WorksPhysics and Astronomy
Giant tunability of magnetoelasticity in FeN system: Platform for unveiling correlation between magnetostriction and magnetic damping
Abstract
Flexible spintronics has opened new avenue to promising devices and applications in the field of wearable electronics. Particularly, miniaturized strain sensors exploiting the spintronic function have attracted considerable attention, in which the magnetoelasticity linking magnetism and lattice distortion is a vital property for high-sensitive detection of strain. This paper reports the demonstration that the magnetoelastic properties of FeN can be significantly varied by partially replacing Fe with Co or Mn. The high quality FeN film exhibits large negative magnetostriction along the [100] direction () of -121 ppm while FeCoN shows of +46 ppm. This wide-range tunability of from -121 to +46 across 0 allows us to thoroughly examine the correlation between the magnetoelasticity and other magnetic properties. The strong correlation between and magnetic damping () is found. The enhanced extrinsic term of is attributable to the large two magnon scattering coming from the large magnetostriction. In addition, the density of states at the Fermi level plays a primal role to determine both and the intrinsic term of . Thanks to the giant tunability and the bipolarity of magnetoelasticity, magnetic nitrides are candidate materials for high-sensitive spintronic strain sensors.
Corresponding author. Email: [email protected]
† Present address: Department of Advanced Materials Science and Engineering, Faculty of Engineering Sciences, Kyushu University, Fukuoka 816-8580, Japan
Flexible electronic devices have rapidly become important in the coming trillion-sensor era, in which wearable devices will spill over. Flexibility is required not only for semiconductor-based electronic devices, but also for spintronic devices, and the vast research field of flexible electronics involves a variety of research topics coming from technological demands and scientific interests, e.g. device fabrication and operation on flexible substrates, and improved performance and new functionalities under the application of mechanical strain1-7. As we look at the current flexible spintronics, miniaturized strain sensors exploiting the spintronic function6 have attracted much attention, where the magnetoelasticity linking magnetism and lattice distortion is a vital property for high-sensitive and multi-directional strain detection. Through the inverse magnetostriction effect, the magnetization vector of a magnetic material changes depending on the magnitude and the direction of mechanical stress applied to the magnet. Thus, large magnetoelastic materials and the elucidation of underlying physical mechanism are keys for the development of high-sensitive devices.
Although there are several magnetoelastic materials, the spintronic applications need to show large magnetoresistance (MR) effect as well as large magnetostriction. Tb-Dy-Fe alloys8 and Fe-Ga alloys9 are well known ferromagnets exhibiting large magnetostriction. However, since no large MR effect has been reported in any giant MR (GMR) or tunneling MR (TMR) devices with Tb-Dy-Fe or Fe-Ga, these materials are excluded from consideration. The recent first-principles calculation10 has predicted that , a ferromagnetic iron nitride exhibits the magnetostriction constant several times larger than that of typical ferromagnetic metals such as Fe, Co, and Ni, and there is a report on experimental investigation for magnetostriction of FeN although the reported value was smaller than the theoretical prediction11. In addition, a large TMR effect in a magnetic tunnel junction12, anomalous Hall effect13, and anomalous Nernst effect13,14 have been reported for systems with FeN. These features make ferromagnetic nitrides a promising material group not only for spintronic devices15,16, but also for flexible spintronic devices. Moreover, epitaxial growth of ferromagnetic nitrides on flexible mica substrates and modulation of magnetic properties by stress application have been reported17, and the FeN does not contain minor metal elements and rare earth elements, which is another advantage from the viewpoint of large-scale fabrication of wearable devices. Thus, it should be clarified to what extend the magnetoelasticity can be enhanced and controlled for ferromagnetic nitrides in order to achieve best performance of flexible spintronic devices.
Here we report that the magnetoelastic properties of FeN can be significantly varied by partially replacing Fe with Co or Mn. As shown in Figure 1a, the Co substitution in FeN corresponds to the electron doping whereas the Mn substitution leads to the electron depletion. This variation in the number of valence electrons gives rise to the shift of the Fermi level () position, and also makes the FeN a suitable platform to examine the correlation between the magnetoelasticity and other magnetic properties experimentally and theoretically. By measuring various magnetic properties such as magnetostriction, saturation magnetization (), magnetic anisotropy constant (), and magnetic damping constant (), we experimentally and theoretically reveal the strong correlation between magnetostriction and magnetic damping.

Figure 1. Concept of element substitutions and structural analysis for magnetic nitrides. (a) Crystal structures of magnetic nitrides; Co substitution into corresponds to electron doping and Mn substitution to hole doping. Out-of-plane and in-plane XRD patterns of the (b) , (c) , and (d) films. Red and blue lines correspond to the results with the out-of-plane and in-plane configurations, respectively.
Co or Mn substitution in films
, (, , and ), and (, , , , and ) films with a thickness of approximately 23 nm were grown on substrates. The exact values of thicknesses, which were estimated from the x-ray reflectivity, were given in the Supplementary Information. Figure 1b, Figure 1c, and Figure 1d display the x-ray diffraction (XRD) patterns for the representative samples of the , , and films, respectively. The red (blue) lines denote the out-of-plane (in-plane) XRD patterns. The 001 and 002 peaks of nitrides appear in the out-of-plane XRD patterns while the 100 and 200 peaks are observed in the in-plane XRD patterns. These facts indicate the epitaxial growth of the nitride films on the STO(001) substrates. From the structural characterization using XRD as well as reflection high-energy electron diffraction patterns (not shown here), it was confirmed that all the samples are epitaxially grown and no secondary phase exists.
Figure 2a shows the magnetization curves of the film measured at room temperature. When an external magnetic field () is applied in the in-plane [100] direction (solid curve), the remanent magnetization () is equal to . On the other hand, is decreased when is applied in the in-plane [110] direction (dashed curve). This difference originates from the cubic symmetry of magnetocrystalline anisotropy in FeN with the [100] easy magnetization axis18,19. From the magnetization curves, and were evaluated for all the samples, where was estimated from the area enclosed between the [100] and [110] magnetization curves.

Figure 2. Magnetization, magnetostriction and magnetization dynamics of magnetic nitrides. (a) In-plane magnetization curves of the film measured at room temperature, where is normalized by . The solid (dashed) curve denotes the result with applied in the in-plane direction (in-plane direction). (b) Illustration of experimental setup of an optical cantilever method. (c) -dependence of at a rotational of 175 Oe applied to the film. (d) dependence of for the (red line), (blue line), and (green line) films. (e) dependence of and (f) for the (red line), (blue line), and (green line) films with the IP configuration. The inset of (e) shows the resonance spectrum together with the fitting result for the film measured at Oe. (g) dependence of and (h) for the (red line), (blue line), and (green line) films with the OOP configuration. The inset of (g) shows the resonance spectrum together with the fitting result for the film measured at kOe.
Magnetoelasticity and magnetization dynamics for nitride films
Figure 2b illustrates the experimental setup for measuring the magnetostriction: optical cantilever method20. A rectangular-shaped sample with the size of 10 mm 20 mm was fixed on one side and illuminated with a laser beam from the vertical direction of the film surface. A rotational of up to 175 Oe was applied in the in-plane direction to induce the magnetostrictive effect, and the degree of deflection of the sample was measured by the position of the reflected laser light (). Since is the angle between the [100] direction of the nitrides and , i.e. is the [100] of nitrides, this measurement setup corresponds to the evaluation of magnetostriction along [100] (). The dependence of at Oe is plotted in Figure 2c.
The obtained sinusoidal curve was numerically fitted and the displacement of () was obtained, allowing us to evaluate with high accuracy (see Supplementary equation (1)). Figure 2d shows the dependence of for the FeCoN, FeN, and FeMnN films. At the saturated state of magnetization by applying Oe, a large magnetostriction, ppm, is obtained for the FeN film, which is three times larger than the previous report ( ppm11) in absolute value and is close to the theoretical value of ppm by the first-principles calculation10. Also, it is noted that ppm is much larger than the values for Fe-Co alloys without high temperature annealing21, which are representative ferromagnets for the conventional spintronics, and is even in the same order of magnitude as that for the representative magnetostrictive material Fe-Ga. In contrast to FeN, FeCoN and FeMnN exhibit small positive and negative , respectively.
The magnetization dynamics of the FeN, FeCoN, and FeMnN films is given in Figure 2e-Figure 2h. Figure 2e and Figure 2f plot the dependence of the ferromagnetic resonance (FMR) frequency () and resonance linewidth () at the in-plane applied along the direction, which is called the IP configuration. The inset of Figure 2e displays the FMR spectrum of the FeN at Oe. The dependences of and are fitted by the following equations:
where is the gyromagnetic ratio, is the in-plane magnetic anisotropy field, is the effective magnetization, is the inhomogeneous field, and is the damping parameter estimated in the IP configuration. The fitting of as a function of was done with the fixed value of rad Oe with the assumption of g-factor of 2, which enabled to evaluate and as fitting parameters. Those values were used for the fitting of as a function of . Finally, was evaluated from these IP configuration measurements. Similar analyses were carried out for the results at applied in the out-of-plane direction (OOP configuration) as shown in Figure 2g and Figure 2h, where the following equations were used: and , where is the saturation field of magnetization by the out-of-plane . corresponds to the intrinsic term of magnetic damping, which is defined as intrinsic while involves both intrinsic and extrinsic terms22,23. This paper defines , and expresses the extrinsic contribution of magnetic damping constant. Although one may think the nonlocal spin relaxation process24 due to the effect of spin pumping to adjacent layers as a component of , that contribution is negligibly small because of small spin-orbit interaction of Ti capping layer in the present layer stacking.
Composition dependences of magnetic properties
Figures 3a, 3b, and 3c plot the and dependences of , , and , respectively. decreases by the Mn substitution into because exhibits ferrimagnetic spin structures25. Although is a ferromagnet26,27, the Co substitution also reduces , which results from the Co atom having a smaller spin magnetic moment than Fe. decreases by the Mn substitution for . In the case of Co substitution, decreases with increasing and its sign changes to negative at . The most striking features are found in the composition dependence of . First, as mentioned above, the large of −121 ppm is achieved for the present high-quality epitaxial film. Next, the value of takes the negative sign for and , and becomes positive at . More specifically, values can be modulated over a wide range from −121 ppm for to +46 ppm for with close to 0 near . This is clear demonstration that the Co substitution in realizes the large tunability and bipolarity of magnetoelastic property. Another finding is that there is no strong correlation between and (see the Co-rich composition) although both are parameters related to the spin-orbit interaction.
Figures 3d and 3e plot the and dependences of and , respectively. The value of , the sum of intrinsic and extrinsic , shows the maximum value of 0.04 for the film and rapidly decreases with the Mn or Co substitution. The value of , corresponding to intrinsic term of , exhibits the composition dependence similar to that of except for and . From the values of and , is obtained as a function of composition as shown in Fig. 3f, in which the composition dependence of the value is also plotted. One can see that the composition dependences of and are fairly in agreement with each other. Moreover, a correlation is also suggested between and except for the Mn or Co rich region. The values of are shown in the Supplementary Information.
Origins of correlation between magnetostriction and magnetic damping
The finding of correlation between and in the magnetic nitrides, especially the strong correlation with extrinsic allows us to deeply understand the underlying mechanisms of magnetostriction and magnetic damping. The origin of is a long-standing issue28 and the correlation between them, which was reported also for the other systems29,30,31,32, has not been understood yet. In this study, we performed the first-principles calculations for and intrinsic . Because the precise ferrimagnetic spin structure has not been determined for , calculations were performed only for ferromagnetic . Fe and Co can exist at both of the two occupied sites33,34 as shown in Figure 1a.
Figure 4a shows the representative results for the density of states (DOS) for the majority and minority spins of , , and around . Note that the contribution from minority spin states much larger than majority spin especially around . In addition, the peak shift toward lower energy side observed for minority spin states by replacing Fe with Co. The dependence of theoretical is given by the black solid circles in Figure 4b and increasing Co content will lead to the reduction of total magnetic moment. However, the calculated is larger than the experimental values measured at 4 K (open star). Here, we notice that if the position of is shifted to the higher energy side, the calculated results are closer to the experimental results. This is simply explained due to the minority spin dominates the conduction band, hence shift toward higher energy side lead to decrease of the total magnetic moment. The red triangles and blue squares represent the results with shifted by 0.2 and 0.3 eV, respectively. The shift by 0.2 eV is appropriate because the shift by 0.3 eV gives rise to the calculated value lower than the experiment at the Co-rich composition. The position with the 0.2 eV shift is close to the peak top of the minority spin DOS of FeN as shown in Figure 4a.

Figure 4. First-principles calculations on electronic structures and magnetic properties of FeCoN. (a) Density of states (DOS) for the majority and minority spins of FeN (red line), FeCoN (blue line), and FeCoN (green line) around , predicted by first-principles calculations. (b) Composition dependence of theoretical and experimental values in FeCoN. The black circles, red triangles, and blue squares represent the calculation results of shifting by 0, 0.2, and 0.3 eV, respectively. The open stars indicate the experimental values measured at 4 K. (c) Relationship between and for FeN, FeCoN, and FeCoN. The position of eV is denoted by the dotted line. (d) Composition dependence of at eV (black squares) and (purple inverted triangles). (e) Dependence of (black squares) and MAE (red circles) of FeN on without modulation of . (f) Calculated dependence of for FeCoN. The black circles and blue triangles show the results when (no shift) and 0.4 / f.u., respectively. The green squares represent the
Using the DOS with the 0.2 eV shift and the Kamberský torque correlation model35, intrinsic values were calculated for FeCoN. Figure 4c shows the calculated values of () on the scattering rate (), in which the intraband component is dominant in the small region whereas the interband component is dominant in the large region. From the resistivity of 110 cm for FeCoN36, the magnitude of is estimated to be 0.01 eV (denoted by the dotted line in Figure 4c), suggesting that the intraband component is dominant for FeN. Figure 4d compares at eV with the experimental values of (intrinsic term of ).
The calculation qualitatively explains the trend of decreasing with increasing Co amount.
The magnitude of is proportional to 37. Thus, the shift away from the peak position of the minority spin DOS of FeN leads to the decrease in magnetic damping.
Figure 4e shows the total energy () and magnetic anisotropy energy (MAE) of FeN as a function of the lattice constant perpendicular to the film surface () without modulation of the valence electron number (). Assuming , where , , and are constants, can be calculated from the following equation38:
Figure 4f shows the dependence of calculated for FeCoN using equation (1), where the black circles represent the results without modulating and the blue triangles represent the results in case that is increased by 0.4 / f.u. The experimental values are also given by the green squares for comparison. By increasing as in the case of calculation for , the calculated results are fairly in agreement with the experimental results. One sees that the experimentally obtained composition dependences of and for FeCoN (Figure 4d and Figure 4f) are well explained by the first-principles calculations. It is important to note that the sign and magnitude of strongly depend on the derivative of MAE on the lattice parameter (d(MAE)/dc). Using second order perturbation analysis (see Supplementary Fig. 3), we clarified that the dominant contribution to the d(MAE)/dc is given by MAE from the spin conserving term in the minority-spin state, implying the crucial role of minority . Therefore, plays a pivotal role to correlate between intrinsic and .
In addition to the discussion about the correlation between “intrinsic” and , we can discuss the correlation between “extrinsic” and observed experimentally. The extrinsic is partly attributable to two-magnon scattering. A previous paper22 mentioned that magnetostriction coupled with nonuniform stresses is a source of effective field for additional spin wave dynamics, which enhances two-magnon scattering and increases the extrinsic .
Figure 5a displays the cross-sectional high-angle annular dark-field scanning transmission electron microscope (HAADF-STEM) image of the STO(001)/FeN. The inset is a fast Fourier transform (FFT) image. The image shown in Figure 5b is obtained by selecting appropriate diffraction spots from the FFT image and applying inverse FFT. The yellow marks denote the misfit dislocations, and the inhomogeneous strain is introduced around them. Since the lattice mismatches between and do not change significantly ( and for and , respectively), we consider the misfit dislocation density hardly depends on . Therefore, the extrinsic is enhanced in a material with large , and is also a useful indicator to investigate the magnitude of magnetostriction constant.

Figure 5. Microstructure of the FeN film on the STO substrate. (a) Cross-sectional HAADF-STEM image of the STO(001)/FeN. The inset shows a FFT image. (b) Inverse FFT image obtained from the inset of (a). The yellow marks show the misfit dislocations.
Giant tunability and bipolarity of magnetoelasticity
We demonstrated that the large negative can be achieved for the epitaxially grown film and the magnetostriction properties can be significantly varied by partially replacing Fe with Co or Mn. The magnitude of was modulated in a wide range from to ppm. This fact means the giant tunability and bipolarity of magnetostriction in the ferromagnetic nitride. We found that the correlation between and experimentally and theoretically. The first-principles calculations indicated that was the leading term to determine the magnitudes for both intrinsic and , suggesting that appropriate control of is indispensable for developing giant magnetoelastic materials. As for the correlation between extrinsic and , the magnetostriction is a source of the two-magnon scattering, resulting in the large extrinsic with increasing . We believe that the findings obtained on the research platform can give a guiding principle for exploring new giant magnetoelastic materials.
We address several advantages of ferromagnetic nitrides as a material for spintronic strain sensors. The giant tunability and bipolarity of magnetostriction are useful to improve the sensitivity of strain detection. The with large negative exhibits the alignment of magnetic moments along the orthogonal direction to the strain direction whereas the with large positive exhibits the moment alignment along the strain direction. For GMR/TMR-based strain sensors with two or more ferromagnetic layers, these characteristics are essential to obtain the large variation in device resistance determined by the relative angles between the adjacent ferromagnetic layers under the strain application. We expect that the large difference in magnetostriction between the and the significantly improves the device performance. As mentioned in the introductory part, the shows the TMR by combining with a standard tunnel barrier material MgO, and the epitaxial layer can be grown on the flexible substrate. Also, we may realize the largescaled device integration thanks to the fact that does not contain minor metal elements and rare earth elements. Therefore, we conclude that magnetic nitrides are leading candidate materials for high-sensitive spintronic strain sensors.
Methods
Sample fabrication
The nitride films with a thickness of approximately 23 nm were grown on STO(001) substrates using molecular beam epitaxy (MBE). STO substrates were ultrasonically cleaned in the order of acetone, ethanol, and deionized water, and then dipped in buffered hydrofluoric acid. Fe and Co were supplied by using electron beam guns, Mn by a Knudsen Cell, and N by a radio-frequency (rf) radical source (Eiko engineering: ER-1000). The deposition rate was fixed at 0.2 Å/s for the total of Fe+Co and Fe+Mn, and the composition ratio was modulated by changing the supply rate ratio. High purity (6N) N₂ gas was supplied at 1.0 sccm and the rf input power was fixed at 300 W. The deposition temperature was set at 450 °C. For the Fe₄₋ᵧCoᵧN (ᵧ = 1.7 and 2.2) films, the temperature was lowered to 400 °C to prevent nitrogen desorption. Subsequently, a 2-nm-thick Ti capping layer was formed on the nitride layers in an MBE chamber to prevent surface oxidation.
Structural characterization
The structures of the samples were characterized by XRD with a Cu-Kα radiation source (SmartLab: Rigaku Corp.). The film thicknesses were evaluated by an x-ray reflectivity method. The surface morphologies and crystal growth orientations were also monitored by reflection high-energy electron diffraction during the film deposition. The microstructure of the STO/FeN was observed by HAADF-STEM (JEM-ARM200F: JEOL Ltd.). The composition ratios of the nitride films were evaluated using a field emission electron probe microanalyzer (JXA-8530F: JEOL Ltd.) with the standard samples for calibration.
Magnetic property measurement
The magnetization curves at room temperature were measured using a vibrating sample magnetometer (TM-VSM2614HGC-KIT, Tamakawa Co., Ltd.). The values of at 4 K were measured employing a superconducting quantum interference device magnetometer (MPMS3: Quantum Design Inc.). The magnetostriction was evaluated using an optical cantilever system30 (Toei Scientific Industrial Co., Ltd.). FMR spectra were measured at room temperature using a vector network analyzer (N5222A: Agilent Technology) and coplanar wave guides. Frequency-domain FMR measurements were carried out, sweeping rf current in the range of 1 20 GHz and varying . For the IP configuration measurements, an rf-compatible prober station (TKSPHE-3V10: Toei Scientific Industrial Co., Ltd.) was used with 200 2400 Oe applied in the in-plane [100] direction of the films. For the OOP configuration measurements, a physical property measurement system (PPMS: Quantum Design Inc.) was used and 13.0 22.5 kOe was applied in the perpendicular direction to the film surface.
First-principles calculation
We performed first-principles density functional calculation using VASP[39] to obtain electronic structures and MAE of series. The projector augmented-wave (PAW) potential was used to describe the behavior of core electrons[40]. The generalized gradient approximation proposed by Perdew, Burke, and Ernzerhof was adopted for the exchange and correlation energies[41]. A unit cell containing 4 Fe (Co) and 1 N atoms was constructed. The virtual crystal approximation (VCA) was used to describe the mixing between Fe and Co atoms[42]. We used the plane-wave cutoff energy of 350 eV for the wave function expansion and k-point mesh for wave vector integration in the first Brillouin zone. The damping was calculated using Torque Correlation Model by Kamberský35. The MAE was calculated by including spin-orbit interaction self-consistently. The magnetostriction constant was estimated by calculating MAE for a particular range of the lattice constant with fixing the volume of unit cell.
Data availability
The data that support the findings of this study are available from the corresponding authors upon reasonable request. Source data are provided with this paper.
Code availability
Computer codes used in this study are available from the corresponding author upon reasonable request.
Acknowledgements
The authors thank S. Kanai, S. Fukami, R. Y. Umetsu, and Y. Sakuraba for support to measure FMR, S. Mizukami and H. Kurebayashi for their valuable comments, I. Narita for technical support to do the composition analysis, and K. Omura and Y. Murakami for help to perform the XRD measurements. This work was partly supported by the Collaborative Research Center on Energy Materials, Institute for Materials Research (IMR), Tohoku University, and the Cooperative Research Project of the Research Institute of Electric Communication, Tohoku University. The magnetization curve and XRD measurements were carried out at the Cooperative Research and Development Center for Advanced Materials, IMR, Tohoku University. The first-principles calculations of the magnetic damping and the magnetostriction were performed on a Numerical Materials Simulator at NIMS. This work was supported by JSPS KAKENHI Grant Numbers JP22K18894 and JP22H04966, and Initiative to Establish Next-generation Novel Integrated Circuits Centers (X-nics) under Grant JPJ011438, the Ministry of Education, Culture, Sports, Science and Technology (MEXT).
Author contributions
Film growth, XRD measurements, and magnetization curve measurements were carried out by K.I. K.I. and T.S. performed magnetostriction measurements with support from Y.E. K.I. and T.S. performed FMR measurements. Y.S. carried out TEM observations. First-principles calculations were carried out by I.K. with support from Y.M. K.I. and T.S. wrote the draft. All the authors discussed the results and commented on the manuscript. T.S. conceived the project.
Competing interests
The authors declare no competing interests.
Correspondence and requests for materials should be addressed to Keita Ito.

Figure 3. Composition dependences of magnetic properties. Composition dependences of (a) , (b) , (c) , (d) , (e) , and (f) together with for the and films.
experimental results.
Supplementary Information
Supplementary Figure S1 shows the x-ray reflectivity (XRR) profile for the film. The black and red lines correspond to the obtained data and the fitting line, respectively.
Figure S1. XRR profile of the film.
Supplementary Table S1 summarizes the film thicknesses of the nitride films estimated from the XRR. The accuracy of the estimated thicknesses is high because the fitting was done with high precision.
| Samples | Thickness (nm) |
| FeN | 27 |
| FeMnN | 21 |
| FeMnN | 25 |
| FeMnN | 25 |
| FeCoN | 22 |
| FeCoN | 21 |
| FeCoN | 25 |
| FeCoN | 21 |
| FeCoN | 22 |
Table S1. The thicknesses of the nitride films estimated from the XRR.
According to the model for the optical cantilever method, the displacement of reflected position of the laser light () is expressed by the following equation20:
where is the coefficient determined by the measurement system geometry, is the magnetostriction constant along [100] direction, () is the substrate (film) thickness, () is the Young’s modulus of the substrate (film), and () is the Poisson’s ratio of the substrate (film). Supplementary Table 2 summarizes and values of S1, S2, S3, S4, and S5. For the evaluation of for all the samples, the and values of were used because accurate and values for each composition are unknown.
The values of , , , and are close, while the values of , , and are larger than that of . This means that obtained values of the and films are slightly overestimated. However, the overestimation of does not affect the main conclusion of this study.
| Materials | (GPa) | |
| SrTiO | 278 | 0.24 |
| FeN | 162 | 0.36 |
| FeMnN (Ferromagnetic) | 202 | 0.31 |
| FeCoN | 217 | 0.32 |
| CoN | 239 | 0.31 |
Table 2. and values of SrTiO, FeN, FeMnN, FeCoN, and CoN.
As mentioned in the main text, the fitting functions for the resonance linewidth () involve the inhomogeneous magnetic field (): for the IP configuration, and for the OOP configuration. Thus, we evaluated the values of together with and . In the case of IP configuration, the measured values of are remarkably scattered as seen in Figure 2f, which gives rise to the estimated values of with significant errors, e.g. Oe for . Thus, we cannot discuss the values of for the IP configuration because of low accuracy of estimation. In contrast to the IP configuration, the OOP configuration leads to the values of with relatively small errors. Supplementary Fig. 2 plots the composition dependence of estimated in the OOP configuration. One sees that the values of are negligibly small and do not show a clear composition dependence.

Figure Supplementary 2. Composition dependence of inhomogeneous magnetic field () estimated in the out-of-plane configuration.
Supplementary Fig. 3 shows the spin-resolved magnetocrystalline anisotropy energies (MAE) for FeN and CoN in the second-order perturbation of spin-orbit interaction as a function of lattice parameter. We clarified that the dominant contribution to the is given by competing term of negative trend of and positive trend of , where indicates the spin-transition process in the second order perturbation from the initial spin state to the intermediate spin state. For FeN, the former is much more dominant than the latter, hence give the large negative magnetostriction. This means that the anisotropy of orbital moment of Fe related to the significantly contributes to the magnetostriction of FeN. However, the latter is slightly more dominant for CoN. Nevertheless, both cases implying the crucial role of minority-spin . Therefore, plays a major role to correlate between intrinsic and .

Figure 3 (PDF p. 37). Spin-resolved MAE for FeN and CoN in the second-order perturbation of spin-orbit interaction as a function of lattice parameter.
Supplementary references
S1. Pandech, N., Sarasamak, K., & Limpijumnong, S. Elastic properties of perovskite (A = Be, Mg, Ca, Sr, and Ba) and (B = Ti, Zr, and Hf): First principles calculations. J. Appl. Phys. 117, 174108 (2015).
S2. Takahashi, T., Burghaus, J., Music, D., Dronskowski, R., & Schneider, J. M. Elastic properties of - probed by nanoindentation and ab initio calculation. Acta Mater. 60, 2054-2060 (2012).
S3. Wu, H., Sun, H., & Chen, C. Superior magnetic and mechanical property of driven by electron correlation and lattice anharmonicity. Phys. Rev. B 91, 064102 (2015).
S4. Wu, Z & Meng, J. Elastic and electronic properties of , , and from first principles. Appl. Phys. Lett. 90, 241901 (2007).
S5. Azouaoui, A., Benzakour, N., Hourmatallah, A., & Bouslykhane, K. Study of structural, electronic, magnetic, elastic, and thermodynamic properties of antiperovskite by first principles and Monte Carlo simulation. Phys. Status Solidi B 258, 2000339 (2021).
References
- [39]Kresse G. & Furthmüller, J. Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set. Phys. Rev. B 54, 11169-11186 (1996).pubmed.ncbi.nlm.nih.gov/9984901
- [40]Blöchl, P. E. Projector augmented-wave method. Phys. Rev. B 50, 17953-17979 (1994).pubmed.ncbi.nlm.nih.gov/9976227
- [41]Perdew, J. P., Burke, K., & Ernzerhof, M. Generalized gradient approximation made simple. Phys. Rev. Lett. 77, 3865-3868 (1996).pubmed.ncbi.nlm.nih.gov/10062328
- [42]Eckhardt, C., Hummer, K., & Kresse, G. Indirect-to-direct gap transition in strained and unstrained SnₓGe₁₋ₓ alloys. Phys. Rev. B 89, 165201 (2014).