region is reached.

Activation energy of local polaron hopping

Finally, we determined the temperature dependence of the hopping rate from FPMD trajectories of Li0.5_{0.5}MnPO4_4 at 600, 700, 800 and 900 K, of 32.7–45.1 ps each (157.5 ps in total). Since every hop changes the OS of exactly two Mn sites, and the cell hosts two polarons, the average of the site transition rates, ⟨Γ⟩=14∑iNi/ttot\langle\Gamma\rangle= \frac{1}{4}\sum_i N_i/t_{\mathrm{tot}}, coincides with the hopping rate per polaron (Methods). The Arrhenius plot (Figure 7a, tdwell≥12t_{\mathrm{dwell}} \ge12 fs) yields an activation energy Ea=0.20±0.03E_a = 0.20 \pm0.03 eV and a prefactor Γ0≃2×1013\Gamma_0 \simeq2 \times10^{13} s−1^{-1} (R2=0.89R^2 = 0.89 from a Poisson-weighted fit). The prefactor, which includes the number of accessible neighbouring sites and the effective attempt frequency, is of the order of 101310^{13} s−1^{-1}, as expected for phonon-assisted adiabatic hopping[9, 12]. Crucially, changing the dwell-time criterion from 4 to 12 fs lowers the absolute rates by only ∼6%\sim6\%, as transient excursions are discarded, and leaves the slope unchanged (Ea=0.20±0.03E_a = 0.20 \pm0.03 eV across tdwell≥4t_{\mathrm{dwell}} \ge4, 8 and 12 fs; Figure 7b): the activation energy is an intrinsic property of the dynamics rather than of the counting procedure.

Figure 7. Thermally activated polaron hopping in Li0.5_{0.5}MnPO4_4. Unit cell, 26 atoms: 4 Mn, 4 P, 16 O, 2 Li; a×b×c≈10.15×6.07×4.81a \times b \times c \approx10.15 \times6.07 \times4.81 Å, two Li+^+ ions and two polarons. a, Arrhenius plot of the hopping rate from FPMD at 600–900 K (trajectories of 32.7–45.1 ps, tdwell≥12t_{\mathrm{dwell}} \ge12 fs). Small symbols: individual Mn sites; large symbols: four-site average ⟨Γ⟩\langle\Gamma\rangle, equal to the hopping rate per polaron, with Poisson uncertainties. The dashed line is a Poisson-weighted linear fit of ln⁡⟨Γ⟩\ln\langle\Gamma\rangle versus 1/T1/T, yielding Ea=0.20±0.03E_a = 0.20 \pm0.03 eV and Γ0≈2×1013\Gamma_0 \approx2 \times10^{13} s−1^{-1} (R2=0.89R^2 = 0.89). b, Arrhenius plots for dwell-time thresholds tdwell≥4t_{\mathrm{dwell}} \ge4, 8 and 12 fs, showing a ∼6%\sim6\% rate variation between 4 and 12 fs and yielding a consistent activation energy Ea=0.20±0.03E_a = 0.20 \pm0.03 eV for all three thresholds.

This barrier can be estimated, without adjustable parameters, from the equilibrium fluctuations of individual cages. Treating each cage volume as a harmonic coordinate, equipartition gives the stiffness:

K=kBT⟨δV2⟩=0.182 eV/A˚6,(2)K = \frac{k_{\mathrm{B}}T}{\langle\delta V^2 \rangle} = 0.182\ \mathrm{eV}/\text{\AA}^{6}, \tag*{(2)}

with ⟨δV2⟩=0.427\langle\delta V^2 \rangle= 0.427 Å6^{6} (0.373 and 0.480 Å6^{6} for Mn3+^{3+} and Mn2+^{2+} cages, respectively; neither environment is rigid, and their fluctuations have comparable amplitude). A hop requires the donor cage to contract and the acceptor cage to expand by ΔV=2.115\Delta V = 2.115 Å3^{3}, each at an elastic cost of 12K(ΔV)2\frac{1}{2}K(\Delta V)^2, so that the total reorganization energy of the two participating cages is:

λV=2×12K(ΔV)2=K(ΔV)2=0.81 eV,(3)\lambda_{\mathrm{V}} = 2 \times\frac{1}{2}K(\Delta V)^2 = K(\Delta V)^2 = 0.81\ \mathrm{eV}, \tag*{(3)}

and the symmetric Marcus barrier is:

Ea=λV4≈0.20 eV.(4)E_a = \frac{\lambda_{\mathrm{V}}}{4} \approx0.20\ \mathrm{eV}. \tag*{(4)}

This independent-cage harmonic estimate of the reorganization energy[8, 33] is comparable to the Arrhenius activation energy of 0.20±0.030.20 \pm0.03 eV obtained under an independent-hop analysis (a quantitative Marcus description additionally requires diabatic energy gaps, covariance and electronic-

coupling estimates). Nonetheless, the conclusion is that the elasticity of the MnO6_6 cages alone sets a barrier of the observed magnitude. The cage stiffness is, moreover, temperature independent: in our simulations, between 600 and 900 K, ⟨δV2⟩\langle\delta V^2\rangle grows linearly with TT, giving K=0.17K = 0.17–0.180.18 eV/Å6^6 and λV/4=0.19\lambda_V/4 = 0.19–0.200.20 eV at each temperature.

The observed 0.20 eV barrier is quantitatively consistent with the migration barrier computed with hybrid functionals (HSE06) for a free electron polaron in MnPO4_4 (196 meV)[14], a functional whose accuracy for olivines is only slightly worse than that of DFT + UU + VV[18, 25]. Because every Mn site in this composition has two Li ions within 4.5 Å, the polaron never has to escape from a bound site: the measured barrier characterizes hopping between Li-adjacent sites, not the escape of a trapped polaron.

Analysis of the hopping pairs reveals that in collinear antiferromagnetic FPMD, hops occur both within the same spin sublattice and between opposite-spin sites. Restricting the Arrhenius analysis exclusively to same-spin hops yields Ea=0.18±0.03E_a = 0.18 \pm0.03 eV, showing that the activation energy is robust against spin selection.

Discussion

The picture that emerges from our simulations establishes the oxygen framework as the central actor in small-polaron transport. In Lix_xMnPO4_4 at finite temperature (i.e., in the range 600–900 K), we find that 1) the extra electrons hop between Mn sites a few times per picosecond while the Li ions remain confined to their sites; 2) the polaron visits all Mn sites while the Li ion migrates, including second-shell sites at ≈5.5\approx5.5 Å from the Li+^+ ion (reached already before Li+^+ migration); 3) freezing the oxygen cage of a single Mn in its Mn3+^{3+} geometry excludes that site from hopping without affecting the others; 4) heavier oxygen slows hopping down through classical framework inertia; 5) the event-averaged donor–acceptor volume asymmetry ΔV\Delta V crosses zero near the electronic switch, consistent with a predominantly breathing reaction coordinate; and 6) a harmonic estimate from cage-volume fluctuations gives λV/4≈0.20\lambda_V /4 \approx0.20 eV, comparable to the Arrhenius activation energy of 0.20±0.030.20 \pm0.03 eV. This agreement supports the relevance of cage elasticity. All these observations point to the same physical mechanism: thermal fluctuations of the MnO6\mathrm{MnO}_6 framework transiently bring the donor and acceptor sites into degeneracy, allowing the electron to transfer, adiabatically in our simulations, and in general with a probability controlled by the diabatic coupling between the two sites[28, 29]. In this sense, the coordination cage is not a passive spectator that relaxes after charge transfer, but part of the reaction coordinate: the oxidation state of a Mn ion and the geometry of its cage evolve as a single coupled variable. Polaron hopping occurs repeatedly while Li+\mathrm{Li}^{+} ions remain in their crystallographic sites, showing that individual local redox transitions do not require simultaneous Li migration. In the 1×1×21 \times1 \times2 supercell, the polaron also visits Mn sites in the second coordination shell of the Li+\mathrm{Li}^{+} ion (≈5.5\approx5.5 Å), the distance at which static calculations locate most of the Li+\mathrm{Li}^{+}–polaron binding, and the Mn2+\mathrm{Mn}^{2+} and Mn3+\mathrm{Mn}^{3+} distance distributions largely overlap at all sites. Therefore, the electrostatic association does not trap the polaron within the first shell. Long-range dissociation in the dilute limit, however, lies beyond the cell sizes accessible here. The oxygen framework governs the local structural reorganization, whereas Li+\mathrm{Li}^{+} ions shape the average electrostatic landscape and enforce charge neutrality at the mesoscale (i.e., Li+\mathrm{Li}^{+} ions and electrons cannot segregate). Their instantaneous positions, however, do not gate or throttle individual hops.

The activation energy extracted from the dynamics (Ea=0.20±0.03E_a = 0.20 \pm0.03 eV) is lower than the barriers computed for Li+\mathrm{Li}^{+} migration in static first-principles calculations (0.25–0.51 eV)[6, 34, 35, 36]. Although a dynamical and a static barrier are not strictly equivalent, this ordering indicates that the timescale separation observed at 900 K may persist, or even widen, upon cooling if the same local environments, hopping mechanism and barrier ordering persist. At room temperature, however, Li/vacancy and polaron ordering, or phase separation into LiMnPO4\mathrm{LiMnPO}_4 and a Li-poor phase, as reported experimentally by Chen and Richardson[37], may modify both the migration barriers and the population of local hopping environments. Muon-spin relaxation yields a lower Li self-diffusion barrier (0.19 ±\pm 0.03 eV)[38], but it probes local Li hopping in stoichiometric LiMnPO4\mathrm{LiMnPO}_4 (x=1x = 1) and is therefore not directly comparable with the partially delithiated compositions simulated here.

Several physical and methodological aspects place these findings in a broader perspective. Our simulations show that local coordination descriptors (such as octahedral volumes and bond-valence sums) track the electronic oxidation state to within a few femtoseconds and, through their elasticity, set the energy scale of the hopping barrier. This provides a physical blueprint for redox-aware machine-learning architectures[19] which, once equipped with long-range electrostatics, will enable the exploration of dilute polaron limits, complex defect clustering and low-temperature kinetics. Regarding electron dynamics, we reiterate that the OS transitions observed in extended Hubbard FPMD are adiabatic, and the calculated hopping rates correspond to the adiabatic upper limit; non-adiabatic electronic transmission factors[28, 29] would modify the kinetic prefactor, but the fundamental gating by the oxygen cage, the Marcus coincidence condition, and the decoupling from lithium motion are governed by the free-energy landscape and remain unchanged. Likewise, while collinear antiferromagnetic FPMD allows hops between opposite-spin sites, restricting the analysis exclusively to same-spin hops yields an essentially identical activation barrier (0.18 ±\pm 0.03 eV), confirming that the extracted barrier is an intrinsic property of the lattice-gated hopping process.

In conclusion, by following oxidation states in real time with extended Hubbard molecular dynamics, we have shown that small-polaron hopping in olivine LixMnPO4\mathrm{Li}_x\mathrm{MnPO}_4 is decoupled from lithium motion and gated by the local oxygen cage: the electron transfers through a geometrically degenerate coincidence state in which donor and acceptor cages are equivalent, at a rate governed by framework inertia and with a barrier of the magnitude set by cage elasticity. From a materials-design perspective, this places the stiffness and flexibility of the anionic framework, rather than the lithium sublattice, at the centre of electronic transport in polyanionic cathodes, and suggests substitution, strain or pressure as levers to tune it independently of ionic diffusion. Tracking oxidation states while selectively constraining or mass-scaling sublattices offers a general methodology to disentangle ionic, electronic and framework degrees of freedom in mixed ionic–electronic conductors.

Methods

Extended Hubbard functionals

DFT +U+V+ U + V[21] generalizes DFT +U+ U[39, 40] by adding to the DFT energy an extended Hubbard correction,

EU+V=∑I,σUI2Tr⁡[nIIσ(1−nIIσ)]−∑I,J,σ∗VIJ2Tr⁡[nIJσnJIσ](5)E_{U+V} = \sum_{I,\sigma} \frac{U^I}{2} \operatorname{Tr}\left[n^{II\sigma}\left(1-n^{II\sigma}\right)\right] - \sum_{I,J,\sigma}^{*} \frac{V^{IJ}}{2} \operatorname{Tr}\left[n^{IJ\sigma}n^{JI\sigma}\right] \tag*{(5)}

where II and JJ are atomic sites, σ\sigma is the spin index, the asterisk indicates that for each II the sum runs over neighbours JJ up to a given distance, and the generalized occupation matrices nmm′IJσ=∑k,vfkvσ⟨ψkvσ∣ϕm′J⟩⟨ϕmI∣ψkvσ⟩n_{mm'}^{IJ\sigma} = \sum_{\mathbf{k},v} f_{\mathbf{k}v}^{\sigma}\langle\psi_{\mathbf{k}v}^{\sigma}|\phi_{m'}^{J}\rangle\langle\phi_{m}^{I}|\psi_{\mathbf{k}v}^{\sigma}\rangle are obtained by projecting the Kohn–Sham states ψkvσ\psi_{\mathbf{k}v}^{\sigma}[41, 42] onto Löwdin-orthogonalized atomic orbitals ϕm\phi_m[27, 43]. The on-site term favours localization on the Mn 3d3d states, while the inter-site term between Mn 3d3d and O 2p2p states accounts for their hybridization[21, 25]. As in ref. 19, we use U=5.1U = 5.1 eV and V=0.7V = 0.7 eV, obtained by averaging the self-consistent values computed with density-functional perturbation theory[22, 23, 24] over all Mn sites and Li concentrations; these parameters preserve the digital change of the Mn OSs and yield intercalation voltages in good agreement with experiments[19]. Forces are computed via the Hellmann–Feynman theorem, including the contributions of the orthogonalized Hubbard projectors[43].

Oxidation states

The OS of each Mn ion is obtained from the eigenvalues of the site-diagonal 3d3d occupation matrix nIIσ\mathbf{n}^{II\sigma} (5×55 \times5 in each spin channel), following ref. 26: states with eigenvalues close to 1 are counted as occupied. As a compact descriptor we use the Löwdin occupation n=∑i,σλiσn = \sum_{i,\sigma}\lambda_i^\sigma, which equals ≃4.98\simeq4.98–5.005.00 for Mn3+\mathrm{Mn}^{3+} and ≃5.20\simeq5.20–5.215.21 for Mn2+\mathrm{Mn}^{2+} in DFT +U+V+ U + V[19].

First-principles molecular dynamics

All calculations were performed with the plane-wave pseudopotential implementation of Quantum ESPRESSO[44, 45], using the PBEsol functional[46] and pseudopotentials from the SSSP library[47] (Mn and Li from GBRV[48], O and P from Pslibrary[49]). Kohn–Sham wavefunctions and charge density were expanded up to kinetic-energy cutoffs of 65 and 780 Ry, respectively, with a Gaussian smearing of 0.005 Ry. For the 25–26-atom unit cell we used a Γ\Gamma-centred 3×4×53 \times4 \times5 k-point grid; the 49-atom supercell was obtained by doubling the unit cell along cc, with a correspondingly reduced grid. The antiferromagnetic ground-state configuration was used throughout[25]. Born–Oppenheimer FPMD was performed in the NVT ensemble using the stochastic velocity-rescaling thermostat[50] and the Verlet integrator with a time step of 4 fs (0.5 fs for the high-resolution trajectory of Supplementary Figs. S2–S4), starting from cells and positions relaxed at 0 K. Simulated systems and trajectory lengths are: Li0.5_{0.5}MnPO4_4 unit cell at 600 (32.7 ps), 700 (41.7 ps), 800 (45.1 ps) and 900 K (38.0 ps), and at 900 K with δt=0.5\delta t = 0.5 fs (5.11 ps, 10,216 frames); Li0.25_{0.25}MnPO4_4 unit cell at 900 K (27.8 ps); Li1/8_{1/8}MnPO4_4 supercell at 900 K, unconstrained and with the Mn2_2O6_6 cage frozen (13.46 ps each), and an extension of the unconstrained run to 33.3 ps (Figure 2).

Constrained dynamics. In the constrained supercell run, the forces acting on the six O atoms of the Mn2_2O6_6 octahedron (Mn–O distances 1.89–2.30 Å) were set to zero, so that these atoms remain at their initial positions, corresponding to a Mn3+^{3+} cage; all other atoms, including Mn2, evolve freely.

Fictitious isotope substitution. The oxygen mass in the equations of motion was set to mO=19m_{\mathrm{O}} = 19, 32 and 79 u, leaving the electronic Hamiltonian unchanged (trajectories of 26.2, 26.8 and 26.0 ps at 900 K, compared with 38.0 ps for mO=16m_{\mathrm{O}} = 16 u).

Hop counting and rates

A transition on site ii is counted when nin_i crosses from one basin (n<5.05n < 5.05 for Mn3+^{3+}, n>5.15n > 5.15 for Mn2+^{2+}) into the other and remains there for at least tdwellt_{\mathrm{dwell}} (one, two or three time steps, i.e. 4, 8 or 12 fs); excursions into the intermediate band 5.05≤n≤5.155.05 \le n \le5.15 do not change the assigned state. The persistence test is applied only to frames in which all Mn sites of the cell lie within one of the two basins: a frame in which any site is in the intermediate band interrupts the dwell count and leaves the assigned states unchanged. The thresholds correspond to the edges of the two basins at three standard deviations of their thermal fluctuations, n3+mode+3σ3+n_{3+}^{\mathrm{mode}} + 3\sigma_{3+} and n2+mode−3σ2+n_{2+}^{\mathrm{mode}} - 3\sigma_{2+}, where nmoden^{\mathrm{mode}} is the peak of the occupation distribution and σ\sigma is obtained from its outer side (away from the inter-basin tail produced by transfer events), σ≈0.011\sigma\approx0.011 for both basins. In the unit cells this gives 5.04 and 5.15–5.16. For the Li–Mn distance analysis of the 33.3 ps supercell trajectory (Figure 2), where the Mn2+^{2+} peak lies slightly lower, the same convention gives n<5.035n < 5.035 (Mn3+^{3+}) and n>5.137n > 5.137 (Mn2+^{2+}). This two-threshold hysteresis and the persistence filter suppress recrossings and short-lived unrelaxed excursions. Since each hop changes the OS of exactly two sites, the number of hops is Nhop=12∑iNiN_{\mathrm{hop}} = \frac{1}{2}\sum_i N_i, and the rate per polaron in a cell with NpolN_{\mathrm{pol}} polarons is Γ=Nhop/(Npolttot)\Gamma= N_{\mathrm{hop}}/(N_{\mathrm{pol}}t_{\mathrm{tot}}); for Li0.5_{0.5}MnPO4_4 (Npol=2N_{\mathrm{pol}} = 2, four Mn sites) this is identical to the site average ⟨Γ⟩=14∑iNi/ttot\langle\Gamma\rangle= \frac{1}{4}\sum_i N_i/t_{\mathrm{tot}}. Statistical uncertainties are estimated as Γ/Nhop\Gamma/\sqrt{N_{\mathrm{hop}}} (Poisson statistics of the hops; the two OS changes produced by one hop are not independent events). Activation energies are obtained from Poisson-weighted least-squares fits of ln⁡⟨Γ⟩\ln\langle\Gamma\rangle versus 1/T1/T (weighted by Nhop=1/σln⁡⟨Γ⟩2N_{\mathrm{hop}} = 1/\sigma_{\ln\langle\Gamma\rangle}^{2}).

Structural descriptors and event averaging

MnO6_6 octahedral volumes were computed as the volume of the convex hull of the six O atoms coordinating each Mn[51], under the minimum-image convention. Bond-valence sums were computed as BVS =∑jexp⁡[(R0−dj)/b]= \sum_j \exp[(R_0 - d_j)/b] over the six Mn–O bonds, with R0=1.790R_0 = 1.790 Å and b=0.37b = 0.37 Å[52]. Normalized cross-correlations C(τ)C(\tau) were computed between the mean-subtracted, variance-normalized time series of each descriptor and of the Löwdin occupation of the same site. Nearest-neighbour Li–Mn distances were evaluated under the minimum-image convention across all periodic boundaries.

For the hop-aligned coincidence analysis (Figure 6c–Figure 6e), transition times t0t_0 were identified from the mid-point of the Löwdin occupation crossing (n=5.10n = 5.10) in the δt=0.5\delta t = 0.5 fs trajectory (N=16N = 16 hops: the donor–acceptor pairs whose transitions occur within 25 fs of each other, whose occupation difference nD−nAn_D-n_A crosses zero within ±15\pm15 fs of their midpoint, and whose complete ±150\pm150 fs window lies inside the 5.11 ps trajectory; with the standard criteria of Supplementary Table S1, 20 hops are counted in this trajectory). Trajectories of donor and acceptor volumes, occupations, and bond-valence sums were aligned at t0t_0 and averaged over a window of ±150\pm150 fs. Single-cage elasticity was extracted from the variance of the octahedral volume ⟨δV2⟩\langle\delta V^2 \rangle evaluated strictly within each oxidation-state basin (excluding transition frames), giving ⟨δV2⟩=0.373\langle\delta V^2 \rangle= 0.373 A˚6\mathring{\mathrm{A}}^{6} for Mn3+\mathrm{Mn}^{3+} and 0.4800.480 A˚6\mathring{\mathrm{A}}^{6} for Mn2+\mathrm{Mn}^{2+} (mean: 0.4270.427 A˚6\mathring{\mathrm{A}}^{6}) in the 900 K high-resolution trajectory, yielding λV=0.81\lambda_V = 0.81 eV.

Data availability

The data supporting the findings of this study will be made available in the Materials Cloud Archive upon publication.

Code availability

DFT + U+VU + V calculations were performed with Quantum ESPRESSO v7.2, open source and available at https://www.quantum-espresso.org.

Acknowledgements

We acknowledge support by the European Commission through the MaX Centre of Excellence for supercomputing applications (grant number 101093374), by the Deutsche Forschungsgemeinschaft (DFG) under Germany’s Excellence Strategy (EXC 2077, No. 390741603, University Allowance, University of Bremen) and Lucio Colombi Ciacchi, the host of the “U Bremen Excellence Chair Program”.

Competing interests

The authors declare no competing interests.

Supplementary Information

Summary of First-Principles Molecular Dynamics Trajectories

Supplementary Table S1 summarizes all DFT + UU + VV-FPMD trajectories analysed in this study, detailing system composition, temperature, fictitious oxygen mass, integration time step, trajectory duration, number of detected oxidation-state transitions, and resulting hopping rates.

CompositionTT (K)mOm_{\mathrm{O}} (u)δt\delta t (fs)Duration (ps)FramesHops (NhopN_{\mathrm{hop}})Rate per polaron (ps−1^{-1})
Arrhenius series (unit cell, 2 polarons)
Li0.5_{0.5}MnPO4_460016 (O)4.032.78,180310.47 ±\pm 0.09
Li0.5_{0.5}MnPO4_470016 (O)4.041.710,414530.64 ±\pm 0.09
Li0.5_{0.5}MnPO4_480016 (O)4.045.111,2661231.36 ±\pm 0.12
Li0.5_{0.5}MnPO4_490016 (O)4.038.09,5121131.49 ±\pm 0.14
Oxygen isotope series (unit cell, 2 polarons, T=900T = 900 K)
Li0.5_{0.5}MnPO4_490016 (O)4.038.09,5121131.49 ±\pm 0.14
Li0.5_{0.5}MnPO4_490019 (F)4.026.26,556881.68 ±\pm 0.18
Li0.5_{0.5}MnPO4_490032 (S)4.026.86,698741.38 ±\pm 0.16
Li0.5_{0.5}MnPO4_490079 (Se)4.026.06,491561.08 ±\pm 0.14
High-resolution trajectory (unit cell, 2 polarons)
Li0.5_{0.5}MnPO4_490016 (O)0.55.1110,216201.96 ±\pm 0.44
Li-dilute trajectory (unit cell, 1 polaron)
Li0.25_{0.25}MnPO4_490016 (O)4.027.86,9481334.79 ±\pm 0.42
Supercell simulations (1×1×21 \times1 \times2, 1 polaron, T=900T = 900 K)
Li1/8_{1/8}MnPO4_4 (free)90016 (O)4.013.463,365775.72 ±\pm 0.65
Li1/8_{1/8}MnPO4_4 (frozen)90016 (O)4.013.463,366735.42 ±\pm 0.63
Li1/8_{1/8}MnPO4_4 (free, long)90016 (O)4.033.38,3141865.59 ±\pm 0.41

Table S1. Supplementary Table S1. Overview of DFT + UU + VV-FPMD simulations and polaron hopping statistics. All runs employ the PBEsol + UU + VV functional with U=5.1U = 5.1 eV and V=0.7V = 0.7 eV. Unit cells: 26 atoms (Li0.5_{0.5}MnPO4_4, a×b×c≈10.15×6.07×4.81a \times b \times c \approx10.15 \times6.07 \times4.81 Å) and 25 atoms (Li0.25_{0.25}MnPO4_4, ≈9.93×6.04×4.84\approx9.93 \times6.04 \times4.84 Å); 1×1×21 \times1 \times2 supercell: 49 atoms (≈9.94×6.03×9.63\approx9.94 \times6.03 \times9.63 Å). Hop counts and rates correspond to the standard dwell-time threshold tdwell≥12t_{\mathrm{dwell}} \ge12 fs. Uncertainties are Γ/Nhop\Gamma/\sqrt{N_{\mathrm{hop}}}. The 33.3 ps free supercell run extends the 13.46 ps one (first 2,960 frames shared). For the δt=0.5\delta t = 0.5 fs run (tdwell≥12t_{\mathrm{dwell}} \ge12 fs = 24 steps), 16 of the hops are used in the event average of Figure 6c–Figure 6e (Methods).

Figure S1. Li migration and Li–Mn distance distributions in the Li0.25MnPO4\mathrm{Li}_{0.25}\mathrm{MnPO}_{4} unit cell at 900 K. Unit cell (25 atoms: 4 Mn, 4 P, 16 O, 1 Li; a×b×c≈9.93×6.04×4.84a \times b \times c \approx9.93 \times6.04 \times4.84 Å) with one Li+\mathrm{Li}^{+} ion and one polaron, 27.8 ps (6,948 frames, δt=4\delta t = 4 fs). a, Displacement of the Li+\mathrm{Li}^{+} ion, which performs six jumps between nearest-neighbour Li sites (≈3\approx3 Å each). Faint line: raw data; solid line: 100 fs running average. b, Split-violin distributions of the instantaneous Li–Mn distance under the minimum-image convention (MIC, range 2.35–4.73 Å) for each Mn site, conditioned on the oxidation state of that site: Mn2+\mathrm{Mn}^{2+} (orange, n>5.15n > 5.15) and Mn3+\mathrm{Mn}^{3+} (blue, n<5.05n < 5.05). All Mn sites lie within the first coordination shell of the Li+\mathrm{Li}^{+} ion, and both oxidation states span the full distance range.

High-temporal-resolution analysis of the electron–lattice coupling

To resolve the electron–lattice coupling below the 4 fs time step of the production runs, we analysed an independent FPMD trajectory of Li0.5MnPO4\mathrm{Li}_{0.5}\mathrm{MnPO}_{4} at T=900T = 900 K with δt=0.5\delta t = 0.5 fs (10,216 frames, 5.11 ps).

Figure S3. Bond-valence sum versus Löwdin occupation at δt=0.5\delta t = 0.5 fs. Li0.5_{0.5}MnPO4_4 at T=900T = 900 K, unit cell, 26 atoms: 4 Mn, 4 P, 16 O, 2 Li; a×b×c≈10.15×6.07×4.81a \times b \times c \approx10.15 \times6.07 \times4.81 Å. a, Scatter plots showing a strong anti-correlation (r=−0.85r = -0.85 for all four sites; ⟨r⟩≃−0.85\langle r \rangle\simeq-0.85). b, Cross-correlations CBVS,n(τ)C_{\mathrm{BVS},n}(\tau): the minima lie at +0.5+0.5, +1.5+1.5, −5.5-5.5 and −0.5-0.5 fs (site average −1.0-1.0 fs), with C(0)=−0.850C(0) = -0.850 versus Cmin⁡=−0.855C_{\min} = -0.855 (Mn3, the largest difference). Peak positions are read on the 0.50.5 fs time grid; a parabolic interpolation shifts them by less than 0.20.2 fs.

Figure S4. Octahedral volume versus bond-valence sum at δt=0.5\delta t = 0.5 fs. Li0.5_{0.5}MnPO4_4 at T=900T = 900 K, unit cell, 26 atoms: 4 Mn, 4 P, 16 O, 2 Li; a×b×c≈10.15×6.07×4.81a \times b \times c \approx10.15 \times6.07 \times4.81 Å. The two geometric descriptors are strongly anti-correlated (r=−0.93r = -0.93 to −0.95-0.95) and their cross-correlation peaks at τ=0\tau= 0, confirming that they evolve synchronously.

References

  1. [1]A. Walsh, A. A. Sokol, J. Buckeridge, D. O. Scanlon, and C. R. A. Catlow. Oxidation states and ionicity. Nat. Mater., 17:958–964, 2018.DOI
  2. [2]A. K. Padhi, K. S. Nanjundaswamy, and J. B. Goodenough. Phospho-olivines as positive-electrode materials for rechargeable lithium batteries. J. Electrochem. Soc., 144:1188–1194, 1997.DOI
  3. [3]G. Hautier et al. Phosphates as lithium-ion battery cathodes: an evaluation based on high-throughput ab initio calculations. Chem. Mater., 23:3495–3508, 2011.
  4. [4]S. K. Martha et al. LiMnPO₄ as an advanced cathode material for rechargeable lithium batteries. J. Electrochem. Soc., 156:A541–A552, 2009.DOI
  5. [5]C. Delacourt, L. Laffont, R. Bouchet, C. Wurm, J.-B. Leriche, M. Morcrette, J.-M. Tarascon, and C. Masquelier. Toward understanding of electrical limitations (electronic, ionic) in LiMPO₄ (M = Fe, Mn) electrode materials. J. Electrochem. Soc., 152:A913–A921, 2005.DOI
  6. [6]D. Morgan, A. Van der Ven, and G. Ceder. LiₓMPO₄ (M = Mn, Fe, Co, Ni) olivine materials. Electrochem. Solid-State Lett., 7:A30–A32, 2004.
  7. [7]M. S. Islam, D. J. Driscoll, C. A. J. Fisher, and P. R. Slater. Atomic-scale investigation of defects, dopants, and lithium transport in the LiFePO₄ olivine-type battery material. Chem. Mater., 17:5085–5092, 2005.DOI
  8. [8]T. Holstein. Studies of polaron motion: Part II. the “small” polaron. Am. Phys., 8:343–389, 1959.
  9. [9]I. G. Austin and N. F. Mott. Polarons in crystalline and non-crystalline materials. Adv. Phys., 18:41–102, 1969.
  10. [10]C. Franchini, M. Reticcioli, M. Setvin, and U. Diebold. Polarons in materials. Nat. Rev. Mater., 6:560–586, 2021.DOI
  11. [11]F. Zhou, K. Kang, T. Maxisch, G. Ceder, and D. Morgan. The electronic structure and band gap of LiFePO₄ and LiMnPO₄. Solid State Commun., 132:181–186, 2004.DOI
  12. [12]D. Emin and T. Holstein. Studies of small-polaron motion IV. adiabatic theory of the Hall effect. Ann. Phys., 53:439–520, 1969.DOI
  13. [13]T. Maxisch, F. Zhou, and G. Ceder. Ab initio study of the migration of small polarons in olivine LiₓFePO₄ and their association with lithium ions and vacancies. Phys. Rev. B, 73:104301, 2006.DOI
  14. [14]S. P. Ong, V. L. Chevrier, and G. Ceder. Comparison of small polaron migration and phase separation in olivine LiMnPO₄ and LiFePO₄ using hybrid density functional theory. Phys. Rev. B, 83:075112, 2011.
  15. [15]B. Ellis, L. K. Perry, D. H. Ryan, and L. F. Nazar. Small polaron hopping in LiₓFePO₄ solid solutions: coupled lithium-ion and electron mobility. J. Am. Chem. Soc., 128:11416–11422, 2006.pubmed.ncbi.nlm.nih.gov/16939264
  16. [16]M. D. Johannes, K. Hoang, J. L. Allen, and K. Gaskell. Hole polaron formation and migration in olivine phosphate materials. Phys. Rev. B, 85:115106, 2012.DOI
  17. [17]R. Car and M. Parrinello. Unified approach for molecular dynamics and density-functional theory. Phys. Rev. Lett., 55:2471–2474, 1985.pubmed.ncbi.nlm.nih.gov/10032153
  18. [18]I. Timrov, F. Aquilante, M. Cococcioni, and N. Marzari. Accurate electronic properties and intercalation voltages of olivine-type Li-ion cathode materials from extended Hubbard functionals. PRX Energy, 1:033003, 2022.DOI
  19. [19]C. Malica and N. Marzari. Teaching oxidation states to neural networks. npj Comput. Mater., 11:212, 2025.arxiv.org/abs/2412.01652
  20. [20]J. Heyd, G. E. Scuseria, and M. Ernzerhof. Hybrid functionals based on a screened Coulomb potential. J. Chem. Phys., 118:8207, 2003.DOI
  21. [21]V. L. Campo Jr and M. Cococcioni. Extended DFT+U+V method with on-site and inter-site electronic interactions. J. Phys. Condens. Matter, 22:055602, 2010.DOI
  22. [22]I. Timrov, N. Marzari, and M. Cococcioni. Hubbard parameters from density-functional perturbation theory. Phys. Rev. B, 98:085127, 2018.DOI
  23. [23]I. Timrov, N. Marzari, and M. Cococcioni. Self-consistent Hubbard parameters from density-functional perturbation theory in the ultrasoft and projector-augmented wave formulations. Phys. Rev. B, 103:045141, 2021.DOI
  24. [24]I. Timrov, N. Marzari, and M. Cococcioni. HP – a code for the calculation of Hubbard parameters using density-functional perturbation theory. Comput. Phys. Commun., 279:108455, 2022.DOI
  25. [25]M. Cococcioni and N. Marzari. Energetics and cathode voltages of LiMPO₄ olivines (M = Fe, Mn) from extended Hubbard functionals. Phys. Rev. Mater., 3:033801, 2019.DOI
  26. [26]P. H.-L. Sit, R. Car, M. H. Cohen, and A. Selloni. Simple, unambiguous theoretical approach to oxidation state determination via first-principles calculations. Inorg. Chem., 50:10259–10267, 2011.DOI
  27. [27]P.-O. Löwdin. On the non-orthogonality problem connected with the use of atomic wave functions in the theory of molecules and crystals. J. Chem. Phys., 18:365–375, 1950.DOI
  28. [28]R. A. Marcus and N. Sutin. Electron transfers in chemistry and biology. Biochim. Biophys. Acta, 811:265–322, 1985.DOI
  29. [29]P. H.-L. Sit, M. Cococcioni, and N. Marzari. Realistic quantitative descriptions of electron transfer reactions: diabatic free-energy surfaces from first-principles molecular dynamics. Phys. Rev. Lett., 97:028303, 2006.
  30. [30]G.-M. Zhao, K. Conder, H. Keller, and K. A. Müller. Giant oxygen isotope shift in the magnetoresistive perovskite La₁₋ₓCaₓMnO₃₊ᵧ. Nature, 381:676–678, 1996.DOI
  31. [31]A. Migliore, P. H.-L. Sit, and M. L. Klein. Evaluation of electronic coupling in transition-metal systems using DFT: application to the hexa-aquo ferric–ferrous redox couple. J. Chem. Theory Comput., 5:307–323, 2009.DOI
  32. [32]J. Reed and G. Ceder. Role of electronic structure in the susceptibility of metastable transition-metal oxide structures to transformation. Chem. Rev., 104:4513–4534, 2004.
  33. [33]R. A. Marcus. On the theory of oxidation-reduction reactions involving electron transfer. I. J. Chem. Phys., 24:966–978, 1956.DOI
  34. [34]J. Shi, Z. Wang, and Y. Q. Fu. Density functional theory study of lithium diffusion at the interface between olivine-type LiFePO₄ and LiMnPO₄. J. Phys. D: Appl. Phys., 49:505601, 2016. doi: 10.1088/0022-3727/49/50/505601.DOI
  35. [35]M. F. Sgroi, R. Lazzaroni, D. Beljonne, and D. Pullini. Doping LiMnPO₄ with cobalt and nickel: a first principle study. Batteries, 3:11, 2017. doi: 10.3390/batteries3020011.
  36. [36]Y. Gao, J. Huang, Y. Liu, and S. Chen. Unexpected role of electronic coupling between host redox centers in transport kinetics of lithium ions in olivine phosphate materials. Chem. Sci., 13:257–262, 2022. doi: 10.1039/D1SC05402C.DOI
  37. [37]G. Chen and T. J. Richardson. Solid solution phases in the olivine-type LiMnPO₄/MnPO₄ system. J. Electrochem. Soc., 156:A756–A762, 2009. doi: 10.1149/1.3167389.
  38. [38]J. Sugiyama, O. K. Forslund, E. Nocerino, N. Matsubara, K. Papadopoulos, Y. Sassa, S. P. Cottrell, A. D. Hillier, K. Ishida, M. Må​nsson, and J. H. Brewer. Lithium diffusion in LiMnPO₄ detected with μ±SR. Phys. Rev. Res., 2:033161, 2020. doi: 10.1103/PhysRevResearch.2.033161.DOI
  39. [39]V. I. Anisimov, J. Zaanen, and O. K. Andersen. Band theory and Mott insulators: Hubbard U instead of Stoner I. Phys. Rev. B, 44:943, 1991.
  40. [40]S. L. Dudarev, G. A. Botton, S. Y. Savrasov, C. J. Humphreys, and A. P. Sutton. Electron-energy-loss spectra and the structural stability of nickel oxide: an LSDA+U study. Phys. Rev. B, 57:1505, 1998.DOI
  41. [41]P. Hohenberg and W. Kohn. Inhomogeneous electron gas. Phys. Rev., 136:B864, 1964.
  42. [42]W. Kohn and L. J. Sham. Self-consistent equations including exchange and correlation effects. Phys. Rev., 140:A1133, 1965.DOI
  43. [43]I. Timrov, F. Aquilante, L. Binci, M. Cococcioni, and N. Marzari. Pulay forces in density-functional theory with extended Hubbard functionals: from nonorthogonalized to orthogonalized manifolds. Phys. Rev. B, 102:235159, 2020.DOI
  44. [44]P. Giannozzi et al. QUANTUM ESPRESSO: a modular and open-source software project for quantum simulations of materials. J. Phys. Condens. Matter, 21:395502, 2009.DOI
  45. [45]P. Giannozzi et al. Advanced capabilities for materials modelling with QUANTUM ESPRESSO. J. Phys. Condens. Matter, 29:465901, 2017.
  46. [46]J. P. Perdew et al. Restoring the density-gradient expansion for exchange in solids and surfaces. Phys. Rev. Lett., 100:136406, 2008.pubmed.ncbi.nlm.nih.gov/18517979
  47. [47]E. Bosoni et al. How to verify the precision of density-functional-theory implementations via reproducible and universal workflows. Nat. Rev. Phys., 6:45–58, 2024.
  48. [48]K. F. Garrity, J. W. Bennett, K. M. Rabe, and D. Vanderbilt. Pseudopotentials for high-throughput DFT calculations. Comput. Mater. Sci., 81:446–452, 2014.DOI
  49. [49]A. Dal Corso. Pseudopotentials periodic table: from H to Pu. Comput. Mater. Sci., 95:337–350, 2014.DOI
  50. [50]G. Bussi, D. Donadio, and M. Parrinello. Canonical sampling through velocity rescaling. J. Chem. Phys., 126:014101, 2007.pubmed.ncbi.nlm.nih.gov/17212484
  51. [51]C. B. Barber, D. P. Dobkin, and H. Huhdanpaa. The quickhull algorithm for convex hulls. ACM Trans. Math. Softw., 22:469–483, 1996.DOI
  52. [52]I. D. Brown and D. Altermatt. Bond-valence parameters obtained from a systematic analysis of the Inorganic Crystal Structure Database. Acta Crystallogr. B, 41:244–247, 1985.DOI

Paper details

vlnc:W_kc7ftp6j
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 2

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents