Intrinsic Negative-U Centers in Freestanding LaAlO3/SrTiO3 Micro-membranes

Abstract

The LaAlO3/SrTiO3 (LAO/STO) interface hosts a rich range of electronic phenomena, including unconventional electron pairing that in quantum dots gives rise to a negative effective charging energy U. Here, we show freestanding LAO/STO micro-membranes naturally hosting negative-U centers, where lateral confinement arises intrinsically, rather than from engineered nanostructures. These centers coexist with gate-tunable superconductivity and can remain stable upon thermal cycling from millikelvin temperatures to room temperature. Transport is in excellent agreement with calculations based on a negative-U Anderson model, and electrostatic simulations indicate characteristic center sizes of 20-80 nm. Our findings suggest that negative-U centers may arise from the intrinsic interfacial inhomogeneity typical of LAO/STO, and should therefore be considered a general feature of the LAO/STO interface. This could have important consequences for the microwave response of interfacial superconducting devices.

Interfaces between complex oxides provide a rich platform for exploring correlated electron phenomena. A notable example is the two-dimensional electron gas (2DEG) at the interface between LaAlO3_3 (LAO) and SrTiO3_3 (STO), which exhibits a remarkable combination of properties, including high mobility¹, strong Rashba spin–orbit coupling², ferromagnetic ordering³, negative compressibility⁴ and gate-controlled superconductivity⁵–⁸. Its low temperature phase diagram resembles that of high-temperature superconductors, with a dome-shaped superconducting phase and a softly gapped state above the superconducting critical temperature TcT_{\mathrm{c}}⁶,⁹. Electron pairing has also been directly observed at temperatures above TcT_{\mathrm{c}} and magnetic fields exceeding the superconducting critical field BcB_{\mathrm{c}}¹⁰–¹⁴. In this regime electron-electron interactions in quantum dots are modeled by a negative effective charging energy UU in the Anderson model¹⁵, in contrast to the positive Coulomb repulsion of conventional semiconductor quantum dots.

Previous negative-UU quantum dot experiments rely on extrinsic confinement imposed by electrostatic gating¹¹,¹² or atomic-force microscopy (AFM)-based sketching¹⁰. However, numerous studies provide strong evidence that even in pristine epitaxial LAO/STO the electronic landscape is intrinsically inhomogeneous, and low-temperature transport is mediated by submicrometric highly conductive “puddles” embedded in a less conductive background¹⁶–²¹. In the superconducting phase, the puddles host local superconductivity and couple via the Josephson effect²²–²⁵. Several mechanisms have been proposed to account for this intrinsic inhomogeneity, including electronic instability associated with negative compressibility and the non-rigidity of the interfacial confinement potential²⁰,²¹, charge segregation mediated by strong Rashba spin–orbit coupling¹⁸, interaction of the interfacial electrons with oxygen vacancies²⁶, and influence of the ferroelastic domain-wall network of STO on the 2DEG¹⁶.

Despite a wealth of experiments on millimeter-scale LAO/STO 2DEGs, insight into the microscopic origins of emergent behavior is hampered by difficulties in fabricating devices at smaller scales²⁷–³². Therefore, the majority of transport studies have focused on as-grown unpatterned heterostructures or macroscopic Hall-bar structures, probing the average properties of the inhomogeneous interface. Insight into microscopic mechanisms is, however, crucial both for a fundamental understanding of the interface and for the development of STO-based micro-scale functional electronics.

Freestanding oxide membranes³³ have opened a new path toward the integration of oxides with semiconductors³⁴ and flexible electronics³⁵ with enhanced control over curvature and strain36. Additionally, when scaled down to the micron-level7,37, freestanding micro-membranes offer a promising platform for realization of micron-scale devices to probe the intrinsic inhomogeneity.

Here, we study electronic devices fabricated from ∼1×2\sim1\times2,µm2^2 freestanding LAO/STO (thickness: 70 nm / 70 nm) micro-membranes realized by spontaneous spalling38 and transferred onto a silicon oxide / silicon substrate (Figure 1a). Two devices were investigated in detail: Dev#1 with the LAO layer facing the substrate and Dev#2 with the opposite orientation (Supplementary Section S1). Growth details are presented in Ref. 37, and fabrication details are reported in Methods. Magneto-transport measurements were performed in a dilution refrigerator at temperature Tbase≈20T_{\mathrm{base}}\approx20 mK, unless stated otherwise (Methods and Supplementary Section S2). Figure 1b shows a device schematic with magnetic field orientations: B∥B_{\parallel} parallel to the membrane plane and current flow, and B⊥B_{\perp} perpendicular to the membrane.

Figure 1. a False color scanning electron micrograph of a micro-membrane on SiO2_2. b Device schematic together with a representation of the array of conductive puddles at the LAO/STO interface (not to scale). A nanometer-sized puddle (red) may represent the intrinsic origin of the observed negative-UU center. Inset: electrochemical potentials of the leads and transitions in a negative-UU center (black) and their evolution with magnetic field (red). c Differential resistance of Dev#1 as a function of VGV_G and ISDI_{SD}, with B∥=25B_{\parallel}=25 mT, to suppress Al-contact superconductivity (TcAl≈1.2T_c^{\mathrm{Al}}\approx1.2 K, BcAl≈10B_c^{\mathrm{Al}}\approx10 mT). d Gate dependence of switching current IsI_s, normal-state resistance RNR_N and their product Is⋅RNI_s\cdot R_N. e Normal-state conductance at B⊥=0.5B_{\perp}=0.5 T vs VGV_G (black trace). The red trace shows the residual ΔG\Delta G after background subtraction.

Although no extrinsic electrostatic confinement was implemented the as-cooled sub-kelvin electronic properties show direct signatures of transport through intrinsic negative-UU centers, superimposed on a background of gate-tunable superconductivity. This indicates that negative-UU centers can emerge without engineered lateral confinement, suggesting an intrinsic origin related to the electronic inhomogeneity of the interfacial 2DEG.

facial 2DEG. The results are well reproduced by rate-equation computations based on a negative-UU Anderson model. From the characteristic energies of the devices and finite element electrostatic simulations we estimate an effective lateral confinement size of ∼20\sim20–80 nm. Finally, we find that the negative-UU confinement can be robust upon thermal cycling from millikelvin temperatures to room temperature, and we discuss the confinement origin and its connection to the inhomogeneous electronic landscape at the LAO/STO interface.

Gate-tunable superconductivity

Figure 1c shows the differential resistance of Dev#1 as a function of gate voltage, VGV_G, and bias current, ISDI_{SD}, revealing a superconducting ground state as previously analyzed in Ref. 7. The switching current, IsI_s, increases with VGV_G (Figure 1d) and the corresponding current density, Jc≈15J_c\approx15–45 nA/µm, is comparable to the highest values reported for high-quality epitaxial bulk samples23. The normal-state resistance, RNR_N, measured at B⊥=1B_{\perp}=1 T, decreases with increasing VGV_G, such that the product Is⋅RN≈114±7I_s\cdot R_N\approx114\pm7 µV remains constant. These observations are consistent with a 2DEG described by a Josephson array as discussed in Refs. 22–24 (Figure 1d). This is further consistent with the gradual transition from the normal to the zero-resistance state as a function of temperature (Supplementary Section S3). The gate dependence of TcT_c and BcB_c follows that of Ref. 7 and is presented in Supplementary Section S3. Over the range −80-80 V ≤VG≤60\le V_G \le60 V, TcT_c increases from 216 to 226 mK (±1\pm1 mK), while B∥=815±15B_\parallel= 815 \pm15 mT and B⊥=150±10B_\perp= 150 \pm10 mT remain constant within experimental error. The anisotropy of the critical field is consistent with the two-dimensional nature of transport, and we estimate a coherence length ξ≈47\xi\approx47 nm and an upper bound of the superconducting thickness d<30d < 30 nm7,39,40 (Supplementary Section S3). The weak VGV_G-dependence of TcT_c, indicates that the superconducting gap is essentially gate-independent in the measured range. Altogether, the extracted parameters agree with previous reports on bulk samples6,8,24,41 and freestanding micro-membranes7, and are consistent with a two-dimensional Josephson array of superconducting puddles, with VGV_G mainly controlling the Josephson coupling between them23.

Evidence of confinement

In addition to the overall decreasing trend, RN(VG)R_N(V_G) exhibits reproducible modulations. These are emphasized in Figure 1e showing the conductance, G=1/RNG = 1/R_N, measured at B⊥=0.5B_\perp= 0.5 T in a narrower VGV_G-range. Distinct conductance peaks are observed on the smoothly increasing background which is associated with increasing carrier density of the 2DEG. To enhance the modulations we subtract a polynomial background and Figure 1e shows the residual conductance, ΔG\Delta G (Supplementary Section S4).

Figure 2a shows ΔG\Delta G as a function of VGV_G and bias voltage VSDV_{\mathrm{SD}}. A diamond pattern of high conductance is observed, resembling the features expected for transport through a quantum dot in Coulomb blockade. This observation implies transport through discrete charge states of a nanoscale region with total capacitance CC, giving a charging energy EC≈e2/C≫kBTE_C \approx e^2/C \gg k_B T, where ee is the electron charge and kBk_B is the Boltzmann constant. Further, the region must be coupled to the source and drain reservoirs via tunnel barriers with coupling strengths Γ≪EC\Gamma\ll E_C (inset of Figure 1b). Within each conductance diamond, the total charge on the nanoscale region is fixed and can be written as Q=(N0+N)eQ = (\mathcal{N}_0 + \mathcal{N})e, where N0\mathcal{N}_0 is the charge at the lowest VGV_G in Figure 2a and N=0,1,2,…\mathcal{N} = 0,1,2,\ldots. Charge variation occurs only at the diamond boundaries, where transport becomes allowed. This finding is notable because, unlike previously reported quantum dots in LAO/STO, which were defined by electrostatic gates11,12,42,43 or by AFM sketching10,44, here there is no extrinsic confinement. Moreover, the device is operated at high electron densities, well away from depletion, as evidenced by the relatively high TcT_c in the superconducting regime9. A similar pattern is observed for Dev#2 as presented in Supplementary Section S5.

Figure 2. a Measured residual conductance, ΔG\Delta G, of Dev#1 as a function of VGV_G and VSDV_{\mathrm{SD}}, at B⊥=0.5B_\perp= 0.5 T (white dashed line in panel c). b Measured zero-bias ΔG\Delta G versus VGV_G and B∥B_\parallel. The white curves show Lorentzian fits of a selected peak/peak pair at B∥=1.5B_\parallel= 1.5, 2.5, 3.5, 4.5, 5.5 T. The symbols correspond to those in Figure 3. c Measured zero-bias ΔG\Delta G versus VGV_G and B⊥B_\perp. Panels b and c are shifted along VGV_G by ≈1.5\approx1.5 V and ≈1.3\approx1.3 V respectively, to align the low-field peak center with panel a; the shift arises from device drift during measurements. d Simulated conductance versus VGV_G and VSDV_{\mathrm{SD}}. e Simulated zero-bias conductance versus VGV_G and B∥B_\parallel. f Simulated zero-bias conductance versus VGV_G and B⊥B_\perp. The numbers on panel e and f indicate the ground-state charge occupancy N\mathcal{N}.

From the diamond VSDV_{\mathrm{SD}}, we extract an addition energy, Eadd≈190±20E_{\mathrm{add}} \approx190 \pm20 μ\mueV for Dev#1 and between 100 and 420 μ\mueV, depending on the charge state, for Dev#2. The lever arm,

α=dVSD/dVG≈(1.0±0.1)⋅10−4\alpha= \mathrm{d}V_{\mathrm{SD}}/\mathrm{d}V_{\mathrm{G}} \approx(1.0 \pm0.1) \cdot10^{-4} for both devices, quantifies the ratio of capacitive coupling between source/drain and gate. The uncertainties are related to broadening of the diamond boundaries. These estimates assume that the applied VSDV_{\mathrm{SD}} drops only across the quantum dot; any series resistance would reduce the voltage drop across the center. The extracted values should therefore be seen as upper limits.

Negative-UU behavior

Figures 2b-c show the magnetic field dependence of the zero-bias conductance, for B∥B_{\parallel} and B⊥B_{\perp} respectively. Data at B≪BcB \ll B_{\mathrm{c}} are excluded as the conductance peaks are masked by the superconducting state (Supplementary Section S4). As B∥B_{\parallel} increases, the peaks remain initially field-insensitive before bifurcation at a pairing field BPB_{\mathrm{P}}, after which they split linearly with field (Figure 2b). For B⊥B_{\perp} the peaks remain unaffected up to the 1 T limit of our setup (Figure 2c). While Coulomb blockade is widely reported and well understood in semiconductor systems and metallic nanoparticles, the observed doubling of Coulomb blockade resonances in field is unusual. It indicates that the zero-field charge ground state consists of even parity states (N=0,2,4,…N = 0,2,4,\ldots), with odd states becoming accessible only at B>BPB > B_{\mathrm{P}} (inset of Figure 1b). This behavior is consistent with transport through a negative-UU center, featuring effective attractive interaction and a paired ground state persisting until BPB_{\mathrm{P}}, as previously observed in patterned LAO/STO devices10–12. The results of Figure 2 show that negative-UU centers can also occur as intrinsic features of the unpatterned LAO/STO interface.

For each peak pair, the peak separation ΔVG(B)\Delta V_{\mathrm{G}}(B) was estimated by fitting G(VG)G(V_{\mathrm{G}}) to a double-Lorentzian line-shape (Figure 3, see Supplementary Section S6 for details). The Landé gg-factor was obtained from the slope of linear fits to ΔVG(B)\Delta V_{\mathrm{G}}(B) as g=1μBddB(αeΔVG)g = \frac{1}{\mu_{\mathrm{B}}}\frac{\mathrm{d}}{\mathrm{d}B}(\alpha e \Delta V_{\mathrm{G}}), where μB\mu_{\mathrm{B}} is the Bohr magneton, while BPB_{\mathrm{P}} was determined by extrapolating ΔVG(B)\Delta V_{\mathrm{G}}(B) to zero. From the extracted values, listed in Figure 3, we estimate U=gμBBPU = g\mu_{\mathrm{B}}B_{\mathrm{P}} to fall within the range from −20-20 to −40 μeV-40\ \mu\mathrm{eV} for both devices. These values are consistent with previously reported negative-UU interactions in zero-,10,11 and one-13,14 dimensional systems with engineered confinement, though slightly smaller in magnitude.

Figure 3. B∥B_{\parallel} dependence of the gate voltage separation between zero-bias conductance peaks in Dev#1 and Dev#2. The symbols correspond to those in Figure 2b and S3. The pairing field, BPB_{\mathrm{P}}, and the Landé gg-factor, gg, are extracted from linear fits (solid lines). For two peak pairs of Dev#2, data points at high fields (filled grey markers) are excluded from the fit. Note that in some cases the very low slope of ΔVG(B)\Delta V_{\mathrm{G}}(B) renders BPB_{\mathrm{P}} ill-defined.

Transport simulations

To model the experimental data, we used the extracted UU, gg, and α\alpha to construct a two-orbital Anderson Hamiltonian for the negative-UU center tunnel-coupled to the leads. Transport was calculated by solving the Pauli master equation and the results for two resonances of Dev#1 are shown in Figure 2d–Figure 2f as a function of VGV_{\mathrm{G}}, VSDV_{\mathrm{SD}}, B∥B_{\parallel} and B⊥B_{\perp} (Supplementary Section S7). The

simulations closely reproduce the experimental data, demonstrating that the intrinsic centers observed in the freestanding micro-membranes can be well described by a negative-UU Anderson model, similarly to extrinsically defined quantum dots in LAO/STO.

Electrostatic simulations of the center size

To gain further insight into the nature of the intrinsic confinement defining the negative-UU centers, we performed electrostatic simulations to estimate the their size and conducted thermal cycling experiments to investigate the robustness of the confinement. The effective size was estimated from the gate potential ΔVG=2e/CG\Delta V_{\mathrm{G}}=2e/C_{\mathrm{G}} required to charge the center with two electrons via the gate. We performed electrostatic simulations of CGC_{\mathrm{G}} modeling the system as a stack of 70 nm LAO, 70 nm STO, a possible vacuum separation of thickness tt between the membrane and the substrate, and 500 nm SiO2_2 (see schematics in Figure 4a). The numerical simulations include the electric field dependence of the dielectric permittivity of STO45. Varying the gate voltage or reversing the LAO/STO order does not significantly affect the results, as the SiO2_2 layer dominates CGC_{\mathrm{G}} (Supplementary § 13). In all the reported simulations we set VG=10V_{\mathrm{G}}=10 V. The negative-UU center is modeled as a grounded circular disk of diameter dd at the LAO/STO interface, and the source and drain electrodes as grounded half ellipses with semi-axis ww and different ratios relative to the membrane width wtw_{\mathrm{t}}. The accumulated charge on the disk, QQ, and the resulting capacitance, CG=Q/VGC_{\mathrm{G}}=Q/V_{\mathrm{G}}, were calculated for various combinations of dd, tt and w/wtw/w_{\mathrm{t}}. Figure 4a shows the corresponding two-electron charging voltage ΔVG\Delta V_{\mathrm{G}} as a function of dd for several tt values at fixed w/wt=0.2w/w_{\mathrm{t}}=0.2, while Figure 4b shows ΔVG(d)\Delta V_{\mathrm{G}}(d) for various w/wtw/w_{\mathrm{t}} at t=50t=50 nm. Matching the simulated values to the experimental ΔVG≈2\Delta V_{\mathrm{G}}\approx2 V yields center diameters between 20 and 80 nm, depending on the parameters selected.

Estimated center diameter as a function of gate capacitance

Figure 4. a Estimated center diameter as a function of gate capacitance CGC_{\mathrm{G}} for a contact aspect ratio w/wt=0.2w/w_{\mathrm{t}} = 0.2 and various vacuum thicknesses tt. The inset shows a schematic of the simulated geometry (top and side views). b Estimated center diameter as a function of CGC_{\mathrm{G}} for a fixed vacuum thickness t=50t = 50 nm and varying contact aspect ratios w/wtw/w_{\mathrm{t}}.

Thermal stability

Finally we consider the reproducibility of the results upon thermal cycling. Remarkably, unlike the tetragonal domain

structure in thin-film LAO/STO16,17, the (VSD,VG)(V_{\mathrm{SD}}, V_{\mathrm{G}}) stability diagram of Dev#1 remains largely unaffected after thermal cycling Tbase→125T_{\mathrm{base}}\rightarrow125 K →Tbase\rightarrow T_{\mathrm{base}} and even after an additional cycle Tbase→300T_{\mathrm{base}}\rightarrow300 K →Tbase\rightarrow T_{\mathrm{base}}, including exposure to ambient conditions at room temperature (Figure 5). On the other hand, in Dev#2, the conductance diamonds disappear after cycling the temperature to 125 K (Supplementary § 10).

Figure 5. a Thermal cycling sequence applied to Dev#1. b Residual conductance of Dev#1 after the first cool-down, after thermal cycling to 125 K, and after thermal cycling to room temperature with exposure to air, at B⊥=0.5B_{\perp}=0.5 T. White dashed lines are guides to the eye.

The thermal stability of at least one device shows that confinement is not induced by extrinsic effects such as surface contamination or mobile impurities, which are known to induce quantum dots in semiconductor nano-channels close to depletion46. Not only do the micro-membrane devices operate far from depletion, but such extrinsic potentials would also randomize upon thermal cycling. Structural defects, such as oxygen vacancies or interstitials, induce potential modulations that are thermally stable below room temperature. However, this mechanism seems unlikely here, since the device operates at large electron densities, and, thus, the defect potential would need to locally deplete the 2DEG while simultaneously leaving a conductive, electrically isolated region within the depleted area. We are not aware of common defects with such dual action. Non-uniform strain fields, arising from the membrane roughness, could generate local potential variations. However, electrostatic simulations indicate that the typical roughness on the STO side, which is the less smooth of the two surfaces, cannot generate potential modulations strong enough to confine charge (Supplementary § 14).

Discussion

The presented observations can be naturally interpreted in the context of the intrinsic electronic inhomogeneity of the LAO/STO interface, commonly described by the puddle picture of transport. In this framework, charge carriers could localize on weakly coupled nanometer-sized puddles, acting as confinement centers. Josephson-array modeling of the superconducting phase has inferred puddle dimensions on the order of 100 nm22–24, consistent with the sizes extracted here for negative-UU centers. In addition, the superconducting properties of freestanding micro-membranes closely match those of thin-film LAO/STO⁷. Furthermore, both puddle formation and negative-UU behavior are intrinsic to the interface.

The development of freestanding oxide membranes is central to current research and technology, and the results presented here show that in these systems negative-UU centers can appear intrinsically. Similar behavior may therefore be expected in membranes prepared by other methods33,47. It is also plausible that these centers originate from interface inhomogeneity and, thus, are not specific to freestanding micro-membranes, but rather a general feature of the LAO/STO interface. The reduced spatial averaging in the micro-membrane devices leaves fewer puddles contributing to transport compared to bulk samples, making individual localized centers a significant contribution to the total conductance. This is consistent with reports on thin-film LAO/STO submicron-scale devices which exhibit a qualitative change in behavior for lateral dimensions below ≈1\approx1 µm, observations which were attributed to the intrinsic interface inhomogeneity29,48.

An open question concerns the origin of interfacial inhomogeneity and its possible link to ferroelastic domains in STO. Although domain sizes typically exceed those of the puddles16,17, domain walls may still act as pinning sites for them. In this context, the high strain in freestanding membranes could modify domain dynamics during thermal cycling, with strain differences between devices potentially accounting for their different thermal-cycling behavior. Alternatively, strain could stabilize monodomain states37, pointing to inhomogeneity mechanisms unrelated to structural domains18–21. Clarifying domain structure in micro-membranes must therefore be the subject of future studies.

In summary, we have reported evidence of weakly gate-tunable superconductivity and negative-UU centers in freestanding LAO/STO micro-membranes on SiO2_2/Si. Unlike previous observations in engineered nanostructures, the negative-UU behavior here emerges intrinsically, without imposed lateral confinement. Transport simulations based on a negative-UU Anderson model reproduce the data with U≈−20U \approx-20 to −40-40 µeV, and electrostatic modeling suggests center sizes of 20–80 nm. One center remains stable after thermal cycling from millikelvin temperatures to room temperature. These results demonstrate that negative-UU centers can form spontaneously at the LAO/STO interface, consistent with an intrinsically inhomogeneous electronic landscape. The nanoscale confinement required for their formation may therefore be a general property of the interface, connected to the same intrinsic inhomogeneity thought to underlie superconductivity in large-scale devices modeled as random Josephson arrays. Our findings may thus offer new opportunities for a deeper understanding of the electronic landscape at the LAO/STO interface, which in turn may help uncover the origin and consequences of both the electronic inhomogeneity and the negative-UU character of this system. The gate-tunable ground state of the LAO/STO offers a unique potential for realizing reconfigurable superconducting electronics, and while the membrane geometry eliminates the bulk volume of STO which imposes large dielectric losses25,49, our findings show that the 2DEG itself hosts intrinsic two level systems which can affect the loss tangent of superconducting devices even far from depletion.

Methods

Device fabrication

For device fabrication, micro-membranes were transferred from the growth substrate onto a p++\mathrm{p}^{++} Si substrate capped with 500 nm of SiO2_2, serving as gate-dielectric. Electrical contacts to the interfacial 2DEG were defined by electron-beam lithography and argon ion Kaufmann milling at 50° with respect to the membrane plane, followed by in-situ Ti/Al (4 nm / 200 nm) evaporation at 70° from two antiparallel in-plane orientations, and 200 nm Al evaporated at 90°.

Magneto-transport measurements

Magneto-transport measurements were performed in a dilution refrigerator with base temperature Tbase≈20T_{\mathrm{base}} \approx20 mK. The series resistance from cryostat filters (6–11 kΩ\Omega) and the contacts (<500 Ω\Omega) was measured from the baseline in the superconducting regime and subtracted (Supplementary § 7). The cryostat was equipped with a vector magnet capable of applying magnetic fields up to 6 T in the direction parallel to the membrane plane and current flow (B∥B_{\parallel}), and up to 1 T perpendicular to the membrane (B⊥B_{\perp}).

Measurements in Figure 1c: A current bias was applied to one electrode, and the voltage was measured at the same electrode, while the other electrode was grounded. The DC current bias, ISDI_{\mathrm{SD}}, was supplied using a voltage source and a 10 MΩ\Omega resistor. An AC excitation of 4 nA was superimposed using the voltage output of a lock-in amplifier and a 1 GΩ\Omega resistor. The AC excitation frequency was 283 Hz. Both AC and DC voltages were measured using a voltage amplifier with a gain of 100. From the AC voltage, the differential resistance was computed as dV/dI\mathrm{d}V/\mathrm{d}I.

Measurements in Fig. 1e, Fig. 2, and Fig. 5: A voltage bias was applied to one electrode, and the current was measured at the opposite electrode. The DC voltage bias, VSDV_{\mathrm{SD}}, was supplied using a voltage source through a 10310^3 divider. Due to instrumental drift, the zero of the DC bias presented an offset, drifting over time; therefore, the plots were corrected for vertical offsets between 20 and 80 μ\mueV. An AC excitation of 30 μ\muV was superimposed using the voltage output of a lock-in amplifier and a 10510^5 divider. The AC excitation frequency was 283 Hz. AC and DC currents were measured using a current-to-voltage converter with a gain of 10610^6. From the AC current, the differential conductance was computed as G=dI/dVG = \mathrm{d}I/\mathrm{d}V.

Transport simulations

Details of the transport simulations are described in Supplementary Section S7.

Electrostatic simulations

The electrostatic simulations were performed using COMSOL. Details are provided in the main text and in Supplementary sections S8, S9. The COMSOL files used for the simulations are available in the data repository.

Data availability

The data that support the findings of this study are openly available at 10.11583/DTU.30893570.

Acknowledgments

This work was supported by the European Research Council through the European Union’s Horizon 2020 research and innovation program (Grant No. 866158) and through the Horizon Europe EIC Pathfinder program Project IQARO (Grant No. 101115190). We also acknowledge support from Ministero dell’Istruzione, dell’Università e della Ricerca for the PRIN PNRR 2022 project FOXES (Prot. P2022TCT72), for the PRIN 2022 project OMEGA (Prot. 2022TCJP8K) and for the PNRR Project PE0000023-NQSTI. F. T. acknowledges support from Villum Fonden via research grant 37338 (SANSIT). N.P. acknowledges funding from the ERC Advanced (NEXUS, grant no. 101054572) and the support from Villum Fonden via research grant VIL73726.

Competing interests

The authors have no conflicts to disclose.

Supplementary Information for Intrinsic Negative-U Centers in Freestanding LaAlO3_3/SrTiO3_3 Micro-membranes

Giulia Meucci; Pinelopi O. Konstantinopoulou; Thies Jansen; Gunjan Nagda; Damon J. Carrad; Emiliano Di Gennaro; Yu Chen; Nicola Manca; Nicolas Bergeal; Manuel Bibes; Alexei Kalaboukhov; Marco Salluzzo; Roberta Citro; Felix Trier; Nini Pryds; Fabio Miletto Granozio; Alessia Sambri; Thomas S. Jespersen

Determining the orientation of LAO/STO membranes relative to the substrate

The micro-membranes were grown with the LAO layer on top of the STO layer, resulting in an upward curvature (∪-shaped) induced by the strain due to the smaller lattice constant of LAO1^{1}. During the transfer from the growth substrate to the device substrate, membranes could be flipped, resulting in a downward curvature (∩-shaped) with the LAO layer facing the substrate. To determine the orientation, we examined the curvature using tilted scanning electron microscopy (SEM) and performed energy-dispersive X-ray spectroscopy (EDX) on the top surface. SEM revealed that Dev#1 exhibited a ∩-shaped curvature, indicating the STO layer on top (Figure S1), while Dev#2 showed a ∪-shaped curvature, with the LAO layer on top (Figure S1). Correspondingly, EDX spectra (Figure S1) show a high Sr signal for Dev#1, whereas Dev#2 exhibits lower Sr intensity and higher La and Al peaks. These observations confirm that Dev#1 had the STO layer on top (∩) and Dev#2 had the LAO layer facing up (∪).

Figure S1. a Tilted-SEM of Dev#1. b Tilted-SEM of Dev#2. c EDX spectra acquired from the top of Dev#1 and Dev#2. The atomic compositions derived from the spectra are shown in panels a and b.

Two-terminal measurements and series resistance

The two-terminal configuration introduced a series resistance, RsR_{\mathrm{s}}, from the contacts and cryostat filters, which can be measured as the baseline value in the superconducting regime (Figure S2,Figure S2). We estimated RsR_{\mathrm{s}} from the slope of a linear fit to total measured DC voltage, VDC,totV_{\mathrm{DC,tot}}, versus the applied DC current, IDCI_{\mathrm{DC}}, in the superconducting regime (Figure S2) and subtracted it from the measured resistance (Figure S2). RsR_{\mathrm{s}} ranges between 6 and 11 kΩ\Omega, with the large device-to-device variation expected from differences in the cryostat filter resistance (6.07–10.66 kΩ\Omega).

Figure S2. a Total DC voltage drop, VSD,totV_{\mathrm{SD,tot}}, measured as a function of applied bias current, IDCI_{\mathrm{DC}} (black solid line), with a linear fit at low bias used to extract the series resistance RsR_{\mathrm{s}} (red dashed line). b Voltage drop across the device, VSD=VSD,tot−Rs⋅IDCV_{\mathrm{SD}} = V_{\mathrm{SD,tot}} - R_{\mathrm{s}} \cdot I_{\mathrm{DC}}, as a function of IDCI_{\mathrm{DC}}. c Total differential resistance, RtotR_{\mathrm{tot}}, measured as a function of IDCI_{\mathrm{DC}}. d Differential resistance of the device, R=Rtot−RsR = R_{\mathrm{tot}} - R_{\mathrm{s}}, as a function of IDCI_{\mathrm{DC}}.

In voltage biased measurements the voltage applied drops both on RsR_{\mathrm{s}} and on the device. To find the effective bias on the device we subtracted Rs⋅IDCR_{\mathrm{s}} \cdot I_{\mathrm{DC}} from the applied value (Figure S2).

Calculation of superconducting parameters

This section details how the parameters of the superconducting phase discussed in the main text were determined:

  • The switching current, IsI_{\mathrm{s}}, was obtained from the data in Figure 1c as the bias current at which the resistance exhibits a maximum when increasing ISDI_{\mathrm{SD}} from the superconducting to the resistive state.

  • The normal-state resistance, RNR_{\mathrm{N}}, was defined as the zero-bias resistance at B⊥=1B_{\perp} = 1 T, where superconductivity was fully suppressed.

  • The critical in-plane (B∥cB_{\parallel}^{\mathrm{c}}) and out-of-plane (B⊥cB_{\perp}^{\mathrm{c}}) magnetic fields were extracted from the zero-bias resistance traces versus BB (Figure S3-Figure S3). The critical field was defined as the value of BB at which the resistance reached half of its normal-state value, taken as the resistance measured at the maximum applied field, B∥=2.5B_{\parallel}=2.5 T, B⊥=0.6B_{\perp}=0.6 T (Figure S3,Figure S3). The VGV_{\mathrm{G}}-dependence of B∥cB_{\parallel}^{\mathrm{c}} and B⊥cB_{\perp}^{\mathrm{c}} is shown in Figure S4.

Figure S3. Differential resistance of Dev#1 as a function of a in-plane magnetic field, B∥B_{\parallel}, b out-of-plane magnetic field, B⊥B_{\perp}, and c temperature, TT, for selected VGV_{\mathrm{G}}. Panels (d–f) display the corresponding traces normalized to the maximum resistance for each trace. The 50% threshold is indicated by a black horizontal line, and the extracted critical values are marked by vertical lines.

Figure S4. Critical magnetic field and critical temperature as a function of VGV_{\mathrm{G}}.

  • The superconducting coherence length was estimated as ξ=Φ02πB⊥c\xi=\sqrt{\frac{\Phi_{0}}{2\pi B_{\perp}^{\mathrm{c}}}}, and the effective thickness of the superconducting layer as d=3Φ0πξB∥cd=\frac{\sqrt{3}\Phi_{0}}{\pi\xi B_{\parallel}^{\mathrm{c}}}, where Φ0\Phi_{0} is the magnetic flux quantum and μ0\mu_{0} is the vacuum permeability[2]. We note that, because the freestanding membranes are curved, the xx-axis may not have been perfectly aligned with the 2DEG plane, potentially leading to an underestimation of B∥cB_{\parallel}^{\mathrm{c}}. Accordingly, the extracted thickness dd should be regarded as an upper bound.

  • The critical temperature, TcT_{\mathrm{c}}, was extracted from the zero-bias resistance traces versus TT at B∥=25B_{\parallel}=25 mT (Figure S3), as the value of TT at which the resistance reached half of its normal-state value, taken as the resistance measured at T=600T=600 mK (Figure S3). The VGV_{\mathrm{G}}-dependence of TcT_{\mathrm{c}} is shown in Figure S4.

Background Conductance Fitting Procedure

Unlike the behavior expected for an isolated quantum dot, the measured conductance does not vanish between the conductance peaks. This is attributed to a parallel conduction channel, which provides a gate-dependent background conductance associated with increasing puddle coupling. To isolate the contribution of center, this background is subtracted from the data. For each voltage bias or magnetic field, the conductance trace as a function of gate voltage is fitted with a fifth-order polynomial, and the resulting background is removed from the corresponding line cut. An example of such a fit is shown in Figure S5.

Figure S5. a Total zero-bias differential conductance of Dev#1 as a function of VGV_{\mathrm{G}} and B∥B_{\parallel}. b Background differential conductance extracted from fifth-order polynomial fits to each trace, at fixed magnetic field. c Residual differential conductance after subtracting the background. d Representative line cuts at B∥=3B_{\parallel}=3 T showing the measured conductance (black), the polynomial background (blue), and the residuals (red).

Negative-UU Center in Dev#2

Figure S6 shows the residual conductance of Dev#2 as a function of VGV_G and VSDV_{SD}, at B⊥=0.1B_\perp= 0.1 T. Similarly to what presented in the main text for Dev#1, the measurements show diamonds of enhanced conductance, indicative of quantum dot behavior. Figure S6 and Figure S6 display the evolution of the zero-bias conductance peaks with magnetic field, again consistent with the behavior observed for Dev#1. The characteristics energies of the device are discussed in the main text and analyzed in Figure 3.

Figure S6. a Residual conductance, ΔG\Delta G, of Dev#2 as a function of VGV_G and VSDV_{SD}, at B⊥=0.1B_\perp= 0.1 T (horizontal white dashed line in panel c). b Zero-bias ΔVG\Delta V_G versus VGV_G and B∥B_\parallel. The white dashed lines show the conductance peak positions obtained from single or double Lorentzian fits. The symbols correspond to those in Figure 3. c Zero-bias ΔVG\Delta V_G versus VGV_G and B⊥B_\perp. The white dashed lines show the conductance peak positions obtained from single Lorentzian fits.

Figure S7 presents additional measurements of the differential conductance of Dev#2 as a function of VGV_G and VSDV_{SD} at different magnetic fields, further illustrating the progressive splitting of the conductance diamonds with increasing field.

Figure S7. Residual conductance, ΔG\Delta G, of Dev#2 versus VGV_G and VSDV_{SD}, at B∥=0B_\parallel= 0 (B⊥=0.1B_\perp= 0.1 T), B∥=2B_\parallel= 2 T and B∥=4B_\parallel= 4 T. White dashed lines are guides to the eye highlighting the conductance diamonds. The top insets show the zero-bias traces.

Figure S8 shows the behavior of Dev#2 after thermal cycling. In contrast to Dev#1, the conductance diamonds disappear after cycling to 125 K.

Figure S8. a Thermal cycling sequence applied to the devices. b Total differential conductance of Dev#2 after the first cool-down, after thermal cycling to 125 K, and after thermal cycling to room temperature with exposure to air, at B⊥=0.1B_{\perp}=0.1 T.

Peak fitting procedure

The zero-bias conductance peaks shown in Figure 2 and Figure S6 were analyzed using a two-step fitting procedure. Peak positions were first estimated for each magnetic field using a peak-finding algorithm, providing initial values for subsequent Lorentzian fits. When two peaks appeared in close proximity, i.e. after peak splitting, a double Lorentzian fit was applied; otherwise, a single Lorentzian was used. An example of the fitting procedure for Dev#1 is presented in Figure S9.

Figure S9. a Zero-bias total differential conductance of Dev#1 as a function of VGV_{\mathrm{G}} and B∥B_{\parallel}. b Peak positions obtained from Lorentzian fits: crosses correspond to single-Lorentzian fits, circles to double-Lorentzian fits. c Conductance traces from panel a at selected B∥B_{\parallel}, together with the corresponding single or double Lorentzian fits. The traces have been vertically offset for clarity.

Transport simulation of a negative-UU center

The transport through the negative-UU center is modeled with a two-orbital Anderson model using the Qmec package1. The Hamiltonian of the quantum dot coupled to the leads is defined by:

H=HQD+HL+Ht.(1)H = H_{QD} + H_L + H_t. \tag*{(1)}

Here the Hamiltonian of the isolated quantum dot is:

HQD=∑i,σεidiσ†diσ+12∑igiμBB(di↑†di↑−di↓†di↓)+∑iUini↑ni↓+∑i≠jn^in^jVij,(2)H_{QD} = \sum_{i,\sigma} \varepsilon_i d^\dagger_{i\sigma}d_{i\sigma} + \frac{1}{2}\sum_i g_i\mu_B B\left(d^\dagger_{i\uparrow}d_{i\uparrow} - d^\dagger_{i\downarrow}d_{i\downarrow}\right) + \sum_i U_i n_{i\uparrow}n_{i\downarrow} + \sum_{i\ne j}\hat{n}_i\hat{n}_j V_{ij}, \tag*{(2)}

where εi\varepsilon_i is the energy of the ii-th orbital given by: εi=αVG+αV0\varepsilon_i = \alpha V_G + \alpha V_0, where α\alpha is the lever arm, VGV_G is the gate voltage and V0V_0 is the voltage offset.

The operator diσ†d^\dagger_{i\sigma} creates a fermion on the quantum dot with spin σ\sigma, so the first term describes the energy cost of adding an electron to the center. The second term describes the Zeeman energy splitting for orbital ii under a magnetic field BB. The third term represents the on-site Hubbard interaction for orbital ii. The last term accounts for the inter-orbital charging energy between different orbitals i≠ji\ne j.

The Hamiltonian of the leads is:

HL=∑α,kεkcα,k†cα,k,(3)H_L = \sum_{\alpha,k}\varepsilon_k c^\dagger_{\alpha,k}c_{\alpha,k}, \tag*{(3)}

where the operator cα,k†c^\dagger_{\alpha,k} creates an electron in lead α\alpha with momentum kk and εk\varepsilon_k is the corresponding energy. Each lead is coupled to the quantum dot through the following tunneling Hamiltonian:

Ht=∑i,α,ktα,k,i,σcα,k†diσ+H.c.,(4)H_t = \sum_{i,\alpha,k} t_{\alpha,k,i,\sigma} c^\dagger_{\alpha,k}d_{i\sigma} + \mathrm{H.c.}, \tag*{(4)}

where tα,k,i,σt_{\alpha,k,i,\sigma} is the coupling between state k,αk,\alpha in the lead and state i,σi,\sigma in the quantum dot, which is related to the tunneling rate Γα=2π∣tα,k,i,σ∣2\Gamma_\alpha= 2\pi\lvert t_{\alpha,k,i,\sigma}\rvert^2.

We calculate the conductance through the dot as function of VGV_G, BB and voltage bias VSDV_{SD} using the Pauli master equation approach, with the corresponding assumptions described in Ref. 3. Within this approach, the states in the leads are occupied according to the Fermi-Dirac distribution: fα(ε)=(e(ε−μα)/kBTα−1)−1f_\alpha(\varepsilon) = \left(e^{(\varepsilon-\mu_\alpha)/k_B T_\alpha}-1\right)^{-1}, where μα\mu_\alpha and TαT_\alpha are the chemical potential and temperature in lead α\alpha. To incorporate the voltage bias, we symmetrically change the chemical potential around zero in both leads.

Table S7 presents the parameters of the model that represent the experimental negative-UU center as described in the main text. For the calculation, the parameters are scaled for numerical stability.

ParameterValue
α\alpha10.24×10−5 eV V−110.24 \times10^{-5}\,\mathrm{eV\,V^{-1}}
V0V_012 V12\,\mathrm{V}
g1g_10.360.36
g2g_20.590.59
U1U_1−4.49×10−6 eV-4.49 \times10^{-6}\,\mathrm{eV}
U2U_2−50.28×10−6 eV-50.28 \times10^{-6}\,\mathrm{eV}
V12V_{12}210×10−6 eV210 \times10^{-6}\,\mathrm{eV}
V21V_{21}210×10−6 eV210 \times10^{-6}\,\mathrm{eV}
tα,k,it_{\alpha,k,i}3.592×10−6 eV3.592 \times10^{-6}\,\mathrm{eV}
ΓL,R\Gamma_{L,R}4.05×10−11 eV4.05 \times10^{-11}\,\mathrm{eV}
TL,RT_{L,R}0.1 K0.1\,\mathrm{K}

Table S7. Parameters used for the transport simulations presented in Figure 2d-Figure 2f.

Electrostatic simulation of the center size

To estimate the size of the center, electrostatic simulations are performed as described in the main text. The results reported in the main text are obtained for a gate voltage VG=10 VV_G = 10\,\mathrm{V} and a micromembrane with the STO layer facing the substrate. However, the results can be generalized to devices with the LAO layer facing the substrate and to a wider gate voltage range spanning the experimental conditions of both Dev#1 and Dev#2. This is because the thick SiO2_2 dielectric dominates the electrostatics. Figure S10 shows the simulated capacitance of 70 nm layers of LAO and STO as a function of VGV_\mathrm{G}. While the intrinsic capacitances of LAO and STO differ by orders of magnitude and the STO capacitance is gate-dependent, introducing the 500 nm SiO2_2 layer between the oxide layer and the gate makes the overall capacitances of the two configurations nearly identical and independent of VGV_\mathrm{G} over the range 1 μ\muV–100 V. This indicates that the choice of VGV_\mathrm{G} and the orientation of the micromembrane have negligible effect on the simulations.

Figure S10. Simulated capacitance as a function of VGV_\mathrm{G} for single layers of LAO (70 nm), STO (70 nm), and SiO2_2 (500 nm), shown with dashed lines, and for bilayers of LAO (70 nm)/SiO2_2 (500 nm) and STO (70 nm)/SiO2_2 (500 nm), shown with solid lines. The schematics on top illustrate the side view of the geometries used in the simulations.

To further confirm this, the simulations shown in Figure 5a were repeated with the opposite micromembrane orientation, and the results are presented in Figure S11.

Figure S11. Estimated center diameter as a function of gate capacitance CGC_\mathrm{G} for a contact aspect ratio w/wt=0.2w/w_\mathrm{t}=0.2 and vacuum thicknesses tvacuum=10t_\mathrm{vacuum}=10 and 100 nm, for two micromembrane orientations: STO on the substrate (circles) and LAO on the substrate (squares).

Surface Roughness

Figure S12 and S12b show atomic-force micrographs of two micromembranes on Si, one with the LAO side facing up and one with the STO side facing up. These images illustrate the typical membrane curvature discussed in § 6, as well as the characteristic surface roughness. As expected from the spalling-based growth, the STO surface appears rougher than the LAO surface. Figure S12 presents a higher-magnification view of panel b, revealing surface steps and roughness on the order of 5–20 nm.

Figure S12. Atomic-force micrograph of LAO/STO micromembrane on Si. a Membrane with the LAO side facing up. b Membrane with the STO side facing up. c Zoom-in of panel b. The inset at the top shows height profiles taken along the white dashed lines in each panel.

To assess the influence of this roughness on the 2DEG, Figure S13 shows electrostatic simulations using a surface profile modeled as kinks with a height of 5 nm and a width of 50 nm. The resulting variations of the dielectric constant of STO and the electric displacement field under a gate voltage of 100 V are displayed. The effect of the roughness is minimal and negligible at the height of the 2DEG (70 nm), indicating that this cannot account for the presence of confinement centers.

Figure S13. a Dielectric constant of STO and b electric displacement field, calculated under an applied gate voltage of 100 V including a surface roughness modeled as kinks with a height of 5 nm and a width of 50 nm, as indicated by the black profile in each panel.

References

  1. [2]²N. Reyren, S. Gariglio, A. Caviglia, D. Jaccard, T. Schneider, and J.-M. Triscone, “Anisotropy of the superconducting transport properties of the LaAlO3/SrTiO3 interface,” Applied Physics Letters 94, 112506 (2009).DOI

Paper details

vlnc:W_mjf9aacb
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents