A strategy for fabricating micro-scale freestanding single-crystalline complex oxide device arrays

Abstract

We present a general fabrication strategy for freestanding single-crystalline complex oxide device arrays via wet chemical etching-based microfabrication processes and epitaxial lift-off. Here, we used 0.5Ba(Zr0.2_{0.2}Ti0.8_{0.8})O3_3-0.5Ba(Zr0.7_{0.7}Ti0.3_{0.3})O3_3 (BCZT) as a model relaxor ferroelectric oxide system and La0.7_{0.7}Sr0.3_{0.3}MnO3_3 as the sacrificial layer for demonstration. Arrays of SrRuO3_3 (SRO) / BCZT / SRO ferroelectric capacitor mesas were first defined and isolated on the growth wafer, and then they were released using epitaxial lift-off with lithography-defined surrounding etching holes, after which the freestanding device arrays were integrated onto a glass substrate. Our proposed strategy sheds light on preparing various freestanding single-crystalline oxide devices and paves the way for their heterogeneous integration onto arbitrary substates.

Introduction

Epitaxial lift-off (ELO) is a technological process designed to obtain freestanding single crystalline films by releasing thin epitaxial layers from their original growth substrates[1]. This technique has been successfully employed on III-V materials over the past 30 years[2, 3, 4] to produce their heterogeneously integrated electronics and optoelectronics[5, 6, 7] that feature device characteristics not possible with film-on-substrate geometry, novel mechanical and electronic functionalities, and reduced costs. Epitaxially grown complex oxides belong to an interesting class of materials that have shown rich physical and functional properties ranging from ferroelectricity[8, 9, 10], high mobility electron-gas[11], superconductivity[12, 13, 14], to engineered interface phenomena[11, 15, 16], however, the extended applications of these exciting phenomena have been limited by the form of rigid films that directly grow on single crystalline oxide substrates for a long time. Inspired by the success of freestanding III-V device applications[2, 5] and the proliferation of research on mechanically stacked 2D heterostructures[17, 18], recently, there is a rapid increase of interests in developing ELO-based processes for obtaining freestanding single-crystalline complex oxides and further achieving their heterogeneous integration[19, 20, 21, 22]. In this experimental scheme, an epitaxially-grown, sacrificial layer (La0.7Sr0.3MnO3\mathrm{La}_{0.7}\mathrm{Sr}_{0.3}\mathrm{MnO}_{3} (LSMO)[19, 20] or Sr3Al2O6\mathrm{Sr}_{3}\mathrm{Al}_{2}\mathrm{O}_{6} (SAO)[21, 22]) is inserted between the oxide substrate and active oxide layers[21, 22, 23] during the growth and is then laterally etched to release the entire top stack, which is then transferred and integrated on various desired materials or substrates[19, 20].

Following several pioneering work in the mid 2010s[19, 21], a wide variety of freestanding single crystalline oxide films have been obtained and heterogeneously integrated with flexible substrates or semiconductors, enabling several unique applications such as flexible oxide electronics[20, 24], high-κ\kappa gating dielectric integrations[25, 26] and extreme strain modulations[27, 28] that cannot be achieved with as-grown complex oxides. Nonetheless, most of current research centers on either obtaining the entire oxide membrane[29, 30, 31] or unitizing a single broken piece of micro-flake for material characterization and prototype device demonstration[26, 32]. The large-scale-compatible fabrication procedures of single-crystalline freestanding complex oxide devices or device arrays remain largely underexplored, compared to well-established III-V materials.

Here, using relaxor ferroelectric 0.5Ba(Zr0.2Ti0.8)O30.5\mathrm{Ba}(\mathrm{Zr}_{0.2}\mathrm{Ti}_{0.8})\mathrm{O}_3-0.5Ba(Zr0.7Ti0.3)O30.5\mathrm{Ba}(\mathrm{Zr}_{0.7}\mathrm{Ti}_{0.3})\mathrm{O}_3 (BCZT) as a model complex oxide system, SrRuO3_3 (SRO) as both top and bottom electrodes, and LSMO as the oxide sacrificial layer, we present detailed microfabrication procedures of obtaining freestanding, isolated SRO/BCZT/SRO capacitor arrays and their heterogeneous integration. 10×1010 \times10 mesas of BCZT metal-insulator-metal (MIM) capacitor arrays were first individually defined and fabricated on the as-grown oxide wafer using standard photolithography and optimized wet chemical etching processes. Etch holes were implemented surrounding each device for lift-off, during which the LSMO etchant was delivered to the sacrificial layer through these etch holes in a controlled manner while the sidewalls of the active device stack remained well-protected. Moreover, the freestanding device arrays were retrieved either individually or as a whole from the growth substrate and integrated onto an alien substrate using a UV-curable adhesive. Our strategy, when combined with appropriate etching protocols, is generally applicable for fabricating many other micro-scale freestanding complex oxide devices or device arrays, which adds more exciting possibilities to the current oxide membrane research.

Epitaxial growth of releasable SRO/BCZT/SRO stack

BCZT, a solid solution of BaTiO3\mathrm{BaTiO}_3, is a lead-free relaxor ferroelectric that features high room temperature dielectric constant[33], large piezoelectric coefficient[33, 34], and strong electro-optic (EO) coupling[35], making it promising for various applications such as energy storage[36], actuators[33], and EO modulators[35]. Recently, a sub-group of the authors reported the epitaxial growth of high quality BCZT thin films using pulsed laser deposition (PLD)[37].

As illustrated in Figure 1a and 1b, the growth of the releasable BCZT device stack used in this work started with the formation of a 20 nm LSMO sacrificial layer on a TiO2_2-terminated SrTiO3_3 (STO) substrate, followed by a sequential deposition of 20 nm SRO bottom electrode layer, a 100 nm BCZT relaxor ferroelectric layer, and a 20 nm SRO top electrode layer in the same chamber. Optimal growth conditions were applied for each layer and reflection high energy electron diffraction (RHEED) was used to monitor the film quality and growth rate in situ. High quality SRO (aSRO=3.93a_{\mathrm{SRO}} = 3.93 Å) and BCZT (aBCZT=4.00a_{\mathrm{BCZT}} = 4.00 Å) films were obtained on LSMO with layer-by-layer growth, as revealed by the RHEED patterns and oscillations in the intensity of the specular spot as shown in Figure 1a. It is noted that LSMO has an in-plane lattice parameter of 3.87 Å, which is close to that of both STO substrate (aSTO=3.91a_{\mathrm{STO}} = 3.91 Å) and SRO layer, and hence the lattice mismatch is of ~ 1.5%. Figure 1c illustrates a representative θ\theta-2θ2\theta scan of the as-grown MIM

Image not extracted

Figure 1. (a) Representative oscillations in the RHEED specular spot intensity and diffraction patterns of LSMO (top), SRO (middle), and BCZT (bottom) layers during the growth. (b) Schematic illustration of the releasable epitaxial SRO/BCZT/SRO device stack. (c) θ\theta-2θ2\theta scan of an as-grown releasable BCZT epitaxial device stack.

epitaxial device stack using high-resolution thin film X-ray diffraction (XRD). The reflections of LSMO 002, SRO 220 and BCZT 002 were clearly observed, indicating a good epitaxial growth of each layer on the STO substrate.

In this experimental scheme, epitaxially grown conductive oxide SRO was employed as both top and bottom electrodes of the BCZT MIM capacitors to improve the metal-to-ferroelectric interface quality. Recently, such all-oxide MIM architecture has shown great promise in achieving excellent device performance such as low switching voltage and high endurance, as demonstrated in another archetypal perovskite ferroelectric BaTiO3\mathrm{BaTiO}_{3}38,39.

Fabrication of micro-scale, isolated all-oxide BCZT MIM capacitors

The entire micro-fabrication procedures for freestanding SRO/BCZT/SRO capacitors include the following three major steps: 1) fabrication of lithography-defined BCZT MIM capacitor arrays on wafer through wet chemical etching, 2) releasing of as-fabricated devices via epitaxial lift-off through surrounding etch holes, and 3) heterogeneous integration of freestanding device arrays on desired alien substrates, as illustrated in Figure 2.

Image not extracted

Figure 2. Schematic illustration of fabrication processes for micro-scale freestanding SRO/BCZT/SRO device arrays.

The on-wafer fabrication processes of all-oxide BCZT MIM capacitor arrays started with the definition of mesa-shaped active device arrays (10×1010 \times10, ∼100×100 μm2\sim100 \times100\ \mu\mathrm{m}^{2} each) using regular photolithography, followed by successive wet chemical etching of top SRO layer and BCZT layer (Figure 3a, bottom left and bottom right). A chemical etchant based on sodium periodate (0.40.4 mol/L NaIO4\mathrm{NaIO}_{4} in DI) was used for removing SRO, which has been reported effective with an intermediate etch rate of ∼2\sim2 nm/s [40]. It is important to note that the NaIO4\mathrm{NaIO}_{4}-based etchant removes SRO exclusively by oxidizing Ru species, which leads to a perfect etch stop at BCZT surface. A slight color change of the sample was noticed when comparing between the optical microscopic images taken before (Figure 3a, top right) and after SRO etching (Figure 3a, bottom left), which has been adopted to monitor the etching process. An etching step of ∼20\sim20 s in NaIO4\mathrm{NaIO}_{4} solution is typically sufficient to remove the SRO layer and no further discernible change in color can be observed even if the sample was left over a much longer time (e.g., ∼5\sim5 min) in the etchant.

Image not extracted

Figure 3. (a) Optical micrographic images of the mesa etch processes on wafer. Top SRO and BCZT layers were chemically etched sequentially (bottom left and bottom right) to form active regions of the SRO/BCZT/SRO device arrays. (b) Representative current-voltage (II-VV) characteristics of exposed top surfaces during etching. The stark contrast of electrical conductivity between metallic SRO and insulating BCZT has been used to monitor etching progresses.

On the other hand, the etchant for BCZT film has not been well established in the literature. Nonetheless, inspired by the chemical etchants reported for processing BaTiO3\mathrm{BaTiO}_{3}, Ba0.5Sr0.5TiO3\mathrm{Ba}_{0.5}\mathrm{Sr}_{0.5}\mathrm{TiO}_{3}, and Pb(ZrxTi1−x)O3\mathrm{Pb}(\mathrm{Zr}_{x}\mathrm{Ti}_{1-x})\mathrm{O}_{3}-based devices [41, 42], which is usually a mixture of buffered hydrofluoric acid (BHF) and acids such as HNO3\mathrm{HNO}_{3}, H2SO4\mathrm{H}_{2}\mathrm{SO}_{4}, HCl and H3PO4\mathrm{H}_{3}\mathrm{PO}_{4}, we optimized the BCZT etchant and etching processes based on BHF and HCl. As shown in Figure S5 and Figure S6, as-received BHF etchant (BOE 7:1) easily leaves significant etching residues despite its effectiveness in removing BCZT, while HCl etchant (HCl : DI = 1 :4, in volume) itself suffers from a slow etch rate, which is likely limited by the insufficient removal of Zr species. Therefore, the optimized BCZT etchant used for this study composes of both BHF and HCl (BHF : HCl : DI = 1 : 10 : 40, in volume), where small amount of HF is added to a diluted aqueous solution of HCl to effectively remove zirconium species, and hence, continuous etching of BCZT is achieved. Etching residues are minimized by gently swirling the container during the wet etching process and ~ 1 nm/s etch rate of BCZT film is typically obtained. An obvious and gradual color change was observed by bare eyes during the BCZT wet etching due to the thinning of the BCZT dielectric layer, which confirms the continuous removal of BCZT and has been used to monitor the etching progress. Figure 3a (bottom right) shows an optical microscopic image of the sample after the BCZT etching step, with the bottom SRO layer exposed. It is important to note that the bottom SRO layer also acts as a good etch stop for this optimized BCZT etchant, as evidenced by the electrical current-voltage (II-VV) measurements (Figure 3b). A two-probe resistance of ~ 1 kΩ was observed through direct tungsten probes on exposed oxide surfaces after BCZT etching, while it remains insulating before the

Optical microscopic images of BCZT wet etching test: (a) after patterning w. AZ1518, (b) BOE (7:1), 10 min, and (c) DI cleaning, overnight

Figure S5. BCZT wet etching test with HF-based etchant. Optical microscopic images of (a) photoresist patterning on a BCZT/SRO/STO test sample, (b) after wet etching in BOE (7:1) for 10 min. All the patterns and oxide films are gone, leaving a large amount of etching residues and a very rough surface. (c) after DI cleaning overnight.

BCZT wet etching test with HCl-based etchant

Figure S6. BCZT wet etching test with HCl-based etchant. (a) to (d) Optical microscopic images of a BCZT device stack before and after consecutive etching by HCl 1:4. The gradual change of color corresponds to the thinning and continuous etching of BCZT film. No discernible difference was observed between (c) and (d), which indicates that BCZT is not effectively removed in HCl-based etchant beyond certain amount of time. (e) and (f) BCZT etching continues by dipping the same piece of sample in BOE etchant for tens of seconds. Therefore, both HF and HCl contents were used to prepare the optimized BCZT etchant.

etching. Therefore, controlled wet etching processing of SRO/BCZT/SRO device stack with an excellent etching selectivity has been achieved.

Representative II-VV and PP-VV characteristics of such an SRO/BCZT/SRO ferroelectric capacitor fabricated on wafer are illustrated in Figure S7. A low switching voltage of <0.4<0.4 V was clearly observed in the system, consistent with previous reports on SRO/BTO/SRO-based ferroelectric systems[38, 39]. Moreover, the switching curve is more symmetric compared to previously reported SRO/BCZT/Ti/Au[37], thanks to the symmetric SRO electrode design.

Representative I-V and P-V characteristics of an SRO/BCZT/SRO capacitor fabricated on wafer

Figure S7. (a) and (b) Representative II-VV and PP-VV characteristics of an SRO/BCZT/SRO capacitor fabricated on wafer.

Epitaxial lift-off and heterogeneous integration

To release as-fabricated BCZT device arrays from the growth substrate, an epitaxial lift-off process with pre-defined surrounding etching holes was adopted. Similar strategy has been widely employed to fabricate freestanding III-V devices[6, 7, 43, 44]; however, to the best of our knowledge, no such attempt has been made on complex oxides. Isolated arrays of individual BCZT capacitors (∼180×180 μm2\sim180 \times180\ \mu\mathrm{m}^{2}) were first defined by photolithography and wet etching of the bottom SRO layer, followed by a partial etching step of the LSMO sacrificial layer in a diluted solution based on potassium iodide (KI) and HCl (Figure 4a) and subsequent photoresist etch holes formation (Figure 4b, left). It is noted that the channels for delivering the etchant to the LSMO sacrificial layer (etching holes) were made outside the active device area to minimize the exposure of BCZT sidewalls to the etchant such that undesired chemical etching-related degradation of the active devices can be minimized, as illustrated in Figure S3. Here, an “LL-shaped” etching holes arrangement design was employed for a proof-of-concept demonstration for complex oxides, which was originally optimized for III-V processing and found effective in mitigating the fracture at the cell centers due to stress accumulation, as reported in a study of freestanding triple-junction III-V solar cells by Gai et al[43]. In general, other surrounding etching hole designs with a different size/density/distribution would also serve the purpose of individual device releasing, although the overall etching time and device yield can be slightly affected.

Image not extracted

Figure 4. (a) Optical micrographs of SRO/BCZT/SRO device arrays after isolation patterning (left), isolation etching (middle), and PR removal (right). (b) Optical micrographic images of the devices after “L-shaped” etching holes formation (left), etching holes opening (middle), and undercut etching (right). (c) Optical micrographic and photographic images of freestanding SRO/BCZT/SRO device arrays after picked up by PDMS (left and right top) and transferred on glass (middle and right bottom).

Image not extracted

(a) without sidewall protection

Image not extracted

(b) with sidewall protection

Figure S3. Schematics of etching holes design of (a) without sidewall protection, and (b) with sidewall protection

After patterning the etching holes structure with photoresist, an additional SRO etching step was applied to “open” the etching holes by removing the bottom SRO layer in exposed regions (Figure 4b, middle). The undercut etching process was carried out by simply dipping the whole sample into the HCl/KI-based LSMO etchant[19, 20]. The etchant was delivered to each individual device through the surrounding etching holes simultaneously, which greatly reduces the overall undercut etching time, and it typically takes 3 to 4 hours to release devices with ∼200 μm\sim200\,\mu\mathrm{m} lateral dimensions (Figure S8). The chances of crack formation are relatively low in those devices during undercut etching and a high yield of 97/100 (without visible film cracks) was achieved, as illustrated in Figure 4b (right). This is primarily attributed to the improved mechanical support from photoresist “anchoring” and controlled etchant delivery through etching holes.

Optical microscopic image showing the undercut etching process

Figure S8. Optical microscopic image showing the undercut etching process, with ‘etched’ regions, ‘unetched’ regions, and PR ‘anchoring’ regions clearly labeled.

The freestanding BCZT device arrays were then picked up from the growth wafer using an elastomeric PDMS stamp and transferred onto a glass substrate, following the transfer printing procedures reported elsewhere[7, 43, 45], as shown in Figure 4c and S9. Here, a thin spin-on-glass-based UV-curable adhesive (∼1 μm\sim1\,\mu\mathrm{m} thick) was employed to facilitate the transfer process. Glass was chosen in this study for the proof-of-concept demonstration (Figure 4c) and other substrates such as silicon, flexible PET or polyimide sheets can be readily used depending on the needs of the actual application. An adhesive-free transfer process might need to be developed in the future for scenarios when the oxide-substrate interface is critical. For instance, a surface tension force-assisted van der Waals bonding method has been demonstrated for integrating freestanding GaAs films onto arbitrary substrates[46], which can be useful for developing similar processes for complex oxides. It is noted that ∼\sim20 more devices got cracked after pickup and transferring (Figure S10), which might be attributed to the over pressing of the PDMS stamp during the transfer process. Additional optimization of processing conditions would further improve the overall yield in the future.

Optical microscopic images of transferred SRO/BCZT/SRO device arrays

Figure S10. Optical microscopic images of transferred SRO/BCZT/SRO device arrays. Devices with cracks formed during the transfer process are labeled with white circles in (a). A zoomed-in image was shown in panel (b).

Discussion and Prospects

On the other hand, so far, electrical characterization of transferred BCZT capacitor arrays remains challenging with the current design of the device configuration, i.e., ∼100\sim100 nm-thick relaxor ferroelectric layer with a 20 nm-thick wing-shaped bottom SRO electrode (Figure 4c, middle) on a “soft” adhesive. Our attempts to directly probe SRO electrodes using tungsten tips in a probe station was not successful due to mechanical damage created on the transferred devices by the probes. To resolve this issue, one may need to explore a proper packaging route to electrically contact those device arrays in the future, including polymer encapsulation, VIA (vertical interconnect access) formation and metal interconnection, as has been widely applied in modern microchip manufacturing[47] and many studies on flexible and stretchable electronics[45, 48, 49]. A schematic of such device packing processes is illustrated in Figure S11.

Schematic design of the device packaging processes

Figure S11. Schematic design of the device packaging processes that could potentially resolve the current electrical characterization issue on transferred capacitor arrays, including “VIA hole formation” and “metal interconnection”.

Nonetheless, the proposed strategy and device fabrications procedures in this work are not only compatible to large-area device processing and packaging, but also generally applicable to many other commonly used complex oxide systems such as BaTiO3_3, PbZrx_xTi1−x_{1-x}O3_3, and PbTiO3_3/STO superlattices with minimal modifications in the specifications of the processes, especially etching proctols. Further, instead of using wet chemical etching that may lead to tapered sidewall profile, the anisotropic dry etching methods such as inductively coupled plasma-reactive ion etching can be applied to accurately define the active device shape (mesa etch step) and maintain vertical sidewalls. Vertical sidewalls are critical in developing freestanding optical devices such as waveguides and electro-optical modulators, as their device performance can be largely impacted by the distortion of device geometry, although the etching selectively can be largely compromised for physical bombardment processes. In the meantime, the etching holes-based releasing strategy still applies in this case.

Moreover, this strategy can be extended to systems using a water-soluble sacrificial layer such as SAO, which have been more popular than LSMO for obtaining freestanding oxide membranes over the years due to its simplicity on film release. The epitaxial lift-off strategy for oxide device arrays presented in this work is in principle compatible with those systems as well, with the potential for unnecessary sacrificial layer lateral etching during the device wet chemical processes such as photoresist developing and wet etching. For water-soluble layers that feature fast releasing such as Sr4Al2O7\mathrm{Sr}_{4}\mathrm{Al}_{2}\mathrm{O}_{7}[50], additional care needs to be taken when designing the on-wafer device processes to minimize the lateral etching, while for most of reported Sr3Al2O6\mathrm{Sr}_{3}\mathrm{Al}_{2}\mathrm{O}_{6} layers that require a few hours or days to release the oxide membranes[21, 51], such effect of lateral etching is expected to be minimal.

Conclusion

In conclusion, we have successfully fabricated freestanding capacitor device arrays of SRO/BCZT/SRO using wet chemical etching-based device fabrication processes and controlled epitaxial lift-off through etching holes. Our work sheds light on the heterogeneous integration of freestanding complex oxides for device applications.

Methods

Epitaxial thin film growth and structural analysis

A TSST PLD system with a 248 nm KrF excimer laser was used to deposit the BCZT device stack on either TiO2_2-terminated STO or GdSrO3_3 (GSO) substrate. LSMO, SRO, and BCZT films were grown under the same growth temperature of 750°C with fixed laser fluence of 1.5 J/cm2^2, while the growth oxygen pressure was tuned accordingly to optimize the film quality (LSMO: 20 mbar, SRO: 100 mbar, and BCZT: 10 mbar). The device stack was then cooled to room temperature at a rate of 5 ∘C5\,^{\circ}\mathrm{C}/min after growth.

The high-resolution thin film out-of-plane X-ray diffraction scan was performed in a Bruker D8 Advance diffractometer using a Ge (004) two bounce monochromator with Cu radiation at room temperature.

A BCZT/LSMO/GSO sample was prepared separately and the entire BCZT film was released following a conventional undercut etching and polymer stamping method[21] to characterize the quality of transferred BCZT film. A comparison of XRD scans before and after transfer are illustrated in Figure S1 and Figure S2 shows piezoelectric force microscopy (PFM) characterization of a transferred BCZT film.

XRD scan of BCZT film before and after transfer

Figure S1. XRD scan of BCZT film (a) before and (b) after transfer. Each reflection is indexed with corresponding material. The insets on the right are the short-angle XRD scans for 42-49° near the most intense 002 reflection of BCZT.

Image not extracted

Figure S2. PFM responses of transferred BCZT films. (a) Schematic illustration of PFM setup for characterizing transferred BCZT film. The box-in-box pattern is shown in terms of phase and amplitude in (b) and (c), respectively. (d) and (e) show the amplitude and phase responses as a function of field. A 100 nm-thick BCZT film was used for the measurement and the shape of BCZT hysteresis loop illustrates the characteristic feature of a relaxor ferroelectric.

Device fabrication

Regular photolithography was employed to form all the required patterns with AZ1518 positive photoresist (Merck KGaA, with 110∘C110^{\circ}\mathrm{C}, 3 min hard bake before etching) and MJB3 (Karl Suss) mask aligner for each wet chemical etching step. Samples with only 1-2 mm lateral dimensions (broken from a 5 mm×5 mm5\ \mathrm{mm} \times5\ \mathrm{mm} as grown substrate) were used for wet etching condition optimization.

Additional care has been taken to handle photolithography processes on those small samples to minimize the edge bead formation, as illustrated in Figure S4. With the use of supporting substrates for spin-coating, relatively flat photoresist films can be obtained.

Image not extracted

Figure S4. Schematics of photoresist spin-coating on small-sized PLD-grown oxide samples. (a) direct spin-coating on small samples without supporting substrates around, which leads to sever edge bead issues, and (b) spin coating on small samples with supporting substrates. Edges bead issue is minimized with supporting substrates, and hence, flat photoresist coating can be obtained. This is particularly important for fabricating devices on small pieces of oxide samples with lateral dimensions smaller than 2 mm.

0.4 mol/L0.4\ \mathrm{mol}/\mathrm{L} NaIO4_4 (>99.8%>99.8\%, Sigma Aldrich) in DI was used as the SRO etchant. The optimized BCZT etchant (BHF : HCl : DI = 1 : 10 : 40) was prepared by first preparing a mixture of HCl (36.5-38 %, VWR Chemicals BDH): DI with 1 : 4 ratio in volume, and then 1 part of BHF (7 : 1, J.T.Baker) was added to 10 parts of the diluted HCl mixture in volume. The stock BCZT etchant can be still effective even after several months. The LSMO etchant was prepared by mixing 4 mg KI, 5 mL HCl, and 200 mL DI water, following the recipe reported elsewhere[19, 20].

Electrical II-VV measurements were carried out on a probe station (M&M Micromanipulator) using a semiconductor analyzer (Agilent 4156C). Tungsten probes were used to directly contact exposed film after each etching step to check its electrical conductivity, and hence, to confirm the etching progress.

Supporting Information

XRD of BCZT before and after transfer; PFM of transferred BCZT; schematics of device fabrication steps; optical microscopic images showing the optimization of BCZT wet etchant; II-VV characteristics of SRO/BCZT/SRO device fabricated on wafer; optical microscopic images showing different device fabrication steps; schematic design of the device packaging processes for device array interconnection.

Author declarations

Author contributions

H.C. and J.R. conceived the idea and designed the experiments. Y.L., H.K., and M.S. grew the samples by PLD and carried out XRD measurements. Y.L. performed PFM measurements. H.C. fabricated devices. H.C. and J.R. wrote the manuscript with input from all other authors.

Acknowledgements

We gratefully acknowledge support from an ARO MURI program (W911NF-21-1-0327). The growth equipment used for the materials synthesis were supported by an Air Force Office of Scientific Research grant (FA9550-22-1-0117).

Conflict of interest

The authors declare no competing financial interests.

Supporting Information

Optical microscopic image showing STO substrate after freestanding SRO/BCZT/SRO device arrays were picked up using PDMS stamp

Figure S9. Optical microscopic image showing STO substrate after freestanding SRO/BCZT/SRO device arrays were picked up using PDMS stamp. PR ‘anchoring’ was left on the substrate.

References

  1. [1]Demeester, P.; Pollentier, I.; De Dobbelaere, P.; Brys, C.; Van Daele, P. Epitaxial lift-off and its applications. Semicond. Sci. Technol. 1993, 8 (6), 1124.DOI
  2. [2]Cheng, C.-W.; Shiu, K.-T.; Li, N.; Han, S.-J.; Shi, L.; Sadana, D. K. Epitaxial lift-off process for gallium arsenide substrate reuse and flexible electronics. Nat. Commun. 2013, 4 (1), 1577.DOI
  3. [3]Van Geelen, A.; Hageman, P.; Bauhuis, G.; Van Rijsingen, P.; Schmidt, P.; Giling, L. Epitaxial lift-off GaAs solar cell from a reusable GaAs substrate. Mater. Sci. Eng., B 1997, 45 (1-3), 162-171.
  4. [4]Yoon, J.; Jo, S.; Chun, I. S.; Jung, I.; Kim, H.-S.; Meitl, M.; Menard, E.; Li, X.; Coleman, J. J.; Paik, U. GaAs photovoltaics and optoelectronics using releasable multilayer epitaxial assemblies. Nature 2010, 465 (7296), 329-333.DOI
  5. [5]Bauhuis, G. J.; Mulder, P.; Haverkamp, E. J.; Huijben, J.; Schermer, J. J. 26.1% thin-film GaAs solar cell using epitaxial lift-off. Sol. Energy Mater. Sol. Cells 2009, 93 (9), 1488-1491.DOI
  6. [6]Gai, B.; Sun, Y.; Lim, H.; Chen, H.; Faucher, J.; Lee, M. L.; Yoon, J. Multilayer-grown ultrathin nanostructured GaAs solar cells as a cost-competitive materials platform for III–V photovoltaics. ACS Nano 2017, 11 (1), 992-999.DOI
  7. [7]Kang, D.; Young, J. L.; Lim, H.; Klein, W. E.; Chen, H.; Xi, Y.; Gai, B.; Deutsch, T. G.; Yoon, J. Printed assemblies of GaAs photoelectrodes with decoupled optical and reactive interfaces for unassisted solar water splitting. Nat. Energy 2017, 2 (5), 1-5.DOI
  8. [8]Dawber, M.; Rabe, K.; Scott, J. Physics of thin-film ferroelectric oxides. Rev. Mod. Phys. 2005, 77 (4), 1083.DOI
  9. [9]Choi, K. J.; Biegalski, M.; Li, Y.; Sharan, A.; Schubert, J.; Uecker, R.; Reiche, P.; Chen, Y.; Pan, X.; Gopalan, V. Enhancement of ferroelectricity in strained BaTiO3 thin films. Science 2004, 306 (5698), 1005-1009.pubmed.ncbi.nlm.nih.gov/15528439
  10. [10]Cohen, R. E. Origin of ferroelectricity in perovskite oxides. Nature 1992, 358 (6382), 136-138.DOI
  11. [11]Ohtomo, A.; Hwang, H. A high-mobility electron gas at the LaAlO3/SrTiO3 heterointerface. Nature 2004, 427 (6973), 423-426.pubmed.ncbi.nlm.nih.gov/14749825
  12. [12]Hong, M.; Liou, S. H.; Kwo, J.; Davidson, B. Superconducting Y-Ba-Cu-O oxide films by sputtering. Appl. Phys. Lett. 1987, 51 (9), 694-696.DOI
  13. [13]Schooley, J.; Hosler, W.; Cohen, M. L. Superconductivity in semiconducting SrTiO3. Phys. Rev. Lett. 1964, 12 (17), 474.
  14. [14]Ahadi, K.; Galletti, L.; Li, Y.; Salmani-Rezaie, S.; Wu, W.; Stemmer, S. Enhancing superconductivity in SrTiO3 films with strain. Sci. Adv. 2019, 5 (4), eaaw0120.DOI
  15. [15]Yadav, A.; Nelson, C.; Hsu, S.; Hong, Z.; Clarkson, J.; Schlepütz, C.; Damodaran, A.; Shafer, P.; Arenholz, E.; Dedon, L. Observation of polar vortices in oxide superlattices. Nature 2016, 530 (7589), 198-201.DOI
  16. [16]Lee, H.; Campbell, N.; Lee, J.; Asel, T.; Paudel, T.; Zhou, H.; Lee, J.; Noesges, B.; Seo, J.; Park, B. Direct observation of a two-dimensional hole gas at oxide interfaces. Nat. Mater. 2018, 17 (3), 231-236.DOI
  17. [17]Novoselov, K.; Mishchenko, A.; Carvalho, A.; Castro Neto, A. 2D materials and van der Waals heterostructures. Science 2016, 353 (6298), aac9439.DOI
  18. [18]Fan, S.; Vu, Q. A.; Tran, M. D.; Adhikari, S.; Lee, Y. H. Transfer assembly for two-dimensional van der Waals heterostructures. 2D Mater. 2020, 7 (2), 022005.DOI
  19. [19]Bakaul, S. R.; Serrao, C. R.; Lee, M.; Yeung, C. W.; Sarker, A.; Hsu, S.-L.; Yadav, A. K.; Dedon, L.; You, L.; Khan, A. I. Single crystal functional oxides on silicon. Nat. Commun. 2016, 7 (1), 1-5.arxiv.org/abs/1511.06832
  20. [20]Bakaul, S. R.; Serrao, C. R.; Lee, O.; Lu, Z.; Yadav, A.; Carraro, C.; Maboudian, R.; Ramesh, R.; Salahuddin, S. High speed epitaxial perovskite memory on fexible substrates. Adv. Mater. 2017, 29 (11).DOI
  21. [21]Lu, D.; Baek, D. J.; Hong, S. S.; Kourkoutis, L. F.; Hikita, Y.; Hwang, H. Y. Synthesis of freestanding single-crystal perovskite films and heterostructures by etching of sacrificial water-soluble layers. Nat. Mater. 2016, 15 (12), 1255-1260.DOI
  22. [22]Ji, D.; Cai, S.; Paudel, T. R.; Sun, H.; Zhang, C.; Han, L.; Wei, Y.; Zang, Y.; Gu, M.; Zhang, Y. Freestanding crystalline oxide perovskites down to the monolayer limit. Nature 2019, 570 (7759), 87-90.DOI
  23. [23]Shen, L.; Wu, L.; Sheng, Q.; Ma, C.; Zhang, Y.; Lu, L.; Ma, J.; Ma, J.; Bian, J.; Yang, Y. Epitaxial lift-off of centimeter-scaled spinel ferrite oxide thin films for flexible electronics. Adv. Mater. 2017, 29 (33), 1702411.DOI
  24. [24]Luo, Z.-D.; Peters, J. J.; Sanchez, A. M.; Alexe, M. Flexible memristors based on single-crystalline ferroelectric tunnel junctions. ACS Appl. Mater. Interfaces 2019, 11 (26), 23313-23319.DOI
  25. [25]Huang, J.-K.; Wan, Y.; Shi, J.; Zhang, J.; Wang, Z.; Wang, W.; Yang, N.; Liu, Y.; Lin, C.-H.; Guan, X. High-κ perovskite membranes as insulators for two-dimensional transistors. Nature 2022, 605 (7909), 262-267.DOI
  26. [26]Yang, A. J.; Han, K.; Huang, K.; Ye, C.; Wen, W.; Zhu, R.; Zhu, R.; Xu, J.; Yu, T.; Gao, P. Van der Waals integration of high-k perovskite oxides and two-dimensional semiconductors. Nat. Electron. 2022, 5 (4), 233-240.DOI
  27. [27]Hong, S. S.; Gu, M.; Verma, M.; Harbola, V.; Wang, B. Y.; Lu, D.; Vailionis, A.; Hikita, Y.; Pentcheva, R.; Rondinelli, J. M. Extreme tensile strain states in La₀.₇Ca₀.₃MnO₃ membranes. Science 2020, 368 (6486), 71-76.DOI
  28. [28]Xu, R.; Huang, J.; Barnard, E. S.; Hong, S. S.; Singh, P.; Wong, E. K.; Jansen, T.; Harbola, V.; Xiao, J.; Wang, B. Y. Strain-induced room-temperature ferroelectricity in SrTiO₃ membranes. Nat. Commun. 2020, 11 (1), 3141.DOI
  29. [29]Gu, K.; Katayama, T.; Yasui, S.; Chikamatsu, A.; Yasuhara, S.; Itoh, M.; Hasegawa, T. Simple method to obtain large-size single-crystalline oxide sheets. Adv. Funct. Mater. 2020, 30 (28), 2001236.
  30. [30]Zhang, B.; Yun, C.; MacManus-Driscoll, J. L. High yield transfer of clean large-area epitaxial oxide thin films. Nano-Micro Letters 2021, 13, 1-14.DOI
  31. [31]Singh, P.; Swartz, A.; Lu, D.; Hong, S. S.; Lee, K.; Marshall, A. F.; Nishio, K.; Hikita, Y.; Hwang, H. Y. Large-area crystalline BaSnO₃ membranes with high electron mobilities. ACS Appl. Electron. Mater. 2019, 1 (7), 1269-1274.DOI
  32. [32]Chen, Z.; Wang, B. Y.; Goodge, B. H.; Lu, D.; Hong, S. S.; Li, D.; Kourkoutis, L. F.; Hikita, Y.; Hwang, H. Y. Freestanding crystalline YBa₂Cu₃O₇−ₓ heterostructure membranes. Phys. Rev. Mater. 2019, 3 (6), 060801.DOI
  33. [33]Liu, W.; Ren, X. Large piezoelectric effect in Pb-free ceramics. Phys. Rev. Lett. 2009, 103 (25), 257602.pubmed.ncbi.nlm.nih.gov/20366285
  34. [34]Xue, D.; Zhou, Y.; Bao, H.; Zhou, C.; Gao, J.; Ren, X. Elastic, piezoelectric, and dielectric properties of Ba(Zr₀.₂Ti₀.₈)O₃-50(Ba₀.₇Ca₀.₃)TiO₃ Pb-free ceramic at the morphotropic phase boundary. J. Appl. Phys. 2011, 109 (5).
  35. [35]Dupuy, A. D.; Kodera, Y.; Garay, J. E. Unprecedented electro-optic performance in lead-free transparent ceramics. Adv. Mater. 2016, 28 (36), 7970-7977.DOI
  36. [36]Silva, J. P.; Silva, J. M.; Oliveira, M. J.; Weingärtner, T.; Sekhar, K. C.; Pereira, M.; Gomes, M. J. High-performance ferroelectric–dielectric multilayered thin films for energy storage capacitors. Adv. Funct. Mater. 2019, 29 (6), 1807196.DOI
  37. [37]Liu, Y.; Wang, Z.; Thind, A. S.; Orvis, T.; Sarkar, D.; Kapadia, R.; Borisevich, A. Y.; Mishra, R.; Khan, A. I.; Ravichandran, J. Epitaxial growth and dielectric characterization of atomically smooth 0.5Ba(Zr₀.₂Ti₀.₈)O₃–0.5(Ba₀.₇Ca₀.₃)TiO₃ thin films. J. Vac. Sci. Technol. A 2019, 37 (1), 011502.DOI
  38. [38]Kumarasubramanian, H.; Ravindran, P. V.; Liu, T.-R.; Song, T.; Surendran, M.; Chen, H.; Buragohain, P.; Tung, I.; Gupta, A. S.; Steinhardt, R. Kinetic control of ferroelectricity in ultrathin epitaxial barium titanate capacitors. arXiv preprint arXiv:2407.13953 2024.DOI
  39. [39]Jiang, Y.; Parsonnet, E.; Qualls, A.; Zhao, W.; Susarla, S.; Pesquera, D.; Dasgupta, A.; Acharya, M.; Zhang, H.; Gosavi, T. Enabling ultra-low-voltage switching in BaTiO₃. Nat. Mater. 2022, 21 (7), 779-785.DOI
  40. [40]Weber, D.; Vőfély, R.; Chen, Y.; Mourzina, Y.; Poppe, U. Variable resistor made by repeated steps of epitaxial deposition and lithographic structuring of oxide layers by using wet chemical etchants. Thin Solid Films 2013, 533, 43-47.DOI
  41. [41]Miller, R. A.; Bernstein, J. J. A novel wet etch for patterning lead zirconate-titanate (PZT) thin-films. Integrated Ferroelectrics 2000, 29 (3-4), 225-231.DOI
  42. [42]Zhang, R.; Yang, C.; Yu, A.; Wang, B.; Tang, H.; Chen, H.; Zhang, J. Wet chemical etching method for BST thin films annealed at high temperature. Appl. Surf. Sci. 2008, 254 (21), 6697-6700.DOI
  43. [43]Gai, B.; Geisz, J. F.; Friedman, D. J.; Chen, H.; Yoon, J. Printed assemblies of microscale triple-junction inverted metamorphic GaInP/GaAs/InGaAs solar cells. Prog Photovolt Res Appl. 2019, 27 (6), 520-527.DOI
  44. [44]Chen, H.; Lee, S.-M.; Montenegro, A.; Kang, D.; Gai, B.; Lim, H.; Dutta, C.; He, W.; Lee, M. L.; Benderskii, A. Plasmonically enhanced spectral upconversion for improved performance of GaAs solar cells under nonconcentrated solar illumination. ACS Photonics 2018, 5 (11), 4289-4295.DOI
  45. [45]Kang, D.; Chen, H.; Yoon, J. Stretchable, skin-conformal microscale surface-emitting lasers with dynamically tunable spectral and directional selectivity. Appl. Phys. Lett. 2019, 114 (4), 041103.DOI
  46. [46]Yablonovitch, E.; Hwang, D.; Gmitter, T.; Florez, L.; Harbison, J. Van der Waals bonding of GaAs epitaxial liftoff films onto arbitrary substrates. Appl. Phys. Lett. 1990, 56 (24), 2419-2421.DOI
  47. [47]Lau, J. H.; Lau, J. H. Advanced packaging; Springer, 2021.
  48. [48]Gao, W.; Ota, H.; Kiriya, D.; Takei, K.; Javey, A. Flexible electronics toward wearable sensing. Acc. Chem. Res. 2019, 52 (3), 523-533.DOI
  49. [49]Kang, J.-H.; Shin, H.; Kim, K. S.; Song, M.-K.; Lee, D.; Meng, Y.; Choi, C.; Suh, J. M.; Kim, B. J.; Kim, H. Monolithic 3D integration of 2D materials-based electronics towards ultimate edge computing solutions. Nat. Mater. 2023, 22 (12), 1470-1477.DOI
  50. [50]Nian, L.; Sun, H.; Wang, Z.; Xu, D.; Hao, B.; Yan, S.; Li, Y.; Zhou, J.; Deng, Y.; Hao, Y. Sr₄Al₂O₇: A New Sacrificial Layer with High Water Dissolution Rate for the Synthesis of Freestanding Oxide Membranes. Adv. Mater. 2024, 2307682.DOI
  51. [51]Peng, B.; Peng, R.-C.; Zhang, Y.-Q.; Dong, G.; Zhou, Z.; Zhou, Y.; Li, T.; Liu, Z.; Luo, Z.; Wang, S. Phase transition enhanced superior elasticity in freestanding single-crystalline multiferroic BiFeO₃ membranes. Sci. Adv. 2020, 6 (34), eaba5847.DOI

Paper details

vlnc:W_mdspwhwu
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents