betaFeedback

WorksPhysics and Astronomy

Oxygen partial pressure induced dielectric phase evolution in PLD deposited Barium Strontium Titanate thin films

Abstract

Barium Strontium Titanate ((BaxSr1-x)TiO3, BST) thin films are amongst the most extensively studied dielectric alloys over the last decade. This is due to the tunability of the dielectric constant and dissipation factor in the underlying ferroelectric and paraelectric states. One important feature of BST is that the competition between the ferroelectric BaTiO3 and the paraelectric SrTiO3 parent phases can be tuned by the A-site alloy concentration, opening a platform for exploring dielectric phase competition. However, the understanding of the interplay between and establishing the control of the dielectric phase from thin film deposition parameters has not been sufficiently reported in the literature. Here, we synthesized a series of SrRuO3/BST/SrRuO3 epitaxial thin film heterostructures by Pulsed Laser Deposition (PLD) from a (Ba0.9Sr0.1)TiO3 target under systematic variation of the oxygen partial pressure during the BST deposition. We mapped the dielectric phase of the film to the oxygen growth pressure, film composition, and film crystal structure. A ferroelectric, relaxor-like, or paraelectric phase can be obtained with relatively moderate change in oxygen growth pressure. Scanning transmission electron microscopy (STEM) analysis further indicates that this pressure-dependent phase evolution is accompanied by a structural transition of the BST lattice from tetragonal toward a nearly cubic phase, with the latter corresponding to the relaxor-like state. The control of the dielectric phase opens a pathway to study phase evolution and enable future computing technologies.

Main text:

Barium Strontium Titanate ((BaxSr1−x\mathrm{Ba}_x\mathrm{Sr}_{1-x})TiO3\mathrm{TiO}_3, BST) is one of the most extensively studied dielectric materials over the last few decades due to its high dielectric constant, relatively low dielectric loss, strong dielectric tunability[1, 2, 3, 4], and efficient energy-storage capability[5]. As a solid solution of barium titanate (BaTiO3\mathrm{BaTiO}_3) and strontium titanate (SrTiO3\mathrm{SrTiO}_3), BST blends the distinct characteristics of its parent compounds: BaTiO3\mathrm{BaTiO}_3 is ferroelectric at room temperature with a transition temperature TC∼120T_C \sim120 °C[6], whereas SrTiO3\mathrm{SrTiO}_3 is paraelectric[7]. Consequently, the Ba/Sr ratio governs the interplay between ferroelectric and paraelectric states in BST, thereby enabling the control of the dielectric properties[8, 9, 10] and intermediate dielectric phases.

Several studies have examined dielectric phase evolution in BST as a function of Ba/Sr ratio. Kacimi-Naciri et al. reported that increasing Sr concentration drives bulk BST from the tetragonal ferroelectric phase toward the cubic paraelectric phase[11]. The Curie temperature TCT_C of bulk BST decreases[12] and the dielectric constant increases[13] with decreasing Ba/Sr ratio. Composition-dependent changes in dielectric behavior and lattice parameters have also been observed in BaxSr1−xTiO3\mathrm{Ba}_x\mathrm{Sr}_{1-x}\mathrm{TiO}_3 thin films[14]. For PLD-grown BST films, it was found that the dielectric constant increases with deposition temperature[15]. It has been reported that impurity phases form in addition to the BST phase at ∼600\sim600 °C, and at temperatures above 880 °C, a barium deficiency is observed in the film[16]. Kaura et al. reported a systematic control of composition and epitaxial strain in BST thin films realizing an MPB-like coexistence of cubic, tetragonal, rhombohedral, and orthorhombic phases, enabling high tunability and, at higher Sr content, relaxor-like behavior driven by a diffuse transition and dipole dispersion[17]. Additionally, the influence of laser fluence[18] and laser spot size[19] on the microstructure of thin films has been reported. On the other hand, Gradauskaite et al. demonstrated that the ferroelectric response of thin films is also governed by interfacial electrostatic boundary conditions at the interfaces[20]. By introducing an in-plane-polarized ferroelectric buffer, an artificial flux-closure configuration is created that mitigates the depolarizing field, enabling stable out-of-plane polarization in BaTiO3\mathrm{BaTiO}_3 from the first unit cell. One of the most sensitive deposition parameters in the complex PLD growth process is the oxygen growth pressure. Lower pressure generally promotes oxygen-vacancy formation while altering the expansion of the laser-generated plasma plume and the kinetic energy of ablated species, thereby influencing the cation stoichiometry, surface morphology, microstructure, growth rate, and crystallographic orientation of oxide thin films[21, 22, 23]. Chen et al. reported the effects of oxygen growth pressure on the cationic Ti/Ba ratio, lattice parameter, and microstructure in the thin film of parent phase BaTiO3\mathrm{BaTiO}_{3}[24]. However, the detailed, correlated effects of BaTiO3\mathrm{BaTiO}_{3}-SrTiO3\mathrm{SrTiO}_{3} phase competition and oxygen growth pressure during thin-film deposition on dielectric-phase stabilization have not been fully or systematically elucidated.

In this work, we demonstrate that a relaxor-like dielectric state can be realized in epitaxial BaxSr1−xTiO3\mathrm{Ba}_{x}\mathrm{Sr}_{1-x}\mathrm{TiO}_{3} thin films through the coupled control of composition and pulsed-laser-deposition conditions. SrRuO3\mathrm{SrRuO}_{3}/BST/SrRuO3\mathrm{SrRuO}_{3} heterostructures were grown from a (Ba0.9Sr0.1)TiO3(\mathrm{Ba}_{0.9}\mathrm{Sr}_{0.1})\mathrm{TiO}_{3} target while systematically varying the oxygen partial pressure during BST deposition. Correlating the dielectric response with film composition and crystal structure reveals that modest changes in oxygen pressure stabilize ferroelectric, relaxor-like, or paraelectric states. STEM analysis further shows that this phase evolution is accompanied by a structural transformation from a tetragonal toward a nearly cubic lattice, with the latter associated with the relaxor-like response. These findings establish oxygen pressure as an effective control parameter for tailoring dielectric phase stability in epitaxial BST, providing a platform for investigating phase competition and developing tunable materials for emerging computing technologies.

Figure 1(a) shows the workflow used in this study: thin-film growth and optimization, film characterization, device fabrication, and electrical measurements. The SrRuO3\mathrm{SrRuO}_{3}/BST/SrRuO3\mathrm{SrRuO}_{3} (SRO/BST/SRO) heterostructures were grown by pulsed laser deposition (PLD) on (110)-oriented GdScO3\mathrm{GdScO}_{3} (GSO) single-crystalline substrates, varying the oxygen pressure during BST deposition (see Methods). Following synthesis, surface and structural characterization was performed using AFM, XRD, XRR, and STEM. The as-grown heterostructures were then patterned into circular capacitors using photolithography and ion-mill etching. The resulting SRO/BST/SRO capacitors were electrically characterized to investigate their polarization-switching behavior. Figure 1(b) shows cross-sectional annular dark-field (ADF-) STEM images of the SRO/BST/SRO heterostructures grown at oxygen pressures of 150 mTorr (top), 100 mTorr (middle), and 50 mTorr (bottom). The BST and top SRO layers of the 150 mTorr heterostructure exhibit a visibly porous and less dense morphology, whereas the corresponding layers in the 100 and 50 mTorr samples appear comparatively dense and continuous. Figure 1(c) shows typical XRD θ\theta–2θ2\theta scans of the SRO/BST/SRO heterostructures with BST films deposited at oxygen pressures ranging from 50 mTorr (green) to 150 mTorr (navy). The top and bottom SRO electrodes are grown at a fixed pressure of 100 mTorr and a slightly lower temperature of 800 °C. The BST 002 peaks gradually shift to higher angles with increasing oxygen pressure, indicating a reduced out-of-plane lattice parameter. The dashed vertical line marks the bulk Ba0.9Sr0.1TiO3\mathrm{Ba}_{0.9}\mathrm{Sr}_{0.1}\mathrm{TiO}_{3} 002 peak, at a higher diffraction angle than the films. Energy-dispersive X-ray spectroscopy (EDS) shows that the Sr concentration varies from 7.4% at 50 mTorr to 4.3% at 100 mTorr and 6.1% at 150 mTorr. Compositional variation and epitaxial strain (coherent for 50 and 100 mTorr films) alter the lattice structure and therefore the films’ dielectric response.

Growth, fabrication, and characterization of Ba₁₋ₓSrₓTiO₃ (BST) films and the evolution of their dielectric response

Figure 1. Growth, fabrication, and characterization of Ba1−x_{1-x}Srx_xTiO3_3 (BST) films and the evolution of their dielectric response. (a) Experimental workflow: pulsed laser deposition of the SrRuO3_3 (SRO)/BST/SRO heterostructure, characterization by AFM, XRD, and XRR, capacitor fabrication by photolithography and ion milling, and electrical polarization measurement. (b) Cross-sectional TEM images of BST capacitors showing the three-layer structure, with BST grown at oxygen pressures of 150 mTorr (top), 100 mTorr (middle), and 50 mTorr (bottom). (c) XRD 2θ2\theta-ω\omega scans of the heterostructures with BST grown at 50–150 mTorr and fixed SRO layers. The BST peak shifts to higher angle, indicating a smaller out-of-plane lattice parameter, as growth pressure increases. (d) PP–EE loops measured at 10 kHz on 25-μ\mum-diameter capacitors; loop shape and size depend on growth pressure. The spacing between yy-ticks is 20 μ\muC/cm2^2. Offsets along the yy-axis are added in (c) and (d) for clarity.

Figure 1(d) shows typical PP–EE hysteresis loops measured on lithographically fabricated 25 μ\mum diameter capacitors (see Methods). The PP–EE loop (10 kHz) of the 100 mTorr capacitor (brick red curve) resembles that of standard ferroelectric BaTiO3\mathrm{BaTiO}_{3}, with a saturation polarization of 27 μC/cm2\mu\mathrm{C}/\mathrm{cm}^{2} and relatively narrow hysteresis with ECE_C = 47 kV/cm[25]. As the growth pressure is reduced from 100 mTorr, the coercive field initially increases, and the hysteresis loop deviates from the standard ferroelectric-like shape. In particular, the PP–EE loop of the BST film grown at 50 mTorr is asymmetric, possibly due to oxygen deficiency[26]. When the oxygen growth pressure increases to 125 mTorr, the PP–EE loop becomes more “S-shaped” or relaxor-like, with reduced saturation polarization and coercive field (magenta). As the pressure increases to 150 mTorr, it becomes more “S-like”, while the saturation polarization and coercive field decrease further (navy). Thus, the dielectric behavior of the BST films evolves remarkably across the growth pressure series. To better understand the evolution of the dielectric phase, frequency-dependent PP–EE loop measurements were performed.

The top panels of Figure 2(a,Figure 2b) show PP–EE hysteresis loops for ferroelectric-like and relaxor-like samples (100 mTorr and 150 mTorr samples, respectively). The ferroelectric-like phase (Figure 2(a), top) changes dramatically over the measured frequency range (10–200 kHz), while the relaxor-like phase (Figure 2(b), top) is much less responsive. The bottom panels of Figure 2(a,Figure 2b) show the frequency dependence of the relative permittivity, calculated as the derivative of the PP–EE loops. Figure 2(c) shows ECE_C vs. frequency and comprehensively illustrates its frequency evolution. The samples with FE-like phase grown at 75–100 mTorr are more susceptible to frequency changes than those with relaxor-like phase grown at 125–150 mTorr. These differences reveal distinct polarization-switching behavior in these systems. In the FE-like 100 mTorr sample, polarization switching is dominated by domain nucleation and domain-wall motion, making EcE_c sensitive to the time available for switching and pinning/depinning. In contrast, the relaxor-like 150 mTorr sample is characterized by more spatially heterogeneous, short-range polar order rather than well-defined long-range ferroelectric domains, resulting in a slimmer PP–EE loop and a weaker frequency dependence[27]. Note that all samples have comparable BST thicknesses of ∼115, 95, and 135 nm for 50, 100, and 150 mTorr samples, respectively, and the same capacitor diameter of 25 microns. The 75–100 mTorr samples with FE-like phases and 125–150 mTorr samples with “S-shaped” relaxor-like phases can also be separated into two groups following the frequency dependence of EcE_c, those with higher (lower) EcE_c together with the larger (smaller) EcE_c vs frequency slope. For example, the difference in EcE_c between 20 and 200 kHz for the 100 mTorr sample (navy) is about five times larger than that of the 150 mTorr sample (red).

Figure 2. Frequency-dependent dielectric behavior of BST films grown at varied oxygen pressure. (a,b) P-E loops (top) and relative permittivity (bottom) versus frequency for the ferroelectric-like phase at 100 mTorr (a) and the relaxor-like phase at 150 mTorr (b). (c) Coercive field (EcE_\mathrm{c}) versus frequency for the full pressure series, with linear fits (dashed). Samples grown at 75–100 mTorr show steeper slopes than those at 125–150 mTorr.

Figure 3(a) shows the frequency dependence of the remanent-to-saturation polarization ratio (Pr/PsP_r/P_s). For all samples, Pr/PsP_r/P_s initially increases with frequency from 20 kHz. However, this increase tends to saturate for the 75–100 mTorr samples, which exhibit predominantly FE-like behavior. In contrast, Pr/PsP_r/P_s continues increasing gradually with frequency for the 125 mTorr sample, suggesting an intermediate response between the FE-like and relaxor-like phase. The 150 mTorr sample exhibits the most pronounced frequency dependence, with Pr/PsP_r/P_s continuing to increase up to 200 kHz, consistent with relaxor-like response. A higher Pr/PsP_r/P_s ratio indicates stronger ferroelectric behavior, greater domain stability, and stronger domain-wall pinning. A lower ratio indicates weaker ferroelectric features and stronger spatially heterogeneous polar disorder, as in relaxor ferroelectrics. Accordingly, the relatively smaller Pr/PsP_r/P_s observed for the 150 mTorr sample compared with the 100 mTorr sample is consistent with the evolution from a predominantly FE-like toward a more relaxor-like phase. Figure 3(b) shows the linear-fit slope of the EcE_c versus frequency curves in Figure 2(c). The slope is larger for predominantly FE-like samples and smaller for samples with relaxor-like characteristics. This trend indicates a reduced frequency sensitivity of the Pr/PsP_r/P_s response in the relaxor-like regime. Figure 3(c) shows the Pr/PsP_r/P_s ratio measured at 10, 50, and 100 kHz across the pressure series. The ratio remains nearly unchanged between 50 and 100 mTorr, corresponding to the FE-like regime. It decreases as the system evolves toward the relaxor-like state at higher growth pressures, such as 125–150 mTorr.

Frequency-dependent dielectric behavior of BST films grown at varied oxygen pressure

Figure 3. Frequency-dependent dielectric behavior of BST films grown at varied oxygen pressure. (a) Pr/PsP_r/P_s versus frequency for the 50–150 mTorr series; the inset shows how Pr/PsP_r/P_s is determined from a FE loop. (b) Slope of the linear fit of the ECE_C versus frequency curve in Figure 2(c), largest for the most ferroelectric samples (75 and 100 mTorr). (c) Pr/PsP_r/P_s at 10, 50, and 100 kHz, peaking at 75–100 mTorr. (d) (left) Out-of-plane lattice constant versus pressure (left) and c/ac/a ratio of three samples from STEM (right); The out-of-plane lattice constant decreases with increasing pressure. The horizontal dashed line marks the bulk BST cc-value. (e) Remnant area of the PP–EE loops at 10, 50, and 100 kHz, and (f) effective loss tangent, tan⁡(δeff)\tan(\delta_{\mathrm{eff}}), at 10 kHz versus pressure; tan⁡(δeff)\tan(\delta_{\mathrm{eff}}) peaks at 100 mTorr and drops significantly at higher pressures. Dashed lines are guides to the eye.

This pressure-dependent trend occurs at all measured frequencies. Figure 3(d) (left) shows the out-of-plane lattice constant across the pressure series. ADF-STEM measurements reveal that the cc-value of the BST lattice parameter decreases with increasing growth pressure, consistent with the XRD trend in Figure 3(d) (left). However, the aa-values change nonlinearly with pressure, leading to the c/ac/a ratio versus the growth pressure retaining tetragonality at 50 and 100 mTorr and approaching cubic at 150 mTorr. The reduction in tetragonality at higher growth pressure is consistent with the evolution of the electrical response toward a relaxor-like state. Figure 3(e) shows the area enclosed by the PP–EE hysteresis loop versus oxygen partial pressure at 10, 50, and 100 kHz. The enclosed hysteresis-loop area represents the energy dissipated per polarization cycle, with a larger area corresponding to greater hysteretic energy loss. The inset shows the PP–EE loop of the 100 mTorr sample measured at 10 kHz, with the enclosed area shaded in purple. The hysteresis-loop area remains relatively large for samples grown at 75 and 100 mTorr, which exhibit FE-like behavior. As the system evolves toward the relaxor-like regime at higher growth pressures, the loop area decreases abruptly. At 10 kHz, the enclosed area decreases by approximately a factor of five between the 100 and 150 mTorr samples. This reduction is consistent with the slimmer hysteresis loops and weaker long-range ferroelectric switching associated with the relaxor-like state. Figure 3(f) shows the effective loss tangent, tan⁡(δeff)\tan(\delta_{\mathrm{eff}}) (Methods), measured at 10 kHz versus oxygen growth pressure. tan⁡(δeff)\tan(\delta_{\mathrm{eff}}) peaks at 100 mTorr and drops sharply at higher pressures, following the dielectric phase evolution. The FE-like film at 100 mTorr has the widest hysteresis loops and largest remnant loop area [Figure 3(e)], consistent with loss dominated by domain switching. In contrast, the relaxor-like films at 125–150 mTorr show slim, S-shaped loops with minimal hysteresis and hence substantially lower loss. In Figure 3(b) to (Figure 3f), the frequency dependence of polarization, Pr/PsP_{\mathrm{r}}/P_{\mathrm{s}}, the out-of-plane c-axis lattice parameter, the area enclosed by the PP–EE hysteresis loop, and effective tangent loss, respectively, all decrease consistently across this pressure interval, providing independent evidence for the phase crossover. This critical pressure regime, therefore, separates the FE-like (red) and relaxor-like (blue) regions.

Next, we measured the temperature dependence of the ferroelectric switching behavior of BST dielectrics, each at three frequencies: 10 kHz (solid curve), 50 kHz (dotted curve), and 100 kHz (dashed curve). For all three samples, the loops gradually become thinner with increasing temperature, indicating a reduction in EcE_{\mathrm{c}}, except on the higher-temperature side of the 150 mTorr sample, which is attributed to increased leakage at elevated temperatures. In contrast, the 100 mTorr sample shows a reduced polarization height as temperature increases, whereas the 50 and 150 mTorr samples show an overall temperature-independent polarization height. Also, the asymmetric bump in the PP–EE loop of the 50 mTorr sample gradually diminished with increasing temperature, and at 200 °C, this feature was almost gone. Figure 4(b) shows the evolution of the Pr/PsP_r/P_s with temperature at different frequencies. Regardless of the sample growth pressure, the change in Pr/PsP_r/P_s looks more pronounced at low frequencies than at higher frequencies. While the Pr/PsP_r/P_s changes non-monotonically with temperature over the measured frequency range for the 50 mTorr sample, particularly for the 100 and 150 mTorr samples, Pr/PsP_r/P_s generally decreases with increasing temperature at each measurement frequency, and increasing the frequency systematically shifts the curves toward higher Pr/PsP_r/P_s values. The temperature dependence indicates reduced polarization stability upon heating, whereas the higher Pr/PsP_r/P_s observed at higher frequencies is consistent with reduced time available for polarization relaxation and back-switching. Figure 4(c) shows the frequency dependence of the EcE_c at various temperatures. The EcE_c overall increases linearly with frequency, consistent with the nature of polarization switching. At higher frequencies, the time available for polarization reversal is reduced, thereby increasing the switching voltage. The only difference in trend is that EcE_c tends to decrease with increasing frequency at 200 °C for the 150 mTorr sample, which is consistent with the broadening of the PP–EE loop and the sudden increase in Pr/PsP_r/P_s, as shown in Figure 4(a) and Figure 4(b), respectively. Figure 4(d) shows the temperature dependence of the slope obtained from the linear fits of the EcE_c versus frequency in Figure 4(c). At room temperature, the 100 mTorr sample with the FEFE-like phase exhibits the strongest frequency dependence of EcE_c, which gradually weakens with increasing temperature. The 150 mTorr sample with the relaxor-like phase exhibits a much weaker frequency dependence that decreases continuously with temperature, becoming negative at 200 °C due to thermally assisted leakage. When the 100 and 150 mTorr curves are compared, overall flat trends are observed with a vertical offset, clearly distinguishing the FE-like and relaxor-like phases. The 50 mTorr curve starts in the intermediate range at room temperature, then spikes at around 120 °C as if it were an FE-like phase; further increasing the temperature returns it to the intermediate phase.

Temperature-dependent dielectric behavior of BST films deposited under varied oxygen growth pressure

Figure 4. Temperature-dependent dielectric behavior of BST films deposited under varied oxygen growth pressure. (a) Temperature evolution of the PP-EE loops. The coercive voltage (EcE_{\mathrm{c}}) and saturation polarization (PsP_{\mathrm{s}}) decrease with temperature, least for the 150 mTorr sample, where the apparent rise in remanent polarization (PrP_{\mathrm{r}}), PsP_{\mathrm{s}}, and EcE_{\mathrm{c}} at low frequency and high temperature is attributed to the onset of leakage. (b) Pr/PsP_{\mathrm{r}}/P_{\mathrm{s}} versus temperature at different frequencies; the ratio changes more at low frequencies. (c) EcE_{\mathrm{c}} versus frequency at various temperatures for the 50 (left), 100 (middle), and 150 mTorr (right) samples, with linear fits (dashed). (d) Slopes of the fits in (c) versus temperature. Dashed lines are guides to the eye.

In conclusion, we demonstrate growth-pressure-mediated control of the structural and dielectric phases in epitaxial SrRuO3_3/BST/SrRuO3_3 heterostructures grown on GdScO3_3 (110) substrates by pulsed-laser deposition. XRD and ADF-STEM measurements reveal a systematic decrease in both the out-of-plane lattice parameter and tetragonality (c/ac/a) as oxygen pressure increases. This structural evolution accompanies a distinct change in dielectric behavior: the 100 mTorr film exhibits a well-defined FE-like hysteresis response, while the 150 mTorr film displays a slim, S-shaped loop with reduced coercive field and polarization, characteristic of a relaxor-like state. Frequency-dependent measurements of EcE_\mathrm{c} and Pr/PsP_\mathrm{r}/P_\mathrm{s} further support these phase assignments. Moreover, temperature-dependent measurements from room temperature up to 200 °C show that the distinct frequency scaling of EcE_\mathrm{c} remains discernible throughout the investigated temperature range. Collectively, these results establish a direct correlation among oxygen growth pressure, lattice symmetry, and dielectric phase evolution in nominal Ba0.9_{0.9}Sr0.1_{0.1}TiO3_3. By leveraging the competition between the ferroelectric BaTiO3_3 and paraelectric SrTiO3_3 end members, oxygen pressure offers an effective route to stabilize and tune FE-like and relaxor-like states in epitaxial BST thin films.

Methods

Target preparation

10% Sr-doped BaTiO3_3 (BST) target is prepared by conventional solid-state reaction. The high-purity (>99%) precursors BaCO3_3, SrCO3_3, and TiO2_2 were mixed in the required stoichiometric proportions. The mixture was ball-milled for 3 hours, then calcined at 900 °C for 6 hours. An additional 10 mol% Ba was added to compensate for potential losses from volatilization during target sintering and thin-film synthesis. The calcined powder was granulated in isopropyl alcohol (IPA) and pressed into a 1-inch diameter, 8 mm thick disk at 35 MPa for 15 minutes. The target was then introduced to the first sintering cycle at 1400 °C for 6 hours, with a ramp rate of 6 °C/min. The target was granulated again with IPA into a smooth paste, and the same pressing and sintering steps were repeated to obtain the final dense one inch in diameter pellet used in the film synthesis.

Thin film synthesis

SRO/BST/SRO thin film heterostructures were deposited on (110)-oriented GdScO3 (GSO) single-crystalline substrate by using a pulsed laser deposition system with a 248 nm KrF excimer laser. Both SRO and BST films were grown from stoichiometric ceramic targets from Target Materials and from in-house preparation, respectively. During the deposition of the top and bottom SRO layers, the substrate temperatures and oxygen pressures were set to 800 °C and 100 mTorr, respectively, while the BST layers were grown at a slightly elevated temperature of 850 °C, and the oxygen pressure was varied from 25 mTorr to 150 mTorr to synthesize the pressure series samples. The repetition rate of 4 Hz, the laser fluence of ∼4.3 J/cm2\sim4.3\ \mathrm{J}/\mathrm{cm}^{2}, and the substrate-to-target distance of 6 cm are used throughout the growth. After the top SRO layers are deposited, the chamber is annealed with oxygen pressure of 500 Torr at 800 °C, then cooled to room temperature at 5 °C/min in this oxygen-rich environment.

X-ray diffraction measurements

XRD measurements are performed on the SRO/BST/SRO heterostructures on (110)-oriented single crystal GSO substrates using a Rigaku Smart Lab X-ray diffractometer. The 2θ−ω2\theta-\omega scans were measured with a two-bounce configuration, two-crystal Ge 220 monochromator, and used a Cu Kα\alpha radiation source (λ=1.5406 A˚\lambda= 1.5406\ \text{\AA}).

Photolithography and Island Capacitor Fabrication

A layer of MEGAPOSIT SPR220 3.0 was applied to the heterostructure and spun at 5000 rpm for 30 seconds. The samples were then soft-baked on a hot plate at 95 °C for 3 minutes. The samples were exposed to ultraviolet light for 8.5 seconds through a hard photomask using a Karl Suss MJB3 Mask Aligner. The sample then underwent a post-exposure bake at 95 °C for 3 minutes. The sample was developed with AZ 726 using a 30-30 DP recipe. The developed sample was attached to a 4-inch wafer using Santovac. To define the circular capacitors, the developed samples were etched using a Nanoquest II Ion Mill, which uses Argon as a source gas at 50 sccms. The etch power was 300 W, and the beam voltage was 320 mA. The chamber was held at 5 °C to prevent the sample from heating during etching, and a SIMS probe was used to monitor the elemental intensities resulting from etching the various layers of the heterostructures, thereby allowing the etch to be precisely stopped at the desired layer height. The sample was tilted at 25 degrees with respect to the ion beam and rotated at 20 rpm to reduce sidewall redeposition and ensure a uniform etch. The samples were then sonicated in acetone and IPA to remove the photoresist, rinsed with DI water, and dried with an N₂ gun.

P-E loop Measurement

All electrical measurements were performed on circular island capacitors with diameters of 25 μm and 30 μm. The initial PP-EE hysteresis loops are measured on the probe station with one micron tungsten probe tips, using the Precision Multiferroic II from Radiant Technologies. In order to extract the coercive electric field (EcE_c) from the PP-EE loops, first the derivative of the polarization (PP) with respect to the applied electric field (EE), i.e., dP/dEdP/dE, is calculated separately for the polarization along increasing E and decreasing E and then fitted with the Gaussian function. The center of these two Gaussian fits gives the Ec+E_c^{+} and Ec−E_c^{-}, from which EC=(∣Ec+∣+∣Ec−∣)/2E_C = (|E_c^{+}| + |E_c^{-}|)/2 is calculated. The dP/dEdP/dE is used to calculate the relative permittivity for the BST dielectric.

Effective Loss Tangent Calculation:

The effective loss tangent, tan⁡(δeff)\tan(\delta_{\mathrm{eff}}), was calculated from voltage and polarization waveforms measured under 10 kHz triangular excitation. To minimize initial transient effects, the second complete cycle was analyzed, and constant offsets were removed. Fourier analysis was used to extract the fundamental components, and the polarization was resolved into a component in phase with the voltage fundamental (PinP_{\mathrm{in}}) and a component lagging it by 90° (PlossP_{\mathrm{loss}}). The effective loss tangent is defined as tan⁡(δeff)=Ploss/Pin\tan(\delta_{\mathrm{eff}}) = P_{\mathrm{loss}}/P_{\mathrm{in}}. This quantity describes the large-signal polarization response, including switching and any measured leakage contributions, rather than the small-signal dielectric loss.

TEM Measurement:

ADF-STEM measurements were performed on TFS Spectra 300, equipped with Dual-X EDS detector, operated at 300 keV with convergence semi-angle of 21.4 mrad. Electron transparent, thin lamella were prepared with standard gallium focused ion beam (FIB) lift-out process and thinning using Thermo Fisher Scientific (TFS) Helios 5 UC. The samples were thinned down at 30 keV with decreasing current from 0.23 nA and 80 pA, and then with a fine polishing process using 5 keV, 41 pA ion beam.

Acknowledgements

The work is supported by ONR grant N000142412744. S. P. and J. H. acknowledge support from ONR grant N000142412744. Transmission electron microscopy experiments were performed at the Michigan Center for Materials Characterization (MC){sup}2`, RRID:SCR_026770) at the University of Michigan. This work was performed in part at the University of Michigan Lurie Nanofabrication Facility and X-ray diffraction facility in Van Vlack Lab.

A meme summarizing this paper can be found at: https://ferroelectronicslab.com/memes/

References

  1. [1]J. Im, O. Auciello, P. K. Baumann, S. K. Streiffer, D. Y. Kaufman and A. R. Krauss, Applied Physics Letters 76 (5), 625-627 (2000).
  2. [2]W. J. Kim, W. Chang, S. B. Qadri, J. M. Pond, S. W. Kirchoefer, D. B. Chrisey and J. S. Horwitz, Applied Physics Letters 76 (9), 1185-1187 (2000).
  3. [3]J. D. Baniecki, R. B. Laibowitz, T. M. Shaw, P. R. Duncombe, D. A. Neumayer, D. E. Kotecki, H. Shen and Q. Y. Ma, Applied Physics Letters 72 (4), 498-500 (1998).
  4. [4]B. H. Park, Y. Gim, Y. Fan, Q. X. Jia and P. Lu, Applied Physics Letters 77 (16), 2587-2589 (2000).
  5. [5]Z. Song, H. Liu, H. Hao, S. Zhang, M. Cao, Z. Yao, Z. Wang, W. Hu, Y. Shi and B. Hu, IEEE Trans Ultrason Ferroelectr Freq Control 62 (4), 609-616 (2015).
  6. [6]Von Hippel, A., R. G. Breckenridge, F. G. Chesley, and Laszlo Tisza, Industrial & Engineering Chemistry, 38(11), 1097-1109 (1946).
  7. [7]W. Zhong, D. Vanderbilt. Physical Review B 53 (9), 5047 (1996).
  8. [8]L. H. Parker, Al F. Tasch. IEEE Circuits and Devices Magazine 6(1) 17-26 (1990).
  9. [9]O. Auciello, J. F. Scott, R. Ramesh. Physics today 51(7) 22-27 (1998).
  10. [10]K. Buse, F. Baller, R. Pankrath, H. Hesse, E. Krätzig. Solid state communications 88(8) 587-591 (1993).
  11. [11]H. Kacimi-Naciri, M. Rguiti, A. Mabrouk, C. Courtois, M. A. Ben Achour, Y. Lorgouilloux, R. Amrousse, N. Faska and A. Bachar, Ceramics International 51 (17) 23801-23813 (2025).
  12. [12]G. Panomsuwan and H. Manuspiya, Materials Research Express 6 (2) (2018).
  13. [13]A. Ioachim, M. I. Toacsan, M. G. Banciu, L. Nedelcu, F. Vasiliu, H. V. Alexandru, C. Berbecaru and G. Stoica, Progress in Solid State Chemistry 35 (2-4), 513-520 (2007).
  14. [14]C. Mansour, M. Benwadih and C. Revenant, AIP Advances 11 (8) (2021).
  15. [15]R. Gupta, V. Gupta and M. Tomar, Vacuum 159, 69-75 (2019).
  16. [16]A. V. Tumarkin, V. I. Al’myashev, S. V. Razumov, M. M. Gaidukov, A. G. Gagarin, A. G. Altynnikov and A. B. Kozyrev, Physics of the Solid State 57 (3), 553-557 (2015).
  17. [17]G. Kaura, S. Mantri, F. Liu, S. Hazra, S. Chen, Y. Si, B. Roul, A. Saha, S. Chowdhury, D. Prajapat, M. Valyvidares, S. B. Krupanidhi, Z. Chen, Y. L. Tang, V. Gopalan, L. W. Martin, L. Bellaiche and S. Das, Advanced Materials, e73172 (2026).
  18. [18]D. Kan and Y. Shimakawa, Applied Physics Letters 99 (8) (2011).
  19. [19]H. Kumarasubramanian, P. V. Ravindran, T.-R. Liu, T. Song, M. Surendran, H. Chen, P. Buragohain, I. C. Tung, A. S. Gupta, R. Steinhardt, I. A. Young, Y.-T. Shao, A. I. Khan and J. Ravichandran, APL Electronic Devices 1 (4) (2025).
  20. [20]E. Gradauskaite, Q. N. Meier, N. Gray, M. F. Sarott, T. Scharsach, M. Campanini, T. Moran, A. Vogel, K. Del Cid-Ledezma, B. D. Huey, M. D. Rossell, M. Fiebig and M. Trassin, Nature Materials 22 (12), 1492-1498 (2023).
  21. [21]L. You, N. T. Chua, K. Yao, L. Chen and J. Wang, Physical Review B 80 (2) (2009).
  22. [22]J. Gonzalo, R.Gómez San Román, J. Perrière, C.N. Afonso, R. Pérez Casero. Applied Physics A 66, 487–491 (1998).
  23. [23]W. Can, B. L. Cheng, S. Y. Wang, H. B. Lu, Y. L. Zhou, Z. H. Chen and G. Z. Yang, Thin Solid Films 485 (1-2), 82-89 (2005).
  24. [24]A. P. Chen, F. Khatkhatay, W. Zhang, C. Jacob, L. Jiao and H. Wang, Journal of Applied Physics 114 (12) (2013).
  25. [25]Y. Jiang, Z. Tian, P. Kavle, H. Pan and L. W. Martin, APL Materials 12 (4) (2024).
  26. [26]T. Friessnegg, S. Aggarwal, R. Ramesh, B. Nielsen, E. H. Poindexter and D. J. Keeble, Applied Physics Letters 77 (1), 127-129 (2000).
  27. [27]S. Zhou, Y. Zhou, L. Li, Z. Fan, W. Yue, Z. Fu, X. Chen, B. Xu, T. Hu, D. Wang and T. Yang, Nature Communications 16 (1), 8456 (2025).

Paper details

vlnc:W_mzj7ku4c
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents