betaFeedback

WorksPhysics and Astronomy

Understanding Carbon Contamination in Proton Conducting Oxides

Abstract

Carbon contamination is a significant concern for proton-conducting oxides in the cerate and zirconate family, particularly for BaCeO3_3. Here, we use first-principles calculations to evaluate carbon stability in SrCeO3_3, BaCeO3_3, SrZrO3_3, and BaZrO3_3. The cerates require more carbon-poor environments to prevent carbonate formation, though this requirement can be loosened through the use of more oxygen-poor growth conditions. Carbonate formation is not the only concern, however. We find that interstitial carbon has lower formation energies in the cerates relative to the zirconates, leading to higher carbon concentrations that compete with the desired oxygen vacancy formation. We also examine the mobility of carbon interstitials, finding that both migration barriers and binding energies to acceptors are lower in the cerates. As a result, the cerates are likely to degrade when exposed to carbon at operating temperatures. Our results show definitively why the cerates are less stable than the zirconates with respect to carbon and elucidate the mechanisms contributing to their instability, thereby helping to explain why alloying with zirconium will enhance their operational efficiency.

Supporting information (SI) for this article is given via a link at the end of the document: Additional data regarding chemical potentials, stability, and defect formation in the cerates and zirconates.

Introduction

Considerable research has been devoted to solid-state proton conductors as electrolytes in solid-state hydrogen fuel cells. [1] Two materials in particular have attracted the majority of scientific attention: barium zirconate, BaZrO3_3 (BZO)[2, 3] and barium cerate, BaCeO3_3 (BCO).4,5 Of these, BCO is often cited for having higher proton conductivities, while BZO is known to be more chemically stable, particularly against CO2_2.6,7

Protons are introduced into the zirconates by creating oxygen vacancies during synthesis and then exposing the materials to water, leading to the reaction:[2]

VO+2+H2O→2Hi+.(1)V_{\mathrm{O}}^{+2} + \mathrm{H}_2\mathrm{O} \rightarrow2\mathrm{H}_{\mathrm{i}}^{+}. \tag*{(1)}

The as-grown material therefore needs to contain a large concentration of oxygen vacancies, which act as electron donors. This can be accomplished through doping with acceptor impurities, which promote the formation of oxygen vacancies that act as compensating donors.[2] [8, 9] However, if another donor species is energetically more favorable than the oxygen vacancy, then acceptor dopants will tend to compensate with that donor instead. That situation will therefore reduce the efficacy of acceptor doping as an oxygen vacancy generator and, consequentially, limit proton incorporation. Carbon impurities may compete with oxygen vacancies in this manner.

In addition, carbon can be detrimental because the cerates are prone to decomposing in carbon-rich atmospheres. 10 Several studies have shown that fuel cells based on BCO must be operated within a narrow temperature window in order to stave off decomposition when exposed to CO2_2. 11–14 The stability of BCO has been improved demonstrably through alloying with BZO, with approximately equal concentrations of Zr and Ce providing the best balance of stability and conductivity. 5,14–16 Similar results have been demonstrated for Zr-doped SrCeO3_3 (SCO).17

In previous work, we have shown that the cerates possess poor overall thermodynamic stability, and that SCO has lower stability than BCO, 18,19 which agrees with experimental observations. 17,20 We have also identified energetically favorable carbon impurity configurations in the zirconates that may compete with the formation of oxygen vacancies. 9 Other studies from our group have investigated similar carbon configurations in other oxides. 21–23 However, we are unaware of any studies aimed at uncovering the atomic-scale reason for these materials’ susceptibility to carbon.

Here, we use first-principles techniques based on density functional theory (DFT) with a hybrid functional to study the stability with respect to carbonates, and the incorporation and mobility of carbon species in SCO, BCO, and the equivalent zirconates, SrZrO3_3 (SZO) and BZO. We evaluate interstitial Ci_i and substitutional C{Ce,Zr}_{\{\mathrm{Ce},\mathrm{Zr}\}} in all four systems. We find that, under equivalent conditions for carbon exposure, the formation energy for carbon species in the cerates is considerably lower than in the zirconates, leading to much higher carbon concentrations in the cerates. We also study carbon impurity migration with the nudged elastic band (NEB) method, along with calculations of binding energies for complexes with the commonly used yttrium acceptor dopant. Our calculations reveal that carbon mobility is higher in the cerates, explaining why they will suffer from degradation in CO2_2-rich environments. Avoiding carbonate-based precursors during synthesis should help limit carbon incorporation. Doing so is critical, because changing the prevalence of native species—including oxygen—will have no effect unless equilibrium with carbonate formation is broken. Our results provide new insights into the microscopic reasons for the detrimental effects of carbon in the cerates relative to the zirconates, thereby guiding future research and development on more chemically stable solid-state proton conductors.

Methodology

Computational Details

Our calculations are based on DFT within the generalized Kohn-Sham scheme, 24 as implemented in the Vienna Ab initio Simulation Package (VASP). 25 We use projector augmented wave (PAW) potentials 26,27 and the hybrid exchange-correlation functional of Heyd, Scuseria, and Ernzerhof (HSE), 28 with 25% mixing of short-range Hartree-Fock exchange. Consistent with our previous work we use a 400 eV plane-wave cutoff energy for zirconates, 9,29,30 and a 500 eV cutoff for cerates. 18,19 We have confirmed that increasing the cutoff energy for zirconates to 500 eV does not affect our findings. The Ba 5s2^2 5p6^6 6s2^2, Sr 4s2^2 4p6^6 5s2^2, Zr 4d2^2 5s2^2, Ce 5s2^2 5p6^6 6s2^2 5d1^1 4f1^1, and O 2s2^2 2p4^4 electrons are treated explicitly as valence. We model bulk SCO, BCO, SZO, and BZO using orthorhombic unit cells, each containing four formula units, and with a 4×\times4×\times3 k-point grid to integrate over the Brillouin zone. BZO has a cubic primitive cell; however, we choose to describe it in an orthorhombic cell to more precisely compare results with the other systems. To evaluate the energetic barriers associated with defect migration we use the NEB method with climbing images. 31

Defect Calculations

To calculate defect properties, we construct supercells that are 2×2×22 \times2 \times2 multiples of the orthorhombic unit cell and thus contain 160 atoms. A 2×2×22 \times2 \times2 kk-point grid is used in each case. We focus specifically on two C configurations in this study: interstitial carbon (Ci\mathrm{C}_{i}) and the substitutional species C{Ce/Zr}\mathrm{C}_{\{\mathrm{Ce/Zr}\}}. Previously, we found these species to be favorable in the zirconates, 9, and we assume that they will be similarly favorable in the cerates. All three configurations are depicted in Figure 1 for the case of BCO; the configurations are very similar in the other systems under study.

Carbon configurations in BaCeO3

Figure 1. Carbon configurations in BaCeO3_3: (a) interstitial carbon, Ci\mathrm{C}_{i} and (b) substitutional carbon, CCe\mathrm{C}_{\mathrm{Ce}}. Images generated using the VESTA 3 software. 32

The formation energy Ef(Dq)E^{f}(D^{q}) of a point defect DD in charge state qq is calculated as: 33

Ef(Dq)=E(Dq)−Ebulk+∑niμi+qEF+Δcorr.(2)E^{f}(D^{q}) = E(D^{q}) - E_{\mathrm{bulk}} + \sum n_i\mu_i + qE_F + \Delta_{\mathrm{corr}}. \tag*{(2)}

E(Dq)E(D^{q}) is the total energy of a supercell containing defect DD in charge state qq; EbulkE_{\mathrm{bulk}} is the total energy of a defect-free supercell; ∣ni∣\lvert n_i\rvert is the number of atoms of species ii added (ni<0n_i < 0) or removed (ni>0n_i > 0) from the system; μi\mu_i is the chemical potential of species ii; EFE_F is the Fermi level referenced to the valence-band maximum (VBM); and Δcorr\Delta_{\mathrm{corr}} is a finite-size correction term. 34,35 The formation energy determines the defect concentration cc via a Boltzmann relation:

c=Nsitesexp⁡(−EfkBT),(3)c = N_{\mathrm{sites}} \exp\left(-\frac{E^{f}}{k_{\mathrm{B}}T}\right), \tag*{(3)}

meaning that lower formation energies result in higher defect concentrations. NsitesN_{\mathrm{sites}} is the number of sites (per unit volume) on which the defect can incorporate. In standard defect formation energy diagrams, EFE_F is the free variable and varies freely from the VBM to the conduction-band minimum (CBM). Because of the exponential relationship between formation energy and defect concentration the actual position of the Fermi level will, to a good approximation, be determined by the intersection of the lowest-energy negatively and positively charged defects, which together ensure charge neutrality.

The chemical potentials μi\mu_i are variables that reflect the abundance of specific elements during synthesis. We express them in terms of deviations Δμi\Delta\mu_i from the total energies of the elemental reference structures, i.e., the ground-state structures of the Sr, Ba, Zr, or Ce metals, or an O atom in O2_2. Assuming conditions close to equilibrium, the Δμi\Delta\mu_i are related by:

Δμ{Sr,Ba}+Δμ{Ce,Zr}+3ΔμO=ΔHf({Sr,Ba}{Ce,Zr}O3),(4)\Delta\mu_{\{\mathrm{Sr,Ba}\}} + \Delta\mu_{\{\mathrm{Ce,Zr}\}} + 3\Delta\mu_{\mathrm{O}} = \Delta H^{f}(\{\mathrm{Sr,Ba}\}\{\mathrm{Ce,Zr}\}\mathrm{O}_3), \tag*{(4)}

where ΔHf({Sr,Ba}{Ce,Zr}O3)\Delta H^{f}(\{\mathrm{Sr,Ba}\}\{\mathrm{Ce,Zr}\}\mathrm{O}_3) is the enthalpy of formation for {Sr,Ba}{Ce,Zr}O3\{\mathrm{Sr,Ba}\}\{\mathrm{Ce,Zr}\}\mathrm{O}_3. Our calculated enthalpies of formation are listed in Table 1.

CompoundΔHf\Delta H^f (eV) (calc)ΔHf\Delta H^f (eV) (exp)
SrCeO3_3−16.87−17.49 36
BaCeO3_3−16.77−17.52 36
SrZrO3_3−17.38−18.28 37
BaZrO3_3−17.29−18.28 37
SrCO3_3−11.98−12.65 38
BaCO3_3−11.91−12.58 38
SrO−5.61−6.14 38
BaO−5.09−5.68 38
ZrO2_2−10.99−11.41 38
CeO2_2−11.29−11.29 38
Y2_2O3_3−19.05−19.75 38

Table 1. Calculated and reported enthalpies of formation (in eV per formula unit) for compounds pertinent to this study.

For the purposes of presenting our results, we will use ΔμO=−2.42\Delta\mu_{\mathrm{O}} = -2.42 eV, as we have done in previous studies, which is representative of sintering SZO in air at 1650 °C. 9,30,39 These conditions favor VOV_{\mathrm{O}} formation, as is desired in device applications. Once ΔμO\Delta\mu_{\mathrm{O}} is chosen, eq 4 fixes the sum of Δμ{Sr,Ba}\Delta\mu_{\{\mathrm{Sr,Ba}\}} and Δμ{Ce,Zr}\Delta\mu_{\{\mathrm{Ce,Zr}\}}. We focus on {Sr,Ba}\{\mathrm{Sr,Ba}\}-poor ({Ce,Zr}\{\mathrm{Ce,Zr}\}-rich) values, where Δμ{Ce,Zr}\Delta\mu_{\{\mathrm{Ce,Zr}\}} is maximized through equilibrium with {Ce,Zr}O2\{\mathrm{Ce,Zr}\}\mathrm{O}_2. These conditions lead to higher carbon concentrations and therefore reflect a worst-case scenario at the chosen oxygen chemical potential. Choosing a specific set of chemical potential conditions is important for purposes of presenting our results; however, other conditions can easily be examined by referring to eq 2. Importantly, our results comparing relative formation energies are not affected by the particular choice of chemical potentials.

We focus on yttrium (Y{Ce,Zr}−\mathrm{Y}_{\{\mathrm{Ce,Zr}\}}^{-}) as the acceptor dopant, since it is the most commonly used dopant in both the cerates and the zirconates. [2] Chemical potentials for Y are chosen at the stability limit for our compounds relative to Y2_2O3_3:

2ΔμY+3ΔμO≤ΔHf(Y2O3).(5)2\Delta\mu_{\mathrm{Y}} + 3\Delta\mu_{\mathrm{O}} \leq\Delta H^f(\mathrm{Y}_2\mathrm{O}_3). \tag*{(5)}

For carbon, we consider values for ΔμC\Delta\mu_{\mathrm{C}} corresponding to the solubility limit by referring to the limiting condition of carbonate formation:

Δμ{Sr,Ba}+ΔμC+3ΔμO≤ΔHf({Sr,Ba}CO3).(6)\Delta\mu_{\{\mathrm{Sr,Ba}\}} + \Delta\mu_{\mathrm{C}} + 3\Delta\mu_{\mathrm{O}} \leq\Delta H^f(\{\mathrm{Sr,Ba}\}\mathrm{CO}_3). \tag*{(6)}

Considering that SrCO3_3 and BaCO3_3 are often used as precursors in synthesis of the cerates and zirconates, 4,10,14 this limiting condition is appropriate. For higher values of ΔμC\Delta\mu_{\mathrm{C}}, the carbonate phases will form preferentially to the zirconates and cerates; thus, for any choice of Δμ{Sr,Ba}\Delta\mu_{\{\mathrm{Sr,Ba}\}} and ΔμO\Delta\mu_{\mathrm{O}}, this condition determines the maximum allowed carbon chemical potential. For more oxygen-rich conditions, the limiting value for ΔμC\Delta\mu_{\mathrm{C}} will decrease; as a result, more oxygen-rich conditions require lower carbon chemical potentials (less carbon in the environment) to avoid destabilizing the zirconates and cerates against their respective carbonate phases.

Results and Discussion

Properties of Point Defects and Impurities

In order to plot defect formation energies, we must choose specific chemical potential conditions. As discussed, we focus on the {Sr,Ba}\{\mathrm{Sr,Ba}\}-poor limit, where ΔμC\Delta\mu_{\mathrm{C}} is maximized (“worst case” conditions). In Table 2, we list the maximum values of ΔμC\Delta\mu_{\mathrm{C}} for ΔμO=−2.42\Delta\mu_{\mathrm{O}} = -2.42 eV, which reflects typical synthesis conditions, and for ΔμO=−1\Delta\mu_{\mathrm{O}} = -1 eV, which represents more O-rich conditions (we include the full chemical potentials in Tables S1 and S2 in the SI). Values of ΔμC\Delta\mu_{\mathrm{C}} will vary linearly within this range. The values in Table 2 show that greater values of ΔμC\Delta\mu_{\mathrm{C}} are permitted in the zirconates as compared to the cerates, which means that the zirconates are stable with respect to carbonates under a broader range of environments. Moving to more O-poor synthesis (i.e., lowering ΔμO\Delta\mu_{\mathrm{O}}) will increase this limit and, correspondingly, the permissible range of carbon conditions.

Using the chemical potential conditions identified in Table 2 for ΔμO=−2.42\Delta\mu_{\mathrm{O}} = -2.42 eV, we plot defect formation energies for CiC_i, C{Ce,Zr}C_{\{\mathrm{Ce,Zr}\}}, VOV_{\mathrm{O}}, and Y{Ce,Zr}Y_{\{\mathrm{Ce,Zr}\}} in the cerates and zirconates in Figure 2. Note that results for other chemical potentials can readily be obtained by referring to eq 2. As we previously discovered for the zirconates,9 Ci+4C_i^{+4} is a very favorable carbon configuration, while CCe0C_{\mathrm{Ce}}^0 is higher in energy. In each case, carbon atoms bond with three neighboring oxygen atoms, with C–O bond lengths ranging from 1.28 Å to 1.30 Å, which matches the geometry of the CO32−\mathrm{CO}_3^{2-} ion (see Figure 1).

CompoundΔμC\Delta\mu_{\mathrm{C}} (eV) (ΔμO=−2.42\Delta\mu_{\mathrm{O}} = -2.42 eV)ΔμC\Delta\mu_{\mathrm{C}} (eV) (ΔμO=−1\Delta\mu_{\mathrm{O}} = -1 eV)
SrCeO3_3−1.43−4.27
BaCeO3_3−1.47−4.30
SrZrO3_3−0.75−3.59
BaZrO3_3−0.77−3.61

Table 2. Maximum carbon chemical potentials (at the {Sr,Ba}\{\mathrm{Sr,Ba}\}-poor limit) in the cerates and zirconates under selected oxygen chemical potential conditions.

Formation energies for oxygen vacancies, yttrium dopants, and carbon impurities in (a) SrCeO₃, (b) BaCeO₃, (c) SrZrO₃, and (d) BaZrO₃

Figure 2. Formation energies for oxygen vacancies, yttrium dopants, and carbon impurities in (a) SrCeO₃, (b) BaCeO₃, (c) SrZrO₃, and (d) BaZrO₃ under O-rich, {Sr,Ba}-poor conditions, and with ΔμO=−2.42\Delta\mu_{\mathrm{O}} = -2.42 eV.

We turn our attention to the Fermi level corresponding to charge neutrality in each system. For SCO, SZO and BZO, charge neutrality will be determined by compensation between Y{Ce,Zr}−Y_{\{\mathrm{Ce,Zr}\}}^- and VO+2V_{\mathrm{O}}^{+2}. In BCO, Ci+4C_i^{+4} will actually be the compensating donor species, and in SCO, the formation energy of Ci+4C_i^{+4} is very close to that of VO+2V_{\mathrm{O}}^{+2} at the position of charge neutrality, meaning that a large concentration of Ci+4C_i^{+4} will be present. In SZO and BZO, Ci+4C_i^{+4} has a much higher formation energy at the Fermi level corresponding to charge neutrality. The Ci+4C_i^{+4} species in BZO has a particularly high formation energy, helping to explain why low-energy acceptor dopants will not promote carbon contamination.40,41 Thus, we expect the cerates to contain higher concentrations of CiC_i species, even when carbonate formation is not thermodynamically favored. Dopants with lower formation energies than YCe−Y_{\mathrm{Ce}}^- would actually compensate with Ci+4C_i^{+4} in SCO. Choosing a dopant with a higher formation energy will decrease the carbon concentration, albeit at the expense of also decreasing the concentration of oxygen vacancies.

Choosing more carbon-poor conditions—as could be accomplished by avoiding the use of carbonate precursors during synthesis—increases the formation energy (and hence decreases the concentration) of both carbon species relative to the other defects. Changing the chemical potentials of host species ({Sr,Ba}\{\mathrm{Sr,Ba}\}, {Ce,Zr}\{\mathrm{Ce,Zr}\}, or O), however, will not qualitatively affect our observations. Indeed, we have checked that formation energies shift only modestly (by at most 0.2–0.3 eV) when moving from {Sr,Ba}\{\mathrm{Sr,Ba}\}-rich to {Sr,Ba}\{\mathrm{Sr,Ba}\}-poor conditions. This finding is directly related to the narrow windows of chemical stability in each compound, which are particularly narrow for the cerates (see Figure S1 in the SI). Furthermore, while changing ΔμO\Delta\mu_{\mathrm{O}} moves each individual formation energy line, it does not change the formation energies of species at the charge neutrality point; it simply has the net effect of shifting the position of the Fermi level (see Figure S2 in the SI).

Chemical potential phase diagrams for SrCeO3, SrZrO3, BaCeO3, and BaZrO3

Figure S1. Chemical potential phase diagrams for (a) SrCeO3_3, (b) SrZrO3_3, (c) BaCeO3_3, (d) BaZrO3_3. Competing phases are indicated.

Defect formation energy diagrams for SCO, BCO, SZO, and BZO under different chemical potential conditions

Figure S2. Defect formation energies for SCO under Sr-poor conditions for (a) ΔμO=−1\Delta\mu_{\mathrm{O}}=-1 eV and (b) ΔμO=−2.42\Delta\mu_{\mathrm{O}}=-2.42 eV; defect formation energies for BCO under Ba-poor conditions for (c) ΔμO=−1\Delta\mu_{\mathrm{O}}=-1 eV and (c) ΔμO=−2.42\Delta\mu_{\mathrm{O}}=-2.42 eV; defect formation energies for SZO under Sr-poor conditions for (e) ΔμO=−1\Delta\mu_{\mathrm{O}}=-1 eV and (f) ΔμO=−2.42\Delta\mu_{\mathrm{O}}=-2.42 eV; and defect formation energies for BZO under Ba-poor conditions for (g) ΔμO=−1\Delta\mu_{\mathrm{O}}=-1 eV and (h) ΔμO=−2.42\Delta\mu_{\mathrm{O}}=-2.42 eV.

This point is important to emphasize: carbon incorporation will not be affected by changing native chemical potentials unless equilibrium with the carbonate species is broken. Using a synthesis route that does not involve carbonate phases is thus essential to limit carbon incorporation. One possible method involves the use of nitrate precursors [Sr(NO3_3)2_2, Ba(NO3_3)2_2, Ce(NO3_3)3_3, and ZrO(NO3_3)2_2], which have previously been used for synthesis of both cerates42,43 and zirconates.44,45 We previously found nitrogen impurities to have high formation energies in the zirconates,9 which, following from the results we have just presented for carbon impurities, suggests that they will also have high formation energies in the cerates. As a result, nitrate precursors would be less deleterious for chemical stability.

Carbon Migration

To further understand carbon contamination, we study carbon mobility in the cerates and zirconates. To do so, we calculate migration barriers for carbon motion using the NEB method. The carbon interstitial will be the most mobile species. Ci+4C_i^{+4} typically prefers to be nestled between two {Ce,Zr}O6\{\mathrm{Ce,Zr}\}\mathrm{O}_6 octahedra, which share one oxygen atom to which a C–O bond is formed. The other two C–O bonds connect Ci+4C_i^{+4} with one oxygen atom in each of the octahedra (left panel of Figure 3). We investigate two primary pathways for Ci+4C_i^{+4} migration, which differ in the way in which the Ci+4C_i^{+4} species can get around these nearby oxygen atoms: passing directly between them in a straight line, or swinging around them by moving out-of-plane. These two possible pathways are shown schematically in Figure 3. We find that the “swinging” mechanism (the lower pathway in Figure 3) is much more

Migration pathway for the carbon interstitial in the cerates and zirconates

Figure 3. Migration pathway for the carbon interstitial (Ci+4\mathrm{C}_{i}^{+4}) in the cerates and zirconates. The top pathway has a higher energetic barrier than the lower pathway.

favorable, even though several new C–O bonds are formed and broken during the process. In the higher-energy “passing-between” pathway (the upper pathway of Figure 3), the saddle-point configuration forces carbon to adopt a two-fold coordination with oxygen, which is unfavorable in light of carbon’s energetic preference to be coordinated with at least three oxygen atoms.

In Table 3, we list migration barriers for the lowest-energy pathways we have calculated for Ci\mathrm{C}_{i} in each material. For materials sharing an A–site cation, the zirconates have larger barriers for migration. It has been suggested that the cubic symmetry of BZO is related to its stability with respect to carbon; 15 however, it is clear that migration barriers alone do not bear out that supposition. The migration barrier for BZO is slightly larger than that of the other materials, but its barrier relative to SZO is in line with the same trend in the cerates, making it difficult to point to symmetry as a determining factor. Overall, the barriers are such that we expect Ci+4\mathrm{C}_{i}^{+4} to be mobile during synthesis, and possibly also during device operation, which is typically at temperatures on the order of 1000 K.

MaterialCi+4\mathrm{C}_{i}^{+4} (eV)Ebind[Ci+4E_{\mathrm{bind}}[\mathrm{C}_{i}^{+4}–Y{Ce,Zr}−]\mathrm{Y}_{\{\mathrm{Ce,Zr}\}}^{-}] (eV)
SrCeO3_31.030.52
BaCeO3_32.130.60
SrZrO3_31.870.95
BaZrO3_32.390.98

Table 3. Calculated migration barriers EbE_b and binding energies (with the yttrium acceptor dopant) EbindE_{\mathrm{bind}} for carbon interstitials in proton-conducting oxides.

An additional important consideration for mobility is the binding energy of complexes between acceptor dopants and carbon impurities.

As acceptors like YZr−\mathrm{Y}_{\mathrm{Zr}}^{-} have an opposite charge to Ci+4\mathrm{C}_{i}^{+4}, there will be a Coulombic binding energy hindering the movement of carbon in highly doped samples. Dopants may in fact trap carbon impurities as they move within the material, potentially decelerating decomposition reactions.

We calculate the binding energy between an acceptor A−A^{-} and a donor D+D^{+} as:

Ebind(AD)=Ef(A−)+Ef(D+)−Ef(AD),(7)E_{\mathrm{bind}}(AD) = E^{f}(A^{-}) + E^{f}(D^{+}) - E^{f}(AD), \tag*{(7)}

where Ef(A−)E^{f}(A^{-}) and Ef(D+)E^{f}(D^{+}) are formation energies of isolated defects and Ef(AD)E^{f}(AD) is the formation energy of a complex containing both defects in close proximity in the same simulation cell. Practically speaking, EbindE_{\mathrm{bind}} is a dissociation energy needed to break apart defect complexes. Given that Ci+4\mathrm{C}_{i}^{+4} is the most significant mobile defect species, we calculate its binding energy with yttrium acceptors in the cerates and zirconates. These energies will need to be overcome, in addition to the migration barriers previously calculated, for carbon to be mobile.

Our calculated binding energies are listed in the second column of Table 3. Clearly, binding energies are significantly smaller in the cerates than in the zirconates, which, coupled with our results for migration barriers, further demonstrates that carbon will be more mobile in the cerates. Combining these binding energies with the calculated migration barriers, we can conclude that carbon will be largely immobile in the zirconates at the operating temperature, but can relatively easily penetrate the cerates. Alloying the cerates with the zirconates will increase binding energies and migration barriers, which helps to explain the better stability observed in alloyed materials. 7,14–17

Conclusions

We have examined the formation and mobility of carbon impurity species in the cerates and zirconates. We show that the cerates have lower chemical stability with respect to carbonates at specific oxygen chemical potentials, and that synthesis at more oxygen-poor conditions will permit a wider range of carbon chemical potentials while avoiding carbonate formation. But carbonate formation is not the only concern: we find that interstitial Ci+4\mathrm{C}_{i}^{+4} can incorporate in both the cerates and the zirconates, and it competes with VO+2\mathrm{V}_{\mathrm{O}}^{+2}, thus hindering prospects for proton conduction. Carbon contamination is particularly severe for the cerates, because of both the lower formation energy of Ci\mathrm{C}_{i} as well as the higher mobility of interstitial carbon, which allows carbon to penetrate into the cerates at typical operating temperatures. Choosing dopants other than yttrium can suppress carbon incorporation, but at the expense of lowering VO\mathrm{V}_{\mathrm{O}} concentrations.

We also find that simply changing host-atom chemical potentials during synthesis cannot suppress carbon incorporation, and thus avoiding exposure to carbon is essential for the cerates; use of precursors other than carbonates could be a promising route. Exposure to carbon during operation will also be detrimental for cerates. Overall, the zirconates are less sensitive to all of these deleterious effects, and therefore, alloying cerates with zirconates will improve stability. For pure cerates, completely avoiding carbon contamination will be crucial for unlocking their performance in proton-conducting applications.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

A.J.E.R. was supported by the National Science Foundation (NSF) Graduate Research Fellowship Program under Grant No. 1650114. Any opinions, findings, and conclusions or recommendations expressed in this material are those of the author(s) and do not necessarily reflect the views of the NSF. M.W.S. acknowledges support from the Naval Research Laboratory Postdoctoral Fellowship through the American Society for Engineering Education. C.G.V.d.W. was supported by the Office of Science of the U.S. Department of Energy (DOE) (Grant No. DE-FG02-07ER46434). We acknowledge the use of the Center for Scientific Computing supported by the California NanoSystems Institute and the Materials Research Science and Engineering Center (MR-SEC) at UC Santa Barbara through NSF DMR 1720256 and NSF CNS 0960316. We also acknowledge computational resources provided through the National Energy Research Scientific Computing Center, a DOE Office of Science User Facility supported by the Office of Science of the U.S. DOE under Contract No. DE-AC02-05CH11231.

Supporting Information (SI): Understanding Carbon Contamination in Proton Conducting Oxides

Andrew J. E. Rowberg; Michael W. Swift; Chris G. Van de Walle

Chemical Potential Tables

As discussed in the main text, we consider two selected oxygen chemical potential conditions: ΔμO=−2.42\Delta\mu_{\mathrm{O}} = -2.42 eV, which corresponds to experimental sintering conditions, [1] and ΔμO=−1\Delta\mu_{\mathrm{O}} = -1 eV, which represents more O-rich conditions. Table 2 in the main text lists the maximum allowed carbon chemical potentials under both of these conditions, assuming Sr/Ba-poor synthesis. In Table S1, we list the full chemical potentials (Δμ{Sr,Ba}\Delta\mu_{\{\mathrm{Sr,Ba}\}}, Δμ{Ce,Zr}\Delta\mu_{\{\mathrm{Ce,Zr}\}} and ΔμC\Delta\mu_{\mathrm{C}}) for the cerates and zirconates for ΔμO=−2.42\Delta\mu_{\mathrm{O}} = -2.42 eV. In Table S2, we do the same for ΔμO=−1\Delta\mu_{\mathrm{O}} = -1 eV.

CompoundΔμ{Sr,Ba}\Delta\mu_{\{\mathrm{Sr},\mathrm{Ba}\}} (eV)Δμ{Ce,Zr}\Delta\mu_{\{\mathrm{Ce},\mathrm{Zr}\}} (eV)ΔμC\Delta\mu_{\mathrm{C}} (eV)
SrCeO3\mathrm{SrCeO}_{3}−3.29-3.29−6.45-6.45−1.43-1.43
BaCeO3\mathrm{BaCeO}_{3}−3.18-3.18−6.45-6.45−1.47-1.47
SrZrO3\mathrm{SrZrO}_{3}−3.97-3.97−6.15-6.15−0.75-0.75
BaZrO3\mathrm{BaZrO}_{3}−3.88-3.88−6.15-6.15−0.77-0.77

Table S1. Chemical potentials in the cerates and zirconates at C-rich, Sr/Ba-poor conditions, with ΔμO=−2.42\Delta\mu_{\mathrm{O}}=-2.42 eV.

CompoundΔμ{Sr,Ba}\Delta\mu_{\{\mathrm{Sr},\mathrm{Ba}\}} (eV)Δμ{Ce,Zr}\Delta\mu_{\{\mathrm{Ce},\mathrm{Zr}\}} (eV)ΔμC\Delta\mu_{\mathrm{C}} (eV)
SrCeO3\mathrm{SrCeO}_{3}−4.71-4.71−9.29-9.29−4.27-4.27
BaCeO3\mathrm{BaCeO}_{3}−4.60-4.60−9.29-9.29−4.31-4.31
SrZrO3\mathrm{SrZrO}_{3}−5.39-5.39−8.99-8.99−3.59-3.59
BaZrO3\mathrm{BaZrO}_{3}−5.30-5.30−8.99-8.99−3.61-3.61

Table S2. Chemical potentials in the cerates and zirconates at C-rich, Sr/Ba-poor conditions, with ΔμO=−1\Delta\mu_{\mathrm{O}}=-1 eV.

Chemical Stability Diagrams

We plot the chemical stability regions (shaded in gray) for the cerates and zirconates in Figure S1. The stability regions for each cerate and zirconate are narrow in Δμ{Ce,Zr}\Delta\mu_{\{\mathrm{Ce},\mathrm{Zr}\}}-vs.-ΔμO\Delta\mu_{\mathrm{O}} space. For each compound, the widths are as follows: 0.05 eV for SCO [Figure S1], 0.39 eV for SZO [Figure S1], 0.26 eV for BCO [Figure S1], and 0.61 eV for BZO [Figure S1]. The narrow widths explain the low variability in formation energies when comparing the Sr/Ba-rich and Sr/Ba-poor limits. Note that Refs. 2,3 considered additional limiting phases for SCO and BCO; however, for the oxygen chemical potentials of interest, the regions where those phases form are not relevant, so we neglect them here.

Effect of Changing ΔμO\Delta\mu_{\mathrm{O}} on Formation Energy Diagrams

As discussed in the main text, changing the oxygen chemical potential does not change the formation energy at the charge neutrality point; instead, it merely shifts the Fermi level at which charge neutrality is achieved to lower energies. We show this trend graphically for each compound in Figure S2, with results for ΔμO=−1\Delta\mu_{\mathrm{O}}=-1 eV in the left column and those for ΔμO=−2.42\Delta\mu_{\mathrm{O}}=-2.42 eV (also shown in Figure 2 in the main text) on the right. Sr/Ba-poor conditions are used throughout.

References

  1. [1]Yajima, T.; Suzuki, H.; Yogo, T.; Iwahara, H. Protonic conduction in SrZrO₃-based oxides. Solid State Ionics 1992, 51, 101–107.DOI
  2. [2]Swift, M.; Janotti, A.; Van de Walle, C. G. Small polarons and point defects in barium cerate. Phys. Rev. B 2015, 92, 214114.DOI
  3. [3]Swift, M.; Van de Walle, C. G. Impact of point defects on proton conduction in strontium cerate. J. Phys. Chem. C 2016, 120, 9562–9568.DOI

Paper details

vlnc:W_mcym66q5
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 10

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents