Abstract

A microwave plasma model of a chemical vapour deposition (CVD) reactor is presented for understanding spatial heteroepitaxial growth of polycrystalline diamond on Si. This work is based on the TM0(n>1)p clamshell style reactor (Seki Diamond/ASTEX SDS 6K, Carat CTS6U, ARDIS-100 style) whereby a simplified H_2 plasma model is used to show the radial variation in growth rate over small samples with different sample holders. The model uses several steps: an electromagnetic (EM) eigenfrequency solution, a frequency-transient EM/plasma fluid solution and transient a heat transfer solution at low and high microwave power density. Experimental growths provide model validation with characterisation using Raman spectroscopy and scanning electron microscopy. This work demonstrates that shallow holders result in non-uniform diamond films, with a radial variation akin to the electron density and temperature distribution at the wafer surface. For the same process conditions, greater homogeneity is observed for taller holders, however, if the height is too extreme, the diamond quality reduces. From a modelling perspective, EM solutions are limited but useful for examining electric field focusing at the sample edges, resulting in accelerated diamond growth. For better accuracy, plasma fluid and heat transfer solutions are imperative for modelling spatial growth variation.

Introduction

Chemical vapour deposition (CVD) has become one of the most popular methods for epitaxial growth of single crystal diamond (SCD) and polycrystalline diamond (PCD) for a wide variety of applications. The basis of this technique requires dissociation of a gaseous hydrocarbon pre-cursor (CH4\mathrm{CH}_{4}) at low pressures using a reactive H2\mathrm{H}_{2} species that is excited either using hot filament (HFCVD) [1, 2, 3, 4, 5, 6, 7] or microwave plasma (MPCVD)[8, 9, 10, 11, 12, 13, 14, 15]. Both HFCVD and MPCVD have their advantages and disadvantages for diamond growth. HFCVD offers easier scalability since the activation region simply depends upon the area covered by the tungsten or tantalum filaments. However, metal incorporation is possible[16, 17], the filament stability is challenging[18] and growth rates are moderately low compared to other methods (∼1.6 μm h−1\sim1.6\,\mu\mathrm{m}\,\mathrm{h}^{-1}). MPCVD does not have filament issues since the plasma is formed using electromagnetic (EM) standing waves and the growth rates are much higher (>10 μm h−1>10\,\mu\mathrm{m}\,\mathrm{h}^{-1})[19], although only over small areas making scalability much harder. This makes MPCVD particularly useful for small, millimetre scale sample growth such as SCD for quantum applications[20, 21].

In MPCVD, understanding the size of the plasma activation region is of huge importance as this directly influences the deposition area and the diamond growth rate. The plasma activation region is affected by several process parameters including forward microwave power, pressure, gas flow rate and temperature in addition to physical parameters such as the sample size, sample holder geometry and of course the reactor topology. The effect of each may be understood empirically or through modelling approaches. Experimental data offers the greatest insight as no CVD reactor is the same as another, especially for bespoke builds. A notable example of this is shown for Asmussen et al. where for SCD, it has been empirically shown that a recessed or ‘pocket’ type sample holder results in less unwanted PCD growth at the sample edges [22, 23, 24]. Significant material and machining costs are required in order to experimentally iterate geometrical adjustments. Modelling becomes extremely useful at this point and a viable approach for growth optimisation for various reactors, offering faster and cheaper insights into how modified stages, sample holders and reactor walls affect the plasma. Numerous reactor modelling studies exist to this end; the various topologies include the cylindrical TM01p\mathrm{TM}_{01p} type cavity such as the ASTEX PDS-18, Seki Diamond SDS 5200 series reactors[25, 26, 27, 28, 29], the TM0(n>1)p\mathrm{TM}_{0(n>1)p} type cavity such as the ARDIS-100, Carat Systems CTS6U, Seki Diamond SDS 6K style clamshell [30, 31, 32, 10, 33], the TM02\mathrm{TM}_{02} dome style cavity as developed by Su et al.[34] and the ellipsoidal egg-shaped cavity such as the AIXTRON reactor[25, 35, 36]. For a comprehensive review of modelling different microwave reactor topologies, we referred to Silva et al. [37].

Plasma modelling is not trivial and requires significant development and experimental validation. Fortunately in this decade a number of commercial packages exist, making this avenue more accessible. One such area which requires more attention from the modelling perspective is the sample holder design. Shivkumar et al. have contributed significant understanding of pillar type models to focus the plasma, corroborated with optical emission spectroscopy[27]. A notably recent study by Sedov et al. combines both modelling and experimental growths of the geometrical effect of recessed and pedestal type sample holders for 2" Si wafers using an E-field model, demonstrating that pedestal holders yielded higher quality diamond films when compared to a recessed holder[38].

In this work, we demonstrate a simple microwave plasma model of the TM0(n>1)p_{0(n>1)p} reactor (Seki Diamond 6K style) that can be implemented in COMSOL Multiphysics® for the purpose of sample holder or ‘puck’ design. The model presented here uses a simplified H2_2 reaction cross-section set currently accessible from the Itikawa database on lxcat.net [39]. A simple experimental validation is achieved using a sample puck of varying height, positioning the sample closer or further away from the plasma. The model is compared with experimental characterisation of thin film diamond growths over small Si wafers (∅=1"\varnothing= 1", t=0.5t = 0.5 mm). In § 2 the EM theory is briefly discussed for TM0(n>1)p_{0(n>1)p} style reactors along with the plasma and heat transfer continuity equations for the finite element model (FEM). In § 3 the modelling implementation is shown, including the boundary conditions and the modelling results for. In § 4 the experimental data is presented, including plasma images from the viewports, Raman spectra and scanning electron microscopy (SEM) images of the films.

Theory

Electromagnetic field

The microwave plasma is sustained by the electric (E) field which accelerates the seed electrons to interact with the H2_2 gas molecules. The shape and location of the microwave plasma activation region is therefore dependent upon the spatial EM field within the resonant chamber. One of the quickest methods of modelling the plasma location is to simply calculate the EM field distribution of the resonant mode through eigenfrequency analysis[28]. Analytically, these standing wave distributions are determined by deriving the Helmholtz resonator solution from the time-harmonic

Maxwell’s equations:

∇⋅E=ρcε0(1)\nabla\cdot\mathbf{E} = \frac{\rho_c}{\varepsilon_0} \tag*{(1)}
∇⋅B=0(2)\nabla\cdot\mathbf{B} = 0 \tag*{(2)}
∇×E=−jμ0μrωH(3)\nabla\times\mathbf{E} = -j\mu_0\mu_r\omega\mathbf{H} \tag*{(3)}
∇×H=jε0ωεrE(4)\nabla\times\mathbf{H} = j\varepsilon_0\omega\varepsilon_r\mathbf{E} \tag*{(4)}

where E\mathbf{E} and H\mathbf{H} are the electric and magnetic fields, respectively, εr\varepsilon_r and μr\mu_r are the relative permittivity and permeability of the medium, respectively, ρc\rho_c is the charge density, ε0\varepsilon_0 and μ0\mu_0 are the permittivity and permeability of vacuum, respectively, B=μrμ0H\mathbf{B} = \mu_r\mu_0\mathbf{H} and ω\omega is the angular frequency.

A Helmholtz resonator solution is obtained using vector identities. For transverse magnetic (TM) modes where Hz=0\mathbf{H}_z = 0 and Ez\mathbf{E}_z is finite:

∇2Ez−k2Ez=0(5)\nabla^2\mathbf{E}_z - k^2\mathbf{E}_z = 0 \tag*{(5)}

where k2=ω2ε0εrμ0μrk^2 = \omega^2\varepsilon_0\varepsilon_r\mu_0\mu_r is defined as the wavenumber. Analytical solutions can be derived based on the coordinate system, or solved for using FEM.

Microwave reactor topologies are typically cylindrical or elliptical since the standing wave patterns are based upon Bessel functions which inherently focus the EE-field, and therefore the plasma, into the central regions of the cavity[28]. For example in cylindrical coordinates, ∇2Ez\nabla^2\mathbf{E}_z becomes a Poisson equation:

∂2Ez∂r2+1r∂Ez∂r+1r2∂2Ez∂θ2+∂2Ez∂z2−k2Ez=0(6)\frac{\partial^2\mathbf{E}_z}{\partial r^2} + \frac{1}{r}\frac{\partial\mathbf{E}_z}{\partial r} + \frac{1}{r^2}\frac{\partial^2\mathbf{E}_z}{\partial\theta^2} + \frac{\partial^2\mathbf{E}_z}{\partial z^2} - k^2\mathbf{E}_z = 0 \tag*{(6)}

The radial component has solutions dependent on Bessel functions and the azimuthal and axial components have solutions based on sinusoidal functions. By imposing boundary conditions, the cylindrical TM Ez\mathbf{E}_z field can be obtained:

Ez(r,θ,z)=Jn(αmnar)cos⁡(nπθ)cos⁡(pπlz)(7)\mathbf{E}_z(r,\theta,z) = J_n\left(\frac{\alpha_{mn}}{a}r\right)\cos(n\pi\theta)\cos\left(\frac{p\pi}{l}z\right) \tag*{(7)}

where JnJ_n is the nthn^{\text{th}} order Bessel function aa and ll are the radius and height of the cylinder, respectively, αmn\alpha_{mn} is the nthn^{\text{th}} root of the mthm^{\text{th}} Bessel function and pp is the integer number of axial standing waves. One can then derive all other components of the field distribution using (1) to (4), however, from this equation it is clear which TM modes will be useful for an MPCVD reactor. From a practical point of view, the substrate should be placed in the centre of the reactor as to be as far from the walls as possible to avoid any etch or re-deposition of wall contaminants. Firstly, this means that p>0p > 0 otherwise the absence of an axial standing wave would directly connect the plasma to the top and bottom of the cylindrical cavity walls. Secondly, in order to achieve a centralised plasma, only TM modes which consider E-fields where m=0m = 0 can be used as this is the only Bessel function where the result is non-zero and finite at r=0r = 0. It has been shown that modes where m>0m > 0 can actually be used to monitor the temperature of a cavity resonator as they are less sensitive to the centre[40, 41]. Bessel functions roughly decay proportional to r−1/2r^{-1/2} and with increasing root and frequency, the E-field is further compressed and concentrated into the centre of the cavity. Thus, the ideal case is to use the highest nn possible although this would make a cavity with a very large radius. This defines the conventional use of cylindrical reactors based on TM0np\mathrm{TM}_{0np} modes as it places the E-field central and at either the top or bottom of the cavity. A sample holder becomes crucial to break this degeneracy by disrupting the E-field and encourages the plasma to be localised to only one of these regions.

While the E-field distribution provides a general idea as to where the plasma is to be localised, the simple EM field eigenfrequency approximation does not take into account the perturbation of the diffuse but conductive gas. The relative permittivity of the conductive gas is complex and can be modelled using the Drude-Lorentz model:

εr=1−ωp2ω2+νm2−j(ωp2νmω(ω2+νm2))(8)\varepsilon_r = 1 - \frac{\omega_p^2}{\omega^2 + \nu_m^2} - j\left(\frac{\omega_p^2\nu_m}{\omega(\omega^2 + \nu_m^2)}\right) \tag*{(8)}
ωp=e2neε0me(9)\omega_p = \sqrt{\frac{e^2 n_e}{\varepsilon_0 m_e}} \tag*{(9)}

where ωp\omega_p is the plasma frequency and νm\nu_m is the electron-species collision frequency, ncn_c is the electron density and ee and mem_e are the electron charge and mass, respectively. To introduce the metallic gas of a certain electron density, the microwave frequency and information on how frequently the electrons interact with the pre-cursor gas is needed. Notable methods to incorporate this are the early Füner models, where at a defined threshold E-field value, nen_e would be finite and zero otherwise[27, 25, 42]. While this method is suitable at high pressure such that the plasma ball is confined within the E-field region, this never allows the plasma to be situated in the nodal regions of the standing wave, which contradict the large pancake plasma shapes typically found in TM0(n>1)p\mathrm{TM}_{0(n>1)p} style reactors at low pressures.

Plasma fluid

To fully incorporate the nuance of pressure in larger area reactors, the fluid model is introduced which allows modelling of the collective behaviour of the electrons, ions and neutral species[43, 44, 29, 45]. These gaseous species are initially distributed homogeneously within the cavity and several energy dependent electron-impact reactions are defined with a rate constant or reaction cross section. An example of a simplified reaction set is shown in Figure 1. The accelerated electrons may result in elastic scattering (e+H2→e+H2\mathrm{e} + \mathrm{H}_{2} \rightarrow\mathrm{e} + \mathrm{H}_{2}), excitation of a species (e+H2→e+H2∗\mathrm{e} + \mathrm{H}_{2} \rightarrow\mathrm{e} + \mathrm{H}_{2}^{*}), ionisation (e+H2→e+H2+\mathrm{e} + \mathrm{H}_{2} \rightarrow\mathrm{e} + \mathrm{H}_{2}^{+}) or attachment or detachment of atoms (e+H2→e+2H\mathrm{e} + \mathrm{H}_{2} \rightarrow\mathrm{e} + 2\mathrm{H}). Additional reactions can also occur with these products, producing a soup of various charged and neutral species. As electrons and ions are produced, electrostatic forces and concentration gradients then result in a plasma fluid diffusing around the high E-field regions. The key advantage of the fluid approach is that the plasma has a finite density, allowing the fluid to be modelled as a function of pressure, temperature and even the gas flow velocity.

Image not extracted

Figure 1. Simplified electron impact cross section reactions with H2_2 from the Biagi (MAGBOLTZ), CCC[46, 47, 48], IST Lisbon, Itikawa[39] and Phelps[49] databases (www.lxcat.net, retrieved on September 3rd, 2021). Data used in this study (denoted ’°’ ) is from the Itikawa database with parameters given in the legend.

For the electrons, the fluid is modelled using continuity equations of motion and energy conservation equations. The equation of motion for the number density is:

∂ne∂t+∇⋅Γe=Re(10)\frac{\partial n_{\mathrm{e}}}{\partial t}+\nabla\cdot\boldsymbol{\Gamma}_{\mathrm{e}}=R_{\mathrm{e}} \tag*{(10)}
Γe=−μeneEa−∇Dene(11)\boldsymbol{\Gamma}_{\mathrm{e}}=-\mu_{\mathrm{e}}n_{\mathrm{e}}\mathbf{E}_{\mathrm{a}}-\nabla D_{\mathrm{e}}n_{\mathrm{e}} \tag*{(11)}

where nen_{\mathrm{e}} is the electron density, Γe\boldsymbol{\Gamma}_{\mathrm{e}} is the electron flux vector, μe\mu_{\mathrm{e}} is the electron mobility, DeD_{\mathrm{e}} is the electron diffusivity, Ea\mathbf{E}_{\mathrm{a}} is the ambipolar field and ReR_{\mathrm{e}} represents the electrons that are either produced or consumed during impact reactions. The first term in Γe\boldsymbol{\Gamma}_{\mathrm{e}} is associated with the ambipolar E-field and is the E-field that is generated by the separation of the ions and the electrons. The second term is associated with drift contributions from concentration gradients. Coupled with (10) is an electron energy conservation equation of a similar form. Energy is either lost or gained from elastic/inelastic reactions with the gaseous species, absorbed from microwave heating in the E-field or accelerated in the electrostatic ambipolar fields:

∂nε∂t+∇⋅Γε+Ea⋅Γe=Sε+Qmwe(12)\frac{\partial n_{\varepsilon}}{\partial t}+\nabla\cdot\boldsymbol{\Gamma}_{\varepsilon}+\mathbf{E}_{\mathrm{a}}\cdot\boldsymbol{\Gamma}_{\mathrm{e}}=S_{\varepsilon}+\frac{Q_{\mathrm{mw}}}{e} \tag*{(12)}
Γε=−μεnεEa−∇Dεnε(13)\boldsymbol{\Gamma}_{\varepsilon}=-\mu_{\varepsilon}n_{\varepsilon}\mathbf{E}_{\mathrm{a}}-\nabla D_{\varepsilon}n_{\varepsilon} \tag*{(13)}

where nεn_{\varepsilon} is the electron energy density, Γε\Gamma_{\varepsilon} is the electron energy flux vector, με\mu_{\varepsilon} is the electron energy mobilty, DεD_{\varepsilon} is the electron energy diffusivity, SεS_{\varepsilon} is the energy gain or loss from impact reactions and QmwQ_{\mathrm{mw}} is the microwave heating of the electrons.

For the heavier gas species such as ions and neutral molecules, the continuity equations are similar to the electrons, however, may include inertial terms from the background gas flow velocity (omitted in this model). For multiple reaction species (H2_2, H2+_2^+ and H2∗_2^*), the continuity relation for the ithi^{\mathrm{th}} specie is:

ρi∂wi∂t=∇⋅Γi+Ri(14)\rho_i \frac{\partial w_i}{\partial t} = \nabla\cdot\Gamma_i + R_i \tag*{(14)}
Γi=ρiwivd(15)\Gamma_i = \rho_i w_i v_d \tag*{(15)}

where ρi\rho_i is the density, wiw_i is the mass fraction, Γi\Gamma_i is the ion flux vector, RiR_i represents the ions that are either produced or consumed in reactions and vdv_d is the species diffusion velocity.

Heat transfer model

In addition to the plasma fluid model, the gas temperature (or neutral/ion species temperature) is calculated over time assuming a simple conductive heat transfer model using a mass averaged gas density, heat capacity, thermal conductivity and the EM power dissipated. The continuity equations for this calculation are:

ρnCp∂T∂t=∇⋅(k∇T)+Qmw(16)\rho_n C_p \frac{\partial T}{\partial t} = \nabla\cdot(k\nabla T) + Q_{\mathrm{mw}} \tag*{(16)}

where ρn=pMn/RT\rho_n = pM_n/RT is the gas density, pp is the pressure, MnM_n is the mean molar mass, RR is the gas constant, TT is the temperature, CpC_p is the heat capacity and kk is the thermal conductivity.

Modelling

Method

The FEM process is split into three separate studies as shown in Figure 2. First, the EM model is run where the eigenfrequencies of the geometry are calculated to ensure that the correct mode is identified (the TM0(n>1)p\mathrm{TM}_{0(n>1)p} type mode where a TM011\mathrm{TM}_{011} distribution is present in the active region of the reactor). This step is crucial for determining if any reactor modifications or the introduced sample holders shift the frequency away from the source generator frequency range. Additionally, higher order modes which are not necessary for diamond growth can also be identified. Secondly, the frequency-transient electromagnetic/plasma model is calculated at the eigenfrequency. The reactor port power is varied and provides a continuous wave to set up the EM standing wave. In this way the EE-field intensity, and therefore the plasma, is power dependent. The electrons and gaseous species are distributed within the cavity and the transient response is modelled from 0 to 10 s to allow the plasma fluid to evolve to a steady state at an initial ignition power and pressure (1.5 kW at 20 mbar) or low microwave power density (MWPD). Subsequently, the MWPD is ramped up to growth conditions or high MWPD (5 kW at 160 mbar) over the simulated time of 1 hour to keep the solution stable. Finally, the third step calculates a heat transfer solution to obtain the gas temperature using the microwave power dissipated in the plasma.

Image not extracted

Figure 2. Finite element modelling process flow using COMSOL Multiphysics®.

The cavity boundary conditions are also shown in Figure 3. The mesh is kept consistent in all steps, utilising a free quadratic with boundary layers at the extremities for the plasma solution. The mesh also forces a distribution of 50 nodes across the Si sample surface to ensure a high resolution for the spatially dependent electron densities. For the first EM eigenfrequency model, the chamber domain is assumed vacuum and the walls are all modelled as metallic impedance boundary conditions (σ>107\sigma> 10^{7} S/m). To reduce computation time in the plasma model, the domain is only confined to the centre of the reactor, marked by the outflow/electron outlet conditions in Figure 3. The gas pressure of this domain is varied from 20 to 160 mbar. For the plasma model, all walls are defined as grounds with additional surface reactions for excited species to relax to neutral species (H2∗→H2\mathrm{H}_2^* \to\mathrm{H}_2, H2+→H2\mathrm{H}_2^+ \to\mathrm{H}_2). The cross-section reactions for the gaseous species have adopted a simplified hydrogen plasma similar to Yamada et al. [29] to reduce computation time with a dataset obtained from the Itikawa database[39] (available on lxcat.net). The reactor port PiP_i is defined as a lumped port with excitation varying from 1.5 to 5 kW. For the heat transfer model, heat flux boundary conditions are imposed to the extremities to ensure that the sample holder stage is at the correct temperature of approximately 800 °C. The heat flux boundaries simulate the cooling of the reactor using a fixed systematic heat transfer coefficient for all sample holder heights (a modelled cooling flux of 850 W m−1^{-1} K for all external boundaries with an ambient temperature of 25 °C). The sample is modelled as a Si wafer (∅=1′′\varnothing= 1'', t=0.5t = 0.5 mm) and is positioned on top of the Mo sample holder puck (∅puck=40\varnothing_{\mathrm{puck}} = 40 to 60 mm, hpuck=1h_{\mathrm{puck}} = 1 to 20 mm). The corners of the sample are rounded with a radius of 0.1 mm and the Mo holder rounded with a radius of 0.2 mm to ensure a high mesh density at the anticipated high E-field regions and avoid convergence errors.

Image not extracted

Figure 3. Simplified schematic of the clamshell reactor (Carat Systems CTS6U). Wall surfaces are modelled as impedance boundary conditions. The dotted line denotes axial symmetry about r=0r = 0. PiP_i denotes a lumped coaxial port boundary condition. The red outflow lines denote the limits of the fluid simulation as electron and heat outlets for the plasma and heat transfer solutions, respectively. P1 denotes the location of the plasma region.

Electromagnetic model

Figure 4 shows the EM eigenfrequency model with the E-field distribution of an ideal TM011_{011} mode and the TM0(n>1)p_{0(n>1)p} reactor without the Mo sample puck. The TM0(n>1)p_{0(n>1)p} reactor mode shows a reasonably similar E-field distribution to the ideal case, demonstrating that the correct mode has been identified. In this mode, there is an E-field node separating the central region and a side lobe. High intensity E-field regions at the edge of the stage are found where a secondary plasma can also be sustained. Figure 5 shows how the calculated resonant frequency of the EM model is perturbed to lower frequencies as a Mo sample puck is introduced. With the current dimensions, the initial unperturbed resonant frequency is calculated at approximately 2.45 GHz with a -3 dB bandwidth of ∼87\sim87 MHz. The results show that wider pucks have less of a frequency shift, while taller pucks alter the resonant frequency by as much as Δf≈−66\Delta f \approx-66 MHz at hpuck=20h_{\mathrm{puck}} = 20 mm. This demonstrates that shorter sample pucks are more favourable for stable operation with a magnetron with a fixed frequency output. Interestingly, this is not so much a problem for solid state sources since the signal generator frequency can varied.

Image not extracted

Figure 4. The base EM eigenfrequency model without the Mo sample holder puck. The E-field is normalised to the maximum value. For comparison and identification of the correct mode, the ideal cylindrical case of the TM011_{011} mode (left side) and the realistic TM0(n>1)p_{0(n>1)p} design (right side) are shown.

Image not extracted

Figure 5. Modelled shift in resonant frequency caused by the Mo sample holder puck of varying dimensions; hpuckh_{\mathrm{puck}} and ∅puck\varnothing_{\mathrm{puck}} denote the height and diameter, respectively. The sample holder has a Si wafer sample on top (∅=1"\varnothing= 1", t=0.5t = 0.5 mm).

After introducing the puck, the E-field distribution of the EM model is shown in Figure 6(a). The E-field is perturbed and high intensity regions occur at the corners of the puck. This is simply because of Maxwell’s equations (1) and (7); the EzE_z field lines should be perpendicular to the Cu stage and the introduction of a metal object creates parallel surfaces that disrupts this condition resulting in a reconfiguration of surface currents. With increasing sample holder puck height, the E-field, and therefore the plasma activation region, is concentrated towards the edges of the holder. The nodal regions of the E-field are also clearly visible either side of the puck where, based on the threshold modelling approach, the plasma could not exist; or if it did, the plasma could exist in multiple regions in the cavity. It is also noted that with increasing sample holder height, the E-field hot spots at the top of the chamber reduce in intensity, decreasing the likelihood for a secondary plasma to ignite at these regions.

Image not extracted

Figure 6. Microwave hydrogen plasma model using the simplified eigenfrequency, plasma coupled and heat transfer solution approach for varying sample holder heights (hpuck=5h_{\mathrm{puck}} = 5 to 20 mm) with a Si wafer on top (∅=1"\varnothing= 1", t=0.5t = 0.5 mm). Model uses cross-section data from the Itikawa database, available on lxcat.net[39].

Plasma Model

The plasma fluid models are shown in Figure 6(b) and 6(c) and clearly demonstrate a focused electron density in the sample region. The calculated electron densities are as high as 2.2×1017 m−32.2 \times10^{17}\ \mathrm{m}^{-3} and 10×1017 m−310 \times10^{17}\ \mathrm{m}^{-3} in the low and high MWPD models, respectively. Based on a ωp=2.45\omega_p = 2.45 GHz, nc=7.45×1016 m−3n_c = 7.45 \times10^{16}\ \mathrm{m}^{-3}, stipulating that at these electron densities, the microwaves are not able to propagate freely through the plasma and thus attenuates, thereby depositing microwave power into the plasma[37]. Note that in the low MWPD solution the electron density distribution is much wider than the E-field result, demonstrating that simple EM solutions are potentially less appropriate for modelling low pressure plasmas. Although PCD diamond growth with low non-diamond carbon impurities typically occurs at high MWPD, the lower pressure solutions are an imperative result for several purposes. The first is that some applications involve nano-crystalline diamond (NCD) and ultra-nanocrystalline diamond (UNCD) which is typically grown at lower power densities[50, 51, 52] as well as hybrid graphene-diamond films[53]. The second is to ensure that the plasma can actually be ignited at the right place in the chamber. Finally, investigating large area growth using lower pressure would be challenging using an EM solution alone. At low MWPD and at large heights of 15 to 20 mm, the sample is pushed further into the the plasma and the fluid moves towards the electron outlets at the side of the stage. This is not favourable as the risk of the plasma pushing to below the stage towards the quartz ring region where the microwaves enter is much greater. At high MWPD, the plasma becomes the familiar elliptical shape situated over the sample with a smaller area and a much higher electron density (ne∼10×1017n_{\mathrm{e}} \sim10 \times10^{17} m−3^{-3}), similar electron densities to those found in previous models of different reactors at growth conditions[44, 54, 45]. At high MWPD, higher Mo sample pucks result in the plasma further focusing towards the edges which will inherently affect the spatial CVD diamond growth rate across the sample.

Heat Transfer Model

The heat transfer solution at high MWPD shows that the temperature of the gas reaches several tens of thousands Kelvin. Although these values are much higher than those reported by Shivkumar et al. in cylindrical TM01p_{01p} type reactors (∼\sim2,500 K) [27], in that study the modelled MWPD was lower (700 W at 30 Torr) which cannot be easily sustained in the TM0(n>1)p_{0(n>1)p} reactor. The gas temperature is hotter at shallower puck heights and decreases significantly as the puck is pushed

Image not extracted

Figure 7. Average gas temperature (solid) and electron temperature (dotted) over the plasma fluid domain region (P1 in Figure 3) at different sample holder heights.

into the plasma. This is likely due to the fact that the sample puck is in direct contact with the heavily cooled Cu stage underneath and an increasing volume of Mo increases the thermal mass of the puck, thereby reducing the temperature. Figure 7 shows the averaged gas and electron temperatures over the ellipse drawn over the plasma region (defined as P1 in Figure 3). Here, it becomes clear that at low MWPD, the plasma is not at thermodynamic equilibrium as the electron temperature (TeT_{\mathrm{e}}) is much higher than the background gas temperature (TgT_{\mathrm{g}}) at low MWPD. Increasing the gas pressure increases the number of electron-hydrogen collisions which increases TgT_{\mathrm{g}} and reduces TeT_{\mathrm{e}}. At high MWPD, for a modelled central substrate temperature of approximately 800 °C, the plasma tends towards a collisional plasma condition.

Experiment

Experimental method

To demonstrate the overall affect of the sample holder height on the CVD diamond process, three Mo pucks were machined (∅=40\varnothing= 40 mm, hpuck=5h_{\mathrm{puck} } = 5, 10 and 15 mm) and used for thin film growths (approximately 1 µm thick) on small Si wafers (∅=1\varnothing= 1”, t=0.5t = 0.5 mm). It is worth stipulating that a fourth puck (hpuck=20h_{\mathrm{puck} } = 20 mm) was also machined, however, stable plasma ignition was not possible. This is likely due to the holder significantly perturbing the resonant frequency of the chamber. The Si wafers were seeded using the ultrasonic seeding process[55, 56]. Briefly, the wafers were solvent cleaned and placed in a nanodiamond colloidal solution with a particles of a positive zeta potential whilst under ultrasonic agitation for 10 minutes. The samples were then rinsed in deionised water, dried using an air gun and placed on the top of the sample holder inside of a TM0(n>1)p\mathrm{TM}_{0(n>1)p} style reactor for CVD diamond growth. Samples were grown using a CH4/H2CH_4/H_2 gas mixture with a CH4CH_4 concentration of 3% in a total flow rate of 300 sccm at a forward microwave power of 5 kW at 160 mbar. The total growth time for all samples was fixed at 30 minutes, followed by a 5 minute cool down ramp to 1.5 kW at 27 mbar. The temperature at growth MWPD was monitored using a Williamson dual wavelength pyrometer (DWF-24-36C), giving initial measured readings of 760, 790 and 780 °C for the 5, 10 and 15 mm growths, respectively. Two samples for each molybdenum puck height were grown at different reactor usage times.

After growth, the samples were examined using Raman spectroscopy and scanning electron microscopy (SEM). Raman spectroscopy was conducted using a Horiba LabRAM HR Evolution with a green laser (λ=532\lambda= 532 nm) and a grating of 600 l/mm from 200 to 2000 cm−1^{-1} to allow for sensitivity to both the diamond and non-diamond carbon content. Line scans were taken at points across the samples (N=20N = 20 points over 22 mm). SEM images were obtained using a Hitachi SU8200 (10 kV at 10 μ\muA) with a working distance of 8 mm.

Microwave Plasma

Figure 8 shows the typical images of a microwave H2/CH4H_2/CH_4 plasma at ignition and at the point of reaching diamond growth conditions with different puck heights in the TM0(n>1)p\mathrm{TM}_{0(n>1)p} reactor. At low power density the plasma emits a purple glow associated with the combined emissions of the Hα_{\alpha} (∼657\sim657 nm), Hβ_{\beta} (∼486\sim486 nm) and the Hγ_{\gamma} (∼437\sim437 nm) lines[57]. As the MWPD is increased, the plasma becomes the familiar green ellipsoid over the sample holder, characteristic of C2_2 emission from the small CH4_4 concentration. The images show that the low pressure plasma extends well beyond the extents of the puck, into where the EM E-Field nodes are calculated to be. The edges of the 15 mm puck are also much brighter compared to the 5 mm puck owing to the E-field focusing. The increase in MWPD results in a smaller and focused ellipsoid above the puck, with the higher 15 mm puck distorting the bottom edges shape of the plasma.

Image not extracted

Figure 8. Photographs of the microwave H2/CH4H_2/CH_4 plasma at low (left column) and high (right column) MWPD for sample puck heights of 5 mm (top row) and 15 mm (bottom row), respectively. Low MWPD plasma is at 1.5 kW at 27 mbar, while high MWPD is 5 kW at 160 mbar with 3% CH4CH_4 in a total flow rate of 300 sccm. Images were taken from the side viewport of the Carat Systems CTS6U using an Apple iPhone 7.

Scanning Electron Microscopy

SEM images of the films are shown in Figure 9 at incremental regions from the centre towards the edge of 1" Si wafer. These images show clear radial variations in growth rate depending on the height of the sample puck. Starting with the film grown at a height of 5 mm, at a radial position of 0 mm (centre of the film) shows a large size distribution with grains as large as ∼1\sim1 μ\mum down to the nanoscale. At 2.5 mm, these large micron size grains are still apparent, however much are fewer in distribution and a larger fraction of nanoscale grains is found. Moving further outwards, the micron size grains begin to disappear, and only nanoscale grain texturing is observed. Finally reaching the edges of the film, the grain size suddenly increases showing significant growth of a microcrystalline film. Next, for the film grown at a height of 10 mm, there is minimal radial grain size variation from 0 up to 10 mm, showing similarly large micron size grains as the 5 mm sample except has coalesced with less nanoscale grains. However, at the edge of the film there is a clear jump again in growth rate with evidence of much larger grains. Finally, for the film grown at a height of 15 mm, the centre of the film also shows minimal radial variation from 0 up to 10 mm with the exception of a much smaller average grain size. In a similar fashion to the previous samples, the growth rate towards the edges of the film is much faster and much larger grains are found.

Image not extracted

Figure 9. SEM images of the CVD diamond films grown at varying Mo sample holder heights (5, 10 and 15 mm). Images are taken at fixed radial distances from the centre of the wafer to the edge. Scale bar represents a 5 μ\mum length.

Raman Spectroscopy

Raman spectra at the centre of the wafers of the thin diamond films grown at different Mo puck heights are shown in Figure 10 (a). The high intensity peak at 520 cm−1\mathrm{cm}^{-1} and the band at approximately 950 cm−1\mathrm{cm}^{-1} are attributed to the first and second order bands of Si[58, 14]. Since the growth time is fairly short, the diamond films are fairly thin, therefore the contribution of the Si substrate is large. The sharp peak at 1332 cm−1\mathrm{cm}^{-1} is attributed to the first order sp3\mathrm{sp}^{3} carbon peak, a signature characteristic of diamond[59, 60, 58, 61, 62]. Amongst this diamond peak are several broad bands associated with various non-diamond carbon impurities. The weak band at approximately 1420 cm−1\mathrm{cm}^{-1} and even weaker band at approximately 1120 cm−1\mathrm{cm}^{-1} are both attributed to trans-polyacetylene (tPA), commonly found in CVD diamond Raman spectra although are only dominant at particularly low grain sizes such as nanocrystalline diamond (NCD)[63, 52, 64]. The broad band at approximately 1310 to 1340 cm−1\mathrm{cm}^{-1} is attributed to the A1g\mathrm{A}_{1g} breathing mode of aromatic sp2\mathrm{sp}^{2} carbon rings, while the peak at around 1580 to 1610 cm−1\mathrm{cm}^{-1} is attributed to the E2g\mathrm{E}_{2g} bond stretching mode in sp2\mathrm{sp}^{2} carbon[64]. The low intensity of these non-diamond carbon signatures compared to the sp3\mathrm{sp}^{3} peak at a laser excitation wavelength of 532 nm implies a low non-diamond carbon impurity concentration; in heavily sp2\mathrm{sp}^{2} incorporated films, these band often dominate the sp3\mathrm{sp}^{3} peak[50, 55].

Figure 10. Raman spectroscopy of CVD diamond on 1” Si wafers grown at holder heights of 5 mm, 10 mm and 15 mm for 30 minutes (5 kW 160 mbar). (a) shows the spectra at the centre of the wafer. The labels ‘d’, ‘D’, ‘G’ and ‘tPA’ denote the contributions from the sp3sp^3 carbon peak in diamond, the D and G bands of sp2sp^2 carbon and trans-polyacetylene, respectively. (b) shows a line scan of the intensity ratio of ‘d’ / ‘G’, or the implied sp3sp^3 / sp2sp^2 or non-diamond carbon ratio. (c) shows the temperature recorded by the pyrometer, where the inset shows a zoom in at the start point. Pyrometer lower limit is 315 °C.

The line scans of the dd / GG ratio in Figure 10 (b) show that there is a significant variation in the diamond growth across the 1" Si wafer. For all samples, the sp3\mathrm{sp}^{3}/ sp2\mathrm{sp}^{2} peak ratio is much higher at the edges of the sample compared to the centre. This implies a much faster growth rate at the edges of the sample which is corroborated in the plasma model by the focusing effect at the samples edges, and therefore an increased plasma and reaction density. At a radial position of approximately 10 mm from the centre, the sp3/sp2\mathrm{sp}^{3}/\mathrm{sp}^{2} peak ratio rapidly decreases for all sample heights. For the film grown at a height of 5 mm, almost no diamond peak is found whereas for the films grown at heights of 10 and 15 mm, the sp3/sp2\mathrm{sp}^{3}/\mathrm{sp}^{2} ratio is fairly similar towards the centre of the film. At the centre, a noticeable hump in the sp3/sp2\mathrm{sp}^{3}/\mathrm{sp}^{2} ratio is found, which gradually disappears with increasing puck height. This variation is again caused by the variation in the plasma density across the sample; as shown in Figure 3 the plasma tends towards the classic central ellipsoidal shape at shallow heights and pushes towards the edges for taller pucks at high MWPD.

Discussion

It is clear from the modelling and experimental results that the Mo sample puck height has a considerable effect on the plasma shape and therefore the spatial diamond growth rate across a 1" Si wafer. For comparison between the model and the experiment, Figure 11 shows line scans of the E-field magnitude, plasma electron density and substrate temperature across the sample from the EM, plasma and heat transfer solutions, respectively. Clear correlations and limitations in the model are identified when compared with the SEM and Raman data. For the EM model, the E-field distribution only shows the high intensity regions at the edges of the sample and almost no sign of the broad hump in the centre. This highlights a limitation of the E-field modelling approach in predicting growth rate variations across small samples. However, the plasma fluid model shows that there is a clear bump at the centre of the film for the 5 mm puck height and then becomes increasingly flatter as the puck height is increased. The electron density alone however implies that the growth rate would be much faster for a shallower puck over a taller puck which does not appear to not be the case from the Raman line scan spectra and the SEM images. The reason is likely due to the temperature at the sample surface during growth. The experimentally measured temperature is shown in Figure 10 (c) where the temperature is marginally lower for the 5 mm puck (∼760\sim760 °C) when compared to the 10 mm (∼790\sim790 °C) and 15 mm (∼780\sim780 °C) pucks. In fact, the films with the most consistent quality are those grown on the 10 mm puck, with growth temperatures closer to the typical CVD diamond growth temperature of ∼800\sim800 °C. Thus, the electron density plasma model is only representative of some spatial growth variation but less accurate when used to compare between holders. The heat transfer solution provides a better insight as is shown in Figure 11, where the temperature line scans show both the radial variation in temperature and that the 10 mm puck has a higher growth temperature than the others, thereby producing a better quality film.

Figure 11. Model line scans over the Si sample surface of (a) the E-field magnitude in the EM model, (b) the plasma electron density and (c) the substrate temperature.

The result from this experiment is that shallower pucks are heavily cooled by the stage which reduces the substrate temperature for a given process growth condition. As the height of the puck increases, the sample is pushed into the plasma and the substrate temperature increases. However, if the puck is too tall, the plasma is largely perturbed and then focuses to the edges and away from the sample substrate. Additionally, since a larger volume of Mo is in contact with the cooled stage, the TgT_{\mathrm{g}} is reduced and therefore the substrate temperature. This model demonstrates that if the users goal is to optimise spatial homogeneity across a sample then this puts precedence on monitoring the spatial temperature across the sample during growth.

Conclusion

Modelling of microwave hydrogen plasmas can offer simple and cost effective insights into how sample holder designs can affect MPCVD processes. This work demonstrates that EM eigenfrequency models show how sample holder pucks of different width and diameter can perturb the reactor frequency where in this instance, taller pucks have a much larger effect on frequency. Additionally, strict EM modelling approaches have some limitations at both low and high MWPD and are generally useful for identifying possible regions for the plasma to spark, but do not necessarily describe the plasma shape. Fully coupled EM/plasma models offer a better description which models the power and pressure size and electron density. Using multi-physics coupling of EM, plasma and heat transfer solutions, the spatial variation in diamond growth can be estimated through variations in the substrate temperature.

Acknowledgements

This project has been supported by Engineering and Physical Sciences Research Council (EP-SRC) under the GaN-DaME program grant (EP/P00945X/1) and the European Research Council (ERC) Consolidator Grant under the SUPERNEMS Project (647471). SEM was carried out in the cleanroom of the ERDF-funded Institute for Compound Semiconductors (ICS) at Cardiff University.

References

  1. [1]R. Sachan, A. Bhaumik, P. Pant, J. Prater, J. Narayan, Diamond film growth by HFCVD on Q-carbon seeded substrate, Carbon 141 (2019) 182–189. doi:10.1016/j.carbon.2018.09.058.DOI
  2. [2]J. Narayan, A. Bhaumik, S. Gupta, P. Joshi, P. Riley, R. Narayan, Role of Q-carbon in nucleation and formation of continuous diamond film, Carbon 176 (2021) 558–568. doi:10.1016/j.carbon.2021.02.049.DOI
  3. [3]M. Amaral, A. Fernandes, M. Vila, F. Oliveira, R. Silva, Growth rate improvements in the hot-filament CVD deposition of nanocrystalline diamond, Diamond and Related Materials 15 (11-12) (2006) 1822–1827. doi:10.1016/j.diamond.2006.07.024.DOI
  4. [4]M. Ali, M. Ürgen, Surface morphology, growth rate and quality of diamond films synthesized in hot filament CVD system under various methane concentrations, Applied Surface Science 257 (20) (2011) 8420–8426. doi:10.1016/j.apsusc.2011.04.097.DOI
  5. [5]G. D. Barber, W. A. Yarbrough, Growth Rate of Diamond on Polycrystalline <110> Diamond Substrates from Carbon Disulfide in Hydrogen by Hot-Filament-Assisted Chemical Vapor Deposition, Journal of the American Ceramic Society 80 (6) (1997) 1560–1566. doi:10.1111/j.1151-2916.1997.tb03016.x.DOI
  6. [6]T. Tabakoya, S. Kanada, Y. Wakui, Y. Takamori, T. Yamada, M. Nagai, et al., High-Rate Growth of Single-Crystalline Diamond (100) Films by Hot-Filament Chemical Vapor Deposition with Tantalum Filaments at 3000 °C, Physica Status Solidi (A) Applications and Materials Science 216 (21) (2019) 4–7. doi:10.1002/pssa.201900244.DOI
  7. [7]X. Liang, L. Wang, H. Zhu, D. Yang, Effect of pressure on nanocrystalline diamond films deposition by hot filament CVD technique from CH4/H2 gas mixture, Surface and Coatings Technology 202 (2) (2007) 261–267. doi:10.1016/j.surfcoat.2007.05.032.DOI
  8. [8]S. Mandal, K. Arts, H. C. Knoops, J. A. Cuenca, G. M. Klemencic, O. A. Williams, Surface zeta potential and diamond growth on gallium oxide single crystal, Carbon 181 (2021) 79–86. doi:10.1016/j.carbon.2021.04.100.DOI
  9. [9]A. Tallaire, O. Brinza, P. Huillery, T. Delord, C. Pellet-Mary, R. Staacke, et al., High NV density in a pink CVD diamond grown with N2O addition, Carbon 170 (2020) 421–429. doi:10.1016/j.carbon.2020.08.048.DOI
  10. [10]J. Weng, F. Liu, L. W. Xiong, J. H. Wang, Q. Sun, Deposition of large area uniform diamond films by microwave plasma CVD, Vacuum 147 (2018) 134–142. doi:10.1016/j.vacuum.2017.10.026.
  11. [11]J. A. Cuenca, M. D. Smith, D. E. Field, F. C-P. Massabau, S. Mandal, J. Pomeroy, et al., Thermal stress modelling of diamond on GaN/III-Nitride membranes, Carbon 174 (2021) 647–661. doi:10.1016/j.carbon.2020.11.067.DOI
  12. [12]P. Achatz, J. A. Garrido, M. Stutzmann, O. A. Williams, D. M. Gruen, A. Kromka, et al., Optical properties of nanocrystalline diamond thin films, Applied Physics Letters 88 (10) (2006) 11–13. doi:10.1063/1.2183366.DOI
  13. [13]F. Bénédic, M. Belmahi, T. Easwarakhanthan, P. Alnot, In situ optical characterization during MPACVD diamond film growth on silicon substrates using a bichromatic infrared pyrometer under oblique incidence, Journal of Physics D: Applied Physics 34 (7) (2001) 1048–1058. doi:10.1088/0022–3727/34/7/305.
  14. [14]V. S. Sedov, A. K. Martyanov, A. A. Khomich, S. S. Savin, V. V. Voronov, R. A. Khmelnitskiy, et al., Co-deposition of diamond and β-SiC by microwave plasma CVD in H2-CH4-SiH4 gas mixtures, Diamond and Related Materials 98 (July) (2019) 107520. doi:10.1016/j.diamond.2019.107520.DOI
  15. [15]F. Fendrych, A. Taylor, L. Peksa, I. Kratochvilova, J. Vlcek, V. Rezacova, et al., Growth and characterization of nanodiamond layers prepared using the plasma-enhanced linear antennas microwave CVD system, Journal of Physics D: Applied Physics 43 (37) (2010). doi:10.1088/0022–3727/43/37/374018.DOI
  16. [16]S. Ohmagari, H. Yamada, N. Tsubouchi, H. Umezawa, A. Chayahara, S. Tanaka, et al., Large reduction of threading dislocations in diamond by hot-filament chemical vapor deposition accompanying W incorporations, Applied Physics Letters 113 (3) (2018). doi:10.1063/1.5040658.DOI
  17. [17]P. Mehta Menon, A. Edwards, C. S. Feigerle, R. W. Shaw, D. W. Coffey, L. Heatherly, et al., Filament metal contamination and Raman spectra of hot filament chemical vapor deposited diamond films, Diamond and Related Materials 8 (1) (1999) 101–109. doi:10.1016/S0925–9635(98)00444–0.
  18. [18]S. Okoli, R. Haubner, B. Lux, Influence of the filament material on low-pressure hot-filament cvd diamond deposition, Le Journal de Physique IV 02 (C2) (1991) C2–923–C2–930. doi:10.1051/jp4:19912111.DOI
  19. [19]A. P. Bolshakov, V. G. Ralchenko, V. Y. Yurov, A. F. Popovich, I. A. Antonova, A. A. Khomich, et al., High-rate growth of single crystal diamond in microwave plasma in CH4/H2 and CH4/H2/Ar gas mixtures in presence of intensive soot formation, Diamond and Related Materials 62 (2016) 49–57. doi:10.1016/j.diamond.2015.12.001.DOI
  20. [20]J. Achard, V. Jacques, A. Tallaire, Chemical vapour deposition diamond single crystals with nitrogen-vacancy centres: A review of material synthesis and technology for quantum sensing applications, Journal of Physics D: Applied Physics 53 (31) (2020). doi:10.1088/1361-6463/ab81d1.DOI
  21. [21]A. Mallik, Microwave Plasma CVD Grown Single Crystal Diamonds – A Review, Journal of Coating Science and Technology 3 (2) (2016) 75–99. doi:10.6000/2369-3355.2016.03.02.4.DOI
  22. [22]S. Nad, J. Asmussen, Analyses of single crystal diamond substrates grown in a pocket substrate holder via MPACVD, Diamond and Related Materials 66 (2016) 36–46. doi:10.1016/j.diamond.2016.03.007.DOI
  23. [23]G. Wu, M. H. Chen, J. Liao, The influence of recess depth and crystallographic orientation of seed sides on homoepitaxial growth of CVD single crystal diamonds, Diamond and Related Materials 65 (2016) 144–151. doi:10.1016/j.diamond.2016.03.011.DOI
  24. [24]A. Charris, S. Nad, J. Asmussen, Exploring constant substrate temperature and constant high pressure SCD growth using variable pocket holder depths, Diamond and Related Materials 76 (March) (2017) 58–67. doi:10.1016/j.diamond.2017.04.010.DOI
  25. [25]M. Füner, C. Wild, P. Koidl, Simulation and development of optimized microwave plasma reactors for diamond deposition, Surface and Coatings Technology 116-119 (1999) 853–862. doi:10.1016/S0257-8972(99)00233-9.DOI
  26. [26]A. M. Gorbachev, V. A. Koldanov, A. L. Vikharev, Numerical modeling of a microwave plasma CVD reactor, Diamond and Related Materials 10 (3-7) (2001) 342–346. doi:10.1016/S0925-9635(00)00503-3.DOI
  27. [27]G. Shivkumar, S. S. Tholeti, M. A. Alrefae, T. S. Fisher, A. A. Alexeenko, Analysis of hydrogen plasma in a microwave plasma chemical vapor deposition reactor, Journal of Applied Physics 119 (11) (2016). doi:10.1063/1.4943025.DOI
  28. [28]F. Silva, X. Bonnin, J. Scharpf, A. Pasquarelli, Microwave analysis of PACVD diamond deposition reactor based on electromagnetic modelling, Diamond and Related Materials 19 (5-6) (2010) 397–403. doi:10.1016/j.diamond.2009.10.032.DOI
  29. [29]H. Yamada, A. Chayahara, Y. Mokuno, Y. Horino, S. Shikata, Simulation of temperature and gas flow distributions in region close to a diamond substrate with finite thickness, Diamond and Related Materials 15 (10) (2006) 1738–1742. doi:10.1016/j.diamond.2006.03.001.DOI
  30. [30]H. Yamada, Numerical simulations to study growth of single-crystal diamond by using microwave plasma chemical vapor deposition with reactive (H, C, N) species, Japanese Journal of Applied Physics 51 (9) (2012). doi:10.1143/JJAP.51.090105.DOI
  31. [31]H. Yamada, A. Meier, F. Mazzocchi, S. Schreck, T. Scherer, Dielectric properties of single crystalline diamond wafers with large area at microwave wavelengths, Diamond and Related Materials 58 (2015) 1–4. doi:10.1016/j.diamond.2015.05.004.DOI
  32. [32]Y. F. Li, J. J. Su, Y. Q. Liu, M. H. Ding, X. L. Li, G. Wang, et al., Design of a new TM021 mode cavity type MPCVD reactor for diamond film deposition, Diamond and Related Materials 44 (2014) 88–94. doi:10.1016/j.diamond.2014.02.010.DOI
  33. [33]V. S. Sedov, A. K. Martyanov, A. A. Khomich, S. S. Savin, E. V. Zav edeev, V. G. Ralchenko, Deposition of diamond films on Si by microwave plasma CVD in varied CH4-H2 mixtures: Reverse nanocrystalline-to-microcrystalline structure transition at very high methane concentrations, Diamond and Related Materials 109 (September) (2020) 108072. doi:10.1016/j.diamond.2020.108072.DOI
  34. [34]J. Su, Y. Li, M. Ding, X. Li, Y. Liu, G. Wang, et al., A dome-shaped cavity type microwave plasma chemical vapor deposition reactor for diamond films deposition, Vacuum 107 (2014) 51–55. doi:10.1016/j.vacuum.2014.04.002.DOI
  35. [35]X. Li, W. Tang, F. Wang, C. Li, L. Hei, F. Lu, A compact ellipsoidal cavity type microwave plasma reactor for diamond film deposition, Diamond and Related Materials 20 (3) (2011) 374–379. doi:10.1016/j.diamond.2011.01.025.DOI
  36. [36]P. Li, Z. Mao, Z. Peng, L. Zhou, Y. Chen, P.-H. Huang, et al., Acoustic separation of circu-lating tumor cells, Proceedings of the National Academy of Sciences of the United States of America 112 (16) (2015) 4970–4975. doi:10.1073/pnas.1504484112.DOI
  37. [37]F. Silva, K. Hassouni, X. Bonnin, A. Gicquel, Microwave engineering of plasma-assisted CVD reactors for diamond deposition, Journal of Physics: Condensed Matter 21 (36) (2009) 364202. doi:10.1088/0953-8984/21/36/364202.DOI
  38. [38]V. Sedov, A. Martyanov, A. Altakhov, A. Popovich, M. Shevchenko, S. Savin, et al., Effect of substrate holder design on stress and uniformity of large-area polycrystalline diamond films grown by microwave plasma-assisted cvd, Coatings 10 (10) (2020) 1–10. doi:10.3390/coatings10100939.DOI
  39. [39]J.-S. Yoon, M.-Y. Song, J.-M. Han, S. H. Hwang, W.-S. Chang, B. Lee, et al., Cross Sections for Electron Collisions with Hydrogen Molecules, Journal of Physical and Chemical Reference Data 37 (2) (2008) 913–931. doi:10.1063/1.2838023.DOI
  40. [40]J. A. Cuenca, D. R. Slocombe, A. Porch, Temperature Correction for Cylindrical Cavity Perturbation Measurements, IEEE Transactions on Microwave Theory and Techniques 65 (6) (2017) 2153–2161. doi:10.1109/TMTT.2017.2652462.DOI
  41. [41]J. A. Cuenca, D. Slocombe, A. Porch, Corrections to "Temperature Correction for Cylindrical Cavity Perturbation Measurements", IEEE Transactions on Microwave Theory and Techniques (2017). doi:10.1109/TMTT.2017.2751550.
  42. [42]M. Füner, C. Wild, P. Koidl, Numerical simulations of microwave plasma reactors for diamond CVD, Surface and Coatings Technology 74-75 (1995) 221–226. doi:10.1016/0257-8972(95)08232-8.DOI
  43. [43]H. Yamada, A. Chayahara, Y. Mokuno, S. I. Shikata, Model of reactive microwave plasma discharge for growth of single-crystal diamond, Japanese Journal of Applied Physics 50 (1 PART 2) (2011). doi:10.1143/JJAP.50.01AB02.
  44. [44]H. Yamada, A. Chayahara, Y. Mokuno, Simplified description of microwave plasma discharge for chemical vapor deposition of diamond, Journal of Applied Physics 101 (6) (2007). doi:10.1063/1.2711811.DOI
  45. [45]K. Hassouni, T. A. Grotjohn, A. Gicquel, Self-consistent microwave field and plasma discharge simulations for a moderate pressure hydrogen discharge reactor, Journal of Applied Physics 86 (1) (1999) 134–151. doi:10.1063/1.370710.DOI
  46. [46]I. Bray, A. T. Stelbovics, Convergent close-coupling calculations, Phys. Rev. A 46 (11) (1992) 6995–7011.
  47. [47]M. C. Zammit, D. V. Fursa, I. Bray, Electron scattering from the molecular hydrogen ion and its isotopologues, Physical Review A - Atomic, Molecular, and Optical Physics 90 (2) (2014) 1–15. doi:10.1103/PhysRevA.90.022711.DOI
  48. [48]M. C. Zammit, J. S. Savage, D. V. Fursa, I. Bray, Complete Solution of Electronic Excitation and Ionization in Electron-Hydrogen Molecule Scattering, Physical Review Letters 116 (23) (2016) 1–5. doi:10.1103/PhysRevLett.116.233201.DOI
  49. [49]S. J. Buckman, A. V. Phelps, Vibrational excitation of D 2 by low energy electrons, The Journal of Chemical Physics 82 (11) (1985) 4999–5011. doi:10.1063/1.448673.DOI
  50. [50]J. A. Cuenca, K. J. Sankaran, P. Pobedinskas, K. Panda, I.-N. Lin, A. Porch, et al., Microwave cavity perturbation of nitrogen doped nano-crystalline diamond films, Carbon 145 (2019) 740–750. doi:10.1016/j.carbon.2018.12.025.DOI
  51. [51]O. A. Williams, O. Douhéret, M. Daenen, K. Haenen, E. Osawa, M. Takahashi, Enhanced diamond nucleation on monodispersed nanocrystalline diamond, Chemical Physics Letters 445 (4-6) (2007) 255–258. doi:10.1016/j.cplett.2007.07.091.DOI
  52. [52]K. J. Sankaran, C.-J. Yeh, S. Kunuku, J. P. Thomas, P. Pobedinskas, S. Drijkoningen, et al., Microstructural Effect on the Enhancement of Field Electron Emission Properties of Nanocrystalline Diamond Films by Li-Ion Implantation and Annealing Processes, ACS Omega 3 (8) (2018) 9956–9965. doi:10.1021/acsomega.8b01104.
  53. [53]A. F. Carvalho, T. Holz, N. F. Santos, M. C. Ferro, M. A. Martins, A. J. Fernandes, et al., Simultaneous CVD synthesis of graphene-diamond hybrid films, Carbon 98 (2016) 99–105. doi:10.1016/j.carbon.2015.10.095.DOI
  54. [54]M. W. Kelly, J. C. Richley, C. M. Western, M. N. Ashfold, Y. A. Mankelevich, Exploring the plasma chemistry in microwave chemical vapor deposition of diamond from C/H/O gas mixtures, Journal of Physical Chemistry A 116 (38) (2012) 9431–9446. doi:10.1021/jp306190n.
  55. [55]O. A. Williams, Nanocrystalline diamond, Diamond and Related Materials 20 (5-6) (2011) 621–640. arXiv:0704.0701, doi:10.1016/j.diamond.2011.02.015.
  56. [56]S. Mandal, Nucleation of diamond films on heterogeneous substrates: a review, RSC Advances 11 (17) (2021) 10159–10182. doi:10.1039/d1ra00397f.DOI
  57. [57]K. W. Hemawan, R. J. Hemley, Optical emission diagnostics of plasmas in chemical vapor deposition of single-crystal diamond, Journal of Vacuum Science & Technology A: Vacuum, Surfaces, and Films 33 (6) (2015) 061302. doi:10.1116/1.4928031.
  58. [58]S. Prawer, R. J. Nemanich, Raman spectroscopy of diamond and doped diamond., Philosophical transactions. Series A, Mathematical, physical, and engineering sciences 362 (1824) (2004) 2537–2565. doi:10.1098/rsta.2004.1451.DOI
  59. [59]C. Ramaswamy, Raman Effect in Diamond, Nature 125 (3158) (1930) 704–704. doi:10.1038/125704b0.DOI
  60. [60]S. Bhagavantam, Relation of Raman Effect to Crystal Structure, Indian Journal of Physics 5 (1930) 169.
  61. [61]D. S. Knight, W. B. White, Characterization of diamond films by Raman spectroscopy, Journal of Materials Research 4 (2) (1989) 385–393. doi:10.1557/JMR.1989.0385.DOI
  62. [62]Z. J. Ayres, J. C. Newland, M. E. Newton, S. Mandal, O. A. Williams, J. V. Macpherson, Impact of chemical vapour deposition plasma inhomogeneity on the spatial variation of sp² carbon in boron doped diamond electrodes, Carbon 121 (2017) 434–442. doi:10.1016/j.carbon.2017.06.008.DOI
  63. [63]K. J. Sankaran, J. Kurian, H. C. Chen, C. L. Dong, C. Y. Lee, N. H. Tai, et al., Origin of a needle-like granular structure for ultrananocrystalline diamond films grown in a N2/CH4plasma, Journal of Physics D: Applied Physics 45 (36) (2012). doi:10.1088/0022–3727/45/36/365303.DOI
  64. [64]A. C. Ferrari, J. Robertson, Interpretation of Raman spectra of disordered and amorphous carbon, Physical Review B 61 (20) (2000) 14095–14107. doi:10.1103/PhysRevB.61.14095.DOI

Paper details

vlnc:W_n5gedjmy
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents