betaFeedback

WorksPhysics and Astronomy

Strong impact of low-level substitution of Mn by Fe on the magnetoelectric coupling in TbMnO3TbMnO_{3}

Abstract

The correlation between static magnetoelectric coupling and magnetic structure was investigated in TbMn0.98Fe0.02O3TbMn_{0.98}Fe_{0.02}O_{3} with magnetic field up to 8 T and down to 2 K. Single-crystal neutron diffraction experiments reveal a substantial increase in the temperature dependence of the incommensurate modulation wave vector of the antiferromagnetic phase as the magnetic field strength increases. Magnetic field-dependent pyroelectric current measurements revealed significantly higher magnetoelectric coupling at magnetic fields below 4 T than in pure TbMnO3. This is due to the higher sensitivity of the incommensurably modulated cycloid structure to weak magnetic fields. Detailed analysis of our data confirmed that the ferroelectric polarization is induced by inverse Dzyaloshinskii-Moriya interaction for magnetic field strength up to 4 T, but at higher fields a departure from theoretical predictions is ascertained, giving evidence for an additional, as yet misunderstood, contribution to magnetoelectric coupling. It shows that a small 2% substitution of Mn3+ by Fe3+ has a strong impact on the magnetic structure, promoting the destabilization of the incommensurably modulated magnetic cycloidal structure of TbMnO3TbMnO_{3} in a magnetic field above 5 T. We demonstrate that the magnetoelectric coupling magnitude can be tuned through suitable substitutional elements, even at low level, inducing local lattice distortions with different electronic and magnetic properties.

Introduction

Magnetoelectric multiferroics, where spontaneous long-range magnetic ordering and ferroelectricity coexist and are coupled, represent a very attractive class of compounds combining rich and fascinating fundamental physics [1, 2]. A key point to be studied in this report is the effect of controlled chemical substitution on the relationship between structure, magnetism, ferroelectricity and magnetoelectric coupling. In this regard, the solid solution TbMn1−xFexO3\mathrm{TbMn}_{1-x}\mathrm{Fe}_x\mathrm{O}_3 proved to be a suitable system to unravel such delicate coupling between magnetism and ferroelectricity [3, 4, 5, 6]. Although the Mn3+\mathrm{Mn}^{3+} cation is Jahn-Teller active, unlike the Fe3+\mathrm{Fe}^{3+} cation, they have the same ionic radius for the 66th coordination, allowing to synthetize isostructural solid solutions in all xx-range. However, the substitution of Mn3+\mathrm{Mn}^{3+} by Fe3+\mathrm{Fe}^{3+} implies a change in the octahedra distortions of perovskite lattice, with high impact on the magnetic and polar properties. Previous experimental studies in TbMn1−xFexO3\mathrm{TbMn}_{1-x}\mathrm{Fe}_x\mathrm{O}_3 at ambient temperature have evidence for the linear decrease of the cooperative Jahn-Teller distortion amplitude for 0≤x≤0.50 \le x \le0.5, and its suppression for higher Fe-concentrations [7]. Furthermore, the octahedra tilting has been found to be sensitive to the amplitude of the Jahn-Teller distortion, which gives clear evidence for the role played by the interplay between structure and magnetism, with impact on the ferroelectric stabilization [7].

TbMnO3\mathrm{TbMnO}_3 is a type-II multiferroic [8] prototype with a large magnetoelectric coupling. Its phase diagram can be summarized as follows. At room conditions, TbMnO3\mathrm{TbMnO}_3 is a paraelectric paramagnet with orthorhombic crystal structure described by the Pbnm\mathit{Pbnm} space group [8]. At TN=41T_\mathrm{N}=41 K, TbMnO3\mathrm{TbMnO}_3 undergoes an antiferromagnetic (AFM) phase transition, with incommensurate sinusoidal collinear order of the Mn3+\mathrm{Mn}^{3+} spins [9, 10]. In this phase, the spins are aligned along the bb-axis with a temperature dependent propagation vector, taking the value qm=(0 0.29 1)\mathbf{q}_\mathrm{m}=(0\ 0.29\ 1) at TNT_\mathrm{N} [9, 10]. Accompanying the magnetic modulation structure, there is a lattice modulation with wavevector found to be kl=2qm\mathbf{k}_\mathrm{l}=2\mathbf{q}_\mathrm{m} [11, 12]. Below TC=28T_\mathrm{C}=28 K, the sinusoidal spin modulation turns into a cycloidal spiral in the bcbc-plane, as revealed by neutron diffraction studies [9, 10]. Whether the magnetic modulation remains incommensurate or changes into commensurate is still a matter of debate, since it becomes weakly temperature dependent below TCT_\mathrm{C} but not completely locking in a fixed commensurate value [9, 10, 11, 13]. The emergence of a spontaneous electric polarization along the cc-axis coincides with the cycloid spin ordering below TCT_\mathrm{C}, implying an intrinsic entanglement between the spiral-type antiferromagnetism and ferroelectricity [8, 14]. According to N. Aliouane et al. [15], TbMnO3\mathrm{TbMnO}_3 exhibits quadratic magnetoelastic coupling in the absence of applied magnetic field. Still, a linear magnetoelastic coupling emerges in TbMnO3_3 when an external magnetic field is applied along the bb-axis, so that ferroelectricity is no longer a secondary effect [15]. The linear magnetoelastic coupling drives a magneto-structural transition from the cycloidal modulated phase, with the spontaneous polarization along the cc-axis, to a phase with the spontaneous polarization along the aa-axis, for a magnetic field higher than 4.5 T [14]. When the external field is applied along the aa-axis, a similar flop is found but at higher critical field of about 9 T [14]. Upon further temperature decrease, a quasi-long-range ordering of the ff electrons spins of the Tb3+^{3+} ions takes place below TNTb≈7T_{\mathrm{N}}^{\mathrm{Tb}} \approx7 K [9, 10].

In general, the isovalent partial substitution of Mn by Fe (TbMn1−x_{1-x}Fex_xO3_3) modifies the sequence of phase transitions [5]. However, for low-level substitution, corresponding to 0<x<0.050 < x < 0.05, the phase sequence is found to be the same as in TbMnO3_3, although both TNT_{\mathrm{N}} and TCT_{\mathrm{C}} decrease with increasing xx, while TNTbT_{\mathrm{N}}^{\mathrm{Tb}} barely shifts [6]. The critical temperatures decrease with increasing xx, gives clear evidence for the destabilization of the magnetic interactions underlying the magnetic properties [6]. The main outcome concerns the decrease of the maximum electric polarization as Fe3+^{3+} content increases towards x=0.04x = 0.04, which has been attributed to the gradual fading out of the cycloidal spin ordering with increasing xx, and the suppression of ferroelectricity for x≥0.05x \geq0.05 [6].

Most of the previous studies in the multiferroic region of the TbMn1−x_{1-x}Fex_xO3_3 solid solution (0<x<0.050 < x < 0.05) relied on polycrystalline samples, losing information regarding the anisotropic properties of both polarization and magnetism [4, 6]. Because such features play important roles in the pure compound, they are assumed to be particularly important in the multiferroic region of the solid solution as well. In particular, the direction of the applied magnetic field should have interesting effects on the magnetic structure, some of which inferred by the direction of polarization switching from the cc- to the aa-axis [14]. To understand in more detail the magnetic structure and magnetoelectric coupling of low-level Fe-substituted TbMnO3_3, we performed a detailed study of the temperature and magnetic field dependence of the ferroelectric polarization of oriented TbMn0.98_{0.98}Fe0.02_{0.02}O3_3 single crystals. Neutron diffraction data in TbMn0.98_{0.98}Fe0.02_{0.02}O3_3 are discussed in connection with the results of polarization measurements, towards the characterization of the magnetoelectric coupling. The systematic study of magnetoelectric phenomena provides a deeper understanding of the effect of the B-site cation on the microscopic mechanisms underlying the magnetic and polar properties in TbMnO3_3.

Experimental Details

High quality TbMn0.98Fe0.02O3\mathrm{TbMn}_{0.98}\mathrm{Fe}_{0.02}\mathrm{O}_3 single crystals were grown by floating zone method in an FZ-T-4000 (Crystal Systems Corporation) mirror furnace, using MnO2\mathrm{MnO}_2, Tb4O7\mathrm{Tb}_4\mathrm{O}_7 and Fe2O3\mathrm{Fe}_2\mathrm{O}_3 as starting materials. The starting powders were mixed in the intended Tb:Mn:Fe stoichiometric ratio, cold pressed into rods and sintered at 1100 °C for 12–14 h in air. Growing was performed in air atmosphere, feed and seed rod were rotated with a speed of 30 rpm in opposite directions and a pulling speed of 6 mm/h was used. The typical length of a grown ingot was between 3 and 5 cm [3, 4]. The obtained ingot was oriented using Laue diffraction patterns and special care was taken to avoid macle. The samples were cut from a macle free region of the oriented ingot. The samples were first characterized by X-ray diffraction and Raman scattering at room temperature, and temperature dependent magnetization and specific heat. The obtained results are in good agreement with published data [3, 4].

The pyroelectric currents were measured in a standard Quantum Design PPMS while heating at a rate of 5 K min−15\ \mathrm{K\,min}^{-1}, after cooling under a fixed applied magnetic field. The pyroelectric current measurements were performed after poling the crystals with an electric field of 100 V mm−1100\ \mathrm{V\,mm}^{-1}, while cooling from a temperature above the Néel temperature. Before measuring, the poling electric field was turned off at 2 K. The temperature dependence of the electric polarization was obtained through time integration of the measured pyroelectric currents.

Single crystal neutron diffraction under applied magnetic field was measured at Wish beamline of the ISIS Neutron and Muon Source at the Rutherford Appleton Laboratory of the Science and Technology Facilities Council. Single crystal neutron diffraction patterns were recorded at fixed temperatures between 5 and 50 K after cooling the sample under an applied magnetic field along the bb-axis, up to 8 T. The sample was inserted in a helium flow Oxford cryostat, placed in such a way that the bb-axis is oriented in the vertical direction, parallel to the applied magnetic field, generated by a 9 T magnet. This magnet has an 80° window in the horizontal and a 30° one in the vertical directions. Due to the magnet surrounding the sample, only a restricted angle range could be measured. With this configuration, limited number of nuclear and magnetic diffraction peaks could be studied as a function of temperature and magnetic field, with the condition that the (hkl)(hkl) peaks have k=0k=0 or k=qMnk=q_{\mathrm{Mn}}.

Results

Polar properties under magnetic field

This section is focused on the temperature dependence of the electric polarization, obtained in the following measurement configurations: E∥aE \parallel a and B∥bB \parallel b, and E∥cE \parallel c and B∥aB \parallel a, bb, and cc, for which the largest effects of the applied magnetic field on the polar properties of TbMn0.98_{0.98}Fe0.02_{0.02}O3_3 are found.

Figure 1 (a) and Figure 1 (b) show the temperature dependence of the pyroelectric current density, J(T)J(T), of TbMn0.98_{0.98}Fe0.02_{0.02}O3_3 measured along the aa- and cc-axes, respectively, under an applied magnetic field (0 – 9 T) along the bb-axis. The corresponding temperature dependence of the electric polarization, along the aa- and cc-axis, obtained from the time integration of the pyroelectric current density, is presented in Figure 1 (c) and Figure 1 (d), respectively. At 0 T, the pyroelectric current density measured along the cc-axis, Jc(T)J_c(T), peaks at TCT_\mathrm{C} = 23 K, as expected according to earlier reports for TbMn0.98_{0.98}Fe0.02_{0.02}O3_3 ceramics, evidencing the onset of the ferroelectric phase, with spontaneous electric polarization along the cc-axis [6]. This anomaly slightly downshifts with increasing magnetic field strength, reaching 21 K at 9 T.

Temperature dependence of pyroelectric current densities and electric polarization

Figure 1. Temperature dependence of the ((a), (b)) pyroelectric current densities and ((c), (d)) electric polarization of TbMn0.98Fe0.02O3\mathrm{TbMn}_{0.98}\mathrm{Fe}_{0.02}\mathrm{O}_3, measured along the aa- and cc-axes under an applied magnetic field along the bb-axis. The insets show a magnified view of the temperature profiles of the pyroelectric current density.

A second anomaly in Jc(T)J_c(T) is observed at lower temperatures, but only for a magnetic field strength above 2 T. This anomaly peaks in opposite sense relatively to the first one, and monotonously upshifts from 6 K, for 2 T, to 14 K, for 9 T. Its amplitude exhibits a non-monotonous magnetic field dependence, being maximum at 5 T. At 0 T, Pc(T)P_c(T) monotonously increases on cooling from TCT_\mathrm{C} = 23 K, and its value at 2 K is 350 μC/m2\mu\mathrm{C}/\mathrm{m}^2, 58% smaller than the maximum polarization observed in TbMnO3_3 after poling in twice higher field (200 Vmm−1^{-1}) [14]. The decrease of the PcP_c value in TbMn0.98_{0.98}Fe0.02_{0.02}O3_3 has been reported as a consequence of the destabilization of the magnetic structure due to the changes in magnetic interactions promoted by Fe3+^{3+} [6]. As the magnetic field increases toward 3 T, Pc(T)P_c(T) shows a maximum, peaking at highest temperatures according to the magnetic field strength, and then shifts to lower temperatures on further magnetic field increase up to 5 T. Interestingly, the value of PcP_c at fixed temperatures decreases at a faster magnetic field rate for B>5.5B > 5.5 T. The Pc(T)P_c(T) curve changes its shape for at 6 T, fading out with decreasing temperature, in such a way that for 9 T, Pc∼0P_c \sim0 below 13 K. Contrarily to TbMnO3_3, the magnetic field evolution of Pc(T)P_c(T), with B∥bB \parallel b is more gradual in this compound [14].

Concerning the temperature dependence of the pyroelectric current density recorded along the aa-axis, Ja(T)J_a(T), a small anomaly at Tc=23T_c = 23 K is already observed for 0 T contrary to pure TbMnO3\mathrm{TbMnO}_3, where no anomaly was detected [14]. As the magnetic field strength increases, the amplitude of this anomaly decreases and downshifts, following a similar temperature trend as observed for Jc(T)J_c(T) (see inset of Figure 1(a)). Due to the similar temperature behavior, we assign this anomaly to the minor electric polarization projection in the measurement direction, due to a small misorientation in the sample. A second anomaly in Ja(T)J_a(T) emerges at low temperatures with the same sign as the first one. The second anomaly peaks at higher temperatures and its amplitude increases as the magnetic field strength increases. These results evidence the enhancement of the electric polarization along the aa-axis as the magnetic field increases, as seen in Figure 1 (c). The maximum electric polarization along the aa-axis, recorded at 2 K and 8 T, is about 70% of the maximum spontaneous polarization value measured at the same temperature along the cc-axis, in the absence of the applied magnetic field. In TbMnO3\mathrm{TbMnO}_{3}, the maximum value of the electric polarization along the aa-axis is about 67% of the maximum value of the electric polarization from the cc-axis, after the magnetically induced polarization flop [14].

Figure 1(e) shows the temperature dependence of the electric polarization measured under applied magnetic field along the aa-axis (B∥aB \parallel a). The pyroelectric current Jc(T)J_{c}(T), shown in the inset of Figure 1(e), exhibits just one anomaly, peaking at TC=23T_{C} = 23 K, weakly dependent on the field strength. However, the amplitude of this anomaly decreases with increasing field strength; consequently, the electric polarization is a decreasing function of the magnetic field strength, gradually converging to the limit value 110 μC/m2\mu\mathrm{C}/\mathrm{m}^{2}, contrarily to what is observed when the magnetic field is applied along the other two crystallographic axes. At 9 T, the value of PcP_{c} at the lowest temperature is 25% of the value obtained in TbMnO3\mathrm{TbMnO}_{3} which, however, was poled at twice higher electric field [14].

Figure 1 (f) depicts the temperature dependence of the electric polarization and pyroelectric current (inset of Figure 1 (f)) measured along the cc-axis, under different magnetic field strength, applied along the same cc-axis. Only one anomaly is observed in Jc(T)J_{c}(T) for all the values of the field strength; as consequence, at a fixed magnetic field, the electric polarization increases monotonously on cooling below TCT_{C}. Moreover, the Jc(T)J_{c}(T) anomaly peaks at Tc=23T_{c} = 23 K for 0 T, monotonously decreasing the peaking temperature as the magnetic field increases, reaching 16 K for 9 T (see inset of Figure 1 (f)). The amplitude of this anomaly also decreases and eventually disappears for B>9B > 9 T, meaning that the electric polarization is a decreasing function of the applied magnetic field along c-axis, reaching negligible values for 9 T. The latter result contrasts with the temperature/magnetic field dependence of the electric polarization of TbMnO3\mathrm{TbMnO}_{3} measured in the same configuration but poled at twice higher electric field [14]. In fact, for B<6B < 6 T, Pc(T)P_{c}(T) is weakly dependent on the magnetic field, increasing with decreasing temperature, although a change of slope of Pc(T)P_{c}(T) is observed just below 10 K [14]. However, as the magnetic field increases further from 6 T, the Pc(T)P_{c}(T) curve profile changes and, for 8 and 9 T, the electric polarization takes non-negligible values between TCT_{C} and 15 K [14].

Neutron diffraction

In this section, we will address the temperature and magnetic field dependencies of the measured nuclear and magnetic diffraction peaks. Figure 2 shows representative neutron diffraction patterns, recorded at fixed temperatures in the 5–50 K range, and fixed magnetic field strength (0–8 T range), applied along the bb-axis. The results recorded for other magnetic field strengths and same temperatures, are shown in Figure S1 of Supplemental Information [16]. Only the upper half part of the detectors panel is presented, with the main observed diffraction peaks indexed. Experimental restrictions, due to the configuration of the magnets, prevented us from collecting enough diffraction peaks to determine the real space spin structure.

Diffraction patterns of TbMn0.98Fe0.02O3 at different fixed temperatures and magnetic fields

Figure 2. Diffraction patterns of TbMn0.98Fe0.02O3\mathrm{TbMn}_{0.98}\mathrm{Fe}_{0.02}\mathrm{O}_3, recorded at different fixed temperatures and magnetic fields of 0 T (a), 4 T (b) and 8 T (c), applied along the bb-axis.

Diffraction patterns of TbMn0.98Fe0.02O3 at different fixed temperatures and magnetic fields

Figure S1. Diffraction patterns of TbMn0.98_{0.98}Fe0.02_{0.02}O3_3, recorded at different fixed temperatures and magnetic fields of (a) 2 T and (b) 6 T, applied along the bb-axis.

Above TN=39T_{\mathrm{N}} = 39 K, only nuclear peaks are observed and are indexed to reflections from the (0 0 2)(0\ 0\ 2), (1 0 5)(1\ 0\ 5) and (1 0 3)(1\ 0\ 3) crystallographic planes. From the analysis of these peaks, the temperature and magnetic field dependence of the aa and cc lattice parameters was determined, as shown in Figure S2 of Supplemental Information for 0 and 8 T, respectively [16]. The lattice parameters slightly decrease with decreasing temperature in the 5–50 K range and their values are magnetic field independent. These results evidence for the negligible influence of both the magnetic phase transitions and the applied magnetic field on the lattice parameters, within the sensitivity of the diffraction technique. However, this does not mean that the magnetic phase transitions do not involve atomic motions, because the inversion center must be broken to the electric polarization appear. Recently, spin-phonon coupling was ascertained from a temperature dependent Raman scattering study in TbMn0.98Fe0.02O3\mathrm{TbMn}_{0.98}\mathrm{Fe}_{0.02}\mathrm{O}_3, where small anomalies in the temperature dependence of the wavenumber of some phonons assigned to Tb-oscillations and symmetrical stretching mode of the oxygen octahedra were detected [3]. However, the magnetoelastic coupling is rather small in this compound to be observed through neutron diffraction techniques.

Temperature dependence of the a and c lattice parameters

Figure S2. Temperature dependence of the aa (a) and cc (b) lattice parameters of TbMn0.98Fe0.02O3\mathrm{TbMn}_{0.98}\mathrm{Fe}_{0.02}\mathrm{O}_{3}, measured at 0 T (red) and 8 T (blue), respectively. The vertical dashed lines mark the critical temperatures and the solid line is a guide for the eyes.

As the temperature lowers from TN=39T_{\mathrm{N}} = 39 K, well-defined magnetic diffraction peaks appear along with the nuclear diffraction peaks (see Figure 2). This is the case of the magnetic superlattice peak attributed to the Mn3+\mathrm{Mn}^{3+} moment ordering with propagation wavevector (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1) (qMnq_{\mathrm{Mn}} is expressed in reciprocal lattice units, r.l.u.), which appears just below TNT_{\mathrm{N}}, as it was also reported for TbMnO3\mathrm{TbMnO}_3 [9, 10, 12]. This peak is observed in the 0 – 8 T magnetic field strength range. On further cooling, a second magnetic superlattice peak appears, but only below TC=23T_{\mathrm{C}} = 23 K. Following Kajimoto et al, we assign this peak to the G-type propagation wavevector (1 qMn 3)(1\ q_{\mathrm{Mn}}\ 3) of the Mn3+\mathrm{Mn}^{3+} moment ordering structure; the intensity of the (1 qMn 3)(1\ q_{\mathrm{Mn}}\ 3) magnetic superlattice peak strongly increases below TCT_{\mathrm{C}} of TbMnO3\mathrm{TbMnO}_3, being negligibly small above this temperature [10]. Due to the limited qq-space covered in this experiment, we could not observe the Tb3+\mathrm{Tb}^{3+} magnetic superlattice peaks. Still, the Tb3+\mathrm{Tb}^{3+} spin ordering is ascertained from the appearance of other magnetic superlattice peaks and a strong diffuse scattering around the (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1) peak. Under applied magnetic field, we observe an additional Bragg peak indexed to (1 0 4)(1\ 0\ 4) and assigned to a (weak) ferromagnetic spin ordering, likely associated with a spin canting induced by the applied field. In the following, we shall address the temperature and magnetic field dependencies of the magnetic diffraction peaks.

Figure 3(a) shows the temperature dependence of the intensity of the magnetic superlattice peak (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1), recorded at 0, 4, 6 and 8 T, as representative examples. On cooling below TN=39T_{\mathrm{N}} = 39 K, the intensity of this reflection increases, and is enhanced by the applied magnetic field, the effect being more pronounced in the temperature range of the ferroelectric phase. A detailed analysis of the temperature dependence of the intensity of the magnetic superlattice peak (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1), reveals a small magnetic field dependent kink at TCT_{\mathrm{C}}, which, for the case of B=0B = 0 T as representative example, can be clearly observed in the inset of Figure 3(a), where the solid line describes the temperature-dependent intensity, I(T)I(T), in the TC<T<TNT_{\mathrm{C}} < T < T_{\mathrm{N}} range, extrapolated for T<TCT < T_{\mathrm{C}}. The small but clear deviation of the experimental intensity on cooling below TCT_{\mathrm{C}} was also reported for TbMnO3\mathrm{TbMnO}_3 [9, 10], and it gives clear evidence for the interplay between magnetism and ferroelectricity in these compounds. On further cooling, the intensity of the reflection exhibits different temperature behavior, depending on the magnetic field strength: while for 0 T and 4 T, a maximum is ascertained at 10 K, a sudden increase of the intensity at 10 K and at 14 K is observed for 6 T and 8 T, respectively. The temperature dependence of the modulation wave number qMnq_{\mathrm{Mn}}, determined from the magnetic superlattice peak (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1) position, recorded for different field strengths, is presented in Figure 3(b). In the absence of an applied magnetic field and at 38 K, qMn=0.278q_{\mathrm{Mn}} = 0.278, which is about 18% smaller than qMn=0.295q_{\mathrm{Mn}} = 0.295 reported for TbMnO3_3 just below TNT_{\mathrm{N}}, which evidences for a longer magnetic modulation wavelength in TbMn0.98_{0.98}Fe0.02_{0.02}O3_3 [9, 10, 17]. In the whole temperature range here explored, qMnq_{\mathrm{Mn}} is a non-monotonous function of temperature, although the temperature dependence is a function of the magnetic field. In the TC<T<TNT_{\mathrm{C}} < T < T_{\mathrm{N}} interval, qMnq_{\mathrm{Mn}} reaches a minimum value at temperatures approaching TCT_{\mathrm{C}} as the magnetic field increases (32 K for 0 T and 24 K for 8 T). The relative variation of qMnq_{\mathrm{Mn}} in the TC<T<TNT_{\mathrm{C}} < T < T_{\mathrm{N}} range is 0.7%, a much smaller value when compared with TbMnO3_3, for which the total variation in the sinusoidal incommensurate phase is 3.7% [17].

Temperature dependencies of the intensity and $q_{\mathrm{Mn}}$ of the magnetic superlattice peak

Figure 3. Temperature dependencies of the (a) intensity and (b) qMnq_{\mathrm{Mn}} of the magnetic superlattice peak (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1), recorded at 0, 4, 6 and 8 T, as representative examples. The vertical dashed lines mark the Mn3+\mathrm{Mn}^{3+} magnetic ordering temperatures at 0 T. The colored arrows point at the critical temperature TCT_{\mathrm{C}} where the pyroelectric current density curve exhibits maximum value, while the black dashed arrows in (b) point the temperatures where anomalous increasing of qMnq_{\mathrm{Mn}} is ascertained. Inset: temperature dependence of the magnetic superlattice peak measured at B=0B = 0 T. The solid line represents the temperature trend of the peak intensity in the TC<T<TNT_{\mathrm{C}} < T < T_{\mathrm{N}} range, extrapolated to T<TCT < T_{\mathrm{C}}.

In the absence of the applied magnetic field, qMn(T)q_{\mathrm{Mn}}(T) of TbMnO3_3 decreases on cooling and remains almost temperature independent below TCT_{\mathrm{C}}, reaching values 0.276 in References [9, 10] and 0.28 in Reference [17]. In TbMn0.98_{0.98}Fe0.02_{0.02}O3_3, qMn(T)q_{\mathrm{Mn}}(T) slightly increases below 35 K and finally saturates near 0.279. Therefore, the temperature dependence is different between TNT_{\mathrm{N}} and TCT_{\mathrm{C}}, although the modulation wavevector in the ferroelectric phase takes similar value, within measurement accuracy, in the pure and iron substituted samples.

The most significant changes induced by the magnetic field concerning the temperature dependence of qMnq_{\mathrm{Mn}} are observed below TCT_{\mathrm{C}}. For B ≤ 5 T, qMn(T)q_{\mathrm{Mn}}(T) is a slowly varying temperature function on cooling in such a way that an almost constant plateau is reached, while for B ≥ 6 T, qMnq_{\mathrm{Mn}} is strongly temperature dependent, increasing as temperature decreases. At 8 T, the relative variation of qMnq_{\mathrm{Mn}} between TCT_{\mathrm{C}} and the base temperature is 0.9 %. The magnetic field threshold (B ~5.5 T) is the one for which the polarization flop is observed (see Figure 1 (c) and Figure 1 (d)). The increasing of qMn(T)q_{\mathrm{Mn}}(T) on cooling from TCT_{\mathrm{C}} contrast with the observations in TbMnO3_3, for which at 5.5 T a decrease on cooling is observed [12].

These results give clear evidence for the interplay between the mechanisms underlying the stabilization of the ferroelectricity and the modulation of the Mn3+\mathrm{Mn}^{3+} spin structure. However, the main difference here observed relatively to TbMnO3_3 concerns the effect of the applied magnetic field, having a stronger effect on the modulation wave vector in the Fe-substituted compound in the whole temperature range, while in TbMnO3_3 the effect is more pronounced in the cycloidal antiferromagnetic phase [12].

In the absence of an applied magnetic field, the (1 0 4) magnetic peak is not observed in the whole temperature range here explored. Under a 1 T strength magnetic field, this reflection appears just below TNT_{\mathrm{N}} and its intensity increases with decreasing temperature and increasing magnetic field strength, respectively, as it can be seen in Figure 4 (a). The appearance of this magnetic peak clearly points out for the stabilization of a ferromagnetic component with increasing the magnetic field. Concomitantly, the intensity of the GG-type Mn3+\mathrm{Mn}^{3+} moment ordering magnetic superlattice peak (1 qMn 3)(1\ q_{\mathrm{Mn}}\ 3), shown in Figure 4 (b), only observed below TCT_{\mathrm{C}} but already at B=0B = 0 T, decreases as the magnetic field increases.

Temperature dependence of magnetic diffraction peak intensities and neutron diffraction patterns

Figure 4. Temperature dependence of (a) the intensity of the (1 0 4)(1\ 0\ 4) magnetic diffraction peak and (b) the intensity of the magnetic superlattice peak (1 qMn 3)(1\ q_{\mathrm{Mn}}\ 3) position for TbMn0.98Fe0.02O3\mathrm{TbMn}_{0.98}\mathrm{Fe}_{0.02}\mathrm{O}_{3}, recorded at different fixed magnetic field strength. The colored arrows point at the critical temperature where the pyroelectric current density curve exhibits maximum value. Inset: neutron diffraction pattern recorded at different fixed temperatures and in the absence of applied field, showing the magnetic superlattice peak (1 qMn 3)(1\ q_{\mathrm{Mn}}\ 3).

The strong changes induced by the applied magnetic field in the neutron diffraction patterns depicted in Figure 2, point for magnetic phase transformations below the Tb3+\mathrm{Tb}^{3+} ordering temperature. The diffuse scattering signal, observed around the (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1) magnetic superlattice peak, which prevails up to 4 T, is ascribed to the quite complex and of short-range (local) ordering of Tb3+\mathrm{Tb}^{3+} spins [9, 10]. On increasing the magnetic field strength, another magnetic satellite peak starts to be observed, emerging from the diffused scattering signal, as it is shown in Figure 5 for T=5T = 5 K. This peak is indexed to the (0 0.38 1)(0\ 0.38\ 1) associated with the modulation of the Tb3+\mathrm{Tb}^{3+} spin structure induced by the applied magnetic field. The intensity and width of this magnetic satellite peak is strongly dependent on the applied magnetic field, and it disappears above 5 T. This result evidences a magnetic field-induced transition of the Tb3+^{3+} spins, with critical field strength of ∼5\sim5 T, which deserve to be further studied.

Neutron diffraction patterns of TbMn0.98Fe0.02O3 under applied magnetic fields

Figure 5. Neutron diffraction patterns of TbMn0.98_{0.98}Fe0.02_{0.02}O3_3 recorded at 5 K under several applied magnetic fields along the bb-axis. The inset shows a detailed view of the neutron diffraction patterns around the (0 qMnq_{\mathrm{Mn}} 1) peak.

Discussion

In this section, we will discuss and correlate the results obtained from polarization and neutron diffraction measurements under magnetic field to unravel the microscopic origin of the magnetically induced ferroelectricity in this compound and its magnetic field dependence. We will address the interplay between magnetism and polar properties, highlighted in Figure 6, which shows the temperature dependence of the pyroelectric current density and the intensity of the magnetic superlattice peak (0 qMnq_{\mathrm{Mn}} 1), for 0, 4, 6 and 8 T magnetic field strength, applied along the bb-axis, respectively.

Temperature dependence of the magnetic superlattice peak intensity and pyroelectric current density

Figure 6. Temperature dependence of the magnetic superlattice peak (0 qMn 10\ q_{\mathrm{Mn}}\ 1) intensity (left) and the pyroelectric current density (right), measured along the cc-axis in different magnetic fields applied along bb-axis. The solid line represents the temperature trend of the peak intensity in the TC<T<TNT_{\mathrm{C}} < T < T_{\mathrm{N}} range, extrapolated to T<TCT < T_{\mathrm{C}}.

The paramagnetic to incommensurate sinusoidal antiferromagnetic phase transition at TNT_{\mathrm{N}} is not revealed by any anomaly in the pyroelectric current density, as expected if the inverse Dzyaloshinskii-Moriya mechanism is assumed only below TCT_{\mathrm{C}}, like in TbMnO3_3 [18, 19]. The magnetically induced ferroelectric phase transition is marked by the anomalous temperature dependence of the (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1) magnetic superlattice peak intensity at TCT_{\mathrm{C}}. At zero magnetic field, the small anomaly in Jc(T)J_{\mathrm{c}}(T) occurring at 8 K, which is likely associated with the Tb3+\mathrm{Tb}^{3+} spin ordering. The correlation between the anomalous temperature dependence of both Jc(T)J_{\mathrm{c}}(T) and the magnetic superlattice peak (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1) intensity holds even for applied fields, but following different behavior: at 4 T, Jc(T)J_{\mathrm{c}}(T) exhibits a downward peak at 4 K and the magnetic superlattice peak intensity reaches a maximum value at 10 K; for 6 and 8 T, the downward peak of Jc(T)J_{\mathrm{c}}(T), whose amplitude increases with the field strength, is accompanied by a sudden increase of the slope of the temperature dependence of the magnetic superlattice peak intensity. The spin cycloid is a polar magnetic structure, generating electric polarization in the spin-plane, perpendicularly to the propagation vector (P∼k×(Si×Sj)P \sim k \times(S_i \times S_j)) [18, 19]. In the bcbc-cycloid phase, the electric polarization is expected to be along the cc-axis, while in the abab-cycloid phase, to be along the aa-axis. During the cycloid plane rotation from the bcbc- to the abab-plane, it is expected an increase of intensity of the (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1) magnetic superlattice peak, simply because in the experimental geometry here described, neutrons probe only the component of magnetic moment perpendicular to the scattering vector, being this component larger when the spins are confined within the abab-plane. The results here presented evidence for a strong interplay between the modulated magnetic Mn3+\mathrm{Mn}^{3+} spin structure and the stabilization of the electric polarization, as expected in type-II multiferroics.

The interplay between the magnetic structure, electric polarization and magnetoelectric coupling is better ascertained by comparative plots at fixed temperatures. For this purpose, we represented in Figure 7 the magnetic field dependence of Pc(T)P_{\mathrm{c}}(T), measured with applied magnetic field along the three crystallographic directions, the modulation wave vector qMnq_{\mathrm{Mn}}, determined from the magnetic superlattice peak (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1) position, and, in inset, the intensity of the magnetic superlattice (1 qMn 3)(1\ q_{\mathrm{Mn}}\ 3) (left axis) and of the ferromagnetic (right axis) peaks. Here, we chose to analyze these quantities as a function of the magnetic field strength at 18 K (for which the aa-axis component of the polarization is not observed up to 8 T), 12 K (for which the polarization rotates with applied magnetic field), and 5 K (to study the Tb3+\mathrm{Tb}^{3+}-spin ordering effect), which represent the overall trend of the aforementioned quantities.

Magnetic field dependence of the electric polarization and modulation wave vector

Figure 7. Magnetic field dependence of the electric polarization PcP_{\mathrm{c}} measured along the cc-axis in external magnetic field applied along the aa-, bb- and cc-axes, and the modulation wave vector qMnq_{\mathrm{Mn}}, calculated from the (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1) peak position, measured at 18 K (a, b), 12 K (c, d) and 5 K (e, f). Insets: magnetic field dependence of the intensity of the (1 qMn 3)(1\ q_{\mathrm{Mn}}\ 3) magnetic superlattice peak (left red) and the (1 0 4)(1\ 0\ 4) magnetic peak (right blue).

For the three chosen representative temperatures, Pc(B)P_{\mathrm{c}}(B) exhibits different magnetic field dependences according to the applied magnetic field direction, mirroring the anisotropic nature of the magnetoelectric coupling. In the 8 to 22 K range, Pc(B)P_{\mathrm{c}}(B) is a linear function of B∥bB \parallel b below and above 4.5 T, although with different slopes; it is a linear function of B∥aB \parallel a only for $B_{\mathrm{a}} < 4 TT; and has a non-linear dependence with B∥cB \parallel c, eventually disappearing above a certain value of magnetic field which depends on temperature.

From the slopes of the linear relation between PcP_c and B∥bB \parallel b strength (BbB_b), we have estimated the effective magnetoelectric coefficient α32=dPc/dBb\alpha_{32}=dP_c/dB_b and its temperature dependence is presented in Figure 8, below and above 4 T.

Temperature dependence of the effective magnetoelectric coefficient of TbMnO3 and TbMn0.98Fe0.02O3

Figure 8. Temperature dependence of the effective magnetoelectric coefficient α32\alpha_{32} of TbMnO3_3 and TbMn0.98_{0.98}Fe0.02_{0.02}O3_3, for (a) Bb<4B_b < 4 T and (b) Bb>4B_b > 4 T. The solid lines are guide for the eyes. Data concerning TbMnO3_3 was taken from Ref. [14].

The effective magnetoelectric coefficient of TbMn0.98_{0.98}Fe0.02_{0.02}O3_3 is negative, mirroring the decrease the polarization with the magnetic field increase. The value of the magnetoelectric coefficient is one order of magnitude larger for Bb>4B_b > 4 T. In both magnetic field ranges, the absolute value α32\alpha_{32} increases monotonously as temperature decreases, giving evidence for the strengthening of the magnetic field dependence of the electric polarization as the temperature/magnetic field decreases/increases down to 8 K.

Comparing with TbMnO3_3, two different regimes are found, as it is clear from Figure 8. For applied magnetic field strength below 4 T, the effective magnetoelectric coefficient α32=dPc/dBb\alpha_{32}=dP_c/dB_b obtained for TbMnO3_3 is exactly 0, meaning that while the polarization does not rotate towards the aa-axis, its value is independent of the applied magnetic field. In contrast, TbMn0.98_{0.98}Fe0.02_{0.02}O3_3 has a finite negative α32\alpha_{32} coefficient for the same temperature and magnetic field strength. This result proves the role played by the Fe3+^{3+} magnetism, that even a low level substitution slightly changes the cycloidal ordering, in agreement with the neutron data that show the promotion of a canted structure already at 1 T applied magnetic field. However, above 4 T, the modulus of the effective magnetoelectric coefficient of TbMnO3_3 becomes higher than the one calculated for TbMn0.98_{0.98}Fe0.02_{0.02}O3_3, due to a sharper rotation of the cycloid ordering with the applied magnetic field. The difference between both values increasing as temperature decreases, in such a way that at 8 K the effective magnetoelectric coefficient of the pure compound is almost 4 times larger than in the Fe-substituted compound. This demonstrates the strong impact of low-level substitution of Mn3+^{3+} by Fe3+^{3+} in the electric polarization dependence on the low applied magnetic field.

Figure 7(b) and Figure 7(d) show the magnetic field dependence of the modulation wave vector qMnq_{\mathrm{Mn}}, recorded at 18 K and 12 K, respectively. Two linear regimes in qMn(Bb)q_{\mathrm{Mn}}(B_b) are ascertained below and above 4.5 T, with a slope increasing from the low to high magnetic field ranges. It is worth to stress that the magnetic field dependence of both Pc(Bb)P_c(B_b) and qMn(Bb)q_{\mathrm{Mn}}(B_b) is rather similar, evidencing for a correlation between PcP_c and the modulated magnetic structure. To discuss the microscopic origin of the magnetically induced ferroelectricity in this compound, we have analyzed the correlation between the electric polarization PcP_c and the (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1) magnetic superlattice peak characteristics, as it better mirrors the cycloidal spin structure underlying the electric polarization. Following the grounds of the spin current model, presented by Y. Yamasaki [20], the electric polarization is predicted to be proportional to the product of sin⁡(2πqMn)\sin(2\pi q_{\mathrm{Mn}}) and the square of the magnetic structural factor. Unfortunately, the geometric properties of the spin cycloid in this compound could not be determined from our experimental results, and the accurate determination of the magnetic structural factor is not possible. However, we can overcome this difficulty looking at the intensity II of the (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1) magnetic superlattice peak, which is proportional to the square of the magnetic structural factor. Figure 9(a) shows PcP_c as a function of I×sin⁡(2πqMn)I \times\sin(2\pi q_{\mathrm{Mn}}), measured at different temperatures and 0 T. The linear regime observed in the absence of applied field evidences that the mechanism underlying the magnetoelectric coupling is based on the spin current model applied to a noncolinear spin structure. Interesting is to study the same dependence but at constant temperature and for different applied magnetic field. This study is performed at 18 K where the polarization flip is not observed in the magnetic field range explored in this work. As it can be observed in Figure 9(b), for B<4B < 4 T, a linear regime is already found, evidencing that the same microscopic mechanism also prevails in this magnetic field range. However, for B>4B > 4 T, a clear deviation of the linear regime is ascertained, enabling us to conclude that the magnetoelectric coupling for B>4B > 4 T is not accurately described by the model in Ref. [20]. Actually, the linear dependence of PcP_c on I×sin⁡(2πqMn)I \times\sin(2\pi q_{\mathrm{Mn}}) is broken for magnetic fields above 4 T, as it can be observed in the inset of Figure 9(b). It is worth to stress that qMnq_{\mathrm{Mn}} is quite temperature independent for B<4B < 4 T, while it becomes strongly temperature dependent for higher fields (see Figure 3(b)). The change of magnetic modulation properties at ∼4\sim4 T is undoubtedly in the basis of the change of microscopic mechanisms underlying ferroelectricity. No similar study has been published in TbMnO3_3, to the best of our knowledge, and therefore this work provides a better understanding of the influence of the applied magnetic field on the microscopic mechanisms that induce electric polarization in this class of multiferroics.

Plots of $P_c$ versus $I \times \sin(2\pi q_{\mathrm{Mn}})$

Figure 9. PcP_c versus I×sin⁡(2πqMn)I \times\sin(2\pi q_{\mathrm{Mn}}) recorded at 0 T for different temperatures (a) and at 18 K with magnetic field B∥bB \parallel b (b). The intensity II and qMnq_{\mathrm{Mn}} values were calculated from the (0 qMn 1)(0\ q_{\mathrm{Mn}}\ 1) magnetic superlattice peak. Inset: PcP_c versus I×sin⁡(2πqMn)I \times\sin(2\pi q_{\mathrm{Mn}}) recorded at 4 T and 6 T, for different temperatures.

Now, we focus on the decrease of PcP_c of TbMn0.98_{0.98}Fe0.02_{0.02}O3_3 for B∥bB \parallel b at 18 K with increasing magnetic field strength. It is worth to stress that at this temperature and for maximum magnetic field strength here applied, no polarization flop occurs. At this temperature, the intensity of the ferromagnetic reflection is a linear increasing function of B∥bB \parallel b, and no anomaly is ascertained at ∼4.5\sim4.5 T (see inset of Figure 7(b)), which gives clear evidence for the increase of the ferromagnetic component induced by the applied magnetic field, likely due to a spin canting. The destabilization of the cycloidal Mn3+^{3+} spin modulation, along with the concomitant appearance of a ferromagnetic component, explain the decrease of the PcP_c. This result obtained for TbMn0.98_{0.98}Fe0.02_{0.02}O3_3 contrasts with the one obtained for pure TbMnO3_3 from which we conclude that the magnetic field promoted spin canting is a consequence of the Fe spins, even in only 2% concentration [14]. Similar magnetic changes are perceived down to 8 K. Future experiments will be performed to confirm this interpretation.

The magnetoelectric coupling at 5 K exhibits different properties. Strictly, qMnq_{\mathrm{Mn}} is no longer a linear function of the applied magnetic field (see Figure 7(f)) and a hint of a downward jump is ascertained at 3.5 T. Interestingly, the magnetic field dependence of the GG-type magnetic superlattice peak (1 qMnq_{\mathrm{Mn}} 3) intensity exhibits a maximum value at 3 T and becomes magnetic field independent above 5 T, while the (1 0 4) magnetic reflection intensity exhibits an s-shaped anomaly at 5 T. Revisiting Figure 7(f), we can assign the aforementioned intensity changes at 5 T to the magnetically induced phase transition. The different behavior described to the one above is a consequence of the Tb3+\mathrm{Tb}^{3+} magnetic ordering on the magnetoelectric coupling at 5 K.

To summarize the results here presented, we propose the magnetoelectric phase diagram of TbMn0.98Fe0.02O3\mathrm{TbMn}_{0.98}\mathrm{Fe}_{0.02}\mathrm{O}_{3} shown in Figure 10, with magnetic fields along the (a) aa-, (b) bb-, and (c) cc-axes.

Magnetoelectric phase diagram of TbMn₀.₉₈Fe₀.₀₂O₃ for magnetic fields along the a-, b-, and c-axes

Figure 10. The magnetoelectric phase diagram of TbMn0.98Fe0.02O3\mathrm{TbMn}_{0.98}\mathrm{Fe}_{0.02}\mathrm{O}_3, with magnetic fields along the (a) aa-, (b) bb-, and (c) cc-axes. Antiferromagnetic structure has incommensurate sinusoidal modulation between TNT_\mathrm{N} and TCT_\mathrm{C} and cycloidal modulation below TCT_\mathrm{C}.

Conclusions

In this work we report a combined experimental study of the temperature and magnetic field dependence of polarization and magnetic structures in TbMn0.98Fe0.02O3\mathrm{TbMn}_{0.98}\mathrm{Fe}_{0.02}\mathrm{O}_3 single crystal. The results show that the low-level of Mn3+\mathrm{Mn}^{3+} substitution for Fe3+\mathrm{Fe}^{3+}, although does not change the phase sequence regarding TbMnO3\mathrm{TbMnO}_3, it causes a higher magnetic field sensitivity of the electric polarization for B<4 TB < 4\ \mathrm{T}. This is due to the changes on the magnetic modulation of the Mn3+\mathrm{Mn}^{3+} spin structure. Two main consequences arise from the magnetic structure changes: i) the value of the electric polarization is lower than in TbMnO3_3, and ii) the magnetoelectric coupling coefficient α32\alpha_{32} at low magnetic fields below 4 T is finite, ranging between -0.005 ns/m to -0.01 ns/m, contrasting with the vanishing value reported for TbMnO3_3, meaning that while the polarization does not rotate towards the a-axis, its value is independent of the applied magnetic field. We attribute this magnetoelectric performance enhancement to the effect of the Fe3+^{3+} magnetism which alters the magnetic interactions in such extent that the magnetic structure allowing for ferroelectricity, according to Dzyaloshinskii–Moriya interaction, is no longer stable at high magnetic fields. Our experimental work evidences that the low-level substitution of Mn3+^{3+} by Fe3+^{3+}, though keeping the same phase sequence, induces significant changes in properties and evidences for the rather delicate balance between the competitive magnetic interactions underlying the ground state of TbMnO3_3.

Acknowledgments

This work was supported by the VEGA 2/0137/19 project, the Czech Science Foundation (Project No. 21-06802S), Project from the European Union and the Czech Ministry of Education, Youth and Sports (Project TERAFIT-CZ.02.01.01/00/22 008/0004594), PTDC/FIS-MAC/29454/2017, NORTE/01/0145/FEDER/028538, IFIMUP: Norte-070124-FEDER-000070;NECL: NORTE-01-0145-FEDER-022096, UIDB/04968/2020, UID/NAN/50024/2019, PTDC/NAN-MAT/28538/2017 and PTDC/FIS/03564/2022.

Competing interests

The authors declare no competing interests.

Strong impact of low-level substitution of Mn by Fe on the magnetoelectric coupling in TbMnO3

A. Maia; R. Vilarinho; P. Proschek; M. Lebeda; M. Mihalik jr.; M. Mihalik; P. Manuel; D. D. Khalyavin; S. Kamba; J. Agostinho Moreira

Magnetic field dependence of the electric polarization $P_c$ measured along the $c$-axis in external magnetic field applied along the $a$-, $b$- and $c$-axes.

Figure S3. Magnetic field dependence of the electric polarization PcP_c measured along the cc-axis in external magnetic field applied along the aa-, bb- and cc-axes.

References

  1. [1]S. Dong, J. M. Liu, S. W. Cheong, and Z. Ren, Multiferroic Materials and Magnetoelectric Physics: Symmetry, Entanglement, Excitation, and Topology, Adv. Phys. 64, 519 (2015).DOI
  2. [2]Y. Tokura, S. Seki, and N. Nagaosa, Multiferroics of Spin Origin, Rep. Prog. Phys. 77, 076501 (2014).DOI
  3. [3]A. Maia, R. Vilarinho, C. Kadlec, M. Lebeda, M. Mihalik, M. Zentková, M. Mihalik, J. A. Moreira, and S. Kamba, Modifying the Magnetoelectric Coupling in TbMnO₃ by Low-Level Fe³⁺ Substitution, Phys. Rev. B 107, 104410 (2023).DOI
  4. [4]M. Mihalik, M. Mihalik, M. Zentková, A. Maia, R. Vilarinho, A. Almeida, J. Agostinho Moreira, J. Pospíšil, and K. Uhlířová, Magnetic Properties of TbMn₀.₉₈Fe₀.₀₂O₃ Single Crystal, J. Magn. Magn. Mater. 549, 168986 (2022).DOI
  5. [5]M. Mihalik, M. Mihalik, Z. Jagličíć, R. Vilarinho, J. A. Moreira, E. Queiros, P. B. Tavares, A. Almeida, and M. Zentková, Magnetic Phase Diagram of the TbMn₁₋ₓFeₓO₃ solid Solution System, Physica B Condens. Matter. 506, 163 (2017).DOI
  6. [6]R. Vilarinho, E. Queirós, D. J. Passos, D. A. Mota, P. B. Tavares, M. Mihalik, M. Zentkova, M. Mihalik, A. Almeida, and J. A. Moreira, On the Ferroelectric and Magnetoelectric Mechanisms in Low Fe³⁺ doped TbMnO₃, J. Magn. Magn. Mater. 439, 167 (2017).
  7. [7]R. Vilarinho, D. J. Passos, E. C. Queirós, P. B. Tavares, A. Almeida, M. C. Weber, M. Guennou, J. Kreisel, and J. A. Moreira, Suppression of the Cooperative Jahn-Teller Distortion and its Effect on the Raman Octahedra-Rotation Modes of TbMn₁₋ₓFeₓO₃, Phys. Rev. B 97, 144110 (2018).DOI
  8. [8]T. Kimura, T. Goto, H. Shintani, K. Ishizaka, T. Arima, and Y. Tokura, Magnetic Control of Ferroelectric Polarization, Nature 426, 55 (2003).pubmed.ncbi.nlm.nih.gov/14603314
  9. [9]M. Kenzelmann, A. B. Harris, S. Jonas, C. Broholm, J. Schefer, S. B. Kim, C. L. Zhang, S.W. Cheong, O. P. Vajk, and J. W. Lynn, Magnetic Inversion Symmetry Breaking and Ferroelectricity in TbMnO₃, Phys. Rev. Lett. 95, 087206 (2005).DOI
  10. [10]R. Kajimoto, H. Yoshizawa, H. Shintani, T. Kimura, and Y. Tokura, Magnetic Structure of TbMnO₃ by Neutron Diffraction, Phys. Rev. B 70, 012401 (2004).
  11. [11]T. Kimura, S. Ishihara, H. Shintani, T. Arima, T. Takahashi, K. Ishizaka, and Y. Tokura, Distorted Perovskite with E_g¹ Configuration as a Frustrated Spin System, Phys. Rev. B 68, 060403 (2003).DOI
  12. [12]T. Arima, T. Goto, Y. Yamasaki, S. Miyasaka, K. Ishii, M. Tsubota, T. Inami, Y. Murakami, and Y. Tokura, Magnetic-Field-Induced Transition in the Lattice Modulation of Colossal Magnetoelectric GdMnO₃ and TbMnO₃ Compounds, Phys. Rev. B 72, 100102 (2005).DOI
  13. [13]T. Goto, T. Kimura, G. Lawes, A. P. Ramirez, and Y. Tokura, Ferroelectricity and Giant Magnetocapacitance in Perovskite Rare-Earth Manganites, Phys. Rev. Lett. 92, 257201 (2004).pubmed.ncbi.nlm.nih.gov/15245056
  14. [14]T. Kimura, G. Lawes, T. Goto, Y. Tokura, and A. P. Ramirez, Magnetoelectric Phase Diagrams of Orthorhombic RMnO₃ (R=Gd, Tb, and Dy), Phys. Rev. B 71, 224425 (2005).DOI
  15. [15]N. Aliouane, D. N. Argyriou, J. Strempfer, I. Zegkinoglou, S. Landsgesell, and M. V. Zimmermann, Field-Induced Linear Magnetoelastic Coupling in Multiferroic TbMnO₃, Phys. Rev. B 73, 020102 (2006).DOI
  16. [16]See Supplemental Material at [URL] for Additional Data on Neutron Diffraction.
  17. [17]S. Quezel, F. Tcheou, J. Rossat-Mignod, G. Quezel, and E. Roudaut, Magnetic Structure of the Perovskite-like Compound TbMnO3, Physica B+C 86–88, 916-918 (1977).DOI
  18. [18]I. A. Sergienko and E. Dagotto, Role of the Dzyaloshinskii-Moriya Interaction in Multiferroic Perovskites, Phys. Rev. B 73, 094434 (2006).
  19. [19]H. Katsura, N. Nagaosa, and A. V. Balatsky, Spin Current and Magnetoelectric Effect in Noncollinear Magnets, Phys. Rev. Lett. 95, 057205 (2005).pubmed.ncbi.nlm.nih.gov/16090916
  20. [20]Y. Yamasaki, H. Sagayama, T. Goto, M. Matsuura, K. Hirota, T. Arima, and Y. Tokura, Electric Control of Spin Helicity in a Magnetic Ferroelectric, Phys. Rev. Lett. 98, 147204 (2007).DOI

Paper details

vlnc:W_na2vnpd6
Version
v1 · latest
Published
Fresh — added to the Hub within the last 30 days
Added
License
CC BY 4.0
Usage

views · 0

downloads · 0

A view counts once per browser per day, a download each time the PDF is requested.

  • Physics and Astronomy

Not recorded for this paper

View statement
Looking for related papers…
Contents